Method for producing polycarbonate resin particles

A batch process using solvent extraction with a specific solubility parameter effectively removes impurities from polycarbonate resin, addressing inefficiencies in existing methods and producing high-quality resin particles for industrial use.

WO2026239890A1PCT designated stage Publication Date: 2026-11-19TEIJIN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016339
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-04-23
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for purifying polycarbonate resin, particularly recycled polycarbonate, are inefficient in removing oligomers, additives, and impurities due to the need for large equipment and frequent cleaning, making them unsuitable for industrial use with varied raw materials.

Method used

A batch process involving repeated solvent extraction with an organic solvent having a solubility parameter of 16 to 30 MPa, followed by filtration and optional washing, effectively removes oligomers and low molecular weight components in a short time, producing high-quality polycarbonate resin particles.

Benefits of technology

The method efficiently produces high-quality polycarbonate resin particles with low oligomer and low molecular weight content, maintaining mechanical properties and impact strength, suitable for industrial-scale recycling and virgin polycarbonate production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

This method for producing polycarbonate resin particles is characterized by repeating steps (A) and (B) at least twice or more in this order. The obtained recycled polycarbonate resin particles from which oligomers, additives, deteriorated substances, impurities and the like are removed is characterized by having excellent mechanical strength. (A) A step for adding an organic solvent having a solubility parameter of 16 to 30 MPa0.5 to polycarbonate resin particles by 3 to 20 times by weight and bringing the polycarbonate resin particles into contact with the organic solvent under stirring; and (B) a step for filtering and removing a part or all of the organic solvent from the mixture of the polycarbonate resin particles and the organic solvent obtained in the step (A) to obtain polycarbonate resin particles.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing polycarbonate resin particles

[0001] This invention relates to a method for producing polycarbonate resin particles by removing oligomers, additives, degradation products, impurities, etc., from polycarbonate resin particles to obtain purified polycarbonate resin particles.

[0002] Plastic materials are used in a wide range of applications, taking advantage of their characteristics such as impact resistance, lightness, and processability. In most current industrial manufacturing methods, plastic materials are not produced as substances with a single molecular weight, but as mixtures with a molecular weight distribution. Of these, low molecular weight components degrade the physical properties of the plastic material, so it is desirable to have a low content. In addition, various additives are added to plastic materials to improve weather resistance, flame retardancy, and design properties, but these additives and their modified products are often low molecular weight components as well, and can impair physical properties, so the amount added is appropriately controlled when using them.

[0003] In recent years, due to concerns about resource depletion and growing environmental awareness, recycling—the collection and remolding of used plastic materials—has become widespread. Polycarbonate refining technology is crucial not only for virgin polycarbonate but also for recycled polycarbonate.

[0004] Poor solvent extraction is a method for removing low molecular weight components and impurities from polycarbonate. Patent documents 1 and 2 propose that acetone extraction is an excellent method that can significantly reduce residual halogenated solvents, monomers, oligomers, etc. Both are batch-type apparatuses in which polycarbonate powder and acetone are placed in a container, stirred, and then the solid and liquid are separated. Patent document 3 proposes a counter-flow continuous counter-flow method using acetone. However, this method requires large tower equipment for industrial use, and since it is based on continuous production, the equipment must be cleaned each time when handling various types of raw materials. Therefore, it presents challenges for industrial adoption, especially in the purification of recycled polycarbonate with a wide variety of raw materials and additives.

[0005] JP-A-63-278929 JP-A-64-6020 JP-A-4-306227

[0006] The object of the present invention is to provide purified polycarbonate resin particles by removing oligomers, additives, degradation products, impurities, etc.

[0007] The inventors of this invention conducted extensive research to achieve this objective and, as a result, discovered that oligomers and low molecular weight components can be efficiently removed in a short time from polycarbonate resin compositions by repeatedly renewing a specific organic solvent in a batch process. This led to the completion of the present invention. In other words, the present invention is as follows.

[0008] 1. A method for producing polycarbonate resin particles, characterized by repeating the following steps (A) and (B) at least twice in this order: (A) A solubility parameter of 16 to 30 MPa, which is 3 to 20 times the weight of the polycarbonate resin particles. 0.5 (B) A step of adding an organic solvent and bringing the polycarbonate resin particles into contact with the organic solvent under stirring. (A) A step of filtering out some or all of the organic solvent from the mixture of polycarbonate resin particles and organic solvent obtained in step (A) to obtain polycarbonate resin particles. 2. Solubility parameter 16-30 MPa 0.5 A method for producing polycarbonate resin particles as described in item 1 above, wherein the organic solvent is acetone. 3. A method for producing polycarbonate resin particles as described in item 1 or 2 above, wherein in step (A), the contact time per step is 5 minutes or more and 60 minutes or less. 4. A method for producing polycarbonate resin particles as described in any of items 1 to 3 above, wherein in step (A), the total contact time with the organic solvent is 20 minutes or more and 360 minutes or less. 5. A solubility parameter used in step (A) is 16 to 30 MPa. 0.5The method for producing polycarbonate resin particles according to any one of paragraphs 1 to 4 above, wherein the organic solvent is recycled from the organic solvent recovered from the (B) process. 6. The method for producing polycarbonate resin particles according to any one of paragraphs 1 to 5 above, wherein the polycarbonate resin particles are recycled polycarbonate resin particles. 7. In the (A) process, the polycarbonate resin particles and the solubility parameter 16 to 30 MPa 0.5 A method for producing polycarbonate resin particles according to any one of paragraphs 1 to 6 above, comprising: dissolving polycarbonate resin particles in a good solvent before and / or after contact with an organic solvent; and subjecting the polycarbonate resin solution to one or more of the following treatments: water washing, acid washing, and alkaline washing.

[0009] The present invention provides a method for producing polycarbonate resin particles that, despite being a batch process, can remove oligomers and low molecular weight components in a short time, thereby obtaining high-quality polycarbonate resin particles. Therefore, its industrial benefits are extremely significant.

[0010] The present invention will now be described in detail. The present invention is a method for producing polycarbonate resin particles, characterized by repeating the following steps (A) and (B) at least twice in this order. (A) A solubility parameter of 16 to 30 MPa, which is 3 to 20 times the weight of the polycarbonate resin particles. 0.5 (B) A step of adding an organic solvent and bringing the polycarbonate resin particles into contact with the organic solvent under stirring. (B) A step of filtering out some or all of the organic solvent from the mixture of polycarbonate resin particles and organic solvent obtained in step (A) to obtain polycarbonate resin particles.

