Naphthalimide compound, resin composition for wavelength conversion, and cured product
Naphthalimide compounds with specific substituents address the lack of light resistance and fluorescence in wavelength conversion by enhancing solubility and fluorescence properties, effectively converting blue to green light.
Patent Information
- Application Number
- PCT/JP2026/014856
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-04-10
- Publication Date
- 2026-11-19
AI Technical Summary
Existing wavelength conversion compounds for color displays lack both high light resistance and excellent fluorescence properties, particularly when converting blue light to green light, and do not consider solubility in solvents effectively.
Development of naphthalimide compounds with specific substituents (R₁ and R₂) that include linear or branched aliphatic hydrocarbon groups with unsaturated carbon bonds, alcoholic hydroxyl groups, or ether bonds, enhancing solubility and fluorescence properties while improving light resistance.
The naphthalimide compounds exhibit excellent solubility, high light resistance, and strong fluorescence properties, effectively converting blue light to green light with enhanced crosslinking abilities.
Smart Images

Figure JP2026014856_19112026_PF_FP_ABST
Abstract
Description
Naphthalimide compounds, wavelength conversion resin compositions, and cured products
[0001] The present invention relates to naphthalimide compounds, preferably naphthalimide compounds useful as wavelength conversion compounds, wavelength conversion resin compositions, and cured products.
[0002] In recent years, color conversion methods have been proposed for color displays that use wavelength conversion compounds that absorb blue light from light-emitting elements and convert it to red or green through wavelength conversion. Examples of prior art disclosing such wavelength conversion compounds include the following: For example, Patent Document 1 (JP 2002-348568 A) discloses the use of a pyridine-phthalimide condensation derivative of a specific structure as a color conversion material, which converts a blue element to a blue-green color close to white, as a color conversion material with a long lifespan and excellent durability. Patent Document 2 (JP 2007-273440 A) discloses a color conversion layer containing a coumarin compound of a specific structure as a green color conversion filter with excellent durability. Patent Document 3 (JP 2012-92077 A) discloses a technology that uses a coumarin compound of a specific structure with light resistance as a light-emitting material for organic EL. Furthermore, Patent Document 4 (Japanese Unexamined Patent Publication No. 2002-317175) discloses a technique using a dibenzo[f,f']diindeno[1,2,3-cd:1',2',3'-lm]perylene derivative of a specific structure as a color conversion material with excellent durability and high conversion efficiency. Moreover, Non-Patent Document 1, for example, discloses that a 4-allylamino-N-phenyl-1,8-naphthalimide derivative of a specific structure, and a copolymer with said derivative, are yellow-green in color and emit stable fluorescence. All of the techniques described in Patent Documents 1 to 4 and Non-Patent Document 1 are recognized as having been devised in terms of the chemical structure of the wavelength conversion compound to be used in order to obtain a specific effect.
[0003] Japanese Patent Publication No. 2002-348568, Japanese Patent Publication No. 2007-273440, Japanese Patent Publication No. 2012-92077, Japanese Patent Publication No. 2002-317175
[0004] Photophysical Properties of new Polymerizable 1,8-Naphthalimides and their Copolymers with Methylmethacryl ate; Ivo Grabchev and Desislava Staneva; 558-562 (2003)
[0005] In displays employing a color conversion method, it is desirable to use only blue light-emitting elements from the viewpoint of cost reduction. On the other hand, regarding the converted color, even if it is green, the range of shades is wide, and there is a need for a desired shade of green. However, even if a compound can convert blue to green, from the viewpoint of improving display performance with the recent development of display technology, when used as a wavelength conversion compound, two properties are required: high light resistance and excellent fluorescence properties such as high fluorescence intensity. In this case, in order to make the properties that the wavelength conversion compound originally possesses the most out of all, it is preferable to consider the relationship with other components, such as solubility in the solvent, in addition to the chemical structure, as well as the chemical structure.
