Optical film, circularly polarizing plate, image display device, reflective circularly polarizing plate, lens, and virtual reality display device
The optical film with multiple anisotropy layers addresses ghost image issues in pancake lenses by maintaining high ellipticity and in-plane phase difference, enhancing image quality in virtual reality display devices.
Patent Information
- Application Number
- PCT/JP2026/016674
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-12-03
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-19
AI Technical Summary
Existing optical films used in pancake lenses for virtual reality display devices suffer from ghost image generation and reduced contrast due to undesirable phase differences caused by stretching during shaping on curved surfaces.
An optical film configuration comprising multiple optical anisotropy layers with specific ellipticity and refractive index properties, including layers with vertically oriented disc-shaped and rod-shaped liquid crystal compounds, to maintain high ellipticity and suppress ghost image generation.
The solution effectively suppresses ghost image generation and maintains high contrast in virtual reality display devices using pancake lenses by ensuring high ellipticity and in-plane phase difference, even after stretching.
Smart Images

Figure JP2026016674_19112026_PF_FP_ABST
Abstract
Description
Optical films, circular polarizers, image display devices, reflective circular polarizers, lenses, and virtual reality display devices.
[0001] The present invention relates to optical films, circular polarizers, image display devices, reflective circular polarizers, lenses, and virtual reality display devices.
[0002] Optical films are sometimes used to convert the polarization state of light emitted from a display device to a different polarization state. For example, they are used as optical compensation films in liquid crystal displays and as anti-reflective films in organic electroluminescent displays (hereinafter also referred to as "organic EL"). They are also sometimes used in virtual reality displays and augmented reality displays, specifically in the image display devices or lenses that make up these devices.
[0003] In particular, in virtual reality display devices employing a folded optical system known as a pancake lens, an optical film is an indispensable component from the standpoint of reducing ghost images. Image display devices using optical films and virtual reality display devices including a pancake lens are described in Patent Documents 1 and 2.
[0004] Japanese Patent Publication No. 2020-519964, U.S. Patent No. 10394040
[0005] In pancake lenses, a method of laminating an optical film onto the spherical or aspherical curved surface of the optical lens is sometimes employed to obtain a wide field of view, low chromatic aberration, low distortion, and excellent MTF (modulation transfer function). However, laminating an optical film onto such a curved surface requires shaping the optical film into a three-dimensional form that includes the curved surface. During this shaping process, the optical film is stretched, which can cause undesirable phase differences to appear in the optical film or alter its original phase differences. As a result, the resulting ellipticity may decrease, potentially leading to problems such as worsened ghosting and reduced contrast.
[0006] The present invention has been made in view of the above problems, and the problem that the present invention aims to solve is to provide an optical film, a circular polarizer, an image display device, a reflective circular polarizer, a lens, and a virtual reality display device that suppress the generation of ghost images when applied to a virtual reality display device using a pancake lens.
[0007] The inventors of the present invention have conducted extensive research on the above-mentioned problems and have found that the above problems can be solved by the following configuration.
[0008] [1] An optical film comprising at least a first optical anisotropy layer and a second optical anisotropy layer laminated together, wherein the first optical anisotropy layer and the second optical anisotropy layer are each independently layers on which a liquid crystal compound is fixed, and the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to one surface of the optical film is 0.90 or more at minimum values in the wavelength range of 450 nm to 650 nm, and the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to one surface of the optical film after isotropically stretching the optical film to 1.1 times its area is 0.90 or more at minimum values in the wavelength range of 450 nm to 650 nm. [2] An optical film comprising a laminate containing at least a first optical anisotropy layer, a second optical anisotropy layer and a third optical anisotropy layer in this order, wherein the first optical anisotropy layer is a layer on which vertically oriented disc-shaped liquid crystal compounds are fixed, or a layer on which horizontally oriented rod-shaped liquid crystal compounds are fixed, the second optical anisotropy layer is a layer on which rod-shaped liquid crystal compounds twisted along a helical axis extending in the thickness direction are fixed, the third optical anisotropy layer is a layer on which vertically oriented rod-shaped liquid crystal compounds are fixed, and the ratio of the refractive index anisotropy Δn of the second optical anisotropy layer at a wavelength of 450 nm to the refractive index anisotropy Δn of the second optical anisotropy layer at a wavelength of 550 nm is 0.87 to 0.99, as in [1]. [3] The optical film according to [1] or [2], wherein the first optical anisotropy layer and the second optical anisotropy layer described above are in direct contact, and the orientations of the liquid crystal molecules with high in-plane refractive index coincide with each other on the surface of the first optical anisotropy layer that is in contact with the second optical anisotropy layer described above, and on the surface of the second optical anisotropy layer that is in contact with the first optical anisotropy layer described above. [4] The optical film according to any one of [1] to [3], wherein the laminate of the first optical anisotropy layer and the second optical anisotropy layer described above has an in-plane phase difference that is substantially λ / 4 with respect to the wavelength λ of the incident visible light. [5] The optical film according to any one of [1] to [4], having at least a curved portion. [6] A circular polarizer comprising the optical film according to any one of [1] to [5] and a polarizer. [7] An image display device comprising the circular polarizer according to [6].[8] A circular polarizer having an optical film as described in any of [1] to [5] and a reflective polarizer. [9] A lens having the circular polarizer described in [8].
[10] A virtual reality display device having the lens described in [9].
[0009] According to the present invention, it is possible to provide an optical film, a circular polarizer, an image display device, a reflective circular polarizer, a lens, and a virtual reality display device that suppress the generation of ghost images when applied to a virtual reality display device using a pancake lens.
[0010] Figure 1 is a schematic cross-sectional view showing an example of an embodiment of the optical film of the present invention. Figure 2 is a schematic cross-sectional view showing an example of an embodiment of the circular polarizer of the present invention. Figure 3 is a diagram showing the relationship between the absorption axis of the polarizer and the in-plane slow axes of the first optical anisotropy layer and the second optical anisotropy layer, respectively, in an example of an embodiment of the circular polarizer of the present invention. Figure 4 is a schematic diagram showing the relationship between the angle between the absorption axis of the polarizer and the in-plane slow axes of the first optical anisotropy layer and the second optical anisotropy layer, respectively, when observed from the direction of the white arrow in Figure 2. Figure 5 is a schematic diagram showing an example of the configuration of a virtual reality display device using the optical film of the present invention. Figure 6 is a schematic diagram showing an example of the configuration of a conventional virtual reality display device. Figure 7 is a schematic diagram illustrating the occurrence of ghosting in a virtual reality display device. Figure 8 is a schematic diagram illustrating the occurrence of ghosting in a virtual reality display device.
[0011] The present invention will now be described in detail. The following descriptions of constituent elements may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In this specification, numerical ranges expressed using "~" mean ranges that include the numbers written before and after "~" as the lower and upper limits. In this specification, an upper or lower limit stated in a numerical range described in steps may be replaced with an upper or lower limit in another numerical range described in steps. In addition, an upper or lower limit stated in a numerical range described in this specification may be replaced with a value shown in the examples. In this specification, each component may be made using one substance alone or using two or more substances in combination. Here, when two or more substances are used in combination for each component, the content for that component refers to the total content of the substances used in combination, unless otherwise specified.
[0012] Furthermore, the terms "liquid crystal composition" and "liquid crystal compound" in this specification also conceptually include materials that no longer exhibit liquid crystal properties due to hardening or other factors.
[0013] In this specification, "orthogonal" or "parallel" includes a range of error that is permissible in the art to which the present invention pertains. For example, it means being within a range of ±5° of an exact angle.
[0014] In this specification, unless otherwise specified, "phase difference" means "in-plane phase difference," or "in-plane retardation," and is denoted as Re(λ). Here, Re(λ) represents the in-plane retardation at wavelength λ, and unless otherwise specified, wavelength λ is 550 nm. Furthermore, retardation in the thickness direction at wavelength λ is denoted as Rth(λ) in this specification. Unless otherwise specified, wavelength λ is 550 nm. In addition, "lagging axis" means the direction in which the refractive index is maximum within the plane.
[0015] The Re(λ), Rth(λ), and orientation of the slow axis of an optical film can be obtained using values measured at wavelength λ, for example, with an AxoScan OPMF-1 (manufactured by OptoScience). By inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d) into AxoScan, the following can be calculated: • Slow axis orientation (°) • Re(λ) = R0(λ) • Rth(λ) = ((nx + ny) / 2 - nz) × d Note that R0(λ) is displayed as a value calculated by AxoScan, but it represents Re(λ).
[0016] In this specification, inverse wavelength dispersion refers to the characteristic that, when the in-plane retardation (Re) value at a specific wavelength (visible light range) is measured, the Re value increases as the measured wavelength increases. It is preferable that the optical anisotropic layer or optical film having inverse wavelength dispersion satisfies Re(450) / Re(550) < 1.00. Furthermore, it is more preferable that it also satisfies Re(650) / Re(550) > 1.00. On the other hand, forward wavelength dispersion refers to the characteristic that, when the in-plane retardation (Re) value at a specific wavelength (visible light range) is measured, the Re value decreases as the measured wavelength increases. It is preferable that the optical anisotropic layer or optical film having forward wavelength dispersion satisfies Re(450) / Re(550) > 1.00 and Re(650) / Re(550) < 1.00. In this specification, visible light refers to electromagnetic waves with wavelengths visible to the human eye, specifically light in the wavelength range of 380 to 780 nm.
[0017] In this specification, unless otherwise specified, ellipticity refers to the ellipticity of the emitted light when linearly polarized light with a predetermined polarization axis angle is incident on one surface of an optical film. An appropriate polarization axis angle is 45° with respect to the lagging axis orientation when the optical film is substantially a λ / 4 wave plate. Alternatively, in the usage configuration of the optical film, the polarization axis orientation of the emitted light can be measured when right-circularly polarized or left-circularly polarized light is incident perpendicularly from the surface opposite to the surface on which the linearly polarized light is incident, and this can be set to an appropriate angle. Here, the ellipticity of the optical film can be obtained, for example, by arranging the optical film and a linear polarizer at an angle adjusted so that the incident polarization is the appropriate polarization axis angle described above, and using an AxoScan OPMF-1, incident light of wavelength λ from the side of the linear polarizer and measuring the ellipticity of the emitted light. Furthermore, the ellipticity of an optical film can be calculated based on the Stokes parameter obtained by measuring the Müller matrix at wavelength λ using AxoScan OPMF-1 for an optical film that is not laminated with a linear polarizer, and multiplying that Müller matrix by the Stokes parameter representing linear polarization with the appropriate polarization axis angle mentioned above. Ellipticity is often used as an indicator of the performance of a λ / 4 plate. Specifically, when linearly polarized light with an appropriate polarization axis angle is incident on a λ / 4 plate, the ellipticity corresponding to the emitted circularly polarized light becomes the evaluation index. The maximum value of ellipticity is 1, and the closer the value is to 1, the closer the emitted light is to perfectly circularly polarized light, indicating a more desirable characteristic. In addition, ellipticity is generally described as +1 for right-circularly polarized light and -1 for left-circularly polarized light, but in this specification, the ellipticity of the obtained emitted light represents its absolute value. That is, the ellipticity of left-circularly polarized light is also interpreted as +1.
[0018] In this specification, "absorption axis" refers to the polarization direction in which the absorbance is maximized in the plane when linearly polarized light is incident on an absorbing linear polarizer. "Reflection axis" refers to the polarization direction in which the reflectance is maximized in the plane when linearly polarized light is incident on a reflective linear polarizer. "Transmission axis" refers to the direction in the plane that is perpendicular to the absorption axis or reflection axis.
[0019] In this specification, the optically anisotropic layer may be any layer exhibiting predetermined optical properties, and is preferably, for example, a layer in which the orientation state of an oriented liquid crystal compound is fixed. The "fixed" state is a state in which the orientation of the liquid crystal compound is maintained. Specifically, it is more preferable that the layer is non-fluid in a temperature range of 0 to 50°C, and under more severe conditions of -30 to 70°C, and that the fixed orientation state can be stably maintained without causing changes in the orientation state due to external fields or external forces.
[0020] In this specification, Plate A and Plate C are defined as follows:
[0021] There are two types of A plates: positive A plates and negative A plates. When the refractive index in the in-plane slow axis direction (the direction in which the refractive index is maximum in the plane) of the film is nx, the refractive index in the direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, a positive A plate satisfies the relationship in equation (A1), and a negative A plate satisfies the relationship in equation (A2). Note that a positive A plate shows a positive value for Rth, and a negative A plate shows a negative value for Rth. Equation (A1) nx > ny ≈ nz Equation (A2) ny < nx ≈ nz Note that the above "≈" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. "Substantially identical" means, for example, that when (ny - nz) × d (where d is the thickness of the film) is -10 to 10 nm, preferably -5 to 5 nm, it is included in "ny ≈ nz", and when (nx - nz) × d is -10 to 10 nm, preferably -5 to 5 nm, it is included in "nx ≈ nz".
[0022] <C Plate> There are two types of C plates: positive C plates and negative C plates. Positive C plates satisfy the relationship in equation (C1), and negative C plates satisfy the relationship in equation (C2). Note that positive C plates show a negative value for Rth, and negative C plates show a positive value for Rth. Equation (C1) nz > nx ≈ ny Equation (C2) nz < nx ≈ ny Note that the above "≈" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. "Substantially identical" means, for example, that (nx - ny) × d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, which is included in "nx ≈ ny".
[0023] In this specification, Δnd, which is the product of the refractive index anisotropy Δn and the thickness d of the optically anisotropic layer, represents the Re (in-plane phase difference) of the optically anisotropic layer when the optically anisotropic layer is a "positive A plate" or a "negative A plate". Furthermore, when the optically anisotropic layer is a "layer formed by fixing a liquid crystal compound that is twisted and oriented along a helical axis extending in the thickness direction", it represents the value obtained by multiplying the in-plane Δn of the liquid crystal compound (Δn = nx - ny) by the film thickness. Furthermore, when the optically anisotropic layer is a "positive C plate" or a "negative C plate", it represents the absolute value of the Rth (thickness direction phase difference) of the optically anisotropic layer.
[0024] The present invention will now be described in detail with reference to the drawings. The following descriptions of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments.
[0025] [Optical Film] An optical film according to a first aspect of the present invention is an optical film comprising at least a first optical anisotropy layer and a second optical anisotropy layer laminated together, wherein the first optical anisotropy layer and the second optical anisotropy layer are each independently layers on which a liquid crystal compound is fixed, and the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to one surface of the optical film is 0.90 or more at minimum values in the wavelength range of 450 nm to 650 nm, and the optical film is isotropically stretched to 1.1 times its area, and then when linearly polarized light is incident perpendicularly to the aforementioned one surface, the ellipticity of the emitted light is 0.90 or more at minimum values in the wavelength range of 450 nm to 650 nm.
[0026] Furthermore, an optical film according to a second aspect of the present invention is an optical film comprising a laminate containing at least a first optical anisotropy layer, a second optical anisotropy layer, and a third optical anisotropy layer in this order, wherein the first optical anisotropy layer is a layer on which vertically oriented disc-shaped liquid crystal compounds are fixed, or a layer on which horizontally oriented rod-shaped liquid crystal compounds are fixed, the second optical anisotropy layer is a layer on which rod-shaped liquid crystal compounds twisted along a helical axis extending in the thickness direction are fixed, and the third optical anisotropy layer is a layer on which vertically oriented rod-shaped liquid crystal compounds are fixed, and the ratio of the refractive index anisotropy Δn of the second optical anisotropy layer at a wavelength of 450 nm to the refractive index anisotropy Δn of the second optical anisotropy layer at a wavelength of 550 nm is 0.87 to 0.99. Furthermore, in the optical film according to the second aspect of the present invention, similar to the first aspect, the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to one surface of the optical film is preferably 0.90 or more at a minimum value in the wavelength range of 450 nm to 650 nm, and it is preferable that after isotropically stretching the optical film so that its area is 1.1 times greater, the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to the aforementioned one surface is preferably 0.90 or more at a minimum value in the wavelength range of 450 nm to 650 nm.