[0011] <Regarding step (A): Solvent extraction> In the method for producing polycarbonate resin particles of the present invention, solvent extraction is performed with the aim of removing impurities such as monomers, oligomers, additives, and modified products thereof from the polycarbonate resin (raw material), which is the raw material, which is low molecular weight components. Solvent extraction involves eluting monomers, oligomers, additives, and modified products thereof present in the polycarbonate resin (raw material) into an organic solvent.

[0012] The organic solvent used in the solvent extraction of the present invention has a solubility parameter of 16 to 30 MPa 0.5 It is preferable to use an organic solvent of 17 to 25 MPa 0.5 is more preferable, and 18 to 22 MPa 0.5 is even more preferable. Within the above range, monomers, oligomers, additives, and modified products thereof present in the polycarbonate resin (raw material) can be efficiently extracted.

[0013] Solubility Parameter (sometimes referred to as δ or SP value. The unit is (MPa 0.5 )] is a value defined by the regular solution theory introduced by Hildebrand, and is determined from the molar heat of vaporization and molar volume of the compound.

[0014] The amount of the organic solvent used is 3 to 20 times by weight, preferably 3 to 10 times, more preferably 4 to 5 times relative to the polycarbonate resin particles. Within the above range, monomers, oligomers, additives, and modified products thereof present in the polycarbonate resin (raw material) can be efficiently extracted. If the amount of the organic solvent used is less than the lower limit, the extraction efficiency will deteriorate, and in addition, poor stirring may occur. If the amount of the organic solvent used exceeds the upper limit, the amount of the organic solvent will be too large, which may be industrially inefficient.

[0015] The solubility parameter is 16 to 30 (MPa 0.5As organic solvents, non-halogenated organic solvents such as acetone, ethyl lactate, methyl ethyl ketone, methyl n-butyl ketone, methyl isobutyl ketone, and diethyl ketone (compounds having a carbonyl group), compounds having an acetyl group such as methyl acetate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, and vinyl acetate, alkyl ethers such as diethyl ether and dibutyl ether, alcohols such as methanol, ethanol, isopropyl alcohol, 1-propanol, 1-butanol, and methoxypropanol, and aromatic hydrocarbons such as ethylbenzene, paraxylene, and mesitylene are preferred. Among these, acetone is more preferred because it can efficiently extract monomers, oligomers, additives, and their modified products, has a low boiling point, and is easy to separate and recover by distillation. Furthermore, two or more of these organic solvents can be used in combination as needed.

[0016] The organic solvent used in solvent extraction in this invention can be a virgin organic solvent or an organic solvent that has been distilled and purified after being used in extraction once. It can also be reused repeatedly without distillation and purification. For example, in the repetition of steps (A) and (B) described later, the organic solvent used in the nth or later repetitions can be used in the solvent extraction in the n-1th or earlier stages. When using a virgin organic solvent in solvent extraction in this invention, it is preferable that the purity be 95% or higher. If the purity is below the lower limit, the extraction efficiency may be poor.

[0017] (A) In step (A), the temperature at which the polycarbonate resin particles come into contact with the organic solvent greatly affects the extraction efficiency. Typically, the temperature should be below the boiling point of the organic solvent used, preferably 10 to 100°C, more preferably 30 to 80°C. When acetone is used as the organic solvent, the temperature should preferably be 10 to 55°C, more preferably 30 to 50°C. It is also preferable to equip the extraction apparatus with a jacket or a heating mechanism.

[0018] <Regarding step (B); filtration treatment> In the method for producing polycarbonate resin particles of the present invention, a step is performed to obtain polycarbonate resin particles by filtering out some or all of the organic solvent from the mixture of polycarbonate resin particles and organic solvent obtained in step (A) described above.

[0019] In step (B), where the organic solvent is filtered out, some or all of the organic solvent is removed. Specifically, it is preferable to remove 30% or more by weight, 40% or more by weight, 50% or more by weight, 60% or more by weight, 70% or more by weight, 80% or more by weight, 90% or more by weight, or 95% or more by weight of the organic solvent, and it is particularly preferable to remove substantially 100% by weight. If some of the organic solvent is removed, virgin organic solvent can be added and further extraction treatment can be performed. The separated organic solvent can be reused as is as the organic solvent in step (A), or it can be industrially distilled to remove elutes and then reused repeatedly.

[0020] Furthermore, it is also preferable to dry the polycarbonate resin particles after filtering out the organic solvent. The drying temperature is preferably 80 to 140°C. The dryer may be a conduction heating type or a hot air drying type, and the polycarbonate resin particles may be left to stand, transported, or stirred. Among these, a grooved or cylindrical dryer in which the polycarbonate resin particles are stirred by the conduction heating type is preferred, and a grooved dryer is particularly preferred.

[0021] <Regarding the repetition of steps (A) and (B)> In the present invention, it is necessary to repeat steps (A) and (B) in this order at least two times. The number of repetitions is preferably 2 to 12 times, more preferably 2 to 5 times, and even more preferably 2 to 3 times from an industrial cost standpoint.

[0022] (A) In step (A), the solvent extraction time per step is preferably 5 minutes or more and 60 minutes or less, more preferably 10 minutes or more and 60 minutes or less, and even more preferably 30 minutes or more and 60 minutes or less. If the solvent extraction time per step is less than the lower limit, the organic solvent may not penetrate the polycarbonate resin sufficiently, and extraction may not be performed sufficiently. On the other hand, if the extraction time per step exceeds the upper limit, the extraction efficiency may be greatly reduced due to the presence of many low molecular weight components such as monomers, oligomers, additives, and modified products thereof in the organic solvent.

[0023] In step (A), the total contact time with the organic solvent in the repeated steps is preferably 20 minutes to 6 hours, more preferably 30 minutes to 3 hours, and even more preferably 30 minutes to 2 hours. Within this range, monomers, oligomers, additives, and their modified products can be efficiently extracted. If the extraction time is too long, fine polycarbonate powder is more likely to be generated, which may reduce the solid-liquid separation efficiency. Furthermore, as mentioned above, it is preferable to reuse the organic solvent recovered from step (B) as the organic solvent in step (A).

[0024] <Regarding other processes> In the present invention, the polycarbonate resin particles in step (A) and the solubility parameter 16 to 30 MPa 0.5 It is also preferable to dissolve the polycarbonate resin particles in a good solvent before and / or after contact with the organic solvent, and then treat the polycarbonate resin solution with one or more of the following: water washing, acid washing, and alkaline washing.

