Sputtering device, method for manufacturing reflective mask blank, and substrate with reflective layer
The sputtering apparatus with an anti-adhesion shield and inclined surfaces addresses contamination issues in ion beam sputtering, ensuring high reflectivity and precision in EUV lithography by deflecting the ion beam away from peripheral components, thus maintaining film quality.
Patent Information
- Application Number
- PCT/JP2026/016092
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-04-22
- Publication Date
- 2026-11-19
AI Technical Summary
Ion beam sputtering in the formation of reflective multilayer films for EUV lithography leads to contamination from surrounding components, affecting the refractive index and reflectivity of the film, which in turn impacts the precision of EUV exposure and patterning.
A sputtering apparatus with an anti-adhesion shield around the target, featuring inclined surfaces to deflect the ion beam away from peripheral components, reducing contamination from the anti-deposition shield.
The solution effectively suppresses contamination, maintaining the reflectivity of the multilayer film and ensuring high-precision patterning in EUV lithography by minimizing sputtered particle interference from peripheral components.
Smart Images

Figure JP2026016092_19112026_PF_FP_ABST
Abstract
Description
Sputtering apparatus, method for manufacturing reflective mask blanks, and substrate with reflective layer
[0001] The present invention relates to a sputtering apparatus for depositing a film on a substrate by irradiating an ion beam from an ion source toward a sputtering target, a method for manufacturing a reflective mask blank, and a substrate with a reflective layer.
[0002] In recent years, EUV lithography, which uses EUV (Extreme Ultra Violet) light with a central wavelength of around 13.5 nm as a light source, has been investigated for further miniaturization of semiconductor devices. In EUV exposure, a reflective optical system and a reflective mask are used due to the characteristics of EUV light. In a reflective mask, a reflective multilayer film that reflects EUV light is formed on the substrate, and an absorber film that absorbs EUV light is patterned on the reflective multilayer film. EUV light incident on the reflective mask from the illumination optical system of the exposure apparatus is reflected in areas without the absorber film (apers) and absorbed in areas with the absorber film (non-apers). The pattern of the absorber film becomes the mask pattern (transfer pattern). As a result, the mask pattern (transfer pattern) is exposed and transferred as a resist pattern to the resist film on the semiconductor wafer through the reduction projection optical system of the exposure apparatus, and subsequent processing is carried out. Reflective mask blanks used in the manufacture of reflective masks have a structure in which a reflective layer that reflects EUV light and an absorbing layer that absorbs EUV light are formed in that order on a substrate such as glass. As the reflective layer, a reflective multilayer film is usually used in which the light reflectivity when EUV light is irradiated onto the layer surface is increased by alternately stacking a low refractive index layer that has a low refractive index for EUV light and a high refractive index layer that has a high refractive index for EUV light. Molybdenum (Mo) layers are usually used as the low refractive index layers of the reflective multilayer film, and silicon (Si) layers are usually used as the high refractive index layers. When manufacturing reflective mask blanks, sputtering is preferably used for forming the reflective multilayer film because it is easy to produce a homogeneous film thickness, the cycle time is short, and the film thickness can be easily controlled. Here, ion beam sputtering is used to form the high refractive index layer and the low refractive index layer that constitute the reflective multilayer film. Ion beam sputtering is a film deposition method in which charged particles are used to strike the surface of a sputtering target, knocking out the sputtered particles from the sputtering target, and depositing the sputtered particles onto a substrate placed opposite the sputtering target to form a thin film.
[0003] For example, Patent Document 1 lists He, Ne, Ar, Kr, Xe, Rn, and N as ion sources. 2A method for manufacturing a reflective mask blank has been proposed, which includes the procedure of forming a reflective multilayer film on a substrate using an ion beam sputtering apparatus that uses a process gas containing at least one inert gas selected from, applies a voltage to a grid to accelerate ions generated, and performs sputtering by colliding the ions with a target. In Patent Document 1, an anti-adhesion shield is placed so as to cover the target, and the effective area of the grid (cm²) 2 The product of the flow rate (sccm) of the process gas supplied to the ion beam sputtering apparatus during film deposition is 3600 (cm²). 2 It is less than or equal to sccm.
[0004] International Publication No. 2022 / 239752
[0005] Unlike magnetron sputtering, ion beam sputtering involves the ion beam traveling in a straight line with a constant diffusion angle, causing it to collide with surrounding components other than the sputtering target. Therefore, when forming a reflective multilayer film using the ion beam sputtering apparatus described in Patent Document 1, sputtered particles are generated when the ion beam collides with surrounding components of the sputtering target, such as the anti-deposition shield. If these sputtered particles, generated on surrounding components other than the sputtering target, become mixed into the film being formed, contamination occurs. In this case, if contamination originating from the sputtering target's surrounding components occurs in the high-refractive-index and low-refractive-index layers constituting the reflective multilayer film, the refractive index of these layers changes. This can potentially reduce reflectivity. In this case, the peak reflectivity of light in the EUV wavelength range on the surface of the reflective multilayer film becomes locally lower in the contaminated area. As a result, a decrease in the intensity of the peak reflectivity of light in the EUV wavelength range on the surface of the reflective multilayer film occurs. A decrease in the intensity of the peak reflectance of light in the EUV wavelength range on the surface of a reflective multilayer film can lead to insufficient EUV exposure to the resist film on the wafer when EUV lithography is performed using a reflective mask fabricated from a reflective mask blank. This results in insufficient patterning within the exposure field, hindering high-precision patterning. Therefore, it is desirable to suppress contamination originating from peripheral components of the sputtering target, such as materials constituting the anti-deposition shield. The present invention aims to provide a sputtering apparatus that suppresses contamination originating from peripheral components other than the sputtering target, such as an anti-deposition shield, a method for manufacturing a reflective mask blank, and a substrate with a reflective layer.
[0006] As a result of diligent research, the present inventors have found that the above-mentioned problems can be solved by the following configuration: (1) A sputtering apparatus that irradiates an ion beam from an ion source toward a sputtering target, causing sputtering particles to fly toward the film-forming surface of a substrate, and deposits a film containing the constituent material of the sputtering target toward the film-forming surface of the substrate, wherein the sputtering apparatus has an anti-adhesion shield arranged around the sputtering target, and in the in-plane direction of the sputtering target, in the region of the anti-adhesion shield opposite to the ion source, the anti-adhesion shield has a first inclined surface other than the outer edge of the anti-adhesion shield, and the first inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target.
[0007] (2) The sputtering apparatus according to (1), wherein the first inclined surface is a surface that slopes from the surface toward the opposite side of the surface as it moves from the sputtering target side toward the outer edge side of the anti-deposition shield. (3) The sputtering apparatus according to (1) or (2), wherein the anti-deposition shield has an opening, a sputtering target is placed in the opening, and when observed from the direction normal to the surface of the sputtering target, a rectangle is drawn virtually that is tangent to the opening and has one side parallel to the direction of projection of the ion beam irradiation direction onto the surface of the sputtering target, and the first inclined surface is in a virtual region enclosed by the rectangle and the opening in the region of the anti-deposition shield opposite to the ion source in the in-plane direction of the sputtering target. (4) The sputtering apparatus according to any one of (1) to (3), wherein in the in-plane direction of the sputtering target, the region of the anti-deposition shield on the ion source side has a region having a surface parallel to the surface of the sputtering target. (5) The sputtering apparatus according to any one of (1) to (3), wherein the anti-adhesion shield has an opening in which a sputtering target is placed, and when observed from the direction normal to the surface of the sputtering target, a rectangle is virtually drawn that is tangent to the opening and has one side parallel to the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and in the in-plane direction of the sputtering target, there is a second inclined surface in the virtual region enclosed by the rectangle and the opening within the region of the anti-adhesion shield on the ion source side, and the second inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target.
[0008] (6) The sputtering apparatus according to (5), wherein in the in-plane direction of the sputtering target, within the region of the anti-deposition shield on the ion source side, within a virtual region enclosed by a rectangle and an opening, the second inclined surface has a different shape from the second inclined surface, or has a flat surface. (7) The sputtering apparatus according to any one of (1) to (3), wherein, when observed from the direction normal to the surface of the sputtering target, a rectangle is virtually drawn that is tangent to the opening and has one side parallel to the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and within the virtual region enclosed by the rectangle and the opening, the second inclined surface exists only in the region enclosed by the rectangle and the opening on the opposite side of the anti-deposition shield on the in-plane direction of the sputtering target, and the second inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target. (8) The sputtering apparatus according to any one of (1) to (7), wherein the anti-adhesion shield has an opening in which a sputtering target is placed, and when observed from the direction normal to the surface of the sputtering target, a line formed by the intersection of a plane including a straight line passing through the center of the opening and extending in the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and the normal to the surface of the sputtering target passing through the center of the opening, and the surface of the anti-adhesion shield, is included in the first inclined surface.
