Resin composition for electrical insulation and insulating sheet

The electrical insulating resin composition with controlled boron elution from boron nitride fillers addresses curing temperature issues, ensuring stable curing reactions for semiconductor device insulating sheets with improved thermal conductivity and insulation.

WO2026239930A1PCT designated stage Publication Date: 2026-11-19NITTO SHINKO KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016788
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-04-28
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing electrical insulating resin compositions containing boron nitride fillers face challenges in controlling the curing reaction initiation temperature due to the elution of boron-containing compounds, leading to unintended excessive or insufficient curing reactions.

Method used

An electrical insulating resin composition is developed with a boron nitride filler that elutes less than 100 ppm boron, combined with a curing agent and accelerator, allowing controlled curing reaction initiation temperature adjustment.

Benefits of technology

The composition achieves stable and controlled curing reactions, enabling the production of insulating sheets with desired properties for semiconductor devices, enhancing thermal conductivity and electrical insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026016788_19112026_PF_FP_ABST
    Figure JP2026016788_19112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a resin composition for electrical insulation, the composition containing a boron nitride filler, an epoxy resin, and a curing agent for the epoxy resin. The amount of boron eluted from the boron nitride filler is less than 100 ppm.
Need to check novelty before this filing date? Find Prior Art

Description

Resin Composition for Electrical Insulation and Insulating Sheet Cross-Reference to Related Applications

[0001] This application claims the priority of Japanese Patent Application No. 2025-079845, and such application is incorporated into the description of the present application by reference.

[0002] The present invention relates to, for example, a resin composition for electrical insulation for forming an insulating sheet used as a member in a semiconductor device. The present invention also relates to, for example, an insulating sheet provided with an insulating layer formed from the aforementioned resin composition for electrical insulation.

[0003] Conventionally, for example, an insulating sheet that is a member constituting a semiconductor device having a semiconductor element and is a member for transmitting heat generated by the semiconductor element to the outside of the device has been known. This type of insulating sheet has at least, for example, an insulating layer that has electrical insulation properties and also thermal conductivity. Such an insulating layer is disposed between at least two members adjacent to the insulating sheet, maintains electrical insulation within the device, transmits heat generated by the semiconductor element to the outside of the device, and can suppress an excessive temperature rise of the semiconductor element.

[0004] The insulating layer of this type of insulating sheet is formed of, for example, a resin composition for electrical insulation containing an epoxy resin, and the resin composition for electrical insulation contains an epoxy resin, an inorganic filler, and a curing agent for the epoxy resin (for example, Patent Document 1).

[0005] The resin composition for electrical insulation described in Patent Document 1 may contain, for example, a boron nitride filler as the inorganic filler, and a phenolic curing agent or an amine curing agent as the curing agent.

[0006] Japanese Unexamined Patent Publication No. 2018-065921

[0007] Incidentally, as described in Patent Document 1, the curing reaction initiation temperature associated with the ring-opening reaction of the epoxy resin cannot always be adequately controlled in electrical insulating resin compositions containing boron nitride fillers. Specifically, the curing reaction initiation temperature of the electrical insulating resin composition may unintentionally become too low, causing the curing reaction of the electrical insulating resin composition to proceed excessively. On the other hand, the curing reaction initiation temperature of the electrical insulating resin composition may unintentionally become too high, causing the curing reaction of the electrical insulating resin composition to not proceed as expected.

[0008] One reason why the curing reaction initiation temperature of electrical insulating resin compositions cannot be controlled is thought to be the elution of boron-containing compounds from boron nitride fillers. In other words, it is believed that boron-containing compounds affect the progress of the ring-opening reaction of the epoxy resin. Note that boron-containing compounds are a general term for compounds that elute from boron nitride fillers, and will sometimes be simply referred to as "eluted boron" below. Therefore, there is a need for an electrical insulating resin composition that contains boron nitride fillers that can affect the curing reaction initiation temperature, while still allowing for control of the curing reaction initiation temperature.

[0009] In view of the above-mentioned problems and requirements, the present invention aims to provide an electrical insulating resin composition that contains a boron nitride filler and allows for control of the curing reaction initiation temperature. The present invention also relates to an insulating sheet comprising an insulating layer formed of the above-mentioned electrical insulating resin composition.

[0010] To solve the above problems, the electrical insulating resin composition according to the present invention comprises a boron nitride filler, an epoxy resin, and a curing agent for the epoxy resin, wherein the amount of boron eluted from the boron nitride filler is less than 100 ppm.

[0011] To solve the above problems, the insulating sheet according to the present invention comprises an insulating layer formed of the above-mentioned electrical insulating resin composition.

[0012] Figure 1A is a schematic cross-sectional view showing a cross-section of an example of the insulating sheet of this embodiment, cut in the thickness direction. Figure 1B is a schematic cross-sectional view showing a cross-section of another example of the insulating sheet of this embodiment, cut in the thickness direction. Figure 2 is a schematic diagram showing an example of how the insulating layer of the insulating sheet is manufactured. Figure 3A is a schematic front view of a semiconductor device. Figure 3B is a schematic cross-sectional view showing the internal structure of an example of a semiconductor device. Figure 3C is a schematic cross-sectional view showing the internal structure of another example of a semiconductor device. Figure 4A is a schematic cross-sectional view partially showing the internal structure of yet another example of a semiconductor device. Figure 4B is a schematic cross-sectional view partially showing the internal structure of yet another example of a semiconductor device. Figure 5A is a graph showing the relationship between the amount of boron eluted from the boron nitride filler in Specific Example 1 and the curing reaction start temperature of the electrical insulating resin composition. Figure 5B is a graph showing the relationship between the amount of boron eluted from the boron nitride filler in Specific Example 2 and the curing reaction start temperature of the electrical insulating resin composition.