[0025] As a suitable solvent, any solvent that is inert to various reactions, such as those used in the production of known polycarbonates, can be used alone or in a mixture. Typical examples include hydrocarbon solvents such as xylene, and halogenated hydrocarbon solvents such as methylene chloride and chlorobenzene. Halogenated hydrocarbon solvents such as methylene chloride are particularly preferred.

[0026] By filtering a solution obtained by dissolving polycarbonate resin particles in a suitable solvent, foreign matter in the polycarbonate resin particles can be reduced during the dissolution filtration process. Alternatively, the polycarbonate resin solution obtained by dissolving polycarbonate resin particles in a suitable solvent may be subjected to one or more of the following treatments: water washing, acid washing, and alkaline washing, after which the suitable solvent is removed to obtain polycarbonate resin particles. Washing treatment can remove salts and other substances, thereby improving the heat resistance of the resulting polycarbonate resin during molding.

[0027] <Polycarbonate Resin Particles> The number average molecular weight (Mn) of the polycarbonate resin particles produced in this invention, as measured by GPC, is preferably greater than 18,000, and more preferably 19,000 or greater. There is no particular upper limit, but 33,000 or less is preferred. If the number average molecular weight is below the above lower limit, the mechanical properties will deteriorate, which is undesirable. Also, if the number average molecular weight exceeds the above upper limit, the fluidity tends to be insufficient, which is undesirable.

[0028] The Mw / Mn of the polycarbonate resin particles manufactured according to the present invention, as measured by GPC, is preferably 2.4 or less, more preferably 2.3 or less, and even more preferably 2.2 or less. If the Mw / Mn is below the above lower limit, the mechanical properties tend to deteriorate, which is undesirable. There are no particular restrictions on the lower limit of Mw / Mn, and it can be arbitrarily set to 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, etc. The lower limit of Mw / Mn may be appropriately selected considering manufacturing efficiency, etc.

[0029] The oligomer component of the polycarbonate resin particles produced in this invention is preferably 0.40% or less, more preferably 0.30% or less, and even more preferably 0.28% or less. If the oligomer component exceeds the above upper limit, the mechanical properties tend to deteriorate, which is undesirable.

[0030] The low molecular weight component of the polycarbonate resin particles produced in this invention is preferably 0.30% or less, more preferably 0.27% or less, even more preferably 0.25% or less, and most preferably 0.20% or less. The polycarbonate resin (raw material) used in this invention contains various additives as low molecular weight components, and also contains modified products in which these additives have deteriorated. When the low molecular weight component exceeds the above upper limit, the mechanical properties, color tone, and weather resistance tend to deteriorate.

[0031] The Charpy impact strength (kJ / m²) of the polycarbonate resin particles produced by the present invention. 2 ) is preferably 13 or higher, and more preferably 14 or higher. If the Charpy impact strength is below the above lower limit, there is a high possibility that the inherent properties of the polycarbonate will not be exhibited.

[0032] <Polycarbonate Resin Particles (Raw Material)> The polycarbonate resin (raw material) used in this invention includes injection-molded products containing polycarbonate resin or pulverized sprues or runners generated during injection molding, extruded products such as films and sheets or pulverized scraps generated during extrusion molding, and pellets or powders produced from these pulverized materials using an extruder. Many of these materials are amorphous and may instantly fuse together when in contact with organic solvents.

[0033] To ensure a sufficient contact area with organic solvents and to prevent fusion, the polycarbonate resin (raw material) used in this invention is in granular form, with an average major diameter of 200 to 5000 μm, more preferably 250 to 4500 μm, and an average particle size of 0.1 to 5 mm, more preferably 0.15 to 4 mm, and even more preferably 0.2 to 3 mm. The polycarbonate resin (raw material) having the above average major diameter and average particle size may be produced by known methods including mechanical pulverization and wet processes, or a commercially available product may be used.

[0034] In mechanical pulverization, for example, polycarbonate resin (raw material) is mechanically pulverized to produce particles having the desired average major diameter and average particle size. According to mechanical pulverization, for example, particles containing polycarbonate resin (raw material) can be produced by the following method.

[0035] Polycarbonate resin (raw material) may be crushed after freezing, or it may be crushed at room temperature. Mechanical crushing can be carried out using known apparatus for crushing polycarbonate resin (raw material). Examples of such apparatus include compression crushers (roll crushers, etc.), impact crushers (impact crushers, hammer mills, etc.), cutting or shearing crushers (cutter mills, reciprocating crushers, low-speed rotary crushers (twin-shaft shearing crushers, etc.), etc.), impact shearing crushers (shredders, etc.), and various fine crushers (ball mills, disc mills, pin mills, hammer mills, turbo mills, jet mills, etc.). Among the above, cutting or shearing crushers are preferred because they can directly supply molded products, have excellent crushing efficiency, and can accommodate the required particle size. Among these, low-speed rotary crushers are preferred because they have an appropriate bulk density even for exterior molded products with high toughness, making it easier to obtain desirable crushed material. Any type of low-speed rotary crusher, such as single-shaft, twin-shaft, or tri-shaft, can be used. In mechanical pulverization, frictional heat generated from the polycarbonate resin (raw material) during pulverization can cause the polycarbonate resin (raw material) particles to fuse together, potentially resulting in particles with the desired average major diameter and average particle size. Therefore, the thermoplastic resin may be cooled and brittle using liquid nitrogen or the like before pulverization.

[0036] According to the mechanical grinding method, the average major diameter, average particle size, and average particle diameter of the produced particles can be adjusted to a desired range by appropriately adjusting the amount of solvent relative to the polycarbonate resin (raw material), or the grinding method or speed.

[0037] In the wet process, for example, a dispersion of polycarbonate resin (raw material) using a surfactant is dried to obtain particles having the desired average major axis, average particle size, and average particle diameter. According to the wet process, for example, particles containing polycarbonate resin can be produced by the following method.

[0038] <Polycarbonate Resin (Raw Material)> As the polycarbonate resin (raw material), those obtained by reacting a dihydric phenol with a carbonate precursor are preferred. Examples of the reaction method include an interfacial polymerization method, a melt transesterification method, a solid-phase transesterification method of a carbonate prepolymer, and a ring-opening polymerization method of a cyclic carbonate compound.

