Ferritic stainless steel and method for producing same
By controlling the composition and performing nitriding treatment to form Ti nitrides and removing surface oxides, ferritic stainless steel achieves enhanced brazing properties with Ni-containing materials, addressing the poor wettability issue and reducing costs.
Patent Information
- Application Number
- PCT/JP2026/016851
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-19
AI Technical Summary
Ferritic stainless steel with high Ti content exhibits poor wettability with Ni-containing brazing materials due to the formation of Ti oxides during brazing, leading to increased brazing defects and costs, especially in high-temperature applications like EGR coolers in automobiles.
Control the composition and perform nitriding treatment on the surface of ferritic stainless steel to generate Ti nitrides, reducing Ti solid solution and suppressing the formation of Ti oxides, followed by pickling to remove any formed oxides, ensuring good brazing properties with Ni-containing brazing materials.
The method achieves improved brazing performance without the need for expensive elements like Nb and Zr, reducing manufacturing costs and enhancing the efficiency of the process.
Smart Images

Figure JP2026016851_19112026_PF_FP_ABST
Abstract
Description
Ferritic stainless steel and method for manufacturing the same
[0001] The present invention relates to ferritic stainless steel and a method for producing the same, and more particularly to ferritic stainless steel that exhibits good brazing properties when brazing at high temperatures using a Ni-containing brazing material, and a method for producing the same.
[0002] In recent years, the problem of global warming caused by environmental pollution has become a major concern, and there is a growing demand for improved fuel efficiency and enhanced exhaust gas purification in automobiles. For this reason, the application of EGR (Exhaust Gas Recirculation) coolers in automobiles is increasing.
[0003] An EGR cooler is a heat exchanger that cools exhaust gas to an appropriate temperature in order to return a portion of the high-temperature exhaust gas discharged from the engine back to the engine. It consists of pipes, plates, fins, side plates, etc. The exhaust gas enters the heat exchanger section from the inlet pipe, where its heat is transferred to the cooling water via heat transfer surfaces such as fins, and then discharged from the outlet pipe. Furthermore, the heat exchanger section of the EGR cooler has a structure in which thin plates are stacked in a fin-like shape, from the viewpoint of weight reduction, compactness, and cost reduction, and brazing using nickel-containing brazing material is used for joining and assembling these parts.
[0004] Therefore, materials used in heat exchangers require excellent brazing properties with Ni-containing brazing materials. Furthermore, because high-temperature exhaust gases pass through, these materials also need oxidation resistance in high-temperature environments. In addition, exhaust gases contain nitrogen oxides (NOx), sulfide oxides (SOx), and hydrocarbons (HC), which condense within the heat exchanger, generating highly corrosive, acidic condensate. Therefore, materials used in heat exchangers also require corrosion resistance at room temperature. In particular, during brazing heat treatment, the materials are exposed to high temperatures, making it crucial to prevent sensitization—where Cr at grain boundaries preferentially reacts with C and N to form a Cr-deficient layer—and thus ensure corrosion resistance.
[0005] For the reasons stated above, these heat exchanger components are exposed to a harsh corrosive environment due to condensed water and other factors, so austenitic stainless steel such as SUS304L (18Cr-8Ni), which has a reduced carbon content and is less prone to sensitization, has been used.
[0006] However, austenitic stainless steel is expensive due to its high nickel content, and it also has problems with its fatigue properties and high-temperature thermal fatigue properties in environments that are subjected to high temperatures, intense vibrations, and restraining forces, such as the parts around an exhaust manifold.
[0007] In recent years, there has been a demand for higher temperatures of inflow gases, and ferritic stainless steel, which is less susceptible to deterioration in thermal fatigue properties, is being used as a material for heat exchangers. In particular, the use of Nb and Zr-containing ferritic stainless steel, which has excellent resistance to condensate corrosion, is being considered because the addition of Nb and Zr stabilizes the C and N in the ferritic stainless steel as carbonitrides, preventing sensitization.
[0008] Furthermore, Ti-containing ferritic stainless steel, like Nb and Zr-containing ferritic stainless steel, can prevent sensitization, has lower raw material and manufacturing costs, and does not raise the recrystallization temperature compared to cases with Nb and Zr addition. For this reason, the use of Ti-containing ferritic stainless steel instead of Nb and Zr is being considered.
[0009] However, Ti-containing ferritic stainless steel generally has the disadvantage of poor wettability with Ni brazing alloy compared to austenitic stainless steel and Nb-containing ferritic stainless steel. When materials with poor wettability are used, the rate of brazing defects increases. In addition, the amount of Ni brazing alloy used increases in order to obtain a sufficient wetting area. In recent years, the price of Ni ingot has continued to rise, so this represents a significant increase in costs.
[0010] The reason why the wettability of Ni brazing material is poor when using Ti-containing ferritic stainless steel is that Ti oxides are generated on the steel plate surface during the brazing heat treatment, which inhibits the spreading of the Ni brazing material. Therefore, suppressing the generation of Ti oxides during brazing to improve the wettability of Ni brazing material is an extremely important issue.
[0011] Conventional knowledge regarding ferritic stainless steels with excellent brazing properties includes, for example, the following:
[0012] Patent Document 1 describes how to achieve a vacuum level of 1 × 10⁻¹⁰ when raising the temperature to 400°C. -2 The pressure should be less than Pa, and the heat treatment should be performed at a soaking temperature of 900 to 1200°C for a soaking time of no more than 120 minutes, with the vacuum level after reaching the soaking temperature set to 10 -2 ~10 1 A ferritic stainless steel is disclosed in which the formation of the Ti oxide film is appropriately controlled by adjusting the Pa, thereby ensuring brazing properties.
[0013] Patent documents 2 to 4 provide ferritic stainless steel and a method for manufacturing the same, which exhibit good brazing properties when brazing at high temperatures using Ni-containing brazing material, by generating a nitrogen-enriched layer on the surface, as a material for EGR coolers.
