Electrical insulating composition and power cable
The electrical insulating composition with polyethylene, thermoplastic elastomer, and polyalkylene glycol in specific ratios addresses water treeing in power cables by trapping water and maintaining spherical water tree shapes, enhancing resistance and insulation.
Patent Information
- Application Number
- PCT/JP2025/017340
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Power cables used in humid or submerged environments suffer from water treeing, which reduces insulation performance due to the formation of water trees that are not adequately addressed by existing compositions containing polyethylene and thermoplastic elastomers.
An electrical insulating composition comprising polyethylene, a thermoplastic elastomer, and polyalkylene glycol within specific content ratios forms a phase structure that suppresses water tree formation by trapping water and maintaining a spherical shape, thereby enhancing water tree resistance.
The composition effectively reduces the number and length of water trees, stabilizes their spherical shape, and maintains high insulation and mechanical properties, preventing dielectric breakdown.
Smart Images

Figure JP2025017340_19112026_PF_FP_ABST
Abstract
Description
Electrical insulation composition and power cable
[0001] This disclosure relates to electrical insulation compositions and power cables.
[0002] Due to its excellent insulating properties, polyethylene is widely used as a base resin for electrical insulating compositions that constitute the insulating layer in power cables and the like (for example, Patent Document 1).
[0003] Japanese Unexamined Patent Publication No. 57-69611
[0004] According to one aspect of the present disclosure, an electrical insulating composition is provided which contains a resin component comprising polyethylene and a thermoplastic elastomer, and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component.
[0005] Figure 1 is a cross-sectional view perpendicular to the axial direction of a power cable according to one embodiment of the present disclosure. Figure 2 is a schematic diagram illustrating the occurrence of water trees in an electrical insulating composition according to one embodiment of the present invention. Figure 3 is a schematic diagram illustrating the occurrence of water trees in a conventional electrical insulating composition. Figure 4 is a schematic cross-sectional view showing a water needle test.
[0006] [Problems this disclosure aims to solve] When power cables are energized in a humid or submerged environment, water treeing may occur in the insulating layer. Therefore, it is necessary to improve the water treeing resistance in the insulating layer, along with the cable characteristics required for power cables.
[0007] The purpose of this disclosure is to provide a technology that can improve water tree resistance while ensuring the characteristics of the cable.
[0008] [Effects of this disclosure] According to this disclosure, it is possible to improve water tree resistance while ensuring cable characteristics.
[0009] [Description of Embodiments of this Disclosure] <Knowledge Obtained by the Inventors> First, the knowledge obtained by the inventors will be explained.
[0010] From a practical standpoint, power cables are required to have high insulation, mechanical properties, flexibility, and low dielectric loss tangent. Furthermore, since power cables are laid in humid or submerged environments, water tree resistance is also required. In humid environments, when a certain electric field is applied to the insulation layer of a power cable, water treeing occurs within the insulation layer, reducing the insulation performance of the power cable.
[0011] Water trees can form through the following mechanism, for example: In humid or submerged environments, water can penetrate the insulation layer of a power cable. When water penetrates the insulation layer while the power cable is energized, the water condenses in areas where localized electric field concentrations occur within the insulation layer. Examples of such localized electric field concentrations include voids and foreign matter in the insulation layer, and irregularities at the interface between the insulation layer and the semiconducting layer. When water condenses in such localized electric field concentrations, the resulting pressure increase of the condensed water causes mechanical strain around the area of water condensation. As a result, tree-like or bow-tie-shaped water trees form within the insulation layer.
[0012] Conventionally, to suppress the occurrence of water trees in the insulating layer of power cables, methods such as compounding a thermoplastic elastomer with polyethylene have been proposed. Thermoplastic elastomers can reduce the number and length of water trees by incorporating foreign matter that serves as the starting point for water tree formation. Furthermore, they can trap water that penetrates the insulating layer, suppressing water aggregation on the polyethylene.
[0013] Incidentally, in recent years, the specifications required for power cables laid in humid or flooded environments have become stricter. Therefore, there is a demand for power cables with even greater water tree resistance than conventional cables.
[0014] Traditionally, water tree resistance was evaluated by immersing the power cable in water and applying an electric field to the insulating layer. In this test, the water pressure and electric field were applied uniformly to the insulating layer. On the other hand, the water needle test is a method for evaluating higher water tree resistance. The water needle test, as will be described in detail later, is a water tree test that uses a water needle that simulates minute foreign matter or minute voids incorporated into the electrical insulating composition.
[0015] The inventors conducted a water needle test on an electrical insulating composition containing polyethylene and a thermoplastic elastomer and found that while the number and length of water trees could be reduced, high water tree resistance could not be consistently obtained. Further investigation revealed that in the above composition system, the shape of the water trees was special, with some parts protruding or distorted.
[0016] Here, the phase structure and the generation of water trees will be explained using Figure 3. Figure 3 is a schematic diagram illustrating the generation of water trees in a conventional electrical insulating composition. As shown in Figure 3, polyethylene constitutes the sea phase 1', and thermoplastic elastomer constitutes the island phase 2' dispersed in the sea phase 1'. When a needle 6 is inserted into such a composition and an electric field is applied, water trees 5' are generated by the aggregation of water that has entered the composition. Water trees 5' selectively advance through the polyethylene sea phase 1' rather than the island phase 2' of the thermoplastic elastomer. Since the island phase 2' is finely dispersed in the sea phase 1', the water trees 5' will advance through the gaps between the island phases 2'. As a result, the water trees 5' may protrude or take on an irregular shape. Such water trees 5' are prone to advancing when the power cable is energized and may significantly reduce its insulating properties.
[0017] Previously, the number and length of water trees were considered important for improving water tree resistance. However, water needle testing revealed that the shape of the generated water trees is also crucial, and that their shape should be close to a spherical shape, free from protrusions and distortions. In other words, even if the number of water trees is reduced or their length is shortened, if their shape is distorted, the dielectric breakdown of the insulating layer caused by water trees cannot be reliably suppressed. The fact that the shape of water trees also affects resistance could not be confirmed by immersion testing, but was only discovered through the more stringent water needle testing.
[0018] The inventors investigated various compositions from the viewpoint of making water trees closer to a spherical shape, and in the process found that mixing in polyethylene glycol is beneficial. A three-component system containing polyethylene glycol can reduce the number of water trees generated and shorten their length, while still making the shape of the generated water trees closer to a spherical shape.
[0019] Furthermore, by setting the additive ratios of polyethylene, thermoplastic elastomer, and polyalkylene glycol within a predetermined range, a high level of balance between cable properties and water tree resistance can be achieved.
[0020] This invention is based on the above findings.
[0021] <Embodiments of this Disclosure> Next, embodiments of this disclosure will be described by listing them.
[0022] [1] One aspect of the present disclosure is an electrical insulating composition comprising a resin component containing polyethylene and a thermoplastic elastomer, and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component. With this configuration, water tree resistance can be improved while ensuring the various characteristics of the cable.
