Mixed composition, and film, optical component, and image display device using same
The mixed composition with a polymer, polymerizable monomer, and generator enhances clarity of refractive index boundaries by controlled polymerization and diffusion, addressing the issue of unclear boundaries in existing optical components.
Patent Information
- Application Number
- PCT/JP2026/016638
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-19
AI Technical Summary
Existing compositions for forming optical components with regions of different refractive indices suffer from unclear boundaries between these regions.
A mixed composition comprising a polymer with a refractive index of 1.59 or less, a polymerizable monomer with a refractive index of 1.60 or more, and a photoacid or photobase generator, where the monomer has two or more reactive groups for ring-opening polymerization, with a specific ratio and structural components to enhance clarity of refractive index boundaries.
The composition improves the clarity of boundaries between regions with different refractive indices by controlled polymerization and diffusion of monomers, resulting in a larger refractive index difference and clearer boundaries.
Smart Images

Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003 
Figure JPOXMLDOC01-APPB-C000004
Abstract
Description
Mixed composition, film using the same, optical component, and image display device.
[0001] The present invention relates to a mixed composition, a film using the same, an optical component, and an image display device.
[0002] In image display devices, diffraction gratings and holographic optical elements are sometimes used as optical components. As a material for forming such optical components, for example, Patent Document 1 below discloses a composition (holographic recording medium) containing polyvinyl acetate (SN-55T) with a refractive index of 1.47 as a binder resin, bisphenoxyethanol full orange acrylate (EA-0200) as a radical polymerizable monomer, and 4-isopropyl-4'-methyldiphenyliodonium tetrakis (pentafluorophenyl) borate (onium salt-based initiator) as an initiator.
[0003] Patent Document 2 below discloses a composition (holographic recording medium) comprising polybutyl methacrylate with a refractive index of 1.48, 1,2-epoxy-1,2,3,4-tetrahydronaphthalene with a refractive index of 1.58, and cyclopentadienylcumene iron(II) hexafluorophosphate as an acid generator.
[0004] International Publication No. 2022 / 153617, JP Publication No. 11-512847
[0005] However, both the composition described in Patent Document 1 and the composition described in Patent Document 2 had room for improvement in terms of the clarity of the boundaries between regions with different refractive indices when forming a film having regions with different refractive indices within the plane.
[0006] Therefore, the present invention aims to provide a mixed composition that can improve the clarity of the boundaries between regions with different refractive indices when a film having regions with different refractive indices in its surface is formed.
[0007] To solve the above problems, the present invention provides the following mixed compositions, a film using the same, an optical component and an image display device. [1] A mixed composition comprising a polymer having a refractive index of 1.59 or less at the wavelength of sodium D lines at 25°C, a polymerizable monomer having a refractive index of 1.60 or more at the wavelength of sodium D lines at 25°C, and a component comprising a photoacid generator or a photobase generator, wherein the polymerizable monomer has two or more reactive groups that undergo a ring-opening polymerization reaction with an acid or base generated from the component, and the amount of polymerizable monomer blended with 100 parts by mass of the polymer is 40 parts by mass or more and 500 parts by mass or less. [2] The mixed composition according to [1], wherein the polymerizable monomer further comprises at least one ring structure, a divalent linking group is interposed between the ring structure and the reactive group, the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles, and the reactive group is an epoxy group or a thiirane group. [3] The mixed composition according to [1], wherein the polymerizable monomer further has at least one ring structure, a sulfur atom or a nitrogen atom is interposed between the ring structure and the reactive group, and the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles. [4] The mixed composition according to [1], wherein the reactive group of the polymerizable monomer is a thiirane group. [5] The mixed composition according to [1], wherein the molecular weight of the polymerizable monomer is 300 or more. [6] The mixed composition according to [1], wherein the weight-average molecular weight of the polymer is 50,000 or less. [7] The mixed composition according to [1], wherein the repeating unit of the polymer is an aromatic ring. [8] A film comprising the mixed composition according to any one of [1] to [7]. [9] A film obtained using the mixed composition according to any one of [1] to [7], wherein the film has two or more regions with different refractive indices in its plane.
[10] The film according to [9], wherein the refractive index difference between the regions is 0.001 or more.
[11] An optical component comprising the film according to [8] or [9]. Image display device having the optical components described in
[12] and
[11] .
[0008] According to the present invention, it is possible to provide a mixed composition that can improve the clarity of the boundary between regions with different refractive indices when a film having regions with different refractive indices in its surface is formed, as well as a film using the same, an optical component, and an image display device.
[0009] This is a schematic plan view showing one embodiment of the film of the present invention. This is a schematic diagram showing a light guide plate type AR glasses, which is one embodiment of the image display device of the present invention.
[0010] Hereinafter, an embodiment of the present invention will be described in detail, with reference to the drawings as appropriate. [Mixed Composition] The mixed composition of the present invention comprises a polymer having a refractive index of 1.59 or less at the wavelength of sodium D lines at 25°C, a polymerizable monomer having a refractive index of 1.60 or more at the wavelength of sodium D lines at 25°C, and a component (hereinafter also referred to as "component A") consisting of a photoacid generator or a photobase generator. The polymerizable monomer has two or more reactive groups that undergo ring-opening polymerization with an acid or base generated from component A, and the amount of polymerizable monomer blended with 100 parts by mass of polymer is 40 parts by mass or more and 500 parts by mass or less. According to the mixed composition of the present invention, when a film having regions with different refractive indices (for example, exposed and unexposed regions) in a plane is formed, the clarity of the boundary between regions with different refractive indices can be improved.
[0011] The reason why the mixed composition of the present invention produces the above-mentioned effects is not entirely clear, but the inventors surmise that it is as follows. That is, for example, when the mixed composition of the present invention is exposed to light, the acid or base generated from component A causes a ring-opening polymerization reaction between the reactive groups of the polymerizable monomers, polymerizing the polymerizable monomers in the exposed area and reducing the concentration of the polymerizable monomers. At this time, since polymerizable monomers move easily within the polymer, polymerizable monomers present in the unexposed area easily diffuse and migrate to the exposed area over time, and the migrated polymerizable monomers polymerize one after another. In this way, the concentration of polymerizable monomers decreases sufficiently in the unexposed area, while the concentration of polymerized polymers of polymerizable monomers increases in the exposed area. As a result, a film having regions with different refractive indices (exposed and unexposed areas) is formed on the surface, and the refractive index difference between the regions with different refractive indices can be made larger, thereby improving the clarity of the boundary between the regions with different refractive indices.
[0012] The mixed composition of the present invention will be described in detail below.
