Heat dissipation substrate and package
The use of a ceramic-metal composite adhesive layer in the heat dissipation substrate and package ensures strong bonding between ceramic and metal components, addressing the limitations of brazing by enhancing bonding strength and thermal conductivity while preventing silver migration.
Patent Information
- Application Number
- PCT/JP2026/016509
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-04-24
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for bonding a ceramic member and a heat dissipation member in electronic components, such as those described in Japanese Patent Publications No. 51-132461 and No. 2015-204426, fail to achieve practically sufficient bonding strength without the use of brazing, which can hinder component placement and lead to thermal stress.
A heat dissipation substrate and package design that utilizes an adhesive layer made of a composite material containing both ceramic and metal, sintered with both the ceramic member and the metal heat dissipation member, eliminating the need for brazing and ensuring strong bonding.
This design achieves practically sufficient bonding strength between the ceramic and metal components, allowing for closer component placement, reduced thermal stress, and improved thermal conductivity without the drawbacks of brazing, such as silver migration.
Smart Images

Figure JP2026016509_19112026_PF_FP_ABST
Abstract
Description
Heat Dissipation Substrate and Package
[0001] The present invention relates to a heat dissipation substrate and a package.
[0002] A substrate on which an electronic component is mounted may be required to have a function of releasing heat from the electronic component. In this case, the substrate may be referred to as a heat dissipation substrate. In particular, a substrate having a cavity in which an electronic component is to be accommodated may be referred to as a package.
[0003] Japanese Patent Laid-Open No. 2015-204426 (Patent Document 1) discloses a package. This package includes a heat sink plate and a ceramic frame. The heat sink plate is a rectangular metal plate, and is for dissipating heat generated from an electronic component mounted on the upper surface thereof. The ceramic frame is joined to the heat sink plate so as to surround a region where the electronic component is placed. The joining is performed by brazing. The brazing temperature is approximately 780°C. The ceramic frame is made of, for example, alumina or aluminum nitride.
[0004] The ceramic frame has a frame shape, and is constituted by a joined body of an upper layer sheet and a lower layer sheet. A metallized film and a plating film are provided on the lower surface of the lower layer sheet. The plating film on the lower surface of the lower layer sheet and the heat sink plate are joined via a brazing material. The inner peripheral end of the lower layer sheet is positioned shifted toward the outer peripheral side relative to the inner peripheral end of the upper layer sheet. Thereby, even when the electronic component is brought close to the inner periphery of the upper layer sheet of the ceramic frame, the electronic component can be mounted while avoiding the fillet of the brazing material.
[0005] The heat sink plate described above is a metal plate. This metal plate is selected because it has high thermal conductivity and can mitigate package warping caused by the difference in linear expansion coefficients during brazing with the ceramic frame. For example, a composite metal plate or a clad metal plate can be used. A composite metal plate is formed, for example, by impregnation. Specifically, it is formed by impregnating a porous, high-melting-point metal plate with Cu. Because the linear expansion coefficient of high-melting-point metals such as tungsten or molybdenum is close to that of ceramics, the linear expansion coefficient of the heat sink plate can be brought closer to that of the ceramic frame. Furthermore, because Cu has excellent thermal conductivity, the heat dissipation performance of the heat sink plate can be improved.
[0006] When it is necessary to bring the coefficient of thermal expansion of the heat sink plate closer to that of the ceramic frame, composite metal plates or clad metal plates are widely used, as described above. However, when the consistency of the coefficients of thermal expansion is not critical, simple metal materials are also widely used; for example, using pure copper can significantly increase thermal conductivity.
[0007] Japanese Patent Publication No. 51-132461 (Patent Document 2) describes a manufacturing method that does not require brazing between a metal plate and a frame-shaped ceramic plate. Specifically, as a first manufacturing method, a frame-shaped unfired ceramic plate (green sheet) is placed on a Mo metal plate, directly bonded by hot pressing, and then fired. In this first manufacturing method, because the surface of the metal plate is flat, mutual penetration between the metal and ceramic is difficult during joining. Therefore, the bonding strength between the metal plate and the ceramic plate is extremely weak. Therefore, as a second manufacturing method, the above publication discloses a manufacturing method in which an unfired ceramic plate is placed on one main surface of a metal plate made of a high-melting-point metal (for example, molybdenum or tungsten) via a layer of metal powder made of the high-melting-point metal, and then fired. According to the above publication, the aforementioned mutual penetration is facilitated by interposing a layer of metal powder. Furthermore, since the metal plate and the metal powder layer are of the same material, they are easy to join, and therefore the bonding strength is increased. Therefore, the joint strength increases.
[0008] Japanese Patent Publication No. 2015-204426 Japanese Patent Publication No. 51-132461
[0009] Japanese Patent Publication No. 51-132461 claims that a high bonding strength can be obtained between a metal plate (heat dissipation member) and a ceramic plate (ceramic member) without the need for brazing. However, according to the inventors' research, this still falls far short of a practical bonding strength. In fact, even decades after the disclosure of Japanese Patent Publication No. 51-132461, the bond between a metal plate (heat dissipation member) and a ceramic frame (ceramic member) is typically achieved by brazing, as disclosed in, for example, Japanese Patent Publication No. 2015-204426.
[0010] The present invention was made to solve the above-mentioned problems, and its objective is to provide a heat dissipation substrate and package that can ensure practically sufficient bonding strength between a ceramic member and a heat dissipation member without requiring brazing between the ceramic member and the heat dissipation member.
[0011] Embodiment 1 is a heat dissipation substrate comprising: a surface electrode having a mounting surface on which electronic components will be mounted and a back surface opposite to the mounting surface in the thickness direction; a ceramic member made of a ceramic material having a first surface supporting the surface electrode and a second surface opposite to the first surface in the thickness direction; a heat dissipation member made of a metal sintered material having an opposing surface facing the second surface of the ceramic member; and an adhesive layer provided between the second surface of the ceramic member and the opposing surface of the heat dissipation member, forming a first interface by contacting the second surface of the ceramic member and a second interface by contacting the opposing surface, wherein the adhesive layer is made of a composite material containing both ceramic and metal, the composite material of the adhesive layer and the ceramic material of the ceramic member are sintered with each other at the first interface, and the composite material of the adhesive layer and the metal sintered material of the heat dissipation member are sintered with each other at the second interface.
[0012] Embodiment 2 is a heat dissipation substrate according to Embodiment 1, wherein the ceramic member is arranged without enclosing a virtual plane perpendicular to the thickness direction that is in contact with the mounting surface of the surface electrode.
[0013] Embodiment 3 is a heat dissipation substrate according to Embodiment 1, wherein the ceramic member is positioned off-center from a virtual plane perpendicular to the thickness direction that is in contact with the mounting surface of the surface electrode.
[0014] Embodiment 4 is a heat dissipation substrate according to any one of Embodiments 1 to 3, further comprising a first wiring section embedded in the ceramic member.
[0015] Embodiment 5 is a heat dissipation substrate according to Embodiment 4, wherein the first wiring portion reaches the adhesive layer, and further comprises a second wiring portion that penetrates the adhesive layer so as to connect the first wiring portion and the heat dissipation member to each other.
[0016] Embodiment 6 is a heat dissipation substrate according to Embodiment 4 or 5, wherein the ceramic member includes a plurality of ceramic layers stacked in the thickness direction, and the first wiring portion includes an inner layer electrode having a portion disposed between the plurality of ceramic layers in the thickness direction, and a via electrode connecting the inner layer electrode and the back surface of the surface electrode to each other.
