Adhesive sheet for manufacturing electronic component

The adhesive sheet addresses the challenge of conforming to uneven surfaces and securing electronic components by using a specialized design with a thermoplastic elastomer and acrylic adhesive, ensuring secure fixation and low outgassing for improved process precision.

WO2026239650A1PCT designated stage Publication Date: 2026-11-19NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/040452
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2025-11-19
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional adhesive sheets struggle to simultaneously achieve conformability to uneven surfaces, secure fixation of electronic components, and minimize outgassing, particularly when applied to components like bump wafers with fine connecting electrodes.

Method used

An adhesive sheet comprising a base material, resin layer, and adhesive layer, with specific sinking rates and TGA weight loss rates, incorporating a thermoplastic elastomer and acrylic adhesive, designed to provide conformability, secure fixation, and low outgassing.

Benefits of technology

The adhesive sheet exhibits excellent conformability to uneven surfaces, secure fixation, and low outgassing, enhancing precision in processes like back-grinding and improving grinding accuracy while preventing components from sticking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2025040452_19112026_PF_FP_ABST
    Figure JP2025040452_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an adhesive sheet for manufacturing an electronic component, the adhesive sheet having excellent unevenness followability and fixability with respect to the electronic component. An adhesive sheet for manufacturing an electronic component according to an embodiment of the present invention comprises a substrate, a resin layer, and an adhesive layer in this order, wherein the penetration ratio of the adhesive sheet in an environment of 100°C, as measured using TMA, is 3.5-60%. In the adhesive sheet for manufacturing an electronic component, the penetration ratio of the adhesive sheet in an environment of 40°C, as measured using TMA, may be 4% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive sheets for electronic component manufacturing

[0001] This invention relates to an adhesive sheet for the manufacture of electronic components.

[0002] Conventionally, in the manufacturing process of electronic components, electronic components such as semiconductor wafers are fixed onto an adhesive sheet and then processed. For example, in the backgrinding process, in which the back surface of a semiconductor wafer is ground to a desired thickness, an adhesive sheet (backgrind tape) is used to fix the semiconductor wafer and protect the surface opposite to the grinding surface (for example, Patent Document 1).

[0003] Some electronic components have uneven surfaces; for example, bump wafers, which are semiconductor wafers with a surface formed of fine connecting electrodes called bumps, are known. Adhesive sheets applied to such uneven surfaces require both surface conformability and the ability to securely fix electronic components. When attaching adhesive sheets to uneven surfaces, it is conceivable to raise the temperature to ensure surface conformability, but in that case, the fluidity of the adhesive layer may become too high, causing the adherend to become rigid. Furthermore, attempting to solve these problems from the constituent materials of the adhesive sheet may result in outgassing problems, making it difficult to achieve both surface conformability and secure fixation of electronic components, as well as to reduce outgassing.

[0004] Patent No. 5501060, Patent No. 6790032, Patent No. 3740451

[0005] The present invention was made to solve the above-mentioned conventional problems, and its objective is to provide an adhesive sheet for manufacturing electronic components that is excellent in terms of conforming to uneven surfaces and fixing electronic components.

[0006] 1. An adhesive sheet for manufacturing electronic components according to an embodiment of the present invention is an adhesive sheet comprising a base material, a resin layer, and an adhesive layer in that order, wherein the sinking rate of the adhesive sheet in a 100°C environment using TMA is 3.5% to 60%. 2. In the adhesive sheet for manufacturing electronic components described in 1 above, the sinking rate of the adhesive sheet in a 40°C environment using TMA may be 4% or less. 3. In the adhesive sheet for manufacturing electronic components described in 1 or 2 above, the TGA weight loss rate of the adhesive sheet at 350°C may be 0% to 35%. 4. In the adhesive sheet for manufacturing electronic components described in any of 1 to 3 above, the resin layer may contain a thermoplastic elastomer. 5. In the adhesive sheet for manufacturing electronic components described in 4 above, the thermoplastic elastomer may be a styrene-based elastomer. 6. In the adhesive sheet for manufacturing electronic components described in any of 1 to 5 above, the resin layer may contain a tackifying resin. 7. 6. In the adhesive sheet for manufacturing electronic components described above, the softening point of the tackifying resin may be 70°C to 130°C. 8. In the adhesive sheet for manufacturing electronic components described above, 6 or 7, the tackifying resin may be an alicyclic hydrocarbon resin. 9. In the adhesive sheet for manufacturing electronic components described above, 1 to 8, the thickness of the resin layer may be 10 μm to 300 μm. 10. In the adhesive sheet for manufacturing electronic components described above, 1 to 9, the adhesive layer may contain an acrylic adhesive. 11. In the adhesive sheet for manufacturing electronic components described above, 1 to 10, the adhesive layer may contain an active energy ray curable adhesive.

[0007] According to the present invention, an adhesive sheet for manufacturing electronic components can be provided that is excellent in terms of conformability to uneven surfaces and fixing properties. Furthermore, this adhesive sheet for manufacturing electronic components is also advantageous in that it has excellent peelability and low outgassing.

[0008] This is a schematic cross-sectional view of an adhesive sheet according to one embodiment of the present invention.

[0009] A. Schematic Figure 1 of the adhesive sheet for manufacturing electronic components is a schematic cross-sectional view of an adhesive sheet for manufacturing electronic components according to one embodiment of the present invention. The adhesive sheet 100 for manufacturing electronic components according to this embodiment comprises a base material 10, a resin layer 20, and an adhesive layer 30 in this order. The adhesive sheet for manufacturing electronic components can be used by attaching electronic components to the adhesive layer. The attached electronic components can be subjected to any appropriate processing. For example, such processing includes back grinding, which involves grinding and polishing the back surface of the electronic component (the surface opposite to the attachment surface). The adhesive sheet may also be used for dicing to separate electronic components into small pieces; surface treatment such as vapor deposition, sputtering, and plating on the electronic component surface; pattern formation on the workpiece surface; coating of the electronic component surface; cleaning of electronic components; removal of a predetermined layer; etc. Hereinafter, the adhesive sheet for manufacturing electronic components will also be simply referred to as the adhesive sheet.

