Conjugated diene polymer composition

The conjugated diene polymer composition with phenothiazine derivative and amine-based antioxidant copolymerization stabilizes diene-based rubbers against oxidative degradation, addressing health and migration issues, and enhancing durability.

WO2026239807A1PCT designated stage Publication Date: 2026-11-19UNIMATEC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015029
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-07-11
Filing Date
2026-04-13
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Diene-based synthetic rubbers are susceptible to oxidative degradation due to unsaturated bonds, leading to loss of properties over time, and existing methods to chemically bond antioxidants to rubber molecules are not general-purpose or practical, posing health risks and migration issues.

Method used

A conjugated diene polymer composition comprising a phenothiazine derivative compound monomer and a conjugated diene monomer with an amine-based antioxidant, copolymerized to stabilize against oxidative degradation.

Benefits of technology

The composition stabilizes diene-based rubber components against oxidative degradation, ensuring safe use and extended lifespan under diverse and harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015029_19112026_PF_FP_ABST
    Figure JP2026015029_19112026_PF_FP_ABST
Patent Text Reader

Abstract

This conjugated diene polymer composition is obtained by adding 0.01-5 parts by weight of an amine-based antioxidant to 100 parts by weight of a conjugated diene polymer that essentially comprises a conjugated diene monomer and a phenothiazine derivative compound monomer represented by the general formula (wherein R1 is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, and R2 is a hydrogen atom or a methyl group) as copolymerization components. This conjugated diene polymer composition makes it possible to stabilize a diene rubber member against oxidative degradation due to oxygen, ozone, heat, light, and the like. As a result, this conjugated diene polymer composition makes it possible to safely utilize the diene rubber member in various and harsh use environments and to prolong the service life of the diene rubber member.
Need to check novelty before this filing date? Find Prior Art

Description

Conjugated diene polymer composition

[0001] This invention relates to a conjugated diene polymer composition. More specifically, it relates to a conjugated diene polymer composition with excellent resistance to oxidative degradation.

[0002] A wide variety of synthetic rubbers, manufactured from natural rubber or fossil resources, are processed into various shapes and used according to their applications. They permeate every corner of our economy and society, providing us with immense convenience and benefits in our lives.

[0003] For example, diene-based synthetic rubbers, such as styrene-butadiene rubber (SBR), offer an excellent balance of properties including strength, abrasion resistance, elasticity, and low-temperature resistance, and are relatively inexpensive, making them widely used in applications such as automobile tires, vibration damping rubber, and hoses. However, due to the unsaturated bonds present in their molecular chains, diene-based synthetic rubbers are susceptible to oxidative degradation from oxygen, ozone, heat, and light, which can cause them to lose their original properties and functions over time. Therefore, antioxidants are added during the manufacturing and molding processes to prevent this.

[0004] In the manufacturing process, non-contaminating phenolic antioxidants tend to be used, while in the molding process, aromatic amine antioxidants with excellent oxidative degradation prevention effects tend to be used. From these, antioxidants suitable for the purpose, application, and usage environment are appropriately selected.

[0005] Regarding aromatic amine antioxidants, the following issues exist: • Antioxidants that pose health risks to humans require occupational safety and health measures to prevent exposure to humans during their use. • Various problems arise from the migration of antioxidants within the rubber molded material, specifically, issues of poor appearance due to surface migration of antioxidants and resulting contamination of other materials, volatilization of antioxidants to the outside due to heat, or extraction of antioxidants by water, oils, solvents, etc. • When rubber molded materials come into direct contact with drinking water or food, or when used in medical components, care must be taken to ensure that the amount of antioxidant leached is acceptable from a health perspective. • In the case of large molded materials such as automobile tires, there is a risk that large amounts of antioxidants may volatilize or leach into the external environment.

[0006] From this perspective, attempts have been made to chemically bond antioxidant components to rubber molecules in order to suppress the elution and volatilization of antioxidants contained in rubber molded materials (Patent Documents 1-4, Non-Patent Documents 1-3). However, the methods described in these documents cannot be said to be general-purpose or practical.

