Pressure-sensitive adhesive sheet
The adhesive sheet with a photopolymerized polymer base and hydrophilic monomer units addresses the challenge of safely and easily removing optical components by heating, ensuring strong adhesion and ease of peeling over time.
Patent Information
- Application Number
- PCT/JP2026/016025
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-04-21
- Publication Date
- 2026-11-19
AI Technical Summary
Existing adhesive sheets for optical components in image display devices are difficult to remove without using hazardous substances like water or ethanol, and they lose adhesion over time, making them hard to peel off after prolonged use.
An adhesive sheet with a photopolymerized polymer base containing 3 to 8% by mass of hydrophilic monomer units, which can be easily peeled off by heating, maintaining strong adhesion during use and after long periods.
The adhesive sheet provides excellent adhesion to substrates, is safely removable, and retains ease of peeling even after extended use, without the need for hazardous solvents and with controlled adhesion strength.
Smart Images

Figure JP2026016025_19112026_PF_FP_ABST
Abstract
Description
Adhesive sheet
[0001] This invention relates to an adhesive sheet. More specifically, to an adhesive sheet that is preferably usable for optical applications and is removable by heating.
[0002] In recent years, image display devices such as liquid crystal displays (LCDs) and organic light-emitting diodes (OLEDs), as well as touch panels that incorporate touch sensors into these image display devices, have become widely used in various fields. Such image display devices and touch panels have a structure in which various optical components such as polarizing films, phase difference films, optical compensation films, touch sensor films, and cover films are laminated onto an image display panel. Adhesive sheets having an adhesive layer are used to bond these optical components together. For example, transparent adhesive sheets are used to bond various optical components in image display devices (see, for example, Patent Documents 1 to 3).
[0003] For bonding the above-mentioned optical components, an optical component with an adhesive layer, in which an adhesive sheet is attached to the optical component, is generally used. After use or in the event of a malfunction, it may be necessary to peel off and recover the materials constituting the optical component. For this reason, the adhesive sheet to which the materials are bonded is sometimes required to be easily peeled off. For example, there is an adhesive sheet known in which the adhesive strength can be reduced by impregnating the interface between the adherend and the adhesive sheet with an aqueous liquid such as water or ethanol after the adhesive sheet has been bonded to the adherend (see, for example, Patent Document 4).
[0004] Japanese Patent Publication No. 2003-238915, Japanese Patent Publication No. 2003-342542, Japanese Patent Publication No. 2004-231723, Japanese Patent Publication No. 2020-23679
[0005] However, if water is used for removal, it is necessary to remove any remaining water from the surface of the adherend by drying. Also, ethanol is a flammable liquid, so caution is required when using it. Furthermore, adhesive sheets that are easy to remove tend to have poor adhesion when attached to an adherend during normal use, so they should be difficult to peel off from the adherend during normal use. Moreover, even if peeling is easy immediately after application, it may be difficult to remove the adhesive sheet if it has been attached to the adherend for a long period of time.
[0006] The present invention aims to solve these problems, and its objective is to provide an adhesive sheet that exhibits excellent adhesion to the substrate during use, is easily and safely removed when intentionally peeled off, and is easily removed even after a long period of time has passed since it was bonded.
[0007] The present invention comprises an adhesive layer that is peelable by heating and contains a photopolymerized polymer as a base polymer, wherein the adhesive layer contains an oligomer containing 3 to 8% by mass of constituent units derived from a hydrophilic monomer, and the adhesive force Fh is obtained when the adhesive layer is bonded to the Sn surface of alkali glass, stored at 50°C for one week, and then peeled off under the conditions of 60°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 2 The adhesive strength is 1.5 to 3.5 N / 25 mm, and the adhesive strength Fn was obtained when the above adhesive layer was bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, and then peeled off under the conditions of 25°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 1 The present invention provides an adhesive sheet with a density of 7N / 25mm or higher.
[0008] The adhesive layer described above was bonded to the Sn surface of alkali glass and stored at room temperature for 24 hours. The adhesive strength Fh was obtained when peeled off under the conditions of 60°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 1 The value is preferably 1.5 to 3.5 N / 25 mm.
[0009] The adhesive layer described above was bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, heated at 60°C for 3 minutes, then stored at room temperature for 1 hour. The adhesive strength Fn was obtained when peeled off under the conditions of 25°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 3 The above adhesive strength Fn 1 It is preferable that it be 80-150% of that.
[0010] The adhesive layer described above was bonded to the Sn surface of alkali glass and stored at room temperature for 24 hours. The adhesive strength Fh was measured when peeled off under the conditions of 60°C, 90% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 3 It is preferable that the value is 1.5 N / 25 mm or higher.
[0011] Preferably, the above adhesive layer has a weight-average molecular weight of 200,000 or more for the sol component soluble in ethyl acetate, and a proportion of 68% by mass or more for the gel component insoluble in ethyl acetate.
[0012] The above adhesive sheet is preferably used to be attached to an optical component.
[0013] The adhesive sheet of the present invention exhibits excellent adhesion to the substrate during use, is easily and safely removed when intentionally peeled off, and remains easily removable even after a long period of time has passed since it was bonded.
[0014] This is a cross-sectional view showing one embodiment of the adhesive sheet of the present invention. This is a cross-sectional view showing one embodiment of the optical laminate of the present invention. This is a cross-sectional view showing another embodiment of the optical laminate of the present invention. This is a cross-sectional view showing one embodiment of the OLED display panel in the optical laminate shown in Figure 3.
[0015] [Adhesive Sheet] The adhesive sheet of the present invention is removable by heating and comprises an adhesive layer containing a photopolymerized polymer as a base polymer. The adhesive layer contains an oligomer containing 3 to 8% by mass of constituent units derived from a hydrophilic monomer. Furthermore, the adhesive strength Fh of the adhesive layer is obtained when it is peeled off under the conditions of 60°C, 50% relative humidity, peeling angle of 180°, and tensile speed of 300 mm / min after being bonded to the Sn surface of alkali glass and stored at 50°C for one week. 2is 1.5 to 3.5 N / 25 mm, and after being bonded to the Sn surface of alkaline glass and stored at room temperature for 24 hours, the adhesive force Fn when peeled under the conditions of 25°C, 50% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min 1 is 7 N / 25 mm or more. In this specification, the above-mentioned pressure-sensitive adhesive layer may be referred to as the "pressure-sensitive adhesive layer of the present invention". In addition, in this specification, room temperature means 20±10°C, and typically means 20°C.
[0016] The pressure-sensitive adhesive sheet of the present invention may be a so-called "substrate-less type" pressure-sensitive adhesive sheet that does not have a substrate (substrate layer), or may be a pressure-sensitive adhesive sheet of a type having a substrate. In this specification, a "substrate-less type" pressure-sensitive adhesive sheet may be referred to as a "substrate-less pressure-sensitive adhesive sheet", and a pressure-sensitive adhesive sheet of a type having a substrate may be referred to as a "substrate-equipped pressure-sensitive adhesive sheet". Examples of the substrate-less pressure-sensitive adhesive sheet include a double-sided pressure-sensitive adhesive sheet composed only of the pressure-sensitive adhesive layer of the present invention, and a double-sided pressure-sensitive adhesive sheet composed of the pressure-sensitive adhesive layer of the present invention and another pressure-sensitive adhesive layer (a pressure-sensitive adhesive layer other than the pressure-sensitive adhesive layer of the present invention). Examples of the substrate-equipped pressure-sensitive adhesive sheet include a single-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on one side of a substrate, a double-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on both sides of a substrate, and a double-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on one side of a substrate and another pressure-sensitive adhesive layer on the other side. The above-mentioned "substrate (substrate layer)" refers to a support, and is a part that is attached to an adherend together with the pressure-sensitive adhesive layer when the pressure-sensitive adhesive sheet of the present invention is used (attached) to the adherend. A release liner that is peeled off during use (attachment) of the pressure-sensitive adhesive sheet is not included in the above-mentioned substrate.
[0017] FIG. 1 is a schematic cross-sectional view showing an embodiment of the pressure-sensitive adhesive sheet of the present invention. The pressure-sensitive adhesive sheet 10 shown in FIG. 1 is a substrate-less double-sided pressure-sensitive adhesive sheet composed of a single pressure-sensitive adhesive layer 2 which is the pressure-sensitive adhesive layer of the present invention, and a release liner L1 and a release liner L2 are provided on both pressure-sensitive adhesive surfaces thereof, respectively.
[0018] (Pressure-sensitive adhesive layer) As described above, the pressure-sensitive adhesive layer of the present invention has the above-mentioned adhesive force Fh 2 ("60°C adhesive force Fh after storage 2The adhesive strength Fh (sometimes referred to as "Fh") is 1.5 to 3.5 N / 25 mm, preferably 2.0 to 3.4 N / 25 mm, and more preferably 2.4 to 3.3 N / 25 mm. 2 If the adhesive strength is 1.5 N / 25 mm or higher, it is less likely to detach when heated and has excellent heat resistance. Adhesion strength Fh at 60°C after storage. 2 If the adhesive strength is 3.5 N / 25 mm or less, the adhesive strength will decrease upon heating even after long-term storage, allowing for easy peeling.
[0019] As described above, the adhesive layer of the present invention has the adhesive strength Fn 1 (“Initial room temperature adhesive force Fn 1 The initial room temperature adhesion Fn (sometimes referred to as ") is 7.0 N / 25 mm or more, preferably 7.2 N / 25 mm or more, and more preferably 7.5 N / 25 mm or more. 1 If the initial room temperature adhesive strength Fn is 7.0 N / 25 mm or higher, it exhibits excellent adhesion to the substrate. 1 From the viewpoint of ensuring that the peeling force is sufficiently reduced when heated, the value should be, for example, 50 N / 25 mm or less.
[0020] Initial room temperature adhesive strength Fn 1 and adhesive strength Fh at 60°C after storage 2 Methods for adjusting the adhesive strength include, for example, selecting the type of base polymer in the adhesive layer of the present invention, adjusting the molecular weight, adjusting the degree of crosslinking, and adjusting the blending amount. Methods for these adjustments include, for example, selecting the type of monofunctional monomer, polyfunctional polymerizable compound (crosslinking agent), and polymerization initiator and adjusting their blending amounts during base polymer formation. Initial room temperature adhesive strength Fn 1 and adhesive strength Fh at 60°C after storage 2 Methods for adjusting the initial 60°C adhesive strength Fh are also included in the present invention, such as selecting the type of component other than the base polymer in the adhesive layer and adjusting the amount of said component. Examples of such components include hydrophilic oligomers and silane coupling agents. These adjustment methods are described later in relation to the initial 60°C adhesive strength Fh 1 , room temperature adhesive strength Fn after storage 2 , high temperature and high humidity adhesive strength Fh 3 , and the adhesion strength Fn at room temperature after heating. 3 The same applies to this matter.
