Fiber bundle assembly and method for producing fiber bundle assembly
The fiber bundle aggregate with a controlled diameter ratio and airflow/vibration method addresses the aggregation issue, ensuring improved feedability and handling stability by minimizing fiber bundle aggregation.
Patent Information
- Application Number
- PCT/JP2026/015776
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-19
Smart Images

Figure JP2026015776_19112026_PF_FP_ABST
Abstract
Description
Fiber bundle aggregate and method for producing fiber bundle aggregate
[0001] The present invention relates to a fiber bundle aggregate and a method for producing the fiber bundle aggregate.
[0002] A fiber bundle includes a plurality of fibers and forms a single integrated shape, and a fiber bundle aggregate is an aggregate of a plurality of such fiber bundles. For example, recycled carbon fiber products are handled as fiber bundle aggregates, and various studies have been conducted on the handleability of such fiber bundle aggregates.
[0003] For example, Patent Document 1 discloses a method for producing a fiber bundle, which includes mixing a plurality of short fibers with a bundling liquid having a viscosity ratio Rη represented by the following formula (1) of greater than 1. Rη = ηy / ηz (1) In formula (1), ηy is the viscosity of the bundling liquid measured at 23°C using a B-type rotational viscometer at a spindle rotation speed of 10 rpm, and ηz is the viscosity of the bundling liquid measured at 23°C using a B-type rotational viscometer at a spindle rotation speed of 100 rpm.
[0004] According to the method described in Patent Document 1, fiber bundles with small fiber bundle sizes can be obtained, and it is stated that using the small-sized fiber bundles can improve the feed efficiency of the fiber bundles to a kneader or the like when producing a fiber-reinforced resin composition.
[0005] JP 2024-086632 A
[0006] As described in Patent Document 1, it is known that the smaller the size of a fiber bundle, the better the handleability it exhibits. However, the present inventors have found that when the size of the fiber bundle is excessively small, it causes the fiber bundles to aggregate with each other and form larger fiber aggregates, which may lead to reduced handleability.
[0007] Accordingly, an object of the present invention is to provide a fiber bundle aggregate that exhibits excellent handleability.
[0008] The present invention achieves the above object by the following means.
[0009] (Aspect 1) A fiber bundle aggregate comprising a plurality of first fiber bundles having a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, and a plurality of second fiber bundles having a maximum fiber bundle diameter greater than 2.0 mm and less than or equal to 10.0 mm and a minimum fiber bundle diameter greater than 0.5 mm and less than or equal to 5.0 mm, wherein the ratio of the number of first fiber bundles to the number of second fiber bundles is 0.18 or less, and the ratio of the number of second fiber bundles to the total number of fiber bundles contained in the fiber bundle aggregate is 0.80 or more. (Aspect 2) The aggregate according to Aspect 1, wherein the first fiber bundles and / or the second fiber bundles contain carbon fibers. (Aspect 3) The aggregate according to Aspect 2, wherein the surfaces of the carbon fibers contained in the first fiber bundles and the second fiber bundles are at least partially covered with residual carbon. (Aspect 4) The aggregate according to any one of aspects 1 to 3, wherein the surfaces of the first fiber bundle and the second fiber bundle are at least partially covered with a resin binder. (Aspect 5) A method for producing the aggregate according to any one of aspects 1 to 4, comprising supplying an airflow while vibrating the fiber bundle aggregate precursor to remove a portion of the fiber bundles and fibers constituting the fiber bundle aggregate precursor. (Aspect 6) The method according to aspect 5, wherein an airflow is supplied while vibrating the fiber bundle aggregate precursor in a vibrating fluidized bed apparatus. (Aspect 7) The method according to aspect 6, wherein the wind speed of the airflow in the vibrating fluidized bed apparatus is 2.0 m / s or less. (Aspect 8) The method according to any one of aspects 5 to 7, further comprising crushing or cutting a fiber composite resin material and then carbonizing it to provide the fiber bundle aggregate precursor, or carbonizing a fiber composite resin material and then crushing or cutting it to provide the fiber bundle aggregate precursor. (Aspect 9) The method according to aspect 8, wherein the cutting length of the cutting is 10.0 mm or less. (Aspect 10) The method according to any one of aspects 5 to 9, further comprising coating the fiber bundles constituting the fiber bundle aggregate precursor with a resin binder before processing in a vibrating fluidized bed apparatus.
