Mixed material for organic electroluminescent element, and organic electroluminescent element
A mixed material of biscarbazole and azine compounds with specific substitutions addresses efficiency and lifespan issues in organic EL devices, achieving high performance and low voltage operation.
Patent Information
- Application Number
- PCT/JP2026/015523
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-04-17
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional organic electroluminescent (EL) devices face challenges in achieving high efficiency, long lifespan, and low driving voltage, particularly in applications like flat panel displays.
A mixed material comprising a biscarbazole compound crosslinked with oxygen, nitrogen, or sulfur atoms, and a predetermined azine compound, specifically an azine compound substituted with dibenzofuran or dibenzothiophene, is used to form organic EL devices, optimizing charge balance and transport properties through precise control of molecular interactions.
The mixed material results in organic EL devices with high efficiency, long lifespan, and low driving voltage, enhancing device characteristics by controlling charge injection and transport.
Smart Images

Figure JP2026015523_19112026_PF_FP_ABST
Abstract
Description
Mixed material for organic electroluminescent devices and organic electroluminescent devices
[0001] The present invention relates to a mixed material for organic electroluminescent devices and an organic electroluminescent device (referred to as an organic EL element) using the same. More specifically, the present invention relates to a mixed material for organic electroluminescent devices comprising a biscarbazole compound crosslinked with oxygen atoms, nitrogen atoms, or sulfur atoms, and a predetermined azine compound, and an organic EL element using the same.
[0002] When a voltage is applied to an organic electroluminescent element, holes are injected from the anode and electrons from the cathode into the light-emitting layer. In the light-emitting layer, the injected holes and electrons recombine to generate excitons. At this time, according to the statistical laws of electron spin, singlet excitons and triplet excitons are generated in a ratio of 1:3. Fluorescent organic EL elements that use emission from singlet excitons are said to have an internal quantum efficiency limited to 25%. On the other hand, phosphorescent organic EL elements that use emission from triplet excitons are known to have an internal quantum efficiency of up to 100% if intersystem crossing from singlet excitons is performed efficiently. However, extending the lifespan of phosphorescent organic EL elements remains a technical challenge.
[0003] More recently, highly efficient organic EL devices utilizing delayed fluorescence have been developed. For example, Patent Document 1 discloses an organic EL device that utilizes the TTF (Triplet-Triplet Fusion) mechanism, one of the mechanisms of delayed fluorescence. The TTF mechanism utilizes the phenomenon in which a singlet exciton is generated by the collision of two triplet excitons, and it is theoretically thought that the internal quantum efficiency can be increased to 40%. However, since its efficiency is lower compared to phosphorescent organic EL devices, further improvements in efficiency are needed.
[0004] On the other hand, Patent Document 2 discloses an organic EL device utilizing the TADF (Thermally Activated Delayed Fluorescence) mechanism. The TADF mechanism utilizes the phenomenon in which reverse intersystem crossing occurs from triplet excitons to singlet excitons in materials with a small energy difference between singlet and triplet levels, and is theoretically thought to be able to increase the internal quantum efficiency to 100%. However, similar to phosphorescent devices, further improvement in lifetime characteristics is required.
[0005] For example, Patent Documents 3 to 5 disclose the use of a mixed host consisting of an azine compound substituted with dibenzofuran or dibenzothiophene and a biscarbazole compound. Patent Document 6 also discloses the use of a mixed host consisting of an azine compound substituted with triphenylene and an oxygen-crosslinked biscarbazole compound, and Patent Documents 7 to 8 disclose the use of a mixed host consisting of an indrocarbazole-substituted azine compound and an oxygen-crosslinked biscarbazole compound. Furthermore, Patent Documents 9 and 10 disclose the use of an oxygen-crosslinked biscarbazole compound alone as a host material.
[0006] However, conventional organic EL elements as described above are not sufficient in terms of reducing the driving voltage, improving luminous efficiency, or extending lifespan, and further improvements are desired.
[0007] WO2010 / 134350, WO2011 / 070963, WO2018093015, Korean Patent No. 101959821, Japanese Patent No. 6891109, WO2022 / 197166, WO2018 / 043435, WO2025 / 047570, WO2011 / 019173, WO2014 / 057684
[0008] In order to apply organic EL elements to display elements such as flat panel displays, it is necessary to improve the luminous efficiency of the elements while simultaneously ensuring sufficient long-life characteristics. In view of the above situation, the present invention aims to provide a practically useful organic EL element and a suitable compound that have high efficiency and long lifespan despite having a low driving voltage.
[0009] As a result of diligent research to solve the above problems, the present inventors have found that by using a mixed material for organic electroluminescent devices consisting of a crosslinked biscarbazole compound having a structure in which two carbazoles are crosslinked by an oxygen atom, a nitrogen atom, or a sulfur atom, and a predetermined azine compound, particularly an azine compound substituted with dibenzofuran or dibenzothiophene, an organic electroluminescent device exhibiting excellent device characteristics can be obtained, thus completing the present invention.
[0010] The present invention relates to a mixed material for an organic electroluminescent device, comprising a compound represented by the following general formula (1) and a compound represented by the following general formula (2).
[0011] Here, X 1 This is a group represented by O, S, or N-Rb. 1 ~Y 12 These are groups that can be independently represented as N or C-Ra. 1 and Ar 2 Each of these is independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group having 2 to 5 aromatic rings linked together. Ra is independently hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, an alkyl group having 1 to 30 carbon atoms, a fluoroalkyl group having 1 to 30 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, a phosphoryl group, a silyl group, a germanium group, a cyano group, a nitro group, or a carboxyl group. If there are two or more Ra in general formula (1), the multiple Ra may be the same or different from each other. Rb is hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 5 aromatic rings of these aromatic groups are linked together.
[0012] In the above general formula (1), Y 1 ~Y 12are each independently a group represented by C-Ra, and it is further preferred that Ra is deuterium. Furthermore, in the aforementioned general formula (1), X 1 is preferably O or S. Further, in the aforementioned general formula (1), the average deuteration rate of hydrogen is preferably 30% or more. More preferably, the average deuteration rate of hydrogen is 40% or more, particularly preferably the average deuteration rate is 50% or more, and still more preferably the average deuteration rate is 80% or more. Here, the average deuteration rate is specifically described as follows: when the average deuteration rate of the compound represented by the aforementioned general formula (1) is 50%, if there are N hydrogen atoms in formula (1), it means that on average N / 2 of the hydrogen atoms are substituted with deuterium. The deuterated product represented by the aforementioned general formula (1) may consist of a compound having a single deuteration rate, or may be a mixture of compounds having different deuteration rates.
[0013] As a preferred embodiment of the aforementioned general formula (1), in consideration of the spread of molecular orbitals on the compound that is closely related to the charge balance that affects device characteristics, and the ease of intermolecular interaction of the molecular orbitals, any of the following Chemical Formula 1-64 to Chemical Formula 1-72, Chemical Formula 1-76 to Chemical Formula 1-83, and Chemical Formula 1-95 to Chemical Formula 1-104 may be mentioned. More preferred are Chemical Formula 1-64, Chemical Formula 1-66, Chemical Formula 1-68, Chemical Formula 1-69, Chemical Formula 1-71, Chemical Formula 1-95, Chemical Formula 1-97, Chemical Formula 1-98, Chemical Formula 1-100 or Chemical Formula 1-103, and still more preferred are Chemical Formula 1-66, Chemical Formula 1-68, Chemical Formula 1-71, Chemical Formula 1-98, Chemical Formula 1-100 or Chemical Formula 1-103. In addition, in the following chemical formulas, s means the average number of substitutions substituted with deuterium (D), and varies according to the average deuteration rate.
[0014]
[0015] Furthermore, in the aforementioned general formula (2), Ar 4 , Ar 5 , and Ar 6Each of these is independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 7 of these aromatic rings are linked together. 2 ~X 4 Each of them is independently N, C-H, or C-D, and at least one of them is N.
[0016] The compound of the general formula (2) can be represented by the following formula (3). In formula (3), symbols common to general formula (2) have the same meaning.
[0017] In the above general formula (3), Ar 10 Ar 11 , and Ar 12 Each of these is independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 3 of these aromatic rings are linked together. 14 ~R 15 Each of these is independently hydrogen, deuterium, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, or a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms. Y is selected from either O or S, and m and n are the number of substitutions, integers from 1 to 3. X 2 ~X 4 This is equivalent to the above general formula (2).
[0018] The compound of general formula (3) can be represented by the following forms (4) to (7), with the form represented by formula (7) being preferred. In formulas (4) to (7), symbols common to general formula (3) have the same meaning.
[0019] In the above general formula (3) and the above general formulas (4) to (7), Ar 10 However, in a preferred embodiment of the present invention, the group is any of the substituted or unsubstituted benzene, pyridine, pyrimidine, triazine, carbazole, dibenzofuran, triphenylene, or a substituted or unsubstituted linked aromatic group in which two or three of these are linked together. In a more preferred embodiment, Ar10 However, these are substituted or unsubstituted benzene, triazine, carbazole, or triphenylene.
[0020] Furthermore, in the general formula (2) above, it is preferable that the average deuteration rate of hydrogen is 30% or more. More preferably, the average deuteration rate of hydrogen is 40% or more, particularly preferably 50% or more, and even more preferably 80% or more.
