Thermally conductive silicone composition
A thermally conductive silicone composition with controlled filler distribution and reaction products addresses pumping-out and curing challenges, ensuring reliable, low-resistance thermal management for electronic components.
Patent Information
- Application Number
- PCT/JP2026/016107
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-04-22
- Publication Date
- 2026-11-19
AI Technical Summary
Existing thermal greases for electronic component packages and power modules face challenges such as poor shelf life, complex curing processes, environmental impact, and issues with pumping out, especially in non-curing types, which compromise reliability and ease of application.
A thermally conductive silicone composition comprising an organopolysiloxane addition reaction product, aluminum nitride and zinc oxide particles with controlled particle size distribution, and a hydrolyzable organopolysiloxane, maintaining appropriate viscosity and providing excellent application workability, good pumping-out resistance, and low thermal resistance.
The composition achieves low thermal resistance when compressed thinly, enhances reliability, and is easy to handle, suitable for modern semiconductor devices with increased heat generation and complex structures, while being transportable at room temperature.
Smart Images

Figure JP2026016107_19112026_PF_FP_ABST
Abstract
Description
Thermally conductive silicone composition
[0001] One aspect of the present invention relates to a thermally conductive silicone composition.
[0002] For thermal management of electronic component packages and power modules, a thermal grease that is thin, compressible, and has excellent penetration into the gap between heat-generating parts and cooling materials is preferable from the viewpoint of heat dissipation performance. Thermal greases can be broadly classified into two types: "hardening type," which can be hardened after being compressed to a desired thickness, and "non-hardening type," which remains grease-like without hardening. Hardening type thermal greases, by hardening after being compressed to a desired thickness, make it less likely for the thermal grease to leak out (pumping out) caused by expansion and contraction due to the repeated thermal history of heating and cooling of the heat-generating parts, thereby improving the reliability of semiconductor packages. However, hardening type thermal greases also have characteristics that are disadvantageous in practical use.
[0003] For example, many addition-curing thermal greases have been proposed in the past for use as thermal greases in electronic component packages and power modules (e.g., Patent Document 1). However, most of these have poor shelf life at room temperature and require freezing or refrigeration, which can make product management difficult. Furthermore, since heating for a certain period of time is required for curing, it leads to a decrease in production efficiency due to the complexity and length of the process, and is also undesirable from the perspective of environmental impact due to the heating process.
[0004] Condensation-curing type thermal greases can also be cited as one type of "curing type" thermal grease (for example, Patent Document 2). Condensation-curing type thermal greases thicken and harden due to moisture in the air, so they can be transported and stored at room temperature if moisture is blocked, and product management is relatively easy. Furthermore, condensation-curing type thermal greases have the advantage that the curing reaction can proceed without a heating process if a certain amount of moisture is present. However, they have a major problem in that low-boiling-point desorbed components are produced during the curing reaction, which can cause odor and contamination of electronic components by the desorbed components.
[0005] On the other hand, "non-curing" thermal greases are generally easy to handle, as they can be transported and stored at room temperature, but they have the drawback of being prone to the aforementioned pumping-out. To reduce pumping-out in "non-curing" thermal greases, increasing the viscosity of the grease is effective. However, this comes at the cost of reduced application ease.
[0006] As mentioned above, while the use of "curing" thermal grease is preferable to improve the reliability of electronic component packages and power modules, it has challenges such as requiring strict temperature control, a complicated curing process, and environmental impact.
[0007] On the other hand, "non-curing" thermal greases are easy to handle and have a low environmental impact, but they are prone to pumping out. Therefore, to ensure the reliability of electronic component packages and power modules, it is necessary to increase the viscosity of the thermal grease, but this comes at the expense of ease of application. Furthermore, in order to compress the thermal grease thinly and achieve low thermal resistance, it is necessary to precisely control the particle size distribution of the thermal conductive filler. Patent document 3 describes a non-curing thermal conductive silicone composition that improves resistance to pumping out by blending a silicone gel crosslinked product, a hydrolyzable organopolysiloxane, and aluminum nitride particles with controlled particle size distribution in specific proportions. However, further improvement in resistance to pumping out is desired.
[0008] Japanese Patent Publication No. 2016-053140, Japanese Patent Publication No. 2011-219664, Japanese Patent Publication No. 2021-098804
[0009] As described above, there is a need for the development of a thermally conductive silicone composition, particularly one suitable for non-curing heat dissipation greases, that maintains an appropriate viscosity despite containing a large amount of thermally conductive filler, exhibits excellent application workability, has good pumping-out resistance, and can be compressed thinly to achieve low thermal resistance.
[0010] The present invention has been made in view of the above circumstances, and aims to provide a thermally conductive silicone composition that has excellent coating workability by maintaining an appropriate viscosity while containing a large amount of thermally conductive filler, has good pumping-out resistance, and provides low thermal resistance when compressed thinly.
[0011] As a result of diligent research to achieve the above objective, the inventors have discovered that a thermally conductive silicone composition comprising an organopolysiloxane addition reaction product having a specific composition, aluminum nitride particles and zinc oxide particles with controlled particle size distribution as thermally conductive fillers, and a hydrolyzable organopolysiloxane in specific proportions, has appropriate viscosity, excellent application workability, good pumping-out resistance, and low thermal resistance when compressed thinly, thus completing the present invention.
