Thermal expansion sheet, method for producing said sheet, and article provided with said sheet

A thermally expandable sheet with differential Gurley flexibility in two directions addresses insertability and shape retention issues by controlling filler orientation and resin composition, ensuring high insertability and durability during bending and adhesive bonding.

WO2026239740A1PCT designated stage Publication Date: 2026-11-19NIKKAN IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/009846
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-03-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing thermally expandable sheets face challenges in insertability due to increased stiffness when fillers are incorporated into the adhesive layer, leading to difficulty in bending and shape retention, which can result in tearing or degradation during insertion between adherends.

Method used

The thermally expandable sheet is designed with differing Gurley flexibility in two directions, where the first direction has higher flexibility for easy insertion and the second direction has lower flexibility for better shape retention, achieved by controlling the orientation and content of fillers and resins, ensuring a coefficient of dynamic friction below 0.6 and incorporating a base material with controlled thickness.

Benefits of technology

This design allows for high insertability and shape retention, preventing tearing and enhancing workability by maintaining stiffness in the insertion direction while facilitating bending, with improved adhesive strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026009846_19112026_PF_FP_ABST
    Figure JP2026009846_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a thermal expansion sheet which is used for the purpose of bonding a plurality of adherends to each other, wherein Gurley stiffness in a first direction and a second direction, which are two different directions along the surface direction of the sheet, are different from each other. In addition, the present invention relates to a method for producing the sheet, and an article provided with the sheet. The present invention can provide a thermal expansion sheet which is capable of exhibiting sufficiently high insertability even when the thermal expansion sheet is bent and inserted into a gap that is formed by a plurality of adherends.
Need to check novelty before this filing date? Find Prior Art

Description

Thermal expansion sheet, method for manufacturing the sheet, and article equipped with the sheet.

[0001] The present invention relates to a thermally expandable sheet, a method for manufacturing the sheet, and an article comprising the sheet. Cross-reference of related applications: This application claims priority to Japanese Patent Application No. 2025-080748, filed on 13 May 2025, the entire description of which is incorporated herein by reference.

[0002] In a thermal expansion sheet that is placed between multiple adherends and whose adhesive layer on its surface expands upon heating to bond the adherends together, there is a need to further improve the insertability when inserting the thermal expansion sheet into the gaps formed by the adherends. Therefore, in order to improve the insertability of the thermal expansion sheet, it has been considered to strengthen the rigidity of the thermal expansion sheet by incorporating a filler into the adhesive layer, as shown in Patent Documents 1 and 2, for example. Here, "rigidity" refers to the property of the thermal expansion sheet not easily bending or wrinkling due to friction with the surface of the adherends when inserting it into the gaps between adherends, for example, and is equivalent to stiffness.

[0003] Patent Document 1: International Publication No. 2023 / 176958 Patent Document 2: Japanese Patent No. 7064636 The entire contents of Patent Documents 1 and 2 are incorporated herein by reference.

[0004] However, as a result of extensive studies conducted by the present inventors to provide a thermally expandable sheet with good workability, simply incorporating a filler into the adhesive layer of the thermally expandable sheet as described in the aforementioned Patent Documents 1 and 2 increases the stiffness of the thermally expandable sheet in all directions along the in-plane direction of the sheet. Therefore, when the thermally expandable sheet is inserted into a gap formed by a plurality of adherends in a state of being bent into a U-shape to conform to the shape of the gap, for example, the thermally expandable sheet may be difficult to bend, or the shape retention after bending may be insufficient, which has been found to possibly rather reduce the insertability. In addition, when the stiffness of the thermally expandable sheet is high, bending can be performed by applying higher pressure, but this bending process may scrape or tear the thermally expandable sheet, leading to a risk of property degradation. The in-plane direction refers to the direction along the surface of the thermally expandable sheet that is in contact with the adherend, and indicates the direction perpendicular to the thickness direction of the thermally expandable sheet.

[0005] The present invention has been made in view of the aforementioned problems, and a main object of the present invention is to provide a thermally expandable sheet that can exhibit sufficiently high insertability even when the thermally expandable sheet is bent and inserted into a gap formed by a plurality of adherends.

[0006] In one aspect, the thermal expansion sheet according to the present invention is as follows: [1] A thermal expansion sheet that is placed between a plurality of adherends and adheres these plurality of adherends to each other by thermal expansion, characterized in that, before thermal expansion, the degree of Gurley flexibility in two different directions, a first direction and a second direction, along the surface direction of the thermal expansion sheet, is different from that of the thermal expansion sheet. [2] The thermal expansion sheet according to [1], characterized in that the first direction is the MD direction, which is the longitudinal direction, and the second direction is the TD direction, which is perpendicular to the first direction, and, before thermal expansion, the degree of Gurley flexibility in the first direction is greater than that in the second direction. [3] The thermal expansion sheet according to [1] or [2], which contains at least flake-like, plate-like, needle-like, fibrous or branch-like fillers, characterized in that, before thermal expansion, the average value of the degree of orientation, which is the angle between the longitudinal axis direction of the fillers and the first direction, when observed by SEM from the thickness direction of the thermal expansion sheet, is 40° or less. [4] The thermal expansion sheet according to [3], characterized in that, in the thermal expansion sheet before heating and expansion, the proportion of fillers having an orientation degree of less than 45° is 55% or more. [5] The thermal expansion sheet according to [3] or [4], wherein the filler contains a filler having an aspect ratio of 1.5 or more and 80 or less. [6] The thermal expansion sheet according to any one of [3] to [5], comprising a base material and an adhesive layer on at least one side of the base material, wherein the adhesive layer contains at least the filler, epoxy resin, curing agent, foaming agent, and elastomer. [7] The thermal expansion sheet according to [6], wherein the content of the filler is 5% by mass or more and less than 80% by mass with respect to 100% by mass of the adhesive layer. [8] The thermal expansion sheet according to [6] or [7], wherein the epoxy resin contains an epoxy resin having a softening point of 60°C or higher. [9] The thermal expansion sheet according to any one of [6] to [8], wherein the epoxy resin contains an epoxy resin with an epoxy equivalent of less than 300.

[10] The thermal expansion sheet according to any one of [6] to [9], wherein the adhesive layer contains two or more epoxy resins, and at least one of the epoxy resins has a molecular weight of 10,000 or more.

[11] The thermal expansion sheet according to any one of [6] to

[10] , wherein the elastomer contains an elastomer having a glass transition temperature (Tg) of 100°C or higher.

[12] The thermal expansion sheet according to any one of [6] to

[11] , wherein the elastomer contains an elastomer having a molecular weight of 100,000 or more.

[13] The thermal expansion sheet according to any one of [1] to

[12] , characterized in that, in the thermal expansion sheet before heating and expansion, if the Gurley flexibility in the first direction is greater than the Gurley flexibility in the second direction, the shape retention in the second direction of the thermal expansion sheet before heating and expansion is higher than the shape retention in the first direction.

[14] The thermal expansion sheet according to any one of [1] to

[13] , wherein the coefficient of dynamic friction of the surface before heating and expansion is 0.6 or less.

[15] A thermally expandable sheet according to any one of [1] to

[14] , wherein the shear adhesive strength after heating and curing is 0.8 MPa or more at 23°C and 0.1 MPa or more when heated at 200°C.

[16] A thermally expandable sheet according to any one of [1] to

[15] , wherein the shear adhesive strength after heating and curing and further treatment in a 200°C environment for 500 hours is 0.1 MPa or more when heated at 200°C.

[17] A thermally expandable sheet according to any one of [1] to

[16] , wherein the shear adhesive strength after heating and curing and further treatment in an 85°C and 85% RH environment for 1000 hours is 0.1 MPa or more when heated at 200°C.

[18] A method for producing a thermally expandable sheet, comprising the step of applying a resin composition containing an epoxy resin, a curing agent, a foaming agent, a filler, an elastomer, and a solvent onto a substrate, characterized in that the resin composition is applied to the substrate while applying shear stress in one direction.

[19] The method for producing a thermally expandable sheet according to

[18] , characterized in that the resin composition contains 20% by mass or more and 80% by mass or less of the solvent based on 100% by mass of the resin composition.

[20] An article comprising a thermally expandable sheet according to any one of [1] to

[17] .

[0007] In other respects, the thermal expansion sheet according to the present invention is as follows: [1] A thermal expansion sheet that is placed between a plurality of adherends and adheres these adherends to each other by thermal expansion, wherein the thermal expansion sheet has a base material with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the base material, the adhesive layer contains a filler, an epoxy resin, and a curing agent, and the ratio of the Gurley flexibility of the thermal expansion sheet in the MD direction to the Gurley flexibility of the thermal expansion sheet in the TD direction (MD direction / TD direction) is 1.1 or more. [2] A thermal expansion sheet that is placed between multiple adherends and bonds these adherends to each other by thermal expansion, wherein the thermal expansion sheet has a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin and a curing agent, the filler includes flake-like, plate-like, needle-like, fibrous or branch-like fillers, and the average degree of orientation of the filler in the thermal expansion sheet before thermal expansion is 40° or less, where the degree of orientation of the filler is the angle between the long axis direction of the filler and the MD direction of the thermal expansion sheet when observed by SEM from the thickness direction of the thermal expansion sheet before thermal expansion. [3] A thermal expansion sheet that is placed between multiple adherends and adheres these adherends to each other by thermal expansion, wherein the thermal expansion sheet has a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin and a curing agent, the filler includes flake-like, plate-like, needle-like, fibrous or branch-like fillers, and the proportion of fillers with an orientation of less than 45° in the thermal expansion sheet before thermal expansion is 55% or more of the total filler: Here, the orientation of the filler is the angle between the long axis direction of the filler and the MD direction of the thermal expansion sheet when observed by SEM from the thickness direction of the thermal expansion sheet before thermal expansion.[4] A thermal expansion sheet that is placed between a plurality of adherends and bonds the plurality of adherends to each other by thermal expansion, wherein the thermal expansion sheet has a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin, a curing agent, and an elastomer, the elastomer contains an elastomer having a glass transition temperature (Tg) of 100°C or higher, and the thermal expansion sheet, before thermal expansion, has a Gurley flexibility in the MD direction greater than the Gurley flexibility in the TD direction. [5] The thermal expansion sheet according to any one of [1] to [4], wherein the adhesive layer is formed by coating a resin composition containing components constituting the adhesive layer and a solvent onto a substrate at a coating speed of 50 to 200 (mm / sec) and removing the solvent. [6] The thermal expansion sheet according to any one of [1] to [5], wherein the adhesive layer is formed using a resin composition containing components constituting the adhesive layer and a solvent, and having a solid content concentration of 25 to 75%. [7] The thermal expansion sheet according to any one of [1] to [6], wherein the Gurley flexibility in the MD direction of the thermal expansion sheet is 53.5 mgf or more. [8] The thermal expansion sheet according to any one of [1] to [7], wherein the base material is a metal film, a resin film, or a nonwoven fabric. [9] The thermal expansion sheet according to any one of [1] to [8], wherein the filler contains a filler with an aspect ratio of 1.5 or more and 80 or less.

