High-carbon cold-rolled steel sheet, high-carbon hot-rolled steel sheet, and spiral spring
The high-carbon steel sheets achieve enhanced strength and fatigue resistance by refining the pearlite structure during hot rolling, addressing the environmental and productivity issues of traditional methods without spheroidizing annealing or patenting treatments.
Patent Information
- Application Number
- PCT/JP2025/037456
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2025-10-24
- Publication Date
- 2026-11-19
AI Technical Summary
Existing manufacturing methods for high-carbon steel sheets used in mainsprings require patenting treatments, which involve environmental impact and reduce productivity, and do not adequately address inclusions that initiate cracks or fatigue failure.
A high-carbon cold-rolled and hot-rolled steel sheet composition with controlled microstructure and inclusion density, achieved through specific chemical elements and processing, eliminating the need for spheroidizing annealing and patenting treatments, while enhancing strength and fatigue resistance.
The solution provides high-strength steel sheets with improved fatigue durability and refined pearlite structure, reducing environmental impact and increasing productivity by omitting unnecessary heat treatments.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
High-carbon cold-rolled steel sheet, high-carbon hot-rolled steel sheet, and spiral spring
[0001] The present invention relates to a high-carbon cold-rolled steel sheet, a high-carbon hot-rolled steel sheet, and a spiral spring having a fine pearlite structure. This application claims priority based on Japanese Patent Application No. 2025-081862, filed in Japan on May 15, 2025, the contents of which are incorporated herein by reference.
[0002] Because high stresses are generated in mainspring products, high strength and fatigue resistance are required.
[0003] Patent Document 1 discloses a cold-rolled carbon steel having a composition of C 0.63-0.85%, Si up to 0.40%, Mn 0.20-0.90%, P up to 0.035%, S up to 0.035%, Al up to 0.060%, Cr up to 0.40%, and N 0.003-0.010%, preferably 0.005-0.008%, with a remainder consisting of at least one microalloying element (Ti, Nb, V, and Zr) with a maximum content of 0.12%.
[0004] Patent Document 2 discloses a method for manufacturing a high-carbon steel sheet, comprising the steps of: producing a steel sheet having a spheroidized cementite and initial ferrite structure by hot rolling, cold rolling, and annealing processes of a steel material with predetermined components; heating the steel sheet and then patenting the heated steel sheet, during which the patenting heat treatment is performed for 60 seconds or more while maintaining the temperature of the solder bath at 500°C or more and 530°C or less; and after the patenting heat treatment, a cooling step and a step of cold rolling to 85% or more, wherein the temperature range when heating the steel sheet before the patenting heat treatment is 800°C or more and 1100°C or less, the interlayer spacing between layered carbides is 0.5 μm or less, and the volume fraction of a fine pearlite phase having a lamellar structure with a long axis to short axis ratio of 10:1 or more is disclosed.
[0005] Special table 2012-518723 publication Special table 2010-528189 publication
[0006] Generally, the main manufacturing method for high-carbon hot-rolled steel sheets used for mainsprings involves a patenting treatment where the raw material is heated to over 900°C and then immersed in a lead bath before cold rolling. This heat treatment, called patenting, is essential before cold rolling. By omitting this heat treatment, CO 2 This is expected to reduce environmental impact through reduction and the elimination of Pb, as well as improve productivity through process streamlining. On the other hand, in order to omit heat treatment, it is necessary to refine the pearlite structure at the stage of hot-rolled steel sheet, which is an intermediate product.
[0007] It is believed that the refinement of the pearlite structure at the hot-rolled steel sheet stage can be achieved by lowering the winding temperature (CT) (increasing the degree of supercooling). On the other hand, lowering the winding temperature may cause problems such as the collapse of the coil shape or deterioration of the sheet shape due to the effects of expansion and heat generation associated with the transformation.
[0008] Furthermore, while the aforementioned Patent Document 1, which represents prior art, explores suppressing cracks that may form due to the notch effect of coarse materials by refining the microstructure through the addition of microalloying elements, it does not adequately address inclusions that serve as crack initiation points. In addition, the manufacturing method disclosed in Patent Document 1 requires patenting processes, including cold rolling, even after the hot rolling process.
[0009] Furthermore, while Patent Document 2 examines the morphology of pearlite from the perspective of suppressing fatigue crack propagation, it does not adequately address the inclusions that serve as the initiation points for crack formation. In addition, patenting processes including cold rolling are required even after the hot rolling process, resulting in a high number of manufacturing steps and challenges to productivity.
[0010] The present invention has been made in view of the above circumstances, and aims to provide high-carbon cold-rolled steel sheets, high-carbon hot-rolled steel sheets, and spiral springs that have high strength (torque characteristics) and high fatigue durability, even without spheroidizing annealing, primary cold rolling, and patenting treatment, by creating a pearlite structure at the hot rolling stage.
[0011] (1) The chemical composition, in mass%, is as follows: C: 0.70% to 0.90%, Si: 0.10% to 0.50%, Mn: 0.20% to 0.50%, Al: 0.003% to 0.015%, Cr: 0.10% to 0.50%, P: 0% to 0.020%, S: 0% to 0.0015%, O: 0% to 0.0030%, N: 0% to 0.0100%, Ti: 0% to 0.02%, Nb: 0% to 0.05%, V: 0% to 0.05%, Cu: 0% to 0.50%, Ni: 0% to 0.50%, B: 0% to 0.010%, Mo: 0% to 0.10%, W The composition is as follows: 0-0.05%, Ta: 0-0.05%, Ca: 0-0.0500%, Mg: 0-0.05%, Sn: 0-0.05%, Sb: 0-0.05%, As: 0-0.05%, REM: 0-0.0050%, and the remainder: Fe and impurities; the surface Vickers hardness is 530 Hv or higher; the area fraction of the pearlite structure is 95% or higher; and the lamellar spacing of the pearlite structure is... The particle size is 20 to 50 nm, the hardness ratio NC1 / NC2 (the ratio of the maximum hardness NC1 to the minimum hardness NC2 of the nanoindentation hardness in the thickness direction) is 2.0 or greater, and, when the thickness is tC, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions formed by the combination of two or more such individual inclusions, is 3.0 particles / mm² within a 1 / 4 tC plane. 2A high-carbon cold-rolled steel sheet characterized by the following: (2) Chemical composition in mass%, Ti: 0.001-0.02%, Nb: 0.001-0.05%, V: 0.001-0.05%, Cu: 0.001-0.50%, Ni: 0.001-0.50%, B: 0.001-0.010%, Mo: 0.001-0.10%, W (1) A high-carbon cold-rolled steel sheet according to (1), characterized in that it contains one or more of the following: 0.001 to 0.05%, Ta: 0.001 to 0.05%, Ca: 0.0001 to 0.050%, Mg: 0.0001 to 0.05%, Sn: 0.001 to 0.05%, Sb: 0.001 to 0.05%, As: 0.001 to 0.05%, REM: 0.0001 to 0.0050%. (3) A high-carbon cold-rolled steel sheet according to (1), characterized in that its chemical composition is, in mass%, Al: 0.003% to 0.010%, Cu: 0.001 to 0.05%, Ni: 0.001 to 0.05%, Mo: 0.001 to 0.05%. (4) In the 1 / 4 tC plane, the number density of coarse inclusions with an average particle size of 10.0 μm or more is 0.5 pieces / mm 2A high-carbon cold-rolled steel sheet according to any one of the characteristics (1) to (3), wherein the carbon content is less than (5) by mass%, and the chemical composition is: C: 0.70% to 0.90%, Si: 0.10% to 0.50%, Mn: 0.20% to 0.50%, Al: 0.003% to 0.015%, Cr: 0.10% to 0.50%, P: 0 to 0.020%, S: 0 to 0.0015%, O: 0 to 0.0030%, N: 0 to 0.0100%, Ti: 0 to 0.02%, Nb: 0 to 0.05%, V: 0 to 0.05%, Cu: 0 to 0.50%, Ni: 0 to 0.50%, B: 0 to 0.010%, Mo: 0 to 0.10%, W The composition is as follows: 0-0.05%, Ta: 0-0.05%, Ca: 0-0.0500%, Mg: 0-0.05%, Sn: 0-0.05%, Sb: 0-0.05%, As: 0-0.05%, REM: 0-0.0050%, and the remainder: Fe and impurities, the surface Vickers hardness is 320-400 Hv, the area fraction of the pearlite structure is 95% or more, and the pearlite structure is flat The uniform lamellar spacing is 80 to 200 nm, the hardness ratio V1 / V2 (the ratio of the maximum hardness V1 to the minimum hardness V2 in the thickness direction of the plate) is 1.10 or greater, and, when the plate thickness is tH, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions formed by the combination of two or more such individual inclusions, is 3.0 particles / mm² within the 1 / 4 tH plane. 2A high-carbon hot-rolled steel sheet characterized by the following: (6) Chemical composition in mass%, Ti: 0.001-0.02%, Nb: 0.001-0.05%, V: 0.001-0.05%, Cu: 0.001-0.50%, Ni: 0.001-0.50%, B: 0.001-0.010%, Mo: 0.001-0.10%, W (5) A high-carbon hot-rolled steel sheet according to (5), characterized in that it contains one or more of the following: 0.001 to 0.05%, Ta: 0.001 to 0.05%, Ca: 0.0001 to 0.050%, Mg: 0.0001 to 0.05%, Sn: 0.001 to 0.05%, Sb: 0.001 to 0.05%, As: 0.001 to 0.05%, REM: 0.0001 to 0.0050%. (7) A high-carbon hot-rolled steel sheet according to (5), characterized in that its chemical composition is, in mass%, Al: 0.003% to 0.010%, Cu: 0.001 to 0.05%, Ni: 0.001 to 0.05%, Mo: 0.001 to 0.05%. (8) In the 1 / 4 tH plane, the number density of coarse inclusions with an average particle size of 10.0 μm or more is 0.5 pieces / mm 2A high-carbon hot-rolled steel sheet according to any one of features (5) to (7), wherein the carbon content is less than (9) by mass%, and the chemical composition is: C: 0.70% to 0.90%, Si: 0.10% to 0.50%, Mn: 0.20% to 0.50%, Al: 0.003% to 0.015%, Cr: 0.10% to 0.50%, P: 0 to 0.020%, S: 0 to 0.0015%, O: 0 to 0.0030%, N: 0 to 0.0100%, Ti: 0 to 0.02%, Nb: 0 to 0.05%, V: 0 to 0.05%, Cu: 0 to 0.50%, Ni: 0 to 0.50%, B: 0 to 0.010%, Mo: 0 to 0.10%, W The composition is as follows: 0-0.05%, Ta: 0-0.05%, Ca: 0-0.0500%, Mg: 0-0.05%, Sn: 0-0.05%, Sb: 0-0.05%, As: 0-0.05%, REM: 0-0.0050%, and the remainder: Fe and impurities; the surface Vickers hardness is 530 Hv or higher; the area fraction of the pearlite structure is 95% or higher; and the lamellar spacing of the pearlite structure is... The nanoscale is 20 to 50 nm, the hardness ratio NB1 / NB2 (the ratio of the maximum hardness NB1 to the minimum hardness NB2 of the nanoindentation hardness in the thickness direction) is 2.0 or greater, and, when the thickness is tB, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions formed by the combination of two or more such individual inclusions, is 3.0 inclusions / mm² within a 1 / 4 tB plane. 2A spiral spring characterized by the following: (10) Chemical composition in mass%, Ti: 0.001-0.02%, Nb: 0.001-0.05%, V: 0.001-0.05%, Cu: 0.001-0.50%, Ni: 0.001-0.50%, B: 0.001-0.010%, Mo: 0.001-0.10%, W (9) A spiral spring characterized by containing one or more of the following: 0.001 to 0.05%, Ta: 0.001 to 0.05%, Ca: 0.0001 to 0.050%, Mg: 0.0001 to 0.05%, Sn: 0.001 to 0.05%, Sb: 0.001 to 0.05%, As: 0.001 to 0.05%, REM: 0.0001 to 0.0050%. (11) A spiral spring according to (9), characterized in that its chemical composition is, in mass%, Al: 0.003% to 0.010%, Cu: 0.001 to 0.05%, Ni: 0.001 to 0.05%, Mo: 0.001 to 0.05%. (12) A spiral spring according to any one of (9) to (11), characterized in that the Vickers hardness of the surface is 580 Hv or more. (13) In the 1 / 4tB surface, the number density of coarse inclusions with an average particle size of 10.0 μm or more is 0.5 pieces / mm 2 A spiral spring according to any one of (9) to (11), characterized in that it is less than [amount].