[0010] The above adhesive sheet exhibits a sinking ratio of 3.5% to 60% in a 100°C environment using thermomechanical analysis (TMA). The sinking ratio using TMA refers to the ratio of the amount of sinking (in μm) measured after 20 minutes of contact with the adhesive layer using a thermomechanical analyzer (TMA) to the thickness of the adhesive sheet. The TMA measurement conditions are: probe diameter: 1.0 mm, mode: needle insertion mode, nitrogen gas flow rate: 50.0 ml / min, and indentation load: 0.99 N.

[0011] In embodiments of the present invention, by having the sinking ratio of TMA in a 100°C environment be within the above range, an adhesive sheet can be obtained that exhibits desirable flexibility at high temperatures and has excellent conformability to the uneven surface of electronic components. If such an adhesive sheet is used, for example, in a back-grinding process, back-grinding with excellent precision can be performed without impairing the flatness of the ground surface. Furthermore, it is prevented that the fluidity of the adhesive sheet becomes too high at high temperatures, preventing the electronic components, which are the adherends, from sticking to the adhesive sheet. In addition, the uniformity of conformability to uneven surfaces can be improved, and as a result, an adhesive sheet can be provided that can contribute to improving the precision of back-grinding.

[0012] Furthermore, by ensuring that the sinking ratio of TMA in a 100°C environment is within the above range, an adhesive sheet with excellent peelability (e.g., peelability after UV irradiation) and low outgassing can be obtained. Providing an adhesive sheet that combines conformability to the uneven surface of electronic components with excellent peelability and low outgassing is a major achievement of the present invention.

[0013] The sinking rate of the above adhesive sheet using TMA in a 100°C environment is preferably 3.5% to 60%, more preferably 15% to 40%, and even more preferably 20% to 35%. Within this range, the above effect becomes significant.

[0014] The sinking ratio of the above adhesive sheet using TMA in a 40°C environment is preferably 4% or less, more preferably 3% or less, and even more preferably 2% or less. Within this range, it is possible to provide an adhesive sheet that exhibits good fixing properties and can contribute to improving the processability of the electronic component to which it is adhered. For example, using the above adhesive sheet can improve the grinding accuracy in the back grinding process. The sinking ratio of the above adhesive sheet using TMA in a 40°C environment may be 0% or more, 0.05% or more, or 0.1% or more.

[0015] The TGA weight loss rate of the above adhesive sheet at 350°C is preferably 0% to 35%, more preferably 0% to 25%, and even more preferably 10% to 25%. Within this range, an adhesive sheet with low outgassing can be obtained. By reducing outgassing, void formation during application is suppressed, and an adhesive sheet that can contribute to improved grinding accuracy can be obtained. The above TGA weight loss rate can be determined by heating to 350°C at a heating rate of 10°C / min, measuring the weight loss after heating for 10 minutes, and calculating it using the formula: weight loss / weight before heating.

[0016] The initial adhesive strength at 23°C when the adhesive layer of the above adhesive sheet is attached to a silicon wafer is preferably 0 N / 20 mm to 15 N / 20 mm, and more preferably 0 N / 20 mm to 10 N / 20 mm. Within this range, an adhesive sheet capable of holding electronic components well can be obtained. The adhesive strength is measured in accordance with JIS Z 0237:2000. Specifically, the adhesive sheet is attached to a stainless steel plate (arithmetic mean surface roughness Ra: 50 ± 25 nm) by one back-and-forth motion of a 2 kg roller, left at 23°C for 30 minutes, and then the adhesive sheet is peeled off under conditions of a peel angle of 180° and a tensile speed of 300 mm / min for measurement. As described later, the adhesive layer may include an active energy ray curable adhesive, but in this specification, "initial adhesive strength" means the adhesive strength before irradiation with active energy rays.

[0017] In one embodiment, the adhesive layer of an adhesive sheet is attached to a silicon wafer, and 1080 mJ / cm² is applied. 2 The adhesive strength at 23°C after irradiation with ultraviolet light is preferably 0 N / 20 mm to 0.4 N / 20 mm, and more preferably 0 N / 20 mm to 0.2 N / 20 mm. The adhesive strength after ultraviolet irradiation can be measured after the adhesive layer is attached to the substrate and then the adhesive surface is irradiated with ultraviolet light.

[0018] The thickness of the adhesive sheet is preferably 1 μm to 300 μm, more preferably 5 μm to 260 μm, even more preferably 10 μm to 200 μm, and particularly preferably 20 μm to 160 μm.

[0019] B. Adhesive layer The adhesive sheet described above can be used by placing the electronic component to be adhered to on the adhesive layer surface.

[0020] The thickness of the adhesive layer is preferably 1.5 μm to 50 μm, more preferably 2 μm to 35 μm, and even more preferably 3 μm to 20 μm. Within this range, an adhesive layer with excellent conformability to uneven surfaces and excellent fixing properties can be obtained.

[0021] The adhesive layer described above contains any suitable adhesive, insofar as the effects of the present invention are obtained. The adhesive may be a pressure-sensitive adhesive or a curing adhesive. In one embodiment, an acrylic adhesive is used. In one embodiment, the adhesive layer described above contains an active energy ray curing adhesive.

[0022] (Active Energy Ray Curable Adhesive) Examples of base polymers constituting the above active energy ray curable adhesive include acrylic polymers, rubber polymers (e.g., natural rubber, chloroprene rubber, styrene-butadiene rubber, nitrile rubber, etc.), polyesters, urethane polymers, polyethers, silicone polymers, polyamides, fluorine polymers, ethylene-vinyl acetate polymers, epoxy resins, vinyl chloride polymers, cyanoacrylate polymers, cellulose polymers (nitrocellulose polymers, etc.), phenolic resins, polyimides, polyolefins, styrene polymers, polyvinyl acetate, polyvinyl alcohol, polyvinyl acetal, polyvinylpyrrolidone, polyvinyl butyral, polybenzimidazole, melamine resins, urea resins, resorcinol polymers, etc. These polymers may be used individually or in combination of two or more. From the viewpoint of adhesion and cost, acrylic polymers and rubber polymers are preferred, and acrylic polymers are more preferred. The term "base polymer" refers to the main component of the polymer contained in the adhesive. The polymer described above is preferably a rubbery polymer that exhibits rubber elasticity in a temperature range near room temperature. In this specification, unless otherwise specified, "main component" refers to a component present in an amount exceeding 50% by weight.

