Low-pressure multi-layer glass and method for manufacturing same
Low-pressure double-glazed glass with glass plates and a crystallized glass sealing layer addresses thermal expansion and manufacturing complexity issues, achieving improved sealing and productivity.
Patent Information
- Application Number
- PCT/JP2026/016795
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional low-pressure double-glazed glass faces challenges in achieving a low thermal expansion coefficient and high manufacturing productivity due to difficulties in sealing glass plates with bismuth-based glass and complex manufacturing processes involving exhaust pipes.
The use of glass plates with low thermal expansion coefficients joined by a sealing layer containing crystallized glass, particularly with a β-quartz solid solution, allows for simultaneous heat treatment and vacuum evacuation, eliminating the need for exhaust ports and improving sealing strength.
The solution results in low-pressure double-glazed glass with reduced thermal expansion and enhanced productivity by ensuring effective sealing and simplifying the manufacturing process.
Smart Images

Figure JP2026016795_19112026_PF_FP_ABST
Abstract
Description
Low-pressure double-glazed glass and method for manufacturing the same
[0001] This invention relates to low-pressure double-glazed glass and a method for manufacturing the low-pressure double-glazed glass.
[0002] Traditionally, low-pressure double-glazed glass with high thermal insulation performance has been used in various fields, including residential construction, transportation (automobiles, ships, aircraft, etc.), and equipment such as refrigerators, freezers, and constant temperature and humidity chambers.
[0003] Low-pressure double-glazed windows have a structure in which two glass plates are arranged with a predetermined gap between them, and their outer edges are sealed with a sealing material. In addition, low-pressure double-glazed windows may be provided with exhaust pipes or exhaust vents to exhaust the internal space, and sealing material is also used to attach the covers that seal these exhaust pipes or vents.
[0004] Patent Document 1 discloses, as an example of such a sealing material, a sealing material containing bismuth-based glass powder and a refractory filler. Patent Document 1 describes that the above sealing material can be sealed at low temperatures, has good thermal stability, is resistant to softening and deformation even when evacuated at high temperatures, and matches the thermal expansion coefficient of the soda glass plate. Patent Document 1 also states that the softening point of the above sealing material is preferably 410°C or higher, 415°C to 500°C, and particularly 420°C to 460°C.
[0005] Japanese Patent Publication No. 2011-84437
[0006] Incidentally, when low-pressure double-glazed windows are installed in houses and other buildings, the temperature difference between the inside and outside can cause warping of the glass panes that make up the low-pressure double-glazed windows. Furthermore, this tendency is more pronounced in refrigerators and freezers that also function as display cases, where the conditions are more severe. For this reason, there is a demand for low-pressure double-glazed windows made of materials with a lower coefficient of thermal expansion.
[0007] However, in low-pressure double-glazed glass, such as that described in Patent Document 1, which consists of two soda-lime glass plates bonded together with a sealing material, there is a problem in that it is difficult to sufficiently lower the coefficient of thermal expansion. Although it is also conceivable to use glass plates with a low coefficient of thermal expansion instead of soda-lime glass plates, it can be difficult to properly seal the gaps between these glass plates with a sealing material using bismuth-based glass, as described in Patent Document 1.
[0008] Furthermore, in the method of manufacturing low-pressure double-glazed glass, as described in Patent Document 1, where two soda glass plates are sealed with a sealing material and then the inside is exhausted using an exhaust pipe or exhaust port, the manufacturing process becomes complicated, making it difficult to increase the productivity of low-pressure double-glazed glass.
[0009] The object of the present invention is to provide low-pressure double-glazed glass and a method for manufacturing the low-pressure double-glazed glass that can be constructed from materials with a low coefficient of thermal expansion and can also increase productivity.
[0010] This document describes various embodiments of low-pressure double-glazed glass and a method for manufacturing the low-pressure double-glazed glass that solve the above problems.
[0011] The low-pressure double-glazed glass according to Embodiment 1 of the present invention is constructed by joining glass plates together via a sealing layer, and has an internal space that is under lower pressure than the outside, and has a thermal expansion coefficient of -30 × 10⁻¹⁰ from 30°C to 380°C. -7 / K ~ +30 × 10 -7 The glass apparatus comprises a first glass plate and a second glass plate, both having a temperature of / K, and a sealing layer provided between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are joined via the sealing layer, forming an internal space surrounded by the first glass plate, the second glass plate, and the sealing layer, the internal space is under lower pressure than the outside, and the sealing layer contains crystallized glass, the crystallized glass contains a β-quartz solid solution as the main crystal.
[0012] The low-pressure multilayer glass according to aspect 2 of the present invention is configured by glass plates being joined to each other via a sealing layer, and is a low-pressure multilayer glass provided with an internal space having a lower pressure than the outside, wherein the thermal expansion coefficient at 30°C to 380°C is -30×10 -7 / K to +30×10 -7 / K, comprising a first glass plate and a second glass plate, and a sealing layer provided between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are joined via the sealing layer, an internal space surrounded by the first glass plate, the second glass plate, and the sealing layer is formed, the pressure inside the internal space is lower than the outside, the sealing layer comprises crystallized glass, and the crystallized glass has a thermal expansion coefficient at 30°C to 380°C of -30×10 -7 / K to +30×10 -7 / K.
[0013] In the low-pressure multilayer glass according to aspect 3, in aspect 1 or aspect 2, it is preferable that the crystallized glass constituting the sealing layer contains, in mol%, SiO 2 48% to 75%, Al 2 O 3 5% to 25%, Li 2 O 5% to 30%, and ZnO 3% to 10%.
[0014] In the low-pressure multilayer glass according to aspect 4, in any one of aspects 1 to 3, it is preferable that the first glass plate and the second glass plate are composed of crystallized glass, the crystal phase transition temperature of crystals in the crystallized glass is 900°C or higher, and the crystal melting temperature is 1200°C or higher.
[0015] In the low-pressure multilayer glass according to aspect 5, in any one of aspects 1 to 3, it is preferable that the first glass plate and the second glass plate are composed of amorphous glass, and the softening point of the amorphous glass is 900°C or higher.
[0016] In the low-pressure multilayer glass according to aspect 6, in any one of aspects 1 to 5, it is preferable that the low-pressure multilayer glass is not provided with an exhaust port for exhausting the inside of the internal space.