[0039] Representative examples of the dihydric phenol used herein include hydroquinone, resorcinol, 4,4'-biphenol, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 2,2-bis(4-hydroxyphenyl)pentane, 4,4'-(p-phenylenediisopropylidene)diphenol, 4,4'-(m-phenylenediisopropylidene)diphenol, 1,1-bis(4-hydroxyphenyl)-4-isopropylcyclohexane, bis(4-hydroxyphenyl) oxide, bis(4-hydroxyphenyl) sulfide, bis(4-hydroxyphenyl) sulfoxide, bis(4-hydroxyphenyl) sulfone, bis(4-hydroxyphenyl) ketone, bis(4-hydroxyphenyl) ester, bis(4-hydroxy-3-methylphenyl) sulfide, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene. A preferred dihydric phenol is a bis(4-hydroxyphenyl)alkane, and among them, bisphenol A is particularly preferred from the viewpoint of impact resistance and is widely used.

[0040] The polycarbonate resin used in this invention may also be recycled polycarbonate resin (raw material). This refers to injection-molded products containing polycarbonate resin or crushed sprue or runner generated during injection molding, extruded products such as films and sheets or crushed scraps generated during extrusion molding, and pellets produced from these crushed materials using an extruder. Post-consumer recycled (PCR) material, post-industrial recycled (PIR) material, or a combination thereof may be used. In this case, there are no particular restrictions on the method of recovering the recycled polycarbonate resin (raw material). Generally, for example, it is possible to use flakes obtained by removing (separating) different resins and other dissimilar materials from recovered products collected by specialized companies such as waste collection companies and recycling companies, crushing, washing, and drying them, or by re-pelletizing them using an extruder.

[0041] <Components other than polycarbonate resin in polycarbonate resin (raw material)> In the present invention, polycarbonate resin (raw material) containing known functional agents such as mold release agents, heat stabilizers, ultraviolet absorbers, flow modifiers, and antistatic agents can be used as components other than polycarbonate resin in the polycarbonate resin (raw material). The main additives that do not pose a problem even if they are included in the polycarbonate resin used as a raw material are listed below.

[0042] (i) Release Agent As the polycarbonate resin (raw material) used in the present invention, those combined with a release agent can also be used within a range that does not impair the effects of the present invention. Examples of the release agent include fatty acid esters, polyolefin waxes (such as polyethylene wax and 1-alkene polymers, and those modified with functional group-containing compounds such as acid-modified compounds can also be used), fluorine compounds (such as fluorine oil typified by polyfluoroalkyl ethers), paraffin wax, and beeswax. Among these, fatty acid esters are preferred from the viewpoints of availability, releasability, and transparency. The release agent is preferably contained in an amount of 0.005 to 0.5 parts by weight, more preferably 0.007 to 0.4 parts by weight, and still more preferably 0.01 to 0.3 parts by weight, relative to 100 parts by weight of the polycarbonate resin (raw material). This is because when the content is at or above the lower limit of the above range, the effect of improving releasability is clearly exhibited, and when it is at or below the upper limit, adverse effects such as mold contamination during molding are reduced.

[0043] Among the above, the fatty acid ester used as a preferred release agent will be described in further detail. Such a fatty acid ester is an ester of an aliphatic alcohol and an aliphatic carboxylic acid. The aliphatic alcohol may be a monohydric alcohol or a dihydric or higher polyhydric alcohol. The number of carbon atoms in the alcohol is preferably in the range of 3 to 32, more preferably in the range of 5 to 30. Examples of such monohydric alcohols include dodecanol, tetradecanol, hexadecanol, octadecanol, eicosanol, tetracosanol, ceryl alcohol, and triacontanol. Examples of such polyhydric alcohols include pentaerythritol, dipentaerythritol, tripentaerythritol, polyglycerol (triglycerol to hexaglycerol), ditrimethylolpropane, xylitol, sorbitol, and mannitol. In fatty acid esters, polyhydric alcohols are more preferably used.

[0044] On the other hand, aliphatic carboxylic acids preferably have 3 to 32 carbon atoms, and aliphatic carboxylic acids with 10 to 22 carbon atoms are particularly preferred. Examples of such aliphatic carboxylic acids include saturated aliphatic carboxylic acids such as decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, hexadecanoic acid (palmitic acid), heptadecanoic acid, octadecanoic acid (stearic acid), nonadecanoic acid, eicosanic acid, and docosanic acid (behenic acid), as well as unsaturated aliphatic carboxylic acids such as palmitoleic acid, oleic acid, linoleic acid, linolenic acid, eicosenoic acid, eicosapentaenoic acid, and cetoleic acid. Among the above, aliphatic carboxylic acids with 14 to 20 carbon atoms are preferred. Saturated aliphatic carboxylic acids are particularly preferred. Since such aliphatic carboxylic acids are usually produced from natural oils and fats such as animal fats (beef tallow and lard, etc.) and vegetable oils (palm oil, etc.), these aliphatic carboxylic acids are usually mixtures containing other carboxylic acid components with different numbers of carbon atoms. Therefore, the production of aliphatic carboxylic acids also consists of mixtures produced from such natural oils and fats containing other carboxylic acid components. For fatty acid esters, an acid value of 20 or less (which can be substantially 0) is preferably used. However, in the case of full esters, it is preferable to contain at least some free fatty acids to improve release properties, and in this respect, an acid value in the range of 3 to 15 is preferably used for full esters. Furthermore, an iodine value of fatty acid esters is preferably 10 or less (which can be substantially 0). These properties can be determined by the method specified in JIS K0070.

[0045] The aforementioned fatty acid esters may be either partial esters or full esters, but partial esters are preferred in terms of better mold release properties and durability, and glycerin monoesters are particularly preferred. Glycerin monoesters mainly consist of glycerin and a fatty acid monoester. Suitable fatty acids include saturated fatty acids such as stearic acid, palmitic acid, behenic acid, arachidic acid, montanic acid, and lauric acid, and unsaturated fatty acids such as oleic acid, linoleic acid, and sorbic acid. Glycerin monoesters mainly composed of stearic acid, behenic acid, and palmitic acid are particularly preferred. These fatty acids are synthesized from natural fatty acids and, as described above, are mixtures. Even in such cases, it is preferable to use glycerin monoesters in the fatty acid ester that account for 60% by weight or more.

[0046] Furthermore, partial esters are often inferior to full esters in terms of thermal stability. To improve the thermal stability of such partial esters, partial esters with a sodium metal content of preferably less than 20 ppm, more preferably less than 5 ppm, and even more preferably less than 1 ppm are used. Fatty acid partial esters with a sodium metal content of less than 1 ppm can be produced by producing fatty acid partial esters by conventional methods and then purifying them by molecular distillation or the like.