[0027] In the optical films according to the first and second embodiments of the present invention (hereinafter, unless otherwise specified, also referred to as "the optical film of the present invention"), the orientation direction of the liquid crystal compound changes continuously at the interface between the first optical anisotropic layer and the second optical anisotropic layer. This reduces the refractive index difference in all directions within the plane, and it is preferable that the first optical anisotropic layer and the second optical anisotropic layer are in direct contact with each other. Specifically, the orientations of the liquid crystal molecules with high in-plane refractive indexes coincide on the surface of the first optical anisotropic layer that is in contact with the second optical anisotropic layer, and on the surface of the second optical anisotropic layer that is in contact with the first optical anisotropic layer. Here, "liquid crystal molecules" refers to the liquid crystal compounds contained in each optical anisotropic layer. Furthermore, "the orientations of the liquid crystals with high in-plane refractive indexes coincide" means that the orientations with the maximum refractive index within the plane (i.e., the in-plane slow axis of each optical anisotropic layer) are parallel to each other. Furthermore, by directly applying a composition for forming a second optical anisotropic layer containing a liquid crystal compound to a first optical anisotropic layer containing a liquid crystal compound, the liquid crystal compound of the second optical anisotropic layer can be oriented so that the orientation direction of the liquid crystal compounds in both layers is continuous at the interface, due to the orientation-regulating force of the liquid crystal compound in the first optical anisotropic layer. This is also preferable from the viewpoint of simplifying the manufacturing process.
[0028] Preferably, the optical film of the present invention has the function of converting emitted light into linearly polarized light when circularly polarized light is incident from at least one surface, and converting emitted light into circularly polarized light when linearly polarized light is incident from the other surface. To realize these functions, it is preferable that the optical film of the present invention has an in-plane phase difference that is substantially λ / 4 with respect to the wavelength λ of the incident visible light. Here, "in-plane phase difference that is substantially λ / 4" means an in-plane phase difference that is 0.20 to 0.30 times the wavelength λ of the incident visible light. Furthermore, even if the first optical anisotropy layer and the second optical anisotropy layer of the optical film of the present invention do not each have an in-plane phase difference that is substantially λ / 4, it is preferable that the laminate of the first optical anisotropy layer and the second optical anisotropy layer has an in-plane phase difference that is substantially λ / 4 with respect to the wavelength λ of the incident visible light. When an optical film is stretched, the film thickness of each optical anisotropy layer becomes thinner, and the optical anisotropy Δnd becomes smaller accordingly. However, in the optical film of the present invention, the lamination of the first optical anisotropy layer and the second optical anisotropy layer can compensate for the optical changes associated with the decrease in Δnd, thus maintaining a high ellipticity even after stretching. Even in cases where the in-plane phase difference cannot be strictly defined for the entire laminate, such as a laminate of the first optical anisotropy layer and the second optical anisotropy layer, it is possible to define the substantial in-plane phase difference of the entire laminate by replacing the linear polarization conversion effect of the laminate with the effect of a single A-plate. In this case as well, "substantially λ / 4 in-plane phase difference" refers to an in-plane phase difference that is 0.20 to 0.30 times the wavelength λ of the incident visible light. In particular, when the first optical anisotropy layer and the second optical anisotropy layer each have predetermined structures and wavelength dispersions described later, the decrease in ellipticity after stretching can be suppressed more effectively.
[0029] The optical film of the present invention, when used in a pancake lens, preferably has a curved portion in at least a part of it, from the viewpoint of achieving a wide viewing angle, low chromatic aberration, low distortion, and excellent MTF (modulation transfer function). Here, the curved portion means a part with a curved shape. The curved shape means a shape having a curvature greater than 0, and includes curved shapes that are developable surfaces and three-dimensional curved shapes. The radius of curvature of the shape having curvature is preferably 10 mm to 120 mm, and more preferably 15 to 90 mm. A developable surface means a surface that can be unfolded into a plane without stretching or contracting each part of the surface, and examples of curved shapes that are developable surfaces include surfaces corresponding to cylindrical surfaces, elliptical cylindrical surfaces, conical surfaces, and elliptical cone surfaces, and may be a convex curved surface or a concave curved surface. A three-dimensional curved surface refers to a curved surface that cannot be formed by the deformation of a plane, that is, a curved surface that is not developable. Examples of three-dimensional curved surfaces include surfaces corresponding to spheres and ellipsoidal surfaces, and surfaces whose cross-section is a parabola or hyperbola (for example, a paraboloid of revolution). These surfaces may be convex or concave. In this invention, it is preferable that the curved surface portion is not a developable surface because the effect of suppressing the generation of ghosting becomes apparent. Furthermore, in this invention, it is preferable that the curved shape of the curved surface portion is lens-shaped. Examples of lens-shaped curved surfaces include spherical shapes and ellipsoidal surfaces, and these may be convex or concave lens shapes.
[0030] <Embodiments of the Optical Film> Hereinafter, embodiments of the optical film of the present invention will be described with reference to the drawings. Figure 1 is a schematic cross-sectional view showing an example of an embodiment of the optical film of the present invention. The optical film 10A has a first optical anisotropy layer 12A, a second optical anisotropy layer 14, and a third optical anisotropy layer 16 in this order. The first optical anisotropy layer 12A is a layer formed by fixing a vertically oriented disc-shaped liquid crystal compound, the second optical anisotropy layer 14 is a layer formed by fixing a rod-shaped liquid crystal compound that is twisted along a helical axis extending in the thickness direction, and the third optical anisotropy layer 16 is a layer formed by fixing a vertically oriented rod-shaped liquid crystal compound. The angle between the in-plane slow axis of the first optical anisotropy layer 12A and the in-plane slow axis on the surface of the second optical anisotropy layer 14 on the first optical anisotropy layer 12A side is preferably in the range of 0 to 20°, as will be described later. Hereinafter, each layer will be described in detail.
[0031] (First optically anisotropic layer 12A) The first optically anisotropic layer 12A is a layer on which vertically oriented disc-shaped liquid crystal compounds are fixed. More specifically, a layer on which vertically oriented disc-shaped liquid crystal compounds are fixed, and the optical axes (axes perpendicular to the disc surface) are aligned in the same direction. The state in which the disc-shaped liquid crystal compounds are vertically oriented means that the disc surface of the disc-shaped liquid crystal compound and the thickness direction of the layer are parallel. It is not required that they be strictly parallel, but it is preferable that the angle between the disc surface and the thickness direction of the layer is in the range of 0 to 20°, and more preferably in the range of 0 to 10°. Furthermore, the state in which the optical axes (axes perpendicular to the disk surface) of a disc-shaped liquid crystal compound are aligned in the same direction does not require them to be strictly in the same direction. Rather, it means that when the orientation of the slow axis is measured at any 20 locations within the plane, the maximum difference in the slow axis orientations (the difference between the two slow axis orientations with the largest difference out of the 20 slow axis orientations) is less than 10°.
[0032] The in-plane retardation of the first optical anisotropy layer 12A at a wavelength of 550 nm is not particularly limited, but from the viewpoint of obtaining a higher ellipticity, 120 to 240 nm is preferred, 130 to 230 nm is more preferred, and 160 to 210 nm is even more preferred.
[0033] As the discotic liquid crystal compound, a known compound can be used. Examples of the discotic liquid crystal compound include the compounds described in paragraphs
[0020] to
[0067] of JP-A-2007-108732 and paragraphs
[0013] to
[0108] of JP-A-2010-244038.
[0034] The discotic liquid crystal compound may have a polymerizable group. In the present specification, the type of the polymerizable group is not particularly limited, but a functional group capable of addition polymerization reaction is preferable. A polymerizable ethylenically unsaturated group or a cyclic polymerizable group is more preferable, and a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group is still more preferable.
[0035] The first optically anisotropic layer 12A is preferably a layer formed by polymerizing and fixing a discotic liquid crystal compound having a vertically aligned polymerizable group.
[0036] The first optically anisotropic layer 12A may exhibit normal wavelength dispersion or reverse wavelength dispersion. The normal wavelength dispersion and reverse wavelength dispersion described above are preferably exhibited in the visible light region. The ratio of the in-plane retardation of the first optically anisotropic layer 12A at a wavelength of 450 nm to the in-plane retardation of the first optically anisotropic layer 12A at a wavelength of 550 nm (Re(450) / Re(550)) is preferably 0.80 to 1.25, more preferably 1.08 to 1.15. The ratio of the in-plane retardation of the first optically anisotropic layer 12A at a wavelength of 650 nm to the in-plane retardation of the first optically anisotropic layer 12A at a wavelength of 550 nm (Re(650) / Re(550)) is preferably 0.90 to 1.20, more preferably 0.92 to 1.00.
[0037] The average thickness of the first optically anisotropic layer 12A is not particularly limited, and is preferably 10 μm or less, more preferably 0.1 to 5.0 μm, and still more preferably 0.3 to 2.0 μm. The above average thickness is determined by measuring the thickness at any 5 or more points of the first optically anisotropic layer 12A and arithmetically averaging the measured values.
[0038] (Second Optical Anisotropic Layer 14) The second optical anisotropic layer 14 is a layer formed by fixing rod-shaped liquid crystal compounds that are twisted and oriented along a helical axis extending in the thickness direction. Preferably, the second optical anisotropic layer 14 is a layer formed by fixing a chiral nematic phase having a so-called helical structure. When forming the above second optical anisotropic layer 14, it is preferable to use at least a rod-shaped liquid crystal compound and a chiral agent described later.
[0039] The torsion angle of the rod-shaped liquid crystal compound (the torsion angle in the orientation direction of the liquid crystal compound) is not particularly limited, but is often greater than 0° and less than or equal to 360°. This allows for the acquisition of emitted light with higher ellipticity for linearly polarized light incident at an oblique angle, and when applied to a virtual reality display device using a pancake lens, the generation of ghost images can be further suppressed (hereinafter also referred to as "the advantages of the present invention"). Therefore, a range of 80±30° (50 to 110°) is preferred, and a range of 80±20° (60 to 100°) is more preferred. The torsion angle is measured using an AxoScan (polarimeter) device from Axometrics Inc. and its device analysis software. Furthermore, the torsion orientation of the rod-shaped liquid crystal compound means that the rod-shaped liquid crystal compound twists from one main surface to the other main surface of the second optical anisotropy layer 14, with the thickness direction of the second optical anisotropy layer 14 as the axis. Accordingly, the orientation direction of the rod-shaped liquid crystal compound differs depending on its position in the thickness direction of the second optical anisotropy layer 14. In torsional orientation, the long axis of the rod-shaped liquid crystal compound is arranged to be parallel to the main surface of the second optical anisotropy layer 14. However, strict parallelism is not required; it is preferable that the angle between the long axis of the rod-shaped liquid crystal compound and the main surface of the second optical anisotropy layer 14 is in the range of 0 to 20°, and more preferably in the range of 0 to 10°.
[0040] The value of the product Δnd, which is the refractive index anisotropy Δn of the second optical anisotropy layer 14 at a wavelength of 550 nm and the thickness d of the second optical anisotropy layer 14, is not particularly limited. However, in terms of achieving superior effects of the present invention, 120 to 240 nm is preferred, 130 to 230 nm is more preferred, and 160 to 210 nm is even more preferred. The above Δnd is measured using an AxoScan (polarimeter) device from Axometrics Inc. and its device analysis software.
[0041] The angle between the in-plane slow axis of the first optical anisotropy layer 12A and the in-plane slow axis on the surface of the second optical anisotropy layer 14 facing the first optical anisotropy layer 12A is preferably in the range of 0 to 20°, and more preferably coincides. Here, the in-plane slow axis refers to the direction in which the in-plane refractive index of each liquid crystal molecule is highest on that plane.
[0042] The type of rod-shaped liquid crystal compound used to form the second optical anisotropy layer 14 is not particularly limited, and known compounds can be cited. Examples of rod-shaped liquid crystal compounds include the forward-wavelength dispersive liquid crystal compounds described in claim 1 of "Japanese Patent Publication No. 11-513019" and paragraphs 0026 to 0098 of "Japanese Patent Application Publication No. 2005-289980", and the reverse-wavelength dispersive liquid crystal compounds described in paragraphs 0041 to 0057 of "Japanese Patent Application Publication No. 2023-029317". The rod-shaped liquid crystal compound may have polymerizable groups. In the present invention, the type of polymerizable group contained in the rod-shaped liquid crystal compound is the same as that described earlier in relation to the first optical anisotropy layer.
[0043] The second optically anisotropic layer 14 is preferably a layer formed by polymerizing a rod-shaped liquid crystal compound having polymerizable groups. In particular, to maximize the effects of the present invention, it is desirable to polymerize a rod-shaped liquid crystal compound having twistedly oriented polymerizable groups to form a layer structure in which the twisted orientation structure is firmly fixed.
[0044] In the optical film according to the first aspect of the present invention, the ratio of the refractive index anisotropy Δn at a wavelength of 450 nm to the refractive index anisotropy Δn at a wavelength of 550 nm of the second optical anisotropy layer 14 (Δn(450) / Δn(550)) is not particularly limited, but 0.68 to 1.20 is preferred, 0.81 to 1.11 is more preferred, and 0.87 to 0.99 is even more preferred in terms of achieving superior effects of the present invention. In the optical film according to the second aspect of the present invention, the ratio of the refractive index anisotropy Δn at a wavelength of 450 nm to the refractive index anisotropy Δn at a wavelength of 550 nm of the second optical anisotropy layer 14 (Δn(450) / Δn(550)) is 0.87 to 0.99. Furthermore, the ratio of the refractive index anisotropy Δn at a wavelength of 650 nm to the refractive index anisotropy Δn at a wavelength of 550 nm of the second optical anisotropy layer 14 (Δn(650) / Δn(550)) is not particularly limited, but in terms of achieving superior effects of the present invention, 0.90 to 1.20 is preferred, 0.92 to 1.04 is more preferred, and 0.96 to 1.00 is even more preferred.
[0045] The second optical anisotropic layer 14 can be formed, for example, using an optical anisotropic layer-forming composition containing a mixture of a forward-wavelength-dispersive liquid crystal compound and an inverse-wavelength-dispersive liquid crystal compound. In this case, the wavelength dispersivity of the second optical anisotropic layer 14 can be adjusted by adjusting the mixing ratio of the forward-wavelength-dispersive liquid crystal compound and the inverse-wavelength-dispersive liquid crystal compound. When multiple types of liquid crystal compounds are used, the content of the inverse-wavelength-dispersive liquid crystal compound (the total amount if multiple inverse-wavelength-dispersive liquid crystal compounds are included) is often 1 to 95% by mass of the total mass of the liquid crystal compound, and is preferably 50 to 90% by mass, and more preferably 60 to 85% by mass, in terms of achieving superior effects of the present invention.
[0046] The average thickness of the second optical anisotropy layer 14 is not particularly limited, but is preferably 10 μm or less, more preferably 0.1 to 5.0 μm, and even more preferably 0.3 to 2.0 μm. The above average thickness is determined by measuring the thickness of any five or more points on the second optical anisotropy layer 14 and taking their arithmetic mean.
[0047] (Third Optical Anisotropy Layer 16) The third optical anisotropy layer 16 is a layer formed by fixing vertically oriented rod-shaped liquid crystal compounds. The state in which the rod-shaped liquid crystal compounds are vertically oriented means that the long axis of the rod-shaped liquid crystal compounds is parallel to the thickness direction of the third optical anisotropy layer 16. It is not required that they be strictly parallel, but it is preferable that the angle between the long axis of the rod-shaped liquid crystal compounds and the thickness direction of the third optical anisotropy layer 16 is in the range of 0 to 20°, and more preferably in the range of 0 to 10°.
[0048] The retardation in the thickness direction of the third optical anisotropy layer 16 at a wavelength of 550 nm is not particularly limited, but -150 to -10 nm is preferred, and -110 to -60 nm is more preferred, in terms of achieving superior effects of the present invention.
[0049] Known compounds can be used as the rod-shaped liquid crystal compound. Examples of rod-shaped liquid crystal compounds include the rod-shaped liquid crystal compound exemplified in the second optical anisotropy layer 14. The rod-shaped liquid crystal compound may have polymerizable groups. The types of polymerizable groups that the rod-shaped liquid crystal compound may have are as described above.
[0050] The third optically anisotropic layer 16 is preferably a layer formed by polymerizing rod-shaped liquid crystal compounds having vertically oriented polymerizable groups.
[0051] The ratio of the retardation in the thickness direction of the third optical anisotropy layer 16 at a wavelength of 650 nm to the retardation in the thickness direction of the third optical anisotropy layer 16 at a wavelength of 550 nm (Δn(650) / Δn(550)) is not particularly limited, but 0.90 to 1.20 is preferred, and 0.92 to 1.12 is more preferred, in terms of achieving superior effects of the present invention.
