Polyimide precursor, polyimide, polyimide varnish thereof, and polyimide film

A polyimide precursor and film with specific ester-type tetracarboxylic dianhydride and diamine structures address solubility and heat resistance issues, providing high solubility and heat resistance up to 350°C without fluorine, suitable for high-temperature applications.

WO2026239960A1PCT designated stage Publication Date: 2026-11-19HONSHU CHEM INDAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017043
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-04-30
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional polyimide films are insoluble in organic solvents and have insufficient heat resistance for high-temperature applications, and the introduction of fluorine atoms to improve solubility raises environmental and health concerns.

Method used

A polyimide precursor and film with specific ester-type tetracarboxylic dianhydride and diamine structures that allow high solubility in various organic solvents without fluorine, achieving heat resistance up to 350°C.

Benefits of technology

The polyimide exhibits excellent solubility in organic solvents and heat resistance, reducing environmental and health risks while enabling high-temperature applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017043_19112026_PF_FP_ABST
    Figure JP2026017043_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a novel polyimide resin material that has sufficient heat resistance and can be dissolved at a high concentration in various organic solvents while suppressing the introduction of fluorine atoms into the polyimide. As a solution to the above problem, a polyimide having one or more repeating structures selected from the repeating structures represented by general formula (1) is provided. (In the formula, R1 and R2 each independently represent a hydrogen atom or a methyl group, and A represents a divalent group represented by general formula (2)). (In the formula, n is 0, 1 or 2; X is a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom, or a sulfonyl group; R3 are each independently a hydrogen atom or a methyl group; and * is a bonding position).
Need to check novelty before this filing date? Find Prior Art

Description

Polyimide precursors, polyimides, their polyimide varnishes, and polyimide films

[0001] This invention relates to a novel polyimide having excellent organic solvent solubility and sufficient heat resistance, as well as a varnish and film of the same polyimide, and a precursor of the same polyimide.

[0002] Polyimide resins obtained by the reaction of tetracarboxylic dianhydride and diamine compounds are generally insoluble, infusible, and ultra-heat-resistant resins with excellent properties such as heat oxidation resistance, heat resistance, radiation resistance, low-temperature resistance, and chemical resistance. For this reason, polyimide resins are used as materials in fields such as insulating coatings, insulating films, semiconductors, electrode protective films, flexible printed circuit boards and other electrical and electronic components, aerospace equipment, and transportation equipment, or as heat-resistant adhesives.

[0003] Conventional polyimide films are insoluble in organic solvents. Therefore, they are obtained by coating a polyamic acid solution, a polyimide precursor, onto a support and subjecting it to high-temperature treatment, thereby removing the solvent and simultaneously performing thermal imidation. However, the high heating temperatures required for thermal imidation (e.g., over 300°C), the tendency for discoloration due to heating, and the inability of parts to withstand high temperatures have limited the applications of polyimide. In this context, conventional methods have involved introducing fluorine atoms or groups containing fluorine atoms into the polyimide backbone to improve its solubility in organic solvents. Recently, concerns have been growing regarding the environmental impact and health risks of some compounds belonging to the perfluoroalkyl and polyfluoroalkyl (PFAS) groups. Furthermore, concerns are also growing regarding the environmental impact and health risks of organic solvents used to dissolve polyimide. For example, N-methylpyrrolidone (NMP) is an effective solvent for dissolving polyimide and can dissolve polymers that cannot be dissolved by other solvents. However, due to concerns about reproductive toxicity, it is treated as a restricted substance under the REACH Regulation.

[0004] Polyimides that use ester-type acidic dianhydrides are one type of polyimide. For example, a polyimide obtained from 1,1-bis(4-hydroxyphenyl)cyclohexane-bis(trimellitate anhydride) and a diamine containing a dimeramine is known as an ester-type acidic dianhydride (Patent Document 1).

[0005] Japanese Patent Publication No. 2020-203981

[0006] Patent Document 1 states that polyimides obtained from 1,1-bis(4-hydroxyphenyl)cyclohexane-bis(trimellitate anhydride) and diamines containing dimeramine have excellent solder heat resistance. However, the softening point of this polyimide is 110°C, which is insufficient for products exposed to high temperatures exceeding 200°C during the manufacturing process of products using polyimide materials, or for applications where polyimide materials have been conventionally used at high temperatures. Against this background, the present invention aims to provide a novel polyimide resin material that has sufficient heat resistance and can be dissolved at high concentrations in various organic solvents without introducing fluorine atoms into the polyimide.

[0007] As a result of diligent research to solve the above-mentioned problems, the present inventors discovered that a polyimide having a repeating structure derived from a specific ester-type tetracarboxylic dianhydride and a diamine has excellent heat resistance and can be dissolved at high concentrations in various organic solvents without introducing fluorine atoms into the polyimide, thus completing the present invention.

[0008] The present invention is as follows: 1. A polyimide precursor having one or more repeating structures selected from the repeating structures represented by general formula (1A). (In the formula, R 1 and R 2 Each of the above independently represents either a hydrogen atom or a methyl group, and A represents a divalent group represented by general formula (2). The dashed line within the benzene ring indicates bonding to either one of the benzene rings. (wherein n represents 0, 1, or 2, X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom, or a sulfonyl group, R 3 ) Each of these independently represents a hydrogen atom or a methyl group, and * indicates a bond position. 2. A polyimide having one or more repeating structures selected from the repeating structures represented by general formula (1). (In the formula, R 1 and R 2 Each of these independently represents either a hydrogen atom or a methyl group, and A represents a divalent group represented by general formula (2). (wherein n represents 0, 1, or 2, X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom, or a sulfonyl group, R 3 ) Each independently represents a hydrogen atom or a methyl group, and * indicates the bond position. 3. The polyimide according to 2. wherein the glass transition temperature is in the range of 210°C to 350°C. 4. A polyimide precursor varnish comprising the polyimide precursor and an organic solvent according to 1. 5. The polyimide precursor varnish according to 4. wherein the organic solvent is at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, sulfoxide-based organic solvents, and alcohol-based organic solvents. 6. The polyimide precursor varnish according to 4. wherein the polyimide precursor is contained in an amount of 5 to 60% by weight relative to the total weight of the polyimide precursor and the organic solvent. 7. A polyimide varnish comprising the polyimide and an organic solvent according to 2. 8. The polyimide varnish according to 7, wherein the organic solvent is at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, sulfoxide-based organic solvents, and alcohol-based organic solvents. 9. The polyimide varnish according to 7, wherein the polyimide is contained in an amount of 5 to 60% by weight relative to the total weight of the polyimide and the organic solvent. 10.2. A polyimide film containing the polyimide according to 7.

[0009] According to the present invention, it is possible to provide a polyimide resin material that has excellent solubility in various organic solvents as well as excellent heat resistance. In addition, since the polyimide of the present invention has one or more repeating structures selected from repeating structures represented by general formula (1) that do not contain fluorine atoms, it is extremely useful in that it reduces the burden on the environment and health.

[0010] This figure shows the ultraviolet-visible light transmittance spectra of the raw material monomer (tetracarboxylic dianhydride) used in the examples. This figure shows the ultraviolet-visible light transmittance spectra of the raw material monomer (diamine) used in the examples. This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films (average film thickness of 35.6 and 18.0 μm) obtained in Example 1, measured according to the measurement method of 5. (1). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films (average film thickness of 51.7 and 18.4 μm) obtained in Example 2, measured according to the measurement method of 5. (1). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide film (average film thickness of 21.0 μm) obtained in Example 3, measured according to the measurement method of 5. (1). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide film (average film thickness of 18.6 μm) obtained in Comparative Example 1 and the polyimide films (average film thickness of 45.1 and 21.1 μm) obtained in Comparative Example 2, measured according to the measurement method of 5. (1). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films obtained in Comparative Example 3 (average film thickness of 27.8 and 18.3 μm) and the polyimide film obtained in Comparative Example 4 (average film thickness of 14.2 μm) using the measurement method in 5. (1). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films obtained in Comparative Example 5 (average film thickness of 35.6 and 14.0 μm) using the measurement method in 5. (1). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films obtained in Examples 1 to 3 (average film thickness of 18.0, 16.0, and 21.0 μm, respectively) using the measurement method in 5. (2). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films obtained in Comparative Examples 1 and 2 (average film thickness of 20.0 μm each) using the measurement method in 5. (2). This figure shows the ultraviolet-visible light transmittance spectra of the polyimide films obtained in Comparative Examples 3 and 4 (average film thickness of 20.0 μm each) using the measurement method in 5. (2). This figure shows the ultraviolet-visible light transmittance spectrum obtained by the measurement method in (2). This figure shows the ultraviolet-visible light transmittance spectrum obtained by the measurement method in 5. (2) for the polyimide film (average film thickness of 14.0 μm) obtained in Comparative Example 5. This figure shows the ultraviolet-visible light transmittance spectrum obtained by the measurement method in 5. (2) for the polyimide film (average film thickness of 29.7 μm) obtained in Comparative Example 6.