[0013] <Polymer> The refractive index of the polymer contained in the mixed composition of the present invention at 25°C at the wavelength of the sodium D line (589 nm) is 1.59 or less. The refractive index of the polymer is the value measured by the minimum angle deviation method, Abbe refractometer, spectroscopic ellipsometry, or from the reflection spectrum of the polymer coating film on the substrate. The method for calculating from the reflection spectrum of the polymer coating film on the substrate is as follows: For a substrate on which a polymer coating film has been formed, the transmission spectrum and reflection spectrum at wavelengths from 300 nm to 800 nm are measured using a visible ultraviolet spectrophotometer (e.g., "V-650" manufactured by JASCO Corporation) with an integrating sphere unit (e.g., "ISV-922" manufactured by JASCO Corporation). Next, the true reflectance spectrum is obtained by smoothing the transmission spectrum and reflectance spectrum by subtracting the increase or decrease due to interference in the reflectance spectrum. From the value of the sodium D line (wavelength 589 nm) at 25°C and the refractive index of the substrate, the refractive index of the polymer coating film at 25°C (wavelength 589 nm) is calculated based on Fresnel's formula (e.g., Hecht Optics I, 5th edition, Maruzen Publishing, 2018, pp. 209-226). This allows us to determine the refractive index of the polymer coating film at the wavelength of the sodium D line (wavelength 589 nm) at 25°C. The refractive index of the polymer may be less than 1.59 or 1.58 or less. A refractive index of 1.59 or less allows for a larger refractive index difference between regions with different refractive indices formed within the film surface, thereby improving the clarity of the boundaries between regions with different refractive indices. Alternatively, the refractive index of the polymer may be 1.40 or higher, 1.46 or higher, 1.48 or higher, 1.50 or higher, 1.51 or higher, 1.52 or higher, or 1.55 or higher.
[0014] The polymer is not particularly limited as long as it has a refractive index of 1.59 or less at a sodium D-line wavelength of 589 nm at 25°C. The repeating units of the polymer may or may not have aromatic rings, but it is preferable that they do. In this case, the compatibility between the polymerizable monomer and the polymer can be improved. In particular, if the polymerizable monomer has at least one ring structure selected from the group consisting of aromatic rings and heterocycles, the compatibility between the polymerizable monomer and the polymer can be further improved, so that the polymerizable monomer can move more easily within the polymer, and as a result the clarity of the boundary can be improved. Examples of aromatic rings include benzene rings, naphthalene rings, anthracene rings, and fluorene rings. Among these, benzene rings are more preferable from the viewpoint of easily lowering the refractive index of the polymer. When the repeating units of the polymer have aromatic rings, the number of aromatic rings may be at least one, but it is preferable that there be two or more. In this case, the compatibility between the polymerizable monomer and the polymer can be effectively improved. The number of aromatic rings may be six or less, four or less, or three or less. A heterocycle is a ring structure in which an atom other than carbon (e.g., nitrogen, oxygen, sulfur, etc.) is included as part of the ring. Examples of heterocycles include pyridine rings, furan rings, thiophene rings, indole rings, pyrrole rings, imidazole rings, piperidine rings, quinoline rings, isoquinoline rings, and pyrimidine rings, as well as rings in which an aromatic ring is fused to one of these rings. The polymer may or may not contain an ester bond (-COO-), but it is preferable that it contains an ester bond. In this case, it becomes easier to adjust the compatibility with the reactive group of the polymerizable monomer and to lower the refractive index of the polymer. In particular, it is preferable that the repeating unit of the polymer is a repeating unit having an aromatic ring and an ester bond, or a repeating unit having an aromatic ring, an ester bond, and an alicyclic structure. In this case, the compatibility between the polymer and the polymerizable monomer is improved and the refractive index of the polymer can be lowered. Examples of such polymers include aromatic polycarbonates and aromatic polyester diols, but the polymer is not limited to these. These can be used individually or in combination of two or more.Examples of aromatic polycarbonates include those containing a bisphenol A structure or a bisphenol Z structure in the main chain. Examples of commercially available aromatic polycarbonates include PCZ-200, FPC-2136, and RX-9137P from Mitsubishi Gas Chemical Co., Ltd. Examples of aromatic polyester diols include polyhexamethylene isophthalate diol, polybutylene terephthalate diol, and polyneopentyl terephthalate diol. Examples of commercially available aromatic polyester diols include Byron 200, Byron 600, and Byron 630 from Toyobo Co., Ltd. Polymers whose repeating units do not have aromatic rings are not particularly limited as long as their refractive index is 1.59 or less, and examples include, but are not limited to, polyvinyl acetate (PVAC), polyvinyl alcohol (PVA), and polyethylene. These can be used individually or in combination of two or more.
[0015] The weight-average molecular weight (hereinafter also referred to as "Mw") of the polymer is not particularly limited, but is preferably 50,000 or less. When the Mw of the polymer is 50,000 or less, the viscosity of the mixed composition decreases, and polymerizable monomers migrate more easily from the unexposed areas to the exposed areas during exposure. Mw refers to the value measured by GPC using standard polystyrene as the molecular weight standard substance. The Mw of the polymer is more preferably 45,000 or less. The Mw of the polymer may be 1,000 or more, 5,000 or more, 6,000 or more, 7,000 or more, 8,000 or more, 9,000 or more, 10,000 or more, 15,000 or more, 20,000 or more, 25,000 or more, or 30,000 or more, 35,000 or more, or 40,000 or more. When the Mw of the polymer is 1,000 or more, the polymer does not move easily even when the mixed composition is exposed. The Mw of the polymer is preferably 9,000 or more. In this case, phase separation is less likely to occur in the film obtained using the mixed composition, making it easier to suppress film whitening.
[0016] <Polymerizable Monomers> The refractive index of polymerizable monomers at 25°C at the wavelength of the sodium D line (589 nm) is 1.60 or higher. When the refractive index of polymerizable monomers is 1.60 or higher, the refractive index difference between regions with different refractive indices (e.g., exposed and unexposed areas) can be increased when forming a film with regions with different refractive indices in the plane, thereby improving the clarity of the boundaries between regions with different refractive indices. The refractive index of polymerizable monomers refers to the value measured from the minimum angle declination method, Abbe refractometer, spectroscopic ellipsometry, or the reflectance spectrum of a polymerizable monomer coating film on a substrate. The method for calculating the refractive index from the reflectance spectrum of a polymerizable monomer coating film on a substrate is as follows: For a substrate on which a polymerizable monomer coating film has been formed, the transmission spectrum and reflectance spectrum from 300 nm to 800 nm are measured using a visible ultraviolet spectrophotometer with an integrating sphere unit (e.g., JASCO Corporation, "ISV-922") (e.g., JASCO Corporation, "V-650"). Next, the true reflection spectrum, obtained by smoothing the transmission and reflection spectra by subtracting the increase or decrease due to interference in the reflection spectrum, is used to calculate the refractive index of the polymerizable monomer coating film at the wavelength of the sodium D line (589 nm) at 25°C based on the value at 589 nm and the refractive index of the substrate, using Fresnel's formula (for example, Hecht Optics I, 5th edition, Maruzen Publishing, 2018, pp. 209-226). This allows us to determine the refractive index of the polymerizable monomer coating film at the wavelength of the sodium D line (589 nm) at 25°C. The refractive index of the polymerizable monomer is preferably 1.65 or higher, more preferably 1.69 or higher, and even more preferably 1.70 or higher. The refractive index of the polymerizable monomer may be 1.90 or lower, 1.85 or lower, or 1.80 or lower. By having the refractive index of the polymerizable monomer within the above range, the refractive index difference between regions with different refractive indices formed within the film surface can be made larger, and the clarity of the boundaries between regions with different refractive indices can be further improved.