[0021] The base polymer contained in the adhesive layer of the present invention is a photopolymerizable polymer. A photopolymerizable polymer is a polymer formed by a polymerization method in which the polymerization reaction of polymerizable components is advanced by irradiation with light such as ultraviolet light. The adhesive layer of the present invention is preferably a solvent-free adhesive layer containing a photopolymerizable polymer as the base polymer. Such an adhesive layer can be manufactured from a solvent-free adhesive composition. In the process of manufacturing the adhesive layer from a solvent-free adhesive composition, there is no need to volatilize and remove the solvent from the coating film of the composition. Therefore, an adhesive sheet equipped with the above adhesive layer is suitable for reducing environmental impact. The adhesive layer of the present invention is preferably a sheet-like pressure-sensitive adhesive (solvent-free adhesive sheet).
[0022] The base polymer is an adhesive component that exhibits tackiness in the adhesive layer of the present invention. The base polymer is not particularly limited, but examples include acrylic polymers, rubber polymers (such as natural rubber polymers and synthetic rubber polymers), silicone polymers, polyester polymers, urethane polymers, polyamide polymers, epoxy polymers, vinyl alkyl ether polymers, and fluorine polymers. One or more of the base polymers may be used.
[0023] The content of the base polymer in the adhesive layer of the present invention is not particularly limited, but is preferably 75% by mass or more (for example, 75 to 99.9% by mass) and more preferably 85% by mass or more (for example, 85 to 99.5% by mass) based on the total amount (100% by mass) of the adhesive layer.
[0024] Acrylic polymers are polymers (polymers) that contain acrylic monomers (acrylic monomers) as essential monomer units (monomer units, monomer constituent units). In other words, acrylic polymers are polymers that contain constituent units derived from acrylic monomers as constituent units. That is, acrylic polymers are polymers that are composed (formed) with acrylic monomers as essential monomer components. In this specification, "(meth)acrylic" refers to either or both of "acrylic" and "methacrylic," and the same applies to other terms. The weight-average molecular weight of the acrylic polymer in the adhesive layer is not particularly limited, but is preferably between 100,000 and 5,000,000.
[0025] The above acrylic polymer is preferably a polymer that contains an alkyl (meth)acrylate having a linear or branched alkyl group as a monomer unit (hereinafter sometimes simply referred to as "alkyl (meth)acrylate").
[0026] Examples of the alkyl methacrylates mentioned above include methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate (n-butyl methacrylate), isobutyl methacrylate, s-butyl methacrylate, t-butyl methacrylate, pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate (n-octyl methacrylate), 2-ethylhexyl methacrylate, and isooctyl methacrylate. Examples include alkyl esters of (meth)acrylates having 1 to 24 carbon atoms in the alkyl group, such as nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl ((meth)acrylate) (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Note that one type of alkyl ester of (meth)acrylate may be used, or two or more types may be used.
[0027] Among alkyl acrylates, alkyl acrylates are preferred over alkyl methacrylates because they can shorten the polymerization time of the acrylic polymer and improve productivity. In particular, alkyl acrylates are preferred when the acrylic polymer is cured by active energy ray polymerization.
[0028] Among these, alkyl (meth)acrylate esters having 1 to 18 carbon atoms in the alkyl group are preferred because they exhibit appropriate adhesive strength to the adherend.
[0029] The proportion of the alkyl (meth)acrylate ester described above is not particularly limited, but in order to exhibit a low dielectric constant and drop impact resistance, it is preferably 60 to 99% by mass, more preferably 75 to 98% by mass, and even more preferably 80 to 97% by mass, relative to 100% by mass of the total amount of monomer components constituting the acrylic polymer.
[0030] In this specification, when referring to "the total amount of monomer components constituting the base polymer," it also includes monomer components that are separately added to the adhesive composition containing the polymer (partial polymer, etc.) blended into the adhesive composition that forms the adhesive layer of the present invention. Furthermore, in this specification, "monomer component" refers to a compound having only one polymerizable functional group and does not include compounds having two or more polymerizable functional groups, such as polyfunctional (meth)acrylates.
[0031] The monomer component preferably contains an alkyl (meth)acrylate having an alkyl group with 8 or more carbon atoms (sometimes referred to as "alkyl (meth)acrylate (A)"). Alkyl (meth)acrylate (A) has a medium-chain to long-chain alkyl group, making it easy to achieve a low dielectric constant while exhibiting high tackiness.
[0032] Examples of the above-mentioned alkyl (meth)acrylate (A) include alkyl (meth)acrylates with 8 to 24 carbon atoms in the alkyl group, such as octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.
[0033] Of the alkyl (meth)acrylate (A) mentioned above, alkyl acrylate is preferred over alkyl methacrylate in that it can shorten the polymerization time of the acrylic polymer and improve productivity. In particular, alkyl acrylate is preferred from the viewpoint of superior UV curability.
[0034] The proportion of the above-mentioned alkyl (meth)acrylate (A) is not particularly limited, but from the viewpoint of appropriately exhibiting basic properties such as tackiness when used as an adhesive sheet, it is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 93% by mass or more, even more preferably 95% by mass or more, and particularly preferably 96% by mass or more, based on 100% by mass of the total amount of monomer components constituting the above-mentioned acrylic polymer. The above proportion may be, for example, 99.9% by mass or less, 99.5% by mass or less, or 99% by mass or less.
[0035] The above-mentioned acrylic polymer may contain, in addition to the above-mentioned alkyl (meth)acrylate, copolymerizable functional group-containing monomers (copolymerizable functional group-containing monomers) as monomer units. In other words, the acrylic polymer may contain functional group-containing monomers as constituent monomer components. Note that only one type of functional group-containing monomer may be used, or two or more types may be used.
[0036] Examples of the functional group-containing monomers include polar group-containing monomers. Examples of the polar group-containing monomers include hydroxyl group-containing monomers, carboxyl group-containing monomers, and monomers having a nitrogen atom-containing ring. The polar group-containing monomers are useful for modifying acrylic polymers, such as ensuring the cohesive force of acrylic polymers. The polar group-containing monomer is preferably at least one selected from the group consisting of hydroxyl group-containing monomers and monomers having a nitrogen atom-containing ring, and more preferably a hydroxyl group-containing monomer.
[0037] Examples of the above hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. Of the above hydroxyl group-containing monomers, 2-hydroxyethyl acrylate (2HEA) and 4-hydroxybutyl acrylate (4HBA) are preferred. Note that only one type of hydroxyl group-containing monomer may be used, or two or more types may be used.
[0038] The proportion of the above-mentioned hydroxyl group-containing monomer is not particularly limited, but from the viewpoint of ensuring cohesive force when used as an adhesive sheet, it is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 1% by mass or more, based on 100% by mass of the total amount of monomer components constituting the above-mentioned acrylic polymer. From the viewpoint of controlling the polarity of the acrylic polymer and ensuring compatibility with other additives, the above proportion is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less.
[0039] Examples of the above-mentioned carboxyl group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid. Note that only one type of carboxyl group-containing monomer may be used, or two or more types may be used.
[0040] The proportion of the above-mentioned carboxyl group-containing monomer is not particularly limited, but from the viewpoint of further suppressing the risk of corrosion of the adherend by acid, it is preferably 3% by mass or less, more preferably 2% by mass or less, even more preferably 1% by mass or less, even more preferably 0.5% by mass or less, and particularly preferably 0.1% by mass or less, based on 100% by mass of the total amount of monomer components constituting the above-mentioned acrylic polymer.
[0041] The adhesive layer of the present invention contains, together with the base polymer, an oligomer containing 3 to 8% by mass of constituent units derived from a hydrophilic monomer. In this specification, an oligomer containing 3 to 8% by mass of constituent units derived from a hydrophilic monomer may be referred to as a "hydrophilic oligomer." In contrast, an oligomer in which the proportion of constituent units derived from a hydrophilic monomer is less than 3% by mass may be referred to as a "hydrophobic oligomer," and an oligomer containing more than 8% by mass of constituent units derived from a hydrophilic monomer may be referred to as a "highly hydrophilic oligomer." In this specification, the weight-average molecular weight of the oligomer is, for example, 1,000 to 30,000. The weight-average molecular weight of the above oligomer is measured by gel permeation chromatography (GPC) and calculated on a polystyrene basis.
[0042] In the adhesive layer of the present invention, the hydrophilic oligomer may or may not be bound to the base polymer, at least in part.
[0043] Acrylic oligomers are preferred as the hydrophilic oligomers. That is, the hydrophilic oligomers are preferably hydrophilic acrylic oligomers. Acrylic oligomers are oligomers that are polymers of monomer components containing (meth)acrylic acid ester in a proportion of 50% by mass or more.
[0044] Examples of the hydrophilic monomers mentioned above include hydroxyl group-containing monomers and carboxyl group-containing monomers. Only one type of hydrophilic monomer may be used, or two or more types may be used.
[0045] Examples of the above-mentioned hydroxyl group-containing monomers include hydroxyalkyl esters of (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.
[0046] Examples of the above-mentioned carboxyl group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0047] The proportion of hydrophilic monomers in the hydrophilic oligomer is 3% by mass or more, preferably 4% by mass or more, based on 100% by mass of the total amount of monomer components constituting the hydrophilic oligomer. When the above proportion is 3% by mass or more, the adhesion force will not decrease sufficiently by heating even after a long period of time has passed since bonding. The above proportion is 8% by mass or less, preferably 7% by mass or less. When the above proportion is 8% by mass or less, compatibility between the base polymer in the adhesive layer and the hydrophilic oligomer can be ensured, and sufficient adhesion to the adherend will be achieved both initially and after a long period of time has passed since bonding.
[0048] The above-mentioned hydrophilic oligomer (preferably a hydrophilic acrylic oligomer) preferably contains an alkyl (meth)acrylate having a linear or branched alkyl group (hereinafter sometimes simply referred to as "alkyl (meth)acrylate") as a constituent monomer component.
[0049] Examples of the alkyl (meth)acrylate esters mentioned above include the alkyl (meth)acrylate esters exemplified and described as monomer components that can constitute the acrylic polymers described above. Among these, methyl methacrylate (MMA) is preferred because it has a high glass transition temperature and relatively high compatibility with the base polymer. One or more of the alkyl (meth)acrylate esters may be used.
[0050] The proportion of alkyl (meth)acrylate in the hydrophilic oligomer is preferably 5 to 60% by mass, more preferably 7 to 55% by mass, and even more preferably 10 to 50% by mass, based on 100% by mass of the total amount of monomer components constituting the hydrophilic oligomer. When the above proportion is 5% by mass or more, it helps to ensure compatibility between the base polymer in the adhesive layer and the hydrophilic oligomer. When the above proportion is 60% by mass or less, the adhesive strength and cohesive strength of the adhesive layer can be ensured, and the adhesion to the adherend is more sufficient both initially and after a long period of time has passed since bonding.
[0051] The above-mentioned hydrophilic oligomer (preferably a hydrophilic acrylic oligomer) preferably contains an alkyl (meth)acrylate having an alicyclic alkyl group (hereinafter sometimes simply referred to as "alicyclic alkyl (meth)acrylate") as a constituent monomer component.