[0014] International Publication No. 2016-013482, International Publication No. 2015-141145, International Publication No. 2016-103565, International Publication No. 2016-017123
[0015] Patent Document 1 states that obtaining sufficient brazing performance requires multiple special heat treatments, which presents the challenge of increased costs due to the increased number of processes. Furthermore, it could not be said that sufficient brazing performance of Ni-containing brazing materials could be ensured for ferritic stainless steel with a high Ti content.
[0016] Patent documents 2 to 4 describe techniques for suppressing the formation of a Ti oxide film by forming a nitrogen-enriched layer and ensuring brazing properties. However, similar to patent document 1, these techniques could not be said to adequately ensure brazing properties for ferritic stainless steel with a high Ti content.
[0017] The present invention has been made in view of the above-mentioned circumstances, and aims to provide a ferritic stainless steel containing Ti that exhibits good brazing properties when brazing is performed at high temperatures using a Ni-containing brazing material.
[0018] Furthermore, the present invention aims to provide a method for manufacturing the above-mentioned ferritic stainless steel.
[0019] To achieve the above objective, the inventors manufactured Ti-containing ferritic stainless steel by varying the composition and manufacturing conditions of the steel, and diligently investigated the high-temperature brazing properties of the manufactured steel using Ni-containing brazing material.
[0020] However, with these Ti-containing ferritic stainless steels, even with precise control of the atmosphere during high-temperature brazing using Ni-containing brazing material, it was not possible to satisfactorily suppress the formation of a Ti oxide film that worsens the wettability of the Ni brazing material. As a result, even when brazing was performed in a high-vacuum hydrogen atmosphere or a high-vacuum nitrogen atmosphere, which have a lower oxygen partial pressure than the atmospheric pressure nitrogen atmosphere frequently used when brazing stainless steels and are advantageous for brazing Ti-containing ferritic stainless steels, the desired brazing performance could not always be obtained. When the desired brazing performance cannot be obtained sufficiently, for example, when brazing overlapping steels, the spread of the brazing material into the gaps in the overlapping portions may not be sufficient.
[0021] Therefore, the inventors attempted to generate TiN by nitriding the surface layer of steel, thereby reducing the Ti concentration in the ferrite matrix of the surface layer and suppressing the diffusion of Ti to the surface and the formation of an oxide film during high-temperature brazing. However, in the case of ferritic stainless steel with a high Ti content, this method was sometimes insufficient to suppress the formation of a Ti oxide film. Furthermore, in the case of ferritic stainless steel with a high Cr content, Cr nitrides were sometimes formed on the surface of the steel sheet during finish annealing (heat treatment) under low-temperature conditions, which reduced brazing properties and corrosion resistance.
[0022] Therefore, the inventors conducted further studies to more effectively suppress the formation of an oxide film on Ti during high-temperature brazing using a Ni-containing brazing material.
[0023] As a result, the following findings were obtained. Prior to brazing, a heat treatment (nitriding treatment) is performed under controlled heat treatment conditions and atmosphere to satisfy the predetermined equation (1) to generate Ti nitrides in an appropriate form on the surface layer of the steel. This reduces the amount of Ti solid solution in the ferrite matrix on the surface layer, effectively preventing the formation of a Ti oxide film during high-temperature brazing. Furthermore, the composition of the stainless steel and the heat treatment (nitriding treatment) conditions are limited to suppress the formation of Cr nitrides. This ensures that sufficiently good brazing performance can be obtained even when performing high-temperature brazing using Ni-containing brazing material. In addition, when manufacturing ferritic stainless steel with the Ti nitrided on the surface layer as described above, an efficient manufacturing process can be applied, which is very advantageous in terms of manufacturing efficiency.
[0024] Furthermore, the inventors considered the possibility that, for example, high temperature, long duration, low hydrogen partial pressure, and high dew point heat treatment (nitriding) conditions could cause oxidation of the outermost surface of the steel sheet during nitriding, potentially reducing brazing performance. The inventors found that, in order to ensure sufficient brazing performance, it is effective to perform pickling after nitriding to remove any oxides that may have formed on the surface. By performing pickling after nitriding, the high-temperature brazing performance using Ni-containing brazing material was further improved.
[0025] This invention was completed after further consideration based on the above findings, and its gist is as follows.
[0026] [1] The composition is as follows, by mass%, containing C: 0.003-0.025%, Si: 0.05-1.00%, Mn: 0.05-1.00%, P: 0.05% or less, S: 0.03% or less, Cr: 16.0-25.0%, Ni: 0.01-0.60%, Ti: 0.25-0.75%, Al: 0.005-0.150%, and N: 0.005-0.025%, with the remainder being Fe and unavoidable impurities, the average Ti concentration in the ferrite phase in the region up to a depth of 20 μm from the surface is 0.2 mass% or less, and the density of Ti nitrides with a size of 1 μm or less in the cross-section of the plate thickness in the said region is 0.03 particles / μm 2 The above is true for ferritic stainless steel. [2] The above component composition further contains one or more selected by mass% from Nb: 0.01 to 0.45%, Cu: 0.01 to 0.80%, V: 0.01 to 0.50%, Mo: 0.10 to 3.00%, B: 0.0003 to 0.0030%, Co: 0.01 to 0.40%, Zr: 0.01 to 1.00%, W: 0.01 to 1.00%, Sn: 0.005 to 0.500%, and REM: 0.001 to 0.100%, the ferritic stainless steel according to [1]. [3] A method for producing ferritic stainless steel according to [1] or [2] above, comprising the steps of: hot rolling a slab having the above component composition to obtain a hot-rolled steel sheet; optionally hot-rolled annealing the hot-rolled steel sheet to obtain a hot-rolled annealed steel sheet; and cold rolling and cold-rolled annealing combined once or twice or more times on the hot-rolled steel sheet or hot-rolled annealed steel sheet, wherein in the final cold-rolled annealing, the dew point is -30°C or lower, and the nitrogen partial pressure is 25 × 10⁻⁶. 3 A method for manufacturing ferritic stainless steel, comprising heat treatment in an atmosphere of nitrogen and hydrogen above Pa, satisfying an annealing temperature T: 900 to 1200°C, an annealing time t: 10 to 300 seconds, and the following equation (1) being satisfied: 2T - (200 [Ti] + 50 [Cr] + 2P + 5D - t) ≥ 880 ... (1) Here, in equation (1), T: annealing temperature (°C), [Ti]: Ti content in the steel (mass%), [Cr]: Cr content in the steel (mass%), D: dew point (°C), P: partial pressure of nitrogen (×10 3Pa), t: annealing time (seconds). [4] A method for producing ferritic stainless steel according to [3], wherein pickling is performed after the final cold-rolled sheet annealing.
