Fire spread prevention material, assembled battery, and automobile

A fire-spread prevention material with an inorganic fiber substrate and low-emissivity metal films addresses the inadequacies of existing materials by enhancing thermal insulation and fire prevention in lithium-ion battery packs, ensuring safety and stability.

WO2026239869A1PCT designated stage Publication Date: 2026-11-19DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015949
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-04-21
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing fire-spread prevention materials for lithium-ion battery packs do not adequately prevent fire spread and require further improvement in thermal insulation and fire prevention properties.

Method used

A fire-spread prevention material comprising an inorganic fiber substrate with sodium silicate and metal films on both sides, where the emissivity of the metal films is lower than the substrate, enhancing radiant heat transfer suppression and thermal insulation.

Benefits of technology

The material effectively prevents fire spread by suppressing radiant heat transfer and promoting heat dissipation, maintaining flexibility and stability during battery cell expansion, and ensuring safe operation of battery packs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015949_19112026_PF_FP_ABST
    Figure JP2026015949_19112026_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] To provide: a fire spread prevention material having improved fire spread prevention properties; an assembled battery using said fire spread prevention material; and an automobile comprising said assembled battery. [Solution] One aspect of the present invention provides a fire spread prevention material, said fire spread prevention material comprising: a fire spread prevention material body that is provided with an inorganic fiber base material which contains inorganic fibers and sodium silicate which is supported on the inorganic fiber base material; and two metal films that are respectively provided to both sides of the fire spread prevention material body so as to be opposite from each other with the fire spread prevention material body therebetween, wherein the emissivity of each of the metal films is lower than the emissivity of the fire spread prevention material body.
Need to check novelty before this filing date? Find Prior Art

Description

Fire-resistant materials, battery packs, and automobiles

[0001] This invention relates to fire-preventing materials, battery packs, and automobiles.

[0002] With the increasing prevalence of electric vehicles, development of automotive battery packs and the battery cells used in them is progressing. Among automotive battery packs, those using lithium-ion battery (LiB) cells, which have particularly high energy density, carry a risk of malfunctions such as thermal runaway. Therefore, technologies to improve the safety of battery cells are being developed.

[0003] For example, Patent Document 1 proposes a heat-absorbing sheet used to prevent rapid temperature rise and thermal runaway (thermal escape) in lithium-ion batteries due to internal short circuits, etc. However, such a heat-absorbing sheet does not necessarily provide sufficient fire spread prevention.

[0004] Therefore, the specified SiO 2 / Na 2 A fire-spread prevention material has been proposed that comprises a layer containing sodium silicate in a molar ratio of 0 and a layer containing inorganic fibers and having a porous structure (see Patent Document 2). However, even with such a fire-spread prevention material, further improvement in fire-spread prevention performance is required.

[0005] Japanese Patent Publication No. 2010-53196, International Publication No. 2022 / 270359

[0006] In view of the above circumstances, the present invention aims to provide a fire-resistant material having superior fire-spread prevention properties, a battery pack using this fire-resistant material, and an automobile equipped with this battery pack.

[0007] According to one aspect of the present invention, a fire-spread prevention material is provided, comprising a fire-spread prevention material body comprising an inorganic fiber substrate containing inorganic fibers and sodium silicate supported on the inorganic fiber substrate, and two metal films provided on both sides of the fire-spread prevention material body, facing each other via the fire-spread prevention material body, wherein the emissivity of each metal film is less than the emissivity of the fire-spread prevention material body.

[0008] According to this embodiment, a fire-resistant material with superior fire-spread prevention properties can be provided.

[0009] Figure 1 is a schematic side view showing the configuration of the fire spread prevention material of this embodiment. Figure 2 is a schematic diagram showing the state of water molecules present in sodium silicate. Figure 3 is a schematic cross-sectional view showing the configuration of the fire spread prevention material body. Figure 4 is a schematic cross-sectional view showing the configuration of the fire spread prevention material body. Figure 5(a) is a schematic plan view showing an embodiment of the fire spread prevention material equipped with an outer casing. Figure 5(b) is a schematic side view and an enlarged view showing a cross-section of the end of an embodiment of the fire spread prevention material equipped with an outer casing. Figure 6 is a schematic diagram showing the configuration of a battery cell assembly for simulated combustion testing.

[0010] Embodiments of the present invention will be described below with reference to the drawings. The various features shown in the embodiments below can be combined with each other. In this specification, the content of Y in X means the proportion (mass%) of Y relative to the total mass of X, and the water content of sodium silicate means the proportion (mass%) of water relative to the total mass of sodium silicate.

[0011] Figure 1 is a schematic side view showing the configuration of the fire-spread prevention material of this embodiment. Figure 2 is a schematic diagram showing the state of water molecules present in sodium silicate. Figures 3 and 4 are schematic cross-sectional views showing the configuration of the fire-spread prevention material body, respectively. The fire-spread prevention material of this embodiment is used by being placed between two adjacent battery cells in a battery pack comprising two or more battery cells. Here, the fire-spread prevention material is required to have thermal insulation properties (fire-spread prevention properties) that suppress heat transfer to adjacent battery cells in the event of an abnormality.

[0012] The fire-spread prevention material 1 shown in Figure 1 comprises a fire-spread prevention material body 11 comprising an inorganic fiber base material containing inorganic fibers and sodium silicate supported on the inorganic fiber base material, and two metal films 12 provided on both sides of the fire-spread prevention material body 11, facing each other via the fire-spread prevention material body 11. The emissivity of each metal film 12 is set to be lower than that of the fire-spread prevention material body 11. With this configuration, the metal films 12 reflect heat from the outside, that is, the radiant heat transfer by the metal films 12 is suppressed, thereby preventing the fire-spread prevention material body 11 from being heated to a high degree. As a result, the heat insulation (heat insulation effect) of the fire-spread prevention material 1 is effectively exhibited.