[0013] Hereinafter, embodiments of the electrical insulating resin composition and the insulating sheet formed from the electrical insulating resin composition according to the present invention will be described with reference to the drawings.

[0014] First, the electrical insulating resin composition of this embodiment will be described in detail. The electrical insulating resin composition of this embodiment is, for example, a composition for forming the insulating layer of an insulating sheet, which will be described later.

[0015] The electrical insulating resin composition of this embodiment comprises an epoxy resin, a boron nitride filler, and a curing agent for the epoxy resin, wherein the amount of boron eluted from the boron nitride filler is less than 100 ppm.

[0016] The electrical insulating resin composition of this embodiment preferably further contains a curing accelerator. More preferably, the electrical insulating resin composition of this embodiment contains a phenolic curing agent and a phosphorus-based curing accelerator, or contains an amine-based curing agent and a boron trifluoride-based curing accelerator.

[0017] (Boron Nitride Filler) The boron nitride filler is in powder form before being incorporated into the electrical insulating resin composition. The shape of each particle of the boron nitride filler is, for example, flaky. The boron nitride filler may also be a hexagonal boron nitride powder.

[0018] The amount of boron eluted from the boron nitride filler is less than 100 ppm. Since the electrical insulating resin composition of this embodiment contains an epoxy resin and a curing agent for the epoxy resin, and the amount of boron eluted from the boron nitride filler is less than 100 ppm, the curing reaction initiation temperature of the electrical insulating resin composition is controlled. Specifically, as will be described in detail later, it is possible to make the curing reaction initiation temperature of the electrical insulating resin composition relatively low or relatively high.

[0019] The amount of boron eluted from the boron nitride filler can be reduced by washing with hydrochloric acid solution or pure water. Therefore, the amount of boron eluted from the boron nitride filler can be adjusted as appropriate by changing the number of times washing with hydrochloric acid solution or pure water is performed.

[0020] The amount of boron eluted from boron nitride filler is measured by the following method. Specifically, 50 mL of 0.1 N sulfuric acid aqueous solution and 50 mg of boron nitride filler are placed in a 50 mL metal-free polypropylene (PP) container, and the mixture is shaken while adjusting the temperature to 25°C. After shaking for 30 minutes, the resulting extract is filtered through a 0.45 μm chromatograph, and the boron in the filtrate is analyzed using an ICP mass spectrometer (e.g., Agilent 8800 from Agilent Technologies). The amount of eluted boron (concentration of element B boron) [ppm] is determined by subtracting the eluted boron concentration in the blank from the eluted boron concentration during measurement, multiplying this difference by the volume of the extract, and dividing by the weighed mass of 50 mg of boron nitride filler.

[0021] The amount of boron eluted from the boron nitride filler is preferably 90 ppm or less, more preferably 80 ppm or less, even more preferably 70 ppm or less, and even more preferably 60 ppm or less. By reducing the amount of eluted boron, it is possible to lower or raise the curing reaction initiation temperature of the electrical insulating resin composition.

[0022] The amount of boron eluted from the boron nitride filler may be 0 ppm, 1 ppm or more, or 5 ppm or more.

[0023] Commercially available boron nitride fillers can be used. Examples of such products include those manufactured by Tokuyama Corporation, 3M Corporation, Denka Corporation, JFE Mineral Corporation, Resona Corporation, Momentive Corporation, DCEI Corporation, PENSC Corporation, or Bestry Corporation.

[0024] The electrical insulating resin composition of this embodiment contains at least boron nitride filler as an inorganic filler, but may further contain inorganic fillers other than boron nitride filler.

[0025] Other inorganic filler materials besides boron nitride include, for example, inorganic nitrides such as aluminum nitride or silicon nitride, inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), titanium oxide (titania), magnesium oxide (magnesia), and zirconium oxide (zirconia), as well as diamond, silicon carbide, talc, clay, and calcium carbonate.

[0026] In this embodiment, the thermal conductivity of the insulating layer (described in detail later) formed with the electrical insulating resin composition can be improved by including at least a boron nitride filler in the electrical insulating resin composition. In the electrical insulating resin composition, the proportion of boron nitride filler among the inorganic fillers may be 95% by mass or more, or 99% by mass or more.

[0027] (Epoxy resin) The electrical insulating resin composition of this embodiment contains an epoxy resin, but may further contain a curable resin other than an epoxy resin. Resins such as epoxy resins bind boron nitride filler particles together.

[0028] The epoxy resin includes, for example, bisphenol A type epoxy resin, modified bisphenol A type epoxy resin, bisphenol F type epoxy resin, modified bisphenol F type epoxy resin, trisphenolmethane type (triphenylmethane type) epoxy resin, novolac type epoxy resin (such as cresol novolac type epoxy resin), biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, or phenol novolac type epoxy resin. One of these epoxy resins can be used alone or two or more can be used in combination. Preferably, the epoxy resin contains at least one selected from bisphenol A type epoxy resin, trisphenolmethane type epoxy resin, and novolac type epoxy resin.

[0029] The epoxy equivalent [g / eq] of the epoxy resin may be, for example, 50 to 200, or for example, 200 to 500. The above epoxy equivalent is measured according to JIS K7236-2001.

