Capacitor, electric circuit, circuit board, and apparatus
The capacitor design optimizes the tantalum oxide film's fluorine content distribution to balance dielectric loss tangent and breakdown voltage, improving capacitor performance by reducing loss tangent while maintaining voltage.
Patent Information
- Application Number
- PCT/JP2026/015644
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-04-17
- Publication Date
- 2026-11-19
AI Technical Summary
Existing capacitors face a trade-off between dielectric loss tangent and breakdown voltage, with fluorine-containing tantalum oxide films exhibiting high loss tangent and high breakdown voltage, limiting their performance improvement.
A capacitor design with a tantalum oxide film having a first portion with high fluorine content and a second portion with lower fluorine content, where the thickness of the second portion is greater inside the porous body than outside, optimizing the dielectric loss tangent and breakdown voltage through a specific thickness ratio.
The design achieves a lower dielectric loss tangent while maintaining a predetermined breakdown voltage, enhancing overall capacitor performance.
Smart Images

Figure JP2026015644_19112026_PF_FP_ABST
Abstract
Description
Capacitors, electrical circuits, circuit boards, and equipment
[0001] This disclosure relates to capacitors, electrical circuits, circuit boards, and equipment.
[0002] Conventionally, fluorine-containing tantalum oxide has been known to be used in capacitors.
[0003] For example, Non-Patent Document 1 states that the relative permittivity of a polycrystalline TaO2F thin film at 1 MHz is 60.
[0004] Patent Document 1 describes a capacitor comprising a dielectric containing an amorphous tantalum compound containing fluorine and oxygen.
[0005] Patent Document 2 describes a capacitor comprising metallic tantalum, a conductor, and a tantalum oxide film. The tantalum oxide film is positioned in contact with the metallic tantalum and between the metallic tantalum and the conductor. The tantalum oxide film includes a first region containing fluorine and a second region located closer to the metallic tantalum than the first region in the thickness direction of the tantalum oxide film. The concentration of fluorine in the second region is lower than the concentration of fluorine in the first region. The tantalum oxide film is formed, for example, by anodic deposition using a fluorine-containing aqueous solution.
[0006] International Publication No. 2022 / 224561, International Publication No. 2023 / 234343
[0007] Journal of Materials Chemistry C, (English), 2020, Issue 14, p.4680-4684
[0008] This disclosure provides a capacitor that is advantageous in that it reduces the dielectric loss tangent while ensuring a predetermined withstand voltage, while incorporating a fluorine-containing tantalum oxide film.
[0009] The capacitor of the present disclosure comprises a porous body including a metallic tantalum-containing portion and a tantalum oxide film, and a conductor, wherein the tantalum oxide film is in contact with the metallic tantalum-containing portion and is disposed between the metallic tantalum-containing portion and the conductor, the tantalum oxide film includes a first portion containing fluorine and a second portion disposed closer to the metallic tantalum-containing portion than the first portion in the thickness direction of the tantalum oxide film, the fluorine content in the second portion is less than the fluorine content in the first portion, and the thickness of the second portion on the inside of the porous body is greater than the thickness of the second portion on the outside of the porous body.
[0010] According to this disclosure, it is possible to provide a capacitor that is advantageous in terms of reducing the dielectric loss tangent while ensuring a predetermined withstand voltage, while incorporating a fluorine-containing tantalum oxide film.
[0011] Figure 1A is a schematic cross-sectional view showing an example of a capacitor of the present disclosure. Figure 1B is a cross-sectional view of the capacitor in the inner part of the porous body enclosed by the dashed line B in Figure 1A. Figure 1C is a cross-sectional view of the capacitor in the outer part of the porous body enclosed by the dashed line C in Figure 1A. Figure 2A is a perspective view schematically illustrating the locations for measuring the thickness of the second portion in the inner and outer parts of the porous body. Figure 2B is a cross-sectional view of the porous body along the cross-section X of Figure 2A. Figure 3A is a perspective view schematically illustrating the locations for measuring the thickness of the second portion in the inner and outer parts of the porous body. Figure 3B is a cross-sectional view of the porous body along the cross-section X of Figure 3A. Figure 4A is a perspective view schematically illustrating the locations for measuring the thickness of the second portion in the inner and outer parts of the porous body. Figure 4B is a cross-sectional view of the porous body along the cross-section X of Figure 4A. Figure 5 is a schematic cross-sectional view showing another example of a capacitor of the present disclosure. Figure 6A is a diagram schematically showing an example of an electrical circuit of the present disclosure. Figure 6B is a schematic diagram showing an example of a circuit board of the present disclosure. Figure 6C is a schematic diagram showing an example of a device of the present disclosure. Figure 7A is a graph showing the relationship between the dielectric loss tangent tanδ of the samples related to Reference Examples 2A to 2D and the ratio of the thickness of the first part to the thickness of the tantalum oxide film. Figure 7B is a graph showing the relationship between the dielectric strength of the samples related to Reference Examples 2A to 2D and the ratio of the thickness of the first part to the thickness of the tantalum oxide film. Figure 8 is a graph showing the results of X-ray diffraction (XRD) measurements of the sample and metallic tantalum related to Example 1. Figure 9 is a graph showing the relationship between the ratio of the number of fluorine atoms to the total number of oxygen atoms and fluorine atoms in the tantalum oxide film in the inner and outer parts of the porous body of the samples related to Example 1 and Comparative Example 1, and the distance from the metallic tantalum-containing part.