[0023] As the above acrylic polymer, for example, a polymer of a monomer raw material containing alkyl (meth)acrylate as the main monomer and a secondary monomer copolymerizable with the main monomer is preferred. Here, the main monomer refers to a component that accounts for more than 50% by weight of the monomer composition in the above monomer raw material. The content of the main monomer is preferably 60 to 100 parts by weight, and more preferably 70 to 99.5 parts by weight, based on 100 parts by weight of the total amount of monomer in the monomer raw material.

[0024] As the alkyl (meth)acrylate, for example, a compound represented by the following formula (1) can be suitably used. CH 2 = C(R 1 ) COOR 2 (1) Here, R in equation (1) above 1 R is a hydrogen atom or a methyl group. 2 R is a branched or linear alkyl group having 1 to 20 carbon atoms (hereinafter, this range of carbon atoms may be referred to as "C1-20"). 2 Preferably, it is a branched or linear C1-14 alkyl group, more preferably a branched or linear C6-14 alkyl group, and even more preferably a branched or linear C8-12 alkyl group.

[0025] Specific examples of the aforementioned alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and the like. These alkyl (meth)acrylates may be used singly or in combination of two or more. Among these, 2-ethylhexyl acrylate (2EHA) and lauryl (meth)acrylate (LA, LMA) are particularly preferred.

[0026] In one embodiment, R 2 is an alkyl (meth)acrylate in which the group is a branched or linear alkyl group having 8 or more carbon atoms. When such a monomer is used as the main monomer, it is possible to obtain a pressure-sensitive adhesive sheet that has a favorable elastic modulus before and after curing, and is particularly excellent in fixability and unevenness conformability. R 2 Examples of the alkyl (meth)acrylate in which the group is a branched or linear alkyl group having 8 or more carbon atoms include 2EHA, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, dodecyl (meth)acrylate, and the like. R 2The content of the alkyl (meth)acrylate-derived structural unit, which is a branched or linear alkyl group having 8 or more carbon atoms, is preferably 60 to 100 parts by weight, and more preferably 70 to 95 parts by weight, per 100 parts by weight of the base polymer.

[0027] The secondary monomers copolymerizable with the main monomer, alkyl (meth)acrylate, can be useful for introducing crosslinking sites into acrylic polymers or for enhancing the cohesive strength of acrylic polymers. Furthermore, it is preferable to use monomers as secondary monomers that have a functional group (functional group a) that can react with the functional group (functional group b) of the carbon-carbon double bond-containing monomer described later. As secondary monomers, for example, the following functional group-containing monomer components can be used individually or in combination of two or more. Carboxylate group-containing monomers: e.g., ethylenically unsaturated monocarboxylic acids such as acrylic acid (AA), methacrylic acid (MAA), and crotonic acid; ethylenically unsaturated dicarboxylic acids such as maleic acid, itaconic acid, and citraconic acid, and their anhydrides (maleic anhydride, itaconic anhydride, etc.); hydroxyl group-containing monomers: e.g., hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate; unsaturated alcohols such as vinyl alcohol and allyl alcohol; ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether; amino group-containing monomers: e.g., aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; epoxy group-containing monomers: e.g., glycidyl (meth)acrylate, methylglycidyl (meth)acrylate, and allyl glycidyl ether; Cyano group-containing monomers: e.g., acrylonitrile, methacrylonitrile; Keto group-containing monomers: e.g., diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetate, vinyl acetate;Monomers containing nitrogen atom rings: e.g., N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, N-(meth)acryloylmorpholine; Monomers containing alkoxysilyl groups: e.g., 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane; Monomers containing isocyanate groups: (meth)acryloylisocyanate, 2-(meth)acryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate.

[0028] In one embodiment, a hydroxyl group-containing monomer is preferably used as the sub-monomer, and 2-hydroxyethyl (meth)acrylate may be more preferably used. Using this monomer, an adhesive sheet can be obtained that has a desirable elastic modulus before and after curing and is particularly excellent in fixing electronic components and conforming to uneven surfaces.

[0029] The content ratio of the constituent units derived from the above-mentioned sub-monomers is preferably 0.1 to 40 parts by weight, and more preferably 1 to 30 parts by weight, per 100 parts by weight of the base polymer. Within this range, an adhesive layer with high cohesive strength and excellent tackiness can be formed.

[0030] Furthermore, when a base polymer having a carbon-carbon double bond is used as the base polymer, as described later, it is preferable to use a sub-monomer having a functional group (functional group a) that can react with the functional group (functional group b) of compound B having a carbon-carbon double bond, as described later. In this case, the type of sub-monomer is determined by the type of compound B. As sub-monomers having functional group a, for example, carboxyl group-containing monomers, epoxy group-containing monomers, hydroxyl group-containing monomers, and isocyanate group-containing monomers are preferred, with hydroxyl group-containing monomers being particularly preferred. By using a hydroxyl group-containing monomer as a sub-monomer, the acrylic polymer has hydroxyl groups. In contrast, by using an isocyanate group-containing monomer as compound B having a carbon-carbon double bond, the hydroxyl group of the acrylic polymer reacts with the isocyanate group of the compound, and a carbon-carbon double bond derived from compound B is introduced into the acrylic polymer.