[10] The thermal expansion sheet according to any one of [1] to [9], wherein the filler content is 5% by mass or more and less than 80% by mass with respect to 100% by mass of the adhesive layer.

[11] The thermal expansion sheet according to any one of [1] to

[10] , wherein the epoxy resin contains an epoxy resin with a softening point of 60°C or higher.

[12] A thermal expansion sheet according to any one of [1] to

[11] , wherein the epoxy resin contains an epoxy resin with an epoxy equivalent of less than 300.

[13] A thermal expansion sheet according to any one of [1] to

[12] , wherein the adhesive layer contains two or more epoxy resins, and at least one of the epoxy resins has a molecular weight of 10,000 or more.

[14] The thermal expansion sheet according to [4], wherein the elastomer contains an elastomer with a molecular weight of 100,000 or more.

[15] The thermal expansion sheet according to any one of [1] to

[14] , wherein the shape retention in the TD direction is higher than the shape retention in the MD direction in the thermal expansion sheet before heating and expansion.

[16] The thermal expansion sheet according to any one of [1] to

[15] , wherein the coefficient of dynamic friction of the surface before heating and expansion is 0.6 or less.

[17] The thermal expansion sheet according to any one of [1] to

[16] , wherein the shear adhesive strength after heating and expansion and curing is 0.8 MPa or more at 23°C and 0.1 MPa or more when heated to 200°C.

[18] An article comprising the thermal expansion sheet according to any one of [1] to

[17] .

[19] The article according to

[18] , wherein the article is a motor.

[0008] The present invention is groundbreaking, based on an unprecedented approach of making the Gurley flexibility of the thermal expansion sheet different in the first and second directions. According to the present invention, for example, in the first direction, the Gurley flexibility is high (i.e., it is stiff), allowing for high insertability, while in the second direction, the Gurley flexibility is low, making it easier to bend. Thus, it is possible to provide a thermal expansion sheet that can achieve both stiffness in the insertion direction and shape retention in the bending direction.

[0009] Figure 1 is a schematic cross-sectional view showing the configuration of a thermal expansion sheet 1 according to one embodiment of the present invention. Figure 2 is a schematic cross-sectional view showing the configuration of a thermal expansion sheet 1 according to another embodiment of the present invention. Figure 3 is a graph showing the measurement results of shear stress when forming the adhesive layer of a thermal expansion sheet according to an embodiment of the present invention. Figure 4 is an explanatory diagram of the evaluation method for a thermal expansion sheet according to an embodiment of the present invention.

[0010] The basic configuration of the thermal expansion sheet 1 according to one embodiment of the present invention will be described below. <Basic configuration of the thermal expansion sheet> Figure 1 is a schematic cross-sectional view showing the configuration of the thermal expansion sheet 1 according to this embodiment.

[0011] The thermal expansion sheet 1 according to this embodiment is a thermal expansion sheet that is placed between multiple adherends and expands when heated at a high temperature, for example, 120°C to 250°C, to bond these adherends together. Before heating and expansion, its thickness is 10 μm or more and 1000 μm or less.

[0012] The thermal expansion sheet 1 according to this embodiment comprises, for example, a base material 10, an adhesive layer 20 formed on both sides of the base material 10, and a primer layer 30 provided between the base material 10 and the adhesive layer 20, as shown in Figure 1. The adhesive layer 20 and the primer layer 30 may be formed on only one side of the base material 10.

[0013] <<Base Material>> The base material 10 functions as a support material that supports the adhesive layer 20.

[0014] Specifically, the base material 10 is preferably in the form of a sheet, and may have a single-layer structure or a laminated structure. Furthermore, the base material 10 may or may not have a porous structure inside.

[0015] The thickness of the base material 10 is preferably, for example, 1 μm to 200 μm, more preferably 10 μm to 150 μm, and particularly preferably 25 μm to 100 μm. For example, when the thermal expansion sheet 1 according to this embodiment is used by inserting it into a motor slot, giving the base material 10 a certain thickness can prevent the thermal expansion sheet 1 from buckling when inserted into the motor slot. Also, by not making the thickness of the base material 10 too large, the sheet can be made easier to fold. For these reasons, it is preferable to set the thickness of the base material 10 within the range described above.

[0016] The material of the base material 10 is not particularly limited and may be an organic material, an inorganic material, a resin film, or a nonwoven fabric. For example, a metal film can be used when electrical conductivity is required for the thermal expansion sheet 1, and a resin film can be used when electrical insulation is required for the thermal expansion sheet 1.

[0017] The metal film is not particularly limited, but for example, copper foil and aluminum foil can be used. The thickness of the metal film is, for example, 1 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 15 μm to 50 μm. When a metal film is used as the material of the base material 10, the thermal conductivity of the thermal expansion sheet 1 can also be increased compared to when an organic material is used.

[0018] Examples of resins included in the resin film include polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate (PEN), and aromatic polyesters; polycarbonate; polyarylate; polyurethane; polyamide resins such as polyamide and polyetheramide; polyimide resins such as polyimide, polyetherimide, and polyamideimide; polysulfone resins such as polysulfone and polyethersulfone; polyetherketone resins such as polyetherketone and polyetheretherketone; polyphenylene sulfide (PPS); and modified polyphenylene oxide. The glass transition temperature of the resin in the resin film is preferably 80°C or higher, but may also be 140°C or higher, or 200°C or higher. Liquid crystal polymer (LCP) may also be used as the resin.

[0019] Examples of nonwoven fabrics include nonwoven fabrics containing fibers such as cellulose fibers, polyester fibers, nylon fibers, aramid fibers, polyphenylene sulfide fibers, liquid crystal polymer fibers, glass fibers, metal fibers, and carbon fibers, as well as mica paper.

[0020] In this embodiment, the base material 10 is preferably electrically insulating, and preferably contains polyimide (PI), polyethylene naphthalate (PEN), or polyphenylene sulfide (PPS). Polyimide, polyethylene naphthalate, and polyphenylene sulfide have high heat resistance and are suitable for cases where the thermal expansion sheet 1 is thermally expanded and cured by heating, or for use of the thermal expansion sheet 1 at high temperatures. Furthermore, polyimide, polyethylene naphthalate, and polyphenylene sulfide have high insulating properties, and are preferred because, for example, the thermal expansion sheet 1 after heat curing can insulate adherends from each other.

[0021] The base material 10 may be a single-layer base material, or it may be a base material consisting of a laminate having a laminated structure in which members are bonded together with a bonding adhesive. In applications where the thermal conductivity of the thermal expansion sheet is required, the base material 10 is preferably a base material consisting of a laminate having a laminated structure in which members are bonded together with a bonding adhesive. By using a bonding adhesive with high thermal conductivity, the thermal conductivity of the base material 10 can be increased. The base material 10 may also contain a filler. By containing a filler in the base material 10, the thermal conductivity and electrical insulation of the thermal expansion sheet 1 can be improved. The type of filler is not particularly limited, and it may be the same type as the filler contained in the adhesive layer and primer layer described later, or it may be a different type.

[0022] <<Adhesive Layer>> The adhesive layer 20 is a layer that expands upon heating and exhibits adhesive strength. In this embodiment, it is formed on both sides of the base material 10 to form the outermost surface of the thermal expansion sheet 1. Since the stiffness of the outermost layer has a significant impact on the overall stiffness of the thermal expansion sheet 1, it is preferable that the adhesive layer 20 be on the outermost layer of the thermal expansion sheet 1.

[0023] The adhesive layer 20 may be a continuous layer formed in a continuous manner, or it may be a discontinuous layer consisting of multiple islands. Examples of discontinuous layers include patterns such as stripes and dots. Furthermore, the surface of the continuously formed adhesive layer 20 may have an uneven shape such as an embossed surface.

[0024] The surface of the adhesive layer 20 may have sufficient adhesiveness to temporarily fix it to the adherend, but when the heat-expandable sheet 1 is inserted into a narrow gap for use, it is preferable that the adhesive layer 20 is non-adhesive (tack-free) before heating and expanding.

[0025] In the thermal expansion sheet 1 according to this embodiment, the coefficient of dynamic friction of the outer surface of the adhesive layer 20 before heating and expanding (i.e., the outermost surface of the thermal expansion sheet 1) is preferably 0.60 or less, more preferably 0.55 or less, and even more preferably 0.50 or less. By making the thermal expansion sheet 1 such that the coefficient of dynamic friction of the outer surface of the adhesive layer 20 before heating and expanding is 0.60 or less, the slipperiness and insertability can be further improved, making it easier to insert into narrow gaps and resulting in a more user-friendly thermal expansion sheet 1. For example, when the thermal expansion sheet 1 is placed between two adherends to bond them together, the thermal expansion sheet 1 can be smoothly inserted into the gap between the adherends, or the other adherend can be smoothly inserted into the gap after the thermal expansion sheet 1 has been placed on one adherend. A specific application is, for example, when manufacturing a motor by bonding a stator core and coils together. As mentioned above, if the thermal expansion sheet has a dynamic friction coefficient of 0.60 or less on the outer surface of the adhesive layer 20, it can be inserted smoothly into the gap of the stator core, and the coil can be inserted more smoothly into the gap that has become narrower after the thermal expansion sheet is inserted. Furthermore, it is preferable that the dynamic friction coefficient of the outer surface of the adhesive layer 20 before heating and expanding is, for example, 0.15 or more. By using a thermal expansion sheet 1 with a dynamic friction coefficient of 0.15 or more on the outer surface, it becomes less likely to fall off between being placed on the surface of the adherend or in the gap formed by multiple adherends and being heated and expanded, resulting in a thermal expansion sheet 1 with high workability. Similarly, even when the coil is inserted into a narrow gap first and the thermal expansion sheet is inserted afterward, it is preferable that the dynamic friction coefficient is within the above range. The coefficient of dynamic friction of the outer surface of the adhesive layer 20 can be measured by rubbing, in accordance with JIS K 7125, using a SUS304 plate whose contact surface with the thermal expansion sheet 1 (before heating and expansion) has been smoothed by #800 buff polishing, with a measurement speed of 100 mm / min and a travel distance of 130 mm.

[0026] In the case where adhesive layers 20 are arranged on both sides of the base material 10, as in the thermal expansion sheet 1 according to this embodiment, it is sufficient that the coefficient of dynamic friction of the outer surface of at least one of the two adhesive layers 20 is within the above range. In particular, it is preferable that the coefficient of dynamic friction of the outer surfaces of both adhesive layers 20 is within the above range.

[0027] The coefficient of dynamic friction of the outer surface of the thermal expansion sheet 1 can be adjusted by, for example, reducing the contact area with the adherend by creating irregularities on the surface of the outermost layer. Furthermore, since using a resin with a high modulus of elasticity in the outermost layer tends to decrease the coefficient of dynamic friction, it can also be adjusted by the resin composition of the outermost layer.

