Photoresponsive particle, photoresponsive material, polymerizable composition, wavelength conversion layer, and wavelength conversion element
A shell-shaped ligand with betaine groups and a polymer portion stabilizes perovskite nanocrystals, addressing durability issues and maintaining emission quantum yield under external stimuli.
Patent Information
- Application Number
- PCT/JP2026/017046
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-15
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-19
AI Technical Summary
Perovskite nanocrystals with iodine at the X-site suffer from reduced emission quantum yield due to desorption of halogen from the surface under external stimuli, leading to durability issues.
A shell-shaped ligand with a betaine group and a polymer portion is used to stabilize perovskite-type nanocrystals, comprising units that promote coordination and reduce desorption, enhancing durability.
The solution provides perovskite nanocrystals with high durability and maintained emission quantum yield under external stimuli.
Smart Images

Figure JP2026017046_19112026_PF_FP_ABST
Abstract
Description
Photoresponsive particles, photoresponsive materials, polymerizable compositions, wavelength conversion layers, and wavelength conversion elements
[0001] This disclosure relates to a photoresponsive, polymerizable composition and a wavelength conversion layer that emit light upon irradiation with light.
[0002] Perovskite nanocrystalline particles, which have a perovskite-type crystal structure and an average particle size on the order of nanometers, are expected to be used as light-emitting materials in self-emissive display devices because they exhibit luminescence properties with a narrow full width at half maximum and high color purity. Furthermore, it is known that the emission wavelength of perovskite nanocrystalline particles can be controlled by changing the halogen composition at the X-site.
[0003] On the other hand, in perovskite nanocrystals (nanoparticles), external stimuli such as light, heat, oxygen, and water cause the halogen constituting the X-site to desorb, resulting in a different halogen composition on the particle surface of the nanocrystal compared to the interior of the nanocrystal. In other words, this is known as a phenomenon in which the emission quantum yield of nanoparticles decreases due to external stimuli. This is thought to be due to the fact that perovskite nanocrystals have a small particle size of several to twenty nanometers and a high specific surface area, and that they are composed of ionic crystals and are susceptible to the influence of polar substances. Patent Document 1 discloses a technique for improving the stability of perovskite nanocrystals in polar solvents by modifying the particle surface with a zwitterionic shell-shaped ligand.
[0004] Japanese Patent Publication No. 2023-81338
[0005] When producing photoresponsive materials or light-emitting layers using perovskite-type nanocrystals protected by shell-like ligands as described in Patent Document 1, CsPbBr 3 High durability can be obtained with compositions that do not contain iodine at the X site, such as CsPb(Br x / I 1-x ) 3Compositions containing iodine at the X-site, such as those mentioned above, had room for improvement in durability. This is presumed to be because iodine has a larger atomic radius than bromine, making it easier to desorb from the nanocrystal surface compared to bromine, and thus more prone to generating defects on the nanocrystal surface that differ from those inside the nanocrystal in halogen compositions. When surface defects are generated, the emission quantum yield decreases. In order to take advantage of the characteristics of perovskite-type nanocrystals, which allow for control of the emission wavelength by changing the halogen composition, it was necessary to achieve high durability with compositions containing iodine at the X-site.
[0006] Therefore, the present invention aims to provide photoresponsive particles containing perovskite-type nanocrystals with high durability and containing iodine at the X-site.
[0007] The photoresponsive particles according to an embodiment of the present invention include a nanoparticle having a perovskite-type crystalline structure containing iodine at the X site, and a shell-shaped ligand comprising a plurality of bonding portions including a structural unit having a betaine group, and a polymer portion that coordinates to the nanoparticle at a plurality of locations via the plurality of bonding portions, wherein the shell-shaped ligand comprises a first unit having the betaine group and constituting the bonding portion, a second unit that reduces the rigidity of the polymer portion, and a third unit that increases the rigidity of the polymer portion.
[0008] Furthermore, the photoresponsive particles according to the embodiment of the present invention have a nanoparticle having a perovskite-type crystalline structure containing iodine at the X site, and a shell-shaped ligand comprising a plurality of binding portions including a structural unit having a betaine group, and a polymer portion that coordinates to the nanoparticle at a plurality of locations via the plurality of binding portions, wherein the shell-shaped ligand has a first unit having the betaine group and constituting the binding portion, a second unit constituting the polymer portion and promoting the coordination of the betaine group to the nanoparticle, and a third unit constituting the polymer portion and suppressing the detachment of the betaine group from the nanoparticle.
[0009] Furthermore, the photoresponsive particles according to an embodiment of the present invention comprise: nanoparticles having a perovskite crystal structure containing iodine at the X site; a first shell-like ligand comprising a plurality of first binding moieties each containing a structural unit having a betaine group, and a first polymer moiety bonded to the nanoparticles at a plurality of positions via the plurality of first binding moieties; and a second shell-like ligand comprising a plurality of second binding moieties each containing a structural unit having a betaine group, and a second polymer moiety bonded to the nanoparticles at a plurality of positions via the plurality of second binding moieties. The first polymer moiety has a first main skeleton, and a second side chain branched from the first main skeleton and having 4 or more rotatable bonds, and the second polymer moiety has a second main skeleton, and a third side chain branched from the second main skeleton and having 3 or less rotatable bonds.
[0010] According to the present invention, it is possible to provide photoresponsive particles including perovskite nanocrystals containing iodine at the X site, which have high durability.
[0011] FIG. 2 is a diagram showing a schematic configuration of a photoresponsive material including photoresponsive particles according to a first embodiment. FIG. 3 is a diagram illustrating the number of rotatable bonds RB of a functional group constituting a second unit according to the first embodiment. FIG. 4 is a diagram illustrating the number of rotatable bonds RB of a functional group constituting a third unit according to the first embodiment. FIG. 5 is a diagram showing the influence of the content ratio of the second unit and the third unit according to the first embodiment on the polymer moiety and the photoresponsive material. FIGS. 6(a) and 6(b) are diagrams illustrating the halogen photoinduced desorption reduction effect of the second unit and the third unit according to the first embodiment. FIG. 7 is a diagram showing a schematic configuration of a photoresponsive material including photoresponsive particles according to a second embodiment. FIG. 8 is a diagram showing a schematic configuration of a polymerizable composition and a photoresponsive cured product according to a third embodiment. FIG. 9 is a diagram showing a schematic configuration of a polymerizable composition and a photoresponsive cured product according to a fourth embodiment. FIG. 10 is a diagram showing schematic configurations of a wavelength conversion layer, a wavelength conversion element, and a light-emitting element array according to fifth, sixth, and seventh embodiments.
[0012] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. The dimensions, materials, shapes, relative arrangements, and the like of the constituent members described in these embodiments are not intended to limit the scope of the present invention.