[0009] (9) The sputtering apparatus according to any one of (5) to (7), wherein the anti-adhesion shield has an opening in which a sputtering target is placed, and the second inclined surface is formed by the intersection of a plane containing a straight line passing through the center of the opening and extending in the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and the normal of the surface of the sputtering target passing through the center of the opening, when observed from the direction normal to the surface of the sputtering target, and the surface of the anti-adhesion shield. (10) The sputtering apparatus according to any one of (1) to (9), used for manufacturing a reflective mask blank. (11) A method for manufacturing a reflective mask blank, comprising the step of forming a functional film on the surface of a substrate using the sputtering apparatus according to any one of (1) to (9). (12) A substrate with a reflective layer, wherein a reflective layer that reflects EUV light and a protective layer for the reflective layer are laminated in this order on the substrate, the reflective layer being a reflective multilayer film in which a low refractive index layer, a Mo layer, and a high refractive index layer, a Si layer, are alternately laminated, and when the substrate with the reflective layer is measured by X-ray fluorescence analysis, the ratio of the detection intensity of AlKα lines to the detection intensity of MoKα lines is 0.0043 or less, and when the substrate with the reflective layer is measured by X-ray fluorescence analysis, the ratio of the detection intensity of YLα lines to the detection intensity of MoKα lines is 0.0008 or less.
[0010] According to the present invention, it is possible to provide a sputtering apparatus that suppresses contamination originating from peripheral members other than the sputtering target, such as anti-adhesion shields, a method for manufacturing a reflective mask blank, and a substrate with a reflective layer.
[0011] This is a schematic diagram showing an example of a sputtering apparatus according to an embodiment of the present invention. This is a schematic diagram showing a first example of a holding part for holding a sputtering target in a sputtering apparatus according to an embodiment of the present invention. (a) is a schematic diagram showing a first example of an anti-adhesion shield in a sputtering apparatus according to an embodiment of the present invention, and (b) is a schematic diagram showing a second example of an anti-adhesion shield in a sputtering apparatus according to an embodiment of the present invention. This is a schematic diagram showing a third example of an anti-adhesion shield in a sputtering apparatus according to an embodiment of the present invention. This is a schematic diagram showing a fourth example of an anti-adhesion shield in a sputtering apparatus according to an embodiment of the present invention. This is a schematic diagram showing a fifth example of an anti-adhesion shield in a sputtering apparatus according to an embodiment of the present invention. This is a schematic diagram showing a second example of a holding part for holding a sputtering target in a sputtering apparatus according to an embodiment of the present invention. This is a schematic cross-sectional view showing one embodiment of a substrate with a reflective layer according to an embodiment of the present invention. (a) to (d) are schematic cross-sectional views showing an example of a manufacturing process for a transfer mask using a reflective mask blank according to an embodiment of the present invention in order of process.
[0012] Embodiments of the present invention will be described below with reference to the drawings. However, the following embodiments are illustrative for illustrating the present invention, and the present invention is not limited to the embodiments shown below. Various modifications and substitutions can be made to the following embodiments without departing from the scope of the present invention. In the following, numerical ranges expressed using "~" mean a range that includes the numbers written before and after "~" as the lower and upper limits. For specific angles, orthogonals, and parallels, unless otherwise specified, the error range includes the error range that is generally accepted in the relevant art. The error range includes the machine accuracy, which is the accuracy of the machine tool itself, and the machining accuracy resulting from the positioning accuracy. Similarly, unless otherwise specified, "same" also includes the error range that is generally accepted in the relevant art.
[0013] A distinctive feature of the sputtering apparatus of the present invention is that it irradiates an ion beam from an ion source toward a sputtering target, causing sputtering particles to fly toward the film-forming surface of a substrate, and forming a film containing the constituent materials of the sputtering target toward the film-forming surface of the substrate, wherein the sputtering apparatus has an anti-adhesion shield arranged around the sputtering target, and in the in-plane direction of the sputtering target, in the region of the anti-adhesion shield opposite to the ion source, the anti-adhesion shield has a first inclined surface other than the outer edge of the anti-adhesion shield, and the first inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target. In this way, by providing the above-mentioned first inclined surface in the region of the anti-adhesion shield opposite to the ion source, the ion beam is less likely to collide with peripheral members such as the anti-adhesion shield other than the sputtering target, and the anti-adhesion shield 32 is less likely to be sputtered by the ion beam, thereby suppressing contamination originating from the anti-adhesion shield, etc.
[0014] <Example of a sputtering apparatus> A sputtering apparatus is a device that irradiates an ion beam from an ion source toward a sputtering target, causing sputtering particles to fly toward the film-forming surface of a substrate, and deposits a film containing the constituent materials of the sputtering target toward the film-forming surface of the substrate. The sputtering apparatus will be described in detail below with reference to Figure 1, but the present invention is not particularly limited to the sputtering apparatus 10 shown in Figure 1. Figure 1 is a schematic diagram showing an example of a sputtering apparatus according to an embodiment of the present invention. Figure 2 is a schematic diagram showing a first example of a holding part that holds a sputtering target in a sputtering apparatus according to an embodiment of the present invention. In Figure 1, the sputtering target 30 shown in Figure 2 is omitted from the illustration.
[0015] The sputtering apparatus 10 shown in Figure 1 comprises a vacuum chamber 12, a substrate holder 13, a rotating shaft 14 for rotating the substrate holder 13, and a drive unit 15 for rotating the rotating shaft 14. A substrate 20 is fixed and placed on the surface 13a of the substrate holder 13. The configuration of the substrate holder 13 is not particularly limited as long as the substrate 20 can be fixed to the surface 13a. For example, the substrate 20 can be fixed to the surface 13a of the substrate holder 13 using a jig (not shown). Also, if there is a conductive film on the back surface of the substrate 20, the substrate holder 13 is configured to have an electrostatic chuck, and the substrate 20 is fixed to the surface 13a of the substrate holder 13 by the electrostatic chuck. The drive unit 15 rotates the substrate holder 13 around the rotating shaft Cs. This allows the substrate 20 to rotate (rotate) within the plane of the film-forming surface during film formation. Therefore, regardless of the incident angle of the ion beam Ib, the sputtered particles adhere to the rotating substrate 20, and a uniform film is formed on the film-forming surface of the substrate 20. For example, a motor is used for the drive unit 15.
[0016] A piping 16 is provided in the vacuum chamber 12. A valve 17a and a vacuum pump 17b are provided in the piping 16 in that order from the vacuum chamber 12 side. The valve 17a opens and closes to connect or disconnect the vacuum pump 17b and the vacuum chamber 12. The configuration of the valve 17a is not particularly limited as long as it can connect or disconnect the vacuum pump 17b and the vacuum chamber 12, and various valves used in ion beam sputtering apparatuses can be used as appropriate. The vacuum pump 17b is a pump for reducing the pressure inside the vacuum chamber 12a, and various pumps used in ion beam sputtering apparatuses can be used as appropriate. For example, the vacuum pump 17b reduces the pressure inside the vacuum chamber 12a to 1.33 × 10⁻⁶. -6 Pa(10 -8 A pump capable of reducing the pressure to approximately Torr is used. The vacuum chamber 12 is equipped with a pressure sensor (not shown) for measuring the pressure inside the vacuum chamber 12a.
[0017] A holding portion 19 for holding a sputtering target 30 (see Figure 2) is provided facing the surface 13a of the substrate holder 13. An ion source 18 is provided for irradiating the sputtering target 30 (see Figure 2) of the holding portion 19 with an ion beam Ib. The configuration of the ion source 18 is not particularly limited as long as it can irradiate the sputtering target 30 with an ion beam Ib. Examples of ion sources 18 include Kaufman type (filament), hollow cathode type, RF type, bucket type, and duoplasmatron type. An inert gas such as argon gas, krypton gas, or xenon gas is used as the sputtering gas introduced into the ion source 18.
