Conductive composite dispersion and method for producing same, capacitor and method for producing same, and conductive laminate and method for producing same

A conductive composite dispersion using π-conjugated conductive polymers and polyanions with specific additives forms a solid electrolyte layer in capacitors, addressing the need for low ESR and heat resistance in high-temperature applications.

WO2026239525A1PCT designated stage Publication Date: 2026-11-19SHIN ETSU POLYMER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/017560
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Capacitors with solid electrolyte layers require low equivalent series resistance (ESR) and good heat resistance, especially in high-temperature environments, which existing technologies struggle to provide effectively.

Method used

A conductive composite dispersion comprising a π-conjugated conductive polymer and a polyanion, combined with specific sugar alcohols, pyridine derivatives, and a thickener, which is applied to form a solid electrolyte layer in capacitors, enhancing heat resistance and reducing ESR.

Benefits of technology

The solution results in capacitors with excellent heat resistance and low initial ESR, suitable for high-temperature environments, while maintaining good conductivity and coating properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000033_0000
    Figure 00000033_0000
Patent Text Reader

Abstract

This conductive composite dispersion comprises: a conductive composite formed of a π-conjugated conductive polymer and a polyanion; water; at least one sugar alcohol having 4-7 carbon atoms and 3-7 hydroxyl groups per molecule; and pyridine or at least one derivative thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive composite dispersion liquid and method for producing the same, capacitor and method for producing the same, and conductive laminate and method for producing the same

[0001] The present invention relates to a conductive composite dispersion liquid containing a π-conjugated conductive polymer and a polyanion, a method for producing the same, a capacitor and a method for producing the same, and a conductive laminate and a method for producing the same.

[0002] A π-conjugated conductive polymer whose main chain is composed of a π-conjugated system forms a conductive composite when doped with a polyanion having an anionic group, and exhibits dispersibility in water. A method for manufacturing a capacitor is disclosed, in which a coating material made from a conductive composite dispersion liquid containing the conductive composite is applied to a dielectric layer provided on the surface of an anode made of a valve metal, dried to form a solid electrolyte layer, and a cathode is arranged to face the solid electrolyte layer (for example, Patent Document 1). According to this disclosure, the performance of the capacitor is improved.

[0003] JP 2014-7422 A

[0004] As for the performance of a capacitor provided with a solid electrolyte layer, low equivalent series resistance (ESR) is required. In addition, assuming that the usage environment of the capacitor will be at a high temperature, it is required that the ESR change rate of the capacitor before and after a heating test is small, that is, the heat resistance is good.

[0005] The present invention provides a capacitor with excellent heat resistance, and a conductive composite dispersion liquid suitable for manufacturing the same.

[0006] [1] A conductive composite dispersion comprising a conductive composite consisting of a π-conjugated conductive polymer and a polyanion, water, one or more sugar alcohols having 4 to 7 carbon atoms in the molecule and 3 to 7 hydroxyl groups, and one or more pyridine or a derivative thereof. [2] The conductive composite dispersion according to [1], wherein the pyridine or a derivative thereof comprises at least one selected from the group consisting of pyridine, 2-hydroxypyridine, 3-hydroxypyridine, 4-hydroxypyridine, 2-methylpyridine, 2,6-dimethylpyridine, and 2,6-dimethyl-4-hydroxypyridine. [3] The conductive composite dispersion according to [1] or [2], wherein the sugar alcohol comprises one or more selected from the group consisting of sorbitol, mannitol, erythritol, inositol, and pentaerythritol. [4] The conductive composite dispersion according to any one of [1] to [3], wherein the content of the conductive composite is 0.8% by mass or more and 2.5% by mass or less with respect to the total mass of the conductive composite dispersion. [5] A conductive composite dispersion according to any one of [1] to [4], further comprising an organic solvent having a boiling point of 150°C or higher at 1 atm. [6] A conductive composite dispersion according to any one of [1] to [5], which does not contain an organic solvent having a boiling point of less than 100°C at 1 atm. [7] A conductive composite dispersion according to any one of [1] to [6], further comprising a thickener. [8] A conductive composite dispersion according to any one of [1] to [7], wherein the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrene sulfonic acid, or the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene) and the polyanion is polystyrene sulfonic acid. [9] A capacitor comprising an anode made of a porous body of valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the side of the dielectric layer opposite to the anode, and a solid electrolyte layer formed between the dielectric layer and the cathode, wherein the solid electrolyte layer is a cured product of a conductive composite dispersion according to any one of [1] to [8].

[10] A conductive laminate comprising a base material and a conductive layer formed on at least a part of the surface of the base material, wherein the conductive layer is a cured product of a conductive composite dispersion according to any one of [1] to [8].

[11] A method for producing a conductive composite dispersion, comprising the step of mixing a conductive composite consisting of a π-conjugated conductive polymer and a polyanion, a dispersion medium, one or more sugar alcohols having 4 to 7 carbon atoms in the molecule and 3 to 7 hydroxyl groups, and one or more pyridine or its derivatives to obtain a conductive composite dispersion.

[12] The method for producing a conductive composite dispersion according to

[11] , comprising obtaining a preliminary dispersion in which the conductive composite is dispersed in the dispersion medium, concentrating the preliminary dispersion, and then mixing one or more sugar alcohols.

[13] A method for producing a capacitor, comprising the step of applying a conductive composite dispersion according to any one of [1] to [8] to the surface of a derivative layer formed on the surface of an anode made of a porous valve metal, and drying to form a solid electrolyte.

[14] A method for manufacturing a conductive laminate, comprising the steps of applying a conductive composite dispersion according to any one of [1] to [8] to at least one surface of a substrate and drying it to form a conductive layer.

[0007] The conductive composite dispersion of the present invention makes it possible to manufacture capacitors with excellent heat resistance. Because the capacitor of the present invention has excellent heat resistance, it can be used even in high-temperature environments. Furthermore, the present invention provides a capacitor that not only has excellent heat resistance but also a low initial ESR.

[0008] This invention is believed to contribute to SDG Goal 12, "Responsible Consumption and Production."

[0009] In this specification and the claims, the lower and upper limits of the numerical range indicated by "~" are to be included within that numerical range.

[0010] This is a cross-sectional view showing one embodiment of a capacitor.

[0011] <Conductive Composite Dispersion> The first aspect of the present invention is a conductive composite dispersion comprising a conductive composite consisting of a π-conjugated conductive polymer and a polyanion, water, one or more specific sugar alcohols, and one or more pyridine or its derivatives.