[0013] <First Embodiment> A photoresponsive material 500 according to the first embodiment will be described with reference to FIG. 1.
[0014] The photoresponsive material 500 according to the present embodiment includes nanoparticles 10 having a perovskite crystal structure (ABX 3 ) that contains iodine at the X site. Furthermore, the photoresponsive material 500 has a shell-shaped ligand 60 that includes a plurality of bonding portions 40 each containing a structural unit having a betaine group 45, and a polymer portion 50 that coordinates to the nanoparticles 10 at a plurality of positions via the plurality of bonding portions 40.
[0015] The photoresponsive material 500 includes a fluid medium 90f as a medium 90 interposed between the plurality of photoresponsive particles 100. The subscript f attached to the medium 90 means that the medium 90 is a fluid, that is, has fluidity. Depending on the usage form such as the transport mode of the photoresponsive material 500 and the stage during the manufacturing process, the medium 90 may be in the form of gas, liquid, sol, gel, powder, green compact, or bulk solid, which have different fluidity. The photoresponsive material 500 includes the photoresponsive particles 100 and the medium 90.
[0016] Note that in FIG. 1, the betaine group 45 is indicated by a pair of positive and negative symbols (a pair of + and -). The pair of positive and negative symbols schematically represents the zwitterionic property of the betaine group 45. In addition, the cross section of the nanoparticle 10 is schematically represented as a cubic crystal cross section, and the cross section of the shell-shaped ligand 60 is schematically represented as a shell-shaped outer shell structure that substantially covers the entire outer surface of the nanoparticle 10 when the nanoparticle 10 is regarded as a core.
[0017] (Nanoparticles) For the nanoparticles 10, semiconductor nanocrystals having a perovskite crystal structure with constituent components of A site (monovalent cation), B site (divalent cation), and X site (monovalent anion containing at least iodide anion as a halide anion) are employed. The perovskite crystal structure is also referred to as a perovskite structure, ABX 3 type crystal structure, ABX 3 type structure. Further, A 2 B'B''X 6The double perovskite crystal structure, represented as shown, is also included in the perovskite crystal structure.
[0018] [A site of perovskite crystal structure] The A site of the perovskite crystal structure employs a monovalent cation. The monovalent cation employed at the A site is an ammonium cation (NH₄). 4 + ), and alkylammonium cations having 6 or fewer carbon atoms, formamidinium cations (HC(NH 2 ) 2 + ), guanidinium cation (C(NH 2 ) 3 + Examples include nitrogen-containing organic compound cations such as imidazolium cation, pyridinium cation, and pyrrolidinium cation, and lithium cation (Li + ), sodium cation (Na + ), potassium cation (K + ), rubidium cation (Rb + ), and cesium cations (Cs + Examples include alkali metal cations such as ).
[0019] Because the monovalent cations employed at these A-sites have small ionic diameters and are small enough to fit within the crystal lattice, the perovskite compound can form a stable three-dimensional crystal.
[0020] A preferred example of an alkylammonium cation having 6 or fewer carbon atoms is the methylammonium cation (CH4). 3 NH 3 + ), ethylammonium cation (C 2 H 5 NH 3 + ), propylammonium cation (C 3 H 7 NH 3 + Examples include:
[0021] From the viewpoint of obtaining high luminescence efficiency, it is preferable to use at least one of methylammonium cation, formamidinium cation, or cesium cation as the A site, and from the viewpoint of suppressing color change, it is more preferable to use cesium cation as the A site. Two or more monovalent cations may be used in combination as the A site.
[0022] If the A-site is a cesium cation, cesium salts can be used as raw materials for the synthesis of luminescent nanocrystals, as described later. Such cesium salts may include cesium chloride, cesium bromide, cesium iodide, cesium hydroxide, cesium carbonate, cesium bicarbonate, cesium bicarbonate, cesium formate, cesium acetate, cesium propionate, cesium pivalate, and cesium oxalate, as appropriate. From these candidate cesium salts, an appropriate one can be used depending on the synthesis method.
[0023] If site A is another alkali metal cation, salts of the above-mentioned cesium compound in which the cesium element is replaced with another alkali metal cation element can be used as raw materials.
[0024] If site A is a nitrogen-containing organic compound cation such as a methylammonium cation, then a neutral compound other than a salt, such as methylamine, can be used as a raw material. Two or more of these raw materials may be used in combination.
[0025] [B-site of perovskite crystal structure] The B-site of the perovskite crystal structure employs a divalent cation, including a divalent transition metal cation or a divalent typical metal cation.
[0026] Divalent transition metal cations include scandium cations (Sc 2+ ), titanium cation (Ti 2 +), vanadium cation (V 2+ ), chromium cation (Cr 2+ ), manganese cation (Mn 2+ ), iron cation (Fe 2+ ), cobalt cation (Co 2+ ), nickel cation (Ni 2+ ), copper cation (Cu 2+), palladium cation (Pd 2+ ), Europium cation (Eu 2+ ), ytterbium cation (Yb 2+ ) will be adopted.
[0027] Divalent typical metal cations include magnesium cations (Mg 2+ ), calcium cation (Ca 2+ ), strontium cation (Sr 2+ ), barium cation (Ba 2+ ), zinc cation (Zn 2+ ), cadmium cation (Cd 2+ ), germanium cation (Ge 2+ ), tin cation (Sn 2+ ), lead cation (Pb 2+ ) may be adopted.
[0028] Among these divalent cations, typical metal cations are preferred in terms of the growth of stable three-dimensional crystals, tin cations or lead cations are more preferred, and lead cations are particularly preferred from the viewpoint of obtaining high luminescence intensity. Two or more of these divalent cations may be used in combination, and the perovskite crystal structure may be a so-called double perovskite type.
[0029] When the B site is a lead cation, lead compounds can be used as raw materials for the synthesis of the nanoparticles (luminescent nanocrystals) described later, and an appropriate one can be used depending on the synthesis method. Examples of lead compounds include lead chloride, lead bromide, lead iodide, lead oxide, lead hydroxide, lead sulfide, lead carbonate, lead formate, lead acetate, lead 2-ethylhexanoate, lead oleate, lead stearate, lead naphthenate, lead citrate, lead maleate, and lead acetylacetonate. When the B site is another divalent metal cation, salts of the above-mentioned lead compounds in which the lead element is replaced with another divalent metal cation element can be used as raw materials. Two or more of these raw materials may be used in combination.
[0030] [X-site of perovskite crystal structure] The X-site of the perovskite crystal structure employs monovalent anions including halide anions, and at least iodide anions (I -It contains ) Other halide anions include fluoride anions (F - ), chloride anion (Cl - ), bromide anion (Br - Examples include the following. Among these, chloride anions and bromide anions are preferred from the viewpoint of forming stable three-dimensional crystals and exhibiting strong luminescence in the visible light range. In particular, the inclusion of bromide anions is preferred from the viewpoint of nanoparticle stability.