[0011] Hereinafter, embodiments of the present invention will be described in detail.

[0012] <Polyimide Precursor and Polyimide of the Present Invention> The polyimide precursor of the present invention is characterized by having one or more repeating structures selected from the repeating structures represented by general formula (1A). (wherein R 1 and R 2 each independently represent a hydrogen atom or a methyl group, A represents a divalent group represented by general formula (2). The dashed line in the benzene ring indicates bonding to any one position on the benzene ring.) (wherein n represents 0, 1 or 2, X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom or a sulfonyl group, R 3 each independently represent a hydrogen atom or a methyl group, and * indicates a bonding position.)

[0013] The polyimide of the present invention is characterized by having one or more repeating structures selected from the repeating structures represented by general formula (1). (wherein R 1 and R 2 each independently represent a hydrogen atom or a methyl group, and A represents a divalent group represented by general formula (2).) (wherein n represents 0, 1 or 2, X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom or a sulfonyl group, R 3 each independently represent a hydrogen atom or a methyl group, and * indicates a bonding position.)

[0014] The polyimide precursor and polyimide of the present invention are, respectively, a polyimide precursor and polyimide having one repeating structure selected from the repeating structures represented by general formula (1A) and general formula (1), and a polyimide precursor and polyimide having multiple repeating structures selected from the repeating structures represented by general formula (1A) and general formula (1), where the multiple may be two, three, four, or more. The number of repeating structures selected from the repeating structures represented by general formula (1A) and general formula (1) is preferably one, two, three, or four, more preferably one, two, or three, even more preferably one or two, and particularly preferably one. Furthermore, it is preferable that the polyimide precursor and polyimide of the present invention each have a repeating structure consisting only of the repeating structures represented by general formula (1A) and general formula (1). When the polyimide precursor and polyimide of the present invention is a polyimide having multiple repeating structures selected from the repeating structures represented by general formula (1A) and general formula (1), there is no restriction on the ratio of each repeating structure to the total repeating structure of the polyimide. Furthermore, the multiple repeating structures may be arranged regularly or may be present randomly within the polyimide.

[0015] In general formula (1A) and general formula (1), R 1 and R 2 Each of these independently represents a hydrogen atom or a methyl group, R 1 and R 2 Both are hydrogen atoms, or R 1 is a hydrogen atom and R 2 It is preferable that R is a methyl group, 1 and R 2 It is particularly preferable that both are hydrogen atoms. R of general formula (1A) 1 and R 2 The repeating structure when both atoms are hydrogen atoms is represented by the general formula (1A-1), and this structure is preferred. (In the formula, A represents the divalent group represented by general formula (2).) R of general formula (1) 1 and R 2The repeating structure when both atoms are hydrogen atoms is represented by the general formula (1-1), and this structure is preferred. (In the formula, A represents a divalent group represented by general formula (2).)

[0016] In general formula (1A) and general formula (1), A represents the divalent group represented by general formula (2). When n in general formula (2) is 0, it is represented by general formula (2-1). (In the formula, R 3 And * are the same as the definition in general formula (2).) In general formula (2-1), the two bond positions are selected from the para, meta, or ortho positions, but the para or meta positions are preferred. When n in general formula (2) is 1, it is represented by general formula (2-2). (In the formula, X, R 3 , and * are the same as the definition of general formula (2). Specific examples of the positions in general formula (2-2) where the two benzene rings and X are bonded include general formulas (2-2-1) to (2-2-4). Among these, general formula (2-2-1) is particularly preferred. (In the formula, X, R 3 , and * are the same as the definitions in general formula (2).) In general formula (2), X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom, or a sulfonyl group. Among these, a direct bond, a methylene group, an oxygen atom, or a sulfonyl group is preferred, a methylene group, an oxygen atom, or a sulfonyl group is more preferred, and a methylene group or a sulfonyl group is particularly preferred. In general formula (2), R 3Each of these independently represents either a hydrogen atom or a methyl group. Among these, it is preferable that both are hydrogen atoms or both are methyl groups, and it is particularly preferable that both are hydrogen atoms. Specific examples of preferred structures in general formula (2) are shown in chemical formulas (2a) to (2p). Among these, chemical formulas (2a), (2b), (2c), (2f), (2g), (2h), (2i), (2j), (2k), or (2n) are more preferred, chemical formulas (2a), (2b), (2c), (2f), (2g), (2h), or (2n) are even more preferred, chemical formulas (2a), (2b), (2c), (2f), (2g), or (2h) are even more preferred, and chemical formulas (2a), (2b), (2c), or (2h) are particularly preferred. (In the formula, * is the same as the definition in general formula (2).)

[0017] Among the above, the repeating structure of the polyimide precursor of the present invention represented by general formula (1A) is preferred when A in general formula (1A-1) is chemical formula (2a) to (2p). Among these, A in general formula (1A-1) is more preferably chemical formula (2a), (2b), (2c), (2f), (2g), (2h), (2i), (2j), (2k), or (2n), even more preferably chemical formula (2a), (2b), (2c), (2f), (2g), (2h), or (2n), even more preferably chemical formula (2a), (2b), (2c), (2f), (2g), or (2h), and particularly preferably chemical formula (2a), (2b), (2c), or (2h). Among the above, the repeating structure of the polyimide of the present invention represented by general formula (1) is preferred when A in general formula (1-1) is chemical formula (2a) to (2p). Among these, A in general formula (1-1) is more preferably chemical formula (2a), (2b), (2c), (2f), (2g), (2h), (2i), (2j), (2k), or (2n), even more preferably chemical formula (2a), (2b), (2c), (2f), (2g), (2h), or (2n), even more preferably chemical formula (2a), (2b), (2c), (2f), (2g), or (2h), and particularly preferably chemical formula (2a), (2b), (2c), or (2h).

[0018] The glass transition temperature of the polyimide of the present invention is preferably in the range of 210°C to 350°C, more preferably in the range of 220°C to 350°C, still more preferably in the range of 250°C to 350°C, and particularly preferably in the range of 260°C to 330°C. The method for measuring the glass transition temperature of the polyimide of the present invention can be carried out based on the methods described in the Examples below. In addition, values obtained by other measurement devices that are substantially equivalent to the measurement method and can be recognized as technically appropriate by those skilled in the art shall also be included in the physical property values. When the glass transition temperature of the polyimide of the present invention falls within the above range, it has excellent heat resistance and can be used in high-temperature manufacturing processes and application scenarios, which is extremely useful.

[0019] The polyimide of the present invention preferably has a coefficient of thermal expansion (CTE) at 100 to 200°C of 15 ppm / °C to 80 ppm / °C when formed into a polyimide film, more preferably 25 ppm / °C to 80 ppm / °C, still more preferably 30 ppm / °C to 80 ppm / °C, and particularly preferably 40 ppm / °C to 80 ppm / °C. The method for measuring the coefficient of thermal expansion (CTE) of the polyimide of the present invention when formed into a polyimide film can be carried out based on the methods described in the Examples below. In addition, values obtained by other measurement devices that are substantially equivalent to the measurement method and can be recognized as technically appropriate by those skilled in the art shall also be included in the physical property values. The thickness of the polyimide film in the method for measuring the coefficient of thermal expansion (CTE) when formed into a polyimide film is preferably in the range of 10 μm to 75 μm.

[0020] The polyimide of the present invention preferably has a light transmittance of 80% or more at a wavelength of 365 nm in a 0.01 wt% N,N-dimethylacetamide (DMAc) solution. The lower limit of such transmittance is more preferably 85% or more, still more preferably 90% or more, and particularly preferably 93% or more. The upper limit of such transmittance is not limited, as a higher transmittance is more preferable.

[0021] The polyimide of the present invention preferably has a light transmittance of 10% or more at a wavelength of 365 nm in a 0.1 wt% N,N-dimethylacetamide (DMAc) solution. The lower limit of such transmittance is more preferably 20% or more, further preferably 25% or more, and particularly preferably 35% or more. The upper limit of such transmittance is not limited because a higher transmittance is more preferable, but it may be 95% or less, 90% or less, 80% or less, 70% or less, 60% or less, 55% or less, or 50% or less.

[0022] The polyimide of the present invention preferably has a light transmittance of 80% or more at a wavelength of 400 nm in a 0.01 wt% N,N-dimethylacetamide (DMAc) solution. The lower limit of such transmittance is more preferably 85% or more, further preferably 90% or more, and particularly preferably 93% or more. The upper limit of such transmittance is not limited because a higher transmittance is more preferable.

[0023] The polyimide of the present invention preferably has a light transmittance of 80% or more at a wavelength of 400 nm in a 0.1 wt% N,N-dimethylacetamide (DMAc) solution. The lower limit of such transmittance is more preferably 85% or more, further preferably 90% or more, and particularly preferably 93% or more. The upper limit of such transmittance is not limited because a higher transmittance is more preferable, but it may be 99% or less, 98% or less, or 95% or less.