[0023] [2] Another aspect of the present disclosure is a power cable comprising: a conductor; and an insulating layer provided on the outer circumference of the conductor and formed from an electrical insulating composition, wherein the electrical insulating composition contains a resin component comprising polyethylene and a thermoplastic elastomer; and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component. With this configuration, water tree resistance can be improved in a power cable while ensuring the cable characteristics.
[0024] [3] In the power cable described in [2] above, the thermoplastic elastomer is at least one of an olefin-based thermoplastic elastomer having olefin units and a styrene-based thermoplastic elastomer having styrene units. This configuration can further improve water tree resistance.
[0025] [4] In the power cable described in [2] or [3] above, the polyethylene is low-density polyethylene. This configuration allows for further improvement of the mechanical properties of the insulating layer.
[0026] In the power cable described in any one of [2] to [4], the polyalkylene glycol is polyethylene glycol. This configuration further improves the water tree resistance of the insulating layer.
[0027] [6] In the power cable described in any one of [2] to [5] above, the electrical insulation composition has a phase structure in which the polyethylene constitutes the sea phase, the thermoplastic elastomer constitutes the island phase dispersed in the sea phase, and the polyalkylene glycol is dispersed in the island phase. With this configuration, cable characteristics and water tree resistance can be achieved at a higher level.
[0028] [7] In the power cable described in any one of [2] to [6] above, the insulating layer has a maximum length of water tree generated by a water needle test of 200 μm or less, and the ratio of the long side to the short side of the water tree is 2.0 or less. Here, the water needle test includes the steps of: providing a flat electrode on the first surface of a block taken from the insulating layer; forming a needle-shaped void at a position opposite to the first surface at a distance of 1 mm, such that the void has a tip with a radius of curvature of 10 μm; injecting artificial seawater with a salinity of 3.8 mass% into the void to form a water needle in the block; and applying an AC voltage of 1000 Hz and 4 kV between the flat electrode and the tip of the water needle for 30 days. With this configuration, the shape of the water tree in the insulating layer can be made small while being close to a spherical shape.
[0029] [8] In the power cable described in any one of [2] to [7] above, when the insulating layer is immersed in artificial seawater with a salinity of 3.8% by mass at room temperature and an AC voltage of 1000 Hz and 4 kV is applied to the insulating layer for 30 days, the number density of water trees generated in the insulating layer and having a length of 50 μm or more is 2,000 trees / cm². 3 It is less than [amount missing]. With this configuration, the occurrence of water trees in the insulating layer can be suppressed.
[0030] [Details of Embodiments of the Disclosure] An embodiment of the Disclosure is described below. However, the Disclosure is not limited to these examples, and all modifications are intended to be included in the meaning and scope equivalent to the claims, as indicated by the claims.
[0031] [One Embodiment of the Present Disclosure] (1) Electrical Insulation Composition The electrical insulation composition of this embodiment is a material that constitutes the insulating layer 130 of the power cable 10, which will be described later. The electrical insulation composition comprises at least a resin component including polyethylene and a thermoplastic elastomer, polyalkylene glycol, and other additives as needed. Hereinafter, the electrical insulation composition will also be simply referred to as "the composition".
[0032] (Polyethylene) Polyethylene constitutes the main component of the resin component. Examples of polyethylene include low-density polyethylene (LDPE: density 0.88 g / cm 3 or more and 0.93 g / cm 3 or less), linear low-density polyethylene (LLDPE: density 0.945 g / cm 3 or less), medium-density polyethylene (MDPE: density 0.93 g / cm 3 or more and 0.942 g / cm 3 or less), high-density polyethylene (HDPE: density 0.942 g / cm 3 or more), and the like.
[0033]
[0033] From the viewpoint of achieving a predetermined phase structure described later in the composition, LDPE is preferable as the polyethylene. According to LDPE, the insulating properties and mechanical properties of the insulating layer can be maintained at a high level. From the viewpoint of maintaining even higher insulating properties and mechanical properties of the insulating layer, the density of LDPE is preferably 0.89 g / cm 3 or more and 0.91 g / cm 3 or less.
[0034] The melt flow rate (MFR) of polyethylene is, for example, preferably 0.8 g / 10 min or more and 2.3 g / 10 min or less. The MFR is a value measured at a temperature of 190°C and a load of 2.16 kg in accordance with JIS K7210.
[0035] (Thermoplastic Elastomer) The thermoplastic elastomer is finely dispersed in polyethylene by mixing with polyethylene. The thermoplastic elastomer has lower crystallinity than polyethylene, and contributes to improving the flexibility of the electrical insulating composition. In addition, since the thermoplastic elastomer is flexible, it easily incorporates foreign matter when mixed with polyethylene, and contributes to suppressing the occurrence of water trees. Moreover, it suppresses the growth of water trees and also contributes to reducing their maximum length.
[0036] The thermoplastic elastomer may be any component that can improve the flexibility of the composition, and for example, known components such as amide-based, ester-based, olefin-based, styrene-based, urethane-based, vinyl chloride-based, and fluorine-based components can be used. Among these, from the viewpoint of fine dispersion when mixed with polyethylene, it is preferable to use at least one of styrene-based and olefin-based elastomers. According to the styrene-based elastomer, electrons can be trapped in the aromatic ring possessed by styrene to form a stable resonance structure. Therefore, even when water aggregates in the captured foreign matter, it is possible to alleviate electric field concentration caused by the aggregation. Moreover, due to its flexibility, the occurrence of mechanical stress cracks can be suppressed. By these means, the occurrence of water trees in the composition can be suppressed. According to the olefin-based elastomer, it is easier to mix with polyethylene compared to the styrene-based elastomer, and the generation of voids in the composition can be suppressed. Thereby, the occurrence of water trees in the composition can be suppressed.
[0037] The styrene-based thermoplastic elastomer is a copolymer containing styrene units as a hard segment and at least one monomer unit selected from ethylene, propylene, butylene, isoprene and the like as a soft segment.
[0038] Examples of the styrene-based thermoplastic elastomer include a styrene-butadiene-styrene block copolymer (SBS), a hydrogenated styrene-butadiene-styrene block copolymer, a styrene-isoprene-styrene copolymer (SIS), a hydrogenated styrene-isoprene-styrene copolymer, a hydrogenated styrene-butadiene rubber, a hydrogenated styrene-isoprene rubber, and a styrene-ethylene-butylene-olefin crystal block copolymer. Two or more of these may be used in combination.
[0039] In this context, "hydrogenation" refers to the addition of hydrogen to a double bond. For example, "hydrogenated styrene-butadiene-styrene block copolymer" means a polymer in which hydrogen has been added to the double bond of a styrene-butadiene-styrene block copolymer. Note that hydrogen is not added to the double bond of the aromatic ring of styrene. "Hydrogenated styrene-butadiene-styrene block copolymer" can be rephrased as styrene-ethylene-butylene-styrene block copolymer (SEBS).
[0040] The styrene unit content in a styrene-based thermoplastic elastomer is not particularly limited, but from the viewpoint of the flexibility of the composition and its miscibility with polyethylene, it is preferable to have a content of 10% to 45% by mass. Furthermore, by keeping the styrene unit content within the above range, a predetermined amount of monomer units, such as ethylene units, can be secured as soft segments, thereby improving the compatibility between the styrene-based thermoplastic elastomer and polyethylene. This allows for stable improvement of the water resistance and insulation properties of the composition.