[0018] As shown in Figure 2, the holding unit 19 includes a sputtering target 30 and an anti-adhesion shield 32 arranged around the sputtering target 30. The sputtering target 30 is irradiated with an ion beam Ib to generate sputtered particles (not shown). The outer shape of the sputtering target 30 is, for example, circular. The anti-adhesion shield 32 has an opening 32a, in which the sputtering target 30 is positioned. The inner shape of the opening 32a is circular, the same as the outer shape of the sputtering target 30. In the in-plane direction Dw of the sputtering target 30, the anti-adhesion shield 32 has a first inclined surface 33 in the region Ro opposite to the ion source 18 (see Figure 1), in addition to the outer edge 32e of the anti-adhesion shield 32. The first inclined surface 33 is a surface that gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds of the sputtering target 30. The anti-deposition shield 32 has a region Ri on the ion source 18 (see Figure 1) side of the anti-deposition shield 32 in the in-plane direction Dw of the sputtering target 30, which has a surface 37 parallel to the surface 30a of the sputtering target 30. In this case, the anti-deposition shield 32 has a configuration in which the first inclined surface 33 is only present in the above-mentioned region Ro, and the configuration of region Ro and region Ri is different, resulting in an asymmetrical configuration. Because the anti-deposition shield 32 has the above-mentioned first inclined surface 33, the ion beam Ib is less likely to collide with the anti-deposition shield 32 other than the sputtering target 30, and the anti-deposition shield 32 is less likely to be sputtered by the ion beam Ib, thereby suppressing contamination originating from peripheral members such as the anti-deposition shield 32 other than the sputtering target 30. The anti-deposition shield 32 is made of, for example, an aluminum alloy or stainless steel. Alternatively, the anti-deposition shield 32 may have a surface made of, for example, Al or Y 2 O 3 It is made of yttrium oxide. The surface of the anti-adhesion shield 32 is the surface 30a of the sputtering target 30.
[0019] The first inclined surface 33 is not particularly limited in its configuration, as long as it is a surface that gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds of the sputtering target 30, as described above. The first inclined surface 33 can be, for example, a flat or curved surface. The thickness direction Ds of the sputtering target 30 is the direction in which the normal (not shown) of the surface 30a of the sputtering target 30 is directed toward the opposite side of the surface 30a of the sputtering target 30. Here, Figure 3(a) is a schematic diagram showing a first example of the anti-adhesion shield of a sputtering apparatus according to an embodiment of the present invention, and Figure 3(b) is a schematic diagram showing a second example of the anti-adhesion shield of a sputtering apparatus according to an embodiment of the present invention. In Figures 3(a) and (b), the same reference numerals are used for components identical to those of the holding portion 19 shown in Figure 2, and their detailed description is omitted. The first inclined surface 33a of the anti-adhesion shield 32 shown in Figure 3(a) is a surface that slopes from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a as you move from the sputtering target 30 side toward the outer edge 32e of the anti-adhesion shield 32. The first inclined surface 33a is a slope composed of planes, its cross-sectional shape is represented by a straight line, and it gradually slopes downward in the thickness direction Ds from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a. The first inclined surface 33b of the anti-adhesion shield 32 shown in Figure 3(b) is a curved surface that slopes from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a as you move from the sputtering target 30 side toward the outer edge 32e of the anti-adhesion shield 32. The first inclined surface 33b is a curved surface, its cross-sectional shape is represented by a curve, and it gradually slopes downward in the thickness direction Ds from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a.
[0020] Furthermore, in the anti-adhesion shield 32, in the in-plane direction Dw of the sputtering target 30, in the region Ro opposite to the ion source 18 (see Figure 1), the anti-adhesion shield 32 has a first inclined surface 33 in addition to the outer edge 32e of the anti-adhesion shield 32, but the invention is not limited to this. For example, in the anti-adhesion shield 32, in the in-plane direction Dw of the sputtering target 30, in the region Ri on the ion source 18 side of the anti-adhesion shield 32, the anti-adhesion shield 32 may have a second inclined surface 34 in addition to the outer edge 32e of the anti-adhesion shield 32.
[0021] The second inclined surface 34 can have the same configuration as the first inclined surface 33 described above. The second inclined surface 34 is also a surface that gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds of the sputtering target 30. More specifically, the second inclined surface 34 can have the same configuration as the first inclined surface 33 shown in Figures 3(a) and (b) described above. For example, the second inclined surface 34a shown in Figure 3(a) is a surface that slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a as you move from the sputtering target 30 side toward the outer edge 32e side of the anti-adhesion shield 32. The second inclined surface 34a is an inclined surface composed of a plane, its cross-sectional shape is represented by a straight line, and it gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds. The second inclined surface 34b shown in Figure 3(b) is a curved surface that slopes from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a, as it moves from the sputtering target 30 side toward the outer edge 32e side of the anti-adhesion shield 32. The second inclined surface 34b is a curved surface, its cross-sectional shape is represented by a curve, and it gradually slopes downward in the thickness direction Ds from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a.
[0022] Figure 4 is a schematic diagram showing a third example of an anti-adhesion shield for a sputtering apparatus according to an embodiment of the present invention. Figure 4 shows the anti-adhesion shield 32 as viewed from the direction normal to the surface 30a of the sputtering target 30. In Figure 4, the same components as those in the holding part 19 shown in Figure 2 are denoted by the same reference numerals, and their detailed descriptions are omitted. As described above, the anti-adhesion shield 32 has an opening 32a, and the sputtering target 30 is positioned in the opening 32a. When observed from the direction normal to the surface 30a of the sputtering target 30, a rectangle 35 is virtually drawn that is tangent to the opening 32a of the anti-deposition shield 32, with one side parallel to the direction Dp obtained by projecting the ion beam irradiation direction onto the surface 30a of the sputtering target 30. In the in-plane direction Dw of the sputtering target 30, the region enclosed by the rectangle 35 and the opening 32a of the anti-deposition shield 32 in region Ro opposite to the ion source 18 (see Figure 1) of the anti-deposition shield 32 is defined as the virtual region Rvo. It is preferable that the first inclined surface 33 is in the virtual region Rvo, but it is also acceptable for the first inclined surface 33 to be present only in the virtual region Rvo. As described above, the first inclined surface 33 is a surface that gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds of the sputtering target 30. However, the first inclined surface 33 may be either the first inclined surface 33a shown in Figure 3(a) or the first inclined surface 33b shown in Figure 3(b). In the in-plane direction Dw of the sputtering target 30, the region Ri of the anti-deposition shield 32 on the ion source 18 side (see Figure 1) has a configuration in which, for example, a region has a surface parallel to the surface 30a of the sputtering target 30. In this case, within the region Ri on the ion source 18 side (see Figure 1), the region enclosed by the rectangle 35 and the opening 32a of the anti-deposition shield 32 is defined as the virtual region Rvi. The virtual region Rvi may be composed of a surface parallel to the surface 30a of the sputtering target 30. The rectangle 35 is circumscribed with the opening 32a, and all of its interior angles are 90°.
[0023] Figure 5 is a schematic diagram showing a fourth example of an anti-adhesion shield for a sputtering apparatus according to an embodiment of the present invention. Figure 5 shows the anti-adhesion shield 32 as viewed from the direction normal to the surface 30a of the sputtering target 30. In Figure 5, the same reference numerals are used for components identical to the holding part 19 shown in Figure 2 and the anti-adhesion shield 32 shown in Figure 4, and their detailed descriptions are omitted. As described above, the anti-adhesion shield 32 has an opening 32a, and the sputtering target 30 is positioned in the opening 32a. When observed from the direction normal to the surface 30a of the sputtering target 30, a rectangle 35 is virtually drawn that is tangent to the opening 32a of the anti-deposition shield 32, with one side parallel to the direction Dp obtained by projecting the ion beam irradiation direction onto the surface 30a of the sputtering target 30. In the in-plane direction Dw of the sputtering target 30, the region enclosed by the rectangle 35 and the opening 32a of the anti-deposition shield 32 within the region Ri on the ion source 18 (see Figure 1) side of the anti-deposition shield 32 is defined as the virtual region Rvi. A configuration can be made in which the second inclined surface 34 is located in the virtual region Rvi. For example, as described above, the second inclined surface 34 is a surface that gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds of the sputtering target 30. However, the second inclined surface 34 may be either the second inclined surface 34a shown in Figure 3(a) or the second inclined surface 34b shown in Figure 3(b).
[0024] Furthermore, in the in-plane direction Dw of the sputtering target 30, within the region Ri on the ion source 18 side (see Figure 1) of the anti-deposition shield 32, the virtual region Rvi enclosed by the rectangle 35 and the opening 32a may have an inclined surface of a different shape from the second inclined surface 34, or it may have a flat surface. Also, with respect to the second inclined surface 34, among the virtual regions Rvo and Rvi enclosed by the rectangle 35 and the opening 32a, the second inclined surface 34 may be present only in the region (virtual region Rvi) enclosed by the rectangle 35 and the opening 32a of the anti-deposition shield 32, on the opposite side of the ion source 18 (see Figure 1) of the anti-deposition shield 32 in the in-plane direction Dw of the sputtering target 30. In this case, for example, the second inclined surface 34 is a surface that gradually slopes downward from the surface 30a of the sputtering target 30 toward the opposite side of the surface 30a in the thickness direction Ds of the sputtering target 30. In this case as well, as described above, the second inclined surface 34 may be either the second inclined surface 34a shown in Figure 3(a) or the second inclined surface 34b shown in Figure 3(b).
