Curing accelerator for epoxy resin, and thermosetting composition containing said curing accelerator

A novel curing accelerator for epoxy resins addresses fluidity and curability issues in semiconductor encapsulation, ensuring safe and efficient encapsulation with reduced benzene generation, improving device reliability and lifespan.

WO2026239772A1PCT designated stage Publication Date: 2026-11-19SAN APRO LTD
0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/013916
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-04-02
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing epoxy resin compositions used for encapsulating semiconductor devices suffer from insufficient fluidity and curability, leading to void formation and wire deformation, and generate benzene as a pollutant during curing, posing health and environmental risks.

Method used

A novel curing accelerator for epoxy resins, composed of specific anionic and neutral ligands coordinated with a cation, exhibits a moderately delayed curing acceleration effect, maintaining fluidity and suppressing benzene generation, ensuring safe and efficient encapsulation of semiconductor devices.

Benefits of technology

The curing accelerator provides appropriate fluidity and curability for encapsulation, forming a cured product with excellent heat resistance and other properties while minimizing benzene generation, enhancing the reliability and lifespan of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026013916_19112026_PF_FP_ABST
    Figure JP2026013916_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a novel curing accelerator for an epoxy resin that exhibits an appropriate delayed curing accelerating effect matching the sealing / molding cycle of a semiconductor element at sealing treatment temperature. A curing accelerator for an epoxy resin according to the present invention contains a salt composed of an anionic ligand represented by formula (a), a neutral ligand represented by formula (ah), and a cation represented by formula (c), or a salt composed of an anionic ligand having a structure in which an anionic ligand represented by formula (a) and a neutral ligand represented by formula (ah) are bonded via a silicon atom, and a cation represented by formula (c).
Need to check novelty before this filing date? Find Prior Art

Description

Curing accelerator for epoxy resins, and thermosetting composition containing the curing accelerator.

[0001] The present invention relates to a novel curing accelerator for epoxy resins, and a thermosetting composition comprising the curing accelerator that is suitable as a semiconductor device encapsulant and the like.

[0002] Semiconductor devices such as IC chips are susceptible to degradation due to external factors such as heat, humidity, light, and physical shock. Therefore, semiconductor devices are often protected by encapsulating them in a hardened encapsulant.

[0003] The sealing materials used in this manner are required to possess properties such as heat resistance, moisture resistance, impact resistance, electrical insulation, adhesion, dimensional stability, and thermal stress relaxation.

[0004] In recent years, semiconductor elements have become more densely packed and integrated to meet the demands of miniaturization, weight reduction, and increased functionality of electronic devices. Consequently, wires are becoming thinner and thinner, and the gap between semiconductor elements and substrates is becoming increasingly narrow. This has led to problems such as void formation and wire deformation or breakage when filling the encapsulant around semiconductor elements.

[0005] Therefore, in addition to the aforementioned performance, the encapsulating material is required to possess both fluidity and curability at the encapsulation processing temperature. Specifically, it is required to maintain good fluidity by suppressing the progression of curing while filling around the semiconductor element, and to cure rapidly after filling.

[0006] Patent Document 1 discloses a composition comprising an epoxy resin, a curing agent, an inorganic filler, and a phosphonium salt represented by the following formula (x) as a sealing material having good fluidity and curability during sealing molding. However, the fluidity and curability of the above composition were still insufficient.

[0007]

[0008] Furthermore, a problem with thermosetting compositions containing the phosphonium salt represented by formula (x) is that a large amount of benzene derived from the phosphonium salt is generated during curing. This is because benzene is an environmental pollutant and continuous ingestion may harm human health.

[0009] Japanese Patent Publication No. 2007-161832

[0010] Therefore, an object of the present invention is to provide a novel epoxy resin curing accelerator that exhibits a moderately delayed curing acceleration effect at the encapsulation temperature, corresponding to the encapsulation molding cycle of a semiconductor device. Another object of the present invention is to provide a novel epoxy resin curing accelerator that exhibits a moderately delayed curing acceleration effect at the encapsulation temperature, corresponding to the encapsulation molding cycle of a semiconductor device, and that suppresses the generation of benzene when exhibiting the curing acceleration effect. Another object of the present invention is to provide a thermosetting composition that, at the encapsulation temperature, possesses fluidity and curability corresponding to the encapsulation molding cycle of a semiconductor device, and forms a cured product with excellent heat resistance and other properties upon curing. Another object of the present invention is to provide a thermosetting composition that, at the encapsulation temperature, possesses fluidity and curability corresponding to the encapsulation molding cycle of a semiconductor device, and forms a cured product with excellent heat resistance and other properties by curing while suppressing the generation of benzene.

[0011] The inventors of the present invention have diligently studied to solve the above problems and have found the following: 1. The following salt has delayed decomposition properties, decomposing over an appropriate period of time at the sealing treatment temperature, and exhibits a moderately delayed curing acceleration effect on epoxy resin that is commensurate with the sealing molding cycle. 2. The following salt generates less benzene when decomposed compared to the phosphonium salt represented by formula (x) above, thus reducing the environmental burden. 3. By adding the following salt to a composition containing epoxy resin and a curing agent, a thermosetting composition is obtained that combines fluidity, curability, and safety, and is suitable for sealing semiconductor devices. The present invention was completed based on these findings.

[0012] In other words, the present invention provides a curing accelerator for epoxy resins comprising a salt composed of an anionic ligand represented by the following formula (a), a neutral ligand represented by the following formula (ah), and a cation represented by the following formula (c), or a salt composed of an anionic ligand having a structure in which the anionic ligand represented by the following formula (a) and the neutral ligand represented by the following formula (ah) are bonded via a silicon atom, and a cation represented by the following formula (c). [In the formula, R 1 The '' represents an alkyl group having 1 to 3 carbon atoms. Ring Z represents an aromatic hydrocarbon ring which may have substituents, or a structure in which two or more aromatic hydrocarbon rings which may have substituents are linked by a single bond or a linking group. m1 and m2 represent the same number from 0.5 to 1, and m3 represents the number from 0.5 to 1.5. The benzene ring shown in the formula may have substituents.

[0013] The present invention also provides a curing accelerator for epoxy resins, wherein the salt is a salt represented by the following formula (1-1). [In the formula, R 1 This represents an alkyl group having 1 to 3 carbon atoms, and the ring Z 1 This represents an aromatic hydrocarbon ring which may have substituents. The benzene ring shown in the formula may have substituents.

[0014] The present invention also provides a curing accelerator for epoxy resins, wherein the salt is a salt represented by the following formula (1-2). [In the formula, R 1 R represents an alkyl group having 1 to 3 carbon atoms. 2 This indicates an organic group. Ring Z 1 This represents an aromatic hydrocarbon ring which may have substituents. The benzene ring shown in the formula may have substituents.

[0015] The present invention also provides a curing accelerator for epoxy resins, wherein the salt is a salt represented by the following formula (1-3). [In the formula, R 1 * represents an alkyl group having 1 to 3 carbon atoms. m1 and m2 are the same, representing a number between 0.5 and 1, and m3 represents a number between 0.5 and 1.5. The benzene ring shown in the formula may have substituents.

[0016] The present invention also relates to the ring Z 1 The present invention provides a curing accelerator for epoxy resins, which is a benzene ring or a naphthalene ring, which may have substituents.

[0017] The present invention further provides the curing accelerator for epoxy resins, wherein the salt contains the salt represented by the formula (1-2) and does not contain the compound represented by the following formula (2), or the salt contains the salt represented by the formula (1-2) and contains the compound represented by the following formula (2), and the content of the compound represented by the formula (2) is 10% by weight or less of the content of the salt represented by the formula (1-2). (wherein, R 2 , ring Z 1 are the same as defined above. R 4 represents an alkyl group)

[0018] The present invention further provides a thermosetting composition comprising the curing accelerator for epoxy resins, an epoxy resin, and a curing agent.