[0030] Epoxy resin products can be obtained from companies such as Mitsubishi Chemical Corporation, Nippon Steel Chemical & Material Corporation, DIC Corporation, ADEKA Corporation, or Nippon Kayaku Co., Ltd.

[0031] (Curing agent) The above-mentioned electrical insulating resin composition contains, as a curing agent, at least one of, for example, a phenolic curing agent or an amine-based curing agent. As a phenolic curing agent, for example, a polymeric curing agent such as a phenolic resin can be used.

[0032] Examples of phenolic resins used as curing agents include phenolic resins having a novolac structure (such as novolac-type phenolic resins), aralkyl-type phenolic resins, dicyclopentadiene-modified phenolic resins, naphthalene-type phenolic resins, or bisphenol-based phenolic resins. Phenolic resins having a novolac structure have at least a structure in which phenolic structures are linked together in the molecule. A typical example of a phenolic resin having a novolac structure is phenol novolac resin. Phenolic resins having a novolac structure may also be, for example, xylene novolac resins (phenol-modified) that further have xylene structures. Note that phenolic curing agents may contain multiple types of phenolic resins.

[0033] The phenolic resin is preferably a phenolic resin having a novolac structure. This allows the cured product of the above-mentioned electrical insulating resin composition to have higher heat resistance, solvent resistance, strength, and hardness.

[0034] The hydroxyl group equivalent [g / eq] of the phenolic resin may be between 50 and 150. The above hydroxyl group equivalent can be calculated from the hydroxyl value measured according to the acetylation method in JIS K0070-1992.

[0035] Phenolic resin products can be obtained from companies such as UBE, Gun-ei Chemical Industry, DIC, or Nippon Kayaku Co., Ltd.

[0036] Examples of amine-based curing agents include aliphatic amine curing agents, alicyclic amine curing agents, aromatic aliphatic amine curing agents, and aromatic amine curing agents.

[0037] Examples of aliphatic amine curing agents include aliphatic diamines (which have a primary amino group in the molecule but no secondary amino group) such as ethylenediamine, 1,3-trimethylenediamine, 1,4-tetramethylenediamine, 1,3-pentamethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,2-propylenediamine, 1,2-butylenediamine, 2,3-butylenediamine, 1,3-butylenediamine, 2-methyl-1,5-pentamethylenediamine, 3-methyl-1,5-pentamethylenediamine, 2,4,4-trimethyl-1,6-hexamethylenediamine, and 2,2,4-trimethyl-1,6-hexamethylenediamine. Furthermore, aliphatic amine compounds include, for example, triamines such as diethylenetriamine, tetramines such as triethylenetetramine (TETA), pentamines such as tetraethylenepentamine, hexamines such as pentaethylenehexamine, and aliphatic polyamines (which have both primary and secondary amino groups in their molecules) such as dicyandiamide (which have both amino and cyano groups in their molecules).

[0038] As the aliphatic amine curing agent, aliphatic amine compounds having a primary amino group and a secondary amino group in the molecule are preferred, and tetramine or pentamine are more preferred.

[0039] Examples of alicyclic amine curing agents include 1,3-cyclopentanediamine, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, 1-amino-1-methyl-4-aminomethylcyclohexane, 1-amino-1-methyl-3-aminomethylcyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(3-methyl-cyclohexylamine), and methyl-2,3 Examples include cyclohexanediamine, methyl-2,4-cyclohexanediamine, methyl-2,6-cyclohexanediamine, 1,3-bis(aminoalkyl)cycloalkane (also known as 1,3-bis(aminomethyl)cyclohexane), 1,4-bis(aminoalkyl)cycloalkane (also known as 1,4-bis(aminomethyl)cyclohexane), isophoronediamine, norbornanediamine, and other alicyclic diamines (which have a primary amino group in their molecule but no secondary amino group).

[0040] Examples of aromatic amine curing agents include 4,4'-diphenylmethanediamine, 2,4'-diphenylmethanediamine, and 4,4'-diaminodiphenylsulfone (which have primary amino groups in their molecules but no secondary amino groups).

[0041] Examples of aromatic aliphatic amine curing agents include 1,3-xylylenediamine and 1,4-xylylenediamine (which have a primary amino group in their molecule but no secondary amino group).

[0042] The amine-based curing agent is preferably a diaminodiphenyl sulfone such as 4,4'-diaminodiphenyl sulfone. This allows the above-mentioned electrical insulating resin composition to have a longer pot life, and the cured product of the above-mentioned electrical insulating resin composition may have higher heat resistance and solvent resistance.

[0043] Amine-based curing agents can be obtained from companies such as Konishi Chemical Industry Co., Ltd., Seika Corporation, Mitsubishi Chemical Corporation, DIC Corporation, ThreeBond Corporation, Ajinomoto Fine Techno Corporation, ADEKA Corporation, or Kumiai Chemical Industry Co., Ltd.

[0044] (Curing Accelerator) Examples of the curing accelerator include phosphorus-based curing accelerators, boron trifluoride-based curing accelerators, imidazole-based curing accelerators, and the like.

[0045] Examples of the phosphorus-based curing accelerator include triphenylphosphine (TPP), tri-p-tolylphosphine (TPTP), tetraphenylphosphonium tetraphenylborate (TPP-K), tetraphenylphosphonium tetra-p-tolylborate (TPP-MK), and the like.