[0006] Regarding these points, the technologies described in the above-mentioned references 1 to 4 all attempt to solve the problem from the perspective of the chemical structure of the wavelength conversion compound used in order to achieve durability, etc. On the other hand, these references 1 to 4 and Non-Patent Document 1 do not propose to simultaneously achieve both high photoresistance and excellent fluorescence properties by also considering the solubility of the wavelength conversion compound, in particular the wavelength conversion compound that converts blue light to green light, in a solvent.
[0007] From the above perspective, the present inventors have aimed to provide a novel compound useful as a material for color displays, taking into consideration not only the chemical structure of the wavelength conversion compound but also its solubility in a solvent, more specifically, a wavelength conversion compound having both high light resistance and excellent fluorescence properties, preferably a wavelength conversion compound that converts blue light to green light.
[0008] In view of the above problems, the inventors have conducted diligent studies and have found that the general formula (1): [In formula (1), R1 and R 2 each independently represent a linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms, which may contain at least one of an unsaturated carbon bond, an alcoholic hydroxyl group, an ether bond and an ester bond, provided that the aforementioned R 1 and R 2 at least one of which contains the aforementioned unsaturated carbon bond (here, in the case where the aforementioned R 1 and R 2 contain the aforementioned ester bond, one carbon atom constituting the aforementioned ester bond shall not be included in the aforementioned number of carbon atoms)], the present inventors have found that the above problems can be solved, and have completed the present invention.
[0009] In addition, another preferred embodiment of the present invention relates to the naphthalimide compound, wherein in formula (1), at least one of the aforementioned R 1 and R 2 contains the aforementioned alcoholic hydroxyl group.
[0010] Further, another preferred embodiment of the present invention relates to the naphthalimide compound, wherein in formula (1), the aforementioned R 1 and R 2 each independently contain the aforementioned unsaturated carbon bond.
[0011] Further still, another aspect of the present invention relates to the naphthalimide compound, wherein the naphthalimide compound represented by general formula (I) is a wavelength conversion compound.
[0012] Another aspect of the present invention also relates to a resin composition for wavelength conversion, comprising the above naphthalimide compound and a binder resin.
[0013] The present invention also relates to a cured product obtained by curing the above resin composition for wavelength conversion, and the cured product which is a wavelength conversion film.
[0014] The naphthalimide compound of the present invention, preferably as a wavelength conversion compound, more preferably as a wavelength conversion compound that converts blue light into green light, has excellent solubility in solvents, high light resistance and excellent fluorescence properties in combination.
[0015] The naphthalimide compound of the present invention has a general formula (1): It has a naphthalimide structure represented by formula (1). Furthermore, substituent R in formula (1) 1 and R 2 However, each independently represents a linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms, which may contain at least one of an unsaturated carbon bond, an alcoholic hydroxyl group, an ether bond, and an ester bond, provided that the R 1 and R 2 At least one of them is said to contain the unsaturated carbon bond. Here, R 1 and R 2 However, if an ester bond is included, the single carbon atom constituting the ester bond shall not be included in the carbon count.
[0016] The structure of the substituent increases the solubility of the naphthalimide compound represented by formula (1) in the solvent, and consequently, the fluorescence properties, such as fluorescence intensity, of the cured product obtained from the wavelength conversion resin composition containing the naphthalimide compound represented by formula (1) are enhanced.
[0017] At the same time, the unsaturated carbon bond enhances the crosslinking properties with other naphthalimide compounds, thereby improving the light resistance of the cured product obtained from the naphthalimide compound represented by formula (1).
[0018] Because it possesses the characteristics described above, the naphthalimide compound represented by formula (1) of the present invention is preferred as a wavelength conversion compound, for example, as a wavelength conversion compound that converts blue light to green light. Specifically, the naphthalimide compound of the present invention can absorb the wavelength of blue light (approximately 450 nm) and convert it into green light with a wavelength of preferably 520 nm to 570 nm.
[0019] The components used in this invention will be described in detail below.
[0020] [Naphthalimide Compound of the Present Invention] The naphthalimide compound of the present invention is represented by formula (1) as described above. In formula (1), the linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms is preferably a linear or branched aliphatic hydrocarbon group such as a methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, tert-butyl group, pentyl group, hexyl group, heptyl group, or octyl group.