[0007] JP 4-264106 JP 5-230132 JP 2009-209268 WO 2020 / 158132 WO 2024 / 247785

[0008] Rubber Chem. Technol., Vol. 45, p. 204 (1972) Rubber Chem. Technol., Vol. 46, p. 106 (1973) Rubber Chem. Technol., Vol. 52, p. 883 (1979)

[0009] In light of these circumstances, the present inventors have previously proposed a technique for stabilizing synthetic polymer materials against oxidative degradation by copolymerizing phenothiazine derivative compounds with various polymerizable unsaturated monomers (Patent Document 5). However, in order to maintain the product life in the diverse and harsh operating environments that diene-based rubber components face, there is a need to further improve their resistance to oxidative degradation.

[0010] The objective of the present invention is to achieve the general formula (Here, R 1 R is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, 2 This is achieved by a conjugated diene polymer composition comprising 100 parts by weight of a conjugated diene polymer, in which a phenothiazine derivative compound monomer (represented by a hydrogen atom or a methyl group) and a conjugated diene monomer are essential copolymer components, and 0.01 to 5 parts by weight of an amine-based antioxidant.

[0011] The conjugated diene polymer composition according to the present invention makes it possible to stabilize diene-based rubber components against oxidative degradation caused by oxygen, ozone, heat, light, etc., and as a result enables the safe use and extended lifespan of diene-based rubber components under diverse and harsh operating environments.

[0012] This graph compares the rate of change in elongation at break (white bars) after an air heating aging test (100°C, 250 hours) for each example and comparative example, with the rate of change in elongation at break (black bars) after immersion in toluene at room temperature for 168 hours, followed by another air heating aging test (100°C, 250 hours).

[0013] The conjugated diene polymer composition of the present invention comprises a conjugated diene polymer and an amine-based antioxidant. The conjugated diene polymer requires a phenothiazine derivative compound monomer [I] and a conjugated diene monomer as copolymer components.

[0014] Phenothiazine derivative compound monomers used in conjugated diene polymers have a general formula (Here, R 1 R is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, 2 (where is a hydrogen atom or a methyl group).

[0015] R 1 Specific examples include methyl group, ethyl group, n-propyl group, n-butyl group, n-pentyl group, n-hexyl group, n-heptyl group, n-octyl group, 2-ethylhexyl group, n-nonyl group, isopropyl group, 2-butyl group, 2-pentyl group, 3-pentyl group, 2-hexyl group, 3-hexyl group, 2-heptyl group, 3-heptyl group, 4-heptyl group, 2-octyl group, 3-octyl group, 4-octyl group, tertiary butyl group, 1,1-dimethyl-1- Examples include propyl group, 1,1-dimethyl-1-butyl group, 1,1-dimethyl-1-pentyl group, 1,1-dimethyl-1-hexyl group, 3-methyl-3-pentyl group, 3-ethyl-3-pentyl group, 3-methyl-3-hexyl group, etc., or cyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, 1-methyl-1-cyclopentyl group, 1-methyl-1-cyclohexyl group, 1-adamantyl group, etc.

[0016] R 2 This is either a hydrogen atom or a methyl group.

[0017] Specific examples of phenothiazine derivative compound monomers [I] include 2-ethenyl-10-methyl-10H-phenothiazine, 2-(1-methylethenyl)-10-methyl-10H-phenothiazine, 3-ethenyl-10-methyl-10H-phenothiazine, and 3-(1-methylethenyl)-10-methyl-10H-phenothiazine.

[0018] The proportion of phenothiazine derivative compound monomer [I] in the conjugated diene polymer is 0.001 to 5.0% by weight, preferably 0.01 to 2.0% by weight, when the total monomer is considered as 100% by weight as the amount of bonded monomers. A lower proportion does not provide sufficient protection against oxidative degradation, while a higher proportion does not provide any improvement in protection against oxidative degradation and is therefore uneconomical.

[0019] Examples of conjugated diene monomers include 1,3-butadiene, isoprene, chloroprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 1,3-heptadiene, 2-phenyl-1,3-butadiene, and 2-chloro-1,3-butadiene, with 1,3-butadiene, isoprene, and chloroprene being preferred. Each can be used alone or in combination of two or more.