[0047] Specifically, one method involves removing gaseous and low-boiling-point substances using a spray nozzle degassing apparatus, then removing polyhydric alcohols such as glycerin using a drip-film distillation apparatus at a distillation temperature of 120-150°C and a vacuum of 0.01-0.03 kPa, and finally obtaining high-purity fatty acid partial esters as distillates using a centrifugal molecular distillation apparatus at a distillation temperature of 160-230°C and a vacuum of 0.01-0.2 Torr. Sodium metal can be removed as a distillation residue. By repeatedly performing molecular distillation on the obtained distillates, the purity can be further increased, and fatty acid partial esters with even lower sodium metal content can be obtained. It is also important to prevent contamination from the external environment by thoroughly cleaning the inside of the molecular distillation apparatus using appropriate methods beforehand and by improving airtightness. Such fatty acid esters are available from specialized suppliers (e.g., Riken Vitamin Co., Ltd.).

[0048] (ii) Phosphorus-based stabilizers The polycarbonate resin (raw material) used in the present invention may also contain various phosphorus-based stabilizers, primarily for the purpose of improving its thermal stability during molding. Examples of such phosphorus-based stabilizers include phosphorous acid, phosphoric acid, phosphonic acid, phosphonic acid, and esters thereof. Furthermore, such phosphorus-based stabilizers may include tertiary phosphines.

[0049] Specifically, examples of phosphite compounds include triphenyl phosphite, tris(nonylphenyl) phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, tris(diethylphenyl) phosphite, tris(di-iso-propylphenyl) phosphite, and tris(di-n-butylphenyl) phosphite. Examples include tris(2,4-di-tert-butylphenyl) phosphite, tris(2,6-di-tert-butylphenyl) phosphite, distearyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl) pentaerythritol diphosphite, phenylbisphenol A pentaerythritol diphosphite, bis(nonylphenyl) pentaerythritol diphosphite, and dicyclohexyl pentaerythritol diphosphite.

[0050] Furthermore, other phosphite compounds that react with divalent phenols to form a cyclic structure may also be used. Examples include 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2,4-di-tert-butylphenyl) phosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl)(2-tert-butyl-4-methylphenyl) phosphite, 2,2'-methylenebis(4-methyl-6-tert-butylphenyl)(2-tert-butyl-4-methylphenyl) phosphite, and 2,2'-ethylidenebis(4-methyl-6-tert-butylphenyl)(2-tert-butyl-4-methylphenyl) phosphite.

[0051] Examples of phosphate compounds include tributyl phosphate, trimethyl phosphate, tricresyl phosphate, triphenyl phosphate, trichlorophenyl phosphate, triethyl phosphate, diphenylcresyl phosphate, diphenylmonoorthoxenyl phosphate, tributoxyethyl phosphate, dibutyl phosphate, dioctyl phosphate, and diisopropyl phosphate, with triphenyl phosphate and trimethyl phosphate being preferred.

[0052] Phosphonite compounds include tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylenediphosphonite, tetrakis(2,4-di-tert-butylphenyl)-4,3'-biphenylenediphosphonite, tetrakis(2,4-di-tert-butylphenyl)-3,3'-biphenylenediphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,4'-biphenylenediphosphonite, tetrakis(2,6-di-tert-butylphenyl)-4,3'-biphenylenediphosphonite, tetrakis(2,6-di-tert-butylphenyl)-3,3'-biphenylenediphosphonite, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenylphosphonite, bis Examples include (2,4-di-tert-butylphenyl)-3-phenyl-phenylphosphonite, bis(2,6-di-n-butylphenyl)-3-phenyl-phenylphosphonite, bis(2,6-di-tert-butylphenyl)-4-phenyl-phenylphosphonite, and bis(2,6-di-tert-butylphenyl)-3-phenyl-phenylphosphonite, with tetrakis(di-tert-butylphenyl)-biphenylenediphosphonite and bis(di-tert-butylphenyl)-phenyl-phenylphosphonite being preferred, and tetrakis(2,4-di-tert-butylphenyl)-biphenylenediphosphonite and bis(2,4-di-tert-butylphenyl)-phenyl-phenylphosphonite being more preferred. Such phosphonite compounds can be used in combination with phosphite compounds having aryl groups substituted with two or more alkyl groups, and this is preferable.

[0053] Examples of phosphonate compounds include dimethyl benzenephosphonate, diethyl benzenephosphonate, and dipropyl benzenephosphonate.

[0054] Examples of tertiary phosphines include triethylphosphine, tripropylphosphine, tributylphosphine, trioctylphosphine, triamylphosphine, dimethylphenylphosphine, dibutylphenylphosphine, diphenylmethylphosphine, diphenyloctylphosphine, triphenylphosphine, tri-p-tolylphosphine, trinaphthylphosphine, and diphenylbenzylphosphine. A particularly preferred tertiary phosphine is triphenylphosphine.

[0055] The phosphorus-based stabilizers described above may be used not only individually but also in combination of two or more. Among the phosphorus-based stabilizers described above, phosphite compounds or phosphonite compounds are preferred. Particularly preferred are tris(2,4-di-tert-butylphenyl)phosphite, tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenylenediphosphonite, and bis(2,4-di-tert-butylphenyl)-phenyl-phenylphosphonite. Combinations of these with phosphate compounds are also preferred.

[0056] (iii) Hindered phenol stabilizers (antioxidants) Polycarbonate resins (raw materials) used in the present invention may also be those that contain hindered phenol stabilizers primarily for the purpose of improving their thermal stability during molding and heat aging resistance. Examples of such hindered phenol stabilizers include α-tocopherol, butylhydroxytoluene, cinapyl alcohol, vitamin E, n-octadecyl-β-(4'-hydroxy-3',5'-di-tert-butylphenol)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, 3, 5-di-tert-butyl-4-hydroxybenzylphosphonate diethyl ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-dimethylenebis(6-α-methylbenzyl-p-cresol) 2,2'-ethyl Lyden-bis(4,6-di-tert-butylphenol), 2,2'-butylidene-bis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), triethylene glycol-N-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[2-t [ert-butyl-4-methyl6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl]terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl) sulfide, 4,4'-di-thiobis(2,6-di-tert-butylphenol), 4,4'-tri-thiobis(2,6-di-tert-butylphenol), 2,2-thiodiethylenebis-[3-(3,5-di-tert-butyl-4-hydroxybenzyl) [Nyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylenebis-(3,5-di-tert-butyl-4-hydroxyhydrocinnamide), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1 Examples include 3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4-hydroxyphenyl)isocyanurate, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 1,3,5-tris-2[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, and tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane. All of these are readily available. The above-mentioned hindered phenol antioxidants may be used alone or in combination of two or more.