[0017] A method for manufacturing low-pressure double-glazed glass according to embodiment 7 of the present invention is a method for manufacturing low-pressure double-glazed glass in which glass plates are joined together via a sealing layer, and an internal space is provided that is under lower pressure than the outside, comprising the steps of: placing a sealing material containing crystalline glass on the main surface of a first glass plate; and placing a second glass plate on the main surface of the first glass plate on which the sealing material is placed, and heat-treating it in a vacuum, wherein the heat treatment precipitates a β-quartz solid solution as the main crystal in the sealing material.
[0018] According to the present invention, it is possible to provide low-pressure double-glazed glass and a method for manufacturing the low-pressure double-glazed glass that can be constructed from a material with a low coefficient of thermal expansion and can also increase productivity.
[0019] Figure 1 is a schematic plan view showing a low-pressure double-glazed glass according to one embodiment of the present invention. Figure 2 is a schematic cross-sectional view showing the portion along line A-A in Figure 1. Figures 3(a) and (b) are schematic plan views illustrating a method for manufacturing low-pressure double-glazed glass according to one embodiment of the present invention.
[0020] Preferred embodiments are described below. However, the following embodiments are merely illustrative, and the present invention is not limited to these embodiments. In addition, in each drawing, components having substantially the same function may be referred to by the same reference numerals.
[0021] [Low-Pressure Double Glazing] Figure 1 is a schematic plan view showing low-pressure double glazing according to one embodiment of the present invention. Figure 2 is a schematic cross-sectional view showing the portion along line A-A in Figure 1.
[0022] The low-pressure double-glazed glass 1 comprises a first glass plate 2, a second glass plate 3, and a sealing layer 4. The low-pressure double-glazed glass 1 is constructed by joining the first glass plate 2 and the second glass plate 3 via the sealing layer 4. The low-pressure double-glazed glass 1 also has an internal space 5 that is under lower pressure than the outside.
[0023] The first glass plate 2 has opposing first main surface 2a and second main surface 2b. The first main surface 2a of the first glass plate 2 is the main surface facing the internal space 5. The second main surface 2b of the first glass plate 2 is the main surface on the opposite side from the internal space 5 and is the outer main surface of the low-pressure double-glazed glass 1.
[0024] The second glass plate 3 has opposing first main surface 3a and second main surface 3b. The first main surface 3a of the second glass plate 3 is the main surface facing the internal space 5. The second main surface 3b of the second glass plate 3 is the main surface on the opposite side from the internal space 5 and is the outer main surface of the low-pressure double-glazed glass 1.
[0025] The sealing layer 4 is provided between the first main surface 2a of the first glass plate 2 and the first main surface 3a of the second glass plate 3. More specifically, the sealing layer 4 has a frame-like shape and is provided between the outer peripheral edge portion 2c of the first main surface 2a of the first glass plate 2 and the outer peripheral edge portion 3c of the first main surface 3a of the second glass plate 3.
[0026] The sealing layer 4, together with the first glass plate 2 and the second glass plate 3, forms an internal space 5. In this embodiment, the sealing layer 4 has a frame-like shape, but the shape of the sealing layer 4 is not particularly limited as long as it can form an internal space 5 together with the first glass plate 2 and the second glass plate 3.
[0027] The first glass plate 2 has a thermal expansion coefficient of -30 × 10⁻¹⁰ between 30°C and 380°C. -7 / K ~ +30 × 10 -7 The temperature is / K. The second glass plate 3 has a coefficient of thermal expansion of -30 × 10 in the range of 30°C to 380°C. -7 / K ~ +30 × 10 -7 It is / K. Furthermore, the sealing layer 4 contains crystallized glass.
[0028] In the first invention of this application, the crystallized glass contained in the sealing layer 4 contains a β-quartz solid solution as the main crystal. Furthermore, in the second invention of this application, the thermal expansion coefficient of the crystallized glass contained in the sealing layer 4 from 30°C to 380°C is -30 × 10 -7 / K ~ +30 × 10 -7 It is K.
[0029] Hereinafter, the first invention and the second invention may be collectively referred to as the present invention. The first invention and the second invention may be implemented individually or in combination.
[0030] Since the low-pressure double-glazed glass 1 of this embodiment has the above configuration, it can be made of a material with a low coefficient of thermal expansion, and productivity can be increased.
[0031] Conventionally, low-pressure double-glazed glass, which consists of two soda-lime glass plates bonded together with a sealant, has had the problem of difficulty in sufficiently lowering the coefficient of thermal expansion. Although it is possible to use a glass plate with a lower coefficient of thermal expansion instead of soda-lime glass, it has been difficult to properly seal these glass plates with a sealant using bismuth-based glass. This is thought to be because the coefficient of thermal expansion of a sealant using bismuth-based glass does not easily match that of a glass plate with a lower coefficient of thermal expansion than soda-lime glass. As a result, undue stress tends to remain in the resulting sealant layer, and the desired sealing strength cannot be obtained in the sealant layer.
[0032] In contrast, the low-pressure double-glazed glass 1 of this embodiment uses a first glass plate 2 and a second glass plate 3 with low coefficients of thermal expansion, and the first glass plate 2 and the second glass plate 3 are joined via a sealing layer 4 containing crystallized glass. In particular, in the first invention, the crystallized glass contained in the sealing layer 4 contains a β-quartz solid solution as the main crystal, so the coefficient of thermal expansion of the sealing layer 4 is lowered. As a result, the coefficient of thermal expansion of the sealing layer 4 can be brought closer to the coefficients of thermal expansion of the first glass plate 2 and the second glass plate 3, so that undue stress does not easily remain in the sealing layer 4, and the desired sealing strength can be obtained in the sealing layer 4. Accordingly, in the low-pressure double-glazed glass 1 of the first invention, the space between the first glass plate 2 and the second glass plate 3, which have low coefficients of thermal expansion, can be well sealed by the sealing layer 4. Furthermore, in the second invention as well, a similar effect can be obtained because the coefficient of thermal expansion of the crystallized glass contained in the sealing layer 4 is lowered.