[0019] The present invention further provides the thermosetting composition, wherein the epoxy resin is a compound represented by the following formula (e). (wherein, ring Z 2 represents an aromatic hydrocarbon ring. Ring Z 3 represents an aromatic hydrocarbon ring, or a linked ring in which two or more aromatic hydrocarbon rings are bonded via a single bond or a linking group. The aromatic hydrocarbon ring may have a substituent. R 11 to R 14 are the same or different and each represent a hydrogen atom or an alkyl group. n 1 represents a number of 0 or more, and n 2 represents a number of 1 or more)

[0020] The present invention further provides the thermosetting composition, wherein the curing agent is a compound represented by the following formula (p). (wherein, ring Z 4 represents an aromatic hydrocarbon ring. Ring Z 5 represents an aromatic hydrocarbon ring, or a linked ring in which two or more aromatic hydrocarbon rings are bonded via a single bond or a linking group. The aromatic hydrocarbon ring may have a substituent. R 15 to R 18 are the same or different and each represent a hydrogen atom or an alkyl group. n 3 represents a number of 0 or more, and n 4 represents a number of 1 or more)

[0021] The epoxy resin curing accelerator of the present invention contains a salt having a phosphonium cation coordinated with an anionic ligand or a silicate anionic ligand. The epoxy resin curing accelerator has a moderately delayed decomposition property that matches the encapsulation molding cycle of semiconductor devices. Specifically, it decomposes after a moderate amount of time that matches the time required to fill the semiconductor device during the encapsulation process. When the epoxy resin curing accelerator decomposes, the anionic ligand or silicate anionic ligand and the phosphonium cation work together to rapidly initiate the ring-opening reaction of the epoxy resin.

[0022] Furthermore, the aforementioned epoxy resin curing accelerator is highly safe because it does not generate much benzene even when decomposed.

[0023] Furthermore, because the thermosetting composition of the present invention contains the epoxy resin curing accelerator, there is an appropriate time lag between heating and the start of curing that matches the encapsulation molding cycle of the semiconductor device. That is, at the encapsulation temperature, viscosity is suppressed for a certain period of time, and excellent fluidity can be maintained. Therefore, even with semiconductor devices that have become denser and more integrated, the thermosetting composition can be filled around the semiconductor device while suppressing the generation of voids and the deformation and breakage of wires. After the elapsed time, the curing reaction accelerating effect of the epoxy resin curing accelerator comes into play, the crosslinking reaction between the epoxy resin and the curing agent proceeds rapidly, and a cured product is quickly formed.

[0024] Furthermore, the aforementioned thermosetting composition is highly safe because it does not easily generate benzene derived from epoxy resin curing accelerators during curing.

[0025] Since the cured product of the thermosetting composition has a high degree of crosslinking, it possesses properties derived from epoxy resin (for example, heat resistance, moisture resistance, impact resistance, electrical insulation, adhesion, thermal stress relaxation, etc.). Therefore, when a semiconductor element is coated or filled with the cured product, degradation of the semiconductor element due to external factors such as heat, moisture, light, and physical impact is suppressed.

[0026] Therefore, the thermosetting composition can be suitably used for encapsulation applications of semiconductor devices (especially high-density and highly integrated semiconductor devices) (for example, transfer encapsulation molding applications), and can contribute to improving the reliability and extending the lifespan of semiconductor devices.

[0027] [Curing accelerator for epoxy resins] The curing accelerator for epoxy resins of the present invention is a compound that has the effect of promoting the ring-opening reaction of epoxy resins (for example, epoxy resins described later), and comprises the following salt (1) or salt (2).

[0028] Salt (1) is a salt composed of an anionic ligand represented by the following formula (a), a neutral ligand represented by the following formula (ah), and a cation represented by the following formula (c) (more specifically, a phosphonium cation).

[0029] Salt (2) is a salt composed of an anionic ligand having a structure in which an anionic ligand represented by the following formula (a) and a neutral ligand represented by the following formula (ah) are bonded via a silicon atom (in this specification, this may be referred to as a "silicate anionic ligand") and a cation represented by the following formula (c) (more specifically, a phosphonium cation).

[0030]

[0031] That is, salt (1) is the salt represented by formula (1) below, and salt (2) is the salt represented by formula (2) below. In the formula below, the anionic ligand represented by formula (a') is a silicate anionic ligand.

[0032]

[0033] In the above formula, R 1 R represents an alkyl group having 1 to 3 carbon atoms. 2 represents an organic group. Ring Z represents an aromatic hydrocarbon ring which may have substituents, or a structure in which two or more aromatic hydrocarbon rings which may have substituents are linked by a single bond or a linking group. m1 and m2 are the same and represent a number from 0.5 to 1, and m3 represents a number from 0.5 to 1.5. The benzene ring shown in the formula may have substituents.

[0034] R​1 The alkyl group has 1 to 3 carbon atoms, and examples include methyl, ethyl, propyl, and isopropyl groups. Among these, methyl or ethyl groups are preferred, and methyl groups are particularly preferred.

[0035] R 2 The group is an organic group, and examples include monovalent hydrocarbon groups, monovalent heterocyclic groups, and substituted oxy groups (e.g., alkoxy groups, aryloxy groups, aralkyloxy groups, acyloxy groups, etc.). Examples of the hydrocarbon group include aliphatic hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups.

[0036] R 2 Preferably, the carbon atom is a monovalent hydrocarbon group or a monovalent heterocyclic group, more preferably a monovalent hydrocarbon group, even more preferably a monovalent aromatic hydrocarbon group, such as a phenyl group or a naphthyl group. 6-14 An aryl group is particularly preferred.

[0037] Ring Z may have substituents, or it may have a structure in which two or more substituents are bonded together by a single bond or a linking group. Examples of the aromatic hydrocarbon rings include aromatic hydrocarbon rings having 6 to 14 carbon atoms, such as benzene rings, naphthalene rings, fluorene rings, and anthracene rings.

[0038] The linking group is a divalent group having one or more atoms, and examples include a divalent hydrocarbon group, a carbonyl group (-CO-), an ether bond (-O-), a thioether bond (-S-), an ester bond (-COO-), an imino group (-NH-), an amide bond (-CONH-), a carbonate bond (-OCOO-), and a group formed by linking multiple such groups.

[0039] Examples of the above-mentioned divalent hydrocarbon groups include linear or branched alkylene groups having 1 to 18 carbon atoms, such as methylene, methylmethylene, dimethylmethylene, ethylene, propylene, and trimethylene groups, and cycloalkylene groups (including cycloalkylidene groups) having 3 to 18 carbon atoms, such as 1,2-cyclopentylene, 1,3-cyclopentylene, cyclopentylidene, 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, and cyclohexylidene groups.

[0040] The ring Z is preferably a benzene ring which may have substituents, a naphthalene ring which may have substituents, or a 9,9-diphenyl-9H-fluorene ring which may have substituents, with a naphthalene ring which may have substituents being particularly preferred.

[0041] Examples of substituents that ring Z may have include halogen groups, hydroxyl groups, and substituted oxy groups (e.g., C 1-4 Alkoxy groups (e.g., methyl group, ethyl group, etc.) 1-4 Examples include alkyl groups.

[0042] The OH group and O shown in formula (a) - The group and the two OH groups shown in formula (ah) are preferably bonded to carbon atoms constituting the aromatic hydrocarbon ring of ring Z. If ring Z contains one aromatic hydrocarbon ring, the OH group shown in formula (a) and O - The group and the two OH groups shown in formula (ah) are carbon atoms constituting the aromatic hydrocarbon ring, and it is preferable that they are bonded to adjacent carbon atoms. When ring Z contains two or more aromatic hydrocarbon rings, the OH group shown in formula (a) and O - The group and the two OH groups shown in formula (ah) may be bonded to one aromatic hydrocarbon ring (for example, adjacent carbon atoms that make up one aromatic hydrocarbon ring) or to separate aromatic hydrocarbon rings.

[0043] Furthermore, the substituents that the benzene ring bonded to the phosphonium cation may have include, for example, alkyl groups (e.g., methyl group, ethyl group, etc.). 1-4Alkyl groups), aryl groups (for example, C such as phenyl groups) 6-14 Examples include aryl groups.

[0044] m1 and m2 both represent the same number between 0.5 and 1, with 1 being preferred.

[0045] m3 represents a number between 0.5 and 1.5, preferably between 0.5 and 1.2, more preferably between 0.6 and 1.2, and even more preferably between 0.6 and 1.0.