[0028] The thickness of the adhesive layer 20 in this embodiment is not particularly limited, but is, for example, 10 μm or more, and may be 20 μm or more. A thickness of 10 μm or more of the adhesive layer 20 is preferable because sufficient adhesive strength can be obtained. On the other hand, the thickness of the adhesive layer 20 is preferably, for example, 200 μm or less. The total thickness of the adhesive layer 20 in the thermal expansion sheet 1 is preferably 0.2 times or more and 8 times or less the thickness of the base material 10, and more preferably 0.4 times or more and 5 times or less. By setting it within this range, as described later, for example, when a filler is included in the adhesive layer 20 and the orientation of the filler is controlled, the influence on the overall stiffness of the thermal expansion sheet 1 can be sufficiently large. The total thickness of the adhesive layer 20 referred to here refers to the total thickness of the adhesive layer contained in one thermal expansion sheet 1. Specifically, when the adhesive layer 10 is arranged on one side of the base material 10, it refers to the thickness of that adhesive layer 20 itself, and when the adhesive layer 20 is arranged on both sides of the base material 10, it refers to the total thickness of the two adhesive layers 20 formed on both sides.

[0029] Specific examples of the adhesive layer 20 according to this embodiment include, for example, one that contains at least an epoxy resin, a curing agent, and a foaming agent, and further includes a filler, an elastomer, a curing accelerator, and other additives as needed.

[0030] <<<Epoxy Resin>>> The adhesive layer 20 according to this embodiment contains, for example, an epoxy resin, which is a thermosetting resin. The epoxy resin is not particularly limited as long as it contains epoxy groups, but for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, hindertoin type epoxy resin, biphenyl type epoxy resin, alicyclic epoxy resin, triphenylmethane type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, naphthol novolac type epoxy resin, dicyclopentadiene / phenol epoxy resin, alicyclic amine epoxy resin, aliphatic amine epoxy resin and epoxy resins modified in various ways therebetween, copolymers of glycidyl methacrylate and other polymerizable unsaturated compounds, epoxy-modified polybutadiene, epoxy-modified silicone, etc. may be used individually or in combination of multiple types. In addition, thermosetting resins other than epoxy resins, such as phenolic resins, may also be used in the adhesive layer 20.

[0031] The epoxy resin content in the adhesive layer 20 is, for example, 1% by mass or more, may be 10% by mass or more, or 25% by mass or more, based on the total mass of the adhesive layer 20. By setting the epoxy resin content to 1% by mass or more, a thermal expansion sheet 1 with excellent adhesive strength and blocking resistance can be obtained. On the other hand, the epoxy resin content is, for example, 90% by mass or less, may be 80% by mass or less, or 70% by mass or less, based on the total mass of the adhesive layer 20. By setting the epoxy resin content to 90% by mass or less, a thermal expansion sheet 1 with a combination of blocking resistance, adhesive strength, and crack resistance can be obtained.

[0032] Furthermore, the epoxy resin may have a melt viscosity at 150°C of, for example, 0.005 Pa·s or more, but may also be 0.03 Pa·s or more, or 0.1 Pa·s or more. By setting the melt viscosity of the epoxy resin to 0.005 Pa·s or more, good foaming properties can be obtained when the thermal expansion sheet 1 is heated and expanded, as well as the tackiness of the adhesive layer 20 can be suppressed, and when the adhesive layer 20 is provided as the outermost layer of the thermal expansion sheet 1 as in this embodiment, the insertability into the gap formed by the adherend can be improved. On the other hand, the melt viscosity at 150°C may be, for example, 10 Pa·s or less, but may also be 5 Pa·s or less, or 2 Pa·s or less. By setting the melt viscosity of the epoxy resin to 10 Pa·s or less, the fluidity of the adhesive layer 20 is increased during heating and expansion, resulting in a thermal expansion sheet 1 with good foaming properties. The melt viscosity can be determined, for example, by measuring it using an ARES-G2 instrument manufactured by T.A. Instruments under the following conditions: heating rate of 50°C / min, temperature range of 23°C to 220°C (held for 10 minutes after reaching 220°C), deformation mode "shear", and frequency of 1 Hz.

[0033] The softening point of the epoxy resin is preferably 60°C or higher, more preferably 70°C or higher, and even more preferably 80°C or higher. By using an epoxy resin with a softening point of 60°C or higher, tack is less likely to occur in the thermal expansion sheet 1. By suppressing tack in the thermal expansion sheet 1, it is possible to prevent the surfaces of the adhesive layer 20 from sticking together when the product is rolled up for storage or transport, and to prevent it from sticking to the wall surface when inserting it into a gap formed by the adherend, making insertion difficult. Furthermore, considering summer and tropical regions, it is preferable that tack does not occur even at 50°C. On the other hand, the softening point of the epoxy resin is preferably 150°C or lower, more preferably 130°C or lower, and even more preferably 110°C or lower. By setting the softening point of the epoxy resin lower than the thermal expansion start temperature of the foaming agent, the foaming agent can be expanded while the epoxy resin is highly flexible, so the adhesive layer 20 can be expanded uniformly. In addition, by lowering the softening point, the fluidity during heating is improved, so the reactivity is increased and it becomes easier to obtain good adhesive strength. The softening point of epoxy resin can be measured using the ring-ball softening point test method specified in JIS K 2207.

[0034] Furthermore, it is desirable that the epoxy resin has a minimum viscosity temperature within the temperature range from the thermal expansion initiation temperature of the foaming agent contained in the adhesive layer 20 to the curing activity temperature in the curing behavior of the epoxy resin, where the viscosity is at its lowest. Using such an epoxy resin is preferable because, when the adhesive layer 20 is heated, the foaming agent can be sufficiently expanded before the resin can be cured, thereby optimizing the expansion rate and adhesive strength of the entire thermal expansion sheet 1. The curing activity temperature in the curing behavior of the epoxy resin can be determined, for example, by looking at the relationship between the temperature measured by a differential scanning calorimetry (DSC) device and the exothermic energy of the curing reaction, and identifying the temperature at which an exothermic peak is observed. The minimum viscosity temperature at which the viscosity of the epoxy resin is at its lowest can be determined, for example, by looking at the relationship between the temperature measured by a viscoelasticity measuring device and the melt viscosity (complex viscosity) of the resin sample, and identifying the temperature at which an off-peak is observed on the complex viscosity curve.

[0035] The epoxy equivalent of the epoxy resin is preferably 5000 g / eq or less, more preferably 1000 g / eq or less, and particularly preferably 300 g / eq or less. Reducing the epoxy equivalent increases the crosslinking density between the epoxy resin and the curing agent, which tends to increase the adhesive strength. When using an epoxy resin with a high softening point to reduce tack, it is preferable to use an epoxy resin with a low epoxy equivalent to further increase the adhesive strength. On the other hand, the epoxy equivalent is, for example, 10 g / eq or more, may be 50 g / eq or more, or 100 g / eq or more. By setting the epoxy equivalent to 10 g / eq or more, reactivity can be suppressed, preventing the reaction from proceeding during storage and reducing storage stability. Here, epoxy equivalent is the weight of resin containing one equivalent of epoxy groups, and can be measured by a method in accordance with JIS K 7236.

[0036] The epoxy resin may be monofunctional, bifunctional, trifunctional, or tetrafunctional or higher-function epoxy resin. If it is bifunctional or higher-function epoxy resin, the crosslinking density between the epoxy resin and the curing agent will be higher, resulting in higher adhesive strength.

[0037] <<<Curing Agent>>> As the curing agent for the adhesive layer 20, a curing agent commonly used in epoxy resin adhesives can be used. The curing agent is preferably solid at 23°C. A curing agent that is solid at 23°C has a longer storage stability (pot life) compared to a curing agent that is liquid at 23°C. The curing agent may also be a latent curing agent. The curing agent may be one that undergoes a curing reaction with heat, or one that undergoes a curing reaction with light. The curing agent may be used alone, or two or more types may be used.

[0038] The reaction initiation temperature of the curing agent is, for example, 110°C or higher, and may also be 130°C or higher. By raising the reaction initiation temperature, curing occurs while the epoxy resin in the adhesive layer 20 is highly flexible and fluid, thus enabling uniform curing. On the other hand, the reaction initiation temperature of the curing agent is, for example, 200°C or lower. By lowering the reaction initiation temperature, deterioration of the resin components in the adhesive layer 20 can be prevented. In addition, when using a heat-resistant resin other than epoxy resin, such as phenolic resin, the deterioration of the resin components is less, so the reaction initiation temperature of the curing agent may be, for example, 300°C or lower. The reaction initiation temperature of the curing agent can be determined by differential scanning calorimetry (DSC).

[0039] Specific examples of curing agents include imidazole-based curing agents, phenol-based curing agents, amine-based curing agents, acid anhydride-based curing agents, isocyanate-based curing agents, and thiol-based curing agents.

[0040] Examples of imidazole-based curing agents include imidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-isopropylimidazole, 2-phenylimidazole, carboxylate salts of imidazole compounds, and adducts with epoxy compounds. Furthermore, it is preferable that the imidazole-based curing agent has hydroxyl groups. Because crystallization occurs through hydrogen bonding between hydroxyl groups, the reaction initiation temperature tends to be high.

[0041] Examples of phenolic curing agents include phenolic resins. Examples of phenolic resins include resol-type phenolic resins and novolac-type phenolic resins. From the viewpoint of crack resistance, phenolic novolac resins with a glass transition temperature (Tg) of 110°C or lower are particularly preferred. Furthermore, a phenolic curing agent and an imidazole-type curing agent may be used in combination. In that case, it is preferable to use an imidazole-type curing agent as a curing catalyst.

[0042] Examples of amine-based curing agents include aliphatic amines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and meta-xylylenediamine (MXDA); aromatic amines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenyl sulfone (DDS); alicyclic amines; dicyandiamide-based curing agents such as polyamidoamine and dicyandiamide (DICY), organic acid dihydrazide-based curing agents, amine adduct-based curing agents, and ketimine-based curing agents can be used.

[0043] Examples of acid anhydride-based curing agents include alicyclic acid anhydrides (liquid acid anhydrides) such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA); and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic dianhydride (PMDA), and benzophenone tetracarboxylic acid (BTDA).

[0044] Examples of isocyanate-based curing agents include blocked isocyanates. Examples of thiol-based curing agents include ester bond-type thiol compounds, aliphatic ether bond-type thiol compounds, and aromatic ether bond-type thiol compounds.

[0045] The curing agent content is theoretically determined so that the number of reactive functional groups in the curing agent is approximately 1:1 to the number of epoxy groups in the epoxy resin. The ratio (equivalent ratio) of the number of reactive functional groups in the curing agent to the number of epoxy groups in the epoxy resin is usually 0.5 to 2.0, preferably 0.8 to 1.2. The curing agent content relative to the total mass of the adhesive layer 20 is, for example, 1% by mass or more and 40% by mass or less. For example, when an amine-based curing agent or an imidazole-based curing agent is used as the main component, the curing agent content is preferably, for example, 1% by mass or more and 15% by mass or less relative to the total mass of the adhesive layer 20. On the other hand, when a phenol-based curing agent is used as the main component, the curing agent content is preferably, for example, 5% by mass or more and 40% by mass or less relative to the total mass of the adhesive layer 20. Furthermore, using an imidazole-based or phenol-based curing agent as the main component means that the mass proportion of the imidazole-based or phenol-based curing agent is the largest in the curing agent.