[0017] Polymerizable monomers are monomers having two or more reactive groups. A reactive group is a group that undergoes a ring-opening polymerization reaction with an acid or base generated from component A as described above. In this invention, the ring-opening polymerization that reacts with an acid or base generated from component A is ring-opening polymerization using cationic polymerization or anionic polymerization. Among these, ring-opening polymerization using cationic polymerization is preferred because the polymerization rate tends to be slower, and it is easier to improve the clarity of the boundary between regions with different refractive indices. Examples of reactive groups that undergo ring-opening polymerization include epoxy groups, oxetane groups, oxazoline groups, thiirane groups, lactones, imide groups, etc. Among these, epoxy groups or thiirane groups are more preferred, and thiirane groups are particularly preferred, because ring-opening polymerization is easily promoted by ring strain, and the clarity of the boundary between regions with different refractive indices can be further improved. In this case, a high refractive index derived from the high electron density of the sulfur atom can be obtained in the film obtained using the mixed composition.
[0018] Examples of polymerizable monomers having two or more reactive groups and a refractive index of 1.60 or higher include, but are not limited to, the compounds described in paragraphs 0030 to 0041 of Japanese Patent Application Publication No. 2024-035818, naphthalene-type epoxy compounds (epoxy compounds having a naphthalene ring), epoxy compounds having a fluorene ring, epoxy compounds having a dinaphthophthothiophene ring, and epoxy compounds having a carbazole ring. These may be used individually or in combination of two or more. The compounds described in paragraphs 0030 to 0041 of Japanese Patent Publication No. 2024-035818 include, specifically, 1,2-bis(2,3-epithiopropylthio)naphthalene, 1,3-bis(2,3-epithiopropylthio)naphthalene, 1,4-bis(2,3-epithiopropylthio)naphthalene, 1,6-bis(2,3-epithiopropylthio)naphthalene, 1,7-bis(2,3-epithiopropylthio)naphthalene, 1,8-bis(2, Examples include 3-epithiopropylthio)naphthalene, 2,3-bis(2,3-epithiopropylthio)naphthalene, 2,6-bis(2,3-epithiopropylthio)naphthalene, 2,7-bis(2,3-epithiopropylthio)naphthalene, 2,7-bis(2,3-epithiobutylthio)naphthalene, 2,7-bis(2,3-epithiopentylthio)naphthalene, and 2,7-bis(2,3-epithiohexylthio)naphthalene.
[0019] Examples of commercially available epoxy compounds containing a naphthalene ring in the molecule include the trade names "Epiclon HP4032," "HP4032D," "HP-4032SS," "HP4700," "HP4710," "HP4770," and "HP5000" (all manufactured by DIC Corporation), and "DGOBINL" (all manufactured by Sugai Chemical Industry Co., Ltd.). Furthermore, examples of commercially available epoxy compounds containing a fluorene ring in the molecule include the trade name "EG-200" (all manufactured by Osaka Gas Chemical Co., Ltd.). In addition, examples of epoxy compounds containing a dinaphthophthothiophene ring in the molecule include "2,12-DGODNT" (all manufactured by Sugai Chemical Industry Co., Ltd.).
[0020] A polymerizable monomer may or may not have at least one more ring structure, but it is preferable that the polymerizable monomer has at least one ring structure. Having at least one ring structure in the polymerizable monomer can improve compatibility with the polymer, and as a result, improve the clarity of the boundary between regions with different refractive indices. Furthermore, it is preferable that the polymerizable monomer has a ring structure having aromaticity according to Hückel's rule. That is, it is preferable that it has a ring structure having 4N + 2 (where N is an integer of 1 or more) π electrons. It is preferable that N is 2 or more. In the polymerizable monomer, a divalent linking group is interposed between the ring structure and the reactive group, and it is preferable that the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles, and the reactive group is an epoxy group or a thiirane group. In this case, it is possible to achieve both a high refractive index derived from the ring structure and high compatibility with the polymer derived from the divalent linking group and the reactive group. Examples of divalent linking groups include -S-, -O-, -CH2-, and -CO-. In particular, -S- and -O- are preferred from the viewpoint of improving the clarity of the boundary between regions with different refractive indices. When the reactive group and the divalent linking group have elements of the same group, it is easier to match the polarization within the monomer molecule and easier to control the ring-opening reaction. Therefore, when the reactive group is a thiirane group, it is preferable that the divalent linking group be -S-. Also, when the reactive group is an epoxy group, it is preferable that the divalent linking group be -O-. Examples of aromatic rings include benzene rings, naphthalene rings, anthracene rings, and fluorene rings. Among these, fused rings such as naphthalene rings, anthracene rings, and fluorene rings are more preferred, and naphthalene rings are particularly preferred. It is preferable that the aromatic ring has aromaticity according to Hückel's rule. That is, it is preferable that the aromatic ring has 4N + 2 (N is an integer of 1 or more) π electrons. It is preferable that N is 2 or more. Specific examples of aromatic rings with N 2 or more include naphthalene rings, anthracene rings, and fluorene rings. A heterocycle is a ring structure in which atoms other than carbon (for example, nitrogen, oxygen, sulfur, etc.) are included as part of the ring.Examples of heterocycles include pyridine rings, furan rings, thiophene rings, indole rings, pyrrole rings, imidazole rings, piperidine rings, quinoline rings, isoquinoline rings, and pyrimidine rings, as well as rings in which aromatic rings are fused to these rings. It is preferable that the heterocycle has aromaticity according to Hückel's rule. That is, it is preferable that the heterocycle has 4N + 2 (where N is an integer of 1 or more) π electrons. It is preferable that N is 2 or more, and more preferably 3 or more. Specific examples of heterocycles with N 2 or more include carbazole rings, benzimidazole rings, benzothiazole rings, naphthothiophene rings, and dinaphthothiophene rings. From the viewpoint of having a high refractive index, the dinaphthothiophene ring is preferred.
[0021] The polymerizable monomer may have a nitrogen atom interposed between the ring structure and the reactive group, and the ring structure may be at least one ring structure selected from the group consisting of aromatic rings and heterocycles. In this case, a high refractive index derived from the high electron density of the nitrogen atom can be obtained in the film obtained using the mixed composition. The nitrogen atom is interposed between the ring structure and the reactive group in the form of -NR-. R may be a hydrogen atom, a hydrocarbon group such as an alkyl group, or a hydrocarbon group partially substituted with a heteroatom. Examples of aromatic rings include benzene rings, naphthalene rings, anthracene rings, and fluorene rings. Among these, fused rings such as naphthalene rings, anthracene rings, and fluorene rings are more preferred, and naphthalene rings are particularly preferred. The aromatic ring preferably has aromaticity according to Hückel's rule. That is, the aromatic ring preferably has 4N + 2 (N is an integer of 1 or more) π electrons. N is preferably 2 or more. Specific examples of aromatic rings with N 2 or more include naphthalene rings, anthracene rings, and fluorene rings. Examples of heterocycles include pyridine rings, furan rings, thiophene rings, indole rings, pyrrole rings, imidazole rings, piperidine rings, quinoline rings, isoquinoline rings, and pyrimidine rings, as well as rings in which aromatic rings are fused to these rings. It is preferable that the heterocycles have aromaticity according to Hückel's rule. That is, it is preferable that the heterocycles have 4N + 2 (where N is an integer of 1 or more) π electrons. It is preferable that N be 2 or more, and more preferable that N be 3 or more. Specific examples of heterocycles with N 2 or more include carbazole rings, benzimidazole rings, benzothiazole rings, naphthothiophene rings, and dinaphthothiophene rings. Among these, the carbazole ring is particularly preferred. A heteroatom is an atom other than a carbon atom. Examples of heteroatoms include oxygen atoms, sulfur atoms, and nitrogen atoms, with nitrogen atoms or sulfur atoms being preferred heteroatoms, and nitrogen atoms being more preferred heteroatoms.