[0046] As salt (1), salts represented by the following formula (1-1) and salts represented by the following formula (1-3) are preferred.

[0047] As for salt (2), a salt represented by the following formula (1-2) is preferred.

[0048]

[0049] R in the above formula 1 , R 2 m1, m2, and m3 are the same as described above. Ring Z 1 This represents an aromatic hydrocarbon ring which may have substituents. The benzene ring and fluorene ring shown in the formula may have further substituents.

[0050] Ring Z 1 Examples of aromatic hydrocarbon rings in ring Z include those similar to those in ring Z. 1 Among these, a benzene ring which may have substituents and a naphthalene ring which may have substituents are preferred, and a naphthalene ring which may have substituents is particularly preferred. Furthermore, examples of substituents are the same as those that may be present on the aromatic hydrocarbon ring in ring Z.

[0051] The substituents that the benzene ring bonded to the phosphonium cation may have include, for example, alkyl groups (e.g., methyl group, ethyl group, etc.). 1-4 Alkyl groups), aryl groups (for example, C such as phenyl groups) 6-14 Examples include aryl groups.

[0052] The substituents that the fluorene ring and the benzene ring bonded to the carbon atom at position 9 of the fluorene ring may have include, for example, a halogen group, a hydroxyl group, and a substituted oxy group (for example, C 1-4 Alkoxy groups (e.g., methyl group, ethyl group, etc.) 1-4 Examples include alkyl groups.

[0053] The salt represented by the above formula (1-1) has a structure in which 1 mole of phosphonium cation is coordinated with 1 mole of an anionic ligand and 1 mole of a neutral ligand.

[0054] Furthermore, the anionic ligand in formula (1-1) has an OH group and O attached to two adjacent carbon atoms in the aromatic hydrocarbon ring. - Each group has a structure in which they are bonded together. In addition, the neutral ligand in formula (1-1) has a structure in which one OH group is bonded to each of two adjacent carbon atoms contained in the aromatic hydrocarbon ring.

[0055] The anionic ligand in formula (1-1) has a bulky aromatic ring and a hydroxyl group is bonded to the α-carbon atom, resulting in low nucleophilicity.

[0056] The salt represented by the above formula (1-2) has a structure in which one mole of silicate anion ligand is coordinated to one mole of phosphonium cation.

[0057] Furthermore, the silicate anion ligand has a structure in which two adjacent carbon atoms constituting the first aromatic hydrocarbon ring and two adjacent carbon atoms constituting the second aromatic hydrocarbon ring are bonded to one silicon atom via an oxygen atom. Therefore, the silicate anion ligand has a bulky aromatic ring and low nucleophilicity because four oxygen atoms are bonded to the silicon atom.

[0058] The salt represented by the above formula (1-3) has a structure in which m1 mole of phosphonium cation is coordinated with m2 moles of anionic ligand and m3 moles of neutral ligand.

[0059] In formula (1-3), m1 and m2 are preferably 1.

[0060] In formula (1-3), the value of m3 is preferably between 0.5 and 1.2, more preferably between 0.6 and 1.2, even more preferably between 0.6 and 1.0, even more preferably between 0.6 and 0.9, and particularly preferably between 0.7 and 0.8.

[0061] m2 + m3 is a number between 1 and 2.5, with 1 to 2 being preferred, 1.3 to 2.0 being more preferred, 1.5 to 2.0 being even more preferred, and 1.6 to 1.9 being particularly preferred.

[0062] The molar ratio of [phosphonium cation / (anionic ligand and neutral ligand)] constituting the salt represented by formula (1-3) is, for example, 1 / 1 to 1 / 2, preferably 1 / 1.5 to 1 / 2, more preferably 1 / 1.6 to 1 / 2, and even more preferably 1 / 1.6 to 1 / 1.9.

[0063] The two benzene rings in the anionic ligand in formula (1-3) are, respectively, an OH group or an O group. - It has a group. An OH group or O in the benzene ring. - The bonding position of the group is preferably the meta or para position relative to the bonding position with the carbon atom at position 9 of the fluorene ring, with the para position being particularly preferred.

[0064] The two benzene rings in the neutral ligand in formula (1-3) each have an OH group. The bonding position of the OH group on the benzene ring is preferably the meta or para position relative to the bonding position with the carbon atom at position 9 of the fluorene ring, with the para position being particularly preferred.

[0065] As described above, the salt is stable because it has an anionic ligand or silicate anionic ligand with low nucleophilicity, and it exhibits delayed decomposition properties, meaning it does not decompose immediately even when subjected to heat treatment. When the salt decomposes due to heat, a phosphonium cation and an anionic ligand or silicate anionic ligand are produced.

[0066] When the salt is decomposed while mixed with epoxy resin, the generated phosphonium cations gather around the oxygen atom of the epoxy group of the epoxy resin, localizing the oxygen atom. In other words, it enhances the δ- charge. The epoxy group of the epoxy resin has a three-membered ring structure formed by two carbon atoms and one oxygen atom, with the carbon atom being δ+ charged and the oxygen atom being δ- charged.

[0067] Furthermore, the anionic ligand or silicate anionic ligand generated by decomposing the salt nucleophilically attacks the carbon atoms constituting the epoxy group. At this time, as described above, the oxygen atoms constituting the epoxy group are localized by the action of the phosphonium cation, so when the carbon atoms are nucleophilically attacked, the bond between the oxygen atoms and the carbon atoms is easily broken, and the epoxy group opens its ring. This initiates the ring-opening reaction of the epoxy resin, accelerating its curing.

[0068] The curing-accelerating effect of phosphonium cations and anionic ligands or silicate anionic ligands on epoxy resins is suppressed while the anionic ligand or silicate anionic ligand coordinates to and neutralizes the phosphonium cation, existing as a salt. However, once the salt decomposes, the effect is rapidly realized. The epoxy resin curing accelerator of the present invention contains a salt with such properties, and therefore exhibits a delayed curing-accelerating effect on epoxy resins.

[0069] The salt represented by formula (1-1) is preferably the salt represented by the following formula (1-1-1) and the salt represented by the following formula (1-1-2), with the salt represented by the following formula (1-1-1) being particularly preferred.

[0070] R in the above formula 1 The same applies as above. R 5 represents a hydrogen atom or a hydroxyl group. The benzene ring and naphthalene ring in the above formula may have substituents other than the groups shown in the above formula.

[0071] The salt represented by formula (1-2) is preferably the salt represented by the following formula (1-2-1) and the salt represented by the following formula (1-2-2), with the salt represented by the following formula (1-2-1) being particularly preferred.

[0072] R in the above formula 1 , R 2 The same applies as described above. The benzene ring and naphthalene ring in the above formula may have substituents other than the groups shown in the above formula.

[0073] As the salt represented by formula (1-3) above, the salt represented by the following formula (1-3-1) is preferred.

[0074] R in the above formula 1 m1, m2, and m3 are the same as described above. The benzene ring and fluorene ring in the above formula may have substituents other than the groups shown in the above formula.

[0075] The melting point of the salt is, for example, 40 to 200°C, preferably 100 to 200°C, more preferably 130 to 190°C, even more preferably 150 to 190°C, and particularly preferably 170 to 190°C, as it is easily melted into the resin.

[0076] The aforementioned salt has a delayed curing-accelerating effect, and there is a suitable time lag between heating and the manifestation of the curing-accelerating effect. If the time lag is too large, it will lead to a decrease in work efficiency, but when using the aforementioned salt, the gel time is about 3 to 30 minutes at a curing temperature of 160°C. By adding the aforementioned salt to the semiconductor device encapsulant, it is possible to secure a suitable working time for filling work in the encapsulation process, thereby improving work efficiency.

[0077] Furthermore, the aforementioned salt does not easily generate benzene even when decomposed. The amount of benzene generated by the method described in the examples is, for example, 100 ppm or less, preferably 80 ppm or less, and more preferably 60 ppm or less. Therefore, it is highly safe.