[0046] <<<Foaming Agent>>> As the foaming agent, a foaming agent generally used in the foam layer of foamed adhesive sheets can be used. The foaming agent may be one that undergoes a foaming reaction due to heat, or one that undergoes a foaming reaction due to light.

[0047] The thermal expansion initiation temperature of the foaming agent is preferably above the softening point of the epoxy resin and below the curing activity temperature of the epoxy resin. The thermal expansion initiation temperature of the foaming agent is, for example, 70°C or higher, and may also be 100°C or higher. By raising the thermal expansion initiation temperature, foaming occurs while the resin components in the adhesive layer 20 are highly flexible and fluid, allowing the adhesive layer 20 to expand more uniformly. On the other hand, the thermal expansion initiation temperature of the foaming agent is, for example, 210°C or lower. By setting the thermal expansion initiation temperature to 210°C or lower, it is possible to more reliably prevent the deterioration of the resin components in the adhesive layer 20.

[0048] Examples of the foaming agent include organic foaming agents and inorganic foaming agents. Examples of the organic foaming agents include azo foaming agents such as azodicarbonamide (ADCA), azobisformamide, and azobisisobutyronitrile, fluorinated alkane foaming agents such as trichloromonofluoromethane, hydrazine foaming agents such as p-toluenesulfonyl hydrazide, semicarbazide foaming agents such as p-toluenesulfonyl semicarbazide, triazole foaming agents such as 5-morpholyl-1,2,3,4-thiatriazole, and N-nitroso foaming agents such as N,N-dinitrosoterephthalamide. On the other hand, examples of the inorganic foaming agents include ammonium carbonate, ammonium hydrogencarbonate, ammonium nitrite, ammonium borohydride, and azides.

[0049] Further, thermally expandable microcapsules may be used as the foaming agent. The thermally expandable microcapsules preferably have a core of a thermal expansion agent such as a hydrocarbon, and a shell of a thermoplastic resin such as an acrylonitrile copolymer having gas barrier properties. When the thermally expandable microcapsules are heated, the thermoplastic resin of the shell softens, and the volume of the thermal expansion agent increases, whereby the capsules expand. For example, vaporization of a low-boiling-point hydrocarbon compound can be utilized for the expansion of the capsules. These foaming agents may be used alone, or two or more types may be used in combination.

[0050] The content of the foaming agent and the volume expansion ratio can be appropriately determined according to the strength and adhesive force required for the cured adhesive layer 20, the expansion ratio required for the thermally expandable sheet 1, and the like. The content of the foaming agent is, for example, 0.5 mass% or more, and may be 2 mass% or more, based on the total mass of the adhesive layer 20. On the other hand, the content of the foaming agent is, for example, 60 mass% or less, and may be 50 mass% or less, based on the total mass of the adhesive layer 20.

[0051] The foaming ratio of the adhesive layer 20 may be, for example, 1.5 times or more, or 3 times or more. On the other hand, the foaming ratio of the adhesive layer 20 may be, for example, 20 times or less, or 15 times or less. The foaming ratio is determined by heating a 50 x 50 mm heat-expandable sheet 1 in a heating furnace set to 200°C for 10 minutes to foam and harden, and then using the following formula based on the thickness before and after heating: Foaming ratio = {(thickness of heat-expandable sheet 1 after heating) - (thickness of base material 10)} / {(thickness of heat-expandable sheet 1 before heating) - (thickness of base material 10)}

[0052] <<<Filler>>> The adhesive layer 20 preferably further contains a filler. The type of filler may be inorganic or organic. The type of filler is not limited, but examples include talc, mica, silica, alumina, kaolin, sericite, calcium carbonate, glass flakes, wollastonite, sepiolite, hydrotalcite, montmorillonite, PMF, gypsum fiber, potassium titanate, phosphate fiber, MOS, xonotlite, dawsonite, acicular calcium carbonate, glass fiber, carbon fiber, silicon carbide, silicon nitride, boron nitride, aluminum nitride, aluminum borate, zinc oxide, silicon oxide, titanium oxide, copper, nickel, magnesium oxide, aluminum oxide, calcium oxide, aluminum hydroxide, magnesium hydroxide, antimony trioxide, zinc borate, molybdenum compounds, titanium dioxide, etc.

[0053] The filler content is preferably 3% to 90% by mass, more preferably 5% to 80% by mass, and more preferably 8% to 65% by mass, based on the total mass of the adhesive layer 20. Increasing the filler content makes it easier to produce a thermally expanded sheet 1 with high rigidity, while decreasing the filler content improves the wettability of the adhesive layer 20 to the adherend, resulting in a thermally expanded sheet 1 with good adhesive strength. If the filler content can be reduced, it is not necessary to use an epoxy resin with a low softening point for the purpose of improving adhesive strength, thus making it possible to produce a thermally expanded sheet 1 that balances both tackiness and adhesive strength. Furthermore, by setting the filler content to 3% to 90% by mass, the filler is more easily dispersed in the epoxy resin, preventing the filler from precipitating and resulting in a thermally expanded sheet 1 with even higher rigidity.

[0054] The shape and aspect ratio of the filler are not specified, but by including a filler with a high aspect ratio in the adhesive layer 20, it may be possible to improve the partial discharge initiation voltage of the adhesive layer 20. By including a filler with a high aspect ratio, the fillers become more likely to intertwine with each other, allowing for the inclusion of numerous microvoids within the adhesive layer 20. As a result, the charge accumulated in the adhesive layer 20 is discharged quickly, making it less likely for large charges to accumulate in the thermal expansion sheet 1, thus reducing the likelihood of damage caused by discharge.

[0055] Furthermore, using a filler with a high aspect ratio may improve the thermal conductivity of the thermal expansion sheet 1 in the thickness direction. When improving the thermal conductivity of a sheet in the thickness direction, it is generally considered best to include spherical fillers to create heat transfer paths in the thickness direction. However, when using a combination of a foaming agent and a filler, as in the thermal expansion sheet 1, using a filler with a high aspect ratio allows the filler to penetrate between the narrow particles of the foaming agent after foaming, making it easier to create heat transfer paths in the thickness direction. This makes it possible to provide a thermal expansion sheet 1 with excellent thermal conductivity.

[0056] <<<Elastomer>>> The adhesive layer 20 may further contain an elastomer. In this specification, elastomer is a broad concept that includes resins that, when incorporated into the adhesive layer 20, can impart toughness and flexibility to the adhesive layer 20 so that it does not break even when subjected to bending or twisting, and is not limited to materials that are commercially available as elastomer materials or rubber materials. Examples of such elastomers include at least one of polyester resin, polyvinyl acetal resin, butyral resin, urethane resin, acrylic resin, acrylic rubber, fluororubber, carboxyl-terminated butadiene nitrile rubber (CTBN), and epoxy-modified butadiene.

[0057] When the adhesive layer 20 contains an elastomer, depending on its compatibility with other materials used, it is preferable to use an elastomer that does not contain carboxyl groups or has a small number of carboxyl groups. By including an elastomer with few carboxyl groups, it is possible to prevent gelation from occurring due to the reaction between the components in the foaming agent and the carboxyl groups in the resin composition in which the materials in the adhesive layer 20 are mixed, resulting in effects such as an improved appearance of the adhesive layer 20.

[0058] When the adhesive layer 20 contains an elastomer, the elastomer content is, for example, 0.5% by mass or more, may be 1% by mass or more, and more preferably 2% by mass or more, based on the total mass of the adhesive layer 20. On the other hand, when the adhesive layer 20 contains an elastomer, the elastomer content is 30% by mass or less, may be 20% by mass or less, and more preferably 15% by mass or less, based on the total mass of the adhesive layer 20. By setting the elastomer content to 2% by mass or more, the flexibility and toughness of the adhesive layer 20 can be increased, further improving the adhesion of the adhesive layer 20 to the substrate 10 and suppressing cracking of the adhesive layer 20. Furthermore, by setting the elastomer content to 30% by mass or less, when thermally expanded, the complex melt viscosity of the thermal expansion sheet 1 when the thermal expansion start temperature of the foaming agent contained in the thermal expansion sheet 1 is reached can be suppressed, allowing the adhesive layer 20 to expand sufficiently. Furthermore, by reducing the elastomer content, the adhesive strength of the adhesive layer 20 can be increased. Therefore, it is not necessary to use epoxy resin with a low softening point to improve adhesive strength, and a thermally expandable sheet 1 that achieves both tackiness and adhesive strength can be made.

[0059] When the adhesive layer 20 contains an elastomer, the glass transition temperature (Tg) of the elastomer is preferably, for example, 100°C or higher and 120°C or lower. By using an elastomer with a Tg of 100°C or higher, the stiffness of the thermal expansion sheet 1 can be further improved and tack can be further reduced. By using an elastomer with a Tg of 120°C or lower, the adhesive layer 20 can be made less prone to cracking. If the flexibility of the adhesive layer 20 is to be further increased, it is preferable to use an elastomer with a Tg of 100°C or higher and an elastomer with a Tg of less than 100°C in combination. The glass transition temperature (Tg) of the elastomer can be measured by thermomechanical analysis (TMA), differential scanning calorimetry (DSC), or dynamic viscoelastic analysis (DMA). For example, it can be measured by DSC in accordance with the method specified in JIS K 7121.

[0060] <<<Curing Accelerator>>> The adhesive layer 20 may further contain a curing accelerator. As the curing accelerator, for example, an imidazole compound can be used. Compared to other curing catalysts, imidazole compounds have the advantage of being easy to use because they can be used as a single catalyst and there are also grades with very fine particle sizes. Specific examples of imidazole compounds include imidazole derivatives such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 2,4-diethylimidazole, and 2-phenyl-4-methyl-5-hydroxyimidazole. Two or more imidazole compounds may be used in combination. Among these, 2-phenyl-4,5-dihydroxymethylimidazole is preferred. The content of the imidazole compound is preferably 0.1% by mass or more and 2.0% by mass or less, more preferably 0.5% by mass or more and 1.5% by mass or less, based on the total mass of the adhesive layer 20.

[0061] <<<Additives>>> The adhesive layer 20 may optionally contain a silane coupling agent, antioxidant, light stabilizer, UV absorber, lubricant, plasticizer, antistatic agent, crosslinking agent, and colorant. Examples of silane coupling agents include epoxy-based silane coupling agents. Examples of antioxidants include phenol-based antioxidants and sulfur-based antioxidants.