[0052] The average thickness of the third optical anisotropy layer 16 is not particularly limited, but is preferably 10 μm or less, more preferably 0.1 to 5.0 μm, and even more preferably 0.3 to 2.0 μm. The above average thickness is determined by measuring the thickness of any five or more points on the third optical anisotropy layer 16 and taking the arithmetic mean of them.
[0053] <Other Embodiments of the Optical Film> In other embodiments of the optical film of the present invention, the first optical anisotropic layer is a positive A plate, the second optical anisotropic layer is a layer in which a disc-shaped liquid crystal compound is fixed in a twisted orientation along a helical axis extending in the thickness direction, and the third optical anisotropic layer is a negative C plate.
[0054] (First Optical Anisotropic Layer) The definition of a positive A plate is as described above, but it is preferable that the positive A plate be a layer on which horizontally oriented rod-shaped liquid crystal compounds are fixed. More specifically, a layer on which horizontally oriented rod-shaped liquid crystal compounds are fixed, and whose long axes are aligned in the same direction. The state in which the rod-shaped liquid crystal compounds are horizontally oriented means that the long axes of the rod-shaped liquid crystal compounds are aligned horizontally and in the same direction with respect to the surface of the optical anisotropic layer. Here, horizontal does not require that they be strictly horizontal, but rather means an orientation in which the inclination angle between the average molecular axis of the liquid crystal compounds in the optical anisotropic layer and the surface of the optical anisotropic layer is less than 20°. Furthermore, "same orientation" does not require that the orientations be strictly the same, but rather means that when the orientation of the lagging axis is measured at any 20 locations in the plane, the maximum difference between the lagging axis orientations at those 20 locations (the difference between the two lagging axis orientations with the largest difference out of the 20 lagging axis orientations) is less than 10°.
[0055] The in-plane retardation of the first optical anisotropy layer (positive A plate) at a wavelength of 550 nm is not particularly limited, but 120 to 240 nm is preferred, 130 to 230 nm is more preferred, and 160 to 210 nm is even more preferred, for reasons that the effects of the present invention are superior.
[0056] (Second Optical Anisotropy Layer) A layer formed by fixing a disc-shaped liquid crystal compound that is twisted or oriented along a helical axis extending in the thickness direction can be described as a layer formed by fixing a rod-shaped liquid crystal compound that is twisted or oriented along a helical axis extending in the thickness direction (second optical anisotropy layer 14) as described above, but in which the rod-shaped liquid crystal compound is replaced with a disc-shaped liquid crystal compound. The twist angle of the second optical anisotropy layer (a layer formed by fixing a disc-shaped liquid crystal compound that is twisted or oriented along a helical axis extending in the thickness direction) and the product Δnd of the refractive index anisotropy Δn and thickness d at a wavelength of 550 nm are the same as the values described above for the layer formed by fixing a rod-shaped liquid crystal compound that is twisted or oriented along a helical axis extending in the thickness direction (second optical anisotropy layer 14).
[0057] (Third Optical Anisotropic Layer) The definition of a negative C plate is as described above, but it is preferable to have a layer in which horizontally oriented disc-shaped liquid crystal compounds are fixed. More specifically, the layer in which horizontally oriented disc-shaped liquid crystal compounds are fixed is a layer in which disc-shaped liquid crystal compounds are horizontally oriented and whose optical axes (axes perpendicular to the disc surface) are aligned in the same direction. The state in which the disc-shaped liquid crystal compounds are horizontally oriented means that the disc surface of the disc-shaped liquid crystal compound and the main surface of the layer are parallel. However, it is not required that they be strictly parallel, and it is preferable that the angle between the disc surface and the main surface of the layer is in the range of 0 to 20°, and more preferably in the range of 0 to 10°.
[0058] The retardation in the thickness direction of the third optical anisotropy layer (negative C plate) at a wavelength of 550 nm is not particularly limited, but 5 to 100 nm is preferred, and 10 to 60 nm is more preferred, for reasons that the effects of the present invention are superior.
[0059] <Other components> The optical film shown in the specific embodiment described above may include other components other than the first optical anisotropy layer to the third optical anisotropy layer described above.
[0060] (Fourth Optical Anisotropy Layer) The optical film shown in the specific embodiment described above may include a fourth optical anisotropy layer on the side of the first optical anisotropy layer opposite to the second optical anisotropy layer. The fourth optical anisotropy layer is preferably a layer formed by fixing a horizontally oriented disc-shaped liquid crystal compound. The state in which the disc-shaped liquid crystal compound is horizontally oriented means that the disc surface of the disc-shaped liquid crystal compound and the main surface of the layer are parallel. However, it is not required that they be strictly parallel, and it is preferable that the angle between the disc surface and the main surface of the layer is in the range of 0 to 20°, and more preferably in the range of 0 to 10°.
[0061] The retardation in the thickness direction at a wavelength of 550 nm of the fourth optical anisotropy layer is not particularly limited, but 5 to 100 nm is preferred, and 10 to 60 nm is more preferred, in terms of achieving superior effects of the present invention.
[0062] Known compounds can be used as the disc-shaped liquid crystal compound. Examples of disc-shaped liquid crystal compounds include the disc-shaped liquid crystal compound exemplified in the first optical anisotropy layer 12A. The disc-shaped liquid crystal compound may have polymerizable groups. The types of polymerizable groups that the disc-shaped liquid crystal compound may have are as described above.
[0063] The fourth optically anisotropic layer is preferably a layer formed by polymerizing a disc-shaped liquid crystal compound having horizontally oriented polymerizable groups.
[0064] The average thickness of the fourth optical anisotropy layer is not particularly limited, but is preferably 10 μm or less, more preferably 0.1 to 5.0 μm, and even more preferably 0.3 to 2.0 μm. The above average thickness is determined by measuring the thickness of any five or more points in the fourth optical anisotropy layer and taking their arithmetic mean.
[0065] (Adhesion Layer) The optical film shown in the specific embodiment described above may have an adhesion layer between each optical anisotropic layer. Examples of known adhesive layers include tack layers and adhesive layers. Suitable adhesives include, for example, an adhesive made of an aqueous solution of polyvinyl alcohol resin, a curable adhesive composition containing a cationic polymerizable compound that hardens by irradiation with active energy rays or heating, or a curable adhesive composition containing a radical polymerizable compound. The thickness of the adhesive layer is preferably about 0.01 to 20 μm, more preferably 0.01 to 10 μm, and even more preferably 0.05 to 5 μm. If the thickness of the adhesive layer is within this range, no lifting or peeling will occur between the laminated optical anisotropic layers, and practically satisfactory adhesive strength can be obtained.
[0066] (Alignment film) The optical film shown in the specific embodiment described above may further have an alignment film. The alignment film may be arranged between each optical anisotropic layer. However, as shown in Figure 1, it is preferable that the optical film 10A does not have an alignment film between each optical anisotropic layer.
[0067] The alignment film can be formed by means of rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer having microgrooves, or accumulation of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearylate) by the Langmuir-Bludget method (LB film). Furthermore, alignment films that exhibit alignment function upon application of an electric field, magnetic field, or light irradiation (preferably polarized light) are also known. The alignment film is preferably formed by rubbing a polymer. It is also preferable to use a photo-alignment film. The thickness of the alignment film is not particularly limited as long as it can exhibit alignment function, but is preferably 0.01 to 5.0 μm, more preferably 0.05 to 2.0 μm, and even more preferably 0.1 to 0.5 μm.
[0068] (Support) The optical film shown in the specific embodiment described above may further have a support. A transparent support is preferred as the support. A transparent support refers to a support having a visible light transmittance of 60% or more, preferably 80% or more, and more preferably 90% or more. Furthermore, a small phase difference is preferred from the viewpoint of suppressing the effect on the polarization degree of transmitted light and facilitating optical inspection of the laminated optical body. Specifically, the size of Re is preferably 10 nm or less, and the absolute value of the size of Rth is preferably 50 nm or less. The thickness of the support is not particularly limited, but is preferably 10 to 200 μm, more preferably 10 to 100 μm, and even more preferably 20 to 90 μm.
[0069] Furthermore, the support may consist of multiple laminated layers. To improve adhesion with the layer provided on top of it, the surface of the support may be subjected to surface treatment (e.g., glow discharge treatment, corona discharge treatment, ultraviolet (UV) treatment, flame treatment). Alternatively, an adhesive layer (undercoat layer) may be provided on top of the support. The support may be a so-called temporary support. For example, after manufacturing an optically anisotropic layer on a temporary support, the optically anisotropic layer may be bonded to another optically anisotropic layer, support, polarizer, etc., and then the temporary support may be peeled off from the optically anisotropic layer as needed. Furthermore, the peeling force between the optically anisotropic layer and the temporary support is not particularly limited, but from the viewpoint of preventing unintended peeling of the optically anisotropic layer, it is preferably 0.01 N / 25 mm or more, and more preferably 0.03 N / 25 mm or more. On the other hand, from the viewpoint of facilitating the peeling of the temporary support, it is preferably 0.5 N / 25 mm or less, and more preferably 0.1 N / 25 mm or less. Furthermore, when multiple optically anisotropic layers are bonded together, it is desirable that the peeling force of each temporary support be adjusted according to the order in which the temporary supports are peeled off. For example, when the temporary support of the second optically anisotropic layer is peeled off first after the first optically anisotropic layer and the second optically anisotropic layer have been bonded together, it is preferable that the peeling force between the first optically anisotropic layer and the temporary support is greater than the peeling force between the second optically anisotropic layer and the temporary support.
[0070] The support may be one that is ultimately incorporated into the optical film without being peeled off. Alternatively, if the optical film is one that is transferred from a temporary support, the support can be used as the transfer destination.
[0071] The type of support is not particularly limited, but for example, films such as cellulose acetate, polycarbonate, polysulfone, polyethersulfone, polyacrylate and polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among these, cellulose acetate film, cyclic polyolefin film, polyacrylate film, and polymethacrylate film are preferred. Commercially available cellulose acetate films (for example, "TD80U" and "Z-TAC" manufactured by Fujifilm Corporation) can also be used.
[0072] When the optical film is stretched or molded, the support preferably has a tanδ peak temperature of 170°C or lower. From the viewpoint of enabling molding at low temperatures, the tanδ peak temperature is preferably 150°C or lower, and more preferably 130°C or lower.
[0073] Here, we describe the method for measuring tanδ. Using a dynamic viscoelasticity measuring device (DVA-200 manufactured by IT Measurement Control Co., Ltd.), a film sample that has been pre-conditioned for more than 2 hours at a temperature of 25°C and a humidity of 60% Rh is used to measure E'' (loss modulus) and E' (storage modulus) under the following conditions, and use these values to determine tanδ (= E'' / E'). Device: DVA-200 manufactured by IT Measurement Control Co., Ltd. Sample: 5 mm, length 50 mm (gap 20 mm) Measurement conditions: Tensile mode Measurement temperature: -150°C to 220°C Heating rate: 5°C / min Frequency: 1 Hz In general, in optical applications, stretched resin substrates are often used, and the stretching treatment often results in a high peak temperature for tanδ. For example, the peak temperature of tanδ for TAC (triacetylcellulose) substrate (TG40, manufactured by Fujifilm Corporation) is 180°C or higher.
[0074] Supports with a tanδ peak temperature of 170°C or lower can be made from a variety of resin substrates without particular limitations. Examples include polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; acrylic resins such as polymethacrylate and polyacrylic acid esters; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide and polyphenylene oxide. Among these, cyclic olefin resins, polyethylene terephthalate, or acrylic resins are preferred due to their readily available market availability and excellent transparency, and cyclic olefin resins or polymethacrylate esters are more preferred.
[0075] Examples of commercially available resin substrates include Technoloy S001G, Technoloy S014G, Technoloy S000, Technoloy C001, Technoloy C000 (Sumika Acrylic Sales Co., Ltd.), Lumirror U-type, Lumirror FX10, Lumirror SF20 (Toray Industries, Inc.), HK-53A (Higashiyama Film Co., Ltd.), Teflex FT3 (Teijin DuPont Films Ltd.), SCSina and SCA40 (Sekisui Chemical Co., Ltd.), Zeonor Film (Optes Co., Ltd.), and Arton Film (JSR Corporation).
[0076] (Optical Interference Layer) The optical film of the present invention may include other functional layers on its interior or surface, to the extent that it does not impair the optical properties. For example, it is preferable to have an optical interference layer to suppress interfacial reflection.
[0077] The optical interference layer may consist of a single layer, or it may be constructed by laminating two or more optical interference layers using methods such as bonding or sequential formation. The thickness of the single layer of optical interference is preferably in the range of 60 nm to 110 nm or 230 nm to 330 nm, more preferably in the range of 75 nm to 100 nm or 245 nm to 300 nm, and most preferably in the range of 80 nm to 95 nm or 260 nm to 285 nm.
[0078] For optically anisotropic layers and adhesive layers having arbitrary refractive indices, the preferred range for the optical interference layer can be generalized using the average refractive index of adjacent layers under the following conditions. That is, if the refractive index of one layer adjacent to the optical interference layer is nA and the average refractive index of the other layer is nL, then it is preferable that the refractive index nI of the optical interference layer is (nA × nL)¹ / ² - 0.03 ≤ nI ≤ (nA × nL)¹ / ² + 0.03, more preferably (nA × nL)¹ / ² - 0.02 ≤ nI ≤ (nA × nL)¹ / ² + 0.02, and most preferably (nA × nL)¹ / ² - 0.01 ≤ nI ≤ (nA × nL)¹ / ² + 0.01. By setting the refractive index of the optical interference layer within this range, the amplitude reflectance on both sides of the optical interference layer can be made to be of roughly the same magnitude, thereby effectively suppressing interfacial reflection. When using general liquid crystal materials and adhesive layers, the refractive index of the optical interference layer is preferably 1.50 to 1.70, and more preferably 1.53 to 1.59.
[0079] Materials that form the optical interference layer can include hard coat materials with crosslinked monomers and photoalignment films. Of these, photoalignment films are preferred because they also play a role in aligning liquid crystals when forming an optical anisotropy layer on top of them using liquid crystal materials.
[0080] <Method for Manufacturing Optical Films> The method for manufacturing optical films is not particularly limited, and known methods can be used. For example, an optical film can be manufactured by preparing first to third optical anisotropic layers and bonding them together in a predetermined order via an adhesion layer (e.g., an adhesive layer or a bonding agent layer). In this case, it is preferable from the viewpoint of productivity to perform the bonding continuously on a long roll. That is, so-called roll-to-roll bonding is desirable. After bonding the films, one or both of the temporary supports may be peeled off. Alternatively, after forming the first optical anisotropic layer, a composition for forming another optical anisotropic layer can be directly applied onto the first optical anisotropic layer, and then the composition can be cured to produce an optical film in which the optical anisotropic layers are directly adjacent to each other (directly laminated). Furthermore, the first to third optical anisotropic layers can be manufactured using an optical anisotropic layer forming composition containing a liquid crystal compound having polymerizable groups that can be formed.
[0081] The following describes in detail a method for producing optically anisotropic layers (first to third optically anisotropic layers) using an optically anisotropic layer-forming composition containing a liquid crystal compound having polymerizable groups.
[0082] The polymerizable liquid crystal compound (hereinafter referred to as "polymerizable liquid crystal compound") contained in the composition for forming an optically anisotropic layer is as described above. Depending on the characteristics of the optically anisotropic layer formed, rod-shaped liquid crystal compounds and disc-shaped liquid crystal compounds are appropriately selected. The content of the polymerizable liquid crystal compound in the composition for forming an optically anisotropic layer is preferably 60 to 99% by mass, and more preferably 70 to 98% by mass, based on the total solid content of the composition for forming an optically anisotropic layer. The solid content refers to the components that can form an optically anisotropic layer after the solvent has been removed, and is considered solid even if its state is liquid.
[0083] The composition for forming an optically anisotropic layer may contain compounds other than the liquid crystal compound having polymerizable groups. For example, the composition for forming the second optically anisotropic layer 14 preferably contains a chiral agent to twist-orient the liquid crystal compound. The chiral agent is added to twist-orient the liquid crystal compound, but if the liquid crystal compound is an optically active compound, such as having an asymmetric carbon in its molecule, the addition of a chiral agent is unnecessary. Also, depending on the manufacturing method and the twist angle, the addition of a chiral agent may not be necessary. The structure of the chiral agent is not particularly limited as long as it is compatible with the liquid crystal compound used in combination. Any known chiral agent (for example, described in "Liquid Crystal Device Handbook," edited by the 142nd Committee of the Japan Society for the Promotion of Science, Chapter 3, Section 4-3, Chiral Agents for TN and STN, p. 199, 1989) can be used. The amount of chiral agent used is not particularly limited and is adjusted to achieve the twist angle described above.