[0041] Olefin-based thermoplastic elastomers (so-called TPOs) are composed of a hard segment comprising at least one olefin unit of polyethylene and polypropylene, and a soft segment comprising an ethylene-α-olefin copolymer unit. Olefin-based thermoplastic elastomers may be copolymer types of olefin units and ethylene-α-olefin copolymer units, or mixed types of olefins and ethylene-α-olefin copolymers. Among these, copolymers are preferable from the viewpoint of miscibility with polyethylene. The α-olefin is a linear or branched α-olefin having 2 to 8 carbon atoms, and examples of ethylene, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, etc., can be used. Note that olefin-based thermoplastic elastomers may be used alone or in combination of two or more types.
[0042] The MFR of the thermoplastic elastomer is preferably 1.5 g / 10 min to 4.5 g / 10 min from the viewpoint of compatibility with polyethylene, and may be 0.8 g / 10 min to 6.5 g / 10 min. By using such an MFR, the above-described phase structure can be stably formed in the resin composition.
[0043] From the perspective of fine dispersion when mixed with polyethylene, it is desirable for thermoplastic elastomers to have a small difference in MFR (Mean Fiber Rate) from that of polyethylene. Specifically, it is desirable for the difference in MFR between polyethylene and thermoplastic elastomer to be 3.0 g / 10 min or less.
[0044] (Polyalkylene glycol) Polyalkylene glycol is composed of repeating alkylene oxide units and has multiple ether groups. When mixed with resin components containing polyethylene and thermoplastic elastomers, polyalkylene glycol is more easily dispersed in thermoplastic elastomers than in polyethylene. Polyalkylene glycol readily captures water and can suppress water aggregation in polyethylene. This suppresses the occurrence and growth of water trees.
[0045] The behavior and dispersibility of polyalkylene glycols in resin compositions tend to differ depending on their molecular weight. According to the inventors' research, the lower the molecular weight of polyalkylene glycol, the easier it is to dissolve at lower temperatures and the more easily it undergoes minute vibrations. An increase in molecules that undergo minute vibrations can lead to an increase in the dielectric loss tangent of the composition. On the other hand, while a higher molecular weight allows for a smaller and more suppressed electrostatic loss tangent, polyalkylene glycols become more compatible with polyethylene and less likely to disperse in thermoplastic elastomers. As a result, the inherent water-capturing effect of polyalkylene glycol becomes less pronounced, and the occurrence of water trees cannot be reliably suppressed. In this regard, the number-average molecular weight of polyalkylene glycol is preferably between 4,000 and 8,000, and may also be between 5,500 and 6,500. By having the above number-average molecular weight, polyalkylene glycol can disperse in thermoplastic elastomers and form the phase structure described later, while maintaining a small dielectric loss tangent of the composition. Hereafter, the number-average molecular weight will also be simply referred to as molecular weight. Furthermore, the number-average molecular weight for polyalkylene glycol is shown as the value measured by gel permeation chromatography (GPC).
[0046] Polyalkylene glycols such as polyethylene glycol and polypropylene glycol can be used. Among these, polyethylene glycol is preferable. Polyethylene glycol has high hydrophilicity and easily captures water, so it can more reliably suppress the occurrence of water trees.
[0047] (Other additives) The composition of this embodiment may further contain, if necessary, crosslinking agents, crosslinking aids, antioxidants, inorganic fillers, lubricants, etc.
[0048] Crosslinking agents can be used to crosslink a composition, thereby improving its mechanical properties (such as tensile properties) and electrical properties. Examples of crosslinking agents include organic peroxides. Specifically, examples of organic peroxides include dicumyl peroxide, 1-(2-tert-butylperoxyisopropyl)-1-isopropylbenzene, 1-(2-tert-butylperoxyisopropyl)-3-isopropylbenzene, 1,3-bis-(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-(tert-butylperoxy)-hexyne-3. Two or more of these may be used in combination.
[0049] Crosslinking aids can accelerate the crosslinking reaction by the crosslinking agent. Examples of crosslinking aids include triallyl cyanurate, triallyl isocyanurate, triallyl isocyanurate prepolymer, trimethyl isocyanurate, 1,3,5-triacryloylhexahydro-1,3,5-triazine, triallyl trimellitate, m-phenylenediamine bismaleimide, dipropargyl terephthalate, and N,N',N'',N'''-tetraallyl terephthalamide. These may be used individually or in combination of two or more.
[0050] Inorganic fillers can trap space charges in the insulating layer 130 and suppress local accumulation of space charges, thereby improving insulation. As inorganic fillers, for example, particles containing at least one of magnesium oxide, silicon dioxide, zinc oxide, aluminum oxide, titanium oxide, and zirconium oxide can be used.
[0051] Examples of antioxidants include 4,4'-thiobis-(6-t-butyl-3-methylphenol), 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,4-bis-[(octylthio)methyl]-o-cresol, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, and bis[2-methyl-4-{3-n-alkyl(C12 or C14)thiopropionyloxy}-5-t-butylphenyl]sulfide. Furthermore, you may use two or more of these in combination.
[0052] The lubricant acts to suppress the aggregation of the inorganic filler and to improve the fluidity of the resin composition during the extrusion molding of the insulating layer 130. The lubricant in this embodiment can be any known material.
[0053] (Resin Composition) The composition of this embodiment contains 60 to 85 parts by mass of polyethylene and 15 to 40 parts by mass of thermoplastic elastomer as resin components. If the content of thermoplastic elastomer is excessively high, the amount of polyethylene decreases, resulting in a lower tensile strength of the insulating layer and making it impossible to meet the mechanical properties required for power cables. On the other hand, if the content of thermoplastic elastomer is excessively low, the desired flexibility cannot be obtained in the insulating layer. Moreover, if there is little thermoplastic elastomer, it becomes difficult to incorporate foreign matter, water treeing is more likely to occur in the polyethylene, and water treeing is more likely to grow. In other words, the desired water tree resistance cannot be maintained in the insulating layer. In this regard, by mixing polyethylene and thermoplastic elastomer in the above ratio, it is possible to achieve a high level of balance between mechanical properties such as tensile strength and water tree resistance. From the viewpoint of achieving an even higher level of balance, it is preferable that the polyethylene content be 65 to 80 parts by mass, or 65 to 75 parts by mass. The content of thermoplastic elastomer may be 20 parts by mass or more and 35 parts by mass or 25 parts by mass or more and 35 parts by mass.
[0054] The composition contains 0.5 parts by mass or more and 1.0 part by mass or less of polyalkylene glycol per 100 parts by mass of the resin component. If the polyalkylene glycol content is excessively low, the occurrence and growth of water trees cannot be sufficiently suppressed, and the water tree resistance becomes significantly low. On the other hand, if the polyalkylene glycol content is excessively high, polar groups (e.g., ether groups) derived from the polyalkylene glycol form a dipole moment, and the energy lost due to its vibration increases. In other words, the dielectric loss tangent becomes larger. In this respect, by setting the polyalkylene glycol content within a predetermined range, it is possible to maintain high water tree resistance while keeping the dielectric loss tangent low. From the viewpoint of achieving both of these at a higher level, it is preferable that the polyalkylene glycol content be 0.65 parts by mass or more and 0.85 parts by mass or less.