[0078] Furthermore, the phosphonium cations produced by the decomposition of the salt (especially the salt represented by formula (1-2)) have low nucleophilicity. Therefore, even if the thermosetting composition containing the salt contains chlorine impurities (for example, chlorine compounds derived from epichlorohydrin, a raw material for the manufacture of epoxy resins), free chlorine (Cl) is not released from the chlorine impurities. - This can suppress the generation of free chlorine (Cl -This prevents corrosion caused by [unspecified factor]. The amount of chlorine generated by the method described in the examples is, for example, 20 ppm or less, preferably 15 ppm or less, and more preferably 10 ppm or less. Therefore, the semiconductor device encapsulant obtained using the salt has high electrical reliability.

[0079] The salt represented by formula (1-1) can be produced, for example, by reacting a phosphonium salt represented by the following formula (a1) with a phenol represented by the following formula (c1) in the presence of a solvent. 1 , ring Z 1 The same applies as above. Also, X in the following equation - This represents a monovalent counter anion, and examples include halogen anions, sulfate anions, nitrate anions, phosphate anions, sulfonate anions, carboxylate anions, and carbonate anions.

[0080] Examples of the aforementioned solvents include alcohol-based solvents such as methanol, ethanol, propanol, and butanol; and ester-based solvents such as butyl acetate and ethyl acetate. These can be used individually or in combination of two or more.

[0081] The amount of solvent used is, for example, 50 to 300% by weight relative to the substrate (the total amount of the phosphonium salt represented by formula (a1) below and the phenols represented by formula (c1) below).

[0082]

[0083] The salt represented by formula (1-2) can be produced, for example, by reacting a phenol represented by formula (c1) with a silane compound represented by formula (d) in the presence of an alkali metal hydroxide (MOH) and a solvent to produce an alkali metal salt of silicate represented by formula (c2), and then reacting the resulting alkali metal salt of silicate with a phosphonium salt represented by formula (a1) in the presence of a solvent.

[0084] R in the following equation 1 , R 2 , ring Z 1 , X - The same applies as above. R 4represents an alkyl group, preferably C 1-3 It is an alkyl group. + This represents an alkali metal ion, preferably a sodium ion.

[0085]

[0086] Examples of the solvent include alcohol-based solvents such as methanol, ethanol, propanol, and butanol; and ester-based solvents such as butyl acetate and ethyl acetate. These can be used individually or in combination of two or more. Among the solvents, it is preferable to include an ester-based solvent, as this suppresses the by-product formation of the compound represented by formula (2) below, yields a reaction product containing the salt represented by formula (1-2) in high purity, and exhibits an excellent delayed curing acceleration effect. The solvent preferably contains 60% by weight or more of the ester-based solvent, more preferably 70% by weight or more, even more preferably 80% by weight or more, particularly preferably 90% by weight or more, and most preferably 95% by weight or more. (In the formula, R 2 , R 4 , ring Z 1 (The same applies as above.)

[0087] The amount of solvent used is, for example, 50 to 300% by weight relative to the substrate (the total amount of phenols represented by formula (c1), silane compounds represented by formula (d), and phosphonium salts represented by formula (a1)).

[0088] The salts represented by formulas (1-3) can be produced, for example, by reacting a phosphonium salt represented by formula (a2) below with a hydroxyphenylfluorene compound represented by formula (c3) below in the presence of a solvent. 1 , m1, m2, m3, X - The same applies as above.

[0089] Examples of the aforementioned solvents include alcohol-based solvents such as methanol, ethanol, propanol, and butanol; and ester-based solvents such as butyl acetate and ethyl acetate. These can be used individually or in combination of two or more.

[0090] The amount of solvent used is, for example, 50 to 300% by weight relative to the substrate (phosphonium salt represented by the following formula (a2) and hydroxyphenylfluorene compound represented by the following formula (c3)).

[0091]

[0092] The epoxy resin curing accelerator contains at least one selected from salt (1) and salt (2). The epoxy resin curing accelerator may also contain other components besides the salts, but the proportion of the salts in the total amount of the epoxy resin curing accelerator (the total amount if two or more types are contained) is, for example, 50% by weight or more, preferably 60% by weight or more, more preferably 70% by weight or more, even more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 99% by weight or more. The upper limit is 100% by weight.

[0093] When the epoxy resin curing accelerator contains a salt represented by formula (1-2), from the viewpoint of improving the delayed curing accelerator effect, it is preferable that the compound represented by formula (2) is not included, or if it is included, the content of the compound represented by formula (2) is 10% by weight or less, more preferably 5% by weight or less, even more preferably 3% by weight or less, and particularly preferably 1% by weight or less.

[0094] The epoxy resin curing accelerator can be manufactured through a process for manufacturing the salt.

[0095] [Thermosetting Composition] The thermosetting composition of the present invention comprises at least one salt selected from salt (1) and salt (2) (or the epoxy resin curing accelerator), an epoxy resin, and a curing agent.

[0096] In the thermosetting composition, the content of the salt (total amount if two or more types are included) is, for example, 0.5 to 10 parts by weight, preferably 1 to 5 parts by weight, per 100 parts by weight of epoxy resin.

[0097] (Epoxy resin) An epoxy resin is a compound (including oligomers and polymers) having at least one epoxy group (preferably two or more) in one molecule.

[0098] There are no particular restrictions on the epoxy resin, and examples include bisphenol-type epoxy resins (e.g., bisphenol A type epoxy resin, bisphenol F type epoxy resin, brominated bisphenol type epoxy resin), biphenyl-type epoxy resin, phenol novolac-type epoxy resin, cresol novolac-type epoxy resin, hydroquinone-type epoxy resin, stilbene-type epoxy resin, triphenolmethane-type epoxy resin, alkyl-modified triphenolmethane-type epoxy resin, triazine skeleton-containing epoxy resin, dicyclopentadiene-modified phenol-type epoxy resin, aryl aralkyl-type epoxy resin, naphthol-type epoxy resin, naphthalene-type epoxy resin, etc. These can be used individually or in combination of two or more.

[0099] As for the epoxy resin, an epoxy resin having two or more epoxy groups and two or more benzene rings in the main chain (hereinafter sometimes referred to as "polyfunctional aromatic epoxy resin") is preferred because it has excellent fluidity and yields a cured product with excellent heat resistance.

[0100] As the polyfunctional aromatic epoxy resin, a compound represented by the following formula (e) is preferred.

[0101] Ring Z in equation (e) above 2 This represents an aromatic hydrocarbon ring. Ring Z 3 This represents an aromatic hydrocarbon ring, or a linked ring in which two or more aromatic hydrocarbon rings are linked by a single bond or a linking group. The aromatic hydrocarbon ring may have substituents.

[0102] Examples of aromatic hydrocarbon rings include benzene rings, naphthalene rings, and anthracene rings, which have 6 to 14 carbon atoms.

[0103] The aromatic hydrocarbon ring may have substituents other than the group shown in the above formula. Examples of such substituents include halogeno groups, oxo groups, hydroxyl groups, and substituted oxy groups (e.g., C 1-4 Alkoxy group, C 6-10 Aryloxy group, C 7-16 Aralkyloxy group, C 1-4 Acyloxy groups, etc.), alkyl groups (e.g., methyl group, ethyl group, etc.) 1-4 (Alkyl alkyl groups, etc.), C 3-8 Examples include cycloalkyl groups.

[0104] The linking group is a divalent group having one or more atoms, and examples include a divalent hydrocarbon group, a carbonyl group (-CO-), an ether bond (-O-), a thioether bond (-S-), an ester bond (-COO-), an amide bond (-CONH-), a carbonate bond (-OCOO-), and a group formed by linking multiple such bonds. The above linking group may have substituents such as a hydroxyl group.

[0105] Examples of divalent hydrocarbon groups include linear or branched alkylene groups having 1 to 18 carbon atoms, such as methylene, methylmethylene, dimethylmethylene, ethylene, propylene, and trimethylene groups, and cycloalkylene groups having 3 to 18 carbon atoms, such as 1,2-cyclopentylene, 1,3-cyclopentylene, cyclopentylidene, 1,2-cyclohexylene, 1,3-cyclohexylene, 1,4-cyclohexylene, and cyclohexylidene groups.

[0106] Ring Z 2 Preferably, the ring is a benzene ring which may have substituents, or a naphthalene ring which may have substituents, and a benzene ring which may have substituents is particularly preferred.

[0107] Ring Z 3 Preferably, the ring is a benzene ring which may have substituents, a naphthalene ring which may have substituents, or a linked ring in which two or more rings selected from the above are linked by a single bond or a linking group.