[0012] To provide high-carbon cold-rolled steel sheets, high-carbon hot-rolled steel sheets, and spiral springs that possess high strength (torque characteristics) and high fatigue durability, even without spheroidizing annealing, primary cold rolling, and patenting treatment, by creating a pearlite structure during the hot rolling process.
[0013] The following describes a high-carbon cold-rolled steel sheet (hereinafter also referred to as a cold-rolled steel sheet), a high-carbon hot-rolled steel sheet, and a spiral spring according to one embodiment of the present invention. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the invention. Furthermore, the numerical limit ranges described below, separated by "~", include both a lower limit and an upper limit. Numerical values indicated as "less than" or "greater than" do not include the numerical range.
[0014] <High-carbon cold-rolled steel sheet> The high-carbon cold-rolled steel sheet according to this embodiment has a predetermined chemical composition described later, the surface hardness of the steel sheet is 530 Hv or higher on a Vickers hardness scale, the area fraction of the pearlite structure is 95% or higher, the lamellar spacing of the pearlite structure is 20 to 50 nm, the hardness ratio NC1 / NC2 of the nanoindation hardness in the thickness direction, where the maximum hardness NC1 is 2.0 and the minimum hardness NC2 is 2.0 or higher, and when the thickness of the sheet is tC, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm or less, or composite inclusions formed by the combination of two or more individual inclusions, is 3.0 inclusions / mm² within a 1 / 4 tC plane. 2 The following applies. In this embodiment, "high carbon" means that the carbon content in the steel is 0.70% or more.
[0015] [Chemical Composition] The chemical composition of the high-carbon cold-rolled steel sheet according to this embodiment will be described below. In the following description, the unit of chemical composition will be "mass %".
[0016] C: 0.70-0.90% Carbon (C) is an element that contributes to increased strength by increasing the area fraction of the cementite phase and refining the lamellar spacing of the pearlite structure. If the C content is less than 0.70%, it becomes difficult to secure a sufficient pearlite structure as the main microstructure. For this reason, the C content is 0.71% or more. Preferably, the C content is 0.70% or more, more preferably 0.72% or more or 0.74% or more. On the other hand, if the C content exceeds 0.90%, protereminate cementite phase may precipitate. In this case, cold rolling becomes difficult and fatigue durability also decreases. For this reason, the C content is 0.90% or less. Preferably, the C content is 0.89% or less or 0.88% or less, more preferably 0.86% or less, 0.84% or less or 0.82% or less.
[0017] Si: 0.10-0.50% Silicon (Si) is an element included for deoxidation. If the Si content is less than 0.10%, deoxidation is insufficient, and oxidative inclusions remain. Therefore, when hot-rolled steel sheets are cold-rolled to an extremely thin state, cracks may form on the surface, causing a decrease in fatigue durability. For this reason, the Si content should be 0.10% or more. Preferably, the Si content should be 0.11% or more or 0.12% or more, more preferably 0.14% or more, 0.16% or more, or 0.18% or more. On the other hand, if the Si content exceeds 0.50%, it promotes the formation of substances that induce red scale when the slab is reheated for hot rolling. When these substances are formed, red scale may form on the surface of the resulting hot-rolled steel sheet, which may reduce the surface quality of the final cold-rolled steel sheet. For this reason, the Si content should be 0.50% or less. Preferably, the Si content is 0.45% or less or 0.40% or less, more preferably 0.35% or less or 0.30% or less.
[0018] Mn: 0.20-0.50% Manganese (Mn) is an effective element for improving the hardenability of steel and increasing its strength. If the Mn content is less than 0.20%, the hardenability of the steel may be insufficient, and sufficient strength may not be obtained. Therefore, the Mn content is 0.20% or more. Preferably, the Mn content is 0.25% or more, more preferably 0.30% or more. On the other hand, if the Mn content exceeds 0.50% by mass, the strength of the steel may increase excessively, leading to a decrease in toughness. Therefore, the Mn content is 0.50% or less. Preferably, the Mn content is 0.48% or less, more preferably 0.45% or less or 0.40% or less.
[0019] Al: 0.003 to 0.015% Aluminum (Al) is effective as a deoxidizer, but since Al oxides act as initiation points for fatigue cracks, it is preferable to keep the Al content as low as possible. Therefore, the Al content is 0.015% or less. Preferably, it is 0.010% or less, 0.009% or less, or 0.008% or less. More preferably, it is 0.070% or less or 0.06% or less. If an attempt is made to excessively reduce the Al content, the refining cost will increase significantly, so the Al content may be 0.003% or more. Preferably, it is 0.004% or more or 0.005% or more.
[0020] Cr: 0.10 to 0.50% Chromium (Cr) is an element that can improve the strength of the steel sheet, that is, the Vickers hardness of the steel sheet surface. If the Cr content is 0.05% or more, the desired Vickers hardness may be obtained, but if the Cr content is less than 0.10%, the performance may not be stable. Therefore, in order to sufficiently obtain such effects, the Cr content is 0.10% or more. Preferably, the Cr content is 0.11% or more, 0.15% or more, or 0.20% or more. On the other hand, if the Cr content exceeds 0.50%, the pearlite transformation will not be completed in the cooling step and will occur after coiling, which may make it impossible to obtain the desired Vickers hardness and microstructure. Therefore, the Cr content is 0.50% or less. Preferably, the Cr content is 0.40% or less, more preferably 0.30% or less or 0.25% or less.
[0021] P: 0.020% or less Phosphorus (P) is an impurity element. P embrittles grain boundaries and reduces cold rollability. Therefore, the P content is 0.020% or less. The P content is preferably as low as possible, preferably 0.018% or less, more preferably 0.015% or less or 0.012% or less. However, if an attempt is made to excessively reduce the P content, the refining cost will increase significantly, so the P content may be 0.0010% or more. The lower limit of the P content is 0%, but in order to reduce the refining cost, the lower limit of the P content may be set to 0.001%, 0.003%, or 0.005%.
[0022] S: 0.0015% or less. Sulfur (S) is an impurity element. S causes the formation of nonmetallic inclusions such as MnS. Such nonmetallic inclusions can become the starting point for crack initiation and fracture during cold rolling, which can lead to a decrease in fatigue durability. Therefore, the S content is 0.0015% or less. It is preferable that the S content be as low as possible, preferably 0.0012% or less or 0.0010% or less. The lower limit of the S content is 0%. Since excessively reducing the S content significantly increases refining costs, the S content may be 0.0001% or more, 0.0003% or more, 0.0005% or more, or 0.0008% or more.
[0023] O: 0.0030% or less. Oxygen (O) forms oxides in steel. If oxides aggregate and coarseen in steel, or if the number density of oxides increases, it may reduce cold rolling properties and the fatigue durability of the final product, the spiral spring. Therefore, the O content is 0.0030% or less. Preferably, the O content is 0.0025% or less, more preferably 0.0020% or less. A lower O content is preferable, with a lower limit of 0%. On the other hand, it is practically difficult to reduce the O content excessively. Therefore, the O content may be 0.0001% or more. In this embodiment, an O content within the range of 0.0001% to 0.0040% is acceptable.
[0024] N: 0.0100% or less. Nitrogen (N) combines with Al in the steel to form AlN. AlN inhibits the coarsening of the pearlite block diameter through a pinning effect, thereby improving cold rolling properties. The lower limit of N content is 0%, but to obtain such effects, the N content may be 0.0020% or more. However, if the N content is excessively high, the effect will saturate, and cold rolling properties may decrease. Therefore, the N content is 0.0100% or less. Preferably, the N content is 0.0080% or less, more preferably 0.0070% or less, and even more preferably 0.0060% or less.
[0025] The cold-rolled steel sheet according to the present embodiment contains the above elements, with the balance being Fe and impurities. Here, the impurities refer to elements that are mixed in due to various factors in raw materials such as ores and scraps, and manufacturing processes when steel is industrially produced, and are elements whose presence is permitted within a range that does not impair the properties of the cold-rolled steel sheet according to the present embodiment.
[0026] In addition to the above elements, the cold-rolled steel sheet according to the present embodiment may contain one or more of Ti, Nb, V, Cu, Ni, B, Mo, W, Ta, Ca, Mg, Sn, Sb, As, and REM. By containing these optional elements, more preferable properties can be obtained for the cold-rolled steel sheet according to the present embodiment. However, even if the cold-rolled steel sheet does not contain these optional components, the desired properties of the cold-rolled steel sheet according to the present embodiment can still be obtained, so the lower limit of these optional elements is 0%. Hereinafter, details of these optional elements will be described.