[0021] In the mixed material for organic electroluminescent devices of the present invention, it is preferable that the proportion of the compound represented by general formula (1) is 20% by mass or more and 70% by mass or less, relative to the total of the compound represented by general formula (1) and the compound represented by general formula (2).
[0022] In the mixed material for organic electroluminescent elements of the present invention, it is preferable that at least one of the compounds represented by general formula (1) and general formula (2) has some or all of its hydrogen replaced with deuterium. More preferably, both the compound represented by general formula (1) and the compound represented by general formula (2) have some or all of their hydrogen replaced with deuterium. The average deuteration rate when hydrogen is replaced with deuterium is preferably 30% or more for each compound. The upper limit is 100%.
[0023] The mixed material for the organic electroluminescent element is used to form at least one layer of an organic electroluminescent element having multiple organic layers between the anode and the cathode, and is preferably a premixed material for forming the organic layer. Preferably, the organic layer is formed by a vapor deposition method, and it is preferable to mix the compound represented by general formula (1) and the compound represented by general formula (2) before vapor deposition to form a premixed material.
[0024] For this premixture, the difference in the 50% weight loss temperature between the compound represented by general formula (1) and the compound represented by general formula (2) is preferably 30°C or less, and more preferably 20°C or less.
[0025] Furthermore, the mixed material for the organic electroluminescent element in the present invention is preferably a molten mixture obtained by melting the compound represented by general formula (1) and the compound represented by general formula (2) by heating under reduced pressure or an inert gas atmosphere. Preferably, the difference between the maximum emission wavelength of the fluorescence emission spectrum of this molten mixture and the maximum emission wavelength of the fluorescence emission spectrum of either the compound represented by general formula (1) or the compound represented by general formula (2) is within ±10 nm.
[0026] Furthermore, the present invention relates to an organic electroluminescent element having a plurality of organic layers between an anode and a cathode, characterized in that at least one of the organic layers contains the above-mentioned mixed material for organic electroluminescent elements.
[0027] Preferably, the organic layer containing the mixed material for the organic electroluminescent element is at least one layer selected from the group consisting of an emissive layer, a hole injection layer, a hole transport layer, an electron transport layer, an electron injection layer, a hole blocking layer, and an electron blocking layer, and more preferably, it is an emissive layer. Furthermore, if the organic layer containing the mixed material for the organic electroluminescent element is an emissive layer, it is preferable that the emissive layer contains at least one luminescent dopant, and more preferably, it contains a compound represented by general formula (1) as a first host, a compound represented by general formula (2) as a second host, and the emissive layer contains at least one luminescent dopant.
[0028] Furthermore, in the organic electroluminescent device of the present invention, it is preferable that the luminescent dopant is an organometallic complex containing at least one metal selected from the group consisting of ruthenium, rhodium, palladium, silver, rhenium, osmium, iridium, platinum, and gold. Alternatively, it is preferable that the luminescent dopant is a thermally activated delayed fluorescence dopant.
[0029] Furthermore, the present invention relates to a method for manufacturing an organic electroluminescent element having a plurality of organic layers including a light-emitting layer between an anode and a cathode, characterized in that it includes the steps of preparing the above-mentioned mixed material for organic electroluminescent elements, and forming a light-emitting layer by evaporating and depositing this mixed material from a single evaporation source.
[0030] According to the present invention, it is possible to realize a practically useful organic EL element that has high efficiency and long lifespan despite having a low driving voltage.
[0031] This is a cross-sectional view showing an example of the structure of an organic EL element. This is the PL spectrum measured in the example (molten mixture M1, compound 1-66, compound 3-70). This is the PL spectrum measured in the example (molten mixture M2, Host B, Host C). This is the PL spectrum measured in the example (molten mixture M3, compound 3-7, Host E).
[0032] The mixed material for organic electroluminescent devices of the present invention comprises a compound represented by the following general formula (1) and a compound represented by the following general formula (2). In order to improve the characteristics of organic EL devices, it is necessary for the material used in the organic layer to have high resistance to charge, and in particular, in the light-emitting layer, it is important to suppress the leakage of excitons and charge to the surrounding layer. That is, improving the bias of the light-emitting region in the light-emitting layer is effective in suppressing this charge / exciton leakage, and in order to do so it is necessary to control the amount of both charges (electrons / holes) injected into the light-emitting layer or the transportability of both charges in the light-emitting layer to a desirable range.
[0033] The dual charge injection transport properties of materials used in organic layers are largely determined by the energy levels of the molecular orbitals and the magnitude of intermolecular interactions. When the mixed material for organic electroluminescent devices of the present invention is used as a material for an organic EL device, it contains a biscarbazole compound that has an energy level that is easily injected with holes and high hole transport properties, as represented by general formula (1), and is crosslinked with oxygen, nitrogen, or sulfur atoms that have a highly durable framework. Therefore, it is believed that this will provide an excellent organic EL device with high efficiency and long lifespan, even at low voltages.
[0034] Furthermore, when using the mixed material for organic electroluminescent devices of the present invention as a material for organic EL devices, it is more effective to use in combination an azine compound having a nitrogen-containing aromatic heterocycle as represented by general formula (2). Preferably, the compound has a structure in which a dibenzofuran or dibenzothiophene group is linked to a nitrogen-containing aromatic heterocycle, as represented by general formula (3). Specifically, such compounds can be shown as those represented by formulas (4) to (7) above. In this way, the substructure in which a dibenzofuran or dibenzothiophene group is linked to a nitrogen-containing aromatic heterocycle is responsible for the electron injection transport ability of the compound, and is particularly capable of high electron injection transport. More preferably, the compound has a structure in which the 1-position of a dibenzofuran or dibenzothiophene group is linked to a nitrogen-containing aromatic heterocycle, as represented by formula (7). In such a structure, the proximity of molecules can be suppressed due to the steric hindrance effect between the dibenzofuran or dibenzothiophene group and the nitrogen-containing aromatic heterocycle, the amount of electron injection transport can be controlled to a desirable range, and it is advantageous that the charge balance in the light-emitting layer, which greatly affects the characteristics of the device, can be optimized. In this way, by using dibenzofuran or dibenzothiophene groups, or substituent species of nitrogen-containing aromatic heterocycles, or by changing the bond positions between substituents, it is possible to control the intermolecular interactions of molecular orbitals that contribute significantly to electron injection transport to the luminescent layer at a high level.
[0035] Furthermore, by using a mixed material containing a compound represented by general formula (1) and a compound represented by general formula (2) that have the structural characteristics described above, the intermolecular interactions between dissimilar materials can be precisely controlled compared to combining dissimilar materials that do not possess these structural characteristics. As a result, the amount of charge injection transport in the light-emitting layer can be controlled to a degree that cannot be achieved with systems that do not possess the above structural characteristics, or with systems that use the compound represented by general formula (1) or the compound represented by general formula (2) alone. In particular, the localization of photochemical / electrochemical loads on each host material when these compounds are used as host materials can be reduced, resulting in a significant improvement in device characteristics.
[0036] Next, we will describe the compounds relating to general formula (1). In the above general formula (1), X 1 is O, S, or N-Rb, preferably O or S, and more preferably O. 1 ~Y 12 These are each independently represented by N or C-Ra. 1 and Ar 2 Each of these is independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 5 of these aromatic groups are linked together, and the aromatic hydrocarbon groups or aromatic heterocyclic groups in the linked case may be the same or different from each other.
[0037] In the above general formula (1), X 1 Even when X is a group represented by S or N-Rb, 1 Similar to oxygen, the electronic bonding pattern and molecular rigidity between carbazole skeletons are maintained, which is thought to result in excellent hole transport ability and durability. In particular, sulfur atom bridged structures tend to have a larger spatial extent of molecular orbitals compared to oxygen atom bridged structures, which is advantageous because it relaxes intermolecular interactions and suppresses charge accumulation and localization in the luminescent layer. Furthermore, in bridged structures represented by N-Rb, the electronic and steric effects of the substituent Rb are thought to control the degree of molecular orbital levels and intermolecular interactions, contributing to the optimization of the charge balance in the luminescent layer.
[0038] Ar 1 and Ar 2Each of these groups is, preferably independently, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 12 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group formed by the linkage of 2 to 5 of these aromatic groups; more preferably, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, or a substituted or unsubstituted linked aromatic group formed by the linkage of 2 of these aromatic hydrocarbon groups. Even more preferably, a substituted or unsubstituted phenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted naphthyl group, or a substituted or unsubstituted triphenylene group; most preferably, an unsubstituted phenyl group. The biphenyl group has a structure in which two benzene rings are linked, but the bond position of each benzene ring may be any of the o-, m-, or p- positions.