[0012] (Knowledge forming the basis of this disclosure) For example, there is a continuous demand to improve the processing performance of electronic devices. The performance of electronic components such as capacitors has a significant impact on the performance of electronic devices into which those electronic components are incorporated. For this reason, an increasing need for small capacitors that can deliver high performance is anticipated. Electrolytic capacitors are known as capacitors, for example. In electrolytic capacitors, a dielectric film consisting of a thin oxide film is formed on the surface of metallic aluminum or metallic tantalum by a chemical conversion treatment of aluminum or tantalum. In electrolytic capacitors, attempts have been made to increase the capacitance of the capacitor mainly by increasing the specific surface area of the dielectric. For example, in tantalum electrolytic capacitors, a dielectric film is formed on a porous tantalum body obtained by sintering fine metallic tantalum powder. On the other hand, there are limitations to such attempts, and it is thought that the performance of capacitors can be further improved if dielectric materials with higher dielectric constants and higher withstand voltages can be developed.
[0013] According to Patent Document 1, dielectric materials containing fluorine-containing amorphous tantalum oxide exhibit a higher relative permittivity than dielectric materials containing fluorine-free tantalum oxide. Thus, it is expected that using fluorine-containing tantalum oxide in a capacitor will increase the capacitance of the capacitor.
[0014] According to Patent Document 2, the dielectric layer, which is a tantalum oxide film, is obtained by anodizing metallic tantalum in an aqueous solution containing fluoride ions. Patent Document 2 also shows that there are conditions under which the dielectric loss tangent of the anodized film is high. Furthermore, according to Patent Document 2, it is understood that by performing additional anodizing in a fluorine-containing aqueous solution after anodizing tantalum in a fluorine-free aqueous solution, the dielectric loss tangent of the dielectric of fluorine-containing amorphous tantalum oxide is lowered.
[0015] On the other hand, increasing the dielectric strength of the dielectric material is also important to improve capacitor performance. For example, a higher dielectric strength allows for a higher operating voltage of the capacitor. Alternatively, it is possible to create a capacitor that maintains the same operating voltage as conventional capacitors even with a thinner dielectric material. In this case, reducing the dielectric thickness can also increase the capacitance of the capacitor.
[0016] According to the inventors' previous studies, it has become clear that the greater the ratio of the thickness of the fluorine-rich portion of the tantalum oxide to the total thickness of the tantalum oxide, the higher the dielectric loss tangent of the tantalum oxide and the higher the breakdown voltage. On the other hand, it has also become clear that the smaller the ratio of the thickness of the fluorine-rich portion of the tantalum oxide to the total thickness of the tantalum oxide, the lower the dielectric loss tangent and the lower the breakdown voltage. In other words, it has been found that there is a trade-off relationship between the reduction of the dielectric loss tangent and the increase in breakdown voltage with respect to the magnitude of the ratio of the thickness of the fluorine-rich portion of the tantalum oxide to the total thickness of the tantalum oxide.
[0017] In light of these circumstances, the inventors diligently investigated whether it was possible to reduce the dielectric loss tangent while ensuring a predetermined dielectric strength, while incorporating a fluorine-containing tantalum oxide film. As a result, it was newly discovered that the dielectric loss tangent can be reduced while ensuring a predetermined dielectric strength by having a predetermined relationship between the thickness of the fluorine-containing areas in the tantalum oxide film on the inner and outer parts of the porous body. Based on this new finding, the inventors completed the capacitor of this disclosure.
[0018] (Embodiments) Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0019] Figure 1A is a schematic cross-sectional view showing an example of a capacitor of the present disclosure. Figure 1B is a cross-sectional view of the capacitor in the inner part of the porous body enclosed by the dashed line B in Figure 1A. Figure 1C is a cross-sectional view of the capacitor in the outer part of the porous body enclosed by the dashed line C in Figure 1A. As shown in Figures 1A to 1C, the capacitor 1a comprises a porous body 10 and a conductor 20. As shown in Figures 1B and 1C, the porous body 10 includes a metallic tantalum-containing portion 10a and a tantalum oxide film 30. The tantalum oxide film 30 is positioned in contact with the metallic tantalum-containing portion 10a. The tantalum oxide film 30 is positioned between the metallic tantalum-containing portion 10a and the conductor 20. The tantalum oxide film 30 includes a first portion 31 and a second portion 32. The first portion 31 contains fluorine. The second portion 32 is positioned closer to the metallic tantalum-containing portion 10a than the first portion 31 in the thickness direction of the tantalum oxide film 30. The fluorine content in the second portion 32 is less than the fluorine content in the first portion 31. The second portion 32 is in contact with, for example, the metallic tantalum-containing portion 10a.
[0020] As shown in Figures 1B and 1C, the thickness d of the second portion 32 in the inner portion 10c of the porous body 10. 2in This is the thickness d of the second portion 32 in the outer part 10s of the porous body 10. 2out It is larger than . In other words, in capacitor 1a, d 2in >d 2outThe condition of is satisfied. According to such a configuration, the dielectric loss tangent tends to be low in the inner portion 10c of the porous body 10, and the withstand voltage tends to be high in the outer portion 10s of the porous body 10. When the capacitor 1a is in use, a relatively low voltage that is susceptible to the influence of voltage drop can be applied to the inner portion 10c of the porous body 10. For this reason, even if the withstand voltage of the inner portion 10c of the porous body 10 is low, the overall withstand voltage of the capacitor 1a is unlikely to be significantly affected. In addition, since the dielectric loss tangent of the inner portion 10c of the porous body 10 is low, the dielectric loss tangent of the capacitor 1a tends to be low. When the capacitor 1a is in use, the outer portion 10s of the porous body 10 is less susceptible to the influence of voltage drop, and a relatively high voltage can be applied thereto. For this reason, the high withstand voltage in the outer portion 10s of the porous body 10 can contribute to increasing the overall withstand voltage of the capacitor 1a. Therefore, d 2in >d 2out By satisfying the condition of, a predetermined withstand voltage is ensured in the capacitor 1a, and the dielectric loss tangent is easily reduced.