[0031] Two or more types of halide anions may be used in combination. In particular, when chloride anions, bromide anions, and iodide anions are used in combination, the emission wavelength of the luminescent nanocrystal can be set to a desired wavelength in the visible range depending on the content ratio of the anion species. That is, when chloride anions, bromide anions, and iodide anions are used in combination, it is preferable because an emission spectrum covering almost the entire visible light range from blue to red can be obtained while maintaining a narrow full width at half maximum, depending on the content ratio of the anion species. Here, the emission has a central wavelength of 450 nm to 500 nm for blue, 500 nm to 570 nm for green, and 620 nm to 740 nm for red.
[0032] The X site may contain monovalent anions other than halide anions. Such monovalent anions other than halide anions include cyanide anions (CN - ), thiocyanate anion (SCN - ), isothiocyanate anion (CNS - Examples include pseudohalide anions such as ). As raw materials for the synthesis of nanoparticles (luminescent nanocrystals) described later, appropriate materials can be selected according to the synthesis method from salts with A-site and B-site countercations, such as cesium chloride and lead bromide, or salts with other cations.
[0033] The X-site of the perovskite-type crystal structure, which is composed of halogens, may contain bromine (Br) in addition to iodine (I).
[0034] (Manufacturing Process) The nanoparticles (luminescent nanocrystals) in this embodiment can be manufactured by the following process. The manufacturing method for the nanoparticles 10 may include a hot injection method, in which raw material liquids are mixed at high temperature, and after the formation of fine particles, rapid cooling is performed to obtain a stable product; a flow synthesis method, in which raw material liquids are sent through piping using a pump or the like and mixed; or a ligand-assisted reprecipitation method, in which fine particles are obtained by reprecipitation utilizing the difference in miscibility of the product with the solvent.
[0035] Furthermore, a room-temperature synthesis method is employed in which fine particles are obtained by mixing a mixture of non-halogenated raw materials for site A and site B, which do not contain components for site X, with a separately prepared raw material solution for site X, under mild conditions of room temperature. In addition, a mechanochemical method is employed in which fine product particles are obtained by reacting solid raw materials with mechanical mixing such as milling or ultrasonic treatment, and an in situ synthesis method is employed in which the reactants are obtained by directly growing crystals after coating the raw material solution onto a substrate.
[0036] (Particle Size) The average particle size of the nanoparticles is preferably 1 nm to 30 nm, more preferably 2 nm to 25 nm, and even more preferably 3 nm to 20 nm. If the average particle size is less than 1 nm, stability may be insufficient. If the average particle size is greater than 30 nm, the quantum confinement effect may not work sufficiently, and the quantum emission yield may decrease.
[0037] In this embodiment, the photoresponsive material may be in the form of nanoparticles protected by a shell-like ligand dispersed in a dispersion solvent such as hexane or toluene, or it may be in the form of not containing a dispersion solvent such as hexane or toluene.
[0038] (Shell-shaped ligand) The shell-shaped ligand 60 has a first unit 61 having a betaine group 45 and constituting the bonding portion 40, a second unit 62 that reduces the rigidity of the polymer portion 50, and a third unit 63 that increases the rigidity of the polymer portion 50.
[0039] In this embodiment, the shell-shaped ligand 60 comprises a first unit 61, a second unit 62, and a third unit 63 arranged in parallel with the main skeleton 55. On the other hand, a shell-shaped ligand comprising the second unit 62 and the third unit 63 arranged in parallel with the main skeleton 55, and also comprising the first unit 61 and the second unit 62 in series, is also adopted in embodiments of the present invention. That is, a configuration in which the second unit 62 and the first unit 61 are arranged in series in the section from the main skeleton 55 to the nanoparticles 10 is also included as a variation of this embodiment.
[0040] From the viewpoint of the stability of the nanoparticles 10 in the medium, the weight-average molecular weight of the shell-shaped ligand 60 is preferably 1,000 or more and 50,000 or less, and more preferably 2,000 or more and 30,000 or less. If the polymerization average molecular weight of the shell-shaped ligand is 50,000 or more, the dispersibility in the medium may decrease.
[0041] (First Unit) The betaine group 45 may be referred to as a betaine structure, betaine moiety, etc. The betaine group 45 refers to a structure in which positive and negative charges are located at non-adjacent positions within the same molecule, and the molecule as a whole has no charge. Examples of betaine groups 45 include sulfobetaine, phosphobetaine, carboxybetaine, etc. From the viewpoint of coordination strength (=bonding stability) with respect to nanoparticles 10, sulfobetaine and phosphobetaine are preferably used as the betaine group 45.
[0042] (Second Unit) The second unit 62 may be an alkyl group, a heteroalkyl group, an aryl group, a heteroaryl group, an aralkyl group, a heteroaralkyl group, a carboxylic acid ester group, a carboxylic acid amide group, or an alkoxy group. These may be further substituted. There may be two or more types of second unit 62. From the viewpoint of promoting coordination to the nanoparticle 10, it is preferable that the number of carbon atoms be 4 or more. The alkyl group and heteroalkyl group may be linear, branched, or cyclic.
[0043] (Third Unit) The third unit 63 may be an alkyl group, a linear group, a heteroalkyl group, an aryl group, a heteroaryl group, an aralkyl group, a heteroaralkyl group, a carboxylic acid ester group, a carboxylic acid amide group, or an alkoxy group. These may be further substituted. The alkyl group and heteroalkyl group may be linear, branched, or cyclic.
[0044] The polymer portion 50 constituting the shell-shaped ligand 60 comprises a main chain (55) and side chains (61, 62, 63) as elements of its molecular structure. The main chain 55 includes linear, branched, and cyclic forms, and may be referred to as the main skeleton 55. In this specification, the side chains (61, 62, 63) refer to functional groups having two or more carbon atoms bonded to the main chain 55, and hydrogen atoms and methyl groups are not considered side chains. Hydrogen atoms and methyl groups extending in a direction intersecting the carbon skeleton constituting the main chain 55 are considered to constitute the main skeleton 55.
[0045] Here, the shell-shaped ligand 60 has a first unit 61 having a betaine group 45 and constituting a bonding portion 40, a second unit 62 that reduces the rigidity of the polymer portion 50, and a third unit 63 that increases the rigidity of the polymer portion 50. A characteristic of the photoresponsive particle 100 is that the polymer portion 50 is configured such that the second unit 62 and the third unit 63, which exhibit opposing effects with respect to the polymer portion 50, and the first unit 41 having a betaine group 45 share the main skeleton 55.
[0046] The inventors have found that the structural features of this embodiment effectively reduce the photo-induced desorption problem, in which halogens are desorbed from the crystal surface of the nanoparticles 10 due to external stimuli such as light irradiation. The estimated mechanism for resolving this photo-induced desorption problem will be explained using Figures 1 to 4.