[0084] The composition for forming an optically anisotropic layer may contain a polymerization initiator. The polymerization initiator used is selected according to the type of polymerization reaction. Examples include thermal polymerization initiators and photopolymerization initiators. The content of the polymerization initiator in the composition for forming an optically anisotropic layer is preferably 0.01 to 20% by mass, and more preferably 0.5 to 10% by mass, based on the total solid content of the composition for forming an optically anisotropic layer.
[0085] Other components that may be included in the optically anisotropic layer-forming composition include, in addition to those mentioned above, polyfunctional monomers, orientation control agents (vertical orientation agents, horizontal orientation agents), surfactants, adhesion improvers, plasticizers, and solvents.
[0086] Methods for applying compositions for forming optically anisotropic layers include curtain coating, dip coating, spin coating, printing coating, spray coating, slot coating, roll coating, slide coating, blade coating, gravure coating, and wire bar coating.
[0087] Next, the formed coating film is subjected to an orientation treatment to orient the polymerizable liquid crystal compounds within the coating film. For example, when forming the first optical anisotropy layer 12A, the disc-shaped liquid crystal compounds are oriented vertically, so that the optical axes (axes perpendicular to the disc surface) of the disc-shaped liquid crystal compounds are aligned in the same direction. When forming the second optical anisotropy layer 14, the rod-shaped liquid crystal compounds are twisted and oriented. When forming the third optical anisotropy layer 16, the rod-shaped liquid crystal compounds are oriented vertically. When forming the fourth optical anisotropy layer, the disc-shaped liquid crystal compounds are oriented horizontally.
[0088] The orientation treatment can be performed by drying or heating the coating film. In the case of thermotropic liquid crystal compounds, the liquid crystal phase formed by the orientation treatment can be transitioned by changes in temperature or pressure. There are no particular restrictions on the conditions for heating the coating film, but the heating temperature is preferably 50 to 250°C, and more preferably 50 to 150°C. The heating time is preferably 10 seconds to 10 minutes. After heating the coating film, it may be cooled as needed before the curing treatment (light irradiation treatment) described later.
[0089] Next, the coating film on which the polymerizable liquid crystal compound is oriented is subjected to a curing treatment. The curing treatment method in this case is not particularly limited, but examples include light irradiation treatment and heat treatment. From the viewpoint of manufacturability, light irradiation treatment is preferred, and ultraviolet irradiation treatment is more preferred. The irradiation conditions for light irradiation treatment are not particularly limited, but 50 to 1000 mJ / cm² is preferred. 2 A certain irradiation dose is preferred. Furthermore, there are no particular restrictions on the atmosphere during the light irradiation treatment, but a nitrogen atmosphere is preferred.
[0090] (Manufacturing of optical film by bonding each layer) The optical film of the present invention can also be manufactured by laminating each optically anisotropic layer after manufacturing it in an individual process. Lamination can be performed using an adhesive layer such as an adhesive or tack.
[0091] From the viewpoint of suppressing interfacial reflection, it is preferable that the refractive index of the adhesive layer between each layer be adjusted (refractive index matching) to match the refractive index of the two layers adjacent to the adhesive layer. It is preferable that the refractive index of the adhesive layer is the value between the average in-plane refractive indices of the two layers adjacent to the adhesive layer. Here, for the first optical anisotropy layer and the second optical anisotropy layer, the average in-plane refractive index can be defined as the average value of the anomalous principal refractive index (ne) and the normal principal refractive index (no) of the horizontally oriented liquid crystal compound. For the third optical anisotropy layer, it can be considered to be the same as the normal principal refractive index (no) of the vertically oriented liquid crystal compound. Furthermore, the above refractive index relationship only needs to hold at any wavelength in the visible range, but the wavelength may be set according to the wavelength to be used. For example, it is preferable that the above relationship holds at a wavelength of 550 nm. It is preferable that the above refractive index relationship holds because it can suppress interfacial reflection between each layer and improve the ellipticity of the light rays obtained using the optical film. The refractive index of the adhesive layer is not particularly restricted as long as the above-mentioned refractive index relationship is satisfied. However, if the adjacent optical anisotropic layer is a liquid crystal compound, the refractive index range of the liquid crystal compound is generally around 1.51 to 1.60, so it is preferable that the refractive index of the adhesive layer be 1.51 to 1.60.
[0092] The refractive indices of the optically anisotropic layer and the adhesive layer can be measured using an Abbe refractive system, a spectroscopic ellipsometer, or the like. Alternatively, the in-plane refractive index can be calculated by measuring the p-wave and s-wave reflectances on the surface using a specular reflectance meter, and then determining the refractive index based on the measured reflectances.
[0093] There are no particular restrictions on the type of adhesive layer, but adhesives or tacks can be used. Examples of high refractive index adhesives include acrylic adhesives and epoxy adhesives. Examples of high refractive index tacks include acrylic adhesives, silicone adhesives, urethane adhesives, epoxy adhesives, and polyimide adhesives. For example, Japanese Patent Application Publication No. 2010-196064 discloses an acrylic adhesive with a refractive index of 1.49 to 1.60.
[0094] The thickness of the adhesive layer can be set arbitrarily, but from the viewpoint of reducing the thickness of the optical film and improving the smoothness of the optical film, it is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. Furthermore, if the adhesive layer is an adhesive, a thickness of 3 μm or more is preferable from the viewpoint of obtaining sufficient adhesive strength. If the adhesive layer is an adhesive, sufficient adhesive strength can be obtained even if the adhesive layer is 3 μm or less. In addition, if the thickness of the adhesive layer is 100 nm or less, visible light does not perceive the refractive index difference, and interfacial reflection can be suppressed more effectively, so a thickness of 100 nm or less is preferable.
[0095] One method for forming an adhesive layer with a thickness of 100 nm or less is to deposit a ceramic adhesive, such as a silicon dioxide (SiOx) layer, onto the adhesive surface of an optically anisotropic layer or a positive C plate. The adhesive surface can be subjected to surface modification treatments such as plasma treatment, corona treatment, and saponification treatment before bonding, or a primer layer can be applied. Furthermore, if there are multiple adhesive surfaces, the type and thickness of the adhesive layer can be adjusted for each surface.
[0096] Specifically, an adhesive layer with a thickness of 100 nm or less can be provided by, for example, the following procedure: (1) The layers to be laminated are bonded to a temporary support made of a glass substrate. (2) A SiOx layer with a thickness of 100 nm or less is formed on both the surface of the layer to be laminated and the surface of the layer to be laminated by vapor deposition or the like. Vapor deposition can be carried out using SiOx powder as the deposition source, for example, using a vapor deposition apparatus (model number ULEYES) manufactured by ULVAC, Inc. It is also preferable to apply plasma treatment to the surface of the formed SiOx layer. (3) After bonding the formed SiOx layers together, the temporary support is peeled off. Adhesion is preferably carried out at a temperature of, for example, 120°C.
[0097] The application of adhesives and tacks to each layer, the formation of adhesive layers such as the SiOx layer, and bonding may be carried out by roll-to-roll or sheet-fed methods. The roll-to-roll method is preferred from the viewpoint of improving productivity and reducing misalignment of each layer. On the other hand, the sheet-fed method is preferred because it is suitable for small-volume, high-mix production and because it allows for the selection of special bonding methods, such as those described above, where the thickness of the adhesive layer is 100 nm or less. Examples of known methods for applying adhesives and tacks to the substrate include roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet.
[0098] In the optical film of the present invention, it is also preferable that there are no adhesive layers between each layer. By directly applying the composition for forming the other optical anisotropic layer onto an already formed optical anisotropic layer, an optical film without adhesive layers between each layer can be manufactured. This is preferable because the absence of adhesive layers can suppress interfacial reflection between layers and improve the ellipticity of the light rays transmitted through the optical film.
[0099] [Circular Polarizer] The circular polarizer of the present invention is a circular polarizer having the optical film of the present invention described above and a polarizer. A circular polarizer is an optical element that converts natural light into circularly polarized light. The circular polarizer of the present invention having the above configuration is suitably used for anti-reflective applications in display devices such as liquid crystal displays (LCDs), plasma display panels (PDPs), organic electroluminescent displays (organic ELs), micro-LED displays, and cathode ray tube displays (CRTs). Furthermore, since the optical film of the present invention maintains a high ellipticity even after stretching, it can maintain high anti-reflective performance even when it is laminated to curved or curved surfaces after stretching in anti-reflective applications on such surfaces.
[0100] A polarizer can be any material that has the function of converting natural light into a specific linearly polarized light, for example, an absorptive polarizer. There are no particular restrictions on the type of polarizer, and commonly used polarizers can be used, for example, iodine-based polarizers, dye-based polarizers using dichroic substances, and polyene-based polarizers. Iodine-based polarizers and dye-based polarizers are generally made by adsorbing iodine or a dichroic dye onto polyvinyl alcohol and then stretching it. A protective film may be placed on one or both sides of the polarizer.
[0101] The polarizer is preferably formed using a composition containing a dichroic substance and a liquid crystal compound having polymerizable groups. Specifically, examples include visible light absorbing substances (dichroic dyes), luminescent substances (fluorescent substances, phosphorescent substances), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes, and inorganic substances (e.g., quantum rods). Conventionally known dichroic substances (dichroic dyes) can also be used. In the present invention, two or more dichroic substances may be used in combination. For example, from the viewpoint of making the light-absorbing anisotropic film closer to black, it is preferable to use in combination at least one dye compound having a maximum absorption wavelength in the range of 370 to 550 nm and at least one dye compound having a maximum absorption wavelength in the range of 500 to 700 nm.
[0102] The thickness of the polarizer is not particularly limited, but a thin design is desirable from the viewpoint of making the circular polarizer thinner and facilitating its attachment to curved or curved surfaces. For example, a thickness of 30 μm or less is preferred, 10 μm or less is more preferred, 6 μm or less is even more preferred, and 4 μm or less is most preferred.
[0103] The luminous efficiency correction single transmittance of the polarizer is not particularly limited, but is preferably 42% or higher, and more preferably 43% or higher, in terms of superior effects of the present invention. There is no particular upper limit, but is preferably 48% or lower. The luminous efficiency correction single transmittance is calculated by the following method: For the polarizer, the transmittance in the absorption axis direction (T) in the wavelength range of 380 to 780 nm is calculated using a spectrophotometer with an integrating sphere [JASCO Corporation's "V7100"]. 1 ) and transmittance (T) in the direction perpendicular to the absorption axis 2) is measured, and the single transmittance at each wavelength is calculated based on the following formula. Single transmittance (%) = (T 1 +T 2 ) / 2 The obtained single transmittance is subjected to visibility correction using the 2-degree field of view (C light source) of JIS Z 8701:1999 "Method of representing colors - XYZ color system and X 10 Y 10 Z 10 color system" to obtain a visibility-corrected single transmittance.
[0104] FIG. 2 shows a schematic cross-sectional view of one embodiment of the circularly polarizing plate 100A. FIG. 3 is a diagram showing the relationship between the absorption axis of the polarizer 20 and the respective in-plane slow axes of the first optically anisotropic layer 12A and the second optically anisotropic layer 14 in the circularly polarizing plate 100A shown in FIG. 2. The arrow of the polarizer 20 in FIG. 3 represents the absorption axis, and the arrows of the first optically anisotropic layer 12A and the second optically anisotropic layer 14 represent the in-plane slow axes in the respective layers. Further, FIG. 4 is a diagram showing the angular relationship between the absorption axis (broken line) of the polarizer 20 and the respective in-plane slow axes (solid lines) of the first optically anisotropic layer 12A and the second optically anisotropic layer 14 when observed from the white arrow in FIG. 2. The rotation angle of the in-plane slow axis is represented with the absorption axis of the polarizer 20 as a reference (0°), positive in the counterclockwise direction and negative in the clockwise direction, when observed from the white arrow in FIG. 2. The twist direction of the liquid crystal compound is determined as right-handed twist (clockwise) or left-handed twist (counterclockwise) based on the in-plane slow axis on the front side (polarizer 20 side) surface in the second optically anisotropic layer 14, when observed from the white arrow in FIG. 2.
[0105] As shown in FIG. 2, the circularly polarizing plate 100A includes a polarizer 20, a first optically anisotropic layer 12A, a second optically anisotropic layer 14, and a third optically anisotropic layer 16 in this order. As shown in FIGS. 3 to 4, when the angle formed by the absorption axis of the polarizer 20 and the in-plane slow axis of the first optically anisotropic layer 12A is φ a1 , φ a1The angle is 80°. More specifically, the in-plane slow axis of the first optical anisotropy layer 12A is rotated by -80° (80° clockwise) with respect to the absorption axis of the polarizer 20. In Figures 3 and 4, the in-plane slow axis of the first optical anisotropy layer 12A is shown at a position of -80°, but the present invention is not limited to this embodiment, and is preferably in the range of -40 to -95°, more preferably in the range of -50 to -85°, and even more preferably in the range of -65 to -85°. In Figure 4, the dashed line shows the case where the absorption axis of the polarizer 20 is shown, but the dashed line in Figure 4 may also be the transmission axis of the polarizer 20. That is, the polarizers may be stacked in orthogonal directions. By rotating the orientation of the polarizer by 90° in this way, it is possible to switch whether the circularly polarized light obtained by the circular polarizer is right-circularly polarized or left-circularly polarized.
[0106] As shown in Figure 3, the in-plane slow axis on the polarizer 20 side surface 121A of the first optical anisotropy layer 12A and the in-plane slow axis on the second optical anisotropy layer 14 side surface 122A of the first optical anisotropy layer 12A are parallel.
[0107] As shown in Figures 3 and 4, the angle between the in-plane slow axis of the first optical anisotropy layer 12A and the in-plane slow axis of the second optical anisotropy layer 14 on the surface 141 facing the first optical anisotropy layer 12A is φ a2 Therefore, φ a2 The angle is 0°. That is, the orientation of the in-plane slow axis on the surface 141 of the second optical anisotropy layer 14 on the first optical anisotropy layer 12A side coincides with the orientation of the in-plane slow axis of the first optical anisotropy layer 12A. However, the present invention is not limited to this embodiment, and it is preferable that the angle between the in-plane slow axis of the first optical anisotropy layer 12A and the in-plane slow axis on the surface 141 of the second optical anisotropy layer 14 on the first optical anisotropy layer 12A side is in the range of 0 to 20°.
[0108] As described above, the second optical anisotropy layer 14 is a layer on which rod-shaped liquid crystal compounds, twisted and oriented along a helical axis extending in the thickness direction, are fixed. Therefore, as shown in Figures 3 to 4, the in-plane slow phase axis on the surface 141 of the second optical anisotropy layer 14 on the side of the first optical anisotropy layer 12A and the in-plane slow phase axis on the surface 142 of the second optical anisotropy layer 14 opposite to the side of the first optical anisotropy layer 12A form a twist angle. The angle between the in-plane slow phase axis on the surface 141 of the second optical anisotropy layer 14 on the side of the first optical anisotropy layer 12A and the in-plane slow phase axis on the surface 142 of the second optical anisotropy layer 14 opposite to the side of the first optical anisotropy layer 12A is 76°. More specifically, the torsion direction of the rod-shaped liquid crystal compound in the second optical anisotropy layer 14 is left-handed (counterclockwise), and the torsion angle is 76°. Therefore, the angle between the absorption axis of the polarizer 20 and the in-plane slow axis on the surface 142 of the second optical anisotropy layer 14 opposite to the first optical anisotropy layer 12A side is φ a3 Therefore, φ a3 The angle is 4°. More specifically, if the absorption axis direction of the polarizer 20 is 0°, the orientation of the in-plane slow axis on the surface 142 of the second optical anisotropy layer 14 opposite to the first optical anisotropy layer 12A side is -4°. In Figures 3 and 4, the twist angle of the rod-shaped liquid crystal compound in the second optical anisotropy layer 14 is shown to be 76°, but the invention is not limited to this embodiment, and as described above, the twist angle of the rod-shaped liquid crystal compound is preferably within the range of 80 ± 30°. In other words, the angle between the in-plane slow axis on the surface 141 of the second optical anisotropy layer 14 on the first optical anisotropy layer 12A side and the in-plane slow axis on the surface 142 of the second optical anisotropy layer 14 opposite to the first optical anisotropy layer 12A side is preferably within the range of 80 ± 30°. Furthermore, while Figures 3 and 4 detail the configuration in which the twist direction of the rod-shaped liquid crystal compound is counterclockwise, a clockwise configuration is also possible if the predetermined angular relationship is satisfied. More specifically, when observing the circular polarizer 100A from the polarizer 20 side, the in-plane slow axis of the first optical anisotropy layer 12A is rotated 80° counterclockwise with respect to the absorption axis of the polarizer 20, and the twist direction of the rod-shaped liquid crystal compound in the second optical anisotropy layer 14 is 76° clockwise (right-handed twist).