[0021] The thickness d of the second portion 32 2in and d 2out is not limited to a specific method. The thickness d of the second portion 32 2in and d 2out can be determined, for example, by analyzing the tantalum oxide film 30 by energy dispersive X-ray spectroscopy (TEM-EDS) using a transmission electron microscope. For example, in a cross-sectional TEM image of the tantalum oxide film 30, TEM-EDS on minute regions is performed in a plurality of regions from a position close to the metal tantalum-containing portion 10a of the tantalum oxide film 30 toward the surface of the tantalum oxide film 30. From the results of TEM-EDS, the ratio of the number of fluorine atoms to the sum of the number of oxygen atoms and the number of fluorine atoms is calculated, and the maximum distance from the metal tantalum-containing portion 10a in the region where the value is less than 0.0001 is determined as the thickness of the second portion 32. In other words, the maximum value of the ratio of the number of fluorine atoms to the sum of the number of oxygen atoms and the number of fluorine atoms in the second portion 32 is, for example, less than 0.0001.
[0022] In capacitor 1a, the method for determining the thickness of the tantalum oxide film 30 is not limited to a specific method. The thickness of the tantalum oxide film 30 can be determined, for example, based on a TEM image of the tantalum oxide film 30.
[0023] For example, the thickness of the first portion 31 may be determined also based on the thicknesses of the second portion 32 and the tantalum oxide film 30 determined according to the above method.
[0024] As shown in FIG. 1B and FIG. 1C, each of the first portion 31 and the second portion 32 is, for example, a layered portion. The tantalum oxide film 30 may include only the first portion 31 and the second portion 32.
[0025] As shown in FIG. 1A, the capacitor 1a includes, for example, an anode lead 50. A part of the anode lead 50 is embedded in the porous body 10. The anode lead 50 contains, for example, a valve metal. The anode lead 50 may include, for example, tantalum, an alloy containing tantalum as a main component, niobium, an alloy containing niobium as a main component, another valve metal, or an alloy containing another valve metal as a main component. In this specification, the main component is the component contained in the largest amount on a mass basis. In the capacitor 1a, the metallic tantalum-containing portion 10a forms, for example, a part of the anode. The tantalum oxide film 30 may be formed along the outer surface of the porous body 10.
[0026] FIG. 2A, FIG. 3A, and FIG. 4A are perspective views for schematically explaining positions for measuring the thickness of the second portion 32 in the inner part 10c and the outer part 10s of the porous body 10. As shown in FIG. 2A, the porous body 10 can have a rectangular parallelepiped shape. FIG. 2B is a cross-sectional view of the porous body 10 taken along cutting plane X in FIG. 2A. As shown in FIG. 3A, the porous body 10 may have a cylindrical shape. FIG. 3B is a cross-sectional view of the porous body taken along cutting plane X in FIG. 3A. As shown in FIG. 4A, the porous body 10 may have a spherical shape. FIG. 4B is a cross-sectional view of the porous body taken along cutting plane X in FIG. 4A. The porous body 10 may have a shape other than a rectangular parallelepiped shape, a cylindrical shape, and a spherical shape.
[0027] As shown in Figures 2A, 3A, and 4A, for example, assuming that the density of the solid containing the porous body 10 and the portion in which the anode lead 50 is embedded is constant regardless of location, the centroid G of the solid is determined. Next, the cross-section X of the solid having the smallest cross-sectional area passing through the centroid G is determined. Then, the minimum dimension a of this cross-section X passing through the centroid G is determined. For example, the portion of the porous body 10 whose shortest distance from the surface of the porous body 10 is a / 4 or less corresponds to the outer portion 10s. In this case, the surface of the porous body 10 is defined as a virtual surface that is a continuous plane or curved surface tangent to the vertices of the convex portions on the actual surface of the porous body 10. Also, the portion of the porous body 10 other than the outer portion 10s corresponds to the inner portion 10c.
[0028] The thickness d of the second portion 32 in the inner part 10c of the porous body 10 2in The position where the measurement is taken is not limited to a specific position as long as that position is included in the inner part 10c. For example, the thickness d of the second part 32 at a position where the shortest distance from the surface of the porous body 10 is a / 3 or more. 2in The thickness d of the second portion 32 in the outer portion 10s of the porous body 10 is measured. 2out The position where the measurement is taken is not limited to a specific position as long as that position is included in the outer part 10s. For example, the thickness d of the second part 32 is measured at a position where the shortest distance from the surface of the porous body 10 is between a / 40 and a / 10. 2out This is measured.