[0033] Furthermore, conventional methods for manufacturing low-pressure double-glazed glass, which involve sealing two soda-lime glass plates with a sealant and then evacuating the interior using an exhaust pipe or outlet, have been problematic because the manufacturing process is complicated, making it difficult to increase the productivity of low-pressure double-glazed glass. In contrast, if a sealant is placed between two glass plates and the sealant is heat-treated in a vacuum, the joining of the first and second glass plates and the vacuum evacuation of the resulting internal space can be performed simultaneously, thus increasing the productivity of low-pressure double-glazed glass. However, when heat-treating in a vacuum using a sealant containing amorphous glass such as bismuth-based glass, it is difficult to properly seal the gap between the glass plates. This is thought to be because when heat-treating under vacuum conditions using a sealant containing amorphous glass such as bismuth-based glass, a large amount of dissolved gas is released when the amorphous glass melts, resulting in the formation of many voids in the resulting sealant layer, and consequently, the desired sealing strength cannot be obtained in the sealant layer.
[0034] In contrast, in the low-pressure double-glazed glass 1 of this embodiment, the sealing layer 4 contains crystallized glass, and when forming the sealing layer 4, the crystalline glass contained in the sealing material is crystallized, as will be explained in the section on the manufacturing method described later. Therefore, even when the sealing material is heat-treated in a vacuum, the crystalline glass can be quickly crystallized after the sealing material is melted, so voids caused by the release of dissolved gases, etc., are less likely to occur in the resulting sealing layer 4. Accordingly, the space between the first glass plate 2 and the second glass plate 3, which have low coefficients of thermal expansion, can be well sealed by the sealing layer 4.
[0035] Thus, when manufacturing the low-pressure double-glazed glass 1 of this embodiment, the heat treatment of the sealing material can be performed in a vacuum, and the joining of the first glass plate 2 and the second glass plate 3 by heat treatment and the vacuum evacuation of the internal space 5 formed thereby can be performed simultaneously. Therefore, the step of vacuum evacuating the internal space 5 via an exhaust port or exhaust pipe after joining the first glass plate 2 and the second glass plate 3 can be omitted, and the manufacturing process is less likely to become complicated. Thus, the productivity of the low-pressure double-glazed glass 1 of this embodiment can be increased.
[0036] Thus, the low-pressure double-glazed glass 1 of this embodiment can be made of a material with a low coefficient of thermal expansion, and productivity can be increased.
[0037] In this embodiment, the content of the β-quartz solid solution contained in the sealing layer 4 is preferably 75% by mass or more, more preferably 80% by mass or more, even more preferably 85% by mass or more, preferably 99% by mass or less, more preferably 97% by mass or less, and even more preferably 95% by mass or less. When the content of the β-quartz solid solution contained in the sealing layer 4 is above the lower limit, the thermal expansion coefficient of the sealing layer 4 can be further reduced. Also, when the content of the β-quartz solid solution contained in the sealing layer 4 is below the upper limit, the adhesion between the first glass plate 2 and the second glass plate 3 and the sealing layer 4 can be further improved.
[0038] In this embodiment, the internal space 5 of the low-pressure double-glazed glass 1 is a vacuum. The pressure inside the internal space 5 is preferably 10 -7 Pa or higher, more preferably 10 -6 Pa or higher, more preferably 10 -5 Pa or higher, preferably 10 2 Pa or less, more preferably 10 0 Pa or less, more preferably 10 -1 It is less than or equal to Pa.
[0039] In this embodiment, a spacer 6 is provided within the internal space 5 of the low-pressure double-glazed glass 1. The spacer 6 is provided to maintain a constant thickness of the internal space 5. In this embodiment, the thickness of the internal space 5 corresponds to the distance between the first main surface 2a of the first glass plate 2 and the first main surface 3a of the second glass plate 3.
[0040] In this embodiment, the spacers 6 are circular, elliptical, square, or rectangular in shape when viewed from above, and a plurality of them are provided at predetermined intervals to withstand atmospheric pressure. However, the spacers 6 may be arranged in a dot pattern, line pattern, or random pattern when viewed from above. Furthermore, it is preferable that the spacers 6 are provided in the internal space 5 inside the sealing layer 4 between the first glass plate 2 and the second glass plate 3. Alternatively, the spacers 6 may be provided outside the sealing layer 4 between the first glass plate 2 and the second glass plate 3. The shape of the spacers 6 and the position in which the spacers 6 are provided are not particularly limited, as long as the thickness of the internal space 5 can be kept constant. Note that the spacers 6 may not be provided at all. In particular, in the low-pressure double-glazed glass 1, since the sealing layer 4 contains crystallized glass, the thickness of the internal space 5 can be stably maintained compared to the case where the sealing layer 4 contains amorphous glass. Therefore, in the low-pressure double-glazed glass 1, the number of spacers 6 can be reduced, and in particular, the thickness of the internal space 5 can be stably maintained even without providing spacers 6 outside the sealing layer 4 between the first glass plate 2 and the second glass plate 3.
[0041] In this embodiment, the low-pressure double-glazed glass 1 is not provided with an exhaust port or exhaust pipe for exhausting air from the internal space 5. As described above, when manufacturing the low-pressure double-glazed glass 1 of this embodiment, the step of vacuuming the internal space 5 through an exhaust port or exhaust pipe after joining the first glass plate 2 and the second glass plate 3 can be omitted, so the low-pressure double-glazed glass 1 does not need to be provided with an exhaust port or exhaust pipe. However, the low-pressure double-glazed glass 1 may have an exhaust port or exhaust pipe for exhausting air from the internal space 5.
[0042] Low-pressure double-glazed glass 1 can be used in the construction sector, such as residential buildings; the transportation sector, such as automobiles, ships, and aircraft; and in equipment such as refrigerators, freezers, and constant temperature and humidity chambers. In particular, low-pressure double-glazed glass 1 can be suitably used in the aforementioned applications in environments with a large temperature difference from the outside air temperature.
[0043] The details of each layer constituting the low-pressure double-glazed glass 1 are described below.
[0044] (First glass plate and second glass plate) The first glass plate 2 and the second glass plate 3 each have a coefficient of thermal expansion of -30 × 10⁻¹⁰ from 30°C to 380°C. -7 / K ~ +30 × 10 -7 / K. Preferably, the first glass plate 2 and the second glass plate 3 are made of the same glass plate. However, the first glass plate 2 and the second glass plate 3 may be made of different glass plates. Also, in a plan view, it is desirable that the first glass plate 2 and the second glass plate 3 are the same size, but they may be different sizes. Hereinafter, the first glass plate 2 and the second glass plate 3 may be collectively referred to simply as glass plates.