[0027] According to the present invention, a ferritic stainless steel containing Ti can be obtained that exhibits good brazing properties when brazing is performed at high temperatures using a Ni-containing brazing material.
[0028] According to the present invention, a ferritic stainless steel exhibiting good brazing properties when brazing at high temperatures using a Ni-containing brazing material can be obtained without the need to include expensive elements such as Nb and Zr. Furthermore, since the ferritic stainless steel of the present invention can be manufactured using a highly efficient manufacturing process, it is also very advantageous in terms of manufacturing costs.
[0029] Figure 1 shows an example of the results observed by SEM analysis of the thickness cross-section of the steel surface layer. Figure 2 shows an example of the results of SEM and EDS analysis performed on the thickness cross-section of the steel surface layer. Figure 3 shows an example of the results of SEM and EDS analysis performed on the thickness cross-section of the steel surface layer before nitriding treatment. Figure 4 is a schematic diagram showing the setup of the Ni-containing brazing material during the brazing spreading test conducted in the example.
[0030] The present invention will be described based on the following embodiments. Note that the following description is an example of a preferred embodiment of the present invention, and the present invention is not limited to the embodiments described below.
[0031] First, the reason for limiting the steel's composition to a predetermined range in this invention will be explained. Note that while the unit for elemental content in the steel's composition is "mass percent," it will be simply referred to as "%" below unless otherwise specified.
[0032] C: 0.003 to 0.025% C is an element inevitably contained in steel. As the C content increases, the strength improves, and as the C content decreases, the workability improves. Here, C needs to be contained in an amount of 0.003% or more to obtain sufficient strength. However, an excessive C content exceeding 0.025% causes a significant decrease in workability, and also tends to cause sensitization due to precipitation of Cr carbides at grain boundaries. Therefore, the C content is set to 0.025% or less. A lower C content is more preferable for corrosion resistance. From this viewpoint, the C content is preferably 0.020% or less. On the other hand, if the C content is too low, refining takes time and the cost increases. From this viewpoint, the C content is preferably 0.010% or more.
[0033] Si: 0.05 to 1.00% Si is an element useful as a deoxidizer. This effect is obtained when the Si content is 0.05% or more. However, if the Si content exceeds 1.00%, the stainless steel is hardened, the workability is significantly reduced, and forming processing becomes difficult. In addition, when the Si content exceeds 1.00%, if brazing is performed in a high-vacuum nitrogen atmosphere having a higher oxygen partial pressure than that of a high-vacuum hydrogen atmosphere, Si oxides are formed on the surface layer of the steel sheet, which may deteriorate the brazability. Therefore, the Si content is set in the range of 0.05 to 1.00%. The Si content is preferably 0.10% or more. Further, the Si content is preferably 0.50% or less, more preferably 0.40% or less, and still more preferably 0.30% or less.
[0034] Mn: 0.05 to 1.00% Mn is used as a deoxidizer for stainless steel, and its effect is obtained when the Mn content is 0.05% or more. However, an excessive Mn content exceeding 1.00% impairs workability due to solid solution strengthening. In addition, it promotes the precipitation of MnS that serves as a corrosion initiation point, and when contained in the passive film, reduces corrosion resistance. Therefore, the Mn content is set to 1.00% or less. Accordingly, the Mn content is set in the range of 0.05 to 1.00%. The Mn content is preferably 0.10% or more. Further, the Mn content is preferably 0.50% or less.
[0035] P: 0.05% or less P is an element inevitably contained in steel. An excessive P content impairs the toughness of the base material and brazed portion, degrades weldability, and facilitates the occurrence of intergranular corrosion. This tendency becomes significant when the P content exceeds 0.05%. Therefore, the P content is set to 0.05% or less. The P content is preferably 0.03% or less. However, since reducing the P content to an extremely low level involves excessive cost increases such as strict selection of raw materials, the P content is preferably 0.01% or more, and more preferably 0.02% or more.
[0036] S: 0.03% or less S is an element inevitably contained in steel. An S content exceeding 0.03% promotes the precipitation of MnS, which easily serves as the starting point of pitting corrosion, and reduces corrosion resistance. In addition, when the S content is high, hot cracking of the brazed portion tends to occur. Therefore, the S content is set to 0.03% or less. The S content is preferably 0.01% or less. However, since excessive S removal leads to an increase in refining time and cost, the S content is preferably 0.0005% or more.
[0037] Cr: 16.0 to 25.0% Cr is an important element for ensuring the corrosion resistance of stainless steel. If the Cr content is less than 16.0%, sufficient corrosion resistance cannot be obtained after brazing treatment. However, if Cr is contained in excess of 25.0%, workability deteriorates, and nitriding treatment at low temperature also facilitates the formation of Cr nitride that degrades brazability and corrosion resistance. Therefore, the Cr content is set in the range of 16.0 to 25.0%. The Cr content is preferably 18.0% or more. Further, the Cr content is 23.0% or less.
[0038] Ni: 0.01-0.60% Ni is an effective element for suppressing the decrease in toughness when ferrite grains coarse during brazing, and it also has the effect of improving corrosion resistance. Ni can be contained in amounts of 0.01% or more. However, if the Ni content exceeds 0.60%, it leads to the formation of an austenite phase in the high-temperature range, which adversely affects hot workability. Furthermore, since Ni is an expensive element, it leads to increased costs. For this reason, the Ni content is kept in the range of 0.01-0.60%. The Ni content is preferably 0.05% or more, and more preferably 0.10% or more. Also, the Ni content is 0.50% or less, and more preferably 0.30% or less.