[0062] <<Primer Layer>> As shown in Figure 1, the thermal expansion sheet 1 may be provided with a primer layer 30 between the substrate 10 and the adhesive layer 20 in order to improve the adhesion between the substrate 10 and the adhesive layer 20. In particular, if the adhesive layer 20 has a filler or contains an epoxy resin with a high softening point, it is preferable to provide a primer layer 30 in order to improve the adhesion between the adhesive layer 20 and the substrate 10 and to prevent peeling during folding or insertion into gaps.

[0063] The primer layer 30 may contain a resin. The resin included in the primer layer 30 is not particularly limited as long as it is a highly flexible resin, such as polyester, polyvinyl chloride, polyvinyl acetate, polyurethane, acrylic, or styrene. If the resin included in the primer layer 30 has functional groups, it will crosslink with the adhesive layer 20 present on the surface of the primer layer 30, thereby making the adhesion between the primer layer 30 and the adhesive layer 20 stronger.

[0064] Furthermore, when the functional groups of the resin contained in the primer layer 30 react with the epoxy resin contained in the adhesive layer 20, it is preferable to set the number of reactive functional groups of the curing agent in the adhesive layer 20 to be less than 1:1 relative to the number of epoxy groups in the epoxy resin. When set in this way, the epoxy resin in the adhesive layer 20 that was not used in the reaction with the curing agent crosslinks with the functional groups of the resin contained in the primer layer 30, thereby making the adhesion between the adhesive layer 20 and the primer layer 30 stronger.

[0065] Furthermore, the primer layer 30 may contain a curing agent for curing the resin contained in the primer layer. Examples of curing agents for curing the resin contained in the primer layer 30 include isocyanate-based curing agents.

[0066] The primer layer 30 may contain a filler. If the primer layer 30 contains a filler, the stiffness of the thermal expansion sheet 1 can be increased. It is preferable that the filler in the primer layer 30 is selected under the same conditions as the filler in the adhesive layer 20.

[0067] The thickness of the primer layer 30 is not particularly limited, but for example it may be 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. Increasing the thickness of the primer layer 30 can improve crack resistance. On the other hand, the thickness of the primer layer 30 may be 10 μm or less. By making the thickness of the primer layer 10 μm or less, it is possible to prevent stress from concentrating in the primer layer and causing fracture when shear stress is applied.

[0068] <Characteristics of Thermal Expansion Sheet 1> Through diligent research, the inventors discovered that when a thermal expansion sheet with high stiffness is intended to fill gaps formed by multiple adherends when heated and expanded, and is then folded to fit the shape of these gaps and inserted into the gaps, it becomes difficult to fold the thermal expansion sheet, and the shape retention after folding becomes insufficient, resulting in reduced insertability. Furthermore, it was found that while a thermal expansion sheet with high stiffness can be folded by applying higher pressure, this may cause the thermal expansion sheet to be scraped or torn, potentially degrading its properties. Therefore, the inventors discovered that by increasing the stiffness in the insertion direction and decreasing the stiffness in the folding direction, it is possible to develop a thermal expansion sheet that is easy to fold and has high insertability. Differentiating the stiffness in two directions along the surface of the thermal expansion sheet is a completely new approach that has not been seen before.

[0069] However, in the thermal expansion sheet 1 according to this embodiment, the stiffness in the first and second directions, which are two different directions along the surface direction of the sheet, is different from that of the sheet before heating and expansion. The stiffness in each direction along the surface direction of the thermal expansion sheet 1 can be evaluated by measuring the Gurley flexibility in each direction along the surface direction of the thermal expansion sheet 1, based on JIS L 1085. The surface direction, as mentioned above, is the direction along the surface of the thermal expansion sheet that is in contact with the adherend, and refers to the direction perpendicular to the thickness direction of the thermal expansion sheet. Of the two directions for evaluating the Gurley flexibility, the direction with high Gurley flexibility is designated as the first direction, and the direction with low Gurley flexibility is designated as the second direction. It is preferable that the first and second directions are orthogonal to each other.

[0070] The Gurley flexibility in the first direction is preferably 20 mgf or more, and more preferably 30 mgf or more or 40 mgf or more, from the viewpoint of further improving the insertability of the thermal expansion sheet. The Gurley flexibility in the first direction is preferably 2000 mgf or less, more preferably 1800 mgf or less or 1600 mgf or less, and can be 1400 mgf or less, 1200 mgf or less, 1000 mgf or less, 800 mgf or less, 600 mgf or less, 400 mgf or less or 200 mgf or less.

[0071] The Gurley flexibility in the second direction is preferably 1800 mgf or less, more preferably 1600 mgf or less or 1400 mgf or less, and can be 1200 mgf or less, 1000 mgf or less, 800 mgf or less, 600 mgf or less, 400 mgf or less, 200 mgf or less, or 100 mgf or less, from the viewpoint of further improving the bendability of the thermal expansion sheet. The Gurley flexibility in the second direction is preferably 15 mgf or more, and more preferably 25 mgf or more or 35 mgf or more.

[0072] The ratio of the Gurley flexibility in the first direction to the Gurley flexibility in the second direction (first direction / second direction) is preferably 1.1 or higher, more preferably 1.5 or higher, or more preferably 2.0 or higher, from the viewpoint of further improving the balance between the insertability and bendability of the thermal expansion sheet. The upper limit of the Gurley flexibility ratio is not particularly limited, but for example, it is 5.0 or less, 4.0 or less, or 3.0 or less.

[0073] Furthermore, through further diligent research, the inventors discovered that when inserting a thermal expansion sheet into the narrow U-shaped gap between the motor coil and stator core, for example, the sheet is often provided in a rolled state during the motor manufacturing process. Therefore, they found that manufacturing efficiency can be improved by setting the MD direction (roll flow direction) of the sheet as the insertion direction, the direction perpendicular to the MD direction, i.e., the TD direction, as the bending direction, and bending the sheet so that creases are created parallel to the MD direction. From these findings, they discovered that in order to obtain a thermal expansion sheet with high insertability, it is preferable to set the MD direction and TD direction as the first and second directions, respectively, and to increase the stiffness of the sheet in the MD direction and decrease the stiffness in the TD direction.

[0074] One method for obtaining such a thermal expansion sheet 1 is to increase the degree of orientation of the filler in the state before heating and expansion. This allows for greater stiffness in a desired direction compared to other directions, with a smaller filler content, compared to cases where the degree of orientation is not controlled. When it is desired that the stiffness differs between the insertion direction and the bending direction, such as when the motor and coil are the adherends as described above, it has been found that increasing the degree of orientation of the filler contained in the thermal expansion sheet is particularly preferable. The degree of orientation of the filler referred to here is, for example, the degree of orientation of the filler in the direction of the long axis of the filler with respect to the MD direction. In this way, in the direction of the long axis of the filler (also called the orientation direction), the filler exerts a physical resistance against the force that tries to deform the thermal expansion sheet, thus increasing the stiffness of the thermal expansion sheet. Furthermore, in the direction perpendicular to the orientation direction of the filler, the force exerted by the filler in a direction that opposes the force that tries to maintain the shape of the resin component contained in the thermal expansion sheet after bending is less likely to act, thus improving the shape retention of the thermal expansion sheet.

[0075] The inventors also identified a conventional problem: if a large amount of filler is included to increase the stiffness of the thermal expansion sheet, there is a risk that the adhesive strength when the thermal expansion sheet is heated and expanded may decrease. They believed that this problem could also be solved by increasing the degree of orientation of the filler before heating and expansion. By increasing the degree of orientation of the filler before heating and expansion, the stiffness of the thermal expansion sheet in the desired direction can be increased with a smaller filler content than when the degree of orientation of the filler is not controlled. As a result, as already mentioned in the section on the filler content in the adhesive layer 20, the wettability of the adhesive layer 20 to the adherend, which contributes to the adhesive strength of the thermal expansion sheet, can be made as large as possible, resulting in a thermal expansion sheet 1 with high adhesive strength. Furthermore, since there is no need to include an epoxy resin with a low softening point in the adhesive layer 20 for the purpose of supplementing the adhesive strength of the thermal expansion sheet 1, effects such as reduced tack formation in the adhesive layer 20 can also be obtained.

[0076] As mentioned above, in order to control the degree of orientation of the filler, the aspect ratio of the filler contained in the adhesive layer 20 is preferably greater than 1, more preferably 1.5 to 80, even more preferably 2 to 60, and most preferably 3 to 40. A filler with a uniform aspect ratio may be used, or multiple types with different aspect ratios may be used in combination. A small aspect ratio is preferable because it makes it less likely for the thixotropy of the resin composition to increase and makes it easier to knead into the resin composition. On the other hand, a large aspect ratio of the filler is preferable because it makes it easier for the degree of orientation of the filler to increase and for the thermal expansion sheet 1 to become stiffer, even if the shear stress applied when the resin composition is applied to the substrate 10 is small. The aspect ratio referred to here is the ratio of the length in the long axis direction to the length in the short axis direction of the filler. The aspect ratio can be measured using a scanning electron microscope (SEM). For example, for any 50 fillers, the length along the major axis is measured with the direction of the largest diameter as the major axis, and the length along the minor axis is measured with the direction of the smallest diameter as the minor axis. The average value of each is then calculated, and the ratio of the average length along the major axis to the average length along the minor axis (average length along the major axis / average length along the minor axis) is calculated to determine the aspect ratio.

[0077] Furthermore, the shape of the filler contained in the adhesive layer 20 according to this embodiment is preferably, for example, flaky, plate-like, needle-like, fibrous, or branch-like, and one or more of these filler shapes can be used.

[0078] Furthermore, it is preferable that the average degree of orientation, which is the angle between the long axis direction of the filler and the MD direction, when observed by SEM from the thickness direction relative to the MD direction of the filler in the adhesive layer 20 before heating and expansion, be 40° or less. The SEM observation is performed as follows: A scanning electron microscope (SEM, Hitachi High-Tech Corporation, SU3800) is used to photograph the surface of the adhesive layer 20 from the thickness direction of the adhesive layer 20. At this time, the observation range and magnification are set so that a certain number of filler particles are included in the field of view, according to the particle size of the filler used. Next, image processing software is used to identify the filler portion from the difference in contrast and measure the length of the long axis of the filler. At least 30, preferably 50, fillers with long long axes are selected, and the angle between their long axis and the MD direction of the thermal expansion sheet 1 is calculated.

[0079] In this embodiment, it is preferable that, before heating and expanding, the proportion of fillers in the adhesive layer 20 with an orientation degree of less than 45° is 55% or more.

[0080] It is desirable that the thermal expansion sheet 1 has higher shape retention in the TD direction than in the MD direction before heating and expansion. By making the thermal expansion sheet 1 such that the sheet can be folded in the TD direction to form a shape that matches the shape of the gap, and deformation in the MD direction will not occur easily, making it less prone to buckling, thus resulting in a thermal expansion sheet 1 that is easy to insert into the gap and easy to place.