[0045] The thermal expansion coefficient of the glass plate is -30 × 10⁻¹⁰ from 30°C to 380°C. -7 / K or higher, preferably -25 x 10 -7 / K or higher, more preferably -20 x 10 -7 / K or higher, more preferably -15 × 10 -7 / K or greater, +30 × 10 -7 / K or less, preferably +25 × 10 -7 / K or less, more preferably +20 × 10 -7 / K or less, more preferably +15 × 10 -7 It is less than or equal to / K.
[0046] The glass plate is preferably crystallized glass. In this case, the crystal phase transition temperature of the crystals in the crystallized glass is preferably 900°C or higher, more preferably 950°C or higher, even more preferably 1000°C or higher, preferably 1500°C or lower, more preferably 1400°C or lower, and even more preferably 1200°C or lower. When the crystal phase transition temperature of the crystals in the crystallized glass is within the above range, the productivity of the low-pressure double-layered glass 1 can be further increased.
[0047] The crystal melting temperature of the crystals in the crystallized glass is preferably 1200°C or higher, more preferably 1250°C or higher, even more preferably 1300°C or higher, preferably 1800°C or lower, more preferably 1650°C or lower, and even more preferably 1500°C or lower. When the crystal melting temperature of the crystals in the crystallized glass is within the above range, the productivity of the low-pressure double-glazed glass 1 can be further increased.
[0048] If the glass plate is crystallized glass, the glass plate can be, for example, Li 2 O-Al 2 O 3 -SiO 2 Glass, or MgO-Al 2 O 3 -SiO 2 Glass can be used, preferably Li 2 O-Al 2 O 3 -SiO 2 Glass can be used. For example, crystallized glass can contain SiO in mol%. 2 50%~80%, Al 2 O 3 10% to 30%, Li 2 Crystallized glass containing 5% to 20% of O can be used.
[0049] The glass plate may be amorphous glass. In this case, the softening point of the amorphous glass is preferably 900°C or higher, more preferably 920°C or higher, even more preferably 950°C or higher, preferably 1500°C or lower, more preferably 1450°C or lower, and even more preferably 1400°C or lower. When the softening point of the amorphous glass is within the above range, the productivity of the low-pressure double-glazed glass 1 can be further increased.
[0050] If the glass plate is amorphous glass, the glass plate may be, for example, quartz glass, alkali-free glass, or SiO 2 - Al 2 O 3 Glass can be used, preferably SiO 2 - Al 2 O 3 Amorphous glass can be used. For example, an amorphous glass can contain SiO in mol%.2 75%~80%, Al 2 O 3 Amorphous glass containing 5% to 15% of ZnO and 5% to 10% of ZnO can be used.
[0051] In this embodiment, the glass plate has a substantially rectangular shape. However, the glass plate may also have a substantially circular shape, and the shape of the glass plate is not particularly limited. The thickness of the glass plate can be, for example, 0.5 mm or more and 10 mm or less. The area of the glass plate in plan view is, for example, 0.1 m². 2 More than 10m 2 The following is possible:
[0052] In this embodiment, the glass plate transmits, for example, at least a portion of the visible wavelength range. Specifically, the light transmittance of the glass plate at a thickness of 3 mm in the wavelength range of 400 nm to 650 nm is preferably 60% or more, more preferably 70% or more, even more preferably 75% or more, and particularly preferably 80% or more. The upper limit of the light transmittance of the glass plate at a thickness of 3 mm in the wavelength range of 400 nm to 650 nm can be, for example, 95%.
[0053] (Sealing layer) The sealing layer contains crystallized glass. Preferably, the crystallized glass contains a β-quartz solid solution as the main crystal. When a β-quartz solid solution is contained as the main crystal in crystallized glass, the grain size tends to be small, so the crystallized glass transmits visible light easily, and the transparency of the crystallized glass can be increased. In addition, when a β-quartz solid solution is contained as the main crystal in crystallized glass, the coefficient of thermal expansion of the crystallized glass can be further reduced.
[0054] Crystallized glass; Crystallized glass has a coefficient of thermal expansion of -30 × 10⁻¹⁰ between 30°C and 380°C. -7 / K or higher, preferably -28 x 10 -7 / K or higher, more preferably -26 × 10 -7 / K or higher, more preferably -25 x 10 -7 / K or greater, +30 × 10 -7 / K or less, preferably +28 × 10 -7 / K or less, more preferably +26 × 10-7 / K or less, more preferably +25 × 10 -7 It is less than or equal to / K.
[0055] Examples of such crystallized glasses include, in mol%, SiO 2 48%~75%, Al 2 O 3 5% to 25%, Li 2 Examples include crystallized glass containing 5% to 30% O and 3% to 10% ZnO.
[0056] SiO 2 SiO is a component that forms the glass skeleton of crystallized glass, and is also a component of β-quartz solid solution. 2 The content is preferably 48% to 75%, more preferably 53% to 70%, and even more preferably 53% to 65% in mole percent. 2 If the content of is above the lower limit mentioned above, the content of β-quartz solid solution can be increased, and the thermal expansion coefficient of the crystallized glass can be further reduced. Also, SiO 2 If the content of is below the above upper limit, it is possible to suppress the softening point of the crystallized glass from becoming too high, and to further improve the softening fluidity of the crystallized glass.
[0057] Al 2 O 3 Al is a component of β-quartz solid solution. 2 O 3 The content is preferably 5% to 25%, more preferably 7% to 15%, and even more preferably 7% to 13% in mole percent. 2 O 3 If the content of is above the lower limit mentioned above, the content of β-quartz solid solution can be increased, and the thermal expansion coefficient of the crystallized glass can be further reduced. Also, Al 2 O 3 If the content is below the above upper limit, it is possible to suppress the softening point from becoming too high, and to further improve the softening fluidity of the crystallized glass.
[0058] Li 2O is a constituent component of the β-quartz solid solution, and is also a component that lowers the softening point of crystallized glass. Li 2 The content of O, in mol%, is preferably 5% to 30%, more preferably 10% to 25%, and even more preferably 10% to 20%. Li 2 When the content of O is equal to or more than the above lower limit value, the content of the β-quartz solid solution can be further increased, and the thermal expansion coefficient of the crystallized glass can be further reduced. In addition, it is possible to prevent the softening point of the crystallized glass from becoming too high, and to further improve the softening fluidity of the crystallized glass. Moreover, Li 2 Even when the content of O is equal to or less than the above upper limit value, the thermal expansion coefficient of the crystallized glass can be further reduced.
