Fuel cell gasket

A fuel cell gasket composition with ethylene-butene-diene rubber and additives maintains flexibility and rebound modulus at low temperatures, addressing the hardening issue of conventional rubber compositions in cold regions.

WO2026239502A1PCT designated stage Publication Date: 2026-11-19STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/017434
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing rubber compositions for fuel cell sealing components lose elasticity and harden in low-temperature environments, impairing their sealing performance in cold regions.

Method used

A fuel cell gasket composition comprising ethylene-butene-diene rubber, paraffinic hydrocarbon oil as a softener, carbon black, organic peroxide as a crosslinking agent, and a polyfunctional carboxylic acid compound as a crosslinking aid, with specific ratios to maintain flexibility and rebound modulus at low temperatures.

Benefits of technology

The gasket maintains excellent rebound modulus and flexibility even at temperatures as low as -30°C, preventing hardening and ensuring effective sealing performance in cold conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a fuel cell gasket with excellent rebound resilience in low-temperature environments. The fuel cell gasket has excellent rebound resilience in low-temperature environments and is characterized by containing the components (A) to (E) listed below. (A) A rubber component having an ethylene-butene-diene rubber as a base material. (B) A paraffinic hydrocarbon oil that serves as a softening agent, contains an alpha-olefin as a main component, and has a pour point of -70°C to -60°C inclusive. (C) Carbon black. (D) A crosslinking agent comprising an organic peroxide. (E) A crosslinking aid that is a polyfunctional carboxylic acid compound.
Need to check novelty before this filing date? Find Prior Art

Description

fuel cell gasket

[0001] This invention relates to a fuel cell gasket with excellent rebound modulus in low-temperature environments.

[0002] A fuel cell is an electrochemical battery that generates electricity through a chemical reaction between hydrogen and oxygen. Fuel cells are widely used in various applications, including as power supply systems for mobile vehicles such as passenger cars, buses, and ships, as well as in factories, office buildings, and homes.

[0003] In fuel cells, a fuel gas such as hydrogen is supplied from the anode side and an oxidizing gas such as air (oxygen) is supplied from the cathode side to a unit cell containing electrodes, thereby causing a chemical reaction for power generation. Therefore, in fuel cells, a sealed structure is formed by gaskets to prevent gases from leaking to the outside from the supply paths of the fuel gas and oxidizing gas.

[0004] For example, Patent Documents 1 to 5 describe fuel cell sealing members or rubber compositions for fuel cell separator sealing members, using ethylene-propylene rubber, ethylene-propylene-diene rubber, or ethylene-butene-diene rubber as rubber components.

[0005] When using such rubber compositions as sealing components for fuel cells, design must be tailored to the external environment in which the fuel cell operates. In particular, when used in cold regions, the lower limit temperature of the rubber composition must be considered. This is because rubber compositions with low cold resistance will lose elasticity and harden in low-temperature environments, potentially impairing the physical properties of the rubber as a sealing component. There are regions where winter temperatures drop to below -30°C, and in order to operate fuel cells without problems even in such cold regions, the cold resistance and rebound modulus of the rubber composition used as a sealing component become crucial.

[0006] Japanese Patent Publication No. 2021-66844, Japanese Patent Publication No. 2021-86791, Japanese Patent Publication No. 2022-152524, International Publication No. 2019 / 003885, International Publication No. 2019 / 216311

[0007] Therefore, in view of the problems of the above-mentioned prior art, the object of the present invention is to provide a fuel cell gasket with excellent rebound modulus in low-temperature environments.

[0008] One aspect of the present invention is a fuel cell gasket with excellent rebound modulus in low-temperature environments, characterized by containing the following components (A) to (E): (A) A rubber component based on ethylene-butene-diene rubber. (B) A paraffinic hydrocarbon oil containing alpha-olefin as its main component, having a pour point of -70°C or higher and -60°C or lower as a softening agent. (C) Carbon black. (D) A crosslinking agent consisting of an organic peroxide. (E) A crosslinking aid which is a polyfunctional carboxylic acid compound.

[0009] In one aspect of the present invention, the content of the softening agent in the fuel cell gasket may be 30% by weight or more.

[0010] Furthermore, in one aspect of the present invention, the content of the rubber component in the fuel cell gasket may be 40% by weight or more.

[0011] Furthermore, in one aspect of the present invention, the carbon black has a nitrogen adsorption specific surface area of ​​20 to 30 m². 2 The content is 15% to 35% by weight of the fuel cell gasket, which is 1g / g. (In this specification, "~" means above the lower limit and below the upper limit. The same applies hereinafter.)