[0046] Examples of the boron trifluoride-based curing accelerator include boron trifluoride aniline, boron trifluoride p-toluidine, boron trifluoride N-methylaniline, boron trifluoride N-ethylaniline, boron trifluoride 2,4-dimethylaniline, boron trifluoride benzylamine, boron trifluoride monoethylamine, boron trifluoride N,N-dimethylaniline, boron trifluoride triethanolamine, boron trifluoride piperidine, boron trifluoride triethylamine, boron trifluoride ethyl ether, boron trifluoride methyl ether, boron trifluoride n-butyl ether, boron trifluoride tetrahydrofuran, boron trifluoride phenol, and the like. Among these, boron trifluoride monoethylamine, boron trifluoride triethanolamine, and boron trifluoride piperidine are preferable.

[0047] Examples of the imidazole-based catalyst include imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxyimidazole, 2-phenyl-4,5-dihydroxydimethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and the like.

[0048] As the above curing accelerator, a commercially available product can be used. Such products are available from, for example, Stella Chemifa Corporation, San-Apro Ltd., Hokko Chemical Industry Co., Ltd., or Shikoku Kasei Holdings Co., Ltd. and the like.

[0049] When the resin composition for electrical insulation of the present embodiment contains a phenolic curing agent as the curing agent, the curing accelerator preferably contains a phosphorus-based curing accelerator. Hereinafter, such an example will be described in detail as Specific Example 1. On the other hand, when the resin composition for electrical insulation of the present embodiment contains an amine-based curing agent as the curing agent, the curing accelerator preferably contains a boron trifluoride-based curing accelerator. Hereinafter, such an example will be described in detail as Specific Example 2.

[0050] (Specific Example 1) In the resin composition for electrical insulation, the eluted boron content of the boron nitride filler is less than 100 ppm, the phenolic curing agent is contained as the curing agent, and the phosphorus-based curing accelerator is contained as the curing accelerator, whereby the curing reaction initiation temperature can be made relatively low. By lowering the curing reaction initiation temperature, it is possible to start the curing reaction of the resin composition for electrical insulation at a lower temperature, or to further accelerate the curing reaction at the same temperature. As described above, when the eluted boron content of the boron nitride filler is in the range of less than 100 ppm, the curing reaction of the resin composition for electrical insulation can be accelerated. Therefore, even if the resin composition for electrical insulation partially contains a component that inhibits the curing reaction, the curing reaction of the resin composition for electrical insulation is accelerated, and a cured product in which the curing reaction has proceeded to a desired degree can be obtained relatively stably and conveniently.

[0051] In the resin composition for electrical insulation of Specific Example 1, the amount of the phenolic curing agent relative to 100 parts by mass of the epoxy resin is preferably 55 parts by mass or more and 65 parts by mass or less.

[0052] The resin composition for electrical insulation of Specific Example 1 preferably contains the boron nitride filler in an amount of 70 mass% or more and 75 mass% or less. The resin composition for electrical insulation of Specific Example 1 preferably contains the epoxy resin in an amount of 15 mass% or more and 20 mass% or less. The resin composition for electrical insulation of Specific Example 1 preferably contains the phenolic curing agent in an amount of 5 mass% or more and 15 mass% or less.

[0053] (Specific Example 2) In an electrical insulating resin composition, the amount of eluted boron from the boron nitride filler is less than 100 ppm, an amine-based curing agent is included as the curing agent, and a boron trifluoride-based curing accelerator is included as the curing accelerator, which allows the curing reaction initiation temperature to be relatively high. By increasing the curing reaction initiation temperature, it is possible to start the curing reaction of the electrical insulating resin composition at a higher temperature, or to further suppress the curing reaction at the same temperature. Thus, by keeping the amount of eluted boron from the boron nitride filler in the range of less than 100 ppm, the curing reaction of the electrical insulating resin composition can be suppressed. Therefore, even if some of the components contained in the electrical insulating resin composition unintentionally promote the curing reaction, the curing reaction can be suppressed, and a cured product with the curing reaction progressing to the desired degree can be obtained relatively stably and easily.

[0054] In the electrical insulating resin composition of Specific Example 2, the amount of amine-based curing agent per 100 parts by mass of epoxy resin is preferably 15 parts by mass or more and 25 parts by mass or less.

[0055] The electrical insulating resin composition of Specific Example 2 preferably contains 70% to 75% by mass of boron nitride filler. The electrical insulating resin composition of Specific Example 2 preferably contains 20% to 25% by mass of epoxy resin. The electrical insulating resin composition of Specific Example 2 preferably contains 3% to 7% by mass of amine-based curing agent.

[0056] In the total mass of the electrical insulating resin composition such as Specific Example 1 or Specific Example 2, the proportion of inorganic fillers such as boron nitride filler, epoxy resin, curing agent (phenol-based curing agent or amine-based curing agent), and curing accelerator may be 95% by mass or more, 98% by mass or more, or 99% by mass or more.

[0057] In the electrical insulating resin composition such as Specific Example 1 or Specific Example 2, the total amount of epoxy resin and curing agent (phenol-based curing agent or amine-based curing agent) relative to 100 parts by mass of inorganic filler such as boron nitride filler may be 35 parts by mass or more and 45 parts by mass or less.