[0017] Embodiment 7 is a heat dissipation substrate according to any one of Embodiments 1 to 3, wherein only the ceramic member is disposed between the surface electrode and the adhesive layer in the thickness direction.
[0018] Embodiment 8 is a package having a cavity in which an electronic component will be housed, comprising: a ceramic member made of a ceramic material having a surface electrode, a first surface supporting the surface electrode, a second surface opposite to the first surface in the thickness direction, and an inner surface surrounding the cavity; a first wiring portion embedded in the ceramic member; a heat dissipation member made of a metal sintered material having an opposing surface facing the second surface of the ceramic member; and an adhesive layer provided between the second surface of the ceramic member and the opposing surface of the heat dissipation member, forming a first interface by contacting the second surface of the ceramic member and a second interface by contacting the opposing surface, wherein the adhesive layer is made of a composite material including both ceramic and metal, the composite material of the adhesive layer and the ceramic material of the ceramic member are sintered with each other at the first interface, and the composite material of the adhesive layer and the metal sintered material of the heat dissipation member are sintered with each other at the second interface.
[0019] Embodiment 9 is the package described in Embodiment 8, wherein the first surface of the ceramic member faces the cavity.
[0020] Embodiment 10 is the package described in Embodiment 8, wherein the ceramic member has a frame shape with through holes corresponding to the cavity.
[0021] Embodiment 11 is a package according to any one of Embodiments 8 to 10, wherein the first wiring portion reaches the adhesive layer, and further comprises a second wiring portion that penetrates the adhesive layer to connect the first wiring portion and the heat dissipation member to each other.
[0022] Embodiment 12 is a package according to any one of Embodiments 8 to 11, wherein the ceramic member includes a plurality of ceramic layers stacked in the thickness direction, and the first wiring portion includes an inner layer electrode having a portion disposed between the plurality of ceramic layers in the thickness direction, and a via electrode connecting the inner layer electrode and the surface layer electrode to each other.
[0023] In one embodiment, the adhesive layer is made of a composite material containing both ceramic and metal. The composite material of the adhesive layer and the ceramic material of the ceramic member are sintered with each other, and the composite material of the adhesive layer and the metal sintered material of the heat dissipation member are sintered with each other. This makes it possible to ensure practically sufficient bonding strength between the ceramic member made of ceramic material and the heat dissipation member made of metal without requiring brazing between the ceramic member and the heat dissipation member.
[0024] Figure 1 is a schematic cross-sectional view showing the configuration of an electronic device according to Embodiment 1. Figure 2 is a schematic cross-sectional view showing the configuration of a package according to Embodiment 1. Figure 3 is a partially enlarged view of Figure 2. Figure 4 is a modified example of Figure 3. Figure 5 is a partial cross-sectional view showing the first step of the manufacturing method of the package in Figure 2. Figure 6 is a partial cross-sectional view showing the second step of the manufacturing method of the package in Figure 2. Figure 7 is a partial cross-sectional view showing the third step of the manufacturing method of the package in Figure 2. Figure 8 is a partial cross-sectional view showing one example of the configuration near the outer end surface of the adhesive layer of the package according to Embodiment 1. Figure 9 is a partial cross-sectional view showing another example of the configuration near the outer end surface of the adhesive layer of the package according to Embodiment 1. Figure 10 is a partial cross-sectional view showing the occurrence of silver migration in the electronic device in Figure 1. Figure 11 is a partial cross-sectional view showing the configuration of an electronic device according to Embodiment 2. Figure 12 is a partial cross-sectional view showing the configuration of an electronic device according to Embodiment 3. Figure 13 is a partial cross-sectional view showing the stress on the bonding layer in the electronic device in Figure 1. Figure 14 is a schematic partial cross-sectional view showing the configuration of an electronic device according to Embodiment 4. Figure 15 is a schematic partial cross-sectional view showing the configuration of an electronic device according to Embodiment 5. Figure 16 is a schematic partial cross-sectional view showing the configuration of an electronic device according to Embodiment 6. Figure 17 is a schematic partial cross-sectional view showing an example of the configuration near the corner formed by the surface and outer surface of the frame in the package of Figure 2. Figure 18 is a schematic partial cross-sectional view showing an example of the configuration near the corner formed by the surface and outer surface of the frame in the package according to Embodiment 7. Figure 19 is a schematic perspective view showing the configuration of a package according to Embodiment 8. Figure 20 is a schematic cross-sectional view showing the configuration of a package according to Embodiment 9. Figure 21 is a partially enlarged view of Figure 20. Figure 22 is a partially enlarged view of Figure 20. Figure 23 is a schematic cross-sectional view showing the configuration of a heat dissipation substrate according to Embodiment 10. Figure 24 is a schematic cross-sectional view showing the configuration of a heat dissipation substrate according to Embodiment 11.
[0025] Embodiments of the present invention will be described below with reference to the drawings. In this specification, unless otherwise specified, "metal" can mean either a pure metal or an alloy. "Alloy" can mean any of a solid solution consisting of multiple metal components, a mixture of multiple metals that are not in solid solution, or an intermetallic compound. The term "green" means the state before firing. Therefore, a component labeled "green" will be fired, but has not yet been fired. The terms "up" and "down" are used to distinguish relative directions and, unless otherwise specified, do not imply any limitation related to the direction of gravity.
[0026] <Embodiment 1> (Outline of the configuration of an electronic device having a package) Figure 1 is a schematic cross-sectional view showing the configuration of an electronic device 100 according to Embodiment 1. Figure 2 is a schematic cross-sectional view showing the configuration of a package 51 having an electronic device 100. The electronic device 100 (Figure 1) has a semiconductor module 90 (electronic device), a heat sink 99, and a solder layer 98 (bonding layer). The solder layer 98 bonds the semiconductor module 90 to the heat sink 99.
[0027] The semiconductor module 90 includes a package 51 having a cavity CV, a semiconductor element 8 (electronic component) housed within the cavity CV, and a mounting material 7 for mounting the semiconductor element 8 onto the package 51. The semiconductor module 90 may also have wires 9 as wiring members for the semiconductor element 8. The wires 9 may be formed by wire bonding. In the example shown in Figure 1, the wires 9 electrically connect the semiconductor element 8 and the surface electrode 35 (Figure 2) to each other.
[0028] The package 51 may be plated at an appropriate timing after the firing process described later. Specifically, a plating layer (not shown) may be formed on the surface of the heat dissipation member 22 and the surface electrode 35. The plating process typically involves forming a nickel plating film (not shown) as a base and a gold plating film (not shown).
[0029] The semiconductor element 8 is mounted on the cavity surface SW1a of the upper surface SW1 of the heat dissipation member 22 of the package 51 via a mounting material 7. The mounting material 7 is conductive. The mounting material 7 may contain silver (Ag). The mounting material 7 may be formed by sintering an Ag paste, and the Ag paste may contain a solvent and nano-sized Ag powder dispersed therein. Alternatively, the mounting material 7 may be formed by curing an epoxy resin in which Ag powder is dispersed. Alternatively, the mounting material 7 may be formed by soldering. This mounting process is typically carried out using a mounting temperature of about 300°C.
[0030] The distance (lateral distance in Figure 1) between the semiconductor element 8 mounted on the package 51 (Figure 1) and the inner surface SF3 of the ceramic member 61 (Figure 2) may be 25 μm or less. This distance may even be zero. In other words, the semiconductor element 8 and the inner surface SF3 of the ceramic member 61 may be in contact. The reason why the semiconductor element 8 can be brought so close to the inner surface SF3 of the ceramic member 61 is that brazing is not used to connect the ceramic member 61 and the heat dissipation member 22 in the package 51. If brazing were used, fillets of brazing material would be formed near the inner surface SF3 in the cavity CV, which would likely hinder the placement of the semiconductor element 8 close to the inner surface SF3. In contrast, in this embodiment, the semiconductor element 8 can be mounted in close proximity to the ceramic member 61, thus allowing for a larger mounting area in the cavity CV. Furthermore, mounting the semiconductor element 8 in close proximity to the ceramic member 61 reduces the length of the wire 9, which usually leads to improved electrical characteristics.