[0039] Here, Ar 1 ~Ar 2 However, specific examples of unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms, unsubstituted aromatic heterocyclic groups having 3 to 30 carbon atoms, or unsubstituted linked aromatic groups in which 2 to 5 aromatic rings of these aromatic groups are linked include, for example, benzene, naphthalene, acenaphthene, acenaphthylene, azulene, anthracene, chrysene, pyrene, phenanthrene, fluorene, triphenylene, thiophene, isothiazole, thiazole, pyrrole, pyrazole, imidazole, triazole, furan, isoxazole, quinoline, isoquinoline, quinoxaline, quinazo Examples of groups obtained by removing hydrogen from phosphorus, thiadiazole, phthalazine, tetrazole, indole, benzofuran, benzothiophene, benzoxazole, benzothiazole, indazole, benzimidazole, benzotriazole, benzoisothiazole, benzothiadiazole, purine, pyranone, coumarin, isocoumarin, chromone, dibenzofuran, dibenzothiophene, dibenzoselenophene, carbazole, phenoxazine, phenothiazine, acridine, or compounds composed of 2 to 5 of these groups. The hydrogens constituting these groups may be deuterated. Furthermore, the linked aromatic groups may be linked in a linear manner or in a branched manner. The same applies to Ra and Rb as to specific examples of these C6 to C30 aromatic hydrocarbon groups.
[0040] Ra is independently hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, an alkyl group having 1 to 30 carbon atoms, a fluoroalkyl group having 1 to 30 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, a phosphoryl group, a silyl group, a germanium group, a cyano group, a nitro group, or a carboxyl group. Preferably, it is hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, and more preferably, it is deuterium, a substituted or unsubstituted phenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted naphthyl group, or a substituted or unsubstituted triphenylene group. The biphenyl group has a structure in which two benzene rings are linked, but the bond position of each benzene ring may be any of the o-, m-, or p- positions. However, if there are two or more Ra in general formula (1), the multiple Ra may be the same or may be different from one another.
[0041] Specific examples of cases where Ra is an alkyl group having 1 to 30 carbon atoms include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl. These may also be deuterated. Preferably, they are deuterated alkyl groups having 1 to 4 carbon atoms. The propyl group and pentyl group may be linked in a linear or branched manner, and the hexyl group and heptyl group may be linked in a linear or cyclic manner, or branched. These may also be deuterated. Preferably, they are deuterated linear or branched propyl groups.
[0042] Furthermore, specific examples of cases where Ra is a fluoroalkyl group having 1 to 30 carbon atoms include fluoromethyl, difluoromethyl, trifluoromethyl, fluoroethyl, trifluoromethylmethyl, and pentafluoroethyl. These may also be deuterated. Preferably, it is a deuterated fluoroalkyl group having 1 to 10 carbon atoms.
[0043] Furthermore, specific examples of cases where Ra is a cycloalkyl group having 3 to 30 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, 1-adamantyl, 2-adamantyl, 1-norbornyl, and 2-norbornyl. These may also be deuterated. Preferably, they are deuterated cycloalkyl groups having 3 to 10 carbon atoms.
[0044] Furthermore, a specific example of the case where Ra is an aralkyl group having 7 to 30 carbon atoms is represented as -M-Z, where an example of M is an alkylene group corresponding to the alkyl group example above, and an example of Z is an aromatic hydrocarbon group. Specific examples of aralkyl groups include benzyl, phenylethyl, and 2-phenylpropan-2-yl. These may also be deuterated. The aromatic hydrocarbon portion of the aralkyl group preferably has 6 to 30 carbon atoms. The alkyl portion preferably has 1 to 10 carbon atoms, and more preferably is a deuterated group.
[0045] Furthermore, if Ra is a phosphoryl group, for example, -P(=O)R f1 R f2 It is a group represented by , and if it is a silyl group, for example, -SiR f1 R f2 R f3 It is a group represented by, and if it is a germanium group, for example, -GeR f1 R f2 R f3 It is a group represented by . Of these, R f1 ~R f3 These R are, independently, substituted or unsubstituted aromatic hydrocarbon groups having 6 to 30 carbon atoms, substituted or unsubstituted aromatic heterocyclic groups having 3 to 30 carbon atoms, alkyl groups having 1 to 30 carbon atoms, fluoroalkyl groups having 1 to 30 carbon atoms, or cycloalkyl groups having 3 to 30 carbon atoms. f1 ~R f3 Specific examples of each group are the Ar 1 ~Ar 2 This is similar to the specific example given in the previous case.
[0046] Rb is hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group having 2 to 5 aromatic rings linked together. Preferably, it is a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, or a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms; more preferably, it is a substituted or unsubstituted phenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted naphthyl group, or a substituted or unsubstituted triphenyl group; more preferably, it is a substituted or unsubstituted phenyl group, a substituted or unsubstituted biphenyl group, or a substituted or unsubstituted triphenyl group. The biphenyl group has a structure in which two benzene rings are linked together, but the bond position of each benzene ring can be any of the o-, m-, or p- positions.
[0047] Specific examples of general formula (1) are shown below, but the compound is not limited to these examples. In the structural formulas below, the number of s substitutions of the substituted deuterium (D) represents the average number and changes depending on the average deuteration rate.
[0048]
[0049]
[0050]
[0051]
[0052]
[0053]
[0054] Among these specifically illustrated example compounds, those that exhibit high performance in terms of luminous efficiency and device lifetime, while also having high thermal stability, are preferably those with chemical formulas 1-2 to 1-3, chemical formulas 1-5 to 1-6, chemical formula 1-9, chemical formulas 1-14 to 1-16, chemical formulas 1-18 to 1-20, chemical formulas 1-30 to 1-35, chemical formulas 1-37 to 1-38, chemical formula 1-40, chemical formulas 1-45 to 1-52, chemical formulas 1-64 to 1-72, chemical formulas 1-76 to 1-83, and chemical formulas 1-95 to 1-104.
[0055] Next, we will explain the compounds related to general formula (2).
[0056] In general formula (2), Ar 4 ~Ar 6 Each is independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, or a substituted or unsubstituted linked aromatic group having 2 to 7 aromatic rings of these aromatic groups linked together. Preferably, it is a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 15 carbon atoms, or a substituted or unsubstituted linked aromatic group having 2 to 3 such aromatic hydrocarbon groups linked together. More preferably, it is a substituted or unsubstituted phenyl group, a substituted or unsubstituted carbazolyl group, a substituted or unsubstituted dibenzothiophenyl group, a substituted or unsubstituted dibenzofuranyl group, or a substituted or unsubstituted linked aromatic group having 2 to 3 aromatic rings of these aromatic groups linked together. 2 ~X 4 Each of these is independently N, C-H, or C-D, and at least one is N. Here D represents deuterium. Preferably, X 2 ~X 4 At least two of them are N, and more preferably X 2 ~X 4 All of them are N.
[0057] Here, Ar 4 ~Ar 6Specific examples of unsubstituted aromatic hydrocarbon groups having 6 to 18 carbon atoms, unsubstituted aromatic heterocyclic groups having 3 to 17 carbon atoms, or linked aromatic groups formed by the linking of 2 to 7 of these aromatic groups include, for example, benzene, naphthalene, acenaphthene, acenaphthylene, azulene, anthracene, chrysene, pyrene, phenanthrene, fluorene, triphenylene, thiophene, isothiazole, thiazole, pyrrole, pyrazole, imidazole, triazole, thiadiazole, furan, isoxazole, quinoline, isoquinoline, quinoxaline, ki Examples of groups derived from nazoline, thiadiazole, phthalazine, tetrazole, indole, benzofuran, benzothiophene, benzoxazole, benzothiazole, indazole, benzimidazole, benzotriazole, benzoisothiazole, benzothiadiazole, purine, pyranone, coumarin, isocoumarin, chromone, dibenzofuran, dibenzothiophene, dibenzoselenophene, carbazole, phenoxazine, phenothiazine, acridine, or compounds composed of 2 to 7 of these linked together. 4 ~Ar 6 Specific examples of unsubstituted C6-C18 aromatic hydrocarbon groups, unsubstituted C3-C17 aromatic heterocyclic groups, or substituted or unsubstituted linked aromatic groups in which 2-7 of these aromatic rings are linked are as described above, but it is preferable that they include aromatic hydrocarbon rings such as triphenylene, chalcogen-containing aromatic heterocyclic rings such as dibenzofuran, nitrogen-containing aromatic heterocyclic rings such as pyridine, pyrimidine, triazine, and carbazole, and that the number of linked aromatic groups is 2-5. Specific examples of these C6-C18 aromatic hydrocarbon groups and C3-C17 aromatic heterocyclic groups are Ar 10 ~Ar 12 , R 14 ~R 15 The same applies to this case as well.
[0058] A preferred embodiment of the compound represented by general formula (2) can be represented by a structure like that of general formula (3) below. More preferably, it can be represented by a structure like that of general formulas (4) to (7) below, and more preferably by a structure like that of general formula (7).
[0059] Here, Ar in general formulas (2) to (7) 4 ~Ar 6 Ar 10 ~Ar 12 This is an unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, an unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, or a linked aromatic group in which 2 to 5 of these aromatic rings are linked together. Preferably, it is a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 15 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 3 of the aromatic hydrocarbon groups are linked together.
[0060] Also, R 14 ~R 15 Each of these is independently hydrogen, deuterium, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, or a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms. Preferably, it is hydrogen, deuterium, or a substituted or unsubstituted phenyl group. More preferably, it is hydrogen or deuterium. Also, R 14 ~R 15 When R is an aromatic hydrocarbon group, 14 ~R 15 It may also condense with a benzene ring or aromatic ring to form a ring.
[0061] R 14 ~R 15 and Ar 10 ~Ar 12 Specific examples of cases where is an unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, or an unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, are as described above, Ar 4 ~Ar 6 This is the same as in the previous case.