[0057] The amount of the above (ii) phosphorus-based stabilizer and / or (iii) hindered phenol-based antioxidant is preferably 0.0001 to 1 part by weight, more preferably 0.001 to 0.5 parts by weight, and even more preferably 0.005 to 0.1 parts by weight per 100 parts by weight of polycarbonate resin (raw material). If the amount of stabilizer is too little compared to the above range, it is difficult to obtain a good stabilization effect, and if it is too much compared to the above range, it may conversely cause a decrease in the physical properties of the material or contamination of the mold during molding.

[0058] In the present invention, polycarbonate resins (raw materials) may also be used that contain antioxidants other than the above-mentioned hindered phenol-based antioxidants. Examples of such other antioxidants include pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-laurylthiopropionate), and glycerol-3-stearylthiopropionate. The amount of these other antioxidants used is preferably 0.001 to 0.05 parts by weight per 100 parts by weight of the polycarbonate resin (raw material).

[0059] (iv) UV absorber: Polycarbonate resins (raw materials) used in the present invention may also contain a UV absorber. Examples of UV absorbers include, specifically, benzophenone-based benzophenones such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, 2-hydroxy-4-bendyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfoxytrihydridebenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxy-5-sodium sulfoxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2'-carboxybenzophenone.

[0060] Specifically, among benzotriazole-based UV absorbers, examples include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, and 2-(2-hydroxy-5-tert-octylphenyl) Examples of polymers having a 2-hydroxyphenyl-2H-benzotriazole skeleton include nyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octoxyphenyl)benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2'-p-phenylenebis(1,3-benzoxazine-4-one), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, as well as copolymers of 2-(2'-hydroxy-5-methacryloxyethylphenyl)-2H-benzotriazole with a vinyl monomer copolymerizable with the monomer, and copolymers of 2-(2'-hydroxy-5-acryloxyethylphenyl)-2H-benzotriazole with a vinyl monomer copolymerizable with the monomer.

[0061] Examples of UV absorbers include, specifically, hydroxyphenyltriazine compounds such as 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-methyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-ethyloxyphenol, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-propyloxyphenol, and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-butyloxyphenol. Furthermore, examples include compounds in which the phenyl group of the above example compounds has been replaced with a 2,4-dimethylphenyl group, such as 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hexyloxyphenol.

[0062] Examples of ultraviolet absorbers include cyclic iminoesters such as 2,2'-p-phenylenebis(3,1-benzoxazine-4-one), 2,2'-(4,4'-diphenylene)bis(3,1-benzoxazine-4-one), and 2,2'-(2,6-naphthalene)bis(3,1-benzoxazine-4-one).

[0063] Examples of UV absorbers include, specifically, cyanoacrylate-based 1,3-bis-[(2'-cyano-3',3'-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0064] Furthermore, the above-mentioned ultraviolet absorber may also be a polymer-type ultraviolet absorber obtained by copolymerizing such ultraviolet-absorbing monomer and / or a photostable monomer having a hindered amine structure with a monomer such as an alkyl (meth)acrylate, by adopting the structure of a monomer compound that can undergo radical polymerization. Examples of the above-mentioned ultraviolet-absorbing monomer include compounds containing a benzotriazole skeleton, a benzophenone skeleton, a triazine skeleton, a cyclic iminoester skeleton, and a cyanoacrylate skeleton in the ester substituent of a (meth)acrylic acid ester.

[0065] Among the above, benzotriazole and hydroxyphenyltriazine types are preferred in terms of ultraviolet absorption capacity, while cyclic iminoester and cyanoacrylate types are preferred in terms of heat resistance and hue. The above ultraviolet absorbers may be used individually or as a mixture of two or more.

[0066] The ultraviolet absorber is preferably used in an amount of 0.01 to 2 parts by weight, more preferably 0.03 to 2 parts by weight, even more preferably 0.04 to 1 part by weight, and particularly preferably 0.05 to 0.5 parts by weight per 100 parts by weight of polycarbonate resin.

[0067] (v) Flow modifiers As the polycarbonate resin (raw material) used in the present invention, a flow modifier may also be used, provided that it does not impair the effects of the present invention. Suitable examples of such flow modifiers include styrene oligomers, polycarbonate oligomers (including highly branched, hyperbranched, and cyclic oligomer types), polyalkylene terephthalate oligomers (including highly branched, hyperbranched, and cyclic oligomer types), highly branched and hyperbranched aliphatic polyester oligomers, terpene resins, and polycaprolactone. Such flow modifiers are used in an amount of preferably 0.1 to 30 parts by weight, more preferably 1 to 20 parts by weight, and even more preferably 2 to 15 parts by weight per 100 parts by weight of the polycarbonate resin (raw material). Polycaprolactone is particularly preferred, and the composition ratio is particularly preferably 2 to 7 parts by weight per 100 parts by weight of the polycarbonate resin (raw material). The molecular weight of polycaprolactone is expressed as a number-average molecular weight and ranges from 1,000 to 70,000, with 1,500 to 40,000 being preferred, 2,000 to 30,000 being more preferred, and 2,500 to 15,000 being even more preferred.

[0068] (vi) Antistatic agent As a polycarbonate resin (raw material) used in the present invention, it is also possible to use one that contains an antistatic agent primarily for the purpose of improving antistatic properties. As an antistatic agent, phosphonium sulfonate salts, phosphite esters, caprolactone polymers, etc. can be used, and phosphonium sulfonate salts are preferably used. Specific examples of such phosphonium sulfonate salts include tetrabutylphosphonium dodecylsulfonate, tetrabutylphosphonium dodecylbenzenesulfonate, tributyloctylphosphonium dodecylbenzenesulfonate, tetraoctylphosphonium dodecylbenzenesulfonate, tetraethylphosphonium octadecylbenzenesulfonate, tributylmethylphosphonium dibutylbenzenesulfonate, triphenylphosphonium dibutylnaphthylsulfonate, and trioctylmethylphosphonium diisopropylnaphthylsulfonate. Among these, tetrabutylphosphonium dodecylbenzenesulfonate is preferred in terms of compatibility with polycarbonate and ease of availability. The amount of antistatic agent is preferably 0.1 to 5.0 parts by weight, more preferably 0.2 to 3.0 parts by weight, even more preferably 0.3 to 2.0 parts by weight, and particularly preferably 0.5 to 1.8 parts by weight, per 100 parts by weight of polycarbonate resin (raw material). This is because an antistatic effect is obtained at 0.1 parts by weight or more, and at 5.0 parts by weight or less, excellent transparency and mechanical strength are achieved, and silvering or peeling does not occur on the surface of the molded product, making it less likely to cause appearance defects.