[0055] (Phase Structure) The composition of this embodiment has a predetermined phase structure by containing polyethylene, thermoplastic elastomer, and polyalkylene glycol in predetermined amounts. The phase structure of the composition of this embodiment will now be explained with reference to Figure 2. Figure 2 is a schematic diagram illustrating the occurrence of water trees in an electrical insulating composition according to one embodiment of the present invention.
[0056] As shown in Figure 2, polyethylene forms the sea phase 1. Thermoplastic elastomer is dispersed in the sea phase 1, forming island phases 2. Since polyalkylene glycol has higher compatibility with thermoplastic elastomer than polyethylene, it is mainly dispersed in island phases 2 rather than sea phases 1. In other words, the amount of polyalkylene glycol present (dispersed) in island phases 2 tends to be greater than that in sea phases 1. As a result, polyalkylene glycol forms the fine phase 3. Although foreign matter 4 may be present in the composition, during mixing, foreign matter 4 tends to be incorporated into the island phases 2 of the thermoplastic elastomer.
[0057] The following mechanism is hypothesized to suppress the generation and growth of water trees due to the phase structure of the composition shown in Figure 2. Specifically, foreign matter 4, which is the starting point for water tree generation, is incorporated into the island phase 2 and surrounded by the fine polyalkylene glycol phase 3. Since polyalkylene glycol has polar groups, the electric field around foreign matter 4 is relaxed. This suppresses the aggregation of water around foreign matter 4 when the insulating layer 130 is immersed in water. In other words, it suppresses the generation of water trees originating from foreign matter 4. Furthermore, when the composition is immersed in water, the water incorporated into the composition can be captured by the highly hydrophilic polyalkylene glycol. Moreover, since the polyalkylene glycol is dispersed in the island phase 2, which is finely dispersed in the sea phase 1, to form the fine phase 3, the captured water can be uniformly dispersed and retained in the composition without localized aggregation. As a result, even when the power cable 10 is energized, the aggregation of water at points where the electric field is concentrated (e.g., foreign matter 4) can be suppressed. Furthermore, since the amount of water contained in the polyethylene sea phase 1 can be reduced, the aggregation of water in the sea phase 1 can also be suppressed. This makes it possible to suppress the generation and growth of water trees. Thus, according to the composition of this embodiment, by having a predetermined phase structure, the generation of water trees can be suppressed and the number density of water trees can be reduced. In addition, the growth of water trees can be suppressed, the size of water trees can be adjusted to be smaller, and the shape of water trees can be controlled to be spherical. These mechanisms can only be realized with the three-component composition of this embodiment.
[0058] (2) Power Cable Next, the power cable of this embodiment will be described using Figure 1. Figure 1 is a cross-sectional view of the power cable according to this embodiment, perpendicular to the axial direction.
[0059] The power cable 10 in this embodiment is configured as a so-called solid-insulated power cable. Furthermore, the power cable 10 in this embodiment is configured to be laid, for example, underwater or on the seabed. The power cable 10 is used, for example, for alternating current.
[0060] Specifically, the power cable 10 includes, for example, a conductor 110, an internal semiconducting layer 120, an insulating layer 130, an external semiconducting layer 140, a shielding layer 150, and a sheath 160.
[0061] The power cable 10 of this embodiment has the remarkable water tree suppression effect described above, and therefore, for example, does not have a metal waterproofing layer such as a so-called aluminum sheath outside the shielding layer 150. In other words, the power cable 10 of this embodiment is constructed with a non-complete waterproofing structure.
[0062] (Conductor (Conductive Part)) The conductor 110 is formed by twisting together a plurality of conductive core wires, for example, pure copper, copper alloy, aluminum, or aluminum alloy.
[0063] (Internal Semiconducting Layer) The internal semiconducting layer 120 is provided so as to cover the outer circumference of the conductor 110. The internal semiconducting layer 120 is semiconductive and is configured to suppress electric field concentration on the surface side of the conductor 110. The internal semiconducting layer 120 includes, for example, at least one of ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-butyl acrylate copolymer, and ethylene-vinyl acetate copolymer, and conductive carbon black.
[0064] (Insulating layer) The insulating layer 130 is provided so as to cover the outer circumference of the internal semiconducting layer 120 and is made of the electrical insulating composition described above. The insulating layer 130 is crosslinked, for example, by heating the electrical insulating composition after it has been extruded, as described above.
[0065] (External Semiconducting Layer) The external semiconducting layer 140 is provided so as to cover the outer circumference of the insulating layer 130. The external semiconducting layer 140 is semiconductive and is configured to suppress electric field concentration between the insulating layer 130 and the shielding layer 150. The external semiconducting layer 140 is made of the same material as the internal semiconducting layer 120, for example.
[0066] (Shielding layer) The shielding layer 150 is provided so as to cover the outer circumference of the outer semiconducting layer 140. The shielding layer 150 is formed, for example, by winding copper tape, or as a wire shield formed by winding multiple soft copper wires. In addition, tape made of rubberized cloth or the like may be wound around the inside or outside of the shielding layer 150.
[0067] (Sheath) The sheath 160 is provided to cover the outer periphery of the shielding layer 150. The sheath 160 is made of, for example, polyvinyl chloride or polyethylene.
[0068] (3) Cable characteristics According to the insulating layer 130 of this embodiment, the following characteristics can be obtained.
[0069] (Water Tree Resistance) In this embodiment, as described above, the insulating layer 130 contains a predetermined amount of polyalkylene glycol in a resin component containing polyethylene and thermoplastic elastomer in a predetermined ratio, thereby providing high water tree resistance to the insulating layer 130. As a result, the number density of water trees in the insulating layer 130 can be kept low.
[0070] The number density of water trees can be measured by performing a strip test on the insulating layer 130. Specifically, the insulating layer 130 or the composition constituting the insulating layer 130 is immersed in artificial seawater with a salinity of 3.8% by mass at room temperature, and an AC voltage of 1000 Hz and 4 kV is applied to the insulating layer 130 or the composition for 30 days. Subsequently, after the voltage is applied, a test piece with a thickness of 0.2 mm is taken from the insulating layer 130, the test piece is stained, and the number of water trees with a length of 50 μm or more is determined, and the number of water trees with a length of 1 cm² is measured. 3 It is best to calculate the number density per unit area. The number density of water trees is 2,000 per cm³. 3 When it is less than 1,200, it is often 1,200 pieces / cm 3 It may be less than 200 pieces / cm 3 It may be less than this. This makes it possible to stably suppress dielectric breakdown of the insulating layer 130 caused by water treeing.
[0071] Furthermore, the density of water trees is not limited, as a lower density is preferable. If no water trees occur, the density of water trees is 0 per cm³. 3 This is the result.