[0062] Also, R 14 ~R 15Specific examples of groups where the group is an aliphatic hydrocarbon group having 1 to 10 carbon atoms include, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups. These may be deuterated. Preferably, the group is a deuterated alkyl group having 1 to 4 carbon atoms. Here, the propyl group and pentyl group may be linked in a linear or branched manner, and the hexyl group and heptyl group may be linked in a linear or cyclic manner, or branched. These may also be deuterated, and preferably, they are deuterated linear or branched propyl groups.
[0063] Specific examples of compounds represented by the general formulas (2) to (7) are shown below, but the examples are not limited to these. In the structural formulas below, the number of s substitutions of the substituted deuterium (D) represents the average number and changes depending on the average deuterated rate.
[0064]
[0065] In this specification, a linked aromatic group refers to an aromatic group in which two or more aromatic rings are linked by a single bond. These linked aromatic groups may be linear or branched. The linking position when benzene rings are linked may be ortho, meta, or para, but para linkage or meta linkage is preferred. The aromatic groups may be aromatic hydrocarbon groups or aromatic heterocyclic groups, and the multiple aromatic groups may be the same or different.
[0066] In this specification, aromatic hydrocarbon groups, aromatic heterocyclic groups, or linked aromatic groups may each have substituents. When substituents are present, preferred substituents are deuterium, halogens, cyano groups, triarylsilyl groups, aliphatic hydrocarbon groups having 1 to 10 carbon atoms, alkenyl groups having 2 to 5 carbon atoms, alkoxy groups having 1 to 5 carbon atoms, or diarylamino groups having 12 to 44 carbon atoms. Here, when the substituent is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, it may be linear, branched, or cyclic. Furthermore, when the above triarylsilyl group or diarylamino group is a substituent of the aromatic hydrocarbon group, aromatic heterocyclic group, or linked aromatic group, silicon and carbon, or nitrogen and carbon, respectively, are bonded by a single bond. The number of substituents is preferably 0 to 5, and more preferably 0 to 2. Note that when calculating the number of carbon atoms in aromatic hydrocarbon groups and aromatic heterocyclic groups that have substituents, the number of carbon atoms of the substituents is not included. However, it is preferable that the total number of carbon atoms including the number of carbon atoms of the substituents satisfies the above range.
[0067] Specific examples of the above substituents include deuterium, cyano, methyl, ethyl, propyl, i-propyl, butyl, t-butyl, pentyl, neopentyl, cyclopentyl, hexyl, cyclohexyl, heptyl, octyl, nonyl, decyl, vinyl, propenyl, butenyl, pentenyl, methoxy, ethoxy, propoxy, butoxy, pentoxy, diphenylamino, naphthylphenylamino, dinaphthylamino, dianthranylamino, diphenylenylamino, and dipyrenylamino. Preferably, deuterium, cyano, methyl, ethyl, t-butyl, propyl, butyl, pentyl, neopentyl, hexyl, heptyl, or octyldiphenylamino, naphthylphenylamino, or dinaphthylamino are used.
[0068] The compounds represented by general formula (1) and general formulae (2) to (7) may be deuterated to contain deuterium, or may contain no deuterium. In addition, both the compound represented by general formula (1) and the compounds represented by general formulae (2) to (7) may contain deuterium, both may contain no deuterium, or only one of them may contain deuterium. When at least one of the compound represented by general formula (1) and the compounds represented by general formulae (2) to (7) is a deuterium-containing compound, the performance (luminous efficiency and service life) of the organic EL device is improved.
[0069] Here, deuterium may be present such that at least part of the hydrogen in Ra, Rb, Ar 1 to Ar 2 , Ar 4 to Ar 6 , Ar 10 to Ar 12 , X 2 to X 4 , and R 14 to R 15 is replaced with deuterium, so that the hydrogen contained in the groups constituting the compound represented by general formula (1) and the compounds represented by general formulae (2) to (7) may be deuterated.
[0070] In addition, each deuteride of the compound represented by general formula (1) and the compounds represented by general formulae (2) to (7) includes both cases of being composed of a single compound and being composed of a mixture of two or more compounds. That is, to specifically explain the deuteration ratio, a deuteration ratio of 50% means that on average half of all hydrogen atoms are substituted with deuterium, and the deuteride may be a single compound or a mixture having different deuteration ratios. In this specification, the deuteration ratio and the average deuteration ratio represent the same meaning.
[0071] When part of the hydrogen in the compound represented by general formula (1) and the compounds represented by general formulae (2) to (7) is deuterium, preferably 30% or more of all hydrogen atoms in the compound represented by general formula (1) and the compounds represented by general formulae (2) to (7) are deuterium, more preferably 40% or more are deuterium, even more preferably 50% or more are deuterium, and particularly preferably 60% or more are deuterium.
[0072] The deuteration rate can be determined by mass spectrometry or proton nuclear magnetic resonance spectroscopy. For example, when determining the rate by proton nuclear magnetic resonance spectroscopy, first, the compound and an internal standard substance are added to a deuterated solvent and dissolved to prepare a sample. The proton concentration [mol / g] of the compound contained in the sample is then calculated from the ratio of the integrated intensity derived from the internal standard substance and the compound. Next, the ratio of the proton concentration of the deuterated compound to the proton concentration of the corresponding non-deuterated compound is calculated, and the deuteration rate of the deuterated compound can be calculated by subtracting this ratio from 1. Furthermore, the deuteration rate of a substructure can be calculated from the integrated intensity of the chemical shift originating from the substructure in question using the same procedure as described above.
[0073] The organic EL element of the present invention includes at least one organic layer comprising a first host represented by general formula (1) and a second host represented by general formulas (2) to (7). Preferably, these are included in the light-emitting layer. In this case, the first host and the second host may be included in the light-emitting layer, for example, in a mixed material for forming the light-emitting layer. The mixed material containing the first host and the second host may also contain a light-emitting dopant or other host material. To form the light-emitting layer, there are two methods: vaporizing and depositing two types of compounds from separate evaporation sources, and pre-mixing two types of compounds to form a premixture, which is then vaporized and deposited from a single evaporation source. The latter method is also called the premixed deposition method and can provide an organic EL element with excellent performance and lifespan.
[0074] The aforementioned premixture is a form of the mixed material and may be obtained by mixing the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7) in powder form, or by melting them by heating under reduced pressure or in an inert gas atmosphere such as nitrogen to obtain a molten mixture. Furthermore, a mixture of these compounds that has been mixed in advance may be sublimated together. On the other hand, the mixed material may be a mixture in which the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7) are ultimately combined, and may be in powder form or in thin film form. In the case of thin film form, the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7) may be contained in the same organic layer, or they may be contained in different organic layers of the element.
[0075] Here, when the mixed material for the organic electroluminescent element in the present invention is a molten mixture of the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7), preferably the difference between the maximum emission wavelength of the fluorescence emission spectrum of the molten mixture and the maximum emission wavelength of the fluorescence emission spectrum of any of the compounds represented by general formula (1) and general formulas (2) to (7) is ±10 nm or more. More preferably, the difference between the maximum emission wavelength of the fluorescence emission spectrum of the molten mixture and the maximum emission wavelengths of the respective fluorescence emission spectra of the compound represented by general formula (1) and general formulas (2) to (7) is ±10 nm or more. The fluorescence emission spectrum refers to the wavelength of the emission peak showing the maximum emission intensity in the emission spectrum observed in the measurement range of 350 nm to 700 nm when a powder sample is irradiated with 340 nm excitation light using a spectrophotometer. Furthermore, the maximum emission wavelength of the fluorescence emission spectrum may be referred to as the PL maximum emission wavelength below.
[0076] Furthermore, if the mixed material for the organic electroluminescent element in the present invention is the above-described premixture, it is preferable that the melting point of at least one of the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7) is 300°C or lower. Preferably, the melting points of both compounds are 300°C or lower. Moreover, it is preferable that the melting point of at least one of the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7) is below the 50% weight loss temperature of the compound. Preferably, the melting points of both compounds are below the 50% weight loss temperature of the respective compound.
[0077] When forming a light-emitting layer using the above-mentioned premixture as the mixed material for the organic electroluminescent element of the present invention, a necessary luminescent dopant material or other host material may be mixed in as needed. In such cases, if a large difference in the temperature at which the desired vapor pressure is achieved occurs when the compound represented by general formula (1) and the compounds represented by general formulas (2) to (7) are included, it is preferable to deposit the luminescent dopant material or other host material from a separate deposition source.
[0078] Furthermore, regarding the ratio of the first host, which consists of the compound represented by general formula (1), to the second host, which consists of any of the compounds represented by general formulas (2) to (7), it is preferable that the ratio of the second host to the total of the two is 10% by mass or more and less than 80% by mass, and more preferably 20% by mass or more and less than 70% by mass. Also, the ratio of the first host to the second host is the same as above even when the first host and the second host are the mixed material or are included in the premixture. Moreover, it is desirable to maintain a constant evaporation rate of the two types of hosts during deposition, and to achieve this, it is preferable that the difference in evaporation temperatures or the difference in 50% weight loss temperatures between the two be within 20°C.
[0079] Next, the structure of the organic EL element of the present invention will be described with reference to the drawings, but the structure of the organic EL element of the present invention is not limited thereto.