[0027] Ti: 0 to 0.02% Titanium (Ti) has the effect of increasing strength by forming carbonitrides, so it may be contained in a range of 0.02% or less as necessary. If the Ti content exceeds 0.02%, coarse angular carbonitrides are likely to form, and deterioration of workability becomes apparent. Therefore, the Ti content is 0.02% or less. The lower limit of the Ti content may be 0.001% or more, or 0.003% or more.
[0028] Nb: 0 to 0.05% Niobium (Nb) has the effect of increasing strength by forming carbonitrides, so it may be contained in a range of 0.05% or less as necessary. If the Nb content exceeds 0.05%, coarse angular carbonitrides are likely to form and deterioration of workability becomes apparent, so the Nb content is preferably 0.02% or less. The lower limit of the Nb content may be 0.001% or more, or 0.003% or more.
[0029] V: 0-0.05% Vanadium (V) has the effect of increasing strength by forming carbonitrides, so it may be included in a range of 0.05% or less as needed. If the V content exceeds 0.05%, coarse, angular carbonitrides are more likely to form, and a deterioration in workability becomes apparent, so the V content should be 0.02% or less. The lower limit of the V content may be 0.001% or more, or 0.003% or more.
[0030] Cu: 0-0.50% Copper (Cu) has the effect of improving the strength (hardness) of steel sheets. Therefore, Cu may be included in a range of 0.50% or less as needed. If the Cu content exceeds 0.50%, there is a risk of hot working cracks occurring during hot rolling due to molten metal embrittlement (Cu embrittlement), so a Cu content of 0.50% or less is preferable. The Cu content may be 0.30% or less, 0.10% or less, or 0.05% or less. The lower limit of the Cu content may be 0.001% or more, or 0.003% or more.
[0031] Ni: 0-0.50% Nickel (Ni) has the effect of preventing molten metal embrittlement (Cu embrittlement) when Cu is included. Therefore, Ni may be included in a range of 0.50% or less as needed. If the Ni content exceeds 0.50%, the cost increases while the above effect saturates, so a Ni content of 0.50% or less is preferable. The Ni content may be 0.30% or less, 0.10% or less, or 0.05% or less. The lower limit of the Ni content may be 0.001% or more, or 0.003% or more.
[0032] B: 0-0.010% Boron (B) has the effect of improving hardenability and thus increasing the strength of the steel sheet. Therefore, if necessary, B may be included in a range of 0.010% or less. If the B content exceeds 0.010%, B-based compounds are formed and the workability of the steel sheet decreases, so a B content of 0.010% or less is preferable. The B content may be 0.03% or less or 0.01% or less, or 0.005% or less or 0.003% or less. The lower limit of the B content may be 0.0001% or more or 0.0003% or more.
[0033] Mo: 0-0.10% Molybdenum (Mo) has the effect of increasing the strength of steel sheets by forming carbonitrides. Therefore, if necessary, Mo may be included in a range of 0.10% or less. If the Mo content exceeds 0.10%, coarse carbonitrides are more likely to be formed, and a deterioration in workability becomes apparent, so a Mo content of 0.10% or less is preferable. The Mo content may be 0.05% or less, 0.03% or less, or 0.01% or less. The lower limit of the Mo content may be 0.001% or more, or 0.003% or more.
[0034] W: 0-0.05% Tungsten (W) has the effect of increasing the strength of steel sheets by forming carbonitrides. Therefore, W may be included in a range of 0.05% or less as needed. On the other hand, if the W content exceeds 0.05%, coarse carbonitrides are more likely to be formed, and a deterioration in workability becomes apparent, so a W content of 0.05% or less is preferable. The W content may be 0.03% or less or 0.01% or less. The lower limit of the W content may be 0.001% or more or 0.003% or more.
[0035] Ta: 0.05% or less. Tantalum (Ta) has the effect of increasing the strength of steel sheets by forming carbonitrides, so it may be included in a range of 0.050% or less as needed. If the Ta content exceeds 0.050%, coarse carbonitrides are more likely to be formed, and the deterioration of workability becomes apparent, so a Ta content of 0.050% or less is preferable. The Ta content may be 0.03% or less or 0.01% or less. The lower limit of the Ta content may be 0.001% or more or 0.003% or more.
[0036] Ca: 0-0.0500% Calcium (Ca) is an effective element for controlling the morphology of sulfides. Specifically, Ca has the effect of reducing coarse and elongated inclusions. Therefore, Ca may be included in a range of 0.0500% or less as needed. If the Ca content exceeds 0.0500%, the effect of controlling the morphology of sulfides becomes saturated, and fatigue durability may decrease due to aggregation or coarsening of the sulfides. Therefore, the Ca content is 0.0500% or less. More preferably, the Ca content is 0.0100% or less, more preferably 0.0080% or less or 0.0050% or less. The Ca content may also be 0.0030% or less, 0.0010% or less or 0.0005% or less. The lower limit of the Ca content may be 0.0001% or more or 0.0003% or more.
[0037] Mg: 0-0.05% Magnesium (Mg) is an element that can control the form of sulfides and also contributes to fatigue durability. To fully obtain the above effects, it is preferable that the Mg content be 0.0001% or more. On the other hand, if the Mg content exceeds 0.05%, it may lead to embrittlement of the steel plate and a decrease in ductility. Therefore, the Mg content is 0.05% or less. The Mg content may also be 0.03% or less, 0.001% or less, or 0.005% or less. The lower limit of the Mo content may be 0.0001% or more, or 0.0003% or more.
[0038] Sn: 0-0.05% Tin (Sn) is an element that is present when scrap is used as a raw material for steel and strongly segregates at grain boundaries. Therefore, a lower Sn content is preferable, and it may be 0%. If the Sn content exceeds 0.05%, it may lead to embrittlement of the steel sheet and a decrease in ductility. Therefore, the Sn content is 0.05% or less. The Sn content may be 0.03% or less or 0.01% or less. The lower limit of the Sn content may be 0.001% or more or 0.003% or more.
[0039] Sb: 0-0.05% Antimony (Sb), like Sn, is present when scrap is used as a steel raw material and is an element that strongly segregates at grain boundaries. Therefore, a lower Sb content is preferable, and it may be 0%. If the Sb content exceeds 0.05%, it may lead to embrittlement of the steel sheet and a decrease in ductility. Therefore, the Sb content is 0.05% or less. The Sb content may be 0.03% or less or 0.01% or less. The lower limit of the Sb content may be 0.001% or more or 0.003% or more.
[0040] As: 0-0.05% Arsenic (As), like Sn, is present when scrap is used as a raw material for steel, and is an element that strongly segregates at grain boundaries. Therefore, a lower As content is preferable, and it may be 0%. If the As content exceeds 0.05%, it may lead to embrittlement of the steel sheet and a decrease in ductility. Therefore, the As content is 0.05% or less. The As content may be 0.03% or less or 0.01% or less. The lower limit of the As content may be 0.001% or more or 0.003% or more.
[0041] REM: 0 to 0.0050% or less. REM is an effective element for reducing MnS, controlling the morphology of inclusions, and improving the workability of steel sheets. To obtain the above effects, the REM content is preferably 0.0001% or more. The REM content is more preferably 0.0003% or more, or 0.0005% or more. On the other hand, if the REM content exceeds 0.0050%, nozzle clogging is more likely to occur during continuous casting. Also, if the REM content exceeds 0.0050%, the number density of the generated REM-based inclusions (oxides and oxysulfides) becomes relatively high, so these REM-based inclusions accumulate on the underside of the curved slab during continuous casting. This can cause internal defects in the steel sheet obtained by rolling the slab, and may further worsen the workability of the steel sheet. Therefore, it is preferable to keep the REM content at 0.0050% or less. The REM content may be 0.0035% or less, 0.0020% or less, or 0.0010% or less.
[0042] REM (Rare Earth Metal) refers to rare earth elements and is a collective term for 17 elements including scandium (Sc, atomic number 21), yttrium (Y, atomic number 39), and lanthanides (15 elements from lanthanum (atomic number 57) to lutesium (atomic number 71)). The cold-rolled steel sheet according to this embodiment contains at least one element selected from these. As a method of inclusion, for example, these elements are often included in the steel as a mischmetal, which is a mixture of these elements. The main components of mischmetal are Ce, La, Nd, and Pr. In this embodiment, the total amount of these rare earth elements contained in the cold-rolled steel sheet is defined as the REM content.
[0043] The cold-rolled steel sheet according to this embodiment contains the above-mentioned elements, with the remainder being Fe and impurities. Here, impurities are elements that are mixed in during the industrial production of steel due to various factors in the raw materials such as ore and scrap, and in the manufacturing process, and are elements whose presence is permissible as long as they do not impair the properties of the cold-rolled steel sheet according to this embodiment.
[0044] The chemical composition described above can be measured using general analytical methods. For example, it can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). C and S can be measured using the combustion-infrared absorption method, and N can be measured using the inert gas fusion-thermal conductivity method. If ladle analysis values or analysis values from the slab are available during the slab manufacturing of cold-rolled steel sheets, the measurement of the chemical composition of the cold-rolled steel sheet may be omitted, and those ladle analysis values may be used instead. Ladle analysis values may also be used for the chemical composition of hot-rolled steel sheets or spiral springs, as described later.
[0045] [Microstructure] Next, the microstructure (metal structure) of the high-carbon cold-rolled steel sheet according to this embodiment will be described.
[0046] (Area fraction of pearlite structure: 95% or more) The pearlite structure has a higher work hardening ability compared to the ferrite phase and bainite structure, making it an effective structure for obtaining high strength (torque characteristics) and excellent fatigue durability. If structures other than pearlite, such as the ferrite phase and bainite structure, are present in more than 5% area fraction, the strength will decrease. Also, when cold-rolled steel sheets are subjected to strong processing, differences in hardness (strength) occur between the microstructures, and these hardness differences can become the starting point for crack initiation, resulting in a decrease in fatigue durability. For the above reasons, it is effective to set the area fraction of the pearlite structure to 95% or more in order to obtain torque characteristics and fatigue durability. Preferably, the area fraction of the pearlite structure is 96% or more or 98% or more. The area fraction of the pearlite structure may be 100%. The structures other than pearlite (the remaining structure) may include one or more of ferrite, bainite, or martensite.
