Catalyst, method for producing catalyst, and method for producing inorganic material
A catalyst structure with a substrate and permeable coating layer addresses the strength loss and contamination issues in FRP thermal recycling, ensuring high-strength fiber recovery with minimal catalyst residue.
Patent Information
- Application Number
- PCT/JP2026/001266
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-01-16
- Publication Date
- 2026-11-19
AI Technical Summary
Existing thermal recycling methods for fiber-reinforced plastics (FRP) result in recovered fibers with lower strength due to high-temperature decomposition, and the use of powdered catalysts leads to catalyst contamination requiring intensive washing.
A catalyst structure with a substrate supporting a catalyst component and a coating layer having openings is used, where the substrate is at least 0.5 cm wide, and the coating layer is formed with controlled cracks to allow reactant access while preventing catalyst peeling.
The catalyst structure maintains high fiber strength and reduces catalyst contamination, enabling easy separation and reuse, with the recovered inorganic materials containing less than 0.5 wt% catalyst residue.
Smart Images

Figure JP2026001266_19112026_PF_FP_ABST
Abstract
Description
Catalyst, method for producing catalyst, and method for producing inorganic material
[0001] The present invention relates to a catalyst, a method for producing the catalyst, and a method for producing an inorganic material. This application claims the priority of Japanese Patent Application No. 2025-080709 filed on May 13, 2025, and for designated countries where incorporation by reference of documents is permitted, the content described in that application is incorporated into this application by reference.
[0002] Fiber-reinforced plastics (FRP) are composite materials widely used in various industries such as aerospace, automotive, and structural / civil engineering. FRP typically uses a thermosetting matrix and glass or carbon fibers as reinforcing materials, and also contains other additives depending on the application and required properties.
[0003] However, as the usage volume increases, recycling of discarded FRP has become an increasingly important issue in the FRP industry. Currently, there are multiple methods for recycling FRP, including mechanical recycling, cement treatment, and chemical recycling, and the widely applied technology is thermal recycling.
[0004] In thermal recycling, FRP waste is heated in an inert atmosphere or an oxygen-containing atmosphere to completely decompose the thermosetting matrix, leaving only fillers and fibers. However, since this process is usually carried out at 500°C or higher, the recovered fibers have lower strength than brand-new fibers, resulting in reduced value. Therefore, it is necessary to develop an FRP recycling process that can recover fibers retaining high strength.
[0005] In this regard, Patent Document 1 describes "A method for producing an inorganic material, comprising a heating step of heating a composite material containing an organic material composed of an organic substance and an inorganic material composed of an inorganic substance in an oxidizing atmosphere in a state of being in contact with a decomposition promoting component that promotes thermal decomposition of the organic material and contains copper as a main component by mass ratio among the transition metal elements contained therein."
[0006] JP 2024-170954 A
[0007] However, in the pyrolysis treatment described in Patent Document 1, a powdered catalyst is used to accelerate the decomposition of the resin. In such a process, the catalyst remains as a contaminant in the recovered material after pyrolysis, requiring an additional resource-intensive washing step to separate the catalyst.
[0008] Therefore, the present invention aims to provide a technology that can reduce catalyst contamination in the thermal decomposition of composite materials.
[0009] To solve the above problems, one aspect of the present invention is a catalyst comprising a substrate, a catalyst component supported on the substrate, and a coating layer covering the catalyst component, wherein the substrate has a maximum width of 0.5 cm or more, and the coating layer has openings.
[0010] Another aspect of the present invention is a method for producing a catalyst, comprising the steps of: applying a coating agent to a catalyst component supported on a substrate having a maximum width of 0.5 cm or more; and drying the coating agent to cause cracks to form a coating layer having openings.