[0081] To increase the degree of orientation of the filler in the adhesive layer 20, it is preferable that the adhesive layer 20 contains two or more epoxy resins, and that the epoxy resins be a combination of one with a molecular weight of 10,000 or less and one with a molecular weight of 10,000 or more. When an epoxy resin with a molecular weight of 10,000 or more is used, the viscosity of the resin composition tends to increase when forming the adhesive layer 20 of the thermal expansion sheet 1, and when the resin composition is applied to the substrate 10, the shear stress on the applied surface increases, resulting in a higher degree of orientation of the filler in the adhesive layer 20. As a result, the stiffness in the MD direction can be efficiently improved, and even with a small amount of filler added, a thermal expansion sheet 1 that achieves both adhesive strength and stiffness can be obtained. On the other hand, when an epoxy resin with a molecular weight of 10,000 or less is used, the viscosity tends to decrease when the thermal expansion sheet 1 is heated and expanded, resulting in good wettability to the adherend and a tendency for higher adhesive strength. Note that the molecular weight referred to here is the weight-average molecular weight or the calculated molecular weight.

[0082] To increase the degree of orientation of the filler in the adhesive layer 20, the molecular weight of the elastomer contained in the adhesive layer 20 is preferably 10,000 or more and 1,000,000 or less, more preferably 50,000 or more and 800,000 or less, and even more preferably 100,000 or more and 500,000 or less. By setting the molecular weight of the elastomer to 10,000 or more, the viscosity of the entire resin composition tends to increase when forming the adhesive layer 20, and when the resin composition is applied to the substrate 10, the shear stress applied to the applied surface increases, and the degree of orientation of the filler in the adhesive layer 20 increases. On the other hand, by setting the molecular weight of the elastomer to 1,000,000 or less, the fluidity of the adhesive layer 20 increases during thermal expansion, allowing the adhesive layer 20 to expand sufficiently. Here, molecular weight refers to weight-average molecular weight or calculated molecular weight. Molecular weight can be measured by gel permeation chromatography (GPC) or the like.

[0083] To increase the degree of orientation of the filler in the adhesive layer 20, it is preferable to use a filler with high oil absorption. When a filler with high oil absorption is used, when it is kneaded into the resin composition, the filler absorbs or retains liquid components such as resin components and solvents, which tends to increase the viscosity of the entire resin composition. When the resin composition is applied to the substrate 10, the shear stress on the applied surface increases, and the degree of orientation of the filler in the adhesive layer 20 increases. The oil absorption amount of the filler is preferably 50 ml / 100 g, more preferably 75 ml / 100 g, and even more preferably 100 ml / 100 g. On the other hand, if the oil absorption amount is 300 ml / 100 g or less, it is preferable because the filler is easier to disperse in the resin composition.

[0084] If the primer layer 30 contains filler, it is desirable that the degree of orientation of the filler in the layer is high, similar to the adhesive layer 20. If the degree of orientation of the filler in the primer layer 30 is high, the stiffness of the thermal expansion sheet 1 in the MD direction will be higher than the stiffness in the TD direction, resulting in high stiffness in the insertion direction, high shape retention after bending, and a thermal expansion sheet 1 that is highly insertable into narrow gaps.

[0085] <Method for manufacturing the thermal expansion sheet 1> The thermal expansion sheet 1 according to this embodiment can be manufactured, for example, by the following procedure and method.

[0086] For example, the primer layer 30 can be formed by applying a primer composition to the substrate 10 so that the thickness after drying is of a desired thickness, and then removing the solvent.

[0087] The primer composition can be prepared, for example, as a varnish or slurry-like substance obtained by dissolving or dispersing the material that forms the primer layer 30 (e.g., polyester resin) in a suitable solvent.

[0088] Methods for applying the primer composition include, for example, various roll-to-roll manufacturing methods in which coating, drying, and winding are performed in a series of steps while unwinding a roll-shaped substrate at a constant speed, as well as spray coating and dip coating. When the primer layer 30 contains a filler, the preferred method for applying the primer composition is one in which shear stress is applied in the longitudinal direction of the substrate 10, i.e., in the MD direction of the thermal expansion sheet 1, during application. Preferred application methods that apply shear stress in the MD direction include, for example, roll coating, transfer roll coating, gravure coating, comma coating, and dip coating, and more preferably reverse roll coating, gravure reverse coating, rod coating, blade coating, bar coating, wire bar coating, die coating, and lip coating. Furthermore, it is desirable to increase the shear stress in the MD direction during application by, for example, increasing the rotation speed of the roll in the case of roll coating, or increasing the injection speed of the primer composition in the case of die coating. When shear stress is applied in the MD direction during application, the degree of orientation of the filler in the primer layer 30 increases, which enhances the stiffness of the thermal expansion sheet 1 in the MD direction while making it easier to ensure shape retention after bending in the TD direction. The primer composition applied to the surface of the substrate by the method described above is dried to form the primer layer 30.

[0089] The adhesive layer 20 can be formed, for example, by applying a resin composition for forming the adhesive layer 20 onto the primer layer 30 formed by the method described above, such that the thickness after drying is an arbitrary thickness, and then removing the solvent.

[0090] The resin composition can be prepared as a varnish or slurry by dissolving or dispersing the material that forms the adhesive layer 20 with the above-described configuration (for example, epoxy resin, etc.) in a suitable solvent.

[0091] The solvent in the resin composition is not particularly limited, and a wide range of solvents commonly used in the manufacture of adhesives, such as MEK (methyl ethyl ketone), can be used. The solvent content in the resin composition is, for example, 20% by mass or more, may be 25% by mass or more, or 30% by mass or more, based on the total mass of the resin composition. By increasing the solvent content in the resin composition, the viscosity of the resin composition is reduced, and air bubbles can be easily released during drying, thus preventing deterioration of the appearance of the adhesive layer 20. On the other hand, the solvent content is, for example, 80% by mass or less, may be 70% by mass or less, or 60% by mass or less, based on the total mass of the resin composition. By decreasing the solvent content, the viscosity of the resin composition is increased, and when the resin composition is applied to the substrate 10, the shear stress applied to the applied surface is increased, and the degree of orientation of the filler in the adhesive layer 20 is increased.

[0092] The resin composition has a viscosity at 23°C of, for example, 40 mPa·s or more, but may also be 120 mPa·s or more, or 170 mPa·s or more. Increasing the viscosity of the resin composition increases the shear stress applied to the coated surface when the resin composition is applied to the substrate 10, thereby increasing the degree of orientation of the filler in the adhesive layer 20. On the other hand, the viscosity at 23°C may be, for example, 10,000 mPa·s or less, but may also be 5,000 mPa·s or less, or 1,000 mPa·s or less. Lowering the viscosity of the resin composition makes it easier for air bubbles to escape during drying, thus preventing deterioration of the appearance of the adhesive layer 20. The viscosity can be determined by measuring it using a single-cylinder rotational viscometer in accordance with JIS Z 8803.

[0093] Methods for applying the resin composition include, for example, various roll-to-roll manufacturing methods in which coating, drying, and winding are performed in a series of steps while unwinding a roll-shaped substrate at a constant speed, as well as spray coating and dip coating. A preferred method for applying the resin composition is one in which shear stress is applied in the longitudinal direction of the substrate 10, i.e., in the MD direction of the thermal expansion sheet 1, during application. Preferred application methods that apply shear stress in the MD direction include, for example, roll coating, transfer roll coating, gravure coating, comma coating, and dip coating, with reverse roll coating, gravure reverse coating, rod coating, blade coating, bar coating, wire bar coating, die coating, and lip coating being more preferred. Furthermore, it is desirable to increase the shear stress in the MD direction during application by, for example, increasing the rotation speed of the roll in the case of roll coating, or increasing the injection speed of the resin composition in the case of die coating. For example, when using roll coating, it is preferable to set the rotation speed of the roll to 2 m / min or higher. Furthermore, when using bar coating, it is preferable to set the bar's movement speed (coating speed) to 2 m / min or more. However, if the viscosity of the resin composition is high, coating may be performed at a slower speed than the above if the degree of orientation of the filler can be controlled. When shear stress is applied in the MD direction during coating, the degree of orientation of the filler in the adhesive layer 20 increases, which enhances the stiffness of the thermal expansion sheet 1 in the MD direction while making it easier to ensure shape retention after bending in the TD direction. The resin composition applied to the surface of the substrate by the method described above is dried at a temperature lower than the thermal expansion start temperature of the foaming agent contained in the adhesive layer 20, for example, 50°C to 110°C, for a time of 30 seconds to 300 seconds to form the adhesive layer 20.

[0094] Furthermore, when forming a primer layer and an adhesive layer 20 on both sides of the substrate 10, it is preferable to first form the primer layer 30a and adhesive layer 20a on one side of the substrate 10 using the method described above, and then form the primer layer 30b and adhesive layer 20b on the opposite side of the same substrate using the method described above.

[0095] <Modified Embodiments> The present invention is not limited to those described above. For example, the thermal expansion sheet 1 according to the present invention does not have to have a primer layer 30 and an adhesive layer 20 on both sides of the base material 10, but may have a primer layer 30 and an adhesive layer 20 on only one side of the base material 10. In addition, depending on the application of the thermal expansion sheet 1, another layer may be provided, or a release paper may be further laminated on the outermost surface of the thermal expansion sheet 1.

[0096] For example, in the case where the thermal expansion sheet 1 according to the present invention is provided with a primer layer 30 and an adhesive layer 20 on both sides of the base material 10, the manufacturing method may involve forming primer layers 30a and 30b on both sides of the base material 10, forming the adhesive layer 20a on the primer layer 30a, and forming the adhesive layer 20b on the primer layer 30b.

[0097] Furthermore, for example, as shown in Figure 2, the primer layer 30 may be omitted and the adhesive layer 20 may be directly laminated onto the substrate 10, or the substrate 10 may be subjected to corona treatment or primer treatment before the adhesive layer 20 is laminated in order to improve the adhesion between the substrate 10 and the adhesive layer 20.

[0098] It is desirable that the thermal expansion sheet 1 of the present invention be easily disassembled after use. One method of disassembly is to degrade the resin and substrate 10 contained in the adhesive layer 20 and primer layer 30 to reduce the adhesive strength. The method of reducing the adhesive strength is not particularly limited, but the adhesive strength may be reduced chemically by treating the adhesive area at high temperature or high humidity for a long time, or by boiling the adhesive area, or it may be physically peeled off by irradiating with a laser.

[0099] The thermal expansion sheet 1 can be used for a variety of applications depending on its physical properties, and its applications are not particularly limited. For example, when it is used to bond the gap between the coil and stator core of a motor, the thickness before heating and expansion is preferably 300 μm or less, more preferably 20 μm to 250 μm. Also, for example, when the thermal expansion sheet 1 is used as a conductive sheet for electronic equipment or electronic devices, it is preferable that it has electrical conductivity, and when it is used as an insulating sheet for electronic equipment or electronic devices, it is preferable that the thermal expansion sheet 1 has electrical insulation properties.