[0080] Figure 1 is a cross-sectional view showing a typical organic EL element structure, where 1 is the substrate, 2 is the anode, 3 is the hole injection layer, 4 is the hole transport layer, 5 is the light-emitting layer, 6 is the electron transport layer, and 7 is the cathode. The organic EL element of the present invention may have an exciton blocking layer adjacent to the light-emitting layer 5, or an electron blocking layer may be present between the light-emitting layer 5 and the hole injection layer 3. The exciton blocking layer can be inserted on either the anode side or the cathode side of the light-emitting layer 5, and it is also possible to insert it on both sides simultaneously.
[0081] The organic EL element of the present invention has an anode 2, a light-emitting layer 5, and a cathode 7 as essential layers. However, it is also preferable to have a hole injection transport layer (hole injection layer, hole transport layer) and an electron injection transport layer (electron transport layer, electron injection layer) in addition to the essential layers, and it is also preferable to have a hole blocking layer between the light-emitting layer 5 and the electron injection transport layer. Note that the hole injection transport layer means either the hole injection layer 3 and the hole transport layer 4, or both, and the electron injection transport layer means either the electron injection layer (not shown) and the electron transport layer 6, or both.
[0082] It is also possible to stack the cathode 7, electron transport layer 6, light-emitting layer 5, hole transport layer 4, hole injection layer 3, and anode 2 on the substrate 1 in the reverse order, and in this case as well, the layers described above can be added or omitted as needed.
[0083] -Substrate- The organic EL element of the present invention is preferably supported on a substrate. There are no particular restrictions on the substrate; any substrate that has been conventionally used in organic EL elements is acceptable, such as those made of glass, transparent plastic, quartz, etc.
[0084] - Anode - As the anode material for organic EL elements, materials consisting of metals, alloys, electrically conductive compounds, or mixtures thereof with a large work function (4 eV or more) are preferably used. Specific examples of such electrode materials include metals such as Au, CuI, indium tincture oxide (ITO), and SnO 2Examples include conductive transparent materials such as ZnO. Alternatively, amorphous materials such as IDIXO (In2O3-ZnO), which can create transparent conductive films, may be used. The anode may be formed by creating a thin film from these electrode materials using methods such as vapor deposition or sputtering, and then forming a pattern of the desired shape using photolithography. Alternatively, if high pattern accuracy is not required (approximately 100 μm or more), the pattern may be formed via a mask of the desired shape during vapor deposition or sputtering of the electrode material. In the case of coatings using organic conductive compounds, wet film formation methods such as printing or coating can also be used. When extracting light from this anode, it is desirable to have a transmittance greater than 10%, and the sheet resistance of the anode is preferably several hundred Ω / □ or less. The film thickness depends on the material, but is usually selected in the range of 10 to 1000 nm, preferably 10 to 200 nm.
[0085] - Cathode - On the other hand, materials consisting of metals (electron-injection metals), alloys, electrically conductive compounds, or mixtures thereof with a small work function (4 eV or less) are used as cathode materials. Specific examples of such electrode materials include sodium, sodium-potassium alloys, magnesium, lithium, magnesium / copper mixtures, magnesium / silver mixtures, magnesium / aluminum mixtures, magnesium / indium mixtures, and aluminum / aluminum oxide (Al 2 O 3Examples include mixtures, indium, lithium / aluminum mixtures, and rare earth metals. Among these, from the viewpoint of electron injection properties and durability against oxidation, mixtures of electron-injection metals and metalloids, which have a larger work function and are more stable, such as magnesium / silver mixtures, magnesium / aluminum mixtures, magnesium / indium mixtures, aluminum / aluminum oxide mixtures, lithium / aluminum mixtures, and aluminum, are preferred. Cathodes can be made by forming thin films of these cathode materials by methods such as vapor deposition or sputtering. Furthermore, the sheet resistance of the cathode is preferably several hundred Ω / □ or less, and the film thickness is usually selected in the range of 10 nm to 5 μm, preferably 50 to 200 nm. In addition, in order to transmit the emitted light, it is advantageous that the luminescence brightness is improved if either the anode or cathode of the organic EL element is transparent or semi-transparent.
[0086] Furthermore, by forming the above-mentioned metal on the cathode with a film thickness of 1 to 20 nm, and then forming the conductive transparent material mentioned in the description of the anode on top of it, a transparent or translucent cathode can be fabricated. By applying this, it is possible to fabricate an element in which both the anode and cathode are transparent.
[0087] -Emitting Layer- The emissive layer is a layer that emits light after excitons are generated by the recombination of holes and electrons injected from the anode and cathode, respectively. The emissive layer preferably contains an organic luminescent dopant material and a host material.
[0088] The host includes the first host and the second host. If necessary, one or more other host materials, such as known host materials, may be used in combination. Preferably, the other host materials are compounds that have hole transport ability, electron transport ability, prevent the emission from becoming longer wavelengths, and have a high glass transition temperature.
[0089] Other host materials are known from numerous patent documents, etc., and can be selected from among them. Specific examples of host materials are not limited to those described in WO2008 / 056746A1 and WO2008 / 146839A1, etc., indolocarbazole derivatives described in WO 2009 / 086028A1 and WO2012 / 077520A1, etc., CBP (N,N-biscarbazollilbiphenyl) derivatives, triazine derivatives described in WO2014 / 185595A1 and WO2018 / 021663A1, etc., indenocarbazole derivatives described in WO2010 / 136109A1 and WO2011 / 000455A1, etc., WO Dibenzofuran derivatives, triazole derivatives, indole derivatives, oxazole derivatives, oxadiazole derivatives, imidazole derivatives, polyarylalkane derivatives, pyrazoline derivatives, pyrazolone derivatives, phenylenediamine derivatives, arylamine derivatives, aminosubstituted chalcone derivatives, styrylanthracene derivatives, fluorenone derivatives, hydrazone derivatives, stilbene derivatives, silazane derivatives, aromatic tertiary amine compounds, styrylamine compounds, aromatic dimethylidene compounds, porphyrin compounds, anthraquinodyne compounds, etc. Examples include polyphenol derivatives, anthrone derivatives, diphenylquinone derivatives, thiopyrandioxide derivatives, heterocyclic tetracarboxylic anhydrides such as naphthaleneperylene, phthalocyanine derivatives, metal complexes of 8-quinolinol derivatives and metal phthalocyanines, various metal complexes represented by metal complexes of benzoxazole and benzothiazole derivatives, polysilane compounds, poly(N-vinylcarbazole) derivatives, aniline copolymers, thiophene oligomers, polythiophene derivatives, polyphenylene derivatives, polyphenylenevinylene derivatives, polyfluorene derivatives, and other polymer compounds.
[0090] Specific examples of other host materials mentioned above are listed below, but are not limited to these.
[0091] When using multiple types of hosts, each host can be deposited from a different deposition source, or multiple types of hosts can be deposited simultaneously from a single deposition source by pre-mixing them into a premixture before deposition.
[0092] For pre-mixing, a method that allows for as uniform a mixture as possible is desirable. Examples include grinding and mixing, heating and melting under reduced pressure or inert gas atmosphere such as nitrogen, and sublimation, but the method is not limited to these.
[0093] The premixture may be in the form of a powder, sticks, or granules.
[0094] Preferred organic luminescent dopant materials include phosphorescent dopants, fluorescent dopants, and thermally activated delayed fluorescence dopants.
[0095] The phosphorescent dopant should contain an organometallic complex comprising at least one metal selected from ruthenium, rhodium, palladium, silver, rhenium, osmium, iridium, platinum, and gold. Specifically, iridium complexes described in J.Am.Chem.Soc.2001,123,4304, JP2013-530515A, US2016 / 0049599A1, US2017 / 0069848A1, US2018 / 0282356A1, or US2019 / 0036043A1, etc., or platinum complexes described in US2018 / 0013078A1, or KR2018 / 094482A, etc., are preferably used, but are not limited to these.
[0096] The phosphorescent dopant material may be contained in the light-emitting layer by one type or by two or more types. The content of the phosphorescent dopant material is preferably 0.1 to 30% by mass, and more preferably 1 to 20% by mass, relative to the host material.
[0097] Phosphorescent dopant materials are not particularly limited, but specific examples include the following:
[0098] While not particularly limited, examples of fluorescent dopants include benzoxazole derivatives, benzothiazole derivatives, benzimidazole derivatives, styrylbenzene derivatives, polyphenyl derivatives, diphenylbutadiene derivatives, tetraphenylbutadiene derivatives, naphthalimide derivatives, coumarin derivatives, condensed aromatic compounds, perinone derivatives, oxadiazole derivatives, oxazine derivatives, aldazine derivatives, pyrrolidine derivatives, cyclopentadiene derivatives, bisstyrylanthracene derivatives, quinacridone derivatives, pyrrolopyridine derivatives, thiadiazolopyridine derivatives, styrylamine derivatives, diketopyrrolopyrrole derivatives, aromatic dimethylidine compounds, metal complexes of 8-quinolinol derivatives and pyromethene derivatives, various metal complexes represented by rare earth complexes and transition metal complexes, polymer compounds such as polythiophene, polyphenylene, and polyphenylenevinylene, and organosilane derivatives. Preferably, these include condensed aromatic derivatives, styryl derivatives, diketopyrrolopyrrole derivatives, oxazine derivatives, pyromethene metal complexes, transition metal complexes, or lanthanide complexes. More preferably, these include naphthalene, pyrene, chrysene, triphenylene, benzo[c]phenanthrene, benzo[a]anthracene, pentacene, perylene, fluorantene, acenaphthofluorantene, dibenzo[a,j]anthracene, dibenzo[a,h]anthracene, benzo[a]naphthalene, hexacene, naphtho[2,1-f]isoquinoline, α-naphthaphenanthidine, phenanthroxazole, quinolino[6,5-f]quinoline, benzothiophanthrene, and the like. These may have alkyl groups, aryl groups, aromatic heterocyclic groups, or diarylamino groups as substituents.
