Porous carbon, porous carbon for power storage devices, powder for power storage devices, electrode for power storage devices, and power storage device

Porous carbon with controlled phenolic groups addresses the rapid capacity loss issue in energy storage devices by maintaining high retention rates under high voltage conditions.

WO2026239876A1PCT designated stage Publication Date: 2026-11-19PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016099
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-04-22
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing energy storage devices using carbon materials experience rapid decreases in capacity retention rate when subjected to relatively high voltages, with the exact cause attributed to certain functional groups in the carbon material.

Method used

Development of porous carbon with a controlled amount of phenolic groups, measured by a temperature-induced desorption method, to maintain a high capacity retention rate over extended periods, characterized by specific surface area, pore distribution, and work function.

Benefits of technology

The porous carbon maintains a high capacity retention rate for energy storage devices even under high voltage conditions, extending the device's effective lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016099_19112026_PF_FP_ABST
    Figure JP2026016099_19112026_PF_FP_ABST
Patent Text Reader

Abstract

This porous carbon includes phenol groups in an amount AP of 0.01 mmol / g or less. The amount AP of phenol groups is measured by a temperature-programmed desorption method (TDS). The amount of CO gas generated when the porous carbon is heated to 1200°C according to TDS is, for example, 0.005-0.2 mmol / g.
Need to check novelty before this filing date? Find Prior Art

Description

Porous carbon, porous carbon for energy storage devices, powder for energy storage devices, electrodes for energy storage devices, and energy storage devices

[0001] This disclosure relates to porous carbon, porous carbon for energy storage devices, powder for energy storage devices, electrodes for energy storage devices, and energy storage devices.

[0002] Conventionally, it is known that carbon materials such as activated carbon are used in energy storage devices.

[0003] For example, Patent Document 1 describes a BET specific surface area of ​​1200 m² measured by nitrogen adsorption. 2 The description includes activated carbon with a concentration of 0.3 ml / g or less, and a pore volume of 0.3 ml / g or more as measured by the t-plot method using nitrogen adsorption. This activated carbon is used as an electrode in electric double-layer capacitors.

[0004] Japanese Patent Publication No. 2004-67498

[0005] The description in the above-mentioned patent document warrants reconsideration from the viewpoint of maintaining a high capacity retention rate of energy storage devices for extended periods under predetermined conditions. Therefore, this disclosure provides a novel porous carbon that is advantageous from this viewpoint.

[0006] This disclosure provides porous carbon, wherein the amount of phenolic groups in the porous carbon, as measured by a temperature-induced desorption method, is 0.01 mmol / g or less.

[0007] According to this disclosure, it is possible to provide a novel porous carbon that is advantageous in that it can maintain a high capacity retention rate of an energy storage device for a long period of time under predetermined conditions.

[0008] Figure 1 is a schematic cross-sectional view showing an example of the porous carbon of this disclosure. Figure 2 is a flowchart showing an example of a method for producing the porous carbon of this disclosure. Figure 3 is a schematic diagram showing an example of the powder for energy storage devices of this disclosure. Figure 4 is a schematic diagram showing an example of an electrode for energy storage devices of this disclosure. Figure 5 is a schematic diagram showing an example of an energy storage device of this disclosure. Figure 6 is a graph showing the time change in the capacity retention rate of electric double-layer capacitors (EDLCs) according to the examples and comparative examples. Figure 7 is a graph showing the pore distribution of porous carbon according to the examples and comparative examples.

[0009] (Knowledge forming the basis of this disclosure) Maintaining a high capacity retention rate for a long period of time in energy storage devices such as EDLCs can enhance the value of the energy storage device. On the other hand, the inventors have found that when an energy storage device equipped with electrodes containing carbon materials such as activated carbon is used under predetermined conditions, the capacity retention rate of the energy storage device tends to decrease in a short time. For example, when a relatively high voltage (e.g., 3.0V or higher) is applied to such an energy storage device, the capacity retention rate of the energy storage device tends to decrease in a short time. The reason for this is not clear, but the inventors considered that some functional group contained in the carbon material may be involved in the rapid decrease in the capacity retention rate of the energy storage device. Further investigation by the inventors revealed that by using a specific porous carbon, the capacity retention rate of the energy storage device can be maintained at a high level for a long period of time even when the energy storage device is used under predetermined conditions. Detailed analysis of this porous carbon revealed that the amount of a predetermined functional group in the porous carbon was relatively low. Based on this new finding, the inventors have completed the porous carbon related to this disclosure.