[0012] <Conductive Composite> The conductive composite of this embodiment comprises a π-conjugated conductive polymer and a polyanion. The polyanion in the conductive composite dops the π-conjugated conductive polymer to form a conductive composite. In the polyanion, only some of the anionic groups dopate the π-conjugated conductive polymer, and there are excess anionic groups that do not participate in doping. Since the excess anionic groups are hydrophilic groups, the conductive composite is water-dispersible.

[0013] (π-conjugated conductive polymers) Any organic polymer whose main chain is composed of a π-conjugated system can be used as a π-conjugated conductive polymer. Examples include polypyrrole-based conductive polymers, polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyphenylene-based conductive polymers, polyphenylene-vinylene-based conductive polymers, polyaniline-based conductive polymers, polyacene-based conductive polymers, polythiophene-vinylene-based conductive polymers, and copolymers thereof. From the viewpoint of stability in air, polypyrrole-based conductive polymers, polythiophenes, and polyaniline-based conductive polymers are preferred, and from the viewpoint of transparency, polythiophene-based conductive polymers are more preferred.

[0014] Examples of polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodine). Thiofen), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyl Poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di Examples include dodecyloxythiophene, poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene).Examples of polypyrrole-based conductive polymers include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole). Examples of polyaniline-based conductive polymers include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-aniline sulfonic acid), and poly(3-aniline sulfonic acid). Among these π-conjugated conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferred due to its excellent conductivity, transparency, and heat resistance. The conductive composite may contain one or more types of π-conjugated conductive polymers.

[0015] (Polyanions) A polyanion is a polymer having two or more monomer units with anionic groups within its molecule. The anionic groups of this polyanion function as dopants for π-conjugated conductive polymers, improving the conductivity of the π-conjugated conductive polymer. The anionic groups of the polyanion are preferably sulfo groups or carboxyl groups. Specific examples of such polyanions include polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having sulfo groups, polymethacrylic acid esters having sulfo groups (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzene sulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), polyisoprene sulfonic acid, and other polymers having sulfo groups, as well as polymers having carboxyl groups such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. Polyanions may be homopolymers formed by the polymerization of a single monomer, or copolymers formed by the polymerization of two or more monomers. Among these polyanions, polymers having sulfo groups are preferred because they can achieve higher conductivity, and polystyrene sulfonic acid is more preferred.

[0016] The weight-average molecular weight Mw of the polyanion is not particularly limited, but is preferably 10,000 to 1,000,000, more preferably 50,000 to 800,000, and even more preferably 100,000 to 600,000. When the weight-average molecular weight Mw of the polyanion is within the above range, the viscosity of the conductive composite dispersion of this embodiment becomes moderately low, and a capacitor with a sufficiently low ESR can be easily manufactured. The weight-average molecular weight Mw of the polyanion is the average molecular weight on a mass basis, determined in terms of pullulan, by measuring it using gel filtration chromatography.

[0017] The polyanion content in the conductive composite dispersion of this embodiment is preferably in the range of 1 to 1000 parts by mass, more preferably 10 to 700 parts by mass, and even more preferably 100 to 500 parts by mass, per 100 parts by mass of the π-conjugated conductive polymer. If the polyanion content is above the lower limit, the doping effect on the π-conjugated conductive polymer tends to be stronger, resulting in higher conductivity. On the other hand, if the polyanion content is below the upper limit, the π-conjugated conductive polymer can be sufficiently contained, thus ensuring sufficient conductivity.

[0018] In the conductive composite dispersion of this embodiment, the content of the conductive composite is preferably 0.1 parts by mass to 3.0 parts by mass, more preferably 0.5 parts by mass to 2.5 parts by mass, and even more preferably 1.0 part by mass to 2.0 parts by mass, based on 100 parts by mass of the total of the conductive composite (total of π-conjugated conductive polymer and polyanion) and water. If the content is above the lower limit of the above range, the conductivity of the cured product of the conductive composite dispersion is further increased. If the content is below the upper limit of the above range, the increase in viscosity of the conductive composite dispersion can be suppressed and the coating properties can be improved.

[0019] The content of the conductive composite (total content of π-conjugated conductive polymer and polyanion) relative to the total mass of the conductive composite dispersion in this embodiment is preferably, for example, 0.1% by mass or more and 3.0% by mass or less, more preferably 0.5% by mass or more and 2.5% by mass or less, and even more preferably 0.8% by mass or more and 2.0% by mass or less. If it is above the lower limit of the above range, the conductivity of the cured product of the conductive composite dispersion is further increased. If it is below the upper limit of the above range, the increase in viscosity of the conductive composite dispersion can be suppressed and the coating properties can be improved.

[0020] (Sugar alcohol) The conductive composite dispersion of this embodiment contains a specific sugar alcohol. The inclusion of the specific sugar alcohol together with pyridine or its derivative can improve the conductivity and heat resistance of the solid electrolyte layer after curing.

[0021] From the viewpoint of fully obtaining the above effects, the sugar alcohol is preferably one in which the number of carbon atoms in the molecule is 4 to 7 and the number of hydroxyl groups is 3 to 7, and one or more selected from the group consisting of sorbitol, mannitol, erythritol, inositol, and pentaerythritol is more preferable, with erythritol being particularly preferred.

[0022] The sugar alcohol content in the conductive composite dispersion of this embodiment is preferably 1.0 part by mass to 30.0 parts by mass, more preferably 3.0 parts by mass to 22.0 parts by mass, even more preferably 5.0 parts by mass to 16.0 parts by mass, and particularly preferably 8.0 parts by mass to 12.0 parts by mass, based on 100 parts by mass of the total of the conductive composite (total of π-conjugated conductive polymer and polyanion) and water. If the content is above the lower limit of the above range, the viscosity of the conductive composite dispersion can be reduced and the coating properties can be further improved. If the content is below the upper limit of the above range, the excess sugar alcohol contained in the conductive composite dispersion can be reduced and the conductivity of the cured product can be improved. As a result, if the content is within the above preferred range, the heat resistance of the solid electrolyte layer, which is the cured product of the conductive composite dispersion, can be further improved and the initial ESR can be good.