[0021] In formula (1), the unsaturated carbon bond is, for example, a carbon-carbon double bond or a carbon-carbon triple bond, preferably a carbon-carbon double bond. The linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms and having an unsaturated carbon bond is preferably a linear or branched alkenyl group having 1 to 6 carbon atoms, and more preferably a linear or branched alkenyl group having 1 to 4 carbon atoms.
[0022] Suitable alkenyl groups include, for example, vinyl group, 1-methylvinyl group, 2-methylvinyl group, allyl group, 2-methylallyl group, 1-methylpropenyl group, 2-methylpropenyl group, butenyl group, pentenyl group, hexenyl group, heptenyl group, or octenyl group.
[0023] And R 1 and R 2 One or two of these contain the unsaturated carbon bond. Furthermore, R 1 and R 2 Since both of these contain the unsaturated carbon bond, the crosslinking ability is further enhanced, and the light resistance of the cured product obtained from the naphthalimide compound represented by formula (1) is also further enhanced. At this time, R 1 or R 2 The number of unsaturated carbon bonds contained in each of them may be one or more, as long as it is structurally permissible. However, R 1 or R 2 The number of unsaturated carbon bonds contained in each is four or less, preferably two or less. The two carbon atoms constituting the unsaturated carbon bonds are considered to be included in the number of carbon atoms constituting the aliphatic hydrocarbon group.
[0024] Furthermore, in formula (1), the alcoholic hydroxyl group refers to a hydroxyl group bonded to a hydrocarbon group, other than a phenolic hydroxyl group directly bonded to an aromatic ring. Such an alcoholic hydroxyl group may be any of primary alcohols, secondary alcohols, or tertiary alcohols, but is more preferably selected from primary hydroxyl groups (primary alcohols). Here, R 1 and R 2 The solubility is enhanced by including one or two of the alcoholic hydroxyl groups.
[0025] Examples of linear or branched aliphatic hydrocarbon groups having 1 to 8 carbon atoms and having an alcoholic hydroxyl group include linear or branched aliphatic hydrocarbon groups having 1 to 6 carbon atoms and having an alcoholic hydroxyl group, and more preferably linear or branched aliphatic hydrocarbon groups having 1 to 4 carbon atoms and having an alcoholic hydroxyl group.
[0026] Preferred aliphatic hydrocarbon groups having such alcoholic hydroxyl groups include, for example, hydroxymethyl, hydroxyethyl, hydroxypropyl, hydroxybutyl, dihydroxypropyl, dihydroxybutyl, hydroxypentyl, hydroxyhexyl, hydroxyheptyl, or hydroxyoctyl groups.
[0027] And R 1 or R 2 Each of these may contain the above-mentioned unsaturated carbon bond, and may also further contain the alcoholic hydroxyl group. In this case, R 1 or R 2 The number of alcoholic hydroxyl groups contained in each may be one or more, as long as it is structurally permissible. However, R 1 or R 2 The number of alcoholic hydroxyl groups contained in each is preferably two or less, from the viewpoint of suppressing an increase in the water solubility of the naphthalimide compound and facilitating handling.
[0028] Examples of linear or branched alkenyl groups having 1 to 8 carbon atoms and possessing an unsaturated carbon bond and an alcoholic hydroxyl group as described above include HO-CH 2-CH = CH - CH 2 - HO-CH 2 -CH = CH - CH 2 -CH 2 - are some examples.
[0029] On the other hand, in formula (1), the linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms and having an ether bond is preferably a linear or branched aliphatic hydrocarbon group having 1 to 6 carbon atoms and having an ether bond, and more preferably a linear or branched aliphatic hydrocarbon group having 1 to 4 carbon atoms and having an ether bond.
[0030] Examples of aliphatic hydrocarbon groups having such ether bonds include those obtained by alkylating the alcoholic hydroxyl group of an aliphatic hydrocarbon group having an alcoholic hydroxyl group to convert it into an ether bond, such as methoxymethyl group, methoxyethyl group, methoxypropyl group, ethoxymethyl group, ethoxyethyl group, and ethoxypropyl group.