[0052] Examples of the above-mentioned alicyclic alkyl (meth)acrylates include dicyclopentanyl acrylate (DCPA), dicyclopentanyl methacrylate (DCPMA), cyclohexyl acrylate (CHA), cyclohexyl methacrylate (CHMA), and isobornyl acrylate (IBXA). One type of the above-mentioned alicyclic alkyl (meth)acrylate may be used, or two or more types may be used.
[0053] In other words, the hydrophilic oligomer is preferably a polymer of a monomer component comprising a hydroxyl group-containing monomer, at least one selected from the group consisting of DCPA, DCPMA, CHA, CHMA, and IBXA, and MMA.
[0054] The proportion of alicyclic alkyl (meth)acrylate in the hydrophilic oligomer is preferably 30 to 90% by mass, more preferably 40 to 88% by mass, and even more preferably 45 to 85% by mass, based on 100% by mass of the total amount of monomer components constituting the hydrophilic oligomer. When the above proportion is 30% by mass or more, the adhesive strength and cohesive strength of the adhesive layer can be ensured, and the adhesion to the adherend is more sufficient both initially and after a long period of time has passed since bonding. When the above proportion is 90% by mass or less, it helps to ensure the compatibility between the base polymer in the adhesive layer and the hydrophilic oligomer.
[0055] The hydrophilic oligomer described above is obtained by polymerizing polymerizable components such as monomer components that constitute the hydrophilic oligomer. Examples of polymerization methods include solution polymerization, bulk polymerization, and emulsion polymerization. Hydrophilic oligomers are preferably formed by solution polymerization. Examples of solvents in solution polymerization include toluene and ethyl acetate. In the polymerization of hydrophilic oligomers, thermal polymerization initiators may be used, and chain transfer agents may be used for the purpose of adjusting the molecular weight. After the formation of the hydrophilic oligomer, low molecular weight components and solvents may be removed from the reaction system, such as the reaction solution, by heating. Examples of low molecular weight components include unreacted monomers, chain transfer agents, thermal polymerization initiators, and their decomposition products (residues).
[0056] Examples of thermal polymerization initiators used in the polymerization of the above-mentioned hydrophilic oligomer include azo polymerization initiators and peroxide polymerization initiators. Examples of azo polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, and 2,2'-azobis(2-methylpropionic acid)dimethyl. Examples of peroxide polymerization initiators include dibenzoyl peroxide, t-butyl permaleate, and lauroyl peroxide. One or more of the above-mentioned thermal polymerization initiators may be used.
[0057] Examples of chain transfer agents used in the polymerization of the above-mentioned hydrophilic oligomers include α-thioglycerol, lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, 2,3-dimercapto-1-propanol, and α-methylstyrene dimer.
[0058] The weight-average molecular weight (Mw) of the hydrophilic oligomer is preferably 1000 or more, more preferably 1200 or more, even more preferably 1400 or more, even more preferably 1500 or more, even more preferably 1700 or more, even more preferably 1800 or more, and particularly preferably 2000 or more, from the viewpoint of ensuring the adhesive strength and cohesive strength of the adhesive layer. Furthermore, the weight-average molecular weight is preferably 30000 or less, more preferably 27000 or less, even more preferably 25000 or less, even more preferably 23000 or less, even more preferably 20000 or less, even more preferably 17000 or less, even more preferably 15000 or less, even more preferably 13000 or less, even more preferably 10000 or less, and particularly preferably 8000 or less. The weight-average molecular weight of the hydrophilic oligomer is measured by gel permeation chromatography (GPC) and calculated on a polystyrene basis.
[0059] The glass transition temperature (Tg) calculated from the monomer components constituting the hydrophilic oligomer is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 105°C or higher. When the glass transition temperature (Tg) is 80°C or higher, adhesive strength can be exhibited even in high-temperature environments such as 60°C. Furthermore, there is no particular upper limit, but from the viewpoint of exhibiting minimum adhesive strength, it is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 135°C or lower.
[0060] The glass transition temperature (Tg) mentioned above is a calculated glass transition temperature derived from the following Fox equation. This calculated glass transition temperature is determined based on the type and amount of each monomer component constituting the hydrophilic oligomer, and therefore can be adjusted by selecting the type and amount of each monomer component.
[0061] The above calculated glass transition temperature (calculated Tg) can be calculated from the following Fox equation [1]: 1 / calculated Tg = W1 / Tg(1) + W2 / Tg(2) + ... + Wn / Tg(n) [1] Here, W1, W2, ... Wn represent the weight fraction (weight %) of each monomer component (1), monomer component (2), ... monomer component (n) that constitute the hydrophilic oligomer, relative to the total monomer components, and Tg(1), Tg(2), ... Tg(n) represent the glass transition temperature (unit is absolute temperature: K) of the homopolymer of monomer component (1), monomer component (2), ... monomer component (n). In this specification, "glass transition temperature (Tg) of homopolymer" (sometimes simply referred to as "Tg of homopolymer") means "glass transition temperature (Tg) of the homopolymer of the monomer," and specifically, the values are given in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1987). For monomer homopolymers not listed in the above literature, except for monomers having a polyorganosiloxane skeleton, the Tg refers to the value obtained by, for example, the following measurement method (see Japanese Patent Publication No. 2007-51271). That is, 100 parts by mass of monomer, 0.2 parts by mass of 2,2'-azobisisobutyronitrile, and 200 parts by mass of ethyl acetate as a polymerization solvent are added to a reactor equipped with a thermometer, stirrer, nitrogen inlet tube, and reflux condenser, and the mixture is stirred for 1 hour while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and the reaction is carried out for 10 hours. Next, the mixture is cooled to room temperature to obtain a homopolymer solution with a solid content of 33% by mass. Then, this homopolymer solution is cast onto a release liner and dried to produce a test sample (sheet-like homopolymer) with a thickness of approximately 2 mm. This test sample is then punched out into a disc shape with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity is measured using a viscoelasticity tester (product name "ARES", manufactured by Rheometrics) in shear mode while applying a shear strain of 1 Hz at a temperature range of -70 to 150°C and a heating rate of 5°C / min. The peak top temperature of tanδ is taken as the Tg of the homopolymer.
[0062] The proportion of the hydrophilic oligomer in the adhesive layer of the present invention is preferably 0.3% by mass or more, more preferably 0.4% by mass or more, even more preferably 0.45% by mass or more, and particularly preferably 0.5% by mass or more, based on 100% by mass of the total amount of the adhesive layer of the present invention. When the above proportion is 0.3% by mass or more, the adhesion to the adherend is more sufficient both initially and after a long period of time has passed since bonding. Furthermore, even after a long period of time has passed since bonding, the adhesion is sufficiently reduced by heating. The above proportion is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 4% by mass or less, even more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. When the above proportion is 10% by mass or less, the adhesion to the adherend is more sufficient both initially and after a long period of time has passed since bonding.
[0063] The adhesive layer of the present invention may contain other components besides the base polymer and hydrophilic oligomer. Examples of these other components include photopolymerizable polyfunctional compounds (polyfunctional monomers and polyfunctional oligomers), polymerization initiators (such as photopolymerization initiators and thermal polymerization initiators), ultraviolet absorbers, antioxidants, silane coupling agents, and rust inhibitors. These other components may be present in the adhesive layer in an unreacted state, or they may participate in the polymerization reaction and be incorporated as constituent units of any of the polymers (or oligomers). It is preferable that oligomers other than hydrophilic oligomers (polyfunctional oligomers, hydrophobic oligomers, highly hydrophilic oligomers) are not included, and for example, the amount of these other components is 50 parts by mass or less, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the hydrophilic polymer. Each of these other components may be used individually or in combination of two or more.
[0064] Examples of the above-mentioned photopolymerizable polyfunctional compounds include polyfunctional monomers and polyfunctional oligomers. Among these, it is preferable that the above-mentioned photopolymerizable polyfunctional compound contains a polyfunctional monomer. Only one type of photopolymerizable polyfunctional compound may be used, or two or more types may be used.
[0065] The adhesive layer of the present invention may contain the above-mentioned photopolymerizable polyfunctional compound in an unreacted state, or it may contain it as a polymer (or oligomer) formed by photopolymerization proceeding in a reaction system containing the above-mentioned photopolymerizable polyfunctional compound. Here, the above-mentioned oligomer (or polymer) may constitute a part of the base polymer by forming a crosslinked structure with the base polymer, or it may not form a crosslinked structure with the base polymer.
[0066] Examples of the polyfunctional monomers include polyfunctional (meth)acrylates containing two or more ethylenically unsaturated double bonds in one molecule. From the viewpoint of ease of introducing crosslinking structures by photopolymerization, polyfunctional (meth)acrylates are preferred as polyfunctional monomers. From the viewpoint of efficiency of the photopolymerization reaction, polyfunctional acrylates are preferred as polyfunctional (meth)acrylates. Examples of polyfunctional (meth)acrylates include difunctional (meth)acrylates, trifunctional (meth)acrylates, and polyfunctional (meth)acrylates with four or more functions. Only one type of polyfunctional monomer may be used, or two or more types may be used.
[0067] Examples of the above-mentioned difunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol dimethacrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, stearic acid-modified pentaerythritol di(meth)acrylate, and di(meth)acryloyl isocyanurate.
[0068] Examples of the above-mentioned trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(acryloyloxyethyl) isocyanurate.
[0069] Examples of polyfunctional (meth)acrylates with four or more functions mentioned above include ditrimethylolpropanetetra(meth)acrylate, pentaerythritoltetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol pentaacrylate, and dipentaerythritol hexa(meth)acrylate.
[0070] The amount of the polyfunctional polymerizable compound and / or structural component derived therefrom in the adhesive layer of the present invention is preferably 0.025 parts by mass or more, more preferably 0.04 parts by mass or more, and even more preferably 0.06 parts by mass or more, based on 100 parts by mass of the total amount of monomer components (monomer components constituting the base polymer and oligomer) in the adhesive layer. When the above amount is 0.025 parts by mass or more, the cohesive force can be increased and the adhesive reliability after bonding to the adherend can be improved. The above amount is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less. When the above amount is 1 part by mass or less, the wettability of the adhesive layer to the adherend can be ensured and the initial adhesive strength to the adherend can be ensured.
[0071] The adhesive layer of the present invention exhibits an adhesive strength Fn when peeled off after being bonded to the Sn surface of alkali glass, stored at 50°C for one week, and then peeled off under the conditions of 25°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 2 However, it is preferably 7.0 N / 25 mm or more, more preferably 7.2 N / 25 mm or more, and more preferably 7.5 N / 25 mm or more. Adhesion strength Fn 2 If the adhesive strength is 7.0 N / 25 mm or higher, it will have excellent adhesion to the substrate even after long-term storage. 2 From the viewpoint of sufficiently reducing the peeling force when heated, the adhesive strength Fn is, for example, 50 N / 25 mm or less. 2 "Adhesion strength Fn at room temperature after storage" 2 It is sometimes referred to as "[...]."