[0012] In other words, the present invention provides a thermally conductive silicone composition comprising the following components (A) to (D) and having a viscosity of 200 Pa·s to 600 Pa·s at 25°C. (A) Addition reaction product of component (a) and component (b): in an amount of 1 to 3% by mass of the total mass of the composition (a) Having at least two aliphatic unsaturated hydrocarbon groups in one molecule, with a kinematic viscosity of 60 mm at 25°C 2 (b) Organopolysiloxane having 1 / s or more (a) Organohydrogenpolysiloxane having 2 or more hydrogen atoms bonded to silicon atoms in one molecule: (a) an amount such that the ratio of the number of hydrogen atoms (SiH groups) bonded to silicon atoms to the total number of aliphatic unsaturated hydrocarbon groups in the component is 0.3 to 0.7 (B) Aluminum nitride particles having a 90% particle diameter of 18.0 μm or less by volume, a 50% particle diameter of 7.0 μm or more and 12.0 μm or less by volume, and a 440 mesh sieve residue of 0.1 mass% or less of the total particles: an amount that is 50 to 60 mass% of the total mass of the composition (C) Zinc oxide particles having a 50% particle diameter of 0.1 μm or more and 1.0 μm or less by volume: an amount that is 30 to 40 mass% of the total mass of the composition, (D) Organopolysiloxane represented by the following general formula (1): an amount of 1 to 10% by mass of the total mass of the composition (In the formula, R 1(These are, independently of each other, monovalent hydrocarbon groups having 1 to 18 carbon atoms, and at least one hydrogen atom bonded to the carbon atom of the monovalent hydrocarbon group may be substituted with a substituent, and n is an integer in the range of 5 to 100).
[0013] Furthermore, a preferred embodiment of the present invention provides a thermally conductive silicone composition having at least one of the following [2] to [4]: [2] The thermally conductive silicone composition according to [1], wherein n in the general formula (1) of the (D) organopolysiloxane is an integer in the range of 10 to 60. [3] The thermally conductive silicone composition according to [1] or [2], wherein the oxygen content of the (B) aluminum nitride particles is 0.25% by mass or less. [4] The specific surface area of the (B) aluminum nitride particles is 0.20 m² 2 / g or more 0.60m 2 A thermally conductive silicone composition according to any one of [1] to [3] above, wherein the amount is less than or equal to / g. Furthermore, a preferred embodiment of the present invention provides a heat dissipation grease containing the above thermally conductive silicone composition.
[0014] The thermally conductive silicone composition of the present invention maintains appropriate viscosity despite containing a large amount of thermally conductive filler. This achieves both excellent application workability and resistance to pumping out, and furthermore, it can be compressed to a thin layer and has low thermal resistance. Therefore, this thermally conductive silicone composition can cope with the increased heat generation, larger size, and more complex structure of semiconductor devices in recent years. In addition, the thermally conductive silicone composition of the present invention can be suitably used as a non-curing type heat dissipation grease. Furthermore, this thermally conductive silicone composition can be transported and stored at room temperature and is easy to handle.
[0015] The present invention will be described in detail below, but the present invention is not limited thereto. In this invention, the maximum and minimum numerical values may include rounded values.
[0016] [Thermally Conductive Silicone Composition] The thermally conductive silicone composition of the present invention contains (A) an organopolysiloxane addition product, (B) aluminum nitride particles, (C) zinc oxide particles, and (D) a hydrolyzable organopolysiloxane in specific proportions. That is, components (A) to (D) above are essential components in the thermally conductive silicone composition of the present invention. The thermally conductive silicone composition of the present invention may contain other components as needed.
[0017] In other words, the present invention is a thermally conductive silicone composition comprising the following components (A) to (D), having a viscosity of 200 Pa·s or more and 600 Pa·s or less at 25°C. (A) Addition reaction product of component (a) and component (b): in an amount of 1 to 3% by mass of the total mass of the composition (a) Having at least two aliphatic unsaturated hydrocarbon groups in one molecule, with a kinematic viscosity of 60 mm at 25°C 2 (b) Organopolysiloxane having 1 / s or more (a) Organohydrogenpolysiloxane having 2 or more hydrogen atoms bonded to silicon atoms in one molecule: (a) an amount such that the ratio of the number of hydrogen atoms (SiH groups) bonded to silicon atoms to the total number of aliphatic unsaturated hydrocarbon groups in the component is 0.3 to 0.7 (B) Aluminum nitride particles having a 90% particle diameter of 18.0 μm or less by volume, a 50% particle diameter of 7.0 μm or more and 12.0 μm or less by volume, and a 440 mesh sieve residue of 0.1 mass% or less of the total particles: an amount that is 50 to 60 mass% of the total mass of the composition (C) Zinc oxide particles having a 50% particle diameter of 0.1 μm or more and 1.0 μm or less by volume: an amount that is 30 to 40 mass% of the total mass of the composition, (D) Organopolysiloxane represented by the following general formula (1): an amount of 1 to 10% by mass of the total mass of the composition (In the formula, R 1 (These are, independently of each other, monovalent hydrocarbon groups having 1 to 18 carbon atoms, and at least one hydrogen atom bonded to the carbon atom of the monovalent hydrocarbon group may be substituted with a substituent, and n is an integer in the range of 5 to 100).
[0018] The thermally conductive silicone composition of the present invention maintains an appropriate viscosity despite containing a large amount of thermally conductive filler, and has good reliability. Furthermore, the thermally conductive silicone composition of the present invention can be thinly compressed to achieve low thermal resistance. Therefore, the reliability of mounted electronic components can be improved. A more preferred embodiment of the present invention is a non-curable heat-dissipating grease composed of the above thermally conductive silicone composition. In the present invention, the term "non-curable" refers to an embodiment in which the composition is used while remaining in a grease state without being cured.
[0019] In a more preferred embodiment of the thermally conductive silicone composition of the present invention, n in the general formula (1) is in the range of 10 to 60. Thereby, more excellent coating workability and pumping-out resistance can be effectively achieved at the same time.