[0039] Ti: 0.25-0.75% Ti preferentially bonds with C and N, and is an element that suppresses the decrease in corrosion resistance (sensitization) due to the precipitation of Cr carbonitrides without the need to include expensive elements such as Nb and Zr. This effect can be obtained with a Ti content of 0.25% or more. However, from the viewpoint of brazing properties, Ti is not a very desirable element. This is because Ti is an element that is reactive with oxygen, and during the brazing process, it generates a dense and continuous Ti oxide film on the surface of the steel, reducing brazing properties. In this invention, Ti is fixed as a nitride on the surface layer of the steel, and the formation of the Ti oxide film is suppressed by reducing the amount of Ti solid solution in the ferrite phase of the surface layer. However, if the Ti content exceeds 0.75%, it becomes extremely difficult to sufficiently suppress the formation of the Ti oxide film. For this reason, the Ti content is in the range of 0.25-0.75%. The Ti content is preferably 0.30% or more. Furthermore, the Ti content is preferably 0.60% or less, and more preferably 0.50% or less.
[0040] Al: 0.005-0.150% Al is a useful element for deoxidation, and its effect can be obtained with a content of 0.005% or more. However, from the viewpoint of brazing properties, Al is not a desirable element, just like Ti. The reason is that, like Ti, Al does not form a dense and continuous Al oxide film during the brazing process (Al 2 O 3This is because an Al oxide film forms on the surface of the steel, and this Al oxide film inhibits the wettability and adhesion of the brazing material, thereby reducing brazing performance. When the Al content exceeds 0.150%, the brazing performance deteriorates significantly due to the formation of the Al oxide film. Therefore, the Al content should be in the range of 0.005 to 0.150%. Preferably, the Al content is 0.050% or less.
[0041] N: 0.005 to 0.025% N is an important element that suppresses the formation of Ti oxide film and improves brazing properties through the heat treatment (nitriding treatment) of steel sheets described later. To obtain such an effect, the N content needs to be 0.005% or more. However, if the N content exceeds 0.025%, sensitization is more likely to occur and workability decreases. For this reason, the N content should be in the range of 0.005 to 0.025%. The N content is preferably 0.007% or more. The N content is preferably 0.020% or less.
[0042] The ferritic stainless steel according to this embodiment may have a composition in which the above components are contained as basic components, with the remainder being Fe and unavoidable impurities. Although oxygen is an unavoidable impurity, a content of 3% or less of oxygen is permitted in order to ensure that the steel is not oxidized.
[0043] The ferritic stainless steel according to this embodiment may optionally contain the following elements in the following content ranges in addition to the above component composition.
[0044] Nb: 0.01-0.45% Like Ti, Nb also bonds with C and N contained in steel, suppressing sensitization. This effect is obtained when the Nb content is 0.01% or higher. On the other hand, if the Nb content exceeds 0.45%, the recrystallization temperature rises, causing disadvantages such as the inability to apply an efficient high-speed pickling process. Furthermore, with the recent surge in Nb prices, Nb content leads to increased costs. Therefore, the Nb content should be reduced as much as possible, and Ti should be included instead. For this reason, when Nb is included, the Nb content should be in the range of 0.01-0.45%. Preferably, the Nb content is 0.25% or less.
[0045] Cu: 0.01-0.80% Cu is an element that enhances corrosion resistance. This effect can be obtained when the Cu content is 0.01% or more. However, if the Cu content exceeds 0.80%, the hot workability will decrease. Therefore, when Cu is included, the Cu content should be in the range of 0.01-0.80%. The Cu content is preferably 0.20% or more. Also, the Cu content is preferably 0.50% or less.
[0046] V: 0.01-0.50% V, like Ti, bonds with C and N contained in the steel, preventing sensitization. This effect is obtained when the V content is 0.01% or higher. On the other hand, if the V content exceeds 0.50%, the workability decreases. Therefore, when V is included, the V content should be in the range of 0.01-0.50%. The V content is preferably 0.05% or higher. Also, the V content is preferably 0.40% or lower.
[0047] Mo: 0.10-3.00% Mo stabilizes the passivation film of stainless steel and improves corrosion resistance. This effect is obtained when the Mo content is 0.10% or higher. However, since Mo is an expensive element, it leads to increased costs. Furthermore, if the Mo content exceeds 3.00%, the workability decreases. Therefore, when Mo is included, the Mo content should be in the range of 0.10-3.00%. The Mo content is preferably 0.50% or higher. Also, the Mo content is 2.50% or lower.
[0048] B: 0.0003 to 0.0030% B is an element that improves secondary processing brittleness. This effect is observed when the B content is 0.0003% or higher. However, if the B content exceeds 0.0030%, ductility decreases due to solid solution strengthening. Therefore, when B is included, the B content should be in the range of 0.0003 to 0.0030%. Preferably, the B content is 0.0015% or less.
[0049] Co: 0.01–0.40% Co, like Ni, is an element that is remarkably effective in suppressing the decrease in toughness when the crystal grains become slightly coarser due to high-temperature brazing. Furthermore, the presence of Co is also advantageous in improving high-temperature strength. These effects can be obtained when the Co content is 0.01% or higher. However, an excess of Co exceeding 0.40% is undesirable because it leads to the formation of an austenite phase in the high-temperature range. Therefore, when Co is included, the Co content should be in the range of 0.01–0.40%.
[0050] Zr: 0.01 to 1.00% Zr, like Ti, has the effect of suppressing sensitization by bonding with C and N. This effect is obtained when the Zr content is 0.01% or more. However, an excess of Zr exceeding 1.00% reduces processability. Also, since Zr is a very expensive element, an excess of Zr leads to increased costs. Therefore, when Zr is included, the Zr content should be in the range of 0.01 to 1.00%. The Zr content is preferably 0.03% or more, more preferably 0.06% or more. Furthermore, the Zr content is preferably 0.60% or less, more preferably 0.30% or less.
[0051] W: 0.01 to 1.00% W, like Mo, has the effect of improving corrosion resistance. This effect is obtained when the W content is 0.01% or more. However, an excess of W exceeding 1.00% increases strength and reduces manufacturability. Therefore, when W is included, the W content should be 0.01 to 1.00%. The W content is preferably 0.10% or more, more preferably 0.30% or more. Also, the W content is preferably 0.80% or less, more preferably 0.60% or less.
