The dry manufacturing method for secondary battery electrodes using a fluororesin-coated current collector foil and thermocompression bonding addresses the inefficiencies of wet methods, achieving low resistance and cost-effective production.
Patent Information
- Application Number
- PCT/JP2026/016602
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-19
AI Technical Summary
The existing wet manufacturing methods for secondary battery electrodes require volatilizing and removing water and solvent, leading to poor economic efficiency, safety concerns, and increased production costs, while adding conductive additives to binders reduces adhesion and further complicates the process.
A dry manufacturing method using a current collector foil coated with a binder layer composed solely of fluororesin, which is bonded to an electrode mixture layer through thermocompression at a predetermined temperature, eliminating the need for conductive additives and ensuring strong adhesion.
This method produces electrodes with low resistance and improved productivity by eliminating the need for conductive additives, reducing production costs and simplifying the manufacturing process.
Smart Images

Figure JP2026016602_19112026_PF_FP_ABST
Abstract
Description
Current collector for secondary battery and electrode for secondary battery
[0001] The present invention relates to a current collector for secondary batteries and an electrode for secondary batteries that are excellent in productivity.
[0002] In recent years, demand for chargeable and dischargeable secondary batteries, such as those for mobile terminals, various wireless devices, electric vehicles, stationary power supplies, and secondary power storage systems, has been increasing rapidly. In such secondary batteries, the electrode used (the electrode for secondary batteries) determines the charge and discharge characteristics. Here, in a general method for manufacturing an electrode for a secondary battery, first, an electrode active material and a binder are dissolved and dispersed in water or a solvent to form an electrode slurry. Next, this electrode slurry is applied onto a current collector foil, and water or the solvent is removed by heat or the like to obtain an electrode for a secondary battery. However, such a wet manufacturing method requires volatilizing and removing water and solvent from the applied electrode slurry, which leads to poor economic efficiency and productivity, as well as concerns over worker safety and adverse environmental impacts. Regarding this problem, a technology for manufacturing electrodes for secondary batteries by a dry process that does not use electrode slurry has been developed.
[0003] In this dry manufacturing method, an electrode for a secondary battery is manufactured by bonding a current collector foil and an electrode mixture sheet. For the bonding between the current collector foil and the electrode mixture sheet, it is required to reduce the resistance value while maintaining sufficient adhesion. From such a viewpoint, as also described in the following Patent Document 1, it is common to mix a conductive auxiliary agent into the binder that joins the current collector foil and the electrode mixture sheet, so as to reduce the resistance value while ensuring adhesion.
[0004] Japanese Unexamined Patent Application Publication No. 2023-107996
[0005] However, mixing a conductive auxiliary agent into the binder lowers the adhesion, and also requires a dispersion technology and a mixing step for the conductive auxiliary agent, which causes problems of reduced productivity and increased production costs.
[0006] The present invention has been made in view of the above circumstances, and an object thereof is to provide a current collector for secondary batteries and an electrode for secondary batteries that have a low resistance value even with only a binder.
[0007] The present invention solves the above problems by (1) providing a current collector 60 for a secondary battery, characterized in that the surface of the current collector foil 50 is coated with a binder layer 40 consisting only of a binder. (2) providing the current collector 60 for a secondary battery described in (1) above, characterized in that the binder mainly consists of a fluororesin. (3) providing an electrode 80 for a secondary battery, comprising an electrode mixture layer 30 containing a carbon material and the current collector 60 for a secondary battery described in (2) above, wherein the binder layer 40 of the current collector 60 for a secondary battery bonds the electrode mixture layer 30 and the current collector foil 50, and the binder layer 40 has a fluorine atom concentration of 9% to 24% in a range of 3 μm from the interface between the current collector foil 50 and the binder layer 40. (4) The above problem is solved by providing the secondary battery electrode 80 described in (3) above, characterized in that, in a peel test in the 90° direction, aggregation and peeling of the electrode mixture layer 30 occurs before interfacial peeling of the binder layer 40. In addition, "coated" in the secondary battery current collector 60 described in (1) above means that the conditions of (4) above are satisfied when this secondary battery current collector 60 is used as the secondary battery electrode 80.