[0109] The circular polarizer described above may have other components besides the optical film and polarizer. The circular polarizer may have an adhesion layer between the optical film and the polarizer. Examples of the adhesion layer include the known adhesive layer and adhesive layer described above. Suitable adhesives include, for example, an adhesive made of an aqueous solution of polyvinyl alcohol resin, a curable adhesive composition containing a cationic polymerizable compound that hardens by irradiation with active energy rays or heating, or a curable adhesive composition containing a radical polymerizable compound. The thickness of the adhesive layer is preferably about 0.01 to 20 μm, more preferably 0.01 to 10 μm, and even more preferably 0.05 to 5 μm. If the thickness of the adhesive layer is within this range, no lifting or peeling will occur between the laminated optical anisotropic layer and the polarizer, and practically satisfactory adhesive strength can be obtained.
[0110] Furthermore, from the viewpoint of productivity, it is preferable to perform the lamination of the optical film and polarizer of the present invention continuously on a long roll. That is, so-called roll-to-roll lamination is desirable. Alternatively, the temporary support of the film may be peeled off after lamination. If the optical film is composed of multiple optical anisotropic layers and these are supplied separately, the optical anisotropic layers may be laminated to each other and then laminated to the polarizer, or the multiple optical anisotropic layers may be laminated sequentially to the polarizer.
[0111] Furthermore, heating or pressurizing the bonded parts in an autoclave or similar device is preferable from the viewpoint of improving adhesion.
[0112] [Image Display Device] The image display device of the present invention comprises the circular polarizing plate of the present invention, that is, the optical film and polarizer of the present invention. The image display device of the present invention may also have an image display panel, and examples of image display panels include liquid crystal display panels, organic EL display panels, and micro LED display panels.
[0113] The image display device of the present invention may have an image display panel, the optical film of the present invention, and a polarizer in this order. It is preferable to use an absorbing linear polarizer as the polarizer. In this case, the optical film of the present invention can provide excellent anti-reflective properties for external light incident from the front and obliquely.
[0114] Furthermore, the image display device of the present invention may have the optical film of the present invention on the side opposite to the image display panel relative to the polarizer. In this case, the optical film of the present invention can convert the light emitted from the image display device into circularly polarized light with high ellipticity. Such an image display device can be suitably used as an image display device for virtual reality display devices employing pancake lenses or for augmented reality display devices.
[0115] Furthermore, the image display device of the present invention may include, in addition to the optical film of the present invention, known components for image display devices such as an anti-reflective layer, an ultraviolet absorbing layer, an impact absorbing layer, a fingerprint-resistant layer, and a hard coat layer.
[0116] [Reflective Circular Polarizer] The reflective circular polarizer of the present invention is a reflective circular polarizer having the optical film of the present invention described above and a reflective polarizer. Examples of reflective polarizers include multilayer polymer reflective polarizers (e.g., APF or DBEF from 3M), cholesteric mirrors, reflective wire grid polarizers (e.g., WGF from Asahi Kasei), and metasurface polarizers. Among these, it is preferable to use a reflective circular polarizer or a reflective linear polarizer.
[0117] [Lens] The lens of the present invention comprises the reflective circular polarizer of the present invention, that is, the optical film of the present invention, and a reflective polarizer.
[0118] The lens of the present invention may have a lens substrate, and it is preferable that it has a lens substrate. Glass or transparent resin is preferred as the material of the lens substrate. It is preferable that the lens substrate does not change the polarization state of the light rays, and it is desirable that the phase difference (Re and Rth) is zero. Furthermore, the lens of the present invention may be a combination of multiple lens substrates.
[0119] The lens may have layers other than the optical film, reflective linear polarizer, and lens substrate of the present invention. Examples of other layers include a half-mirror, an anti-reflective layer, an ultraviolet absorbing layer, and a hard coat layer. Examples of a half-mirror include a vapor-deposited film of a metal such as aluminum.
[0120] The lens may also further include an absorptive linear polarizer. The reflective linear polarizer and the absorptive linear polarizer may be included in a laminated optical body provided together with the optical film. Furthermore, if the lens consists of a combination of multiple lens substrates, the optical film, reflective linear polarizer, and absorptive linear polarizer of the present invention may each be bonded to a separate lens substrate.
[0121] Specific examples of the lens configuration of the present invention are as follows: • A lens having a reflective linear polarizer, the optical film of the present invention, a lens substrate, and a half-mirror in that order. • A lens having an absorptive linear polarizer, a reflective linear polarizer, the optical film of the present invention, a lens substrate, and a half-mirror in that order. • A lens having the optical film of the present invention, a reflective linear polarizer, an absorptive linear polarizer, and a lens substrate in that order. Preferred embodiments of each component included in the above configuration examples are as described above.
[0122] The shape of the lens substrate is not particularly limited, but it is preferable that at least one surface is curved. When the lens substrate has a curved surface, aberrations in the displayed image can be corrected in a virtual reality display device, resulting in a higher quality display. The curved surface may be part of a sphere or an aspherical surface.
[0123] As lens substrates, convex lenses, concave lenses, and meniscus lenses can be used. As convex lenses, biconvex lenses, plano-convex lenses, and convex meniscus lenses can be used. As concave lenses, biconcave lenses, plano-concave lenses, and concave meniscus lenses can be used.
[0124] The lens of the present invention can be suitably used as a pancake lens in a virtual reality display device.
[0125] [Molding Method] As a method for attaching the optical film and circular polarizer of the present invention to a curved or curved surface, for example, thermoforming or vacuum forming can be used. Specifically, examples include insert molding as described in Japanese Patent Application Publication No. 2004-322501, vacuum forming as described in International Publication No. 2010 / 1867 and Japanese Patent Application Publication No. 2012-116094, injection molding, pressure forming, reduced pressure coating, in-mold transfer, and die pressing. Heating during molding is also preferable, preferably between 80°C and 170°C, and more preferably between 100°C and 150°C. Furthermore, heating or pressurizing in an autoclave or the like after molding is also preferable from the viewpoint of improving adhesion.
[0126] [Virtual Reality Display Device] The virtual reality display device of the present invention is a virtual reality display device having the lens of the present invention described above. Figure 5 schematically shows an example of the configuration of a virtual reality display device using the lens of the present invention. The virtual reality display device 1000 shown in Figure 5 has a lens 2 and an image display device 3. The lens 2 has a reflective linear polarizer 21, a first optical film 22, a lens substrate 23, and a half mirror 24 in this order. The image display device 3 has a second optical film 31, an absorptive linear polarizer 32, and an image display panel 33.
[0127] In the virtual reality display device 1000 shown in Figure 5, both the first optical film 22 and the second optical film 31 are optical films of the present invention. That is, the lens 2 shown in Figure 5 is an example of the lens configuration of the present invention, and the image display device 3 is an example of the image display device configuration of the present invention.
[0128] To explain the operation of the image display device and the virtual reality display device using the lens of the present invention, Figure 6 schematically shows an example of the configuration of a conventional virtual reality display device. The virtual reality display device 1001 shown in Figure 6 has, from left to right in the figure, a reflective linear polarizer 100, a first phase difference layer 200, a lens substrate 600, a half mirror 300, a second phase difference layer 400, and an image display device 500.
[0129] The virtual reality display device 1001 can reduce the overall thickness of the headset by folding light rays using the following mechanism. Specifically, a portion of the light rays emitted from the image display device 500, a light ray 70, is converted to circular polarization by the second phase difference layer 400, then passes through the half mirror 300, is converted to linear polarization by the first phase difference layer 200, and then incident on the reflective linear polarizer 100 and reflected. After that, the light ray 70 passes through the first phase difference layer 200 again, is converted to circular polarization, and is reflected by the half mirror 300. At this time, the polarization state of the light ray 70 is converted to circular polarization in the opposite direction to the circular polarization before reflection by the half mirror 300. The light ray 70 reflected by the half mirror 300 then passes through the first phase difference layer 200 again, is converted to linear polarization, and is incident on the reflective linear polarizer 100. At this time, the light rays incident on the reflective linear polarizer 100 are linearly polarized, perpendicular to the linear polarization when they first entered the reflective linear polarizer 100. Therefore, they pass through the reflective linear polarizer 100 and the light rays 70 are delivered to the user's eyes. In this way, the virtual reality display device 1001 can reduce the overall thickness of the headset by folding the light rays 70 between the half mirror 300 and the reflective linear polarizer 100.
[0130] According to the inventors' research, as shown in Figure 7, in the conventional virtual reality display device 1001, a portion of the light rays (light rays 71) emitted from the image display device 500 are emitted without being refolded between the half mirror 300 and the reflective linear polarizer 100, and may be perceived as a ghost image. The inventors believe that the reason for this is that some of the light rays emitted from the image display device 500, within a certain wavelength range, are not converted into perfectly linearly polarized light when they pass through the second phase difference layer 400, then the half mirror 300, and then the first phase difference layer 200, but instead become elliptically polarized light. The reasons why the light rays become elliptically polarized are thought to be insufficient ellipticity of the circularly polarized light obtained by the first phase difference layer 200 or the second phase difference layer 400, or that the in-plane phase difference (Re) of the first phase difference layer 200 and the second phase difference layer 400 are different, or that the lagging axis orientations of the first phase difference layer 200 and the second phase difference layer 400 are not orthogonal to each other.
[0131] In contrast, the image display device 3 of the present invention includes an absorbing linear polarizer 32, an image display panel 33, and a second optical film 31, which is the optical film of the present invention. Since the optical film of the present invention can make the in-plane phase difference λ / 4 phase difference over a wide wavelength range of visible light, the second optical film 31 can convert linearly polarized light to circularly polarized light with high ellipticity, and can also convert circularly polarized light to linearly polarized light over a wide wavelength range of visible light.
[0132] In an image display device 3 having such a second optical film 31, the light rays 70 emitted from the image display panel 33 and transmitted through the absorbing linear polarizer 32, the second optical film 31, and the half mirror 24 become ideally circularly polarized over a wide wavelength range in the visible region. Therefore, it is possible to reduce the amount of light rays (light rays 71 shown in Figure 7) that are emitted without traveling back and forth between the reflective linear polarizer 21 and the half mirror 24, resulting in ghost images.
[0133] Furthermore, the light rays that pass through the half-mirror 24 on the first pass and reach the first optical film 22 are ideally circularly polarized over a wide wavelength range of visible light and have no polarization axis. Therefore, when assembling the lens 2 having the reflective linear polarizer 21 and the first optical film 22, even if the slow axis orientation of the first optical film 22 is not perpendicular to the slow axis orientation of the second optical film 31, the ghost image does not increase. In other words, when manufacturing the virtual reality display device 1000 to which the image display device 3 is applied, precise angle adjustment when assembling the lens 2 becomes unnecessary, thus greatly simplifying the lens assembly process. This can contribute to reducing the manufacturing cost of the virtual reality display device. Furthermore, the optical film of the present invention can convert linearly polarized light incident at an oblique angle into circularly polarized light with high ellipticity. In virtual reality display devices using pancake lenses, there are also light rays that are emitted from the image display device at a large angle, and these can cause ghost images, but the image display device using the optical film of the present invention can effectively suppress ghost images caused by such light rays.
[0134] Next, the operation of the lens of the present invention will be described.
[0135] According to the inventors' investigation, as shown in Figure 8, in the conventional virtual reality display device 1000, a portion of the light rays (light rays 72) emitted from the image display device 500 sometimes travel back and forth between the half mirror 300 and the reflective linear polarizer 100 two or more times, resulting in the appearance of a ghost image. The inventors believe that the cause of this is that some of the light rays (linearly polarized) reflected by the reflective linear polarizer 100, within a certain wavelength range, are not converted to perfectly circular polarization when transmitted through the first phase difference layer 200, but instead become elliptically polarized. When the light rays emitted from the first phase difference layer 200 are elliptically polarized, they are reflected by the half mirror 300 and then transmitted back through the first phase difference layer 200 again. The light rays contain a component parallel to the reflection axis of the reflective linear polarizer 100, which is then reflected again by the reflective linear polarizer 100, resulting in the generation of light rays 72 that travel back and forth repeatedly.
[0136] In contrast, the lens 2 of the present invention has a first optical film 22, which is the optical film of the present invention. Since the optical film of the present invention can make the in-plane phase difference a λ / 4 phase difference over a wide wavelength range of visible light, the first optical film 22 can convert linearly polarized light into ideal circularly polarized light and also convert circularly polarized light into ideal linearly polarized light over a wide wavelength range of visible light.
[0137] In a lens 2 having such a first optical film 22, linearly polarized light reflected from the reflective linear polarizer 21 is converted into ideal circularly polarized light over a wide wavelength range in the visible region when it passes through the first optical film 22. Next, when reflected by the half mirror 24, the light ray is converted into circularly polarized light in the opposite direction to the circularly polarized light before reflection by the half mirror 24, but this is also ideally circularly polarized light. Furthermore, the light ray that has passed through the first optical film 22 again is converted into ideal linearly polarized light and transmits through the reflective linear polarizer 21 with high efficiency. In other words, it is possible to reduce the number of light rays that travel back and forth between the reflective linear polarizer 21 and the half mirror 24 two or more times (light rays 72 shown in Figure 8), and the generation of ghost images can be suppressed. Furthermore, the optical film of the present invention can also convert linearly polarized light incident at an oblique angle into circularly polarized light with high ellipticity. In virtual reality display devices using pancake lenses, light rays may be incident on the lens surface at a very large angle, which can cause ghost images. However, the lens using the optical film of the present invention can effectively suppress ghost images caused by such light rays.
[0138] Furthermore, as shown in Figures 5 to 8, pancake lenses sometimes have an optical film bonded to the spherical or aspherical surface of the optical lens in order to obtain a wide field of view, low chromatic aberration, low distortion, and excellent MTF (modulation transfer function). In this case, the optical film may be stretched and molded isotropically in the central part of the lens. However, the stretching of the optical film during this molding process can change the phase difference that the optical film originally had, resulting in a decrease in the resulting ellipticity, which can worsen ghost images or reduce contrast. In contrast, the optical film of the present invention can maintain a high ellipticity even when stretched isotropically. Therefore, the lens 2 using the optical film of the present invention can effectively suppress ghost images caused by such molding.
[0139] As described above, the optical film of the present invention is particularly useful in various optical devices, such as virtual reality display devices and augmented reality display devices, due to its structure and characteristics. High-quality display performance can be achieved by devising the combination and arrangement of each layer.
[0140] The features of the present invention will be further described in detail below with reference to examples. The materials, amounts used, proportions, processing content, and processing procedures shown below can be modified as appropriate, as long as they do not depart from the spirit of the present invention. Furthermore, configurations other than those shown below are also possible, as long as they do not depart from the spirit of the present invention.
[0141] [Example 1] <Preparation of optical film> (Preparation of cellulose acylate film) The following composition was placed in a mixing tank, stirred, and then heated at 90°C for 10 minutes. The resulting composition was then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content concentration of the dope was 23.5% by mass, and the solvent of the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).
[0142] --------------------------------------------------------------------------- Cellulose acylate dope ------------------------------------------------------------ Cellulose acylate (acetyl substitution degree 2.86, viscosity-average degree of polymerization 310) 100 parts by mass of sugar ester compound 1 (shown in formula (S4) below) 6.0 parts by mass of sugar ester compound 2 (shown in formula (S5) below) 2.0 parts by mass of silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 parts by mass of solvent (methylene chloride / methanol / butanol)
[0143]
[0144]
[0145] The dope prepared as described above was cast using a drum film-forming machine. The dope was cast from the die onto a metal support cooled to 0°C, and then the resulting web (film) was peeled off. The drum was made of stainless steel (SUS).