[0020] In a more preferred embodiment of the thermally conductive silicone composition of the present invention, the oxygen content of the aluminum nitride particles is 0.25 mass% or less. Thereby, the thermal resistance can be reduced more effectively.
[0021] In a more preferred embodiment of the thermally conductive silicone composition of the present invention, the specific surface area of the aluminum nitride particles is 0.20 m 2 / g or more and 0.60 m 2 / g or less. Thereby, the thermal resistance can be reduced more effectively.
[0022] Hereinafter, the components (A) to (D) will be described in more detail.
[0023] Component (A) The component (A) is an organopolysiloxane addition reaction product obtained by a hydrosilylation reaction of the following component (a) and component (b). The component (A) is the base polymer of the thermally conductive silicone composition of the present invention. (a) Having at least two aliphatic unsaturated hydrocarbon groups in one molecule, and a kinematic viscosity at 25°C of 60 mm 2(b) an organopolysiloxane having a ratio of 1 / s or more, (a) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule: an amount such that the ratio of the number of hydrogen atoms (SiH groups) bonded to silicon atoms to the total number of aliphatic unsaturated hydrocarbon groups in component (a) above is 0.3 to 0.7. The amount of component (A) blended in the thermally conductive silicone composition is 1 to 3% by mass of the total mass of the composition, more preferably 1.2 to 2.5% by mass, and most preferably 1.5 to 2% by mass.
[0024] (a) The kinematic viscosity of component is 60 mm at 25°C. 2 The value is 1 / s or more, preferably 100 mm 2 It is preferable that the kinematic viscosity is 1 / s or higher. If the kinematic viscosity is below the above lower limit, the resulting thermally conductive silicone composition may undergo expansion and contraction due to the repeated heating and cooling of the heating element, which may cause pumping out. In addition, if the kinematic viscosity is below the above lower limit, it may cause heterogeneity of the addition reaction product. The upper limit of the kinematic viscosity of component (a) is not particularly limited, but for example, 1,000,000 mm at 25°C. 2 It is preferable that it be less than or equal to / s, and more preferably 30,000 mm 2 It is less than or equal to / s, and more preferably 5,000 mm 2 It is preferable that the value be less than or equal to / s. In this invention, the kinematic viscosity is the value measured at 25°C using an Ostwald viscometer (the same applies hereinafter).
[0025] Component (a) has at least two aliphatic unsaturated hydrocarbon groups, preferably 2 to 50. If the number of aliphatic unsaturated hydrocarbon groups is less than two, the pumping-out resistance of the resulting thermally conductive silicone composition may decrease. The organopolysiloxane of component (a) may be a single type or a combination of two or more types. The aliphatic unsaturated hydrocarbon group is preferably a monovalent hydrocarbon group having an aliphatic unsaturated bond and having 2 to 8 carbon atoms, more preferably 2 to 6 carbon atoms. More preferably an alkenyl group, such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl groups. Among these, vinyl is preferred. The aliphatic unsaturated hydrocarbon group may be bonded to a silicon atom at the end of the molecular chain, to a silicon atom in the middle of the molecular chain, or to both.
[0026] (a) In the organopolysiloxane of component (a), organic groups other than aliphatic unsaturated hydrocarbon groups bonded to the silicon atom include unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms. Examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups; or groups in which some or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, bromine, or chlorine, or cyano groups, for example, chloromethyl, chloropropyl, bromoethyl, trifluoropropyl, and cyanoethyl groups. Among these, the methyl group is preferred.
[0027] The component (a) may be an organopolysiloxane having at least two aliphatic unsaturated hydrocarbon groups in one molecule, and its molecular structure is not particularly limited. Examples thereof include organopolysiloxanes having a linear structure, a branched structure, a partially branched structure, or a linear structure having a cyclic structure. In particular, an organopolysiloxane having a linear structure in which the main chain is composed of repeating diorganosiloxane units and both molecular chain terminals are blocked with triorganosiloxy groups is preferred. The organopolysiloxane having a linear structure may partially have a branched structure or a cyclic structure. The weight average molecular weight of the organopolysiloxane may be a value that makes the kinematic viscosity of the organopolysiloxane fall within the above-mentioned range.
[0028] The component (b) is an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule. The organohydrogenpolysiloxane preferably has 3 to 100, more preferably 5 to 20 hydrogen atoms bonded to silicon atoms (hereinafter referred to as SiH groups). The SiH groups in the molecule of the organohydrogenpolysiloxane undergo a hydrosilylation reaction with the aliphatic unsaturated hydrocarbon groups contained in the component (a), preferably in the presence of a platinum group metal catalyst, to form a crosslinked structure.
[0029] In the organohydrogenpolysiloxane of component (b), examples of organic groups other than hydrogen atoms bonded to silicon atoms include unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms. For example, alkyl groups such as methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, tert-butyl group, pentyl group, neopentyl group, hexyl group, cyclohexyl group, octyl group, nonyl group and decyl group, aryl groups such as phenyl group, tolyl group, xylyl group and naphthyl group, aralkyl groups such as benzyl group, phenylethyl group and phenylpropyl group, or groups obtained by substituting part or all of the hydrogen atoms of these groups with halogen atoms such as fluorine, bromine and chlorine, cyano groups and the like, such as chloromethyl group, chloropropyl group, bromoethyl group, trifluoropropyl group, cyanoethyl group and the like. Among them, methyl group is preferred.
[0030] The component (b) may be any organohydrogenpolysiloxane having the above properties, and its molecular structure is not particularly limited. Examples thereof include organohydrogenpolysiloxanes having a linear structure, a branched chain structure, a cyclic structure, a partially branched structure, or a linear structure with a cyclic structure. Preferred are organohydrogenpolysiloxanes having a linear structure or a cyclic structure.