[0023] The sugar alcohol content relative to the total mass of the conductive composite dispersion in this embodiment is preferably, for example, 0.1% by mass or more and 20% by mass or less, more preferably 1.0% by mass or more and 18.0% by mass or less, even more preferably 3.0% by mass or more and 15.0% by mass or less, and most preferably 4.0% by mass or more and 10.0% by mass or less. If the content is above the lower limit of the above range, the viscosity of the conductive composite dispersion can be reduced and the coating properties can be further improved. If the content is below the upper limit of the above range, the excess sugar alcohol contained in the conductive composite dispersion can be reduced and the conductivity of the cured product can be improved.

[0024] (Pyridine or its derivatives) The conductive composite dispersion of this embodiment contains pyridine or its derivatives (hereinafter sometimes collectively referred to as "pyridines"). By including pyridines, the heat resistance of the solid electrolyte layer made from the cured product of the conductive composite dispersion of this embodiment can be significantly improved. Pyridine has chemical formula C 5 H5 It is a heterocyclic aromatic compound represented by N. In this embodiment, a derivative of pyridine refers to a compound in which one or more hydrogen atoms bonded to pyridine are substituted with any functional group. Examples of any functional group include a hydroxyl group, a C1-C3 alkyl group, and a monovalent group obtained by removing one of the hydrogen atoms present in a C1-C3 alkyl alcohol.

[0025] Specific preferred pyridines include, for example, at least one selected from the group consisting of pyridine, 2-hydroxypyridine, 3-hydroxypyridine, 4-hydroxypyridine, 2-methylpyridine, 2,6-dimethylpyridine, and 2,6-dimethyl-4-hydroxypyridine.

[0026] The pyridine content in the conductive composite dispersion of this embodiment is preferably 1.0 part by mass to 30.0 parts by mass, more preferably 1.0 part by mass to 20.0 parts by mass, and even more preferably 1.0 part by mass to 10.0 parts by mass, based on 1,000 parts by mass of the total of the conductive composite (total of π-conjugated conductive polymer and polyanion) and water. Within the above range, the heat resistance of the solid electrolyte layer can be further improved.

[0027] The pyridine content in the conductive composite dispersion of this embodiment is preferably, for example, 0.1% by mass or more and 2.0% by mass or less, more preferably 0.1% by mass or more and 1.5% by mass or less, and even more preferably 0.1% by mass or more and 1.0% by mass or less. Within this range, the heat resistance of the solid electrolyte layer can be further improved.

[0028] In this embodiment, the pH of the conductive composite dispersion at 25°C after the addition of pyridines is preferably 2.0 to 4.0, more preferably 2.0 to 3.5, and even more preferably 2.0 to 3.0. Within this range, chemical erosion of the component in contact with the conductive composite dispersion can be reduced, and the heat resistance of the solid electrolyte layer can be further improved.

[0029] (Thickener) The conductive composite dispersion of this embodiment may contain one or more thickeners as optional components. The thickener is an additive in which a polymer is the active ingredient, and can adjust the viscosity and rheological properties of the conductive composite dispersion. In other words, by adding a thickener, the viscosity of the conductive composite dispersion can be increased, thereby improving its applicability. It is preferable that the amount of thickener added be as small as possible, and if the desired viscosity can be obtained by adding the sugar alcohol, the thickener may not be added at all.

[0030] The polymer, which is the active ingredient of the thickener, is a polymer other than the aforementioned π-conjugated conductive polymer and polyanion, and examples include polyvinylpyrrolidone, cellulose ether resin, polyacrylic acid resin, polyurethane resin, carboxyvinyl polymer, and polyvinyl alcohol. Among these, polyvinylpyrrolidone is preferred because it increases the transparency of the formed conductive layer, reduces haze, and further improves adhesion to the substrate.

[0031] The amount of the thickener relative to the total mass of the conductive polymer dispersion in this embodiment is preferably, for example, 1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and even more preferably 7 to 20 parts by mass, per 1000 parts by mass of the total of the π-conjugated conductive polymer and polyanion. This range is preferable because it increases the transparency of the formed conductive layer, reduces haze, and further improves adhesion to the substrate.

[0032] (Dispersion Medium) The dispersion medium contained in the conductive composite dispersion is preferably an aqueous dispersion medium containing water, since the conductive composite is hydrophilic. It may also contain a dispersion medium other than water. The dispersion medium other than water is not particularly limited as long as it does not significantly impair the dispersibility of the conductive composite. Since the conductive composite has excess anionic groups derived from polyanions and has high dispersibility in water, the dispersion medium other than water is preferably a water-soluble organic solvent. Here, a water-soluble organic solvent is an organic solvent whose solubility in 100 g of water at 20°C is 1 g or more, and examples include alcohol-based solvents, ketone-based solvents, and ester-based solvents. The water-soluble organic solvent contained as the dispersion medium may be one type or two or more types. A non-water-soluble organic solvent is an organic solvent whose solubility is less than 1 g.

[0033] The water content relative to the total mass of the conductive composite dispersion is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. It is also preferable that it be 99% by mass or less. When water is included at or above the lower limit, the dispersibility of the conductive composite contained in the conductive composite dispersion is increased, the viscosity is reduced, and the ESR of the capacitor having a solid electrolyte layer formed from the conductive composite dispersion can be further reduced. Furthermore, the conductivity of the conductive layer formed from the conductive composite dispersion can be further increased.

[0034] (High-boiling point solvent) The conductive composite dispersion of this embodiment may further contain, as an optional component, one or more organic solvents (high-boiling point solvents) having a boiling point of 150°C or higher at 1 atmosphere (101325 Pascals). Preferably, the boiling point is 250°C or lower. By including a high-boiling point solvent, the effect of improving the conductivity of the cured product of the conductive composite dispersion can be obtained.

[0035] Examples of high-boiling point solvents include water-soluble organic solvents and water-insoluble organic solvents. Here, the definitions of water-soluble organic solvents and water-insoluble organic solvents are the same as described above.