[0008] The current collector for secondary batteries according to the present invention can produce electrodes for secondary batteries with low resistance while bonding the electrode mixture layer and the current collector foil with sufficient strength, even if the binder layer does not contain a conductive additive, by performing thermocompression bonding at a predetermined temperature. This eliminates the need for a step of mixing a conductive additive into the binder, enabling improved productivity and reduced production costs.
[0009] This is a schematic cross-sectional view of a current collector and an electrode for a secondary battery according to the present invention.
[0010] The current collector 60 and electrode 80 for secondary batteries according to the present invention will be described with reference to the drawings. Here, Figure 1 is a schematic cross-sectional view of the current collector 60 and electrode 80 for secondary batteries according to the present invention. First, as shown in Figure 1(b), the current collector 60 for secondary batteries according to the present invention is constructed by coating one surface of the current collector foil 50 with a binder layer 40. In particular, in the current collector 60 for secondary batteries according to the present invention, the binder layer 40 is composed only of a binder that does not contain a conductive additive. Furthermore, as shown in Figure 1(d), the electrode 80 for secondary batteries according to the present invention is constructed by joining an electrode mixture layer 30 containing a carbon material with the current collector 60 for secondary batteries according to the present invention.
[0011] Furthermore, there are no particular limitations on the electrode mixture layer 30 of the present invention, and a sheet of well-known electrode mixtures used in general secondary batteries can be used. For example, an electrode mixture layer 30 for the negative electrode may be a mixture of graphite, which is the electrode active material and carbon material, and stretchable polytetrafluoroethylene (hereinafter referred to as PTFE). The carbon material in the negative electrode is generally prepared in a blending amount of 20 wt% to 99.9 wt%. For example, an electrode mixture layer 30 for the positive electrode may be a mixture of LFP (lithium iron phosphate) as the electrode active material, PTFE, and acetylene black as the carbon material. Here, stretchable PTFE refers to PTFE resin that becomes fibrous (fibrillated) when shear force is applied, and examples include emulsion polymerized PTFE fine powder. Furthermore, there are no particular limitations on the PTFE used as long as it is stretchable. For example, it may be a mixture of PTFE that is partially fibrillated, or it may be PTFE that is not entirely fibrillated. In other words, any PTFE that contains PTFE that becomes fibrous (fibrillated) when a certain shear force is applied can be used. In addition, a PTFE suitable for the present invention is preferably one with an average primary particle diameter of 100 nm to 450 nm, and is particularly preferably one that is approximately the same as the particle diameter of the electrode active material containing the aggregates in the aggregated state. With this configuration in which the particle diameter of the aggregated PTFE and the electrode active material (including the aggregates) are approximately the same, the dispersibility of the PTFE and the electrode active material is high, and mixing in the powder state can be performed easily and uniformly.
[0012] Furthermore, there are no particular limitations on the current collector foil 50 of the present invention. It can be appropriately selected depending on whether it is used for the positive or negative electrode, and the type of electrode active material contained in the electrode mixture layer 30. For example, well-known metal foils commonly used in secondary batteries, such as copper, nickel, titanium, aluminum, stainless steel, and their alloys, can be used. A typical example of current collector foil 50 for the negative electrode is copper foil, and a typical example of current collector foil 50 for the positive electrode is aluminum foil.
[0013] Furthermore, as mentioned above, the binder layer 40 (binder) does not contain a conductive additive (generally carbon materials are often used) and is composed solely of binder components. Examples of binders used in the present invention include fluororesin-based, carboxymethylcellulose-based, and styrene-butadiene rubber-based binders, and among these, it is particularly preferable to use one whose main component is a fluororesin such as vinylidene fluoride.
[0014] Next, a method for manufacturing the electrode 80 (negative electrode) for a secondary battery according to the present invention will be described using [Example 1].