[0013] Here, the emissivity of each metal film 12 is defined as ε x , and the emissivity of the fire spread prevention material main body 11 is defined as ε y , it is preferable that ε y / ε x is approximately 3 or more and 30 or less, more preferably approximately 3.5 or more and 25 or less, and even more preferably approximately 4 or more and 20 or less. When ε y / ε x satisfies the above relationship, the effect of suppressing radiative heat transfer by the metal films 12 can be further enhanced. The specific value of the emissivity ε of each metal film 12 x is preferably approximately 0.2 or less, more preferably approximately 0.01 or more and 0.2 or less, even more preferably approximately 0.03 or more and 0.18 or less, and particularly preferably approximately 0.05 or more and 0.16 or less.

[0014] In the present embodiment, as shown in Figure 1, each metal film 12 has a size that encloses the fire spread prevention material main body 11, that is, a size that protrudes beyond the fire spread prevention material main body 11. With such a configuration, radiative heat transfer from the side surface (peripheral surface) of the fire spread prevention material main body 11 can also be easily suppressed. This configuration is also preferable from the viewpoint of heat dissipation performance. Note that each metal film 12 may have the same size as the fire spread prevention material main body 11 in plan view (when viewed from the upper side or the lower side in Figure 1). In addition, as shown in Figure 1, the fire spread prevention material main body 11 is exposed from between the two metal films 12. According to such a configuration, even if there is a difference in thermal expansion coefficient between the fire spread prevention material main body 11 and each metal film 12, and the fire spread prevention material main body 11 and each metal film 12 are slightly deformed due to expansion and contraction during charge and discharge of the battery cell or expansion caused by deterioration of the battery cell, they can easily follow each other's deformation. As a result, deterioration of the fire spread prevention material main body 11 and each metal film 12 can be easily prevented.

[0015] The thermal conductivity of each metal film 12 is preferably greater than that of the fire-preventing material body 11. In this case, not only is the radiant heat transfer suppression effect of the metal film 12 exhibited, but the heat dissipation effect of the metal film 12 is also exhibited, and thus the heat insulation (heat insulation effect) of the fire-preventing material 1 is obtained more effectively. Furthermore, since heat dissipation from the battery cells can also be promoted, a deterioration suppression effect of the battery cells can also be expected. The specific value of the thermal conductivity of each metal film 12 is not particularly limited, but it is preferably about 50 W / mK to 500 W / mK, more preferably about 100 W / mK to 450 W / mK, even more preferably about 150 W / mK to 400 W / mK, and particularly preferably about 200 W / mK to 350 W / mK. This makes it possible to further improve the heat dissipation effect of the metal film 12. Examples of constituent materials for each metal film 12 include aluminum, iron, gold, silver, copper, nickel, platinum, or alloys containing these. For example, brass and stainless steel can be used as alloys.

[0016] It is preferable that at least one of the two metal films 12 is a metal foil, and more preferably that both are metal foils. In this case, the fire-spread prevention material 1 can be manufactured relatively easily by separately manufacturing the fire-spread prevention material body 11 and each metal film 12, and then assembling them. It is preferable that at least a portion of at least one of the two metal films 12 is in contact with the fire-spread prevention material body 11. The contact area ratio between each metal film 12 and the fire-spread prevention material body 11 is preferably about 60% or more, more preferably about 70% or more, even more preferably about 80% or more, particularly preferably about 90% or more, and may be 100%. With this configuration, the radiant heat transfer suppression effect and heat dissipation effect of the metal films 12 can be further enhanced.

[0017] Each metal film 12 is not limited to metal foil, but can also be formed directly on the surface of the fire-preventing material body 11. Examples of such methods include physical film formation methods such as vapor deposition, sputtering, and ion plating, chemical film formation methods such as CVD, and electroless plating. These methods may be used individually or in combination of two or more. The thickness of each metal film 12 is not particularly limited, but is preferably 0.01 μm to 200 μm, more preferably 0.1 μm to 150 μm, and even more preferably 1 μm to 100 μm. By using metal films 12 of such thickness, it is possible to fully exert the radiant heat transfer suppression effect and heat dissipation effect of the metal films 12 while preventing an increase in the overall mass of the fire-preventing material 1.

[0018] In the fire-resistant material body 11, it is preferable that the sodium silicate has a water content of 30% by mass or more at 30°C. That is, it is preferable that the sodium silicate contains an appropriate amount of moisture at room temperature. This allows the fire-resistant material body 11 to maintain high flexibility. As a result, it is possible to wind the fire-resistant material body 11 into a roll, that is, to manufacture the fire-resistant material body 11 in a roll-to-roll manner. Such characteristics make it suitable for mass production of the fire-resistant material body 11, and by extension, the fire-resistant material 1.

[0019] Furthermore, the fire-preventing material body 11 can retain a sufficient amount of moisture even when heated to temperatures above 100°C. As a result, in the event of an abnormality, the removal of moisture requires more energy than the heat of vaporization of water, and good heat insulation (heat-insulating effect) is exhibited. Therefore, even if one battery cell ignites in the event of an abnormality, the spread of fire to adjacent battery cells can be prevented or delayed. Note that sodium silicate is Na 2 O・nSiO 2 ・mH 2 It is a compound represented by O (where m represents 0 or a positive number).

[0020] The water content of sodium silicate at 30°C is preferably about 30 mass% or more and 60 mass% or less, more preferably about 30 mass% or more and 55 mass% or less, even more preferably about 35 mass% or more and 50 mass% or less, and particularly preferably about 35 mass% or more and 45 mass% or less. In this case, since sodium silicate contains a more appropriate amount of water, the fire spread prevention material main body 11 can maintain sufficiently high flexibility. In particular, when the water content of sodium silicate at 30°C is equal to or less than the above upper limit, it is possible to suitably prevent the surface of the fire spread prevention material main body 11 from becoming sticky and difficult to handle. For these reasons, the productivity of the fire spread prevention material main body 11 (fire spread prevention material 1) and the assembled battery can be further enhanced. The water content of sodium silicate can be measured (determined) by the method described in the Examples.

