Method for forming epitaxial film, and epitaxial wafer

By forming epitaxial films on a gallium oxide semiconductor substrate with an offset angle of 0.7° to 5.0°, the method addresses hillock issues in conventional Ga film growth, achieving higher growth rates and improved wafer quality.

WO2026239722A1PCT designated stage Publication Date: 2026-11-19NOVEL CRYSTAL TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/007381
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-02-27
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional epitaxial growth methods for Ga films on the (001) plane of a substrate using MOCVD or MOVPE result in high likelihood of linear hillocks, necessitating slow growth rates, which prolongs processing time and hampers mass production of epitaxial wafers.

Method used

Forming an epitaxial film on a substrate with a main surface inclined from the (001) plane at an offset angle of 0.7° to 5.0°, allowing for a growth rate of 1 μm/h while suppressing linear hillocks and impurity incorporation.

Benefits of technology

Enables faster epitaxial film growth with reduced hillocks and controlled impurity concentration, enhancing the production efficiency and reliability of epitaxial wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026007381_19112026_PF_FP_ABST
    Figure JP2026007381_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a method for forming an epitaxial film 12, the method including a film formation step for forming an epitaxial film 12 comprising a gallium oxide semiconductor on a main surface 11 of a substrate 10 comprising a gallium oxide semiconductor by MOCVD or MOVPE using an organic metal raw material. The main surface 11 is a surface inclined at an offset angle phi of 0.7° to 5.0° from the (001) plane in the [010] direction.
Need to check novelty before this filing date? Find Prior Art

Description

Epitaxial Film Formation Method and Epitaxial Wafer

[0001] The present invention relates to an epitaxial film formation method and an epitaxial wafer.

[0002] Conventionally, Ga with the (001) plane as the main surface 2 O 3 A technique for epitaxially growing a Ga film on a substrate by metalorganic chemical vapor deposition (MOCVD or MOVPE) is known (see Non-Patent Document 1). 2 O 3

[0003] Prakash P. Sundaram, et al., "Characterization of (001) β-Ga2O3 Schottky diodes with drift layer grown by MOCVD", Applied Physics Letters, 2023, 122, 232105.

[0004] Ga 2 O 3 When a Ga film is epitaxially grown on the (001) plane of a substrate by MOCVD or MOVPE, compared to the case of growing on other main planes of Ga such as the (010) plane or the (100) plane, linear hillocks are more likely to occur. 2 O 3 2 O 3

[0005] Therefore, in order to suppress the occurrence of linear hillocks as much as possible, it is necessary to significantly reduce the growth rate of the Ga film. In the film formation method described in Non-Patent Document 1, the growth of the Ga film by MOCVD on the (001) plane of the Ga substrate is performed at a low speed of about 0.62 μm / h. 2 O 3 2 O 3 2 O 3

[0006] As described above, since the film formation process of the Ga film requires a large amount of time, Ga with the (001) plane as the main surface 2 O 3 2 O 3 ​​​​​​​Ga using a substrate 2 O 3 Epitaxial wafers present challenges in terms of mass production.

[0007] The object of the present invention is to apply Ga to a substrate made of gallium oxide semiconductor by MOCVD or MOVPE 2 O 3 The objective is to provide a method for forming an epitaxial film by epitaxial growth, which allows for the growth of an epitaxial film made of a gallium oxide semiconductor on the (001) plane at a higher growth rate than conventional methods while suppressing the generation of linear hillocks, and to provide an epitaxial wafer manufactured using this method.

[0008] One aspect of the present invention provides, in order to achieve the above objective, a method for forming an epitaxial film and an epitaxial wafer.