[0058] In the electrical insulating resin composition, such as in Specific Example 1 or Specific Example 2, the total of 100 parts by mass of the inorganic filler such as boron nitride filler, epoxy resin, and curing agent (phenol-based curing agent or amine-based curing agent) may be less than 45 parts by mass of epoxy resin and curing agent (phenol-based curing agent or amine-based curing agent) in total (when the total is 100 parts by mass). The electrical insulating resin composition may contain 10 parts by mass or more of epoxy resin and curing agent (phenol-based curing agent or amine-based curing agent) in total out of the above total of 100 parts by mass, or 20 parts by mass or more.

[0059] In the electrical insulating resin composition, the content of phenolic resin may be 50 parts by mass or more and 70 parts by mass or less per 100 parts by mass of epoxy resin. In the electrical insulating resin composition, the content of amine-based curing agent may be 10 parts by mass or more and 30 parts by mass or less per 100 parts by mass of epoxy resin. In the electrical insulating resin composition, the content of curing accelerator may be 0.50 parts by mass or more and 1.50 parts by mass or less per 100 parts by mass of epoxy resin.

[0060] The electrical insulating resin composition of this embodiment may further contain additives such as antioxidants.

[0061] Next, the insulating sheet 10 of this embodiment will be described in detail. <Insulating Sheet> The insulating sheet 10 of this embodiment is formed from the electrical insulating resin composition described above and is in the form of a sheet, as shown in Figures 1A and 1B, respectively. The insulating sheet 10 of this embodiment may be formed in the shape of a rectangle, or it may be formed in the shape of a strip (long sheet).

[0062] The insulating sheet 10 of this embodiment may have only an insulating layer 11, as shown in Figure 1A, or it may have an insulating layer 11 and a base material 12 that overlaps one side of the insulating layer 11, as shown in Figure 1B.

[0063] The base material 12 is, for example, a metal foil or a metal plate. The type of metal contained in the base material 12 is not particularly limited, but may be, for example, copper or aluminum. In other words, the base material 12 may be copper foil, aluminum foil, aluminum foil, or an aluminum plate.

[0064] The insulating layer 11 described above contains the electrical insulating resin composition described above and is, for example, in a B-stage state. Before the insulating layer 11 reaches a fully cured state (C-stage state), it can be used in applications as a pressure-sensitive adhesive sheet.

[0065] The thickness (total thickness) of the insulating layer 11 is not particularly limited and may be, for example, 20 μm or more, 50 μm or more, and preferably 100 μm or more. The thickness (total thickness) of the insulating layer 11 may be 300 μm or less, and preferably 200 μm or less. The insulating layer 11 may be a single layer or a laminate of multiple layers. At least one layer constituting the insulating layer 11 is formed of the above-mentioned electrical insulating resin composition.

[0066] Since the insulating layer 11 of the insulating sheet 10 in this embodiment is configured as described above, the curing reaction initiation temperature is controlled, similar to the electrical insulating resin composition described above.

[0067] In this embodiment, when the insulating layer 11 is sufficiently cured (C-stage state), the dielectric breakdown voltage of the insulating layer 11 is, for example, 5.0 kV or higher. However, the above dielectric breakdown voltage may be, for example, 30.0 kV or lower.

[0068] In this embodiment, when the insulating layer 11 is sufficiently cured (C-stage state), the thermal conductivity of the insulating layer 11 is, for example, 5 W / m·K or higher. However, the above thermal conductivity may be 35 W / m·K or lower.

[0069] Next, we will explain the manufacturing method of the insulating sheet described above.

[0070] <Method for Manufacturing an Insulating Sheet> The method for manufacturing an insulating sheet is a method for manufacturing an insulating sheet (the insulating sheet 10 described above) which comprises at least an insulating layer formed of the above-described electrical insulating resin composition. The above manufacturing method comprises, for example, a step of forming a pre-curing insulating layer (pre-curing insulating layer formation step) by volatilizing the organic solvent from a coating liquid containing at least the above-described boron nitride filler, epoxy resin, epoxy resin curing agent, and organic solvent, and a step of producing an insulating layer in a B-stage state by B-stage the pre-curing insulating layer (B-stage formation step).

[0071] For example, in the above manufacturing method, first, a coating liquid containing the compounding components that will constitute the insulating layer 11 and an organic solvent, and a coating sheet are prepared. As the coating sheet, a transfer sheet Z or a substrate 12 is used. As the transfer sheet Z, a general type such as a resin film with a release treatment on its surface is used. The substrate 12 is as described above. Next, in the pre-curing insulating layer formation step, a coating liquid is applied to the surface of the transfer sheet Z or the substrate 12 (coating sheet) to form a film on the transfer sheet Z or the substrate 12. Furthermore, the organic solvent is evaporated from the film to form a pre-curing insulating layer 11a, and two laminated sheets W are prepared, for example, in which the dried film (pre-curing insulating layer) overlaps one side of the transfer sheet Z or the substrate 12 (see Figure 2).

[0072] Next, in the B-stage preparation process described above, two laminated sheets W are prepared, and the two laminated sheets W, W are stacked on top of each other so that the two pre-cured insulating layers 11a are in contact with each other, as shown in Figure 2, for example, and then subjected to a heat and pressure treatment (hereinafter also referred to as a heat press treatment). This causes the curing reaction in the two pre-cured insulating layers 11a to proceed separately while they are integrated. In this way, an insulating layer 11 in the B-stage state is produced.

[0073] In preparing the coating solution described above, for example, the boron nitride filler and epoxy resin mentioned above are mixed with an organic solvent. A general method can be used for mixing.

[0074] Examples of organic solvents that can be used include ethyl acetate, methyl ethyl ketone (MEK), and toluene.