[0052] Sn: 0.005 to 0.500% Sn has the effect of further enhancing the high corrosion resistance of stainless steel. To obtain this effect, the Sn content is set to 0.005% or more. On the other hand, an excessive Sn content exceeding 0.500% leads to deterioration of workability. Therefore, when Sn is contained, the Sn content is set to 0.005 to 0.500%. The Sn content is preferably 0.010% or more, more preferably 0.020% or more. Further, the Sn content is preferably 0.400% or less, more preferably 0.300% or less.
[0053] REM: 0.001 to 0.100% REM (rare earth metals) improves oxidation resistance, suppresses the formation of oxide scale, and improves the corrosion resistance of welded portions. This effect is obtained when the REM content is 0.001% or more. However, if REM is contained in excess exceeding 0.100%, productivity such as pickling performance is deteriorated, and cost increases. Therefore, when REM is contained, the REM content is set to 0.001 to 0.100%. The REM content is preferably 0.004% or more, more preferably 0.006% or more. Further, the REM content is preferably 0.040% or less, more preferably 0.020% or less. Note that REM is a general term for a total of 17 elements including Sc, Y, and lanthanoid elements. As REM, one or more of these 17 elements can be contained, and the REM content referred to herein is the total content of these elements.
[0054] The component composition of the ferritic stainless steel according to the present embodiment has been described above.
[0055] Further, in the ferritic stainless steel of the present invention, it is extremely important to appropriately control the component composition of the steel within the above-mentioned ranges, and to perform heat treatment with a controlled atmosphere to achieve the following nitriding effect in the surface layer portion of the steel.
[0056] The average Ti concentration contained in the ferrite phase in the region from the surface to a depth of 20 μm in the depth direction is 0.2 mass% or less, and the density (number density) of Ti nitrides with a size of 1 μm or less in the sheet thickness cross section of the aforementioned region is 0.03 pieces / μm 2As a result of the above nitriding treatment effect, the formation of a continuous and dense oxide film of Ti on the surface can be suppressed, and consequently, the brazing performance is improved when brazing at high temperatures using Ni-containing brazing material.
[0057] Here, this nitriding effect is obtained by the bonding of nitrogen in the atmosphere with Ti in the steel. The inventors believe that the mechanism by which this nitriding effect suppresses the formation of Ti oxide films is as follows: Through nitriding, Ti present in the surface layer of the steel bonds with nitrogen in the atmosphere and is fixed to the surface layer as Ti nitride, reducing the amount of Ti dissolved in the ferrite phase near the surface. As a result, the amount of Ti diffused to the surface during brazing is greatly reduced, and consequently, the formation of Ti oxide films is suppressed.
[0058] Here, the average Ti concentration in the ferrite phase in the region up to a depth of 20 μm from the surface (average Ti concentration in the ferrite phase) is 0.2 mass% or less, and the density of Ti nitrides with a size of 1 μm or less in the cross-sectional area of the plate thickness in the said region is 0.03 particles / μm 2 If the above conditions are not met, the formation of a Ti oxide film on the surface cannot be sufficiently suppressed. Therefore, the average Ti concentration in the ferrite phase in the region up to a depth of 20 μm from the surface is 0.2 mass% or less, and the density of Ti nitrides with a size of 1 μm or less in the cross-section of the plate thickness in the said region is 0.03 particles / μm 2 The above is correct. Preferably, the average Ti concentration is 0.1% by mass or less. Also, the density of Ti nitrides with a size of 1 μm or less in the cross-section of the plate thickness is 0.04 particles / μm. 2 That concludes the explanation. The lower limit of the average Ti concentration is not particularly limited, and the average Ti concentration may be 0.0 mass%. Furthermore, the upper limit of the density of Ti nitrides with a size of 1 μm or less in the cross-section of the plate thickness is not particularly limited, and the density may, for example, be 0.07 particles / μm. 2 The following is acceptable:
[0059] The average Ti concentration in the ferrite phase in the region up to a depth of 20 μm from the surface and the density of Ti nitrides in the cross-section of the steel plate in the said region are measured as follows. Figure 1 shows an example of the results observed by SEM analysis of the cross-section of the steel plate in the said region (steel surface layer). Figure 2 shows an example of the results of SEM and EDS analysis performed on the cross-section of the steel plate in the said region. Figure 3 shows, for reference, the results of SEM and EDS analysis performed on the cross-section of the steel surface layer before nitriding treatment. The average Ti concentration and the density of Ti nitrides are measured, for example, by observing the cross-section of the steel plate using a scanning electron microscope (SEM) and an energy-dispersive X-ray spectrometer (EDS) for SEM analysis, with a depth of 20 μm from the surface of the steel plate and an area of 600 μm. 2 Multiple observation areas are sampled (see Figure 1). The average Ti concentration in the ferrite phase in the region up to a depth of 20 μm from the surface can be calculated by performing point analysis using EDS at three locations other than the precipitates within each observation area (Pt4, Pt5, and Pt6 in Figure 2) and calculating the average value of the mass % of Ti. Furthermore, the density of Ti nitrides smaller than 1 μm in size in the plate thickness cross-section of the region up to a depth of 20 μm from the surface can be calculated by performing point analysis of the precipitate components within each observation area using EDS, counting the number of Ti nitrides smaller than 1 μm, dividing by the observation area, and calculating the average value.
[0060] Furthermore, the Ti nitrides referred to here are precipitates formed by a predetermined heat treatment (nitriding treatment). To suppress the decrease in corrosion resistance (sensitization) due to the precipitation of Cr carbonitrides, Ti carbonitrides that are present in the steel before nitriding treatment and are relatively large in size are excluded from the measurement range (see Figure 1). Specifically, in precipitates analyzed by EDS, if the mass percentage of Ti is 1.0% or more and the mass percentage of O is about the same as that of the base material (3% or less), then those precipitates are considered to be Ti nitrides formed by the nitriding treatment. Since the shape of the precipitates is irregular, only precipitates that can be completely enclosed by a circle with a diameter of 1 μm, i.e., Ti nitrides with a size of 1 μm or less, are considered to have been produced by the nitriding treatment (see Figure 1). For the measurement method of the average Ti concentration and the density of the Ti nitrides, please refer to the description in the examples.