[0011] Another aspect of the present invention is a method for producing an inorganic material, comprising the steps of: introducing a composite material containing an organic material and an inorganic material into a processing apparatus; and heating the composite material together with a catalyst to cause thermal decomposition and extract the inorganic material. The catalyst comprises a substrate, a catalyst component supported on the substrate, and a coating layer covering the catalyst component, wherein the substrate has a maximum width of 0.5 cm or more, and the coating layer has openings.
[0012] The present invention provides a technology that can reduce catalyst contamination in the thermal decomposition of composite materials. Other problems, configurations, and effects will be clarified by the following description of embodiments.
[0013] Figure 1 is a cross-sectional view of the catalyst of this embodiment. Figure 2 is a diagram showing the method for manufacturing the inorganic material of this embodiment. Figure 3A is a photograph showing a wire-shaped catalyst coated with SiO2 wrapped around a composite material. Figure 3B is a photograph of glass fibers recovered after thermal decomposition of the composite material using a wire-shaped catalyst coated with SiO2. Figure 4 is a photograph showing a composite material sandwiched between two SiO2-coated catalysts using a copper plate. Figure 5A is a photograph showing a wire-shaped catalyst that is not coated with SiO2 wrapped around a composite material. Figure 5B is a photograph of glass fibers recovered after thermal decomposition of the composite material using a wire-shaped catalyst that is not coated with SiO2.
[0014] The embodiments and examples of the present invention will be described below with reference to text and drawings. However, the structures, materials, and other specific configurations shown in the present invention are not limited to the embodiments and examples discussed herein, and can be appropriately combined and improved without changing the gist of the invention. Furthermore, elements not directly related to the present invention will be omitted from the illustrations.
[0015] Figure 1 is a schematic cross-sectional view of a catalyst 10 to which one embodiment of the present invention is applied.
[0016] The catalyst 10 is used to accelerate the thermal decomposition treatment of composite materials such as fiber-reinforced plastics (FRP) containing inorganic and organic materials.
[0017] The catalyst 10 is a structure (which can also be called a "catalyst structure") having a substrate 11, a catalyst component 12, and a coating layer 13.
[0018] The substrate 11 acts as a carrier for supporting the catalyst component. Specifically, as a carrier, the substrate 11 increases the reaction area and improves reaction efficiency by widely dispersing the catalyst component. In addition, the substrate 11 stabilizes the catalyst component and extends the lifespan of the catalyst.
[0019] The base material 11 is preferably in a form and size that makes it easy to separate and recover from the inorganic material remaining after thermal decomposition. For example, the base material 11 may be plate-shaped, linear, cylindrical, prismatic, spherical, honeycomb-shaped, or a variation thereof. Linear materials may be wire-shaped, mesh-shaped, or fibrous. They may also be combinations thereof.
[0020] When the catalyst 10 is used in combination with a composite material, the size of the base material 11 is, for example, 0.5 cm or more in terms of one side, diameter, or maximum width (the point where the distance between any two points is longest), preferably 1 cm or more.
[0021] When the catalyst 10 is fixed in the reaction vessel, there are no particular restrictions on the size of the substrate 11; it should be a size that is easy to fix to the reaction bed and easy to replace.
[0022] The material of the base material 11 can be selected based on its thermal stability, chemical stability, and mechanical strength. Examples of base material 11 include metals such as copper, iron, titanium, and aluminum, or inorganic oxides such as copper oxide, iron oxide, titanium oxide, aluminum oxide, and silicon oxide. Among these, copper is preferred. The surface of the base material 11 may also function as a catalyst component 12.
[0023] By using such a substrate 11, it is possible to maintain the activity of the catalyst component 12 while improving the recoverability and reusability in post-treatment processes.
[0024] The catalyst component (catalytically active component) 12 is a component that lowers the temperature of thermal decomposition of the composite material to be treated and promotes thermal decomposition, and is not limited as long as it has that function. The catalyst component 12 is selected from, for example, copper, zinc, chromium, cobalt, magnesium, manganese, tin, iron, cerium, nickel, tungsten, aluminum, titanium, or compounds consisting of combinations thereof. The catalyst component 12 may also be a metal oxide such as copper oxide, iron oxide, manganese oxide, cerium oxide, titanium oxide, or aluminum oxide. Furthermore, the catalyst component 12 may also be a composite oxide.