[0024] The method for measuring the light transmittance of the above N,N-dimethylacetamide (DMAc) solution for the polyimide of the present invention can be carried out based on the method described in the Examples below. In addition, values obtained by other measuring devices that are substantially equivalent to the aforementioned measurement method and can be technically recognized as appropriate by those skilled in the art are also included in the physical property values.

[0025] (When having repeating structures other than the repeating structures represented by general formula (1A) and general formula (1)) The polyimide precursor and polyimide of the present invention may have repeating structures other than the repeating structures represented by general formula (1A) and general formula (1), in addition to the repeating structures represented by general formula (1A) and general formula (1). In this case, the content of the repeating structures represented by general formula (1A) and general formula (1) is preferably in the range of 50 mol% or more and 100 mol% or less of the total polyimide precursor and polyimide. The lower limit of such content is preferably 60 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and particularly preferably 100 mol%, i.e., the repeating structures consisting only of the repeating structures represented by general formula (1A) and general formula (1). The repeating structures represented by general formula (1A) and general formula (1) and the repeating structures other than the repeating structures represented by general formula (1A) and general formula (1) may be arranged regularly or may be present randomly in the polyimide. The repeating structures represented by general formula (1A) and general formula (1) may each have only one selected type, or two or more types, but it is preferable to have only one type.

[0026] The polyimide precursor having a repeating structure represented by general formula (1A) of the present invention may include the following repeating structure, but it is preferable that it does not include this repeating structure. In the repeating structure, the dashed line in the benzene ring indicates that it is bonded to either one of the benzene rings. Furthermore, the polyimide having a repeating structure represented by general formula (1) of the present invention may include the following repeating structures, but it is preferable that it does not include such repeating structures.

[0027] <Method for Producing Polyimide of the Present Invention> The method for producing polyimide of the present invention is not particularly limited. As a method for producing polyimide, for example, a compound represented by chemical formula (3a) as an acid dianhydride represented by general formula (3) described later, and a compound represented by chemical formula (4b) as a diamine represented by general formula (4) described later, can be polymerized to obtain a polyimide precursor (polyamic acid) (corresponding to the repeating structure when A in general formula (1A-1) is chemical formula (2b)), and a polyimide precursor can be imidized to produce polyimide (corresponding to the repeating structure when A in general formula (1-1) is chemical formula (2b)). The reaction equation for the method for producing polyimide in this case is shown below.

[0028] (Tetracarboxylic acid dianhydride represented by general formula (3)) A tetracarboxylic acid dianhydride represented by general formula (3) can be used as a raw material for the production of the polyimide of the present invention. (In the formula, R 1 , R 2 This is the same as the definition of general formula (1). Specifically, examples of tetracarboxylic dianhydrides represented by general formula (3) include compounds represented by chemical formulas (3a) to (3c). Among these, compounds represented by chemical formula (3a) or (3b) are preferred, and compounds represented by chemical formula (3a) are particularly preferred. By using two or three tetracarboxylic dianhydride compounds represented by general formula (3), a polyimide precursor having two or more repeating structures selected from those represented by general formula (1A) and a polyimide having two or more repeating structures selected from those represented by general formula (1) can be obtained. Since it is particularly preferable for the polyimide precursor and polyimide of the present invention to have only one repeating structure selected from those represented by general formula (1A) and to have only one repeating structure selected from those represented by general formula (1), it is preferable to use one tetracarboxylic dianhydride compound represented by general formula (3).

[0029] (Tetracarboxylic acid dianhydrides other than the tetracarboxylic acid dianhydride represented by general formula (3)) As a raw material for the production of the polyimide of the present invention, tetracarboxylic acid dianhydrides other than the tetracarboxylic acid dianhydride represented by general formula (3) can be used, as long as they do not interfere with the effects of the present invention. Examples of tetracarboxylic acid dianhydrides that can be used include 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 4,4'-oxydiphthalic acid anhydride, 3,3',4,4'-diphenyl sulfide tetracarboxylic acid dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic acid dianhydride, 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, and 1,3-bis(3,4-dicarboxyphenoxy Cyphenoxy)benzene dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)-3,3'-dimethylbiphenyl dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]ether dianhydride, bis[4-(3,4-dicarboxyphenoxy)phenyl]sulfone dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 1,1-bis[4-(3,4- Dicarboxyphenoxy)phenyl]cyclohexane dianhydride, 1,1-bis[4-(3,4-dicarboxyphenoxy)phenyl]cyclodecane dianhydride, 1,1-bis[4-(3,4-dicarboxyphenoxy)phenyl]-3,3,5-trimethylcyclohexane dianhydride, 9,9-bis[4-(3,4-dicarboxyphenoxy)-3-methylphenyl]fluorene dianhydride, hydroquinone-bis(trimellitate anhydride), resorcinol-bis(trimellitate anhydride) (Trimellitate anhydride), 1,5-dihydroxynaphthalene-bis(trimellitate anhydride), 2,6-dihydroxynaphthalene-bis(trimellitate anhydride), 2,7-dihydroxynaphthalene-bis(trimellitate anhydride), 4,4'-dihydroxybiphenyl-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-dimethylbiphenyl-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3',5,5'-Tetramethylbiphenyl-bis(trimellitate anhydride), 4,4'-Dihydroxy-2,2',3,3',5,5'-Hexamethylbiphenyl-bis(trimellitate anhydride), 4,4'-Dihydroxydiphenyl ether-bis(trimellitate anhydride), 4,4'-Dihydroxydiphenyl sulfide-bis(trimellitate anhydride), 4,4'-Dihydroxydiphenyl sulfone-bis(trimellitate anhydride), 4,4'-Dihydroxybenzophenone-bis(trimellitate anhydride), 1,1'-Bis(4-hydroxyphenyl)ethane-bis(trimellitate anhydride), 2,2'-Bis(4-hydroxyphenyl)propane-bis(trimellitate anhydride), 2,2'-Bis(4-hydroxy-3-methylphenyl)propane-bi Examples include bis(trimellitate anhydride), 1,1'-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane-bis(trimellitate anhydride), 1,1'-bis(4-hydroxyphenyl)cyclodecan-bis(trimellitate anhydride), 9,9'-bis(4-hydroxy-3-methylphenyl)fluorene-bis(trimellitate anhydride), cyclobutane-1,2,3,4-tetracarboxylic dianhydride, 1,3-dimethylcyclobutane-1,2,3,4-tetracarboxylic dianhydride, 1,2,3,4-tetramethylcyclobutane-1,2,3,4-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic dianhydride, and cyclohexane-1,2,4,5-tetracarboxylic dianhydride.

[0030] (Diamine represented by general formula (4)) A diamine represented by general formula (4) can be used as a raw material for the production of the polyimide of the present invention. (In the formula, A is the same as defined in general formula (1).) In general formula (4), A is the same as defined in general formula (1) and represents the divalent group represented by general formula (2). The preferred embodiment of A in general formula (4) is the same as in general formula (1). Specifically, examples of diamines when n in general formula (2) of A in general formula (4) is 0 include 1,4-diaminobenzene (the compound represented by the chemical formula (4a) below), 1,4-diamino-2-methylbenzene, 1,3-diaminobenzene (the compound represented by the chemical formula (4b) below), 1,3-diamino-2-methylbenzene, 1,3-diamino-4-methylbenzene, and 1,3-diamino-5-methylbenzene. Specifically, examples of diamines when n in general formula (2) of A in general formula (4) is 1 include the compounds represented by the chemical formulas (4c) to (4p) below. Among these, compounds represented by chemical formulas (4a) to (4p) are preferred as diamines represented by general formula (4), compounds represented by chemical formulas (4a), (4b), (4c), (4f), (4g), (4h), (4i), (4j), (4k), or (4n) are more preferred, compounds represented by chemical formulas (4a), (4b), (4c), (4f), (4g), (4h), or (4n) are even more preferred, compounds represented by chemical formulas (4a), (4b), (4c), (4f), (4g), or (4h) are even more preferred, and compounds represented by chemical formulas (4a), (4b), (4c), or (4h) are particularly preferred. By using two or more diamines represented by general formula (4), it is possible to obtain a polyimide precursor having two or more repeating structures selected from those represented by general formula (1A) and a polyimide having two or more repeating structures selected from those represented by general formula (1). It is particularly preferable that the polyimide precursor and polyimide of the present invention have only one repeating structure selected from those represented by general formula (1A) and only one repeating structure selected from those represented by general formula (1). Therefore, it is preferable to use one diamine represented by general formula (4).