[0021] The water content of sodium silicate at 100°C is preferably about 15 mass% or more and 35 mass% or less, more preferably about 18 mass% or more and 32 mass% or less, and even more preferably about 21 mass% or more and 29 mass% or less. In this case, sodium silicate contains sufficient water even at 100°C, and becomes porous by foaming when heated to 100°C or higher. As a result, during an abnormality, the latent heat of vaporization of water and the heat insulating property (heat insulating effect) due to the porous structure are satisfactorily exhibited. Therefore, during an abnormality, even if one battery cell ignites, the spread of fire to adjacent battery cells can be prevented or delayed.

[0022] Sodium silicate preferably has a moisture content reduction rate of about 0.75 mass% / °C or less in the temperature range from 30°C to 100°C, more preferably about 0.65 mass% / °C or less, and even more preferably about 0.55 mass% / °C or less. In this case, since the fire spread preventing material main body contains sufficient moisture in the temperature range of 30°C or higher and 100°C or lower, it can contribute to the improvement of the productivity of the fire spread preventing material main body 11 (fire spread preventing material 1) and the assembled battery due to good flexibility, as well as the stable operation of the assembled battery. The above moisture content reduction rate (mass% / °C) can be calculated by the following Formula 1. Formula 1: Moisture content reduction rate (mass% / °C) = ([Moisture content of sodium silicate at 30°C] - [Moisture content of sodium silicate at 100°C]) / [Moisture content of sodium silicate at 30°C] × 100

[0023] Here, as shown in Figure 2, the water molecules present in sodium silicate are classified into I: free water, II: water molecules hydrogen-bonded to OH, III: water molecules adsorbed on Na (constituent element), and IV: water molecules present as OH. The order of evaporation (desorption) as water molecules is considered to follow the sequence of I→II→III→IV (provided that these processes may proceed simultaneously).

[0024] Therefore, in the fire spread preventing material that has become porous in the high temperature region, sodium silicate exhibits high heat insulating properties by containing the aforementioned water molecules. Furthermore, from the perspective of increasing the moisture content in the low temperature (normal temperature) region and the high temperature region, Na contained in sodium silicate 2 It is preferable to increase the ratio of O (that is, to lower the SiO 2 / Na 2 O molar ratio). Specifically, the SiO 2 / Na 2 O molar ratio is preferably about 3.3 or less, more preferably about 2.7 or less, even more preferably about 1 to 2.5, and particularly preferably about 1.2 to 2.3.

[0025] Furthermore, the fire-spread prevention performance of the fire-spread prevention material 1 can be evaluated by heating one side of the fire-spread prevention material 1 to 550°C and measuring the time it takes for the surface temperature of the other side of the fire-spread prevention material 1 to reach 200°C (hereinafter also referred to as "time to reach 200°C"). The time to reach 200°C on the other side of the fire-spread prevention material 1 is preferably about 100 seconds or more, more preferably about 110 seconds or more, even more preferably about 130 seconds or more, and particularly preferably about 150 seconds or more. The upper limit of the time to reach 200°C is not particularly limited, but for example, it is about 200 seconds. Such a time to reach 200°C may be between 100 seconds and 200 seconds. If the fire-spread prevention material 1 exhibits a time to reach 200°C within the above range, it can be judged to have excellent fire-spread prevention properties. The surface temperature can be measured by the method described in the examples.

[0026] Furthermore, since the battery cells repeatedly expand and contract during charging and discharging of the battery pack, it is preferable that the fire-spread prevention material 1 has the flexibility to follow the expansion and contraction of the battery cells. In this case, good flexibility can be imparted to the fire-spread prevention material 1 by combining an inorganic fiber base material supporting sodium silicate (i.e., the fire-spread prevention material body 11) with, for example, a polyurethane sheet material. As a result, the mechanical load on the battery cells can be reduced by following the expansion and contraction of the battery cells, and the battery pack can be repeatedly and stably operated (charged and discharged).

[0027] The proportion of sodium silicate in the fire-preventing material body 11 (the whole of sodium silicate and inorganic fiber base material) is preferably 60% by mass or more and 98% by mass or less, more preferably 70% by mass or more and 95% by mass or less, and even more preferably 75% by mass or more and 90% by mass or less. In this case, it becomes easier to impart superior fire-preventing properties to the fire-preventing material body 11, and it is also possible to reduce the weight of the fire-preventing material body 11. The proportion of inorganic fiber base material in the fire-preventing material body 11 is preferably 1% by mass or more and 40% by mass or less, more preferably 1% by mass or more and 35% by mass or less, even more preferably 5% by mass or more and 35% by mass or less, particularly preferably 8% by mass or more and 30% by mass or less, and most preferably 10% by mass or more and 20% by mass or less. In this case, it becomes easier to impart superior fire-preventing properties to the fire-preventing material body 11.

[0028] An inorganic fiber substrate is a substrate (e.g., a sheet) composed primarily of inorganic fibers. Such an inorganic fiber substrate has multiple voids (pores) formed between the inorganic fibers. In other words, the inorganic fiber substrate has a porous structure. For example, by preparing a relatively high-viscosity sodium silicate, applying it to one surface of the inorganic fiber substrate, and then drying it, a layer containing sodium silicate can be unevenly distributed on one surface of the inorganic fiber substrate. Alternatively, for example, by preparing a relatively low-viscosity sodium silicate, impregnating the inorganic fiber substrate, and then drying it, sodium silicate can be filled into the voids of the inorganic fiber substrate.

[0029] In this specification, inorganic fibers are fibrous materials having a length of approximately 1 mm or more and an aspect ratio (length / width) of approximately 100 or more. Preferably, the length (fiber length) of the inorganic fibers is approximately 3 mm to 12 mm. Preferably, the width (fiber diameter) of the inorganic fibers is approximately 3 μm to 10 μm. When the inorganic fibers constituting the inorganic fiber substrate have the above fiber length and fiber diameter, the inorganic fiber substrate tends to have excellent shape processability before drying during the manufacturing process. From a similar viewpoint, preferably, the average fiber diameter of the inorganic fibers is approximately 5 μm to 10 μm. Here, the average fiber diameter is a value measured by microscopic observation such as a scanning electron microscope (SEM) or an optical microscope.