[0025] The catalyst component 12 may be supported on the substrate 11 during the manufacturing process of the catalyst 10. Alternatively, the surface of the substrate 11 may function as the catalyst component 12. Furthermore, the surface of the substrate 11 may change into an oxide and function as the catalyst component 12.
[0026] The content of catalyst component 12 is preferably at least 0.0001 wt% relative to the total catalyst 10 in order to exhibit catalytic function.
[0027] The coating layer 13 is a layer that covers the entire catalyst component 12 and is a layer that suppresses the peeling of the catalyst component (e.g., copper oxide) 12. On the other hand, it has a plurality of openings 131 to allow oxygen, which contributes to the thermal decomposition of the composite material, to pass through. The openings 131 exist as countless cracks throughout the entire surface of the coating layer 13.
[0028] If the opening 131 is too large, it will not be able to effectively prevent the peeling of the catalyst component 12, leading to catalyst contamination. Conversely, if it is too small, the catalyst will not be able to fully exhibit its performance. Therefore, the size of the opening is, for example, 10 nm to 500 nm at its maximum width (the point where the distance between any two points is longest), preferably 20 nm to 200 nm.
[0029] The coating layer 13 is selected from silicon dioxide (SiO2), aluminum oxide (Al2O3), titanium dioxide (TiO2), zirconium oxide (ZrO2), boron (B), or a compound of these, and is preferably silicon dioxide (SiO2), aluminum oxide (Al2O3), or titanium dioxide (TiO2).
[0030] The thickness of the coating layer 13 is 20 nm to 100 μm, preferably 5 nm to 10 μm.
[0031] <Method for Manufacturing the Catalyst> The catalyst 10 according to this embodiment has a structure in which a catalyst component 12 is supported on a substrate 11, and the surface of the catalyst component 12 is further covered with a permeable coating layer 13. The manufacturing method using a metal oxide as the catalyst component 12 will be described below.
[0032] First, the substrate (e.g., copper plate, copper wire) 11 is cleaned before the manufacturing process. Preferably, the cleaning process uses an organic solvent such as acetone to remove organic impurities, oil, fine particles, etc., from the surface of the substrate 11. Such pretreatment improves the adhesion and uniformity of the coating layer in subsequent processes.
[0033] Next, the substrate 11, after cleaning, is subjected to oxidation treatment or heating in air, which oxidizes the metal on its surface and forms a metal oxide (e.g., copper(II) oxide). This oxidation treatment can be carried out, for example, by heating in air, using a chemical oxidizing agent, or by plasma oxidation.
[0034] Next, a coating layer 13 made of a permeable inorganic oxide is formed on the surface of the catalyst component 12. Examples of materials that make up the coating layer 13 include silicon dioxide (SiO2), titanium dioxide (TiO2), and aluminum oxide (Al2O3). Among these, silicon dioxide (SiO2), which has excellent chemical stability, permeability, and film-forming properties, is preferred.
[0035] The coating layer 13 can be formed, for example, by a dip coating method based on the sol-gel method or the colloid method.
[0036] Specifically, first, a mixed solution (i.e., a coating agent) is prepared by dispersing an appropriate amount of sol and colloid (in the case of SiO2, SiO2 sol and colloidal silica) in an organic solvent such as isopropyl alcohol. Here, the sol is a solution in which fine metal oxide particles with an average particle diameter of 1 to 10 nm are dispersed in water or an organic solvent. The colloid is a solution in which particles slightly larger than those in the sol, with an average particle diameter of 10 to 100 nm, are dispersed.