[0031] And R 1 or R 2 Each of these may contain the above-mentioned unsaturated carbon bond, and may also further contain the ether bond. In this case, R 1 or R 2 The number of ether bonds contained in each of them may be one or more, as long as it is structurally permissible. However, R 1 or R 2 The number of ether bonds contained in each is, for example, five or less.
[0032] Examples of linear or branched aliphatic hydrocarbon groups having 1 to 8 carbon atoms and possessing unsaturated carbon bonds and ether bonds include CH 3 -O-CH 2 -CH = CH - CH 2 - , CH 3 -CH 2 -O-CH 2 -CH = CH - CH 2 - are some examples.
[0033] Furthermore, as a linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms and having an ester bond, preferably a linear or branched aliphatic hydrocarbon group having 1 to 6 carbon atoms and having an ester bond, and more preferably a linear or branched aliphatic hydrocarbon group having 1 to 4 carbon atoms and having an ester bond.
[0034] Examples of aliphatic hydrocarbon groups having such ester bonds include those obtained by acyling the alcoholic hydroxyl group of an aliphatic hydrocarbon group having an alcoholic hydroxyl group to convert it into an ester bond, such as acetoxymethyl group, acetoxyethyl group, and acetoxypropyl group.
[0035] And R 1 or R 2 Each of these may contain the above-mentioned unsaturated carbon bond, as well as a structure further containing the ester bond. In this case, R 1 or R 2 The number of ester bonds contained in each may be one or more, as long as it is structurally permissible. However, R 1 or R 2 The number of ester bonds contained in each of these is, for example, five or less.
[0036] Examples of linear or branched aliphatic hydrocarbon groups having 1 to 8 carbon atoms and possessing unsaturated carbon bonds and ester bonds include CH 3 -C(=O)-O-CH 2 -CH = CH - CH 2 - , CH 3 -CH 2 -C(=O)-O-CH 2 -CH = CH - CH 2 - , CH 3 -OC(=O)-CH 2 -CH = CH - CH 2 - , CH 3 -CH 2 -OC(=O)-CH 2 -CH = CH - CH 2 - are some examples.
[0037] That is, R 1 or R 2Each of these may contain any combination of the above-mentioned alcoholic hydroxyl group, ether bond, and ester bond.
[0038] Preferably, in formula (1), R 1 and R 2 At least one of them contains an alcoholic hydroxyl group. Specifically, in formula (1), R 1 and R 2 One of these is a linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms and possessing an unsaturated carbon bond, and the other is a linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms and possessing an alcoholic hydroxyl group.
[0039] Particularly preferred is R in formula (1). 1 and R 2 Each of these independently contains an unsaturated carbon bond. Specifically, in formula (1), R 1 and R 2 Both are straight-chain or branched aliphatic hydrocarbon groups having 1 to 8 carbon atoms and possessing unsaturated carbon bonds.
[0040] A more preferred naphthalimide compound represented by formula (1) in the present invention is, for example, a compound represented by the following formulas (1-a) to (1-p).
[0041] The naphthalimide compound of the present invention can be produced, for example, by the following method: formula (2) and NH 2 R 2 (In the formula, R 2 It can be obtained by a substitution reaction with (which has the same meaning as the definition in formula (1) above). Also, formula (3) and XR 2It can also be obtained by a substitution reaction with (wherein R2 has the same meaning as defined in formula (1) above, and X is a leaving group such as a halogen atom). (In formula (2), X is a leaving group such as a halogen atom, and R 1 (This has the same meaning as the definition in formula (1) above.) (In formula (3), R 1 (This has the same meaning as the definition in formula (1) above.)
[0042] As described above, the naphthalimide compound represented by formula (1) of the present invention may be provided in the form of a wavelength conversion resin composition together with a binder resin and, optionally, other components such as a crosslinking agent, a photopolymerization initiator, and a solvent.
[0043] In this case, the content of the naphthalimide compound represented by formula (1) in the wavelength conversion resin composition is preferably, for example, 0.5% to 30% by mass as solid content relative to the total solid content of the wavelength conversion resin composition. By having the content within this numerical range, the wavelength conversion film obtained after curing can have excellent fluorescence properties and exhibit high light resistance.