[0030] The inorganic fibers constituting the inorganic fiber base material may be one type or multiple types. The constituent material of the inorganic fibers constituting the inorganic fiber base material may be silica (SiO₂). 2 ), alumina (Al 2 O 3 Examples include silica (SiO2), carbon, and silicon carbide (SiC). Among these, the constituent material of inorganic fibers is silica (SiO2). 2 ) and alumina (Al 2 O 3 Preferably, it includes at least one selected from the group consisting of ). In this case, higher fire spread prevention properties can be imparted to the fire spread prevention material, and the inorganic fiber base material tends to have excellent shape processability before drying during the manufacturing process.

[0031] Examples of such inorganic fibers include glass fibers, silica fibers, alumina-silica fibers, alumina fibers, basalt fibers, and rock wool. Among these, it is preferable that the inorganic fiber base material contains at least one of glass fibers, silica fibers, and alumina-silica fibers. In this case, the above effects can be further improved.

[0032] The inorganic fiber content in the inorganic fiber base material is preferably 60% by mass or more and 100% by mass or less, more preferably 70% by mass or more and 98% by mass or less, even more preferably 80% by mass or more and 95% by mass or less, and particularly preferably 85% by mass or more and 93% by mass or less. In this case, the fire spread prevention material body 11 (fire spread prevention material 1) can provide excellent fire spread prevention properties.

[0033] The inorganic fiber substrate may further contain an organic binder. The organic binder is, for example, an organic material that binds the inorganic fibers together, and may be used alone or in combination of multiple types. As the organic binder, for example, a resin having a glass transition temperature of room temperature (e.g., 25°C) or lower, a water-soluble resin, etc., can be used. Specific examples of organic binders include, for example, acrylic resins, polyvinyl alcohol resins (such as vinylon), epoxy resins, cellulose such as cellulose microfibrils, and polyvinyl chloride resins.

[0034] Here, acrylic resin refers to a polymer containing at least one monomer unit selected from the group consisting of acrylic acid and its derivatives (such as acrylic acid esters), and methacrylic acid and its derivatives (such as methacrylic acid esters). Cellulose microfibrils refer to microfibrillated cellulose fibers. In particular, it is preferable that the organic binder contains at least one selected from the group consisting of acrylic resins, polyvinyl alcohol resins, and epoxy resins. In this case, a fire-resistant material body (fire-resistant material) with higher fire-spread prevention properties tends to be obtained.

[0035] The content of the organic binder in the inorganic fiber base material is preferably 0% by mass or more and 40% by mass or less, more preferably 2% by mass or more and 30% by mass or less, even more preferably 5% by mass or more and 20% by mass or less, and particularly preferably 7% by mass or more and 15% by mass or less. In this case, it becomes easier to obtain a fire-resistant material body 11 (fire-resistant material 1) with superior fire-spread prevention properties.

[0036] The inorganic fiber substrate may further contain inorganic particles. Examples of constituent materials for the inorganic particles include silica, aluminum hydroxide, zinc oxide, magnesium carbonate, and aluminum silicate. Examples of silica-containing particles include precipitated silica, fumed silica, and colloidal silica. Precipitated silica is an amorphous silica particle obtained by the sedimentation method, a type of wet process, and has a porous structure.

[0037] The average particle size of the inorganic particles is preferably 0.01 μm to 100 μm, more preferably 0.1 μm to 80 μm, even more preferably 0.5 μm to 80 μm, and particularly preferably 1 μm to 50 μm. Here, the average particle size of the inorganic particles is the value of the volume cumulative particle size D50 measured by a laser diffraction particle size analyzer. Inorganic particles having such an average particle size are easy to handle and are easier to distribute more uniformly in an inorganic fiber substrate.

[0038] The inorganic particle content in the inorganic fiber substrate is preferably 20% to 50% by mass, more preferably 25% to 45% by mass, and even more preferably 30% to 40% by mass. Including inorganic particles in this amount enhances heat insulation and provides a fire-resistant material body 11 with superior fire-spread prevention properties. Furthermore, it is possible to obtain an inorganic fiber substrate (and consequently, a fire-spread prevention material body 11) that is lighter and has higher mechanical strength. From the viewpoint of increasing the mechanical strength of the inorganic fiber substrate, it is preferable that the inorganic fiber substrate does not contain precipitated silica, and more preferably does not contain inorganic particles.

[0039] The inorganic fiber base material may contain a flocculant such as a polyamidine polymer. The flocculant content in the inorganic fiber base material is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.3% by mass or more and 4% by mass or less, and even more preferably 0.5% by mass or more and 3% by mass or less. The inorganic fiber base material may contain sodium silicate (sodium silicate other than sodium silicate with a water content of 30% by mass or more at 30°C), or it may not contain such sodium silicate. If such sodium silicate is included, the sodium silicate content in the inorganic fiber base material is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0040] As the inorganic fiber base material, it is preferable to use a base material that has excellent sodium silicate retention (support). The inorganic fiber base material is preferably a nonwoven fabric, and more preferably a sheet formed by a wet papermaking method (wet papermaking sheet). Wet papermaking sheets are particularly preferable from the viewpoint of having excellent sodium silicate retention. In the wet papermaking method, an inorganic fiber base material (nonwoven fabric) is produced by dispersing materials (inorganic fibers, organic binder, etc.) in water, forming the dispersion on a papermaking screen, and drying it. By this method, an inorganic fiber base material (nonwoven fabric) having substantially uniformly dispersed voids can be easily obtained. Therefore, wet papermaking sheets tend to have substantially uniformly dispersed voids and have excellent sodium silicate retention.

[0041] The apparent density of the inorganic fiber substrate is 0.08 g / cm³. 3 0.2g / cm or more 3 The following is preferable: The basis weight of the inorganic fiber base material is 100 g / m². 2 170g / m or less 2 The following is preferable: The thickness of the inorganic fiber base material is preferably 0.2 mm to 3 mm.