[0010] The fiber bundle assembly of the present invention exhibits good handling properties.
[0011] Figure 1 is a schematic diagram illustrating the manufacturing process of recycled carbon fiber products.
[0012] The embodiments of the present invention will be described in detail below. However, the present invention is not limited to the embodiments described below, and can be implemented with various modifications within the scope of the gist of the invention. Furthermore, in the description of the drawings, the same elements are denoted by the same reference numerals, and redundant explanations are omitted.
[0013] <<Fiber Bundle Assembly>> The fiber bundle assembly of the present invention contains a plurality of first fiber bundles having a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, and a plurality of second fiber bundles having a maximum fiber bundle diameter greater than 2.0 mm and less than or equal to 10.0 mm and a minimum fiber bundle diameter greater than 0.5 mm and less than or equal to 5.0 mm, wherein the ratio of the number of first fiber bundles to the number of second fiber bundles is 0.18 or less, and the ratio of the number of second fiber bundles to the total number of fiber bundles contained in the fiber bundle assembly is 0.80 or more.
[0014] In conventional fiber bundle assemblies, small fiber bundles, i.e., first fiber bundles with a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, tend to cause the fiber bundles to aggregate with each other, making it easier to form larger fiber aggregates, which can lead to poor handling of the fiber bundle assemblies.
[0015] Furthermore, large fiber aggregates worsen handling during compounding, leading to problems such as poor conveying in feeders and blockage of flow paths. Therefore, conventional fiber bundle aggregates have a feeding problem in that they cannot stably maintain a consistent amount of additive to the compound.
[0016] In contrast, the fiber bundle aggregate of the present invention contains a plurality of first fiber bundles having a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, and a plurality of second fiber bundles having a maximum fiber bundle diameter greater than 2.0 mm and less than or equal to 10.0 mm and a minimum fiber bundle diameter greater than 0.5 mm and less than or equal to 5.0 mm, wherein the ratio of the number of first fiber bundles to the number of second fiber bundles is 0.18 or less, and the ratio of the number of second fiber bundles to the total number of fiber bundles contained in the fiber bundle aggregate is 0.80 or more.
[0017] In the fiber bundle aggregate of the present invention, the ratio of the number of first fiber bundles to the number of second fiber bundles is 0.18 or less. As a result, the number of first fiber bundles is small, and fiber bundle aggregation is less likely to occur, thus suppressing deterioration of handling properties due to fiber bundle aggregation.
[0018] Furthermore, the second fiber bundle is larger than the first fiber bundle and less likely to promote aggregation, so it may mainly constitute the fiber bundle aggregate of the present invention.
[0019] While there is no intention to limit the scope, in particular, when the fiber bundle aggregate is a recycled carbon fiber product, fine fiber bundles and fibers are generated during the manufacturing process of recycled carbon fibers. Specifically, as shown in Figure 1, a fiber bundle aggregate precursor 200 is obtained by crushing or cutting the fiber composite resin material 100 (Figures 1(a) and (b)) and then performing dry distillation, or by dry distilling the fiber composite resin material 100 and then crushing or cutting it. In this invention, the fiber bundle aggregate precursor may be the aforementioned fiber bundle aggregate precursor 200 with a resin binder added and mixed, which is preferable from the viewpoint of bundling properties. In these processes, particularly in the process of adding and mixing the resin binder to the fiber bundle aggregate precursor 200, when the fiber bundle aggregate precursor and the resin binder are mixed, the fiber bundles and fibers contained in the fiber bundle aggregate precursor 200 are broken, resulting in the fineness of the fiber bundles and fibers contained in the fiber bundle aggregate precursor 200 (Figures 1(c) and (d)), which makes it easy for the above-mentioned problems to occur. The manufacturing process for the fiber bundle aggregate precursor described above may be carried out continuously with the process using the vibrating fluidized bed described later, or it may be carried out in a separate location.
[0020] The present invention has been found to exhibit surprisingly good feedability in a fiber bundle assembly, provided that the first fiber bundle and the second fiber bundle satisfy the specific relationship described above. This relationship was derived from the relationship between the first fiber bundle and the second fiber bundle obtained by the fiber bundle assembly manufacturing method described later. Furthermore, the fiber bundle assembly manufacturing method described later allows for the effective removal of the first fiber bundle while suppressing the destruction of the second fiber bundle, thus enabling the development of excellent feedability without significantly impairing yield, etc.