[0072] Furthermore, the insulating layer 130 can suppress the growth of water trees, causing them to form a spherical shape and shortening their length. Specifically, the insulating layer should have a maximum water tree length of 200 μm or less as determined by a water needle test, and a ratio of the long side to the short side of the water tree of 2.0 or less. The maximum length is the longest value obtained when multiple water trees are randomly sampled. The ratio of the long side to the short side is the average value of multiple randomly sampled water trees.
[0073] Here, the water needle test is performed using the following procedure, as shown in Figure 4.
[0074] First, a hexahedron block IB is taken from the insulating layer 130. After taking block IB, a flat electrode FE is placed on the first face S1 of block IB. Next, with the flat electrode FE in place, a needle-shaped void is formed along the normal direction from the second face S2 opposite to the first face S1 of block IB. At this time, the needle-shaped void is formed at a position opposite to the first face S1 of block IB, with a distance d of 1 mm, so that the tip has a radius of curvature of 10 μm. Next, with the void formed in block IB, artificial seawater with a salinity of 3.8 mass% is injected into the void. This forms a water needle WN inside block IB. In this state, an AC voltage of 1000 Hz and 4 kV is applied between the flat electrode FE and the tip of the water needle WN for 30 days. Then, after applying voltage, the test specimen of the insulating layer 130 was stained, and the shape and maximum length of the water tree extending from the tip of the water needle WN were measured.
[0075] The shape of a water tree can be evaluated by the ratio of its long side to its short side for each water tree. If this ratio is 2.0 or less, the water tree can be judged to be not irregularly shaped and to be close to a spherical shape. The maximum length of a water tree refers to the length of the longest water tree generated in the insulating layer 130, and it is preferable that it be 200 μm or less. The shorter the maximum length of the water tree and the closer its shape is to a spherical shape, the more stably dielectric breakdown of the insulating layer 130 caused by water trees can be suppressed.
[0076] Furthermore, the shape of the water trees generated in the composition is preferably spherical, and the ratio of spherical to spherical is preferably close to 1. In other words, the ratio of the long side to the short side is preferably between 1.0 and 2.0. Also, the maximum length of the water trees generated in the composition is not limited, as it is preferable that it be as small as possible. If no water trees are generated, the maximum length of the water trees will be 0 μm.
[0077] (Dielectric Loss Tangent) When an alternating electric field is applied to the insulating layer 130, energy loss may occur. This loss includes, for example, loss due to leakage current, loss due to dielectric polarization, and loss due to partial discharge. Due to such losses, the current phase lags behind the lossless current flowing through an ideal electrical insulating composition. In this case, the lag angle δ is called the dielectric loss angle, and the tangent is called the dielectric loss tangent (tanδ). In this embodiment, although a polyalkylene glycol having polar groups is mixed, its content is within a predetermined range, so the dielectric loss tangent of the insulating layer 130 can be kept low. The dielectric loss tangent can be kept lower than in the case of an uncrosslinked insulating layer 130 by crosslinking it.
[0078] Specifically, in this embodiment, the dielectric loss tangent when an AC electric field of 4 kV / mm at a frequency of 60 Hz and a temperature of 90°C is applied to the composition constituting the insulating layer 130 is preferably 0.05% or less. Since a smaller dielectric loss tangent is preferable, its lower limit is not particularly limited. However, in the electrical insulating composition of this embodiment, the dielectric loss is, for example, 0.001% or more.
[0079] (Tensile Strength) The insulating layer 130 contains predetermined amounts of polyethylene and thermoplastic elastomer, and therefore has excellent mechanical properties. Specifically, the tensile strength of the insulating layer 130 should be, for example, 10.0 MPa or higher. The higher the tensile strength of the insulating layer 130, the better, and there is no particular upper limit, but for example, it should be 50 MPa or less. The method for measuring tensile strength will be described in detail in the examples.
[0080] (4) Method for manufacturing a power cable Next, the method for manufacturing a power cable according to this embodiment will be described.
[0081] As shown in Figure 2, the method for manufacturing a power cable according to this embodiment includes, for example, a composition preparation step S100, a conductor preparation step S200, an extrusion step S300, a crosslinking step S400, a shielding layer formation step S500, and a sheath formation step S600.
[0082] (S100: Composition preparation step) First, the electrical insulating composition constituting the insulating layer 130 of this embodiment is prepared.
[0083] In this embodiment, polyethylene and thermoplastic elastomer are used as resin components, polyalkylene glycol having a predetermined number-average molecular weight, and other additives such as crosslinking agents and crosslinking aids are mixed (kneaded) in a mixer to form a mixed material. Examples of mixers include open roll mixers, banba mixers, pressurized kneaders, single-screw mixers, and multi-screw mixers. Kneading may be performed only once or in multiple stages.
[0084] Once the mixture is formed, it is granulated using an extruder. This forms the pelletized composition that constitutes the insulating layer 130. A twin-screw extruder with high kneading capabilities may be used to perform the mixing and granulation processes in a single step.
[0085] (S200: Conductor preparation process) Meanwhile, a conductor 110 is prepared by twisting together multiple conductor core wires.
[0086] (S300: Extrusion process) Once the composition preparation process S100 and the conductor preparation process S200 are completed, in the extrusion process S300, an insulating layer 130 is formed using the above-described resin composition to cover the outer circumference of the conductor 110.
[0087] In this embodiment, for example, a three-layer simultaneous extruder is used to simultaneously form the inner semiconducting layer 120, the insulating layer 130, and the outer semiconducting layer 140.
[0088] Specifically, in the three-layer simultaneous extruder, for example, the composition for the internal semiconducting layer is fed into extruder A, which forms the internal semiconducting layer 120.
[0089] The pelletized composition described above is introduced into the extruder B for forming the insulating layer 130. At this time, the set temperature of the extruder B is set to a temperature that is 5°C to 50°C higher than the melting point of the resin component. The set temperature is adjusted as appropriate based on the linear speed and extrusion pressure.
[0090] Furthermore, the extruder C, which forms the outer semiconducting layer 140, is fed an outer semiconducting layer composition containing the same material as the resin composition for the inner semiconducting layer that was fed into extruder A.
[0091] Next, the extruded materials from extruders A to C are guided to a common head, and the inner semiconducting layer 120, insulating layer 130, and outer semiconducting layer 140 are simultaneously extruded onto the outer circumference of the conductor 110 from the inside out. This forms the extruded material that will become the cable core.
[0092] (S400: Crosslinking process) Once the extrusion process S300 is completed, the insulating layer 130 is crosslinked in the crosslinking process S400 of this embodiment. For example, the extruded material is introduced into a crosslinking tube pressurized with nitrogen gas or the like, and the insulating layer 130 is crosslinked inside the crosslinking tube by heating with radiation from an infrared heater or by heat transfer through a heat transfer medium such as high-temperature nitrogen gas or silicone oil.
[0093] Afterward, the cable core is cooled, for example, by water cooling.
[0094] As a result, a cable core is formed, consisting of a conductor 110, an internal semiconducting layer 120, an insulating layer 130, and an external semiconducting layer 140.