[0020] Examples of polymerizable unsaturated monomers other than conjugated diene monomers used in conjugated diene polymers include aromatic vinyl monomers, nitrile group-containing unsaturated monomers, alkyl acrylate monomers, acrylamide, vinyl acetate, methyl vinyl ether, ethyl vinyl ether, ethylene, propylene, isobutylene, piperine, vinyl chloride, vinylidene chloride, etc., which may be used individually or in combination of two or more.

[0021] Specific examples of aromatic vinyl monomers include styrene, α-methylstyrene, 3-methylstyrene, 4-methylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-ethylstyrene, and 4-tertiary butylstyrene.

[0022] Examples of nitrile group-containing unsaturated monomers include acrylonitrile and methacrylonitrile.

[0023] Examples of alkyl acrylate monomers include methyl acrylate, ethyl acrylate, and butyl acrylate.

[0024] When the conjugated diene polymer is a copolymer of a phenothiazine derivative compound monomer [I] and a conjugated diene monomer with other polymerizable unsaturated monomers, the copolymerization form may be any of a random copolymer, a block copolymer, an alternating copolymer, or a graft copolymer.

[0025] Specific examples of conjugated diene polymers include monomer [I], styrene and butadiene random copolymers, monomer [I] and butadiene random copolymers, monomer [I] and isoprene random copolymers, monomer [I], butadiene and acrylonitrile random copolymers, monomer [I] and chloroprene rubber random copolymers, monomer [I], butadiene and isobutylene random copolymers, and the like.

[0026] There are no particular restrictions on the molecular weight of the diene polymer, but for example, the weight-average molecular weight Mw is between 100,000 and 1,000,000. Note that the weight-average molecular weight is the polystyrene-equivalent molecular weight measured by gel permeation chromatography.

[0027] Regarding the production method of conjugated diene polymers, radical polymerization, anionic polymerization, cationic polymerization, or coordination polymerization methods are used from the perspective of the active species in the polymerization reaction, and solution polymerization, bulk polymerization, emulsion polymerization, suspension polymerization, and gas-phase polymerization methods are used from the perspective of the phase state of the polymerization reaction. Conjugated diene polymers are produced by polymerization methods suitable for the type and application of each polymer.

[0028] As the amine-based antioxidant, an aromatic amine-based antioxidant is preferably used, and a paraphenylenediamine-based antioxidant is even more preferably used. Specific examples include N-isopropyl-N′-phenyl-p-phenylenediamine, N-octyl-N′-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine, N-(1,4-dimethylpentyl)-N′-phenyl-p-phenylenediamine, N-(1-methylheptyl)-N′-phenyl-p-phenylenediamine, N-(1-ethyl-3-methylpentyl)-N′-phenyl-p-phenylenediamine, N-cyclohexyl-N′-p-phenylenediamine, N,N′-dicyclohexyl-p-phenylenediamine, N,N′-di2-butyl-p-phenylenediamine, N,N′-bis(2-methylphenyl)-p-phenylenediamine, N,N′-diphenyl-p-phenylenediamine, and N,N′-dinaphthyl-p-phenylenediamine.

[0029] Furthermore, amine-ketone condensates can also be used, with specific examples including 2,2,4-trimethyl-1,3-dihydroquinoline, 2,2,4-trimethyl-1,3-dihydroquinoline polymer, 6-methoxy-2,2,4-trimethyl-1,3-dihydroquinoline, 6-methoxy-2,2,4-trimethyl-1,3-dihydroquinoline polymer, 6-ethoxy-2,2,4-trimethyl-1,3-dihydroquinoline, 6-ethoxy-2,2,4-trimethyl-1,3-dihydroquinoline polymer, acetone and diphenylamine condensate, acetone and N-phenyl-2-naphthylamine, etc.

[0030] These can be used individually or in combination of two or more amine-based antioxidants.

[0031] The amine-based antioxidant is used in a ratio of 0.01 to 5 parts by weight, preferably 0.1 to 2 parts by weight, per 100 parts by weight of the conjugated diene polymer. If the amine-based antioxidant is used in a smaller proportion than this, a sufficient oxidative degradation prevention effect cannot be obtained, while if it is used in a larger proportion, no improvement in the oxidative degradation prevention effect can be expected, making it uneconomical.