[0031] (Details of the package configuration of the electronic device) Referring to Figure 2, the package 51 has a cavity CV in which the semiconductor element 8 (Figure 1) will be housed. The package 51 has a surface electrode 35, a ceramic member 61, a first wiring section 71, a heat dissipation member 22, and an adhesive layer 40.
[0032] The heat dissipation member 22 has an upper surface SW1, a lower surface SW2 opposite to the upper surface SW1, and an outer wall surface SW4 connecting the upper surface SW1 and the lower surface SW2. In this embodiment 1, the upper surface SW1 faces the cavity CV. Specifically, the upper surface SW1 includes a cavity surface SW1a that faces the cavity CV in the thickness direction. This improves the heat dissipation performance of the semiconductor element 8. In this embodiment 1, the upper surface SW1 also has a peripheral surface SW1b located outside the cavity surface SW1a. The peripheral surface SW1b may surround the cavity surface SW1a. The cavity surface SW1a may be approximately flat. The peripheral surface SW1b may be approximately flat. In the example shown in Figure 2, the upper surface SW1 is approximately flat.
[0033] The heat dissipation member 22 is made of a metal sintered material. In this specification, the metal sintered material means a sintered material that is substantially made of metal. The metal sintered material is substantially a metal material as described above, but may also contain ceramic as an additive. The volume percentage of metal in the metal sintered material is preferably 90% by volume or more, and more preferably 95% by volume or more. This makes it possible to obtain a heat dissipation member 22 with low thermal resistance and electrical resistance and a low coefficient of linear expansion. The volume percentage may be 100%, in which case the metal sintered material contains only metal.
[0034] The metal sintered material may contain at least one high-melting-point metal selected from the group consisting of tungsten (W) and molybdenum (Mo), and copper (Cu). A sufficient proportion of Cu ensures high thermal conductivity. Furthermore, a sufficient proportion of high-melting-point metal allows the coefficient of thermal expansion of the heat dissipation member to approach that of ceramics such as alumina. This approximation of the coefficient of thermal expansion is useful for suppressing thermal stress between the heat dissipation member 22 and the ceramic member 61. The proportion of Cu is, for example, 10% by volume or more and 80% by volume or less. The volume percentage is determined by comparing the weight percentage measured by elemental analysis, such as energy-dispersive X-ray spectroscopy (EDX), with the density values of each element (Cu: 8.96, W: 19.3, Mo: 10.28 (unit: g / cm³)). 3 It can be calculated by ( ). For the sake of simplifying the composition, the metal sintered material may contain only one of W and Mo. In other words, the metal sintered material may be a copper-tungsten alloy or a copper-molybdenum alloy. Note that clad materials manufactured by bonding a copper layer with a tungsten or molybdenum layer are not considered metal sintered materials as defined herein. The thickness of the heat dissipation member 22 is, for example, 0.5 mm or more and 2 mm or less.
[0035] The ceramic member 61 has a top surface SF1 (the first surface of the ceramic member in this embodiment) that supports the surface electrode 35, a bottom surface SF2 (the second surface of the ceramic member) opposite to the top surface SF1 in the thickness direction, an inner surface SF3 surrounding the cavity CV, and an outer surface SF4 opposite to the inner surface SF3. The ceramic member 61 may have a frame shape with a through hole HP corresponding to the cavity CV. The through hole HP extends from the top surface SF1 toward the heat dissipation member 22. The peripheral surface SW1b (the opposing surface in this embodiment) of the heat dissipation member 22 faces the bottom surface SF2 of the ceramic member 61 in the thickness direction.
[0036] The outer edge of the ceramic member 61 may have a rectangular shape in the in-plane direction perpendicular to the thickness direction. The size of each side of the rectangular shape is, for example, 4 mm to 40 mm. The thickness of the ceramic member 61 is, for example, 0.1 mm to 1 mm. The ceramic member 61 is made of a ceramic material. This makes it possible to improve the heat resistance of the package 51 compared to when the ceramic member 61 is made of a resin material. Because the ceramic material is an insulator, the top surface SF1 of the ceramic member 61 can be made an electrically insulated surface from the heat dissipation member 22. The ceramic material includes, for example, alumina as its main component. In this case, the ceramic material may also include additives, for example, silicon oxide, manganese oxide, or both. The composition of the ceramic member 61 can be confirmed by elemental analysis, for example, EDX.
[0037] The adhesive layer 40 is provided between the bottom surface SF2 of the ceramic member 61 and the peripheral surface SW1b of the heat dissipation member 22. The adhesive layer 40 forms a first interface FC1 by contacting the bottom surface SF2 of the ceramic member 61 and a second interface FC2 by contacting the peripheral surface SW1b of the heat dissipation member 22. The adhesive layer 40 also has an outer end surface SA4 facing outwards from the package 51. At least a portion of the adhesive layer 40 is in contact with the peripheral surface SW1b of the top surface SW1 of the heat dissipation member 22. In the example shown in Figure 2, it is also in contact with a portion of the cavity surface SW1a of the top surface SW1 of the heat dissipation member 22. The adhesive layer 40 may be arranged to be in contact with only (not all) a portion of the cavity surface SW1a, as shown in Figure 2, in which case the adhesive layer 40 has an inner end surface SA3 facing towards the cavity CV. In this embodiment, the inner end surface SA3 of the adhesive layer 40 protrudes inward from the inner surface SF3 of the ceramic member 61 (in other words, toward the cavity CV), but the position of the inner end surface SA3 is not limited to this. As a modification, the inner end surface SA3 of the adhesive layer 40 may be flush with the inner surface SF3 of the ceramic member 61, or it may be recessed outward from the inner surface SF3 (in other words, in the opposite direction to the cavity CV).
[0038] The adhesive layer 40 is made of a composite material containing both metal and ceramic. The composite material of the adhesive layer 40 and the ceramic material of the ceramic member 61 are sintered together at the first interface FC1. The composite material of the adhesive layer 40 and the metal sintered material of the heat dissipation member 22 are sintered together at the second interface FC2. Note that, since Cu has a low melting point, the Cu of the adhesive layer 40 and the Cu of the heat dissipation member 22 may melt and join together. The ceramic member 61 and the heat dissipation member 22 are fixed together by utilizing the sintering at the first interface FC1 and the second interface FC2. This eliminates the need to use brazing material to join the ceramic member 61 and the heat dissipation member 22 together. Brazing material usually contains Ag, and by avoiding the use of brazing material, the presence of Ag, an element prone to migration, between the ceramic member 61 and the heat dissipation member 22 can be avoided. The volume ratio of metal in the adhesive layer 40 is smaller than the volume ratio of metal in the heat dissipation member 22.
[0039] The metal in the composite material may include at least one high-melting-point metal selected from the group consisting of W and Mo, and Cu. The main component of the ceramic in the composite material is, for example, alumina. In addition to alumina as the main component, the ceramic may contain additives, such as silicon oxide and manganese oxide.
[0040] The composite material may contain materials common to the ceramic material of the ceramic member 61. This reduces the difference in sintering temperatures between the adhesive layer 40 and the ceramic member 61 when they are fired simultaneously. The composite material of the adhesive layer 40 may also contain materials common to the metal sintering material of the heat dissipation member 22. This ensures more reliable bonding strength between the adhesive layer 40 and the heat dissipation member 22 when they are fired simultaneously.