[0146] After the casting process, the obtained web (film) was peeled from the drum and dried for 20 minutes in a tenter device at 30-40°C during film transport, using clips to hold both ends of the web in place. Subsequently, the web was further dried by zone heating while being transported on a roll. The obtained web was knurled and then wound up. The resulting cellulose acylate film had a thickness of 40 μm, an in-plane retardation of 1 nm at a wavelength of 550 nm, and a thickness-direction retardation of 26 nm at a wavelength of 550 nm.
[0147] The aforementioned cellulose acylate film is passed through a dielectric heating roll at a temperature of 60°C to raise the film surface temperature to 40°C. Then, an alkaline solution with the composition shown below is applied to the band surface of the film using a bar coater at a rate of 14 ml / m². 2 The material was coated and then transported for 10 seconds under a steam-type far-infrared heater manufactured by Noritake Co., Ltd., heated to 110°C. Subsequently, using the same bar coater, 3 ml / m of pure water was applied. 2 The film was then applied. Next, it was washed with water using a fountain coater and dewatered with an air knife three times, and then transported to a 70°C drying zone for 10 seconds to dry, thereby producing an alkaline saponified cellulose acylate film.
[0148] -------------------------------------------------- Alkaline solution -------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.8 parts by mass Isopropanol 63.7 parts by mass Surfactant: C 14 H 29 O(CH2CH2O) 20H 1.0 parts by mass Propylene glycol 14.8 parts by mass --------------------------------------------------
[0149] (Formation of the alignment film) An alignment film coating solution 1 with the following composition was continuously applied to the surface of a cellulose acylate film that had undergone alkali saponification treatment using a #14 wire bar. The resulting coating was then dried with hot air at 60°C for 60 seconds, and then with hot air at 100°C for 120 seconds to obtain the alignment film 1.
[0150] -------------------------------------------------- Orientation film coating solution 1 -------------------------------------------------- Modified polyvinyl alcohol as shown below 28 parts by mass Citric acid ester (AS3, manufactured by Sankyo Chemical Co., Ltd.) 1.2 parts by mass Photopolymerization initiator (Irgacure 2959, manufactured by BASF) 0.84 parts by mass Glutaraldehyde 2.8 parts by mass Water 699 parts by mass Methanol 226 parts by mass --------------------------------------------------
[0151] Modified polyvinyl alcohol
[0152] (Formation of optically anisotropic layer (A1)) The orientation film 1 prepared above was continuously subjected to rubbing. At this time, the longitudinal direction of the long film (cellulose acetate film) and the transport direction were parallel, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was set to 80°. Taking the width direction of the film as the angle reference (0°), and observing the film from the side being rubbed, when the counterclockwise direction is represented as a positive value, the longitudinal direction of the film (transport direction) is 90°. At this time, the rotation axis of the rubbing roller is -10°.
[0153] On the alignment film treated with the rubbing process described above, an optically anisotropic layer-forming composition (A1) containing a disc-shaped liquid crystal compound of the following composition was applied using a Gieser coating machine to form a composition layer. Subsequently, the obtained composition layer was heated with 110°C hot air for 2 minutes to dry the solvent and mature the alignment of the disc-shaped liquid crystal compound. Then, the obtained composition layer was irradiated with UV light at 80°C (500 mJ / cm²). 2 The orientation of the disc-shaped liquid crystal compound was fixed by performing the following procedure, and an optical anisotropy layer (A1) corresponding to the second optical anisotropy layer was formed. The average thickness of the optical anisotropy layer (A1) was 1.6 μm. The in-plane retardation (i.e., Δnd) at a wavelength of 550 nm was 196 nm. The average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface. Furthermore, the angle of the in-plane slow axis of the optical anisotropy layer (A1) was parallel to the rotation axis of the rubbing roller, with the film width direction taken as 0°, and when observed from the optical anisotropy layer (A1) side and the counterclockwise direction represented as a positive value, the in-plane slow axis direction of the optical anisotropy layer (A1) was -10°.
[0154] -------------------------------------------------- Composition for forming an optically anisotropic layer (A1) -------------------------------------------------- 80 parts by mass of the following disc-shaped liquid crystal compound 1 20 parts by mass of the following disc-shaped liquid crystal compound 2 20 parts by mass of the following vertical alignment agent 1 2 parts by mass of the following foaming inhibitor 1 2 parts by mass of the following acrylate monomer 1 5 parts by mass of the following surfactant 1 0.1 parts by mass of the following photopolymerization initiator (Api307, manufactured by Shenzhen UV-ChemTech LTD) 4 parts by mass of methyl ethyl ketone 102 parts by mass of cyclopentanone 238 parts by mass --------------------------------------------------
[0155] Disc-shaped liquid crystal compound 1
[0156] Disc-shaped liquid crystal compound 2
[0157] Vertical alignment agent 1
[0158] Foam inhibitor 1
[0159] Acrylate monomer 1
[0160] Surfactant 1 [A to C in each repeating unit represent the content (mass%) relative to the total repeating units, with a / b / c = 70 / 25 / 5. Weight-average molecular weight: 18500.]
[0161] (Formation of optically anisotropic layer (C1)) An optically anisotropic layer-forming composition (C1) containing a rod-shaped liquid crystal compound of the following composition was applied to the cellulose acylate film prepared above using a Gieser coating machine to form a composition layer. Then, holding both ends of the film, a cooling plate (9°C) was placed on the side of the film where the coating was formed, at a distance of 5 mm from the film, and a heater (75°C) was placed on the opposite side of the film where the coating was formed, at a distance of 5 mm from the film, and the film was dried for 2 minutes. Next, the obtained film was heated with hot air at 60°C for 1 minute, and while purging with nitrogen to maintain an atmosphere with an oxygen concentration of 100 ppm by volume or less, it was irradiated with a 365 nm UV-LED at a dose of 100 mJ / cm². 2 The surface was irradiated with ultraviolet light. Subsequently, an optically anisotropic layer (C1) was formed on the resulting coating by annealing it with hot air at 120°C for 1 minute. The resulting optically anisotropic layer (C1) was then exposed to UV light (ultra-high pressure mercury lamp; UL750; manufactured by HOYA) at room temperature, passing through a wire grid polarizer, at a rate of 7.9 mJ / cm². 2By irradiating with a wavelength of 313 nm, a composition layer with orientation control capability was formed on the surface. The thickness of the formed optically anisotropic layer (C1) was 0.7 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -100 nm. That is, if Δnd is defined as the product of Δn in the thickness direction and the thickness d, then Δnd was 100 nm. The average inclination angle of the rod-shaped liquid crystal compound with respect to the film surface in the direction of the long axis was 90°, confirming that it was oriented perpendicular to the film surface.
[0162] -------------------------------------------------- Composition for forming an optically anisotropic layer (C1) -------------------------------------------------- The following rod-shaped liquid crystal compound (A) 100 parts by mass Polymerizable monomer (A-400, manufactured by Shin Nakamura Chemical Industry Co., Ltd.) 4.0 parts by mass Polymerization initiator S-1 (oxime type) 5.0 parts by mass Photoacid generator D-1 3.0 parts by mass Polymer M-1 2.0 parts by mass Vertical alignment agent S01 2.0 parts by mass Photo-aligning polymer A-1 2.0 parts by mass Methyl ethyl ketone 42.3 parts by mass Methyl isobutyl ketone 627.5 parts by mass --------------------------------------------------
[0163] Rod-shaped liquid crystal compound (A) (a mixture of the following compounds, corresponding to a forward-wavelength dispersive liquid crystal compound)
[0164] Polymerization initiator S-1
[0165] Photoacid Generator D-1
[0166] Polymer M-1 [The numerical values within each repeating unit represent the content (mass%) relative to the total number of repeating units. The content of the repeating unit on the left was 80% by mass, and the content of the repeating unit on the right was 20% by mass. Weight-average molecular weight: 48000]
[0167] Vertical alignment agent S01
[0168] Photo-oriented polymer A-1 [In the following formula, a, b, and c represent the content (mass%) of each repeating unit relative to the total number of repeating units, where a is 34% by mass, b is 26% by mass, and c is 40% by mass. The weight-average molecular weight is 100,000. Me represents a methyl group.]
[0169] (Formation of optically anisotropic layer (B1)) Next, an optically anisotropic layer-forming composition (B1) containing a rod-shaped liquid crystal compound of the following composition was applied to the optically anisotropic layer (C1) prepared above using a Gieser coating machine, and heated with 80°C hot air for 60 seconds. Subsequently, the obtained composition layer was irradiated with UV at 80°C (500 mJ / cm²). 2 The orientation of the liquid crystal compound was fixed by performing the following procedure to form an optically anisotropic layer (B1). The average thickness of the optically anisotropic layer (B1) was 2.7 μm, and Δnd at a wavelength of 550 nm was 197 nm. The liquid crystal compound was twisted to the left, with a twist angle of 76°. The in-plane slow axis direction of the optically anisotropic layer (B1) (orientation axis angle of the liquid crystal compound) was 10° on the air side and 86° on the side in contact with the optically anisotropic layer (C1), when the width direction of the film is taken as 0° and the counterclockwise direction is expressed as a positive value when observed from the optically anisotropic layer (B1) side.
[0170] -------------------------------------------------- Composition for forming an optically anisotropic layer (B1) -------------------------------------------------- The above rod-shaped liquid crystal compound (A) 26 parts by mass The following rod-shaped liquid crystal compound (B) 36 parts by mass The following rod-shaped liquid crystal compound (C) 17 parts by mass The following rod-shaped liquid crystal compound (D) 16 parts by mass The following rod-shaped liquid crystal compound (E) 4 parts by mass The above polymerization initiator S-1 0.5 parts by mass The following surfactant 2 0.04 parts by mass The following left-handed chiral agent (L1) 0.18 parts by mass Methyl ethyl ketone 54 parts by mass Cyclopentanone 181 parts by mass --------------------------------------------------
[0171] Rod-shaped liquid crystal compound (B) (corresponds to an inverse wavelength-dispersive liquid crystal compound. tBu represents a tert-butyl group.)
[0172] Rod-shaped liquid crystal compound (C) (corresponds to inverse wavelength dispersive liquid crystal compound)
[0173] Rod-shaped liquid crystal compound (D) [This corresponds to an inverse wavelength-dispersive liquid crystal compound; the group adjacent to the acryloyloxy group in the following formula represents a propylene group (a group in which a methyl group is substituted for an ethylene group).]
[0174] Rod-shaped liquid crystal compound (E) (Me represents a methyl group.)
[0175] Surfactant 2 [The numerical value in each repeating unit represents the content (mass %) relative to the total repeating units. Weight-average molecular weight: 18000]
[0176] Left-hand torsion chiral agent (L1) (Bu represents a butyl group.)
[0177] Following the procedure described above, a laminate (B1-C1) was fabricated in which an optically anisotropic layer (C1) and an optically anisotropic layer (B1) were directly laminated onto a long cellulose acylate film.
[0178] The surface side of the optically anisotropic layer (A1) formed on the long cellulose acylate film prepared above and the surface side of the optically anisotropic layer (B1) of the laminate (B1-C1) formed on the long cellulose acylate film prepared above were bonded together using Lintec's adhesive sheet "NCF-D692(5)" (thickness 5um) such that the longitudinal direction of the optically anisotropic layer (A1) and the longitudinal direction of the optically anisotropic layer (B1) were parallel. At this time, the orientation of the in-plane slow axis on the surface of the optically anisotropic layer (B1) facing the optically anisotropic layer (A1) coincided with the orientation of the slow axis of the optically anisotropic layer (A1). Next, the cellulose acylate film and orientation film 1 on the optically anisotropic layer (A1) side were peeled off, exposing the surface of the optically anisotropic layer (A1) that was in contact with the cellulose acylate film. In this way, an optical film (C1-B1-PSA-A1) was obtained in which an optically anisotropic layer (C1), an optically anisotropic layer (B1), and an optically anisotropic layer (A1) were laminated in this order on a long cellulose acylate film.
[0179] [Example 2] <Fabrication of Optical Film> (Formation of Optical Anisotropic Layer (A2)) An optical anisotropic layer (A2) was fabricated using the same procedure as for the optical anisotropic layer (A1) described above. The obtained optical anisotropic layer (A2) had an average thickness of 1.6 μm, an in-plane retardation of 196 nm at a length of 550 nm, and an in-plane slow phase axis direction of -10°. In addition, the average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0180] (Formation of optically anisotropic layer (B2)) An optically anisotropic layer (B2) was formed in the same manner as for the optically anisotropic layer (B1) described above, except that the optically anisotropic layer forming composition (B1) described above was applied to the optically anisotropic layer (A2) prepared above using a Gieser coating machine. The average thickness of the optically anisotropic layer (B2) was 2.7 μm, and Δnd at a wavelength of 550 nm was 197 nm. The liquid crystal compound was twisted to the left, and the twist angle was 76°. The in-plane slow axis direction of the optically anisotropic layer (B2) (orientation axis angle of the liquid crystal compound) coincided with the in-plane slow axis direction of the optically anisotropic layer (A2) on the side in contact with the optically anisotropic layer (A2). Furthermore, the in-plane slow phase axis direction at the air interface was 94°, when the film width direction was taken as 0° and observed from the optical anisotropy layer (B2) side, with counterclockwise direction represented by a positive value.
[0181] Following the procedure described above, a laminate (A2-B2) was fabricated in which an optically anisotropic layer (A2) and an optically anisotropic layer (B2) were directly laminated onto a long cellulose acylate film.
[0182] (Formation of optically anisotropic layer (C2)) An optically anisotropic layer (C2) was fabricated using the same procedure as for the optically anisotropic layer (C1) described above. The obtained optically anisotropic layer (C2) had a film thickness of 0.7 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -100 nm. Furthermore, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0183] The surface side of the optically anisotropic layer (B2) of the laminate (A2-B2) prepared above and the surface side of the optically anisotropic layer (C2) prepared above were bonded together using Lintec's adhesive sheet "NCF-D692 (5)" so that their longitudinal directions were parallel to each other. Next, the cellulose acylate film and orientation film 1 on the optically anisotropic layer (A2) side of the laminate (A2-B2) were peeled off, exposing the surface of the optically anisotropic layer (A2) that was in contact with the cellulose acylate film. In this way, an optical film (C2-PSA-B2-A2) was obtained in which the optically anisotropic layer (C2), optically anisotropic layer (B2), and optically anisotropic layer (A2) were laminated in this order on a long cellulose acylate film.
[0184] [Example 3] <Fabrication of Optical Film> (Formation of Optical Anisotropic Layer (A3)) An optical anisotropic layer (A3) was fabricated using the same procedure as for the optical anisotropic layer (A1) described above, except that the film thickness and the angle of the rubbing treatment were adjusted. The obtained optical anisotropic layer (A3) had an average thickness of 1.6 μm, an in-plane retardation of 194 nm at a length of 550 nm, and an in-plane slow phase axis direction of -11°. In addition, the average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0185] (Formation of optically anisotropic layer (B3)) An optically anisotropic layer (B3) was formed on the optically anisotropic layer (A3) prepared above using the same procedure as for the optically anisotropic layer (B2), except that the optically anisotropic layer formation composition containing the rod-shaped liquid crystal compound was replaced with the optically anisotropic layer formation composition (B3) described below, and the film thickness was adjusted. The average thickness of the optically anisotropic layer (B3) was 2.0 μm, and Δnd at a wavelength of 550 nm was 191 nm. The liquid crystal compound was twisted to the left, and the twist angle was 77°. The in-plane slow axis direction of the optically anisotropic layer (B3) (orientation axis angle of the liquid crystal compound) coincided with the in-plane slow axis direction of the optically anisotropic layer (A3) on the side in contact with the optically anisotropic layer (A3). Furthermore, the in-plane slow phase axis direction at the air interface was 92°, when the film width direction was taken as 0° and observed from the optical anisotropy layer (B3) side, with counterclockwise direction represented by a positive value.
[0186] -------------------------------------------------- Composition for forming an optically anisotropic layer (B3) -------------------------------------------------- The above rod-shaped liquid crystal compound (A) 45 parts by mass The above rod-shaped liquid crystal compound (B) 27 parts by mass The above rod-shaped liquid crystal compound (C) 13 parts by mass The above rod-shaped liquid crystal compound (D) 12 parts by mass The above rod-shaped liquid crystal compound (E) 3 parts by mass The above polymerization initiator S-1 0.5 parts by mass The above surfactant 2 0.04 parts by mass The above left-hand torsion chiral agent (L1) 0.24 parts by mass Methyl ethyl ketone 54 parts by mass Cyclopentanone 181 parts by mass --------------------------------------------------
[0187] Following the procedure described above, a laminate (A3-B3) was fabricated in which an optically anisotropic layer (A3) and an optically anisotropic layer (B3) were directly laminated onto a long cellulose acylate film.