[0010] The embodiments of this disclosure will be described below with reference to the drawings. This disclosure is not limited to the embodiments described below. The embodiments described below are all comprehensive or specific examples. Therefore, the numerical values, shapes, materials, components, arrangement positions of components, and connection configurations shown in the embodiments below are examples and are not intended to limit this disclosure. In addition, components in the embodiments below that are not described in an independent claim indicating the highest-level concept will be described as optional components. Also, in the drawings, components with the same reference numerals may not be described. Furthermore, the drawings are schematic representations of each component for ease of understanding, and the shapes and dimensional ratios may not be accurately represented.

[0011] (Embodiment) Figure 1 is a schematic cross-sectional view showing an example of the porous carbon of the present disclosure. As shown in Figure 1, the porous carbon 1a has pores of various sizes. Amount of phenol groups on the surface of the porous carbon 1a, including the inside of the pores, as measured by the temperature desorption method (TDS) A P The amount is 0.01 mmol / g or less. With this configuration, when an energy storage device equipped with an electrode containing porous carbon 1a is used at a relatively high voltage (e.g., 3.0V), the capacity retention rate of the energy storage device tends to remain high for a long time. The reason for this is not clear, but it is thought that the phenolic groups contained in the carbon material are involved in the rapid decrease in the capacity retention rate of the energy storage device. Amount of phenolic groups A P This can be determined, for example, according to the method described in the examples.

[0012] Amount A of the phenol group mentioned above P Preferably, the concentration is 0.005 mmol / g or less, more preferably 0.001 mmol / g or less, and even more preferably 0.0005 mmol / g or less. In this case, when an energy storage device equipped with electrodes containing porous carbon 1a is used at a relatively high voltage, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a longer period of time.

[0013] Amount A of the phenol group mentioned above Pis, for example, 0 mmol / g or more, and may be 0 mmol / g.

[0014] As shown in Figure 1, the porous carbon 1a has, for example, macropores 11, mesopores 12, and micropores 13. The definition of pores in this specification follows the definition of the International Union of Pure and Applied Chemistry (IUPAC). Pores having a pore diameter of 2 nm or less are micropores, pores having a pore diameter of 2 nm to 50 nm are mesopores, and pores having a pore diameter of 50 nm or more are macropores.

[0015] Amount A of phenolic groups P is 0.01 mmol / g or less, the amount A of CO gas generated when the porous carbon 1a is heated to 1200°C according to TDS is not limited to a specific value. CO The amount A of CO gas CO is, for example, 0.005 mmol / g or more and 0.2 mmol / g or less. In this case, when an electricity storage device provided with an electrode containing the porous carbon 1a is used at a relatively high voltage, the capacity retention rate of the electricity storage device is more likely to remain high for a long time. The amount A of CO gas CO can be determined, for example, according to the method described in the Examples.

[0016] As long as the amount A of phenolic groups P is 0.01 mmol / g or less, the work function of the porous carbon 1a is not limited to a specific value. The work function of the porous carbon 1a is, for example, 5.0 eV or less. In this case, when an electricity storage device provided with an electrode containing the porous carbon 1a is used at a relatively high voltage, the capacity retention rate of the electricity storage device is more likely to remain high for a long time. The work function of a material is determined as the sum of the bulk term and the surface term. The bulk term is determined by the substance, and the surface term is determined by the surface state of the material. When the work function of the porous carbon 1a is 5.0 eV or less, the surface of the porous carbon 1a is considered to be in a desirable state from the viewpoint that the capacity retention rate of the electricity storage device is kept high for a long time when used at a relatively high voltage. The work function of the porous carbon 1a can be measured, for example, according to the method described in the Examples.

[0017] Amount A of phenolic groups PAs long as the concentration is 0.01 mmol / g or less, the pore distribution of the porous carbon 1a is not limited to a specific distribution. The pore distribution of the porous carbon 1a has, for example, a first peak of 2 nm or less and a second peak of 3 nm to 6 nm. In this case, when an energy storage device equipped with electrodes containing porous carbon 1a is used at a relatively high voltage, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a longer period of time.