[0047] Furthermore, the area ratio of each microstructure is measured by the following method. In addition, the area ratio of each microstructure is measured by the following method in parts (such as spiral springs) using hot-rolled and cold-rolled steel sheets described later. A test piece is taken so that the thickness cross-section of the cold-rolled steel sheet can be observed. In this case, it is preferable to take the test piece from a position 1 / 4 of the way down the width direction of the cold-rolled steel sheet. After revealing the microstructure by nital etching of the observation surface, a micrograph is taken using a scanning electron microscope at a magnification of 5000x, with the field of view centered at a position 1 / 4 of the thickness from the surface of the steel sheet, covering 20 μm in the thickness direction and 30 μm in the direction perpendicular to the thickness and parallel to the rolling direction. Micrographs are taken for 5 fields of view. In each micrograph, the region exhibiting a lamellar structure is identified as pearlite, and the area ratio of pearlite is obtained by calculating the average of their area ratios.
[0048] Furthermore, the rolling direction of cold-rolled steel sheets is determined by the following method: A test piece is taken from the cold-rolled steel sheet so that the thickness cross-section can be observed. After finishing the thickness cross-section of the taken test piece with mirror polishing, it is observed using an optical microscope at magnifications of 100x, 200x, 500x, and 1000x. Depending on the size of the inclusion, the observation result at an appropriate magnification that allows the inclusion dimensions to be measured is selected. The observation range is 500 μm or wider and covers the entire thickness of the sheet, and areas with dark brightness are determined to be inclusions. Multiple fields of view may be used for observation. Next, using the thickness cross-section initially observed using the method described above as a reference, the sheet is rotated in 5° increments within the range of 0° to 180° around the thickness axis, and the surfaces parallel to these rotated surfaces are observed in the same way as described above. The average length of the major axes of multiple inclusions in each cross-section is calculated for each cross-section. The cross-section that yields the highest average length of the major axes of the obtained inclusions is identified. The direction parallel to the long axis of the inclusion in the cross-section is determined as the rolling direction. The rolling direction is determined in the same way as above for parts made from hot-rolled and cold-rolled steel sheets (such as spiral springs). However, if the rolling direction can be determined in advance (for example, when taking a test piece from a steel strip), this determination of the rolling direction is unnecessary and can be omitted.
[0049] (Lamellar spacing of pearlite structure: 20-50 nm) If the lamellar spacing of the pearlite structure is less than 20 nm, the cold workability during molding may decrease. For this reason, the lamellar spacing of the pearlite structure is 20 nm or more. Preferably, the lamellar spacing of the pearlite structure is 22 nm or more, 25 nm or more, 27 nm or more, or 30 nm or more. On the other hand, if the lamellar spacing of the pearlite structure is greater than 50 nm, the desired strength (torque characteristics) may not be obtained. For this reason, the lamellar spacing of the pearlite structure is 50 nm or less. Preferably, the lamellar spacing of the pearlite structure is 48 nm or less, 45 nm or less, 42 nm or less, 40 nm or less, or 37 nm or less.
[0050] Here, the lamellar spacing of the pearlite structure means the average distance between the center points in the thickness direction of each of the adjacent ferrite phase and cementite phase constituting the lamellae. The lamellar spacing may be determined, for example, by regarding one layer of the ferrite phase and one layer of the cementite phase as one set of layers, and measuring how many sets of layers are intersected by a line segment of a predetermined length in the direction perpendicular to the extending direction of the layers in the structure observation. Note that layers that are not completely intersected by the line segment at both ends of the line segment are excluded from the measurement targets.
[0051] Specifically, in the present embodiment, the lamellar spacing of the pearlite structure is determined as follows. First, a sample is taken from a position 1 / 4 of the sheet thickness away from the surface of the steel sheet such that a cross section parallel to the rolling direction and the thickness direction of the steel sheet serves as the observation surface. Subsequently, the observation surface is mirror-polished, etched with a picral etchant, and then subjected to structure observation using a scanning electron microscope (SEM). The magnification is set to 5000 times (measurement area: 80 μm × 150 μm), and 10 locations where the cementite layer crosses perpendicularly to the paper surface of the structure photograph are selected. By performing the measurement after etching with the picral etchant, information in the depth direction can be obtained, so that the locations crossing the cementite layer perpendicularly can be identified. By selecting 10 or more such locations and performing measurement, the lamellar spacing S is determined at each location, and the average thereof is taken as the "lamellar spacing". The measurement method of the lamellar spacing at each location is as follows. First, a straight line is drawn perpendicular to the cementite layers so as to cross 10 to 30 cementite layers, and the length of the straight line (line segment length) is defined as L. Further, the number of sets of layers, each consisting of one ferrite phase layer and one cementite phase layer, intersected by the straight line is defined as N. At this time, the lamellar spacing S at the relevant location is determined by S = L / (N × 2). Note that the lamellar spacing of the pearlite structure can also be measured by the above method for parts (such as spiral springs) using the hot-rolled steel sheet and cold-rolled steel sheet described later.
[0052] (Number density of inclusions in the 1 / 4t C plane: 3.0 pieces / mm 2 or less) In the cold-rolled steel sheet, the number density of inclusions having an average particle size of 1.0 to 10.0 μm (1.0 μm or more and 10.0 μm or less) is 3.0 pieces / mm 2In extreme cases, inclusions can act as a starting point for premature fracture, potentially preventing the achievement of high fatigue durability. Therefore, the number density of inclusions in cold-rolled steel sheets should be kept at 3.0 inclusions / mm². 2 The following is specified. This results in high fatigue durability. Preferably, the number density of inclusions is 2.5 pieces / mm³. 2 Below, 2.0 pieces / mm 2 The following or 1.5 pieces / mm 2 The following is the case: A lower number density of inclusions is preferable, so the lower limit is 0 inclusions / mm³. 2 Inclusions with an average particle size of less than 1.0 μm do not affect fatigue durability and are therefore not counted as inclusions as defined in this embodiment. Furthermore, coarse inclusions with an average particle size exceeding 10.0 μm can serve as fracture initiation points. In other words, coarse inclusions with an average particle size exceeding 10.0 μm will fracture prematurely regardless of their number, preventing the desired fatigue durability from being achieved. Therefore, in this embodiment, the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0 inclusions / mm². 2 It is preferable that the number density of coarse inclusions with an average particle size exceeding 10.0 μm, as obtained by the method for calculating the number density of inclusions described later, is 0.5 inclusions / mm³. 2 If the value is less than 10.0 μm, the number density of coarse inclusions with an average particle size greater than 10.0 μm is 0 particles / mm³. 2 We conclude that the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0.4 pieces / mm³. 2 Below, 0.3 pieces / mm 2 Less than or equal to 0.2 pieces / mm 2 The following is also acceptable.
[0053] In this embodiment, "inclusions" refers to individual inclusions of oxides, sulfides, and nitrides, as well as composite inclusions formed by the combination of two or more such individual inclusions.
[0054] The number density of inclusions in cold-rolled steel sheets is calculated by the following method. First, five samples are taken from each cold-rolled steel sheet. The collected test pieces are embedded in resin. The resin-embedded test pieces are polished in the thickness direction, and when the thickness is t, the surface is mirror-polished so that the 1 / 4t surface (a surface parallel to the surface of the cold-rolled steel sheet, located 1 / 4 of the thickness away from the surface of the cold-rolled steel sheet) becomes the surface. The observation area within the polished surface is observed using a scanning electron microscope (SEM) equipped with a compositional analysis function. The observation area is 1.2 mm × 1.6 mm. The longer side of the observation area corresponds to the rolling direction of the cold-rolled steel sheet. During observation, 48 non-overlapping fields of view of 200 μm × 200 μm are selected, and each field of view is observed at a magnification of 500x.
[0055] In the observation area, particles (precipitates or inclusions) with an equivalent circle diameter of 1.0 μm or more are identified based on the Z contrast of the backscattered electron image. In the backscattered electron image, particles are shown with a darker contrast compared to the matrix. The equivalent circle diameter refers to the diameter of a circle when the area of the particle is converted to a circle of the same area. For each identified particle, elemental concentration analysis is performed using energy-dispersive X-ray spectroscopy (EDX). The standardless method is used for EDX analysis (elemental concentration analysis). The acceleration voltage is set to 20 kV, and the elements to be quantified are Si, Mn, P, S, Cr, Ti, Nb, Cu, Ni, Ca, N, O, Al, and Mg.
[0056] In the EDX analysis results of each particle, when the total mass percentage content of the above-mentioned quantitative elements is set to 100%, particles in which the sum of O content, S content, and N content is 10% or more by mass percentage are identified as individual oxide, sulfide, and nitride inclusions, and composite inclusions, respectively.
[0057] Based on the total number of individual and composite inclusions of oxides, sulfides, and nitrides with an equivalent circular diameter of 1.0 μm or more, identified in each observation area of the five test specimens, and the total area of each observation area in the five test specimens, the number density (pieces / mm³) of individual and composite inclusions of oxides, sulfides, and nitrides with an equivalent circular diameter of 1.0 μm or more was calculated. 2The number density of inclusions can also be measured using the above method for parts (such as spiral springs) made from hot-rolled and cold-rolled steel sheets, as described later.
[0058] (Vickers hardness: 530 Hv or higher) In the cold-rolled steel sheet of this embodiment, the Vickers hardness of the steel sheet surface is 530 Hv or higher. This makes it possible to obtain excellent torque characteristics. The Vickers hardness of the steel sheet surface is preferably 535 Hv or higher, 540 Hv or higher, or 550 Hv or higher. There is no need to set an upper limit for the Vickers hardness, but for example, it may be 700 Hv or less, 670 Hv or less, 650 Hv or less, or 620 Hv or less.
[0059] Vickers hardness is measured in accordance with JIS Z2244:2024, with a test force of 9.807 N. The measurement point is preferably at least 50 mm away from the edge of the cold-rolled steel sheet. The Vickers hardness is obtained by measuring the hardness at five arbitrary points and calculating the average value of the obtained measurements.
[0060] Furthermore, the Vickers hardness can also be measured using the above method for parts (such as spiral springs) made from hot-rolled and cold-rolled steel sheets, as described later. However, if the measurement point cannot be located at least 50 mm away from the edge, the Vickers hardness should, in principle, be measured at the center of the width. The thickness of the cold-rolled steel sheet is not particularly limited, but may be, for example, 0.100 to 0.400 mm. The preferred lower limit for the thickness of the cold-rolled steel sheet is 0.140 mm, 0.160 mm, or 0.180 mm, and the preferred upper limit is 0.350 mm, 0.300 mm, 0.250 mm, or 0.230 mm.