[0031] (Diamines other than the diamine represented by general formula (4)) As a raw material for producing the polyimide precursor and polyimide of the present invention, at least one diamine other than the diamine represented by general formula (4) can be used, as long as it does not hinder the effects of the present invention. More specifically, it is preferable to use at least one diamine selected from aromatic diamines containing at least one aromatic group selected from a phenylene group, a naphthylene group, and a biphenylene group in its structure, and aliphatic diamines having a total number of carbon atoms in the range of 1 to 40, and containing or not containing elements from the group consisting of oxygen, sulfur, silicon, and nitrogen in its structure. When such diamines are used, it is possible to produce polyimide precursors and polyimides that include repeating structures of polyimide precursors other than the repeating structure represented by general formula (1A), and repeating structures of polyimides other than the repeating structure represented by general formula (1).Aromatic diamines other than those represented by the general formula (4) that can be used are not particularly limited, but aromatic diamines containing at least one aromatic group selected from a phenylene group, a naphthylene group, and a biphenylene group in their structure are preferred. Specifically, for example, 2,4-diaminotoluene, 2,5-diaminotoluene, 2,4-diaminoxylene, 2,4-diaminodurene, 4,4'-methylenebis(3-ethylaniline), 4,4'-methylenebis(2-ethylaniline), 4,4'-methylenebis(3,5-dimethylaniline), 4,4'-methylene 3,5-diethylaniline, 4,4'-methylenebis(2,6-diethylaniline), 2,4'-diaminodiphenyl ether, 2,2'-diaminodiphenyl ether, 4,4'-diamino-2,2'-bis(trifluoromethyl)diphenyl ether, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzanilide, benzidine, 3,3'-dihydroxybenzidine, 3,3'-dimethoxybenzidine, o-tolidine, 2,2'-bis(trifluoromethyl)benzidine, 1,4-bis (4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(3-aminophenoxy)phenyl)sulfone, bis(4-(4-aminophenoxy)phenyl)sulfone, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, 2,2-bis(4-aminophenoxy) Examples include phenyl)hexafluoropropane, p-terphenylenediamine, 4-aminophenyl-4'-aminobenzoate, 4-amino-2-methylphenyl-4'-aminobenzoate (M-APAB), hydroquinone bis(4-aminobenzoate), methylhydroquinone bis(4-aminobenzoate), methoxyhydroquinone bis(4-aminobenzoate), phenylhydroquinone bis(4-aminobenzoate), bis(4-aminophenyl) terephthalate, and bis(4-amino-2-methylphenyl) terephthalate.Furthermore, bisaminophenols having a hydroxyl group adjacent to the amino group bonded to the aromatic ring of the aromatic diamine may be used. Specific examples of such bisaminophenols include, but are not limited to, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, and 3,3'-diamino-4,4'-dihydroxybiphenyl. Also, bisaminobenzoic acid having a carboxyl group adjacent to the amino group bonded to the aromatic ring of the aromatic diamine may be used. At least one aromatic diamine selected from the aromatic diamines specifically listed above is more preferable. Two or more of these may be used in combination (copolymerization).

[0032] While not particularly limited, aliphatic diamines with a total number of carbon atoms in the range of 1 to 40, and containing or not containing elements from the group consisting of oxygen, sulfur, silicon, and nitrogen in their structure, are preferred. Specifically, for example, trans-1,4-cyclohexanediamine (t-CHDA), cis-1,4-cyclohexanediamine, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(3-methylcyclohexylamine), 4,4'-methylenebis(3-ethylcyclohexylamine), 4,4'-methylenebis(3,5-dimethylcyclohexylamine), 4,4'-methylenebis(3,5-diethylcyclohexylamine), isophoronediamine, 1,4-cyclohexanebis(methylamine), 2, Examples include 5-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 3,8-bis(aminomethyl)tricyclo[5.2.1.0]decane, 1,3-diaminoadamantane, 2,2-bis(4-aminocyclohexyl)propane, 2,2-bis(4-aminocyclohexyl)hexafluoropropane, 1,3-propanediamine, 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonameethylenediamine, dimeramine, and siloxane-containing diamines, with at least one aliphatic diamine selected from these being more preferred. Two or more of these may be used in combination (copolymerized). Furthermore, these aliphatic diamines may be used in combination with the aforementioned aromatic diamines. Dimer amines are diamine compounds obtained by substituting the two terminal carboxyl groups of a dimer acid with aminomethyl groups or amino groups. Industrially obtained dimer acids may contain arbitrary amounts of monomeric acids with 18 carbon atoms, trimer acids with 54 carbon atoms, and other polymerized fatty acids with 20 to 54 carbon atoms, depending on the degree of purification.

[0033] (Step to obtain polyimide precursor (polyamic acid)) In the step to obtain the polyimide precursor (polyamic acid) of the present invention, specifically, for example, it can be synthesized by first dissolving a diamine in a polymerization solvent and then gradually adding a tetracarboxylic dianhydride to this solution. The amount of tetracarboxylic dianhydride used is usually in the range of 0.8 to 1.2 molar times, preferably 0.9 to 1.2 molar times, more preferably 0.95 to 1.1 molar times, and even more preferably 1.0 to 1.1 molar times, relative to the diamine. The solution is usually stirred using a mechanical stirrer or the like at a temperature usually in the range of 0 to 100°C, preferably 20 to 60°C, for usually 0.5 to 150 hours, preferably 1 to 72 hours. At this time, the monomer concentration is usually in the range of 5 to 50% by weight, preferably 10 to 40% by weight. By carrying out polymerization within this monomer concentration range, a uniform polyimide precursor (polyamic acid) with a high degree of polymerization can be obtained. If the degree of polymerization of the polyimide precursor (polyamic acid) increases too much, making the polymerization solution difficult to stir, it can be diluted with the same solvent as appropriate. By performing polymerization within the above monomer concentration range, a sufficiently high degree of polymerization of the polymer can be achieved, and sufficient solubility of the monomer and polymer can be ensured. If polymerization is performed at a concentration lower than the above range, the degree of polymerization of the polyimide precursor (polyamic acid) may not be sufficiently high, and if polymerization is performed at a concentration higher than the above monomer concentration range, the solubility of the monomer and the resulting polymer may be insufficient.

[0034] Any solvent can be used for polymerization of polyimide precursors (polyamic acid) as long as it dissolves the raw material monomers (tetracarboxylic dianhydride and diamine), the resulting polyimide precursor (polyamic acid), and the imidized polyimide. The structure and type of the solvent are not particularly limited. For example, glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, and sulfoxide-based organic solvents are suitable, and at least one organic solvent selected from these can be used. Among these, at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, ketone-based organic solvents, and amide-based organic solvents is more preferred, and at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, and ketone-based organic solvents is even more preferred.Preferred specific organic solvents include glycol-based organic solvents such as propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), 3-methoxy-n-butyl acetate, diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, triethylene glycol, triethylene glycol dimethyl ether (Tri-GL), ethyl cellosolve (ethylene glycol monoethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), 2-methyl cellosolve acetate, ethyl cellosolve acetate, and butyl cellosolve acetate; and ester-based organic solvents such as ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, and milk. Examples of organic solvents include methyl acid and ethyl lactate, amide-based organic solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone, ketone-based organic solvents such as cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone and methyl isobutyl ketone, lactone-based organic solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone and α-methyl-γ-butyrolactone, carbonate-based organic solvents such as ethylene carbonate and propylene carbonate, ether-based organic solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, dimethoxyethane, diethoxyethane and dibutyl ether, and sulfoxide-based organic solvents such as dimethyl sulfoxide.Among these, at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol, triethylene glycol dimethyl ether (Tri-GL), ethyl cellosolve (ethylene glycol monoethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone, and methyl isobutyl ketone. Preferably, at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, n-butyl acetate, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, methyl ethyl ketone, and methyl isobutyl ketone is preferred, at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, N,N-dimethylformamide, and cyclohexanone is even more preferred, and at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, and cyclohexanone is particularly preferred. Two or more of these solvents may be used in mixture form. The polymerization reaction to obtain the polyimide precursor (polyamic acid) can be carried out in air or in an inert gas such as nitrogen, and it is preferable to carry it out in an inert gas such as nitrogen.

[0035] In addition, in the production of polyimide precursors by this method, an alcohol component having a terminal olefinic group may be added in addition to the aforementioned diamine component and tetracarboxylic dianhydride component in order to convert the polyimide precursor into an ester derivative having a terminal olefinic group. Examples of alcohol components having a terminal olefinic group include 2-acryloyloxyethyl alcohol, 1-acryloyloxy-3-propyl alcohol, 2-acrylamidoethyl alcohol, methylol vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, and 2-hydroxy-3-t-butoxypropyl acrylate. Examples include 2-hydroxy-3-cyclohexyloxypropyl acrylate, 2-methacryloyloxyethyl alcohol, 1-methacryloyloxy-3-propyl alcohol, 2-methacrylamidoethyl alcohol, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-phenoxypropyl methacrylate, 2-hydroxy-3-t-butoxypropyl methacrylate, and 2-hydroxy-3-cyclohexyloxypropyl methacrylate.