[0044] [Binder Resin] In the present invention, the binder resin is not particularly limited, but it is preferably a resin having acidic functional groups such as carboxyl groups and phenolic hydroxyl groups. In particular, it is preferably a polymer having carboxyl groups, for example, a copolymer of an ethylene-based unsaturated monomer having one or more carboxyl groups and another copolymerizable ethylene-unsaturated monomer. For example, cyclomer P(ACA)Z320 (manufactured by Daicel Corporation) is preferred as the binder resin. In addition, epoxy (meth)acrylate resins having carboxyl groups may be used as binder resins other than copolymers.
[0045] The binder resin content in the wavelength conversion resin composition is, for example, 15% to 90% by mass as solid content, relative to the total solid content of the wavelength conversion resin composition.
[0046] [Photopolymerization Initiators] Photopolymerization initiators impart radiation sensitivity to the wavelength conversion resin composition of the present invention. That is, they are compounds that generate active species capable of initiating polymerization of the binder resin and crosslinking agent upon exposure to radiation such as visible light, ultraviolet light, far-infrared rays, and X-rays. Examples of such photopolymerization initiators include thioxanthone compounds, acetophenone compounds, biimidazole compounds, triazine compounds, and O-acyloxime compounds. Specific examples include CGI-325, Irgacure OXE01, and Irgacure OXE02 from BASF Japan, N-1919 and NCI-831 from ADEKA, and Omnirad TPO N and Omnirad 819 from IGM Resins.
[0047] The content of the photopolymerization initiator in the wavelength conversion resin composition is, for example, 0.01% to 20% by mass relative to the solid content of the binder resin.
[0048] [Solvent] Examples of solvents used in the wavelength conversion resin composition of the present invention include (poly)alkylene glycol alkyl ethers, keto alcohols, (poly)alkylene glycol monoalkyl ether acetates, ketones, aromatic hydrocarbons such as toluene and xylene, and esters such as ethyl acetate. Examples include propylene glycol methyl ether (PGME) and 2-methoxy-1-methyl ethyl acetate (PGMeA). Preferably, propylene glycol methyl ether is used.
[0049] The solvent content in the wavelength conversion resin composition is, for example, 20% to 80% by mass relative to the solid content of the binder resin.
[0050] [Crosslinking Agent] The wavelength conversion resin composition of the present invention may contain a crosslinking agent to adjust the physical properties of the resulting cured product, such as elasticity and hardness. Here, a crosslinking agent refers to a compound having two or more polymerizable functional groups to adjust the physical properties of the resulting cured product, such as elasticity and hardness. Examples of polymerizable functional groups include ethylenically unsaturated groups, oxyranyl groups, oxetanyl groups, N-alkoxymethylamino groups, etc. For example, dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd.) can be used.
[0051] The crosslinking agent content in the wavelength conversion resin composition is, for example, 0.5% to 20% by mass relative to the solid content of the binder resin.
[0052] [Other components] The wavelength conversion resin composition of the present invention may optionally contain dyes, pigments, thermal polymerization initiators, fillers, resins without acidic functional groups, surfactants, antioxidants, ultraviolet absorbers, anti-aggregation agents, etc., other than the xanthene compounds of the present invention.
[0053] [Wavelength Conversion Resin Composition] The wavelength conversion resin composition of the present invention may be produced by mixing a naphthalimide compound represented by formula (1), a binder resin, and, if necessary, other components such as a crosslinking agent, a photopolymerization initiator, and a solvent in a mixer.
[0054] [Cured product] The cured product of the present invention is obtained by forming a coating film using the above-mentioned wavelength conversion resin composition, irradiating the obtained coating film with light such as ultraviolet light by attaching a mask having a predetermined pattern to it, and developing it with an alkaline developer to wash out the unexposed areas.