[0036] Examples of high-boiling-point water-soluble organic solvents include alcohol-based solvents, ether-based solvents, ketone-based solvents, nitrogen-containing solvents, and sulfur-containing solvents. Examples of alcohol-based solvents include polyhydric alcohols such as ethylene glycol (boiling point 198°C), 1,2-propanediol (also known as propylene glycol, boiling point 188°C), 1,3-propanediol (boiling point 214°C), 1,2-butanediol (boiling point 194°C), 1,3-butanediol (boiling point 207°C), 1,4-butanediol (boiling point 228°C), dipropylene glycol (boiling point 232°C, mixture of isomers), and diethylene glycol (boiling point 245°C). Examples of ether-based solvents include diethylene glycol dimethyl ether (boiling point 162°C) and diethylene glycol diethyl ether (boiling point 188°C). Examples of ketone-based solvents include methyl amyl ketone (boiling point 151°C) and diacetone alcohol (boiling point 168°C). Examples of nitrogen atom-containing solvents include N-methylpyrrolidone (boiling point 202°C), N-methylacetamide (boiling point 206°C), dimethylacetamide (boiling point 165°C), and N,N-dimethylformamide (boiling point 153°C). Examples of sulfur atom-containing solvents include dimethyl sulfoxide (boiling point 189°C).

[0037] Examples of high-boiling-point, water-insoluble organic solvents include hydrocarbon solvents. Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents and aromatic hydrocarbon solvents. Examples of aliphatic hydrocarbon solvents include nonane (boiling point 151°C), decane (boiling point 174°C), and dodecane (boiling point 216°C). Examples of aromatic hydrocarbon solvents include propylbenzene (boiling point 159°C) and isopropylbenzene (boiling point 152°C).

[0038] Among the above examples, high-boiling point alcohol-based solvents are preferred because they provide an even greater effect in improving conductivity. Among high-boiling point alcohol-based solvents, ethylene glycol (boiling point 198°C), 1,2-propanediol (boiling point 188°C), 1,3-propanediol (boiling point 214°C), diethylene glycol (boiling point 245°C), and dimethyl sulfoxide (boiling point 189°C) are preferred because they exhibit superior effects such as improved conductivity.

[0039] The content of the high-boiling-point solvent in the conductive composite dispersion is preferably, for example, 10 parts by mass or more and 2000 parts by mass or less, more preferably 100 parts by mass or more and 1000 parts by mass or less, and even more preferably 500 parts by mass or more and 900 parts by mass or less, per 100 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion). Within this range, the ESR of the capacitor having a solid electrolyte layer formed from the conductive composite dispersion can be further reduced. In addition, the conductivity of the conductive layer formed from the conductive composite dispersion can be further improved.

[0040] The content of the high-boiling-point solvent relative to the total mass of the conductive polymer-containing liquid in this embodiment is preferably, for example, 0.1% by mass or more and 20% by mass or less, more preferably 1.0% by mass or more and 18.0% by mass or less, even more preferably 3.0% by mass or more and 15.0% by mass or less, and most preferably 6.0% by mass or more and 12.0% by mass or less. If it is above the lower limit of the above range, the ESR and conductivity can be further improved. If it is below the upper limit of the above range, the increase in viscosity of the conductive composite dispersion can be kept low.

[0041] (Low Boiling Point Solvents) The conductive composite dispersion of this embodiment preferably does not contain organic solvents (low boiling point solvents) having a boiling point of less than 100°C at 1 atmosphere. The absence of low boiling point solvents has the effect of improving the storage stability of the conductive composite dispersion.

[0042] (Optional Additives) The conductive composite dispersion liquid may contain other optional additives. The content ratio thereof is appropriately determined according to the type of the additive, and may be, for example, 1 to 1000 parts by mass relative to 100 parts by mass in total of the π-conjugated conductive polymer and the polyanion. Here, the optional additives are compounds other than the conductive composite, the sugar alcohol, pyridine or a derivative thereof, the thickener, the high-boiling-point solvent, and the dispersion medium.

[0043] Examples of the optional additives include surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, ultraviolet absorbers, and the like. Examples of the surfactants include nonionic, anionic, and cationic surfactants, and nonionic surfactants are preferred from the viewpoint of storage stability. Further, a polymeric surfactant such as polyvinyl alcohol may be added. Examples of the inorganic conductive agents include metal ions, conductive carbon, and the like. The metal ions can be generated by dissolving a metal salt in water. Examples of the antifoaming agents include silicone resins, polydimethylsiloxane, silicone oil, and the like. Examples of the coupling agents include silane coupling agents having a vinyl group, an amino group, an epoxy group, or the like. Examples of the antioxidants include phenolic antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, saccharides, and the like. Examples of the ultraviolet absorbers include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, benzoate-based ultraviolet absorbers, and the like.

[0044] <<Method for Producing Conductive Composite Dispersion Liquid>> Examples of the method for producing the conductive composite dispersion liquid according to the first aspect of the present invention include a method of mixing a conductive composite, a dispersion medium, one or more of the sugar alcohols, and one or more of pyridine or a derivative thereof, and adding optional components (for example, a high-boiling-point solvent, a thickener, etc.) as necessary.

[0045] In producing the conductive composite dispersion liquid of the first aspect, it is preferable to obtain a preliminary dispersion liquid in which the conductive composite is dispersed in the dispersion medium, concentrate the preliminary dispersion liquid, and then mix one or more types of the sugar alcohol. When produced by the procedure of mixing the sugar alcohol into the preliminary dispersion liquid with an increased concentration of the conductive composite, the effect of eliminating the loss of the sugar alcohol can be obtained. That is, if a procedure is adopted in which the conductive composite dispersion liquid is treated by an ultrafiltration method after the sugar alcohol is added to increase the concentration of the conductive composite, the sugar alcohol will permeate through the ultrafiltration membrane and be lost out of the system.

[0046] The preliminary dispersion liquid in which the conductive composite is dispersed in water can be obtained by chemically oxidatively polymerizing a monomer that forms a π-conjugated conductive polymer in an aqueous solution of a polyanion by a known method. A commercially available product may be used as the preliminary dispersion liquid.

[0047] «Method for producing capacitor» A capacitor can be produced by a production method including the step of applying the conductive composite dispersion liquid of the first aspect to the surface of a dielectric layer formed on the surface of an anode composed of a porous body of a valve metal, and drying it to form a solid electrolyte layer.

[0048] The method for producing a capacitor preferably includes: a step of oxidizing the surface of an anode composed of a porous body of a valve metal to form a dielectric layer (dielectric formation step); a step of disposing a cathode at a position opposite to the dielectric layer (cathode formation step); and a step of forming a solid electrolyte layer on at least a part of the surface of the dielectric layer (film formation step). Hereinafter, each step will be described with reference to Figure 1.