[0009] [1] A method for forming an epitaxial film, comprising a film formation step of forming an epitaxial film made of a gallium oxide semiconductor on the main surface of a substrate made of a gallium oxide semiconductor by MOCVD or MOVPE using an organometallic raw material, wherein the main surface is a surface inclined from the (001) surface in the

[010] direction at an offset angle of 0.7° or more and 5.0° or less. [2] The method for forming an epitaxial film according to [1] above, wherein in the film formation step, the epitaxial film is formed at a growth rate of 1 μm / h or more. [3] The method for forming an epitaxial film according to [1] or [2] above, wherein the offset angle is 1.1° or more. [4] The method for forming an epitaxial film according to [1] or [2] above, wherein the offset angle is 2.0° or more. [5] The device comprises a substrate made of a gallium oxide semiconductor and an epitaxial film made of a gallium oxide semiconductor on the substrate, wherein the main surface of the substrate is a surface inclined from the (001) plane in the

[010] direction at an offset angle of 0.7° or more and 5.0° or less, and the density of linear hillocks present on the surface of the epitaxial film is 10 units / cm 2 The following applies, and the concentration of C contained in the epitaxial film is 1 × 10⁻⁶ 16 cm -3The epitaxial wafers are as follows: [6] The epitaxial wafer according to [5] above, wherein the offset angle is 1.1° or more. [7] The epitaxial wafer according to [5] above, wherein the offset angle is 2.0° or more.

[0010] According to the present invention, Ga is applied to a substrate made of a gallium oxide semiconductor by MOCVD or MOVPE. 2 O 3 The present invention provides a method for forming an epitaxial film by epitaxial growth, which allows for the growth of an epitaxial film made of a gallium oxide-based semiconductor on the (001) plane at a higher growth rate than conventional methods while suppressing the generation of linear hillocks, and also provides an epitaxial wafer manufactured using this method.

[0011] FIG. 1 is a vertical cross-sectional view of an epitaxial wafer according to an embodiment of the present invention. FIG. 2 is an observation image of the surface of the epitaxial film of an epitaxial wafer obtained by growing the epitaxial film for 1 hour on the main surface of a substrate having an offset angle φ of 0.1°. FIG. 3 is an observation image of the surface of the epitaxial film of an epitaxial wafer obtained by growing the epitaxial film for 1 hour on the main surface of a substrate having an offset angle φ of 0.5°. FIG. 4 is an observation image of the surface of the epitaxial film of an epitaxial wafer obtained by growing the epitaxial film for 1 hour on the main surface of a substrate having an offset angle φ of 2.0°. FIG. 5A is a graph showing the relationship between the offset angle φ of the main surface of the substrate and the growth rate of the epitaxial film, obtained from the evaluation of samples α, β, and γ. FIG. 5B is a graph showing the X-ray diffraction patterns of the epitaxial films of samples α, β, and γ. FIG. 6 is an observation image of the surface of the epitaxial film of an epitaxial wafer obtained by growing the epitaxial film for 4 hours on the main surface of a substrate having an offset angle φ of 0.5°. FIG. 7 is an observation image of the surface of the epitaxial film of an epitaxial wafer obtained by growing the epitaxial film for 4 hours on the main surface of a substrate having an offset angle φ of 2.0°. FIG. 8A is a graph showing the relationship between the offset angle φ of the main surface of the substrate and the length of linear hillocks generated on the surface of the epitaxial film in an epitaxial wafer where the thickness of the epitaxial film is approximately 4 μm or 13 μm. FIG. 8B is a graph showing the relationship between the offset angle φ of the main surface of the substrate and the density of linear hillocks generated on the surface of the epitaxial film in an epitaxial wafer where the thickness of the epitaxial film is approximately 4 μm. FIG. 9 is a graph showing the relationship between the offset angle φ of the main surface of the substrate and the critical thickness of the epitaxial film.

[0012] (Configuration of Epitaxial Wafer) FIG. 1 is a vertical cross-sectional view of an epitaxial wafer 1 according to an embodiment of the present invention. The epitaxial wafer 1 includes a substrate 10 made of a gallium oxide-based semiconductor, and an epitaxial film 12 made of a gallium oxide-based semiconductor formed on the main surface 11 of the substrate 10 by epitaxial crystal growth.

[0013] Here, the gallium oxide-based semiconductor refers to Ga 2 O 3or Ga added with one or both of Al and In 2 O 3 , ideally having a composition represented by (Ga x Al y In (1-x-y) ) 2 O 3 (0<x≤1, 0≤y<1, 0<x+y≤1). When Al is added to Ga 2 O 3 , the bandgap is widened, and when In is added, the bandgap is narrowed. Note that the crystal of the gallium oxide-based semiconductor described above typically has a β-type crystal structure. The substrate 10 and the epitaxial film 12 may contain conductivity-type impurities such as Si.

