Capacitor
By structuring capacitors with a first cathode layer of small silver particles and a second layer of larger silver particles, the capacitor achieves reduced initial equivalent series resistance, addressing the ESR challenges in existing designs.
Patent Information
- Application Number
- PCT/JP2026/015784
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-04-20
- Publication Date
- 2026-11-19
AI Technical Summary
Existing capacitors face challenges in maintaining low initial equivalent series resistance (ESR) due to the structure and composition of their cathode layers, particularly when using inorganic conductive layers or solid electrolyte layers containing conductive polymers.
The capacitor design includes a specific arrangement of cathode layers, where a first cathode layer with smaller silver-containing particles is in contact with an inorganic conductive layer, and a second cathode layer with larger silver-containing particles is formed on top, optimizing the interfacial and bulk resistances to reduce ESR.
This configuration significantly reduces the initial ESR by ensuring low interfacial and bulk resistances, facilitating easier electricity extraction and improved capacitor performance.
Smart Images

Figure JP2026015784_19112026_PF_FP_ABST
Abstract
Description
Capacitor Cross-reference of related applications
[0001] This disclosure claims priority with respect to Japanese Patent Application No. 2025-80682, filed with the Japan Patent Office on 13 May 2025, and the entirety of the said patent application is incorporated herein by reference.
[0002] This disclosure relates to capacitors.
[0003] Examples of capacitors include those comprising a solid electrolyte layer containing a conductive polymer, and those comprising an inorganic conductive layer containing a conductive inorganic compound. The solid electrolyte layer and the inorganic conductive layer are formed on the anode via a dielectric layer. A cathode layer is formed on the surface of the solid electrolyte layer and the inorganic conductive layer in order to extract electricity from the anode via the solid electrolyte layer and the inorganic conductive layer. The cathode layer contains a layer containing silver particles with high conductivity.
[0004] For example, Patent Document 1 proposes a method for manufacturing a solid electrolytic capacitor, characterized by forming a solid electrolyte made of manganese dioxide on a sintered pellet of valve-acting metal powder, then immersing the sintered pellet in a suspension of fine silver particles, removing it, and baking it at a predetermined temperature to directly form a silver layer on the solid electrolyte.
[0005] Patent document 2 proposes a solid electrolytic capacitor comprising an anode, a dielectric layer disposed on the surface of the anode, and a solid electrolyte layer disposed on the surface of the dielectric layer and made of zinc oxide having an conductivity of 1 (S / cm) or more.
[0006] Japanese Patent Publication No. 5-144684 Japanese Patent Publication No. 2017-103412
[0007] One aspect of the present disclosure relates to a capacitor comprising: an anode body having a porous portion on at least its surface; a dielectric layer covering at least a portion of the surface of the anode body; an inorganic conductive layer covering at least a portion of the surface of the dielectric layer; and a cathode layer covering at least a portion of the surface of the inorganic conductive layer, wherein the inorganic conductive layer comprises a conductive inorganic compound; the cathode layer comprises a first cathode layer in contact with the inorganic conductive layer and covering at least a portion of the surface of the inorganic conductive layer; and a second cathode layer covering at least a portion of the surface of the first cathode layer, wherein the first cathode layer comprises a first group of particles containing silver; the second cathode layer comprises a second group of particles containing silver; the average particle diameter d1 of the first group of particles is smaller than the average pore diameter P of the pores restricted by the surface of the anode body covered by the inorganic conductive layer and the dielectric layer; and the average particle diameter d2 of the second group of particles is larger than the average particle diameter d1.
[0008] According to this disclosure, it is possible to provide a capacitor comprising an inorganic conductive layer containing a conductive inorganic compound that has a low initial ESR.
[0009] This is a schematic cross-sectional view of a capacitor according to one embodiment of the present disclosure.
[0010] Novel features of the present invention are described in the appended claims, but the present invention, both in terms of structure and content, and in conjunction with other objects and features of the present invention, will be better understood by the following detailed description in conjunction with the drawings.
[0011] The present invention provides a capacitor comprising an inorganic conductive layer containing a conductive inorganic compound, which has a low initial equivalent series resistance (ESR).
[0012] In capacitors comprising an inorganic conductive layer or a solid electrolyte layer containing a conductive polymer, a cathode layer is formed on the surface of the inorganic conductive layer or solid electrolyte layer. A typical cathode layer includes a carbon layer containing conductive carbon and a silver particle-containing layer. Conventionally, the required performance could be met by interposing the carbon layer between the solid electrolyte layer or inorganic conductive layer and the silver particle-containing layer.
[0013] However, in the case of inorganic conductive layers, it has become clear that forming the cathode layers in the order of a first cathode layer containing a group of silver-containing particles with a small average particle diameter d1 and a second cathode layer containing a group of silver-containing particles with an average particle diameter d2 larger than d1 results in a lower initial ESR than forming the cathode layers in the order of a carbon layer and a silver particle-containing layer. This effect is unique to inorganic conductive layers and cannot be obtained in the case of solid electrolyte layers containing conductive polymers, even if the first and second cathode layers are formed as described above.
[0014] Technical (1) In view of the above, a capacitor according to one aspect of the present disclosure comprises an anode body having a porous portion on at least its surface, a dielectric layer covering at least a portion of the surface of the anode body, an inorganic conductive layer covering at least a portion of the surface of the dielectric layer, and a cathode layer covering at least a portion of the surface of the inorganic conductive layer. The inorganic conductive layer contains a conductive inorganic compound. The cathode layer comprises a first cathode layer in contact with the inorganic conductive layer and covering at least a portion of the surface of the inorganic conductive layer, and a second cathode layer covering at least a portion of the surface of the first cathode layer. The first cathode layer contains a first group of particles containing silver. The second cathode layer contains a second group of particles containing silver. The average particle diameter d1 of the first group of particles is smaller than the average pore diameter P of the pores restricted by the surface of the anode body covered by the inorganic conductive layer and the dielectric layer. The average particle diameter d2 of the second group of particles is larger than the average particle diameter d1.
[0015] In this disclosure, a first cathode layer is provided, which includes a first group of silver-containing particles that are in contact with the inorganic conductive layer and cover at least a portion of its surface. The average particle diameter d1 of the first group of particles is smaller than the average pore diameter P of the pores restricted by the surface of the anode body on which the inorganic conductive layer and dielectric layer are formed. As a result, the interfacial resistance between the inorganic conductive layer and the first cathode layer can be kept low. Furthermore, by forming a second cathode layer using a second group of silver-containing particles with a relatively large average particle diameter d2, the bulk resistance of the second particles can be kept low, and the interfacial resistance between the first cathode layer and the second cathode layer can be kept relatively low. Therefore, it becomes easier to extract electricity from the anode body, and the initial ESR can be significantly reduced compared to the case where a carbon layer is provided.