[0015] To explain briefly, first, 97 wt% of spherical graphite with a particle size of approximately 16 μm and 3 wt% of PTFE fine powder produced by emulsion polymerization were weighed out and kneaded at 20°C, 10 Hz, and 10 minutes using a Laboplast Mill (registered trademark) manufactured by Toyo Seiki Seisakusho Co., Ltd. to prepare an electrode mixture for the negative electrode. Next, this electrode mixture was rolled between two rollers with a clearance of 400 μm maintained at 80°C to obtain a negative electrode electrode mixture sheet 30a with a thickness of approximately 200 μm, as shown in Figure 1(a).
[0016] Next, a copper foil with a thickness of 8 μm was prepared as the current collector foil 50. Then, a 12 wt% N-methyl-2-pyrrolidone solution of vinylidene fluoride as the fluororesin (hereinafter referred to as PVDF / NMP solution) was prepared. Next, the PVDF / NMP solution was coated onto the current collector foil 50 (copper foil) using a bar coater and dried at 120°C for 1 hour to form a binder layer 40. This yielded the current collector 60 (negative electrode) for a secondary battery according to the present invention, as shown in Figure 1(b).
[0017] Next, as shown in Figure 1(c), the electrode composite sheet 30a for the negative electrode was placed on the binder layer 40 of the current collector 60 (negative electrode) for the secondary battery, and pressed with a roll press while being heated to a temperature of 170°C or higher, at which the binder layer 40 (PVDF) melts. As a result, as shown in Figure 1(d), the binder layer 40 melts and softens due to the heat, and penetrates into the electrode composite sheet 30a side due to the pressure, and then hardens upon cooling. As a result, the current collector foil 50 and the electrode composite sheet 30a (electrode composite layer 30) are joined via the binder layer 40, forming the secondary battery electrode 80 (negative electrode) according to the present invention. At this time, the binder layer 40 melts and thins due to thermocompression bonding, reducing the resistance value of the binder layer 40 itself, and the electrode composite layer 30 and the current collector foil 50 are in partial contact, resulting in a low resistance value for the secondary battery electrode 80.
[0018] Next, the method for manufacturing the electrode 80 (positive electrode) for secondary batteries according to the present invention will be briefly described. First, 95 wt% of LFP (lithium iron phosphate) with a particle size of approximately 8 μm, 3 wt% of PTFE, and 2 wt% of acetylene black as a carbon material were weighed out and kneaded at 20°C, 10 Hz, and 10 minutes using a Laboplast Mill (registered trademark) manufactured by Toyo Seiki Seisakusho Co., Ltd. to prepare an electrode mixture for the positive electrode. Next, this electrode mixture was rolled between two rollers with a clearance of 400 μm maintained at 80°C to obtain a positive electrode electrode mixture sheet 30a with a thickness of approximately 200 μm, as shown in Figure 1(a).
[0019] Next, an aluminum foil with a thickness of 11 μm was prepared as the current collector foil 50. Then, a PVDF / NMP solution of 12 wt% vinylidene fluoride was prepared. Next, the PVDF / NMP solution was coated onto the current collector foil 50 (aluminum foil) using a bar coater and dried at 120°C for 1 hour to form a binder layer 40. This yielded the current collector 60 (positive electrode) for a secondary battery according to the present invention, as shown in Figure 1(b).
[0020] Next, as shown in Figure 1(c), the electrode mixture sheet 30a for the positive electrode was placed on the binder layer 40 of the current collector 60 (positive electrode) for the secondary battery, and pressed with a roll press while being heated to a temperature of 170°C or higher, at which the binder layer 40 (PVDF) melts. As a result, as shown in Figure 1(d), the binder layer 40 melts and softens due to the heat, and penetrates into the electrode mixture sheet 30a side due to the pressure, and then hardens upon cooling. As a result, the current collector foil 50 and the electrode mixture sheet 30a (electrode mixture layer 30) are joined via the binder layer 40, forming the electrode 80 (positive electrode) for the secondary battery according to the present invention. At this time, the binder layer 40 melts and thins due to thermocompression bonding, reducing the resistance value of the binder layer 40 itself, and the electrode mixture layer 30 and the current collector foil 50 are in partial contact, resulting in a low resistance value for the electrode 80 for the secondary battery.