[0029] d 2in >d 2out As long as the conditions are met, the thickness d of the second part in the outer part 10s 2out The thickness d of the second portion in the inner part 10c relative to the inner part 10c 2in ratio d 2in / d 2out It is not limited to a specific value. Ratio d 2in / d 2out For example, it is 1.4 or higher. In this case, the dielectric loss tangent of capacitor 1a tends to be lower. From the viewpoint of reducing the dielectric loss tangent of capacitor 1a, ratio d 2in / d 2out The ratio d is preferably 1.5 or greater, more preferably 1.6 or greater, and even more preferably greater than 1.6. 2in / d 2out The ratio d may be 1.8 or higher, 2.0 or higher, or 3.0 or higher. 2in / d 2out For example, it is 20.0 or less.
[0030] The thickness of the tantalum oxide film 30 is not limited to a specific value. For example, the tantalum oxide film 30 is 1 μm or less. In this case, the tantalum oxide film 30 can be formed by anodizing metallic tantalum. For example, the tantalum oxide film 30 is an anodic oxide film. For example, the tantalum oxide film 30 is 1 nm or more.
[0031] The maximum value of the ratio of the number of fluorine atoms to the total number of oxygen atoms in the first part 31 is not limited to a specific value. For example, the maximum value is 0.15 or less. In this case, the fluorine contained in the first part 31 is less likely to diffuse toward the porous body 10 due to the effects of electric fields and heat, and the dielectric loss tangent of the capacitor 1a tends to be lower. The maximum value of the above ratio may be 0.14 or less, 0.13 or less, 0.12 or less, 0.10 or less, 0.09 or less, or 0.08 or less. For example, the maximum value of the above ratio is 0.0001 or more.
[0032] As described above, the maximum value of the ratio of fluorine atoms to the total number of oxygen atoms in the second part 32 is, for example, less than 0.0001. In this case, the fluorine contained in the second part 32 is less likely to diffuse toward the porous body 10 due to the effects of electric fields and heat, and the dielectric loss tangent of the capacitor 1a tends to be lower. The maximum value of this ratio in the second part 32 may be 0.00009 or less, 0.00008 or less, 0.00007 or less, 0.00006 or less, 0.00005 or less, or 0.00004 or less.
[0033] The method for determining the ratio of fluorine atoms to the total number of oxygen atoms in the first part 31 and the second part 32 is not limited to a specific method. The ratio can be determined, for example, by TEM-EDS.
[0034] The first portion 31 may contain crystalline material or amorphous material. Even if the first portion 31 contains amorphous material, the tantalum oxide film 30 tends to have a high relative permittivity, and the capacitor 1a tends to have a high capacitance. For example, if a broad halo pattern is shown in the XRD pattern of the target using Cu-Kα lines at diffraction angles 2θ from 10° to 50°, it can be determined that the target is amorphous.
[0035] The second part 32 may contain crystalline material or amorphous material.
[0036] As shown in Figure 1A, the conductor 20 is arranged, for example, around the porous body 10. The capacitor 1a includes, for example, an insulator 2d. The insulator 2d electrically insulates the conductor 20 from the anode lead 50.
[0037] In capacitor 1a, the material of the conductor 20 is not limited to a specific material. The conductor 20 may contain valve metals such as aluminum, tantalum, niobium, and bismuth, or it may contain noble metals such as gold and platinum, or it may contain nickel. The conductor 20 may also contain carbon materials such as graphite, a solidified silver-containing paste, or both a solidified silver-containing paste and a carbon material.
[0038] The porous body 10 made of metallic tantalum is, for example, a sintered body of metallic tantalum powder.
[0039] As shown in Figures 1B and 1C, the capacitor 1a includes, for example, an electrolyte 40. The electrolyte 40 is disposed between the tantalum oxide film 30 and the conductor 20 in the thickness direction of the tantalum oxide film 30. In this case, the capacitor 1a is provided as, for example, an electrolytic capacitor. The electrolyte 40 is in contact with, for example, the conductor 20 and the tantalum oxide film 30, and fills the space between the conductor 20, which includes pores derived from the porous body 10, and the tantalum oxide film 30. In the capacitor 1a, the electrolyte 40 is, for example, in layers. The electrolyte 40 may be omitted in the capacitor 1a. In this case, the conductor 20 may be in contact with the tantalum oxide film 30.
[0040] The electrolyte 40 is not limited to a specific electrolyte. The electrolyte 40 includes, for example, at least one selected from the group consisting of manganese oxide, an electrolyte solution, and a conductive polymer. Examples of conductive polymers are polypyrrole, polythiophene, polyaniline, and derivatives thereof. The electrolyte 40 may also be a manganese compound such as manganese oxide. The electrolyte 40 may also include a solid electrolyte.
[0041] The dielectric loss tangent of capacitor 1a is, for example, 0.09 or less at 120 Hz. The value obtained by dividing the withstand voltage of capacitor 1a by the thickness of the tantalum oxide film 30 is, for example, 0.4 V / nm or more.
[0042] The method for forming the tantalum oxide film 30 is not limited to a specific method. The tantalum oxide film 30 is formed, for example, by a method comprising the following (I) and (II): (I) A porous body of metallic tantalum is brought into contact with an aqueous solution that does not contain fluorine (fluoride ions), and an anodic deposition is performed on the metallic tantalum to form an oxide layer in contact with the metallic tantalum. (II) The oxide layer formed in (I) is brought into contact with an aqueous solution that contains fluorine (fluoride ions), and an anodic deposition is performed on the metallic tantalum to obtain a tantalum oxide film 30 containing a first portion 31 and a second portion 32 that contain fluorine.