[0036] <Varnish of Polyimide Precursors> A polyimide precursor (polyamic acid) can be used to make a varnish containing the polyimide precursor (polyamic acid) and an organic solvent. The organic solvent used to dissolve the polyimide precursor (polyamic acid) can be appropriately selected according to the intended use and processing conditions of the varnish, and is not particularly limited. For example, glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, sulfoxide-based organic solvents, and alcohol-based organic solvents are suitable, and at least one organic solvent selected from these can be used. Among these, at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, ketone-based organic solvents, and amide-based organic solvents is more preferred, and at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, and ketone-based organic solvents is even more preferred.Preferred specific organic solvents include, as glycol-based organic solvents, propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), 3-methoxy-n-butyl acetate, diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, triethylene glycol, triethylene glycol dimethyl ether (Tri-GL), ethyl cellosolve (ethylene glycol monoethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), 2-methyl cellosolve acetate, ethyl cellosolve acetate and butyl cellosolve acetate; as ester-based organic solvents, ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate and ethyl lactate; and as amide-based organic solvents, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-propyl Roridone and N-ethyl-2-pyrrolidone; as ketone organic solvents, cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone and methyl isobutyl ketone; as lactone organic solvents, γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone and α-methyl-γ-butyrolactone; as carbonate organic solvents, ethylene carbonate and propylene carbonate; as ether organic solvents Examples of organic solvents include tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, dimethoxyethane, diethoxyethane, and dibutyl ether, as well as sulfoxide-based organic solvents such as dimethyl sulfoxide, and as alcohol-based organic solvents such as isopropyl alcohol, diacetone alcohol, methyl isobutylcarbinol (4-methyl-2-pentanol), butyl alcohol, isobutyl alcohol, pentanol, 3-methyl-2-butanol, and 3-methyl-3-methoxybutanol.Among these, at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol, triethylene glycol dimethyl ether (Tri-GL), ethyl cellosolve (ethylene glycol monoethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone, and methyl isobutyl ketone. Preferably, at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, n-butyl acetate, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, methyl ethyl ketone, and methyl isobutyl ketone is preferred, more preferably at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, N,N-dimethylformamide, and cyclohexanone is preferred, and particularly preferred at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, and cyclohexanone is preferred. Two or more of these solvents may be used in mixture form.

[0037] When a polyimide precursor (polyamic acid) is dissolved in an organic solvent to form a varnish, the solid content concentration can be appropriately selected according to the application of the varnish and is not particularly limited. For example, when forming a thin film, although it depends on the molecular weight of the polyimide, the manufacturing method, and the thickness of the thin film to be manufactured, it is preferable to have a solid content concentration of 5% by weight or more. If the solid content concentration is too low, it becomes difficult to form a thin film of sufficient thickness, and conversely, if the solid content concentration is too high, the solution viscosity may be too high, making coating difficult. Methods for preparing a varnish containing a polyimide precursor (polyamic acid) and an organic solvent include, for example, preparing the polyimide precursor (polyamic acid) by polymerization reaction as described above, or mixing a polyimide precursor (polyamic acid) that has been polymerized and isolated in advance with the above solvent and dissolving it in air or an inert gas such as nitrogen at a temperature range from room temperature to below the boiling point of the solvent for 1 to 48 hours. Furthermore, the varnish containing the polyimide precursor (polyamic acid) may contain additives such as mold release agents, fillers, silane coupling agents, crosslinking agents, end encapsulants, antioxidants, defoaming agents, leveling agents, thermal polymerization initiators, photopolymerization initiators, sensitizers, and surfactants as needed. The resulting varnish can be used, for example, to produce polyimide in the form of thin films or tapes. The varnish can also be used to produce processed polyimide products such as polyimide thin films and laminates. As a manufacturing method, for example, the polyimide precursor (polyamic acid) varnish can be cast onto a support such as a glass substrate using a doctor blade, and a polyimide thin film can be formed by imidization using a "thermal imidization method" of the polyimide precursor (polyamic acid) described later, using a hot air dryer, infrared drying oven, vacuum dryer, inert oven, etc.

[0038] <Step of imidizing the polyimide precursor> The method for imidizing the obtained polyimide precursor (polyamic acid) will be described below. Known imidizing methods can be applied, for example, the "thermal imidizing method" which thermally cyclizes the polyimide precursor (polyamic acid) film, the "solution thermal imidizing method" which cyclizes the polyimide precursor (polyamic acid) solution at high temperature, and the "chemical imidizing method" which uses a dehydrating agent can be applied as appropriate. In order to produce the polyimide of the present invention, since the polyimide of the present invention has excellent solubility in organic solvents, among these, the imidizing method by the "solution thermal imidizing method" or the "chemical imidizing method" is preferred, and the "chemical imidizing method" is more preferred.

[0039] Specifically, in the "thermal imidation method," a polyimide precursor (polyamic acid) solution is coated onto a substrate or the like, and dried at 50 to 200°C, preferably 60 to 150°C, to form a polyimide precursor (polyamic acid) film. Then, the film is heated under an inert gas or reduced pressure at 150 to 400°C, preferably 200 to 350°C, for 1 to 12 hours to thermally dehydrate and cyclize the film, thereby completing the imidation process and obtaining the polyimide of the present invention. In this way, a thin film of the polyimide of the present invention can be obtained.

[0040] In the "solution thermal imidation method," by adding a basic catalyst as needed, the polyimide precursor (polyamic acid) solution obtained by polymerization in the step of obtaining the polyamic acid is heated for 0.5 to 12 hours at a temperature of 100 to 250°C, preferably 150 to 220°C, in the presence of an azeotrope such as xylene or toluene, either in parallel with the polymerization reaction of the polyimide precursor (polyamic acid), to complete the imidation while removing the by-product water from the system, thereby obtaining the polyimide solution of the present invention.

[0041] In the "chemical imidation method," a polyimide precursor (polyamic acid) solution, adjusted to a suitable viscosity for easy stirring, is mixed with an organic acid anhydride and a dehydrating cyclizing agent (chemical imidizing agent) consisting of amines as a basic catalyst, while stirring with a mechanical stirrer or the like. The mixture is typically stirred at 0 to 100°C, preferably 10 to 50°C, for 1 to 72 hours to complete the chemical imidation. The organic acid anhydride that can be used is not particularly limited, but examples include acetic anhydride and propionic anhydride. Acetic anhydride is preferably used due to the ease of handling and purification of the reagent. As a basic catalyst, pyridine, triethylamine, quinoline, etc., can be used, and pyridine is preferably used due to the ease of handling and separation of the reagent, but is not limited to these. The amount of organic acid anhydride in the chemical imidizing agent is preferably in the range of 1 to 10 times the theoretical dehydration amount of the polyimide precursor (polyamic acid), and more preferably in the range of 1 to 5 times the molar amount. Furthermore, the amount of basic catalyst is preferably in the range of 0.1 to 2 times the amount of organic acid anhydride, and more preferably in the range of 0.1 to 1 time the amount of organic acid anhydride.

[0042] In the "solution thermal imidation method" and the "chemical imidation method," catalysts, chemical imidizing agents, and by-products such as carboxylic acids (hereinafter referred to as impurities) are mixed into the reaction solution, so these may be removed and the solution purified. Known methods can be used for purification. For example, the simplest method is to drop the imidized reaction solution into a large amount of poor solvent under stirring to precipitate polyimide, then recover the polyimide powder and wash it repeatedly until the impurities are removed. In this case, suitable solvents that can be used are alcohols such as water, methanol, ethanol, and isopropanol, which precipitate polyimide, efficiently remove impurities, and dry easily, and these may be used in mixtures. If the concentration of the polyimide solution when precipitation is performed by dropwise addition to the poor solvent is too high, the precipitated polyimide will form granular clumps, and there is a possibility that impurities will remain in these coarse particles, and it may take a long time to dissolve the obtained polyimide powder in the solvent. On the other hand, if the concentration of the polyimide solution is too low, a large amount of poor solvent will be required, which is undesirable as it increases the environmental burden due to waste solvent treatment and increases manufacturing costs. Therefore, the upper limit of the concentration range of the polyimide solution when it is dropped into the poor solvent is preferably 20% by weight or less, more preferably 10% by weight or less, and the lower limit of this concentration range is preferably 1% by weight or more. The amount of poor solvent used at this time is preferably equal to or greater than the amount of the polyimide solution. The obtained polyimide powder is recovered, and the residual solvent is removed by vacuum drying or hot air drying to obtain polyimide. There are no restrictions on the drying temperature and time as long as the temperature does not alter the polyimide and the residual solvent does not decompose, but it is preferable to dry it in a temperature range of 30 to 200°C for 48 hours or less.