[0018] In the pore distribution of porous carbon 1a, for example, the second peak is the largest peak below 6 nm. In this case, when an energy storage device equipped with electrodes containing porous carbon 1a is used at relatively high voltages, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a longer period of time.

[0019] The pore distribution of the porous carbon 1a does not have a peak in the range of 2 nm to 2.5 nm, for example. In this case, when an energy storage device equipped with electrodes containing porous carbon 1a is used at a relatively high voltage, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a longer period of time.

[0020] Amount of phenol group A P As long as the concentration is 0.01 mmol / g or less, the BET specific surface area of ​​porous carbon 1a is not limited to a specific value. The BET specific surface area of ​​porous carbon 1a is, for example, 800 m 2 It is 1 / g or more. In this case, when an energy storage device equipped with electrodes containing porous carbon 1a is used at a relatively high voltage, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a longer period of time. The BET specific surface area of ​​porous carbon 1a is determined, for example, by N2 gas adsorption measurement based on Japanese Industrial Standard (JIS) Z 8830:2013. Specifically, by performing a BET plot analysis on the desorption side of an N2 gas adsorption / desorption isotherm, the amount of N2 gas required to form a monolayer is calculated, and the BET specific surface area is calculated based on that amount of N2 gas.

[0021] The BET specific surface area of ​​porous carbon 1a is preferably 900 m². 2 It is 1 / g or more. The BET specific surface area of ​​porous carbon 1a is, for example, 3000 m². 2 It is less than / g and 2800m2 It may be less than / g.

[0022] The total pore volume of porous carbon 1a is not limited to a specific value. The total pore volume of porous carbon 1a can be, for example, 0.2 to 4.0 cm³. 3 It is / g, and ranges from 0.4 to 3.8 cm. 3 / g is also acceptable.

[0023] Amount A of the phenol group mentioned above P As long as the concentration is 0.01 mmol / g or less, the method for producing porous carbon 1a is not limited to a specific method. Figure 2 is a flowchart showing an example of a method for producing porous carbon according to the present disclosure. As shown in Figure 2, the method for producing porous carbon 1a includes, for example, pre-calcination S1 and final calcination S2.

[0024] In pre-calcination S1, zinc organic acid, or a mixture of organic acid and zinc precursor, is calcined at a temperature of 1000°C or lower under an inert gas atmosphere, removing excess components as gases such as hydrogen, water, carbon monoxide, and carbon dioxide. In addition, micropores and mesopores are formed in the remaining carbon, and the zinc is evaporated and removed to obtain a calcined carbon body.

[0025] In the main firing S2, the carbon sintered body obtained in the pre-firing S1 is fired at 1000°C or higher under an inert gas atmosphere to remove the terminal hydrogen of the carbon. This yields porous carbon 1a.

[0026] Pre-firing S1 and main firing S2 may be performed separately. Pre-firing S1 and main firing S2 may also be performed continuously. In this case, the cooling time in pre-firing S1 and the heating time in main firing S2 can be omitted, and the productivity of porous carbon 1a tends to increase.

[0027] As described above, in pre-calcination S1, zinc organic acid, or a mixture of organic acid and zinc precursor, is calcined at a temperature of 1000°C or lower to perform carbonization, pore formation, and zinc removal. During carbonization and pore formation, hydrogen, water, carbon monoxide, and carbon dioxide are removed as gases from the zinc organic acid, or the mixture of organic acid and zinc precursor, during the heating process. In addition, micropores and mesopores are formed on the surface of the remaining carbon by zinc oxide, which serves as a template. Furthermore, during zinc removal, the zinc oxide template is reduced and evaporated.

[0028] Firing in an atmospheric environment causes carbon in the raw material to combine with oxygen in the atmosphere, resulting in a combustion reaction that produces carbon dioxide. This leads to the loss of carbon. For this reason, pre-firing S1 is preferably carried out in an inert gas atmosphere. The type of inert gas is not limited to a specific type. From an economic standpoint, the inert gas is preferably nitrogen gas or argon gas, and more preferably nitrogen gas. Pre-firing S1 may be carried out while replacing the inert gas atmosphere with a gas flow rate of 0.1 to 10.0 liters / minute.