[0031] Furthermore, other copolymerization components besides the aforementioned sub-monomers can be used for purposes such as increasing the cohesive strength of the acrylic polymer. Examples of such copolymer components include vinyl ester monomers such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene, substituted styrene (α-methylstyrene, etc.), and vinyltoluene; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, cyclopentyl di(meth)acrylate, and isobornyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as aryl (meth)acrylate (e.g., phenyl (meth)acrylate), aryloxyalkyl (meth)acrylate (e.g., phenoxyethyl (meth)acrylate), and arylalkyl (meth)acrylate (e.g., benzyl (meth)acrylate); olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether; and the like. Other copolymerization components besides these secondary monomers can be used individually or in combination of two or more. The amount of such other copolymerization components is, for example, 2 to 20 parts by weight per 100 parts by weight of the total amount of monomer in the monomer raw material.

[0032] Furthermore, for the purpose of crosslinking treatment of the acrylic polymer and the like, a polyfunctional monomer can be used as a copolymerizable component. As the polyfunctional monomer, one or more of hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, urethane acrylate and the like can be used. The amount of the polyfunctional monomer is, for example, 30 parts by weight or less based on 100 parts by weight of the total amount of monomers in the monomer raw material.

[0033] The acrylic polymer can be obtained by any appropriate polymerization method. Examples thereof include a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method and the like.

[0034] Preferably, a carbon-carbon double bond is introduced into the base polymer (preferably an acrylic polymer). By using the base polymer having a carbon-carbon double bond, a pressure-sensitive adhesive layer that is curable with active energy rays (typically ultraviolet rays) can be formed.

[0035] Any appropriate method can be adopted as the method for producing the base polymer having a carbon-carbon double bond. For example, a method of reacting Polymer A having a functional group a with Compound B having a functional group (functional group b) capable of reacting with the functional group a and a carbon-carbon double bond is mentioned. In this case, the reaction is preferably carried out so that the carbon-carbon double bond does not disappear, and for example, a condensation reaction, an addition reaction or the like can be adopted. As Polymer A, for example, as described above, a polymer obtained by copolymerizing an alkyl (meth)acrylate as a main monomer and a comonomer having a functional group a is used.

[0036] Examples of the combination of the functional group a and the functional group b include a combination of a carboxy group and an epoxy group, a combination of a carboxy group and an aziridyl group, and a combination of a hydroxyl group and an isocyanate group. Among these, the combination of a hydroxyl group and an isocyanate group is preferred from the viewpoint of reaction traceability. From the viewpoint of polymer design and the like, a combination in which the acrylic polymer has a hydroxyl group and the above compound has an isocyanate group is particularly preferred.

[0037] Examples of the compound having a carbon-carbon double bond and the functional group b include, for example, isocyanate group-containing monomers (isocyanate group-containing compounds). Among these, 2-(meth)acryloyloxyethyl isocyanate is more preferred.

[0038] The blending amount of the isocyanate group-containing monomer is preferably 1 to 40 parts by weight, more preferably 5 to 30 parts by weight, and even more preferably 8 to 15 parts by weight, relative to 100 parts by weight of the polymer before the carbon-carbon double bond is introduced (i.e., polymer A).

[0039] In addition, the carbon-carbon double bond may be introduced such that the hydroxyl group originally possessed by polymer A remains. In this way, the degree of crosslinking can be increased when the pressure-sensitive adhesive layer is heated. In this case, the molar ratio (a / b) of the hydroxyl group as the functional group a to the isocyanate group as the functional group b suitably exceeds 1, and is preferably 1.1 or more.

[0040] The weight average molecular weight Mw of the base polymer (preferably an acrylic polymer) is preferably 10 × 10 4 to 500 × 10 4 , more preferably 20 × 10 4 to 200 × 10 4 , even more preferably 30 × 10 4 to 100 × 10 4 . Within such a range, a pressure-sensitive adhesive layer with little adhesive residue and excellent adhesion can be formed. In this specification, Mw refers to a value in terms of standard polystyrene obtained by GPC.

[0041] Preferably, the adhesive contains a crosslinking agent. Examples of crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, amine-based crosslinking agents, and the like. These crosslinking agents can be used individually or in combination of two or more.

[0042] The content ratio of the above crosslinking agent is preferably 0.1 to 10 parts by weight, and more preferably 0.2 to 8 parts by weight, per 100 parts by weight of the base polymer of the adhesive. Within this range, an adhesive layer with appropriately adjusted nanoindenter modulus can be formed.

[0043] In one embodiment, an isocyanate-based crosslinking agent is preferably used. Isocyanate-based crosslinking agents are preferred because they can react with a variety of functional groups. Specific examples of the above-mentioned isocyanate-based crosslinking agents include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HL"), and isocyanurate derivative of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HX"); and the like. Preferably, a crosslinking agent having three or more isocyanate groups is used.

[0044] The above-mentioned isocyanate-based crosslinking agent is preferably added in such a way that the number of functional groups of the isocyanate-based crosslinking agent is 10 mol% to 50 mol%, and more preferably 20 mol% to 40 mol%, relative to the number of functional groups in the base polymer that can react with the isocyanate-based crosslinking agent. Adding it in such amounts allows for the formation of an adhesive layer with appropriately adjusted nanoindenter modulus.

[0045] The above adhesive may further contain any suitable additives as needed. Examples of such additives include photopolymerization initiators, tackifiers, plasticizers (e.g., trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers), pigments, dyes, fillers, antioxidants, conductive materials, ultraviolet absorbers, light stabilizers, release modifiers, softeners, surfactants, flame retardants, antioxidants, solvents, and the like.

[0046] C. Resin Layer The storage modulus A of the resin layer at 40°C is preferably 0.6 MPa to 7 MPa, more preferably 0.6 MPa to 5 MPa, and even more preferably 0.6 MPa to 3 MPa. Within this range, an adhesive sheet can be provided that exhibits good fixation properties and contributes to improving the processability of the electronic component to which it is adhered. The storage modulus A can be measured using a dynamic viscoelasticity measuring device on a sample cut to an 8 mmΦ size, under conditions of a frequency of 1 Hz and a strain of 1%.