[0042] Sodium silicate may be unevenly distributed on one side of the inorganic fiber substrate, or it may be impregnated into the inorganic fiber substrate. That is, the fire-spread prevention material body 11 may have a two-layer structure consisting of an inorganic fiber substrate 2 and a layer 3 containing sodium silicate SS, as shown in Figure 3, or it may have a one-layer structure in which sodium silicate SS is impregnated into the inorganic fiber substrate 2, as shown in Figure 4. The sodium silicate unevenly distributed or impregnated into the inorganic fiber substrate may be in liquid form or gel form, but it is preferably in gel form. Since gel-like sodium silicate is easily supported on the inorganic fiber substrate, it is less likely to fall off the inorganic fiber substrate during the manufacture of the fire-spread prevention material body 11. The two-layer fire-spread prevention material body 11 can be formed, for example, by preparing relatively high-viscosity sodium silicate SS, applying it to one side of the inorganic fiber substrate 2, and then drying it, thereby unevenly distributing the layer 3 containing sodium silicate SS on one side of the inorganic fiber substrate 2. Suitable coating methods for this process include gravure coating, slot die coating, knife coating, blade coating, comma coating, reverse roll coating, and inkjet coating.

[0043] On the other hand, a single-layer fire-spread prevention material body 11 can be manufactured, for example, by preparing relatively low-viscosity sodium silicate SS, impregnating it into an inorganic fiber base material 2, applying pressure as necessary, and then drying it to fill the voids in the inorganic fiber base material 2 with sodium silicate SS. Preferably, any of the above fire-spread prevention material body 11 is manufactured by a roll-to-roll method, where the inorganic fiber base material 2 wound into a roll is fed out, sodium silicate SS is supplied and dried, and then wound into a roll. As described above, the fire-spread prevention material body 11 can maintain high flexibility even during its manufacture. Therefore, the operation of winding the fire-spread prevention material body 11 into a roll can be performed smoothly, and cracks and the like are less likely to occur in the fire-spread prevention material body 11 even after it has been wound into a roll.

[0044] The drying temperature is not particularly limited, but is preferably around 80°C to 130°C, more preferably around 90°C to 120°C, and even more preferably around 100°C to 115°C. Drying within this temperature range makes it possible to adjust the moisture content of sodium silicate to the desired range in a relatively short time. The drying time is set appropriately according to the drying temperature, and is preferably around 0.1 minutes to 15 minutes, more preferably around 0.5 minutes to 12.5 minutes, even more preferably around 1 minute to 10 minutes, particularly preferably around 1.5 minutes to 10 minutes, and most preferably around 2 minutes to 7.5 minutes.

[0045] In the configuration example shown in Figure 3, it is preferable that layer 3 and, in the configuration example shown in Figure 4, the fire-spread prevention material body 11 (hereinafter referred to as the "sodium silicate-containing portion") absorb heat in a temperature range of 100°C to 300°C. Furthermore, it is preferable that the mass loss rate when the sodium silicate-containing portion is heated from 100°C to 300°C at a rate of 10°C / min is 15% by mass or more. The endothermic reaction of the sodium silicate-containing portion is thought to occur because the water in the sodium silicate-containing portion (for example, water molecules in sodium silicate SS) undergoes an endothermic reaction in a temperature range of 100°C to 300°C. On the other hand, the mass loss of the sodium silicate-containing portion is thought to occur as a result of this endothermic reaction.

[0046] Therefore, the mass loss rate when the sodium silicate-containing portion is heated from 100°C to 300°C at a rate of 10°C / min correlates with the amount of water and heat absorbed in the sodium silicate-containing portion. For this reason, it is presumed that a mass loss rate of 15% by mass or more in the sodium silicate-containing portion results in a large amount of heat absorbed within the above temperature range, thus providing sufficient fire-spread prevention in the fire-spread prevention material. The heat absorbed in the sodium silicate-containing portion can be confirmed, for example, by performing thermogravimetric-differential thermal analysis (TG-DTA) and observing the presence or absence of an endothermic peak within the temperature range of 100°C to 300°C.

[0047] When the sodium silicate-containing portion is heated from 100°C to 300°C at a rate of 10°C / min, the mass loss rate is preferably 15% to 30% by mass, more preferably 17% to 28% by mass, even more preferably 20% to 25% by mass, particularly preferably 23% to 25% by mass, and most preferably 23.5% to 25% by mass. In this case, a fire-resistant material body 11 with superior fire-spread prevention properties is easily obtained. The above mass loss rate can be calculated using the following formula 2. Formula 2: Mass loss rate (mass%) = [Mass loss of sodium silicate-containing portion] / [Mass of sodium silicate-containing portion at 100°C] × 100

[0048] Here, the mass loss of the sodium silicate-containing portion is the difference between the mass of the sodium silicate-containing portion at 100°C and the mass of the sodium silicate-containing portion at 300°C. If there are multiple sodium silicate-containing portions, the mass loss rate of each sodium silicate-containing portion may be within the above range, or the sum of the mass loss rates of all sodium silicate-containing portions may be within the above range.

[0049] The fire-spread prevention material 1 preferably has insulating properties. In this case, for example, the side of each metal film 12 opposite to the fire-spread prevention material body 11 can be protected with a resin sheet material, or the fire-spread prevention material body 11 and the two metal films 12 can be housed in an outer casing 5, which will be described later, thereby providing the fire-spread prevention material 1 with high insulating properties. Here, having insulating properties means that the electrical resistivity measured by volume resistivity measurement is 1 × 10⁻⁶. 8 This means that the density is Ω·cm or greater. The fire-spread prevention material 1 may be in the form of a sheet (for example, a flat plate), or it may be processed into a predetermined shape. The predetermined shape may be appropriately set according to the shape of the installation location of the fire-spread prevention material 1.