[0047] (Structural control by composition of polymer portion) Here, Figures 2A and 2B illustrate the number of rotatable bonds RB of the functional groups constituting the second and third units according to the first embodiment. Figure 3 illustrates the effect of the content ratio of the second and third units according to the first embodiment on the polymer portion and the photoresponsive material. Figures 4 (a) and (b) illustrate the halogen light-induced desorption reduction effect of the second and third units according to the first embodiment.
[0048] In this embodiment, the photoresponsive particle 100 has three units of polymer portion 50 arranged in parallel along the longitudinal direction of the main skeleton 55, each unit having a different effect on the main skeleton 55.
[0049] The first unit 61 has a betaine group 45 and includes a bonding portion 40. That is, the first unit 61 is an element of the shell-shaped ligand 60 that constitutes the bonding portion 40 that bonds the polymer portion 50 (main skeleton 55) to the nanoparticle 10.
[0050] On the other hand, the second unit 62 has the effect of reducing the rigidity of the polymer portion 50. In this specification, the rigidity of the polymer portion 50 corresponds to the bending rigidity with respect to elastic deformation when the polymer portion 50 is bent in a direction intersecting the direction along the skeleton length of the main skeleton 55. The second unit 62 can be rephrased as a unit containing a functional group having a flexible skeleton that is not easily inhibited by bending of the polymer portion 50. The third unit 63 can be rephrased as a unit containing a functional group having a rigid skeleton that inhibits bending of the polymer portion 50.
[0051] Here, regarding the connections within a unit, we consider the number of rotatable connections RB as an indicator of rotatability.
[0052] For example, when the bond between carbon atoms is a so-called sigma bond composed solely of sp3 bonds, the carbon atoms can rotate around the bond axis. On the other hand, when the bond between carbon atoms is a double or triple bond composed of sp2-sp3 hybrid orbitals, the rotation of the carbon atoms around the bond axis is restricted. Thus, whether the bond between carbon atoms is a single bond, a double bond, or a triple bond affects whether the rotational degree of freedom of one carbon atom is high or low. Furthermore, partial bonds in cyclic structures do not increase the rotational degree of freedom because their rotation is restricted. This is also true for carbon-oxygen bonds, etc. In other words, the cumulative number of single bonds contained in the functional group extending from the main skeleton 55 is an indicator that structurally reflects the degree of deformation freedom of the functional group (the side chain) of interest, and this is treated as the number of rotatable bonds RB. However, bonds with hydrogen atoms and single bonds at the ends of the polymer chain, although rotatable, do not affect the synthesis of the polymer region and are therefore excluded from the cumulative count of the number of rotatable bonds (RB).
[0053] The shell-shaped ligand 60 is configured such that a second unit that reduces the bending rigidity of the polymer portion 50, a third unit that increases the bending rigidity of the polymer portion 50, and a first unit that constitutes a bonding portion 40 between the polymer portion 50 and the nanocrystal 10 are arranged in parallel to form the main framework 55. In other words, the shell-shaped ligand 60 has a structure in which the second unit that reduces the bending rigidity of the polymer portion 50, the third unit that increases the bending rigidity of the polymer portion 50, and the first unit that constitutes a bonding portion 40 between the polymer portion 50 and the nanocrystal 10 are made of copolymer.
[0054] Figure 2A illustrates (n) hexyl methacrylate (n-HMA) and 2-ethylhexyl methacrylate (EHMA), which have a high rotatable bond count RB and constitute the second unit 62, respectively. Figure 2B illustrates isobonyl methacrylate (IBMA) and ethyl methacrylate (EMA), which have a low rotatable bond count RB and constitute the third unit 63, respectively. In the figures, the symbol ○ is added to rotatable carbon-carbon bonds, overlapping with the "-" symbol indicating interatomic bonds. Note that the functional groups shown in Figures 2A and 2B each contain an ester bond -C0- at the site of attachment to the main skeleton. Such an ester bond contains two rotatable bonds.
[0055] For chemically synthesized polymers like the shell-shaped ligand 60, identifying their mechanical properties based on their microscopic molecular structure is difficult, especially considering statistical variability. On the other hand, it is known that there is a positive correlation between the bending stiffness G (GPa) and the glass transition temperature Tg (°C) of polymers. In other words, instead of identifying the microscopic molecular structure, it is possible to use phase transition as a macroscopic indicator to determine the mechanical properties of polymers.
[0056] Figure 3(a) shows the results of the glass transition temperature Tg (°C) of the polymer portion 50 when the copolymerization ratio of the second unit 62 and the third unit 63 is changed by the IB ratio = IB / (IB + EH), as investigated by the present inventors. In this investigation, the content ratio of the first unit 61 constituting the shell-shaped ligand 60 (polymer portion 50) was fixed. It can be seen that the glass transition temperature Tg changes almost linearly from approximately -30°C to approximately +40°C in the range of content ratios from 100% second unit 62 to 100% third unit 63.
[0057] Figure 3(a) shows that the glass transition temperature Tg of the polymer portion 50 is well controlled with respect to the ratio of the second unit 62, which contains a 2-ethylhexyl group EH with 8 rotatable bonds RB, to the third unit 63, which contains an isobonyl group (IB) with 3 rotatable bonds RB. In other words, Figure 3(a) shows that the mechanical structure of the polymer portion 50 is well controlled with respect to the copolymerization ratio of the second unit 62 and the third unit 63. Here, EH is a 2-ethylhexyl group derived from 2-ethylhexyl methacrylate (EHMA), and IB is an isobonyl group derived from isobonyl methacrylate (IBMA).
[0058] (Stabilization of quantum emission yield under light irradiation by composition of polymer portion) Figure 3(b) shows the quantum emission yield PLQY value after 6 hours of light irradiation of a photoresponsive material 500 equipped with a shell-shaped ligand 60, under the same conditions as the study results in Figure 3(a), where the copolymerization ratio of the first unit is fixed and the IB ratio = IB / (IB + EH) is changed. The present invention shows that in the polymer portion 50 constituting the shell-shaped ligand 60, the quantum emission yield PLQY after 6 hours exhibits a semicircular (∩-shaped) profile with respect to the content ratio of the second unit 62 and the third unit 63. In other words, the present inventors have found that by having a predetermined structure in the polymer portion 50 constituting the shell-shaped ligand 60 that corresponds to a predetermined content ratio range of the second and third units, the decrease in the quantum emission yield of the photoresponsive material 500 is reduced. Furthermore, the inventors have found that the polymer portion 50 constituting the shell-shaped ligand 60 exhibits the effect of reducing the photo-induced desorption phenomenon of halogens from the surface of the nanoparticles 10 by having a predetermined structure corresponding to a predetermined content ratio range of the second and third units. In this case, the halogen composition I / (Br+I) of the shell-shaped ligand is 57 / 100, and it is a red (center wavelength 630 nm) perovskite-type nanocrystalline phosphor.