[0029] The heating rate in pre-firing S1 is not limited to a specific value. In pre-firing S1, for example, the temperature may be raised from a predetermined temperature to a desired temperature at a heating rate of about 3 to 20°C / min. The range of temperatures that can be reached in pre-firing S1 is not limited to a specific range, as it depends on the firing method, the type of firing furnace, the processing time (holding time), and the amount of raw material processed. From the viewpoint of sufficiently removing oxygen-containing functional groups of carbon and reduced zinc, the range of temperatures that can be reached is preferably 910 to 1000°C, which is above the boiling point of zinc, 907°C. In pre-firing S1, the processing time (holding time) for maintaining the above-mentioned temperature range is not limited to a specific value, as it depends on the firing method, the type of firing furnace, and the amount of raw material processed. The processing time in pre-firing S1 is, for example, 0.5 to 20 hours, preferably 1 to 15 hours. Pre-firing S1 may be carried out under a reduced pressure atmosphere. The firing method for pre-firing S1 may be batch type or continuous type. Examples of furnaces for pre-firing S1 include core-tube type furnaces, box furnaces, rotary kiln furnaces, and conveyor furnaces. When pre-firing S1 is batch-type, the raw materials are placed in a crucible and fired. The crucible is not limited to a specific type. Examples of crucibles include those made of alumina, quartz, and carbon.

[0030] In the main firing S2, as described above, the carbon calcined body obtained in the pre-firing S1 is calcined at 1000°C or higher under an inert gas atmosphere to remove the terminal hydrogen of the carbon and obtain porous carbon 1a. The type of inert gas is not limited to a specific type. From an economic standpoint, the inert gas is preferably nitrogen gas or argon gas, and more preferably nitrogen gas. The main firing S2 may be carried out while replacing the inert gas atmosphere with a gas flow rate of 0.1 to 10.0 liters / min.

[0031] The heating rate in the main firing S2 is not limited to a specific value. In the main firing S2, for example, the temperature may be raised from a predetermined temperature to a desired temperature at a heating rate of about 3 to 20°C / min. The achievable temperature range in the pre-firing S1 is not limited to a specific range, as it depends on the firing method, the type of firing furnace, the processing time (holding time), and the amount of raw material processed. From the viewpoint of sufficiently removing terminal hydrogen from carbon, the achievable temperature range is preferably 1700 to 2000°C, and more preferably 1800 to 1900°C. In the main firing S2, the processing time (holding time) during which the temperature is maintained within the achievable temperature range is not limited to a specific value, as it depends on the firing method, the type of firing furnace, and the amount of raw material processed. The processing time in the main firing S2 is, for example, 0.5 to 20 hours, and preferably 1 to 15 hours. The main firing S2 may be carried out under a reduced pressure atmosphere. The firing method for the main firing S2 may be batch type or continuous type. Examples of furnaces used for the main firing S2 include core-tube type furnaces, box furnaces, rotary kiln furnaces, and conveyor furnaces. When the main firing S2 is performed at 1200°C or higher, the firing furnace is preferably a stationary core-tube type furnace or a box furnace. When the main firing S2 is performed in a batch manner, the raw materials are placed in a crucible and fired. From the viewpoint of heat resistance, the crucible is preferably made of carbon.

[0032] The raw materials for porous carbon 1a include, for example, at least one selected from the group consisting of zinc citrate, zinc hydrogen citrate, zinc oxalate, zinc fumarate, zinc succinate, zinc caffeate, zinc chlorogenicate, zinc ferulate, zinc quinate, zinc lactate, zinc malonate, zinc gluconate, zinc tartrate, zinc malate, zinc benzoate, zinc picolinate, and zinc octolate. Two or more types of organic zinc acids may be used as raw materials for porous carbon 1a. The organic zinc acids may be hydrated or anhydrous.

[0033] The raw material of the porous carbon 1a is not limited to the above-mentioned organic acid zinc, and may be a mixture of an organic acid and a zinc precursor. Examples of the organic acid are known organic acids such as citric acid, oxalic acid, fumaric acid, succinic acid, caffeic acid, chlorogenic acid, ferulic acid, quinic acid, lactic acid, malonic acid, gluconic acid, tartaric acid, malic acid, benzoic acid, picolinic acid, and octylic acid. Examples of the zinc precursor are known zinc precursors such as zinc hydroxide, zinc nitrate, zinc sulfate, zinc acetate, zinc chloride, zinc carbonate, and zinc oxide.