[0041] The linear expansion coefficient of the composite material of the adhesive layer 40 may be larger than the linear expansion coefficient of the ceramic material of the ceramic member 61 and smaller than the linear expansion coefficient of the heat dissipation member 22. Such a relationship between the linear expansion coefficients is naturally obtained, for example, when the ceramic of the composite material of the adhesive layer 40 is the same as the ceramic material of the ceramic member 61, and the metal of the composite material of the adhesive layer 40 is the same as the sintered metal material of the heat dissipation member.
[0042] The composite material preferably contains 20 vol% or more and 80 vol% or less of ceramic. By containing 20 vol% or more of ceramic, the bonding strength of the ceramic member 61 to the ceramic material is enhanced. Further, the composite material of the adhesive layer 40 preferably contains 20 vol% or more and 80 vol% or less of metal. By containing 20 vol% or more of metal, the bonding strength of the heat dissipation member 22 to the sintered metal material is enhanced. The adhesive layer 40 may consist only of a ceramic material and a metal material. Therefore, the adhesive layer 40 does not need to contain an organic material. The adhesive layer 40 preferably does not contain Ag. The composition of the composite material can be confirmed, for example, by performing elemental analysis such as EDX.
[0043] The thickness of the adhesive layer 40 (the dimension in the vertical direction in FIG. 2) may be 5 μm or more and 50 μm or less. When the thickness is 5 μm or more, the thickness of the layer can be made approximately uniform while using generally used powders of about 0.5 μm or more and 2 μm or less as the ceramic powder and metal powder for forming the adhesive layer 40. In addition, the effect of the adhesive layer 40 can be more sufficiently obtained. When the thickness is 50 μm or less, the screen printing method can be easily applied as a method for forming the adhesive layer 40.
[0044] The surface layer electrode 35 is provided on the top surface SF1 of the ceramic member 61. The surface layer electrode 35 may contain copper (Cu) and at least one high-melting-point metal selected from the group consisting of tungsten (W) and molybdenum (Mo). The surface layer electrode 35 may be made of a sintered material containing Cu at a higher volume ratio than the sintered metal material of the heat dissipation member 22.
[0045] Figure 3 is a partially enlarged view of Figure 2. The first wiring section 71 is embedded in the ceramic member 61 and connected to the back surface (bottom surface in the figure) of the surface electrode 35. In this embodiment 1, the ceramic member 61 includes a plurality of ceramic layers LY1 and LY2 stacked in the thickness direction. The boundary between ceramic layers LY1 and LY2 (dashed line in the figure) may be virtual. The first wiring section 71 includes an inner layer electrode 71i having a portion positioned between the plurality of ceramic layers LY1 and LY2 in the thickness direction, and a via electrode 71v connecting the inner layer electrode 71i and the surface electrode 35 to each other.
[0046] Figure 4 is a modified version of Figure 3. In this modified version, the first wiring portion 71 reaches the adhesive layer 40. In this case, the first wiring portion may be a via electrode that penetrates the ceramic member 61 in the thickness direction, as shown in Figure 4. In this modified version, the package 51 also has a second wiring portion 72 that penetrates the adhesive layer 40 so as to connect the first wiring portion 71 and the heat dissipation member 22 to each other. The second wiring portion 72 may be a via electrode that penetrates the adhesive layer 40 in the thickness direction, as shown in Figure 4. The presence of the second wiring portion 72 allows the first wiring portion 71 and the heat dissipation member 22 to be electrically connected to each other.
[0047] (Package Manufacturing Method) Figures 5 to 7 are schematic cross-sectional views showing the first to third steps of the manufacturing method for package 51 (Figure 2).
[0048] Referring to Figure 5, a green sheet 61G is formed, which includes a portion that will become the ceramic member 61 (Figure 2) when fired. Generally, the green sheet is formed from a slurry using the doctor blade method. The slurry is obtained by mixing the powder that will become the components of the sintered body with a resin, plasticizer, and solvent using a ball mill. The powder for the slurry to form the ceramic member 61 is, for example, 50% by weight or more of Al as the main component. 2 O 3 Powder and SiO 2 A mixed powder may consist of a Si-containing powder corresponding to 5-17% by weight in terms of conversion, and a Mn-containing powder corresponding to 3-14% by weight in terms of MnO conversion.2 O 3 The average particle size of the powder is preferably 0.4 μm to 2.5 μm, and more preferably 1.3 μm to 1.7 μm. Using this slurry, a green sheet 61G can be formed by the doctor blade method. Next, a green surface electrode 35G, which will become the surface electrode 35 when fired, is formed on one surface of the green sheet 61G (the top surface in Figure 5), and a green adhesive layer 40G, which will become the adhesive layer 40 when fired, is formed on the other surface of the green sheet 61G (the bottom surface in Figure 5). These formations may be carried out by printing the paste using a screen printing method. The printed paste is dried, for example, at a temperature of 110°C for 5 minutes.
[0049] The paste for the green surface electrode 35G contains metal powder. The metal powder may include Cu powder and powder of at least one high-melting-point metal selected from the group consisting of W and Mo. The average particle size of the high-melting-point metal powder may be 0.5 μm or more and 10 μm or less, preferably 0.5 μm or more and 3 μm or less, and more preferably 0.5 μm or more and 1.5 μm or less. The average particle size of the Cu powder may be 1.5 μm or more and 5.0 μm or less. The paste may also contain ceramic powder as an additive as needed. The composition and average particle size of the ceramic powder may be the same as those of the green sheet 61G. The paste is manufactured by kneading this metal powder (and optionally ceramic powder) together with a resin and a solvent. As a variation, instead of printing the paste, a green sheet formed from a slurry of a material similar to the paste may be laminated.
[0050] The paste for the green adhesive layer 40G contains metal powder and ceramic powder. The metal powder may contain Cu powder and powder of at least one high-melting-point metal selected from the group consisting of W and Mo. The composition and / or average particle size of the metal powder for the green adhesive layer 40G may be the same as that used in the slurry for the green sheet 22G described later. The composition and / or average particle size of the ceramic powder for the green adhesive layer 40G may also be the same as that used in the slurry for the green sheet 61G described above. The paste is produced by kneading these metal powders and ceramic powders together with a resin and a solvent. As a variation, instead of printing the paste, a lamination of green sheets formed from a slurry of materials similar to the paste may be performed.
[0051] Next, through holes HP are formed to constitute the cavity CV (Figure 2). This formation is done, for example, by punching.
[0052] Referring to Figure 6, a green sheet 22G is formed by firing to become the heat dissipation member 22 (Figure 2). The powder for the slurry to form the heat dissipation member 22 may be a mixed powder containing Cu powder and high-melting-point metal powder. Therefore, in this manufacturing method, unlike the impregnation method in which Cu is supplied by impregnation into already sintered high-melting-point metal, Cu and high-melting-point metal are mixed together in powder form. The average particle size of the high-melting-point metal powder may be 0.5 μm or more and 10 μm or less, preferably 0.5 μm or more and 3 μm or less, and more preferably 0.5 μm or more and 1.5 μm or less. The average particle size of the Cu powder may be 1.5 μm or more and 5.0 μm or less. The above mixed powder may also contain ceramic powder as an additive. The composition and average particle size of the ceramic powder may be the same as that of the green sheet 61. Also, for example, SiO with an average particle size of 7 nm or more and 200 nm or less. 2 It may contain powders or other similar substances.