[0059] ZnO is a component that improves the weather resistance of crystallized glass. In addition, ZnO has the effect of improving the softening fluidity of crystallized glass. The content of ZnO, in mol%, is preferably 0% to 15%, more preferably 0% to 10%, and even more preferably 3% to 10%. When the content of ZnO is within the above range, the thermal expansion coefficient of the crystallized glass can be further reduced.
[0060] The crystallized glass may contain B 2 O 3 It may contain. B 2 O 3 is a component that forms the glass skeleton of crystallized glass, and is a component that lowers the softening point of crystallized glass. B 2 O 3 The content of, in mol%, is preferably 0% to 23%, more preferably 10% to 16%, and even more preferably 10% to 15%. B 2 O 3 When the content of is equal to or more than the above lower limit value, it is possible to prevent the softening point of the crystallized glass from becoming too high, and to further improve the softening fluidity of the crystallized glass. B 2 O 3 When the content of is equal to or less than the above upper limit value, it is possible to suppress an increase in the proportion of the residual glass phase (a decrease in the precipitation amount of the β-quartz solid solution), whereby the thermal expansion coefficient of the crystallized glass can be further reduced.
[0061] Note that the crystallized glass may contain MgO, CaO, SrO, or BaO as a component for improving weather resistance. These components also have the effect of improving the fluidity of the crystallized glass. The content of MgO+CaO+SrO+BaO, in terms of mol%, is preferably 0% to 10%, more preferably 0% to 5%, and even more preferably 0.1% to 2%. When the content of MgO+CaO+SrO+BaO is equal to or less than the above upper limit value, it is possible to suppress an increase in the proportion of the residual glass phase (a decrease in the precipitation amount of β-quartz solid solution), which makes it possible to further lower the thermal expansion coefficient of the crystallized glass.
[0062] Further, the crystallized glass may contain La as a component for improving weather resistance. 2 O 3 , ZrO 2 , or Bi 2 O 3 . Among these, ZrO 2 and Bi 2 O 3 also have the effect of improving the fluidity of the crystallized glass. The content of La 2 O 3 +ZrO 2 +Bi 2 O 3 , in terms of mol%, is preferably 0% to 10%, more preferably 0% to 5%, and even more preferably 0.1% to 2%. When the content of La 2 O 3 +ZrO 2 +Bi 2 O 3 is equal to or less than the above upper limit value, it is possible to suppress an increase in the proportion of the residual glass phase (a decrease in the precipitation amount of β-quartz solid solution), which makes it possible to further lower the thermal expansion coefficient of the crystallized glass.
[0063] Further, in addition to the above components, the crystallized glass may contain Na within a range that does not impair the effects of the present invention. 2 O, K 2 O, MnO, P 2 O 5 , MoO 2 , TiO 2 , or V 2 O 5It may also contain the following. The total amount of these components is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less in mole percent.
[0064] The softening point of the powder before crystallization of crystallized glass (crystalline glass powder) is preferably 500°C or higher, more preferably 550°C or higher, even more preferably 600°C or higher, preferably 1000°C or lower, more preferably 950°C or lower, and even more preferably 900°C or lower. When the softening point of the crystalline glass powder is above the lower limit, sufficient softening fluidity can be more reliably ensured. Furthermore, when the softening point of the crystalline glass powder is below the upper limit, the glass plate can be sealed more stably in a temperature range that does not cause thermal deformation.
[0065] The crystallization temperature of the powder before crystallization of crystallized glass (crystalline glass powder) is preferably 600°C or higher, more preferably 650°C or higher, even more preferably 700°C or higher, preferably 1100°C or lower, more preferably 1050°C or even more preferably 1000°C or lower. When the crystallization temperature of the crystalline glass powder is above the lower limit, crystallization can be performed even more effectively by crystallizing after sufficient softening and flow. Furthermore, when the crystallization temperature of the crystalline glass powder is below the upper limit, crystal precipitation can be performed more stably in a temperature range that does not cause thermal deformation of the glass plate, and the desired coefficient of thermal expansion can be obtained more reliably.
[0066] The crystal phase transition temperature of the crystals in the crystallized glass is preferably 900°C or higher, more preferably 920°C or higher, even more preferably 950°C or higher, preferably 1500°C or lower, more preferably 1400°C or lower, and even more preferably 1200°C or lower. When the crystal phase transition temperature of the crystals in the crystallized glass is above the lower limit, the internal space 5 of the low-pressure double-glazed glass 1 can be sealed even more stably. Furthermore, when the crystal phase transition temperature of the crystals in the crystallized glass is below the upper limit, the softening and fluidity of the crystallized glass can be further improved.
[0067] The crystal melting temperature of the crystals in the crystallized glass is preferably 1200°C or higher, more preferably 1250°C or higher, even more preferably 1300°C or higher, preferably 1800°C or lower, more preferably 1650°C or lower, and even more preferably 1500°C or lower. When the crystal melting temperature of the crystals in the crystallized glass is within the above range, the productivity of the low-pressure double-glazed glass 1 can be further increased.
[0068] The content of crystallized glass in the sealing layer 4 is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more. When the content of crystallized glass in the sealing layer 4 is equal to or greater than the lower limit of the above value, the space between the first glass plate 2 and the second glass plate 3, which have low coefficients of thermal expansion, can be sealed even more reliably by the sealing layer 4. The sealing layer 4 may be composed solely of crystallized glass.
[0069] Fire-resistant filler; The sealing layer 4 may contain a fire-resistant filler. The fire-resistant filler is a component that adjusts the thermal expansion coefficient of the sealing layer 4.
[0070] Examples of fire-resistant fillers include cordierite, willemite, alumina, zirconium phosphate, zircon, zirconia, tin oxide, mullite, silica, β-eucryptite, β-spodumene, or zirconium tungstate phosphate.
[0071] The amount of fire-resistant filler contained in the sealing layer 4 is preferably 1% by mass or more, more preferably 3% by mass or more, preferably 30% by mass or less, and more preferably 20% by mass or less. When the amount of fire-resistant filler contained in the sealing layer 4 is above the lower limit, the thermal expansion coefficient of the sealing layer 4 can be brought closer to the desired value. Furthermore, when the amount of fire-resistant filler contained in the sealing layer 4 is below the upper limit, the adhesion between the first glass plate 2 and the second glass plate 3 and the sealing layer 4 can be further improved.