[0108] In the above formula, "-Z 3 The group indicated by "-" is ring Z 3is a group obtained by removing two hydrogen atoms from the structural formula of, and examples thereof include groups represented by the following formulas (z-1) to (z-4). The aromatic hydrocarbon ring in the following formulas may have a substituent.

[0109] R in the formula (e) 11 to R 14 are the same or different and each represent a hydrogen atom or an alkyl group. Examples of the alkyl group include C such as methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group and the like 1-5 alkyl groups.

[0110] n in the formula (e) 1 represents the average value of the degree of polymerization of the repeating unit shown in the parentheses in the formula, is a number of 0 or more, and is preferably a number of 0 to 3.

[0111] n in the formula (e) 2 represents the average value of the degree of polymerization of the repeating unit shown in the square brackets in the formula, is a number of 1 or more, and is preferably a number of 1 to 10.

[0112] Accordingly, as the polyfunctional aromatic epoxy resin, a compound represented by the following formula (e-1) is still more preferable. In the following formula (e-1), ring Z 3 , n 1 , n 2 , R 11 to R 14 are the same as defined above. The benzene ring in the following formula (e-1) may have a substituent in addition to the groups shown in the formula.

[0113] Among the polyfunctional aromatic epoxy resins, an arylaralkyl type epoxy resin and / or a bisphenol type epoxy resin is particularly preferable.

[0114] The proportion of the polyfunctional aromatic epoxy resin in the total amount of the epoxy resin contained in the thermosetting composition is preferably 50% by weight or more, more preferably 60% by weight or more, still more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The upper limit is 100% by weight.

[0115] The epoxy equivalent (g / eq.) of the epoxy resin is, for example, 150 to 500, preferably 200 to 400, more preferably 200 to 350, and even more preferably 250 to 320.

[0116] The softening point of the epoxy resin is, for example, 80°C or lower, preferably 70°C or lower, and more preferably 60°C or lower. Alternatively, the softening point may be, for example, 30°C or higher, preferably 40°C or higher, and more preferably 50°C or higher.

[0117] The melt viscosity of the epoxy resin at 150°C, as measured by an ICI viscometer, is, for example, 1 Pa·s or less, preferably 0.5 Pa·s or less, and particularly preferably 0.3 Pa·s or less. Furthermore, the melt viscosity is, for example, 0.01 Pa·s or more. The melt viscosity is measured by an ICI viscometer in accordance with ASTM D4287.

[0118] (Curing agent) The curing agent is a compound that forms a crosslinked structure with the epoxy resin and has at least two reactive groups (= reactive functional groups) that are reactive with epoxy groups.

[0119] Examples of the reactive functional groups include hydroxyl groups, phenolic hydroxyl groups, carboxyl groups, amino groups, and thiol groups.

[0120] As a curing agent, compounds having two or more hydroxyl groups and a benzene ring in the main chain are preferred, as they exhibit excellent reactivity with epoxy resins and can form a high-density crosslinked structure, resulting in a cured product with excellent heat resistance, moisture resistance, impact resistance, adhesion, and electrical insulation properties. Phenolic aralkyl resins are particularly preferred.

[0121] The proportion of phenol aralkyl resin in the total amount of curing agent contained in the thermosetting composition is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The upper limit is 100% by weight.

[0122] As the phenol aralkyl resin, a compound represented by the following formula (p) is preferred.

[0123] Ring Z in the aforementioned formula (p) 4 represents an aromatic hydrocarbon ring. Ring Z 5 represents an aromatic hydrocarbon ring, or a linked ring in which two or more aromatic hydrocarbon rings are bonded via a single bond or a linking group. The aromatic hydrocarbon ring may have a substituent.

[0124] Ring Z 4 Examples of the aromatic hydrocarbon ring in Ring Z include the same examples as the aromatic hydrocarbon ring in Ring Z 2 . As Ring Z, a benzene ring which may have a substituent or a naphthalene ring which may have a substituent is preferable, and a benzene ring which may have a substituent is particularly preferable. Examples of the aforementioned substituent include the same examples as the substituent that the aromatic hydrocarbon ring in the epoxy resin may have. 4

[0125] Examples of the aromatic hydrocarbon ring and the linking group in Ring Z 5 include the same examples as the aromatic hydrocarbon ring and the linking group in Ring Z 3 .

[0126] The group represented by "-Z" in the aforementioned formula (p) 5 - is a group obtained by removing two hydrogen atoms from the structural formula of Ring Z, and examples thereof include the same groups as the group represented by "-Z" in the aforementioned formulas (e) and (e-1) 5 - 3 .

[0127] As the group represented by "-Z" in the aforementioned formula (p) 5 -, the groups represented by the aforementioned formulas (z-1) to (z-4) are preferable, the group represented by the aforementioned formula (z-1) or the group represented by the aforementioned formula (z-4) is more preferable, and the group represented by the aforementioned formula (z-4) is still more preferable.

[0128] R in the aforementioned formula (p) 15 to R 18 are identical or different and each represent a hydrogen atom or an alkyl group. Examples of the alkyl group include C such as methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, s-butyl group, t-butyl group and the like 1-5 alkyl groups.

[0129] ​n in formula (p) 3 This represents the average degree of polymerization of the repeating units indicated in parentheses in the above formula, and is a number greater than or equal to 0 (for example, a number between 0 and 10), preferably a number greater than or equal to 1.

[0130] n in formula (p) 4 represents the average degree of polymerization of the repeating units shown in the square brackets in the above formula, and is a number of 1 or more, preferably a number between 1 and 10.

[0131] Therefore, as a curing agent, a compound represented by the following formula (p-1) is even more preferred. In the following formula, ring Z 5 , n 3 , n 4 , R 15 ~R 18 The same applies as described above. The benzene ring in the following formula (p-1) may have substituents other than those shown in the formula.

[0132] The OH equivalent (g / eq.) of the curing agent is, for example, 150 to 400, preferably 170 to 350, more preferably 180 to 300, and even more preferably 190 to 250.

[0133] The softening point of the hardening agent is, for example, 100°C or lower, preferably 95°C or lower, and more preferably 90°C or lower. Alternatively, the softening point may be, for example, 30°C or higher, preferably 40°C or higher, and more preferably 50°C or higher.

[0134] The melt viscosity of the curing agent at 150°C, as measured by an ICI viscometer, is, for example, 1 Pa·s or less, preferably 0.5 Pa·s or less, and particularly preferably 0.3 Pa·s or less. Furthermore, the viscosity is, for example, 0.01 Pa·s or more.

[0135] In the thermosetting composition, the content of the curing agent is, for example, 50 to 150 parts by weight, preferably 70 to 130 parts by weight, per 100 parts by weight of epoxy resin.

[0136] Furthermore, it is preferable that the ratio of epoxy resin to curing agent content is in the range of 0.8 to 1.3, where the ratio of the total number of epoxy groups (Ep) in the contained epoxy resin to the number of reactive functional groups (Rf) in the contained curing agent (Ep / Rf).

[0137] (Inorganic filler) The thermosetting composition preferably contains an inorganic filler in addition to the above components.

[0138] The thermosetting composition, by containing an inorganic filler, has the effect of reducing the thermal expansion coefficient of the epoxy resin. Furthermore, when the thermosetting composition containing the inorganic filler is used as a semiconductor device encapsulant, the difference in thermal expansion between the wire and the semiconductor chip is suppressed, resulting in the effect of mitigating thermal stress. Therefore, even when the operating temperature of the semiconductor device rises, wire breakage and other issues can be avoided, thereby improving the reliability of the semiconductor device.

[0139] Examples of inorganic fillers include silicas such as fused silica, crystalline silica, and cristobalite; metal oxides such as alumina, titanium oxide, and magnesium oxide; and nitrides such as silicon nitride, aluminum nitride, and boron nitride. These can be used individually or in combination of two or more. Among these, silicas are preferred for their excellent thermal stress relaxation properties. Alumina is preferred for its excellent heat dissipation properties.

[0140] The average particle size of the inorganic filler can be appropriately selected depending on the application, but is, for example, 0.1 to 50 μm, preferably 10 to 50 μm, and more preferably 20 to 40 μm. The average particle size is the volume-average particle size measured by laser diffraction.