[0059] (Estimation of the stabilization effect of the copolymer composition of the polymer portion on the halogen composition of the nanoparticle surface,) and an estimation model of the effect of reducing photodesorption, including the mechanism of stabilization of the halogen composition of the nanoparticle surface by the composition of the polymer portion estimated by the present inventors, will be explained using Figures 4(a) and 4(b).
[0060] Figure 4(a) shows, from left to right, the steps of synthesizing a photoresponsive material 500 containing photoresponsive particles 100, obtaining a polymerizable composition 200 containing a polymerizable compound as a medium by removing the solvent, and obtaining a coating film by spreading the polymerizable composition 200 on a substrate. Furthermore, Figure 4(a) shows, from left to right, the steps of obtaining a photoresponsive cured product 300 by UV curing the coating film, and the steps of evaluating the lightfastness of the photoresponsive cured product 300 by irradiating it with blue light.
[0061] Figure 4(b) schematically shows the action of the second unit 62 in the synthesis process of the photoresponsive material 500 in Figure 4(a) (b-1), and the action of the third unit 63 in the photo-irradiated environment of the photoresponsive material 500 to the photoresponsive cured product 300 in Figure 4(a) (b-2).
[0062] As shown in Figure 4(b-1), the flexibility of the polymer 50 is ensured by the second unit having a high number of rotational bonds RB, which provides flexibility and ensures the degree of freedom of movement of the polymer portion 50 while it deforms. This ensures that the betaine group 45 has an opportunity to come into contact with the surface of the nanoparticle 10 and promotes the coordination of the betaine group 45 to the surface of the nanoparticle 10.
[0063] As shown in Figure 4(b-2), the third unit 63, which has a low degree of rotational freedom, imparts rigidity to the polymer portion 50, thereby suppressing the detachment of the betaine groups 45 that are coordinated to the nanoparticles 10 due to the high mobility of the polymer portion 50.
[0064] The inventors estimate that by providing a second unit 62 and a third unit 63 in parallel, each having a different effect on the rigidity of the polymer portion 50, the coordination promotion and desorption suppression of the betaine group 45 will work effectively. In other words, the inventors estimate that by providing the photoresponsive particle 100 with a second unit 62 and a third unit 63 that have different effects on the rigidity of the polymer portion 50, the photo-induced desorption effect and coordination inhibition effect of the betaine group 45 will be suppressed.
[0065] The ease of coordination and resistance to detachment of the betaine group 45 of the shell ligand 60 to the surface of the nanoparticle 10 can be designed based on the number of rotatable bonds RB of the second and third units. The number of rotatable bonds RB represents the number of rotatable single bonds present in the side chain, excluding bonds to hydrogen atoms, terminal single bonds excluding bonds to hydrogen atoms, and partial bonds in cyclic structures. A larger number of rotatable bonds increases the degree of structural freedom, making coordination easier. A smaller number of rotatable bonds decreases the degree of structural freedom, making detachment more difficult.
[0066] From the viewpoint of suppressing detachment from the nanoparticles 10, the third unit 63 is adopted to have three or fewer rotatable bonds. The third unit 63 is adopted to have at least one of the following groups: methyl ester group, ethyl ester group, isopropyl ester group, isovonyl ester group, and cyclohexyl ester group.
[0067] The second unit 62 employs a number of rotatable bonds RB that is at least one greater than the number of rotatable bonds of the third unit 63. The number of rotatable bonds RB of the second unit 62 is set to 4 or more, preferably 7 or more. As shown in Figure 2A, the second unit 62 employs at least one of the group consisting of isobonyl groups and ethyl groups.
[0068] As the shell ligand, it is preferable to use a copolymer obtained by polymerizing at least three types of monomers, each containing a first side chain 71, a second side chain 72, and a third side chain 73. Using a copolymer obtained by polymerizing three types of monomers offers advantages in terms of raw material availability and ease of manufacture. The positional relationship between the first unit 61, the second unit 62, and the third unit 63 within the shell ligand 60 is not relevant.
[0069] The aforementioned modified form also includes a shell-shaped ligand in which a second side chain 72 and a third side chain 73 are arranged in parallel with the main skeleton 55, and a first side chain 71 and a second side chain 72 are arranged in series. In other words, a form in which the second side chain 72 and the first side chain 71 are arranged in series in the section from the main skeleton 55 to the nanoparticle 10 is also included as a modified form of this embodiment.
[0070] (Alternative expressions for shell-shaped ligand / photoresponsive particle) The shell-shaped ligand 60 and photoresponsive particle 100 of this embodiment can be described using the following alternative expressions.
[0071] The photoresponsive particle 100 comprises a nanoparticle 10 and a shell-shaped ligand 60 comprising a plurality of bonding portions 40 containing structural units having betaine groups 45, and a polymer portion 50 that coordinates to the nanoparticle 10 at multiple locations via the plurality of bonding portions 40. Here, the nanoparticle 10 has a perovskite-type crystalline structure containing iodine at the X site. Furthermore, the shell-shaped ligand 60 has a first unit 61 having betaine groups 45 and constituting the bonding portion 40. In addition, the shell-shaped ligand 60 has a second unit 62 that constitutes the polymer portion 50 and promotes the coordination of the betaine groups 45 to the nanoparticle 10, and a third unit 63 that constitutes the polymer portion 50 and suppresses the detachment of the betaine groups 45 from the nanoparticle 10.
[0072] (Method for forming a shell - Method for forming a betaine polymer) To form a shell, first a polymer compound is synthesized having a first side chain 71 having a betaine group, a second side chain 72 that promotes coordination to the nanoparticles 10, and a third side chain 73 that suppresses detachment from the nanoparticles 10. The shell is formed by coordinating the synthesized polymer compound to the nanoparticles. Methods of coordination include coordination in a liquid phase and coordination in a solid phase. From the viewpoint of reaction controllability, coordination in a liquid phase is preferred.
[0073] The method for producing the above polymer compound is not particularly limited as long as the above structure is obtained, but it can be produced by, for example, the following methods (i) and (ii).
[0074] In other words, (i) a polymer compound can be produced by first producing a monomer containing at least a betaine group, and then polymerizing such monomer. Furthermore, (ii) a polymer compound can be produced by first synthesizing a polymer backbone, and then bonding the betaine group-containing moieties to the polymer backbone by polymer reaction.
[0075] From the viewpoint of the availability of monomers and the control of the amount of functional groups, it is preferable to manufacture them by the method shown in (i). Below, a method for synthesizing copolymers of a monomer having a first side chain 71, a monomer having a second side chain 72, and a monomer having a third side chain 73 using the method shown in (i) will be described in detail.