[0061] Next, a preferred method for manufacturing the ferritic stainless steel of the present invention will be described.
[0062] Molten steel with the above-mentioned component composition is melted using known methods such as converters, electric furnaces, and vacuum melting furnaces, and then formed into steel material (slabs) by continuous casting or ingot-splitting method. This steel material is heated at 1100 to 1250°C for 1 to 24 hours, or hot-rolled directly without heating to produce hot-rolled steel sheets. Hot-rolled steel sheets may usually be hot-rolled and annealed by hot-rolling at 800 to 1100°C for 1 to 10 minutes to produce hot-rolled and annealed steel sheets, but hot-rolled and annealing may be omitted depending on the application.
[0063] Next, cold rolling and cold-rolled sheet annealing are combined to produce the product. It is preferable to perform cold rolling with a reduction ratio of 50% or more to improve shape correction, ductility, bendability, and press formability. Furthermore, the combination of cold rolling and cold-rolled sheet annealing may be performed once or two or more times.
[0064] Here, in order to obtain the ferritic stainless steel of the present invention, a predetermined heat treatment (nitriding treatment) is performed. The heat treatment is preferably performed during the final cold-rolled sheet annealing (finish annealing) after cold rolling. This is because performing the heat treatment during the final cold-rolled sheet annealing (finish annealing) after cold rolling allows for nitriding of the steel sheet without increasing the number of steps, which is advantageous in terms of manufacturing efficiency. However, this heat treatment (nitriding treatment) may be performed in a separate process from the cold-rolled sheet annealing, for example, after the components have been cut from the steel sheet. Furthermore, when the predetermined heat treatment (nitriding treatment) is performed during the final cold-rolled sheet annealing, the conditions for cold-rolled sheet annealing other than the final cold-rolled sheet annealing are not particularly limited, and for example, known conditions can be adopted.
[0065] The following describes the conditions for the heat treatment (nitriding treatment).
[0066] Dew point of the atmosphere: Below -30°C. If the dew point exceeds -30°C, an oxide film will form on the surface of the steel, preventing nitrogen in the atmosphere from penetrating the steel, and thus preventing the surface layer of the steel from being nitrided. For this reason, the dew point should be below -30°C. Preferably, the dew point is below -40°C. The lower limit of the dew point is not limited, but as an example, the dew point may be above -70°C.
[0067] Partial pressure of nitrogen in the atmosphere: 25 × 10 3 The partial pressure of nitrogen in an atmosphere above Pa is 25 × 10⁻⁶ 3 Below Pa, a sufficient amount of nitrogen does not penetrate the steel, and the nitriding treatment effect cannot be obtained. Therefore, the partial pressure of nitrogen in the atmosphere should be 25 × 10⁻⁶. 3 The pressure should be Pa or higher. The remainder other than nitrogen should be hydrogen. Due to the reducing properties of hydrogen, the partial pressure of oxygen in the heat treatment atmosphere can be reduced, making it easier to remove the passive film or oxide film on the surface of the steel sheet, and thus making the nitriding effect more pronounced. The remainder may contain inert gases other than hydrogen, such as argon. The remainder may also contain unavoidable impurities. Examples of unavoidable impurities include O 2 H 2 O, CO, CO 2 Examples include the following. The partial pressure of nitrogen in the atmosphere is, for example, 10¹ × 10¹⁰. 3 It may be less than or equal to Pa.
[0068] Processing temperature (annealing temperature for the final cold-rolled sheet annealing) T: 900 to 1200°C. The heat treatment is considered to have started when the temperature of the steel sheet reaches the processing temperature. Heat treatment (nitriding treatment) is performed by holding the steel sheet at the processing temperature for a certain period of time. The temperature of the steel sheet can be measured, for example, by connecting a thermocouple to the steel sheet. As mentioned above, if the heat treatment is performed at the time of the final cold-rolled sheet annealing, the processing temperature corresponds to the annealing temperature. If the processing temperature is below 900°C, nitrogen in the processing atmosphere does not penetrate the steel and the nitriding treatment effect cannot be obtained. Also, in nitriding treatment at low temperatures below 900°C, Cr nitrides are more easily formed. For this reason, the processing temperature should be 900°C or higher. Preferably, the processing temperature is 950°C or higher. However, if the processing temperature exceeds 1200°C, the steel will deform, so the processing temperature should be 1200°C or lower. More preferably, the processing temperature is 1150°C or lower, and even more preferably 1100°C or lower.
[0069] Processing time (annealing time for the final cold-rolled sheet annealing) t: 10 to 300 seconds. Heat treatment is started when the steel sheet temperature reaches the above processing temperature. Nitriding is performed by maintaining a constant processing time at the predetermined processing temperature. If the processing time is less than 10 seconds, nitrogen in the processing atmosphere will not penetrate the steel sufficiently, and a sufficient nitriding effect will not be obtained. On the other hand, if the processing time exceeds 300 seconds, the nitriding effect will saturate, the outermost surface of the steel sheet will oxidize, and there is a concern that the brazing properties will decrease. For this reason, the processing time should be in the range of 10 to 300 seconds. Preferably, the processing time is in the range of 30 to 300 seconds.
[0070] Furthermore, to obtain good brazing properties in steels with different Ti and Cr content, the heat treatment (nitriding) conditions are strictly limited. For steels with higher Ti content, to achieve a sufficient nitriding effect, heat treatment is performed at a higher temperature, higher hydrogen partial pressure, lower dew point, and longer treatment time. Also, for steels with higher Cr content, a higher treatment temperature and lower nitrogen partial pressure are required to suppress the formation of Cr nitrides.
[0071] As described above, within a limited range of conditions, better brazing properties can be obtained with higher processing temperatures, longer processing times, higher hydrogen partial pressure, lower dew point, and lower Ti and Cr content in the steel.