[0095] (S500: Shielding layer formation process) Once the crosslinking process S400 is completed, a shielding layer 150 is formed on the outside of the outer semiconducting layer 140 by winding, for example, copper tape around it.
[0096] (S600: Sheath formation process) Once the shielding layer 150 is formed, polyvinyl chloride is fed into the extruder and extruded to form a sheath 160 on the outer circumference of the shielding layer 150.
[0097] Based on the above, the power cable 10 is manufactured.
[0098] (5) Summary of this embodiment This embodiment provides one or more of the following effects.
[0099] (a) The electrical insulating composition of this embodiment comprises, as a resin component, 60 to 85 parts by mass of polyethylene, 15 to 40 parts by mass of thermoplastic elastomer, and 0.5 to 1.0 part by mass of polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less per 100 parts by mass of the resin component. By including polyethylene and thermoplastic elastomer in predetermined ratios, a high level of both flexibility and tensile properties can be achieved in the insulating layer 130. The thermoplastic elastomer can incorporate foreign matter, for example, derived from polyethylene, and the generation of water trees originating from these foreign matter can be suppressed in the insulating layer 130. The polyalkylene glycol, when dispersed in the thermoplastic elastomer, can mitigate electric field concentration on foreign matter. Moreover, because polyalkylene glycol has high hydrophilicity, it can capture water incorporated into the composition and retain it in a finely dispersed state without agglomerating within the composition. This suppresses the agglomeration of water due to electric field concentration, thereby suppressing the generation and growth of water trees. As a result, the insulating layer can improve water tree resistance along with the cable's various characteristics.
[0100] (b) The composition has a phase structure in which polyethylene constitutes the sea phase, thermoplastic elastomer constitutes the island phase dispersed in the sea phase, and polyalkylene glycol is dispersed in the island phase. With such a phase structure, the effects of (a) described above can be obtained more reliably.
[0101] (c) The thermoplastic elastomer may be at least one of an olefin-based thermoplastic elastomer and a styrene-based thermoplastic elastomer. With a styrene-based thermoplastic elastomer, a stable resonance structure can be formed by styrene, so even if water aggregates around incorporated foreign matter, the electric field concentration due to that aggregation can be mitigated. With an olefin-based thermoplastic elastomer, it is easy to mix with polyethylene and can suppress the formation of voids, so the generation of water trees originating from voids can be suppressed.
[0102] (d) It is preferable that the polyalkylene glycol be polyethylene glycol (PEG). PEG has high hydrophilicity and is better able to capture water, so the occurrence of water trees can be suppressed more reliably.
[0103] (e) In the insulating layer 130 of this embodiment, the maximum length of water trees generated by the water needle test is preferably 200 μm or less, and the ratio of the long side to the short side of the water tree is preferably 2.0 or less. Since the insulating layer 130 is formed from the above composition, it has excellent water tree resistance, and the growth of water trees is suppressed. As a result, the size of the generated water trees can be reduced, and their shape can be controlled to be spherical. As a result, dielectric breakdown of the insulating layer 130 caused by water trees can be stably suppressed.
[0104] (f) According to the insulating layer 130 of this embodiment, even when an AC voltage of 1000 Hz and 4 kV is applied for 30 days while the insulating layer 130 is immersed in artificial seawater with a salinity of 3.8 mass% at room temperature, the number density of water trees generated in the insulating layer 130 that have a length of 50 μm or more is 2,000 trees / cm². 3 It is desirable that the value be less than the specified value. Since the insulating layer 130 is formed from the above-described composition, it has excellent water tree resistance, and the occurrence of water trees is suppressed. As a result, dielectric breakdown of the insulating layer 130 caused by water trees can be stably suppressed.
[0105] (g) According to the insulating layer 130 of this embodiment, a high dielectric loss tangent can be maintained by having a polyalkylene glycol content of 0.5 to 1.0 parts by mass. Specifically, when an AC electric field of 4 kV / mm at a frequency of 60 Hz at a temperature of 90°C is applied to the insulating layer 130, the dielectric loss tangent should be 0.05% or less.
[0106] <Other Embodiments of the Disclosure> Although embodiments of the Disclosure have been described in detail above, the Disclosure is not limited to the embodiments described above and can be modified in various ways without departing from its essence.
[0107] In the embodiments described above, a case in which the power cable 10 does not need to have a waterproofing layer was explained, but this disclosure is not limited to this case. The power cable 10 may have a simple waterproofing layer. Specifically, the simple waterproofing layer is, for example, made of metal laminate tape. The metal laminate tape has, for example, a metal layer made of aluminum or copper and an adhesive layer provided on one or both sides of the metal layer. The metal laminate tape is wrapped, for example, vertically around the outer circumference of the cable core (outer than the outer semiconducting layer). The waterproofing layer may be provided outside the shielding layer, or it may also serve as the shielding layer. With such a configuration, the cost of the power cable 10 can be reduced.
[0108] Although the installation environment of the power cable 10 was not mentioned in the embodiments described above, the power cable 10 may be configured to be installed, for example, on land, underwater, or on the seabed. Alternatively, the power cable 10 may be configured, for example, as a so-called overhead wire (overhead insulated wire).
[0109] In the above embodiment, three layers were extruded simultaneously when forming the cable core, but the layers may be extruded one by one.
[0110] Next, embodiments relating to this disclosure will be described. These embodiments are examples of this disclosure and the disclosure is not limited to these embodiments.
[0111] (1) Preparation of materials The following materials were prepared for preparing the resin composition. Low-density polyethylene (LDPE) was prepared as polyethylene. The density d of LDPE is 0.90 g / cm³. 3 The MFR was 1.2 g / 10 min. Hydrogenated styrene-butadiene styrene block copolymer (SEBS) was prepared as a thermoplastic elastomer. The styrene content of SEBS was 17% by mass, and the MFR was 4.8 g / 10 min. An olefin-based thermoplastic elastomer (TPO) was prepared as a thermoplastic elastomer, with the hard segment being polypropylene and the soft segment being ethylene-propylene rubber. The MFR of TPO was 0.6 g / 10 min. Several polyethylene glycols (PEG1-5) with different number average molecular weights were prepared as polyalkylene glycols. The number average molecular weights were 6,000 for PEG1, 2,000 for PEG2, 4,500 for PEG3, 8,000 for PEG4, and 10,000 for PEG5. Dicumyl peroxide (DCP) was prepared as another additive.
[0112] (2) Preparation of the resin composition In this embodiment, the resin composition was prepared by mixing the materials described above.
[0113] Specifically, in samples 1 to 5, as shown in Table 1 below, 70 parts by mass of LDPE and 30 parts by mass of SEBS were mixed as resin components, and the amount of PEG added per 100 parts by mass of resin component was appropriately changed in the range of 0 to 1.5 parts by mass to prepare an electrical insulating composition. In addition, 1.6 parts by mass of DCP was added per 100 parts by mass of resin component.
[0114]
[0115] Furthermore, in Samples 6 to 9, the electrical insulating compositions were prepared in the same manner as in Sample 3, except that the type of polyalkylene glycol was changed from PEG1 to PEG2 to PEG5, as shown in Table 2 below.