[0076] Monomers for introducing the first side chain 71, the second side chain 72, and the third side chain 73 into the polymer compound include vinyl ether derivatives, acrylate derivatives, methacrylate derivatives, α-olefin derivatives, and aromatic vinyl derivatives. Among these monomers, acrylate derivatives or methacrylate derivatives are preferred from the viewpoint of ease of monomer production. As monomers having a phosphobetaine group, for example, 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (MPC) can be used. As monomers having a sulfobetaine group, for example, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propane-1-sulfonic acid can be used. As carboxybetaine, for example, 3-[[2-(methacryloyloxy)ethyl]dimethylammonio]propionate can be used. Examples of monomers having a second side chain that promotes coordination to the nanoparticles 10 include propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, and cyclic trimethylolpropaneformal (meth)acrylate. Examples of monomers having a third side chain that suppresses detachment from nanoparticles 10 include methyl (meth)acrylate, ethyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, 3,3,5-trimethylcyclohexyl acrylate, isobornyl (meth)acrylate, and 1-adamantyl (meth)acrylate.
[0077] Polymerization methods for the above monomers include radical polymerization and ionic polymerization. Living polymerization can also be used for the purpose of controlling molecular weight distribution or structure. Industrially, radical polymerization is preferred.
[0078] Any solvent can be used as the solvent during synthesis. To improve the uniformity of the reaction, it is preferable to use a solvent that has high solubility for the monomer and polymerization initiator. Since betaine groups are highly hydrophilic and monomers are often relatively hydrophobic, it is preferable to use an amphiphilic solvent. Examples of such solvents include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 1-pentanol, 1-hexanol, and 2,2,2-trifluoroethanol.
[0079] Radical polymerization can be carried out by using a radical polymerization initiator, irradiation with light such as radiation or laser light, a combination of a photopolymerization initiator and light irradiation, or heating. The radical polymerization initiator can be any compound that generates radicals and initiates a polymerization reaction, and is selected from compounds that generate radicals through the action of heat, light, radiation, or oxidation-reduction reactions.
[0080] Examples of radical polymerization initiators include azo compounds, organic peroxides, inorganic peroxides, organometallic compounds, and photopolymerization initiators.
[0081] More specifically, radical polymerization initiators include azo compounds such as 2,2'-azobisisobutyronitrile (AIBN) and 2,2'-azobis(2,4-dimethylvaleronitrile); organic peroxides such as benzoyl peroxide (BPO), tert-butyl peroxypivalate, and tert-butyl peroxyisopropyl carbonate; inorganic peroxides such as potassium persulfate and ammonium persulfate; redox initiators such as hydrogen peroxide-iron(II) salt systems, BPO-dimethylaniline systems, and cerium(IV) salt-alcohol systems; and photopolymerization initiators such as acetophenone systems, benzoin ether systems, and ketal systems. Two or more of these radical polymerization initiators may be used in combination.
[0082] The polymerization temperature of the monomer varies depending on the type of polymerization initiator used, and is not particularly limited. However, polymerization is generally carried out at temperatures between -30°C and 150°C, with a more preferred temperature range being 40°C to 120°C.
[0083] The amount of polymerization initiator used in this process is preferably 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the monomer, and the amount used should be adjusted so that a polymer compound with the target molecular weight distribution is obtained.
[0084] Furthermore, any polymerization method can be used, including solution polymerization, suspension polymerization, emulsion polymerization, dispersion polymerization, precipitation polymerization, and bulk polymerization, and is not particularly limited to any particular method.
[0085] The resulting polymer compounds can be purified as needed. There are no particular restrictions on the purification method, and methods such as reprecipitation, dialysis, and column chromatography can be used.
[0086] The structure of the fabricated shell-like ligand can be identified using various instrumental analyses. Suitable analytical instruments include nuclear magnetic resonance (NMR) and gel permeation chromatography (GPC).
[0087] In the copolymer, the molar ratio of monomers having the first side chain 71 is preferably 2 to 50, and more preferably 6 to 45, with respect to the total amount of monomers in the copolymer being 100.
[0088] The molar ratio of monomers having a second side chain is preferably 10 to 90, with the total amount of monomers in the copolymer being 100.
[0089] The molar ratio of monomers having a third side chain is preferably 10 to 90, with the total amount of monomers in the copolymer being 100.
[0090] When the copolymerization composition ratio falls within the above range, the shell-like ligands are more easily coordinated to the nanoparticles and less likely to desorb, improving the durability of the photoresponsive material.
[0091] Furthermore, other monomers may be copolymerized. The amount of substance is sometimes expressed as molar concentration.
[0092] The content of the shell-like ligand in the photoresponsive material is preferably 1 to 1000 parts by mass, preferably 5 to 500 parts by mass, and more preferably 10 to 300 parts by mass, with the nanoparticle content being 100 parts by mass. If the content is less than 1 part by mass, the shell effect may not be fully exhibited, and stability may not be improved. If the content is greater than 1000 parts by mass, the solubility and dispersibility of the shell-like ligand in the medium may decrease, and the stability of the photoresponsive material may not be improved. The content of the shell-like ligand in the photoresponsive material can be appropriately adjusted according to the type and application of the nanoparticles and shell-like ligand.
[0093] (Method for purifying nanoparticles) Nanoparticles synthesized by the above method can be purified by methods such as centrifugation to remove impurities from the synthesis process, and then used as raw materials for photoresponsive materials. When performing centrifugation, it is common to add a large excess of a polar solvent such as ethyl acetate as a poor solvent to the reaction solution (crude solution). However, when a large amount of polar solvent such as ethyl acetate is used, not only does the amount of centrifugation processing increase, but there is also the problem that the luminescence properties of the nanoparticles will deteriorate if the centrifugation process is not performed immediately. This is because the halogen and ligands coordinated to the nanoparticles are desorbed by the polar solvent. Therefore, although purification methods that use large amounts of polar solvent are preferred at the laboratory level, they have low applicability to industries that require large-scale processing. In this embodiment, the amount of polar solvent added during centrifugation is preferably 300 parts or less, and more preferably 100 parts or less, relative to the crude solution. When more than 300 parts of polar solvent are used relative to the crude solution, the luminescence properties of the nanoparticles may deteriorate as described above. Reducing the amount of polar solvent also reduces the time constraints before starting centrifugation.
[0094] <Second Embodiment> The photoresponsive particles 120 and photoresponsive material 520 according to the second embodiment will be described with reference to Figure 5.