[0031] The organohydrogenpolysiloxane preferably has a kinematic viscosity at 25°C of 1 to 1,000 mm 2 / s, more preferably 10 to 200 mm 2 / s. When the kinematic viscosity of the organohydrogenpolysiloxane is at or above the above lower limit, there is no risk of deterioration in the physical properties of the resulting thermally conductive silicone composition. In addition, when the kinematic viscosity of the organohydrogenpolysiloxane is at or below the above upper limit, there is no risk that the resulting thermally conductive silicone composition will have poor spreadability. The organohydrogenpolysiloxanes may be used singly or in combination of two or more thereof.
[0032] The blending amount of component (b) in the above (A) addition reaction product is an amount such that the ratio of the number of SiH groups in component (b) to the total number of aliphatic unsaturated hydrocarbon groups in component (a) is 0.3 to 0.7, preferably 0.4 to 0.6. If the blending ratio of component (b) to component (a) is less than the above lower limit, the hydrosilylation reaction between component (a) and component (b) will not proceed sufficiently, resulting in insufficient crosslinking. As a result, sufficient pumping-out resistance may not be obtained. If the blending ratio of component (b) to component (a) exceeds the above upper limit, the crosslinking density becomes too high, which may increase the viscosity of the thermally conductive silicone composition and degrade the coating workability.
[0033] The hydrosilylation reaction between component (a) and component (b) is preferably carried out in the presence of a conventionally known platinum group metal catalyst. Examples of platinum group metal catalysts include platinum-based, palladium-based, and rhodium-based catalysts. Among these, platinum or platinum compounds, which are relatively easy to obtain, are preferred. Examples include elemental platinum, platinum black, chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, and platinum coordination compounds. The platinum group metal catalyst may be a single type or a combination of two or more types.
[0034] The amount of platinum group metal catalyst added should be an effective amount as a catalyst. That is, it should be an effective amount necessary to promote the hydrosilylation reaction between component (a) and component (b) to obtain the addition product, i.e., the silicone gel crosslinked product. Preferably, the amount is 0.1 to 500 ppm, more preferably 1 to 200 ppm, on a mass basis converted to platinum group metal atoms, relative to the total mass of component (a) and component (b) (i.e., the total mass of component (A)). If the amount of catalyst added is within the above preferred range, sufficient catalytic effect can be obtained economically.
[0035] When obtaining the addition product (silicone gel crosslinked product) of component (a) and component (b) by hydrosilylation reaction, a reaction control agent may be added to ensure the reaction proceeds uniformly. Conventional reaction control agents can be used. Examples of such agents include acetylene compounds such as acetylene alcohols (e.g., ethynylmethyldecylcarbinol, 1-ethynyl-1-cyclohexanol, 3,5-dimethyl-1-hexyne-3-ol), various nitrogen compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole, organophosphorus compounds such as triphenylphosphine, oxime compounds, and organochloro compounds.
[0036] The amount of reaction control agent is preferably 0.05 to 5% by mass, and more preferably 0.1 to 1% by mass, relative to the total mass of components (a) and (b) (i.e., the total mass of component (A)). It is preferable that the amount of reaction control agent is within the above range, as this allows the hydrosilylation reaction to proceed more uniformly. The reaction control agent may be diluted with organo(poly)siloxane, toluene, or the like to improve its dispersibility in the silicone composition.
[0037] (B) Component (B) is aluminum nitride particles in which the 90% particle diameter by volume is 18.0 μm or less, the 50% particle diameter by volume is 7.0 μm or more and 12.0 μm or less, and the residue after 440 mesh sieving is 0.1% by mass or less of the total. These aluminum nitride particles are blended into the thermally conductive silicone composition as a thermally conductive filler to impart thermal conductivity.
[0038] The 90% particle diameter of the above aluminum nitride particles is 18.0 μm or less, preferably 17.7 μm or less. There is no lower limit to the 90% particle diameter, but it can be, for example, 14.0 μm or more. In this invention, the 90% particle diameter is the particle diameter at which the cumulative distribution based on volume in particle size distribution measurement by laser light diffraction reaches 90%.
[0039] The 50% particle diameter of the above aluminum nitride particles is 7.0 μm or more and 12.0 μm or less, preferably 8.0 μm or more and 11.5 μm or less. In the present invention, the 50% particle diameter is the particle diameter at which the cumulative distribution based on volume in particle size distribution measurement by laser light diffraction becomes 50%, and is the so-called median diameter.
[0040] The residue of the aluminum nitride particles after sieving through a 440-mesh sieve is 0.1% by mass or less of the total particles, preferably 0.05% by mass or less. There is no particular lower limit for the residue after sieving through a 440-mesh sieve, and the smaller the amount, the better. For example, it can be 0.00% by mass or more. In this invention, the residue after sieving through a 440-mesh sieve refers to the mass percentage of particles that do not pass through the sieve and remain on the mesh when aluminum nitride particles are sieved through a 440-mesh sieve. A 440-mesh sieve is a sieve with 440 mesh openings per inch, and its opening size (pore diameter) is approximately 32 μm.
[0041] In the present invention, the particle size can be measured, for example, using the "SALD-2300 Laser Diffraction Particle Size Distribution Analyzer" manufactured by Shimadzu Corporation.
[0042] If aluminum nitride particles do not satisfy at least one of the following requirements: 90% particle diameter based on volume, 50% particle diameter based on volume, and 440-mesh sieve residue, the compressibility of the resulting thermally conductive silicone composition will deteriorate, making it impossible to compress it thinly, and therefore low thermal resistance may not be obtained.