[0099] The fluorescent dopant material may be contained in the light-emitting layer by one type or by two or more types. The content of the fluorescent dopant material is preferably 0.1 to 20% by mass, and more preferably 1 to 10% by mass, relative to the host material.
[0100] Examples of thermally activated delayed fluorescence dopants are not particularly limited, but include metal complexes such as tin complexes and copper complexes, indolocarbazole derivatives described in WO2011 / 070963A1, cyanobenzene derivatives and carbazole derivatives described in Nature 2012, 492, 234, phenazine derivatives, oxadiazole derivatives, triazole derivatives, sulfone derivatives, phenoxazine derivatives, and acridine derivatives described in Nature Photonics 2014, 8, 326.
[0101] Thermally activated delayed fluorescence dopant materials are not particularly limited, but specific examples include the following:
[0102] The thermally activated delayed fluorescence dopant material may be contained in the light-emitting layer as a single type or as two or more types. Furthermore, the thermally activated delayed fluorescence dopant may be used in mixture with phosphorescent dopants or fluorescent dopants. The content of the thermally activated delayed fluorescence dopant material is preferably 0.1 to 50 wt%, and more preferably 1 to 30 wt%, relative to the host material.
[0103] -Injection Layer- An injection layer is a layer provided between the electrode and the organic layer to reduce the driving voltage and improve the luminescence brightness. There are hole injection layers and electron injection layers, and they may be present between the anode and the light-emitting layer or hole transport layer, and between the cathode and the light-emitting layer or electron transport layer. The injection layer can be provided as needed.
[0104] -Hole Blocking Layer- In a broad sense, the hole blocking layer functions as an electron transport layer. It consists of a hole blocking material that has the ability to transport electrons while having a significantly low ability to transport holes. By blocking holes while transporting electrons, it is possible to improve the probability of electron-hole recombination in the light-emitting layer.
[0105] -Electron Stopping Layer- In a broad sense, the electron stopping layer functions as a hole transport layer, and by transporting holes while blocking electrons, it can improve the probability of electrons and holes recombining in the light-emitting layer.
[0106] As the material for the electron blocking layer, known electron blocking layer materials can be used, and the material for the hole transport layer described later can be used as needed. The thickness of the electron blocking layer is preferably 3 to 100 nm, and more preferably 5 to 30 nm.
[0107] -Exciton Blocking Layer- An exciton blocking layer is a layer designed to prevent excitons, generated by the recombination of holes and electrons within the light-emitting layer, from diffusing into the charge transport layer. By inserting this layer, it becomes possible to efficiently confine excitons within the light-emitting layer, thereby improving the light-emitting efficiency of the device. In devices where two or more light-emitting layers are adjacent to each other, the exciton blocking layer can be inserted between two adjacent light-emitting layers.
[0108] As the material for the exciton blocking layer, known exciton blocking layer materials can be used. For example, 1,3-dicarbazolylbenzene (mCP) and bis(2-methyl-8-quinolinolate)-4-phenylphenolatealuminum(III) (BAlq) can be used.
[0109] - Hole Transport Layer - The hole transport layer consists of a hole transport material that has the function of transporting holes, and the hole transport layer can be a single layer or multiple layers.
[0110] The hole transport material has either hole injection or transport properties, or electron barrier properties, and may be either organic or inorganic. Any compound from conventionally known compounds can be selected and used for the hole transport layer. Examples of such hole transport materials include porphyrin derivatives, arylamine derivatives, triazole derivatives, oxadiazole derivatives, imidazole derivatives, polyarylalkane derivatives, pyrazoline derivatives and pyrazolone derivatives, phenylenediamine derivatives, arylamine derivatives, aminosubstituted chalcone derivatives, oxazole derivatives, styrylanthracene derivatives, fluorenone derivatives, hydrazone derivatives, stilbene derivatives, silazane derivatives, aniline copolymers, and conductive polymer oligomers, particularly thiophene oligomers. However, it is preferable to use porphyrin derivatives, arylamine derivatives and styrylamine derivatives, and more preferably arylamine derivatives.
[0111] - Electron Transport Layer - The electron transport layer consists of a material that has the function of transporting electrons, and the electron transport layer can be a single layer or multiple layers.
[0112] The electron transport material (which may also serve as a hole-blocking material) only needs to have the function of transferring electrons injected from the cathode to the light-emitting layer. Any compound from conventionally known compounds can be selected and used for the electron transport layer. Examples include polycyclic aromatic derivatives such as naphthalene, anthracene, and phenanthroline; tris(8-quinolinolate)aluminum(III) derivatives; phosphine oxide derivatives; nitro-substituted fluorene derivatives; diphenylquinone derivatives; thiopyrandioxide derivatives; carbodiimide; fluorenylidene methane derivatives; anthraquinodimethane derivatives and anthrone derivatives; bipyridine derivatives; quinoline derivatives; oxadiazole derivatives; benzimidazole derivatives; benzothiazole derivatives; indolocarbazole derivatives; and polymer materials that incorporate these materials into a polymer chain or use these materials as the main chain of the polymer.
[0113] In the method for manufacturing an organic electroluminescent element of the present invention, it is preferable to have a step of mixing a compound represented by general formula (1) (first host) and compounds represented by general formulas (2) to (7) (second host) to form a premixture, and then evaporating the obtained premixture from a single deposition source to deposit and form an emissive layer. By premixing the two host materials in this way, the performance of the organic EL element can be improved. Powder mixing or melt mixing can be used as the mixing method.
[0114] The premixture obtained by the above premixing preferably has a 50% weight loss temperature difference of 20°C or less between the first host material and the second host material. Here, the 50% weight loss temperature refers to the temperature at which the weight decreases by 50% when the temperature is raised from room temperature to 550°C at a rate of 10°C per minute in a TG-DTA measurement under reduced pressure of nitrogen gas flow (1 Pa). Around this temperature, vaporization by evaporation or sublimation is considered to occur most actively.
[0115] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples and can be implemented in various forms as long as it does not exceed the gist of the invention.
[0116] Representative examples of the synthesis of compounds 1-3, 1-66, 3-1, 3-7, 3-66, and 3-70 are shown. Other compounds were synthesized using similar methods. The deuteration rate was determined by proton nuclear magnetic resonance spectroscopy.
[0117] Synthesis Example 1: Compounds (1-3) were synthesized according to the following reaction. To 2.0 g (5.8 mmol) of compound (a), 0.91 g (5.8 mmol) of compound (b), 0.11 g of copper iodide, 0.15 g of 8-quinolinol, 0.90 g of potassium carbonate, and 50 g of 1,3-dimethyl-2-imidazolidinone were added, and the mixture was stirred at 190°C for 24 hours under a nitrogen atmosphere. After cooling to room temperature, the mixture was purified by silica gel column chromatography to obtain 1.1 g (2.6 mmol, 44% yield) of compound (c) as a white solid.
[0118] To 3.0 g (7.1 mmol) of compound (c) obtained above, 3.3 g (14.2 mmol) of compound (d), 0.14 g of copper iodide, 0.25 g of 8-quinolinol, 1.0 g of potassium carbonate, and 20 g of 1,3-dimethyl-2-imidazolidinone were added, and the mixture was stirred at 190°C for 48 hours under a nitrogen atmosphere. After cooling to room temperature, the mixture was purified by silica gel column chromatography and crystallization to obtain 3.3 g (5.8 mmol, yield 81%) of compound (1-3) as a white solid.
[0119] Synthesis Example 2 Compounds 1-66 were synthesized according to the following reaction. To 2.0 g (5.77 mmol) of compound (a), 0.84 g (5.20 mmol) of compound (e), 0.11 g of copper iodide, 0.18 g of 8-quinolinol, 0.81 g of potassium carbonate, and 100 g of 1,3-dimethyl-2-imidazolidinone were added, and the mixture was stirred at 190°C for 24 hours under a nitrogen atmosphere. After cooling to room temperature, the mixture was purified by silica gel column chromatography to obtain 0.84 g (1.96 mmol, yield 34%) of compound (f) as a white solid.
[0120] Next, 0.98 g (2.26 mmol) of compound (f) obtained above was mixed with 50 ml of deuterated benzene (C6D6) and 3 g of trifluoromethanesulfonic acid (TfOH), and heated and stirred at 50°C for 5 hours under a nitrogen atmosphere. The reaction mixture was added to 25 ml of a heavy aqueous solution of sodium carbonate (2.0 g), rapidly cooled, separated, and purified to obtain 0.6 g (1.36 mmol) of the deuterated compound (g). Note that the number of s substitutions in the substituted deuterium (D) represents the average number.