[0032] In the case of a member formed by crosslinking the conjugated diene polymer composition of the present invention, various additives commonly used in the production of such crosslinked members can be used in addition to the conjugated diene polymer and the amine-based antioxidant. Specific examples include crosslinking agents, crosslinking accelerators, crosslinking acceleration auxiliaries, reinforcing materials, fillers, softeners, plasticizers, tackifiers, lubricants, peptizing agents, and pigments.

[0033] As the crosslinking agent, a crosslinking agent suitable for the crosslinking method corresponding to the type of each diene rubber and its application is used. For example, sulfur is used in sulfur crosslinking, and organic peroxides such as benzoyl peroxide and dicumyl peroxide are used in organic peroxide crosslinking. Various crosslinking agents suitable for quinone dioxime crosslinking, metal oxide crosslinking, and thiourea crosslinking are also used.

[0034] Examples of the crosslinking accelerator include sulfenamides, guanidines, aldehyde-ammonia compounds, aldehyde-amine compounds, thioureas, thiazoles, thiurams, dithiocarbamate salts, and xanthates, which are appropriately selected according to the type of diene rubber, processing conditions, and properties of the final product. In this case, the above compounds may be used alone or in combination of two or more thereof.

[0035] As the crosslinking acceleration auxiliary, a metal oxide such as zinc oxide or a higher fatty acid such as stearic acid may be used alone or in combination of two or more thereof.

[0036] In addition to the crosslinking agent and the crosslinking accelerator, various additives, fillers and the like commonly used in the production of molded members can be used.

[0037] The conjugated diene polymer composition can be prepared using an open-type kneading apparatus or a closed-type kneading apparatus. For example, compounding ingredients excluding the crosslinking agent and the crosslinking accelerator, the diene copolymer and the aromatic amine-based antioxidant are mixed by a Banbury mixer or a pressure kneader, then the crosslinking agent and the crosslinking accelerator are added to the resulting mixture, and the mixture is blended using an open roll or the like, whereby the conjugated diene polymer composition can be prepared.

[0038] Crosslinking of the conjugated diene polymer composition is carried out by primary crosslinking at about 100 to 200°C for about 1 to 60 minutes, and optionally oven crosslinking (secondary crosslinking) at about 120 to 200°C for about 1 to 20 hours.

[0039] When the conjugated diene polymer is a thermoplastic elastomer, the conjugated diene polymer composition of the present invention may be simply heat-molded without crosslinking to produce the member. In that case, in addition to the amine-based antioxidant, various additives, fillers and the like commonly used in the production of the molded member are mixed. Molding of the conjugated diene polymer composition is performed by a method suitable for a desired molded member, such as extrusion molding, injection molding, compression molding and the like.

[0040] Next, the present invention will be specifically described with reference to Examples. The present invention, including its effects, is not limited to these Examples.

[0041] Reference Example 1 A 1000 ml four-necked flask equipped with a magnetic stirrer, a thermometer, a reflux tube, a nitrogen gas inlet tube and a discharge tube was charged with 0.40 g of 3-ethenyl-10-methyl-10H-phenothiazine (MePTZV). Subsequently, after the inside of the flask was purged with nitrogen gas, 200 g of a 15% toluene solution of 1,3-butadiene (product of Tokyo Chemical Industry), 10 g of styrene and 2.0 ml of tetrahydrofuran were sequentially added. Then, while introducing nitrogen gas into the container, 0.50 ml of n-butyllithium hexane solution (1.6 mol / L) was added to initiate the polymerization reaction. As the polymerization progressed, the temperature of the reaction solution rose from 20°C to a maximum temperature of 80°C. At 40 minutes after the start of polymerization, 0.8 ml of methanol was added to terminate the polymerization reaction. The obtained reaction solution was poured into 500 ml of methanol to precipitate a styrene-butadiene copolymer. This was dried under reduced pressure at 100°C for 2 hours to obtain 40 g of styrene-butadiene copolymer A.