[0053] Next, the green sheet 22G and the configuration shown in Figure 5 are stacked on top of each other to form the green structure KG. The green structure KG is a structure that combines the green sheet 22G (first green member), the green sheet 61G (second green member), and the green adhesive layer 40G (third green member), and in this example, the green surface electrode 35G is also combined. When a break is performed as described later, trenches (not shown) may be formed on the upper and lower surfaces of the green structure KG at the position where the break will occur (see the dashed line in the figure) by machining with a cutting edge CT or by laser processing with a laser processing device (not shown).
[0054] Next, the green structure KG is fired. The firing temperature is, for example, 1100°C to 1400°C. By firing at a temperature of 1100°C or higher, the laminate can be heated to a temperature higher than the melting point of Cu. This makes it possible to form a high-quality heat dissipation member 22 containing Cu. On the other hand, by firing at a temperature of 1400°C or lower, it is possible to avoid process difficulties caused by excessively high firing temperatures. For example, it is possible to avoid excessive evaporation of Cu during firing. As mentioned above, plating may be performed at any timing after the firing process. Also, mounting of the semiconductor element 8 (Figure 1) may be performed at any timing after the firing process (or after the plating process if plating is performed).
[0055] Furthermore, if the green adhesive layer 40G were laminated onto a flat metal plate serving as a heat dissipation member, similar to the technology described in the aforementioned Japanese Patent Publication No. 51-132461, the bonding strength between the heat dissipation member and the adhesive layer after firing the green adhesive layer 40G would be extremely low. Also, if the green adhesive layer 40G were laminated onto a metal plate that has microscopic irregularities due to being made of a metal sintering material, rather than a flat metal plate as described above, the number of contact points between the metal powder in the green adhesive layer 40G and the surface of the metal plate would increase. As a result, the bonding strength between the adhesive layer 40 obtained by firing the green adhesive layer 40G and the metal plate would increase somewhat compared to the aforementioned case, but there is still considerable room for improvement. In contrast to these methods, according to this embodiment, the green adhesive layer 40G is laminated onto a green sheet 22G that will become the heat dissipation member 22, and these are fired simultaneously. This allows the metal powder in the green adhesive layer 40G to penetrate the green sheet 22G more effectively. Therefore, the bonding strength between the adhesive layer 40 and the heat dissipation member 22 after firing is significantly improved compared to the two methods described above.
[0056] Referring to Figure 7, a sintered body KF is obtained from the green structure KG by the firing process described above. In other words, the heat dissipation member 22, the ceramic member 61, the adhesive layer 40, and the surface electrode 35 are formed by simultaneous firing. Next, a break process is performed on the sintered body KF to generate cracks along the dashed line BR, starting from the trenches mentioned above. This break process yields a package 51 (Figure 2) from the sintered body KF (Figure 7). As a modification, instead of the break process, a cutting process may be performed before firing to form trenches. Furthermore, to increase manufacturing efficiency, multiple packages 51 may be obtained from a single sintered body KF.
[0057] Figure 8 is a schematic partial cross-sectional view in a cross-sectional view parallel to the thickness direction, showing one example of the configuration of the package 51 near the outer end surface SA4 of the adhesive layer 40. In this cross-sectional view, the outer surface SF4 of the ceramic member 61 has a lower end JF4, and the outer wall surface SW4 of the heat dissipation member 22 has an upper end JW4. As described above, a break process (or cutting process) is performed along the dashed line BR (Figure 7), and at least before the firing process, the lower end JF4 and the upper end JW4 are in approximately the same position in the direction perpendicular to the thickness direction (lateral direction in Figure 8), i.e., in the in-plane direction, and the outer end surface SA4 of the adhesive layer 40 extends in the thickness direction so as to roughly connect them.
[0058] Strictly speaking, due to factors such as sintering shrinkage during the firing process, a slight misalignment may occur in the in-plane direction between the lower end JF4 of the ceramic member 61 and the upper end JA4a of the adhesive layer 40, as shown in Figure 9. Even in this case, the misalignment can be easily reduced to within 0.1 mm by applying a break or cut process. Note that in Figure 9, the upper end JA4a of the adhesive layer 40 is shifted outward (to the right in the figure) relative to the lower end JF4 of the ceramic member 61, but this misalignment may be reversed. Similarly, a slight misalignment may occur in the in-plane direction between the lower end JA4b of the adhesive layer 40 and the upper end JW4 of the heat dissipation member 22. Even in this case, the misalignment can be easily reduced to within 0.1 mm by applying a break or cut process. Note that in Figure 9, the upper end JW4 of the heat dissipation member 22 is shifted outward (to the right in the figure) relative to the lower end JA4b of the adhesive layer 40, but this misalignment may be reversed. The breaking process makes it easy to keep all four positions—the lower end JF4, the upper end JA4a, the lower end JA4b, and the upper end JW4—within a range of 0.1 mm in the in-plane direction (lateral direction in Figure 9).
[0059] (Effects) According to this embodiment 1, the adhesive layer 40 (Figure 2) is made of a composite material containing both ceramic and metal. The composite material of the adhesive layer 40 and the ceramic material of the ceramic member 61 are sintered with each other, and the composite material of the adhesive layer 40 and the metal sintered material of the heat dissipation member 22 are sintered with each other. As a result, practically sufficient bonding strength can be ensured between the ceramic member 61 made of ceramic material and the heat dissipation member 22 made of metal without requiring brazing between the ceramic member 61 and the heat dissipation member 22.
[0060] When the heat dissipation member 22 contains both Cu and a high-melting-point metal, the improvement in the thermal conductivity of the heat dissipation member 22 due to the inclusion of Cu and the suppression of the coefficient of linear expansion of the heat dissipation member 22 due to the inclusion of the high-melting-point metal can be appropriately adjusted according to the application of the package. When the composite material of the adhesive layer 40 also includes a material similar to such a metal sintered material, the similarity of the materials makes it possible to more reliably ensure the bonding strength between the heat dissipation member 22 and the adhesive layer 40.
[0061] The surface electrode 35 may be made of a sintered material containing Cu in a higher volume ratio compared to the metal sintered material of the heat dissipation member 22. This results in the linear expansion coefficient of the surface electrode 35 being higher than that of the heat dissipation member 22. Considering that the thickness of the surface electrode 35 is usually smaller than that of the heat dissipation member 22, in a configuration in which a ceramic member 61 made of ceramic material is placed between the surface electrode 35 and the heat dissipation member 22, the above-described relationship of linear expansion coefficients makes it easier to balance the thermal stress in the package 51. Therefore, warping of the package 51 under temperature changes can be suppressed. The thickness of the surface electrode 35 is preferably 5 μm or more and 200 μm or less. If the thickness is 5 μm or more, it becomes easier to balance the thermal stress as described above, so the effect of suppressing warping of the package 51 can be obtained more fully. Furthermore, the surface electrode 35 can fully obtain its function as a conductive layer. If the thickness is 200 μm or less, peeling of the surface electrode 35 can be made less likely.
[0062] Unlike typical brazing materials, the adhesive layer 40 does not need to contain silver (Ag). This prevents the occurrence of Ag migration from the adhesive layer 40. In particular, when a surface electrode 35, insulated from the heat dissipation member 22 by the ceramic member 61, is provided on the top surface SF1 of the ceramic member 61, this prevents insufficient electrical insulation between the heat dissipation member 22 and the surface electrode 35 due to such migration. If the adhesive layer 40 contained Ag, as in a typical brazing material layer, Ag migration would be likely to occur if a negative potential was applied to the surface electrode 35 for a long period of time, based on the potential of the heat dissipation member 22.