[0188] (Formation of optically anisotropic layer (C3)) An optically anisotropic layer (C3) was fabricated using the same procedure as for optically anisotropic layer (C1) described above, except for adjusting the film thickness. The obtained optically anisotropic layer (C3) had a film thickness of 0.6 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -90 nm. Furthermore, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0189] The surface side of the optically anisotropic layer (B3) of the laminate (A3-B3) prepared above and the surface side of the optically anisotropic layer (C3) prepared above were bonded together using Lintec's adhesive sheet "NCF-D692(5)" so that their longitudinal directions were parallel to each other. Next, the cellulose acylate film and alignment film 1 on the optically anisotropic layer (A3) side of the laminate (A3-B3) were peeled off, exposing the surface of the optically anisotropic layer (A3) that was in contact with the cellulose acylate film. In this way, an optical film (C3-PSA-B3-A3) was obtained in which the optically anisotropic layer (C3), optically anisotropic layer (B3), and optically anisotropic layer (A3) were laminated in this order on a long cellulose acylate film.
[0190] [Example 4] <Fabrication of Optical Film> (Formation of Optical Anisotropic Layer (A4)) An optical anisotropic layer (A4) was fabricated using the same procedure as for the optical anisotropic layer (A1) described above, except that the film thickness and the angle of the rubbing treatment were adjusted. The obtained optical anisotropic layer (A4) had an average thickness of 1.5 μm, an in-plane retardation of 190 nm at a wavelength of 550 nm, and an in-plane slow phase axis direction of -14°. In addition, the average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0191] (Formation of optically anisotropic layer (B4)) An optically anisotropic layer (B4) was formed on the optically anisotropic layer (A4) prepared above using the same procedure as for the optically anisotropic layer (B2), except that the optically anisotropic layer formation composition containing the rod-shaped liquid crystal compound was replaced with the optically anisotropic layer formation composition (B4) described below, and the film thickness was adjusted. The average thickness of the optically anisotropic layer (B4) was 1.1 μm, and Δnd at a wavelength of 550 nm was 183 nm. The liquid crystal compound was twisted to the left, and the twist angle was 81°. The in-plane slow axis direction of the optically anisotropic layer (B4) (orientation axis angle of the liquid crystal compound) coincided with the in-plane slow axis direction of the optically anisotropic layer (A4) on the side in contact with the optically anisotropic layer (A4). Furthermore, the in-plane slow phase axis direction at the air interface was 85°, when the film width direction was taken as 0° and observed from the optical anisotropy layer (B4) side, with counterclockwise direction represented by a positive value.
[0192] -------------------------------------------------- Composition for forming an optically anisotropic layer (B4) -------------------------------------------------- 100 parts by mass of the above rod-shaped liquid crystal compound (A) 0.5 parts by mass of the above polymerization initiator S-1 0.04 parts by mass of the above surfactant 2 0.04 parts by mass of the above left-hand torsion chiral agent (L1) 0.43 parts by mass of methyl ethyl ketone 54 parts by mass of cyclopentanone 181 parts by mass --------------------------------------------------
[0193] Following the procedure described above, a laminate (A4-B4) was fabricated in which an optically anisotropic layer (A4) and an optically anisotropic layer (B4) were directly laminated onto a long cellulose acylate film.
[0194] (Formation of optically anisotropic layer (C4)) An optically anisotropic layer (C4) was fabricated using the same procedure as for optically anisotropic layer (C1) described above, except for adjusting the film thickness. The obtained optically anisotropic layer (C4) had a film thickness of 0.6 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -90 nm. Furthermore, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0195] The surface side of the optically anisotropic layer (B4) of the laminate (A4-B4) prepared above and the surface side of the optically anisotropic layer (C4) prepared above were bonded together using Lintec's adhesive sheet "NCF-D692(5)" so that their longitudinal directions were parallel to each other. Next, the cellulose acylate film and orientation film 1 on the optically anisotropic layer (A4) side of the laminate (A4-B4) were peeled off, exposing the surface of the optically anisotropic layer (A4) that was in contact with the cellulose acylate film. In this way, an optical film (C4-PSA-B4-A4) was obtained in which the optically anisotropic layer (C4), optically anisotropic layer (B4), and optically anisotropic layer (A4) were laminated in this order on a long cellulose acylate film.
[0196] [Comparative Example 1] <Preparation of Optical Film> (Formation of Optical Anisotropic Layer (S1)) An optical anisotropic layer (S1) was prepared using the same procedure as for the optical anisotropic layer (A1) described above, except that the film thickness and the angle of the rubbing treatment were adjusted. The obtained optical anisotropic layer (S1) had an average thickness of 3.0 μm, an in-plane retardation of 141 nm at a length of 550 nm, and an in-plane slow phase axis direction of -45°. In addition, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 0°, confirming that it was oriented horizontally with respect to the film surface.
[0197] -------------------------------------------------- Composition for forming an optically anisotropic layer (S1) -------------------------------------------------- The above rod-shaped liquid crystal compound (A) 8 parts by mass The above rod-shaped liquid crystal compound (B) 45 parts by mass The above rod-shaped liquid crystal compound (C) 22 parts by mass The above rod-shaped liquid crystal compound (D) 20 parts by mass The above rod-shaped liquid crystal compound (E) 5 parts by mass The above polymerization initiator S-1 0.5 parts by mass The above surfactant 2 0.04 parts by mass Methyl ethyl ketone 54 parts by mass Cyclopentanone 181 parts by mass --------------------------------------------------
[0198] (Formation of optically anisotropic layer (C5)) An optically anisotropic layer (C5) was fabricated using the same procedure as for optically anisotropic layer (C1) described above, except for adjusting the film thickness. The obtained optically anisotropic layer (C4) had a film thickness of 0.5 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -68 nm. Furthermore, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0199] The surface side of the optically anisotropic layer (S1) prepared above and the surface side of the optically anisotropic layer (C5) prepared above were bonded together using Lintec's adhesive sheet "NCF-D692(5)" so that their longitudinal directions were parallel to each other. Next, the cellulose acylate film and alignment film 1 of the optically anisotropic layer (S1) were peeled off, exposing the surface of the optically anisotropic layer (S1) that was in contact with the cellulose acylate film. In this way, an optical film (C5-PSA-S1) was obtained in which the optically anisotropic layer (C5) and the optically anisotropic layer (S1) were laminated in this order on a long cellulose acylate film.
[0200] [Example 5] <Fabrication of Optical Film> (Formation of Optical Anisotropic Layer (A5)) An optical anisotropic layer (A5) was fabricated on the photo-alignment film 5 in the same manner as in Example 1, except that the alignment film 1 was changed to the photo-alignment film 5 shown below. The obtained optical anisotropic layer (A5) had an average thickness of 1.6 μm, an in-plane retardation of 196 nm at a wavelength of 550 nm, and an in-plane slow phase axis direction of -10°. In addition, the average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0201] (Formation of photo-alignment film 5) A photo-alignment film forming solution E2 with the following composition was continuously applied to the surface of the cellulose acylate film that had undergone alkali saponification treatment using a wire bar. The support on which the coating film was formed was dried with hot air at 134°C for 75 seconds, and then polarized ultraviolet light (8 mJ / cm²) was irradiated onto the coating film. 2 A photo-alignment film 5 was formed by using an ultra-high pressure mercury lamp. The thickness of the photo-alignment film 5 was 0.7 μm.
[0202] ------------------------------------------------------------------- Photo-alignment film forming coating solution E2 ------------------------------------------------------------------- ・100.00 parts by mass of the polymer PA-1 below ・6.00 parts by mass of the acid generator PAG-1 below ・0.60 parts by mass of diisopropylethylamine ・625.4 parts by mass of butyl acetate ・156.3 parts by mass of methyl ethyl ketone -------------------------------------------------------------------
[0203] Polymer PA-1 [In the formula below, the numerical values listed for each repeating unit represent the content (mass%) of each repeating unit relative to the total number of repeating units. Weight-average molecular weight: 45,000]
[0204] Acid Generator PAG-1
[0205] (Formation of Optical Anisotropic Layer (B5)) An optical anisotropic layer (B5) was formed on the optical anisotropic layer (A5) prepared above using the same procedure as for the optical anisotropic layer (B2), except that the optical anisotropic layer formation composition containing the rod-shaped liquid crystal compound was replaced with the optical anisotropic layer formation composition (B5) described below, and the film thickness was adjusted. The average thickness of the optical anisotropic layer (B5) was 3.6 μm, and the Δnd at a wavelength of 550 nm was 197 nm. The liquid crystal compound was twisted to the left, and the twist angle was 77°. The in-plane slow axis direction of the optical anisotropic layer (B5) (orientation axis angle of the liquid crystal compound) coincided with the in-plane slow axis direction of the optical anisotropic layer (A5) on the side in contact with the optical anisotropic layer (A5). Furthermore, the in-plane slow phase axis direction at the air interface was 93°, when the film width direction was taken as 0° and observed from the optical anisotropy layer (B5) side, with counterclockwise direction represented by a positive value.
[0206] -------------------------------------------------- Composition for forming an optically anisotropic layer (B5) -------------------------------------------------- The above rod-shaped liquid crystal compound (B) 35 parts by mass The above rod-shaped liquid crystal compound (C) 17 parts by mass The above rod-shaped liquid crystal compound (D) 15 parts by mass The above rod-shaped liquid crystal compound (E) 4 parts by mass The following rod-shaped liquid crystal compound (F) 29 parts by mass The above polymerization initiator S-1 0.5 parts by mass The above surfactant 2 0.04 parts by mass The above left-hand torsion chiral agent (L1) 0.34 parts by mass Methyl ethyl ketone 54 parts by mass Cyclopentanone 181 parts by mass --------------------------------------------------
[0207] Rod-shaped liquid crystal compound (F)
[0208] Following the above procedure, a laminate (A5-B5) was fabricated in which an optically anisotropic layer (A5) and an optically anisotropic layer (B5) were directly laminated on a photo-aligned film 5 of a long cellulose acylate film.
[0209] (Formation of optically anisotropic layer (C6)) An optically anisotropic layer (C6) was fabricated using the same procedure as for optically anisotropic layer (C1) described above, except for adjusting the film thickness. The obtained optically anisotropic layer (C6) had a film thickness of 0.7 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -100 nm. Furthermore, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0210] The surface side of the optically anisotropic layer (B5) of the laminate (A5-B5) prepared above and the surface side of the optically anisotropic layer (C6) prepared above were bonded together using Lintec's adhesive sheet "NCF-D692(5)" so that their longitudinal directions were parallel to each other. Next, the cellulose acylate film on the optically anisotropic layer (A5) side of the laminate (A5-B5) was peeled off together with the photo-alignment film 5, exposing the surface of the optically anisotropic layer (A5) that was in contact with the cellulose acylate film. In this way, an optical film (C6-PSA-B5-A5) was obtained in which the optically anisotropic layer (C6), optically anisotropic layer (B5), and optically anisotropic layer (A5) were laminated in this order on a long cellulose acylate film.
[0211] [Example 6] <Preparation of Optical Film> (Formation of Optical Anisotropic Layer (A6)) An optical anisotropic layer (A6) was formed in the same manner as for the optical anisotropic layer (B2) described above, except that the optical anisotropic layer forming composition containing the rod-shaped liquid crystal compound was replaced with the optical anisotropic layer forming composition (A6) described below, and coated onto the photo-alignment film 5 using a Gieser coating machine. The average thickness of the optical anisotropic layer (A6) was 2.7 μm, Δnd at a wavelength of 550 nm was 196 nm, and the in-plane slow phase axis direction was 110°. In addition, the average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 0°, confirming that it was oriented horizontally with respect to the film surface.
[0212] -------------------------------------------------- Composition for forming an optically anisotropic layer (A6) -------------------------------------------------- The above rod-shaped liquid crystal compound (A) 29 parts by mass The above rod-shaped liquid crystal compound (B) 35 parts by mass The above rod-shaped liquid crystal compound (C) 17 parts by mass The above rod-shaped liquid crystal compound (D) 15 parts by mass The above rod-shaped liquid crystal compound (E) 4 parts by mass The above polymerization initiator S-1 0.5 parts by mass The above surfactant 2 0.04 parts by mass Methyl ethyl ketone 54 parts by mass Cyclopentanone 181 parts by mass --------------------------------------------------
[0213] (Formation of optically anisotropic layer (B6)) Corona discharge treatment was performed on the surface side of the optically anisotropic layer (A6) prepared above. The conditions for the corona discharge treatment were an output intensity of 2.5 kW, a line speed of 18 m / min, an electrode length of 1.4 m, and a gap distance of 2 mm. An optically anisotropic layer (B6) was formed on the optically anisotropic layer (A6) that had been treated with corona discharge above, using the same procedure as for the optically anisotropic layer (B2) above, except that the optically anisotropic layer formation composition containing the liquid crystal compound was changed to the optically anisotropic layer formation composition (B6) described below and the film thickness was adjusted. The average thickness of the optically anisotropic layer (B6) was 1.5 μm, and Δnd at a wavelength of 550 nm was 180 nm. The liquid crystal compound was twisted to the right, and the twist angle was 93°. The in-plane slow axis direction of the optically anisotropic layer (B6) (the orientation axis angle of the liquid crystal compound) coincided with the in-plane slow axis direction of the optically anisotropic layer (A6) on the side in contact with the optically anisotropic layer (A6). Furthermore, the in-plane slow axis direction at the air interface was 23°, when the film width direction is taken as 0° and observed from the optically anisotropic layer (B6) side, with counterclockwise direction represented as a positive value.
[0214] -------------------------------------------------- Composition for forming an optically anisotropic layer (B6) -------------------------------------------------- 40 parts by mass of the above disc-shaped liquid crystal compound 1 60 parts by mass of the above disc-shaped liquid crystal compound 2 0.1 parts by mass of the above vertical alignment agent 1 3 parts by mass of the following vertical alignment agent 2 2 parts by mass of the above foaming inhibitor 1 5 parts by mass of the following right-twist chiral agent (L2) 0.1 parts by mass of the above surfactant 1 1 part by mass of photopolymerization initiator (Api307, manufactured by Shenzhen UV-ChemTech LTD) 1 part by mass of methyl ethyl ketone 102 parts by mass of cyclopentanone 238 parts by mass --------------------------------------------------
[0215] Right-handed chiral agent (L2)
[0216] Vertical alignment agent 2
[0217] Following the above procedure, a laminate (A6-B6) was fabricated in which an optically anisotropic layer (A6) and an optically anisotropic layer (B6) were directly laminated on a photo-aligned film 5 of a long cellulose acylate film.
[0218] (Formation of Optical Anisotropic Layer (C7)) An optical anisotropic layer (C7) was prepared using the same procedure as for the optical anisotropic layer (C1) described above, except that the optical anisotropic layer formation composition (C1) was changed to the optical anisotropic layer formation composition (C7) described below and the film thickness was adjusted. The obtained optical anisotropic layer (C7) had a film thickness of 0.6 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was 70 nm. Furthermore, the average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 0°, confirming that it was oriented horizontally with respect to the film surface.