[0012] According to the present invention, it is possible to realize a fuel cell gasket with excellent rebound modulus in low-temperature environments.

[0013] The fuel cell gasket according to the present invention will be described in detail below. However, the present invention is not limited to the following examples and can be modified as appropriate without departing from the spirit of the invention.

[0014] One aspect of the present invention is a fuel cell gasket with excellent rebound modulus in low-temperature environments, characterized by containing the following components (A) to (E): (A) A rubber component based on ethylene-butene-diene rubber. (B) A paraffinic hydrocarbon oil containing alpha-olefin as its main component, having a pour point of -70°C or higher and -60°C or lower as a softening agent. (C) Carbon black. (D) A crosslinking agent consisting of an organic peroxide. (E) A crosslinking aid which is a polyfunctional carboxylic acid compound.

[0015] As described above, this invention investigates fuel cell gaskets with excellent rebound modulus in low-temperature environments. Generally, when the temperature of rubber materials is lowered from room temperature, the rubbery elasticity is gradually lost, and the randomly moving molecular arrangement freezes, becoming glassy and solidifying at low temperatures. More specifically, rubber materials exhibit their unique elasticity through two processes: interatomic motion within the molecules and free rotational motion of the molecular chain structure. However, at low temperatures, interatomic motion within the molecules decreases, and the free rotational motion of the molecular chain structure also decreases at low temperatures. As a result, the rubber hardens and loses its elasticity.

[0016] Rubber hardens and breaks into pieces when it falls below a certain temperature (the glass transition temperature: the temperature at which the liquid state crystallizes). Basically, the glass transition temperature of rubber equals the glass transition temperature of raw rubber. As an exception, the softer the intermolecular chains and the weaker the forces acting on them, the more resistant to low temperatures it becomes. Therefore, it is possible to lower the glass transition temperature by adding chemicals that increase the molecular chain mobility of raw rubber. The following describes each component used in this invention.

[0017] (A. Rubber component) Regarding the rubber component, a rubber component based on ethylene-butene-diene rubber (EBT) is used. As a rubber component, for example, ethylene-propylene-diene rubber (EPDM, EPT) could also be considered, but the inventors of this invention investigated the physical properties under low-temperature conditions and found that ethylene-butene-diene rubber (EBT) is preferable.

[0018] Rubber components based on EBT (electrolytic bead metal) exhibit excellent high-temperature resistance, chemical resistance, and gas barrier properties, and can maintain flexibility even at low temperatures where conventional materials could not achieve this. Therefore, they are suitable as materials for harsh environments such as fuel cell applications.

[0019] Regarding the rubber component, it is preferable to formulate it so that its content in the fuel cell gasket (weight ratio to the total rubber composition synthesized) is 40% by weight or more. This is the ratio found in the examples described later.

[0020] (B. Softener) The softener (plasticizer) used is a paraffinic hydrocarbon oil containing alpha-olefin as its main component, with a pour point of -70°C or higher and -60°C or lower. The softener (plasticizer) reduces hardness and improves flexibility and low-temperature elasticity. It can also improve processability and fluidity. Polyalphaolefin (PAO) can be used as an example of a softener.

[0021] Softeners loosen the intermolecular bonds of polymers, thereby increasing the softness (flexibility and pliability) of rubber. They are particularly used to improve low-temperature properties (maintaining flexibility at low temperatures). By appropriately selecting a softener, the glass transition temperature (Tg) can be lowered, preventing the rubber from hardening in cold environments and maintaining its performance at low temperatures.

[0022] Regarding the amount of softener added, it is preferable to blend the softener so that its content relative to the fuel cell gasket is 20 to 40% by weight, and more preferably 30% by weight or more. By blending 30% by weight or more of the softener, a rebound modulus of 30% at -30°C can be achieved, as shown in the examples described later.

[0023] (C. Carbon Black) Carbon black is added as a filler. This enhances the strength, tensile strength, abrasion resistance, and UV resistance of the rubber, and also imparts some conductivity.

[0024] For example, it is preferable to use high-structure carbon of GPF (General Purpose Furnace) grade as the carbon black, with a nitrogen adsorption specific surface area of ​​20 to 30 m². 2 It is preferable that the amount is / g. Furthermore, it is preferable that the carbon black content in the fuel cell gasket is 15 to 35% by weight.