[0061] (Hardness ratio of maximum hardness NC1 to minimum hardness NC2 of nanoindentation hardness in the thickness direction: 2.0 or more) In the cold-rolled steel sheet of this embodiment, the hardness ratio of maximum hardness NC1 to minimum hardness NC2 of nanoindentation hardness in the thickness direction is 2.0 or more. Nanoindentation hardness is derived from the lamellar spacing of pearlite. That is, a hardness ratio of maximum hardness NC1 to minimum hardness NC2 of nanoindentation hardness in the thickness direction of the sheet is 2.0 or more, which indicates that there is variation in the lamellar spacing of pearlite in the thickness direction. If the lamellar spacing of pearlite is constant in the thickness direction, cracks that occur on the surface of the cold-rolled steel sheet, for example, may propagate in the thickness direction. On the other hand, if there is variation in the lamellar spacing of pearlite in the thickness direction, as in the cold-rolled steel sheet of this embodiment, the propagation of cracks in the thickness direction can be suppressed. In this embodiment, a cold-rolled steel sheet having a hardness ratio of 2.0 or higher between the maximum hardness NC1 and the minimum hardness NC2 of nanoindentation hardness in the thickness direction can be obtained with excellent durability. The hardness ratio of 2.1 or higher between the maximum hardness NC1 and the minimum hardness NC2 of nanoindentation hardness in the thickness direction may be 2.1 or higher or 2.2 or higher. There is no need to specifically define an upper limit, but it may be 2.8 or lower, 2.6 or lower, 2.5 or lower, or 2.4 or lower.
[0062] The hardness ratio of nanoindentation hardness can be calculated by the following method. Nanoindentation hardness is measured in accordance with JIS Z2255:2003. JIS Z2255:2003 is a standard that defines the measurement method for "ultra-micro load hardness". In general, it is more often called "nanoindentation hardness" rather than "ultra-micro load hardness". For this reason, in this embodiment, it is called "nanoindentation hardness". The specific measurement method is as follows. The cross section parallel to the rolling direction (L cross section) was polished so that it would be the observation surface. The observation surface was mirror polished using diamond paste, and then finished polished using colloidal silica. Nanoindentation hardness was measured from the front to the back of the observation surface using a nanoindentation device equipped with a Berkovich indenter, covering the entire thickness at intervals of 3 to 5 μm in the thickness direction, and HTL0.5 was measured. This was done at three or more locations, and at least 100 measurement points were secured for evaluation. If the number of measurement points is less than 100, the total thickness measurement will be continued until the number of measurement points exceeds 100. Even if the number of measurement points exceeds 100 during the total thickness measurement, the measurement will continue until all measurement points for that total thickness are completed. The measurement conditions are a loading rate and unloading rate of 50 μN / s, a maximum load of 500 μN, and a holding time of 10 seconds. Among the obtained measured values (HTL 0.5), the maximum and minimum values are determined, and the value obtained by dividing the maximum value by the minimum value is calculated as the hardness ratio of the nanoindentation hardness.
[0063] <High-carbon hot-rolled steel sheet> Next, the high-carbon hot-rolled steel sheet according to this embodiment will be described. The high-carbon hot-rolled steel sheet according to this embodiment (hereinafter also referred to as the hot-rolled steel sheet) has a predetermined chemical composition, the Vickers hardness of the surface of the hot-rolled steel sheet is 320 Hv or more and 400 HV or less, and when the thickness of the hot-rolled steel sheet is tH, in the microstructure in the 1 / 4 tH region, which is the region from 1 / 8 tH to 3 / 8 tH of the thickness from the surface of the hot-rolled steel sheet, the area fraction of the pearlite structure is 95% or more, and The average lamellar spacing of the structure is 80 nm or more and 200 nm or less; the hardness ratio V1 / V2 of the Vickers hardness in the thickness direction of the hot-rolled steel sheet, where the maximum hardness V1 is 1.10 or more; and the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 μm or more and 10.0 μm or less, or composite inclusions formed by the combination of two or more of the above individual inclusions, is 3.0 inclusions / mm². 2 The following applies. The thickness of the hot-rolled steel sheet is not particularly limited, but may be, for example, 1.60 to 4.80 mm. The preferred lower limit for the thickness of the hot-rolled steel sheet is 2.00 mm or 2.20 mm, and the preferred upper limit is 4.00 mm or 3.80 mm.
[0064] [Chemical Composition] The hot-rolled steel sheet of this embodiment is the same hot-rolled steel sheet used for the high-carbon cold-rolled steel sheet of this embodiment described above. Therefore, the chemical composition of the hot-rolled steel sheet is the same as the chemical composition of the cold-rolled steel sheet described above.
[0065] [Microstructure] Next, the microstructure (metal structure) of the hot-rolled steel sheet will be described. In this embodiment, the hot-rolled steel sheet has a microstructure in which 95% or more of the area is pearlite, and the average lamellar spacing of the pearlite structure is 80 to 200 nm (80 nm or more, and 200 nm or less).
[0066] (Area fraction of pearlite structure: 95% or more) Having pearlite structure as the main structure means that the area fraction of pearlite structure to the total structure is 95% or more. Preferably, it is 96% or more or 98% or more. If the area fraction of pearlite structure is less than 95%, the desired hardness cannot be obtained, and if structures other than pearlite structure (bainite, ferrite, martensite) are included in an area fraction of more than 5%, these structures become points of strain concentration, causing fracture initiation and reducing cold rolling performance. Also, if the area fraction of pearlite structure is less than 95%, the fatigue durability of the final product, the spiral spring, may decrease. The area fraction of pearlite structure may be 100%. Structures other than pearlite (remaining structure) may include one or more of ferrite, bainite, or martensite. The method for measuring the microstructure and number density of inclusions, etc., of hot-rolled steel sheets is the same as the method for measuring cold-rolled steel sheets.
[0067] (Lamelar spacing of pearlite structure: 80-200 nm) From the viewpoint of exhibiting the high work hardening ability of the pearlite structure in cold-rolled steel sheets, the initial lamellar spacing before cold rolling, that is, the lamellar spacing in hot-rolled steel sheets, is important. If the average lamellar spacing of the pearlite structure in hot-rolled steel sheets exceeds 200 nm, it may be difficult to sufficiently increase the hardness of the resulting cold-rolled steel sheet even if the hot-rolled steel sheet is subjected to cold rolling at a high cold rolling rate. For this reason, the average lamellar spacing of the pearlite structure in hot-rolled steel sheets is 200 nm or less. Preferably it is 170 nm or less, or 150 nm or less, and more preferably 130 nm or less, or 120 nm or less. On the other hand, if the initial lamellar spacing before cold rolling is less than 80 nm, the strength may increase significantly due to cold rolling at a high cold rolling rate, and good cold rollability may not be ensured. Therefore, the average lamellar spacing of the pearlite structure in hot-rolled steel sheets is 80 nm or more. Preferably, it is 85 nm or more, 90 nm or more, or 100 nm or more. The lamellar spacing can be adjusted by adjusting the cooling rate from the austenite phase and the winding temperature, as described later, in addition to adjusting the chemical composition mentioned above.
[0068] (Number density of inclusions in the 1 / 4 tH plane: 3.0 inclusions / mm²)2 (See below) The average particle size is 1.0 to 10.0 μm (1.0 μm or larger, 10.0 μm or smaller), and the number density of inclusions is 3.0 particles / mm³. 2 High durability can be achieved with the following: 3.0 pieces / mm 2 In ultra-high performance materials, inclusions act as triggers for premature fracture, preventing high fatigue durability from being achieved. Therefore, the number density of inclusions should be 3.0 inclusions / mm². 2 High durability can be achieved by following the guidelines below. Preferably, 2.5 pieces / mm 2 Below, 2.0 pieces / mm 2 The following or 1.5 pieces / mm 2 The following applies: Coarse inclusions with an average particle size exceeding 10.0 μm can serve as fracture initiation points. Therefore, in this embodiment, the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0 inclusions / mm². 2 It is preferable that the number density of coarse inclusions with an average particle size exceeding 10.0 μm be 0.5 pieces / mm³. 2 If the value is less than 10.0 μm, the number density of coarse inclusions with an average particle size greater than 10.0 μm is 0 particles / mm³. 2 We conclude that the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0.4 pieces / mm³. 2 Below, 0.3 pieces / mm 2 Less than or equal to 0.2 pieces / mm 2 The following is also acceptable.
[0069] (Vickers hardness: 320-400 Hv) In the hot-rolled steel sheet of this embodiment, the surface Vickers hardness is 320 HV or higher. By increasing the hardness of the hot-rolled steel sheet, the strength of the cold-rolled steel sheet and the final product (spiral spring) after cold rolling can be sufficiently increased. If necessary, the surface Vickers hardness may be 330 HV or higher, 340 Hv or higher, or 350 Hv or higher. If the surface Vickers hardness is 400 Hv or higher, there is a possibility of sheet fracture during cold rolling, so it should be 400 Hv or lower. The Vickers hardness may also be 390 Hv or lower, 380 Hv or lower, or 370 Hv or lower.
[0070] The method for measuring Vickers hardness in hot-rolled steel sheets is the same as the method for measuring it in cold-rolled steel sheets described above.
[0071] (Vickers hardness ratio: 1.10 or higher) In the hot-rolled steel sheet of this embodiment, the hardness ratio V1 / V2 of the maximum hardness V1 to the minimum hardness V2 of the Vickers hardness in the thickness direction is 1.10 or higher. This makes it possible to obtain excellent durability by cold-rolling the hot-rolled steel sheet of this embodiment. The Vickers hardness ratio V1 / V2 may be 1.13 or higher, 1.15 or higher, 1.17 or higher, or 1.18 or higher. There is no need to specifically set an upper limit for the Vickers hardness ratio V1 / V2, but it may be 1.30 or lower, 1.28 or lower, 1.26 or lower, or 1.24 or lower. The Vickers hardness ratio V1 / V2 can be calculated by the following method.