[0016] Furthermore, in capacitors equipped with a solid electrolyte layer containing a conductive polymer instead of an inorganic conductive layer, it is difficult to keep the initial ESR low even if a cathode layer including the first and second cathode layers described above is provided. In this case, the ESR is significantly higher compared to the case where a cathode layer including a conventional carbon layer and a second cathode layer is provided. Thus, the behavior of the initial ESR accompanying the formation of the first and second cathode layers is completely different between capacitors equipped with a solid electrolyte layer and capacitors equipped with an inorganic conductive layer.
[0017] Technology (2) In Technology (1) described above, it is preferable that each first particle constituting 90% or more by mass of the first particle group has a particle diameter of 10 nm or more and 200 nm or less. In this case, the first particles are more easily packed into the pores on the surface of the anode body covered with the inorganic conductive layer and the dielectric layer. Therefore, the interfacial resistance between the inorganic conductive layer and the first cathode layer can be further reduced.
[0018] Technology (3) In Technology (1) or Technology (2) described above, it is preferable that the average particle diameter d2 is larger than the average pore diameter P. In this case, the entry of second particles into the pores on the surface of the anode body covered with the inorganic conductive layer and the dielectric layer is suppressed. In the formed second cathode layer, a low bulk resistance of the second particles can be obtained, and the interfacial resistance between the second particles can be kept low. Therefore, it is easier to draw electricity through the first cathode layer by the second cathode layer. Such a second cathode layer is easily formed in a state that protrudes from the main surface of the anode body covered with the inorganic conductive layer and the dielectric layer.
[0019] Technology (4) In any one of the above technologies (1) to (3), it is preferable that each second particle constituting 90% or more by mass of the second particle group has a maximum diameter of 1 μm or more and 5 μm or less. In a second cathode layer containing such second particles, it is easy to obtain a low bulk resistance of the second particles, and the interfacial resistance between the second particles can be kept low. Therefore, it is easy to draw electricity through the first cathode layer by the second cathode layer.
[0020] Technology (5) In any one of the above technologies (1) to (4), the first cathode layer may not contain conductive carbon particles or may contain conductive carbon particles. Preferably, the content of conductive carbon particles in the first cathode layer is 60 volume% or less. In this case, the effect of reducing interfacial resistance by the first group of particles is easily obtained between the inorganic conductive layer and the first cathode layer.
[0021] Technology (6) In any one of the above technologies (1) to (5), it is preferable that the average thickness of the second cathode layer is greater than the average thickness of the first cathode layer. In this case, the first cathode layer reduces the interfacial resistance between the inorganic conductive layer and the first cathode layer, and the second cathode layer makes it easier to obtain higher conductivity of the cathode layer.
[0022] Technology (7) In any one of the above technologies (1) to (6), the cathode layer may further comprise a carbon layer containing conductive carbon particles interposed between the first cathode layer and the second cathode layer. Because the first cathode layer is in direct contact with the inorganic conductive layer, the interfacial resistance with the inorganic conductive layer can be kept low. Therefore, even when the cathode layer includes a carbon layer, electricity can be drawn through the first cathode layer. Thus, the initial ESR of the capacitor can be kept even lower.
[0023] Technology (8) In any one of the above technologies (1) to (7), the inorganic compound may include manganese oxide. In this case, the initial ESR of the capacitor can be further reduced.
[0024] Technology (9) In any one of the above technologies (1) to (8), the inorganic compound may also contain zinc oxide. In this case, it is preferable that the inorganic conductive layer further contains a dopant in a content of 0.5 atomic% to 15 atomic% relative to the zinc oxide. Such an inorganic conductive layer makes it easier to obtain higher conductivity. In addition, the low interfacial resistance between the inorganic conductive layer and the first cathode layer makes it possible to further reduce the initial ESR of the capacitor.
[0025] Technology (10) In the above technology (9), it is preferable that the dopant is at least one selected from the group consisting of aluminum and gallium. By using such a dopant, the conductivity of the inorganic conductive layer containing zinc oxide can be further enhanced.
[0026] Technology (11) In any one of the above technologies (1) to (10), it is preferable that the anode body is at least one selected from the group consisting of a molded body of particles containing a valve-acting metal and a sintered body of the molded body. Such an anode body has deep pores even after the dielectric layer and the inorganic conductive layer are formed. In this disclosure, the first cathode layer is formed using a first group of particles with a relatively small average particle diameter d1 in contact with the surface of the inorganic conductive layer. Therefore, even if the pore depth is deep, the interfacial resistance between the inorganic conductive layer and the first cathode layer can be reduced, and the initial ESR in the capacitor can be kept low.
[0027] Technology (12) In the above technology (11), it is preferable that the valve metal includes at least tantalum. In this case, by using tantalum, the anode body has the rigidity to withstand the grain growth of the inorganic electrolyte, and defects such as cracks in the anode can be suppressed.
[0028] The capacitors of this disclosure will be described in more detail below, including the above-mentioned technologies (1) to (12), with reference to the drawings as necessary. However, this disclosure is not limited to the examples described below. Furthermore, at least one of the above-mentioned technologies (1) to (12) may be combined with at least one of the elements described below, to the extent that it is not technically inconsistent. Each figure is schematic, and the proportions of the dimensions (e.g., thickness) of each component may differ from those of actual components.
[0029] In the following description, specific numerical values and materials may be given as examples, but other numerical values and other materials may be applied as long as they allow the invention relating to this disclosure to be implemented. In this specification, the description "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be read as "greater than or equal to numerical value A and less than or equal to numerical value B". In the following description, when lower and upper limits of numerical values relating to specific physical properties or conditions are given as examples, either of the given lower limits and either of the given upper limits may be arbitrarily combined, as long as the lower limit does not exceed the upper limit. In the following description, when examples of components or methods are listed, unless otherwise specified, only one of the listed examples may be used, or multiple of the listed examples may be used in combination.
[0030] [Capacitor] A capacitor according to one aspect of the present disclosure comprises an anode body (first electrode) having a porous portion on at least its surface, a dielectric layer covering at least a portion of the surface of the anode body, an inorganic conductive layer covering at least a portion of the surface of the dielectric layer, and a cathode layer (second electrode) covering at least a portion of the surface of the inorganic conductive layer. The inorganic conductive layer contains a conductive inorganic compound. The capacitor comprises, for example, at least one capacitor element comprising the first electrode, the second electrode, the dielectric layer, and the inorganic conductive layer. The capacitor may comprise two or more capacitor elements.
[0031] (Anode) The anode may include valve metals, alloys containing valve metals, and compounds containing valve metals. The anode may contain one of these materials or a combination of two or more. As valve metals, aluminum, tantalum, niobium, and titanium are preferably used.