[0049] [Dielectric formation step] In this step, the surface of the anode 11 composed of a porous body of a valve metal is oxidized to form the dielectric layer 12. The method for forming the dielectric layer 12 is not particularly limited, and examples thereof include a method of anodizing the surface of the anode 11 in a chemical conversion electrolytic solution such as an aqueous ammonium adipate solution, an aqueous ammonium borate solution, and an aqueous ammonium phosphate solution.

[0050] [Cathode Formation Process] In this process, a cathode 13 is placed opposite the dielectric layer 12. The method of arranging the cathode 13 is not particularly limited, and examples include forming the cathode 13 using a conductive paste such as carbon paste or silver paste, or arranging a metal foil such as aluminum foil opposite the dielectric layer 12.

[0051] [Film Formation Process] In this process, the aforementioned conductive composite dispersion is applied to at least a portion of the surface of the dielectric layer 12 and dried to form a solid electrolyte layer 14.

[0052] For example, the conductive composite dispersion can be applied by dip coating, comma coating, reverse coating, lip coating, microgravure coating, etc. Of these, the method of immersing the anode 11 in the conductive composite dispersion under reduced pressure is preferred. With the dip method, the conductive composite dispersion can be sufficiently applied to the interior of the porous structure on the surface of the dielectric layer 12. After immersion, it is removed and the next drying process is carried out.

[0053] Examples of drying methods include room temperature drying, hot air drying, and far-infrared drying. Among these, hot air drying is preferred. The drying temperature is preferably 100 to 180°C, and more preferably 120 to 150°C. The drying time is preferably 0.2 to 1 hour. After the drying process, the capacitor can be assembled by conventional methods.

[0054] <Capacitor> The capacitor comprises an anode made of a porous body of valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the side of the dielectric layer opposite to the anode, and a solid electrolyte layer formed between the dielectric layer and the cathode, wherein the solid electrolyte layer contains a cured product of the conductive composite dispersion of the first embodiment.

[0055] An example of an embodiment of the capacitor described above will be explained with reference to Figure 1. The capacitor 10 shown in Figure 1 comprises an anode 11 made of a porous valve metal, a dielectric layer 12 made of an oxide of the valve metal, a solid electrolyte layer 14 formed on the surface of the dielectric layer 12, and a cathode 13 provided on the outermost side. The cathode 13 is provided on the opposite side from the anode 11, with the dielectric layer 12 and the solid electrolyte layer 14 in between.

[0056] Examples of valve metals constituting the anode 11 include aluminum, tantalum, niobium, titanium, hafnium, zirconium, zinc, tungsten, bismuth, and antimony. Of these, aluminum, tantalum, and niobium are preferred. Specific examples of the anode 11 include aluminum foil that has been etched to increase its surface area and then oxidized, or sintered tantalum particles or niobium particles whose surfaces have been oxidized to form pellets. Materials processed in this way become porous bodies with irregularities formed on their surfaces.

[0057] In this embodiment, the dielectric layer 12 is a layer formed by oxidation of the surface of the anode 11, and is formed, for example, by anodizing the surface of the metal anode 11 in an electrolyte solution such as an aqueous solution of ammonium adipate. Similar to the anode 11, the dielectric layer 12 also has irregularities formed on it.

[0058] In this embodiment, the cathode 13 can be a conductive layer formed from a conductive paste or a metal layer made of a conductive material such as aluminum foil.

[0059] In this embodiment, the solid electrolyte layer 14 is formed on the surface of the dielectric layer 12. The solid electrolyte layer 14 covers at least a portion of the surface of the dielectric layer 12, and may cover the entire surface of the dielectric layer 12. The thickness of the solid electrolyte layer 14 may be constant or not; for example, a thickness of 1 μm or more and 100 μm or less is possible.

[0060] The composition of the components contained in the solid electrolyte layer 14 reflects the composition of the coated conductive composite dispersion. The content of the sugar alcohol per 100 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion) contained in the solid electrolyte layer 14 is preferably, for example, 100 parts by mass or more and 5000 parts by mass or less, more preferably 200 parts by mass or more and 2000 parts by mass or less, and even more preferably 300 parts by mass or more and 1000 parts by mass or less. Within the above range, the ESR of the capacitor is further reduced.

[0061] The pyridine content per 100 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion) contained in the solid electrolyte layer 14 is preferably, for example, 1 part by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 70 parts by mass or less, and even more preferably 20 parts by mass or more and 50 parts by mass or less. Within the above range, the heat resistance of the capacitor is further improved.

[0062] The amount of an optional thickening agent per 1000 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion) contained in the solid electrolyte layer 14 is preferably, for example, 1 to 50 parts by mass, more preferably 3 to 25 parts by mass, and even more preferably 5 to 15 parts by mass. Within this range, the heat resistance of the capacitor is further improved.

[0063] [Electrolyte] The capacitor may have an electrolyte impregnating the solid electrolyte layer. Examples of solvents constituting the electrolyte include alcohol-based solvents such as ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, and glycerin; lactone-based solvents such as γ-butyrolactone, γ-valerolactone, and δ-valerolactone; sulfur-based solvents such as sulfolane, dimethyl sulfoxide, and dimethyl sulfone; amide-based solvents such as N-methylformamide, N,N-dimethylformamide, N-methylacetamide, and N-methylpyrrolidinone; nitrile-based solvents such as acetonitrile and 3-methoxypropionitrile; and water. The electrolytes constituting the electrolyte solution include, for example, adipic acid, glutaric acid, succinic acid, benzoic acid, isophthalic acid, phthalic acid, terephthalic acid, maleic acid, toluic acid, enanthic acid, malonic acid, formic acid, decanedicarboxylic acids such as 1,6-decanedicarboxylic acid and 5,6-decanedicarboxylic acid, octanedicarboxylic acids such as 1,7-octanedicarboxylic acid, organic acids such as azelaic acid and sebacic acid; or boric acid, polyhydric alcohol complex compounds of boric acid obtained from boric acid and polyhydric alcohols; inorganic acids such as phosphoric acid, carbonic acid and silicic acid are used as anionic components, and primary amines (methylamine, ethylamine, propylamine, Examples include electrolytes with cationic components such as butylamine, ethylenediamine, secondary amines (dimethylamine, diethylamine, dipropylamine, methylethylamine, diphenylamine, etc.), tertiary amines (trimethylamine, triethylamine, tripropylamine, triphenylamine, 1,8-diazabicyclo(5,4,0)-undecene-7, etc.), and tetraalkylammonium (tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, methyltriethylammonium, dimethyldiethylammonium, etc.).