[0072] Other additives; The sealing layer 4 may contain other additives in addition to the above components, as long as they do not impair the effects of the present invention. Examples of other additives include Fe-Mn-O based inorganic pigments. The content of other additives in the sealing layer 4 can be, for example, 5% by mass or less.
[0073] The thickness of the sealing layer 4 can be appropriately set according to the thickness of the internal space 5, within a range that does not reduce the sealing strength of the low-pressure double-glazed glass 1. The thickness of the sealing layer 4 is preferably 20 μm or more, more preferably 50 μm or more, preferably 2000 μm or less, and more preferably 1000 μm or less. The width of the sealing layer 4 is, for example, 0.1 mm or more and 10 mm or less.
[0074] (Spacer) For example, glass, metal, resin, or ceramics can be used as the spacer 6. The spacer 6 may be made of the same crystallized glass as the sealing layer 4.
[0075] The thickness of the spacer 6 can be appropriately set according to the thickness of the internal space 5, within a range that does not obstruct the visibility of the low-pressure double-glazed glass 1. The thickness of the spacer 6 is preferably 20 μm or more, more preferably 50 μm or more, preferably 2000 μm or less, and more preferably 1000 μm or less. The width of the spacer 6 is, for example, 50 μm or more and 2000 μm or less. The spacing between the spacers 6 can be, for example, 1 mm or more and 100 mm or less.
[0076] The manufacturing method for low-pressure double-glazed glass 1 will be described below.
[0077] [Method for Manufacturing Low-Pressure Double-Glazed Glass] In the method for manufacturing low-pressure double-glazed glass 1, first, a first glass plate 2, a second glass plate 3, and a sealing material containing crystalline glass are prepared. The glass plates described above can be used as the first glass plate 2 and the second glass plate 3.
[0078] Next, a sealing material is placed on the first main surface 2a of the first glass plate 2. For example, as shown in Figure 3(a), a sealing layer forming paste 4A is applied to the outer peripheral edge portion 2c of the first main surface 2a of the first glass plate 2 in a frame-like shape.
[0079] The sealing layer forming paste 4A can be formed by mixing glass powder with Vehicle. Alternatively, the sealing layer forming paste 4A may be formed by mixing glass powder and refractory filler powder to form a composite powder, and then mixing it with Vehicle. As the glass powder, crystalline glass prepared to have the composition of the crystallized glass constituting the sealing layer 4 can be used. As the refractory filler, the filler described in the sealing layer section above can be used.
[0080] Average particle size D of glass powder 50 The average particle size D of the glass powder is preferably 20 μm or less, more preferably 0.5 μm to 15 μm, and even more preferably 1 μm to 15 μm. 50 If the average particle size D is within the above range, the density of the crystallized glass can be further increased, and the sealing performance of the sealing layer 4 can be further improved. 50 "This refers to a volume-based cumulative particle size distribution curve measured by laser diffraction, where the cumulative amount, starting from the smallest particles, reaches 50%.
[0081] The vehicle contains a solvent and a resin. The solvent is added to dissolve the resin and uniformly disperse glass powder, etc. The resin is added to adjust the viscosity of the sealing layer paste 4A. Surfactants, thickeners, etc. may also be added to the vehicle as needed.
[0082] Examples of resins that can be used include acrylic resins such as acrylic acid esters, ethyl cellulose, polyethylene glycol derivatives, nitrocellulose, polymethylstyrene, polyethylene carbonate, or methacrylic acid esters. Furthermore, from the viewpoint of good thermal decomposition properties, the resin is preferably acrylic acid ester or ethyl cellulose.
[0083] As solvents, for example, pine oil, N,N'-dimethylformamide (DMF), α-terpineol, higher alcohols, γ-butyllactone (γ-BL), tetralin, butylcarbitol acetate, ethyl acetate, isoamyl acetate, diethylene glycol monoethyl ether, diethylene glycol monoethyl ether acetate, benzyl alcohol, toluene, 3-methoxy-3-methylbutanol, triethylene glycol monomethyl ether, triethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monobutyl ether, propylene carbonate, or N-methyl-2-pyrrolidone can be used. In particular, α-terpineol is preferred as the solvent from the viewpoint of high viscosity and good solubility of resins, etc.
[0084] The sealing layer forming paste 4A can be prepared, for example, by mixing glass powder or composite powder with Vehicle and then uniformly kneading it in, for example, a three-roll mill. The sealing layer forming paste 4A can also be applied to the first main surface 2a of the first glass plate 2 using, for example, a dispensing machine such as a dispenser or a screen printing machine.
[0085] Next, the sealing layer forming paste 4A applied to the first main surface 2a of the first glass plate 2 is pre-fired. The pre-fired temperature can be, for example, 300°C or higher and 600°C or lower. The pre-fired time can be, for example, 5 minutes or higher and 60 minutes or lower. Before pre-fired, the sealing layer forming paste 4A may be dried in advance to dry the solvent contained in the sealing layer forming paste 4A.
[0086] Next, as shown in Figure 3(b), a spacer 6 is placed on the first main surface 3a of the second glass plate 3. As the spacer 6, a material obtained by applying paste to the first main surface 3a of the second glass plate 3 and pre-firing it may be used. Alternatively, the spacer 6 may be placed on the first main surface 2a of the first glass plate 2.
[0087] Next, the second glass plate 3 is placed on the first main surface 2a of the first glass plate 2, and the first glass plate 2 and the second glass plate 3 are superimposed. At this time, the first glass plate 2 is superimposed from the side with the first main surface 2a to which the sealing layer forming paste 4A is applied. The second glass plate 3 is superimposed from the side with the first main surface 3a to which the spacer 6 is placed.
[0088] Next, the laminate, in which the second glass plate 3 is placed on the first main surface 2a of the first glass plate 2, is heat-treated in a vacuum. This forms a sealing layer 4 between the first glass plate 2 and the second glass plate 3, thereby joining the first glass plate 2 and the second glass plate 3. The heat treatment in a vacuum can be performed, for example, by placing the laminate, in which the second glass plate 3 is placed on the first main surface 2a of the first glass plate 2, in a vacuum firing furnace and raising the temperature to the desired heat treatment temperature while evacuating the vacuum.