[0021] The fiber bundle aggregate of the present invention may also be applied to resin composite materials. Main means of compounding such resin composite materials include melt extrusion molding of a compound composed of the fiber bundle aggregate and resin.
[0022] The reasons why the effects of the present invention manifest themselves are thought to be as follows.
[0023] The aforementioned first fiber bundle is an extremely fine fiber bundle. Therefore, even when the process of obtaining an aggregate of fiber bundles of a certain size, such as the aforementioned second fiber bundle, is carried out with precision, the first fiber bundle is considered an unavoidable component that inevitably occurs, albeit in very small amounts. Furthermore, even in very small amounts, this first fiber bundle is thought to have a function similar to a so-called flocculation promoter in subsequent processes, promoting the aggregation of fiber bundles and thereby impairing subsequent feedability. In response to this, we have found a relationship between the first fiber bundle and the second fiber bundle in which the flocculation-promoting effect of the first fiber bundle is not sufficiently expressed.
[0024] Furthermore, we also considered simply isolating the second fiber bundle. In this regard, although the weight ratio of the first fiber bundle to the entire fiber bundle assembly is very small, the size of the first fiber bundle is small compared to the other fiber bundles, so the number of first fiber bundles relative to the entire fiber bundle assembly is very large. Moreover, the fiber bundle is an aggregate of very thin fibers, with each fiber having a diameter of only a few micrometers, and the first fiber bundles are mixed in, filling the gaps between the second fiber bundles. For these reasons, it was extremely difficult to simply isolate the second fiber bundle without causing the generation of first fiber bundles by destroying the second fiber bundles.
[0025] For example, manual removal is not feasible from a productivity standpoint. Furthermore, removal using a sieve that allows the first fiber bundle to pass through but not the second fiber bundle can remove the first fiber bundles in the area directly in contact with the sieve, but it cannot remove the first fiber bundles in the gaps between the second fiber bundles. Attempting to remove these first fiber bundles may exacerbate the damage to the second fiber bundles.
[0026] Therefore, the fiber bundle aggregate of the present invention is not limited to the method of manufacturing the fiber bundle aggregate described later, but it can be said that the present invention has found a relationship between the first fiber bundle and the second fiber bundle such that the first fiber bundle is effectively removed while suppressing the destruction of the second fiber bundle, and as a result, the effect of promoting the aggregation of the first fiber bundle is not fully expressed.
[0027] In the present invention, the ratio of the number of first fiber bundles to the number of second fiber bundles (number of first fiber bundles / number of second fiber bundles) is not particularly limited, but may be 0.18 or less, 0.16 or less, 0.14 or less, 0.12 or less, or 0.10 or less, and may also be 0.00 or more, 0.02 or more, 0.04 or more, or 0.06 or more.
[0028] In the present invention, the ratio of the number of second fiber bundles to the total number of fiber bundles included in the fiber bundle assembly (number of second fiber bundles / total number of fiber bundles included in the fiber bundle assembly) is not particularly limited, but may be 0.80 or more, 0.84 or more, 0.88 or more, or 0.92 or more, and may also be 1.00 or less, 0.98 or less, 0.96 or less, or 0.94 or less.
[0029] In the present invention, the fiber bundles constituting the fiber bundle aggregate are not particularly limited, but examples include carbon fibers, inorganic fibers (glass fibers, metal fibers, etc.), organic fibers (resin fibers), etc.
[0030] In the present invention, examples of carbon fibers include recycled carbon fibers. Recycled carbon fibers are generally produced by crushing or cutting fiber composite resin materials such as Carbon Fiber Reinforced Plastics (CFRP), prepregs, and Carbon Fiber Reinforced Thermo Plastics (CFRTP), and then dry-drying them, or by dry-drying them and then crushing or cutting them. In this manufacturing process, the size of the carbon fiber bundles is reduced, so the method of the present invention can be particularly preferably used when the fiber bundle aggregate contains carbon fibers.
[0031] <First Fiber Bundle> In the present invention, the first fiber bundle is contained in the fiber bundle aggregate of the present invention, and has a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less.
[0032] In this invention, the "maximum fiber bundle diameter" and the "minimum fiber bundle diameter" are values that can be determined by the following method. Fiber bundles are randomly selected from a fiber bundle assembly and arranged on a white plate so that the fiber bundles do not overlap. Then, an image obtained by photographing from a vertical direction opposite to the white plate is binarized using the image analysis software ImageJ (WayneRasband), and the fiber bundle diameter of the fiber bundles can be measured. For a given fiber bundle, the "maximum fiber bundle diameter" indicates the maximum fiber bundle diameter, and the "minimum fiber bundle diameter" indicates the minimum fiber bundle diameter.