[0042] This copolymer A is 1It was confirmed by H-NMR that the MePTZV copolymerization amount was 0.85%, the bound styrene content was 24%, and the vinyl bond content was 55%. Further, when the molecular weight of this copolymer A was measured under the following measurement conditions using gel permeation chromatography (HPLC system 20A manufactured by Shimadzu Corporation), the number average molecular weight (Mn) was 230,000, the weight average molecular weight (Mw) was 269,000 (both are polystyrene equivalent values), and Mw / Mn was 1.17. MePTZV copolymerization amount (wt%) = (M / 3)×239×100 / [(Hc / 5)×104 + ((Hb / 2)+(Ha / 4))×54 + (M / 3)×239] Ha: Peak integrated value at 4.3-5.0 ppm Hb: Peak integrated value at 5.0-6.1 ppm Hc: Peak integrated value at 6.1-7.7 ppm M: Peak integrated value at 3.2-3.4 ppm Column: Shodex GPC KF-807L×4 Detector: RID-20A Measurement temperature: 40°C Sample concentration: 0.2% THF solution Carrier (THF) flow rate: 1.0 mL / min

[0043] Reference Example 2 In Reference Example 1, the polymerization reaction was carried out using 0.04 g of MePTZV, to obtain 40 g of styrene-butadiene copolymer B. This copolymer B 1 It was confirmed by H-NMR that the MePTZV copolymerization amount was 0.09%, the bound styrene content was 25%, and the vinyl bond content was 55%. Further, this copolymer B had a number average molecular weight (Mn) of 240,000, a weight average molecular weight (Mw) of 281,000, and Mw / Mn of 1.17.

[0044] Reference Example 3 In Reference Example 1, the polymerization reaction was carried out without using MePTZV, to obtain 40 g of styrene-butadiene copolymer C. This copolymer C 1 It was confirmed by H-NMR that the bound styrene content was 25%, and the vinyl bond content was 54%. Further, this copolymer C had a number average molecular weight (Mn) of 250,000, a weight average molecular weight (Mw) of 288,000, and Mw / Mn of 1.15.

[0045] The styrene-butadiene copolymers A, B, or C obtained in Reference Examples 1-3 were subjected to a heating test in air at 80°C for 168 hours, and the Mooney viscosity (PML) before and after the test was measured. 1+4 The thermal stability of the uncrosslinked rubber was measured at 100°C and used as an indicator of its thermal stability. The results obtained are shown in Table 1 below. Table 1 Styrene-butadiene copolymer A B C MePTZV copolymer amount (wt%) 0.85 0.09 0 Before test PML 1+4 35 32 34 Hue (visual inspection) Colorless Colorless Colorless After heating test at 80°C for 168 hours PML 1+4 32 30 150 Hue (visual observation) Colorless Colorless yellow In styrene-butadiene copolymers A or B copolymerized with MePTZV, there was almost no change in Mooney viscosity before and after the heating test. On the other hand, in styrene-butadiene copolymer C, which was not copolymerized with MePTZV, thermal curing progressed in the heating test, and a significant increase in Mooney viscosity was observed.

[0046] Example 1 Styrene-butadiene copolymer A obtained in Reference Example 1 100 parts by weight FEF carbon black (Tokai Carbon Products Seast GSO) 50 parts by weight Stearic acid (Miyoshi Oil & Fat Products TST) 2.0 parts by weight Sulfur (Hosoi Chemical Industry Products Precipitated Sulfur) 1.5 parts by weight Zinc oxide (Sakai Chemical Industry Products Zinc Oxide No. 2) 3.0 parts by weight Crosslinking accelerator CBS (Ouchi Shinko Chemical Industry Products Noxellar CZ-G) 1.8 parts by weight Crosslinking accelerator DPG (Ouchi Shinko Chemical Industry Products Noxellar D) 1.5 parts by weight Amine-based antioxidant 6PPD 1.0 parts by weight (Ouchi Shinko Chemical Industry Products Nocrack 6C; N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine) Each of the above components was mixed in an open roll to obtain a conjugated diene polymer composition. This was subjected to primary crosslinking at 160°C for 20 minutes using a 100-ton press molding machine to obtain a sheet-like crosslinked material with a thickness of approximately 2 mm.