[0043] (Polyimide Varnish of the Present Invention) The polyimide of the present invention obtained by the above method can be dissolved in an organic solvent to form a varnish containing polyimide and an organic solvent. The organic solvent used to dissolve the polyimide can be appropriately selected according to the intended use and processing conditions of the varnish, and is not particularly limited, but suitable examples include glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, sulfoxide-based organic solvents, and alcohol-based organic solvents, and at least one organic solvent selected from these can be used. Among these, at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, ketone-based organic solvents, and amide-based organic solvents is more preferred, and at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, and ketone-based organic solvents is even more preferred.Preferred specific organic solvents include, as glycol-based organic solvents, propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol, triethylene glycol dimethyl ether (Tri-GL), ethyl cellosolve (ethylene glycol monoethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), 2-methyl cellosolve acetate, ethyl cellosolve acetate and butyl cellosolve acetate; as ester-based organic solvents, ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate and ethyl lactate; and as amide-based organic solvents, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone. Examples of ketone organic solvents include cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone, and methyl isobutyl ketone; examples of lactone organic solvents include γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, and α-methyl-γ-butyrolactone; examples of carbonate organic solvents include ethylene carbonate and propylene carbonate; examples of ether organic solvents include tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, dimethoxyethane, diethoxyethane, and dibutyl ether; examples of sulfoxide organic solvents include dimethyl sulfoxide; and examples of alcohol organic solvents include isopropyl alcohol, diacetone alcohol, methyl isobutylcarbinol (4-methyl-2-pentanol), butyl alcohol, isobutyl alcohol, pentanol, 3-methyl-2-butanol, and 3-methyl-3-methoxybutanol.Among these, at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol, triethylene glycol dimethyl ether (Tri-GL), ethyl cellosolve (ethylene glycol monoethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone, and methyl isobutyl ketone. A suitable organic solvent is preferred, more preferably at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), 1-methoxy-2-propanol (PGME), diethylene glycol dimethyl ether, triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, n-butyl acetate, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, cyclopentanone, cyclohexanone, methyl ethyl ketone, and methyl isobutyl ketone. A more preferable organic solvent is at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, N,N-dimethylformamide, and cyclohexanone. A particularly preferable organic solvent is at least one organic solvent selected from propylene glycol methyl ether acetate (PGMEA), triethylene glycol dimethyl ether (Tri-GL), ethyl acetate, and cyclohexanone.From the viewpoint of coatability, the organic solvent content in polyimide varnish is preferably in the range of 5 to 60% by weight of polyimide relative to the total weight of polyimide and organic solvent, more preferably in the range of 5 to 50% by weight, and particularly preferably in the range of 10 to 40% by weight. The organic solvent content should be adjusted according to the desired thickness of the coating film and the application method, taking into account the solubility of polyimide. Two or more types of organic solvents may be used in mixture form. When two or more types of organic solvents are mixed, it is preferable that their total content is within the above range.

[0044] The polyimide varnish of the present invention preferably has a transmittance of 80% or more at a wavelength of 365 nm in a 0.01% by weight solution. The lower limit of this transmittance is more preferably 85% or more, even more preferably 90% or more, and particularly preferably 93% or more. There is no upper limit to this transmittance, as higher transmittance is preferable. The polyimide varnish of the present invention preferably has the above transmittance within this range when the organic solvent used is N,N-dimethylacetamide (DMAc).

[0045] The polyimide varnish of the present invention preferably has a transmittance of 10% or more at a wavelength of 365 nm in a 0.1% by weight solution. The lower limit of this transmittance is more preferably 20% or more, even more preferably 25% or more, and particularly preferably 35% or more. The upper limit of this transmittance is not limited as higher transmittance is preferable, but it may be 95% or less, 90% or less, 80% or less, 70% or less, 60% or less, 55% or less, or 50% or less. The polyimide varnish of the present invention preferably has the above transmittance within this range when the organic solvent used is N,N-dimethylacetamide (DMAc).

[0046] The polyimide varnish of the present invention preferably has a transmittance of 80% or more at a wavelength of 400 nm in a 0.01% by weight solution. The lower limit of this transmittance is more preferably 85% or more, even more preferably 90% or more, and particularly preferably 93% or more. There is no upper limit to this transmittance, as higher transmittance is preferable. The polyimide varnish of the present invention preferably has the above transmittance within this range when the organic solvent used is N,N-dimethylacetamide (DMAc).

[0047] The polyimide varnish of the present invention preferably has a transmittance of 80% or more at a wavelength of 400 nm in a 0.1% by weight solution. The lower limit of this transmittance is more preferably 85% or more, even more preferably 90% or more, and particularly preferably 93% or more. The upper limit of this transmittance is not limited, as a higher transmittance is preferable, but it may be 99% or less, 98% or less, or 95% or less. The polyimide varnish of the present invention preferably has the above transmittance within this range when the organic solvent used is N,N-dimethylacetamide (DMAc).

[0048] Furthermore, the method for measuring the light transmittance of the polyimide varnish of the present invention can be measured based on the method described in the examples below. In addition, values ​​obtained by other measuring devices that are substantially equivalent to the said measurement method and that a person skilled in the art would recognize as technically appropriate are also included in the said physical property values.

[0049] The polyimide of the present invention is extremely useful because its excellent solubility in organic solvents allows it to be applied to a wide range of polyimide uses and processing conditions. Furthermore, the varnish obtained by dissolving the polyimide of the present invention has lower viscosity compared to conventionally known polyimides, resulting in excellent handling and processability even when other resin components, additives, or fillers are added, allowing it to be applied to a wide range of uses and processing conditions.

[0050] <Molded articles of the polyimide of the present invention> Various processed articles listed below can be manufactured using the polyimide of the present invention. The polyimide of the present invention can be used to manufacture molded articles such as thin films, sheets, tapes, containers, threads, lenses, tubes, pellets, and foams. Furthermore, the polyimide of the present invention can be used as a resin material for electronic devices and electronic device components used therein, as well as for mechanical parts (e.g., impellers, fan gears, gears, bearings, motor parts, cases), automotive parts (e.g., automotive mechanism parts, engine parts, engine compartment parts, electrical components, interior parts), cooking utensils and utensils, dental instruments, optical instrument parts (e.g., lenses, films), medical device parts and materials, dental device parts and materials, valves, pipes, nozzles, filters, membranes, sporting goods, leisure goods, cable ties, and other articles, and can be molded into these articles.

[0051] (Polyimide film (thin film)) There are no restrictions on the thickness of the polyimide film of the present invention, but it is preferably in the range of 1 μm to 200 μm. More preferably it is in the range of 10 μm to 150 μm, even more preferably in the range of 10 μm to 100 μm, and particularly in the range of 10 μm to 75 μm.

[0052] The glass transition temperature of the polyimide film of the present invention is preferably in the range of 210°C to 350°C, more preferably in the range of 220°C to 350°C, even more preferably in the range of 250°C to 350°C, and particularly preferably in the range of 260°C to 330°C. The glass transition temperature of the polyimide film of the present invention can be measured based on the method of the examples described below. Values ​​obtained by other measuring devices that are substantially equivalent to the said measurement method and that can be recognized as technically appropriate by those skilled in the art are also included in the said physical property values.

[0053] The coefficient of thermal expansion (CTE) of the polyimide film of the present invention is preferably in the range of 15 ppm / °C to 80 ppm / °C, more preferably in the range of 25 ppm / °C to 80 ppm / °C, even more preferably in the range of 30 ppm / °C to 80 ppm / °C, and particularly preferably in the range of 40 ppm / °C to 80 ppm / °C. The method for measuring the coefficient of thermal expansion (CTE) of the polyimide film of the present invention can be measured based on the method of the examples described later. Values ​​obtained by other measuring devices that are substantially equivalent to the said measurement method and that can be recognized as technically appropriate by those skilled in the art are also included in the said physical property values. The film thickness of the polyimide film in the method for measuring the coefficient of thermal expansion (CTE) when it is made into a polyimide film is preferably in the range of 10 μm to 75 μm.

[0054] The polyimide film of the present invention can be characterized by at least one of the transmittances of light at a wavelength of 300 nm, 350 nm, 400 nm, and 450 nm, measured using a spectrochromator / haze meter (COH7700, manufactured by Nippon Denshoku Industries Co., Ltd.) at wavelengths of 400 to 700 nm (at 10 nm intervals). Values ​​obtained by other measuring devices that are substantially equivalent to the said measurement method and that can be recognized as technically appropriate by those skilled in the art are also included in the said physical property values. The total light transmittance of the polyimide film of the present invention is preferably 80% or more, more preferably 85% or more, even more preferably 87% or more, and particularly preferably 88% or more. There is no upper limit to the total light transmittance, as higher transmittance is preferable, but it may be 99% or less, 95% or less, or 92% or less. The transmittance of the polyimide film of the present invention at a wavelength of 400 nm is preferably 10% or more, more preferably 20% or more, even more preferably 30% or more, and particularly preferably 50% or more. There is no upper limit to this transmittance, as higher transmittance is preferable; however, it may be 80% or less, 70% or less, or 65% or less. The transmittance of the polyimide film of the present invention at a wavelength of 450 nm is preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, and particularly preferably 83% or more. There is no upper limit to this transmittance, as higher transmittance is preferable; however, it may be 95% or less, or 90% or less.