[0072] The sample was polished so that the cross-section parallel to the rolling direction and in the thickness direction (L-section) would serve as the observation surface. The observation surface was mirror-polished using diamond paste, and then finished polished using colloidal silica. The Vickers hardness was measured at intervals of 100 to 200 μm from the front to the back of the observation surface. This was done at five or more locations, ensuring at least 100 measurement points for evaluation. If the number of measurement points was less than 100, the total thickness measurement was continued until the number of measurement points exceeded 100. Even if the number of measurement points exceeded 100 during the total thickness measurement, the measurement was continued until all measurements of the total thickness were completed. The Vickers hardness measurement was performed in accordance with JIS Z2244:2024, with a test force of 0.9807 N. From the obtained measurement points, the maximum value V1 and minimum value V2 were determined, and the value V1 / V2 obtained by dividing the maximum value V1 by the minimum value V2 was calculated as the Vickers hardness ratio.
[0073] <Spiral Spring> The spiral spring according to this embodiment is obtained by forming the cold-rolled steel sheet of this embodiment described above into a spring shape. Specifically, after primary winding, the spiral spring is manufactured by secondary winding in the opposite direction to the primary winding. That is, the area fraction of the pearlite structure is 95% or more, the lamellar spacing of the pearlite structure is 20 to 50 nm, and the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions of two or more individual inclusions, within the plane of the 1 / 4 t thickness of the sheet is 3.0 inclusions / mm². 2The hardness of the spring surface is 530 Hv or higher. Here, the "spiral spring" in this embodiment refers to "number 3400 spiral spring" as defined in JIS B 0103:2015, which is a spring that has a spiral shape in a plane.
[0074] In this embodiment, when the plate thickness of the spiral spring is tB, the area fraction of the pearlite structure in the 1 / 4 tB region is 95% or more, the lamellar spacing of the pearlite structure is 20 nm or more and 50 nm or less, the hardness ratio NB1 / NB2 of the nanoindentation hardness in the plate thickness direction of the spiral spring (maximum hardness NB1 to minimum hardness NB2) is 2.0 or more, and the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 μm or more and 10.0 μm or less, or composite inclusions formed by the combination of two or more individual inclusions, is 3.0 inclusions / mm². 2 Below, the hardness of the spring surface is 530 Hv or higher.
[0075] The Vickers hardness is preferably 535 Hv or higher, 540 Hv or higher, or 550 Hv or higher. There is no need to set an upper limit for the Vickers hardness, but for example, it may be 700 Hv or lower, 670 Hv or lower, 650 Hv or lower, or 620 Hv or lower. In the case of the spiral spring according to this embodiment, which is the final product (spiral spring), the torque characteristics can be improved by performing heat treatment (strain aging) at a temperature range of 200 to 300°C for 15 to 45 minutes after the cold-rolled steel sheet has been formed into a spring shape, in order to increase the elastic limit. Therefore, low-temperature annealing may be performed as needed. The hardness of the spiral spring can be increased by going through such a heat treatment process. For example, the Vickers hardness of the surface of the spiral spring can be made 580 Hv or higher by the above heat treatment. However, the aforementioned heat treatment is not mandatory, and the Vickers hardness of the surface of the spiral spring will be the same as that of the cold-rolled steel sheet described above (specifically, the lower limit of the Vickers hardness will be 530 HV). The method for measuring Vickers hardness will also be the same as that used for the cold-rolled steel sheet described above.
[0076] Regardless of whether the above heat treatment is performed, the chemical composition, microstructure (metal structure), lamellar spacing of the pearlite structure, and number density of inclusions (including coarse inclusions exceeding 10.0 μm) of the spiral spring of this embodiment, including their preferred ranges, are basically the same as those of the aforementioned cold-rolled steel sheet, which is the raw material. Therefore, the description of these requirements is omitted.
[0077] <Method for Manufacturing High-Carbon Cold-Rolled Steel Sheets> Next, a preferred method for manufacturing the high-carbon cold-rolled steel sheets of this embodiment will be described. The high-carbon cold-rolled steel sheets of this embodiment can be manufactured by a manufacturing method that includes the following steps.
[0078] (I) A steelmaking (refining and casting) process to produce a slab having the above chemical composition. (II) A slab heating process to heat the slab to 1100°C or higher. (III) A hot rolling process to obtain a high-carbon hot-rolled steel sheet by finishing-rolling the heated slab with an exit temperature of 820 to 920°C. (IV) A cooling process including a primary cooling process to cool the high-carbon hot-rolled steel sheet to 500 to 600°C at an average cooling rate of 50 to 80°C / second, followed by a secondary cooling process (pearlite transformation process) to restore the temperature to a maximum of (cooling stop temperature + 60)°C by air cooling for 1 to 10 seconds to transform the structure into pearlite, followed by cooling to 450 to 520°C at an average cooling rate of less than 5 to 20°C / second. (V) A winding process to wind the high-carbon hot-rolled steel sheet at a winding temperature of 450 to 520°C. (VI) Pickling process to remove scale from the surface of the high-carbon hot-rolled steel sheet after the winding process. (VII) Cold rolling process to obtain high-carbon cold-rolled steel sheet by cold-rolling the high-carbon hot-rolled steel sheet with a total reduction ratio of 90% or more.
[0079] Generally, a known method for manufacturing high-carbon cold-rolled steel sheets used in spiral springs and the like involves sequentially performing hot rolling, pickling, spheroidizing annealing, primary cold rolling, patenting, and secondary cold rolling. On the other hand, in the manufacturing method of this embodiment, which includes the above steps (I) to (VII), by creating a pearlite structure at the hot rolling and winding stages, it is possible to omit the spheroidizing annealing, primary cold rolling, and patenting processes that were conventionally performed, and to provide high-carbon cold-rolled steel sheets with high strength (torque characteristics) and excellent fatigue durability. Furthermore, high-carbon steel sheets obtained by this manufacturing method can be suitably applied to spiral springs and the like.
[0080] The following describes the preferred conditions for each process. For processes and conditions not described below, known conditions may be adopted.
[0081] [Steelmaking (refining and casting) process] Similar to general steel plates, molten steel is produced using, for example, blast furnace molten iron as a raw material, and then through converter refining and secondary refining, slabs and other cast pieces are obtained by continuous casting. Subsequently, these cast pieces are subjected to hot rolling or cold rolling, as described later, to obtain cold-rolled steel plates.
[0082] In this embodiment, after decarburization in the converter, the steel is subjected to vacuum degassing in a vacuum degassing device (DH, RH, etc.) during secondary refining, along with adjusting the steel's composition, and cast slabs are obtained by continuous casting. At this time, from the viewpoint of reducing the number density of individual oxide, sulfide, and nitride inclusions, and composite inclusions formed by the combination of two or more such individual inclusions, the total oxygen content (T.O.) in the molten steel is adjusted to 0.0030% or less by mass and S: 0.0015% or less, thereby reducing the number density of inclusions in the final cold-rolled steel sheet to 3.0 pieces / mm². 2 The following is possible. Preferably, the T.O content is 0.0030% or less, more preferably 0.0020% or less.
[0083] To reduce the number density of inclusions, after adjusting all components, in vacuum degassing treatment such as RH, Al generated during Al deoxidation is removed. 2 O 3To allow these elements to float to the surface, a sufficient reflux time must be ensured. This time (required reflux time) depends on the dimensions of the ladle used to adjust the composition of the added elements and other factors (for example, the capacity of the vacuum degassing equipment if the composition adjustment is performed during vacuum degassing). Therefore, it is not possible to uniformly determine the required reflux time. However, a person skilled in the art can easily determine the required reflux time for each refining apparatus, including the ladle, by analyzing the number density of inclusions in cold-rolled steel sheets, etc., obtained from tests with varying reflux times. However, when adding Ca, after adjusting the composition of elements other than Ca, Al produced during Al deoxidation, etc., must be removed. 2 O 3 To make it float, a vacuum degassing treatment is performed for a sufficient reflux time, after which Ca is added to the molten steel.
[0084] [Slab Heating Process] In the slab heating process, the slab having the above chemical composition is heated to 1100°C or higher before the hot rolling process. The heating temperature of the slab is set to 1100°C or higher in order to sufficiently redissolve the carbonitrides. If the heating temperature of the slab exceeds 1300°C, the effect will saturate, so it is preferable to keep it at 1300°C or lower.
[0085] Furthermore, the heating time in the slab heating process is preferably 30 minutes or longer. If the heating time is less than 30 minutes, the temperature may not rise uniformly to the interior of the slab, and the carbonitrides may not be sufficiently redissolved. If the redissolution of carbonitrides is insufficient, coarse carbonitrides may remain, and these coarse carbonitrides may act as the starting point for cracks during cold rolling, or the fatigue properties of the resulting cold-rolled steel sheet may deteriorate. On the other hand, if the heating time exceeds 120 minutes, the effect of sufficiently redissolving the carbonitrides becomes saturated. Also, excessively long heating times lead to decreased productivity and increased manufacturing costs. Therefore, a heating time of 120 minutes or less is preferable.
[0086] While it is preferable to manufacture the slabs to be heated by continuous casting from a productivity standpoint, they may also be manufactured by other casting methods (e.g., ingot casting).
[0087] [Hot Rolling Process] The hot rolling process in this embodiment is broadly divided into rough rolling and finish rolling.
[0088] (Rough Rolling) The heated slab is subjected to rough rolling to adjust the plate thickness, etc. The rough rolling is sufficient to obtain a rough bar of the desired dimensions and shape, and the conditions are not particularly limited. In rough rolling, the rough bar may be heated using an induction heating device such as a bar heater or edge heater to homogenize its temperature.
[0089] (Finish Rolling) Next, the roughly rolled slab is finished rolled to produce a high-carbon hot-rolled steel sheet. The exit temperature (finishing temperature) in this finishing roll is set to 820 to 920°C. If the exit temperature of the finishing roll exceeds 920°C, the austenite phase may coarseen, and the cold-rollability may decrease. For this reason, the upper limit of the exit temperature for finishing is 920°C or less, preferably 900°C or less, and more preferably 880°C or less. On the other hand, the lower limit of the exit temperature for finishing roll is sufficient if it is Ar3 or higher from the viewpoint of suppressing the coarsening of the austenite phase. However, if the finishing temperature is excessively low, the deformation resistance of the steel sheet increases, placing a great burden on the rolling mill and causing equipment trouble. For this reason, the lower limit of the exit temperature for finishing roll is set to 820°C or higher.
[0090] The thickness of hot-rolled steel sheets is determined by considering the reduction ratio during subsequent cold rolling. For example, it may be between 2.0 mm and 4.0 mm.
[0091] [Cooling Process] After the finish rolling is completed and before winding, controlled cooling of the hot-rolled steel sheet is performed. Controlled cooling is carried out in three stages: a primary cooling process, a secondary cooling process (pearlite transformation process), and a tertiary cooling process.