[0047] The storage modulus of the resin layer at 100°C is preferably 0.6 MPa to 30 MPa, more preferably 0.6 MPa to 20 MPa, and even more preferably 0.6 MPa to 10 MPa. Within this range, an adhesive sheet can be provided that exhibits desirable flexibility at high temperatures and has excellent conformability to the uneven surfaces of electronic components. Furthermore, it prevents the fluidity of the adhesive sheet from becoming too high at high temperatures, thus preventing the electronic components, as the adherends, from sticking to the adhesive sheet. The storage modulus can be measured using a dynamic viscoelasticity measuring device on a sample cut to an 8 mmΦ size, under conditions of a frequency of 1 Hz and a strain of 1%.

[0048] The thickness of the resin layer is preferably 10 μm to 300 μm, more preferably 20 μm to 280 μm, even more preferably 30 μm to 250 μm, even more preferably 30 μm to 200 μm, and particularly preferably 20 μm to 100 μm. Within this range, the above effects of the present invention become remarkable. Furthermore, it is possible to provide an adhesive sheet with excellent grinding accuracy in the back-grinding process.

[0049] The above resin layer is composed of any suitable resin composition, as long as the effects of the present invention are obtained. Examples of resin compositions constituting the resin layer include thermoplastic elastomers, vinyl acetate resins, acrylic resins, silicone resins, vinyl alkyl ether resins, polyester resins, polyamide resins, urethane resins, fluorinated resins, and the like. Preferably, the above resin layer contains a thermoplastic resin, and more preferably a thermoplastic elastomer or a vinyl acetate resin. Examples of thermoplastic elastomers include styrene elastomers. The resin content in the resin layer is preferably more than 50 parts by weight per 100 parts by weight of the resin layer.

[0050] In one embodiment, a styrene-based elastomer is used as the thermoplastic elastomer. Due to its frequency dependence, styrene-based elastomers behave hard in the high-speed range and soft in the low-speed range. Therefore, if an adhesive sheet comprising a resin layer containing a styrene-based elastomer is used in the backgrinding process, the adhesive sheet will be highly flexible and have excellent conformability to uneven surfaces when applied, while becoming hard during the grinding process with a high-speed rotary drill, thereby improving grinding accuracy. Furthermore, because styrene-based elastomers have a high softening point, using them allows for the creation of an adhesive sheet that does not become excessively fluid at high temperatures during application and can uniformly conform to uneven surfaces. In addition, because styrene-based elastomers have low outgassing, using them can suppress void generation during application, resulting in an adhesive sheet that can contribute to improved grinding accuracy. Furthermore, because styrene-based elastomers have excellent chemical resistance, using them makes it possible to obtain adhesive sheets suitable for use in processes involving chemicals (for example, the Advanced Package manufacturing process for next-generation semiconductors).

[0051] Examples of styrene-based elastomers include styrene-butadiene copolymer (SB), styrene-isoprene copolymer (SI), styrene-isoprene-styrene block copolymer (SIS), styrene-butadiene-styrene block copolymer (SBS), styrene-isobutylene-styrene copolymer (SIBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-ethylene-propylene block copolymer (SEP), styrene-ethylene-propylene-styrene block copolymer (SEPS), and modified versions thereof. Among these, SEBS, SBS, SIS, and SIBS are preferred, with SEBS being particularly preferred. These copolymers are preferably block copolymers.

[0052] In the styrene-based elastomer described above, the content ratio of styrene-derived structural units is preferably 5 to 75 parts by weight, more preferably 10 to 70 parts by weight, even more preferably 10 to 50 parts by weight, particularly preferably 10 to 40 parts by weight, and most preferably 15 to 30 parts by weight, per 100 parts by weight of the styrene-based elastomer. Within this range, an adhesive sheet can be obtained that has appropriate elasticity and enables back grinding with excellent grinding accuracy.

[0053] In one embodiment, an acid-modified styrene elastomer (preferably acid-modified SEBS, SBS, SIS, or SIBS) is used as the styrene elastomer. Examples of acids used for the acid modification include maleic acid and maleic anhydride, with maleic acid modification being preferred. By using an acid-modified styrene elastomer, the molecular weight can be adjusted or a crosslinked structure can be formed by using a crosslinking agent (e.g., an epoxy crosslinking agent) in combination. The acid value of the acid-modified styrene elastomer is preferably 5 mg (CH3ONa) / g or more, more preferably 7 mg (CH3ONa) / g or more, and even more preferably 7 mg (CH3ONa) / g to 25 (CH3ONa) / g. The acid value here is calculated by neutralizing 1 g of the base polymer with sodium methoxide (CH3ONa). 3 This refers to the weight (mg) of ONa. Furthermore, the acid value of the base polymer can be measured in accordance with JIS K0070:1992.

[0054] The above resin composition may contain any suitable additives as needed. Examples of such additives include tackifying resins, plasticizers, pigments, dyes, fillers, antioxidants, conductive materials, antistatic agents, ultraviolet absorbers, light stabilizers, release modifiers, softeners, surfactants, flame retardants, antioxidants, crosslinking agents, and the like.

[0055] In one embodiment, the resin composition includes a tackifying resin. That is, the resin layer may include a tackifying resin. In particular, when the resin composition includes a styrene-based elastomer, it is preferable to use the elastomer and the tackifying resin in combination. By using a tackifying resin in combination, an adhesive sheet can be obtained that exhibits elasticity at high temperatures and has excellent conformability to uneven surfaces of electronic components.

[0056] As the tackifying resin described above, any suitable tackifying resin can be used as long as the effects of the present invention are obtained. Specific examples of tackifying resins include rosin-based tackifying resins (e.g., unmodified rosin, modified rosin, rosin-phenol resins, rosin-ester resins, etc.), terpene-based tackifying resins (e.g., terpene resins, terpene-phenol resins, styrene-modified terpene resins, aromatic-modified terpene resins, hydrogenated terpene resins), hydrocarbon-based tackifying resins (e.g., aliphatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aromatic hydrocarbon resins (e.g., styrene resins, xylene resins, etc.), aliphatic-aromatic petroleum resins, aliphatic-alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, coumarone-indene resins, etc.), phenol-based tackifying resins (e.g., alkylphenol resins, xylene-formaldehyde resins, resol, novolac, etc.), ketone-based tackifying resins, polyamide-based tackifying resins, epoxy-based tackifying resins, elastomer-based tackifying resins, and the like. Preferably, the tackifying resin is a hydrocarbon-based tackifying resin (preferably an alicyclic hydrocarbon-based resin), a terpene-based tackifying resin, or a rosin-based tackifying resin, and more preferably an alicyclic hydrocarbon-based resin. The tackifying resin may be used alone or in combination of two or more types.