[0032] The anode body has a porous portion at least on its surface. Within this porous portion, the anode body has multiple fine pits or pores. Therefore, the anode body has a surface with fine irregularities. This shape makes it easier to obtain a large surface area for the anode body, thus facilitating the acquisition of a larger capacitance.
[0033] An anode body (such as an anode foil) having a porous surface can be obtained, for example, by roughening a sheet-like metal substrate such as a metal foil. Roughening may be performed, for example, by etching. Through roughening, a porous portion is formed on the surface, and at the same time, a metal core integrated with the porous portion is formed on the inner part of the metal foil. Etching may be performed, for example, while applying an electric current, or by chemical etching.
[0034] The anode body may be a porous molded body of particles containing valve metal or a porous sintered body thereof. In both the porous molded body and the sintered body, the entire anode body typically has a porous structure. The molded body and the sintered body may be in sheet form, or they may be rectangular parallelepipeds, cubes, or similar shapes. Such an anode body may be formed, for example, by pressure molding valve metal particles into a desired shape, or by further sintering a pressure-molded body.
[0035] The anode body is preferably at least one selected from the group consisting of a molded body of particles containing a valve metal and a sintered body of the molded body. In this case, the valve metal preferably contains at least tantalum. Such an anode body has deep pores even after the dielectric layer and the inorganic conductive layer are formed. In this disclosure, the first cathode layer is formed using a first group of particles with a relatively small average particle diameter d1, in contact with the surface of the inorganic conductive layer. Therefore, even if the pore depth is deep, the interfacial resistance between the inorganic conductive layer and the first cathode layer can be reduced.
[0036] One end of a lead member (such as an anode lead terminal) is connected to the anode body. If the anode body is an anode foil, the lead member (such as an anode lead terminal) may be connected to the anode foil by welding or other means.
[0037] When the anode body is a porous molded body or sintered body, a part of a metal lead member (such as a lead wire) may be embedded in the molded body or sintered body. The lead wire is also referred to as an anode wire. The anode wire may be a metal wire. Examples of the material of the anode wire include the valve action metals mentioned above, copper, or copper alloys. A part of the anode wire is embedded in the anode body, and the remaining part protrudes outward from the end face of the anode body. The solid electrolytic capacitor may include an anode section including such an anode body and an anode wire partially embedded in the anode body.
[0038] (Dielectric Layer) The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer may be an oxide film.
[0039] For example, the dielectric layer which is an oxide film may be formed on the surface of the anode body by subjecting the anode body to a chemical conversion treatment. The chemical conversion treatment may be performed, for example, by immersing the anode body in a chemical conversion solution to anodize the surface of the anode body. As the chemical conversion solution, for example, a solution containing an acid such as phosphoric acid or adipic acid, or a salt thereof may be used. The oxide film may be formed using a vapor phase method, or may be formed by heating the anode body in an atmosphere containing oxygen to oxidize the surface.
[0040] The dielectric layer may include an oxide of a valve action metal. For example, when tantalum is used as the valve action metal, the dielectric layer contains Ta 2 O 5 . When aluminum is used as the valve action metal, the dielectric layer contains Al 2 O 3 . However, the dielectric layer is not limited to these specific examples.
[0041] (Inorganic Conductive Layer) In the capacitor of the present disclosure, the inorganic conductive layer contains a conductive inorganic compound and covers at least a part of the surface of the dielectric layer. In the present disclosure, the conductive inorganic compound includes those classified as semiconductors. The inorganic compound also includes degenerate semiconductors that can become semiconductors or electrical conductors by adding a dopant. The inorganic compound may be at least one selected from metal oxides, metal nitrides, metal carbides, metal salts, and the like.
[0042] The inorganic compound preferably contains at least a metal oxide. The metal contained in the metal oxide is, for example, a metal other than a valve action metal. Examples of such a metal include transition metals, and at least one selected from Group 11 metals to Group 14 metals of the periodic table. The metal oxide may contain oxygen vacancies. When the metal oxide contains oxygen vacancies, the conductivity of the metal oxide may be increased.
[0043] Above all, the inorganic compound preferably contains at least one selected from the group consisting of manganese oxide, zinc oxide, tin oxide, indium oxide, copper chromium oxide, and titanium oxide. Among these, the inorganic compound preferably contains at least one selected from the group consisting of manganese oxide and zinc oxide.
[0044] Examples of the manganese oxide include MnO, Mn 2 O 4 , Mn 2 O 3 , and at least one selected from the group consisting of MnO 2 . Above all, the manganese oxide preferably contains at least manganese dioxide (MnO 2 ). The manganese oxide may contain oxygen vacancies. The inorganic compound preferably contains manganese oxide. In this case, the inorganic conductive layer may further contain a dopant (such as a metal or a metal atom) as necessary.
[0045] It is also preferable that the inorganic compound contains zinc oxide (zinc oxide: such as ZnO). The zinc oxide may contain oxygen vacancies. The zinc oxide may contain zinc oxide represented by ZnO 1-x (0≦x≦0.25). Here, x may be greater than 0. In this specification, the notation "ZnO" includes zinc oxide containing oxygen vacancies unless otherwise specified.
[0046] When the inorganic compound contains zinc oxide, the inorganic conductive layer preferably further contains a dopant (such as a metal or metal atom). Examples of dopants include at least one selected from the group consisting of aluminum (Al), gallium (Ga), boron (B), and indium (In). Among these, at least one selected from the group consisting of Al and Ga is preferred. The presence of a dopant in the inorganic conductive layer enhances the conductivity of the zinc oxide. In this disclosure, the interfacial resistance between the inorganic conductive layer and the cathode layer is kept low, allowing a large amount of electricity to be drawn from the anode through the inorganic conductive layer and the cathode layer. The inorganic conductive layer containing zinc oxide may further contain fluorine.
[0047] In the inorganic conductive layer, the dopant content is preferably 0.5 atomic% to 15 atomic% relative to the inorganic compound, more preferably 0.8 atomic% to 12 atomic%, and even more preferably 1.0 atomic% to 10 atomic%. The dopant content is the atomic ratio (atomic%) of the metal element in the dopant, when the total content of the metal element in the inorganic conductive layer is taken as 100 atomic%. The total content of the metal element in the inorganic conductive layer is the sum (atomic%) of the total content of the metal element in the inorganic compound in the inorganic conductive layer and the total content of the metal element in the dopant in the inorganic conductive layer. The content of each metallic element is determined by time-of-flight secondary ion mass spectrometry (TOF-SIMS), energy-dispersive X-ray analysis based on scanning electron microscope (SEM-EDX) images, or X-ray photoelectron spectroscopy (XPS) on a cross-section of the inorganic conductive layer. For example, the SU8700 manufactured by Hitachi High-Tech Corporation is used as the SEM. Samples for analysis are formed, for example, by exposing the cross-section of the inorganic conductive layer in accordance with the procedure for preparing imaging samples described later.