[0092] (Primary Cooling Process) In the primary cooling process, the hot-rolled steel sheet is cooled from the exit temperature of the finish rolling described above to a primary cooling stop temperature T1 of 500 to 600°C at an average cooling rate CR1 of 50 to 80°C / second. If the average cooling rate CR1 is less than 50°C / second, protereminate ferrite phase and / or protereminate cementite phase may precipitate, and it may not be possible to achieve an area fraction of 95% or more of the pearlite structure in the 1 / 4 tH region. For this reason, it is preferable to set the average cooling rate CR1 to 50°C / second or higher. More preferably, it is 60°C / second or higher. On the other hand, if the average cooling rate CR1 exceeds 80°C / second, it may not be possible to cool the hot-rolled steel sheet uniformly, and variations in material properties may occur. For this reason, it is preferable to set the average cooling rate CR1 of the primary cooling process to 80°C / second or lower, and more preferably, 70°C / second or lower. The lower limit of the temporary cooling stop temperature T1 is 500°C. If the temporary cooling stop temperature T1 is below 500°C, other tissues other than pearlite tissue, such as bainite tissue, will appear, making it difficult to achieve a pearlite tissue area fraction of 95% or more.
[0093] Ae1 (°C) can be calculated using the following formula (1): Ae1 (°C) = 723 - 10.7 × [Mn] + 29.1 × [Si] + 16.9 × [Cr] ... (1)
[0094] (Secondary Cooling Process (Pearlite Transformation Process)) In the secondary cooling process, the hot-rolled steel sheet after the primary cooling process is air-cooled and / or slowly cooled for 1.0 to 10.0 seconds. Most of the transformation into pearlite occurs during the secondary cooling process, so it can also be called the pearlite transformation process. However, pearlite transformation does not only occur during the secondary cooling process, and can also occur during other processes.
[0095] In the secondary cooling process (pearlite transformation process), the material is restored for 1 to 10 seconds after the end of the primary cooling so that the temperature is (T1 + 60)°C or lower from the primary cooling stop temperature T1. During this restoration, air cooling without water cooling is permitted, but water cooling is performed as needed to prevent the temperature from rising above (T1 + 60)°C. From the viewpoint of varying the lamellar spacing of the pearlite, the material is restored to a temperature of 20°C or higher from the primary cooling temperature. In other words, the restoration temperature (temperature rise in the secondary cooling process) is set to 20°C or higher. Therefore, in the pearlite transformation process, air cooling or the amount of water injected is limited so that the temperature after restoration is (T1 + 20)°C or higher. This process makes it possible to obtain a hot-rolled steel sheet with varying lamellar spacing by mixing pearlite structures that have transformed from low to high temperatures. This results in a hot-rolled steel sheet with a Vickers hardness ratio V1 / V2 of 1.1 or higher. Furthermore, by cold-rolling this hot-rolled steel sheet as described below, a cold-rolled steel sheet with a nanoindentation hardness ratio NC1 / NC2 of 2.0 or higher can be obtained. Note that when a hot-rolled steel sheet with a lamellar structure created by conventional patenting is used, the nanoindentation hardness ratio NC1 / NC2 (or NB1 / NB2) will be less than 2.0, and the Vickers hardness ratio V1 / V2 will be less than 1.1.
[0096] (Tertiary Cooling Process) After the secondary cooling process is completed, the material is cooled to the winding temperature CT. If the average cooling rate CR3 in the temperature range up to the winding temperature CT is too fast, the risk of fracture during cold rolling increases due to overcooling at the edges of the steel sheet. Therefore, the average cooling rate CR3 in the tertiary cooling process should be set to 5°C / second or more and 20°C / second or less.
[0097] [Winding Process] After the tertiary cooling process, the hot-rolled steel sheet is wound up. The winding temperature CT of the hot-rolled steel sheet is 450 to 520°C. More preferably 500°C or lower, and more preferably 480°C or lower. By controlling the winding temperature CT to 520°C or lower, the decomposition reaction of pearlite after winding can be suppressed, and layered lamellae can be retained. This makes it possible to enhance work hardening during the cold rolling process. Since overcooling can cause low-temperature transformation phases to occur at the edges of the steel sheet, etc., and may cause sheet fracture, a winding temperature of 450°C or higher is preferred. More preferably 470°C or higher. Note that the end temperature of the tertiary cooling and the winding temperature CT are the same.
[0098] Through the above process, a hot-rolled steel sheet according to this embodiment is obtained.
[0099] [Pickling Process] Next, the manufactured hot-rolled steel sheets are pickled to remove scale (surface oxide layer) from the surface of the steel sheets.
[0100] [Cold Rolling Process] After the pickling process, the hot-rolled steel sheet is cold-rolled to obtain a high-carbon cold-rolled steel sheet. The total reduction ratio in cold rolling is preferably 90.0% or more. By setting it to 90.0% or more, the lamellar spacing of the pearlite structure in the cold-rolled steel sheet can be set to 20 nm or more and 50 nm or less. The total reduction ratio in cold rolling is more preferably 91% or more. Furthermore, by controlling the lamellar spacing to 20 nm or more and 50 nm or less, the Vickers hardness of the surface of the cold-rolled steel sheet can be set to 530 Hv or more.
[0101] The thickness of the cold-rolled steel sheet is preferably 0.180 mm or more and 0.260 mm or less, more preferably 0.160 mm or more and 0.250 mm or less, and even more preferably 0.180 mm or more and 0.240 mm or less.
[0102] From the viewpoint of suppressing strain aging during cold rolling, it is preferable to perform cold rolling at a steel sheet temperature of 110°C or lower. Preferably, cold rolling is performed at 100°C or lower, more preferably 80°C or lower, and even more preferably 60°C or lower. For example, in order to suppress the rise in steel sheet temperature, it is preferable to set the reduction ratio per pass to 5% or lower.
[0103] One effect of suppressing strain aging during cold rolling is that the increase in strength due to strain aging is suppressed. As a result, the cold workability of cold-rolled steel sheets when spring-forming is improved, and the effect of achieving equivalent hardness in subsequent aging treatment can be enjoyed.
[0104] <Method for manufacturing high-carbon hot-rolled steel sheets> The method for manufacturing high-carbon hot-rolled steel sheets according to this embodiment can employ the above steps (I) to (VI). If the pickling step is omitted, high-carbon hot-rolled steel sheets may be manufactured by the above steps (I) to (V).
[0105] <Method for Manufacturing a Spiral Spring> Furthermore, the following method can be applied to the method for manufacturing the spiral spring according to this embodiment. First, the cold-rolled steel sheet obtained by the above manufacturing method is cold-formed into a spring shape, and then, if necessary, heat treatment (strain aging) is preferably performed at a temperature range of 200 to 300°C for 15 to 45 minutes. By applying such a manufacturing method, the spiral spring according to this embodiment can be suitably manufactured.
[0106] Next, embodiments of the present invention will be described. The conditions in the embodiments are merely examples of conditions adopted to confirm the feasibility and effectiveness of the present invention, and the present invention is not limited to these examples of conditions. The present invention can adopt various conditions as long as they do not depart from the spirit of the invention and achieve the objectives of the present invention.
[0107] A slab having the chemical composition (ladle analysis value) listed in Table 1 (provided the reflux time in the steelmaking process is as shown in Tables 2A and 2B) was hot-rolled under the conditions shown in Tables 2A and 2B, and then wound to obtain a hot-rolled steel sheet having the thickness shown in Table 2B. For the obtained hot-rolled steel sheet, the Vickers hardness of the surface, the area fraction of the pearlite structure in the 1 / 4 region, the Vickers hardness ratio V1 / V2, and the number density of inclusions were determined using the method described above. The results are shown in Table 5. In Tables 2A and 2B, values that deviate from the preferred manufacturing method for high-carbon hot-rolled steel sheets of this embodiment are underlined. In the equipment of this embodiment, when the reflux time is 11 minutes or more, the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0.5 pieces / mm² for both hot-rolled and cold-rolled steel sheets. 2It can be set to less than 3.0 inclusions / mm³, and the number density of composite inclusions can be set to 3.0 inclusions / mm³. 2 The following was possible.
[0108] Subsequently, the obtained hot-rolled steel sheet was cold-rolled under the conditions shown in Table 3 to obtain a cold-rolled steel sheet. For the obtained cold-rolled steel sheet, the Vickers hardness of the surface, the area fraction of the pearlite structure in the 1 / 4 region, the hardness ratio of nanoindentation hardness NC1 / NC2, and the number density of inclusions were determined using the method described above. The results are shown in Tables 4A and 4B. In Table 3, values that deviate from the preferred manufacturing method for high-carbon cold-rolled steel sheets of this embodiment are underlined.
[0109] Furthermore, in both the hot-rolled steel sheets shown in Table 5 and the cold-rolled steel sheets shown in Tables 4A and 4B, the microstructure of the remaining structure other than the pearlite structure (limited to steel sheets where the area ratio of the pearlite structure is less than 100%) contained one or more of the ferrite phase, bainite structure, and martensite.
[0110] Furthermore, hot-rolled steel sheets were obtained by hot-rolling under the conditions shown in Table 6 and then coiling the material. Subsequently, the obtained hot-rolled steel sheets were patented under the conditions shown in Table 6, and test specimens were taken. The Vickers hardness of the surface, the area fraction of the pearlite structure in the 1 / 4 region, the hardness ratio of the Vickers hardness V1 / V2, and the number density of inclusions were measured using the method described above. In addition, cold-rolled steel sheets were obtained by cold-rolling the patented hot-rolled steel sheets. The results of measurements of the obtained cold-rolled steel sheets, including the Vickers hardness of the surface, the area fraction of the pearlite structure in the 1 / 4 region, the hardness ratio of the nanoindentation hardness NC1 / NC2, and the number density of inclusions, are also shown in Table 6.