[0095] As shown in Figure 5, the photoresponsive particle 120 comprises a nanoparticle 10 having a perovskite-type crystalline structure containing iodine at the X site. Furthermore, as shown in Figure 5, the photoresponsive particle 120 comprises a first shell-like ligand 66 including a plurality of first bonding portions 41 containing structural units having betaine groups 45, and a first polymer portion 51 bonded to the nanoparticle 10 at multiple locations via the plurality of first bonding portions 41. Furthermore, as shown in Figure 5, the photoresponsive particle 120 comprises a second shell-like ligand 67 including a plurality of second bonding portions 42 containing structural units having betaine groups 45, and a second polymer portion 52 bonded to the nanoparticle 10 at multiple locations via the plurality of second bonding portions 42. Furthermore, the first polymer portion 51 has a first main skeleton 57 and a second side chain 72 branching from the first main skeleton 57 and having 4 or more rotatable bonds, and the second polymer portion 52 has a second main skeleton 58 and a third side chain 73 branching from the second main skeleton 58 and having 3 or fewer rotatable bonds. The second side chain 72 has 4 or more rotatable bonds RB, and the third side chain 73 has 3 or fewer rotatable bonds RB. In addition, the second side chain 72 has 4 or more rotatable bonds than the rotatable bonds RB of the third side chain 73.
[0096] The photoresponsive particles 120 and the medium 90 interposed between the photoresponsive particles 120 according to this embodiment comprise the photoresponsive material 520 according to this embodiment. The photoresponsive material 120 differs from the photoresponsive particles 100 in that it comprises two shell-like ligands 66, 67, each having a second side chain 72 with a relatively high number of rotatable bonds RB and a third side chain 73 with a relatively low number of rotatable bonds RB.
[0097] (Two shell-like ligands) The shell-like ligand 66, i.e., the first shell-like ligand 66, has a second side chain 72 (second unit 62) with a relatively high number of rotatable bonds RB, which is a side chain that is bound to the first main chain 57 and not coordinated to the nanoparticles 10. On the other hand, the shell-like ligand 67, i.e., the second shell-like ligand 67, has a third side chain 73 (third unit 63) with a relatively low number of rotatable bonds RB, which is a side chain that is bound to the second main chain 58 and not coordinated to the nanoparticles 10.
[0098] The first shell-shaped ligand 66 has a first unit 61 having a betaine group 45 and a second unit 62 that promotes coordination to the nanoparticles 10. The first shell-shaped ligand 66 has a plurality of first bonding portions 41 including structural units having a betaine group 45 and a first polymer portion 51 that coordinates to the nanoparticles 10 at a plurality of locations via the plurality of first bonding portions 41. The second shell-shaped ligand 67 is the same as the first shell-shaped ligand 66 except that it has at least a third unit 63 that suppresses the detachment of the betaine group 45 from the nanoparticles 10.
[0099] In this embodiment, the photoresponsive particle 120 contains, for each of the first shell-shaped ligand 66 and the second shell-shaped ligand 67, 100% of the second side chain 72 (second unit 62) and the third side chain 73 (third unit 63) as ligand components other than the first side chain. In this embodiment, the shell-shaped ligand with a high relative ratio (molar ratio) of the second side chain 72 (second unit 62) to the third side chain 73 (third unit 63) is designated as the first shell-shaped ligand 66m, and the one with a relatively lower ratio is designated as the second shell-shaped ligand 67m.
[0100] The weight ratio of the first shell-shaped ligand 61 to the second shell-shaped ligand 62 is preferably 1 / 99 to 99 / 1, and more preferably 10 / 90 to 90 / 10.
[0101] It is preferable to use at least two types of copolymers A and B, which include copolymer A obtained by polymerizing at least two types of monomers including a first side chain 71 and a second side chain 72, and copolymer B obtained by polymerizing at least two types of monomers including a first side chain 71 and a third side chain 73. The embodiment using at least two types of copolymers A and B as shell ligands is highly convenient in terms of structural control during synthesis.
[0102] <Third and Fourth Embodiments> Next, the polymerizable composition 530 according to the third embodiment and the photoresponsive cured product 540 according to the fourth embodiment will be described using Figures 6A and 6B, respectively.
[0103] The polymerizable composition 530 according to the third embodiment differs from the photoresponsive material 500 according to the first embodiment in that, as shown in Figure 6A, it contains a polymerizable compound 70 such that it is dispersed or dissolved with the photoresponsive particles 100 in the medium 93 containing the photoresponsive material 500. The medium 90 in this embodiment is fluid and may therefore be referred to as medium 90f.
[0104] The photoresponsive cured product 540 according to the fourth embodiment differs from the polymerizable composition 530 according to the third embodiment in that, as shown in Figure 6B, it comprises a polymer 75 derived from the polymerizable compound 70, which is thickened or cured, of the polymerizable compound 70 contained in the polymerizable composition 530. The photoresponsive cured product 540 can be rephrased as comprising a photoresponsive material 500 and a polymer 75 derived from the polymerizable compound 70. The medium 90 in this embodiment is a solid that has been cured and whose fluidity has been reduced by the polymer 75, and is therefore sometimes referred to as medium 90s.
[0105] (Polymerizable Compounds) Polymerizable compounds can undergo polymerization reactions upon receiving energy such as light, heat, or electromagnetic waves, increasing the viscosity of liquid or paste-like intermediates containing themselves and causing them to harden. Polymerizable compounds that undergo polymerization reactions upon irradiation with light are sometimes referred to as photopolymerizable compounds.
[0106] In order to make the photoresponsive material of this embodiment a polymerizable composition that hardens in response to external stimuli, polymerizable monomers can also be used as a medium. Polymerizable monomers include UV monomers, UV dimers, UV oligomers that can be cured by ultraviolet light, thermally polymerizable monomers, thermally polymerizable dimers, thermally polymerizable oligomers, etc., which may be referred to as photopolymerizable compounds and thermally polymerizable compounds, respectively. These may be used individually or in combination of two or more types.
[0107] Examples of radical polymerizable compounds include monofunctional (meth)acrylate compounds, difunctional (meth)acrylate compounds, trifunctional or more functional (meth)acrylate compounds, hydroxyl group-containing (meth)acrylate compounds, carboxyl group-containing (meth)acrylate compounds, and vinyl compounds.
[0108] Examples of monofunctional (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, and 3,3,5-trimethylcyclohexyl acrylate. Tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, isobornyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, and cyclic trimethylolpropaneformal (meth)acrylate can be used.
[0109] Examples of difunctional (meth)acrylate compounds include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol 200 di(meth)acrylate, polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, and polyethylene glycol 600 Di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol 400 di(meth)acrylate, polypropylene glycol 700 di(meth)acrylate, neopentyl glycol di(meth)acrylate, neopentyl glycol PO-modified di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate can be used.
[0110] Examples of trifunctional or more (meth)acrylate compounds include trimethylolpropane triacrylate, trimethylolpropane EO-modified tri(meth)acrylate, trimethylolpropane PO-modified tri(meth)acrylate, glycerin propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(acryloxyethyl) isocyanurate, and EO-modified pentaerythritol tetraacrylate.