[0063] Referring to Figures 8 and 9, by minimizing the misalignment between the lower end JF4 of the ceramic member 61 and the upper end JA4a of the adhesive layer 40, and minimizing the misalignment between the lower end JA4b of the adhesive layer 40 and the upper end JW4 of the heat dissipation member 22, stress concentration caused by these misalignments can be suppressed. Therefore, delamination between the lower end JF4 of the outer surface SF4 of the ceramic member 61 and the upper end JW4 of the outer wall surface SW4 of the heat dissipation member 22 is prevented.
[0064] <Embodiment 2> Figure 10 is a schematic partial cross-sectional view showing the occurrence of Ag migration in an electronic device 100 having the package 51 according to Embodiment 1 described above. The adhesive layer 40 has an inner end EI that extends into the cavity CV. As mentioned above, the adhesive layer 40 does not need to contain Ag, but the mounting material 7 often needs to contain Ag. Therefore, Ag migration may occur along the path MG (dashed arrow in Figure 10).
[0065] Figure 11 is a schematic partial cross-sectional view showing the configuration of the electronic device 100 according to this second embodiment, which has a package 52 instead of package 51 (Figure 10). In both the case of package 51 and package 52, the composite material of the adhesive layer 40 does not need to contain Ag. On the other hand, unlike package 51, in package 52, a space PS is provided between the inner end EI of the adhesive layer 40 and the bottom surface SF2 of the ceramic member 61 in the thickness direction (vertical direction in the figure). Note that the other configurations are substantially the same as those of the first embodiment described above, so the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0066] According to this second embodiment, Ag migration from the mounting material 7 must proceed along the path MG (dashed arrow in Figure 11) that bypasses the space PS. Therefore, a decrease in electrical insulation between the heat dissipation member 22 and the top surface SF1 of the ceramic member 61 due to Ag migration is suppressed. In particular, if a surface electrode 35 insulated from the heat dissipation member 22 by the ceramic member 61 is provided, it is possible to avoid insufficient electrical insulation between the heat dissipation member 22 and the surface electrode 35 due to such migration.
[0067] <Embodiment 3> Figure 12 is a schematic partial cross-sectional view showing the configuration of the electronic device 100 according to this third embodiment, which has a package 53 instead of a package 51 (Figure 10). In both the case of package 51 and package 53 (Figures 10 and 12), the composite material of the adhesive layer 40 does not need to contain Ag. On the other hand, unlike package 51, in package 53, a space PS is provided between the inner end EI of the adhesive layer 40 and the upper surface SW1 of the heat dissipation member 22 in the thickness direction (vertical direction in the figure). Note that the other configurations are substantially the same as those of Embodiment 1 described above, so the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0068] According to this third embodiment, Ag migration from the mounting material 7 must proceed along the path MG (dashed arrow in Figure 12) that bypasses the space PS. Therefore, a decrease in electrical insulation between the heat dissipation member 22 and the top surface SF1 of the ceramic member 61 due to Ag migration is suppressed. In particular, if a surface electrode 35 insulated from the heat dissipation member 22 by the ceramic member 61 is provided, it is possible to avoid insufficient electrical insulation between the heat dissipation member 22 and the surface electrode 35 due to such migration.
[0069] <Embodiment 4> Figure 13 is a schematic partial cross-sectional view showing the stress TS generated in the solder layer 98 due to temperature changes in an electronic device 100 having a package 51 according to Embodiment 1 described above. Stress TS tends to occur along the in-plane direction (lateral direction in the figure). In the package 51, the lower surface SW2 of the heat dissipation member 22 and the outer wall surface SW4 may be at approximately a right angle AGr. In that case, stress TS is generated perpendicular to the interface between the outer wall surface SW4 and the solder layer 98. As a result, if the stress TS is large, it is likely to lead to delamination at that interface.
[0070] Figure 14 is a schematic cross-sectional view showing the configuration of the electronic device 100 according to this fourth embodiment, which has a package 54 instead of a package 51 (Figure 13). In the package 54, the lower surface SW2 of the heat dissipation member 22 and the outer wall surface SW4 form an obtuse angle AGo. The obtuse angle AGo is, for example, 92° or more and 100° or less. The obtuse angle AGo can be obtained, for example, by buffing the package 51 (Figure 13), which has a right angle AGr, while holding it by hand or the like. Note that the other configurations are substantially the same as the configurations of any of the embodiments 1 to 3 described above, so the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0071] According to this fourth embodiment, the outer wall surface SW4 is inclined rather than perpendicular to the in-plane direction. This makes it less likely for stress TS to lead to delamination at the interface between the outer wall surface SW4 and the solder layer 98. Therefore, the solder layer 98 can be made less prone to delamination.
[0072] <Embodiment 5> Figure 15 is a schematic partial cross-sectional view showing the configuration of the electronic device 100 according to Embodiment 5, wherein the electronic device 100 has a package 55 instead of a package 51 (Figure 2). The cross-sectional view is parallel to the thickness direction and is a cross-sectional view passing through the center of the heat dissipation member 22. In the package 51 (Figures 1 and 2: Embodiment 1), the lower surface SW2 of the heat dissipation member 22 may be flat. In contrast, in the package 55 (Figure 15), the lower surface SW2 of the heat dissipation member 22 has a convex shape VX at the center of the heat dissipation member 22. The other configurations are substantially the same as those of any of Embodiments 1 to 4 described above, so the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0073] According to this embodiment 5, when joining the heat dissipation member 22 to the heat sink 99 (more generally, another member) by forming a solder layer 98 using solder that has been melted by heating (more generally, a fluid material for forming a bonding layer), the convex shape VX pushes the bonding material outwards from the center of the heat dissipation member 22 to the peripheral area. This makes it easier to ensure the bonding strength of the solder layer 98 in the peripheral area around the center. Since delamination of the solder layer 98 is more likely to occur from the peripheral area than from the center, ensuring the bonding strength of the solder layer 98 in the peripheral area can prevent delamination of the solder layer 98.
[0074] The reference line LS (Figure 15) is a straight line connecting one end and the other end (right end and left end in the figure) of the heat dissipation member 22. The convex shape VX protrudes beyond the reference line LS. The height difference of the lower surface SW2 in the direction perpendicular to the reference line LS, with respect to the reference line LS, is preferably 10 μm or more and 100 μm or less. The above effect can be obtained more fully when the height difference is 10 μm or more. When the height difference is 100 μm or less, it is possible to prevent the formation of areas where the thickness of the solder layer 98 is locally excessive. The thermal conductivity of the solder layer 98 is not necessarily higher than that of the heat dissipation member 22, so if the thickness of the solder layer 98 is excessive, the heat dissipation characteristics may deteriorate.
[0075] Unlike Embodiment 6, which will be described later, in Embodiment 5, the lower surface SW2 does not have a portion that is set back from the reference line LS (the portion above the reference line LS in Figure 12). Therefore, the height difference in Embodiment 5 is equal to the dimension by which the convex shape VX protrudes from the reference line LS in a direction perpendicular to the reference line LS.