[0219] -------------------------------------------------- Composition for forming an optically anisotropic layer (C7) -------------------------------------------------- 4 parts by mass of the above disc-shaped liquid crystal compound 1 1 part by mass of the above disc-shaped liquid crystal compound 2 95.0 parts by mass of the following disc-shaped liquid crystal compound 3 12.0 parts by mass of the above acrylate monomer 1 3.0 parts by mass of the above polymerization initiator S-1 (oxime type) 0.2 parts by mass of diisopropylethylamine 102 parts by mass of methyl ethyl ketone 238 parts by mass -------------------------------------------------- Composition for forming an optically anisotropic layer (C7) -------------------------------------------------- 4 parts by mass of the above disc-shaped liquid crystal compound 1 1 part by mass of the above disc-shaped liquid crystal compound 2 95.0 parts by mass of the following disc-shaped liquid crystal compound 3 12.0 parts by mass of the above acrylate monomer 1 3.0 parts by mass of the above polymerization initiator S-1 (oxime type) 0.0 parts by mass of diisopropylethylamine 0.2 parts by mass of methyl ethyl ketone 102 parts by mass of cyclopentanone 238 parts by mass --------------------------------------------------
[0220] Disc-shaped liquid crystal compound 3
[0221] The surface side of the optically anisotropic layer (B6) of the laminate (A6-B6) prepared above and the surface side of the optically anisotropic layer (C7) prepared above were bonded together using Lintec's adhesive sheet "NCF-D692 (5)" so that their longitudinal directions were parallel to each other. Next, the cellulose acylate film on the optically anisotropic layer (A6) side of the laminate (A6-B6) was peeled off together with the photo-alignment film 5, exposing the surface of the optically anisotropic layer (A6) that was in contact with the cellulose acylate film. In this way, an optical film (C7-PSA-B6-A6) was obtained in which the optically anisotropic layer (C7), optically anisotropic layer (B6), and optically anisotropic layer (A6) were laminated in this order on a long cellulose acylate film.
[0222] [Example 7] <Fabrication of Optical Film> (Formation of Optical Anisotropic Layer (A7)) An optical anisotropic layer (A7) was fabricated on the photo-alignment film 5 in the same manner as in Example 1, except that the alignment film 1 was replaced with the photo-alignment film 5. The obtained optical anisotropic layer (A7) had an average thickness of 1.5 μm, an in-plane retardation of 187 nm at a wavelength of 550 nm, and an in-plane slow phase axis direction of -11°. In addition, the average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0223] (Formation of optically anisotropic layer (C8)) An optically anisotropic layer (C8) was fabricated in the same manner as the optically anisotropic layer (C1) described above. The thickness of the obtained optically anisotropic layer (C8) was 0.6 μm. The in-plane retardation at a wavelength of 550 nm was 0 nm, and the retardation in the thickness direction at a wavelength of 550 nm was -90 nm. That is, if Δnd is defined as the product of Δn in the thickness direction and the thickness d, then Δnd was 90 nm. The average inclination angle of the rod-shaped liquid crystal compound in the direction of the long axis with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface.
[0224] (Formation of optically anisotropic layer (B7)) Next, an optically anisotropic layer (B7) was fabricated on the optically anisotropic layer (C8) prepared above, in the same manner as the optically anisotropic layer (B1) above. The average thickness of the obtained optically anisotropic layer (B7) was 2.6 μm, and Δnd at a wavelength of 550 nm was 192 nm. The liquid crystal compound was twisted to the left, and the twist angle was 79°. The in-plane slow axis direction of the optically anisotropic layer (B7) (orientation axis angle of the liquid crystal compound) was 11° on the air side and 89° on the side in contact with the optically anisotropic layer (C8), when the width direction of the film is taken as 0° and the counterclockwise direction is expressed as a positive value when observed from the optically anisotropic layer (B7) side.
[0225] Following the procedure described above, a laminate (B7-C8) was fabricated in which an optically anisotropic layer (C8) and an optically anisotropic layer (B7) were directly laminated onto a long cellulose acylate film.
[0226] The surface side of the optically anisotropic layer (A7) formed on the long cellulose acylate film prepared above and the surface side of the optically anisotropic layer (B7) of the laminate (B7-C8) formed on the long cellulose acylate film prepared above were bonded together using Lintec's adhesive sheet "NCF-D692(5)" (thickness 5um) such that the longitudinal direction of the optically anisotropic layer (A7) and the longitudinal direction of the optically anisotropic layer (B7) were parallel. At this time, the orientation of the in-plane slow axis on the surface of the optically anisotropic layer (B7) facing the optically anisotropic layer (A7) coincided with the orientation of the slow axis of the optically anisotropic layer (A7). Next, the cellulose acylate film and photo-alignment film 5 on the optically anisotropic layer (A7) side were peeled off, exposing the surface of the optically anisotropic layer (A7) that was in contact with the cellulose acylate film. In this way, an optical film (C8-B7-PSA-A7) was obtained in which an optically anisotropic layer (C8), an optically anisotropic layer (B7), and an optically anisotropic layer (A7) were laminated in this order on a long cellulose acylate film.
[0227] <Evaluation of Ellipticity> For each fabricated optical film, light of each wavelength was incident perpendicularly from the optical anisotropy layer side using AxoScan OPMF-1, and the Müller matrix in the wavelength range of 450 nm to 650 nm was measured. The Müller matrix was multiplied by the Stokes parameter representing linear polarization with an appropriate polarization axis angle, and the ellipticity for each wavelength was calculated from the obtained Stokes parameter. The results are shown in Table 1. For ellipticity under perpendicular incidence, the minimum value of ellipticity in the wavelength range of 450 nm to 650 nm (minimum ellipticity) was used as the evaluation index. The minimum ellipticity under perpendicular incidence is preferably 0.90 or higher, and more preferably 0.92 or higher. Next, each fabricated optical film was isotropically stretched so that its area was 1.1 times larger, and the ellipticity under perpendicular incidence was measured in the same manner as above. The results are shown in Table 1. The minimum ellipticity under perpendicular incidence after stretching is preferably 0.90 or higher, and more preferably 0.92 or higher. Furthermore, light of each wavelength was incident on each fabricated optical film at a polar angle of 40°, and measurements were taken in 15° increments from 0° to 165° azimuth angles. At each azimuth angle, the Müller matrix was measured in the wavelength range of 450 nm to 650 nm, and the ellipticity at each wavelength was calculated from the obtained Stokes parameter by multiplying the Müller matrix by the Stokes parameter representing linear polarization with an appropriate polarization axis angle. The results are shown in Table 1. For the ellipticity at a polar angle of 40° incidence, the minimum value of the ellipticity in the wavelength range of 450 nm to 650 nm was found at each measured azimuth angle, and the minimum value of that value at each azimuth angle was used as an evaluation index. The minimum ellipticity at a polar angle of 40° incidence is preferably 0.80 or higher, and more preferably 0.85 or higher.
[0228] <Evaluation of Ghosting in Virtual Reality Display Devices> (Fabrication of Image Display Device, Lens, and Virtual Reality Display Device) The Meta Quest3 virtual reality display device manufactured by Meta Corporation, which employs a pancake lens, was disassembled, and the image display device and lens were removed. The image display device of the Meta Quest3 is a liquid crystal display device, and an optical film consisting of an absorbing linear polarizer and a λ / 4 wave plate was bonded to its surface. The optical film was peeled off, and the respective optical films of the example and comparative example were bonded to the surface of the absorbing linear polarizer so that the side with the optical anisotropy layer faced the absorbing linear polarizer, and the cellulose acylate film of the optical film was peeled off. At this time, the films were bonded at an angle such that the orientation of the absorption axis of the absorbing linear polarizer and the longitudinal direction of each optical film were parallel. Furthermore, an anti-reflective film "DSG-17" manufactured by Dai Nippon Printing Co., Ltd. was bonded to create an image display device.
[0229] Furthermore, the lens of Meta Quest 3 was a pancake lens combining two plano-convex lenses, and an optical film, which was a λ / 4 wave plate, was bonded to the plano-convex lens closer to the image display device. This optical film was peeled off, and in its place, the optical films of the example and comparative example were bonded. However, at this time, the optical anisotropy layer side of each optical film was bonded to the anti-reflective film "DSG-17" so that the side of the optical anisotropy layer was facing the anti-reflective film, and the cellulose acylate film of the optical film was peeled off. Then, it was bonded to the plano-convex lens to fabricate the lens. The fabricated image display device and lens were assembled as before to create a virtual reality display device. Note that a reflective linear polarizer was used for the plano-convex lens on the side farther from the image display device of Meta Quest 3. At this time, the orientation of the reflection axis of the reflective linear polarizer and the longitudinal direction of the optical film were at an angle perpendicular to each other.
[0230] (Evaluation of Ghost Visibility) A black and white checkerboard pattern was displayed on the image display device of each virtual reality display device that was fabricated. The virtual reality display device was worn, and the displayed black and white checkerboard pattern was observed visually, and the ghost visibility was evaluated based on the following four evaluation criteria. AA: No ghosts are visible. A: A slight ghost is visible but not bothersome. B: A weak ghost is visible. C: A moderately strong ghost is visible. D: A strong ghost is visible. The results are shown in Table 1.
[0231] <Evaluation of Display Performance of Organic EL Display Device> (Fabrication of Linear Polarizer) The surface of a cellulose triacetate film TJ25 (manufactured by Fujifilm Corporation: 25 μm thick) support was subjected to alkali saponification treatment. Specifically, the support was immersed in a 1.5 N sodium hydroxide aqueous solution at 55°C for 2 minutes, then washed in a water bath at room temperature, and further neutralized with 0.1 N sulfuric acid at 30°C. After neutralization, the support was washed in a water bath at room temperature and further dried with hot air at 100°C to obtain a polarizer protective film. A roll-shaped polyvinyl alcohol (PVA) film with a thickness of 60 μm was continuously stretched in the longitudinal direction in an iodine aqueous solution and dried to obtain a polarizer with a thickness of 13 μm. The luminous efficiency correction single transmittance of the polarizer was 43%. At this time, the absorption axis direction and the longitudinal direction of the polarizer coincided. The polarizer protective film was attached to one side of the above polarizer using the PVA adhesive described below to fabricate a linear polarizer.
[0232] (Preparation of PVA adhesive) A PVA adhesive was prepared by dissolving 100 parts by mass of a polyvinyl alcohol resin having an acetoacetyl group (average degree of polymerization: 1200, degree of saponification: 98.5 mol%, degree of acetoacetylation: 5 mol%) and 20 parts by mass of methylolmelamine in pure water at a temperature of 30°C, and adjusting the solid content concentration to 3.7% by mass as an aqueous solution.
[0233] (Fabrication of circular polarizers) The optical anisotropy layer surfaces of the optical films of the examples and comparative examples were continuously bonded to the polarizer surface (the side opposite the polarizer protective film) of the elongated linear polarizer prepared above using an ultraviolet-curing adhesive. Subsequently, the cellulose acylate film was peeled off each optical film. In this way, circular polarizers were prepared, each consisting of an optical film and a linear polarizer. At this time, the optical films were bonded so that the longitudinal direction of each optical film and the direction of the absorption axis of the linear polarizer were parallel. Furthermore, the optical anisotropic layers (A1) and (B1) of Example 1, (A2) and (B2) of Example 2, (A3) and (B3) of Example 3, (A4) and (B4) of Example 4, (A5) and (B5) of Example 5, (A6) and (B6) of Example 6, and (A7) and (B7) of Example 7 all have an in-plane phase difference that is substantially λ / 4 with respect to the wavelength λ of the incident light, due to the configuration of these optical anisotropic layers. However, each of the above optical anisotropic layers does not have an in-plane phase difference that is substantially λ / 4 on its own.
[0234] (Fabrication of Organic EL Display Device) An Apple iPhone 14 Pro equipped with an organic EL panel was disassembled, and the front glass plate and circular polarizer were removed. Using a SEM-EDX (SU-8030, Hitachi High-Tech Corporation), it was confirmed that a thin film sealing layer made of silicon nitride (SiN) or silicon oxynitride (SiON) was formed on the surface of the organic EL panel. The circular polarizers fabricated above were bonded to the surface of the disassembled organic EL panel via a pressure-sensitive adhesive SK-2057 (manufactured by Soken Chemical Co., Ltd.) to create an evaluation panel.
[0235] (Evaluation of Display Performance) (Front View) The fabricated evaluation panel was observed from the front under bright light, and the color tint was evaluated according to the following criteria. The results are shown in Table 1 below. A: No color tint is visible at all, or only slightly visible. (Acceptable) B: Color tint is visible, but the reflected light is small and there is no problem in use. (Acceptable)
[0236] (Diagonal Direction) A black display was shown on the fabricated organic EL display device, and under bright light, a fluorescent lamp was projected from an extreme angle of 55°, and the reflected light was observed from all directions. The azimuth angle dependence of the color tint was evaluated according to the following criteria. The results are shown in Table 1. A: No color tint is visible at all. B: A slight color tint is visible. (Acceptable) C: A slight color tint is visible, but the reflected light is small and there is no problem in use. (Acceptable) D: A color tint is visible, and the reflected light is large; unacceptable.
[0237] In Table 1, the "Optical Anisotropy Layer and Adhesive Layer" column shows the type and lamination order of the optical anisotropy layer included in the optical film of each example and comparative example. For example, "A1" represents the optical anisotropy layer (A1). Also, "PSA" represents the adhesive sheet. In Table 1, the "Δnd (550 nm)" column shows the value of Δnd for each layer at a wavelength of 550 nm. For optical anisotropy layers (C1) to (C5), Δnd is the product of the refractive index anisotropy Δn in the thickness direction and the thickness d. Also, the "Wavelength Dispersion" column shows the ratio of Δnd at a wavelength of 450 nm to Δnd at a wavelength of 550 nm for each layer.
[0238]
[0239] As shown in Table 1 above, it was confirmed that the optical film of the present invention can obtain high ellipticity over a wide wavelength range in both perpendicular and oblique incidence. As a result, image display devices and virtual reality display devices using lenses containing the optical film of the present invention suppressed ghost images across the entire field of view, resulting in good visibility. Furthermore, organic EL display devices containing the optical film of the present invention showed good display performance in black display. Moreover, it was confirmed that the optical film of the present invention can maintain high ellipticity even after stretching. As a result, it is considered that the optical film of the present invention can effectively suppress ghost images even when used in virtual reality display devices having curved lenses.
[0240] 1000, 1001 Virtual reality display device 2 Lens 3,500 Image display device 10A Optical film 12A First optical anisotropy layer 14 Second optical anisotropy layer 16 Third optical anisotropy layer 20 Polarizer 100A Circular polarizer 21, 100 Reflective linear polarizer 22 First optical film 23, 600 Lens substrate 24, 300 Half mirror 31 Second optical film 32 Absorbing linear polarizer 33 Image display panel 70 Light rays that form the main image 71, 72 Light rays that form the ghost image 200 First phase difference layer 400 Second phase difference layer
Claims
1. An optical film comprising at least a first optical anisotropy layer and a second optical anisotropy layer laminated together, wherein the first optical anisotropy layer and the second optical anisotropy layer are each independently layers on which a liquid crystal compound is fixed, and the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to one surface of the optical film is 0.90 or more at minimum values in the wavelength range of 450 nm to 650 nm, and the ellipticity of the emitted light when linearly polarized light is incident perpendicularly to one surface of the optical film after isotropically stretching the optical film to 1.1 times its area is 0.90 or more at minimum values in the wavelength range of 450 nm to 650 nm.
2. An optical film comprising a laminate containing at least a first optical anisotropy layer, a second optical anisotropy layer, and a third optical anisotropy layer in this order, wherein the first optical anisotropy layer is a layer on which vertically oriented disc-shaped liquid crystal compounds are fixed, or a layer on which horizontally oriented rod-shaped liquid crystal compounds are fixed, the second optical anisotropy layer is a layer on which rod-shaped liquid crystal compounds are torsionally oriented along a helical axis extending in the thickness direction are fixed, the third optical anisotropy layer is a layer on which vertically oriented rod-shaped liquid crystal compounds are fixed, and the ratio of the refractive index anisotropy Δn of the second optical anisotropy layer at a wavelength of 450 nm to the refractive index anisotropy Δn of the second optical anisotropy layer at a wavelength of 550 nm is 0.87 to 0.
99.
3. The optical film according to claim 1 or 2, wherein the first optical anisotropic layer and the second optical anisotropic layer are in direct contact, and the orientations of high in-plane refractive index of liquid crystal molecules coincide with each other on the surface of the first optical anisotropic layer that is in contact with the second optical anisotropic layer and on the surface of the second optical anisotropic layer that is in contact with the first optical anisotropic layer.
4. The optical film according to claim 1 or 2, wherein the laminate of the first optical anisotropy layer and the second optical anisotropy layer has an in-plane phase difference that is substantially λ / 4 with respect to the wavelength λ of the incident visible light.
5. The optical film according to claim 1 or 2, having at least a curved portion.
6. A circular polarizer comprising the optical film according to claim 1 or 2 and a polarizer.
7. An image display device having the circular polarizer described in claim 6.
8. A reflective circular polarizer comprising the optical film according to claim 1 or 2 and a reflective polarizer.
9. A lens having the circular polarizer described in claim 8.
10. A virtual reality display device having the lens described in claim 9.