[0072] Therefore, in order to achieve good brazing properties, the following equation (1) must be satisfied: 2T - (200 [Ti] + 50 [Cr] + 2P + 5D - t) ≥ 880 ... (1) Here, in equation (1), T: processing (annealing) temperature (°C), [Ti]: Ti content in the steel (mass%), [Cr]: Cr content in the steel (mass%), D: dew point (°C), P: partial pressure of nitrogen (×10 3 Pa) and t are the processing (annealing) time (seconds). To obtain better brazing properties, the calculated value on the left side of equation (1) is preferably 1000 or more (≧1000). However, the calculated value on the left side of equation (1) may be 1800 or less as an example.
[0073] Furthermore, under nitriding conditions of high temperature, long duration, low hydrogen partial pressure, and high dew point, the outermost surface of the steel sheet may oxidize during the nitriding process, potentially reducing its brazing properties. In such cases, to ensure sufficient brazing properties, it is preferable to perform pickling after the nitriding process (or after the final cold-rolled sheet annealing if the nitriding process was performed during the final cold-rolled sheet annealing) to remove any oxides that may have formed on the surface. As a result, the brazing properties when using Ni-containing brazing materials can be further improved.
[0074] The pickling method is not particularly limited. For example, if the appearance has turned a deep yellow or blue, it can be determined that a thick oxide film (Ti,Cr oxide) has formed, and pickling can be performed. The reason for the formation of the oxide film is thought to be that, under atmospheric conditions of low hydrogen partial pressure and high dew point, the oxygen partial pressure in the atmosphere is high, causing Ti,Cr oxide to form. Alternatively, it is thought that the Ti nitride formed on the outermost surface was oxidized by contact with oxygen in the atmosphere during a long nitriding treatment, and changed into Ti oxide. As for the pickling conditions, electrolytic pickling can be performed two or more times, varying the electrolysis time, in a mixed acid solution of nitric acid and hydrochloric acid at a temperature of 20 to 50°C. This makes it possible to remove the oxide formed on the outermost surface.
[0075] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples.
[0076] Steel having the component composition shown in Table 1 was melted in a 50 kg small vacuum melting furnace to obtain steel ingots. These steel ingots were heated to 1150°C in a furnace purged with Ar gas, and then hot-rolled to 3.5 mm thick hot-rolled steel sheets. Next, these hot-rolled steel sheets were hot-rolled annealed at 950°C for 1 minute. After that, the surface was shot-blasted with glass beads, then pickled by immersion in a sulfuric acid solution at 80°C, followed by immersion in a mixed acid of nitric acid and hydrofluoric acid at 55°C for 60 seconds to remove scale.
[0077] Subsequently, the sheets were cold-rolled to a thickness of 0.8 mm, and cold-rolled sheets were annealed under the conditions shown in Table 2 to obtain cold-rolled annealed steel sheets. This cold-rolled sheet annealing also served as the heat treatment (nitriding treatment) described above. After cold-rolled sheet annealing, the appearance of the cold-rolled annealed steel sheets was observed. Sheets that had turned a deep yellow or blue color were judged to have formed a thick oxide film (Ti, Cr oxide), and electrolytic pickling was performed at least twice in a mixed acid solution of nitric acid and hydrochloric acid at a temperature of 35°C, with varying electrolysis times.
[0078] The cold-rolled annealed steel sheets thus obtained underwent the following procedures: (1) the effect of nitriding treatment was measured (average Ti concentration on the surface and density of Ti nitrides smaller than 1 μm). Furthermore, (2) high-temperature brazing was performed using Ni-containing brazing material, and the brazing properties of the cold-rolled annealed steel sheets after brazing were evaluated.
[0079] (1) Measurement of the effect of nitriding treatment For each of the cold-rolled annealed steel sheets described above, the average Ti concentration contained in the ferrite phase in the region up to a depth of 20 μm from the surface and the density of Ti nitrides with a size of 1 μm or less in the cross-section of the sheet thickness in the said region were measured as follows. As the measuring equipment, a scanning electron microscope (SEM) Miniscope™ TM3030plus manufactured by Hitachi High-Tech Corporation and an energy-dispersive X-ray spectrometer (EDS) AZtecOne manufactured by Oxford Instruments were used. The cross-section of the steel sheet thickness was observed by SEM analysis, and four observation areas with a depth of 20 μm and a width of 30 μm from the surface of the steel sheet were sampled. The average Ti concentration contained in the ferrite phase was calculated by performing point analysis at 3 locations other than precipitates within each region at 5 μm intervals from the surface of the steel sheet using the EDS, and calculating the average value of the Ti concentration (mass%) of a total of 12 points. Furthermore, the density of Ti nitrides smaller than 1 μm was calculated from the average value of the precipitate densities within each region. Specifically, the components of the precipitates were analyzed, and because detection of N by EDS was difficult, if the mass percentage of Ti in the analyzed precipitate was 1.0% or more and the mass percentage of O was about the same as the base material (3% or less), the precipitate was identified as a Ti nitride formed by the nitriding treatment. The density of Ti nitrides smaller than 1 μm was calculated by counting the number of Ti nitrides smaller than 1 μm among the identified Ti nitrides, dividing by the observation area to calculate the density of the Ti nitrides, and then calculating the average value of the densities at four locations. The Ti nitrides referred to here are precipitates formed by the nitriding treatment. In order to suppress the decrease in corrosion resistance (sensitization) due to the precipitation of Cr carbonitrides, Ti carbonitrides that were present in the steel plate before the nitriding treatment and were relatively large in size were excluded from the measurement range. Specifically, as shown in Figure 1, because the shape of the precipitates is irregular, only precipitates that can be completely enclosed by a circle with a diameter of 1 μm, i.e., Ti nitrides with a size of 1 μm or less, were considered to have been produced by the nitriding treatment. The measurement results are shown in Table 2.