[0116]
[0117] Furthermore, in samples 10 to 14, as shown in Table 3 below, the addition ratios of LDPE and SEBS as resin components were appropriately changed, and an electrical insulating composition was prepared using 0.75 parts by mass of PEG per 100 parts by mass of resin components. DCP was added at a rate of 1.6 parts by mass per 100 parts by mass of resin components.
[0118] In Sample 15, an electrical insulating composition was prepared in the same manner as in Sample 12, except that the type of thermoplastic elastomer was changed from styrene-based to olefin-based.
[0119]
[0120] (3) Evaluation Method The electrical insulating composition of each prepared sample was evaluated as follows.
[0121] (Water tree length, water tree shape) After forming the electrical insulating composition described above, an insulator was produced by press molding the electrical insulating composition at 120°C for 10 minutes. A block was taken from this insulator and the water needle test shown in Figure 4 was performed.
[0122] The conditions for the water needle test were set as follows: Radius of curvature of the water needle tip: 10 μm Distance from the flat plate electrode on the first surface of the block to the tip of the water needle: 1 mm Salinity of the artificial seawater in the water needle: 3.8 mass% Frequency: 1000 MHz AC voltage: 4 kV
[0123] After the water needle test, the block was dried and then stained by boiling it in a methylene blue solution. After staining the block, the area near the tip of the water needle was sliced to form observation slices. Subsequently, the observation slices were observed under an optical microscope to confirm the water trees that had formed near the tip of the water needle in the observation slices.
[0124] At this time, the maximum length of water trees generated in the observation slice was measured. The "maximum length of water trees" was determined by rounding the length of the longest water tree in 10 blocks randomly selected from the insulating layer of each sample. The ratio of the long side to the short side of the water trees generated in the observation slice was calculated. The ratio of the long side to the short side was obtained by averaging the values of 10 randomly selected water trees.
[0125] (Water Tree Number Density) After forming the above-mentioned electrical insulating composition, two insulating sheets with a thickness of 1 mm were produced by press molding the electrical insulating composition at 120°C for 10 minutes. After producing the insulating sheets, a predetermined semiconducting sheet was sandwiched between the two insulating sheets to form a laminated sheet. After forming the laminated sheet, the base resin of the insulating sheet was crosslinked by press molding the laminated sheet at 180°C for 30 minutes. After crosslinking the insulating sheet, wiring was formed on the semiconducting sheet.
[0126] Next, with the laminated sheet immersed in artificial seawater at room temperature (27°C) with a salinity of 3.8% by mass, an alternating electric field of 1000 Hz and 4 kV / mm was applied to the insulating sheet between the semiconducting sheet and the aqueous solution for 30 days.
[0127] After applying a predetermined alternating electric field, the laminated sheet was dried and then boiled and stained with a methylene blue aqueous solution. After staining the laminated sheet, it was sliced to a thickness of 200 μm along the lamination direction (i.e., the direction perpendicular to the main plane of the laminated sheet) to form observation slices. Subsequently, the observation slices were observed using an optical microscope to observe water trees that had formed in the creepage direction of the semiconducting sheet or perpendicular to the main plane of the semiconducting sheet in the insulating sheet of the observation slice. At this time, the number density of water trees that had formed in the insulating sheet and had a length of 50 μm or more was measured. In Tables 1 and 2 described below, the "number density of water trees" was calculated by rounding the average number of water trees in 10 randomly selected observation slices.
[0128] (Dielectric Loss Tangent) After forming the above-mentioned electrical insulating composition, an insulating sheet having a thickness of 0.2 mm was produced by press molding the electrical insulating composition at 180°C for 30 minutes. At this time, the resin component of the insulating sheet was crosslinked by pressing the insulating sheet at 180°C for 30 minutes.
[0129] Next, a Schering bridge was used to apply an AC electric field of 9 kV / mm at 90°C to the insulating sheet, and the dielectric loss tangent was measured. In this example, a dielectric loss tangent of 0.05% or less was denoted as "A," and a value exceeding 0.05% was denoted as "B."
[0130] (Tensile Strength) After forming the electrical insulating composition described above, an insulating sheet with a thickness of 0.2 mm was produced by press molding the electrical insulating composition at 180°C for 30 minutes. At this time, the resin component of the insulating sheet was crosslinked by pressing the insulating sheet at 180°C for 30 minutes. Next, the tensile strength of the insulating sheet was measured in accordance with JIS C3005. Specifically, the tensile strength of the insulating sheet was measured by pulling the insulating sheet at a tensile speed of 200 mm / min using a JIS-3 dumbbell.
[0131] (4) Evaluation Results The evaluation results are summarized in Tables 1 to 3.
[0132] As shown in Table 1, in samples 2 to 4, it was confirmed that by setting the PEG content to 0.5 to 1.0 parts by mass per 100 parts by mass of resin component, it was possible to maintain a low dielectric loss tangent while increasing tensile strength and achieving excellent cable characteristics. Furthermore, it was confirmed that the water tree length could be 200 μm or less, and the water tree shape could be configured with a long-side / short-side ratio of 2.0 or less. In addition, the number density of water trees was 2,000 trees / cm³. 3 It was confirmed that the levels were less than the specified amount. From these findings, it was confirmed that the occurrence and growth of water trees can be suppressed even when electrolyzed using a predetermined amount of PEG.
[0133] In contrast, in Sample 1, it was confirmed that mixing a thermoplastic elastomer with polyethylene could suppress the generation of water trees and reduce their number density. However, in Sample 1, because polyalkylene glycol was not added, the water tree length exceeded 200 μm, and the ratio of the long side to the short side of the water trees exceeded 2.0. In Sample 1, it is presumed that water trees were generated by electrolysis and grew larger and distorted in shape as a result.
[0134] Furthermore, in Sample 5, although PEG was added as polyalkylene glycol, its content exceeded 1.0 part by mass (1.5 parts by mass). As a result, while water tree resistance remained high, the dielectric loss tangent increased. This is presumed to be because the number of polar groups increased with the increase in PEG, and the dielectric loss tangent increased due to the influence of the electric field.
[0135] As shown in Table 2, in samples 3, 7, and 8, by adjusting the molecular weight of PEG to the range of 4,000 to 8,000, it was confirmed that high water tree resistance could be obtained by suppressing the dielectric loss tangent, reducing the water tree length, making the water tree shape closer to a spherical shape, and further suppressing the water tree generation density. In particular, in sample 3, the number average molecular weight of PEG was 6,000, which was in the range of 5,500 to 6,500, so it was confirmed that a good balance between reducing the dielectric loss tangent and improving water tree resistance could be achieved at a higher level than in samples 7 and 9.