[0055] The polyimide film of the present invention can be characterized by at least one selected from the transmittance at a wavelength of 400 nm and the transmittance at a wavelength of 450 nm, measured using an ultraviolet-visible-near-infrared spectrophotometer (Shimadzu Corporation UV-3600) equipped with an integrating sphere, using wavelengths from 185 nm to 600 nm (1 nm intervals). Values ​​obtained by other measuring devices that are substantially equivalent to the said measurement method and that can be recognized as technically appropriate by those skilled in the art are also included in the said physical property values. The transmittance at a wavelength of 400 nm of the polyimide film of the present invention is preferably 10% or more, more preferably 20% or more, even more preferably 30% or more, and particularly preferably 50% or more. There is no upper limit to such transmittance, as higher transmittance is preferable, but it may be 80% or less, 70% or less, or 65% or less. The transmittance of the polyimide film of the present invention at a wavelength of 450 nm is preferably 70% or more, more preferably 75% or more, even more preferably 80% or more, and particularly preferably 83% or more. There is no upper limit to such transmittance, as higher transmittance is preferable, but it may be 95% or less, or 90% or less.

[0056] (Electronic Devices) In the present invention, electronic devices and electronic devices used therein are collectively referred to as electronic devices. Specifically, examples of electronic devices include mobile phones, smartphones, personal computers, mobile routers, data center communication equipment, base stations, radar, robots, drones, wearable computers, measuring and testing equipment used in various industries such as automobiles, aircraft, manufacturing, agriculture, logistics, and civil engineering, high-speed wireless communication equipment, electronic organizers, digital still cameras, video cameras, electronic paper, televisions, players, various audio equipment, in-vehicle displays such as car navigation systems and instrument panels, calculators, printers, scanners, copiers, refrigerators, and washing machines. Specifically, examples of electronic devices include semiconductors, electronic displays, and electrical and electronic components. Examples of electrical and electronic components include capacitors, printed circuits, connectors, various sensors, inductors, switches, and housings. From the viewpoint of processability, the materials used in these electronic devices are required to be soluble in organic solvents, and depending on the application, they are also required to have heat resistance or optical transparency.More specifically, the polyimide of the present invention is used for materials such as passivation films, buffer coat films, and interlayer insulating films in semiconductor devices, as well as photosensitive materials, semiconductor packaging materials, semiconductor encapsulants, base films for flexible printed circuit boards, transparent substrates and cover films for display devices (e.g., liquid crystal displays, plasma displays, organic EL displays, flexible displays, foldable displays, rollable displays, 3D displays), touch panels, organic EL lighting, and solar cells; and materials for optical films (e.g., conductive Examples of suitable applications include optical plates, polarizing plates, polarizing plate protective films, phase difference films, light diffusion films, viewing angle expansion films, reflective films, anti-reflective films, anti-glare films, brightness enhancement films, prism sheets, and light guide films), insulating materials for electronic components, materials for wiring boards such as flexible printed circuit boards and metal-clad laminates, light-emitting materials for organic EL devices, materials for optical sensors, materials for optical radar, materials for 3D displays, adhesive layers, cover films, thin-film adhesives, rigid substrates, carrier tapes for TABs, antenna element components, copper-clad laminates, filters, substrate exterior materials, liquid crystal alignment films, and structural components. Among these, materials such as passivation films, buffer coat films, and interlayer insulating films in semiconductor devices, as well as photosensitive materials, semiconductor packaging materials, semiconductor encapsulants, base films for flexible printed circuit boards, adhesive layers, cover films, thin-film adhesives, copper-clad laminates, rigid substrates, TAB carrier tapes, antenna element members, or filter substrate exterior materials are more preferably used. Materials such as passivation films, buffer coat films, and interlayer insulating films in semiconductor devices, as well as photosensitive materials, base films for flexible printed circuit boards, adhesive layers, cover films, thin-film adhesives, and copper-clad laminates are even more preferably used. Materials such as passivation films, buffer coat films, and interlayer insulating films in semiconductor devices, as well as photosensitive materials, semiconductor packaging materials, semiconductor encapsulants, base films for flexible printed circuit boards, cover films, and copper-clad laminates are particularly preferably used.

[0057] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The analytical method in the present invention is as follows: <Analytical Method> 1. Measurement of the solubility of polyimide Approximately 0.1 g of the obtained polyimide powder was added to 1.0 g of each solvent listed in Table 3, which had been dehydrated by molecular sieving (moisture content less than 100 ppm), and stirred with a mechanical stirrer and left overnight. The dissolution state of the polyimide powder was observed visually. If it was completely dissolved, additional powder was added as needed, and the upper limit amount at which dissolution was observed was recorded. At this time, even if the shape of the powder was lost, if the liquid was cloudy, it was considered that it had not dissolved. In addition, no heating was performed during the observation, and it was confirmed at room temperature. In the measurement results, if the upper limit amount at which dissolution was observed was found, that value was recorded; if the measurement was not continued until it was observed that it was not dissolved, the value at which it was last added plus "or more" was recorded; and if it was observed that it was not dissolved on the first addition of polyimide powder to the solvent, that value plus "less" was recorded.

[0058] 2. Measurement of Glass Transition Temperature (Tg) and Coefficient of Thermal Expansion (CTE) of Polyimide The polyimide films prepared in the examples and comparative examples were measured using the following apparatus, and the Tg of the film and the CTE at 100-200°C were determined from the TMA curve obtained under the following measurement conditions. Apparatus: TMA 7100 (manufactured by Hitachi High-Tech Science Co., Ltd.) [Measurement Conditions] Condition: Load 49 mN Temperature range: 30°C to 350°C Heating rate: 10°C / min. Measurement mode: Tensile

[0059] 3. Measurement of UV-Visible Light Transmittance of Raw Material Monomers A 1% by weight dimethyl sulfoxide solution of the raw material monomer was prepared, and the transmittance at wavelengths of 200 to 800 nm was measured using a UV-Vis spectrophotometer.

[0060] 4. Measurement of UV-Vis light transmittance of polyimide varnish Polyimide powder was dissolved in dimethyl sulfoxide to prepare varnish of a predetermined concentration, and the transmittance at wavelengths of 200 to 800 nm was measured using a UV-Vis spectrophotometer.

[0061] 5. Measurement of UV-Visible Light Transmittance of Polyimide Film (1) The transmittance and total light transmittance of the polyimide film were measured using a spectrochromator and haze meter (COH7700, manufactured by Nippon Denshoku Industries Ltd.) at wavelengths of 400 to 700 nm (10 nm intervals). (2) The transmittance of the polyimide film was measured using an ultraviolet, visible, and near-infrared spectrophotometer (UV-3600, manufactured by Shimadzu Corporation) equipped with an integrating sphere at wavelengths of 185 nm to 600 nm (1 nm intervals).

[0062] <Synthesis of Polyimide, Preparation of its Varnish, and Production of Film> The components used in the synthesis of polyimide, preparation of its varnish, and production of film are shown below. [Tetracarboxylic acid dianhydride] Compound (3a): Compound represented by chemical formula (3a) Compound (A): Compound represented by chemical formula (A) Compound (B): Compound represented by chemical formula (B) [Diamines] m-PDA: Compound represented by chemical formula (4b) 4,4'-MDA: Compound represented by chemical formula (4c) 4,4'-DAS: Compound represented by chemical formula (4h) TFMB: Compound represented by chemical formula (C) MED-J: Compound represented by chemical formula (D) [Organic solvents] <Glycol-based organic solvents> PGMEA: Propylene glycol methyl ether acetate Tri-GL: Triethylene glycol dimethyl ether <Amide-based organic solvents> DMAc: N,N-dimethylacetamide <Ester-based organic solvents> Ethyl acetate <Ketone-based organic solvents> CPN: Cyclopentanone

[0063] (Evaluation of UV-Visible Light Transmittance of Polyimide Raw Material Monomers) The tetracarboxylic dianhydrides (3a) and (A), and the diamines (m-PDA, 4,4'-MDA, 4,4'-DAS, and TFMB) were evaluated by measuring their UV-Visible light transmittance using the measurement method described above. The transmittance spectra of the tetracarboxylic dianhydrides are shown in Figure 1, and the transmittance spectra of the diamines are shown in Figure 2. The transmittance values ​​for each monomer at wavelengths of 365 nm and 400 nm are shown in Table 1.

[0064]

[0065] It was found that compound (3a) does not have high light transmittance at wavelengths of 365 nm and 400 nm, and that it hardly transmits light at a wavelength of 365 nm.