[0080] (2) Evaluation of Brazing Properties A 40 mm square brazing spread test piece was cut from each of the cold-rolled annealed steel sheets described above, ultrasonically degreased in acetone, and then subjected to a brazing spread test. Figure 4 is a schematic diagram showing the setup of the Ni-containing brazing material during the brazing spread test. The Ni-containing brazing material was made into a pellet of 12 mmΦ (diameter) × 1 mmH (height) and placed on top of the test piece. The sample was then placed horizontally in the furnace. The conditions for the brazing heat treatment will be described later. After the brazing heat treatment, the appearance of the test piece was photographed using a one-shot 3D shape measuring machine. The brazing material area and the base material area (test piece) were separated based on the difference in color tone and height, and the area of the brazing material area was measured. The brazing spread rate was calculated from the area ratio of the Ni-containing brazing material before and after the brazing heat treatment (area of brazing material after brazing heat treatment / area of brazing material before brazing heat treatment). After brazing, the brazing properties were evaluated according to the following criteria. The evaluation results are shown in Table 2. ◎ (Pass, Excellent): Wax spread rate is 2.0 or higher ○ (Pass, Good): Wax spread rate is 1.8 or higher but less than 2.0 × (Fail): Wax spread rate is less than 1.8
[0081] In all of the brazing performance evaluations described above, JIS standard BNi-7 (Ni matrix of 14 mass% Cr-10 mass% P), a low-melting-point Ni-containing brazing material, was used as the Ni-containing brazing material. Brazing was performed in a sealed furnace. Furthermore, the brazing heat treatment pattern was set to a heating rate of 100°C / min. Since the brazing material contains an organic binder to turn the metal powder into a paste, it was held at 600°C for 5 minutes to decompose the binder. To ensure uniform sample temperature during heating, soaking was performed at 800°C, lower than the solidus temperature, for 5 minutes. After soaking, the temperature was raised again and held at 1080°C, above the liquidus temperature, for 10 minutes. After that, the furnace atmosphere was maintained and the sample was cooled to 200°C, followed by nitrogen gas cooling. To suppress the formation of Ti oxides in Ti-containing ferritic stainless steel, the furnace atmosphere (brazing atmosphere) was created by first drawing the furnace to high vacuum and then using an inert gas to create a high-vacuum nitrogen atmosphere of approximately 20 Pa and a high-vacuum hydrogen atmosphere of approximately 20 Pa. The dew point was set to -50°C. Brazing properties that received a rating of ○ or ◎ in both the high-vacuum nitrogen atmosphere and the high-vacuum hydrogen atmosphere were judged to have good brazing properties.
[0082]
[0083]
[0084] Table 2 shows that in Invention Examples No. 1 to 14, where the component composition and the effect of nitriding treatment (average Ti concentration on the surface, density of Ti nitrides smaller than 1 μm) were within the appropriate range, the brazing spread rate of the Ni-containing brazing material was satisfactory, indicating good brazing properties. Furthermore, when the value on the left side of the predetermined equation (1) was 1000 or more, and pickling was also performed after nitriding treatment, the brazing properties could be further improved. Specifically, in Nos. 3, 8, and 12, excellent brazing properties were observed, with an evaluation of ◎, in both high-vacuum hydrogen atmospheres and high-vacuum nitrogen atmospheres during brazing heat treatment. From the above, it can be seen that the Invention Examples show good brazing properties even when brazing at high temperatures using Ni-containing brazing material. In contrast, in Comparative Examples No. 15 to 30, where the component composition and the effect of nitriding treatment were outside the appropriate range, good brazing properties could not be obtained in at least one of the high-vacuum hydrogen atmosphere and high-vacuum nitrogen atmosphere during brazing heat treatment.
[0085] According to the present invention, even when brazing is performed at high temperatures using a Ni-containing brazing material, a ferritic stainless steel exhibiting good brazing properties can be obtained. Such a ferritic stainless steel can be suitably applied to heat exchanger components of exhaust heat recovery devices and EGR coolers assembled by brazing, and is extremely useful in industry.
Claims
1. The material has a composition in mass% of the following elements: C: 0.003-0.025%, Si: 0.05-1.00%, Mn: 0.05-1.00%, P: 0.05% or less, S: 0.03% or less, Cr: 16.0-25.0%, Ni: 0.01-0.60%, Ti: 0.25-0.75%, Al: 0.005-0.150%, and N: 0.005-0.025%, with the remainder being Fe and unavoidable impurities. The average Ti concentration in the ferrite phase in the region up to a depth of 20 μm from the surface is 0.2 mass% or less, and the density of Ti nitride particles with a size of 1 μm or less in the cross-sectional area of the plate thickness in the said region is 0.03 particles / μm. 2 That concludes the description of ferritic stainless steel.
2. The ferritic stainless steel according to claim 1, wherein the component composition further contains, by mass%, one or more selected from: Nb: 0.01 to 0.45%, Cu: 0.01 to 0.80%, V: 0.01 to 0.50%, Mo: 0.10 to 3.00%, B: 0.0003 to 0.0030%, Co: 0.01 to 0.40%, Zr: 0.01 to 1.00%, W: 0.01 to 1.00%, Sn: 0.005 to 0.500%, and REM: 0.001 to 0.100%.
3. A method for producing ferritic stainless steel according to claim 1 or 2, comprising the steps of: hot-rolling a slab having the above-mentioned component composition to obtain a hot-rolled steel sheet; optionally hot-rolled annealing the hot-rolled steel sheet to obtain a hot-rolled annealed steel sheet; and subjecting the hot-rolled steel sheet or hot-rolled annealed steel sheet to a combination of cold-rolling and cold-rolled annealing one or more times, wherein in the final cold-rolled annealing, the dew point is -30°C or lower, and the nitrogen partial pressure is 25 × 10⁻⁶. 3 A method for manufacturing ferritic stainless steel, comprising heat treatment in an atmosphere of nitrogen and hydrogen above Pa, satisfying an annealing temperature T: 900 to 1200°C, an annealing time t: 10 to 300 seconds, and the following equation (1) being satisfied: 2T - (200 [Ti] + 50 [Cr] + 2P + 5D - t) ≥ 880 ... (1) Here, in equation (1), T: annealing temperature (°C), [Ti]: Ti content in the steel (mass%), [Cr]: Cr content in the steel (mass%), D: dew point (°C), P: partial pressure of nitrogen (×10 3 Pa), t: Annealing time (seconds).
4. The method for producing ferritic stainless steel according to claim 3, wherein the final cold-rolled sheet is pickled after the annealing.