[0025] In Figures 4 and 5, the region Rs between the outer edge 32e of the anti-adhesion shield 32 and the rectangle 35 is divided into a first region Rso and a second region Rsi by a line Ls that passes through the center C of the opening 32a of the anti-adhesion shield 32 and is perpendicular to the direction Dp described above. If the virtual region Rvo described above is composed of a first inclined surface 33, the first region Rso may be composed of an inclined surface continuous with the first inclined surface 33, or it may be composed of a surface parallel to the surface 30a of the sputtering target 30. If the virtual region Rvi described above is composed of a second inclined surface 34, the second region Rsi may be composed of an inclined surface continuous with the second inclined surface 34, or it may be composed of a surface parallel to the surface 30a of the sputtering target 30. If the virtual region Rvi is not composed of a second inclined surface 34, the second region Rsi may be composed of, for example, a surface parallel to the surface 30a of the sputtering target 30.
[0026] Figure 6 is a schematic diagram showing a fifth example of an anti-adhesion shield for a sputtering apparatus according to an embodiment of the present invention. Figure 6 shows the anti-adhesion shield 32 as observed from the direction normal to the surface 30a of the sputtering target 30. In Figure 6, the same reference numerals are used for components identical to the holding part 19 shown in Figure 2, and their detailed descriptions are omitted. As shown in Figure 6, when observed from the direction normal to the surface 30a of the sputtering target 30, it is preferable that the first inclined surface 33 contains a line L1 formed by the intersection of a plane Pp, which includes a straight line Lp passing through the center C of the opening 32a of the anti-adhesion shield 32 and extending in the direction Dp obtained by projecting the ion beam irradiation direction onto the surface 30a of the sputtering target 30, and the normal to the surface 30a of the sputtering target 30 (not shown) passing through the center C of the opening 32a, and the surface 32d of the anti-adhesion shield 32. This makes it less likely for the ion beam to collide with the anti-adhesion shield 32 other than the sputtering target 30, and makes it less likely for the anti-adhesion shield 32 to be sputtered.
[0027] Furthermore, as shown in Figure 6, when observed from the normal direction to the surface 30a of the sputtering target 30, a line L is formed when a plane Pp, which includes a straight line Lp passing through the center C of the opening 32a of the anti-adhesion shield 32 and extending in the direction Dp obtained by projecting the ion beam irradiation direction onto the surface 30a of the sputtering target 30, intersects with the surface 32d of the anti-adhesion shield 32, and the normal (not shown) of the surface 30a of the sputtering target 30 that passes through the center C of the opening 32a. 2 However, it is preferable that it be included in the second inclined surface 34. This makes the anti-adhesion shield 32 even less susceptible to sputtering.
[0028] In the sputtering apparatus 10 shown in Figure 1, the configuration of the holding portion 19 is not particularly limited to the configuration shown in Figure 2. Figure 7 is a schematic diagram showing a second example of a holding portion for holding a sputtering target in a sputtering apparatus according to an embodiment of the present invention. In Figure 7, the same components as those in the holding portion 19 shown in Figure 2 are denoted by the same reference numerals, and their detailed descriptions are omitted.
[0029] The holding unit 19 shown in FIG. 2 holds one sputtering target 30, while the holding unit 40 shown in FIG. 7 holds four sputtering targets 30. The sputtering target 30 has a circular outer shape as described above. The holding unit 40 includes a frame 41, a rotating shaft portion 42, a housing 43, and a deposition-preventing shield 44. The frame 41 is a quadrangular prism-shaped member with four continuous surfaces 41a, 41b, 41c, and 41d. The sputtering target 30 is fixed to each of the four continuous surfaces 41a, 41b, 41c, and 41d. A total of four sputtering targets 30 are fixed to the frame 41. The rotating shaft portion 42 is provided in the interior 41e of the frame 41. The rotating shaft portion 42 is connected to the frame 41. The rotating shaft portion 42 is rotatable about the rotating shaft 42c. The rotating shaft portion 42 is connected to a motor (not shown). The motor causes the rotating shaft portion 42 to rotate about the rotating shaft 42c. The rotation direction of the motor is not limited. That is, although the rotation direction of the motor is illustrated as clockwise in FIG. 7, it may be rotated counterclockwise. The housing 43 accommodates the frame 41. The housing 43 is provided with a deposition-preventing shield 44.
[0030] The anti-deposition shield 44 has an opening 44a, in which the sputtering target 30 is positioned. The inner shape of the opening 44a is circular, the same as the outer shape of the sputtering target 30. The rotating shaft portion 42 rotates about the rotation axis 42c as described above, thereby changing the sputtering target 30 positioned in the opening 44a of the anti-deposition shield 44. The anti-deposition shield 44 can have the same configuration as the anti-deposition shield 32 (see Figure 2, etc.), so a detailed explanation is omitted. In the anti-deposition shield 44 as well, in the in-plane direction Dw of the sputtering target 30, the region Ri of the anti-deposition shield 32 on the ion source 18 side (see Figure 1) is composed of, for example, a surface 47 parallel to the surface 30a of the sputtering target 30. The outer edge portion 42e of the anti-deposition shield 44 corresponds to the outer edge portion 32e of the anti-deposition shield 32. The first inclined surface 45 of the anti-adhesion shield 44 corresponds to the first inclined surface 33 of the anti-adhesion shield 32. The second inclined surface 46 of the anti-adhesion shield 44 corresponds to the second inclined surface 34 of the anti-adhesion shield 32.
[0031] By using the holding section 40, it becomes possible to switch between four sputtering targets and irradiate them with an ion beam Ib to deposit films, thereby forming a multilayer film composed of multiple types of films with different compositions. When forming a multilayer film, the four sputtering targets are selected according to the composition of the multiple types of films that constitute the multilayer film to be deposited. For example, if the multilayer film is a reflective multilayer film in which low refractive index Mo layers and high refractive index Si layers are alternately stacked, one of the four sputtering targets is a molybdenum sputtering target and one is a silicon sputtering target. Furthermore, when forming a protective layer on the multilayer film, the remaining sputtering target among the four sputtering targets is made of the constituent material of the protective layer. This allows for the formation of both a reflective multilayer film and a protective layer. The protective layer is, for example, a Ru layer, in which case a Ru sputtering target is used. Preferably, the molybdenum sputtering target and the silicon sputtering target are formed on opposite sides of the frame 41. This prevents contamination of the silicon sputtering target by atoms sputtered from the molybdenum sputtering target. It also prevents contamination of the molybdenum sputtering target by atoms sputtered from the silicon sputtering target.
[0032] The holding section 40 is configured to hold, for example, four sputtering targets 30, but it is not particularly limited to this configuration; there can be multiple sputtering targets. The shape of the frame can also be appropriately adapted to the number of sputtering targets.
[0033] FIG. 8 is a schematic cross-sectional view showing an embodiment of the substrate with a reflective layer according to the embodiment of the present invention. The substrate 50 with a reflective layer shown in FIG. 8 has a configuration in which a reflective layer 52 that reflects EUV light and a protective layer 53 of the reflective layer 52 are laminated in this order on a substrate 51. The reflective layer 52 is a reflective multilayer film in which Mo layers as low-refractive-index layers and Si layers as high-refractive-index layers are alternately laminated. The protective layer 53 is composed of, for example, a Ru layer. When the substrate 50 with a reflective layer is measured by X-ray fluorescence analysis, the ratio of the detection intensity of Al Kα rays to the detection intensity of Mo Kα rays is 0.0043 or less, and when the substrate 50 with a reflective layer is measured by X-ray fluorescence analysis (XRF), the ratio of the detection intensity of Y Lα rays to the detection intensity of Mo Kα rays is 0.0008 or less. The ratio of the detection intensity of Al Kα rays to the detection intensity of Mo Kα rays is preferably 0.0040 or less, and more preferably 0.0030 or less. The ratio of the detection intensity of Y Lα rays to the detection intensity of Mo Kα rays is preferably 0.0004 or less. When the substrate 50 with a reflective layer is analyzed by X-ray fluorescence analysis, the lower limit of the ratio of the detection intensity of Al Kα rays to the detection intensity of Mo Kα rays is not particularly limited, and may be 0, or 0.0020 or more. In addition, the lower limit of the ratio of the detection intensity of Y Lα rays to the detection intensity of Mo Kα rays is not particularly limited, and may be 0. The analysis by X-ray fluorescence analysis can be performed by making X-rays incident from the reflective layer 52 side of the substrate 50 with a reflective layer. For the analysis by X-ray fluorescence analysis, for example, "X-ray Fluorescence Spectrometer ZSX Primus II" manufactured by Rigaku Corporation is used.