[0034] When two or more types of organic acid zinc are used in combination, the mixing ratio of the organic acid zinc is not limited to a specific value. On the other hand, from the viewpoint of complex formation between the organic acid and zinc, the molar ratio of the amount of the zinc precursor to the amount of the organic acid in the mixture of the organic acid and the zinc precursor is preferably 0.8 to 2.2, and more preferably 1.0 to 2.0. The method for mixing the organic acid and the zinc precursor may be a wet method or a dry method.

[0035] The porous carbon 1a may be provided, for example, as porous carbon for electrical storage devices.

[0036] A powder for electrical storage devices containing the porous carbon 1a can be provided. FIG. 3 is a diagram schematically illustrating an example of the powder for electrical storage devices of the present disclosure. As shown in FIG. 3, the powder 2a for electrical storage devices contains the porous carbon 1a.

[0037] The average particle diameter of the porous carbon 1a in the powder 2a for electrical storage devices is not limited to a specific value. The average particle diameter of the porous carbon 1a is, for example, 5 to 20 μm. This average particle diameter is, for example, the median diameter (D50) in the volume-based particle size distribution obtained by laser diffraction particle size distribution measurement.

[0038] An electrode for electrical storage devices containing the porous carbon 1a can be provided. FIG. 4 is a diagram schematically illustrating an example of the electrode for electrical storage devices of the present disclosure. As shown in FIG. 4, the electrode 3a for electrical storage devices contains the porous carbon 1a. For this reason, when the electrical storage device provided with the electrode 3a for electrical storage devices is used at a relatively high voltage, the capacity retention rate of the electrical storage device is likely to be kept high for a long time.

[0039] In the electrode 3a for the energy storage device, the porous carbon 1a is arranged on or near the surface of the electrode 3a. The electrode 3a for the energy storage device includes, for example, a current collector 31. The current collector 31 is, for example, a metal foil such as copper foil and aluminum foil. The electrode 3a for the energy storage device can be manufactured, for example, by applying a slurry in which porous carbon 1a is dispersed onto the current collector 31 and drying the resulting coating. In addition to porous carbon 1a, the slurry may also contain a conductive additive and a binder. The conductive additive may be, for example, a conductive additive known as a conductive additive for electrodes for energy storage devices, such as acetylene black. The binder may be a conductive additive known as a binder for electrodes for energy storage devices. Examples of binders include styrene-butadiene rubber-based binders, fluororesins such as polytetrafluoroethylene (PTFE), and polypyrinidene fluoride (PDVF).

[0040] An energy storage device equipped with an electrode 3a for energy storage devices can be provided. Figure 5 is a schematic diagram showing an example of the energy storage device of this disclosure. As shown in Figure 5, the energy storage device 5a includes a first electrode 51, a first terminal 51t, a second electrode 52, a second terminal 52t, and an electrolyte 53. The first terminal 51t is electrically connected to the first electrode 51. The second terminal 52t is electrically connected to the second electrode 52. The electrolyte 53 is disposed between the first electrode 51 and the second electrode 52. The electrolyte 53 may contain an electrolyte solution or may be a solid electrolyte. If the electrolyte 53 contains an electrolyte solution, a separator may be disposed between the first electrode 51 and the second electrode 52.

[0041] When an external power supply is connected between the first terminal 51t and the second terminal 52t, a voltage is applied between the first electrode 51 and the second electrode 52, and energy is stored in the energy storage device 5a. When an external load is connected between the first terminal 51t and the second terminal 52t, discharge occurs in the energy storage device 5a, and the electrical energy stored in the energy storage device 5a is supplied to the external load.

[0042] In the energy storage device 5a, at least one selected from the group consisting of the first electrode 51 and the second electrode 52 is the electrode 3a for the energy storage device. In this case, when the energy storage device 5a is used at a relatively high voltage, the capacity retention rate of the energy storage device 5a is likely to be kept high for a long time. Only one of the first electrode 51 and the second electrode 52 may be the electrode 3a for the energy storage device, or both the first electrode 51 and the second electrode 52 may be the electrode 3a for the energy storage device.