[0033] In the present invention, the maximum fiber bundle diameter of the first fiber bundle is not particularly limited, but may be 2.0 mm or less, 1.8 mm or less, 1.5 mm or less, or 1.3 mm or less, and may also be greater than 0.0 mm, 0.2 mm or more, 0.4 mm or more, or 0.6 mm or more.
[0034] In the present invention, the minimum fiber bundle diameter of the first fiber bundle is not particularly limited, but may be 1.0 mm or less, 0.7 mm or less, 0.5 mm or less, or 0.3 mm or less, and may also be greater than 0.0 mm, 0.1 mm or more, 0.2 mm or more, or 0.3 mm or more.
[0035] In the present invention, the first fiber bundle may contain carbon fibers. For details of the carbon fibers included in the first fiber bundle of the present invention, refer to the above description relating to the fiber bundle assembly of the present invention.
[0036] In the present invention, if the first fiber bundle contains carbon fibers, the surface of the carbon fibers contained in the first fiber bundle may be at least partially covered with residual carbon, i.e., the carbon fibers may be recycled carbon fibers. In this case, for details of recycled carbon fibers, refer to the above description relating to the fiber bundle assembly of the present invention.
[0037] In the present invention, residual carbon is the residue remaining after the resin component has been carbonized when a fiber composite material containing resin and fiber bundles is thermally decomposed to extract regenerated fibers. The preferred range for the amount of residual carbon in the fiber bundle aggregate of the present invention is more than 0.0% by weight and 20.0% by weight or less of the total amount of the fiber bundle aggregate, and the more preferable lower limit may be 1.0% by weight or more, 2.0% by weight or more, or 5.0% by weight or more. Furthermore, the more preferable upper limit may be 18.0% by weight or less, 16.0% by weight or less, or 15.0% by weight or less. Residual carbon has the effect of binding individual fibers together and holding the fiber bundle. When the amount of residual carbon is within the above range, the residual carbon acts as a binding force between individual fibers, making it easier to hold the fiber bundle and ensuring the relative ratio of fiber materials, thus making it easier to maintain the functionality of the fiber material, which is preferable.
[0038] In the present invention, the first fiber bundle may be at least partially coated with a resin binder.
[0039] The resin binder in the present invention is not particularly limited, but aqueous dispersions of polyether resins, polyester resins, acrylic resins, epoxy resins, polyamide resins, polyurethane resins, etc., are preferably used.
[0040] The binder content in the fiber bundle aggregate of the present invention is not particularly limited, but is preferably 0.1% by weight or more and 10.0% by weight or less, and more preferably 1.0% by weight or more and 5.0% by weight or less. When the binder content is within the above range, it is easier to ensure the cohesiveness of the fiber bundles, the relative ratio of the fiber materials can be ensured, and the functionality of the fiber materials can be easily maintained, which is preferable.
[0041] <Second Fiber Bundle> In the present invention, the second fiber bundle is contained in the fiber bundle aggregate of the present invention, and has a maximum fiber bundle diameter greater than 2.0 mm and less than or equal to 10.0 mm, and a minimum fiber bundle diameter greater than 0.5 mm and less than or equal to 5.0 mm.
[0042] In the present invention, the maximum fiber bundle diameter of the second fiber bundle is not particularly limited, but may be more than 2.0 mm, 2.5 mm or more, 3.0 mm or more, 3.5 mm or more, or 4.0 mm or more, and may be 10.0 mm or less, 9.0 mm or less, 8.0 mm or less, or 7.0 mm or less.
[0043] Further, in the present invention, the minimum fiber bundle diameter of the second fiber bundle is not particularly limited, but may be more than 0.5 mm, 0.6 mm or more, 1.0 mm or more, or 2.0 mm or more, and may be 5.0 mm or less, 4.5 mm or less, 4.0 mm or less, or 3.0 mm or less.
[0044] In the present invention, the second fiber bundle may contain carbon fibers. For details of the carbon fibers contained in the second fiber bundle of the present invention, the above description regarding the fiber bundle aggregate of the present invention can be referred to.