[0048] The inorganic conductive layer mainly contains an inorganic compound (or, if dopants are included, the inorganic compound and dopants). The content of the inorganic compound (or the total of the inorganic compound and dopants) in the inorganic conductive layer is preferably 80% by mass or more, and more preferably 90% by mass or more. The content of the inorganic compound (or the total of the inorganic compound and dopants) in the inorganic conductive layer is 100% by mass or less. The inorganic conductive layer may also be composed only of the inorganic compound (or the inorganic compound and dopants) in the inorganic conductive layer.
[0049] The surface of the anode body covered with an inorganic conductive layer and a dielectric layer has a fine uneven surface shape depending on the shape of the surface of the porous portion of the anode body. The average pore diameter P of the pores restricted on the surface of the anode body covered with the inorganic conductive layer and dielectric layer is, for example, 100 nm or more and 2 μm or less.
[0050] The average pore diameter P can be determined from an image (hereinafter referred to as "Image A") that allows observation of the cross-sections of the inorganic conductive layer and the cathode layer. The pore diameter of each pore is the opening diameter of each pore restricted by the surface of the anode body covered with the inorganic conductive layer and the dielectric layer in "Image A". The average pore diameter P can be determined by averaging the opening diameters of a plurality of arbitrarily selected pores (for example, 50) present on the surface in "Image A".
[0051] Image A is captured, for example, by SEM. For example, the SU8700 manufactured by Hitachi High-Tech Corporation is used as the SEM. A sample for imaging is prepared, for example, by the following procedure: A capacitor or capacitor element is embedded in a curable resin and the curable resin is cured. The cured material is wet-polished or dry-polished to expose a cross-section parallel to the thickness direction of the cathode layer (a cross-section in which the layer structure of the inorganic conductive layer and the cathode layer can be confirmed). A sample for imaging is obtained by smoothing the exposed cross-section with mechanical polishing or ion milling. In this specification, when observing the cross-section of a capacitor (including the cross-section of the components of the capacitor), a sample can be prepared in accordance with the above, an SEM image can be taken, and the observation can be made based on the taken image.
[0052] The inorganic conductive layer may be formed by a liquid-phase method or a gas-phase method. In the gas-phase method, the inorganic conductive layer may be formed using at least one selected from the group consisting of sputtering, vapor deposition, chemical vapor deposition (CVD), and atomic layer deposition (ALD).
[0053] In the liquid-phase method, an inorganic conductive layer can be formed by applying a solution containing, for example, an inorganic compound (or its precursor) and, if necessary, a dopant (or its precursor) to an anode covered with a dielectric layer and heating it. The solution used may be, for example, a metal salt containing a metal element contained in the inorganic compound, or a metal salt containing a metal element contained in the dopant, dissolved in a solvent.
[0054] The solution may further contain additives other than those listed above. For example, the solution may contain components that enhance the solubility of inorganic compounds (or their precursors) or dopants (or their precursors). Examples of such components include at least one selected from the group consisting of basic components (such as monoethanolamine, diethanolamine, triethanolamine, and ethylenediamine), mercaptopurines, and acetylacetone. From the viewpoint of improving the wettability of the solution to the surface of the dielectric layer, the solution may contain surfactants. As the solvent, organic solvents, water, or mixtures thereof are used. The inorganic conductive layer may contain components derived from the additives.
[0055] The concentration of each component in the solution is selected as appropriate. For example, the concentration of the inorganic compound or its precursor in the solution may be 0.01 mol / L or more and 10 mol / L or less, or 0.1 mol / L or more and 5 mol / L or less. The concentration of the dopant or its precursor is adjusted so that the dopant content (atomic %) relative to the inorganic compound is within the above range. The concentration of the component that enhances the solubility of the inorganic compound (or its precursor) or dopant (or its precursor) can be selected according to the type of component, the solubility and concentration of the inorganic compound (or its precursor) or dopant (or its precursor), etc., and may be, for example, 0.01 mol / L or more and 10 mol / L or less.
[0056] When using precursors of inorganic compounds or dopants, heating decomposes the precursor (such as a salt) to produce the inorganic compound or dopant. Depending on the type of inorganic compound, heating may be carried out in the atmosphere, nitrogen gas, or water vapor. For example, heating in an atmosphere containing oxygen atoms, such as air or water vapor, makes it easier to obtain inorganic oxides or inorganic oxides with added dopants. For example, heating may be carried out in a heated water vapor atmosphere. The heating conditions (temperature, time, pressure, etc.) are selected according to the components contained in the solution. The heating temperature may be, for example, 150°C to 400°C, or 200°C to 300°C. The heating time may be 1 minute to 30 minutes, or 5 minutes to 15 minutes.
[0057] If necessary, the process of applying the solution to the anode covered with the dielectric layer and heating it may be repeated. The thickness of the inorganic conductive layer may be adjusted by adjusting the number of repetitions.
[0058] If necessary, further heat treatment may be performed after the above heating. This heat treatment is carried out at a higher temperature than the above heating temperature. By performing heat treatment at a higher temperature, the conductivity of the inorganic conductive layer can be improved. The heat treatment temperature in the heat treatment process may be 250°C or higher and 500°C or lower. In that case, the heat treatment time in the heat treatment process may be 10 minutes or higher and 5 hours or lower. The atmosphere for the heat treatment can be found in the description of heating above. Other conditions are adjusted, for example, depending on the type of inorganic compound or dopant.
[0059] (Cathode Layer) The cathode layer covers at least a portion of the surface of the inorganic conductive layer. In this disclosure, the cathode layer includes at least a first cathode layer and a second cathode layer. The first cathode layer is in contact with the inorganic conductive layer and covers at least a portion of the surface of the inorganic conductive layer. The second cathode layer may directly or indirectly cover at least a portion of the surface of the first cathode layer. The cathode layer may further include an intermediate cathode layer interposed between the first cathode layer and the second cathode layer. The second cathode layer is in contact with the surface of the first cathode layer or the intermediate cathode layer and may cover at least a portion of this surface.
[0060] (First Cathode Layer) The first cathode layer contains a first group of particles containing silver. The average particle diameter d1 of the first group of particles is smaller than the average pore diameter P of the surface of the anode body covered with an inorganic conductive layer and a dielectric layer. Therefore, the first group of particles containing highly conductive silver is densely packed into the pores of the surface of the anode body covered with an inorganic conductive layer and a dielectric layer. Furthermore, in this disclosure, the first cathode layer covering at least a portion of the surface of the inorganic conductive layer is in contact with the inorganic conductive layer. These features reduce the interfacial resistance between the inorganic conductive layer and the first cathode layer.
[0061] When the first cathode layer and the inorganic conductive layer are in contact, it means that the inorganic conductive layer and the first cathode layer are in direct contact. It is preferable that no other layers, such as conventional carbon layers containing conductive carbon, are interposed between the inorganic conductive layer and the first cathode layer.