[0014] The epitaxial film 12 is formed on the main surface 11 of the substrate 10 by MOCVD or MOVPE.

[0015] The main surface 11 of the substrate 10 is an offset (001) plane, specifically a plane inclined from the (001) plane in the

[010] direction at an offset angle φ of 0.7° or more and 5.0° or less. By setting the offset angle φ within the range of 0.7° or more and 5.0° or less, the occurrence of linear hillocks (protrusion-like defects) on the surface of the epitaxial film 12 is suppressed, and the density of linear hillocks present on the surface of the epitaxial film 12 can be 10 pieces / cm 2 or less.

[0016] When the offset angle φ is in the range of 0.7° or more and 5.0° or less, even when the epitaxial film 12 is formed at a growth rate of 1 μm / h or more, the occurrence of linear hillocks on the surface of the epitaxial film 12 is suppressed, and the density of linear hillocks present on the surface of the epitaxial film 12 can be 10 pieces / cm 2 or less.

[0017] Further, it has been confirmed that when the offset angle φ is 0.7° or more and 5.0° or less, unintended incorporation of impurities into the epitaxial film 12 can be suppressed. For example, the concentration of C (carbon) contained in the epitaxial film 12 is 1×10 16 cm -3The following is true: By reducing the concentration of C in the epitaxial film 12, the conductivity of the epitaxial film 12 can be controlled with high precision.

[0018] Furthermore, linear hillocks on the surface of the epitaxial film 12 are more likely to occur as the thickness of the epitaxial film 12 increases, and the upper limit of the thickness of the epitaxial film 12 that can suppress the occurrence of linear hillocks (called the critical film thickness) changes depending on the magnitude of the offset angle φ.

[0019] To ensure a large critical film thickness, the offset angle φ is preferably 1.1° or greater, and more preferably 2.0° or greater.

[0020] Furthermore, as mentioned above, the offset angle φ is set to 5.0° or less. This is to suppress defects that occur in the epitaxial film 12 as the surface orientation of the main surface 11 of the substrate 10 approaches (010).

[0021] Furthermore, the same effect can be obtained regardless of whether the inclination direction of the main surface 11 from the (001) plane toward the

[010] direction is positive or negative. For example, in the cross-sectional view of Figure 1, the main surface 11 is inclined counterclockwise from the (001) plane with an offset angle φ, but it may also be inclined clockwise with an offset angle φ.

[0022] Since the epitaxial film 12 is formed by epitaxial growth on the substrate 10, the crystal orientations of the substrate 10 and the epitaxial film 12 are aligned. Therefore, the plane orientation of the main surface of the epitaxial film 12 is the same as the plane orientation of the main surface 11 of the substrate 10.

[0023] The effect of suppressing the generation of linear hillocks on the surface of the epitaxial film 12 by controlling the offset angle φ can be obtained regardless of how large the size of the epitaxial wafer 1 is (for example, a diameter of 2 inches or more). In other words, the diameter of the epitaxial wafer 1 may be 2 inches or more.

[0024] (Method for forming an epitaxial film) The method for forming an epitaxial film 12 according to an embodiment of the present invention will be described below.

[0025] A method for forming an epitaxial film 12 according to an embodiment of the present invention includes a film formation step of forming an epitaxial film 12 made of a gallium oxide semiconductor on the main surface 11 of a substrate 10 made of a gallium oxide semiconductor using MOCVD or MOVPE with organometallic raw materials.

[0026] The above-mentioned organometallic raw materials are Ga raw materials for the epitaxial film 12, and include, for example, trimethylgallium (TMG), triethylgallium (TEG), etc.

[0027] In the above film formation process, an epitaxial film 12 can be formed at a growth rate of 1 μm / h or more. For example, by setting the supply amount of organometallic raw material to 1 μmol / min or more and 1000 μmol / min or less, the growth rate of the epitaxial film 12 can be set to 1 μm / h or more.