[0055] Examples of the above-mentioned alkaline developer include aqueous solutions of alkali metal hydroxides such as potassium carbonate, sodium carbonate, potassium hydroxide, and sodium hydroxide; aqueous solutions of quaternary ammonium hydroxide; and alkaline aqueous solutions such as amine solutions. Any of the following development methods can be used, including the liquid-filling method, dipping method, agitation immersion method, step-paddle development method, inverted development method, and spray method. Subsequently, the resulting patterned cured material is subjected to post-baking for thermal curing, resulting in a product with excellent heat resistance and chemical resistance. The post-baking temperature is generally 50 to 270°C.
[0056] The cured product of the present invention possesses both high light resistance and excellent fluorescence properties, making it suitable for use as a wavelength conversion film for displays such as micro-LED displays, organic EL displays, and liquid crystal displays, as well as for lighting.
[0057] The wavelength conversion film can be used in any way that allows it to absorb the wavelength of blue light and convert it into green light. For example, the wavelength conversion film may be laminated on a blue micro-LED chip, or it may be used as an interposition between a blue LED chip and a green color filter, but is not limited to these.
[0058] The present invention will be described in detail below with reference to examples and comparative examples, but it goes without saying that the present invention is not limited to the following examples. Unless otherwise specified, the "parts" and "%" shown are based on mass.
[0059] [Synthesis Example 1] Preparation of the naphthalimide compound of Example 1 To a 50 ml flask were added 1.0 g (3.2 mmol) of N-allyl-4-bromo-1,8-naphthalimide, 1.4 g (25.3 mmol) of allylamine, and 5.0 g of NMP, and the mixture was reacted at 100°C for 5 hours. The reaction solution was poured into water, the precipitated crystals were filtered, washed with water and then dried, to obtain 0.8 g of N-allyl-4-(allylamino)-1,8-naphthalimide. It was confirmed by 1H-NMR spectrum measurement that the obtained compound was a compound represented by the following formula. 1H NMR (400 MHz, DMSO-d6): δ = 6.66 to 8.67 (Ar), 8.04 (NH), 5.94 (NH-CH 2 -CH=CH 2 ), 5.86 (N-CH 2 -CH=CH 2 ), 5.15 (NH-CH 2 -CH=CH 2 ), 5.02 (N-CH 2 -CH=CH 2 ), 4.58 (N-CH 2 -CH=CH 2 ), 4.58 (NH-CH 2 -CH=CH 2 )
[0060] [Synthesis Example 2] Preparation of the naphthalimide compound of Example 2 To a 50 ml flask were added 1.0 g (3.0 mmol) of N-(2-methylallyl)-4-bromo-1,8-naphthalimide, 1.4 g (25.3 mmol) of allylamine, and 5.0 g of NMP, and the mixture was reacted at 100°C for 5 hours. The reaction solution was poured into water, the precipitated crystals were filtered, washed with water and then dried, to obtain 0.8 g of N-(2-methylallyl)-4-(allylamino)-1,8-naphthalimide. It was confirmed by 1H-NMR spectrum measurement that the obtained compound was a compound represented by the following formula. 1 H NMR (400 MHz, DMSO-d6): δ = 6.66 to 8.67 (Ar), 8.04 (NH), 5.92 (NH-CH 2 -CH=CH 2 ), 5.15 (NH-CH 2 -CH=CH 2 ), 4.72 (N-CH2 -C(CH 3 ) = CH 2 ), 4.48(N-CH2-C(CH 3 ) = CH 2 ), 4.02 (NH-CH 2 -CH=CH 2 ), 1.70 (N-CH 2 -C(CH 3 ) = CH 2 )