[0022] In one embodiment, the polymerizable monomer has at least one ring structure, with a sulfur atom or nitrogen atom interposed between the ring structure and the reactive group, and it is preferable that the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles, and it is more preferable that it has at least one ring structure, with a sulfur atom interposed between the ring structure and the reactive group, and the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles. When the polymerizable monomer has the above structure, it is possible to achieve both a high refractive index derived from the sulfur atom or nitrogen atom and high compatibility with the polymer derived from the ring structure.
[0023] The number of reactive groups in the polymerizable monomer may be two or more, but is preferably six or less, more preferably four or less, and even more preferably three or less. When the number of reactive groups is six or less, the refractive index difference between regions with different refractive indices (e.g., exposed and unexposed regions) can be made larger when forming a film with regions with different refractive indices in the plane, and the clarity of the boundary between regions with different refractive indices can be further improved.
[0024] The molecular weight of the polymerizable monomer is not particularly limited, but may be 200 or more, 250 or more, 300 or more, 310 or more, 320 or more, or 330 or more. Here, molecular weight refers to the average molecular weight when the polymerizable monomer has repeating units, and the average molecular weight is a value measured by methods such as LC / MS. When the molecular weight of the polymerizable monomer is 200 or more, when a film is formed that has regions with different refractive indices in its surface (e.g., exposed and unexposed regions), the refractive index difference between regions with different refractive indices can be made larger, and the clarity of the boundary between regions with different refractive indices can be improved. In addition, bleeding of the polymerizable monomer to the film surface is less likely to occur, so the clarity of the boundary between regions with different refractive indices in the film can be further improved. The molecular weight of the polymerizable monomer may be 600 or less, 550 or less, 500 or less, 450 or less, 400 or less, 390 or less, or 350 or less. When the molecular weight of the polymerizable monomer is 390 or less, the polymerizable monomer tends to move more easily from the unexposed areas to the exposed areas during partial exposure. This allows for a larger difference in refractive index between regions with different refractive indices (e.g., exposed and unexposed areas) when forming a film with regions of different refractive indices within its surface, thereby improving the clarity of the boundaries between these regions. Furthermore, it can suppress discoloration of the film when forming a film with regions of different refractive indices within its surface.
[0025] The molecular weight of the polymerizable monomer may be between 200 and 600, 250 and 550, 300 and 500, 300 and 390, 310 and 450, 320 and 400, or 330 and 390. When the molecular weight of the polymerizable monomer satisfies the above range (particularly between 300 and 390), the polymerizable monomer tends to move more easily from the unexposed areas to the exposed areas during partial exposure. This tends to increase the refractive index difference between areas with different refractive indices when forming a film with areas of different refractive indices within the plane (e.g., exposed and unexposed areas), thereby improving the clarity of the boundaries between areas with different refractive indices. Furthermore, discoloration of the film can be suppressed when forming a film with areas of different refractive indices within the plane.
[0026] The polymerizable monomer is preferably a compound represented by the following formula (A). R 1 -X 1 -Z-X 2 -R 2 (A) [In formula (A), Z represents a ring structure, X 1 and X 2 each independently represent a divalent linking group, R 1 and R 2 each independently represent a reactive group. Examples of the ring structure represented by Z include the ring structures described above. Z is preferably an aromatic ring or a heterocyclic ring. X 1 and X 2 Examples of the divalent linking group represented by include the divalent linking groups described above. X 1 and X 2 each independently is preferably a divalent group containing an oxygen atom, a sulfur atom or a nitrogen atom, and is more preferably a divalent group represented by -O-, -S-, -NR-, *1-R 11 -O-, *2-R 12 -S- or *3-R 13 -NR-. R 11 and R 12 each independently represent an alkanediyl group having 1 to 12 carbon atoms such as a methylene group, an ethylene group, and a propylene group. R 11 and R 12 each independently is preferably an alkanediyl group having 1 to 6 carbon atoms. *1, *2 and *3 each independently represent a bond to the reactive group represented by R 1 or R 2 . R represents a hydrogen atom, a hydrocarbon group such as an alkyl group, or a hydrocarbon group partially substituted with a hetero atom. The reactive groups represented by R 1 and R 2 each independently represent a group that undergoes a ring-opening polymerization reaction with an acid or base generated from Component A, and examples thereof include an epoxy group, an oxetane group, an oxazoline group, a thiirane group, a lactone, and an imide group. R 1 and R 2 each independently is preferably an epoxy group or a thiirane group. R 1 and R 2It is preferable that these are the same reactive group.
[0027] The amount of polymerizable monomer (hereinafter also referred to as "X") blended with 100 parts by mass of polymer is 40 parts by mass or more and 500 parts by mass or less. When X is 40 parts by mass or more and 500 parts by mass or less, when a film is formed having regions with different refractive indices in the plane (for example, exposed and unexposed regions), the refractive index difference between regions with different refractive indices can be made larger, and the clarity of the boundary between regions with different refractive indices can be improved. More preferably, X is 50 parts by mass or more, even more preferably 100 parts by mass or more, and particularly preferably 200 parts by mass or more. When X is 50 parts by mass or more, when a film is formed having regions with different refractive indices in the plane (for example, exposed and unexposed regions), the refractive index difference between regions with different refractive indices can be made larger, and the clarity of the boundary between regions with different refractive indices can be improved. More preferably, X is 450 parts by mass or less, more preferably 400 parts by mass or less, and particularly preferably 350 parts by mass or less. When X is 450 parts by mass or less, it facilitates the migration of polymerizable monomers from unexposed areas to exposed areas during exposure of the mixed composition. This increases the refractive index difference between areas with different refractive indices (e.g., exposed and unexposed areas) when forming a film with areas of different refractive indices within the plane, thereby improving the clarity of the boundaries between these areas. It also makes it easier to suppress discoloration of the film obtained by exposure of the mixed composition. When two or more polymers and / or polymerizable monomers are used, X is defined as the total amount of polymerizable monomers relative to 100 parts by mass of the total amount of polymers.