[0037] By using inorganic oxide sols and colloids in combination, their respective properties can be utilized complementaryly. In other words, inorganic oxide sols have excellent wettability and adhesion to the substrate surface, enabling the formation of dense films, but they tend to shrink significantly during drying and are prone to cracking. In contrast, the particles in colloids have a large particle size and shrink less, forming a skeletal structure within the film, contributing to stress relief due to drying shrinkage, film thickness retention, and improved mechanical strength. By mixing the two in an appropriate ratio, it is possible to induce appropriate cracking during the drying process, forming openings that allow reactants to come into contact with the catalyst component 12, while simultaneously achieving stability, permeability, and functionality for the coating layer 13 as a whole.
[0038] Next, the substrate 11 supporting the catalyst component (e.g., copper(II) oxide) 12 is immersed (dipped) in the coating agent for a certain period of time, and then pulled out while adjusting the pulling speed. As a result, a thin film of the coating agent is applied to the surface of the substrate 11.
[0039] The method of applying the coating agent is not limited to the dip coating method described above, and other known methods may be used. For example, a coating layer 13 of a predetermined thickness can be formed on the substrate surface by any of the following methods: spray coating, spin coating, brush coating, roll coating, slot die coating, electroplating, chemical vapor deposition, physical vapor deposition, thermal vapor deposition, or a combination thereof.
[0040] After dip coating, the coating is typically subjected to a heat treatment (thermosetting) at a temperature of 80 to 170°C (preferably 100 to 160°C) for 1 to 60 minutes (preferably 5 to 15 minutes) for drying, during which the solvent volatilizes and the coating agent hardens. During this heat treatment process, cracks naturally occur in the coating layer 13 due to drying shrinkage.
[0041] The coating layer 13 thus formed can be seen from the cross-sectional SEM (Scanning Electron Microscope) image to be composed of countless openings (cracks) throughout its entire surface.
[0042] In the present embodiment, the crack-like openings formed in this manner are actively utilized. That is, these openings are formed so as to penetrate the coating layer 13, and serve to allow the catalyst component present therein to come into contact with the treatment target. As a result, the coating layer 13 functions as a selectively permeable structure that physically protects the catalyst component 12, suppresses peeling, and enables contact with the reactant.
[0043] The catalyst 10 obtained in this manner has a structure in which the catalyst component 12 (for example, copper(II) oxide) is supported on the base material 11, and the surface thereof is further partially or entirely covered with the permeable coating layer 13. With this configuration, effects such as prevention of falling off of the catalyst component 12, selective reactivity, and improvement in durability can be obtained.
[0044] <Method for producing inorganic material (method for recovering inorganic material)> FIG. 2 is a flowchart showing the method for producing an inorganic material of the present disclosure (hereinafter, appropriately simply referred to as "the production method of the present disclosure").
[0045] The production method of the present disclosure is a method for producing an inorganic material by removing the components of the organic material from a composite material containing the inorganic material and the organic material. As the composite material, for example, so-called "waste plastic" obtained from wastes of home electric appliances (washing dryers, refrigerators, vacuum cleaners, water heaters, etc.), aircraft, railway vehicles, automobiles, industrial products, and the like can be used. A typical composite material is discarded fiber-reinforced plastic (FRP). Therefore, the production method of the present disclosure can also be referred to as a "composite material recycling method", an "inorganic material recycling method", or an "inorganic material recovery method". The produced inorganic material can be reused, for example, as a recycled material as part of a new composite material.
[0046] The inorganic material in the composite material to be separated (recovered) may be a virgin material or a recycled material. As the recycled material, for example, an inorganic material produced by the production method of the present disclosure can be used. Hereinafter, when simply referring to "inorganic material", the inorganic material may be either a virgin material or a recycled material unless otherwise specified.