[0034] The substrate 50 with a reflective layer shown in FIG. 8 can be manufactured using the sputtering apparatus 10 shown in FIG. 1 described above. Specifically, Mo films and Si films are alternately formed on the surface 51a (film formation target surface) of the substrate 51 in the order of Mo film, Si film, Mo film, and Si film by an ion beam sputtering method, so as to form a reflective multilayer film in which Mo layers and Si layers are alternately laminated. After forming the reflective layer 52, a Ru layer, for example, is formed as the protective layer 53 on the reflective layer 52 by an ion beam sputtering method using the sputtering apparatus 10 shown in FIG. 1.
[0035] The sputtering apparatus 10 shown in FIG. 1 is used, for example, in the production of reflective mask blanks. The method for producing a reflective mask blank includes a step of forming a functional film on the surface of a substrate using the sputtering apparatus 10 shown in FIG. 1. Here, examples of the functional film include a reflective multilayer film constituting a reflective layer, a protective film constituting a protective layer, an absorber film, and a conductive film. The reflective mask blank will be described in detail later. The above-described substrate 50 with a reflective layer is used as a precursor of a reflective mask blank. In this case, the substrate 51 of the substrate 50 with a reflective layer can be used as the substrate of the reflective mask blank. The substrate 50 with a reflective layer is manufactured by the method for manufacturing a reflective mask blank. Hereinafter, the reflective mask blank will be described.
[0036] (Reflective Mask Blank) [Substrate for Mask Blank] The substrate for a mask blank preferably has a low coefficient of thermal expansion. The coefficient of thermal expansion of the substrate for a mask blank at 20°C is 0±1.0×10 -7 / °C is preferable, and 0±0.3×10 -7 / °C is more preferable. Examples of materials with a low coefficient of thermal expansion include SiO 2 -TiO 2 based glass and the like, but are not limited thereto, and substrates of crystallized glass precipitated with β-quartz solid solution, quartz glass, metallic silicon, metals and the like can also be used. SiO 2 -TiO 2 based glass is preferably quartz glass containing 90 to 95 mass% of SiO 2 and 5 to 10 mass% of TiO 2 .
[0037] The side of the substrate on which the reflective multilayer film is laminated (hereinafter also referred to as the "first main surface") preferably has high surface smoothness. The surface smoothness of the first main surface can be evaluated by its surface roughness. The surface roughness of the first main surface is preferably 0.15 nm or less in terms of root mean square roughness Rq. The surface roughness can be measured with an atomic force microscope, and the surface roughness will be described as root mean square roughness Rq based on JIS (Japanese Industrial Standards) - B0601. The first main surface is preferably surface-processed to a predetermined flatness in order to improve the pattern transfer accuracy and positional accuracy of the reflective mask obtained using a reflective mask blank. In a predetermined area of the first main surface of the substrate (for example, an area of 132 mm × 132 mm), the flatness is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. The flatness can be measured with a flatness meter manufactured by Fujifilm Corporation. The size and thickness of the substrate are determined as appropriate based on the design values of the mask, etc. For example, the outer dimensions may be 6 inches (152 mm) square and the thickness 0.25 inches (6.3 mm). Furthermore, it is preferable that the substrate has high rigidity in order to prevent deformation due to film stress of the film (reflective multilayer film, absorber film, etc.) formed on the substrate. For example, the Young's modulus of the substrate is preferably 65 GPa or higher.
[0038] [Reflective Multilayer Film] The reflective multilayer film provided on one side of the reflective mask blank is not particularly limited as long as it has the desired properties as a reflective film for the EUV mask blank. The reflective multilayer film preferably has a high reflectivity to EUV light. Specifically, when EUV light is incident on the surface of the reflective multilayer film at an incident angle of 6°, the maximum reflectivity of EUV light around a wavelength of 13.5 nm is preferably 60% or more, and more preferably 65% or more. Similarly, even when a protective layer is laminated on the reflective multilayer film, the maximum reflectivity of EUV light around a wavelength of 13.5 nm is preferably 60% or more, and more preferably 65% or more.
[0039] Reflective multilayer films can achieve high reflectivity of EUV light, and therefore, typically, a reflective multilayer film is used in which a high refractive index layer, which exhibits a high refractive index for EUV light, and a low refractive index layer, which exhibits a low refractive index for EUV light, are alternately stacked multiple times. The reflective multilayer film may be stacked in multiple cycles, with one cycle consisting of a stacked structure in which a high refractive index layer and a low refractive index layer are stacked in this order from the substrate side, or it may be stacked in multiple cycles, with one cycle consisting of a stacked structure in which a low refractive index layer and a high refractive index layer are stacked in this order. As the high refractive index layer, a Si layer or a layer containing Si can be used. As the Si-containing material, a Si compound containing one or more elements selected from the group consisting of B, C, N, and O can be used. By using a high refractive index layer containing Si, a reflective mask with excellent reflectivity of EUV light can be obtained. As the low refractive index layer, a layer containing a metal selected from the group consisting of Mo, Ru, Rh, and Pt, or an alloy thereof, can be used. Si layers are widely used for the high refractive index layer, and Mo layers are widely used for the low refractive index layer. In other words, Mo / Si reflective multilayer films are the most common. However, reflective multilayer films are not limited to this, and Ru / Si reflective multilayer films, Mo / Be reflective multilayer films, Mo compound / Si compound reflective multilayer films, Si / Mo / Ru reflective multilayer films, Si / Mo / Ru / Mo reflective multilayer films, and Si / Ru / Mo / Ru reflective multilayer films can also be used.
[0040] The film thickness of each layer constituting the reflective multilayer film and the number of repeating units in the layer can be appropriately selected according to the film material used and the required EUV light reflectance of the reflective layer. Taking a Mo / Si reflective multilayer film as an example, to create a reflective multilayer film with a maximum EUV light reflectance of 60% or more, a Mo film with a film thickness of 2.3 ± 0.1 nm and a Si film with a film thickness of 4.5 ± 0.1 nm should be stacked so that the number of repeating units is between 30 and 60.
[0041] Each layer constituting the reflective multilayer film can be formed to a desired thickness using the sputtering apparatus described above. When a reflective multilayer film is fabricated using ion beam sputtering, ion particles are supplied from an ion source to a sputtering target made of a high refractive index material and a sputtering target made of a low refractive index material. If the reflective multilayer film is a Mo / Si reflective multilayer film, for example, by ion beam sputtering, first a Si layer of a predetermined thickness is deposited on the substrate using a Si target. Then, a Mo layer of a predetermined thickness is deposited using a Mo target. By stacking these Si and Mo layers for 30 to 60 periods, with each period representing one cycle, a Mo / Si reflective multilayer film is formed.
[0042] [Protective Layer] The reflective mask blank may have a protective layer on the side opposite to the substrate side of the reflective multilayer film. The protective layer is provided to protect the reflective multilayer film from damage during the etching process (usually a dry etching process) when a pattern is formed on the absorber film by the etching process. A material that can achieve the above objective is a material containing at least one element selected from the group consisting of Ru and Rh. That is, it is preferable that the protective layer contains at least one element selected from the group consisting of Ru and Rh. More specifically, the above materials include elemental Ru metal, Ru alloys containing Ru and one or more metals selected from the group consisting of Si, Ti, Nb, Mo, Rh, and Zr, and Rh-based materials such as elemental Rh metal, Rh alloys containing Rh and one or more metals selected from the group consisting of Si, Ti, Nb, Ru, Ta, Mo, and Zr, Rh-containing nitrides containing the above Rh alloy and nitrogen, and Rh-containing oxynitrides containing the above Rh alloy, nitrogen, and oxygen. Furthermore, as materials that can achieve the above objectives, Al and nitrides containing these metals and nitrogen, and Al 2 O 3Examples include the following. Among these, Ru metal element, Ru alloy, Rh metal element, or Rh alloy are preferred as materials that can achieve the above objectives. As Ru alloys, Ru-Si alloy or Ru-Rh alloy is preferred, and as Rh alloys, Rh-Si alloy or Rh-Ru alloy is preferred.