[0028] (Component A) Component A consists of a photoacid generator or a photobase generator. Preferably, component A consists of a photoacid generator. When component A is a photoacid generator, polymerization efficiency is good, ring-opening polymerization can proceed efficiently, and as a result, the clarity of the boundary between regions with different refractive indices can be improved. A photoacid generator is a substance that absorbs light and generates acid as an active species, thereby promoting ring-opening polymerization. Examples of photoacid generators include, but are not limited to, diazonium salt compounds, quinone diazide compounds, sulfone compounds, sulfonic acid ester compounds, quinone diazide compounds, sulfonimide compounds, iodonium salt compounds, sulfonium salt compounds, phosphonium salt compounds, and oxonium salt compounds. In the present invention, from the viewpoint of acid generation efficiency, it is preferable that at least one selected from the group of iodonium salt photoacid generators and sulfonium salt photoacid generators is used, and sulfonium salt photoacid generators are more preferable. Specific examples of iodonium salt-based photoacid generators include photoacid generators that are arsenate-type iodonium salts such as diphenyliodonium hexafluoroarsenate, di(4-chlorophenyl)iodonium hexafluoroarsenate, di(4-bromphenyl)iodonium hexafluoroarsenate, and phenyl(4-methoxyphenyl)iodonium hexafluoroarsenate; 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluorophosphate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium tri(pentafluoroethyl)trifluorophosphate (e.g., IK-1 manufactured by Sunapro Co., Ltd.), 4-methylphenyl-4-(2-methylpropyl)phenyliodonium hexafluorophosphate (e.g., IRGACURE® 250 manufactured by BASF), and bis(C) 10~14Photoacid generators that are phosphate-based iodonium salts such as alkylphenyl)iodonium hexafluorophosphate (e.g., WPI-113 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.); photoacid generators that are antimonate-based iodonium salts such as 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluoroantimonate (e.g., WPI-116 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.); iodonium salt-based photoacid generators such as IK-1FG (manufactured by Sunapro Co., Ltd.); 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrakis(pentafluorophenyl) borate, 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl) borate (e.g., BLUESIL® PI manufactured by ELKEM SILICONES). Examples of photoacid generators include, but are not limited to, borate-based iodonium salts such as 2074, and triphenyliodonium triflate. Specific examples of sulfonium salt-based photoacid generators include, but are not limited to, borate-based sulfonium salts (e.g., products manufactured by Sunapro Co., Ltd.: CPI-110B, CPI-310B, CPI-410B, etc., and Omnirad 290 manufactured by IGM Resins B.V., etc.), phosphate-based sulfonium salts (products manufactured by Sunapro Co., Ltd.: CPI-210S, VC-1S, CPI-410S, etc.), other sulfonium salt-based photoacid generators (products manufactured by Sunapro Co., Ltd.: CPI-310FG, VC-1FG, etc.), triphenylsulfonium triflate, triphenylsulfonium hexafluoroantimonate, etc. These may be used individually or in combination of two or more. Among the above photoacid generators, triphenylsulfonium hexafluoroantimonate is preferred because it has a particularly high acid generation efficiency and thus facilitates the ring-opening polymerization reaction. A photobase generator is a substance that absorbs light and generates a base as an active species, thereby promoting ring-opening polymerization. Examples of photobase generators include, but are not limited to, various compounds that generate amines, amidines, guanidines, phosphazenes, carbenes, etc., as bases.Specific examples of photobase generators include, for example, 2-benzyl-2-(dimethylamino)-1-[4-(morpholino)phenyl]-1-butanone, 2-(dimethylamino)-2-(4-methylbenzyl)-1-(4-morpholinophenyl)butan-1-one, 2-nitrobenzyl 4-hydroxypiperidine-1-carboxylate, 4,5-dimethoxy-2-nitrobenzyl 2,6-dimethylpiperidine-1-carboxylate, 1-(9,10-dioxo-9,10-dihydroanthracene-2-yl)ethylcyclohexylcarbamate, 1-(9,10-dioxo-9,10-dihydroanthracene-2-yl)ethyl 1H-imidazole-1-carboxylate, 3,4,6,7,8,9-hexahydro-2H-pyrimido[1,2-a]pyrimidine-1- Ium 2-(3-benzoylphenyl)propanoate, diaminomethaneiminium 2-(3-benzoylphenyl)propanoate, (Z)-N-(((bis(dimethylamino)methylene)amino)(isopropylamino)methylene)propane-2-aminium 2-(3-benzoylphenyl)propanoate, 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidium n-butyltriphenylborate, (Z)-{[bis(dimethylamino)methylidene]amino}-N-cyclohexyl(cyclohexylamino)methaniminium tetrakis(3-fluorophenyl)borate, 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidium 2-(3-benzoylphenyl)propionate, 9-antrylmethyl Examples include, but are not limited to, N,N-diethylcarbamate, (E)-1-piperidino-3-(2-hydroxyphenyl)-2-propen-1-one, 2-nitrophenylmethyl 4-methacryloyloxypiperidine-1-carboxylate, tetramethylguanidium tetrakis(3-fluorophenyl)borate, tetramethylguanidium tetrakis(4-fluorophenyl)borate, salts containing protonated DBU and tetrakis(3-fluorophenyl)borate anion, and salts containing benzylated DBU and tetrakis(3-fluorophenyl)borate anion. These may be used individually or in combination of two or more.Among the aforementioned photobase generators, 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidinium 2-(3-benzoylphenyl)propionate (manufactured by FUJIFILM Wako Pure Chemical Corporation, WPBG-266) is preferred due to its particularly high base generation efficiency.
[0029] The blending amount of Component A relative to 100 parts by mass of the polymerizable monomer is not particularly limited as long as it is more than 0 parts by mass, and may be 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, 3 parts by mass or more, or 4 parts by mass or more, preferably 3 parts by mass or more, and more preferably 4 parts by mass or more. When the blending amount of Component A relative to 100 parts by mass of the polymerizable monomer is 4 parts by mass or more, the clarity of the boundary between regions with different refractive indices can be further improved when a film having regions with different refractive indices in the in-plane direction (for example, exposed areas and unexposed areas) is formed. The blending amount of Component A relative to 100 parts by mass of the polymerizable monomer may be 15 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less. When two or more types of Component A are used, the sum of the blending amounts of these Components A is defined as the blending amount of Component A.
[0030] In the mixed composition, the blending amount of Component A relative to the total of 100 parts by mass of the polymer and the polymerizable monomer is preferably 1 part by mass or more and 5 parts by mass or less, more preferably 2 parts by mass or more and 4 parts by mass or less.
[0031] (Solvent) The mixed composition of the present invention may further contain a solvent. When the mixed composition of the present invention further contains a solvent, the viscosity of the mixed composition of the present invention can be reduced, and coating is facilitated. For this reason, formation of the film of the present invention is facilitated. The solvent is preferably one capable of dissolving the polymer and the polymerizable monomer, and is preferably a solvent inert to the photopolymerization reaction of the polymerizable monomer.
[0032] Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide-based solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These solvents may be used alone or in combination of two or more thereof.