[0064] The capacitor is not limited to the above configuration; a separator may be provided between the dielectric layer and the cathode. An example of a capacitor with a separator between the dielectric layer and the cathode is a wound capacitor. Examples of separators include sheets (including nonwoven fabrics) made of cellulose, polyvinyl alcohol, polyester, polyethylene, polystyrene, polypropylene, polyimide, polyamide, polyvinylidene fluoride, etc., and glass fiber nonwoven fabrics. The density of the separator is, for example, 0.1 g / cm³. 3 1.0g / cm or more 3 The following are examples: When a separator is provided, a method can be applied in which carbon paste or silver paste is impregnated into the separator to form the cathode.

[0065] <<Method for Manufacturing Conductive Laminates>> A conductive laminate can be manufactured by a manufacturing method that includes the step of coating a conductive composite dispersion according to the first embodiment of the present invention onto at least a portion of the surface of a substrate to form a conductive layer.

[0066] Methods for coating (applying) the conductive composite dispersion to any surface of a substrate include, for example, methods using coaters such as gravure coaters, roll coaters, curtain flow coaters, spin coaters, bar coaters, reverse coaters, kiss coaters, fountain coaters, rod coaters, air doctor coaters, knife coaters, blade coaters, cast coaters, and screen coaters; methods using sprayers such as air sprayers, airless sprayers, and rotor dampening devices; and immersion methods such as dipping.

[0067] The amount of conductive composite dispersion applied to the substrate is not particularly limited, but for example, 0.01 to 10.0 g / m² of non-volatile components is recommended. 2 A range of [specified range] is preferred.

[0068] A conductive layer can be formed by drying a coating film made of a conductive composite dispersion applied to a substrate, removing at least a portion of the dispersion medium, and curing it. Methods for drying the coating film include heat drying and vacuum drying. For heat drying, for example, methods such as hot air heating and infrared heating can be used. When heat drying is applied, the heating temperature is set appropriately according to the dispersion medium used, but is usually in the range of 50°C to 200°C. Here, the heating temperature is the set temperature of the drying apparatus. A suitable drying time within the above heating temperature range is preferably 0.5 minutes to 30 minutes, and more preferably 1 minute to 15 minutes.

[0069] <<Conductive Laminate>> The conductive laminate comprises a substrate and a conductive layer formed on at least a portion of the surface of the substrate, wherein the conductive layer includes a cured product of the conductive composite dispersion of the first embodiment.

[0070] [Conductive Layer] The area in which the conductive layer is formed may be the entire surface of any surface of the substrate, or it may be only a part of it. In a conductive film, it is preferable that a conductive layer of substantially uniform thickness is formed on substantially the entire surface of one or the other surface of the film substrate. If the conductive layer is formed on only a part of the surface of the substrate, for example, the conductive layer may be a fine conductive pattern such as a circuit or an electrode, or the area with the conductive layer and the area without the conductive layer may exist on the same surface and be roughly separated.

[0071] The average thickness of the conductive layer is preferably, for example, 10 nm to 100 μm, more preferably 20 nm to 50 μm, and even more preferably 30 nm to 30 μm. If the average thickness of the conductive layer is above the lower limit, high conductivity can be achieved, and if it is below the upper limit, the adhesion of the conductive layer to the substrate is further improved.

[0072] The composition of the components contained in the conductive layer reflects the composition of the coated conductive composite dispersion. The content of the sugar alcohol per 100 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion) contained in the conductive layer is preferably, for example, 100 parts by mass or more and 5000 parts by mass or less, more preferably 200 parts by mass or more and 2000 parts by mass or less, and even more preferably 300 parts by mass or more and 1000 parts by mass or less. Within the above range, the conductivity of the conductive layer is good.

[0073] The pyridine content per 100 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion) contained in the conductive layer is preferably, for example, 1 part by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 70 parts by mass or less, and even more preferably 20 parts by mass or more and 50 parts by mass or less. Within this range, the heat resistance of the conductive layer is further improved.

[0074] The amount of an optional thickening agent per 1000 parts by mass of the conductive composite (total of π-conjugated conductive polymer and polyanion) contained in the conductive layer is preferably, for example, 1 part by mass or more and 50 parts by mass or less, more preferably 3 parts by mass or more and 25 parts by mass or less, and even more preferably 5 parts by mass or more and 15 parts by mass or less. Within this range, the adhesion of the conductive layer to the substrate is further improved, and the heat resistance is also further improved.

[0075] [Substrate] The substrate may be made of an insulating material or a conductive material. The shape of the substrate is not particularly limited, and examples include flat shapes such as films and substrates. Examples of insulating materials include glass, synthetic resins, and ceramics. Examples of conductive materials include metals, conductive metal oxides, and carbon.

[0076] (Film Substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. Examples of the film substrate include plastic films made of synthetic resins. Examples of the synthetic resins include ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene elastomer, polyester elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, and cellulose acetate propionate. From the viewpoint of improving adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably a polyester resin, and among these, polyethylene terephthalate is preferred.

[0077] The synthetic resin for the film substrate may be amorphous or crystalline. The film substrate may be unstretched or stretched. The film substrate may be subjected to surface treatments such as corona discharge treatment, plasma treatment, or flame treatment to further improve the adhesion of the conductive layer.

[0078] The average thickness of the film substrate is preferably 5 μm to 500 μm, and more preferably 20 μm to 200 μm. If the average thickness of the film substrate is above the lower limit, it becomes less likely to break, and if it is below the upper limit, sufficient flexibility as a film can be ensured. The average thickness of the film substrate is the average value obtained by measuring the thickness at 10 randomly selected locations.

[0079] (Glass Substrate) Examples of glass substrates include alkali-free glass substrates, soda-lime glass substrates, borosilicate glass substrates, and quartz glass substrates. Since the presence of alkaline components in the substrate tends to reduce the conductivity of the conductive layer, alkali-free glass is preferred among the glass substrates. Here, alkali-free glass refers to a glass composition in which the content of alkaline components is 0.1% by mass or less of the total mass of the glass composition.

[0080] The average thickness of the glass substrate is preferably 100 μm to 3000 μm, and more preferably 100 μm to 1000 μm. If the average thickness of the glass substrate is above the lower limit, it becomes less prone to breakage, and if it is below the upper limit, it contributes to thinning the conductive laminate. The average thickness of the glass substrate is the average value obtained by measuring the thickness at 10 randomly selected locations.