[0141] The inorganic filler may be surface-treated with a coupling agent, such as a silane coupling agent, to increase the bonding strength with the epoxy resin.

[0142] The shapes of inorganic fillers include, for example, spherical (perfectly spherical, nearly spherical, ellipsoidal, etc.), polyhedral, rod-shaped (cylindrical, prismatic, etc.), plate-shaped, flake-shaped, and irregularly shaped. Inorganic fillers also include hollow, porous, and solid inorganic fillers.

[0143] As an inorganic filler, a spherical inorganic filler is preferred in terms of improving fluidity.

[0144] In the thermosetting composition, the content of the inorganic filler is, for example, 5 parts by weight or more, preferably 8 parts by weight or more, and more preferably 10 parts by weight or more, per 1 part by weight of epoxy resin. Alternatively, the content of the inorganic filler is, for example, 20 parts by weight or less, preferably 15 parts by weight or less, per 1 part by weight of epoxy resin.

[0145] In the total amount of the thermosetting composition, the content of the inorganic filler is, for example, 60% by weight or more (for example, 60 to 95% by weight), preferably 70% by weight or more, and more preferably 80% by weight or more.

[0146] (Other components) The thermosetting composition may contain one or more other components in addition to the components mentioned above. Examples of other components include coupling agents, colorants, flame retardants, ion trapping agents, antioxidants, adhesion promoters, and release agents.

[0147] Examples of coupling agents include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-(thyranylmethoxy)propyltrimethoxysilane.

[0148] Examples of colorants include carbon black, phthalocyanine blue, and phthalocyanine green.

[0149] Examples of release agents include montanic acid waxes, montanic acid ester waxes, partially saponified montanic acid waxes, montanic acid metal salts, polyethylene waxes, oxidized polyethylene waxes, polytetrafluoroethylene, fluorine waxes, polydimethyl silicone, and modified silicone resins.

[0150] Examples of ion trapping agents include hydrotalcite and bismuth hydroxide.

[0151] The content of other components in the total amount of the thermosetting composition is, for example, 5% by weight or less, preferably 3% by weight or less, more preferably 1.5% by weight or less, even more preferably 1% by weight or less, even more preferably 0.5% by weight or less, particularly preferably 0.3% by weight or less, and most preferably 0.2% by weight or less.

[0152] The thermosetting composition contains a salt that exhibits delayed decomposition. Therefore, even when the thermosetting composition is subjected to heat treatment, its viscosity is suppressed and its fluidity is maintained until the salt decomposes. Once the salt decomposes, the generated phosphonium cation and anionic ligand or silicate anionic ligand act cooperatively to rapidly initiate the ring-opening reaction of the epoxy resin, so that the cross-linking reaction between the epoxy resin and the curing agent proceeds rapidly and a cured product is formed.

[0153] The gel time of the thermosetting composition is approximately 3 to 30 minutes at a curing temperature of 160°C. This ensures a suitable working time for filling operations in the encapsulation molding of semiconductor devices, thereby improving work efficiency.

[0154] The thermosetting composition has a pot life suitable for filling operations and also offers good work efficiency due to the rapid progression of the curing reaction. The time from the start of curing to the completion of curing of the thermosetting composition (the difference between the time at the inflection point of the rise in torque value and the time at the inflection point when a constant torque value is reached after curing, as determined by the method described in the examples) is, for example, 130 seconds or less, preferably 125 seconds or less, more preferably 120 seconds or less, and even more preferably 110 seconds or less. The lower limit of the time is, for example, 30 seconds.

[0155] The thermosetting composition has excellent fluidity at the sealing temperature. The spiral flow value of the thermosetting composition obtained by the method described in the examples is preferably 80 cm or more, more preferably 85 cm or more, even more preferably 90 cm or more, even more preferably 100 cm or more, even more preferably 110 cm or more, and particularly preferably 120 cm or more. The upper limit of the flow value is, for example, 200 cm, preferably 150 cm, and more preferably 130 cm.

[0156] The cured product of the thermosetting composition has a high degree of crosslinking, and the torque value obtained by the method described in the examples is, for example, 1 kgf·cm or more, preferably 2 kgf·cm or more, more preferably 2.5 kgf·cm or more, and particularly preferably 3 kgf·cm or more. Therefore, the cured product has heat resistance, moisture resistance, impact resistance, electrical insulation, adhesion, thermal stress relaxation, etc. derived from epoxy resin.

[0157] Because the thermosetting composition has the above-mentioned structure, by utilizing the time difference until the curing reaction begins, it can be filled around the semiconductor element, thereby sealing the semiconductor element while suppressing the generation of voids and the deformation and breakage of wires, even in semiconductor elements with high density and high integration.

[0158] Accordingly, the thermosetting composition can be suitably used as, for example, a encapsulant for semiconductor devices (especially a one-component encapsulant, a solid encapsulant, or a encapsulant for transfer molding), an adhesive (e.g., an interlayer adhesive for multilayer substrates, a die bonding agent, an adhesive for mounting), a coating agent, a molding material (e.g., sheets, films, fiber-reinforced plastics), a encapsulant for liquid crystal display elements, a encapsulant for organic EL elements, a printed circuit board material, a 3D printing material, and the like.

[0159] If the thermosetting composition is used as a encapsulant for a semiconductor element, for example, the semiconductor element can be encapsulated by filling the area around the semiconductor element with the thermosetting composition and curing the filled thermosetting composition.

[0160] More specifically, a semiconductor element sealed with a cured product of the thermosetting composition can be obtained through the following steps: 1. A semiconductor element with electrodes is placed on a lead frame, and the electrodes and the lead frame are electrically connected by wire bonding. 2. The wire-bonded semiconductor element is placed in a mold, and the thermosetting composition is injected into the mold by a method such as transfer molding, and the thermosetting composition is cured by heat treatment.

[0161] The heat treatment temperature is, for example, 150 to 200°C. The heat treatment time is, for example, 1 to 3 hours. When a transfer molding method is used, the injection pressure of the thermosetting composition into the mold is, for example, 10 to 100 MPa.

[0162] When a semiconductor element is sealed using the thermosetting composition, the thermosetting composition has a suitable time lag before the curing reaction begins, allowing it to fill the area around the semiconductor element. This allows the semiconductor element to be coated and filled with the cured product of the thermosetting composition without generating voids or causing defects such as wire deformation or breakage. Furthermore, because the semiconductor element is coated and filled with the cured product of the thermosetting composition, degradation due to external factors such as heat, humidity, light, and physical shock is suppressed, resulting in high reliability and a long lifespan.

[0163] Semiconductor elements coated and filled with the cured product of the aforementioned thermosetting composition are suitable for electronic devices such as smartphones and tablet terminals, which are becoming increasingly high-performance and multi-functional.

[0164] The configurations and combinations thereof described above are merely examples, and additions, omissions, substitutions, and modifications to the configurations are permitted as appropriate, without departing from the spirit of the present invention. Furthermore, the present invention is not limited by its embodiments.

[0165] The present invention will be described more specifically below with reference to examples, but the present invention is not limited to these examples.

[0166] Example 1 (Preparation of curing accelerator for epoxy resin) 135 g of dimethyl carbonate and 262 g of triphenylphosphine were dissolved in 384 g of methanol in a pressurized reaction vessel. The reaction was carried out at 130°C for 80 hours under sealed pressure to obtain a methyltriphenylphosphonium methylcarbonate solution. Titration revealed that the concentration of methyltriphenylphosphonium cation was 30% in the solution.

[0167] 198 g of phenyltrimethoxysilane and 320 g of 2,3-dihydroxynaphthalene were dissolved in 800 g of ethyl acetate and stirred until uniformly dissolved. 924 g of the methyltriphenylphosphonium / methylcarbonate solution was then added dropwise to obtain a precipitate. If crystals did not form, seed crystals were added as necessary.

[0168] The resulting precipitate was collected by filtration, washed with methanol, and then dried. This yielded a salt represented by the following formula (1-2-1a). The structure of the salt is as follows: 1 The characteristics were confirmed by 1H-NMR, mass spectrometry, and elemental analysis. The melting point of the obtained salt was 198°C. The melting point was defined as the temperature at which the sample melted when placed on a stainless steel test stand and gradually heated. The obtained salt was used as a curing accelerator.