[0043] The energy storage device 5a is not limited to a specific type of energy storage device. For example, the energy storage device 5a is an EDLC. The energy storage device 5a may also be a secondary battery. An example of a secondary battery is a lithium-ion secondary battery.

[0044] (Note) Based on the above description, the following technologies are disclosed. (Technology 1) A porous carbon wherein the amount of phenol groups of the porous carbon, as measured by the thermal desorption method, is 0.01 mmol / g or less. (Technology 2) The porous carbon according to Technology 1, wherein the amount of CO gas generated when the porous carbon is heated to 1200°C according to the thermal desorption method is 0.005 mmol / g or more and 0.2 mmol / g or less. (Technology 3) The porous carbon according to Technology 1 or 2, having a work function of 5.0 eV or less. (Technology 4) The porous carbon according to any one of Technology 1 to 3, wherein the pore distribution of the porous carbon has a first peak of 2 nm or less and a second peak of 3 nm or more and 6 nm or less. (Technology 5) 800 m 2 (Technology 6) A porous carbon having a BET specific surface area of ​​1 / g or more, as described in any one of the Techniques 1 to 4. (Technology 7) A porous carbon for energy storage devices, comprising the porous carbon described in any one of the Techniques 1 to 5. (Technology 8) An electrode for energy storage devices, comprising the porous carbon described in any one of the Techniques 1 to 5. (Technology 9) An energy storage device equipped with the electrode for energy storage devices described in Technique 8.

[0045] The present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples.

[0046] <Example 1> 6.0 g of white zinc citrate (Zn3(C6H5O7)2) manufactured by Sigma-Aldrich was placed in a quartz inner case as a raw material, and the quartz inner case containing the white powder was placed in the center of the furnace tube of a rotary kiln RK-0330 manufactured by Motoyama. The furnace tube was not rotated, in other words, the raw material was not stirred, and the material was heated and calcined while it was standing. The atmosphere temperature was raised from 25°C to 950°C at a heating rate of 3°C / min under a nitrogen gas atmosphere, and the atmosphere temperature was maintained at 950°C for 6 hours to pre-calcine the raw material, which carried out carbonization accompanied by pore formation, reduction of zinc oxide, and evaporation removal of zinc. This obtained the pre-calcined product according to Example 1. The pre-calcined product according to Example 1 was a black powder with a mass of 0.15 g, and the yield in the pre-calcination was 2.5% by mass.

[0047] Furthermore, 2.55 g of the pre-calcined material according to Example 1, obtained through multiple pre-calcinations, was heated in an argon atmosphere from 25°C to 1800°C at a heating rate of 10°C / min, and the atmosphere temperature was maintained at 1800°C for 2 hours for the main calcination. This is thought to have removed the terminal hydrogen of the porous carbon. In this way, the porous carbon according to Example 1 was obtained. The porous carbon according to Example 1 was a black powder, and its mass was 2.41 g. The yield in the main calcination was 94.5% by mass.

[0048] <Example 2> Porous carbon according to Example 2 was obtained in the same manner as in Example 1, except that zinc benzoate (Zn(C6H5COO)2) manufactured by Fujifilm Wako Pure Chemical Industries was used instead of zinc citrate.

[0049] <Comparative Example 1 and Comparative Example 2> For Comparative Example 1 and Comparative Example 2, porous carbon materials derived from coconut shells, such as activated carbon YP-50F manufactured by Kuraray Co., Ltd., were used as the porous carbon.

[0050] (EDLC Capacity Retention Rate) Porous carbon, conductive additive, and binder according to each example and comparative example were mixed in a mortar in the following proportions while adding an appropriate amount of water to prepare a porous carbon-containing slurry according to each example and comparative example. Carboxymethylcellulose and styrene-butadiene rubber (SBR) were used as the binder. This porous carbon-containing slurry was coated onto a current collector, which was an aluminum foil with a thickness of 30 μm, to form a coating film, and the coating film was dried and press-molded. After that, the current collector on which the porous carbon-containing film was formed was punched out in a square shape with a side length of 20 mm in a plan view to produce electrodes according to each example and comparative example. <Formulation of Porous Carbon, Conductive Additive, and Binder> Porous carbon according to each example and comparative example: 85 parts by mass Conductive additive (acetylene black): 5 parts by mass Binder: 10 parts by mass

[0051] The electrolyte was prepared by adding the organic salt triethylmethylammonium tetrafluoroborate (TEMA-BF4) to the non-aqueous solvent propylene carbonate (PC) to a concentration of 1.0 mol / L.