[0033] The content of the solvent is preferably 50 to 98% by mass based on 100% by mass of the total amount of the mixed composition. In other words, the content of the solid content in the mixed composition is preferably 2 to 50% by mass, more preferably 5 to 30% by mass. When the content of the solid content is 50% by mass or less, the viscosity of the mixed composition decreases, so that the thickness of the film becomes substantially uniform, and the film tends to be less likely to have unevenness. Further, the content of the solid content can be determined in consideration of the thickness of the film to be produced.
[0034] (Additives) The mixed composition of the present invention may further contain additives such as a polymerization inhibitor, a sensitizer, a leveling agent, a stabilizer, a surfactant, an antistatic agent, a lubricant, an antifouling agent, an ultraviolet absorber, an antioxidant, and a dispersant, as necessary.
[0035] [Film] In one embodiment, the film of the present invention contains the mixed composition described above. The film containing the mixed composition described above refers to a film that has been coated with the mixed composition described above onto a glass substrate or the like, but has not been exposed to light. The film containing the mixed composition described above makes it possible to improve the clarity of the boundaries between regions with different refractive indices when a film having regions with different refractive indices in its plane is formed. For example, when a part of the film of the present invention is exposed to light to form regions with different refractive indices (exposed and unexposed regions) in its plane, the difference in refractive index between these regions can be increased. As a result, the clarity of the boundaries between regions with different refractive indices can be improved, and excellent diffraction characteristics can be obtained.
[0036] In one embodiment, the film of the present invention is obtained using the mixed composition described above. The film obtained using the mixed composition described above refers to a film obtained by applying the mixed composition described above to a glass substrate or the like, and then exposing at least a portion of it to light. The film obtained using the mixed composition described above has two or more regions with different refractive indices in its surface. Here, the regions with different refractive indices are adjacent to each other. Furthermore, the regions with different refractive indices may be arranged alternately. For example, regions with high refractive indices and regions with low refractive indices may be arranged alternately.
[0037] Figure 1 is a schematic plan view showing one embodiment of the film of the present invention, and is a view of the film 1 in the direction of its thickness. In the film 1, regions with a high refractive index 2 and regions with a low refractive index 3 are arranged alternately in a stripe pattern along direction X.
[0038] In film 1, the width d1 of the high refractive index region 2 and the width d2 of the low refractive index region 3 may be the same or different. The width d1 of multiple regions 2 may be the same or different. The width d2 of multiple regions 3 may be the same or different. The widths of the high refractive index region 2 or the low refractive index region 3 may be constant or different. If they are not constant, the maximum width of each region 2 or 3 is taken as the width d1 or d2. The width d1 of the high refractive index region 2 and the width d2 of the low refractive index region 3 are preferably 0.1 μm to 50 μm, more preferably 0.25 μm to 25 μm, and even more preferably 0.5 μm to 10 μm. Film 1 may have other regions, such as a boundary, between the high refractive index region 2 and the low refractive index region 3, and the width of these other regions may be, for example, 0 μm to 50 μm.
[0039] The film of the present invention makes it possible to increase the refractive index difference between regions 2 and 3 with different refractive indices when regions with different refractive indices are formed in the plane. As a result, the clarity of the boundary between regions with different refractive indices can be improved, and excellent diffraction characteristics can be obtained. The refractive index difference between regions with different refractive indices (hereinafter also referred to as "Δn") is not particularly limited as long as it is greater than 0, but it is preferably 0.001 or more. In this case, since the refractive index difference between regions with different refractive indices when regions with different refractive indices are formed in the plane is sufficiently large, excellent diffraction characteristics can be obtained. Examples of films obtained using the above-described mixed composition include a film obtained by exposing a part of the above-described mixed composition, and a film obtained by exposing a part of the above-described mixed composition to form exposed and unexposed parts, and then exposing the unexposed part. Δn is more preferably 0.005 or more, even more preferably 0.015 or more, and still more preferably 0.030 or more. Δn may also be 0.100 or less, 0.080 or less, 0.060 or less, 0.050 or less, or 0.040 or less, or 0.035 or less. Δn can be determined, for example, based on the diffraction efficiency (%) and the following formula (B).
[0040] (In the above formula (B), d is the thickness of the film (nm), λ is the wavelength of the incident light (nm), and θ0 is the angle of incidence of the incident light (°).) The diffraction efficiency is calculated based on the intensity of the incident light P0, the intensity of the emitted diffracted light P1, and the following formula (A). Diffraction efficiency (%) = 100 × P1 / P0 ... (A) When the film of the present invention has an exposed area and an unexposed area, the unexposed area has a lower refractive index than the exposed area because the concentration of polymerizable monomer polymer is lower than that of the exposed area. Even if the unexposed area is later exposed to become a second exposed area, the second exposed area will have a lower refractive index than the exposed area. The above-mentioned exposed area and unexposed area can be formed by a photomask having an aperture or by two-beam interference exposure using laser light.
[0041] [Optical component] The optical component of the present invention comprises the above-described film. The above-described film can sufficiently increase the refractive index difference between regions with different refractive indices when regions with different refractive indices (e.g., exposed and unexposed regions) are formed in its surface, thereby improving the clarity of the boundary between regions with different refractive indices. Therefore, the optical component of the present invention provides excellent diffraction characteristics. The thickness of the above-described film is not particularly limited, but is preferably 1 to 50 μm. From the viewpoint of reducing the weight of the optical component, the thickness of the above-described film is more preferably 1 to 20 μm, and even more preferably 1 to 10 μm. The optical component of the present invention may further comprise a substrate that supports the above-described film. Examples of substrates include transparent substrates (e.g., glass substrates and resin substrates) and opaque substrates (silicon substrates, glass epoxy substrates). When forming an optical component comprising the above-described film, the substrate is preferably a glass substrate from the viewpoint of excellent total reflectivity. The thickness of the substrate is not particularly limited, but is preferably 10 to 8000 μm. When the substrate is a glass substrate or a resin substrate, the thickness of the substrate is more preferably 100 μm to 1000 μm. The refractive index of the above substrate at 25°C at the wavelength of sodium d-lines is preferably 1.5 or higher from the viewpoint of excellent total reflectivity. The refractive index may also be 1.7 or higher, or 1.9 or higher. Examples of optical components include diffraction gratings and holographic optical elements (HOEs).
[0042] [Image Display Device] The image display device of the present invention has the above-mentioned optical components. In one embodiment, the image display device of the present invention comprises an optical component composed of a diffraction grating and a light guide plate that guides light incident through the optical component. In this case, since excellent diffraction characteristics are obtained by the optical component, leakage of light guided by the light guide plate is suppressed, light is guided efficiently, and the quality of the displayed image can be improved. The image display device of the present invention may further comprise an optical component composed of a diffraction grating that emits light from the light guide plate. Preferably, this diffraction grating is also composed of the optical component of the present invention. In this case, since excellent diffraction characteristics are obtained by the optical component of the present invention, light is efficiently emitted from the light guide plate by the diffraction grating. Therefore, the image display device of the present invention can further improve the quality of the displayed image. The light guide plate is composed of a transparent plate. Examples of transparent plates include glass substrates and resin substrates. In one embodiment, the image display device of the present invention further comprises an image projection unit that projects image light onto the optical component. Examples of image projection units include microprojectors equipped with microdisplays. The microprojector may further include a lens between the microdisplay and the optical component that adjusts the spread of the image light from the microdisplay and directs it into the optical component. More preferably, the image display device may be a virtual image display device such as AR glasses using a light guide plate, a holographic screen, a head-mounted display, or a head-up display.