[0100] The thermal expansion sheet 1 is placed in a narrow gap formed by multiple adherends, and in order to bond these multiple adherends, the shear adhesive strength of the thermal expansion sheet 1 after heating and expansion is preferably 0.8 MPa or more, more preferably 0.9 MPa or more, and even more preferably 1.0 MPa or more at 23°C. The upper limit of the shear adhesive strength at 23°C is not particularly limited, but is for example 30 MPa or less, 20 MPa or less, or 10 MPa or less. Furthermore, the shear adhesive strength at 200°C is preferably 0.1 MPa or more, more preferably 0.15 MPa or more, and particularly preferably 0.2 MPa or more. The upper limit of the shear adhesive strength at 200°C is not particularly limited, but is for example 10 MPa or less, 7.5 MPa or less, or 5 MPa or less.

[0101] Furthermore, when the heat-expandable sheet 1 is used in a high-temperature environment, such as when the adherend is a motor coil and stator core, the shear adhesive strength of the heat-expandable sheet 1 after heating and expanding and then being treated at 200°C for 500 hours is preferably 0.1 MPa or more, more preferably 0.15 MPa or more, and even more preferably 0.2 MPa or more at 200°C. The upper limit of the above shear adhesive strength is not particularly limited, but is, for example, 5 MPa or less, 4 MPa or less, or 3 MPa or less.

[0102] When the heat-expandable sheet 1 is used in a high-temperature environment, such as when the adherend is a motor coil and stator core, it is preferable that the shear adhesive strength of the heat-expandable sheet 1 after further heating and expansion and treatment at 85°C and 85% RH for 1000 hours is, for example, 0.1 MPa or more, more preferably 0.15 MPa or more, and even more preferably 0.2 MPa or more at 200°C. The upper limit of the above shear adhesive strength is not particularly limited, but for example it is 5 MPa or less, 4 MPa or less, or 3 MPa or less.

[0103] The shear adhesive strength of the thermal expansion sheet 1 was measured by the following method. Using a 110°C rubber roll, a thermal expansion sheet 1 cut to 12.5 × 25 mm was fixed to an SPCC plate. Spacers with a thickness of 0.175 mm were placed on both sides of the thermal expansion sheet 1, and another SPCC plate was placed on top of them. The gap between the SPCC plates was fixed using a fixing jig (clamp, etc.). The thermal expansion sheet 1 between the SPCC plates was thermally expanded and hardened, and this was used as a sample. At this time, the gap between the two SPCC plates was fixed at 0.175 mm. The sample, which had undergone an arbitrary heat treatment, was tested using a universal testing machine (AGS-10kNX, Shimadzu Corporation, load cell capacity: 10kN) under an arbitrary test atmosphere and a test speed of 5 mm / min. The two SPCC plates of the sample were pulled in opposite directions along the surface direction of the sample, and the applied pressure at which the sample broke was measured as the shear adhesive strength.

[0104] The thermal expansion sheet 1 can be used as a conductive sheet for electronic equipment or electronic devices if it has electrical conductivity, or as an insulating sheet for electronic equipment or electronic devices if it has electrical insulation properties.

[0105] Furthermore, various modifications of the embodiments and combinations of parts of the embodiments are permitted, as long as they do not contradict the spirit of the present invention.

[0106] The present invention will be described in more detail below with specific examples, but it goes without saying that the present invention is not limited to these. Here, thermal expansion sheets of Examples 1 to 12 were manufactured and their physical properties were evaluated.

[0107] <<Formation of Adhesive Layer 20a>> Resin compositions were prepared by mixing MEK with formulations G1 to G9 listed in Table 1 to obtain the solid content shown in Table 2. Each resin composition was then applied to the substrate 10 using a Baker applicator to a thickness of 50 μm after drying. The viscosity of these resin compositions was measured in accordance with JIS Z 8803 using a single-cylinder rotational viscometer (VT-06, manufactured by Rion Co., Ltd.) at a temperature of 23°C and a rotational speed of 62.5 rpm, and the results are shown in Table 3. As the substrate 10, Kapton® 100EN, manufactured by Toray DuPont, with a thickness of 25 μm was used. The adhesive layer 20a was formed by drying this at 110°C for 90 seconds to remove the solvent.

[0108] In this embodiment, the shear stress of the resin composition coating method used to form the adhesive layer 20a was simulated using the following method, and the results are shown in Figure 3. <<Measurement of Shear Stress>> Using a rheometer (ARES-G2 manufactured by T.A. Instruments Co., Ltd.), a double-cylinder jig consisting of a cup with an inner diameter of 26 mm and a rotor with an outer diameter of 25 mm was used to evaluate the shear stress by measuring the flow curve at 23°C in the range of shear rate from 0.01 to 100 / second. The vertical axis of the graph shows shear stress (stress, unit: Pa), and the horizontal axis shows shear rate (unit: 1 / s). The shear stress was measured when the shear rate (rotor rotation speed) was varied for each resin composition in Example 4 (NV 75% in the graph), Example 5 (NV 70% in the graph), a reference example with the same composition as Example 5 but with a solid content concentration of 65% by mass (NV 65% in the graph), and a reference example with a solid content concentration of 60% by mass (NV 60% in the graph). The shear stress was measured when the shear rate (rotor rotation speed) was varied in each of these resin compositions. In this experiment, the shear rate can be considered to be a pseudo-reproduction of the coating speed when coating the resin composition along a certain direction. <<Evaluation regarding shear stress>> From the results in Figure 3, it was found that in all cases, the shear stress tends to increase as the shear rate (coating speed) increases. From this, it was found that in the results of Examples 11 and 12, in which the coating speed was varied, when the material was produced under conditions of high shear stress, the stress that orients the filler in the resin composition is sufficiently large, the degree of filler orientation is high, and it was possible to obtain a thermal expansion sheet with different Gurley flexibility in the first direction and the second direction. Furthermore, the results in Figure 3 show that, at the same shear rate, the higher the solid content concentration of the resin composition, i.e., the higher the viscosity of the resin composition, the higher the shear stress tends to be. From this, it can be seen that in the results of Examples 4 and 5, in which the viscosity of the resin composition was varied by changing the solid content concentration of the resin composition, and in the results of Examples 1, 2, and 3, in which the viscosity of the resin composition was varied by changing the amount of high molecular weight elastomer added, when manufactured under conditions of high shear stress, it was possible to obtain a thermal expansion sheet with a higher degree of filler orientation and a greater difference in Gurley flexibility between the first and second directions.

[0109]

[0110]

[0111] The components in Table 1 are as follows: A: Epoxy resin "EPICLON (registered trademark) N-690", epoxy equivalent 210-240 g / eq, softening point 85-95°C, weight-average molecular weight 1,400-1,500 (manufactured by DIC Corporation) B-1: Curing agent "jER Cure (registered trademark) Dicy7", amine equivalent 21 g / eq (manufactured by Mitsubishi Chemical Corporation) B-2: Curing agent "Reditop (registered trademark) PSM-4326", hydroxyl group equivalent 105 g / eq (manufactured by Gun-ei Chemical Industry Co., Ltd.) C: Curing accelerator "ADEKA Hardener (registered trademark) EH-5046S" (manufactured by ADEKA Corporation) D-1: Elastomer "Eslec (registered trademark) KS-6Z" (manufactured by Sekisui Chemical Co., Ltd.), glass transition temperature 113°C, calculated molecular weight 108,000 D-2: Elastomer "Nipol (registered trademark)" AR12 (manufactured by Zeon Corporation) D-3: Elastomer "Vamac (registered trademark) GLS" (manufactured by DuPont), glass transition temperature -24°C, weight-average molecular weight 280,000 E: Foaming agent "Matsumoto Microsphere (registered trademark) FN-100SSD" (manufactured by Matsumoto Oil & Fat Pharmaceutical Co., Ltd.), thermal expansion start temperature 120-130°C F-1: Needle-shaped filler "FTL-100" aspect ratio 19 (manufactured by Ishihara Sangyo Co., Ltd.) F-2: Flake-shaped filler "Repco Mica S-XF" aspect ratio 15 (manufactured by Repco) F-3: Needle-shaped filler "WFB15" aspect ratio 17 (manufactured by Nippon Talc Co., Ltd.)

[0112] <<Formation of adhesive layer 20b>> The same resin composition as adhesive layer 20a was applied to the side of the substrate 10 opposite to the side on which adhesive layer 20a was formed, using a Baker-type applicator, so that the thickness after drying was 50 μm. Adhesive layer 20b was formed by drying this at 110°C for 90 seconds to remove the solvent.

[0113] <<Evaluation of Thermal Expansion Sheets>> The thermal expansion sheets prepared as described above were subjected to the following evaluation tests.

[0114] <<<Filler Orientation Degree>>> The degree of filler orientation was evaluated by the average value of the orientation degree, which is the angle between the long axis direction of the filler and the MD direction when the thermal expansion sheet was observed with SEM from the thickness direction, and the percentage of fillers within the observation range whose orientation degree is less than 45°.

[0115] <<<Gurley Flexibility>>> A 25.4 mm x 25.4 mm sheet was cut from a thermal expansion sheet before heating and expansion, and this was used as a test specimen. The Gurley flexibility was measured in accordance with JIS L 1085 using the following procedure. A Gurley flexibility tester manufactured by Toyo Seiki Seisakusho was used for the measurement. The test specimen, chucked in a movable arm, was rotated left and right at a specified speed to bring the lower end of the thermal expansion sheet 1 into contact with the pendulum. The scale was read when the lower end of the thermal expansion sheet 1 separated from the pendulum, and the flexibility was calculated from the average of five measured values. For example, when measuring the Gurley flexibility in the MD direction, the test specimen was chucked so that the MD direction of the test specimen was parallel to the vertical direction, and the test specimen was moved left and right while the pendulum was in contact with the lower end of the test specimen. This caused the test specimen to bend in a direction perpendicular to the MD direction, pushing the pendulum, and the lower end of the test specimen separated from the pendulum when the deflection of the test specimen reached its maximum. When measuring the Gurley flexibility in the TD direction, the test specimen is chucked to a movable arm so that its TD direction is parallel to the vertical direction, and the measurement is performed using the same principle. The Gurley flexibility was measured in both the MD and TD directions. Furthermore, based on the Gurley flexibility measured in this way, the direction in which the Gurley flexibility was high was designated as the first direction and the direction in which the Gurley flexibility was low was designated as the second direction for each embodiment, and the ratio of the Gurley flexibility in the first direction to the Gurley flexibility in the second direction (1st / 2nd) was determined. In order to increase the stiffness of the thermal expansion sheet in the MD direction and facilitate bending in the TD direction, the MD direction is the first direction and the TD direction is the second direction, and the ratio of the Gurley flexibility in the MD direction to the Gurley flexibility in the TD direction (MD / TD) is preferably 1.1 or higher, more preferably 1.5 or higher, and more preferably 2.0 or higher.