[0121] To 3.1 g (7.1 mmol) of compound (g) obtained above, 3.1 g (12.9 mmol) of compound (h), 0.13 g of copper iodide, 0.21 g of 8-quinolinol, 0.98 g of potassium carbonate, and 20 g of 1,3-dimethyl-2-imidazolidinone were added, and the mixture was stirred at 190°C for 48 hours under a nitrogen atmosphere. After cooling to room temperature, the mixture was purified by silica gel column chromatography and crystallization to obtain 2.3 g (3.9 mmol, yield 55%) of compound (1-66) as a white solid. Note that the number of substitutions of s in the substituted deuterium (D) represents the average number.
[0122] Here, the average deuterated rate of compound (1-66) obtained above was determined by proton nuclear magnetic resonance spectroscopy. A sample was prepared by dissolving 5.0 mg of compound (1-66) and 2.0 mg of dimethyl sulfone as an internal standard in 1.0 ml of deuterated tetrahydrofuran. The average proton concentration (mol / g) of compound (1-66) contained in the sample was calculated from the integrated intensity ratio derived from the internal standard and compound (1-66). Similarly, the average proton concentration (mol / g) of the non-deuterated compound (1-66) (compound (1-3)) was also calculated. Next, the ratio of the proton concentration of compound (1-66) to the proton concentration of compound (1-3) was calculated and subtracted from 1 to obtain an average deuterated rate of 88% for compound (1-66).
[0123] Synthesis Example 3 Compound 3-1 was synthesized according to the following reaction. To 2.0 g (4.2 mmol) of compound (i), 1.8 g (5.0 mmol) of compound (j), 12.0 mg of CX21 [allylchloro[1,3-bis(2,6-diisopropylphenyl)imidazole-2-ylidene]palladium(II), CAS number: 478980-03-9], 1.7 g of potassium carbonate, 200 g of m-xylene, and 50 g of water were added, and the mixture was stirred at 110°C for 2 days under a nitrogen atmosphere. After cooling to room temperature, 100 ml of water was added, and the organic phase was extracted using m-xylene. The organic phase was then converted to MgSO4. 4 By drying and concentrated drying using [method / method], 2.6 g of a pale yellow solid was obtained. The obtained solid was purified by silica gel column chromatography and crystallization to obtain 1.5 g of compound (3-1) as a yellow solid (yield 55%). (APCI-TOFMS, m / z 641[M+H]) + ).
[0124] Synthesis Example 4 Compounds 3-7 were synthesized according to the following reaction. To 2.0 g (4.2 mmol) of compound (i) were added 1.8 g (5.0 mmol) of compound (k), 12.0 mg of CX21, 1.7 g of potassium carbonate, 300 g of m-xylene, and 50 g of water, followed by stirring at 110°C for 2 days under a nitrogen atmosphere. After cooling to room temperature, 100 ml of water was added, the organic phase was extracted with m-xylene, and the organic phase was treated with MgSO 4 , dried, and concentrated to dryness to obtain 2.5 g of a pale yellow solid. The obtained solid was purified by silica gel column chromatography and further purified by crystallization, to obtain 1.6 g (yield 60%) of compound (3-7) as a pale yellow solid. (APCI-TOFMS, m / z 626[M+H] + ).
[0125] Synthesis Example 5 Compound 3-66 was synthesized according to the following reaction. To 2.1 g (4.2 mmol) of compound (L) were added 1.9 g (5.0 mmol) of compound (M), 12.0 mg of CX21, 1.7 g of potassium carbonate, 100 g of m-xylene, and 50 g of water, followed by stirring at 110°C for 2 days under a nitrogen atmosphere. After cooling to room temperature, 100 ml of water was added, the organic phase was extracted with m-xylene, and the organic phase was treated with MgSO 4 , dried, and concentrated to dryness to obtain 2.7 g of a pale yellow solid. The obtained solid was purified by silica gel column chromatography and further purified by crystallization, to obtain 1.1 g (yield 40%) of compound (3-66) as a yellow solid. (APCI-TOFMS, m / z 670[M+H] + ). The number of substitutions s of the substituted deuterium (D) means an average value.
[0126] Here, the average deuterated rate of compound (3-66) obtained above was determined by proton nuclear magnetic resonance spectroscopy. A sample was prepared by dissolving 5.0 mg of compound (3-66) and 2.0 mg of dimethyl sulfone as an internal standard in 1.0 ml of deuterated tetrahydrofuran. The average proton concentration (mol / g) of compound (3-66) contained in the sample was calculated from the integrated intensity ratio derived from the internal standard and compound (3-66). Similarly, the average proton concentration (mol / g) of the non-deuterated compound (compound (3-1)) was also calculated. Next, the ratio of the proton concentration of compound (3-66) to the proton concentration of compound (3-1) was calculated and subtracted from 1 to obtain an average deuterated rate of 89% for compound (3-66).
[0127] Synthesis Example 6 Compound 3-70 was synthesized according to the following reaction. To 2.1 g (4.2 mmol) of compound (L), 1.8 g (5.0 mmol) of compound (N), 12.0 mg of CX21, 1.7 g of potassium carbonate, 200 g of m-xylene, and 50 g of water were added, and the mixture was stirred at 110°C under a nitrogen atmosphere for 2 days. After cooling to room temperature, 100 ml of water was added, and the organic phase was extracted using m-xylene. The organic phase was then converted to MgSO4. 4 By drying and concentrated drying using [method / method], 2.6 g of a pale yellow solid was obtained. The obtained solid was purified by silica gel column chromatography and crystallization to obtain 1.2 g of compound (3-70) as a yellow solid (yield 45%). (APCI-TOFMS, m / z 654[M+H]) + ). Note that the number of substitutions of s in the substituted deuterium (D) represents the average number.
[0128] Here, the average deuterated rate of compound (3-70) obtained above was determined by proton nuclear magnetic resonance spectroscopy. A sample was prepared by dissolving 5.0 mg of compound (3-70) and 2.0 mg of dimethyl sulfone as an internal standard in 1.0 ml of deuterated tetrahydrofuran. The average proton concentration (mol / g) of compound (3-70) contained in the sample was calculated from the integrated intensity ratio derived from the internal standard and compound (3-70). Similarly, the average proton concentration (mol / g) of the non-deuterated compound (3-70) (compound (3-7)) was also calculated. Next, the ratio of the proton concentration of compound (3-70) to the proton concentration of compound (3-7) was calculated and subtracted from 1 to obtain an average deuterated rate of 89% for compound (3-70).
[0129] The compounds used in the examples and comparative examples are shown below.
[0130] The reaction was carried out in the same manner as in Synthesis Examples 1, 3-4, to synthesize Example compounds 1-3, 1-5, 1-6, 1-9, 3-104, and Comparative Examples Host A, Host B, Host C, Host D, and Host E. The reaction was also carried out in the same manner as in Synthesis Examples 2, 5-6, to synthesize the deuterated Example compounds 1-64, 1-65, 1-64, 1-65b, 1-66, 1-67, 1-68, 1-69, 1-70, 1-71, 1-72, 1-76, 1-77, 1-78, 1-79, 1-80, 1-81, 1-82, 1-83, 1-95, 1-96, 1-97, 1-98, 1-99, 1-100, 1-101, 1-102, 1-103, 1-104, and 3-112.
[0131] The deuteration rate of the synthesized deuteride was calculated in the same manner as in synthesis examples 2, 5-6. The results are shown in Table 1.
[0132] Example 1 A glass substrate on which an anode made of ITO with a thickness of 110 nm was formed was used to deposit each thin film by vacuum deposition at a vacuum of 4.0 × 10⁻⁶. -5The layers were stacked using Pa. First, compound A and compound B were co-deposited onto ITO from different deposition sources to form a hole injection layer to a thickness of 10 nm. At this time, the co-deposit was performed under deposition conditions where the concentration of compound B was 3 mass%. Next, compound A was formed to a thickness of 110 nm as the first hole transport layer. Next, compound C was formed to a thickness of 10 nm as the second hole transport layer. Next, compound D was formed to a thickness of 5 nm as the electron blocking layer. Next, compounds 1-3 were co-deposited as the first host, compound 3-1 as the second host, and compound E as the luminescent dopant from different deposition sources to form a luminescent layer to a thickness of 40 nm. At this time, the co-deposit was performed under deposition conditions where the concentration of compound E was 5 mass% and the mass ratio of the first host to the second host was 60:40. Next, compound F was formed to a thickness of 5 nm as the hole blocking layer. Next, compound G was formed to a thickness of 30 nm as the electron transport layer. Furthermore, a 1 nm thick layer of LiF was formed on the electron transport layer as an electron injection layer. Finally, an 70 nm thick layer of Al was formed on the electron injection layer as a cathode to fabricate an organic EL device.
[0133] Examples 2-45, Comparative Examples 1-10 Organic EL elements were fabricated in the same manner as in Example 1, except that the compounds shown in Tables 2 and 3 were used as the first and second hosts, respectively, and that they were in a predetermined mass ratio.
[0134]
[0135]
[0136] Examples 46-47, Comparative Examples 11-13 Organic EL elements were fabricated in the same manner as in Example 1, except that the compounds shown in Table 3 were used as the first and second hosts, and the preliminary mixture obtained by grinding and mixing them in a mortar was co-deposited from a single evaporation source.