[0025] (D. Crosslinking Agent) Organic peroxides are used as crosslinking agents. The use of organic peroxides promotes the crosslinking reaction of rubber, forming a three-dimensional network structure. In addition, the crosslinking agent affects the resilience, permanent deformation rate, and heat resistance of the rubber.

[0026] As an example of a crosslinking agent, molecular formula C 14 H 28 O 4 1,1-(t-butylperoxy)cyclohexane and the like can be used as radical crosslinking agents, and those that function as polymerization initiators for vinyl monomers, heat curing agents for unsaturated polyester resins, or crosslinking agents for polyolefins or synthetic rubbers are used.

[0027] (E. Crosslinking Aids) Crosslinking aids are polyfunctional carboxylic acid compounds. When used in combination with organic peroxides, which are crosslinking agents, crosslinking aids promote the crosslinking reaction, improving crosslink density and enhancing heat resistance and dimensional stability. Examples of polyfunctional carboxylic acid compounds include acrylates.

[0028] As an example of a crosslinking aid, molecular formula C 12 H 18 O 4 1,6-hexanediol diacrylate and the like can be used as crosslinking aids for bifunctional monomers.

[0029] (F. Other Compounds) In the present invention, an anti-aging agent, an inorganic white filler, or the like may be incorporated as other compounds. The anti-aging agent suppresses oxidative degradation and ozone, improves durability and extends service life, and is particularly effective as a countermeasure against thermal aging. In addition, the inorganic white filler contributes to cost reduction and dimensional stability improvement, but on the other hand, excessive addition affects strength, processability and the like. In the case of the inorganic white filler, insulating properties are improved unlike carbon black.

[0030] As the anti-aging agent, for example, a phenolic antioxidant is used. In addition, as the inorganic white filler, calcium carbonate or the like is used.

[0031] (Gasket for Fuel Cell) In general, a fuel cell has a cell stack structure in which a plurality of units (cells) each constituted by an electrolyte membrane, electrode plates (cathode, anode) and separators are combined. As described above, the fuel cell generates electricity by the reaction between hydrogen and oxygen. In order to prevent leakage of these hydrogen gas and oxygen gas, and to properly drain water generated in the fuel cell, the gasket for a fuel cell according to the present invention is mainly used as a sealing member for sealing between the respective separators constituting the cell stack.

[0032] Furthermore, in the present invention, as described above, even when the fuel cell is used in a cold region where the air temperature is -30°C or lower, the gasket for a fuel cell used in the fuel cell does not solidify due to low temperature and fail to function, so that a gasket for a fuel cell excellent in impact resilience in a low temperature environment is realized.

[0033] Hereinafter, the present invention will be described in more detail by way of Examples, but the present invention is not limited to the following Examples at all.

[0034] (Preparation of Rubber Compositions) In the examples, rubber compositions constituting the fuel cell gasket according to the present invention were prepared. The following were used for each composition: ・Rubber component (base material): EBT-K8370EM rubber or EBT-K9330M rubber (manufactured by Mitsui Chemicals, Inc.) ・Softener (plasticizer): PAO401 (manufactured by Nippon Steel Chemical & Material Co., Ltd.) ・Carbon black: SPHERON 5200 (manufactured by Cabot Japan Co., Ltd.) ・Inorganic filler: Calcium carbonate (whiteSB) (manufactured by Shiraishi Calcium Co., Ltd.) ・Crosslinking agent: Organic peroxide (PERHEXA-C or PERCUMYL-D) (manufactured by NOF Corporation) ・Crosslinking aid: Viscort #230 (manufactured by Osaka Organic Chemical Industry Co., Ltd.) ・Anti-aging agent: RD (manufactured by Seikoh PMC Co., Ltd.)

[0035] Furthermore, as a comparative example, EPT (ethylene-propylene-diene rubber) was used instead of EBT (ethylene-butene-diene rubber) for the rubber component. The rubber component used was EPT 9090M (manufactured by Mitsui Chemicals, Inc.).

[0036] (Investigation of rubber composition blending ratios) Regarding the blending ratios of rubber compositions, we used AI-based machine learning to investigate blending ratios that can achieve excellent rebound modulus in low-temperature environments. Past experimental results were mainly used as training signals for depth learning. As an example of the investigation, we aimed to improve two properties, rebound modulus and volume resistivity, as described later, and selected three components: a softener, carbon black, and a crosslinking aid. We then performed reinforcement learning with three variables and two objectives. Through this, we investigated the correlation between the softener and carbon black, the softener and the crosslinking aid, and the carbon black and the crosslinking aid in improving the rebound modulus of rubber, and the correlation between the softener and carbon black, the softener and the crosslinking aid, and the carbon black and the crosslinking aid in improving the volume resistivity of rubber. The blending ratios necessary to achieve the two objectives were then predicted by AI.