[0116] <<<Shape Retention>>> Shape retention was evaluated by the following method. A thermal expansion sheet was cut to 20 mm x 20 mm before heating and expansion. As shown in Figure 4, the test piece was folded 180° in the center, and a 200 g weight was placed on the fold for 5 seconds to perform the folding process. Five seconds after removing the weight, the angle A between both ends of the test piece and the fold was measured with a protractor, and the shape retention was evaluated from the measured value. When the angle A is small, the shape retention of the thermal expansion sheet 1 can be evaluated as high. When evaluating the shape retention in the MD direction, the folding process was performed so that the fold was perpendicular to the MD direction, and when evaluating the shape retention in the TD direction, the folding process was performed so that the fold was perpendicular to the TD direction. Furthermore, based on angle A, in each embodiment, among the MD and TD directions, the direction in which the Gurley flexibility was high in the aforementioned evaluation of Gurley flexibility was designated as the first direction, and the direction in which the Gurley flexibility was low was designated as the second direction. The ratio of angle A in the second direction to angle A in the first direction (second / first) was then determined. In order to increase the stiffness of the thermal expansion sheet in the MD direction and facilitate bending in the TD direction, the MD direction is the first direction and the TD direction is the second direction, and the ratio of angle A in the TD direction to angle A in the MD direction (TD / MD) is preferably 0.95 or less, more preferably 0.93 or less, and even more preferably 0.91 or less.

[0117] <<<Tackiness Evaluation>>> Tackiness was evaluated using a tacking tester (Lesca "TAC1000"). The evaluation was conducted under room temperature conditions (23°C), with the probe and stage temperatures set to 23°C, 40°C, and 60°C. The thermal expansion sheet 1 was placed on the stage with the adhesive layer side facing upwards before heating and expansion. A 5 mm diameter probe was pressed against the sample at a pressing speed of 1.0 mm / second and a pressing load of 200 gf. The load of 10 gf was held for 1 second, and the probe was pulled up at a pulling speed of 10.0 mm / second. The peak value (gf) at the time of pulling up was read, and the tack value was calculated using the following formula. A tack value of 5 gf or less was judged as ○. Tack value (gf) = (Peak value when the sample is placed on the stage and measured) - (Peak value when the sample is not placed on the stage) <<<Shear adhesive strength>>> A thermal expansion sheet cut to 12.5 x 25 mm before heating and expansion was fixed to an SPCC board using a 110°C rubber roll. Spacers with a thickness of 0.175 mm were placed on both sides of the thermal expansion sheet, and another SPCC board was placed on top of them. The gap between the SPCC boards was fixed using a fixing jig (clamp, etc.). The thermal expansion sheet between the SPCC boards was heated to 160°C at a heating rate of 50°C / min, and then held at 160°C for 5 min to expand and harden. This was used as a sample for evaluating shear adhesive strength. At this time, the gap between the two SPCC boards was fixed at 0.175 mm. Using a universal testing machine (AGS-10kNX manufactured by Shimadzu Corporation, load cell capacity: 10kN), two SPCC plates of the shear adhesion strength evaluation sample were pulled in opposite directions along the surface direction of the sample at a test speed of 5 mm / min in a 200°C atmosphere, and the applied pressure at which the sample broke was defined as the shear adhesion strength.

[0118]

[0119] <<Discussion>> As shown in Examples 1 to 12 in Table 3, we were able to realize a thermally expandable sheet having an adhesive layer formed from a resin composition of various types, in which the Gurley flexibility differs between a first direction (for example, the MD direction) and a second direction (for example, the TD direction), which are different from each other. With these thermally expandable sheets, it is possible to increase the Gurley flexibility in one of the first and second directions while also increasing the bendability (shape retention) in the other of the first and second directions. In particular, Examples 3 to 5, 7 to 10 and 12, in which the average degree of orientation of the filler is 40° or less and the proportion of fillers with an orientation of less than 45° is 55% or more, are preferable because the difference in the Gurley flexibility between the MD direction and the TD direction of the thermally expandable sheet can be made to a degree that is clearly distinguishable, such as 5 or more, 10 or more, and 20 or more. Furthermore, a comparison between Example 8 and Example 11 shows that by using a thermal expansion sheet in which the average degree of orientation of the filler is 40° or less, or in which the proportion of fillers with an orientation of less than 45° is 55% or more, it is possible to sufficiently increase the Gurley flexibility in the MD direction even with a small filler content, and to achieve a value that is clearly larger than the Gurley flexibility in the TD direction. As a result, it is particularly preferable because it can achieve not only stiffness in the MD direction and ease of bending in the TD direction, but also higher adhesive strength.

[0120] The results from Examples 3, 4, 7, and 8 show that the effects of the present invention described above can be obtained regardless of the filler content or shape. Furthermore, regarding the aspect ratio of the filler, it is not limited to those given in the examples, but as mentioned above, when the aspect ratio is greater than 1, it tends to be easier to control the degree of orientation of the filler.

[0121] The epoxy resin used in this embodiment is not limited to that which is used here. Other types can be used as appropriate, depending on the required properties such as adhesive strength and tackiness.

[0122] In this embodiment, an example containing an elastomer is given, but the elastomer is not essential to achieve the effects of the present invention. As shown in Examples 1 to 12, an elastomer within a suitable molecular weight range can be used to increase the degree of filler orientation by adjusting the viscosity of the resin composition, but the viscosity of the resin composition can also be controlled by changing the type of epoxy resin used in combination, so from this point of view as well, the elastomer is not an essential component.

[0123] In addition, insertability tests were conducted on the thermal expansion sheets of Examples 1 to 12. A thermal expansion sheet cut to 30 mm x 100 mm before heating and a commercially available stator core for automobile motors were prepared. The thermal expansion sheet was bent into a U-shape in the TD direction to match the shape of the slot in the stator core, and the thermal expansion sheet was inserted into the slot along the MD direction. In all cases of the thermal expansion sheets of Examples 1 to 12, it was possible to insert them into the slot properly while maintaining the bent shape. Thus, the thermal expansion sheets of Examples 1 to 12 showed good insertability.

[0124] According to the present invention, it is possible to provide a thermal expansion sheet that exhibits sufficiently high insertability even when the thermal expansion sheet is folded and inserted into a gap formed by multiple adherends. The thermal expansion sheet of the present invention is useful for electrical equipment. In particular, the adhesive sheet of the present invention is useful as an adhesive sheet for bonding coils to slots in the stator core or rotor core in rotating electrical machines such as motors and generators of electric vehicles and hybrid vehicles.

[0125] 1. Thermal expansion sheet 10. Substrate 20a, 20b. Adhesive layer 30a, 30b. Primer layer

Claims

1. A thermal expansion sheet that is placed between multiple adherends and bonds these adherends to each other by thermal expansion, wherein the thermal expansion sheet comprises a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin, and a curing agent, and the ratio of the Gurley flexibility of the thermal expansion sheet in the MD direction to the Gurley flexibility of the thermal expansion sheet in the TD direction (MD direction / TD direction) is 1.1 or more.

2. A thermal expansion sheet that is placed between multiple adherends and bonds these adherends to each other by thermal expansion, wherein the thermal expansion sheet has a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin, and a curing agent, the filler includes flake-shaped, plate-shaped, needle-shaped, fibrous, or branch-shaped fillers, and the average degree of orientation of the filler in the thermal expansion sheet before thermal expansion is 40° or less. Here, the degree of orientation of the filler is the angle between the long axis direction of the filler and the MD direction of the thermal expansion sheet when observed by SEM from the thickness direction of the thermal expansion sheet before thermal expansion.

3. A thermal expansion sheet that is placed between multiple adherends and bonds these adherends to each other by thermal expansion, wherein the thermal expansion sheet has a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin, and a curing agent, the filler includes flake-shaped, plate-shaped, needle-shaped, fibrous, or branch-shaped fillers, and the proportion of fillers having an orientation of less than 45° in the thermal expansion sheet before thermal expansion is 55% or more of the total filler: Here, the orientation of the filler is the angle between the long axis direction of the filler and the MD direction of the thermal expansion sheet when observed by SEM from the thickness direction of the thermal expansion sheet before thermal expansion.

4. A thermal expansion sheet that is placed between a plurality of adherends and bonds these adherends to each other by thermal expansion, wherein the thermal expansion sheet has a substrate with a thickness of 1 to 200 μm and an adhesive layer with a thickness of 10 to 200 μm laminated on at least one side of the substrate, the adhesive layer contains a filler, an epoxy resin, a curing agent, and an elastomer, the elastomer includes an elastomer having a glass transition temperature (Tg) of 100°C or higher, and the thermal expansion sheet, before thermal expansion, has a Gurley flexibility in the MD direction greater than the Gurley flexibility in the TD direction.

5. The thermal expansion sheet according to any one of claims 1 to 4, wherein the adhesive layer is formed by coating a resin composition containing the components constituting the adhesive layer and a solvent onto a substrate at a coating speed of 50 to 200 mm / sec, and then removing the solvent.

6. The thermal expansion sheet according to any one of claims 1 to 4, wherein the adhesive layer is formed using a resin composition comprising the components constituting the adhesive layer and a solvent, and having a solid content concentration of 25 to 75%.

7. The thermal expansion sheet according to any one of claims 1 to 4, wherein the Gurley flexibility of the thermal expansion sheet in the MD direction is 53.5 mgf or more.

8. The thermal expansion sheet according to any one of claims 1 to 4, wherein the substrate includes a metal film, a resin film, or a nonwoven fabric.

9. The thermal expansion sheet according to any one of claims 1 to 4, wherein the filler contains a filler having an aspect ratio of 1.5 or more and 80 or less.

10. The thermal expansion sheet according to any one of claims 1 to 4, wherein the content of the filler is 5% by mass or more and less than 80% by mass, based on 100% by mass of the adhesive layer.

11. The thermal expansion sheet according to any one of claims 1 to 4, wherein the epoxy resin contains an epoxy resin having a softening point of 60°C or higher.

12. The thermal expansion sheet according to any one of claims 1 to 4, wherein the epoxy resin contains an epoxy resin with an epoxy equivalent of less than 300.

13. The thermal expansion sheet according to any one of claims 1 to 4, wherein the adhesive layer contains two or more epoxy resins, and at least one of the epoxy resins has a molecular weight of 10,000 or more.

14. The thermal expansion sheet according to claim 4, wherein the elastomer contains an elastomer with a molecular weight of 100,000 or more.

15. A thermal expansion sheet according to any one of claims 1 to 4, wherein, before heating and expansion, the shape retention in the TD direction is higher than the shape retention in the MD direction.

16. The thermal expansion sheet according to any one of claims 1 to 4, wherein the coefficient of dynamic friction of the surface before thermal expansion is 0.6 or less.

17. A thermally expandable sheet according to any one of claims 1 to 4, wherein the shear adhesive strength after thermal expansion and curing is 0.8 MPa or more at 23°C and 0.1 MPa or more when heated to 200°C.

18. An article comprising a thermal expansion sheet as described in any one of claims 1 to 4.

19. The article according to claim 18, wherein the article is a motor.