[0047] The inorganic material contained in the composite material is composed of an inorganic substance. Examples of the inorganic substance include inorganic fibers, inorganic fillers, and metals. Examples of the inorganic fibers include glass fibers, asbestos fibers, carbon fibers, silica fibers, silica-alumina fibers, alumina fibers, zirconia fibers, potassium titanate fibers, Tyranno fibers, silicon carbide fibers, and metal fibers. These fibers may be used alone or in combination of two or more thereof. These fibers are used in forms such as continuous fibers, long fibers, short fibers, and chopped strands, and in forms such as unidirectional materials, plain weaves, and non-woven fabrics. However, the fiber shape or fiber state is not limited to these fiber shapes or fiber states. Further, the inorganic material 105 may contain a filler such as silica, titania, or zirconia, and other inorganic compounds commonly used in composite materials.
[0048] The organic material is composed of an organic substance, and the organic substance includes, for example, resins such as thermosetting resins and thermoplastic resins. Examples of the thermosetting resins include epoxy resins, phenol resins, urea resins, melamine resins, unsaturated polyester resins, silicone resins, polyimide resins, bismaleimide resins, and thermosetting urethane resins. Examples of the thermoplastic resins include polyethylene, polypropylene, polystyrene, acrylonitrile butadiene styrene, polyvinyl chloride, methacrylic resins, polyethylene terephthalate, polybutylene terephthalate, polyvinyl alcohol, polyamide, and polycarbonate. One type of the resin may be used alone, or two or more types thereof may be used at any arbitrary ratio and proportion.
[0049] The organic material preferably contains a thermosetting resin. Since the thermosetting resin is cured by heating, the organic material is difficult to melt, and it is difficult to separate the inorganic material contained together with the organic material from the organic material. However, according to the production method of the present disclosure, since the thermal decomposition temperature of the organic material can be made lower than in the conventional art, the organic material can be easily thermally decomposed, and the inorganic material can be taken out (produced) from the composite material.
[0050] The composite material may optionally contain additives such as flame retardants, antioxidants, light stabilizers, dispersants, lubricants, plasticizers, antistatic agents, pigments, and dyes, as required.
[0051] The manufacturing method disclosed herein includes an input step S1 in which a composite material is introduced into a processing apparatus (also called a reaction vessel), and a heating step S2 in which the introduced composite material is thermally decomposed.
[0052] The heating step S2 is a process of thermally decomposing the composite material by heating it under a controlled atmosphere using oxygen or an oxygen-containing gas mixture. Because heating step S2 uses oxygen, it is also called combustion or oxidative decomposition.
[0053] The heating step S2 involves heating the composite material and the catalyst 10 while bringing them into contact. The method of contact can be achieved by stirring and mixing the composite material and the catalyst 10. It is not necessary to uniformly mix the entire composite material and the catalyst 10; for example, the composite material and the catalyst 10 may coexist in the same reaction vessel.
[0054] Furthermore, as a method of contact, the catalyst 10 may be pre-installed in the reaction vessel in a fixed or piled state, and the composite material may pass, flow, or be introduced over it. With such a configuration, the catalyst 10 can also function as a fixed-bed reactor structure, and the contact method can be selected according to the scale and purpose of the reaction apparatus.
[0055] In heating step S2, the temperature at which the organic material is thermally decomposed is, for example, 450°C or lower, preferably 440°C or lower, more preferably 420°C or lower, and even more preferably 400°C or lower. Heating at these temperatures suppresses the thermal degradation of the inorganic material, which has a significant impact when the recycled inorganic material is reused.
[0056] The heating time in heating step S2 is not particularly limited, but for example, it is between 5 minutes and 5 hours.
[0057] Through thermal decomposition of organic materials, solid organic materials are transformed into exhaust gases. These exhaust gases, which may contain carbon dioxide, are released into the environment as appropriate.
[0058] On the other hand, the inorganic materials contained in the composite material remain in the reaction vessel. Therefore, the inorganic materials can be easily removed from the reaction vessel.
[0059] If the catalyst 10 is fixed in the reaction vessel, it can be used continuously. It can also be recovered and reused.