[0043] The aluminum nitride particles preferably have an oxygen content of 0.25% by mass or less. By using these aluminum nitride particles, the thermal resistance of the resulting thermally conductive silicone composition can be further reduced. The oxygen content of the aluminum nitride particles is preferably 0.25% by mass or less, and more preferably 0.15% by mass or less. There is no lower limit to the oxygen content, but for example, it should be 0.05% by mass or more. In this invention, the oxygen content is measured by an oxygen-nitrogen analyzer and can be analyzed by comparison with silicon nitride in a standard sample. As the oxygen-nitrogen analyzer, Shimadzu Corporation's "EMGA-920" can be used.
[0044] The aluminum nitride particles preferably have a specific surface area of 0.20 m². 2 / g or more 0.60m 2It is preferable that the particle size is less than or equal to / g. By using these aluminum nitride particles, the thermal resistance of the resulting thermally conductive silicone composition can be further reduced and the application workability can be improved. The specific surface area of the aluminum nitride particles is 0.20 m². 2 / g or more 0.60m 2 Preferably less than / g, and 0.25m 2 / g or more 0.50m 2 A value of less than or equal to / g is more preferable. In this invention, the specific surface area can be measured using the BET method, for example, the "BELSORP MAX G high-precision gas adsorption amount measuring device" manufactured by Microtrac-Bel.
[0045] The shape of the aluminum nitride particles is not particularly limited and can be spherical, irregular, needle-shaped, etc.
[0046] The amount of aluminum nitride particles is 50 to 60% by mass of the total mass of the composition, preferably 53 to 58% by mass. If the amount of aluminum nitride particles is greater than the upper limit, the thermally conductive silicone composition will have poor extensibility. Conversely, if the amount of aluminum nitride particles is less than the lower limit, the resulting thermally conductive silicone composition will have poor thermal conductivity.
[0047] (C) Component (C) is zinc oxide particles having a volume-based 50% particle diameter of 0.1 μm or more and 1.0 μm or less. These zinc oxide particles are incorporated into the thermally conductive silicone composition as a thermally conductive filler to impart thermal conductivity.
[0048] The above 50% particle size is 0.1 μm or more and 1.0 μm or less, preferably 0.2 to 0.8 μm or less. If the 50% particle size of zinc oxide particles is less than the above lower limit, the viscosity of the thermally conductive silicone composition may increase, and the application workability may deteriorate. Also, if the 50% particle size of zinc oxide particles is greater than the above upper limit, the compressibility of the thermally conductive silicone composition may deteriorate, and the thermal resistance may worsen. The 50% particle size can be determined, for example, as the average value (median diameter) based on volume in particle size distribution measurement by laser diffraction.
[0049] The shape of zinc oxide particles is not particularly limited and can be spherical, irregularly shaped, needle-shaped, etc.
[0050] The amount of zinc oxide particles is 30 to 40% by mass of the total mass of the composition, preferably 33 to 38% by mass. If the amount of zinc oxide particles is greater than the upper limit, the thermally conductive silicone composition will have poor extensibility. Conversely, if the amount of zinc oxide particles is less than the lower limit, the resulting thermally conductive silicone composition will have poor thermal conductivity.
[0051] Component (D) Component (D) is a hydrolyzable organopolysiloxane represented by the following general formula (1). This hydrolyzable organopolysiloxane is blended to treat the surface of components (B) and (C), which are thermally conductive fillers in the present invention, and plays a role in assisting in the high-filling of the thermally conductive fillers. (In the formula, R 1 (These are, independently of each other, monovalent hydrocarbon groups having 1 to 18 carbon atoms, and at least one hydrogen atom bonded to the carbon atom of the monovalent hydrocarbon group may be substituted with a substituent, and n is an integer in the range of 5 to 100).
[0052] In general formula (1), R 1 This is a monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably a monovalent saturated aliphatic hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 1 to 6 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, preferably 6 to 10 carbon atoms, more preferably 6 to 8 carbon atoms, and even more preferably 6 carbon atoms. 1 R is more preferably a monovalent saturated aliphatic hydrocarbon group. 1 These monovalent hydrocarbon groups may also be groups in which at least one hydrogen atom bonded to the carbon atom is substituted with a substituent. Examples of substituents include halogen atoms such as fluorine, chlorine, bromine, and iodine.
[0053] Examples of the above-mentioned monovalent saturated aliphatic hydrocarbon group include linear alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups; branched alkyl groups such as isopropyl, isobutyl, tert-butyl, isopentyl, and neopentyl groups; and cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups. Alternatively, halogen-substituted alkyl groups may be used, in which some or all of the hydrogen atoms bonded to the carbon atoms of the above-mentioned monovalent saturated aliphatic hydrocarbon group are substituted with halogen atoms. Examples of halogen-substituted alkyl groups include chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, and bromopropyl groups.
[0054] Examples of the monovalent aromatic hydrocarbon group include aryl groups such as phenyl and tolyl groups, and aralkyl groups such as benzyl and 2-phenylethyl groups. Alternatively, a halogen-substituted aryl group may be used, in which some or all of the hydrogen atoms bonded to the carbon atom of the monovalent aromatic hydrocarbon group are substituted with halogen atoms. Examples of halogen-substituted aryl groups include α,α,α-trifluorotolyl and chlorobenzyl groups.
[0055] R 1 Of the above, methyl groups, ethyl groups, 3,3,3-trifluoropropyl groups, and phenyl groups are preferred. More preferably, methyl groups, ethyl groups, and phenyl groups are preferred, and methyl groups are particularly preferred.