[0043] The thickness of the protective layer is not particularly limited as long as it can perform its function as a protective layer. In terms of maintaining the reflectance of EUV light reflected by the reflective multilayer film, the thickness of the protective layer is preferably 1 to 60 nm, more preferably 1 to 10 nm, even more preferably 1.5 to 6 nm, and particularly preferably 2 to 5 nm. It is also preferable that the material of the protective layer is elemental Ru metal, Ru alloy, elemental Rh metal, or Rh alloy, and that the thickness of the protective layer is the preferred thickness described above.
[0044] The protective layer may be a single-layer film or a multilayer film consisting of multiple layers. If the protective layer is a multilayer film, it is preferable that each layer constituting the multilayer film is made of the preferred material described above. Furthermore, if the protective layer is a multilayer film, it is also preferable that the total thickness of the multilayer film is within the preferred range described above.
[0045] The protective layer can be formed using known film deposition methods such as magnetron sputtering and ion beam sputtering. When forming an Rh layer as a protective layer by magnetron sputtering, it is preferable to use an Rh target as the target and Ar gas as the sputtering gas.
[0046] [Absorber Film] The absorber film of a reflective mask blank is required to have high contrast between the EUV light reflected by the reflective multilayer film and the EUV light reflected by the absorber film when the absorber film is patterned. The patterned absorber film (absorber film pattern) may function as a binary mask by absorbing EUV light, or it may function as a phase-shift mask that reflects EUV light while interfering with the EUV light from the reflective multilayer film to produce contrast.
[0047] When an absorber film pattern is used as a binary mask, the absorber film must absorb EUV light and have a low reflectivity of EUV light. Specifically, when EUV light is irradiated onto the surface of the absorber film, the maximum reflectivity of EUV light around a wavelength of 13.5 nm is preferably 2% or less. The absorber film may contain one or more metals selected from the group consisting of Ta, Ti, Sn, and Cr, as well as one or more components selected from the group consisting of O, N, B, Hf, and H. Among these, it is preferable to include N or B. By including N or B, the crystalline state of the absorber film can be made amorphous or microcrystalline. The crystalline state of the absorber film is preferably amorphous. This improves the smoothness and flatness of the absorber film. Furthermore, when the smoothness and flatness of the absorber film are high, the edge roughness of the absorber film pattern is reduced, and the dimensional accuracy of the absorber film pattern can be improved. When using an absorber membrane pattern as a binary mask, the thickness of the absorber membrane is preferably 40 to 70 nm, and more preferably 50 to 65 nm.
[0048] When an absorber film pattern is used as a phase shift mask, the reflectivity of the absorber film for EUV light is preferably 2% or higher. To obtain a sufficient phase shift effect, the reflectivity of the absorber film is preferably 9 to 15%. When an absorber film is used as a phase shift mask, the contrast of the optical image on the wafer is improved and the exposure margin is increased. Examples of materials for forming a phase shift mask include elemental Ru metal, Ru alloys containing Ru and one or more metals selected from the group consisting of Cr, Au, Pt, Re, Hf, Ta, Ti, and Si, alloys of Ta and Nb, oxides containing Ru alloy or TaNb alloy and oxygen, nitrides containing Ru alloy or TaNb alloy and nitrogen, and oxynitrides containing Ru alloy or TaNb alloy, oxygen, and nitrogen. Examples of materials for forming a phase shift film include elemental Ir metal, Ir alloys containing Ir and one or more metals selected from the group consisting of Ta, Cr, W, Re, and Si. When using an absorber membrane pattern as a phase shift mask, the thickness of the absorber membrane is preferably 30 to 60 nm, and more preferably 35 to 55 nm.
[0049] The absorber film may be a single layer or a multilayer film consisting of multiple layers. If the absorber film is a single layer, the number of steps in mask blank manufacturing can be reduced, improving production efficiency. If the absorber film is a multilayer film, the layer located on the opposite side of the absorber film from the protective layer may be an anti-reflective film used when inspecting the absorber film pattern with inspection light (for example, wavelength 193-248 nm).
[0050] Absorber films can be formed using known film deposition methods such as magnetron sputtering and ion beam sputtering. For example, when forming a Ta nitride (TaN) film as an absorber film using magnetron sputtering, a Ta target is used, and Ar gas and N 2 By supplying a gas containing gas and performing sputtering, an absorber film can be formed.
[0051] [Conductive Film] The reflective mask blank may have a conductive film on the side of the substrate opposite to the first main surface (second main surface). By providing a conductive film, the reflective mask blank can be handled by an electrostatic chuck. The conductive film may include one or more first elements selected from the group consisting of Cr and Ta.
[0052] The conductive film contains one or more first elements selected from the group consisting of Cr and Ta. The conductive film may also contain one or more second elements selected from the group consisting of B, C, N, and O. However, the composition of the conductive film is different from the composition of the protective layer, which will be described in detail later. Note that different compositions include not only cases where different elements are contained in the conductive film and the protective layer, but also cases where two or more of the same elements are contained in the conductive film and the protective layer, and the element content ratios are different in the conductive film and the protective layer. The conductive film preferably contains either Cr or Ta as the first element, and more preferably contains Cr. The conductive film preferably contains N as the second element. The conductive film may also preferably contain Cr as the first element and at least N as the second element. Examples of specific materials that constitute the conductive film include elemental Cr, CrN, CrO, CrON, CrB, CrBN, CrC, CrCN, CrOC, elemental Ta, TaN, TaO, TaON, TaB, TaBN, TaC, TaCN, TaOC, CrTaO, and CrTaN, with elemental Cr, CrN, TaN, or TaBN being preferred. Notation such as "CrON" refers to a material containing Cr, O, and N, and the content ratio of these elements is not limited.
[0053] The conductive film preferably has a low sheet resistance. The sheet resistance of the conductive film is preferably 200 Ω / □ or less, and more preferably 100 Ω / □ or less. The thickness of the conductive film is preferably 10 to 1000 nm, and more preferably 100 to 500 nm. The back surface conductive film can be formed using known film formation methods, such as sputtering methods including magnetron sputtering and ion beam sputtering, CVD, vacuum deposition, and electrolytic plating.
[0054] [Other Films] Reflective mask blanks may have other films. Examples of other films include interlayers and hard mask films.
[0055] (Interlayer) The interlayer is a film provided between the protective layer and the reflective multilayer. The interlayer is a separate layer from the protective layer and is made of a material with a different composition from the protective layer. The material constituting the interlayer is preferably a material containing one or more elements selected from the group consisting of Ru, Rh, Pd, Ir, and Pt (hereinafter also referred to as "specific elements"). Among these, a material containing one or more elements selected from the group consisting of Ru and Rh is preferred, and a material containing Ru is preferred. The interlayer may consist only of the above-mentioned specific elements, or it may contain other elements. Other elements include one or more elements selected from the group consisting of Si, Ti, Cr, Zr, Nb, Mo, Pd, and Ta. In addition, it may contain at least one of B, C, N, and O as other elements. When the interlayer contains the above-mentioned specific elements, the content of the specific elements is preferably more than 50 atomic percent, more preferably 60 atomic percent or more, even more preferably 80 atomic percent or more, and particularly preferably 90 atomic percent or more. The interlayer may consist only of specific elements. The thickness of the interlayer is preferably 0.3 to 10.0 nm, more preferably 0.5 to 5.0 nm, even more preferably 0.5 to 2.5 nm, and particularly preferably 0.5 to 1.5 nm. It is also preferable to adjust the sum of the thickness of the interlayer and the thickness of the protective film so that it falls within the preferred range for the thickness of the protective film.
[0056] (Hard Mask Film) The hard mask film is preferably positioned on the side opposite to the protective layer of the absorber film. The hard mask film is preferably made of a material highly resistant to dry etching, such as a Cr-based film or a Si-based film. Examples of Cr-based films include materials containing Cr and one or more elements selected from the group consisting of Cr and O, N, C, and H. Specifically, examples include CrO and CrN. Examples of Si-based films include materials containing Si and one or more elements selected from the group consisting of Si and O, N, C, and H. Specifically, examples include SiO 2Examples include SiO, SiN, SiO, SiC, SiCO, SiCN, and SiCON. When a hard mask film is formed on the absorber film, dry etching can be performed even if the minimum line width of the absorber film pattern becomes small. Therefore, it is effective for miniaturizing the absorber film pattern. The hard mask film can be formed using known film deposition methods such as magnetron sputtering and ion beam sputtering.
[0057] A reflective mask is obtained by patterning the absorber film in a reflective mask blank to form an absorber film pattern. In a reflective mask, the openings of the absorber film reflect more EUV light, making it suitable for use as a reflective mask for exposure with EUV light.