[0052] For each example and each comparative example, a pair of electrodes was prepared, and with lead wires connected to each electrode, each electrode was vacuum-dried at 110°C. A cellulose nonwoven fabric was punched out into a square shape with sides of 25 mm in a plan view, and then vacuum-dried at 110°C. Using the electrodes from each example and each comparative example, the separator made of the nonwoven fabric was sandwiched between the pair of electrodes, set in a heat-sealable outer material, injected the electrolyte, and vacuum-impregnated with the electrolyte. In addition, the outer material was heat-sealed to produce the EDLCs from each example and each comparative example.

[0053] Float tests were performed on EDLCs according to each example and comparative example. In the float tests, each EDLC according to each example and comparative example was charged with a predetermined current in a 25°C atmosphere until the voltage of the pair of electrodes reached 3.5 [V], and then discharged with a predetermined current until the voltage of the pair of electrodes reached a predetermined voltage. The discharge current amount mAh was recorded. In the float tests, each EDLC according to each example and comparative example was placed in a 50°C constant temperature bath, charged with a predetermined current until the voltage of the pair of electrodes reached 3.5V, maintained at 3.5V for a predetermined time, and then discharged and returned to a 25°C atmosphere for cell characteristic evaluation. This process was repeated to perform float tests for 2500 hours. Based on the results of the float tests, the capacity retention rate of each EDLC according to each example and comparative example was evaluated.

[0054] Figure 6 is a graph showing the time evolution of the capacity retention rate of EDLCs in the examples and comparative examples. In the graph shown in Figure 6, the vertical axis represents the capacity retention rate, and the horizontal axis represents the time during which the ambient temperature of the EDLC and the voltage of the pair of electrodes were maintained at 50°C and 3.5V, respectively. The capacity retention rate is expressed as a percentage of the ratio of the discharge current capacity at a specific point in time to the initial discharge current capacity. Table 1 shows the capacity retention rates of the EDLCs in each example and comparative example at a point in time when the time during which the ambient temperature and the voltage of the pair of electrodes were maintained at 50°C and 3.5V, respectively, was 1000 hours.

[0055] As shown in Figure 6 and Table 1, the capacity retention rate of the EDLC in the example was maintained at a higher rate for a longer period than that of the EDLC in the comparative example. Therefore, it was suggested that the porous carbon in the example contributes to maintaining the capacity retention rate of the energy storage device for a long period of time when a relatively high voltage is applied to the energy storage device.

[0056] (TDS) Samples for TDS analysis were obtained from porous carbons related to each example and comparative example. Using a device consisting of a heating furnace with a temperature controller (NETZSCH STA449 F5) directly connected to a JEOL mass spectrometer (JMS-Q1500GC), the behavior and changes in the amount of gas components generated from each sample as the temperature increased were detected as a function of temperature. For the measurement, the temperature of the heating furnace was maintained at 100°C for 1 hour with He gas flowing at a flow rate of 100 mL / min, and then the temperature of the heating furnace was increased from 100°C to 1200°C at a rate of 20°C / min, and maintained at 1200°C for 30 minutes. Based on the TDS analysis, the amount of phenol groups and the amount of CO gas generated in each porous carbon were determined. The results are shown in Table 1.

[0057] (Work Function) Using a Hitachi High-Technologies AFM5000 surface potential microscope (KFM), the surface potential of porous carbon in each example and comparative example was measured, and the work function of porous carbon in each example and comparative example was determined. The results are shown in Table 1.

[0058] As shown in Table 1, the amount of phenol groups in the porous carbon of Examples 1 and 2, as measured by TDS, was 0.01 mmol / g or less. On the other hand, the amount of phenol groups in the porous carbon of Comparative Examples 1 and 2 exceeded 0.01 mmol / g. A comparison between the examples and comparative examples suggests that when the amount of phenol groups in porous carbon, as measured by TDS, is 0.01 mmol / g or less, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a long period of time when a relatively high voltage is applied to the energy storage device.