[0043] In anodic formation, for example, an electrolyte is placed between the anode and cathode, and a voltage ranging from a few volts [V] to several hundred volts [V] is applied between the anode and the cathode. For example, a voltage ranging from 5 volts [V] to 300 volts [V] is applied. When metallic tantalum is the anode, anions attracted to the metallic tantalum combine with the ionized tantalum to form a chemical formation film. At that time, ions or atoms, which are impurities from the electrolyte present around the anode, may be incorporated into the chemical formation film. For this reason, in anodic formation using metallic tantalum as the anode, it is practically impossible to form a film consisting of only two specific elements, such as tantalum and oxygen. For this reason, for example, the second part 32 may contain other elements other than tantalum and oxygen, such as fluorine, at a concentration such that the ratio of the number of atoms of other elements to the sum of the number of atoms of oxygen and other elements is less than 0.0001.
[0044] Thickness d of the second part 32 2in and d 2out This can be adjusted by the rate at which the voltage is swept during the anodic formation described above, the current density applied, and the magnitude of the voltage applied between the anode and cathode. For example, the faster the rate at which the voltage is swept during the anodic formation described in (II) above, the greater the thickness d 2in The thickness d 2out It tends to become larger. The voltage drop caused by the resistive component of the electrolyte is larger in the inner part of the porous body 10 than in the outer part of the porous body 10. Therefore, in anodic formation, a difference is created between the effective voltage applied in the inner part of the porous body 10 and the effective voltage applied in the outer part of the porous body 10, making it difficult for fluorine to be incorporated in the inner part of the porous body. Also, in anodic formation in (II) above, the larger the voltage applied between the anode and cathode, the greater the thickness d of the second part 32. 2in and d 2out All of them will become smaller.
[0045] Figure 5 is a schematic cross-sectional view showing another example of the capacitor of this disclosure. Capacitor 1b shown in Figure 5 is configured in the same manner as capacitor 1a, except for parts that are not specifically described. Components of capacitor 1b that are the same as or correspond to components of capacitor 1a are denoted by the same reference numerals, and detailed descriptions are omitted. The description of capacitor 1a also applies to capacitor 1b, unless otherwise technically contradictory.
[0046] As shown in Figure 5, in capacitor 1b, the tantalum oxide film 30 includes, for example, a third portion 33. The third portion 33 is located between the first portion 31 and the conductor 20 in the thickness direction of the tantalum oxide film 30. The fluorine content in the third portion 33 is less than the fluorine content in the first portion 31. With this configuration, the dielectric loss tangent of capacitor 1b tends to be lower.
[0047] Figure 6A is a schematic diagram showing an example of an electrical circuit of the present disclosure. The electrical circuit 3 includes a capacitor 1a. The electrical circuit 3 may be an active circuit or a passive circuit. The electrical circuit 3 may be a discharge circuit, a smoothing circuit, a decoupling circuit, or a coupling circuit. Because the electrical circuit 3 includes a capacitor 1a, the electrical circuit 3 is more likely to exhibit the desired performance. For example, noise is more easily reduced in the electrical circuit 3. The electrical circuit 3 may include a capacitor 1b instead of a capacitor 1a.
[0048] Figure 6B is a schematic diagram showing an example of a circuit board of the present disclosure. As shown in Figure 6B, the circuit board 5 is equipped with a capacitor 1a. For example, an electrical circuit 3 including the capacitor 1a is formed on the circuit board 5. Because the circuit board 5 is equipped with a capacitor 1a, the circuit board 5 is more likely to exhibit the desired performance. The circuit board 5 may be an embedded board or a motherboard. The circuit board 5 may be equipped with a capacitor 1b instead of capacitor 1a.
[0049] Figure 6C is a schematic diagram showing an example of the device of this disclosure. As shown in Figure 6C, the device 7 includes a capacitor 1a. The device 7 includes, for example, a circuit board 5 including a capacitor 1a. Because the device 7 includes a capacitor 1a, it is easier for the device 7 to exhibit the desired performance. The device 7 may be an electronic device, a communication device, a signal processing device, or a power supply device. The device 7 may be a server, an AC adapter, an accelerator, or a flat panel display such as a liquid crystal display (LCD). The device 7 may be a USB charger, a solid state drive (SSD), an information terminal such as a PC, smartphone, or tablet PC, or an Ethernet switch. The device 7 may include a capacitor 1b instead of a capacitor 1a.
[0050] (Note) Based on the above description, the following technologies are disclosed. (Technology 1) A capacitor comprising: a porous body containing a metallic tantalum portion and a tantalum oxide film; and a conductor, wherein the tantalum oxide film is in contact with the metallic tantalum portion and disposed between the metallic tantalum portion and the conductor; the tantalum oxide film includes a first portion containing fluorine and a second portion disposed in the thickness direction of the tantalum oxide film at a position closer to the metallic tantalum portion than the first portion; the fluorine content in the second portion is less than the fluorine content in the first portion; and the thickness of the second portion in the inner part of the porous body is greater than the thickness of the second portion in the outer part of the porous body. (Technology 2) The capacitor according to Technology 1, wherein the first portion contains amorphous material. (Technology 3) The capacitor according to Technology 1 or 2, wherein the ratio of the thickness of the second portion in the inner part of the porous body to the thickness of the second portion in the outer part of the porous body is 1.4 or more. (Technology 4) The capacitor according to any one of Technology 1 to 3, wherein the maximum value of the ratio of the number of fluorine atoms to the sum of the number of oxygen atoms and fluorine atoms in the first part is 0.15 or less. (Technology 5) The capacitor according to any one of Technology 1 to 4, wherein the maximum value of the ratio of the number of fluorine atoms to the sum of the number of oxygen atoms and fluorine atoms in the second part is less than 0.0001. (Technology 6) The capacitor according to any one of Technology 1 to 5, wherein the tantalum oxide film includes a third part disposed between the first part and the conductor in the thickness direction of the tantalum oxide film, and the fluorine content in the third part is less than the fluorine content in the first part. (Technology 7) The capacitor according to any one of Technology 1 to 6, further comprising an electrolyte disposed between the tantalum oxide film and the conductor in the thickness direction of the tantalum oxide film. (Technology 8) An electrical circuit comprising the capacitor according to any one of Technology 1 to 7. (Technology 9) A circuit board comprising the capacitor according to any one of Technology 1 to 7. (Technical 10) An apparatus comprising a capacitor as described in any one of Technical 1 to 7.