[0056] In general formula (1), n is an integer in the range of 5 to 100, preferably 5 to 80, and more preferably 10 to 60. If the value of n is greater than or equal to the lower limit, oil bleeding from the thermally conductive silicone composition is suppressed, and pumping-out resistance is improved. If the value of n is less than or equal to the upper limit, the wettability between the addition reaction product and the thermally conductive filler is sufficient, the increase in viscosity of the thermally conductive silicone composition is suppressed, and good application workability is obtained. Component (D) may be one of the hydrolyzable organopolysiloxanes alone or a combination of two or more.
[0057] The amount of hydrolyzable organopolysiloxane blended is preferably 1 to 10% by mass, and more preferably 3 to 6% by mass, relative to the total mass of the composition. Blending hydrolyzable organopolysiloxane within this range allows the thermally conductive silicone composition to be within an appropriate viscosity range and also provides superior resistance to pumping out.
[0058] Another aspect of the present invention provides a thermally conductive silicone composition comprising the following components (a) and (b), and components (B) to (D): (a) Having at least two aliphatic unsaturated hydrocarbon groups in one molecule, with a kinematic viscosity of 60 mm at 25°C. 2 (b) Organopolysiloxane having 1 / s or more (a) Organohydrogenpolysiloxane having 2 or more hydrogen atoms bonded to silicon atoms in one molecule: (a) an amount such that the ratio of the number of hydrogen atoms (SiH groups) bonded to silicon atoms to the total number of aliphatic unsaturated hydrocarbon groups in the component is 0.3 to 0.7 (B) Aluminum nitride particles having a 90% particle diameter of 18.0 μm or less by volume, a 50% particle diameter of 7.0 μm or more and 12.0 μm or less by volume, and a 440 mesh sieve residue of 0.1 mass% or less of the total particles: an amount that is 50 to 60 mass% of the total mass of the composition (C) Zinc oxide particles having a 50% particle diameter of 0.1 μm or more and 1.0 μm or less by volume: an amount that is 30 to 40 mass% of the total mass of the composition, (D) Organopolysiloxane represented by the following general formula (1): an amount of 1 to 10% by mass of the total mass of the composition (In the formula, R 1(1) is a monovalent hydrocarbon group having 1 to 18 carbon atoms, and at least one hydrogen atom bonded to the carbon atom of the monovalent hydrocarbon group may be substituted with a substituent, and n is an integer in the range of 5 to 100). Details of component (a), component (b), and components (B) to (D) are as described above. The amount of component (a) and component (b) in the above composition is such that the amount of the addition reaction product of component (a) and component (b) is 1 to 3% by mass of the total mass of the composition, more preferably 1.2 to 2.5% by mass, and most preferably 1.5 to 2% by mass. The above thermally conductive silicone composition may contain an optional platinum group metal catalyst and reaction regulator. Details and amounts of the platinum group metal catalyst and reaction regulator are as described above.
[0059] Other Components: In addition to the components described above, the thermally conductive silicone composition of the present invention may contain any additives. For example, to prevent degradation of the thermally conductive silicone composition, conventionally known antioxidants such as 2,6-di-tert-butyl-4-methylphenol may be included as needed. Furthermore, dyes, pigments, flame retardants, anti-settling agents, or thixotropic enhancers may be added as needed. The amount of additives should be adjusted appropriately within a range that does not impair the effects of the present invention. For example, it is preferable to have an amount of 0.01 to 1.0% by mass relative to the total mass of the composition.
[0060] Process for producing a thermally conductive silicone composition A method for producing a thermally conductive silicone composition is described in detail below. The method for producing a thermally conductive silicone composition is not particularly limited, but one example is to mix the above-mentioned components (a) and (b) and components (B) to (D), or components (A) to (D), and other components added as needed, using a mixer such as Trimix, Twinmix, Planetary Mixer (all registered trademarks of mixers manufactured by Inoue Seisakusho Co., Ltd.), Ultra Mixer (registered trademark of mixers manufactured by Mizuho Kogyo Co., Ltd.), Hibis Mix (registered trademark of mixers manufactured by Primix Co., Ltd.), etc.
[0061] The thermally conductive silicone composition may be mixed while heating. The heating conditions are not particularly limited, but the temperature is usually 25 to 220°C, preferably 40 to 200°C, and particularly preferably 50 to 200°C, and the time is usually 3 minutes to 24 hours, preferably 5 minutes to 12 hours, and particularly preferably 10 minutes to 6 hours. Degassing may also be performed during heating. The mixing conditions are not particularly limited, but it is preferable to heat and mix at 100 to 180°C using a Trimix or planetary mixer.
[0062] One method for producing the thermally conductive silicone composition of the present invention is to first hydrosilylate components (a) and (b) to prepare an addition product (A), and then mix the addition product (A) with components (B) to (D) to obtain a thermally conductive silicone composition. Alternatively, one method is to heat and mix a mixture obtained by mixing components (a) and (b) with components (B) to (D) to hydrosilylate components (a) and (b) to obtain a thermally conductive silicone composition containing the addition product (A). The addition products of components (a) and (b) are silicone gel crosslinks. In the latter method, the formation of crosslinks can be confirmed, for example, by the thickening of the reaction mixture.
[0063] The thermally conductive silicone composition of the present invention has a viscosity (also called absolute viscosity) measured at 25°C of 200 Pa·s or more and 600 Pa·s or less, preferably 250 Pa·s or more and 500 Pa·s or less. If the viscosity at 25°C is above the lower limit, the thermally conductive silicone composition can exhibit better resistance to pumping out. Furthermore, if it is below the upper limit, there is no risk of deterioration in the application workability of the thermally conductive silicone composition.