[0111] Furthermore, the obtained cold-rolled steel sheets were subjected to heat treatment equivalent to that of the final product, at a temperature range of 200°C to 260°C for 15 to 45 minutes, and then their Vickers hardness and fatigue durability were evaluated. Fatigue durability was evaluated by conducting tests in accordance with "Fatigue Test Method for Thin Spring Sheets" in "Journal of Spring Engineering, No. 41 (1996), pp. 53-64," and determining the fatigue limit. The fatigue limit was 107 The stress at which failure did not occur after up to one test cycle was used to evaluate fatigue durability according to the following evaluation criteria: <Evaluation Criteria> A: Fatigue limit of 800 MPa or higher (Pass) B: Fatigue limit of 750 MPa or higher and less than 800 MPa (Pass) C: Fatigue limit less than 750 MPa (Fail)
[0112] As can be seen from Tables 4A, 4B, and 5, the inventive examples had a predetermined chemical composition, and all of the following were within the scope of the present invention: the area fraction of the pearlite structure, the lamellar spacing of the pearlite structure, the nanoindentation hardness (or Vickers hardness), the hardness ratio of these hardnesses, and the number density of inclusions. As a result, high strength (torque characteristics) and excellent fatigue durability were obtained. Note that since the area fraction of the pearlite structure, the lamellar spacing of the pearlite structure, the surface Vickers hardness, and the nanoindentation hardness do not fundamentally change after heat treatment (strain aging) at a temperature of 200 to 300°C for 15 to 45 minutes, these measurements were omitted after heat treatment (strain aging) at a temperature of 200 to 300°C for 15 to 45 minutes. Furthermore, the cold-rolled manufacturing methods No. E2, E9, E10, and E15 shown in Table 4, and the hot-rolled manufacturing methods No. D2, D9, D10, and D15 shown in Table 5, use steels No. A2, A9, A10, and A15, respectively, with a Cr content of 0.05% or more and less than 0.10%. However, the area fraction of the pearlite structure, the lamellar spacing of the pearlite structure, the nanoindentation hardness (or Vickers hardness), the hardness ratio of these hardnesses, and the number density of inclusions were all within the scope of the present invention. As a result, high strength (torque characteristics) and excellent fatigue durability were obtained.
[0113] In contrast, the comparative examples had a chemical composition, and at least one of the following factors—the surface area of the pearlite structure, the lamellar spacing of the pearlite structure, the surface Vickers hardness, the nanoindentation hardness (or Vickers hardness), the hardness ratio of these hardnesses, and the number density of inclusions—fell outside the scope of the present invention, resulting in inferior strength (torque characteristics) and fatigue durability. Note that cold rolling methods No. e2, e18, and e21 shown in Table 4 are all examples where the plates fractured due to a decrease in cold rolling properties.
[0114]
[0115]
[0116]
[0117]
[0118]
[0119]
[0120]
[0121]
[0122]
[0123] According to the above-described embodiment of the present invention, by creating a pearlite structure during the hot rolling process, it is possible to provide high-carbon cold-rolled steel sheets and high-carbon hot-rolled steel sheets with high strength (torque characteristics) and high fatigue durability, even without omitting spheroidizing annealing, primary cold rolling, and patenting treatment. Therefore, since high-carbon hot-rolled steel sheets and high-carbon cold-rolled steel sheets can be suitably applied to spiral springs and the like, high-carbon hot-rolled steel sheets and high-carbon cold-rolled steel sheets according to the above-described embodiment of the present invention have high industrial applicability.
Claims
1. The chemical composition, in mass%, is as follows: C: 0.70% to 0.90%, Si: 0.10% to 0.50%, Mn: 0.20% to 0.50%, Al: 0.003% to 0.015%, Cr: 0.10% to 0.50%, P: 0 to 0.020%, S: 0 to 0.0015%, O: 0 to 0.0030%, N: 0 to 0.0100%, Ti: 0 to 0.02%, Nb: 0 to 0.05%, V: 0 to 0.05%, Cu: 0 to 0.50%, Ni: 0 to 0.50%, B: 0 to 0.010%, Mo: 0 to 0.10%, W: 0 to 0.05%. Ta: 0-0.05%, Ca: 0-0.0500%, Mg: 0-0.05%, Sn: 0-0.05%, Sb: 0-0.05%, As: 0-0.05%, REM: 0-0.0050%, and the remainder: Fe and impurities, the surface Vickers hardness is 530 Hv or higher, the area fraction of the pearlite structure is 95% or higher, the lamellar spacing of the pearlite structure is 20-50 nm, the hardness ratio NC1 / NC2 of the nanoindentation hardness in the thickness direction from maximum hardness NC1 to minimum hardness NC2 is 2.0 or higher, When the plate thickness is tC, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions formed by the combination of two or more of the above individual inclusions, is 3.0 inclusions / mm² within a 1 / 4 tC plane. 2 The following describes a high-carbon cold-rolled steel sheet characterized by the following:
2. The chemical composition, in mass%, is: Ti: 0.001-0.02%, Nb: 0.001-0.05%, V: 0.001-0.05%, Cu: 0.001-0.50%, Ni: 0.001-0.50%, B: 0.001-0.010%, Mo: 0.001-0.10%, W: 0.001-0.05%, Ta: 0.001-0.05%, Ca: 0.0001-0.0500%, Mg: 0.0001-0.05%, Sn: 0.001-0.05%, Sb: 0.001-0.05%, As: 0.001-0.05%. The high-carbon cold-rolled steel sheet according to claim 1, characterized by containing one or more of the following: REM: 0.0001 to 0.0050%.
3. The high-carbon cold-rolled steel sheet according to claim 1, characterized in that its chemical composition is, in mass percent, Al: 0.003% to 0.010%, Cu: 0.001 to 0.05%, Ni: 0.001 to 0.05%, and Mo: 0.001 to 0.05%.
4. Within the 1 / 4tC plane, the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0.5 inclusions / mm². 2 A high-carbon cold-rolled steel sheet according to any one of claims 1 to 3, characterized in that it is less than [amount missing].
5. The chemical composition, in mass%, is as follows: C: 0.70%–0.90%, Si: 0.10%–0.50%, Mn: 0.20%–0.50%, Al: 0.003%–0.015%, Cr: 0.10%–0.50%, P: 0–0.020%, S: 0–0.0015%, O: 0–0.0030%, N: 0–0.0100%, Ti: 0–0.02%, Nb: 0–0.05%, V: 0–0.05%, Cu: 0–0.50%, Ni: 0–0.50%, B: 0–0.010%, Mo: 0–0.10%, W: 0–0.05%. Ta: 0-0.05%, Ca: 0-0.0500%, Mg: 0-0.05%, Sn: 0-0.05%, Sb: 0-0.05%, As: 0-0.05%, REM: 0-0.0050%, and the remainder: Fe and impurities, the surface Vickers hardness is 320-400 Hv, the area fraction of the pearlite structure is 95% or more, the average lamellar spacing of the pearlite structure is 80-200 nm, and the hardness ratio V1 / V2 of the maximum hardness V1 to the minimum hardness V2 of the Vickers hardness in the thickness direction is 1.10 or more. When the plate thickness is tH, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions formed by the combination of two or more such individual inclusions, is 3.0 particles / mm² within the 1 / 4 tH plane. 2 The following describes a high-carbon hot-rolled steel sheet characterized by the following:
6. The chemical composition, in mass%, is as follows: Ti: 0.001-0.02%, Nb: 0.001-0.05%, V: 0.001-0.05%, Cu: 0.001-0.50%, Ni: 0.001-0.50%, B: 0.001-0.010%, Mo: 0.001-0.10%, W: 0.001-0.05%, Ta: 0.001-0.05%, Ca: 0.0001-0.0500%, Mg: 0.0001-0.05%, Sn: 0.001-0.05%, Sb: 0.001-0.05%, As: 0.001-0.05%. The high-carbon hot-rolled steel sheet according to claim 5, characterized in that it contains one or more of the following: REM: 0.0001 to 0.0050%.
7. The high-carbon hot-rolled steel sheet according to claim 5, characterized in that its chemical composition is, in mass percent, Al: 0.003% to 0.010%, Cu: 0.001 to 0.05%, Ni: 0.001 to 0.05%, and Mo: 0.001 to 0.05%.
8. Within the 1 / 4 tH plane, the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0.5 inclusions / mm². 2 A high-carbon hot-rolled steel sheet according to any one of claims 5 to 7, characterized in that it is less than [amount missing].
9. The chemical composition, in mass%, is as follows: C: 0.70%–0.90%, Si: 0.10%–0.50%, Mn: 0.20%–0.50%, Al: 0.003%–0.015%, Cr: 0.10%–0.50%, P: 0–0.020%, S: 0–0.0015%, O: 0–0.0030%, N: 0–0.0100%, Ti: 0–0.02%, Nb: 0–0.05%, V: 0–0.05%, Cu: 0–0.50%, Ni: 0–0.50%, B: 0–0.010%, Mo: 0–0.10%, W: 0–0.05%. Ta: 0-0.05%, Ca: 0-0.0500%, Mg: 0-0.05%, Sn: 0-0.05%, Sb: 0-0.05%, As: 0-0.05%, REM: 0-0.0050%, and the remainder: Fe and impurities, the surface Vickers hardness is 530 Hv or higher, the area fraction of the pearlite structure is 95% or higher, the lamellar spacing of the pearlite structure is 20-50 nm, and the hardness ratio NB1 / NB2 of the nanoindentation hardness in the thickness direction, from the maximum hardness NB1 to the minimum hardness NB2, is 2.0 or higher. When the plate thickness is tB, the number density of individual inclusions of oxides, sulfides, and nitrides with an average particle size of 1.0 to 10.0 μm, or composite inclusions formed by the combination of two or more of the above individual inclusions, is 3.0 particles / mm² within a 1 / 4 tB plane. 2 A spiral spring characterized by the following:
10. The chemical composition, in mass%, is: Ti: 0.001-0.02%, Nb: 0.001-0.05%, V: 0.001-0.05%, Cu: 0.001-0.50%, Ni: 0.001-0.50%, B: 0.001-0.010%, Mo: 0.001-0.10%, W: 0.001-0.05%, Ta: 0.001-0.05%, Ca: 0.0001-0.0500%, Mg: 0.0001-0.05%, Sn: 0.001-0.05%, Sb: 0.001-0.05%, As: 0.001-0.05%. A spiral spring according to claim 9, characterized in that it contains one or more of the following: REM: 0.0001 to 0.0050%.
11. The spiral spring according to claim 9, characterized in that its chemical composition is, in mass percent, Al: 0.003% to 0.010%, Cu: 0.001 to 0.05%, Ni: 0.001 to 0.05%, and Mo: 0.001 to 0.05%.
12. The spiral spring according to any one of claims 9 to 11, characterized in that the Vickers hardness of the surface is 580 Hv or more.
13. Within the 1 / 4tB surface, the number density of coarse inclusions with an average particle size exceeding 10.0 μm is 0.5 inclusions / mm². 2 A spiral spring according to any one of claims 9 to 11, characterized in that it is less than [a certain value].