[0057] In one embodiment, the tackifying resin is an alicyclic hydrocarbon resin. By using an alicyclic hydrocarbon resin, a resin layer with excellent chemical resistance can be formed. Furthermore, an adhesive sheet can be obtained that preferably exhibits elasticity at high temperatures and has excellent conformability to the uneven surface of electronic components. Examples of alicyclic hydrocarbon resins include resins obtained by cyclization-dimerization and polymerization of diene components in the spent C4-C5 fraction, resins obtained by polymerization of cyclic monomers such as cyclopentadiene, and resins obtained by intranuclear hydrogenation of aromatic hydrocarbon resins.

[0058] The softening point of the tackifying resin is preferably 70°C to 130°C, more preferably 80°C to 128°C, even more preferably 85°C to 125°C, and particularly preferably 90°C to 120°C. Within this range, a resin layer with excellent chemical resistance can be formed. In this specification, the softening point refers to the temperature at which a square resin plate of 10 mm or more in length sinks 1 mm when a 50 N load is applied to an indenter with a cross-sectional area of ​​1 mm and a length of 3 mm.

[0059] The content of the tackifying resin is preferably 20 to 350 parts by weight, and more preferably 10 to 300 parts by weight, per 100 parts by weight of the resin in the resin composition. Within this range, an adhesive sheet can be obtained that exhibits good elasticity at high temperatures and has excellent conformability to the uneven surface of electronic components. Furthermore, a resin layer with excellent chemical resistance can be formed.

[0060] In one embodiment, the resin layer (resin composition) contains a crosslinking agent. The inclusion of a crosslinking agent allows for adjustment of the cohesive force of the resin layer.

[0061] Any suitable crosslinking agent can be used as the crosslinking agent, as long as the effects of the present invention are obtained. Examples of such crosslinking agents include epoxy crosslinking agents, isocyanate crosslinking agents, melamine crosslinking agents, peroxide crosslinking agents, as well as urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, carbodiimide crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, and amine crosslinking agents. Among these, epoxy crosslinking agents are preferred.

[0062] Examples of the epoxy crosslinking agents mentioned above include N,N,N',N'-tetraglycidyl-m-xylenediline, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500NP"), ethylene glycol Licol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, product name "Denacol") Examples include "EX-611"), glycerol polyglycidyl ether (manufactured by Nagase ChemteX, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, diglycidyl adipic acid ester, diglycidyl o-phthalate ester, triglycidyl-tris(2-hydroxyethyl) isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. The content of the epoxy crosslinking agent can be set to any appropriate amount depending on the elasticity of the desired resin layer, and is typically 0.01 to 10 parts by weight, more preferably 0.03 to 5 parts by weight, per 100 parts by weight of the base polymer.

[0063] D. Substrate The substrate may be composed of any suitable resin. Examples of such resins include polyethylene resins, polypropylene resins, polybutene resins, polymethylpentene resins and other polyolefin resins, polyurethane resins, polyester resins, polyimide resins, polyetherketone resins, polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, fluorine resins, silicone resins, cellulose resins, ionomer resins, and the like.

[0064] In one embodiment, a substrate made of a polyester resin is used as the substrate. A substrate made of a polyester resin preferably has rigidity, and by using such a substrate, it is possible to prevent misalignment when fixing electronic components.

[0065] The thickness of the above-mentioned substrate is preferably 2 μm to 300 μm, more preferably 5 μm to 200 μm, and even more preferably 10 μm to 200 μm.

[0066] In one embodiment, a substrate with a thickness of 30 μm to 200 μm (preferably a substrate made of polyester resin) is used. Using a substrate of such thickness makes it possible to prevent misalignment when fixing electronic components.

[0067] E. Method for Manufacturing Adhesive Sheets The above-mentioned adhesive sheet can be manufactured by any suitable method. For example, an adhesive sheet can be obtained by coating a substrate with the above-mentioned adhesive resin composition to form a resin layer, and then transferring a separately coated adhesive layer to the resin layer. Various coating methods can be employed, such as bar coater coating, air knife coating, gravure coating, gravure reverse coating, reverse roll coating, lip coating, die coating, dip coating, offset printing, flexographic printing, and screen printing.

[0068] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The test and evaluation methods in the examples are as follows. Unless otherwise specified, "parts" and "%" are based on weight.

[0069] (1) The storage modulus G' of a resin layer was measured using a dynamic viscoelasticity measuring device (TA Instruments Co., Ltd., product name "ARES-G2") at a measurement frequency of 1 Hz, a strain of 1%, and at 40°C and 100°C. Specifically, a sheet without a substrate and with a thickness of 50 μm was prepared using the normal resin composition obtained in the examples and comparative examples. This sheet was laminated to a thickness of 1.0 mm or more, punched out to a size of φ8 mm using a jig, and set on the probe of the ARES-G2. Measurements were taken from -50°C to 200°C at a heating rate of 5°C / min. From the obtained data, the values ​​of the storage modulus G' at 40°C and 100°C were extracted. In addition, the storage modulus G' at 40°C and 100°C was measured in the same manner with a measurement frequency of 0.1 Hz.