[0089] Furthermore, when performing the heat treatment in a vacuum as described above, it is preferable to leave a small gap between the first glass plate 2 and the second glass plate 3, and to overlap the first glass plate 2 and the second glass plate 3 so that the gap is closed when the sealing layer forming paste 4A softens and flows due to the heat treatment. For example, the gap can be formed by overlapping the first glass plate 2 and the second glass plate 3 with a slight offset when placing the second glass plate 3 on the first main surface 2a of the first glass plate 2, or by placing the second glass plate 3 on the first main surface 2a of the first glass plate 2 so that a part of the second glass plate 3 does not come into contact with the sealing layer forming paste 4A.
[0090] In the manufacturing method of the low-pressure double-glazed glass 1, the paste 4A for forming the sealing layer is fired by heat treatment, and a β-quartz solid solution as the main crystal is precipitated in the sealing layer 4. The heat treatment temperature is preferably 600°C or higher, more preferably 650°C or higher, even more preferably 700°C or higher, preferably 1000°C or lower, more preferably 950°C or lower, and even more preferably 900°C or lower. When the heat treatment temperature is above the lower limit, the β-quartz solid solution can be precipitated more easily in the sealing layer 4. When the heat treatment temperature is below the upper limit, the internal space 5 can be sealed more reliably by the sealing layer 4.
[0091] The heat treatment time (maximum temperature holding time) is preferably 10 minutes or more, more preferably 20 minutes or more, preferably 500 minutes or less, and more preferably 250 minutes or less. When the heat treatment time is within the above range, the β-quartz solid solution can be precipitated more easily in the sealing layer 4.
[0092] Furthermore, the heating rate during heat treatment (especially the heating rate near the crystallization start temperature of crystalline glass) is preferably 3°C / min or more, more preferably 5°C / min or more, even more preferably 7°C / min or more, particularly preferably 10°C / min or more, and preferably 30°C / min or less. When the heating rate during heat treatment is within the above range, the thermal expansion coefficient of the sealing layer 4 can be further reduced.
[0093] Furthermore, it is preferable to slowly cool the above-mentioned laminate after heat treatment. In this case, since the crystal growth of the crystalline glass continues even during the cooling process, the β-quartz solid solution can be made to precipitate more easily in the sealing layer 4. The rate of cooling (absolute value) during slow cooling is preferably 5°C or higher, preferably 100°C or lower, and more preferably 50°C or lower.
[0094] Vacuum evacuation is performed when the pressure in the internal space 5 is preferably 10 -6 Pa or higher, more preferably 10 -5 Pa or higher, preferably 10 0 Pa or less, more preferably 10 -1 It is preferable to perform the procedure so that the pressure is below Pa.
[0095] In the manufacturing method of the low-pressure double-glazed glass 1 of this embodiment, a first glass plate 2 and a second glass plate 3 with low coefficients of thermal expansion are used, and a β-quartz solid solution is precipitated as the main crystal in the sealing layer 4, thus lowering the coefficient of thermal expansion of the sealing layer 4. As a result, the coefficient of thermal expansion of the sealing layer 4 can be brought closer to the coefficients of thermal expansion of the first glass plate 2 and the second glass plate 3, making it less likely for undue stress to remain in the sealing layer 4, and allowing the desired sealing strength to be obtained in the sealing layer 4. Therefore, the space between the first glass plate 2 and the second glass plate 3, which have low coefficients of thermal expansion, can be well sealed by the sealing layer 4.
[0096] Furthermore, in the manufacturing method of the low-pressure double-glazed glass 1 of this embodiment, the crystalline glass contained in the sealing material is crystallized when forming the sealing layer 4. Therefore, even when the sealing material is heat-treated in a vacuum, the crystalline glass can be quickly crystallized after the sealing material is melted, making it difficult for voids to form in the resulting sealing layer 4. Consequently, the space between the first glass plate 2 and the second glass plate 3, which have low coefficients of thermal expansion, can be well sealed by the sealing layer 4. Thus, in the manufacturing method of the low-pressure double-glazed glass 1 of this embodiment, the sealing material can be heat-treated in a vacuum, and the joining of the first glass plate 2 and the second glass plate 3 by heat treatment and the vacuum evacuation of the internal space 5 formed thereby can be performed simultaneously. Therefore, in the manufacturing method of the low-pressure double-glazed glass 1 of this embodiment, the step of vacuum evacuating the internal space 5 via an exhaust port or exhaust pipe after joining the first glass plate 2 and the second glass plate 3 can be omitted, making the manufacturing process less complicated. Thus, the manufacturing method of the low-pressure double-glazed glass 1 of this embodiment can increase the productivity of the low-pressure double-glazed glass 1.
[0097] The present invention will be described in more detail below based on specific examples. The present invention is not limited in any way to the following examples, and can be implemented with appropriate modifications without changing its essence.
[0098] (Example 1) SiO in mol% 2 57.5%, Li 2 O 15%, B 2 O 3 12%, Al2 O 3 A raw material batch was prepared by mixing raw material powders to achieve a glass composition of 9% and 6.5% ZnO, and then uniformly mixing them. The raw material batch was placed in a platinum crucible and melted at 1400°C to 1600°C until homogeneous. The resulting molten glass was poured into a pair of molding rolls and molded while rapidly cooling to obtain a film-like glass. The film-like glass was dry-milled for 10 hours using a ball mill, and then classified using a metal sieve with a mesh size of 100 μm to determine the average particle size D 50 This yielded glass powder with a particle size of 10 μm.
[0099] The softening point and crystallization temperature of the obtained glass powder were measured using a macro-type DTA (differential thermal analysis) apparatus in an atmospheric environment at a heating rate of 10°C / min. The softening point was determined by the temperature of the fourth inflection point in the obtained chart, and the crystallization temperature was determined by the exothermic peak temperature due to crystal precipitation. The softening point was found to be 646°C, and the crystallization temperature was 746°C. Furthermore, after heat-treating the obtained glass powder at 700°C for 30 minutes, the precipitated crystals were measured by X-ray diffraction. The main crystal was a β-quartz solid solution, and the amount of precipitated β-quartz solid solution calculated from the XRD spectrum was 89% by mass. The density of the obtained glass powder was 2.46 g / m³. 3 Furthermore, using a micro-type DTA (differential thermal analysis) device, the crystal phase transition temperature of the β-quartz solid solution after crystallization was 980°C, and the crystal melting temperature was 1310°C.