[0060] As described above, the catalyst 10 is not a fine powder or anything like that, but has a form and size that makes it easy to separate from the remaining inorganic material, so it does not become intricately mixed with the inorganic material.
[0061] In this case, if the catalyst content in the recovered inorganic material is less than 0.5 wt%, it can be considered uncontaminated.
[0062] According to the manufacturing method of this disclosure, the catalyst components contained in the catalyst 10 are prevented from being detached by the coating layer 13, and therefore do not become mixed with the inorganic material to an extent that would be considered contamination.
[0063] Next, embodiments of the present invention will be described. However, the present invention is not limited to these embodiments.
[0064] <Example 1> [Catalyst Production] To use copper(II) oxide as the active catalyst component, a copper wire with a diameter of 1 mm was prepared as the base material 11.
[0065] In addition, a coating solution with the following composition was prepared.
[0066] - 1 part by weight of SiO2 sol (Nissan Chemical ST-OXS): Average particle size of SiO2: 5 nm, SiO2:Isopropyl alcohol (IPA) = 2:8 (= 20% SiO2) (weight ratio) - 2 parts by weight of colloidal silica (Nissan Chemical IPA-ST): Particle size of SiO2: 10-15 nm, SiO2:Isopropyl alcohol (IPA) = 3:7 (= 30% SiO2) (weight ratio) - 15 parts by weight of isopropyl alcohol (IPA) The copper wire was dip-coated by immersing it in the coating solution and then pulling it out. After dip coating, the copper wire was dried in an oven at 150°C for 10 minutes to form a coating layer 13.
[0067] Upon examining the cross-section of the coating layer 13, it was found that its thickness was less than 300 nm, and countless openings with a maximum width of 80 nm were observed throughout the entire surface.
[0068] [Recovery of Inorganic Materials from Composite Materials] Composite material to be subjected to pyrolysis treatment: Dimensions: 10 mm x 10 mm x 10 mm Organic material: Bisphenol A-based epoxy resin Inorganic material: Glass fiber Organic material: Glass fiber = 60:40 (volume ratio) The catalyst 10 prepared above was wrapped around the composite material, placed in an atmosphere containing air, heated to 400°C at a heating rate of 10°C / min, and held for 2 hours. The temperature and time were determined based on prior experiments to pyrolyze the composite material and completely recover the inorganic materials.
[0069] Figure 3A shows a photograph of the composite material to be treated, wound around a copper wire coated with an SiO2 coating layer 13. Figure 3B shows a photograph of the inorganic material recovered after thermal decomposition.
[0070] The weight of the recovered inorganic material was measured. The amount of impurities (catalyst components) contained in the recovered inorganic material was found to be less than 0.5 wt%, confirming that the recovered inorganic material was not contaminated with catalysts.
[0071] <Example 2> The experiment was conducted using the same procedure as in Example 1, except that the copper wire was replaced with a copper plate, and the composite material to be treated was sandwiched between two copper plates (catalyst 10) and subjected to thermal decomposition treatment.
[0072] Figure 4 shows the composite material 101 to be processed sandwiched between catalysts (two copper plates coated with an SiO2 coating layer) 10P. The composite material 101 contains an inorganic material (glass fiber) 105 and an organic material 106.
[0073] When the weight of the recovered inorganic material was measured, it was confirmed that it was not contaminated with catalyst.
[0074] <Example 3> The experiment was carried out using the same procedure as in Example 1, except that the SiO2 particles in the coating solution were replaced with Al2O3 particles.
[0075] When the weight of the recovered inorganic material was measured, it was confirmed that it was not contaminated with catalyst.
[0076] <Example 4> The experiment was carried out using the same procedure as in Example 1, except that the SiO2 particles in the coating solution were replaced with TiO2 particles.
[0077] When the weight of the recovered inorganic material was measured, it was confirmed that it was not contaminated with catalyst.