[0081] (Manufacturing Example 1) Production of Polystyrene Sulfonic Acid 206 g of sodium styrene sulfonate was dissolved in 1000 ml of deionized water, and while stirring at 80°C, 1.14 g of ammonium persulfate oxidizing agent solution, which had been previously dissolved in 10 ml of water, was added dropwise for 20 minutes, and the solution was stirred for 12 hours. 1000 ml of sulfuric acid diluted to 10% by mass was added to the obtained sodium polystyrene sulfonate-containing solution, and approximately 1000 ml of solvent was removed from the polystyrene sulfonic acid-containing solution by ultrafiltration. Next, 2000 ml of deionized water was added to the remaining solution, and approximately 2000 ml of solvent was removed by ultrafiltration, and the polystyrene sulfonic acid was washed with water. This washing operation was repeated three times. The water in the obtained solution was removed under reduced pressure to obtain colorless solid polystyrene sulfonic acid.

[0082] (Manufacturing Example 2) Preparation of Conductive Polymer Aqueous Dispersion A solution of 14.2 g of 3,4-ethylenedioxythiophene and 36.7 g of polystyrene sulfonic acid dissolved in 2000 ml of deionized water was mixed at 20°C. The resulting mixed solution was kept at 20°C and, while stirring, a solution of 29.64 g of ammonium persulfate and 8.0 g of ferric sulfate oxidation catalyst dissolved in 200 ml of deionized water was slowly added and stirred for 3 hours to allow the reaction to proceed. 2000 ml of deionized water was added to the resulting reaction solution and approximately 2000 ml of solvent was removed by ultrafiltration. This operation was repeated three times. Then, 200 ml of sulfuric acid diluted to 10% by mass and 2000 ml of deionized water were added to the resulting solution and approximately 2000 ml of solvent was removed by ultrafiltration. 2000 ml of deionized water was added to the remaining solution and approximately 2000 ml of the solution was removed by ultrafiltration. This procedure was repeated three times. Furthermore, 2000 ml of deionized water was added to the obtained solution, and approximately 2000 ml of solvent was removed by ultrafiltration. This procedure was repeated five times to obtain a 1.2% by mass polystyrene sulfonic acid-doped poly(3,4-ethylenedioxythiophene) aqueous dispersion (i.e., PEDOT-PSS aqueous dispersion). Further ultrafiltration was performed to obtain a PEDOT-PSS aqueous dispersion with a non-volatile component concentration of 1.7% by mass.

[0083] (Production Example 3) Preparation of conductive polymer aqueous dispersion A 1.2% by mass PEDOT-PSS aqueous dispersion was obtained in the same manner as in Production Example 2, and then ultrafiltration was performed to obtain a PEDOT-PSS aqueous dispersion with a non-volatile component concentration of 2.0% by mass.

[0084] (Manufacturing Example 4) Preparation of Capacitor Element After connecting anode lead terminals to etched aluminum foil (anodic foil), a voltage of 40V was applied in a 10% by mass aqueous solution of ammonium adipate to perform chemical conversion (oxidation treatment) to form dielectric layers on both sides of the aluminum foil and obtain an anode foil. Next, opposing aluminum anode foils, each with anode lead terminals welded to both sides of the anode foil, were laminated on both sides of the anode foil via a cellulose separator, and this was wound into a cylindrical shape to obtain a capacitor element.

[0085] (Manufacturing Example 5) A driving electrolyte was obtained by mixing 77 g of ethylene glycol, 23 g of polyethylene glycol #300, and 1 g of p-hydroxybenzoic acid.

[0086] (Example 1) To 70 g of PEDOT-PSS aqueous dispersion obtained in Production Example 2, 30 g of deionized water, 0.46 g of 4-hydroxypyridine, 10 g of 1,3-propanediol, and 10 g of erythritol were added and stirred for 30 minutes to obtain a paint composition (conductive composite dispersion). The pH of the paint composition was 2.5. Next, the paint composition was immersed in the capacitor element obtained in Production Example 4 under reduced pressure, and then dried in a hot air dryer at 160°C for 60 minutes to form a solid electrolyte containing a conductive composite on the surface of the dielectric layer, thereby obtaining a capacitor element. Finally, the capacitor element with the solid electrolyte layer formed above and the driving electrolyte obtained in Production Example 5 were loaded into an aluminum case, sealed with sealing rubber, and then heated at 125°C for 30 minutes with an applied voltage of 40 V to produce a capacitor.

[0087] (Example 2) To the 80 g PEDOT-PSS aqueous dispersion obtained in Production Example 2, 20 g of deionized water, 0.53 g of 4-hydroxypyridine, 10 g of 1,3-propanediol, and 10 g of erythritol were added and stirred for 30 minutes to obtain a paint composition with a pH of 2.5. The capacitor was prepared in the same manner as in Example 1, except for this step.

[0088] (Example 3) To 90 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 10 g of deionized water, 0.59 g of 4-hydroxypyridine, 10 g of 1,3-propanediol, and 10 g of erythritol were added and stirred for 30 minutes to obtain a paint composition with a pH of 2.5. The capacitor was prepared in the same manner as in Example 1, except for this step.

[0089] (Comparative Example 1) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 1, except that 10 g of deionized water was added instead of 10 g of erythritol.

[0090] (Example 4) To 100 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 0.66 g of 3-hydroxypyridine, 10 g of diethylene glycol, and 10 g of erythritol were added and stirred for 30 minutes to obtain a paint composition with a pH of 2.4. The capacitor was prepared in the same manner as in Example 1, except for this step.

[0091] (Example 5) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 4, except that 0.66 g of 4-hydroxypyridine was added instead of 0.66 g of 3-hydroxypyridine.

[0092] (Example 6) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 5, except that 0.5 g of erythritol was added instead of 10 g.

[0093] (Example 7) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 5, except that 2 g of erythritol was added instead of 10 g.

[0094] (Example 8) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 5, except that 18 g of erythritol was added instead of 10 g.

[0095] (Example 9) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 5, except that 30 g of erythritol was added instead of 10 g.

[0096] (Example 10) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 4, except that 10 g of sorbitol was added instead of 10 g of erythritol.

[0097] (Example 11) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 4, except that 10 g of mannitol was added instead of 10 g of erythritol.

[0098] (Example 12) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 5, except that 0.85 g of 2,6-dimethyl-4-hydroxypyridine was added instead of 0.66 g of 4-hydroxypyridine.