[0028] Furthermore, in the above film formation process, for example, the growth temperature is 800°C or higher, 2 The supply ratio (VI / III ratio) of oxygen contained in the oxygen source gas (such as gas) and Ga, Al, and In contained in the organometallic source gas is set to 10,000 or less.

[0029] (Quality Evaluation of Epitaxial Films) The following describes the results of the quality evaluation of epitaxial films 12 deposited under several different conditions. This quality evaluation was performed by observing the presence or absence of linear hillocks on the surface of epitaxial films 12 deposited under several different conditions, as well as the length and density of the linear hillocks.

[0030] Figure 2 shows an observation image of the surface of the epitaxial film 12 of an epitaxial wafer 1 (referred to as sample α) on the main surface 11 of a substrate 10 with an offset angle φ of 0.1°, where the epitaxial film 12 was grown for 1 hour.

[0031] Figure 3 shows an observation image of the surface of the epitaxial film 12 of an epitaxial wafer 1 (referred to as sample β) on the main surface 11 of a substrate 10 with an offset angle φ of 0.5°, where the epitaxial film 12 was grown for 1 hour.

[0032] Figure 4 shows an observation image of the surface of the epitaxial film 12 of an epitaxial wafer 1 (referred to as sample γ) on the main surface 11 of a substrate 10 with an offset angle φ of 2.0°, where the epitaxial film 12 was grown for 1 hour.

[0033] The diameters of samples α, β, and γ are all 2 inches. Furthermore, in all samples α, β, and γ, the substrate 10 and epitaxial film 12 are made of β-Ga 2 O 3 It consists of the above. Furthermore, the epitaxial films 12 of samples α, β, and γ were all formed by MOCVD under the same growth conditions.

[0034] Figures 2, 3, and 4 show images of the surface of the epitaxial film 12 as observed with an optical microscope. A 1 mm scale bar is displayed in the lower right corner of Figures 2, 3, and 4.

[0035] From the observation images in Figures 2 to 4, it can be confirmed that the linear hillocks on the surface of the epitaxial film 12 decrease as the offset angle φ of the main surface 11 of the substrate 10 increases.

[0036] Furthermore, the thicknesses of the epitaxial films 12 in samples α, β, and γ were 2.8 μm, 3.5 μm, and 4.2 μm, respectively. From this, it was found that the growth rates of the epitaxial films 12 in samples α, β, and γ were approximately 2.8 μm / h, 3.5 μm / h, and 4.2 μm / h, respectively.

[0037] Figure 5A is a graph showing the relationship between the offset angle φ of the main surface 11 of the substrate 10 and the growth rate of the epitaxial film 12, obtained from the evaluation of samples α, β, and γ. Figure 5A shows that the larger the offset angle φ of the main surface 11 of the substrate 10, the faster the growth rate of the epitaxial film 12.

[0038] Furthermore, the inventors have confirmed that when forming an epitaxial film 12 by the HVPE method, there is no change in the growth rate of the epitaxial film 12 when the offset angle φ of the main surface 11 of the substrate 10 is 0.5° and when it is 2.0°. Therefore, the phenomenon that the growth rate of the epitaxial film 12 increases as the offset angle φ of the main surface 11 of the substrate 10 increases is considered to be a phenomenon unique to MOCVD and MOVPE.

[0039] Figure 5B is a graph showing the X-ray diffraction patterns of the epitaxial films 12 of samples α, β, and γ. Figure 5B shows that as the offset angle φ of the main surface 11 of the substrate 10 increases, the intensity of the (-401) peak, which is thought to be caused by linear hillocks, and the peak of miscellaneous crystals in the X-ray diffraction pattern of the epitaxial film 12 decreases.

[0040] Table 1 shows the concentrations of various impurity elements contained in the epitaxial films 12 of samples α, β, and γ, obtained by SIMS analysis. In Table 1, "Measured Value" is the measured concentration of each impurity element, and "BGL" is the background level (detection limit) of each impurity.