[0064] The thermally conductive silicone composition of the present invention can be compressed into a thin layer, thereby providing low thermal resistance. The thickness of the thermally conductive silicone composition when compressed is preferably 10 to 40 μm, and more preferably 10 to 35 μm. The thermally conductive silicone composition of the present invention preferably has a thermal conductivity of 4.0 to 7.0 W / m·K.
[0065] The thermally conductive silicone composition of the present invention achieves both excellent application workability and resistance to pumping out. Furthermore, the thermally conductive silicone composition achieves low thermal resistance when compressed into a thin layer. Therefore, it improves the reliability of the mounted electronic components. Another preferred embodiment of the present invention provides a non-curing type heat dissipation grease. The heat dissipation grease obtained from the thermally conductive silicone composition of the present invention has excellent application workability and resistance to pumping out by maintaining an appropriate viscosity. Preferably, the heat dissipation grease has a thermal conductivity of 4.0 to 7.0 W / m·K. In addition, the thermally conductive silicone composition of the present invention is easy to handle because it can be transported and stored at room temperature. Therefore, the thermally conductive silicone composition of the present invention is suitable for providing semiconductor packages having the composition.
[0066] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The methods for measuring the kinematic viscosity, particle size, oxygen content, and specific surface area of each component in the following examples and comparative examples are as follows: The kinematic viscosity is the value at 25°C measured with an Ostwald viscometer. The 50% particle size is the average value (median diameter) on a volume basis in particle size distribution measurement by laser diffraction. The 90% particle size is the particle size when the cumulative distribution on a volume basis in particle size distribution measurement by laser diffraction reaches 90%. The 440-mesh sieve residue is the mass percentage of particles that did not pass through the sieve and remained on the mesh when the particles were passed through a 440-mesh sieve. The oxygen content is the value measured using the Shimadzu EMGA-920 oxygen-nitrogen analyzer. The specific surface area is the value measured using the Microtrac-Bell BELSORP MAX G high-precision gas adsorption analyzer according to the BET method.
[0067] Furthermore, the measurement methods for each evaluation test in the examples and comparative examples are as follows: [Viscosity] The viscosity of each thermally conductive silicone composition was measured at 25°C using a spiral viscometer type PC-1T (Malcolm Corporation) (rotor A at 10 rpm, shear rate 6 [1 / s]).
[0068] [Thickness and Thermal Resistance] Each thermally conductive silicone composition was sandwiched between two 12.7 mm diameter aluminum plates and compressed at 25°C for 1 hour under a pressure of 0.14 MPa to prepare a test specimen for thermal resistance measurement. The thermal resistance of the cured thermally conductive silicone was measured using this test specimen. Furthermore, the thickness of the test specimen was measured using a coolant-proof micrometer MDC-25MX (manufactured by Mitutoyo Corporation), and the thickness of the cured thermally conductive silicone was calculated from the difference between this thickness and the thickness of the aluminum plates, which had been measured in advance. A thermal diffusivity measuring device, xenon flash analyzer LFA447 Nanoflash (manufactured by NETZSCH), was used for the thermal resistance measurement.
[0069] [Pumping-out Resistance] 0.1 ml of each thermally conductive silicone composition was sandwiched between a nickel-plated copper plate and a glass plate with a 0.1 mm spacer in between, and compressed for 15 minutes using two 1.8 kgf (17.65 N) clips. This was then placed vertically in a thermal shock tester that repeatedly cycled between -40°C / 30 min and 125°C / 30 min, and removed after 1,000 cycles. The vertical displacement immediately after removal was measured. The thermal history described above causes the thermally conductive silicone composition to repeatedly expand and contract. The less likely the silicone composition is to flow out vertically downward due to expansion and contraction, i.e., the smaller the vertical displacement, the better the pumping-out resistance is considered to be.
[0070] [Preparation of Thermally Conductive Silicone Composition] The components used in the examples and comparative examples are as follows: (A) Component (a-1): Both ends are sealed with dimethylvinylsilyl groups, with a kinematic viscosity of 600 mm at 25°C. 2 Dimethylpolysiloxane having / s (vinyl group amount = 0.00014 mol / g) (b-1): Represented by the following formula (2), with a kinematic viscosity of 100 mm at 25°C 2 Methylhydrogendimethylpolysiloxane (SiH content = 0.0055 mol / g) containing / s (In formula (2) above, the order of the siloxane units in parentheses is not limited to the above; it may be random or have a block structure.)
[0071] (B) Component Aluminum nitride particles having the particle size distribution shown in Table 1 below
[0072] (C) Components C-1: Zinc oxide particles with a particle diameter of 0.3 μm, representing 50% of the volume C-2 (for comparison): Zinc oxide particles with a particle diameter of 0.08 μm, representing 50% of the volume C-3 (for comparison): Zinc oxide particles with a particle diameter of 5 μm, representing 50% of the volume
[0073] (D) Component D-1: Represented by the following formula (3), with a kinematic viscosity of 30 mm at 25°C. 2 / s organopolysiloxane
[0074] Other components (E) Platinum group metal catalyst: A solution obtained by dissolving a platinum-divinyltetramethyldisiloxane complex in the above (a-1) dimethylpolysiloxane (platinum atom content: 1% by mass as platinum atoms)
[0075] (F) Reaction control agent: Ethinylcyclohexanol represented by the following formula (4)
[0076] [Examples 1-5, Comparative Examples 1-6] Preparation of Thermally Conductive Silicone Compositions A thermally conductive silicone composition was prepared by combining components (a-1), (b-1), and (B) to (F) in the amounts shown in Tables 2-3 below, using the method described below. Components (a-1), (B), (C), and (D) were added to a vertical kneading and stirring machine (Trimix, manufactured by Inoue Seisakusho Co., Ltd.) with a capacity of 5 liters in the amounts shown in Tables 2-3 below, and mixed under reduced pressure at 170°C for 1 hour. The mixture was cooled to below 40°C, and then component (b-1) in an amount that resulted in the SiH / Vi (number ratio) shown below, and (E) platinum group metal catalyst and (F) reaction control agent in the amounts shown in Tables 2-3 below were added to this mixture. The mixture was mixed at 150°C for 2 hours to prepare a thermally conductive silicone composition. The viscosity of the reaction mixture increased before and after heating and mixing at 150°C for 2 hours. This confirmed that component (a-1) and component (b-1) reacted to form an addition product. Therefore, the obtained product is a thermally conductive silicone composition containing the addition product of component (a-1) and component (b-1). For each thermally conductive silicone composition obtained by this method, the viscosity, thickness, and thermal resistance were measured according to the method described above, and the pumping-out resistance was evaluated. The results are shown in Tables 2 and 3.