[0061] [Synthesis Example 3] Preparation of the Naphthalimide Compound of Example 3 1.0 g (3.2 mmol) of N-allyl-4-bromo-1,8-naphthalimide, 1.9 g (25.3 mmol) of propanolamine, and 5.0 g of NMP were added to a 50 ml flask and reacted at 100°C for 5 hours. The reaction solution was drained into water, the precipitated crystals were filtered, washed with water, and dried to obtain 0.8 g of N-allyl-4-(allylamino)-1,8-naphthalimide. ¹H-NMR spectroscopy confirmed that the obtained compound was represented by the following formula. 1 H NMR (400MHz, DMSO-d6): δ = 6.73-8.64 (Ar), 7.75 (NH), 5.87 (N-CH 2 -CH=CH 2 ), 5.05 (N-CH 2 -CH=CH 2 ), 4.58 (OH), 4.41 (N-CH 2 -CH=CH 2 ), 3.53 (NH-CH 2 -CH 2 -CH 2 -OH), 3.50(NH-CH 2 -CH 2 -CH 2 -OH), 1.84(NH-CH 2 -CH 2 -CH 2 -OH)
[0062] [Synthesis Example 4] Preparation of the Naphthalimide Compound of Example 4 1.0 g (3.0 mmol) of N-(2-methylallyl)-4-bromo-1,8-naphthalimide, 1.8 g (24.2 mmol) of propanolamine, and 5.0 g of NMP were added to a 50 ml flask and reacted at 100°C for 5 hours. The reaction solution was drained into water, the precipitated crystals were filtered, washed with water, and dried to obtain 0.9 g of N-(2-methylallyl)-4-(allylamino)-1,8-naphthalimide. ¹H-NMR spectroscopy confirmed that the obtained compound was represented by the following formula: ¹H-NMR (400 MHz, DMSO-d6): δ = 6.70-8.65 (Ar), 7.75 (NH), 4.69 (N-CH) 2 -C(CH 3 ) = CH 2 ), 4.90 (OH), 4.80 (N-CH 2 -C(CH 3 ) = CH 2 ), 3.53 (NH-CH 2 -CH 2 -CH 2 -OH), 3.50(NH-CH 2 -CH 2 -CH 2 -OH), 1.84(NH-CH 2 -CH 2 -CH 2 -OH), 1.70(N-CH 2 -C(CH 3 ) = CH 2 )
[0063] [Comparative Examples 1-6] Compounds having the structures shown below were also used as Comparative Examples 1-6.
[0064] Comparative Example 1:
[0065] Comparative Example 2:
[0066] Comparative Example 3:
[0067] Comparative Example 4:
[0068] Comparative Example 5:
[0069] Comparative Example 6:
[0070] [Test Example 1] Evaluation of Fluorescence 1. Measurement of Incident and Reflected Wavelengths 0.01 g of each fluorescent compound from the Naphthalimide Compound of the Example and the Comparative Example were mixed with 0.99 g of resin (Cychromer P(ACA)Z320, manufactured by Daicel Corporation) and Propylene glycol methyl ether (PGME) solvent to prepare the resin compositions of the Example and the Comparative Example. The solutions of the obtained resin compositions were coated onto a glass plate to a thickness of 2 μm and pre-baked on a hot plate at 100°C for 3 minutes. After cooling, the fluorescence properties of the obtained coating film were measured using a JASCO FP-8600 spectrofluorometer under the conditions of excitation wavelength: 200-600 nm and fluorescence wavelength: 300-700 nm to obtain a 3D map of the fluorescence properties. Specifically, the emission spectra corresponding to each excitation wavelength were measured while changing the excitation wavelength and displayed as spectral maps. The conversion wavelength was identified from the emission spectrum at the blue wavelength (450 nm). The results are shown in Table 1 below.
[0071] 2. Measurement of Fluorescence Intensity (Relative Value) In the emission spectrum at a blue wavelength (450 nm), the compound with the strongest intensity at a specific conversion wavelength was that of Example 1, and its intensity was set to 100. The fluorescence intensities of the other examples and comparative examples are the intensities at the strongest conversion wavelength and were calculated as relative values to the intensity of Example 1. The results are shown in Table 1 below.