[0062] Each first particle constituting the first particle group contains silver. The first particle may be a silver particle or a silver alloy particle. The first particle group may consist of silver particles and silver alloy particles. The silver particles may contain impurities that are inevitably present.
[0063] Each first particle constituting the first particle group is, for example, a silver-containing particle with a particle diameter of 200 nm or less. The particle diameter of the first particles is the maximum diameter of each first particle in an image in which the cross-section of the first cathode layer can be observed (for example, "Image A" above). In addition to facilitating high-density filling of the pores with first particles, it is preferable that each first particle constituting 90% or more by mass of the first particle group has a particle diameter of 10 nm or more and 200 nm or less, from the viewpoint of facilitating high-density filling of the pores and facilitating higher conductivity of the first cathode layer.
[0064] In an image in which at least the cross-section of the first cathode layer can be observed (for example, "Image A" above), a plurality of (for example, 50) first particles are arbitrarily selected, and the average particle diameter d1 is determined by averaging the particle diameters of each first particle.
[0065] The first cathode layer may contain conductive particles other than the first particles. Examples of such conductive particles include silver-containing particles and conductive carbon particles. Silver-containing particles are silver-containing particles having a particle size outside the particle size range of the first particle group. Examples of conductive carbon particles include graphite particles, carbon black, and amorphous carbon particles. The first cathode layer may contain one type of conductive particle other than the first particles, or a combination of two or more types.
[0066] From the viewpoint of easily obtaining a lower ESR of the capacitor, the volume ratio of the first particles is preferably 40% or more by volume of the total particles (specifically conductive particles) contained in the first cathode layer, more preferably 60% or more by volume, and even more preferably 80% or more by volume. The volume ratio of the first particles is 100% or less by volume of the total particles (specifically conductive particles) contained in the first cathode layer.
[0067] From the viewpoint of easily obtaining a lower ESR of the capacitor, it is also preferable that the first cathode layer does not contain conductive carbon particles. Similarly, when the first cathode layer contains conductive carbon particles, the content (volume ratio) of conductive carbon particles in the first cathode layer is preferably 60 volume% or less, more preferably 40 volume% or less, and even more preferably 20 volume% or less.
[0068] The volume ratio of the first particles can be determined, for example, from an SEM image (such as "Image A") that allows observation of a cross-section of the first cathode layer. From the cross-sectional image, a plurality of first particles (for example, 50 particles) are arbitrarily selected in a region of a predetermined size within the first cathode layer (for example, a rectangular region of 3 μm vertically and 4 μm horizontally), and the total area S1 of the cross-sections of these first particles is determined. The total area S0 of all particles contained within the above region (for example, all conductive particles) is determined. Then, the area ratio (area %) of the first particles is calculated from S1 / (S1+S0) × 100. This area ratio is taken as the volume ratio (volume %) of the first particle group in the first cathode layer. The volume ratio of conductive carbon particles can also be determined in a similar manner to the volume ratio of the first particles.
[0069] The average thickness of the first cathode layer is preferably 0.1 μm to 10 μm, more preferably 0.1 μm to 5.0 μm, and even more preferably 0.2 μm to 3.0 μm. When the average thickness of the first cathode layer is within this range, the interfacial resistance between the inorganic conductive layer and the first cathode layer can be further reduced, and high conductivity of the first cathode layer can be easily obtained.
[0070] The average thickness of the first cathode layer can be determined, for example, from an SEM image (such as "Image A") that allows observation of a cross-section of the first cathode layer. The average thickness is obtained by determining the thickness of the first cathode layer at any multiple locations (for example, 10 locations) in the cross-sectional image and averaging the results.
[0071] Each cathode layer, such as the first cathode layer, second cathode layer, and intermediate cathode layer, is distinguished by the particle size and state of conductive particles in an SEM image (e.g., "Image A") that allows observation of the cross-section of the cathode layer. For example, the first cathode layer and the second cathode layer are distinguished when comparing the abundance ratio of silver-containing particles, specifically first particles with a particle size of 200 nm or less and second particles with a particle size of 1 μm or more, and the layer that is in contact with the inorganic conductive layer and has a larger volume ratio of first particles is defined as the first cathode layer. For particle identification in each cathode layer, for example, TOF-SIMS may be used for samples in which each cathode layer is exposed, or SEM-EDX or XPS based on SEM images (e.g., "Image A") may be used.
[0072] (Second Cathode Layer) The second cathode layer contains a second group of silver-containing particles. The average particle diameter d2 of the second group of particles is larger than the average particle diameter d1 of the first group of particles in the first cathode layer. Because the particle diameter of the second particles constituting the second group of particles is large, the bulk resistance of the second particles and the interfacial resistance between the second particles are kept low. High conductivity of the second cathode layer is obtained, thereby ensuring high conductivity of the cathode layer.
[0073] The average particle diameter d2 of the second particle group is larger than the average pore diameter P of the surface of the anode body covered with the dielectric layer and the inorganic conductive layer. This suppresses the filling of the pores of the second particles into the surface of the anode body covered with the dielectric layer and the inorganic conductive layer, and further maintains a low interfacial resistance between the inorganic conductive layer and the first cathode layer.
[0074] Each second particle constituting the second particle group contains silver. The second particles may be silver particles or silver alloy particles. The second particle group may consist of silver particles and silver alloy particles. The silver particles may contain impurities that are inevitably present.
[0075] The shape of the second particle is not particularly limited and may be spherical, ellipsoidal, flake-shaped, columnar, or the like.
[0076] Each second particle constituting the second particle group is, for example, a silver-containing particle with a particle diameter of 1 μm or more. The particle diameter of the second particles is the maximum diameter of each second particle in an image in which the cross-section of the second cathode layer can be observed (for example, the image "Image A" above). From the viewpoint of ensuring higher conductivity and facilitating the extraction of electricity by the second cathode layer through the inorganic conductive layer and the first cathode layer, it is preferable that each second particle constituting 90% or more by mass of the second particle group has a particle diameter of 1 μm or more and 5 μm or less.
[0077] From the viewpoint of easily obtaining higher conductivity in the second cathode layer, the volume ratio of the second particles is preferably 60 volume% or more of the total particles (specifically conductive particles) contained in the second cathode layer, more preferably 80 volume% or more, and even more preferably 90 volume% or more. The volume ratio of the second particles is 100 volume% or less of the total particles (specifically conductive particles) contained in the second cathode layer.
[0078] The volume ratio of the second particle is determined, for example, from an SEM image (such as "Image A") that allows observation of the cross-section of the second cathode layer, similar to the case of the volume ratio of the first particle in the first cathode layer.
[0079] The average thickness of the second cathode layer is preferably greater than the average thickness of the first cathode layer. This is because the first cathode layer ensures high current collection between the inorganic conductive layer and the first cathode layer, while the second cathode layer ensures higher conductivity for the entire cathode layer.