[0076] <Embodiment 6> Figure 16 is a schematic partial cross-sectional view showing the configuration of the electronic device 100 according to Embodiment 6, wherein the electronic device 100 has a package 56 instead of package 55 (Figure 15). This cross-sectional view, like Figure 15 described above, is parallel to the thickness direction and is a cross-sectional view passing through the center of the heat dissipation member 22. In package 57 (Figure 16), the lower surface SW2 of the heat dissipation member 22 has a concave shape VC outside the center, in addition to the convex shape VX in Embodiment 5 described above. To obtain the concave shape VC, for example, heat treatment can be performed in the cavity CV of package 55 (Figure 15: Embodiment 5) while placing a weight at the position where the concave shape VC is to be formed. Note that the other configurations are substantially the same as those of Embodiment 5 described above, so the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0077] According to this embodiment 6, by having a convex shape VX, effects similar to those of embodiment 5 can be obtained. Here, in package 51 (Figure 15: Embodiment 1), the lower surface SW2 of the heat dissipation member 22 has a simple convex shape. Therefore, when joining the heat dissipation member 22 to the heat sink 99 (more generally, another member) by forming a solder layer 98 using solder that has been melted by heating (more generally, a fluid material for forming a bonding layer), the lower surface SW2 of package 51 tends to tilt unintentionally from the horizontal plane, as shown by arrow NC (Figure 15), with the protruding part of the convex shape VX as a fulcrum. In contrast, according to this embodiment 6, by having a concave shape VC on the lower surface SW2 of the heat dissipation member 22, the end of the lower surface SW2 of the heat dissipation member 22 can be brought closer to the heat sink 99. This makes it possible to suppress the tilting of the heat dissipation member 22.
[0078] The concave shape VC is positioned behind the reference line LS (above the reference line LS in Figure 13). Therefore, the height difference in this embodiment 6 is the sum of the dimension by which the convex shape VX protrudes from the reference line LS in the direction perpendicular to the reference line LS, and the dimension by which the concave shape VC is set back from the reference line LS in the direction perpendicular to the reference line LS. In this embodiment 6 as well, similar to the embodiment 5 described above, it is preferable that the height difference in the direction perpendicular to the reference line LS is 10 μm or more and 100 μm or less.
[0079] <Embodiment 7> Figure 17 is a schematic partial cross-sectional view showing an example of the configuration near the corner AS formed by the top surface SF1 and the outer surface SF4 of the ceramic member 61 in the package 51 according to Embodiment 1 described above. The corner AS may be an unrounded corner. Figure 18 is a schematic partial cross-sectional view showing an example of the configuration near the corner AP formed by the top surface SF1 and the outer surface SF4 of the ceramic member 61 in the package 57 according to Embodiment 7. The corner AP is rounded, and specifically has a radius of curvature of 0.1 mm or more and 0.5 mm or less. Note that the other configurations are substantially the same as the configurations of any of Embodiments 1 to 6 described above, so the same or corresponding elements are denoted by the same reference numerals and their descriptions are not repeated.
[0080] According to this embodiment, the corner AP of the ceramic member 61 has a radius of curvature of 0.1 mm or more and 0.5 mm or less. A radius of curvature of 0.1 mm or more makes the corner AP less likely to chip when subjected to impact. A radius of curvature of 0.5 mm or less prevents an excessive reduction in the area of the top surface SF1 of the ceramic member 61 due to the rounding of the corner AP. In particular, when a surface electrode 35 (Figure 2) is provided on the top surface SF1 of the ceramic member 61, ensuring a sufficient area of the top surface SF1 of the ceramic member 61 makes it easier to secure the bonding area between the top surface SF1 of the ceramic member 61 and the surface electrode 35. Therefore, they can be bonded to each other with high strength.
[0081] <Embodiment 8> In the previously described Embodiment 1, the package 51 (Figure 2: Embodiment 1) has a single cavity CV, but the package may have multiple cavities. Figure 19 is a schematic perspective view showing the configuration of the package 51M according to Embodiment 8. In Figure 19, a dot pattern is applied to the surface electrode 35 for clarity. The package 51M has cavities CV1 and CV2. The ceramic member 61M of the package 59M has an inner surface that surrounds the multiple cavities CV1 and CV2. In the example shown in Figure 19, the surface electrode 35 includes a portion that functions as a wiring pattern. As in the case of Figure 2, the surface electrode 35 may have a portion to which the wire 9 will be connected.
[0082] Furthermore, since the configuration other than that described above is substantially the same as that of Embodiment 1, the same reference numerals are used for the same or corresponding elements, and their descriptions are not repeated. In addition, in any of the above-described embodiments, multiple cavities may be provided instead of one cavity, as in Embodiment 10.
[0083] <Embodiment 9> Figure 20 is a schematic cross-sectional view showing the configuration of a package 58 according to Embodiment 9. The package 58 includes a surface electrode 31, a ceramic member 68, a first wiring section 71, a heat dissipation member 22, and an adhesive layer 40. The package 58 may also have a second wiring section 72. As shown in Figures 21 and 22, the surface electrode 31 has a mounting surface SM and a back surface SB opposite to the mounting surface SM in the thickness direction. The mounting surface SM is not the surface to which the wire 9 (Figure 1) will be joined, but the surface to which the electronic component (for example, a semiconductor element 8 (Figure 1)) itself will be mounted. This mounting may be performed by joining the electronic component to the mounting surface SM using a mounting material 7 (see Figure 1).
[0084] The ceramic member 68 has a cavity surface SF5 (the first surface of the ceramic member in this embodiment) that supports the surface electrode 31, a bottom surface SF2 (the second surface of the ceramic member) opposite to the cavity surface SF5 in the thickness direction, and an inner surface SF3 that surrounds the cavity CV. The bottom surface SF2 may also have a portion opposite to the top surface SF1 in the thickness direction. The material of the ceramic member 68 may be the same as that of the ceramic member 61 (Embodiment 1).
[0085] The ceramic member 61 of the package 51 (Figure 1) according to the above-described embodiment 1 has a through hole HP corresponding to the cavity CV. In contrast, the ceramic member 68 of the package according to embodiment 9 (Figure 20) has a blind hole HS corresponding to the cavity CV. The blind hole HS extends from the top surface SF1 toward the heat dissipation member 22, but does not penetrate the ceramic member 68. Correspondingly, the ceramic member 68 has a cavity surface SF5 that faces the cavity CV in the thickness direction. More specifically, in the example shown in Figure 20, the ceramic member 68 has a plate-shaped base portion 68a and a frame portion 68b located on the base portion 68a. The inner surface SF3 of the ceramic member 68 is provided by the frame portion 68b. With the above structure, insulation between the heat dissipation member 22 and the surface electrode 31 (see, for example, the one on the right in Figure 20) can be ensured. The heat dissipation member 22 and the surface electrode 31 (see, for example, the one on the left in Figure 20) may be electrically connected to each other via the first wiring section 71 and the second wiring section 72. The boundary between the base section 68a and the frame section 68b (dashed line in the figure) may be hypothetical.
[0086] Figures 21 and 22 are enlarged views of a portion of Figure 20. Unlike in Embodiment 1 (Figure 3), in Embodiment 9 the first wiring section 71 is connected to the back surface (bottom surface in the figure) of the surface electrode 31 having a mounting surface SM. As a modification, the package 58 may have an additional surface electrode 35 (Figure 2: Embodiment 1) in addition to the surface electrode 31 having a mounting surface SM. The surface electrode 35 does not need to have a mounting surface SM. The package 58 may further have a first wiring section 71 (Figure 2) connected to the back surface of this surface electrode 35.
[0087] In this embodiment, the heat dissipation member 22 has an upper surface SW1 (the opposing surface in this embodiment) that faces the bottom surface SF2 of the ceramic member 68. The adhesive layer 40 is provided between the bottom surface SF2 of the ceramic member and the upper surface SW1 of the heat dissipation member 22, forming a first interface FC1 by contacting the bottom surface SF2 of the ceramic member 68, and a second interface FC2 by contacting the upper surface SW1 of the heat dissipation member 22. With this configuration, as in the first embodiment described above, it is possible to ensure practically sufficient bonding strength between the ceramic member 68, which is made of ceramic material, and the heat dissipation member 22, which is made of metal, without requiring brazing between the ceramic member 68 and the heat dissipation member 22.