[0047] The following tests and measurements were performed using the obtained sheet-like crosslinked material. Mooney scorch test: In accordance with JIS K6300-1:2013 corresponding to ISO 289-1 (125℃). Minimum Mooney viscosity (ML min) and scorch time (t5) were measured using a Mooney viscometer AM-3 manufactured by Toyo Seiki Seisakusho. Physical properties under normal conditions: In accordance with JIS K6251:2017 corresponding to ISO 37 and JIS K6253:2017 corresponding to ISO 7619-1. Air heating aging test: In accordance with JIS K6257 corresponding to ISO 188 (100℃, 250 hours). Combined test: After immersion in toluene at room temperature for 168 hours, air drying was performed, followed by an air heating aging test at 100℃ for 250 hours. Ozone degradation test: In accordance with JIS K6259-1:2015 corresponding to ISO 1431. Using a JIS No. 3 dumbbell before and after toluene immersion (room temperature, 168 hours), the observation area (20mm between gauge marks) was 10%. Under extension conditions, cracks on the sample surface were observed after exposure to an ozone concentration of 50 pphm, 40°C, and test durations of 2, 4, 8, or 24 hours. Crack ranks were assigned as follows: A for a small number of cracks, B for many, and C for countless cracks. Crack depth was determined according to the following criteria: 1: Cracks visible with a 10x magnifying glass, but not visible to the naked eye; 2: Cracks visible to the naked eye, but depth not visible; 3: Less than 1 mm; 4: 1-3 mm; 5: 3 mm or more (including cracks that appear likely to cause the specimen to fracture).

[0048] Comparative Example 1: In Example 1, the amine-based antioxidant 6PPD was not used.

[0049] Comparative Example 2: In Example 1, instead of copolymer A, styrene-butadiene copolymer C obtained in Reference Example 3 was used.

[0050] Comparative Example 3: In Comparative Example 2, the amine-based antioxidant 6PPD was not used.

[0051] Example 2 In Example 1, TMQ (Nocrac 224, a product of Ouchi Shinko Chemical Industry Co., Ltd.; 2,2,4-trimethyl-1,2-dihydroquinoline polymer) was used in the same amount (1.0 part by weight) as 6PPD as an amine-based antioxidant.

[0052] Comparative Example 4: In Comparative Example 2, TMQ (Nocrack 224) was used in the same amount (1.0 part by weight) as 6PPD as the amine-based antioxidant.

[0053] Example 3 In Example 1, ETMQ (Nocrac AW-N, a product of Ouchi Shinko Chemical Industry; 6-ethoxy-1,2-dihydro-2,2,4-trimethylquinoline) was used in the same amount (1.0 part by weight) as the amine antioxidant instead of 6PPD.

[0054] Comparative Example 5: In Comparative Example 2, ETMQ (Nocrack AW-N) was used in the same amount (1.0 part by weight) as 6PPD as the amine-based antioxidant.

[0055] Example 4 In Example 1, IPPD (Nocrac 810-NA; N-isopropyl-N'-p-phenylenediamine), a product of Ouchi Shinko Chemical Industry, was used in the same amount (1.0 part by weight) as the amine antioxidant instead of 6PPD.

[0056] Comparative Example 6: In Comparative Example 2, IPPD (Nocrack 810-NA) was used in the same amount (1.0 part by weight) as 6PPD as the amine-based antioxidant.