[0041]

[0042] Table 1 shows that in all three samples (α, β, and γ), the concentrations of almost all impurity elements are approximately equal to or below the background level. Specifically, H is 1 × 10⁻⁶. 17 cm -3 Below, C is 1 x 10 16 cm -3 Below, Si is 1 × 10 15 cm -3 Below, Mg is 6 × 10 13 cm -3 Below, Al is 1 × 10⁻⁶ 15 cm -3 Below, Fe is 3 × 10 14 cm -3 Below, Sn is 3 × 10 15 cm -3 The following applies:

[0043] ​Figure 6 shows an observation image of the surface of the epitaxial film 12 of an epitaxial wafer 1 (referred to as sample δ) on the main surface 11 of a substrate 10 with an offset angle φ of 0.5°, where the epitaxial film 12 was grown for 4 hours.

[0044] Figure 7 shows an observation image of the surface of the epitaxial film 12 of an epitaxial wafer 1 (referred to as sample ε) on the main surface 11 of a substrate 10 with an offset angle φ of 2.0°, where the epitaxial film 12 was grown for 4 hours.

[0045] The diameters of samples δ and ε are both 2 inches. Furthermore, in both samples δ and ε, the substrate 10 and epitaxial film 12 are made of β-Ga 2 O 3 It consists of the above. Furthermore, the epitaxial films 12 of samples δ and ε were both formed by MOCVD under the same growth conditions.

[0046] Figures 6 and 7 show images of the surface of the epitaxial film 12 as observed with an optical microscope. A 1 mm scale bar is shown in the lower right corner of Figures 6 and 7.

[0047] Comparing Figure 3 and Figure 6, it can be seen that when the offset angle φ of the main surface 11 of the substrate 10 is 0.5°, the number and size of linear hillocks increase as the growth time increases from 1 hour to 4 hours. On the other hand, comparing Figure 4 and Figure 7, when the offset angle φ of the main surface 11 of the substrate 10 is 2.0°, the number of linear hillocks does not increase even when the growth time increases from 1 hour to 4 hours (both are zero). This is because as the offset angle φ increases, the upper limit of the thickness of the epitaxial film 12 that can suppress the generation of linear hillocks (critical film thickness) increases.

[0048] Figure 8A is a graph showing the relationship between the offset angle φ of the main surface 11 of the substrate 10 and the length of the linear hillock formed on the surface of the epitaxial film 12 in an epitaxial wafer 1 where the thickness of the epitaxial film 12 is approximately 4 μm or 13 μm. Note that the straight line passing through the data plot points when the thickness of the epitaxial film 12 is approximately 13 μm is drawn with the same slope as the straight line passing through the data plot points when the thickness of the epitaxial film 12 is approximately 4 μm.

[0049] Figure 8B is a graph showing the relationship between the offset angle φ of the main surface 11 of the substrate 10 and the density of linear hillocks formed on the surface of the epitaxial film 12 in an epitaxial wafer 1 where the thickness of the epitaxial film 12 is approximately 4 μm.

[0050] From the values ​​at the intersection of the line passing through the plotted data points and the horizontal axis in Figure 8A (0.626, 0) when the thickness of the epitaxial film 12 is approximately 4 μm, and from the values ​​at the intersection of the line passing through the plotted data points and the horizontal axis in Figure 8B (0.674, 0) when the thickness of the epitaxial film 12 is approximately 4 μm, it can be seen that when the thickness of the epitaxial film 12 is approximately 4 μm, the generation of linear hillocks on the surface of the epitaxial film 12 can be suppressed if the offset angle φ is approximately 0.7° or greater.

[0051] In other words, when the offset angle φ is 0.7°, the upper limit of the thickness of the epitaxial film 12 at which the generation of linear hillocks is suppressed (critical film thickness) is approximately 4 μm.

[0052] Furthermore, from the value (1.01, 0) at the intersection of the line passing through the plotted data point and the horizontal axis when the thickness of the epitaxial film 12 is approximately 13 μm in Figure 8A, it can be seen that when the thickness of the epitaxial film 12 is approximately 13 μm, the generation of linear hillocks on the surface of the epitaxial film 12 can be suppressed if the offset angle φ is approximately 1.1° or greater.