[0137] Example 48 As shown in Table 3, compounds 1-66 and 3-70 were used as the first and second hosts, and a preliminary mixture H1 was obtained by grinding and mixing them in a mortar. The preliminary mixture was placed in a vacuum chamber, heated to 300°C under reduced pressure of 100 Pa or less, cooled to room temperature, and then pulverized and mixed to obtain a molten mixture M1. An organic EL element was fabricated in the same manner as in Example 1, except that this molten mixture was co-deposited from a single evaporation source.
[0138] Comparative Example 14 As shown in Table 3, Host C and Host B were used as the first and second hosts, and a preliminary mixture H2 was obtained by grinding and mixing them in a mortar. The preliminary mixture was placed in a vacuum chamber, heated to 300°C under reduced pressure of 100 Pa or less, cooled to room temperature, and then pulverized and mixed to obtain a molten mixture M2. An organic EL element was fabricated in the same manner as in Example 1, except that this molten mixture was co-deposited from a single evaporation source.
[0139] Comparative Example 15 As shown in Table 3, Host E and compound 3-7 were used as the first and second hosts, and a preliminary mixture H3 was obtained by grinding and mixing them in a mortar. The preliminary mixture was placed in a vacuum chamber, heated to 300°C under reduced pressure of 100 Pa or less, cooled to room temperature, and then pulverized and mixed to obtain a molten mixture M3. An organic EL element was fabricated in the same manner as in Example 1, except that this molten mixture was co-deposited from a single evaporation source.
[0140] Comparative Example 16 As shown in Table 3, Host E and compound 3-70 were used as the first and second hosts, and a preliminary mixture H4 was obtained by grinding and mixing them in a mortar. The preliminary mixture was placed in a vacuum chamber, heated to 300°C under reduced pressure of 100 Pa or less, cooled to room temperature, and then pulverized and mixed to obtain a molten mixture M4. An organic EL element was fabricated in the same manner as in Example 1, except that this molten mixture was co-deposited from a single evaporation source.
[0141] The photoluminescence (PL: fluorescence emission) spectra of the powders of the molten mixtures M1 to M3, and compounds 1-66, 3-70, Host B, Host C, and Host E prepared in the above examples and comparative examples were measured. A spectrofluorometer (FP-6500, JASCO) was used to measure the PL spectra. The powder samples were sandwiched between two quartz substrates, and irradiated with 340 nm excitation light in the powder state. The PL spectra observed in the measurement range of 350 nm to 700 nm were measured.
[0142] The PL spectra obtained in the above measurements are shown in Figures 2 to 4. The wavelengths at the maximum peaks of each spectrum were defined as the maximum PL emission wavelengths and are summarized in Table 4.
[0143]
[0144] The evaluation results of the fabricated organic EL elements are shown in Table 3. In the table, voltage and current efficiency are given for a driving current of 10 mA / cm. 2 These are values for time and represent initial characteristics. LT70 is the time it takes for the brightness to decrease from an initial brightness of 9000 nits to 70%, and represents the lifetime characteristic. The numbers for the first host and second host are the numbers assigned to the example compounds above, and the mass ratio is first host:second host. Note that all characteristics are expressed as relative values with the characteristics of Comparative Example 3 set to 100%.
[0145] These results show that the organic EL elements according to Examples 1-13 and 16-44, in which the first host compound and the second host compound were mixed in a predetermined mixing ratio, exhibited longer lifespan characteristics compared to Comparative Examples 1-3 and 5-7, and in addition, showed good voltage and efficiency characteristics. Similarly, the organic EL elements according to Examples 14-15 and 45 exhibited longer lifespan characteristics compared to Comparative Examples 4 and 8, the organic EL elements according to Examples 46-47 exhibited longer lifespan characteristics compared to Comparative Examples 9-11, and the organic EL element according to Example 48 exhibited longer lifespan characteristics compared to Comparative Examples 12-14, and all examples showed good voltage and efficiency characteristics, all of which were advantageous for practical use.
[0146] Table 5 shows the 50% weight loss temperature (T50) of the compounds used in the examples and comparative examples.
[0147]
[0148] According to the present invention, by using a predetermined mixed material for organic electroluminescent devices, it is possible to realize a practically useful organic EL element that is low voltage, highly efficient, and has a long lifespan.
[0149] 1. Substrate, 2. Anode, 3. Hole injection layer, 4. Hole transport layer, 5. Light-emitting layer, 6. Electron transport layer, 7. Cathode
Claims
1. A mixed material for organic electroluminescent elements, comprising a compound represented by the following general formula (1) and a compound represented by the following general formula (2). (Here, in general formula (1), X 1 is a group represented by O, S, or N-Rb. Y 1 to Y 12 are each independently a group represented by N or C-Ra. Ar 1 and Ar 2 are each independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 5 aromatic rings of these aromatic groups are linked. Ra is independently hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, an alkyl group having 1 to 30 carbon atoms, a fluoroalkyl group having 1 to 30 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, an aralkyl group having 7 to 30 carbon atoms, a phosphoryl group, a silyl group, a germanium group, a cyano group, a nitro group, or a carboxy group. When two or more Ra are present in general formula (1), the plurality of Ra may be the same as or different from each other. Rb is hydrogen, deuterium, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 30 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 5 aromatic rings of these aromatic groups are linked. Further, in the general formula (2), Ar 4 , Ar 5 , and Ar 6 are each independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 7 of these aromatic rings are linked. X 2 to X 4 are each independently N, C-H, or C-D, and at least one is N.) 2. The mixed material for an organic electroluminescent element according to claim 1, characterized in that the general formula (2) is represented by the following formula (3). (In the above general formula (3), Ar 10 Ar 11 , and Ar 12 Each of these is independently a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms, or a substituted or unsubstituted linked aromatic group in which 2 to 3 of these aromatic rings are linked together. 14 ~R 15 Each of these is independently hydrogen, deuterium, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 18 carbon atoms, or a substituted or unsubstituted aromatic heterocyclic group having 3 to 17 carbon atoms. Y is selected from either O or S, and m and n are the number of substitutions, integers from 1 to 3. X 2 ~X 4 This is equivalent to the above general formula (2).
3. The mixed material for organic electroluminescent elements according to claim 2, characterized in that the general formula (3) is represented by any of the following formulas (4) to (7). (Here, Ar 10 Ar 11 Ar 12 , R 14 , R 15 m and n are equivalent to those in the general formula (3) above.
4. The mixed material for an organic electroluminescent element according to claim 3, characterized in that the general formula (3) is represented by the general formula (7).
5. Ar in the general formula (3) 10 The mixed material for organic electroluminescent devices according to claim 2, characterized in that it is a substituted or unsubstituted benzene, pyridine, pyrimidine, triazine, carbazole, dibenzofuran, triphenylene, or a substituted or unsubstituted linked aromatic group in which two to three of these are linked together.
6. The mixed material for an organic electroluminescent element according to claim 1, wherein at least one of the compounds represented by general formula (1) and the compound represented by general formula (2) has some or all of its hydrogen replaced by deuterium, and the average deuteration rate is 30% or more.
7. The mixed material for an organic electroluminescent element according to claim 1, wherein both the compound represented by general formula (1) and the compound represented by general formula (2) have some or all of their hydrogen replaced by deuterium, and the average deuteration rate of both is 30% or more.
8. The mixed material for organic electroluminescent devices according to claim 1, which is used to form at least one layer of an organic electroluminescent device having a plurality of organic layers between an anode and a cathode, and is a premixture in which a compound represented by general formula (1) and a compound represented by general formula (2) are premixed in order to form the organic layer.
9. The mixed material for an organic electroluminescent element according to claim 8, characterized in that the difference in the 50% weight loss temperature between the compound represented by general formula (1) and the compound represented by general formula (2) is 30°C or less.
10. The mixed material for an organic electroluminescent element according to claim 1, characterized in that it is a molten mixture obtained by melting the compound represented by general formula (1) and the compound represented by general formula (2) by heating under reduced pressure or in an inert gas atmosphere.
11. The mixed material for an organic electroluminescent element according to claim 10, characterized in that the difference between the maximum emission wavelength of the fluorescence emission spectrum of the molten mixture and the maximum emission wavelength of the fluorescence emission spectrum of either the compound represented by general formula (1) or the compound represented by general formula (2) is ±10 nm or more.
12. An organic electroluminescent element having a plurality of organic layers between an anode and a cathode, characterized in that at least one of the organic layers contains the mixed material for organic electroluminescent elements described in any one of claims 1 to 11.
13. The organic electroluminescent element according to claim 12, wherein the organic layer containing the mixed material for the organic electroluminescent element is at least one layer selected from the group consisting of an emissive layer, a hole injection layer, a hole transport layer, an electron transport layer, an electron injection layer, a hole blocking layer, and an electron blocking layer.
14. The organic electroluminescent element according to claim 13, wherein the organic layer containing the mixed material for the organic electroluminescent element is an emissive layer, and comprises a compound represented by general formula (1) as a first host, a compound represented by general formula (2) as a second host, and the emissive layer contains at least one luminescent dopant.
15. A method for manufacturing an organic electroluminescent element having a plurality of organic layers including a light-emitting layer between an anode and a cathode, characterized by comprising the steps of preparing a mixed material for organic electroluminescent elements according to any one of claims 1 to 11, and depositing the mixed material for organic electroluminescent elements from a single evaporation source to form a light-emitting layer.