[0169]

[0170] Example 2 (Preparation of curing accelerator for epoxy resin) 198 g of phenyltrimethoxysilane and 220 g of catechol were dissolved in 700 g of ethyl acetate, and a solution of 371 g of ethyltriphenylphosphonium bromide in 500 g of ethyl acetate was added dropwise to obtain a precipitate. The obtained precipitate was collected by filtration in the same manner as in Example 1, washed, and dried to obtain a salt represented by the following formula (1-2-2a) (melting point: 145°C), which was used as the curing accelerator.

[0171]

[0172] Example 3 The procedure was carried out in the same manner as in Example 1, except that methanol was used instead of ethyl acetate. This yielded a salt represented by the following formula (1-2-1a) (melting point: 165°C). The salt contained 1.5% by weight of the compound represented by the following formula (3). The salt was used as a curing accelerator.

[0173]

[0174] Example 4 (Preparation of curing accelerator for epoxy resin) 320 g of 2,3-naphthalenediol and 1000 g of isopropyl alcohol were placed in a reaction vessel and stirred until uniformly dissolved. 924 g of methyltriphenylphosphonium methylcarbonate solution, prepared in the same manner as in Example 1, was added dropwise, and a yellow liquid was formed at the bottom of the reaction vessel. The resulting yellow liquid was collected and dried. This yielded a salt represented by the following formula (1-1-1a) (melting point: 60°C), which was used as a curing accelerator.

[0175]

[0176] Example 5 (Preparation of curing accelerator for epoxy resin) The procedure was the same as in Example 4, except that 220 g of catechol was used instead of 320 g of 2,3-dihydroxynaphthalene. This yielded a salt represented by the following formula (1-1-2a) (melting point: 50°C), which was used as the curing accelerator.

[0177]

[0178] Example 6 was carried out in the same manner as in Example 4, except that 126 g of pyrogallol was used instead of 320 g of 2,3-dihydroxynaphthalene. This yielded a salt represented by the following formula (1-1-2b) (melting point: 40°C), which was used as a curing accelerator.

[0179]

[0180] Example 7 157 g of 9,9-bis(4-hydroxyphenyl)fluorene was dissolved in 3000 g of ethyl acetate. 260 g of methyltriphenylphosphonium methylcarbonate solution, prepared in the same manner as in Example 1, was added to obtain a precipitate. The obtained precipitate was collected by filtration, washed with ethyl acetate, and then dried. This yielded a salt represented by the following formula (1-3-1a) (melting point: 180°C). The obtained salt was used as a curing accelerator.

[0181]

[0182] Example 8 165 g of 9,9-bis(3-methyl-4-hydroxyphenyl)fluorene was dissolved in 3000 g of ethyl acetate. A methanol (300 g) solution of 100 g of ethyltriphenylphosphonium bromide was added dropwise to this solution. A precipitate was obtained. The obtained precipitate was collected by filtration, washed with ethyl acetate, and dried. This yielded a salt represented by the following formula (1-3-1b) (melting point: 175°C). The obtained salt was used as a curing accelerator.

[0183]

[0184] Comparative Example 1 The procedure was carried out in the same manner as in Example 4, except that the amount of 2,3-naphthalenediol used was changed from 320 g to 160 g. However, no yellow liquid was produced after the reaction. Therefore, the solvent was evaporated from the reaction solution using an evaporator, but the compound decomposed in the process, and no salt was obtained. This is thought to be because the neutral ligand was not produced due to the insufficient amount of 2,3-naphthalenediol used, and as a result, the stability of the produced salt was significantly reduced.

[0185] Comparative Example 2 The procedure was carried out in the same manner as in Example 4, except that 320 g of 2,3-naphthalenediol was replaced with 166 g of orthophthalic acid. No yellow liquid was produced after the reaction. Therefore, the solvent was evaporated from the reaction solution using an evaporator to obtain the salt represented by the following formula.

[0186]

[0187] Example 10 100 parts by weight of the epoxy resin below, 74 parts by weight of the curing agent below, and 3 parts by weight of the salt represented by formula (1-2-1a) obtained in Example 1 as a curing accelerator were mixed in a mixer, kneaded at 98°C for 8 minutes using a hot roll, then cooled and further pulverized to obtain thermosetting composition (1).

[0188] Epoxy resin (compound represented by the following formula (e-1-1), where n' is 2.3, manufactured by Nippon Kayaku Co., Ltd., trade name "NC3000", softening point 58°C, epoxy equivalent 273, ICI viscosity at 150°C: 0.04-0.1 Pa·s)

[0189] - Hardening agent (compound represented by the following formula (p-1-1), where n'' is 1.6, manufactured by Meiwa Kasei Co., Ltd., trade name "MEH-7851ss", softening point 67°C, hydroxyl group equivalent 204, ICI viscosity at 150°C: 0.04-0.44 Pa·s)

[0190] The performance of the obtained thermosetting composition (1) was evaluated by the following method: Fluidity: For thermosetting composition (1), the performance was evaluated according to the method of EMMI 1-66, with a mold temperature of 165°C and an injection pressure of 70 kg / cm². 2 The flow value (in cm) of a spiral flow (spiral shape: width 5 mm, thickness 3 mm, maximum flow length 750 mm) after a curing time of 30 minutes was measured and used as an indicator of fluidity. As a result, the flow value was 130 cm. Note that a higher flow value indicates better fluidity.

[0191] Curability 1: For the thermosetting composition (1), a Curlastometer (registered trademark) Type 7 (manufactured by A&D Co., Ltd.) was used to cure the composition at a temperature of 165°C under the conditions of die P-200 and amplitude angle ±1 / 4°. The time at the inflection point of the rise in torque value (T1 (seconds)) and the time at the inflection point when a constant torque value was reached after curing (T2 (seconds)) were measured. As a result, T1 was 55 seconds, T2 was 145 seconds, and the time from the start to the completion of the curing reaction, calculated from the difference between T1 and T2 (seconds), was 90 seconds. The torque value after curing was 3.5 kgf·cm. A smaller difference between T1 and T2 indicates better work efficiency due to the rapid progress of the curing reaction. A larger torque value after curing indicates better curability.

[0192] Curability 2: A thermosetting composition (1) was heated at 175°C for 60 minutes to obtain a cured product (1). The obtained cured product (1) was used as a test specimen, and differential scanning calorimetry (DSC) was performed under the following conditions in accordance with JIS K 7121:2012 to measure the glass transition temperature (Tg). Note that a higher Tg indicates a higher crosslinking density, and thus higher heat resistance, moisture resistance, and electrical insulation. <Analysis conditions> Measurement device: Differential scanning calorimetry "DSC-60Plus", manufactured by Shimadzu Corporation Temperature range: -50 to 150°C Heating rate: 10°C / min

[0193] Safety: A thermosetting composition (1) was heated at 170°C for 60 minutes to obtain a cured product (2). The obtained cured product (2) was used as a test specimen. Under atmospheric pressure, 3.0 g of the test specimen and 20 mL of DMF were placed in a sealed container and extracted at 100°C for 24 hours. Subsequently, the benzene concentration (ppm) in the extract was measured using gas chromatography under the following conditions. A lower benzene concentration indicates higher safety. <Measurement conditions> Measurement device: Gas chromatography "GC-2014", Shimadzu Corporation Column: DB-1

[0194] Reliability: A thermosetting composition (1) was heated at 175°C for 60 minutes to obtain a cured product (3). The obtained cured product (3) was used as a test specimen. Under atmospheric pressure, 3.0 g of the test specimen and 20 mL of DMF were placed in a sealed container and extracted at 100°C for 24 hours. Subsequently, the chlorine concentration (ppm) in the extract was measured using ion chromatography. A lower chlorine concentration indicates higher electrical reliability. <Measurement conditions> Measurement device: Gas chromatography "GC-2014", manufactured by Shimadzu Corporation Column: DB-1 Measurement device: Ion chromatography "Dionex Inuvion Core", manufactured by Thermo Fisher Scientific

[0195] Examples 11-17 and Comparative Examples 3-10: Thermosetting compositions were obtained in the same manner as in Example 10, except that the curing accelerators listed in the table below were used instead of the salt represented by formula (1-2-1a). The performance of the obtained thermosetting compositions was evaluated in the same manner as in Example 10. The results are shown in Tables 1-3 below. Note that the flow value and cured torque value are shown with the flow value or cured torque value of Example 10 set to 100.