[0057] The results obtained in Examples 1-4 and Comparative Examples 1-6 are shown in Tables 2-3. Note that in Comparative Example 3, the 100% modulus change rate could not be measured due to fracture. Table 2 Measurement Results Actual-1 Ratio-1 Ratio-2 Ratio-3 Mooney Scorch Test MLmin (pts) 27 25 29 22 t5 (min) 12.3 16.2 12.2 14.4 Normal Physical Hardness (Duro A) 69 70 69 67 100% Modulus (MPa) 3.3 3.7 3.3 3.4 Breaking Strength (MPa) 16.9 16.7 16.1 15.5 Elongation at Break (%) 410 370 390 380 Thermal aging test (100℃, 250 hours) Hardness change (Duro A) +8 +7 +9 +10 100% Modulus change rate (%) +106 +76 +91 +85 Strength change rate at break (%) +7 -2 +7 +15 Elongation change rate at break (%) -41 -39 -35 -27 Combined test (toluene immersion / thermal aging test) Hardness change (Duro A) +8 +8 +12 +17 100% Modulus change rate (%) +139 +127 +206 - Strength change rate at break (%) +8 +6 -4 -33 Elongation change rate at break (%) -51 -50 -63 -79 Ozone degradation test (before toluene immersion) 2 hours No cracks No cracks No cracks B-1 4 hours A-2 C-2 A-2 B-2 8 hours A-3 B-3 A-3 C-3 24 hours A-4 B-4 A-4 C-4 Ozone degradation test (after toluene immersion) 2 hours A-1 B-1 B-1 B-1 4 hours A-2 B-2 B-2 B-2 8 hours A-3 B-3 B-3 B-3 24 hours A-4 B-4 B-4 B-4 Table 3 Measurement results Actual -2 Ratio -4 Actual -3 Ratio -5 Actual -4 Ratio -6 Mooney's scorch test (125℃) MLmin (pts) 24 29 25 31 25 29 t5 (min) 15.4 13.9 15.1 13.9 12.7 13.9. Physical properties: Hardness in normal conditions (Duro A) 68 69 68 68 67 68 100% Modulus (MPa) 3.0 3.3 3.2 3.2 3.1 3.4 Breaking strength (MPa) 17.0 16.4 17.1 17.7 16.8 16.8 Elongation at Break (%) 410 380 400 400 410 390 Heat aging test (100℃, 250 hours) Hardness change (Duro A) +7 +7 +7 +8 +9 +8 100% Modulus change rate (%) +90 +103 +113 +81 +94 +79 Strength change rate at break (%) +8 +9 +5 +5 -2 +4 Elongation change rate at break (%) -34 -31 -35 -33 -43 -36 Combined test (toluene immersion / heat aging test) Hardness change (Duro A) +9 +6 +8 +8 +8 +10 100% Modulus change rate (%) +107 +94 +109 +109 +123 +124 Strength change rate at break (%) +8 -4 +1 -10 +6 -12 Change in elongation at break (%) -43 -50 -47 -56 -48 -58 Ozone degradation test (before toluene immersion) 2 hours A-1 A-1 No cracks No cracks No cracks No cracks 4 hours A-2 B-2 B-2 B-2 No cracks No cracks 8 hours A-3 B-3 B-3 B-3 No cracks A-2 24 hours A-4 B-4 B-4 B-4 No cracks A-4 Ozone degradation test (after toluene immersion) 2 hours B-1 B-1 B-1 B-1 No cracks B-1 4 hours B-2 C-2 C-2 C-2 C-2 C-2 8 hours B-3 C-3 C-3 C-3 C-3 C-3 24 hours B-4 B-4 B-4 B-4 B-4 B-4 .

[0058] From the above results, the following can be concluded: (1) A molded member obtained by crosslinking a composition in which a phenothiazine derivative compound [I] is copolymerized with a conjugated diene copolymer to which an amine-based antioxidant is added can have improved heat aging resistance after an antioxidant extraction test using a liquid medium (see Figure 1). (2) Furthermore, it is also possible to improve ozone resistance before the antioxidant extraction test using a liquid medium (see Tables 2-3).

Claims

1. General formula (Here, R 1 R is a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, 2 A conjugated diene polymer composition comprising 100 parts by weight of a conjugated diene polymer in which a phenothiazine derivative compound monomer (where is a hydrogen atom or a methyl group) and a conjugated diene monomer are essential copolymer components, and 0.01 to 5 parts by weight of an amine-based antioxidant.

2. The conjugated diene polymer composition according to claim 1, wherein the conjugated diene polymer is a copolymer of a phenothiazine derivative compound monomer [I] and a conjugated diene monomer.

3. The conjugated diene polymer composition according to claim 1, wherein the conjugated diene polymer is a copolymer of a phenothiazine derivative compound monomer compound [I], a conjugated diene monomer, and a polymerizable unsaturated monomer other than a conjugated diene monomer.

4. The conjugated diene polymer composition according to claim 1, 2, or 3, wherein a conjugated diene polymer is used in which 0.001 to 5.0% by weight of a phenothiazine derivative compound monomer [I] is copolymerized, when the total monomer is considered as 100% by weight as the amount of bonded monomers.

5. The conjugated diene polymer composition according to claim 1, wherein the amine antioxidant is an aromatic amine antioxidant.

6. The conjugated diene polymer composition according to claim 5, wherein the aromatic amine antioxidant is a paraphenylenediamine antioxidant.

7. The conjugated diene polymer composition according to claim 1, wherein the amine-based antioxidant is an amine-ketone condensate.