[0051] The present disclosure will be further described below with reference to examples. Note that the following examples are illustrative and the present disclosure is not limited to these examples.
[0052] <Reference Examples 1A to 1D> A flat plate of metallic tantalum was immersed in a container filled with acetone and ultrasonic cleaning was performed for 10 minutes to clean the surface of the metallic tantalum. After that, the acetone adhering to the surface of the metallic tantalum was evaporated and the surface of the metallic tantalum was washed with pure water. Then the metallic tantalum was dried in the air. In this way, an anode foil was obtained.
[0053] The anode foil and the platinum foil as the counter electrode were arranged at predetermined intervals so as to be immersed in a phosphoric acid aqueous solution. The portion of the anode foil not immersed in the phosphoric acid aqueous solution was connected to the positive electrode of the power supply, and the portion of the platinum foil not immersed in the phosphoric acid aqueous solution was connected to the negative electrode of the power supply. In Reference Examples 1A, 1B, 1C, and 1D, voltages of 60V, 50V, 40V, and 30V were applied between the anode foil and the platinum foil for predetermined times, respectively, to form an oxide layer containing Ta2O5 on the surface of the anode foil. The anode foil was removed from the phosphoric acid aqueous solution, washed with pure water, and then dried in the air.
[0054] Next, the anode foil on which the oxide layer was formed and the platinum foil as the counter electrode were placed at predetermined intervals so as to be immersed in a mixed aqueous solution of NaF and sodium phosphate buffer. The portion of the anode foil not immersed in the mixed aqueous solution was connected to the positive electrode of the power supply, and the portion of the platinum foil not immersed in the mixed aqueous solution was connected to the negative electrode of the power supply. A voltage of 90V was applied between the anode foil and the platinum foil for a predetermined time to form a fluorine-containing tantalum oxide film. In this way, samples according to Reference Examples 1A to 1D were obtained, in which a fluorine-containing tantalum oxide film was formed on the surface of a flat plate-shaped metallic tantalum.
[0055] (TOF-SIMS) Fragments of a predetermined size were cut from the samples related to Reference Examples 1A to 1D, and samples for time-of-flight secondary ion mass spectrometry (TOF-SIMS) were prepared by resin embedding. TOF-SIMS was performed on the samples prepared from the samples related to Reference Examples 1A to 1D using the TOF-SIMS 5 instrument manufactured by ION-TOF, and the compositional analysis of the tantalum oxide film in the depth direction was performed. As a result, the thickness d of the tantalum oxide film in the samples related to Reference Examples 1A to 1D was determined. r0 , the thickness d of the part corresponding to the first part 31 above r1 , and the thickness d of the part corresponding to the second part 32 r2 The thickness d of the tantalum oxide film was determined. r0 The thickness d of the part corresponding to the first part 31 r1 ratio d r1 / d r0 The result was calculated and is shown in Table 1.
[0056]
[0057] <Reference Examples 2A to 2D> An anode lead made of rod-shaped metallic tantalum was embedded in metallic tantalum powder at one end in the longitudinal direction, and the tantalum powder was molded into a rectangular parallelepiped to obtain a molded body. This molded body was sintered to obtain an anode body with a porous structure in which one end of the anode lead was embedded.
[0058] Next, the anode was immersed in an aqueous phosphoric acid solution, and a voltage of 60V, 50V, 40V, or 30V was applied to the anode using an anode lead for a predetermined time to form an oxide layer containing Ta2O5 on the surface of the anode. The anode was then removed from the aqueous phosphoric acid solution, washed with pure water, and dried in the air.
[0059] Next, the anode body with the oxide layer formed on it was immersed in a mixed aqueous solution of NaF and sodium phosphate buffer, and a voltage of 90V was applied to the anode body for a predetermined time using an anode lead. This formed a fluorine-containing tantalum oxide film on the surface of the anode body. The anode body was removed from the mixed solution, washed with pure water, and dried in a drying oven adjusted to 100°C for 10 minutes to obtain samples according to Reference Examples 2A to 2D. The conditions for forming the oxide layer and the conditions for forming the fluorine-containing tantalum oxide film in Reference Examples 2A to 2D were adjusted to be the same as those in Reference Examples 1A to 1D, respectively. Therefore, the ratio d1 / d0 in the samples according to Reference Examples 2A to 2D is the same as the ratio d1 / d0 in the samples according to Reference Examples 1A to 1D, respectively. r1 / d r0 It was assumed that this is the same. The ratio d1 / d0 is the thickness d1 of the part corresponding to the first part 31 relative to the thickness d0 of the tantalum oxide film.