[0058] <Method for Manufacturing Reflective Mask Blanks> As described above, the method for manufacturing reflective mask blanks includes a step of forming a functional film on the surface of a substrate using the sputtering apparatus 10 shown in Figure 1. The method for forming each film (functional film) of the reflective mask blank is as described above. A reflective mask blank can be manufactured by sequentially forming each of the above films on the first main surface of a mask blank substrate. Alternatively, a conductive film may be formed on the second main surface. For example, the mask blank substrate is the substrate 51 shown in Figure 8. Specifically, a method for manufacturing a reflective mask blank involves forming a reflective multilayer film on the mask blank substrate using the sputtering apparatus described above. Next, a protective layer is formed on the reflective multilayer film using the sputtering apparatus described above, an absorber film is formed on the protective layer, and a hard mask film is formed on the absorber film. Furthermore, the method for manufacturing a mask blank may include manufacturing procedures for films other than those described above. For example, after forming a reflective multilayer film using the sputtering apparatus described above, an intermediate film may be formed on the reflective multilayer film, and a protective layer may be formed on the intermediate film. In this case, when forming a reflective multilayer film, then forming the interlayer film on the reflective multilayer film, and then forming a protective layer on the interlayer film, it is preferable to carry out the formation continuously without exposure to the atmosphere from the start of interlayer film formation to the end of protective layer formation. Furthermore, it is also preferable to carry out the formation continuously without exposure to the atmosphere from the start of reflective multilayer film formation to the end of protective layer formation.
[0059] <Method for Manufacturing Transfer Masks> Figures 9(a) to 9(d) are schematic cross-sectional views showing an example of the manufacturing process for a transfer mask using a reflective mask blank according to an embodiment of the present invention, in order of the steps.
[0060] Figure 9(a) shows a state in which a resist pattern 70 has been formed on a reflective mask blank 60 in which a conductive film 69, a substrate 62, a reflective multilayer film 64, a protective layer 66, and an absorber film 68 are stacked in this order. A known method can be used to form the resist pattern 70. For example, a resist is applied to the absorber film 68 of the reflective mask blank 60, and exposure and development are performed to form the resist pattern 70. The resist pattern 70 corresponds to the transfer pattern of the resist film formed on the semiconductor substrate using a transfer mask. Then, using the resist pattern 70 in Figure 9(a) as a mask, the absorber film 68 is etched and patterned to remove the resist pattern 70, forming the absorber film pattern 68pt shown in Figure 9(b), and a laminate having the absorber film pattern 68pt is obtained. The absorber film pattern 68pt is a transfer pattern. Next, as shown in Figure 9(c), a resist pattern 72 corresponding to the frame of the exposure area is formed on the laminate shown in Figure 9(b), and dry etching is performed using the resist pattern 72 in Figure 9(c) as a mask. Dry etching is carried out until the substrate 62 is reached. After dry etching, the resist pattern 72 is removed to obtain the transfer mask 74 shown in Figure 9(d).
[0061] Dry etching for forming the absorber film pattern 68pt can be performed using, for example, a Cl-based gas or an F-based gas. The resist pattern 70 and resist pattern 72 can be removed by known methods, such as removal with a cleaning solution. Examples of cleaning solutions include sulfuric acid-hydrogen peroxide aqueous solution (SPM), sulfuric acid, ammonia water, ammonia-hydrogen peroxide aqueous solution (APM), OH radical cleaning water, and ozonated water. If the reflective mask blank 60 has an etching mask film, the etching mask film may be patterned using the resist pattern 70 as a mask, and dry etching may be performed using the pattern of the etching mask film as a mask. Also, if the reflective mask blank 60 has an etching mask film, a step to remove the etching mask film may be performed in the step to obtain the transfer mask. Furthermore, in the step to remove the resist pattern 70 or resist pattern 72 as described above, the etching mask film may also be removed at the same time. The absorber film pattern 68pt (transfer pattern) obtained by patterning the absorber film 68 of the reflective mask blank 60 is suitable for use in a transfer mask 74 used for exposure with EUV light.
[0062] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. Of the following examples 1 to 6 of substrates with reflective layers, Example 6 is an example, and Examples 1 to 5 are comparative examples.
[0063] <Example 1> In Example 1, a substrate 50 with a reflective layer as shown in Figure 8 was fabricated. TiO 2 -SiO 2 A glass substrate (square with outer dimensions of 152 mm x 152 mm and a thickness of 6.3 mm) was used. The thermal expansion coefficient of this glass substrate at 20°C is 0.02 x 10⁻⁶. -7 / °C, Young's modulus 67 GPa, Poisson's ratio 0.17, specific stiffness 3.07 × 10⁻⁶ 7 I understand 2 / s 2The glass substrate was polished to form a smooth surface with a surface roughness (rms) of 0.15 nm or less and a flatness of 100 nm or less. A 100 nm thick Cr film was deposited on the back side of the substrate 51 using magnetron sputtering to create a highly dielectric coating with a sheet resistance of 100 Ω / □. The substrate 51 was fixed to a flat electrostatic chuck via the formed Cr film, and an ion beam sputtering apparatus was used to alternately deposit Mo films and Si films on the surface of the substrate 51, repeating this process for 40 cycles to form a Mo / Si reflective multilayer film with a total thickness of 272 nm ((2.3 nm + 4.5 nm) × 40) as a reflective layer 52. Furthermore, a 2.5 nm thick Ru layer was formed on the Mo / Si reflective multilayer film as a protective layer 53 using ion beam sputtering. The ion beam sputtering apparatus used had an Al anti-deposition shield positioned to cover the sputtering target. The anti-deposition shield has a circular opening, into which the sputtering target is positioned. The anti-deposition shield used had its outermost surface coated with Al thermal spraying. The anti-deposition shield was constructed with planes parallel to the surface of the sputtering target in both the region on the ion source side and the region on the opposite side of the ion source. In Table 1 below, "Planar" is indicated in the "Upstream" and "Downstream" columns of the "Anti-deposition Shield Shape". Ar gas was used as the process gas. The parameters for the process gas during film formation were: F (sccm (standard cubic centimeter per minute)), the nominal diameter of the grid portion with the grid-like openings (indicated as "Nominal Diameter of Grid" in Table 1 below), r (cm) of the grid portion with the grid-like openings, and S (cm) of the grid's effective area. 2 The product of the effective area S of the grid and the flow rate F of the Ar process gas during film deposition (F × S) is as shown in Table 1 below. The beam voltage is 600V, and the pressure inside the vacuum chamber is 2.7 × 10⁻⁶. -2 Pa was used.
[0064] [XRF Intensity Ratio] For each example of substrate with a reflective film, XRF measurements were performed, and the ratio of the detected intensity of AlKα lines to the detected intensity of MoKα lines (indicated as "Al peak intensity / Mo peak intensity" in Table 1 below) and the ratio of the detected intensity of YLα lines to the detected intensity of MoKα lines (indicated as "Y peak intensity / Mo peak intensity" in Table 1 below) were calculated. If the intensity of YLα lines could not be detected, "-" was written in the "Y peak intensity / Mo peak intensity" column of Table 1 below. Rigaku's "ZSX Primus II" was used for the XRF measurements.
[0065] [Increase / Decrease in Peak Reflectance] For each of the substrates with reflective layers in Examples 2 to 6, EUV light was incident at an incident angle of 6° on the surface of the protective Ru layer. The reflected light in the EUV wavelength range at this time was measured using an EUV reflectometer, and the minimum value of the in-plane distribution of peak reflectance in the EUV wavelength range was determined for each of the substrates with reflective layers in Examples 2 to 6. Using the minimum value of the in-plane distribution of peak reflectance in the EUV wavelength range of Example 1 as the reference, the increase / decrease in peak reflectance for Examples 2 to 6 was calculated by (minimum value of the in-plane distribution of peak reflectance in the EUV wavelength range for each of Examples 2 to 6) / (minimum value of the in-plane distribution of peak reflectance in the EUV wavelength range of Example 1). Since Example 1 was used as the reference, the increase / decrease in peak reflectance of Example 1 was set to 0 (%). Note that a positive value of the increase / decrease in peak reflectance represents the increase in peak reflectance, and a negative value represents the decrease in peak reflectance.