[0075] When applying the coating solution to the transfer sheet Z or the substrate 12 (coating sheet), general coating methods such as die coating and reverse coating can be used. The temperature during coating is usually room temperature (15-25°C).

[0076] The temperature required to volatilize the organic solvent in the coating solution may be, for example, 60°C to 150°C.

[0077] The hot pressing treatment is carried out under temperature, pressure, and time conditions that can remove defects (e.g., voids) inside the pre-curing insulating layer 11a. For example, the conditions for the hot pressing treatment are a temperature of 80°C to 150°C, a pressure of 2 MPa to 10 MPa, and a duration of 5 minutes to 60 minutes. By performing the hot pressing treatment, the insulating layer 11 enters the B-stage state.

[0078] Next, a semiconductor device equipped with the insulating layer 11 described above will be explained in detail.

[0079] <Semiconductor Devices> Examples of semiconductor devices include so-called power semiconductor devices, which are equipped with power diodes for rectification and power transistors for switching and amplification. Examples of power transistors include thyristors, power MOSFETs (metal-oxide-semiconductor field-effect transistors), and IGBTs (isolated gate bipolar transistors).

[0080] The semiconductor device 100 is rectangular in shape, as shown in Figures 3A to 3C, for example, and includes an insulating sheet 10 inside. The semiconductor device 100 has the insulating layer 11 described above and a heat dissipation member 20 to which the insulating layer 11 is bonded (see, for example, Figures 3A and 3B). The following will describe in detail the state in which the insulating sheet 10 described above is arranged so that its thickness direction is the vertical direction. In the following description, the thickness direction of the semiconductor device may be referred to as the "vertical direction," "up and down direction," or "perpendicular direction," and the direction perpendicular to the "thickness direction" may be referred to as the "horizontal direction," "horizontal direction," or "surface direction."

[0081] The semiconductor device 100 has a rectangular parallelepiped body and two terminals T, T protruding upward from the top surface of the body. The semiconductor device 100 has a semiconductor element 30 in the center of the thickness direction and the center of the planar direction. The semiconductor device 100 further includes two lead frames 40 which are conductive paths connected to the semiconductor element 30, a metal plate-shaped heat dissipation member 20, and an insulating sheet 10 (for example, an insulating layer 11 in a C-stage state, which will be described later) disposed between the heat dissipation member 20 and the semiconductor element 30.

[0082] The main body of the semiconductor device 100 further comprises a rectangular frame-shaped case 50 and a molded resin 60 that fills the inside of the case 50 and in which semiconductor elements 30 and the like are embedded. The upper surface of the molded resin 60 forms the upper surface of the main body.

[0083] The semiconductor element 30 may be a packaged element or a bare chip.

[0084] Each of the two lead frames 40 is formed by bending a strip-shaped metal plate at approximately a right angle at one point along its length. Each lead frame 40 has a portion extending horizontally from the bent portion and a portion extending upward. A semiconductor element 30 is positioned on the upper surface of the horizontally extending portion of one lead frame 40a. The upper end of the vertically extending portion of one lead frame 40a protrudes above the upper surface of the molded resin 60, forming one terminal T. This lead frame 40a forms a conductive path in the semiconductor device 100 and is configured to transmit the heat generated by the semiconductor element 30 to the outside of the semiconductor element 30. The other lead frame 40b is similar to the one lead frame 40a in that the upper end of the vertically extending portion forms the other terminal T.

[0085] Each lead frame 40 is formed from a general-purpose metal such as iron, copper, aluminum, or nickel. Each lead frame is preferably made of copper because it has good conductivity and a relatively high specific heat. The copper lead frame 40 may be made of pure copper or a copper alloy. Each lead frame 40 may also be surface-treated, such as by plating.

[0086] The heat dissipation member 20 is located at the bottom of the semiconductor device 100. An insulating sheet 10 (for example, an insulating layer 11 in the C-stage state, described later) is placed between the heat dissipation member 20 and the horizontally extending portion of one of the lead frames 40. The outer surface of the heat dissipation member 20 is exposed at the bottom of the semiconductor device 100.

[0087] The semiconductor device 100 described above is configured to dissipate heat from the semiconductor element 30 to the outside through the heat dissipation member 20. In other words, the semiconductor device 100 described above is configured so that the heat generated in the internal semiconductor element 30 is mainly transferred to the outside via the lower surface of the heat dissipation member 20. The semiconductor device 100 described above may also be used with a refrigerant-circulating heat sink or heat dissipation fins for atmospheric heat dissipation in contact with the lower surface of the heat dissipation member 20. Furthermore, the semiconductor device 100 described above may also be used with a component with a relatively large heat capacity (for example, a housing) in contact with the lower surface of the heat dissipation member 20.

[0088] The heat dissipation member 20 has good thermal conductivity. It is preferable that the heat dissipation member 20 is made of a material with high surface hardness and resistance to scratches, in order to ensure good adhesion when in contact with the heat sink or heat sink fins. Furthermore, it is preferable that the heat dissipation member 20 is made of a material with relatively high rigidity, in order to resist deformation when in contact with the heat sink or heat sink fins. From the above viewpoint, it is preferable that the heat dissipation member 20 is made of aluminum. The aluminum heat dissipation member 20 may be made of pure aluminum or an alloy containing aluminum (aluminum alloy).

[0089] The insulating layer 11 of the insulating sheet 10 described above is placed, for example, between a horizontally extending portion of one lead frame 40 and the heat dissipation member 20, and is bonded to the heat dissipation member 20 in a C-stage state (sufficiently cured state).