[0060] (Dielectric Loss Tangent) The dielectric properties of the samples related to Reference Examples 2A to 2D were evaluated according to the AC impedance method. In this evaluation, the amplitude was adjusted to 500 mV. In addition, the dielectric loss tangent tanδ was calculated from the resistance values at five different frequencies within the range of 200 Hz to 80 Hz while varying the frequency, and the dielectric loss tangent tanδ at 120 Hz was calculated from the approximate straight line obtained from the five data points.
[0061] Figure 7A is a graph showing the relationship between the dielectric loss tangent tanδ of the samples related to Reference Examples 2A to 2D and the ratio d1 / d0 of the thickness of the first region to the thickness of the tantalum oxide film. In Figure 7A, the vertical axis represents the dielectric loss tangent tanδ at 120 Hz, and the horizontal axis represents the ratio d1 / d0. Figure 7A shows that the larger the ratio d1 / d0, the higher the dielectric loss tangent tanδ.
[0062] (Withstand Voltage) Samples from Reference Examples 2A to 2D were immersed in an aqueous phosphoric acid solution, and their withstand voltage was evaluated according to chronovoltammetry using SUS316L as the counter electrode. The constant current value in chronovoltammetry was set to 300 μA, and the voltage value after 5 minutes was taken as the withstand voltage. The evaluation was performed at room temperature (20°C to 30°C). The thickness of the tantalum oxide film in each sample was the same as the thickness of the tantalum oxide film d in Reference Examples 1A to 1D. r0 The value used was calculated by dividing the withstand voltage value by the thickness of the tantalum oxide film 30 to obtain the withstand voltage [V / nm].
[0063] Figure 7B is a graph showing the relationship between the dielectric strength of the samples related to Reference Examples 2A to 2D and the ratio d1 / d0 of the thickness of the first part to the thickness of the tantalum oxide film. In Figure 7B, the vertical axis represents the dielectric strength [V / nm], and the horizontal axis represents the ratio d1 / d0. According to Figure 7B, it can be seen that the greater the ratio d1 / d0, the higher the dielectric strength of the tantalum oxide film.
[0064] Figures 7A and 7B show that as the ratio d1 / d0 increases, the dielectric strength increases, but the dielectric loss tangent also increases. On the other hand, as the ratio d1 / d0 decreases, the dielectric loss tangent decreases, but the dielectric strength decreases.
[0065] <Example 1> An anode lead made of rod-shaped metallic tantalum was embedded in metallic tantalum powder at one end in the longitudinal direction, and the tantalum powder was molded into a rectangular parallelepiped to obtain a molded body. This molded body was sintered to obtain an anode body with a porous structure in which one end of the anode lead was embedded.
[0066] Next, the anode was immersed in an aqueous phosphoric acid solution, and a voltage of 50V was applied to the anode using an anode lead for a predetermined time to form an oxide layer containing Ta2O5 on the surface of the anode. The anode was then removed from the aqueous phosphoric acid solution, washed with pure water, and dried in the air.
[0067] Next, the anode body with the oxide layer formed on it was immersed in a mixed aqueous solution of NaF and sodium phosphate buffer. Using an anode lead, the voltage was swept up to 90V at a rate of 0.4V / min, and the 90V voltage was applied for a predetermined time. This formed a fluorine-containing tantalum oxide film on the surface of the anode body. The anode body was removed from the mixed solution, washed with pure water, and dried in a drying oven adjusted to 100°C for 10 minutes to obtain the sample according to Example 1.
[0068] <Comparative Example 1> A sample according to Comparative Example 1 was obtained in the same manner as in Example 1, except that the voltage sweep rate when forming a fluorine-containing tantalum oxide film using a mixed aqueous solution of NaF and sodium phosphate buffer was changed to 0.1 V / min.
[0069] (X-ray diffraction) An XRD pattern was obtained by 2θ / θ scanning of a sample prepared from the sample according to Example 1 using the X'Pert PRO X-ray diffractometer manufactured by PANalytical. Cu-Kα rays were used as the X-ray source, with the voltage adjusted to 45 kV and the current adjusted to 40 mA. The wavelength of the Cu-Kα rays is 0.15418 nm. Figure 8 is a graph showing the results of X-ray diffraction (XRD) measurements of the sample according to Example 1 and metallic tantalum. In Figure 8, the vertical axis shows the diffraction intensity [counts per second (cps)], and the horizontal axis shows the diffraction angle 2θ. As shown in Figure 8, the XRD measurement results of the sample according to Example 1 showed that although diffraction peaks originating from metallic tantalum were confirmed, an overall broad profile was observed. Therefore, it was shown that the fluorine-containing tantalum oxide contained in the tantalum oxide film of the sample according to Example 1 is amorphous.
[0070] (TEM-EDS) Samples for TEM-EDS were prepared by cutting out fragments of a predetermined size from the inner and outer parts of the porous bodies in the samples of Example 1 and Comparative Example 1 using a focused ion beam (FIB). Here, the outer and inner parts of the porous body were determined according to Figures 2A and 2B and their descriptions. Fragments from the inner part of the porous body were taken from areas where the shortest distance from the surface of the porous body was between (1 / 3)a and (1 / 2)a. Fragments from the outer part of the porous body were taken from areas where the shortest distance from the surface of the porous body was between (1 / 30)a and (1 / 25)a. Here, a is the minimum dimension a as described using Figures 2A and 2B, etc.