[0100] Next, using the obtained glass powder, a low-pressure double-layered glass 1 (excluding the spacer 6) shown in Figures 1 and 2 was fabricated. Specifically, an acrylic resin as a resin and α-terpineol as a solvent were appropriately added to the glass powder to prepare a paste for forming a sealing layer. In addition, glass plates (manufactured by Nippon Electric Glass Co., Ltd., trade name "Firelight", thermal expansion coefficient: -1 × 10⁻⁶) were used as the first glass plate 2 and the second glass plate 3. -7A glass plate with a temperature of 30°C to 380°C, dimensions of 100 mm x 100 mm x 5 mm, crystal phase transition temperature of crystals in crystallized glass: 990°C, crystal melting temperature: 1350°C was prepared. Next, a sealing layer forming paste was applied to the outer peripheral edge portion 2c of the first main surface 2a of the first glass plate 2 using a dispenser to form a frame shape with a width of 1 mm and a thickness of 0.3 mm, and dried at 120°C for 15 minutes. At this time, the application conditions using the dispenser were a gap of 300 μm and a discharge pressure of 0.7 kg / cm². 2 The nozzle diameter was set to 0.33 inches and the discharge speed to 50 mm / s. After drying, the paste for forming the sealing layer was pre-fired at 350°C for 15 minutes. Next, the second glass plate 3 was placed on the first main surface 2a of the first glass plate 2 and placed in a vacuum firing furnace. Next, while evacuating the vacuum firing furnace, the laminate of the second glass plate 3 placed on the first main surface 2a of the first glass plate 2 was heat-treated at 700°C for 30 minutes to form a sealing layer 4 between the first glass plate 2 and the second glass plate 3, thereby obtaining a low-pressure double-layered glass 1. The thermal expansion coefficient of the obtained sealing layer 4 at 30°C to 380°C was measured using a thermal expansion measuring instrument (manufactured by Netzsch) and was found to be 2.1 × 10⁻⁶. -7 The temperature was / K. Furthermore, the thermal insulation performance of the obtained low-pressure double-glazed glass 1 was evaluated using a radiation thermometer. In the evaluation of thermal insulation performance, the fabricated low-pressure double-glazed glass 1 was placed on a hot plate heated to 200°C, and the change in surface temperature of the side not in direct contact with the hot plate was measured with a radiation thermometer. For comparison, double-glazed glass sealed at atmospheric pressure was used. As a result, the temperature rise of the surface of the fabricated low-pressure double-glazed glass 1 was significantly suppressed compared to double-glazed glass sealed at atmospheric pressure, and it was confirmed that the internal space was well sealed.
[0101] (Comparative Example 1) Bismuth-based glass as glass powder (composition: Bi in mol%) 2 O 3 40%, B 2 O 3Low-pressure double-glazed glass was fabricated in the same manner as in Example 1, except that 30% of ZnO (30%) and BaO (10%) were used. However, in Comparative Example 1, which used bismuth-based glass as the sealant, the sealing strength of the sealing layer was insufficient, and the internal space could not be sealed.
[0102] 1...Low-pressure double-glazed glass 2...First glass plate 2a, 3a...First main surface 2b, 3b...Second main surface 2c, 3c...Peripheral edge portion 3...Second glass plate 4...Sealing layer 4A...Paste for forming sealing layer 5...Internal space 6...Spacer
Claims
1. Low-pressure double-glazed glass, which is constructed by joining glass plates together via a sealing layer, and has an internal space that is under lower pressure than the outside, and has a thermal expansion coefficient of -30 × 10⁻¹⁰ from 30°C to 380°C. -7 / K ~ +30 × 10 -7 Low-pressure double-layered glass comprising: a first glass plate and a second glass plate, which are both / K; and a sealing layer provided between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are joined via the sealing layer, forming an internal space surrounded by the first glass plate, the second glass plate, and the sealing layer, the internal space is under lower pressure than the outside, the sealing layer contains crystallized glass, and the crystallized glass contains a β-quartz solid solution as the main crystal.
2. Low-pressure double-glazed glass, which is constructed by joining glass plates together via a sealing layer and has an internal space that is under lower pressure than the outside, and has a thermal expansion coefficient of -30 × 10⁻¹⁰ from 30°C to 380°C. -7 / K ~ +30 × 10 -7 The device comprises a first glass plate and a second glass plate, both having a coefficient of thermal expansion of -30 × 10¹⁰°C, and a sealing layer provided between the first glass plate and the second glass plate, wherein the first glass plate and the second glass plate are joined via the sealing layer, forming an internal space surrounded by the first glass plate, the second glass plate, and the sealing layer, the internal space is under lower pressure than the outside, the sealing layer contains crystallized glass, and the crystallized glass has a coefficient of thermal expansion of -30 × 10¹⁰°C from 30°C to 380°C. -7 / K ~ +30 × 10 -7 Low-pressure double-glazed glass with a K rating.
3. The crystallized glass constituting the sealing layer contains, in mol%, SiO 2 48% to 75%, Al 2 O 3 5% to 25%, Li 2 O 5% to 30%, and ZnO 3% to 10%, the low-pressure multi-layer glass according to claim 1 or 2.
4. The low-pressure double-glazed glass according to claim 1 or 2, wherein the first glass plate and the second glass plate are composed of crystallized glass, the crystal phase transition temperature of the crystals in the crystallized glass is 900°C or higher, and the crystal melting temperature is 1200°C or higher.
5. The low-pressure double-glazed glass according to claim 1 or 2, wherein the first glass plate and the second glass plate are made of amorphous glass, and the softening point of the amorphous glass is 900°C or higher.
6. The low-pressure double-glazed glass according to claim 1 or 2, wherein the low-pressure double-glazed glass is not provided with an exhaust port for exhausting the internal space.
7. A method for manufacturing low-pressure double-glazed glass, wherein glass plates are joined together via a sealing layer, and an internal space with lower pressure than the outside is provided, comprising the steps of: placing a sealing material containing crystalline glass on the main surface of a first glass plate; and placing a second glass plate on the main surface of the first glass plate on which the sealing material is placed, and heat-treating it in a vacuum, wherein the heat treatment causes a β-quartz solid solution as the main crystal to precipitate in the sealing material.