[0080] The average thickness of the second cathode layer may be 5 μm or more and 20 μm or less, or 8 μm or more and 15 μm or less.
[0081] The average thickness of the second cathode layer is determined in the same way as the average thickness of the first cathode layer, for example, from an SEM image (such as "Image A") that allows observation of the cross-section of the second cathode layer.
[0082] (Intermediate Cathode Layer) The intermediate cathode layer is interposed between the first cathode layer and the second cathode layer. The intermediate cathode layer is a cathode layer different from both the first and second cathode layers. The intermediate cathode layer contains conductive particles. Examples of conductive particles include conductive carbon particles and metal particles other than those in the first and second particle groups. The intermediate cathode layer may contain one type of conductive particle, or two or more types.
[0083] The intermediate cathode layer is preferably a carbon layer containing conductive carbon particles. Because the first cathode layer is in contact with the inorganic conductive layer, the interfacial resistance between the inorganic conductive layer and the cathode layer can be kept low. Therefore, even if the cathode layer contains a carbon layer, a large amount of electricity can be drawn, and the initial ESR can be kept low.
[0084] Examples of conductive carbon particles include graphite particles, carbon black, and amorphous carbon particles. The carbon layer may contain one type of conductive carbon particle, or a combination of two or more types. The carbon layer may also contain at least graphite particles.
[0085] (Formation of each cathode layer) The first cathode layer, the second cathode layer, and the intermediate cathode layer are each formed by applying a paste containing conductive particles contained in each cathode layer to the surface of a base layer and allowing it to solidify. The paste containing conductive particles is prepared, for example, by dispersing the conductive particles in a liquid dispersion medium. Examples of dispersion mediums include organic media, water, or mixtures thereof.
[0086] The paste may optionally contain a binder (such as a resin binder). The resin binder may be a thermosetting resin (or a composition thereof) or a thermoplastic resin (or a composition thereof).
[0087] The paste is applied to the substrate layer, for example, by a known coating method. The paste may also be applied to the substrate layer by means of coating or dipping, for example.
[0088] The paste coating is solidified by drying or heating, forming each cathode layer. The coating may also be solidified by drying, which removes volatile components such as liquid dispersion media. Alternatively, the coating may be solidified by solidifying the binder contained in the paste. Drying may be performed by heating, hot air drying, or reduced pressure drying.
[0089] (Other) Capacitors may be either chip type or multilayer type. For example, a capacitor may include two or more stacked capacitor elements. The configuration of the capacitor elements is selected, for example, depending on the type of capacitor.
[0090] In a capacitor element, one end of a cathode lead terminal is electrically connected to the cathode layer (more specifically, the second cathode layer). The cathode lead terminal is joined to the second cathode layer, for example, by applying a conductive adhesive to the second cathode layer and bonding it to the second cathode layer via this conductive adhesive. One end of an anode lead terminal is electrically connected to the anode body or anode wire. The other end of each lead terminal is drawn out from the resin casing or case. The other end of each terminal exposed from the resin casing or case is used for soldering to the substrate on which the capacitor is to be mounted, etc.
[0091] The capacitor element is sealed using a resin casing or case. For example, the capacitor element and the resin material for the casing (e.g., uncured thermosetting resin and filler) may be placed in a mold, and the capacitor element may be sealed with the resin casing by a transfer molding method, compression molding method, or the like. In this case, the other end of each lead terminal drawn out from the capacitor element is exposed from the mold. Examples of thermosetting resins include epoxy resin.
[0092] Alternatively, a capacitor may be formed by housing the capacitor elements in a bottomed case such that the other end of each lead terminal is located on the opening side of the bottomed case, and then sealing the opening of the bottomed case with a sealing material. As the material for the bottomed case, metals such as aluminum, stainless steel, copper, iron, brass, or alloys thereof can be used.
[0093] The capacitors disclosed herein have a low initial ESR and can be used in a variety of applications.
[0094] Figure 1 is a schematic cross-sectional view of a capacitor according to one embodiment of the present disclosure. The capacitor 10 includes an anode wire 110, an anode body 111, a dielectric layer 112, an inorganic conductive layer 120 containing an inorganic compound, and a cathode layer 131. The cathode layer 131 includes a first cathode layer 131a and a second cathode layer 131b, which are stacked in order from the inorganic conductive layer 120 side. The capacitor 10 further includes an anode wire 110, an anode lead terminal 141, a cathode lead terminal 142, a conductive adhesive 143, and a resin casing 144. One end of the anode wire 110 is embedded in the anode body 111. The other end of the anode wire 110 is connected to the anode lead terminal 141. The cathode lead terminal 142 is connected to the cathode layer 131 via the conductive adhesive 143. The conductive adhesive 143 may be formed from a metal paste (such as silver paste). The anode 111, dielectric layer 112, inorganic conductive layer 120, and cathode layer 131 constitute a capacitor element. The capacitor element, a portion of the anode lead terminal 141, and a portion of the cathode lead terminal 142 are covered by a resin casing 144.
[0095] In this disclosure, the first cathode layer 131a in contact with the inorganic conductive layer 120 includes a first group of particles containing silver. The second cathode layer 131b covering at least a portion of the surface of the first cathode layer 131a includes a second group of particles containing silver. The average particle diameter d1 of the first group of particles is smaller than the average pore diameter P of the surface of the anode body 111 covered with the inorganic conductive layer 120 and the dielectric layer 112. In addition, the average particle diameter d2 of the second group of particles is larger than the average particle diameter d1. These features allow the interfacial resistance between the inorganic conductive layer 120 and the first cathode layer 131a to be kept low, and the first cathode layer 131a and the second cathode layer 131b provide high conductivity to the cathode layer 131. Therefore, the initial ESR of the capacitor can be kept low. Between the first cathode layer 131a and the second cathode layer 131b, an intermediate cathode layer (not shown) containing a conductive material may be provided as needed. An example of an intermediate cathode layer is a carbon layer containing conductive carbon particles.
[0096] [Examples] The present disclosure will be described below in detail based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0097] Examples 1-14 and Comparative Examples 1-14 Capacitors for the examples and comparative examples were fabricated using the following procedure.
[0098] (1) Formation of Tantalum Sintered Body and Dielectric Layer Tantalum powder (average particle size 1.9 μm or more and 2.5 μm or less) was filled into a predetermined molding die, and one end of an anode wire was embedded in the tantalum powder. A tantalum wire was used as the anode wire. Subsequently, a rectangular parallelepiped molded body was obtained by pressure molding the tantalum powder.
[0099] The resulting molded body was sintered under reduced pressure at a temperature in the range of 1300°C to 1400°C. In this way, a porous anode body (tantalum sintered body) in which a portion of the anode wire was embedded was obtained.