[0072] The adhesive layer of the present invention exhibits an adhesive strength Fh when peeled off after being bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, and then peeled off under the conditions of 60°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 1 However, it is preferably 1.5 N / 25 mm or more, more preferably 1.8 N / 25 mm or more, and even more preferably 2.0 N / 25 mm or more. Adhesion force Fh 1 If the adhesive strength is 1.5 N / 25 mm or higher, it is less likely to detach during heating and has excellent heat resistance. 1 Adhesion strength Fh is preferably 3.5 N / 25 mm or less, more preferably 3.2 N / 25 mm or less, and even more preferably 3.0 N / 25 mm or less. 1 If the adhesive strength is 3.5 N / 25 mm or less, the adhesive strength will decrease upon heating and it will be easily peeled off. In this specification, the above adhesive strength Fh 1 "Initial 60°C Adhesion Fh" 1 It is sometimes referred to as "[...]."
[0073] The adhesive layer of the present invention has an initial adhesive strength Fh at 60°C. 1 and adhesive strength Fh at 60°C after storage 2 Regarding this, the value represented by the following formula (1) (adhesion change rate at 60°C) is preferably 50% or less, more preferably 45% or less, and even more preferably 35% or less. When the adhesion change rate at 60°C is 50% or less, the phenomenon in which the adhesive strength increases due to long-term storage and becomes difficult to peel off by heating can be suppressed. Furthermore, from the viewpoint of excellent heat resistance, the adhesion change rate at 60°C is preferably -5% or more, but may be 0% or more, 10% or more, 20% or more, or 30% or more. [(Adhesion Fh 2 - Adhesion Fh 1 ) / Adhesion Fh 1 ] × 100 [%] (1)
[0074] The adhesive layer of the present invention was bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, heated at 60°C for 3 minutes, then stored at room temperature for 1 hour, and the adhesive strength Fn was obtained when peeled off under the conditions of 25°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 3However, it is preferably 7.0 N / 25 mm or more, more preferably 7.2 N / 25 mm or more, and more preferably 7.5 N / 25 mm or more. Adhesion strength Fn 3 If the adhesive strength is 7.0 N / 25 mm or higher, the adhesive sheet will have excellent adhesion to the substrate even after being peeled off at high temperatures, and the adhesive sheet can be reused. 3 From the viewpoint of sufficiently reducing the peeling force when heated, the adhesive strength Fn is, for example, 50 N / 25 mm or less. 3 "Adhesion strength Fn at room temperature after heating" 3 It is sometimes referred to as "[...]."
[0075] In the adhesive layer of the present invention, the adhesive strength Fn 3 Adhesion Fn 1 It is preferable that it be 80% or more, more preferably 90% or more, even more preferably 100% or more, and may be 110% or more. When it is 80% or more, the adhesion to the substrate is equal to or better than that at the time of initial use even after peeling at high temperature, and the reusability of the adhesive sheet is excellent. Also, the adhesive strength Fn 3 Adhesion Fn 1 It is preferably 150% or less, more preferably 140% or less, even more preferably 130% or less, and may also be 120% or less. When it is 150% or less, the adhesion to the substrate does not increase significantly from the initial use after peeling at high temperature, the peeling force can be sufficiently reduced when heated further, and the adhesive sheet has excellent reusability.
[0076] The adhesive layer of the present invention exhibits an adhesive strength Fh when peeled off after being bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, and then peeled off under the conditions of 60°C, 90% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 3 However, it is preferably 1.5 N / 25 mm or more, more preferably 1.7 N / 25 mm or more, and even more preferably 2.0 N / 25 mm or more. Adhesion force Fh 3 If the adhesive strength is 1.5 N / 25 mm or higher, it is less likely to detach when heated, even in high-temperature and high-humidity environments, and has excellent heat resistance. 3Adhesion strength Fh is preferably 4.0 N / 25 mm or less, more preferably 3.5 N / 25 mm or less, and even more preferably 3.0 N / 25 mm or less. 3 If the adhesive strength is 4.0 N / 25 mm or less, the adhesive strength will decrease upon heating, even in a high-humidity environment, and it can be easily peeled off. That is, the adhesive strength Fh 3 When the adhesive strength Fh is within the above range, it is possible to achieve both adhesion to the substrate and peelability by heating, even in a high-humidity environment, and it has excellent reliability in humidification heat. 3 "High temperature and high humidity adhesive strength Fh" 3 It is sometimes referred to as "[...]."
[0077] In the adhesive layer of the present invention, the proportion of gel insoluble in ethyl acetate (gel fraction) is preferably 68% by mass or more, more preferably 69% by mass or more, and even more preferably 70% by mass or more. When the gel fraction is 68% by mass or more, adhesive residue is less likely to remain on the adherend after peeling by heating. From the viewpoint of ensuring sufficient adhesion to the adherend, the gel fraction is preferably 80% by mass or less, more preferably 77% by mass or less, and even more preferably 75% by mass or less. The gel fraction can be calculated as follows.
[0078] First, approximately 0.1 g (mass: W) of the adhesive layer to be identified as the gel fraction is taken. 1 A sample of 0.2 mg was taken and a porous membrane made of tetrafluoroethylene resin with an average pore size of 0.2 μm was prepared (mass: W 2 Wrapped in mg and tied with kite string (mass: W 3 Tie the package with a weight (mg) to obtain a wrapper. Next, immerse this wrapper in approximately 50 mL of ethyl acetate solution and leave it standing in the ethyl acetate solution at room temperature (typically 23°C) for 7 days. Next, remove the wrapper containing the gel component, which is insoluble in ethyl acetate, from the ethyl acetate solution and dry the wrapper at 130°C for 1 hour. After that, measure the total mass (W) of the wrapper. 4 Measure (mg). Then, W 1 ~W 4 The gel fraction is calculated by substituting the value of into the following formula: Gel fraction (mass%) = [(W 4 -W 2 -W 3 ) / W 1] × 100
[0079] In the adhesive layer of the present invention, the weight-average molecular weight of the sol component soluble in ethyl acetate is preferably 200,000 or more, more preferably 300,000 or more, and even more preferably 400,000 or more. When the weight-average molecular weight is 200,000 or more, adhesive residue is less likely to remain on the adherend after peeling by heating. From the viewpoint of ensuring sufficient adhesion to the adherend, the weight-average molecular weight is preferably 900,000 or less, more preferably 800,000 or less, and even more preferably 700,000 or less. The weight-average molecular weight of the sol component can be determined as follows.
[0080] First, approximately 0.1 g of sample is taken from the adhesive layer to be identified as sol molecular weight, wrapped in a porous membrane made of tetrafluoroethylene resin with an average pore size of 0.2 μm, and tied with kite string to obtain a package. Next, this package is immersed in approximately 50 mL of ethyl acetate solution and left to stand in the ethyl acetate solution at room temperature (typically 23°C) for 7 days. Next, the package containing the ethyl acetate insoluble portion is separated from the ethyl acetate solution containing the ethyl acetate soluble sol portion. Next, the ethyl acetate solution containing the sol portion is subjected to reduced-pressure drying at 30°C to evaporate the ethyl acetate and obtain a solid. Next, this solid is weighed. Next, the molecular weight of the sol portion is measured by GPC (gel permeation chromatography). For example, using a GPC measuring device (product name "HLC-8120GPC", manufactured by Tosoh Corporation), the weight-average molecular weight of the sol portion can be determined by polystyrene equivalent value under the following measurement conditions. [GPC Measurement Conditions] • Column: Two TSKgel GMHHR-H(S) columns in series (manufactured by Tosoh Corporation) • Column size: 7.8 mmφ × 30 cm • Column temperature: 40°C • Eluent: Tetrahydrofuran (THF) • Flow rate: 0.5 ml / min • Sample injection volume: 100 μl • Sample concentration: 0.1% by mass • Standard sample: Polystyrene • Detector: Differential refractometer (RI)
[0081] The adhesive layer of the present invention preferably has a coefficient of thermal expansion (linear expansion coefficient) expressed as the ratio of the thickness at 60°C to the thickness at 25°C, of 0.30% or more, more preferably 0.40% or more, and even more preferably 0.45% or more. A coefficient of thermal expansion of 0.30% or more can mitigate stress concentration on the adhesive surface due to dimensional changes in the bonded materials. The coefficient of thermal expansion is preferably 0.60% or less, more preferably 0.58% or less, and even more preferably 0.55% or less. A coefficient of thermal expansion of 0.60% or less can suppress peeling of the adhesive layer due to excessive deformation caused by heat. The coefficient of thermal expansion can be calculated by measuring the dimensional change when the adhesive layer is cut into approximately 5 mm squares and the temperature is changed from 25°C to 60°C, using the following formula. The dimensional change can be obtained, for example, by performing TMA measurement in compression mode using a "TMA / SS6000" manufactured by Hitachi High-Tech Science Corporation. Coordinate of thermal expansion [%] = (thickness at 60°C - thickness at 25°C) / thickness at 25°C × 100
[0082] The haze of the adhesive layer of the present invention (according to JIS K7136) is not particularly limited, but is preferably 1.0% or less, and more preferably 0.8% or less. When the haze is 1.0% or less, excellent transparency and excellent appearance can be obtained. The above haze is not particularly limited, but theoretically it may be 0%, and in practice it may be more than 0.01%. The above haze can be measured, for example, by preparing an adhesive layer (thickness: 100 μm), leaving it at normal conditions (23°C, 50% RH) for at least 24 hours, and then attaching it to a glass slide (for example, one with a total light transmittance of 92% and a haze of 0.2%) as a sample, and measuring it using a haze meter (manufactured by Murakami Color Technology Laboratory Co., Ltd., product name "HM-150N") or an equivalent product. Furthermore, it is preferable that the haze of the adhesive layer of the present invention after storage at 60°C for 24 hours is within the above range.
[0083] The total light transmittance (according to JIS K7361-1) of the adhesive layer of the present invention in the visible light wavelength range is not particularly limited, but is preferably 90% or more, more preferably 91% or more, and even more preferably 92% or more. When the total light transmittance is 90% or more, excellent transparency and excellent appearance can be obtained. The above total light transmittance is not particularly limited, but theoretically it is the value obtained by subtracting the light loss due to reflection at the air interface (Fresnel loss) from 100%, and in practice it may be 95% or less. The above total light transmittance can be measured, for example, by taking an adhesive layer (thickness: 100 μm), leaving it at normal conditions (23°C, 50% RH) for at least 24 hours, peeling off the release liner if one is present, and attaching it to a glass slide (for example, one with a total light transmittance of 92% and haze of 0.2%) as a sample, and measuring it using a haze meter (manufactured by Murakami Color Technology Laboratory Co., Ltd., product name "HM-150N") or an equivalent product.
[0084] The water contact angle of the adhesive layer of the present invention is preferably 80° or higher, more preferably 85° or higher, and even more preferably 90° or higher. When the water contact angle is 80° or higher, adhesion to various plastics can be ensured. The water contact angle is preferably 120° or lower, more preferably 115° or lower, and even more preferably 110° or lower. When the water contact angle is 120° or lower, sufficient adhesion to glass can be achieved. The water contact angle is measured in accordance with JIS R3257. The water contact angle can be adjusted by the type of base polymer and oligomer in the adhesive layer of the present invention, the type and amount of crosslinking agent, the thickness of the adhesive layer, the type of release liner (more precisely, the type and amount of release agent), etc.