[0043] Figure 2 is a schematic diagram showing an AR glasses using a light guide plate, which is one embodiment of the image display device of the present invention. The image display device 100 shown in Figure 2 comprises an optical component 10 composed of a diffraction grating, a light guide plate 20 that guides light incident from the optical component 10, an optical component 30 composed of a diffraction grating that emits light from the light guide plate 20, and a microprojector as an image projection unit 40 that projects image light onto the optical component 10. As the diffraction grating, for example, the film 1 shown in Figure 1 can be used. The image projection unit 40 comprises a microdisplay 41 and a lens 42. The lens 42 is positioned between the microdisplay 41 and the optical component 10. Light propagates through the light guide plate 20 by total internal reflection. When the optical components 10 and 30 are composed of diffraction gratings, they have excellent diffraction characteristics, so with the image display device 100, leakage of light propagating through the light guide plate 20 is suppressed, back-image distortion is suppressed, and the quality of the image is also improved.
[0044] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0045] (Example 1) 100 parts by mass of aromatic polycarbonate (PCZ-200, manufactured by Mitsubishi Gas Chemical Co., Ltd., weight-average molecular weight Mw 44000), which has a refractive index of 1.58 at the wavelength of sodium D line at 25°C, 233 parts by mass of polymerizable monomer (1,6-bis(2,3-epithiopropylthio)naphthalene, molecular weight 336.54, reactive group: thiirane group), which has a refractive index of 1.70 at the wavelength of sodium D line at 25°C and is represented by the following formula (2), and triphenylsulfonium hexafluoroantimonate (VC-1S, manufactured by Sunapro Co., Ltd.), which is a photoacid generator (component A), were mixed. A solvent (propylene glycol monomethyl ether acetate) was added to the resulting mixture to dilute it so that the solid content was 30% by mass, and a mixed composition was prepared. At this time, the amount of component A blended with 100 parts by mass of the total of polymer and polymerizable monomer was 3.0 parts by mass. This mixed composition was spin-coated onto a glass substrate and dried to obtain a film.
[0046]
[0047] (Example 2) A mixed composition was prepared in the same manner as in Example 1, except that the amount of polymerizable monomer per 100 parts by mass of polymer was changed from 233 parts by mass to 100 parts by mass. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0048] (Example 3) A mixed composition was prepared in the same manner as in Example 1, except that the weight-average molecular weight Mw of the polymer was changed from 44,000 to 8,000. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0049] (Example 4) A mixed composition was prepared in the same manner as in Example 1, except that the amount of polymerizable monomer per 100 parts by mass of polymer was changed from 233 parts by mass to 500 parts by mass. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0050] (Example 5) A mixed composition was prepared in the same manner as in Example 1, except that the amount of polymerizable monomer per 100 parts by mass was changed from 233 parts by mass to 43 parts by mass. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0051] (Example 6) A mixed composition was prepared in the same manner as in Example 1, except that the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.69 and represented by the following formula (3) (2,12-DGODNT, manufactured by Sugai Chemical Industry Co., Ltd., molecular weight 428.50, reactive group: epoxy group). A film was then obtained using this mixed composition in the same manner as in Example 1.
[0052]
[0053] (Example 7) A mixed composition was prepared in the same manner as in Example 1, except that the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.65 and represented by the following formula (4) (DGOBINL, manufactured by Sugai Chemical Industry Co., Ltd., molecular weight 398.15, reactive group: epoxy group). A film was then obtained using this mixed composition in the same manner as in Example 1.
[0054]
[0055] (Example 8) A mixed composition was prepared in the same manner as in Example 1, except that the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.60 and represented by the following formula (5) (DIC Corporation HP-4032SS, molecular weight 272.30, reactive group: epoxy group). A film was then obtained using this mixed composition in the same manner as in Example 1.
[0056]
[0057] (Example 9) A mixed composition was prepared in the same manner as in Example 1, except that the polymer was changed from aromatic polycarbonate to polyvinyl acetate (PVAC, weight-average molecular weight Mw 15000) with a refractive index of 1.46 and represented by the following formula (6), and the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.65 and represented by the above formula (4) (DGOBINL, manufactured by Sugai Chemical Industry Co., Ltd., molecular weight 398.15, reactive group: epoxy group). A film was then obtained using this mixed composition in the same manner as in Example 1.
[0058]
[0059] (Comparative Example 1) A mixed composition was prepared in the same manner as in Example 1, except that the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.69 and represented by the following formula (7) (2,12-DODNTMA, manufactured by Sugai Chemical Industry Co., Ltd., molecular weight 424.47, reactive group: -), and NCI-730 manufactured by ADEKA Corporation (3.0 parts by mass per 100 parts by mass of the total of the polymer and polymerizable monomer) was used as a photoradical polymerization initiator instead of component A. A film was then obtained using this mixed composition in the same manner as in Example 1. Note that "reactive group" refers to "a group that undergoes a ring-opening polymerization reaction with an acid or base generated from component A as described above," and since the polymerizable monomer in Comparative Example 1 does not have such a reactive group, the reactive group was set to "-". For the same reason, the reactive group was set to "-" in the following Comparative Examples 2 to 5.
[0060]
[0061] (Comparative Example 2) A mixed composition was prepared in the same manner as in Example 1, except that the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.63 and represented by the following formula (8) (BINLA, manufactured by Sugai Chemical Industry Co., Ltd., molecular weight 394.43, reactive group: -), and NCI-730, manufactured by ADEKA Corporation (3.0 parts by mass per 100 parts by mass of the total of the polymer and polymerizable monomer) was used as a photoradical polymerization initiator instead of component A. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0062]
[0063] (Comparative Example 3) A mixed composition was prepared in the same manner as in Example 1, except that the polymer was changed from aromatic polycarbonate to polyvinyl acetate (weight-average molecular weight Mw 15000) represented by formula (6) above, having a refractive index of 1.46; the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer (2,12-DODNTMA, manufactured by Sugai Chemical Industry Co., Ltd., molecular weight 424.47, reactive group: -) represented by formula (7) above, having a refractive index of 1.69; and NCI-730 manufactured by ADEKA Corporation (3.0 parts by mass per 100 parts by mass of the total of the polymer and polymerizable monomer) was used as a photoradical polymerization initiator instead of component A. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0064] (Comparative Example 4) A mixed composition was prepared in the same manner as in Example 1, except that the polymer was changed from aromatic polycarbonate to a resin (a1) with a refractive index of 1.65 and represented by the following structural formula (9) (weight-average molecular weight Mw8000, l:m:n = 6.9:64.4:28.7 in the following structural formula (9)), the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer with a refractive index of 1.56 and represented by the following formula (10) (EA-0300 manufactured by Osaka Gas Chemical Co., Ltd., fluorene-based bifunctional acrylate, reactive group: -), and NCI-730 (3.0 parts by mass per 100 parts by mass of the total of the polymer and polymerizable monomer) was used as a photoradical polymerization initiator instead of component A. Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0065]
[0066]
[0067] (Comparative Example 5) A mixed composition was prepared in the same manner as in Example 1, except that the polymer was changed from aromatic polycarbonate to polymethyl methacrylate (PMMA) resin (weight-average molecular weight Mw90000) with a refractive index of 1.46, the polymerizable monomer was changed from 1,6-bis(2,3-epithiopropylthio)naphthalene to a polymerizable monomer represented by the following formula (11) with a refractive index of 1.53 (EBEcryl150, manufactured by Daicel Ornex, reactive group: -), and NCI-730 was used as a photoradical polymerization initiator instead of component A (3.0 parts by mass per 100 parts by mass of the total of the polymer and polymerizable monomer in the mixed composition). Then, a film was obtained using this mixed composition in the same manner as in Example 1.