[0196]

[0197]

[0198]

[0199]

[0200] From the table above, it can be seen that the thermosetting composition of the present invention possesses both excellent fluidity and excellent curability at the sealing treatment temperature. Furthermore, it can be seen that the time required from the start to the completion of the curing reaction of the thermosetting composition is short, and the curing reaction proceeds rapidly after it starts. Moreover, the thermosetting composition of the present invention is safer because the generation of benzene, a harmful substance, is significantly suppressed during curing compared to the thermosetting composition of the comparative example. In addition, thermosetting compositions often contain chlorine impurities derived from the raw materials, but free chlorine (Cl) is released from the chlorine impurities. - This can suppress the generation of free chlorine (Cl - It is highly reliable because it can prevent corrosion caused by ) . Furthermore, since the cured product of the thermosetting composition has a high Tg, it has a high crosslinking density and is found to have excellent heat resistance, moisture resistance, and electrical insulation properties.

[0201] In summary, the configuration of the present invention and its variations are listed below. [1] A curing accelerator for epoxy resins comprising a salt composed of an anionic ligand represented by formula (a), a neutral ligand represented by formula (ah), and a cation represented by formula (c), or an anionic ligand having a structure in which the anionic ligand represented by formula (a) and the neutral ligand represented by formula (ah) are bonded via a silicon atom, and a cation represented by formula (c). [2] The curing accelerator for epoxy resins according to [1], wherein the salt is a salt represented by formula (1-1). [3] The curing accelerator for epoxy resins according to [1], wherein the salt is a salt represented by formula (1-2). [4] The curing accelerator for epoxy resins according to [1], wherein the salt is a salt represented by formula (1-3). [5] The ring Z 1The epoxy resin curing accelerator according to any one of [1] to [4], wherein is a benzene ring or a naphthalene ring which may have substituents. [6] The epoxy resin curing accelerator according to [2] or [5], wherein the salt contains a salt represented by formula (1-2) and does not contain a compound represented by formula (2), or contains a salt represented by formula (1-2) and contains a compound represented by formula (2), and the content of the compound represented by formula (2) is 10% by weight or less of the content of the salt represented by formula (1-2). [7] A thermosetting composition comprising the epoxy resin curing accelerator according to any one of [1] to [6], an epoxy resin, and a curing agent. [8] The thermosetting composition according to [7], wherein the epoxy resin is a compound represented by formula (e). [9] The thermosetting composition according to [7] or [8], wherein the curing agent is a compound represented by formula (p).

[10] Use as a curing accelerator for epoxy resins a salt comprising an anionic ligand represented by formula (a), a neutral ligand represented by formula (ah), and a cation represented by formula (c), or a salt comprising an anionic ligand having a structure in which the anionic ligand represented by formula (a) and the neutral ligand represented by formula (ah) are bonded via a silicon atom, and a cation represented by formula (c).

[11] The use according to

[10] , wherein the salt is the salt represented by formula (1-1).

[12] The use according to

[10] , wherein the salt is the salt represented by formula (1-2).

[13] The use according to

[10] , wherein the salt is the salt represented by formula (1-3).

[14] The ring Z 1 The use according to any one of

[10] to

[13] , wherein is a benzene ring or a naphthalene ring which may have substituents.

[15] The use according to

[12] or

[14] , wherein the salt contains a salt represented by formula (1-2) and does not contain a compound represented by formula (2), or contains a salt represented by formula (1-2) and contains a compound represented by formula (2), and the content of the compound represented by formula (2) is 10% by weight or less of the content of the salt represented by formula (1-2).

[16] Use of a thermosetting composition comprising an epoxy resin curing accelerator according to any one of [1] to [6], an epoxy resin, and a curing agent as a semiconductor device encapsulant.

[0202] The epoxy resin curing accelerator of the present invention has appropriate delayed decomposition properties that match the encapsulation molding cycle of semiconductor devices. When the epoxy resin curing accelerator decomposes, the anionic ligand and phosphonium cation work together to rapidly initiate the ring-opening reaction of the epoxy resin. The thermosetting composition of the present invention can be suitably used for encapsulation applications of semiconductor devices and can contribute to improving the reliability and extending the lifespan of semiconductor devices.

Claims

1. A curing accelerator for epoxy resins comprising a salt composed of an anionic ligand represented by the following formula (a), a neutral ligand represented by the following formula (ah), and a cation represented by the following formula (c), or a salt composed of an anionic ligand having a structure in which the anionic ligand represented by the following formula (a) and the neutral ligand represented by the following formula (ah) are bonded via a silicon atom, and a cation represented by the following formula (c). [In the formula, R 1 The '' represents an alkyl group having 1 to 3 carbon atoms. Ring Z represents an aromatic hydrocarbon ring which may have substituents, or a structure in which two or more aromatic hydrocarbon rings which may have substituents are linked by a single bond or a linking group. m1 and m2 represent the same number from 0.5 to 1, and m3 represents the number from 0.5 to 1.

5. The benzene ring shown in the formula may have substituents.

2. The epoxy resin curing accelerator according to claim 1, wherein the salt is a salt represented by the following formula (1-1). [In the formula, R 1 This represents an alkyl group having 1 to 3 carbon atoms, and the ring Z 1 This represents an aromatic hydrocarbon ring which may have substituents. The benzene ring shown in the formula may have substituents.

3. The epoxy resin curing accelerator according to claim 1, wherein the salt is a salt represented by the following formula (1-2). [In the formula, R 1 R represents an alkyl group having 1 to 3 carbon atoms. 2 This indicates an organic group. Ring Z 1 This represents an aromatic hydrocarbon ring which may have substituents. The benzene ring shown in the formula may have substituents.

4. The epoxy resin curing accelerator according to claim 1, wherein the salt is a salt represented by the following formula (1-3). [In the formula, R 1 This represents an alkyl group having 1 to 3 carbon atoms. m1 and m2 represent the same number between 0.5 and 1, and m3 represents the same number between 0.5 and 1.

5. The benzene ring shown in the formula may have substituents.

5. The ring Z 1 The epoxy resin curing accelerator according to claim 2 or 3, wherein is a benzene ring or naphthalene ring which may have substituents.

6. The curing accelerator for epoxy resins according to Claim 3, wherein the salt contains the salt represented by the formula (1-2) and does not contain the compound represented by the following formula (2), or contains the salt represented by the formula (1-2) and the compound represented by the following formula (2), and the content of the compound represented by the formula (2) is 10% by weight or less of the content of the salt represented by the formula (1-2). (wherein, R 2 , ring Z 1 are the same as defined above. R 4 represents an alkyl group) 7. A thermosetting composition comprising an epoxy resin curing accelerator according to any one of claims 1 to 4, an epoxy resin, and a curing agent.

8. The thermosetting composition according to claim 7, wherein the epoxy resin is a compound represented by the following formula (e). (In the formula, ring Z 2 This represents an aromatic hydrocarbon ring. Ring Z 3 R represents an aromatic hydrocarbon ring, or a linked ring in which two or more aromatic hydrocarbon rings are linked by a single bond or a linking group. The aromatic hydrocarbon ring may have substituents. 11 ~R 14 n represents the same or different hydrogen atom or alkyl group. 1 n represents a number greater than or equal to 0. 2 (This represents a number greater than or equal to 1.) 9. The thermosetting composition according to claim 7, wherein the curing agent is a compound represented by the following formula (p). (In the formula, ring Z 4 This represents an aromatic hydrocarbon ring. Ring Z 5 R represents an aromatic hydrocarbon ring, or a linked ring in which two or more aromatic hydrocarbon rings are linked by a single bond or a linking group. The aromatic hydrocarbon ring may have substituents. 15 ~R 18 n represents the same or different hydrogen atom or alkyl group. 3 n represents a number greater than or equal to 0. 4 (This represents a number greater than or equal to 1.)