[0100] Next, a dielectric layer composed of tantalum oxide was formed on the surface of the tantalum sintered body by chemical conversion treatment (anodic oxidation). A silane coupling agent was then applied to the surface of the tantalum sintered body covered with the dielectric layer.
[0101] (2) Formation of an inorganic conductive layer An inorganic conductive layer containing the materials shown in the table (inorganic compounds and dopants as necessary) was formed on the surface of the tantalum sintered body covered with a dielectric layer obtained in (1) above, according to the following procedure.
[0102] First, a tantalum sintered body covered with a dielectric layer was immersed in a solution containing an inorganic compound precursor and then removed. The tantalum sintered body with the solution adhering to it was then heat-treated. The immersion and heat treatment were repeated as needed. In this way, a tantalum sintered body (device) covered with an inorganic conductive layer and a dielectric layer was obtained.
[0103] Solutions containing precursors of inorganic compounds were prepared by dissolving a salt containing the metal element (Zn, Mn, etc.) present in the inorganic compound (precursor of the inorganic compound) and, if necessary, a salt containing the metal element (Ga, Al, etc.) present in the dopant (precursor of the dopant) in a solvent.
[0104] For example, when forming an inorganic conductive layer containing ZnO as an inorganic compound and Ga as a dopant, zinc acetate dihydrate and gallium nitrate n hydrate were used as precursors. When forming an inorganic conductive layer containing ZnO as an inorganic compound and Al as a dopant, zinc acetate dihydrate and aluminum nitrate nonahydrate were used as precursors. In addition, 2-methoxyethanol was used as the solvent, and monoethanolamine and, if necessary, a surfactant for improving wettability were added to the solution. In the solution, the concentration of the inorganic compound precursor was 1.0 mol / L, and the concentration of monoethanolamine was 1.0 mol / L. The concentration of the dopant precursor was determined so that the dopant content (atomic %) obtained by the procedure described above was the value shown in the table. Furthermore, the tantalum sintered body covered with the dielectric layer was immersed in the above solution for 3 minutes, and then heat-treated at 260°C for 10 minutes. This immersion and heating was repeated 10 times. Next, heat treatment was performed at 400°C for 1 hour.
[0105] Also, as an inorganic compound, MnO 2 When forming an inorganic conductive layer containing the inorganic compound, manganese nitrate hexahydrate was used as the precursor of the inorganic compound, and water (distilled water) was used as the solvent. The concentration of the inorganic compound precursor in the obtained manganese nitrate aqueous solution was controlled by its specific gravity. The specific gravity of the manganese nitrate aqueous solution was between 1.2 and 1.9. A tantalum sintered body covered with a dielectric layer was immersed in the manganese nitrate aqueous solution for 3 minutes and then removed. The tantalum sintered body with the aqueous solution attached was heat-treated in a superheated steam atmosphere at a temperature in the range of 200°C to 260°C.
[0106] (3) Formation of the cathode layer A cathode layer with the layer configuration shown in the table was formed on the inorganic conductive layer of the element using a conductive paste containing the conductive particles shown in the table, following the procedure below. More specifically, the first cathode layer was formed by applying a conductive paste for forming the first cathode layer onto the inorganic conductive layer and heating it. When forming the second cathode layer or the intermediate cathode layer on the first cathode layer, each layer was formed by applying a conductive paste for forming these cathode layers and heating the coating. When forming the second cathode layer on the intermediate cathode layer, the second cathode layer was formed in accordance with the above. The thickness of each cathode layer after heating was adjusted by adjusting the number of times the conductive paste was applied so that it matched the thickness shown in the table. In this way, a capacitor comprising an anode, a dielectric layer, an inorganic conductive layer, and a cathode layer was fabricated. A total of 20 capacitors were fabricated for each example using the same procedure.
[0107] For the formation of the cathode layer, silver paste (number 1), silver paste (number 2), silver paste (number 3), and / or carbon paste were used. Each paste was heated under the following conditions to form each cathode layer.
[0108] The first silver paste was prepared by dispersing silver particles (first particle group) with a particle size (maximum diameter) of 10 nm to 200 nm in a liquid organic medium (ethylene glycol). The coating film of the first silver paste was heated and dried at a temperature of 200°C to 220°C for 2 hours.
[0109] The second silver paste contains silver particles (second particle group) with a particle size (maximum diameter) of 0.5 μm to 5 μm and a thermosetting resin. The coating film of the second silver paste was solidified by heating at a temperature of 200°C to 220°C for 10 minutes.
[0110] The carbon paste contains graphite particles with a particle size (maximum diameter) of 30 nm to 70 nm and a liquid dispersion medium. The carbon paste coating was heat-dried at a temperature of 190°C to 210°C for 10 minutes.
[0111] The third silver paste was prepared by dispersing silver particles (first particle group) with a particle size (maximum diameter) of 10 nm to 200 nm and graphite particles (maximum diameter) of 30 nm to 70 nm in a liquid organic medium. The volume ratio of the first particle group to the graphite particles was 4:6. The coating film of the third silver paste was heated and dried at a temperature of 200°C to 220°C for 2 hours.
[0112] (4) Evaluation (4-1) Average particle diameter and average pore diameter From the cross-sectional image of the capacitor, the average particle diameter d1 of the first particle group was determined for the first cathode layer or second cathode layer containing the first particle group using the procedure described above. The average particle diameter d2 of the second particle group in the first cathode layer or second cathode layer containing the second particle group was determined using the same procedure. As a result, the average particle diameter d1 of the first particle group was approximately 70 nm, and the average particle diameter d2 of the second particle group was approximately 3 μm.
[0113] From the cross-sectional image of the capacitor, the average pore diameter P on the surface of the tantalum sintered body covered with an inorganic conductive layer and a dielectric layer was determined using the procedure described above. As a result, the average pore diameter P in the example was approximately 200 nm to 400 nm.
[0114] (4-2) Initial ESR Under conditions of 20°C, the initial ESR (mΩ) of each capacitor at a frequency of 100 kHz was measured using a four-terminal LCR meter (Keysight Technologies, E4980A) with a voltage of 500 mV (DC bias: 0). The average value (mΩ) for 20 capacitors was then calculated. The average ESR of each example is expressed as a relative value to the average ESR of a comparative example capacitor, which has a common conductive layer composition and includes a cathode layer composed of a carbon layer as the first cathode layer and a second cathode layer containing a second group of particles.
[0115] Comparative Examples 15 and 16: Capacitors for Comparative Examples 15 and 16 were fabricated in the same manner as in Example 1 and Comparative Example 1, except that a solid electrolyte layer made of a conductive polymer was formed instead of an inorganic conductive layer.
[0116] The solid electrolyte layer was formed by the following procedure: A tantalum sintered body covered with a dielectric layer (after treatment with a silane coupling agent), obtained by the same procedure as in Example 1 or Comparative Example 1 (1), was immersed in a liquid dispersion containing a conductive polymer. The removed tantalum sintered body was dried. This immersion and drying process was repeated several times to form the solid electrolyte layer.