[0050] The predetermined shape may be, for example, a shape that conforms to the shape of the installation location of the fire-spread prevention material 1 (such as the surface shape of a member positioned opposite the fire-spread prevention material 1). Specific examples of the shape include a sheet-like shape with irregularities on its surface, a sheet-like shape with curved sections at angles of 90° or more, etc. The shape of the irregularities (shape of the convex and concave parts) is not particularly limited and may be rectangular in cross-section, V-shaped in cross-section, U-shaped in cross-section, etc. The fire-spread prevention material 1 processed into the predetermined shape can be manufactured by the manufacturing method described later, thereby preventing separation and breakage of the inorganic fiber base material and sodium silicate. The absence of separation and breakage in the fire-spread prevention material 1 can be confirmed, for example, by observing the cross-section of the fire-spread prevention material 1 using a scanning electron microscope (SEM).

[0051] The thickness of the fire-spread prevention material body 11 (the thickness of one fire-spread prevention material 1 in the configuration examples of Figures 3 and 4) is preferably about 5 mm or less, preferably about 1 mm to 5 mm, more preferably about 1.2 mm to 4 mm, and even more preferably about 1.5 mm to 3 mm. In this case, a fire-spread prevention material body 11 with higher fire-spread prevention performance can be obtained, and the space required for the fire-spread prevention material 1 within the battery pack can be suppressed. Note that multiple fire-spread prevention material bodies 11 may be used stacked together.

[0052] As shown in Figure 5, the fire-spread prevention material 1 may further include an outer casing 5 that houses the fire-spread prevention material body 11 and the two metal films 12. In other words, the fire-spread prevention material 1 can also be said to include a fire-spread prevention material body 11 and an outer casing 5 that houses an assembly of the two metal films 12 provided on both sides of the fire-spread prevention material body 11. By housing the above assembly (sodium silicate SS) inside the outer casing 5, the amount of moisture escaping from the fire-spread prevention material 1 can be adjusted (reduced). Figure 5(a) is a schematic plan view showing an embodiment of the fire-spread prevention material with an outer casing. Figure 5(b) is a schematic side view and an enlarged view showing a cross-section of the end of the fire-spread prevention material with an outer casing.

[0053] The water vapor transmission rate of the outer casing 5 at 40°C and 90% RH is 15 g / m². 2It is preferable that the amount be approximately 10 g / m² or less per day. 2 It is more preferable that the amount is less than or equal to 5 g / m² / day. 2 It is even more preferable that the amount is less than or equal to 1 g / m² / day. 2 It is particularly preferable that the value be approximately 0.01 g / m³ or less. The lower limit of the water vapor transmission rate of the outer casing 5 at 40°C and 90% RH is 0.01 g / m³. 2 It is approximately / day. The water vapor transmission rate of the outer casing 5 at 40°C and 90% RH is 0.01 g / m³. 2 / day or more 15g / m 2 It may be approximately 1 / day or less. By setting the water vapor permeability of the outer casing 5 within the above range, the amount of moisture escaping from the fire-preventing material 1 can be more reliably controlled (reduced). Furthermore, the pressure of the water vapor generated within the outer casing 5 can also create a force that presses each metal film 12 against the fire-preventing material body 11, which is thought to improve the adhesion between them. Therefore, the fire-preventive effect is further improved. The water vapor permeability (water vapor transmission rate) is measured according to the method specified in JIS K 7129-2:2019.

[0054] The outer casing 5 houses a composite of inorganic fiber substrate 2 and sodium silicate SS (fire-spread prevention material body 11) inside by sealing the outer periphery of two sheet materials 5a and 5b with a sealing portion 50. The sealing portion 50 is formed by joining the outer periphery of the two sheet materials 5a and 5b by methods such as fusion bonding (ultrasonic bonding, high-frequency bonding, thermal bonding). Alternatively, one sheet material can be folded in half, and its outer periphery can be sealed with a sealing portion to house the composite of inorganic fiber substrate 2 and sodium silicate SS inside. In this embodiment, each sheet material 5a and 5b is a laminate having a base layer 51, a sealing layer 52 provided on the inner side of the base layer 51, and a protective layer 53 provided on the outer side of the base layer 51.

[0055] The base layer 51 has the function of providing mechanical strength to the sheet materials 5a and 5b, and the function of regulating (blocking) the permeation of moisture (water vapor). The base layer 51 may be made of metal foil. Examples of materials that make up this metal foil include aluminum or aluminum alloy, nickel or nickel alloy, stainless steel, etc. The thickness of the base layer 51 is not particularly limited, but is preferably about 5 μm to 100 μm, more preferably about 8 μm to 80 μm, and even more preferably about 12 μm to 60 μm. In this case, appropriate water vapor permeability and sufficient flexibility of the sheet materials 5a and 5b can be ensured.

[0056] The seal layer 52 has the function of sealing the outer casing 5 by being fused to it. Examples of constituent materials (fusible materials) for the seal layer 52 include polyethylene (LDPE, LLPDE), polypropylene, ethylene-vinyl acetate copolymer, polyethylene terephthalate, polybutylene terephthalate, polyvinyl chloride, polyvinylidene chloride, ethylene-vinyl alcohol copolymer, polystyrene, polyacrylonitrile, ethylene-(meth)acrylic acid copolymer, and polymethylpentene. Polypropylene is more preferred as the constituent material of the seal layer 52, and unstretched polypropylene is even more preferred. The thickness of the seal layer 52 is not particularly limited, but is preferably about 5 μm to 200 μm, more preferably about 10 μm to 100 μm, even more preferably about 20 μm to 120 μm, and particularly preferably about 30 μm to 80 μm. This makes it possible to improve sealing performance while ensuring the flexibility of each sheet material 5a, 5b.

[0057] The protective layer 53 has the function of protecting the base layer 51 (preventing corrosion of the base layer 51, etc.). Relatively hard resin materials are used as constituent materials for the protective layer 53. Examples of such hard resin materials include polyamide resins (nylon), acrylic resins, polyimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polycarbonate resins, polyvinyl butyral resins, polyarylate resins, fluorine resins, polyester resins, etc. The thickness of the protective layer 53 is not particularly limited, but is preferably about 5 μm to 100 μm, more preferably about 10 μm to 50 μm, and even more preferably about 15 μm to 30 μm.