[0068]
[0069] <Evaluation> (Preparation of evaluation film 1) A glass substrate (refractive index = 1.51) with a thickness of 0.5 mm and surface dimensions of 50 mm x 50 mm was spin-coated with the mixed compositions of the examples and comparative examples at 1000 rpm for 0.5 minutes, and then dried at 80°C for 3 minutes to obtain an unexposed film with a thickness of 2000 nm. A photomask was then placed on the obtained unexposed film, and exposure was performed through the photomask to form a film (thickness d = 2000 nm) in which exposed and unexposed areas were alternately formed in a certain direction. At this time, a photomask was used which had 500 slits with a width of 10 μm and a length of 50 mm, and the distance between adjacent slits was 10 μm. In this way, evaluation film 1 consisting of a glass substrate and a film was obtained. (Preparation of evaluation film 2) A glass substrate (refractive index = 1.51) with a thickness of 0.5 mm and surface dimensions of 50 mm x 50 mm was spin-coated with the mixed compositions of the examples and comparative examples at 1000 rpm for 0.5 minutes, and then dried at 80°C for 3 minutes to obtain an unexposed film with a thickness of 2000 nm. The obtained unexposed film was then exposed to light over its entire surface to obtain evaluation film 2.
[0070] (1) Clarity of the boundary between the exposed and unexposed areas The evaluation film 1 obtained as described above was examined using a differential interference microscope under reflected light illumination to observe the boundary between the unexposed and exposed areas (magnification: 20x) in the vicinity of the boundary between the exposed and unexposed areas, and whether a boundary could be observed between the exposed and unexposed areas. The clarity of the boundary was then evaluated based on the following criteria. The results are shown in Tables 1 and 2. (Criteria) A...The boundary between the exposed and unexposed areas can be observed clearly and without interruption B...The boundary between the exposed and unexposed areas can be observed without interruption C...The boundary between the exposed and unexposed areas can be observed with some interruption D...The boundary between the exposed and unexposed areas cannot be observed
[0071] (2) Refractive index difference (Δn) For the evaluation film 1 obtained as described above, an automatic absolute reflectance measurement system (manufactured by JASCO Corporation) was used to measure the intensity P1 of the emitted diffracted light by irradiating the surface of the film with thickness d (nm) with light of wavelength λ = 589 nm at an incident angle θ0 that maximizes the diffraction efficiency. The intensity P0 of the incident light was measured by removing the evaluation film 1 from the automatic absolute reflectance measurement system and directly measuring the intensity of the light. The diffraction efficiency was then calculated based on the intensity P1 of the diffracted light, the intensity P0 of the incident light, and the following formula (A). Diffraction efficiency (%) = 100 × P1 / P0 ... (A) On the other hand, the refractive index difference Δn was calculated based on the diffraction efficiency calculated as described above and the following formula (B). Example 1 was 0.035, Example 2 was 0.026, and Comparative Examples 1 to 5 were 0.000.
[0072]
[0073] (3) The evaluation film 2 obtained as described above was set up so that the angle between the colored floor surface of the film and the floor surface was 45°, with the colored floor surface of the film being set to 0°. Then, with the light from the three-wavelength fluorescent lamp shining on the entire surface of the film from above, the coloring of the film was observed visually from a position directly in front of the film surface, along a direction parallel to the floor surface. (Reference) A...No coloring B...Coloring (yellow) present
[0074] (4) Using a film whitening spectrophotometer (CM-3700A, Konica Minolta), the haze of the exposed area of evaluation film 2 was measured in accordance with JIS K 7105. The whitening of the film was evaluated based on the following criteria: (Criteria) A...Haze less than 1.50 B...Haze 1.50 or more
[0075]
[0076]
[0077] As shown in Tables 1 and 2, the evaluation results for boundary clarity were "A," "B," or "C" for Examples 1 to 9, while for Comparative Examples 1 to 5, it was "D." Therefore, it was confirmed that the mixed composition of the present invention can increase the refractive index difference between regions with different refractive indices when regions with different refractive indices are formed within a plane, thereby improving the clarity of the boundary between regions with different refractive indices (exposed and unexposed areas).
[0078] 1...Film, 2...Region with high refractive index, 3...Region with low refractive index, d1...Width of region 2, d2...Width of region 3, 10, 30...Optical components, 20...Light guide plate, 40...Image projection unit, 41...Microdisplay, 42...Lens, 100...Image display device.
Claims
1. A mixed composition comprising a polymer having a refractive index of 1.59 or less at the wavelength of sodium D lines at 25°C, a polymerizable monomer having a refractive index of 1.60 or more at the wavelength of sodium D lines at 25°C, and a component comprising a photoacid generator or a photobase generator, wherein the polymerizable monomer has two or more reactive groups that undergo a ring-opening polymerization reaction with an acid or base generated from the component, and the amount of polymerizable monomer blended with 100 parts by mass of the polymer is 40 parts by mass or more and 500 parts by mass or less.
2. The mixed composition according to claim 1, wherein the polymerizable monomer further has at least one ring structure, a divalent linking group is interposed between the ring structure and the reactive group, the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles, and the reactive group is an epoxy group or a thiirane group.
3. The mixed composition according to claim 1, wherein the polymerizable monomer further has at least one ring structure, a sulfur atom or a nitrogen atom is interposed between the ring structure and the reactive group, and the ring structure is at least one ring structure selected from the group consisting of aromatic rings and heterocycles.
4. The mixed composition according to claim 1, wherein the reactive group of the polymerizable monomer is a thiirane group.
5. The mixed composition according to claim 1, wherein the molecular weight of the polymerizable monomer is 300 or more.
6. The mixed composition according to claim 1, wherein the weight-average molecular weight of the polymer is 50,000 or less.
7. The mixed composition according to claim 1, wherein the repeating units of the polymer have aromatic rings.
8. A film comprising the mixed composition according to any one of claims 1 to 7.
9. A film obtained using the mixed composition described in any one of claims 1 to 7, wherein the film has two or more regions with different refractive indices within its surface.
10. The film according to claim 9, wherein the refractive index difference between the regions is 0.001 or more.
11. An optical component comprising the film described in claim 8.
12. An image display device comprising the optical component described in claim 11.