[0085] The thickness of the adhesive layer of the present invention is preferably 10 μm or more, and more preferably 20 μm or more. When the above thickness is 10 μm or more, the adhesive strength necessary for the adhesive can be provided. From the viewpoint of handling and ease of cutting, the above thickness is preferably 500 μm or less, more preferably 400 μm or less, even more preferably 300 μm or less, even more preferably 200 μm or less, and particularly preferably 150 μm or less.
[0086] The adhesive layer of the present invention is formed from an adhesive composition. The adhesive composition is not particularly limited, but examples include a composition in which a mixture of monomer components constituting a base polymer (sometimes referred to as a "monomer mixture") or a partially polymerized thereof and a hydrophilic oligomer are essential components. In this specification, the "monomer mixture" includes cases where it is composed of a single monomer component and cases where it is composed of two or more monomer components. Furthermore, the "partially polymerized monomer mixture" may also be referred to as a "prepolymer," "syrup," etc., and means a composition in which one or more monomer components of the "monomer mixture" are partially polymerized.
[0087] The above base polymer is formed by photopolymerization of a monomer mixture and / or a partial polymer. The polymerizable components (including monofunctional monomers and polyfunctional polymerizable compounds for introducing crosslinking structures) may be polymerized in a single step or in multiple steps. In the multi-step polymerization method, first, a prepolymer composition containing a partial polymer (a mixture of a polymer of monofunctional monomers and unreacted monofunctional monomers) is prepared by polymerizing monofunctional monomers (pre-polymerization). Next, a polyfunctional polymerizable compound as a crosslinking agent is added to the prepolymer composition, and then the polymerization reaction proceeds in a reaction system containing the partial polymer and the polyfunctional polymerizable compound (main polymerization).
[0088] The above adhesive composition may contain polymerization initiators, chain transfer agents, emulsifiers, etc., used for the radical polymerization of the monomer component. The weight-average molecular weight of the polymer can be controlled by the amount of polymerization initiator and chain transfer agent used and the reaction conditions, and the appropriate amounts used are adjusted according to their types.
[0089] Photopolymerization initiators can be used for the polymerization of monomer components. One type of polymerization initiator may be used, or two or more types may be used.
[0090] The above-mentioned photopolymerization initiators are not particularly limited, but examples include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators. Other examples include acylphosphine oxide-based photopolymerization initiators and titanocene-based photopolymerization initiators. Examples of the above-mentioned benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one, and anisole methyl ether. Examples of the above acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of the above α-ketol-based photopolymerization initiators include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of the above aromatic sulfonyl chloride-based photopolymerization initiators include 2-naphthalenesulfonyl chloride. Examples of the above photoactive oxime-based photopolymerization initiators include 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of the above benzoin-based photopolymerization initiators include benzoin. Examples of the above benzyl-based photopolymerization initiators include benzyl. Examples of the benzophenone-based photopolymerization initiators mentioned above include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexylphenyl ketone. Examples of the ketal-based photopolymerization initiators mentioned above include benzyldimethyl ketal.Examples of the thioxanthone-based photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone. Examples of the acylphosphine oxide-based photopolymerization initiators include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Examples of the titanocene-based photopolymerization initiators include bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrole-1-yl)-phenyl)titanium. The amount of photopolymerization initiator used can be the usual amount, for example, it can be selected from a range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of monomer component.
[0091] The above adhesive composition may contain other components besides those described above, as long as they do not impair the effects of the present invention. Examples of these other components include those described and illustrated as other components that may be included in the adhesive layer of the present invention. Each of these other components may be used individually or in combination of two or more.
[0092] The above adhesive composition is preferably solvent-free. That is, it is preferable that the above adhesive composition does not contain or substantially contains organic solvents. The above organic solvent is not particularly limited as long as it is an organic compound used as a solvent, but examples include hydrocarbon solvents such as cyclohexane, hexane, and heptane; aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate and methyl acetate; ketone solvents such as acetone and methyl ethyl ketone; and alcohol solvents such as methanol, ethanol, butanol, and isopropyl alcohol. The above organic solvent may be a mixed solvent containing two or more organic solvents.
[0093] In the above-mentioned adhesive composition, "substantially free of organic solvents" means that organic solvents are not actively incorporated except in cases where they are inevitably mixed in. Specifically, an adhesive composition in which the content of organic solvents is 1.0% by mass or less (preferably 0.5% by mass or less, and more preferably 0.2% by mass or less) relative to 100% by mass of the total amount of the adhesive composition can be said to be substantially free of organic solvents.
[0094] The above adhesive compositions can be prepared by known or conventional methods. For example, a photopolymerizable adhesive composition can be prepared by mixing a mixture of monomer components or a partial polymer thereof with a hydrophilic oligomer and, if necessary, other components.
[0095] The adhesive layer of the present invention can be produced, for example, by applying the adhesive composition to the release surface of a release liner or a substrate to form an adhesive composition layer, and then solidifying the adhesive composition layer by polymerization induced by light irradiation. In addition, heating, drying, etc. may be performed in addition to light irradiation as needed.
[0096] Examples of light used in the above photopolymerization include ionizing radiation such as alpha rays, beta rays, gamma rays, neutron rays, and electron beams, as well as active energy rays such as ultraviolet rays, with ultraviolet rays being particularly preferred.
[0097] A known coating method may be used for applying (coating) the above adhesive composition. For example, coaters such as gravure roll coaters, reverse roll coaters, kiss roll coaters, dip roll coaters, bar coaters, knife coaters, spray coaters, comma coaters, and direct coaters may be used.
[0098] After curing a monomer mixture or a partially polymer thereof by light irradiation to form an adhesive layer, a solution containing an additive may be applied to the adhesive layer, allowing the additive to penetrate from one side of the adhesive layer in the thickness direction. This allows the adhesive layer to be imparted with the desired properties due to the additive. Furthermore, the transparency of the adhesive layer is maintained as the additive penetrates in solution form. Subsequently, the adhesive layer is dried by heating or other means. This process returns the adhesive layer to a state close to that before application. That is, since the adhesive layer has been cured once, its physical properties such as adhesive strength and elastic modulus are restored to a state close to that before the above solution was applied. Because the adhesive layer is cured before the additive is added, once the composition, curing conditions, and physical properties of the adhesive composition are determined, there is no need to redesign the composition by adding an additive, and the thickness of the adhesive layer can be easily changed. Furthermore, the desired properties imparted to the adhesive layer can be controlled by changing the subsequent coating conditions of the additive solution. In this way, the control of the physical properties of the adhesive layer and the control of the required characteristics by additives can be separated, so there is no need to redesign the adhesive layer from scratch when changing the thickness of the adhesive layer or the amount of additives added, which is efficient.
[0099] (Substrate) The above substrate is not particularly limited, but examples include various optical films such as plastic films, anti-reflective (AR) films, anti-glare (AG) films, polarizing plates, and phase difference plates. Examples of materials for the above plastic films include polyester resins such as polyethylene terephthalate (PET), acrylic resins such as polymethyl methacrylate (PMMA), polycarbonate, triacetylcellulose (TAC), polysulfone, polyarylate, polyimide, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, ethylene-propylene copolymer, cyclic olefin polymers such as the trade name "Arton" (cyclic olefin polymer, manufactured by JSR Corporation) and the trade name "Zeonor" (cyclic olefin polymer, manufactured by Nippon Zeon Co., Ltd.), and fluorine polymers. Note that one or more of these plastic materials may be used.
[0100] The surface of the substrate on the side with the adhesive layer may be subjected to surface treatments such as physical treatments like corona discharge treatment, plasma treatment, sandblasting, ozone exposure treatment, flame exposure treatment, high-voltage electric shock exposure treatment, or ionization radiation treatment; chemical treatments like chromic acid treatment; or surface treatments such as easy adhesion treatment with a coating agent (primer) in order to improve adhesion and retention with the adhesive layer. It is preferable that the surface treatment to improve adhesion is applied to the entire surface of the substrate on the side with the adhesive layer.
[0101] The adhesive sheet of the present invention may have a release liner on the adhesive surface until use. The release liner protects the adhesive surface that comes into contact with the adhesive layer until use, and is peeled off when the adhesive layer is used. If the adhesive sheet of the present invention is a double-sided adhesive sheet, each adhesive surface may be protected by two release liners, or it may be protected by a single release liner with both sides being release surfaces, in a roll-like configuration. The release liner is used as a protective material for the adhesive layer and is peeled off when it is applied to the substrate. Furthermore, if the adhesive sheet is a substrate-less adhesive sheet, the release liner also serves as a support for the adhesive layer. Note that the release liner is not necessarily required.
[0102] Examples of substrates for the above-mentioned release liner include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polyethylene naphthalate film, polybutylene terephthalate film, polyurethane film, ethylene vinyl acetate film, ionomer resin film, ethylene-(meth)acrylic acid copolymer film, ethylene-(meth)acrylic acid ester copolymer film, polystyrene film, polycarbonate film, polyimide film, and fluororesin film. Crosslinked films of these are also acceptable. Furthermore, laminated films of these may also be used.
[0103] It is preferable that the release surface of the above-mentioned release liner (particularly the surface in contact with the adhesive layer) is subjected to a release treatment. Examples of release agents used in the release treatment include alkyd, silicone, fluorine, unsaturated polyester, polyolefin, and wax-based release agents.
[0104] The thickness of the release liner is not particularly limited, but is, for example, about 20 to 150 μm.
[0105] (Applications) The adhesive sheet of the present invention is preferably used for optical applications, that is, for bonding to optical components. More specifically, it is used, for example, for bonding optical components (for bonding optical components) or for manufacturing products using the above-mentioned optical components (optical products). Using the adhesive sheet of the present invention for optical applications provides excellent reliability.
[0106] The adhesive sheet of the present invention is used, for example, in optical components of electrical and electronic equipment to attach (mount) various members or parts to predetermined locations (e.g., housing, front panel, window portion, etc.). "Electrical and electronic equipment" refers to equipment that falls under at least one of either electrical equipment or electronic equipment. Examples of such electrical and electronic equipment include image display devices such as liquid crystal displays, organic / inorganic electroluminescent displays, and plasma displays, as well as portable electronic devices. Examples of such image display devices include image display devices in portable electronic devices, in-vehicle displays, and digital signage (electronic billboards). The image display device may be in a rigid or flexible form (structure), or it may be a foldable or rollable form (structure).
[0107] Examples of the above-mentioned portable electronic devices include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices (e.g., wristwear-type devices worn on the wrist like watches, modular devices attached to a part of the body with clips or straps, eyewear-type devices including glasses (monocular and binocular types, including head-mounted types), clothing-type devices attached to shirts, socks, hats, etc. as accessories, earwear-type devices attached to the ears like earphones, etc.), digital cameras, digital video cameras, audio equipment (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game consoles, electronic dictionaries, electronic organizers, e-books, in-car information systems, portable radios, portable televisions, portable printers, portable scanners, and portable modems. In this specification, "portable" means not merely being able to carry something, but having a level of portability that allows an individual (a typical adult) to carry it relatively easily.