[0058] The thickness of the outer casing 5 is not particularly limited, but is preferably about 250 μm or less, more preferably about 200 μm or less, and even more preferably about 100 μm or less. In this case, it becomes easier to set the water vapor permeability of the outer casing 5 within the above range. As a result, the amount of moisture escaping from the fire-preventing material 1 can be suitably adjusted (reduced), and thus the fire-preventing performance is further improved. Note that the sheet materials 5a and 5b are not limited to a three-layer configuration, but may be a single-layer (1 layer) configuration, a two-layer configuration, or a configuration of four or more layers, depending on the required characteristics.

[0059] Although a fire-spread prevention material 1 according to one embodiment has been described above, the fire-spread prevention material of the present invention is not limited to the above embodiment. Another embodiment of the present invention provides a battery pack comprising two or more battery cells and the fire-spread prevention material 1 disposed between adjacent battery cells. This battery pack is, for example, a lithium-ion battery. Another embodiment of the present invention provides an automobile comprising an automobile body and the above battery pack mounted on the automobile body. Furthermore, it may be provided in each of the following embodiments.

[0060] (1) A fire-spread prevention material comprising a fire-spread prevention material body comprising an inorganic fiber base material containing inorganic fibers and sodium silicate supported on the inorganic fiber base material, and two metal films provided on both sides of the fire-spread prevention material body facing each other via the fire-spread prevention material body, wherein the emissivity of each metal film is less than the emissivity of the fire-spread prevention material body.

[0061] (2) In the fire-spread prevention material described in (1) above, the emissivity of each metal film is set to ε x The emissivity of the fire-preventing material body is set to ε y When this is the case, ε y / ε x A fire-resistant material with a value between 3 and 30.

[0062] (3) A fire-spread prevention material according to (1) or (2) above, wherein the emissivity of each metal film is 0.2 or less.

[0063] (4) A fire-spread prevention material according to any one of (1) to (3) above, wherein the fire-spread prevention material body is exposed from between the two metal films.

[0064] (5) A fire-spread prevention material according to any one of (1) to (4) above, wherein the thermal conductivity of each metal film is greater than the thermal conductivity of the fire-spread prevention material body.

[0065] (6) A fire-spread prevention material according to any one of (1) to (5) above, wherein the thickness of each metal film is 0.01 μm or more and 200 μm or less.

[0066] (7) A fire-spread prevention material according to any one of (1) to (6) above, wherein at least one of the two metal films is a metal foil.

[0067] (8) A fire-spread prevention material according to any one of (1) to (7) above, wherein at least one of the two metal films is in contact with the fire-spread prevention material body, at least a portion of which is in contact with the fire-spread prevention material body.

[0068] (9) A fire-spread prevention material according to any one of (1) to (8) above, wherein the thickness of the fire-spread prevention material body is 5 mm or less.

[0069] (10) A fire-spread prevention material according to any one of (1) to (9) above, further comprising an outer casing that houses the fire-spread prevention material body and the two metal films.

[0070] (11) In the fire-spread prevention material described in (10) above, the outer casing has a water vapor transmission rate of 15 g / m³ at 40°C and 90% RH. 2 A fire-spread prevention material having a density of 250 μm or less and a thickness of 250 μm or less.

[0071] (12) A battery pack comprising two or more battery cells and a fire-spread prevention material according to any one of (1) to (11) above, disposed between adjacent battery cells.

[0072] (13) An automobile comprising an automobile body and a battery pack as described in (12) above, mounted on the automobile body. Of course, this is not limited to this.

[0073] Finally, while various embodiments relating to this disclosure have been described, these are presented as examples only and are not intended to limit the scope of the invention. These novel embodiments can be implemented in a variety of other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their variations are included in the scope and spirit of the invention, as well as in the claims and their equivalents.

[0074] The following will provide a more detailed explanation of fire-spread prevention materials using the following examples and comparative examples, however, fire-spread prevention materials are not limited to the following examples.

[0075] 1. Preparation of materials <Sodium silicate> SS:SiO 2 / Na 2 O molar ratio 2.0 to 2.3, gel-like <Inorganic fiber> F1: Glass fiber (average fiber diameter 10 μm) <Organic binder> B1: Vinylon fiber (average fiber diameter 5 μm) <Metal foil> 100 mm long x 100 mm wide x 12 μm thick, and emissivity ε x 0.04 aluminum foil

[0076] 2. Preparation of Inorganic Fiber Substrate (Wet-Formed Sheet) 6.5 parts by mass of inorganic fiber F1 and 0.7 parts by mass of organic binder B1 were added to 100 parts by mass of pure water and mixed for 2 hours in a homomixer manufactured by Tokushu Kika Kogyo Co., Ltd. to obtain a dispersion. This dispersion was formed on a papermaking screen and dried in a Yankee dryer to produce a wet-formed sheet (nonwoven fabric). The wet-formed sheet had dimensions of 100 mm (length) x 100 mm (width) x 0.8 mm (thickness) and a basis weight of 120 g / m². 2 That was the case.

[0077] 3. Preparation of the fire-spread prevention material: 900 g / m of sodium silicate SS. 2 To achieve this, a wet-formed sheet (inorganic fiber base material) was impregnated with sodium silicate, compressed with a roller, and then dried at 115°C for 3 minutes. This produced a single-layer fire-resistant material body in which sodium silicate was filled into the voids of the wet-formed sheet. The thickness of the resulting fire-resistant material body was 0.8 mm. The emissivity ε of the fire-resistant material body was also determined. y It is approximately 0.9. The above emissivity is measured using an infrared spectrophotometer or thermography.

[0078] 4. Preparation of fire-spread prevention material (Example 1) A fire-spread prevention material was obtained by fixing the four corners of aluminum foil to both sides of the fire-spread prevention material body with double-sided tape. (Example 2) The fire-spread prevention material body was placed in an aluminum pouch bag (Technostat Industries Co., Ltd., "ST-678", thickness 102 μm, water vapor transmission rate 0.1 g / m²) 2 The material was stored in a container (40°C, 90% RH or less) and its opening was sealed to create an outer casing. This resulted in a fire-resistant material equipped with an outer casing. The aluminum pouch bag has a 7 μm thick aluminum foil in the center of the thickness direction of the sheet material.