[0045] In the present invention, when the second fiber bundle contains carbon fibers, the surfaces of the carbon fibers contained in the second fiber bundle may be at least partially coated with residual carbon, that is, the carbon fibers may be recycled carbon fibers. At this time, for details of the recycled carbon fibers and residual carbon, the above description regarding the first fiber bundle of the present invention can be referred to.
[0046] In the present invention, the second fiber bundle may be at least partially coated with a resin binder. For details of the resin binder, the above description regarding the first fiber bundle of the present invention can be referred to.
[0047] <<Method for Producing Aggregate>> The method of the present invention for producing an aggregate comprises supplying an air flow while applying vibration to a fiber bundle aggregate precursor to remove part of the fiber bundles and fibers constituting the fiber bundle aggregate precursor.
[0048] Thereby, fiber bundles with small fiber bundle diameters, that is, relatively light fiber bundles and part of the fibers can be removed.
[0049] Conventional methods classify fiber bundles by, for example, the mesh size of a sieve. With such methods, it has been particularly difficult to remove fiber bundles and fibers of a specific size, such as the first fiber bundle of the present invention, which has a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, and in which the ratio of the maximum fiber bundle diameter to the minimum fiber bundle diameter (maximum fiber bundle diameter / minimum fiber bundle diameter) is large.
[0050] Furthermore, while the total number of fiber bundles and fibers that can be removed by the method of the present invention is large, their total weight is less than 1.0% of the total mass of the fiber bundle aggregate precursor before some of the fiber bundles and fibers are removed by the method of the present invention. Therefore, it has been difficult to efficiently remove such trace amounts of fiber bundles and fibers.
[0051] In contrast, the method of the present invention removes some of the fiber bundles and fibers that constitute the fiber bundle aggregate precursor by supplying an airflow while vibrating the fiber bundle aggregate precursor. Since the fiber bundles and fibers are broken down and miniaturized, it has not been common to apply an airflow with a velocity high enough to cause the fiber bundles and fibers to float in a fluidized bed apparatus or the like. However, by using a vibrating fluidized bed apparatus, i.e., a vibrating fluidized bed apparatus, the fiber bundles and fibers float slightly due to the vibration, so it is possible to remove some of the fiber bundles and fibers even with an airflow with a relatively low velocity that does not easily cause the fiber bundles and fibers to become miniaturized.
[0052] As described above, the total weight of fiber bundles and fibers that can be removed by the method of the present invention is less than 1.0% of the total mass of the fiber bundle aggregate precursor. Therefore, removing these fiber bundles and fibers will reduce the yield by about 1.0%, but this will result in a fiber bundle aggregate with significantly improved feedability.
[0053] In the present invention, supplying airflow while vibrating the fiber bundle aggregate precursor can be done, for example, by a vibrating fluidized bed apparatus, but the present invention is not limited thereto.
[0054] In the present invention, the process may further include coating the fiber bundles constituting the fiber bundle aggregate precursor with a resin binder before processing in a vibrating fluidized bed apparatus.
[0055] In the present invention, the wind speed of the airflow is not particularly limited, but may be 2.0 m / s or less, 1.8 m / s or less, 1.6 m / s or less, 1.4 m / s or less, or 1.0 m / s or less, and may also be 0.2 m / s or more, 0.4 m / s or more, 0.6 m / s or more, or 0.8 m / s or more. In the present invention, the wind speed of the airflow is the maximum wind speed of the airflow actually received by the fiber bundle aggregate precursor by the airflow provided by the drying apparatus.
[0056] <Fiber Bundle Assembly Precursor> In the present invention, the fiber bundle assembly precursor contains fiber bundles and fibers. In the present invention, the fiber bundle assembly precursor may contain, in addition to the first fiber bundle and the second fiber bundle of the present invention, fiber bundles and fibers that are finer than the first fiber bundle.
[0057] For details regarding the fiber bundles and fibers constituting the fiber bundle aggregate precursor of the present invention, please refer to the above description concerning the fiber bundle aggregate of the present invention.
[0058] The method of the present invention may further include crushing or cutting a fiber composite resin material and then carbonizing it to provide a fiber bundle aggregate precursor, or carbonizing a fiber composite resin material and then crushing or cutting it to provide a fiber bundle aggregate precursor.
[0059] <Fiber Composite Resin Material> In the present invention, the fiber composite resin material is crushed or cut by the method of the present invention, and then subjected to carbonization, or carbonized, and then crushed or cut to provide a fiber bundle aggregate precursor.