[0108] A particularly preferred application of the adhesive sheet of the present invention is for bonding two cover members together, such as being placed between cover members of an optical product. It is especially preferable that the adhesive layer of the present invention is directly laminated to one of the cover members. Furthermore, the adhesive layer of the present invention may be directly laminated to the cover member, or it may be laminated via another layer such as a polarizing film.
[0109] Furthermore, the cover member is provided on the surface of the optical product to protect the inside of the optical product (for example, a touch sensor or an image display device). Examples of the cover member include a cover glass and a plastic cover. The adhesive sheet of the present invention is preferably used for bonding a cover glass and a plastic cover. That is, the adhesive sheet of the present invention is preferably used for bonding a glass plate and a plastic film. The plastic film is preferably a transparent plastic film (particularly PET film, polycarbonate film, or cyclic olefin polymer film).
[0110] The adhesive sheet of the present invention has the property of peeling off when heated. Therefore, the adhesive sheet of the present invention can be used for the peeling and recovery of optical components. The adhesive sheet of the present invention can be peeled off by heating it to, for example, 55°C or higher, preferably 60°C or higher.
[0111] The adhesive sheet of the present invention exhibits excellent adhesion to the substrate during use, is easily and safely removed when intentionally needed, and remains easily removable even after a long period of time has passed since application. Furthermore, it remains easily and safely removed when intentionally needed, even after storage in a high-temperature, high-humidity environment. Moreover, it maintains high adhesive strength and excellent adhesion to the substrate even after being heated and returned to room temperature, making it reusable.
[0112] [Optical member with adhesive layer] By bonding the adhesive layer of the present invention to an optical member, an optical member with an adhesive layer can be obtained, comprising an optical member and the adhesive layer of the present invention attached to at least one surface of the optical member. The adhesive layer of the optical member with an adhesive layer may or may not have a release liner on its adhesive surface until use.
[0113] The adhesive-coated optical component of the present invention may be one in which the adhesive layer of the present invention is bonded to a cover member of an optical product. The cover member is provided on the surface of the optical product (for example, the surface opposite to the side equipped with another cover member, polarizing film, or image display device of an OLED display panel) and protects the interior of the optical product (for example, a touch sensor or image display device). Examples of the cover member include the cover glass and plastic cover mentioned above. The optical product may be equipped with a polarizing film or an OLED display panel on the surface of the touch sensor.
[0114] The cover member in the adhesive-layered optical member of the present invention may have a functional layer such as a hard coat layer, an anti-reflective layer, or an anti-glare layer. An example of such a cover member is a plastic film on which the functional layer is formed. When the cover member is a plastic film having the functional layer, the adhesive-layered optical member of the present invention has the configuration of [functional layer / plastic film / adhesive layer of the present invention]. In such cases, when misalignment occurs when the adhesive-layered optical member of the present invention is attached to the surface of an optical product (for example, another cover member), or when peeling occurs near the bent part when the optical product is repeatedly bent, the adhesive-layered optical member can be peeled off the optical product by heating and attached to a new cover member.
[0115] [Optical Laminate] By providing the adhesive layer or adhesive sheet of the present invention on the surface of a laminate comprising a touch sensor and an image display device, an optical laminate (optical laminate of the present invention) comprising an image display device, a touch sensor, and the adhesive layer of the present invention in this order can be obtained. The optical laminate may comprise the touch sensor and the adhesive layer as single layers or as multiple layers. When multiple touch sensors are provided, it is preferable that the touch sensors are laminated with an adhesive layer in between. When multiple adhesive layers are provided, the multiple adhesive layers may be the same layer in terms of composition, thickness, etc., or may be different layers. The adhesive layer used between the touch sensor and the image display device, or the adhesive layer used between multiple touch sensors, may be the adhesive layer of the present invention, or other adhesive layers other than the adhesive layer of the present invention. The image display device is one of those described above.
[0116] The optical laminate may include the cover member described above. The cover member may be one of the cover members described above. The cover member may be bonded to another cover member or other layer constituting the optical laminate via the adhesive layer of the present invention. If misalignment occurs when the optical member with the adhesive layer, to which the adhesive layer of the present invention has been bonded to the cover member, is bonded to another cover member, or if peeling occurs near the bent portion when the optical laminate is repeatedly bent, the optical member with the adhesive layer can be peeled off from the optical laminate by heating and replaced with a new cover member. The optical laminate may also have a polarizing film on the surface of the touch sensor (the surface on which the cover member is attached).
[0117] Figures 2 and 3 show one embodiment of the optical laminate of the present invention. The optical laminate 1 shown in Figure 2 comprises, in this order, an image display device 5, a touchscreen panel 6 which is a display panel with a built-in touch sensor provided on the image display device 5, a polarizing film 4, a cover member 31, and a cover member 32. The touchscreen panel 6 and the polarizing film 4 are bonded together by an adhesive layer (adhesive sheet) 21, and the polarizing film 4 and the cover member 31 are bonded together by an adhesive layer (adhesive sheet) 22. The adhesive layers 21 and 22 may be the adhesive layer of the present invention or other adhesive layers. The cover members 31 and 32 are bonded together by an adhesive layer (adhesive sheet) 23. The adhesive layer 23 is the adhesive layer of the present invention.
[0118] Figure 3 shows one embodiment of the optical laminate of the present invention when a polarizing film is not used. The optical laminate 1 shown in Figure 3 comprises, in this order, an image display device 5, a touchscreen panel 6 provided on the image display device 5, an OLED display panel 100, a cover member 31, and a cover member 32. The OLED display panel 100 and the cover member 31 are bonded together by an adhesive layer 21. The adhesive layer 21 may be the adhesive layer of the present invention or another adhesive layer. The cover member 31 and the cover member 32 are bonded together by an adhesive layer 23. The adhesive layer 23 is the adhesive layer of the present invention.
[0119] Figure 4 shows one embodiment of the OLED display panel 100. The OLED display panel 100 includes a red OLED element 12R formed by stacking a transparent electrode 11a, a red OLED layer 10R that emits red light, and a back electrode 11b in that order; a green OLED element 12G formed by stacking a transparent electrode 11a, a green OLED layer 10G that emits green light, and a back electrode 11b in that order; and a blue OLED element 12B formed by stacking a transparent electrode 11a, a blue OLED layer 10B that emits blue light, and a back electrode 11b in that order. Each of the OLED elements 12R, 12G, and 12B of multiple colors is arranged sequentially on a substrate 13. A TFT (Thin Film Transistor) layer 14 is formed on the surface of the substrate 13 where each OLED element is arranged, and is connected to the back electrode 11b of each of the OLED elements 12R, 12G, and 12B of multiple colors.
[0120] In the OLED display panel 100, a color filter 15 is positioned on the viewing side (upper side in Figure 4) of each of the multiple-color OLED elements 12R, 12G, and 12B. The color filter 15 includes a red colored layer 15R, a green colored layer 15G, and a blue colored layer 15B, with a black matrix layer 16 provided between each colored layer. The color filter 15 is positioned so that the red colored layer 15R, the green colored layer 15G, and the blue colored layer 15B face the red OLED element 12R, the green OLED element 12G, and the blue OLED element 12B, respectively. The transparent electrode 11a is either a cathode or an anode, but is generally provided as a cathode. The back electrode 11b functions as the counter electrode to the transparent electrode 11a. The back electrode 11b is either an anode or a cathode, but is generally provided as an anode on the substrate 13. A bonding layer 17 is provided between the substrate 13 and the color filter 15. The bonding layer 17 is light-transmitting.
[0121] As shown in Figure 4, the white ambient light W passes, for example, through the red colored layer 15R, then through the transparent electrode 11a and the red OLED layer 10R that emits red light, is reflected by the back electrode 11b, and then passes again through the red OLED layer 10R, the transparent electrode 11a, and the red colored layer 15R, and the reflected light G enters the observer's eye. The OLED display panel 100 also has a microcavity structure. A first optical path C1 is formed in which a portion of the light emitted from the OLED layers 10R, 10G, and 10B proceeds to the transparent electrode 11a side without proceeding to the back electrode 11b side and is emitted to the outside through the transparent electrode 11a, and a second optical path C2 is formed in which the remaining portion of the light emitted from the OLED layers 10R, 10G, and 10B proceeds to the back electrode 11b side and is reflected by the back electrode 11b, and then is emitted to the outside through the OLED layers 10R, 10G, 10B and the transparent electrode 11a. The OLED layers 10R, 10G, and 10B are designed to have different thicknesses so that the light components corresponding to each color reinforce each other through interference between the direct light and the reflected light.
[0122] The embodiments described above are provided to facilitate understanding of the present invention and are not intended to limit it.
[0123] The present invention will be described in more detail below with reference to examples, but the present invention is not limited in any way by these examples. The units of the blending amounts of each component shown in the table are "parts by mass," which represent relative amounts.
[0124] [Production Example 1: Preparation of Oligomer A] First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 60 parts by mass of dicyclopentanyl methacrylate (DCPMA), 40 parts by mass of methyl methacrylate (MMA), 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 2 hours, and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove toluene, chain transfer agent, and unreacted monomers. This yielded a solid acrylic oligomer (Oligomer A). Oligomer A had a weight-average molecular weight of 5100 and a glass transition temperature of 130°C. Oligomer A is a hydrophobic oligomer.
[0125] [Production Example 2: Preparation of Oligomer B] First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 47.5 parts by mass of DCPMA, 47.5 parts by mass of MMA, 5 parts by mass of 2-hydroxyethyl methacrylate (HEMA), 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of AIBN as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 2 hours, and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove toluene, chain transfer agent, and unreacted monomers. This yielded a solid acrylic oligomer (oligomer B). The weight-average molecular weight of oligomer B was 5600, and the glass transition temperature was 120°C. Oligomer B is a hydrophilic oligomer.
[0126] [Production Example 3: Preparation of Oligomer C] First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 65 parts by mass of isobornyl acrylate (IBXA), 30 parts by mass of MMA, 5 parts by mass of 4-hydroxybutyl acrylate (4HBA), 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of AIBN as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 2 hours, and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove toluene, chain transfer agent, and unreacted monomers. This yielded a solid acrylic oligomer (Oligomer C). The weight-average molecular weight of Oligomer C was 5100, and the glass transition temperature was 120°C. Oligomer C is a hydrophilic oligomer.
[0127] [Production Example 4: Preparation of Oligomer D] First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 45 parts by mass of IBXA, 40 parts by mass of cyclohexyl methacrylate (CHMA), 10 parts by mass of MMA, 5 parts by mass of 4HBA, 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of AIBN as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 2 hours, and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated at 130°C to volatilize and remove toluene, chain transfer agent, and unreacted monomers. This yielded a solid acrylic oligomer (Oligomer D). Oligomer D had a weight-average molecular weight of 5500 and a glass transition temperature of 105°C. Oligomer D is a hydrophilic oligomer.