[0079] (Comparative Example 1) A fire-spread prevention material was obtained by fixing the four corners of aluminum foil to one side of the fire-spread prevention material body with double-sided tape. (Comparative Example 2) The aluminum foil was omitted, and the fire-spread prevention material body was used as the fire-spread prevention material. (Comparative Example 3) The fire-spread prevention material body was enclosed in a pouch bag (Fujimori Kogyo Co., Ltd., "MW-062", thickness 74 μm, water vapor transmission rate 0.05 g / m²) 2The material was stored in a container (40°C, 90% RH or less) and its opening was sealed to create an outer casing. This resulted in a fire-resistant material equipped with an outer casing.

[0080] 4. Measurement and Evaluation 4-1. Measurement of Moisture Content The mass change up to 1000°C was measured for the fire-resistant material body using a thermogravimetric analyzer (NETZSCH Japan, "High-Sensitivity Differential Thermal Balance STA 2500 Regulus"). The difference between the measurement value at 1000°C and the mass of the wet-formed sheet was defined as the "solid content," and the moisture content and water content of sodium silicate SS at 30°C were determined from this solid content value and the thermogravimetric measurement value.

[0081] 4-2. Evaluation of fire spread prevention properties One fire spread prevention material, one thin aluminum plate (thickness: 0.5 mm), a K-type thermocouple, two glass fiber sheets (thickness per sheet: 0.6 mm), and an aluminum block (500 g) were stacked in this order on a hot plate (MSA Factory Co., Ltd., "PA8015") heated to 550°C. The time it took for the temperature of the back surface of the fire spread prevention material (the surface temperature opposite the hot plate) to reach 200°C was measured. The fire spread prevention materials used were those from Example 1, Comparative Example 1, and Comparative Example 2.

[0082] These results are shown in Table 1 below. The fire-spread prevention material in the example was confirmed to have excellent fire-spread prevention properties.

[0083] 4-3. Simulated Combustion Test The following simulated combustion tests were conducted using the fire-spread prevention materials of Example 1, Example 2, and Comparative Example 3. Figure 6 is a schematic diagram showing the configuration of the battery cell assembly for the simulated combustion test. First, four battery cells ("laminated type", "capacity approximately 56 Ah") were prepared. The size of one battery cell was 256 mm in length, 216 mm in width, and 8 mm in thickness, and its weight was 1.0 kg. One sheet of fire-spread prevention material was placed between each adjacent battery cell. Bakelite plates were placed above and below this laminate and fixed with a restraining jig. This created the battery cell assembly. A heater was provided on the lower bakelite plate so as to contact the first battery cell.

[0084] In the above-described battery cell assembly, the fire-spread prevention material of Example 1 was placed between the first and second battery cells, the fire-spread prevention material of Example 2 was placed between the second and third battery cells, and the fire-spread prevention material of Comparative Example 3 was placed between the third and fourth battery cells. As shown in Figure 6, with the battery cell assembly positioned horizontally, 800W of power was input to the heater, and the time interval from when the battery cell located directly in front of (to the left of) the fire-spread prevention material under evaluation ignited until the battery cell located directly behind (to the right of) the fire-spread prevention material under evaluation ignited was measured and defined as the ignition interval.

[0085] The results are shown in Table 2 below. In these simulated combustion tests, it was confirmed that the fire-spread prevention materials of each example had a longer ignition interval and superior fire-spread prevention properties compared to the fire-spread prevention materials of the comparative examples.

[0086] 1: Fire-spread prevention material, 11: Fire-spread prevention material body, 12: Metal film, 2: Inorganic fiber base material, 3: Layer, 5: Outer body, 5a: Sheet material, 5b: Sheet material, 50: Sealing part, 51: Base material layer, 52: Sealing layer, 53: Protective layer, SS: Sodium silicate

Claims

1. A fire-spread prevention material comprising: a fire-spread prevention material body comprising an inorganic fiber base material containing inorganic fibers and sodium silicate supported on the inorganic fiber base material; and two metal films provided on both sides of the fire-spread prevention material body, facing each other via the fire-spread prevention material body, wherein the emissivity of each metal film is less than the emissivity of the fire-spread prevention material body.

2. In the fire-spread prevention material according to claim 1, the emissivity of each metal film is ε x The emissivity of the fire-preventing material body is set to ε y When this is the case, ε y / ε x A fire-resistant material with a value between 3 and 30.

3. A fire-spread prevention material according to claim 1, wherein the emissivity of each metal film is 0.2 or less.

4. A fire-spread prevention material according to claim 1, wherein the fire-spread prevention material body is exposed from between the two metal films.

5. A fire-spread prevention material according to claim 1, wherein the thermal conductivity of each metal film is greater than the thermal conductivity of the fire-spread prevention material body.

6. A fire-spread prevention material according to claim 1, wherein the thickness of each metal film is 0.01 μm or more and 200 μm or less.

7. A fire-spread prevention material according to claim 1, wherein at least one of the two metal films is a metal foil.

8. A fire-spread prevention material according to claim 1, wherein at least one of the two metal films is in contact with the fire-spread prevention material body, at least a portion of which is in contact with the fire-spread prevention material body.

9. A fire-spread prevention material according to claim 1, wherein the thickness of the fire-spread prevention material body is 5 mm or less.

10. A fire-spread prevention material according to claim 1, further comprising an outer casing that houses the fire-spread prevention material body and the two metal films.

11. In the fire-spread prevention material according to claim 10, the outer casing has a water vapor transmission rate of 15 g / m³ at 40°C and 90% RH. 2 A fire-spread prevention material having a density of 250 μm or less and a thickness of 250 μm or less.

12. A battery pack comprising two or more battery cells and a fire-spread prevention material according to any one of claims 1 to 11, disposed between adjacent battery cells.

13. An automobile comprising an automobile body and a battery pack according to claim 12 mounted on the automobile body.