[0060] In the present invention, examples of fiber composite resin materials include, but are not limited to, CFRP, prepreg, and CFRTP.
[0061] In this case, the cutting length is not particularly limited, but may be 10.0 mm or less, 9.0 mm or less, 8.0 mm or less, 7.0 mm or less, or 5.0 mm or less, and may also be 1.0 mm or more, 2.0 mm or more, 3.0 mm or more, or 4.0 mm or more. Here, "cutting length" means the maximum cutting width of the fiber composite resin material.
[0062] Furthermore, in the present invention, the carbonization of the fiber composite resin material can be carried out by known methods for carbonization of fiber composite resin materials, and is not particularly limited.
[0063] The present invention will be described in more detail with reference to the following embodiments, but the scope of the present invention is not limited to these embodiments. In the embodiments described later, a vibrating fluidized bed that can also be used as a drying apparatus is described, but it is sufficient that the first fiber bundle can be removed, and for example, the drying function may be performed separately.
[0064] <Example 1> <Provision of Fiber Bundle Aggregate Precursor> 100 kg of CFRP was prepared as the fiber composite resin material. After carbonization and cutting to a cutting length of 6 mm, the fiber composite resin material was subjected to classification to remove coarse particles and fine powder to obtain a fiber bundle aggregate precursor.
[0065] <Addition and Mixing of Resin Binder> An aqueous dispersion of polyether-type urethane was added to the fiber bundle aggregate precursor as a resin binder and mixed using a mixer.
[0066] <Drying of Fiber Bundle Assembly Precursors> Using a vibrating fluidized bed apparatus as a drying device, the fiber bundle assembly precursor was dried at 150°C for 200 seconds to obtain fiber bundle assemblies. At this time, the airflow supplied to the fiber bundle assembly precursor by the vibrating fluidized bed apparatus was 0.6 m / s, and vibration was applied to the fiber bundle assembly precursor by the vibrating plate inside the vibrating fluidized bed apparatus. It was visually confirmed that the fiber bundle assembly precursor was floating above the vibrating plate and flowing well.
[0067] <Measurement of Fiber Bundle Diameter> Multiple fiber bundles constituting a fiber bundle assembly were randomly selected and arranged on a white board so that the fiber bundles did not overlap. Then, images obtained by photographing from a vertical direction opposite to the white board were binarized using the image analysis software ImageJ (WayneRasband), and the maximum and minimum fiber bundle diameters of more than 200 fiber bundle assemblies were measured. Subsequently, the fiber bundles were classified into first fiber bundles, second fiber bundles, and other fiber bundles, and the number of each fiber bundle was measured. The number of fiber bundles was measured by visually counting them after examining the images of the captured fiber bundles.
[0068] <Yield Evaluation> The mass of fiber bundles and fiber bundle assemblies removed by airflow treatment was measured in an extremely dry state, and the yield was calculated using the following formula: (Yield) = (Mass of fiber bundle assemblies after airflow treatment) / {(Mass of fiber bundle assemblies after airflow treatment) + (Mass of fiber bundles and fibers removed by airflow treatment)}.
[0069] <Evaluation of Feedability> The feedability of the fiber bundle assemblies when supplied at a supply rate of 3 kg / h using a twin screw feeder K2-ML-D5-T35 (manufactured by Coperion K-Tron) was evaluated according to the following criteria: ×: The supply amount decreased and stable supply could not be achieved. △: The supply amount fluctuated, but stable supply was achieved. ○: The supply amount did not fluctuate and stable supply was achieved.
[0070] <Example 2> The fiber bundle aggregate of Example 2 was obtained in the same manner as in Example 1, except that the wind speed during drying was set to 0.9 m / s.
[0071] <Example 3> The fiber bundle aggregate of Example 3 was obtained in the same manner as in Example 1, except that the wind speed during drying was set to 1.5 m / s.
[0072] <Example 4> A fiber bundle assembly of Example 4 was obtained in the same manner as in Example 1, except that the cutting length of the fiber composite resin material was set to 3.0 mm.
[0073] <<Comparative Example 1>> A fiber bundle aggregate of Comparative Example 1 was obtained in the same manner as in Example 1, except that the wind speed during drying was 0.4 m / s.