[0021] Furthermore, the positive and negative electrodes 80 for the secondary battery, manufactured in this manner, are stacked alternately in multiple layers with separators in between, then housed in a predetermined case, and after the positive and negative terminals are connected, a well-known electrolyte is filled into the case to form a secondary battery.
[0022] [Comparative Example 1] An electrode for a secondary battery was prepared in the same manner as in [Example 1], except that 50 wt% carbon black was added to the binder as a conductive additive.
[0023] [Comparative Example 2] A negative electrode for a secondary battery was manufactured in the same manner as in [Example 1], except that the current collector 60 for the secondary battery and the electrode mixture sheet 30a were joined by pressing alone without heating.
[0024] [Comparative Example 3] A negative electrode for a secondary battery was manufactured in the same manner as in [Comparative Example 1], except that the current collector 60 for the secondary battery and the electrode mixture sheet 30a were joined by pressing alone without heating.
[0025] Next, peel tests were performed on [Example 1] and [Comparative Example 1] to [Comparative Example 3]. The peel tests were conducted as 90° peel tests in accordance with JIS Z0237 2009 based on JIS K6854-1, and were carried out as follows. First, electrode test pieces were prepared by cutting the secondary battery electrodes of [Example 1] and [Comparative Example 1] to [Comparative Example 3] to a size of 1 cm x 7 cm. One end of the test piece was left unbonded to the current collector foil 50 and the electrode mixture layer 30. Next, double-sided tape was attached to a metal plate and fixed so that the current collector foil 50 was facing upwards. Next, a peel test jig was fixed to the current collector foil 50 at the unbonded end of the electrode test piece. Next, the jig was held at a 90° angle to the electrode test piece and pulled up at a constant speed of 50 mm / min. The peel state was then checked in the section from 1 cm to 6 cm from the start.
[0026] Furthermore, the volume resistivity of [Example 1] and [Comparative Example 1] to [Comparative Example 3] was obtained as follows. First, the secondary battery electrodes of [Example 1] and [Comparative Example 1] to [Comparative Example 3] were cut to 3 cm x 4 cm, and the resistance value in the thickness direction was measured. Then, the volume resistivity (Ω・cm) in the thickness direction was calculated from the obtained resistance value.
[0027] Furthermore, the atomic concentration of fluorine at the interface of the binder layer 40 in [Example 1] and [Comparative Example 1] to [Comparative Example 3] was obtained as follows. First, the secondary battery electrodes of [Example 1] and [Comparative Example 1] to [Comparative Example 3] were embedded in resin and then polished to expose the cross-section. Next, the atomic concentration of fluorine in the range from the interface between the current collector foil 50 and the binder layer 40 to the electrode mixture layer 30 side was measured quantitatively by energy-dispersive X-ray spectroscopy (EDX).
[0028] These results are shown in [Table 1]. The delamination state was evaluated as follows: delamination at the interface between the binder layer 40 and the electrode mixture layer 30 was marked with an "x", and cohesive delamination within the electrode mixture layer 30 was marked with a "○".
[0029] From the peel test results in [Table 1], peeling was observed at the interface between the binder layer 40 and the electrode mixture layer 30 in the electrode test pieces of [Comparative Example 2] and [Comparative Example 3], which did not undergo thermal melting. However, in the electrode test pieces of [Example 1] and [Comparative Example 1], which underwent thermocompression bonding, no peeling was observed at the interface of the binder layer 40, and instead, cohesive peeling was observed within the electrode mixture layer 30. From this, it is considered that in [Example 1] and [Comparative Example 1], which underwent thermocompression bonding, the current collector foil 50 and the electrode mixture layer 30 were firmly bonded by the binder layer 40, and the electrode mixture layer 30 ruptured and peeled off before the bonded interface. Conversely, in [Comparative Example 2] and [Comparative Example 3], which did not undergo thermal melting, the adhesion by the binder layer 40 was weak, and it is considered that peeling occurred at the interface. From this, it can be seen that by performing thermocompression bonding at a predetermined temperature, the current collector foil 50 and the electrode mixture layer 30 are firmly bonded by the binder layer 40.