[0077] In the examples and comparative examples, the amounts of component (a-1) and component (b-1) were blended in such an amount that the blending ratio of component (a-1) and component (b-1) was as shown below, and the amount of the resulting addition product in parts by mass was as shown in Table 2 or 3. A-1: Ratio of the number of SiH groups in component (b-1) to the total number of vinyl groups in component (a-1) = 0.5 A-2: Ratio of the number of SiH groups in component (b-1) to the total number of vinyl groups in component (a-1) = 0.6 A-3 (Comparative Example): Ratio of the number of SiH groups in component (b-1) to the total number of vinyl groups in component (a-1) = 0.8 A-4 (Comparative Example): Ratio of the number of SiH groups in component (b-1) to the total number of vinyl groups in component (a-1) = 0.2
[0078]
[0079]
[0080] As shown in Table 3, the thermally conductive silicone composition of Comparative Example 1 has high viscosity. The thermally conductive silicone composition of Comparative Example 2 has a large vertical displacement distance, which is an indicator of pumping-out resistance. The thermally conductive silicone compositions of Comparative Examples 3 and 4, which use aluminum nitride particles that do not have the particle size distribution specified in the present invention, cannot be compressed thinly and low thermal resistance cannot be obtained. The thermally conductive silicone composition of Comparative Example 5, which uses zinc oxide particles with too small a median diameter, cannot be obtained as a paste-like composition. The thermally conductive silicone composition of Comparative Example 6, which uses zinc oxide particles with too large a median diameter, also cannot be compressed thinly and low thermal resistance cannot be obtained. In contrast, as shown in Table 2, the thermally conductive silicone compositions of Examples 1 to 5 have appropriate viscosity, resulting in excellent application workability and low thermal resistance when compressed thinly. Furthermore, the above thermally conductive silicone compositions have a small vertical displacement distance, which is an indicator of pumping-out resistance, and are less prone to silicone composition flow due to expansion and contraction caused by thermal history.
[0081] As described above, the thermally conductive silicone composition of the present invention has an appropriate viscosity despite containing a large amount of thermally conductive filler, and can achieve good pumping-out resistance, making it useful as a non-curing type heat dissipation grease. Furthermore, the thermally conductive silicone composition of the present invention is useful for addressing the increasing heat generation, size, and structural complexity of semiconductor devices in recent years.
[0082] It should be noted that the present invention is not limited to the embodiments described above. The embodiments described above are illustrative, and any configuration that is substantially identical to the technical idea described in the claims of the present invention and achieves similar effects is included within the technical scope of the present invention.
Claims
1. A thermally conductive silicone composition comprising the following components (A) to (D), having a viscosity of 200 Pa·s to 600 Pa·s at 25°C: (A) Addition reaction product of component (a) and component (b): in an amount of 1 to 3% by mass relative to the total mass of the composition (a) Having at least two aliphatic unsaturated hydrocarbon groups in one molecule, with a kinematic viscosity of 60 mm at 25°C 2 (b) Organopolysiloxane having 1 / s or more (a) Organohydrogenpolysiloxane having 2 or more hydrogen atoms bonded to silicon atoms in one molecule: (a) an amount such that the ratio of the number of hydrogen atoms (SiH groups) bonded to silicon atoms to the total number of aliphatic unsaturated hydrocarbon groups in the component is 0.3 to 0.7 (B) Aluminum nitride particles having a 90% particle diameter of 18.0 μm or less by volume, a 50% particle diameter of 7.0 μm or more and 12.0 μm or less by volume, and a 440 mesh sieve residue of 0.1 mass% or less of the total particles: an amount that is 50 to 60 mass% of the total mass of the composition (C) Zinc oxide particles having a 50% particle diameter of 0.1 μm or more and 1.0 μm or less by volume: an amount that is 30 to 40 mass% of the total mass of the composition, (D) Organopolysiloxane represented by the following general formula (1): an amount of 1 to 10% by mass of the total mass of the composition (In the formula, R 1 (These are, independently of each other, monovalent hydrocarbon groups having 1 to 18 carbon atoms, and at least one hydrogen atom bonded to the carbon atom of the monovalent hydrocarbon group may be substituted with a substituent, and n is an integer in the range of 5 to 100).
2. The thermally conductive silicone composition according to claim 1, wherein n in the general formula (1) of the (D) organopolysiloxane is an integer in the range of 10 to 60.
3. The thermally conductive silicone composition according to claim 1, wherein the oxygen content of the (B) aluminum nitride particles is 0.25% by mass or less.
4. The specific surface area of the aluminum nitride particles (B) is 0.20 m². 2 / g or more 0.60m 2 The thermally conductive silicone composition according to claim 1, wherein the amount is less than or equal to / g.
5. A heat dissipation grease comprising the thermally conductive silicone composition according to any one of claims 1 to 4.