[0071] Using a JEM-ARM200F transmission electron microscope manufactured by JEOL Ltd., TEM-EDS was performed on minute regions of the above-mentioned samples prepared from the inner and outer parts of the porous materials in Example 1 and Comparative Example 1. TEM-EDS was performed in 12 minute regions, starting from a position close to the metallic tantalum-containing portion of the tantalum oxide film and moving toward the surface of the tantalum oxide film. In each minute region, the ratio of the number of fluorine atoms to the sum of the number of oxygen atoms and fluorine atoms (F / (F+O)) was determined. Figure 9 is a graph showing the relationship between the ratio F / (F+O) in the inner and outer parts of the porous materials of the samples in Example 1 and Comparative Example 1 and the distance from the metallic tantalum-containing portion.
[0072] Figure 9 shows that in the samples of Example 1 and Comparative Example 1, the tantalum oxide film is formed on the metallic tantalum-containing portion of the porous material in both the inner and outer parts. In addition, it is understood that the tantalum oxide film contains a first region with a high fluorine concentration and a second region with a low fluorine concentration. From the TEM-EDS results, the maximum distance from the metallic tantalum-containing portion in a minute region where the ratio F / (F+O) is less than 0.0001 was determined as the thickness of the second region. The thickness of the tantalum oxide film was also determined from the TEM image of the tantalum oxide film. The thickness of the first region was determined by subtracting the thickness of the second region from the thickness of the tantalum oxide film. The results are shown in Table 2.
[0073]
[0074] (Dielectric Loss Tangent and Dielectric Strength) The dielectric loss tangent tanδ and dielectric strength of the samples in Example 1 and Comparative Example 1 were measured in the same manner as in Reference Examples 2A to 2D. The results are shown in Table 3. The dielectric strength of Example 1 and Comparative Example 1 was calculated using the thickness of the tantalum oxide film on the outer surface for reasons described later.
[0075]
[0076] As shown in Table 3, the dielectric strength of the sample according to Example 1 was equivalent to that of the sample according to Comparative Example 1. On the other hand, the dielectric loss tangent tanδ of the sample according to Example 1 was lower than that of the sample according to Comparative Example 1. Thickness d of the second portion of the tantalum oxide film in the inner part of the porous material of the sample according to Example 1. 2in The thickness d of the second portion of the tantalum oxide film on the outer side of the porous material 2out It is thought that the greater thickness contributes to the lower dielectric loss tangent tanδ. On the other hand, the fact that the breakdown voltage in Example 1 is the same as in Comparative Example 1 despite the smaller ratio d1 / d0 in the inner part of the porous body is thought to be because the ratio d1 / d0 on the surface of the porous body is the same in both Example 1 and Comparative Example 1. When measuring the breakdown voltage and when using the capacitor, the voltage drop due to the electrolyte or conductor in contact with the tantalum oxide film is greater in the inner part of the porous body than in the outer part. For this reason, the effective voltage applied to the tantalum oxide film is greater in the outer part of the porous body. This is why the thickness of the outer part was used as the film thickness of the tantalum oxide film when calculating the breakdown voltage in Example 1 and Comparative Example 1. Thus, if the ratio d1 / d0 in the outer part of the porous body of the sample in Example 1 is the same as or close to the ratio d1 / d0 in the outer part of the porous body of the sample in Comparative Example 1, a predetermined breakdown voltage can be ensured. In this way, the sample shown in Example 1 reduced the dielectric loss tangent while ensuring a predetermined breakdown voltage. Furthermore, the electrolyte or conductor in contact with the tantalum oxide film during voltage withstand measurement and capacitor use is not limited to a specific electrolyte or conductor.
[0077] The capacitor relating to this disclosure is advantageous in that it reduces the dielectric loss tangent while ensuring a predetermined withstand voltage.
Claims
1. A capacitor comprising: a porous body containing a metallic tantalum-containing portion and a tantalum oxide film; and a conductor, wherein the tantalum oxide film is in contact with the metallic tantalum-containing portion and is disposed between the metallic tantalum-containing portion and the conductor; the tantalum oxide film includes a first portion containing fluorine and a second portion located closer to the metallic tantalum-containing portion than the first portion in the thickness direction of the tantalum oxide film; the fluorine content in the second portion is less than the fluorine content in the first portion; and the thickness of the second portion on the inside of the porous body is greater than the thickness of the second portion on the outside of the porous body.
2. The capacitor according to claim 1, wherein the first portion includes amorphous material.
3. The capacitor according to claim 1, wherein the ratio of the thickness of the second portion in the inner part of the porous body to the thickness of the second portion in the outer part of the porous body is 1.4 or more.
4. The capacitor according to claim 1, wherein the maximum value of the ratio of the number of fluorine atoms to the total number of oxygen atoms and fluorine atoms in the first part is 0.15 or less.
5. The capacitor according to claim 1, wherein the maximum value of the ratio of the number of fluorine atoms to the total number of oxygen atoms and fluorine atoms in the second part is less than 0.0001.
6. The capacitor according to claim 1, wherein the tantalum oxide film includes a third portion disposed between the first portion and the conductor in the thickness direction of the tantalum oxide film, and the fluorine content in the third portion is less than the fluorine content in the first portion.
7. The capacitor according to claim 1, further comprising an electrolyte disposed between the tantalum oxide film and the conductor in the thickness direction of the tantalum oxide film.
8. An electrical circuit comprising the capacitor described in any one of claims 1 to 7.
9. A circuit board comprising the capacitor described in any one of claims 1 to 7.
10. An apparatus comprising a capacitor according to any one of claims 1 to 7.