[0037] Following the above considerations, in the examples and comparative examples, each of the above compositions was blended in the proportions shown in Table 1 below. The values ​​for the examples in Table 1 represent the mass proportion of each composition when the rubber component (base material) is 100 parts by mass.

[0038] Regarding the preparation of test pieces, after mastication of the rubber component, carbon black was added and kneaded, a plasticizer, a crosslinking aid, and an anti-aging agent were added, the mixture was placed in a mold for test piece preparation, and crosslinked with a crosslinking agent to obtain a compound. The crosslinking was performed at 170°C for 10 minutes.

[0039]

[0040] Regarding the prepared rubber composition, the properties of the rubber composition were measured by applying each of the tests listed below.

[0041] (Compressive Stress Relaxation Test) The compressive stress relaxation test was performed based on Chinese national standard GB / T1685-2008 (equivalent to Japanese Industrial Standard JIS K6263). This test is carried out to investigate the compressive stress relaxation characteristics by applying a specified compressive deformation to a cylindrical or ring-shaped test piece, and determining the change between the compressive force and the initial compressive force when the deformation is maintained at a specified temperature for a specified time.

[0042] A cylindrical test piece with a diameter of 13.0 mm ± 0.5 mm and a thickness of 6.3 mm ± 0.3 mm was prepared, and the test piece was compressed to 25% ± 2% of the specified deformation amount using a compressive force measuring device at standard temperature and humidity. Thereafter, the stress after 30 minutes, 3 hours, 6 hours, 24 hours, 72 hours, and 168 hours was measured, and the initial compressive force after 30 minutes was defined as F 0 (N), the compressive force after t hours was defined as F t (N), and the compressive stress relaxation R after t hours C (t) was defined as R C (t) = [(F 0 - F t ) / F 0 × 100 (%), each value was calculated, and the median of the obtained values was rounded to the nearest integer and presented.

[0043] (Compression Set Test) The compression set test was performed based on Chinese national standard GB / T7759.1-2015 (equivalent to Japanese Industrial Standard JIS K6262). This test determines the sag resistance of a rubber material by measuring the permanent strain caused by compression of the rubber material.

[0044] A cylindrical test specimen with a diameter of 29.0 mm ± 0.5 mm and a thickness of 12.5 mm ± 0.5 mm was prepared. This test specimen was subjected to strain using a compression device consisting of a compression plate for compressing the specimen, a spacer for applying a specified strain, and a holder for fixing the compression plate. After a predetermined time, the test specimen was released from the compression device and left on a wooden board for 30 minutes ± 3 minutes, and its height was measured. The compression set CS (%) was calculated as the original thickness h of the test specimen. 0 (mm), thickness h of the test specimen removed from the compression device 1 (mm), spacer thickness h s (mm) Let CS = [(h 0 -h 1 ) / (h 0 -h s The result was calculated as ) × 100 (%), performed on three test specimens, and the average value was rounded to an integer.

[0045] (Rebound Modulus Test) The rebound modulus test was conducted in accordance with the Chinese standard GB / T1681-2009 (equivalent to the Japanese Industrial Standard JIS K6257). The rebound modulus represents the ratio of the rebound energy to the energy applied when a pendulum with a spherical striking end strikes a test specimen at a specified mass and speed.

[0046] A cylindrical test specimen with a diameter of 29.0 mm ± 0.5 mm and a thickness of 12.5 mm ± 0.5 mm was prepared. The rebound modulus of this specimen was measured at room temperature, -40°C, -30°C, and -20°C using a Schob-type rebound modulus tester SB-M1 (manufactured by Toyo Seiki Co., Ltd.). For low temperatures, the test specimen was placed in a freezer set to the respective temperature for one week before measurement.

[0047] The rebound modulus test was evaluated using ◎, ○, and × based on the following criteria: Room temperature: ○: 50% or more, ×: less than 50% -40℃: ◎: 15% or more, ○: 10% or more but less than 15%, ×: less than 10% -30℃: ◎: 30% or more, ○: 20% or more but less than 30%, ×: less than 20% -20℃: ◎: 30% or more, ○: 20% or more but less than 30%, ×: less than 20%

[0048] (Acid Resistance Test) The acid resistance test was conducted in accordance with the Chinese standard GB / T1690-2010 (equivalent to the Japanese Industrial Standard JIS K6258). In the acid resistance test, the rubber material is immersed in an acidic solution, and the change in mass before and after immersion is measured to determine the liquid resistance of the rubber material to the acidic solution.