[0053] In other words, when the offset angle φ is 1.1°, the critical thickness of the epitaxial film 12 is approximately 13 μm.

[0054] Furthermore, as can be seen from Figures 8A and 8B, when the offset angle φ is 2.0° or greater, the generation of linear hillocks on the surface of the epitaxial film 12 is reliably suppressed. From the relationship between the offset angle φ and the critical film thickness of the epitaxial film 12 when the film thickness of the epitaxial film 12 is approximately 4 μm and 13 μm, it can be inferred that when the offset angle φ is 2.0°, the critical film thickness of the epitaxial film 12 is approximately 36.6 μm.

[0055] Figure 9 is a graph showing the relationship between the offset angle φ of the main surface 11 of the substrate 10 and the critical film thickness of the epitaxial film 12. Figure 9 shows that as the offset angle φ of the main surface 11 of the substrate 10 increases, the critical film thickness of the epitaxial film 12 increases. For example, when the offset angle φ is 3.0°, the critical film thickness is approximately 60 μm, when the offset angle φ is 4.0°, the critical film thickness is approximately 80 μm, and when the offset angle φ is 5.0°, the critical film thickness is approximately 100 μm.

[0056] (Effects of the Embodiment) According to the embodiment of the present invention, by controlling the offset angle φ of the main surface 11 of the substrate 10 made of a gallium oxide semiconductor from the (001) plane, an epitaxial film 12 made of a gallium oxide semiconductor can be formed by MOCVD or MOVPE at a growth rate of 1 μm / h or more while suppressing the generation of linear hillocks.

[0057] The linear hillocks on the surface of the epitaxial film 12 cause leakage in semiconductor devices manufactured using the epitaxial wafer 1. Therefore, according to the embodiment of the present invention, leakage in semiconductor devices manufactured using the epitaxial wafer 1 can be reduced and reliability can be improved.

[0058] Although embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and various modifications can be made without departing from the spirit of the invention. Furthermore, the components of the above embodiments can be arbitrarily combined without departing from the spirit of the invention.

[0059] Furthermore, the embodiments described above do not limit the invention as claimed. It should also be noted that not all combinations of features described in the embodiments are necessarily essential for solving the problem of the invention.

[0060] Ga is processed on a substrate made of gallium oxide semiconductor by MOCVD or MOVPE. 2 O 3The present invention provides a method for forming an epitaxial film by epitaxial growth, which allows for the growth of an epitaxial film made of a gallium oxide semiconductor on the (001) plane at a higher growth rate than conventional methods while suppressing the generation of linear hillocks, and an epitaxial wafer manufactured using this method.

[0061] 1...Epitaxial wafer, 10...Substrate, 11...Main surface, 12...Epitaxial film

Claims

1. A method for forming an epitaxial film, comprising a film formation step of forming an epitaxial film made of a gallium oxide semiconductor on the main surface of a substrate made of a gallium oxide semiconductor by MOCVD or MOVPE using organometallic raw materials, wherein the main surface is a surface inclined from the (001) surface in the [010] direction at an offset angle of 0.7° or more and 5.0° or less.

2. The method for forming an epitaxial film according to claim 1, wherein the epitaxial film is formed at a growth rate of 1 μm / h or more in the film formation step.

3. The method for forming an epitaxial film according to claim 1 or 2, wherein the offset angle is 1.1° or more.

4. The method for forming an epitaxial film according to claim 1 or 2, wherein the offset angle is 2.0° or more.

5. The apparatus comprises a substrate made of a gallium oxide semiconductor and an epitaxial film made of a gallium oxide semiconductor on the substrate, wherein the main surface of the substrate is inclined from the (001) plane in the [010] direction at an offset angle of 0.7° or more and 5.0° or less, and the density of linear hillocks present on the surface of the epitaxial film is 10 units / cm³. 2 The following applies, and the concentration of C contained in the epitaxial film is 1 × 10⁻⁶ 16 cm -3 The following is an epitaxial wafer.

6. The epitaxial wafer according to claim 5, wherein the offset angle is 1.1° or more.