[0030] Next, from the volume resistivity (Ω·cm) results, [Example 1], [Comparative Example 1], and [Comparative Example 3] showed resistivity values of 57 Ω·cm, 47 Ω·cm, and 35 Ω·cm, respectively, which are equivalent to or lower than those of [Example 1]. However, [Comparative Example 2], which does not contain a conductive additive and does not undergo thermocompression bonding, showed a remarkably high volume resistivity of 9631 Ω·cm compared to the others. From this, it can be seen that even a binder layer 40 without a conductive additive can have its resistance reduced by performing thermocompression bonding at a predetermined temperature, as in [Example 1], and can achieve a volume resistivity comparable to that of [Comparative Example 1] and [Comparative Example 3], which contain a conductive additive.
[0031] Next, from the measurement results of the atomic number concentration of fluorine, Comparative Example 2, which did not involve thermal melting or the use of a conductive additive, showed a high atomic number concentration of 24.4% because a layer consisting only of the binder layer 40 was present at the interface. Comparative Examples 1 and 3, on the other hand, contained a conductive additive in the binder layer 40, resulting in a relatively lower atomic number concentration of fluorine at 8.5% and 8.7%, respectively. Example 1, which did not contain a conductive additive but underwent penetration by thermal melting, showed a relatively lower atomic number concentration of fluorine at 13.2%, similar to Comparative Examples 1 and 3, as the binder layer 40 components penetrated towards the electrode mixture layer 30. However, at an atomic number concentration of fluorine of 20%, the binder layer 40 is compressed by about 80%, and a thin binder layer 40 exists in parts. In these parts, electrons may jump over the binder layer 40 and conduct electricity, potentially resulting in a volume resistivity of 100 Ω·cm or less. Therefore, in the secondary battery electrode 80 according to the present invention, the atomic concentration of fluorine in the range from the interface of the binder layer 40 to the electrode mixture layer 30 side up to 3 μm is set to 9% to 24%.
[0032] As described above, the current collector 60 for secondary batteries according to the present invention can produce a secondary battery electrode 80 with low resistance while bonding the electrode mixture layer 30 and the current collector foil 50 with sufficient strength, even if the binder layer 40 does not contain a conductive additive, by performing thermocompression bonding at a predetermined temperature. This eliminates the need for a step of mixing a conductive additive into the binder, making it possible to improve productivity and reduce production costs.
[0033] Furthermore, the materials, mixing ratios, manufacturing methods, manufacturing procedures, and layer thicknesses of the current collector 60, electrode 80, electrode mixture layer 30, binder layer 40, and current collector foil 50 for the secondary battery shown in this example are merely examples. Necessary procedures may be added as appropriate, and the invention can be modified without departing from the spirit of the present invention.
[0034] 30 Electrode mixture layer 40 Binding layer 50 Current collector foil 60 Current collector for secondary battery 80 Electrode for secondary battery
Claims
1. A current collector for a secondary battery, characterized in that the surface of the current collector foil is coated with a binder layer consisting solely of a binder.
2. The current collector for a secondary battery according to claim 1, characterized in that the binder is mainly composed of fluororesin.
3. An electrode for a secondary battery comprising an electrode mixture layer containing a carbon material and a current collector for a secondary battery as described in claim 2, wherein the binder layer of the current collector for a secondary battery bonds the electrode mixture layer and the current collector foil, and the binder layer has a fluorine atom concentration of 9% to 24% in a range of 3 μm from the interface between the current collector foil and the binder layer.
4. The electrode for a secondary battery according to claim 3, characterized in that, in a peel test in the 90° direction, aggregation and delamination of the electrode mixture layer occurs before interfacial delamination of the binder layer.