[0117] A polymerization solution was prepared by mixing 3,4-ethylenedioxythiophene, p-iron(III) toluenesulfonate, and 1-butanol. After immersing the anode in the polymerization solution, the anode was removed from the polymerization solution and heat-treated in the atmosphere. In this case, p-iron(III) toluenesulfonate functions as an oxidizing agent. In this way, a conductive polymer layer containing poly(3,4-ethylenedioxythiophene) (PEDOT) was formed on the dielectric layer. The formation of the conductive polymer layer described above was repeated multiple times to form a solid electrolyte layer consisting of a conductive polymer layer of a predetermined thickness.
[0118] The evaluation results are shown in Tables 1A to 4A and Tables 1B to 4B. In the tables, E1 to E14 are examples, and C1 to C16 are comparative examples.
[0119]
[0120]
[0121] As shown in Tables 1A and 1B, the initial ESR was significantly reduced in the example containing a first group of silver particles ranging from 10 nm to 200 nm, compared to the comparative example in which the first cathode layer in contact with the inorganic conductive layer is a carbon layer.
[0122]
[0123]
[0124] As shown in Tables 2A and 2B, in C6 to C8, where the cathode layer on the surface of the inorganic conductive layer was formed only with a first cathode layer containing a first group of silver particles, the initial ESR increased significantly compared to C2, where the first cathode layer in contact with the inorganic conductive layer was a carbon layer. Similarly, in C9, where the cathode layer was formed only with a first cathode layer using a second group of silver particles with a particle size of 0.5 μm to 5.0 μm, the initial ESR also increased significantly compared to C2. In contrast, in E2, E6, and E7, where the same first cathode layer as C6 to C8 and a second cathode layer containing a second group of silver particles were formed, the initial ESR was significantly reduced compared to C2. In E2, E6, and E7, the initial ESR was also significantly reduced compared to C6 to C8, where the thickness of the first cathode layer was the same.
[0125] When the cathode layer is composed of a first cathode layer containing a first particle group and a second cathode layer containing a second particle group, a reduction in initial ESR was observed even when the first cathode layer contained conductive carbon (comparison between C2 and E8). Furthermore, when the cathode layer consists of a first cathode layer containing a first particle group and a second cathode layer containing a second particle group, the initial ESR was significantly reduced even when an intermediate cathode layer containing conductive carbon was formed between these cathode layers (comparison between C2 and E9).
[0126]
[0127]
[0128] When the dopant of the inorganic conductive layer was Al, the reduction effect on the initial ESR was confirmed, similar to the case with Ga (comparison between Tables 1A and 1B and Tables 3A and 3B).
[0129]
[0130]
[0131] As shown in Tables 4A and 4B, the inorganic conductive layer is MnO 2 When these were included, a reduction in initial ESR was obtained, similar to when ZnO and dopants were included (comparison of E14 and C14 with E1 and C1 in Tables 1A and 1B).
[0132] When the conductive layer is a solid electrolyte layer containing a conductive polymer, even if a first cathode layer containing a first group of silver particles and a second cathode layer containing a second group of silver particles are provided, the initial ESR increases significantly compared to when the first cathode layer is a carbon layer (comparison of C15 and C16). Comparing C15 and C16 with E1 and C1 in Tables 1A and 1B, it can be said that the behavior of the initial ESR is completely different depending on the composition of the first cathode layer, whether the conductive layer is an inorganic conductive layer containing an inorganic compound or a solid electrolyte layer containing a conductive polymer.
[0133] Although the present invention has been described in relation to preferred embodiments at present, such disclosure should not be interpreted restrictively. Various modifications and alterations will undoubtedly become apparent to those skilled in the art in the field to which the invention pertains by reading the above disclosure. Accordingly, the appended claims should be interpreted as encompassing all modifications and alterations without departing from the true spirit and scope of the invention.
[0134] 10: Capacitor 110: Anode wire 111: Anode body 112: Dielectric layer 120: Inorganic conductive layer 131: Cathode layer 131a: First cathode layer 131b: Second cathode layer 141: Anode lead terminal 142: Cathode lead terminal 143: Conductive adhesive 144: Resin casing
Claims
1. A capacitor comprising: an anode body having a porous portion on at least its surface; a dielectric layer covering at least a portion of the surface of the anode body; an inorganic conductive layer covering at least a portion of the surface of the dielectric layer; and a cathode layer covering at least a portion of the surface of the inorganic conductive layer, wherein the inorganic conductive layer contains a conductive inorganic compound; the cathode layer comprises a first cathode layer in contact with the inorganic conductive layer and covering at least a portion of the surface of the inorganic conductive layer; and a second cathode layer covering at least a portion of the surface of the first cathode layer, wherein the first cathode layer contains a first group of particles containing silver; the second cathode layer contains a second group of particles containing silver; the average particle diameter d1 of the first group of particles is smaller than the average pore diameter P of the pores restricted by the surface of the anode body covered by the inorganic conductive layer and the dielectric layer; and the average particle diameter d2 of the second group of particles is larger than the average particle diameter d1.
2. The capacitor according to claim 1, wherein each first particle constituting 90% or more by mass of the first particle group has a particle diameter of 10 nm or more and 200 nm or less.
3. The capacitor according to claim 1 or 2, wherein the average particle diameter d2 is larger than the average pore diameter P.
4. The capacitor according to claim 1 or 2, wherein each second particle constituting 90% or more by mass of the second particle group has a maximum diameter of 1 μm or more and 5 μm or less.
5. The capacitor according to claim 1 or 2, wherein the first cathode layer does not contain conductive carbon particles, or contains conductive carbon particles, and the content of conductive carbon particles in the first cathode layer is 60 volume% or less.
6. The capacitor according to claim 1 or 2, wherein the average thickness of the second cathode layer is greater than the average thickness of the first cathode layer.
7. The capacitor according to claim 1 or 2, wherein the cathode layer further comprises a carbon layer containing conductive carbon particles interposed between the first cathode layer and the second cathode layer.
8. The capacitor according to claim 1 or 2, wherein the inorganic compound comprises manganese oxide.
9. The capacitor according to claim 1 or 2, wherein the inorganic compound comprises zinc oxide, and the inorganic conductive layer further comprises a dopant in a content of 0.5 atomic% to 15 atomic% relative to the zinc oxide.
10. The capacitor according to claim 9, wherein the dopant is at least one selected from the group consisting of aluminum and gallium.
11. The anode body is at least one selected from the group consisting of a molded body of particles containing a valve-acting metal and a sintered body of the molded body, the capacitor according to claim 1 or 2.
12. The capacitor according to claim 11, wherein the valve-acting metal includes at least tantalum.