[0059] As shown in Table 1, the amount of CO gas generated when the porous carbon according to Example 1 and Example 2 was heated to 1200°C according to the TDS was relatively low, falling within the range of 0.005 mmol / g to 0.2 mmol / g. On the other hand, the amount of CO gas generated when the porous carbon according to Comparative Example 1 and Comparative Example 2 was heated to 1200°C according to the TDS exceeded 0.2 mmol / g. A comparison between the examples and comparative examples suggests that if the amount of CO gas generated when the porous carbon is heated to 1200°C according to the TDS is between 0.005 mmol / g and 0.2 mmol / g, the capacity retention rate of the energy storage device is likely to be maintained for a long period of time.

[0060] As shown in Table 1, the work function of the porous carbon in Examples 1 and 2 was relatively low, at 5.0 eV or less. On the other hand, the work function of the porous carbon in Comparative Examples 1 and 2 exceeded 5.0 eV. A comparison between the examples and comparative examples suggests that when the work function of porous carbon is 5.0 eV or less, the capacity retention rate of the energy storage device is more likely to be maintained at a high level for a long period of time when a relatively high voltage is applied to the energy storage device. It is considered that a work function of 5.0 eV or less is desirable for the surface of the porous carbon from the viewpoint of maintaining a high capacity retention rate for a long period of time.

[0061]

[0062] (BET specific surface area and pore distribution) The BET specific surface area and pore distribution of porous carbon for each example and comparative example were determined by N2 gas adsorption measurement based on JIS Z 8830:2013. Using an automatic specific surface area / pore distribution analyzer manufactured by Anton Paar, nitrogen gas was adsorbed onto the sample at a relative pressure of 77 K, and an adsorption isotherm was obtained. The BET specific surface area of ​​the sample was determined from the obtained nitrogen gas adsorption isotherm using the BET method. The results are shown in Table 2. In addition, the pore distribution of the sample was determined using the DFT method. The applicable range of the BET method was defined as P / P0 = 0.1 to 0.3, where linearity is observed.

[0063] Figure 7 is a graph showing the pore distribution of porous carbon in the examples and comparative examples. The graph in Figure 7 is the log differential pore volume distribution, and the vertical axis is dV / (logd) [cm]. 3 The horizontal axis shows the pressure [ / g], and the horizontal axis shows the pore diameter [nm]. From the pore distribution shown in Figure 7, the pore diameters corresponding to the peaks in the pore distribution in the range of 2 to 6 nm were identified. The results are shown in Table 2. In addition, Table 3 shows whether or not there are peaks in the pore distribution in a specific range of pore diameters.

[0064]

[0065]

[0066] As shown in Figure 7 and Table 3, the pore distribution of the porous carbon in each example had a peak below 2 nm and also a peak between 3 nm and 6 nm. On the other hand, the pore distribution of the porous carbon in each Comparative Example 2 did not have a peak between 3 nm and 6 nm. Comparing the examples and comparative examples, it is thought that having peaks in the pore distribution of porous carbon at both 2 nm and below and between 3 nm and 6 nm makes it easier to maintain a high capacity retention rate for energy storage devices over a long period of time.

[0067] The porous carbon of this disclosure can be used as an electrode material for energy storage devices such as EDLCs and secondary batteries.

Claims

1. Porous carbon, wherein the amount of phenolic groups in the porous carbon, as measured by the temperature-induced desorption method, is 0.01 mmol / g or less.

2. The porous carbon according to claim 1, wherein the amount of CO gas generated when the porous carbon is heated to 1200°C according to the temperature-induced desorption method is 0.005 mmol / g or more and 0.2 mmol / g or less.

3. The porous carbon according to claim 1, having a work function of 5.0 eV or less.

4. The porous carbon according to claim 1, wherein the pore distribution of the porous carbon has a first peak of 2 nm or less and a second peak of 3 nm or more and 6 nm or less.

5. 800m 2 The porous carbon according to claim 1, having a BET specific surface area of ​​1 / g or more.

6. Porous carbon for energy storage devices, comprising the porous carbon described in any one of claims 1 to 5.

7. Powder for energy storage devices comprising porous carbon as described in any one of claims 1 to 5.

8. An electrode for an energy storage device comprising porous carbon according to any one of claims 1 to 5.

9. An energy storage device comprising electrodes for an energy storage device as described in claim 8.