[0066] <Examples 2-4> The flow rate F of the Ar process gas during film deposition, the nominal diameter of the portion of the grid where the grid-like openings are provided, the radius r of the portion of the grid where the grid-like openings are provided, the effective area S of the grid, and the product of the effective area S of the grid and the flow rate F of the Ar process gas during film deposition (F × S) are as shown in Table 1 below. Substrates with reflective layers shown in Figure 8 were fabricated using the same procedure as in Example 1. For the substrates with reflective layers in Examples 2-4, XRF measurements were performed as described above, and the ratio of the detection intensity of AlKα lines to the detection intensity of MoKα lines (indicated as "Al peak intensity / Mo peak intensity" in Table 1 below) and the ratio of the detection intensity of YLα lines to the detection intensity of MoKα lines (indicated as "Y peak intensity / Mo peak intensity" in Table 1 below) were calculated. For the substrates with reflective layers in Examples 2-4, the increase / decrease rate of the peak reflectivity was calculated as described above.
[0067] <Example 5> The outermost surface is Y 2 O 3 A substrate with a reflective layer was fabricated using the same procedure as in Example 1, except that an anti-adhesion shield sprayed with yttrium oxide was used. For the substrate with a reflective layer in Example 5, XRF measurements were performed as described above, and the ratio of the detection intensity of AlKα lines to the detection intensity of MoKα lines (indicated as "Al peak intensity / Mo peak intensity" in Table 1 below) and the ratio of the detection intensity of YLα lines to the detection intensity of MoKα lines (indicated as "Y peak intensity / Mo peak intensity" in Table 1 below) were calculated. For the substrate with a reflective layer in Example 5, the increase / decrease rate of the peak reflectance was calculated as described above.
[0068] <Example 6> A substrate with a reflective layer was fabricated using the same procedure as in Example 1, except that the anti-adhesion shield was configured to have a first inclined surface in the region opposite to the ion source, in addition to the outer edge of the anti-adhesion shield. The first inclined surface has the configuration shown in Figure 3(a), and is a curved surface that slopes from the surface of the sputtering target toward the opposite side of the surface as it moves from the sputtering target side toward the outer edge of the anti-adhesion shield. The first inclined surface was made into an inclined surface composed of a curved surface. In Table 1 below, "Plane" is written in the "Upstream side" column of "Anti-adhesion shield shape" and "Curved surface" is written in the "Downstream side" column. For the substrate with a reflective layer of Example 6, the above-described XRF measurement was performed, and the ratio of the detection intensity of AlKα lines to the detection intensity of MoKα lines (in Table 1 below, "Al peak intensity / Mo peak intensity") and the ratio of the detection intensity of YLα lines to the detection intensity of MoKα lines (in Table 1 below, "Y peak intensity / Mo peak intensity") were calculated. For the substrate with a reflective layer in Example 6, the increase / decrease rate of the peak reflectance was calculated as described above.
[0069]
[0070] As shown in Table 1, Example 6 contained less aluminum in the reflective film compared to Examples 1-4, and less yttrium in the reflective film compared to Example 5, thus suppressing contamination originating from the anti-adhesion shield. As a result, Example 6 showed improved reflectivity compared to Examples 1-5. The entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2025-082094, filed on May 15, 2025, are incorporated herein by reference as disclosure of the present invention.
[0071] 10 Sputtering apparatus 12 Vacuum chamber 12a Interior 13 Substrate holder 13a, 37, 47, 51a Surface 14 Rotating shaft 15 Drive unit 16 Piping 17a Valve 17b Vacuum pump 18 Ion source 19, 40 Holding unit 20 Substrate 30 Sputtering target 30a Surface 32, 44 Anti-adhesion shield 32a Opening 32d Surface 32e Outer edge 33, 33a, 33b, 45 First inclined surface 34, 34a, 34b, 46 Second inclined surface 35 Rectangle 41 Frame 41a, 41b, 41c, 41d Surface 41e Interior 42 Rotating shaft part 42c Rotating shaft 42e Outer edge 43 Housing 44a Opening 50 51, 62 Substrate with reflective layer 52 Reflective layer 53 Protective layer 60 Reflective mask blank 64 Reflective multilayer film 66 Protective layer 68 Absorber film 68pt Absorber film pattern 69 Conductive film 70, 72 Resist pattern 74 Transfer mask C Center Cs Rotation axis Dp Direction Ds Thickness direction Dw In-plane direction Ib Ion beam Pp Plane Ri, Ro, Rs Region Rsi Second region Rso First region Rvi, Rvo Virtual region
Claims
1. A sputtering apparatus comprising: irradiating an ion beam from an ion source toward a sputtering target, causing sputtering particles to fly toward the film-forming surface of a substrate, and forming a film containing the constituent materials of the sputtering target toward the film-forming surface of the substrate, wherein the sputtering apparatus has an anti-adhesion shield disposed around the sputtering target, and in the in-plane direction of the sputtering target, in the region of the anti-adhesion shield opposite to the ion source, the anti-adhesion shield has a first inclined surface other than the outer edge of the anti-adhesion shield, and the first inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target.
2. The sputtering apparatus according to claim 1, wherein the first inclined surface is a surface that is inclined from the surface toward the opposite side of the surface as it moves from the sputtering target side toward the outer edge side of the anti-adhesion shield.
3. The sputtering apparatus according to claim 1, wherein the anti-adhesion shield has an opening, the sputtering target is positioned in the opening, and when observed from the direction normal to the surface of the sputtering target, a rectangle is virtually drawn that is tangent to the opening and has one side parallel to the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and the first inclined surface is located in a virtual region enclosed by the rectangle and the opening, in the region of the anti-adhesion shield opposite to the ion source in the in-plane direction of the sputtering target.
4. The sputtering apparatus according to claim 1 or 2, wherein, in the in-plane direction of the sputtering target, the region of the anti-deposition shield on the ion source side has a region having a surface parallel to the surface of the sputtering target.
5. The sputtering apparatus according to claim 1, wherein the anti-adhesion shield has an opening, the sputtering target is positioned in the opening, and when observed from the direction normal to the surface of the sputtering target, a rectangle is virtually drawn that is tangent to the opening and has one side parallel to the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and in the in-plane direction of the sputtering target, there is a second inclined surface in the virtual region enclosed by the rectangle and the opening within the region of the anti-adhesion shield on the ion source side, and the second inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target.
6. The sputtering apparatus according to claim 5, wherein, in the in-plane direction of the sputtering target, within the region of the anti-deposition shield on the ion source side, the virtual region enclosed by the rectangle and the opening has an inclined surface of a different shape from the second inclined surface, or a flat surface.
7. The sputtering apparatus according to claim 1, wherein the anti-adhesion shield has an opening, the sputtering target is positioned in the opening, and when observed from the direction normal to the surface of the sputtering target, a rectangle is virtually drawn that is tangent to the opening and has one side parallel to the direction in which the irradiation direction of the ion beam is projected onto the surface of the sputtering target, and within the virtual region enclosed by the rectangle and the opening, in the in-plane direction of the sputtering target, there is a second inclined surface only in the region enclosed by the rectangle and the opening on the side of the anti-adhesion shield opposite to the ion source side, and the second inclined surface is a surface that gradually slopes downward from the surface of the sputtering target toward the opposite side of the surface in the thickness direction of the sputtering target.
8. The sputtering apparatus according to claim 1, wherein the anti-adhesion shield has an opening, the sputtering target is positioned in the opening, and the first inclined surface is formed by the intersection of a plane including a straight line passing through the center of the opening and extending in the direction of the projection of the irradiation direction of the ion beam onto the surface of the sputtering target, the normal of the surface of the sputtering target passing through the center of the opening, and the surface of the anti-adhesion shield.
9. The sputtering apparatus according to any one of claims 5 to 7, wherein the anti-adhesion shield has an opening, the sputtering target is positioned in the opening, and the second inclined surface is formed by the intersection of a plane including a straight line passing through the center of the opening and extending in the direction of the projection of the irradiation direction of the ion beam onto the surface of the sputtering target, the normal of the surface of the sputtering target passing through the center of the opening, and the surface of the anti-adhesion shield.
10. A sputtering apparatus according to claim 1 or 2, used for manufacturing reflective mask blanks.
11. A method for manufacturing a reflective mask blank, comprising the step of forming a functional film on the surface of a substrate using the sputtering apparatus described in claim 1 or 2.
12. A substrate with a reflective layer, wherein a reflective layer that reflects EUV light and a protective layer for the reflective layer are laminated in this order on a substrate, wherein the reflective layer is a reflective multilayer film in which a low refractive index layer, a Mo layer, and a high refractive index layer, a Si layer, are alternately laminated, and when the substrate with the reflective layer is measured by X-ray fluorescence analysis, the ratio of the detection intensity of AlKα lines to the detection intensity of MoKα lines is 0.0043 or less, and when the substrate with the reflective layer is measured by X-ray fluorescence analysis, the ratio of the detection intensity of YLα lines to the detection intensity of MoKα lines is 0.0008 or less.