[0049] A cylindrical test specimen with a diameter of 29.0 mm ± 0.5 mm and a thickness of 12.5 mm ± 0.5 mm was prepared. This test specimen was immersed in a 20% hydrochloric acid (HCl) solution for 168 hours, and the change in mass of the test specimen after immersion relative to the mass of the test specimen before immersion (%) was used as an indicator of acid resistance.

[0050] (Resistance Measurement Test) The resistance measurement test was conducted in accordance with the Chinese standard GB / T1692-2008 (equivalent to the Japanese Industrial Standard JIS K6271-1). In this example, however, it was conducted in accordance with JIS K6911.

[0051] A flat test specimen measuring 150 mm in length, 150 mm in width, and 1 mm in height was prepared. The surface resistivity (Ω / □) and volume resistivity (Ω・cm) were measured when 1000 V was applied to this specimen for 60 seconds.

[0052] Regarding the resistance measurement test, the following criteria were used to evaluate the results as ◎, ○, or ×: <Surface resistivity> ◎: 1.0 × 10 14 Ω / □ or more ○: 1.0×10 13 Ω / □ or more 1.0×10 14 Ω / □ less than ×: 1.0 × 10 13 Ω / □ <Volume resistivity> ◎: 1.0 × 10 13 Ω・cm or more ○: 1.0×10 12 Ω・cm or more 1.0×10 13 Less than Ω・cm ×: 1.0 × 10 12 Less than Ω·cm

[0053] Table 2 shows the results of the compression stress relaxation test, compression set test, rebound modulus test, acid resistance test, and resistance measurement test conducted on each rubber composition prepared based on the compounding ratios in Table 1.

[0054]

[0055] As shown in the results in Table 2, it was found that by creating rubber compositions using each of the compositions specified in the present invention, it is possible to obtain rubber compositions (fuel cell gaskets) that have properties that allow them to be used in general even in low-temperature environments. For example, in the case of the comparative example (EPT), the evaluation of the rebound modulus was × (less than 20%) at -20°C and × (less than 20%) at -30°C, whereas in the case of the example (EBT), the rebound modulus was ○ to ◎ at -20°C and almost ○ at -30°C, showing a significant improvement in the rebound modulus in low-temperature environments. In particular, the rubber compositions of Example 17 and Example 18 received an ◎ evaluation of the rebound modulus at -20°C to -40°C, demonstrating that rubber compositions (fuel cell gaskets) with excellent properties even in low-temperature environments could be created. Thus, it was found that the present invention allows for performance equivalent to or better than that of ordinary EPDM while maintaining low-temperature characteristics.

[0056] As described above, the present invention has made it possible to realize a fuel cell gasket with excellent rebound modulus in low-temperature environments.

[0057] Although one embodiment of the present invention and each example have been described in detail above, it will be readily apparent to those skilled in the art that many modifications are possible without substantially departing from the novel aspects and effects of the present invention. Therefore, all such modifications are included within the scope of the present invention.

[0058] For example, any term that appears at least once in the specification or drawings alongside a broader or synonymous term may be replaced with that different term anywhere in the specification or drawings. Furthermore, the configuration of the fuel cell gasket is not limited to that described in the embodiment of the present invention and each example, and various modifications are possible.

Claims

1. A fuel cell gasket having excellent rebound modulus in low-temperature environments, characterized by containing the following components (A) to (E): (A) A rubber component based on ethylene-butene-diene rubber. (B) A paraffinic hydrocarbon oil containing alpha-olefin as its main component, having a pour point of -70°C or higher and -60°C or lower as a softening agent. (C) Carbon black. (D) A crosslinking agent consisting of an organic peroxide. (E) A crosslinking aid which is a polyfunctional carboxylic acid compound.

2. The fuel cell gasket according to claim 1, characterized in that the content of the softening agent in relation to the fuel cell gasket is 30% by weight or more.

3. The fuel cell gasket according to claim 2, characterized in that the content of the rubber component in the fuel cell gasket is 40% by weight or more.

4. The carbon black has a nitrogen adsorption specific surface area of ​​20 to 30 m². 2 The fuel cell gasket according to claim 3, characterized in that the content is / g and the content relative to the fuel cell gasket is 15 to 35% by weight.