[0069] In addition to the polycarbonate resin (raw material) used in this invention, polycarbonate resins containing various additives such as bluing agents, fluorescent dyes, flame retardants, and dyes and pigments can also be used. These can be appropriately selected and used within a range that does not impair the effects of the present invention.

[0070] The bluing agent is typically contained in polycarbonate resin (raw material) at a concentration of 0.05 to 3.0 ppm (by weight). Representative examples of bluing agents include Bayer's Macrolex Violet B and Macrolex Blue RR, and Clariant's Polysynthrene Blue RLS.

[0071] Examples of fluorescent dyes (including fluorescent whitening agents) include coumarin-based fluorescent dyes, benzopyran-based fluorescent dyes, perylene-based fluorescent dyes, anthraquinone-based fluorescent dyes, thioindigo-based fluorescent dyes, xanthene-based fluorescent dyes, xanthone-based fluorescent dyes, thioxanthene-based fluorescent dyes, thioxanthone-based fluorescent dyes, thiaidine-based fluorescent dyes, and diaminostilbene-based fluorescent dyes. The fluorescent dyes (including fluorescent whitening agents) are preferably blended in an amount of 0.0001 to 0.1 parts by weight per 100 parts by weight of polycarbonate resin (raw material).

[0072] Examples of flame retardants include metal sulfonate salt-based flame retardants, halogen-containing compound-based flame retardants, phosphorus-containing compound-based flame retardants, and silicon-containing compound-based flame retardants. Among these, metal sulfonate salt-based flame retardants are preferred. The flame retardant is usually blended in an amount of 0.01 to 1 part by weight, and more preferably in the range of 0.05 to 1 part by weight, per 100 parts by weight of polycarbonate resin (raw material).

[0073] The present invention will be described in more detail by the following examples, but the present invention is not limited thereto. The evaluation was carried out according to the following method. <<Evaluation Method>> (i) Weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn) The weight-average molecular weight (Mw), number-average molecular weight (Mn), and molecular weight distribution (Mw / Mn) were measured using GPC by the following method. 10 mg of the obtained polycarbonate resin particles were dissolved in 5 mL of chloroform, and 5 μL was introduced into a GPC apparatus set to the following conditions for measurement. The weight-average molecular weight (Mw) and number-average molecular weight (Mn) were calculated in polystyrene equivalent using the above measurement method, and the molecular weight distribution (Mw / Mn) was determined. (Measurement conditions) Equipment: GPC system manufactured by Tosoh Corporation (HLC-8420GPC) Detector: CH-2 (UV) Column: TSKgel superHZM-M Flow rate: 0.35 mL / min Column temperature: 40.0 °C Standard substance: TSK standard polystyrene Eluent: Chloroform

[0074] (ii) Oligomer components and low molecular weight components The amount of oligomer components and low molecular weight components was measured using GPC by the following method. 50 mg of the obtained polycarbonate resin particles were dissolved in 5 mL of chloroform, and 20 μL was introduced into a GPC instrument set to the following conditions for measurement. In the GPC chart obtained by the above measurement method, components with an elution time of 6.15 minutes or more and less than 9.7 minutes were considered oligomer components, and components with an elution time of 9.7 minutes or more were considered low molecular weight components. The ratio (%) of the peak area of ​​each component to the total peak area was calculated and expressed as area %. (Measurement conditions) Equipment: Waters Co., Ltd. GPC system (Waters2695) Column: Tosoh Corporation TSKgel SuperH3000 Guard column: Tosoh TSKguardcolumn superH-L Flow rate: 0.6 mL / min Detector: Waters2489 Detection conditions: UV 254 nm Column temperature: 40.0 °C Standard substance: TSK standard polystyrene Eluent: Chloroform

[0075] (iii) Charpy impact strength The obtained polycarbonate resin particles were placed in a small twin-screw mixer (Xplore Instruments, model: MC15HT), mixed for 2 minutes at a barrel temperature of 270°C and a screw rotation speed of 100 rpm, and molded in an attached injection molding machine (Xplore Instruments, model: IM12) at a cylinder temperature of 270°C and a mold temperature of 80°C to obtain a bending test specimen with a width of 10 mm, a length of 80 mm, and a thickness of 4 mm. Using the obtained bending test specimen, the notched Charpy impact strength was measured in accordance with ISO 179, and the average value of five specimens was calculated.

[0076] [Reference Example 1] In a 100L container equipped with a stirrer, 7.5 kg of recycled polycarbonate resin pellets MT01300C manufactured by Matta (Xiamen) Technology and 60 kg of methylene chloride were charged. The mixture was stirred and dissolved at room temperature. Then, acid (20 kg of pure water and 20 g of concentrated hydrochloric acid (35-37%)) was added, stirred, and after separation, the organic phase was recovered. 20 kg of pure water was added to the recovered polycarbonate resin solution for washing, and the process of separating and recovering the organic phase was repeated twice until the electrical conductivity of the aqueous phase was 50 μS / cm or less. This solution was passed through a 1 μm mesh filter and placed in a kneader filled with 80°C hot water. The methylene chloride was evaporated while stirring and grinding, and the mixture was dried at 120°C to obtain recycled polycarbonate resin powder. Using the obtained recycled polycarbonate resin powder, the weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components were evaluated using the method described above. The evaluation results are shown in Table 1. Charpy impact strength was also evaluated. The evaluation results are shown in Table 2.

[0077] [Example 1] 100 g of recycled polycarbonate resin powder obtained in Reference Example 1 and 400 mL of acetone were placed in a 500 mL flask and stirred at 40°C for 30 minutes. After stirring, only the acetone was filtered out. Another 400 mL of acetone was added, stirred at 40°C for 30 minutes, and then dried at 120°C for 16 hours to obtain recycled polycarbonate resin particles. All acetone used was fresh reagent-grade acetone manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The obtained recycled polycarbonate resin powder was evaluated using the above method for weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components. The evaluation results are shown in Table 1. Charpy impact strength was also evaluated. The evaluation results are shown in Table 2.