[0128] [Production Example 5: Preparation of Oligomer E] First, in a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing 45 parts by mass of DCPMA, 45 parts by mass of MMA, 10 parts by mass of HEMA, 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent was stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of AIBN as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 2 hours, and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove toluene, chain transfer agent, and unreacted monomers. This yielded a solid acrylic oligomer (oligomer E). The weight-average molecular weight of oligomer E was 5300, and the glass transition temperature was 115°C. Oligomer E is a highly hydrophilic oligomer.
[0129] [Production Example 6: Preparation of Prepolymer Composition A] A monomer mixture consisting of 58 parts by mass of 2-ethylhexyl acrylate (2EHA), 39 parts by mass of lauryl acrylate (LA), and 3 parts by mass of 4HBA was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.) and 0.05 parts by mass of another photopolymerization initiator (trade name "Omnirad 651", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, obtaining a prepolymer composition A with a polymerization rate of approximately 10%. This prepolymer composition A is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0130] [Production Example 7: Preparation of Prepolymer Composition B] A monomer mixture consisting of 62 parts by mass of 2EHA, 35 parts by mass of LA, and 3 parts by mass of 4HBA was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.) and 0.05 parts by mass of another photopolymerization initiator (trade name "Omnirad 651", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, yielding a prepolymer composition B with a polymerization rate of approximately 10%. This prepolymer composition B is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0131] [Production Example 8: Preparation of Prepolymer Composition C] A monomer mixture consisting of 60 parts by mass of 2EHA, 39 parts by mass of LA, and 1 part by mass of 4HBA was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.) and 0.05 parts by mass of another photopolymerization initiator (trade name "Omnirad 651", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, yielding a prepolymer composition C with a polymerization rate of approximately 10%. This prepolymer composition C is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0132] [Production Example 9: Preparation of Prepolymer Composition D] A monomer mixture consisting of 57 parts by mass of 2EHA, 39 parts by mass of LA, and 4 parts by mass of 4HBA was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.) and 0.05 parts by mass of another photopolymerization initiator (trade name "Omnirad 651", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, yielding a prepolymer composition D with a polymerization rate of approximately 10%. This prepolymer composition D is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0133] [Production Example 10: Preparation of Prepolymer Composition E] A monomer mixture consisting of 58 parts by mass of 2EHA, 39 parts by mass of LA, and 3 parts by mass of 4HBA was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.) and 0.05 parts by mass of another photopolymerization initiator (trade name "Omnirad 651", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, obtaining a prepolymer composition E with a polymerization rate of approximately 10%. This prepolymer composition E is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0134] [Production Example 11: Preparation of Prepolymer Composition F] A monomer mixture consisting of 48 parts by mass of 2EHA, 32 parts by mass of LA, 3 parts by mass of 4HBA, and 17 parts by mass of ethyl carbitol acrylate (CBA) was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.) and another 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 651", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, yielding a prepolymer composition F with a polymerization rate of approximately 10%. This prepolymer composition F is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0135] [Production Example 12: Preparation of Prepolymer Composition G] A monomer mixture consisting of 70 parts by mass of n-octyl acrylate (NOAA), 20 parts by mass of n-butyl acrylate (BA), 2 parts by mass of N-vinylpyrrolidone (NVP), and 8 parts by mass of 4HBA was mixed with 0.05 parts by mass of a photopolymerization initiator (trade name "Omnirad 819", manufactured by IGM Resins B.V.) and 0.05 parts by mass of another photopolymerization initiator (trade name "Omnirad 184", manufactured by IGM Resins B.V.). Then, under a nitrogen atmosphere, ultraviolet light was irradiated to polymerize a portion of the monomer components in the mixture, yielding a prepolymer composition G with a polymerization rate of approximately 10%. This prepolymer composition G is a partially polymerized product containing a photopolymerized product (photopolymerized polymer P1a) and monomer components that have not undergone the polymerization reaction (residual monomer).
[0136] [Example 1] (Preparation of adhesive composition) An adhesive composition was prepared by mixing 100 parts by mass of prepolymer composition A obtained in Production Example 6, 1 part by mass of oligomer B obtained in Production Example 2, 0.06 parts by mass of dipentaerythritol hexaacrylate (trade name "KAYARAD DPHA", manufactured by Nippon Kayaku Co., Ltd.) as a polyfunctional polymerizable compound, and 0.3 parts by mass of silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.).
[0137] (Preparation of Adhesive Sheet) Next, the above adhesive composition was applied to the release surface of a first release liner (product name "Diafoil MRF", thickness 38 μm, manufactured by Mitsubishi Chemical Corporation) having a release surface on one side to form a coating film. Next, the release surface of a second release liner (product name "Diafoil MRN", thickness 38 μm, manufactured by Mitsubishi Chemical Corporation) having a release surface on one side was bonded onto the coating film on the first release liner. Next, ultraviolet light was irradiated onto the coating film between the release liners from the second release liner side to photo-cure the coating film and form an adhesive layer with a thickness of 50 μm (ultraviolet irradiation step). For ultraviolet irradiation, a black light lamp (manufactured by Toshiba Corporation) was used as the light source, and the illuminance was set to 5.0 mW / cm². 2 The integrated irradiation light dose is 1500 mJ / cm². 2In the ultraviolet irradiation step, a photopolymerization reaction proceeds in the coating film in a reaction system containing the aforementioned residual monomer and a polyfunctional polymerizable compound, forming a photopolymerized polymer P1b having a photocrosslinked structure. Furthermore, since this photopolymerization reaction proceeds around the aforementioned photopolymerized polymer P1a, the photopolymerized polymer P1b is formed around the photopolymerized polymer P1a. The adhesive layer formed in this step contains such photopolymerized polymers P1a and P1b as base polymers.
[0138] Next, after peeling the first release liner from the adhesive layer, the adhesive layer on the second release liner was dried in a 130°C hot air oven for 3 minutes. This volatilized and removed any unreacted monomers in the adhesive layer. After cooling at room temperature, the release surface of the third release liner (product name "Diafoil MRF", thickness 38 μm, manufactured by Mitsubishi Chemical Corporation), which has a release surface on one side, was bonded onto the adhesive layer on the second release liner.
[0139] As described above, the adhesive sheet with a release liner of Example 1 (second release liner / adhesive sheet (thickness 100 μm) / third release liner) was prepared.
[0140] [Examples 2-5, Comparative Examples 1-3, 5] Adhesive compositions were prepared in the same manner as in Example 1, except that the type and amount of prepolymer composition and oligomer, the thickness of the adhesive sheet, etc. were changed as shown in Table 1. Adhesive sheets with release liners for each example were then prepared in the same manner as in Example 1.
[0141] [Comparative Example 4] (Preparation of Adhesive Composition) An adhesive composition was prepared by mixing 100 parts by mass of the prepolymer composition G obtained in Production Example 12, 1.5 parts by mass of oligomer A obtained in Production Example 1, 0.09 parts by mass of dipentaerythritol hexaacrylate (trade name "KAYARAD DPHA", manufactured by Nippon Kayaku Co., Ltd.) as a polyfunctional polymerizable compound, 0.5 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.), and 0.02 parts by mass of an additional photopolymerization initiator (trade name "Omnirad 819", manufactured by IGM Resins B.V.).
[0142] (Preparation of adhesive sheet) A release liner adhesive sheet for Comparative Example 4 was prepared in the same manner as in Example 5, except that the above adhesive composition was used.
[0143] <Evaluation> The following evaluations were performed on the adhesive sheets with release liners of the examples and comparative examples.
[0144] (1) Initial room temperature adhesive strength (Fn 1 For each adhesive sheet in Examples 1 to 5 and Comparative Examples 1 to 5, a peel test was performed to determine the adhesive strength Fn 1 The following measurements were taken. Specifically, they are as follows:
[0145] Preparation Steps: First, the third release liner was peeled off the adhesive sheet with a release liner (second release liner / adhesive sheet / third release liner). Next, the exposed adhesive sheet was laminated to a polyethylene terephthalate (PET) film (product name "Lumirror S10", thickness 50 μm, manufactured by Toray Industries, Inc.) whose surface had been plasma-treated. This obtained a laminated film. For the plasma treatment, a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Chemical Co., Ltd.) was used, with a voltage of 160 V, a frequency of 10 kHz, and a processing speed of 5000 mm / min. For lamination, the adhesive sheet was pressed onto the PET film by moving a 2 kg hand roller back and forth once in an environment of 25 °C. Next, a laminated film piece measuring 10 mm wide x 100 mm long was cut from the laminated film. This laminated film comprises the PET film, the adhesive sheet piece, and the second release liner in this order in the thickness direction. Next, the second release liner was peeled off from the adhesive sheet piece on the PET film. Then, the exposed adhesive sheet piece (10 mm wide x 100 mm long) was bonded to the Sn surface of an alkali glass plate prepared by the float method to obtain a laminate.
[0146] Heating and pressurizing step: Next, the laminate was subjected to a heating and pressurizing treatment at 50°C, 0.5 MPa, and for 15 minutes. This caused the adhesive sheet pieces to be pressed against the alkali glass plate.
[0147] Storage step: Next, the laminate was left to stand at room temperature for 24 hours.
[0148] Measurement Steps: Next, a 180° peel test was performed to peel an adhesive sheet piece from the alkali glass plate in the laminate, and the force required for peeling (peel force) was measured. A tensile testing machine (product name "Autograph AG-50NX plus", manufactured by Shimadzu Corporation) was used for this measurement. Specifically, in this measurement, under the conditions of 25°C, 50% relative humidity, a peel angle of 180°, and a tensile speed of 300 mm / min (first condition), the adhesive sheet piece was peeled from the alkali glass plate by pulling one end of the adhesive sheet piece in the longitudinal direction on the alkali glass plate, and the adhesive force was measured. The peel length was set to 50 mm, and the average value of the measured peel forces was defined as the adhesive force. Adhesion force Fn measured in the measurement step of the initial peel test 1 (N / 25mm) is shown in Table 1.
[0149] (2) Initial 60°C adhesion (Fh 1 ) For each adhesive sheet in Examples 1 to 5 and Comparative Examples 1 to 5, the first condition was replaced in the measurement step with the second condition (60°C, 50% relative humidity, 180° peel angle, and 300 mm / min tensile speed), except that the initial room temperature adhesive strength (Fn) was the same as above. 1 Similar to the above, initial 60°C adhesion Fh 1 The following measurements were taken. The results are shown in Table 1.
[0150] (3) Room temperature adhesive strength after storage (Fn 2 ) For each adhesive sheet in Examples 1 to 5 and Comparative Examples 1 to 5, the initial room temperature adhesive strength (Fn) was the same as above, except that the laminate was stored at 50°C for one week during the storage step. 1 ) Store in the same manner as above. After storage, the adhesive strength Fn at room temperature 2 The following measurements were taken. The results are shown in Table 1.