[0074] <<Comparative Example 2>> A fiber bundle assembly for Comparative Example 2 was obtained in the same manner as for Comparative Example 1, except that the wind speed during drying was 2.4 m / s.
[0075] <<Comparative Example 3>> A fiber bundle assembly of Comparative Example 3 was obtained in the same manner as in Comparative Example 1, except that the cutting length of the fiber composite resin material was set to 3.0 mm.
[0076] <<Comparative Example 4>> A fiber bundle assembly of Comparative Example 4 was obtained in the same manner as in Comparative Example 1, except that a fluidized bed apparatus was used as the drying apparatus, the vibrations applied to the fiber bundle assembly precursor by the vibrating plate of the vibrating fluidized bed apparatus were reduced so that the fiber bundle assembly precursor did not float above the vibrating plate, i.e., it was in a stationary state in which the fiber bundle assembly precursor was not flowing as confirmed by visual inspection, and the wind speed of the airflow during drying was 0.6 m / s.
[0077] <<Comparative Example 5>> A fiber bundle aggregate of Comparative Example 5 was obtained in the same manner as in Comparative Example 1, except that the resin binder was not added and mixed, and the fiber bundle aggregate precursor was not dried.
[0078] The conditions for implementation in Examples 1 to 4 and Comparative Examples 1 to 5, and the evaluation results of the obtained fiber bundle assemblies are shown in Table 1 below.
[0079]
[0080] As is clear from Table 1 above, fiber bundle assemblies according to the present invention were obtained in Examples 1 to 4. Furthermore, the fiber bundle assemblies according to the present invention showed relatively good feedability compared to the fiber bundle assemblies of Comparative Examples 1 to 5. Therefore, it was confirmed that a fiber bundle assembly containing a plurality of first fiber bundles with a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, and a plurality of second fiber bundles with a maximum fiber bundle diameter greater than 2.0 mm and less than or equal to 10.0 mm and a minimum fiber bundle diameter greater than 0.5 mm and less than or equal to 5.0 mm, wherein the ratio of the number of first fiber bundles to the number of second fiber bundles is 0.18 or less, and the ratio of the number of second fiber bundles to the total number of fiber bundles contained in the fiber bundle assembly is 0.80 or more, exhibits excellent feedability.
[0081] 100 Fiber composite resin material 200 Fiber bundle aggregate precursor
Claims
1. A fiber bundle assembly comprising a plurality of first fiber bundles having a maximum fiber bundle diameter of 2.0 mm or less and a minimum fiber bundle diameter of 1.0 mm or less, and a plurality of second fiber bundles having a maximum fiber bundle diameter greater than 2.0 mm and less than or equal to 10.0 mm and a minimum fiber bundle diameter greater than 0.5 mm and less than or equal to 5.0 mm, wherein the ratio of the number of first fiber bundles to the number of second fiber bundles is 0.18 or less, and the ratio of the number of second fiber bundles to the total number of fiber bundles included in the fiber bundle assembly is 0.80 or more.
2. The aggregate according to claim 1, wherein the first fiber bundle and / or the second fiber bundle contains carbon fibers.
3. The aggregate according to claim 2, wherein the surfaces of the carbon fibers contained in the first fiber bundle and the second fiber bundle are at least partially covered with residual carbon.
4. The aggregate according to any one of claims 1 to 3, wherein the surfaces of the first fiber bundle and the second fiber bundle are at least partially covered with a resin binder.
5. A method for producing an aggregate according to any one of claims 1 to 4, comprising supplying an airflow to a fiber bundle aggregate precursor while vibrating it to remove a portion of the fiber bundles and fibers constituting the fiber bundle aggregate precursor.
6. The method according to claim 5, wherein an airflow is supplied to a fiber bundle aggregate precursor while vibrating in a vibrating fluidized bed apparatus.
7. The method according to claim 6, wherein the wind speed of the airflow in the vibrating fluidized bed apparatus is 2.0 m / s or less.
8. The method according to any one of claims 5 to 7, further comprising crushing or cutting a fiber composite resin material and then carbonizing it to provide the fiber bundle aggregate precursor, or carbonizing a fiber composite resin material and then crushing or cutting it to provide the fiber bundle aggregate precursor.
9. The method according to claim 8, wherein the cutting length of the cut is 10.0 mm or less.
10. The method according to any one of claims 5 to 9, further comprising coating the fiber bundles constituting the fiber bundle aggregate precursor with a resin binder before processing in a vibrating fluidized bed apparatus.