[0099] (Example 13) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 5, except that 0.55 g of pyridine was added instead of 0.66 g of 4-hydroxypyridine.

[0100] (Comparative Example 2) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 13, except that 10 g of deionized water was added instead of 10 g of erythritol.

[0101] (Comparative Example 3) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 4, except that 10 g of deionized water was added instead of 10 g of erythritol.

[0102] (Example 14) A capacitor was prepared in the same manner as in Example 2, except that 0.01 g of polyvinylpyrrolidone (manufactured by Nippon Shokubai Co., Ltd., product name: PVP K-90) was added to the paint composition of Example 2 to obtain a paint composition with a pH of 2.5.

[0103] (Example 15) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 14, except that 10 g of sorbitol was added instead of 10 g of erythritol.

[0104] (Example 16) To 100 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 2, 0.66 g of 4-hydroxypyridine, 10 g of 1,3-propanediol, 10 g of erythritol, and 0.01 g of polyvinylpyrrolidone (manufactured by Nippon Shokubai Co., Ltd., product name: PVP K-90) were added and stirred for 30 minutes to obtain a paint composition with a pH of 2.5. The capacitor was prepared in the same manner as in Example 14, except for this part.

[0105] (Example 17) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 16, except that 0.66 g of 3-hydroxypyridine was added instead of 0.66 g of 4-hydroxypyridine.

[0106] (Example 18) A paint composition with a pH of 2.5 and a capacitor were prepared in the same manner as in Example 16, except that 0.85 g of 2,6-dimethyl-4-hydroxypyridine was added instead of 0.66 g of 4-hydroxypyridine.

[0107] (Comparative Example 4) To 100 g of the PEDOT-PSS aqueous dispersion obtained in Production Example 3, 0.44 g of imidazole, 10 g of diethylene glycol, and 10 g of sorbitol were added and stirred for 30 minutes to obtain a paint composition with a pH of 2.5. The capacitor was prepared in the same manner as in Example 10, except for this step.

[0108] [pH Measurement] The pH was measured at 25°C using a commercially available pH meter and a standard method.

[0109] [Measurement of Equivalent Series Resistance] For capacitors fabricated using the conductive composite dispersions of each example, the equivalent series resistance (ESR) (unit: mΩ) at 100 kHz was measured using an LCR meter ZM2376 (manufactured by NF Circuit Design Block Co., Ltd.). After measuring the initial ESR (before testing), the capacitors were left to stand in a 145°C incubator for 500 hours. Subsequently, the ESR (after testing) was measured again. These measurement results are shown in Table 1.

[0110]

[0111] The conductive composite dispersion produced in the embodiment of the present invention contains pyridine or its derivative and a specific sugar alcohol. The capacitor produced using the conductive composite dispersion of this embodiment showed a low rate of change in ESR before and after the heat resistance test, demonstrating remarkably excellent heat resistance.

[0112] On the other hand, the conductive composite dispersions of Comparative Examples 1 to 3 did not contain sugar alcohols, and therefore the heat resistance of the capacitors was poor. The conductive composite dispersion of Comparative Example 4 did not contain pyridine or its derivatives, but instead contained imidazole, and therefore, despite containing sugar alcohols, it had poor heat resistance.

[0113] 10...Capacitor, 11...Anode, 12...Dielectric layer, 13...Cathode, 14...Solid electrolyte layer

Claims

1. A conductive composite dispersion comprising a conductive composite consisting of a π-conjugated conductive polymer and a polyanion, water, one or more sugar alcohols having 4 to 7 carbon atoms in the molecule and 3 to 7 hydroxyl groups, and one or more pyridines or derivatives thereof.

2. The conductive composite dispersion according to claim 1, wherein the pyridine or its derivative comprises at least one selected from the group consisting of pyridine, 2-hydroxypyridine, 3-hydroxypyridine, 4-hydroxypyridine, 2-methylpyridine, 2,6-dimethylpyridine, and 2,6-dimethyl-4-hydroxypyridine.

3. The conductive composite dispersion according to claim 2, wherein the sugar alcohol comprises one or more selected from the group consisting of sorbitol, mannitol, erythritol, inositol, and pentaerythritol.

4. The conductive composite dispersion according to claim 3, wherein the content of the conductive composite is 0.8% by mass or more and 2.5% by mass or less with respect to the total mass of the conductive composite dispersion.

5. The conductive composite dispersion according to claim 4, further comprising an organic solvent having a boiling point of 150°C or higher at 1 atmosphere.

6. The conductive composite dispersion according to claim 5, which does not contain an organic solvent having a boiling point of less than 100°C at 1 atmosphere.

7. The conductive composite dispersion according to claim 6, further comprising a thickening agent.

8. The conductive composite dispersion according to claim 7, wherein the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrene sulfonic acid, or the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene) and the polyanion is polystyrene sulfonic acid.

9. A capacitor comprising an anode made of a porous body of valve metal, a dielectric layer made of an oxide of the valve metal, a cathode made of a conductive material provided on the dielectric layer opposite to the anode, and a solid electrolyte layer formed between the dielectric layer and the cathode, wherein the solid electrolyte layer is a cured product of the conductive composite dispersion according to any one of claims 1 to 8.

10. A conductive laminate comprising a substrate and a conductive layer formed on at least a portion of the surface of the substrate, wherein the conductive layer is a cured product of a conductive composite dispersion according to any one of claims 1 to 8.

11. A method for producing a conductive composite dispersion, comprising the steps of mixing a conductive composite consisting of a π-conjugated conductive polymer and a polyanion, a dispersion medium, one or more sugar alcohols having 4 to 7 carbon atoms in the molecule and 3 to 7 hydroxyl groups, and one or more pyridines or derivatives thereof to obtain a conductive composite dispersion.

12. A method for producing a conductive composite dispersion according to claim 11, comprising obtaining a preliminary dispersion in which the conductive composite is dispersed in the dispersion medium, concentrating the preliminary dispersion, and then mixing in one or more of the sugar alcohols.

13. A method for manufacturing a capacitor, comprising the step of applying a conductive composite dispersion according to any one of claims 1 to 8 to the surface of a derivative layer formed on the surface of an anode made of a porous valve metal, and drying it to form a solid electrolyte.

14. A method for manufacturing a conductive laminate, comprising the step of applying a conductive composite dispersion according to any one of claims 1 to 8 to at least one surface of a substrate and drying it to form a conductive layer.