[0072] [Test Example 2] Lightfastness: Evaluation of the color stability of the coating film after phototherapy. A resin composition was prepared by mixing 0.01 g of the naphthalimide compound from the example or the fluorescent compound from the comparative example, 0.99 g of binder resin (Cychromer P(ACA)Z320 manufactured by Daicel Corporation), photopolymerization initiator OXE-02, and Propylene glycol methyl ether (PGME) solvent. The solution of the obtained resin composition was applied to a glass plate to a thickness of 2 μm and pre-baked on a hot plate at 100°C for 3 minutes. After cooling, the obtained coating film was exposed to light at an intensity of 200 mJ. The chromaticity of the cured film after exposure was 1 (L). * (1), a * (1), b *(1)) was measured using a spectrophotometer (CM-5, manufactured by Konica Minolta, Inc.). After that, the glass plate was placed in a lightfastness tester (SUNTESTCPS+, manufactured by Toyo Seiki Corporation) and tested at 60 W / m². 2 The glass plate was left at 60°C for 24 hours. After removing the glass plate, the chromaticity was 2 (L). * (2), a * (2), b * (2)) was measured, and the color difference ΔE*ab was calculated in the same manner as the evaluation of the color stability of the coating film after the thermal history described above, and the color stability of the coating film after the light history was evaluated. The results are shown in Table 1 below. ◎: △E * ab ≤ 5% ○: 5% < △E * ab ≤ 10% △: 10% < △E * ab ≤ 15% ×: 15% < △E * ab
[0073] [Test Example 3] Solubility: Measurement of Solubility 0.3 g of the naphthalimide compound from each example or the fluorescent compound from the comparative example was added to 10 g of Propylene glycol methyl ether (PGME) solvent in a 200 mL sample bottle. A stirring bar was added and the mixture was stirred at 20°C for 15 minutes, then left to stand at 25°C for 10 minutes. Dissolution was observed visually and judged. The results are shown in Table 1 below. ○: Completely dissolved △: Partially dissolved ×: Almost completely dissolved and precipitated
[0074]
[0075] From the results in Table 1 above, it can be seen that Comparative Examples 4 to 6, whose structures are completely different from the naphthalimide compound represented by formula (1) according to the present invention in terms of their basic skeleton, had remaining issues in both light resistance and solubility compared to Examples 1 to 4.
[0076] Furthermore, although it has the same basic skeleton as the naphthalimide compound of the structure represented by formula (1) according to the present invention, the group R 1 and R 2 Comparative Examples 1 and 2, which have structures that do not contain linear or branched aliphatic hydrocarbon groups, also showed remaining issues in both light resistance and solubility compared to Examples 1 to 4.
[0077] Furthermore, it has the same basic skeleton as the naphthalimide compound of the structure represented by formula (1) according to the present invention, and R 2 Although it has an unsaturated carbon bond at the R position, 1 Comparative Example 3, which has a structure that does not have a linear or branched aliphatic hydrocarbon group at the position, also showed that it still had issues with both light resistance and solubility compared to Examples 1 to 4.
[0078] In other words, as shown in Examples 1 to 4, the naphthalimide compounds according to the present invention possess structural features not found in conventional materials, and thus possess high light resistance, excellent fluorescence properties, and solubility. Furthermore, as shown in Examples 1 and 2, the group R 1 and R 2 If the group has an unsaturated carbon bond and is a straight-chain or branched aliphatic hydrocarbon group, it can be said to have particularly high light resistance.
Claims
1. General formula (1): [In formula (1), R 1 and R 2 Each independently represents a linear or branched aliphatic hydrocarbon group having 1 to 8 carbon atoms, which may contain at least one of an unsaturated carbon bond, an alcoholic hydroxyl group, an ether bond, and an ester bond, provided that the R 1 and R 2 At least one of them contains the unsaturated carbon bond (where R 1 and R 2 A naphthalimide compound represented as follows: (However, if it contains an ester bond, the one carbon atom constituting the ester bond is not included in the number of carbon atoms.) 2. In equation (1), the R 1 and R 2 The naphthalimide compound according to claim 1, wherein at least one of the components comprises the alcoholic hydroxyl group.
3. In formula (1), the aforementioned R 1 and R 2 are each independently the naphthalimide compound according to claim 1, which contains the aforementioned unsaturated carbon bond.
4. The naphthalimide compound according to any one of claims 1 to 3, wherein the naphthalimide compound represented by the general formula (I) is a wavelength conversion compound.
5. A wavelength conversion resin composition comprising a naphthalimide compound according to any one of claims 1 to 3 and a binder resin.
6. A cured product obtained by curing the wavelength conversion resin composition described in claim 5.