[0078] <Comparative Example 1> The experiment was conducted using the same procedure as in Example 1, except that dip coating was not performed and no coating layer 13 was formed.
[0079] Figure 5A shows a photograph of the composite material to be treated, wound around a copper wire without the coating layer 13. Figure 5B shows a photograph of the inorganic material recovered after thermal decomposition.
[0080] The recovered inorganic materials showed black contaminants originating from the catalyst.
[0081] <Comparative Example 2> The experiment was conducted using the same procedure as in Example 1, except that the copper wire was replaced with copper powder (average particle size: 2-4 μm) and the coating layer 13 was not formed.
[0082] When the weight of the recovered inorganic material was measured, it was confirmed that it was contaminated with catalyst.
[0083] <Comparative Example 3> The experiment was conducted using the same procedure as in Comparative Example 2, except that copper powder was replaced with copper plates. The method of thermal decomposition treatment, in which the composite material to be treated is sandwiched between two copper plates (catalyst 10), is the same as in Example 2.
[0084] When the weight of the recovered inorganic material was measured, it was confirmed that it was contaminated with catalyst.
[0085] 10: Catalyst, 11: Substrate, 12: Catalyst component, 13: Coating layer, 131: Opening 10P: Catalyst, 101: Composite material, 105: Inorganic material, 106: Organic material
Claims
1. A catalyst comprising a base material, a catalyst component supported on the base material, and a coating layer covering the catalyst component, wherein the base material has a maximum width of 0.5 cm or more, and the coating layer has openings.
2. The catalyst according to claim 1, wherein the openings exist as cracks throughout the entire coating layer and have a maximum width of 10 to 200 nm.
3. The catalyst according to claim 1, wherein the catalyst component is selected from compounds consisting of copper, zinc, chromium, cobalt, magnesium, manganese, tin, iron, cerium, nickel, tungsten, aluminum, titanium, or combinations thereof.
4. A catalyst according to claim 1, wherein the content of the catalyst component is at least 0.0001 wt% of the total catalyst.
5. The catalyst according to claim 1, wherein the substrate is in the form of a plate, wire, mesh, fiber, honeycomb, or a combination thereof.
6. The catalyst according to claim 1, wherein the coating layer is selected from silicon dioxide, aluminum oxide, titanium oxide, zirconium oxide, boron, or a compound of these.
7. A method for producing a catalyst, comprising the steps of: applying a coating agent to a catalyst component supported on a substrate having a maximum width of 0.5 cm or more; and drying the coating agent to cause cracks to form a coating layer having openings.
8. A method for manufacturing an inorganic material, comprising: an input step of introducing a composite material containing an organic material and an inorganic material into a processing apparatus; and a heating step of heating the composite material together with a catalyst, wherein the catalyst comprises a substrate, a catalyst component supported on the substrate, and a coating layer covering the catalyst component, the substrate having a maximum width of 0.5 cm or more, and the coating layer having openings.
9. A method for producing an inorganic material according to claim 8, wherein the openings exist as cracks throughout the entire coating layer and have a maximum width of 10 to 200 nm.
10. A method for producing an inorganic material according to claim 8, wherein the catalyst component is selected from compounds consisting of copper, zinc, chromium, cobalt, magnesium, manganese, tin, iron, cerium, nickel, tungsten, aluminum, titanium, or combinations thereof.
11. A method for producing an inorganic material according to claim 8, wherein the content of the catalyst component is at least 0.0001 wt% relative to the total amount of the catalyst.
12. A method for producing an inorganic material according to claim 8, wherein the substrate is in the form of a plate, wire, mesh, fiber, honeycomb, or a combination thereof.
13. A method for producing an inorganic material according to claim 8, wherein the coating layer is selected from silicon dioxide, aluminum oxide, titanium oxide, zirconium oxide, boron, or a compound of these.
14. A method for producing an inorganic material according to claim 8, wherein the amount of catalyst components in the inorganic material removed after the heating step is less than 0.5 wt%.