[0090] As the heat dissipation member 20, for example, an aluminum plate made of A1100, A1050, or A5052 with a thickness of 0.1 mm to 10 mm can be used.

[0091] The insulating layer 11 is placed inside the semiconductor device 100 to electrically insulate the lead frame 40 from the heat dissipation member 20. The heat dissipation member 20 and the lead frame 40 are bonded together by the insulating layer 11. The semiconductor device 100 is configured to transfer heat from one lead frame 40a on the upstream side of the heat dissipation path, through the insulating layer 11, to the heat dissipation member 20 on the downstream side of the heat dissipation path.

[0092] Although Figure 3B uses a plate-shaped heat dissipation member as an example, the heat dissipation member 20 may also be a heat dissipation fin 20x, as shown in Figure 3C.

[0093] Figures 3B and 3C show a state in which only the insulating layer 11 is placed between the heat dissipation member 20 and the lead frame 40. However, as shown in Figure 4A, for example, the semiconductor device 100 may have a substrate 12 of the insulating sheet 10 and a heat transfer material (generally referred to as TIM), with the insulating layer 11 positioned closer to the lead frame 40 than the substrate 12, and the heat transfer material (TIM) placed between the substrate 12 and the heat dissipation member 20. A general commercially available product can be used as such a heat transfer material. On the other hand, as shown in Figure 4B, for example, the semiconductor device 100 may have a substrate 12 of the insulating sheet 10 and a heat transfer material (TIM), with the insulating layer 11 positioned closer to the heat dissipation member 20 than the substrate 12, and the heat transfer material (TIM) placed between the substrate 12 and the lead frame 40.

[0094] In the semiconductor device 100, the insulating sheet 10 adheres well to the substrate between the lead frame 40 and the heat dissipation member 20. For example, the insulating layer 11 in the C-stage state adheres well to both the lead frame 40 and the heat dissipation member 20.

[0095] The semiconductor device 100 described above is manufactured by, for example, arranging the heat dissipation member 20, insulating layer 11, lead frame 40, and semiconductor element 30, etc., in the positions shown in Figure 3B. The insulating layer 11 is a part of the components that make up the semiconductor device 100.

[0096] The electrical insulating resin composition and insulating sheet of this embodiment are as illustrated above, but the present invention is not limited to these examples. That is, various forms commonly used in electrical insulating resin compositions and insulating sheets can be adopted as long as they do not impair the effects of the present invention.

[0097] The matters disclosed herein include: (1) an electrical insulating resin composition comprising a boron nitride filler, an epoxy resin, and a curing agent for the epoxy resin, wherein the amount of boron eluted from the boron nitride filler is less than 100 ppm. The electrical insulating resin composition having the above configuration allows control of the curing reaction initiation temperature while containing the boron nitride filler. (2) The electrical insulating resin composition according to (1) further comprising a curing accelerator, wherein the curing agent comprises a phenolic curing agent, and the curing accelerator comprises a phosphorus curing accelerator. (3) The electrical insulating resin composition according to (1) further comprising a curing accelerator, wherein the curing agent comprises an amine curing agent, and the curing accelerator comprises a boron trifluoride curing accelerator. (4) an insulating sheet comprising an insulating layer formed of an electrical insulating resin composition according to any one of (1) to (3) above. The insulating layer of the insulating sheet having the above configuration allows control of the curing reaction initiation temperature while containing the boron nitride filler.

[0098] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0099] An electrical insulating resin composition was prepared as described below, and an insulating layer was formed using this electrical insulating resin composition. Then, an insulating sheet consisting only of the insulating layer was manufactured. The formulations for manufacturing the insulating sheets for each example and comparative example are shown in Tables 1 and 2.

[0100] <Raw materials for insulating sheet (insulating layer)> (A) Boron nitride filler Boron nitride filler (BN filler) Commercially available product However, various boron nitride fillers with different numbers of washes using hydrochloric acid aqueous solution and pure water were used in each example and each comparative example. (B) Epoxy resins (B-1) Trisphenolmethane type epoxy resin Epoxy equivalent: 168 [g / eq] Product name "EPPN-502H" (manufactured by Nippon Kayaku Co., Ltd.) (B-2) Bisphenol A type epoxy resin Epoxy equivalent: 475 [g / eq] Product name "YD-011" (manufactured by Nippon Steel Chemical & Material Co., Ltd.) (B-3) Novolac type epoxy resin (o-cresol novolac type) Epoxy equivalent: 208 [g / eq] Product name "YDCN-704" (manufactured by Nippon Steel Chemical & Material Co., Ltd.) (C) Curing agents (C-1) Phenolic curing agent (novolac type phenol resin) Hydroxyl group equivalent: 105 [g / eq] Product name "GS-200" (manufactured by Gun-ei Chemical Industry Co., Ltd.) (C-2) Amine-based curing agent (4,4'-diaminodiphenylsulfone) Product name: "Seika Cure-S" (manufactured by Seika Co., Ltd.) (D) Curing accelerator (D-1) Tetraphenylphosphonium tetraphenylborate (TPP-K) Commercial product (D-2) Boron trifluoride monoethylamine Commercial product

[0101] <Manufacturing of Insulating Sheet (Insulating Layer)> (Each Example and Each Comparative Example) The above amounts of raw materials and organic solvent (methyl ethyl ketone MEK) were mixed at 23°C to prepare a coating solution. Furthermore, each prepared coating solution was applied to a transfer sheet (PET film) by die coating. It was left to stand at 80-120°C for 3 minutes to evaporate the organic solvent and form a pre-curing insulating layer. In this way, two laminated sheets were made by laminating the transfer sheet and the pre-curing insulating layer. The two laminated sheets were stacked so that the pre-curing insulating layers were in contact with each other, and then a hot press treatment was performed. The conditions for the hot press treatment were a temperature of 120°C, a pressure of 5 MPa or more, and a duration of 50 minutes. By performing the hot press treatment, an insulating layer with a thickness of 120 μm and in the B stage state was manufactured.