[0066] <Example 1> 5 mmol of m-PDA (compound represented by chemical formula (4b)) was dissolved in dehydrated N,N-dimethylacetamide (DMAc). Next, 5 mmol of the compound represented by chemical formula (3a) was added to this solution. Polymerization was carried out using a stirring bar for 48 hours, and then DMAc was added to dilute the solution to a solid content of 5% by weight. After uniform dilution, 50 mmol of acetic anhydride and 25 mmol of pyridine were added, and the reaction was carried out for a further 24 hours. When the obtained polyimide solution was added dropwise to 10 times the weight of methanol, powder precipitated immediately. The precipitated powder was filtered off, washed with methanol at room temperature, and then dried under reduced pressure (less than 1 kPa) at 60°C. The solubility of the dried powder in various solvents was measured using the analytical method described above. The dried powder was dissolved in DMAc solvent to prepare a polyimide varnish. This varnish was cast onto a glass plate and dried under reduced pressure (less than 1 kPa) at 250°C for 1 hour to obtain a polyimide film. Polyimide films with different film thicknesses were prepared. The obtained polyimide films were used for thermal property analysis using the analytical method described above.

[0067] <Examples 2, 3 and Comparative Examples 1-6> Polyimide powders and polyimide films were prepared in the same manner as in Example 1, except that the tetracarboxylic dianhydride and diamine used in Example 1 were replaced with the compounds listed in Table 2, and various analyses were performed.

[0068]

[0069] <Evaluation of Solubility in Organic Solubility and Thermal Properties of Polyimides> The solubility in organic solvents and thermal properties were evaluated using the above method with respect to the polyimides obtained in Examples 1-3 and Comparative Examples 1-6. The results are shown in Table 3.

[0070] The polyimide of Comparative Example 1 has good solubility in glycol-based, amide-based, ester-based, and ketone-based organic solvents, but it is a polyimide that uses a monomer containing a fluorine atom, raising concerns about environmental impact and health risks. The polyimide of Example 1 is a polyimide that uses compound (3a) as the tetracarboxylic dianhydride and m-PDA, an aromatic diamine that does not contain a fluorine atom and has one aromatic ring, as the diamine. Compared to the polyimide of Comparative Example 2, which is a polyimide of the same diamine (m-PDA) and compound (A), a tetracarboxylic dianhydride containing a fluorine atom, the polyimide of Example 1 had equally good organic solvent solubility in ketone-based organic solvents, and superior organic solvent solubility in glycol-based, amide-based, and ester-based organic solvents. Compared to the polyimide of Comparative Example 4, which is a polyimide of the same diamine (m-PDA) and compound (B), a tetracarboxylic dianhydride that does not contain a fluorine atom, it was revealed that the polyimide of Example 1 can dissolve at high concentrations in a variety of organic solvents. The polyimide of Example 1 was found to be highly soluble in a variety of organic solvents at very high concentrations compared to the polyimide of Comparative Example 3, which was obtained using compound (B) and TFMB, a diamine containing a fluorine atom. The polyimide of Comparative Example 5 is a polyimide using compound (3a) as the tetracarboxylic dianhydride and TFMB, a diamine containing a fluorine atom, as the diamine. The polyimide of Example 1 was found to have superior organic solvent solubility compared to the polyimide of Comparative Example 5, despite not containing a fluorine atom. Furthermore, in terms of thermal properties, the polyimide of Example 1 had a Tg of 276.4°C, indicating that it possessed sufficient heat resistance as a polyimide. The polyimides of Examples 2 and 3 are polyimides using compound (3a) as the tetracarboxylic dianhydride and 4,4'-MDA and 4,4'-DAS, aromatic diamines that do not contain a fluorine atom and have two aromatic rings, as the diamine. Similar to Example 1, it was found to have excellent solubility in a variety of organic solvents and excellent heat resistance.The polyimide of Comparative Example 6 is a polyimide that does not contain fluorine atoms in either the tetracarboxylic dianhydride or the diamine. Regarding heat resistance, it was found that its Tg was significantly lower and its CTE value was higher compared to the polyimides of Examples 1-3 and Comparative Examples 1-5, indicating that its heat resistance was inferior. Furthermore, it was found that its organic solvent solubility in glycol-based and ester-based organic solvents was inferior to that of the polyimides of Examples 1-3. From the above, it was found that the polyimide of the present invention is very useful because it has excellent solubility in various organic solvents and excellent heat resistance. In addition, compared to the polyimides of Comparative Examples 1-4, the polyimide solutions of Examples 1-3 were found to have low viscosity and good fluidity even when high-concentration solutions were prepared, as observed during the dropping operation to obtain the polyimide powder, when the varnish was stirred, and when the glass bottle containing the varnish was tilted. The polyimide varnishes of Examples 1-3 are very useful because they have low viscosity and excellent fluidity even at high concentrations.

[0071] <Evaluation of Light Transmittance of Polyimide Varnish> The polyimide varnishes obtained in Example 3 and Comparative Example 5 were evaluated for light transmittance at wavelengths of 365 nm and 400 nm. The results are summarized in Table 4.

[0072] Regarding the light transmittance of polyimide varnish, it was found that while the light transmittance value of the fluorine-free polyimide in Example 3 was slightly lower than that of Comparative Example 5, which is a polyimide containing fluorine atoms, it had a similar level of transmittance.

[0073] <Evaluation of UV-Visible Light Transmittance of Polyimide Films> Using the polyimide films obtained in Examples 1-3 and Comparative Examples 1-6, the UV-Visible light transmittance was measured by the method described in 5. (1) above. Note that TT (%) in Table 5 represents the total light transmittance, T 400 (%), T 450The (%) values ​​represent the light transmittance (%) at wavelengths of 400 nm and 450 nm, respectively. The ultraviolet-visible light transmittance spectra of each polyimide film obtained by this method are shown in Figures 3 to 8. In addition, the ultraviolet-visible light transmittance was measured using the method described in 5. (2) above. Note that the T values ​​in Table 6 are shown below. 300 (%), T 350 (%), T 400 (%) and T 450 The percentages (%) represent the light transmittance (%) at wavelengths of 300 nm, 350 nm, 400 nm, and 450 nm, respectively. The ultraviolet-visible light transmittance spectra of each polyimide film obtained by this method are shown in Figures 9 to 13.

[0074]

[0075]

[0076] In the evaluation of the ultraviolet-visible light transmittance of the raw material monomers, compound (3a) showed lower transmittance at a wavelength of 400 nm compared to the other monomers, and hardly transmitted light at a wavelength of 365 nm. Nevertheless, the total light transmittance of the polyimide films obtained using compound (3a) in Examples 1 to 3 was approximately 90%, which was comparable to that of Comparative Examples 1 to 6. Furthermore, the total light transmittance of general glass and transparent resin films is also approximately 90%, indicating that the transparency was comparable to these. In addition, it was found that the polyimides of Examples 1 and 3 were not significantly inferior to those of Comparative Examples 1 to 6 in terms of transmittance at a wavelength of 400 nm.

Claims

1. A polyimide precursor having one or more repeating structures selected from the repeating structures represented by general formula (1A). (In the formula, R 1 and R 2 Each of the above independently represents either a hydrogen atom or a methyl group, and A represents a divalent group represented by general formula (2). The dashed line within the benzene ring indicates bonding to either one of the benzene rings. (wherein n represents 0, 1, or 2, X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom, or a sulfonyl group, R 3 Each of these independently represents a hydrogen atom or a methyl group, and * indicates the bond position.

2. A polyimide having one or more repeating structures selected from the repeating structures represented by general formula (1). (In the formula, R 1 and R 2 Each of these independently represents either a hydrogen atom or a methyl group, and A represents a divalent group represented by general formula (2). (wherein n represents 0, 1, or 2, X represents a direct bond, a methylene group, an isopropylidene group, an oxygen atom, a carbonyl group, a sulfur atom, or a sulfonyl group, R 3 Each of these independently represents a hydrogen atom or a methyl group, and * indicates the bond position.

3. The polyimide according to claim 2, wherein the glass transition temperature is in the range of 210°C to 350°C.

4. A polyimide precursor varnish comprising the polyimide precursor described in claim 1 and an organic solvent.

5. The polyimide precursor varnish according to claim 4, wherein the organic solvent is at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, sulfoxide-based organic solvents, and alcohol-based organic solvents.

6. The polyimide precursor varnish according to claim 4, comprising 5 to 60% by weight of the polyimide precursor with respect to the total weight of the polyimide precursor and the organic solvent.

7. A polyimide varnish comprising the polyimide and organic solvent according to claim 2.

8. The polyimide varnish according to claim 7, wherein the organic solvent is at least one organic solvent selected from glycol-based organic solvents, ester-based organic solvents, lactone-based organic solvents, amide-based organic solvents, ketone-based organic solvents, carbonate-based organic solvents, ether-based organic solvents, sulfoxide-based organic solvents, and alcohol-based organic solvents.

9. The polyimide varnish according to claim 7, wherein the polyimide is contained in an amount of 5 to 60% by weight relative to the total weight of the polyimide and the organic solvent.

10. A polyimide film comprising the polyimide described in claim 2.