[0078] [Example 2] 100 g of recycled polycarbonate resin powder obtained in Reference Example 1 and 400 mL of acetone, which was used in the second extraction in Example 1 and recovered by filtration, were placed in a 500 mL flask. After stirring at 40°C for 30 minutes, only the acetone was filtered out. Another 400 mL of acetone was added, stirred at 40°C for 30 minutes, and then dried at 120°C for 16 hours to obtain recycled polycarbonate resin particles. The second acetone used was a new reagent-grade acetone manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The obtained recycled polycarbonate resin powder was evaluated for weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components using the method described above. The evaluation results are shown in Table 1.

[0079] [Example 3] 100 g of recycled polycarbonate resin powder obtained in Reference Example 1 and 400 mL of acetone were placed in a 500 mL flask and stirred at 40°C for 30 minutes. Half of the acetone (200 mL) was filtered and removed. 200 mL of acetone was then added, stirred at 40°C for 30 minutes, and dried at 120°C for 16 hours to obtain recycled polycarbonate resin particles. The first and second additional acetone used were fresh reagent-grade acetone manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The obtained recycled polycarbonate resin powder was evaluated for weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components using the method described above. The evaluation results are shown in Table 1.

[0080] [Example 4] Recycled polycarbonate resin particles were obtained in the same manner as in Example 1, except that the contact time per session and the number of repetitions were changed. Using the obtained recycled polycarbonate resin powder, the weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components were evaluated using the method described above. The evaluation results are shown in Table 1.

[0081] [Example 5] Recycled polycarbonate resin particles were obtained in the same manner as in Example 1, except that the number of repetitions and the total extraction time were changed. Using the obtained recycled polycarbonate resin powder, the weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components were evaluated using the method described above. The evaluation results are shown in Table 1.

[0082] [Example 6] Recycled polycarbonate resin particles were obtained in the same manner as in Example 5, except that the number of repetitions and the total extraction time were changed. Using the obtained recycled polycarbonate resin powder, the weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components were evaluated using the method described above. The evaluation results are shown in Table 1.

[0083] [Example 7] Recycled polycarbonate resin particles were obtained in the same manner as in Example 1, except that the contact time per step and the total extraction time were changed. Using the obtained recycled polycarbonate resin powder, the weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components were evaluated using the method described above. The evaluation results are shown in Table 1.

[0084] [Comparative Example 1] 100 g of recycled polycarbonate resin powder obtained in Reference Example 1 and 400 mL of acetone were placed in a 500 mL flask, stirred at 40°C for 60 minutes, the acetone was filtered off, and the mixture was dried at 120°C for 16 hours to obtain recycled polycarbonate resin particles. The acetone used was fresh reagent-grade acetone manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. The obtained recycled polycarbonate resin powder was evaluated for weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components using the method described above. The evaluation results are shown in Table 1. The Charpy impact strength was also evaluated. The evaluation results are shown in Table 2.

[0085] [Comparative Example 2] Recycled polycarbonate resin particles were obtained in the same manner as in Comparative Example 1, except that the total extraction time was changed. Using the obtained recycled polycarbonate resin powder, the weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components were evaluated using the method described above. The evaluation results are shown in Table 1.

[0086] [Comparative Example 3] 20 g of recycled polycarbonate resin powder obtained in Reference Example 1 and 110 mL of acetone were charged into a double-tube chromatography column with a joint (3846-20 / 300-4L-W, manufactured by Asahi Seisakusho Co., Ltd.). Warm water was circulated around the outside to bring the system to 40°C. Then, 40°C acetone was introduced from below at a flow rate of 57 mL / h and discharged from the top. After 120 minutes, the acetone was discharged from the bottom, the polycarbonate resin powder was removed from the top, and dried at 120°C for 16 hours to obtain recycled polycarbonate resin particles. The obtained recycled polycarbonate resin powder was evaluated for weight-average molecular weight (Mw), number-average molecular weight (Mn), molecular weight distribution (Mw / Mn), oligomer components, and low molecular weight components using the method described above. The evaluation results are shown in Table 1.

[0087]

[0088]

[0089] As is clear from the comparison in Table 1 above, the method for producing polycarbonate resin particles of the present invention can remove oligomer components and low molecular weight components in a shorter time than conventional batch-type acetone extraction that does not renew the acetone. Furthermore, as can be seen from Table 2, the Charpy impact strength is also increased despite the short time.

[0090] The present invention provides a method for producing polycarbonate resin particles that can efficiently purify polycarbonate resin particles by removing oligomer components and low molecular weight components in a short time. Furthermore, because it is a batch process, it can be flexibly switched when handling various types of raw materials. In particular, the present invention provides a method for producing polycarbonate resin particles that is suitable for recycled polycarbonate resin particles, and the resulting polycarbonate resin particles can be suitable for a wide variety of applications where virgin polycarbonate resin is used.

Claims

1. A method for producing polycarbonate resin particles, characterized by repeating the following steps (A) and (B) in this order at least two times. (A) Solubility parameter of 16-30 MPa, 3-20 times the weight of polycarbonate resin particles 0.5 (B) A step of adding an organic solvent and bringing the polycarbonate resin particles into contact with the organic solvent under stirring. (B) A step of filtering out some or all of the organic solvent from the mixture of polycarbonate resin particles and organic solvent obtained in step (A) to obtain polycarbonate resin particles.

2. Solubility parameter: 16–30 MPa 0.5 A method for producing polycarbonate resin particles according to claim 1, wherein the organic solvent is acetone.

3. The method for producing polycarbonate resin particles according to claim 1, wherein in step (A), the contact time per step is 5 minutes or more and 60 minutes or less.

4. A method for producing polycarbonate resin particles according to claim 1, wherein in step (A), the total contact time with the organic solvent is 20 minutes or more and 360 minutes or less.

5. (A) Solubility parameter to be used in step 16 to 30 MPa 0.5 The method for producing polycarbonate resin particles according to claim 1, wherein the organic solvent is a recycled organic solvent recovered from step (B).

6. The method for producing polycarbonate resin particles according to claim 1, wherein the polycarbonate resin particles are recycled polycarbonate resin particles.

7. (A) In step (A), polycarbonate resin particles and solubility parameter 16 to 30 MPa 0.5 A method for producing polycarbonate resin particles according to claim 1, comprising dissolving polycarbonate resin particles in a good solvent before and / or after contact with an organic solvent, and subjecting the polycarbonate resin solution to one or more of the following treatments: water washing, acid washing, and alkaline washing.