[0070] (2) Adhesion The adhesive layer of the adhesive sheet was attached to a silicon wafer, and the adhesive strength of the adhesive sheet to the wafer was measured according to the method in accordance with JIS Z 0237:2000 (bonding conditions: 2 kg roller, one reciprocation, tensile speed: 300 mm / min, peel angle: 180°, measurement temperature: 23°C). In addition, the adhesive layer of the adhesive sheet was attached to a polyethylene terephthalate film (Toray Industries, Ltd., product name "Lumirror S10", thickness: 25 μm), and the adhesive strength of the adhesive sheet to the polyethylene terephthalate film was measured by peeling the adherend from the adhesive sheet according to the method in accordance with JIS Z 0237:2000 (bonding conditions: 2 kg roller, one reciprocation, tensile speed: 300 mm / min, peel angle: 180°, measurement temperature: 23°C). Furthermore, after attaching to the adherend as described above, 1030 mJ / cm was applied to the adhesive layer. 2 The adhesive strength after irradiation with ultraviolet light was measured using the method described above.

[0071] (3) Using a TMA sinking depth thermomechanical analyzer (TA-instrument Co., Ltd., product name "TMA Q400"), a φ3.0 mm probe was used, and the sinking depth of the adhesive sheet was measured from the adhesive layer side in needle insertion mode under the following conditions: nitrogen gas flow rate: 50.0 ml / min, indentation load: 0.99 N, measurement ambient temperature: 40°C, heating rate: 5°C / min, indentation load time: 10 min. Measurements were performed with N=5, and the average value of N=3, excluding the maximum and minimum values ​​from these measurements, was taken as the sinking depth of the sample. The sinking depth of the adhesive sheet was also measured in the same manner as above, except that the measurement ambient temperature was set to 100°C. The sinking ratio was calculated from the thickness of the adhesive sheet and the measured sinking depth by TMA measurement.

[0072] (4) Using an outgassing thermogravimetric analyzer (TA Instruments, product name "TGA"), the weight loss of the adhesive sheet was measured after heating from 0°C to 370°C and holding for 10 min. Specifically, a 10 mg sample was cut from the adhesive sheet obtained in the examples and comparative examples, and the sample was placed in the analyzer. The amount of outgassing was measured by measuring the weight loss after heating from 0°C to 350°C at a heating rate of 10°C / min and holding at 350°C for 10 min.

[0073] (5) Bump-following ability (bump embedding ability) The appearance of the adhesive was measured when the sample was heated to 80°C with a load of 2.5 kN and held for 5 min using a vacuum press device (manufactured by Mikado Technos Co., Ltd., product name "VACUUM STAR") and held for 5 min. Specifically, a 10 mg sample was cut from the adhesive sheets of the examples and comparative examples to a size of 5 cm x 5 cm, and the adhesive sheet was set in the device so as to be attached to the bump surface of the bump wafer (5 cm x 5 cm). The bump embedding ability was evaluated by observing the appearance of the sample after it was heated to 80°C and heated and pressed with a load of 2.5 kN for 5 min. Images of the bump wafer were taken with a microscope at 10x magnification and binarized to obtain a black and white image. The images were compared with images of bump wafers without tape, and a sample was judged as passing (○) if the whiteness ratio of 80% or more and 100% or less was passed, and failing (×) otherwise.

[0074] (6) Softening point of tackifying resin Based on the B50 method, a load of 50 N was applied to a resin piece formed from a square plate of tackifying resin with a side length of 10 mm or more using an indenter with a cross-sectional area of ​​1 mm and a length of 3 mm. The temperature at which the piece sank 1 mm was measured, and this temperature was defined as the softening point of the tackifying resin.

[0075] [Production Example 1] Preparation of Acrylic Polymer A: 100 parts by weight of 2-ethylhexyl acrylate (2-EHA), 20 parts by weight of hydroxyethyl acrylate (HEA), 0.2 parts by weight of polymerization initiator (manufactured by Nippon Oil & Fats Co., Ltd., trade name "Niper BW"), and toluene were mixed. The resulting mixture was polymerized at 60°C under a nitrogen gas stream to obtain an acrylic copolymer with a weight-average molecular weight (Mw) of approximately 380,000. To a toluene solution containing 100 parts by weight of the acrylic copolymer, 16 parts by weight of methacryloyloxyethyl isocyanate (MOI) and 0.06 parts by weight of butyltin dilaurate were added to carry out the MOI addition reaction to prepare acrylic polymer A having a carbon-carbon double bond.

[0076] [Example 1] A resin layer-forming composition (I) was prepared by mixing 100 parts by weight of maleic acid-modified styrene-ethylene-butylene-styrene block copolymer (a) (SEBS: styrene moiety / ethylene-butylene moiety (weight ratio) = 15 / 85, manufactured by ENEOS Material, trade name "DYNARON 8600P"), 80 parts by weight of alicyclic hydrocarbon tackifier (manufactured by ENEOS Material, trade name "HA-105", softening point: 80°C), 3 parts by weight of epoxy crosslinking agent (manufactured by Mitsui Chemicals, trade name "Takenate D-101"), 3 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "Omnirad 127D"), and toluene as a solvent. This resin layer-forming composition (I) was applied to a PET substrate (thickness: 38 μm) to a dry thickness of 30 μm, and dried to form a resin layer. Furthermore, to a toluene solution of the acrylic polymer A, 3 parts by weight of an isocyanate crosslinking agent (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate L") and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "Omnirad" (Omnirad 127): 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one) were added per 100 parts by weight of the solids content of the acrylic polymer to prepare an adhesive. This adhesive was coated onto a release liner to obtain an ultraviolet-curable adhesive layer (thickness: 5 μm). The obtained adhesive layer was transferred onto the resin layer on the substrate to obtain an adhesive sheet. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0077] [Example 2] An adhesive sheet was obtained in the same manner as in Example 1, except that the thickness of the resin layer was 60 μm. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0078] [Example 3] An adhesive sheet was obtained in the same manner as in Example 1, except that the thickness of the resin layer was 100 μm. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0079] [Example 4] An adhesive sheet was obtained in the same manner as in Example 1, except that the thickness of the resin layer was 150 μm. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0080] [Example 5] An adhesive sheet was obtained in the same manner as in Example 1, except that the thickness of the resin layer was 250 μm. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0081] [Example 6] An adhesive sheet was obtained in the same manner as in Example 1, except that the amount of tackifying resin added during resin layer formation was 20 parts by weight. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0082] [Example 7] An adhesive sheet was obtained in the same manner as in Example 1, except that the amount of tackifying resin added during resin layer formation was 50 parts by weight. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0083] [Example 8] An adhesive sheet was obtained in the same manner as in Example 1, except that the amount of tackifying resin added during resin layer formation was 100 parts by weight. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 1.