[0102] The amount of eluted boron from the boron nitride filler used in each example and comparative example was measured by the method described above. The measurement results of the amount of eluted boron are shown in Tables 1 and 2.

[0103]

[0104]

[0105] <Performance Evaluation of the Insulating Layer> The curing reaction initiation temperature was measured for the insulating layers produced in each example and comparative example as follows.

[0106] (Curing reaction start temperature of insulating layer (electrical insulating resin composition)) The curing reaction start temperature of the insulating layer of each example and comparative example was measured by differential scanning calorimetry (DSC) analysis as follows. The measurement results of the curing reaction start temperature are shown in Tables 1 and 2. (Details of measurement method by DSC analysis) Amount of sample: Approximately 8.0 mg of the insulating layer before curing was weighed. Measurement atmosphere: Nitrogen gas. Measurement conditions: (1) Hold at 30°C for 1 minute. (2) Heat up to 250°C at a heating rate of 3°C / min. Analysis method: A chart is created with temperature (°C) on the horizontal axis and heat flow (W) on the vertical axis. Based on the curve of the chart, the slope (ΔW / ΔT) of the curve from each arbitrary temperature (Ts) up to +10°C (T+10) is determined. The temperature at which the slope is 0.1 [mW / °C] or more (a specific temperature among the above Ts) is taken as the curing reaction start temperature. The slope (ΔW / ΔT) is calculated by the following formula. Note that the heat flow corresponding to Ts is represented by Ws. Slope (ΔW / ΔT) [W / °C] = [(W+10)-Ws] / [(T+10)-Ts]) Furthermore, graphs showing the relationship between the amount of boron eluted from the boron nitride filler measured as described above and the curing reaction initiation temperature are shown in Figures 5A and 5B. Figure 5A is a graph when a phenol-based curing agent is used as the curing agent and a phosphorus-based curing accelerator is used as the curing accelerator. Figure 5B is a graph when an amine-based curing agent is used as the curing agent and a boron trifluoride-based curing accelerator is used as the curing accelerator.

[0107] As can be seen from Tables 1 and 2, and Figures 5A and 5B, the curing reaction initiation temperature of the insulating layer (electrical insulating resin composition) could be controlled to be relatively low or relatively high. Specifically, in the insulating layer of the insulating sheet in the examples, since the amount of eluted boron from the boron nitride filler was less than 100 ppm, when a phenol-based curing agent was included as the curing agent and a phosphorus-based curing accelerator was included as the curing accelerator, the curing reaction initiation temperature of the insulating layer could be made relatively low. Therefore, the curing reaction of the insulating layer could be accelerated. On the other hand, in the insulating layer of the insulating sheet in the examples, since the amount of eluted boron from the boron nitride filler was less than 100 ppm, when an amine-based curing agent was included as the curing agent and a boron trifluoride-based curing accelerator was included as the curing accelerator, the curing reaction initiation temperature of the insulating layer could be made relatively high. Therefore, the curing reaction of the insulating layer could be suppressed. Because the curing reaction of the insulating layer can be controlled in this way, for example, before manufacturing the insulating layer, it is possible to know in advance whether the curing reaction of the insulating layer is likely to be accelerated or inhibited, based on the fact that the amount of eluted boron from the boron nitride filler is a relatively small predetermined amount. Therefore, the temperature or time of the heat treatment to advance the curing reaction of the insulating layer can be adjusted in advance, and thus an insulating layer with a desired degree of curing can be stably obtained.

[0108] The insulating layer of the insulating sheet of the present invention is suitably used, for example, by being attached to each adherend between two adherends that should be electrically insulated from each other. Moreover, it is used to transfer heat from one adherend to the other. For example, the insulating layer is suitably used in semiconductor devices by being placed between a conductive member, such as a lead frame in contact with a semiconductor element, and a heat dissipation member, in order to transfer heat generated by the semiconductor element to the heat dissipation member, and to electrically insulate the conductive member and the heat dissipation member.

[0109] 100: Semiconductor device, 10: Insulating sheet, 11: Insulating layer, 12: Substrate, 20: Heat dissipation component, 30: Semiconductor element, 40: Lead frame, 50: Case, 60: Molding resin.

Claims

1. An electrical insulating resin composition comprising a boron nitride filler, an epoxy resin, and a curing agent for the epoxy resin, wherein the amount of boron eluted from the boron nitride filler is less than 100 ppm.

2. The electrical insulating resin composition according to claim 1, further comprising a curing accelerator, wherein the curing agent comprises a phenolic curing agent, and the curing accelerator comprises a phosphorus curing accelerator.

3. The electrical insulating resin composition according to claim 1, further comprising a curing accelerator, wherein the curing agent comprises an amine-based curing agent, and the curing accelerator comprises a boron trifluoride-based curing accelerator.

4. An insulating sheet comprising an insulating layer formed of an electrical insulating resin composition as described in any one of claims 1 to 3.