[0136] On the other hand, in sample 6, the number average molecular weight was 2,000, and because an excessively low molecular weight PEG was used, high water tree resistance was maintained, but it was confirmed that the dielectric loss tangent exceeded 0.05%. This is presumed to be because the molecular weight of the PEG was excessively low, making it prone to minute vibrations at high temperatures. On the other hand, in sample 9, the number average molecular weight was 10,000, and because an excessively high molecular weight PEG was used, it was confirmed that high water tree resistance could not be maintained. In particular, although the water tree length was made small and the water tree shape was made spherical, it was confirmed that the water tree generation density was high. This is presumed to be because the PEG dispersed into the polyethylene, which is the sea phase, and became less likely to exist in the island phase of the thermoplastic elastomer, so the effect of electric field relaxation by PEG could not be fully obtained.
[0137] As shown in Table 3, in samples 11 to 13, it was confirmed that high cable properties and water tree resistance could be maintained by mixing 60 to 85 parts by mass of LDPE and 15 to 40 parts by mass of thermoplastic elastomer as resin components.
[0138] In contrast, in sample 10, 50 parts by mass of LDPE and 50 parts by mass of thermoplastic elastomer were added, resulting in an excessive amount of thermoplastic elastomer. Consequently, the tensile strength was less than 10.0 MPa, confirming that high mechanical properties could not be obtained. On the other hand, in sample 14, no thermoplastic elastomer was added, resulting in shorter water tree lengths and the formation of spherical water trees. However, it was confirmed that the number density of water trees was high. This is presumed to be because the absence of thermoplastic elastomer led to electric field concentration due to foreign matter and increased water aggregation within the polyethylene matrix, making water trees more likely to form.
[0139] Furthermore, in Sample 15, it was confirmed that olefin-based thermoplastic elastomers, like styrene-based thermoplastic elastomers, could suppress the occurrence and growth of water trees. In other words, it was confirmed that water tree resistance could be improved.
[0140] As described above, by mixing polyethylene and thermoplastic elastomer as resin components in a predetermined ratio, and adding polyalkylene glycol, it is possible to achieve a high level of both cable properties and water tree resistance.
[0141] <Note> The nature of this disclosure is described below.
[0142] (Note 1) An electrical insulating composition comprising a resin component containing polyethylene and a thermoplastic elastomer, and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component.
[0143] (Note 2) A power cable comprising a conductor and an insulating layer provided on the outer circumference of the conductor and formed from an electrical insulating composition, wherein the electrical insulating composition contains a resin component including polyethylene and a thermoplastic elastomer and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component.
[0144] (Note 3) The power cable according to Note 2, wherein the thermoplastic elastomer is at least one of an olefin-based thermoplastic elastomer having an olefin unit and a styrene-based thermoplastic elastomer having a styrene unit.
[0145] (Note 4) The polyethylene is low-density polyethylene, as described in Note 2 or Note 3, for the power cable.
[0146] (Note 5) The density of the polyethylene is 0.89 g / cm³. 3 0.91g / cm or more 3The following is the power cable described in Appendix 4.
[0147] (Note 6) The power cable described in any one of Notes 2 to 4, wherein the polyalkylene glycol is polyethylene glycol.
[0148] (Note 7) The power cable according to any one of Notes 2 to 6, wherein the electrical insulating composition has a phase structure in which polyethylene constitutes the sea phase, the thermoplastic elastomer constitutes the island phase dispersed in the sea phase, and the polyalkylene glycol is dispersed in the island phase.
[0149] (Note 8) The insulating layer has a maximum water tree length of 200 μm or less generated by a water needle test, and the ratio of the long side to the short side of the water tree is 2.0 or less. Hereinafter, the water needle test includes the steps of: providing a flat electrode on the first surface of a block taken from the insulating layer; forming a needle-shaped void at a position opposite to the first surface at a distance of 1 mm, such that the void has a tip with a radius of curvature of 10 μm; injecting artificial seawater with a salinity of 3.8 mass% into the void to form a water needle within the block; and applying an AC voltage of 1000 Hz and 4 kV between the flat electrode and the tip of the water needle for 30 days. The power cable according to any one of Notes 2 to 7.
[0150] (Note 9) When the insulating layer is immersed in artificial seawater with a salinity of 3.8% by mass at room temperature, and an AC voltage of 1000 Hz and 4 kV is applied to the insulating layer for 30 days, the number density of water trees with a length of 50 μm or more that are generated in the insulating layer is 2,000 trees / cm². 3 A power cable that is less than one of the specifications listed in Appendix 2 to Appendix 8.
[0151] (Note 10) The power cable described in any one of Notes 2 to 8, wherein the dielectric loss tangent of the insulating layer is 0.05% or less when an AC electric field of 4 kV / mm is applied at a temperature of 90°C and a frequency of 60 Hz.
[0152] 1. Sea phase (polyethylene) 2. Island phase (thermoplastic elastomer) 3. Polyalkylene glycol 4. Foreign matter 5. Water tree 6. Needle 10. Power cable 110. Conductor 120. Inner semiconducting layer 130. Insulating layer 140. Outer semiconducting layer 150. Shielding layer 160. Sheath
Claims
1. An electrical insulating composition comprising a resin component containing polyethylene and a thermoplastic elastomer, and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component.
2. A power cable comprising a conductor and an insulating layer provided on the outer circumference of the conductor and formed from an electrical insulating composition, wherein the electrical insulating composition contains a resin component including polyethylene and a thermoplastic elastomer and a polyalkylene glycol having a number average molecular weight of 4,000 or more and 8,000 or less, wherein the polyethylene content is 60 parts by mass or more and 85 parts by mass or less, the thermoplastic elastomer content is 15 parts by mass or more and 40 parts by mass or less, and the polyalkylene glycol content is 0.5 parts by mass or more and 1.0 part by mass or less per 100 parts by mass of the resin component.
3. The power cable according to claim 2, wherein the thermoplastic elastomer is at least one of an olefin-based thermoplastic elastomer having olefin units and a styrene-based thermoplastic elastomer having styrene units.
4. The power cable according to claim 2, wherein the polyethylene is low-density polyethylene.
5. The power cable according to claim 2, wherein the polyalkylene glycol is polyethylene glycol.
6. The power cable according to claim 2, wherein the electrical insulating composition has a phase structure in which polyethylene constitutes a sea phase, the thermoplastic elastomer constitutes an island phase dispersed in the sea phase, and the polyalkylene glycol is dispersed in the island phase.
7. The insulating layer has a maximum water tree length of 200 μm or less generated by a water needle test, and the ratio of the long side to the short side of the water tree is 2.0 or less, wherein the water needle test includes the steps of: providing a flat electrode on the first surface of a block taken from the insulating layer; forming a needle-shaped void at a position opposite to the first surface at a distance of 1 mm, such that the void has a tip with a radius of curvature of 10 μm; forming a water needle in the block by injecting artificial seawater with a salinity of 3.8 mass% into the void; and applying an alternating voltage of 1000 Hz and 4 kV between the flat electrode and the tip of the water needle for 30 days, as described in claim 2.
8. When the insulating layer is immersed in artificial seawater with a salinity of 3.8% by mass at room temperature, and an AC voltage of 1000 Hz and 4 kV is applied to the insulating layer for 30 days, the number density of water trees with a length of 50 μm or more generated in the insulating layer is 2,000 trees / cm³. 3 The power cable according to claim 2, which is less than [a certain value].