[0088] Furthermore, in this embodiment 9, the first wiring section 71, in addition to its function as an electrical wiring section, also functions as a thermal path that guides heat from electronic components (for example, semiconductor elements 8 (Figure 1)) mounted on the surface electrode 31 toward the heat dissipation member 22. This function as a thermal path is particularly enhanced when the surface electrode 31 and the heat dissipation member 22 are connected to each other by the first wiring section 71 and the second wiring section 72.
[0089] Furthermore, since the other configurations are substantially the same as those of any of the embodiments 1 to 8 described above, the same reference numerals are used for the same or corresponding elements, and their descriptions are not repeated.
[0090] <Embodiment 10> Figure 23 is a schematic cross-sectional view showing the configuration of the heat dissipation substrate 151 according to Embodiment 10. The heat dissipation substrate 151 roughly corresponds to the package 58 (Figure 20: Embodiment 9) in which the ceramic member 68 is replaced with the ceramic member 161. In other words, the heat dissipation substrate 151 roughly corresponds to the package 58 (Figure 20: Embodiment 9) in which the frame portion 68b is omitted. Therefore, unlike the package 58 (Figure 20), the heat dissipation substrate 151 (Figure 23) does not need to have a cavity CV in which electronic components will be housed. Therefore, the ceramic member 68 (Figure 23) does not have a blind hole HS (Figure 20: Embodiment 9) corresponding to the cavity CV. The ceramic member also does not have a through hole HP (Figure 2: Embodiment 1) corresponding to the cavity CV.
[0091] The ceramic member 161 may be positioned without enclosing a virtual plane PV perpendicular to the thickness direction that is in contact with the mounting surface SM of the surface electrode 31. Furthermore, the ceramic member 161 may be positioned outside the virtual plane PV. In other words, the ceramic member 161 does not need to intersect the virtual plane PV. Both arrangements can be achieved, for example, by ensuring that the top surface SF1 of the ceramic member 61 is flat. This simplifies the manufacturing process of heat dissipation substrates used in semiconductor modules that do not require packaging, resulting in an inexpensive heat dissipation substrate. The thickness of the ceramic member 161 is, for example, 0.1 mm or more and 1 mm or less.
[0092] Furthermore, since the other components are substantially the same as those in Embodiment 9 described above, the same reference numerals are used for the same or corresponding elements, and their descriptions are not repeated.
[0093] <Embodiment 11> Figure 24 is a schematic cross-sectional view showing the configuration of a heat dissipation substrate 152 according to Embodiment 11. The heat dissipation substrate 152 has a ceramic member 162 instead of a ceramic member 161 (Figure 23). Only the ceramic member 162 is arranged between the surface electrode 31 and the adhesive layer 40 in the thickness direction. This arrangement is achieved, for example, by not incorporating any wiring into the ceramic member 162, as shown in Figure 24.
[0094] Furthermore, since the other components are substantially the same as those in Embodiment 10 described above, the same reference numerals are used for the same or corresponding elements, and their descriptions are not repeated.
[0095] According to this embodiment 11, the effect of electrically insulating the surface electrode 31 and the heat dissipation member 22 with the ceramic member 162 can be enhanced.
[0096] The multiple embodiments described above may be freely combined with one another. Although the invention has been described in detail, the above description is illustrative in all embodiments and does not limit the invention thereto. It is understood that countless modifications not illustrated can be envisioned without falling outside the scope of the invention.
[0097] 7: Mounting material 8: Semiconductor element (electronic component) 9: Wire 22: Heat dissipation member 31, 35: Surface electrode 40: Adhesive layer 51, 51M, 52-58, 59M: Package 61, 61M, 68, 161, 162: Ceramic member 71: First wiring section 71i: Inner electrode 71v: Via electrode 72: Second wiring section 90: Semiconductor module 98: Solder layer 99: Heat sink 100: Electronic device 151, 152: Heat dissipation substrate CV, CV1, CV2: Cavity FC1: First interface FC2: Second interface LY1: Ceramic layer LY2: Ceramic layer SM: Mounting surface
Claims
1. A heat dissipation substrate comprising: a surface electrode having a mounting surface on which electronic components will be mounted and a back surface opposite to the mounting surface in the thickness direction; a ceramic member made of a ceramic material having a first surface that supports the surface electrode and a second surface opposite to the first surface in the thickness direction; a heat dissipation member made of a metal sintered material having an opposing surface facing the second surface of the ceramic member; and an adhesive layer provided between the second surface of the ceramic member and the opposing surface of the heat dissipation member, forming a first interface by contacting the second surface of the ceramic member and a second interface by contacting the opposing surface, wherein the adhesive layer is made of a composite material containing both ceramic and metal, the composite material of the adhesive layer and the ceramic material of the ceramic member are sintered with each other at the first interface, and the composite material of the adhesive layer and the metal sintered material of the heat dissipation member are sintered with each other at the second interface.
2. A heat dissipation substrate according to claim 1, wherein the ceramic member is arranged without enclosing a virtual plane perpendicular to the thickness direction that is in contact with the mounting surface of the surface electrode.
3. A heat dissipation substrate according to claim 1, wherein the ceramic member is positioned off-center from a virtual plane perpendicular to the thickness direction that is in contact with the mounting surface of the surface electrode.
4. A heat dissipation substrate according to any one of claims 1 to 3, further comprising a first wiring portion embedded in the ceramic member.
5. A heat dissipation substrate according to claim 4, wherein the first wiring portion reaches the adhesive layer, and further comprises a second wiring portion that penetrates the adhesive layer to connect the first wiring portion and the heat dissipation member to each other.
6. A heat dissipation substrate according to claim 4, wherein the ceramic member includes a plurality of ceramic layers stacked in the thickness direction, and the first wiring portion includes an inner layer electrode having a portion disposed between the plurality of ceramic layers in the thickness direction, and a via electrode connecting the inner layer electrode and the back surface of the surface electrode to each other.
7. A heat dissipation substrate according to any one of claims 1 to 3, wherein only the ceramic member is disposed between the surface electrode and the adhesive layer in the thickness direction.
8. A package having a cavity in which an electronic component will be housed, comprising: a surface electrode; a ceramic member made of a ceramic material having a first surface supporting the surface electrode, a second surface opposite to the first surface in the thickness direction, and an inner surface surrounding the cavity; a first wiring portion embedded in the ceramic member; a heat dissipation member made of a metal sintered material having an opposing surface facing the second surface of the ceramic member; and an adhesive layer provided between the second surface of the ceramic member and the opposing surface of the heat dissipation member, forming a first interface by contacting the second surface of the ceramic member and a second interface by contacting the opposing surface, wherein the adhesive layer is made of a composite material including both ceramic and metal, the composite material of the adhesive layer and the ceramic material of the ceramic member are sintered with each other at the first interface, and the composite material of the adhesive layer and the metal sintered material of the heat dissipation member are sintered with each other at the second interface.
9. The package according to claim 8, wherein the first surface of the ceramic member faces the cavity.
10. The package according to claim 8, wherein the ceramic member has a frame shape with through holes corresponding to the cavity.
11. A package according to any one of claims 8 to 10, wherein the first wiring portion reaches the adhesive layer, and further comprises a second wiring portion that penetrates the adhesive layer to connect the first wiring portion and the heat dissipation member to each other.
12. A package according to any one of claims 8 to 10, wherein the ceramic member comprises a plurality of ceramic layers stacked in the thickness direction, and the first wiring portion comprises an inner layer electrode having a portion disposed between the plurality of ceramic layers in the thickness direction, and a via electrode connecting the inner layer electrode and the surface layer electrode to each other.