[0084] [Examples 9-11] Adhesive sheets were obtained in the same manner as in Example 1, except that the copolymer shown in Table 1 was used instead of maleic acid-modified styrene-ethylene-butylene-styrene block copolymer (a). The obtained adhesive sheets were subjected to the above evaluation. The results are shown in Table 1. The copolymers used are as follows: Copolymer (b): Maleic acid-modified styrene-ethylene-butylene-styrene block copolymer: Styrene unit ratio: 12% by weight Copolymer (c): Maleic acid-modified styrene-ethylene-butylene-styrene block copolymer: Styrene unit ratio: 20% by weight Copolymer (d): Maleic acid-modified styrene-ethylene-butylene-styrene block copolymer: Styrene unit ratio: 42% by weight

[0085] [Examples 12-14, Comparative Example 7] Adhesive sheets were obtained in the same manner as in Example 1, except that the type and amount of tackifying resin used during resin layer formation were as shown in Table 1 or Table 2. The obtained adhesive sheets were subjected to the above evaluation. The results are shown in Tables 1 and 2. The contents of the tackifying resins used are as follows. YS Polystar T100: Terpene phenol-based tackifying resin, manufactured by Yasuhara Chemicals Co., Ltd., product name "YS Polystar T100", softening point: 100℃ HA125: Alicyclic hydrocarbon-based tackifying resin, manufactured by ENEOS Material Co., Ltd., product name "HA125", softening point: 125℃ YS Polystar T125: Terpene phenol-based tackifying resin, manufactured by Yasuhara Chemicals Co., Ltd., product name "YS Polystar T125", softening point: 125℃ YS Polystar S145: Terpene phenol-based tackifying resin, manufactured by Yasuhara Chemicals Co., Ltd., product name "YS Polystar S145", softening point: 145℃

[0086] [Comparative Example 1] 50 parts by weight of butyl acrylate (BA), 50 parts by weight of ethyl acrylate (EA), 5 parts by weight of acrylic acid (AA), 0.1 parts by weight of hydroxyethyl acrylate (HEA), 0.1 parts by weight of polymerization initiator (manufactured by Nippon Oil & Fats Co., Ltd., trade name "Niper BW"), and toluene as a solvent were mixed, and the resulting mixture was polymerized at 60°C under a nitrogen gas stream to obtain acrylic polymer C1. To the toluene solution of acrylic polymer C1, 1 part by weight of epoxy crosslinking agent (manufactured by Mitsui Chemicals, trade name "Takenate D-101") and 0.1 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "Omnirad 369E") were added per 100 parts by weight of the solids content of the acrylic polymer to prepare a resin layer forming composition (C1). An adhesive sheet was obtained in the same manner as in Example 1, except that a resin layer was formed using this resin layer-forming composition (C1). The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 2.

[0087] [Comparative Example 2] An adhesive sheet was obtained in the same manner as in Comparative Example 1, except that the thickness of the resin layer was 150 μm. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 2.

[0088] [Comparative Example 3] A resin layer-forming composition (C3) was prepared by mixing 100 parts by weight of a vinyl acetate copolymer (manufactured by Mitsui Dow Polychemicals, trade name "EV-550", vinyl acetate content: 14%) with toluene as a solvent. An adhesive sheet was obtained in the same manner as in Example 1, except that this resin layer-forming composition (C3) was used. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 2.

[0089] [Comparative Example 4] An adhesive sheet was obtained in the same manner as in Comparative Example 3, except that a vinyl acetate copolymer (manufactured by Mitsui Dow Polychemicals, trade name "EV-550") was replaced with a vinyl acetate copolymer (manufactured by Mitsui Dow Polychemicals, trade name "EV-250", vinyl acetate content: 28%). The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 2.

[0090] [Comparative Example 5] An adhesive sheet was obtained in the same manner as in Comparative Example 3, except that a vinyl acetate copolymer (manufactured by Mitsui Dow Polychemicals, trade name "EV-550") was replaced with a vinyl acetate copolymer (manufactured by Mitsui Dow Polychemicals, trade name "EV-150", vinyl acetate content: 33%). The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 2.

[0091] [Comparative Example 6] An adhesive sheet was obtained in the same manner as in Example 1, except that the thickness of the resin layer was 350 μm. The obtained adhesive sheet was subjected to the above evaluation. The results are shown in Table 2.

[0092]

[0093]

[0094] 10 Base material 20 Resin layer 30 Adhesive layer 100 Adhesive sheet

Claims

1. An adhesive sheet comprising a base material, a resin layer, and an adhesive layer in that order, wherein the sinking ratio of the adhesive sheet in a 100°C environment using TMA is 3.5% to 60%, for use in the manufacture of electronic components.

2. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the sinking rate of the adhesive sheet using TMA in a 40°C environment is 4% or less.

3. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the TGA weight loss rate of the adhesive sheet at 350°C is 0% to 35%.

4. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the resin layer comprises a thermoplastic elastomer.

5. The adhesive sheet for manufacturing electronic components according to claim 4, wherein the thermoplastic elastomer is a styrene-based elastomer.

6. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the resin layer includes an adhesive-granulating resin.

7. The adhesive sheet for manufacturing electronic components according to claim 6, wherein the softening point of the tackifying resin is 70°C to 130°C.

8. The adhesive sheet for manufacturing electronic components according to claim 6, wherein the tackifying resin is an alicyclic hydrocarbon resin.

9. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the thickness of the resin layer is 10 μm to 300 μm.

10. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the adhesive layer comprises an acrylic adhesive.

11. The adhesive sheet for manufacturing electronic components according to claim 1, wherein the adhesive layer comprises an active energy ray curable adhesive.