[0151] (4) Adhesive strength at 60℃ after storage (Fh 2 ) For each adhesive sheet in Examples 1 to 5 and Comparative Examples 1 to 5, the initial 60°C adhesive strength (Fh) was the same as above, except that the laminate was stored at 50°C for one week during the storage step. 1 Store in the same manner as above. Adhesion Fh at 60°C 2 The following measurements were taken. The results are shown in Table 1.
[0152] (5) High temperature and high humidity adhesive strength (Fh3 ) For each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 to 5, except that in the measurement step, the first condition was replaced with conditions of 60°C, 90% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min (third condition), the above initial room-temperature adhesive force (Fn 1 ) was measured in the same manner to obtain the high-temperature high-humidity adhesive force Fh 3 . The results are shown in Table 1.
[0153] (6) Room-temperature peel force after heating (Fn 3 ) For each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 to 5, except that in the storage step, the laminate was stored at room temperature for 24 hours, heated at 60°C for 3 minutes, and then stored at room temperature for 1 hour, the above initial room-temperature adhesive force (Fn 1 ) was measured in the same manner to obtain the room-temperature adhesive force Fn after heating 3 . The results are shown in Table 1.
[0154] (7) Gel fraction For the pressure-sensitive adhesive layer of each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 to 5, the gel fraction was determined as follows. First, about 0.1 g (mass: W 1 mg) of a sample was collected, wrapped in a tetrafluoroethylene resin porous membrane with an average pore size of 0.2 μm (trade name "Nitoflon NTF1122", mass: W 2 mg, manufactured by Nitto Denko Corporation), and tied with kite string (mass: W 3 mg) to obtain a wrapped body. Next, this wrapped body was immersed in about 50 mL of ethyl acetate solution, and allowed to stand in the ethyl acetate solution at room temperature (typically 23°C) for 7 days. Next, the wrapped body enclosing the gel fraction, which is the ethyl acetate-insoluble matter, was taken out from the ethyl acetate solution, and this wrapped body was dried at 130°C for 1 hour. Thereafter, the mass of the entire wrapped body (W 4 mg) was measured. Then, the gel fraction (mass%) was calculated by substituting the values of W 1 to W 4 into the following formula. The results are shown in Table 1. Gel fraction (mass%) = [(W 4 -W 2 -W 3 ) / W 1 ×100
[0155] (8) Weight-average molecular weight of sol For the adhesive layers of each adhesive sheet in Examples 1 to 5 and Comparative Examples 1 to 5, the weight-average molecular weight of the sol was determined as follows. Specifically, first, about 0.1 g of sample was taken from the adhesive layer and wrapped in a porous membrane made of tetrafluoroethylene resin with an average pore size of 0.2 μm (product name "Nitoflon NTF1122", manufactured by Nitto Denko Corporation), and tied with kite string to obtain a package. Next, this package was immersed in about 50 mL of ethyl acetate solution and left to stand in the ethyl acetate solution at room temperature (typically 23°C) for 7 days. Next, the package containing the ethyl acetate insoluble portion and the ethyl acetate solution containing the ethyl acetate soluble sol portion were separated. Next, the ethyl acetate solution containing the sol portion was dried under reduced pressure at 30°C and the ethyl acetate was evaporated to obtain the solid portion. Next, this solid portion was weighed. Next, using a GPC measuring device (product name "HLC-8120GPC", manufactured by Tosoh Corporation), the weight-average molecular weight (Mw) of the sol component was determined by GPC (gel permeation chromatography) based on the polystyrene equivalent value under the following measurement conditions. The results are shown in Table 1. [GPC measurement conditions] ・Column: Two TSKgel GMHHR-H(S) (manufactured by Tosoh Corporation) in series ・Column size: 7.8 mmφ × 30 cm ・Column temperature: 40℃ ・Eluent: Tetrahydrofuran (THF) ・Flow rate: 0.5 ml / min ・Sample injection volume: 100 μl ・Sample concentration: 0.1 mass% ・Standard sample: Polystyrene ・Detector: Differential refractometer (RI)
[0156] (9) Expansion Rate The adhesive layer of each adhesive sheet from Examples 1 to 5 and Comparative Examples 1 to 5 was cut into approximately 5 mm squares, and TMA measurement was performed in compression mode using "TMA / SS6000" manufactured by Hitachi High-Tech Science Co., Ltd. The dimensional change from 25°C to 60°C was measured and the expansion rate was calculated as follows: Expansion rate [%] = (thickness at 60°C - thickness at 25°C) / thickness at 25°C × 100
[0157]
[0158] As shown in Table 1, the adhesive sheets of the examples were found to have high initial and room-temperature adhesive strength, and excellent adhesion to the substrate when used, even after long-term storage. Furthermore, the adhesive strength at 60°C was low both initially and after storage, and it was found that they could be easily peeled off intentionally, even after long-term storage. Thus, the adhesive sheets of the examples can be peeled off from the substrate by heating without using water or ethanol, making peeling simple and safe. In addition, they maintained high adhesive strength and excellent adhesion to the substrate even after storage in a high-temperature, high-humidity environment or after being heated and returned to room temperature, and also had excellent reusability.
[0159] On the other hand, when the proportion of hydrophilic monomers in the oligomer was high (Comparative Example 1), it could be peeled off by heating, but the initial and room temperature adhesive strength was low, and it was judged to have poor adhesion to the adherend. When a hydrophobic oligomer was used (Comparative Example 2), the initial 60°C adhesive strength was low and it could be peeled off by heating, but after long-term storage, the 60°C adhesive strength was high and it was judged that it could not be easily peeled off from the adherend. When no hydrophilic oligomer was used and the proportion of hydrophilic monomers was high (Comparative Example 3), the initial and room temperature adhesive strength was low, and after long-term storage, the 60°C adhesive strength was high and it was judged that it could not be easily peeled off from the adherend. Furthermore, when no hydrophobic oligomer was used and a prepolymer with a high proportion of hydrophilic monomers was used (Comparative Example 4), the 60°C adhesive strength was high both initially and after long-term storage and it was judged that it could not be easily peeled off from the adherend. When no hydrophilic oligomer was used (Comparative Example 5), the initial room temperature adhesive strength was low, and after long-term storage, the 60°C adhesive strength was high and it was judged that it could not be easily peeled off from the adherend.
[0160] Hereinafter, variations of the invention according to the present disclosure will be described. [Appendix 1] A pressure-sensitive adhesive sheet that is peelable by heating and includes a pressure-sensitive adhesive layer containing a photopolymerized polymer as a base polymer, wherein the pressure-sensitive adhesive layer contains an oligomer containing 3 to 8 mass% of a structural unit derived from a hydrophilic monomer, and after the pressure-sensitive adhesive layer is bonded to the Sn surface of alkali glass and stored at 50°C for 1 week, the pressure-sensitive adhesive force Fh when peeled under the conditions of 60°C, 50% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min 2 is 1.5 to 3.5 N / 25 mm, and after the pressure-sensitive adhesive layer is bonded to the Sn surface of alkali glass and stored at room temperature for 24 hours, the pressure-sensitive adhesive force Fn when peeled under the conditions of 25°C, 50% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min 1 is 7 N / 25 mm or more. [Appendix 2] The pressure-sensitive adhesive sheet according to Appendix 1, wherein after the pressure-sensitive adhesive layer is bonded to the Sn surface of alkali glass and stored at room temperature for 24 hours, the pressure-sensitive adhesive force Fh when peeled under the conditions of 60°C, 50% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min 1 is 1.5 to 3.5 N / 25 mm. [Appendix 3] The pressure-sensitive adhesive sheet according to Appendix 1 or 2, wherein after the pressure-sensitive adhesive layer is bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, heated at 60°C for 3 minutes, and then stored at room temperature for 1 hour, the pressure-sensitive adhesive force Fn when peeled under the conditions of 25°C, 50% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min 3 is 80 to 150% of the pressure-sensitive adhesive force Fn 1 . [Appendix 4] The pressure-sensitive adhesive sheet according to any one of Appendices 1 to 3, wherein after the pressure-sensitive adhesive layer is bonded to the Sn surface of alkali glass and stored at room temperature for 24 hours, the pressure-sensitive adhesive force Fh when peeled under the conditions of 60°C, 90% relative humidity, a peeling angle of 180°, and a tensile speed of 300 mm / min 3 is 1.5 N / 25 mm or more. [Appendix 5] The pressure-sensitive adhesive sheet according to any one of Appendices 1 to 4, wherein the pressure-sensitive adhesive layer has a weight-average molecular weight of 200,000 or more for the sol content soluble in ethyl acetate, and a proportion of the gel content insoluble in ethyl acetate of 68 mass% or more. [Appendix 6] The pressure-sensitive adhesive sheet according to any one of Appendices 1 to 5, which is used for bonding to an optical member.
[0161] 1 Optical laminate 2 Adhesive layer 21, 22, 23 Adhesive layer (adhesive sheet) 31, 32 Cover member 4 Polarizing film 5 Image display device 6 Touchscreen panel 10 Adhesive sheet 100 OLED display panel L1, L2 Release liner
Claims
1. The adhesive layer is removable by heating and contains a photopolymerized polymer as the base polymer, wherein the adhesive layer contains an oligomer containing 3 to 8% by mass of constituent units derived from a hydrophilic monomer, and the adhesive force Fh is measured when the adhesive layer is bonded to the Sn surface of alkali glass, stored at 50°C for one week, and then peeled off under the conditions of 60°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 2 The adhesive strength is 1.5 to 3.5 N / 25 mm, and the adhesive strength Fn was obtained when the adhesive layer was bonded to the Sn surface of alkali glass, stored at room temperature for 24 hours, and then peeled off under the conditions of 25°C, 50% relative humidity, peeling angle of 180°, and tensile speed of 300 mm / min. 1 An adhesive sheet with a rating of 7N / 25mm or higher.
2. The adhesive strength Fh when the adhesive layer is attached to the Sn surface of alkali glass, stored at room temperature for 24 hours, and then peeled off under the conditions of 60°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 1 The adhesive sheet according to claim 1, wherein the N / 25 mm is 1.5 to 3.5 N.
3. The adhesive layer was bonded to the Sn surface of the alkali glass and stored at room temperature for 24 hours, then heated at 60°C for 3 minutes, and then stored at room temperature for 1 hour. The adhesive strength Fn was obtained when peeled off under the conditions of 25°C, 50% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 3 The adhesive force Fn 1 The adhesive sheet according to claim 1 or 2, wherein the amount is 80 to 150% of the total.
4. The adhesive strength Fh when the adhesive layer is attached to the Sn surface of alkali glass, stored at room temperature for 24 hours, and then peeled off under the conditions of 60°C, 90% relative humidity, peel angle of 180°, and tensile speed of 300 mm / min. 3 The adhesive sheet according to claim 1 or 2, wherein the strength is 1.5 N / 25 mm or more.
5. The adhesive sheet according to claim 1 or 2, wherein the adhesive layer has a weight-average molecular weight of 200,000 or more of sol components soluble in ethyl acetate, and a proportion of 68% by mass or more of gel components insoluble in ethyl acetate.
6. An adhesive sheet according to claim 1 or 2, used for bonding to an optical component.