[0111] Examples of hydroxyl group-containing (meth)acrylate compounds include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate, as well as 2-hydroxyethyl acryloyl phosphate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, dipropylene glycol (meth)acrylate, fatty acid-modified glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, glycerin di(meth)acrylate, and 2-hydroxy-3-acryloyloxypropyl methacrylate.
[0112] Examples of carboxyl group-containing (meth)acrylate compounds include β-carboxyethyl (meth)acrylate, mono(meth)acryloyloxyethyl succinate, and ω-carboxypolycaprolactone mono(meth)acrylate.
[0113] Examples of vinyl compounds that can be used include vinyl acetate, vinyl benzoate, vinyl pivalate, vinyl butyrate, vinyl methacrylate, and N-vinylpyrrolidone.
[0114] Cationic polymerizable compounds can be either photopolymerizable or thermally polymerizable. These may be used individually or in combination of two or more types. Typical cationic polymerizable compounds include, for example, epoxy compounds, oxacene compounds, and vinyl ether compounds.
[0115] The amount of polymerizable compound used, including the radical polymerizable compound and cationic polymerizable compound described above, is preferably 1 to 99 parts by mass, more preferably 5 to 95 parts by mass, and even more preferably 10 to 90 parts by mass, per 100 parts by mass of the polymerizable composition.
[0116] (Polymerization Initiators) Polymerization reactions generally involve the combined use of polymerization initiators and polymerizable compounds. Polymerization initiators are compounds that generate active species that initiate polymerization reactions upon irradiation with active energy rays or heat, and known polymerization initiators can be used. The main active species that initiate polymerization reactions include radical polymerization initiators that generate radicals and cationic polymerization initiators that generate acids, and these may be used in combination. Examples of photoradical polymerization initiators that generate radicals using active energy rays include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl methyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butane, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl Acetophenones such as [phenyl]propanone], 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl]-2-methylpropan-1-one; benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; phosphines such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; and other phenylglyoxylic methyl esters.
[0117] Among photoradical polymerization initiators, preferred are acetophenones, phosphines, and oxime ester compounds, typified by aminoketones. These can be used individually or in combination depending on the desired properties of the cured product. When using a radical polymerization initiator, the amount used is preferably 0.01 to 100 parts by mass, and more preferably 0.1 to 50 parts by mass, per 100 parts by mass of the total solid content in the composition.
[0118] (Nanoparticle Content) The content of nanoparticles in the polymerizable composition is preferably 6% by weight or more and 30% by weight or less. If it is lower than 6% by weight, the shell-like ligands may easily detach, and sufficient durability may not be obtained. If it is higher than 30% by weight, the amount of polymerizable compound will be relatively small, and sufficient curability may not be obtained.
[0119] (Other Additives) In this embodiment, the polymerizable composition may be mixed with, if necessary, oxygen scavengers, antioxidants, scattering agents such as titanium dioxide, surfactants, fungicides, light stabilizers, and other additives that impart various properties.
[0120] The polymerizable composition 530 according to the third embodiment comprises a shell-shaped ligand 60 having a predetermined structure relative to the nanoparticles 10, which are perovskite-type nanocrystals, similar to the photoresponsive material 500 according to the first embodiment. That is, the polymerizable composition 530 according to the third embodiment has a shell-shaped ligand 60 comprising a second unit 62 and a third unit 63 that have opposing effects on the (bending) rigidity of the main skeleton 55 of the polymer portion 50. As a result, the betaine groups 45 coordinated to the surface of the nanoparticles 10 are stabilized in the polymerizable composition 530 according to the third embodiment, and the photo-induced desorption phenomenon of the halogen composition on the surface of the nanoparticles 10 is reduced, similar to the photoresponsive material 500.
[0121] The photoresponsive cured product 540 according to the fourth embodiment is provided with a shell-shaped ligand 60 having a predetermined structure relative to the nanoparticles 10, which are perovskite-type nanocrystals, similar to the photoresponsive material 500 according to the first embodiment. That is, the photoresponsive cured product 540 according to the fourth embodiment has a shell-shaped ligand 60 comprising a second unit 62 and a third unit 63 that have opposing effects on the (bending) rigidity of the main skeleton 55 of the polymer portion 50. As a result, in the photoresponsive cured product 540 according to the fourth embodiment, the betaine groups 45 coordinated to the surface of the nanoparticles 10 are stabilized, and the photo-induced desorption phenomenon of the halogen composition on the surface of the nanoparticles 10 is reduced, similar to the photoresponsive material 500.
[0122] <Embodiments 5, 6, and 7> The wavelength conversion layer according to the 5th embodiment, the wavelength conversion element according to the 6th embodiment, and the light-emitting element array according to the 7th embodiment will be described in order with reference to Figure 7. Figure 7 shows the cross-sectional structure of the light-emitting element array 570 according to the 7th embodiment.
[0123] (Wavelength Conversion Layer) The wavelength conversion layer 550 according to the fifth embodiment is formed by creating a layer of photoresponsive cured material 540 (photoresponsive effect film) on a support substrate (not shown). The wavelength conversion layer 550 can be rephrased as a wavelength conversion layer obtained by curing a coating film formed by applying the polymerizable composition 530 shown in Figure 4(a). The wavelength conversion layer 550 of this embodiment has an emitting surface 200 that emits light whose wavelength has been converted to a predetermined color, and a light-receiving surface 220 that optically couples with a light source such as a light-emitting element, on its front and back sides in the D1 direction, as shown in Figure 7. In other words, the wavelength conversion layer 550 can be rephrased as a photoresponsive cured material 540 that has a light-receiving surface 220 that optically couples with a light source.
[0124] The wavelength conversion layer 550 is self-supporting when impregnated into a resin film or laminated onto a resin film, and is therefore sometimes referred to as a wavelength conversion film. Support configurations for the wavelength conversion layer include a laminated configuration in which wavelength conversion layers with different emission colors are stacked in the D1 direction, and a parallel arrangement configuration in which they are arranged in parallel in a plane intersecting the D1 direction. The wavelength conversion layer 550 is obtained by coating a polymerizable composition 530 onto a support member (substrate), curing it, and then forming it into a film, sheet, or pattern.
[0125] (Method for forming the wavelength conversion layer) The method for forming the wavelength conversion layer 550 is not particularly limited. For example, one method involves coating a polymerizable composition 530 onto a substrate, pre-drying it, and then curing the coating film by heat treatment or irradiation with active energy rays. Coating is synonymous with the process of applying. The thickness of the cured wavelength conversion layer 550 is preferably 0.1 to 200 μm, more preferably 1 to 100 μm.
[0126] In active energy ray irradiation, the active energy rays are appropriately selected electromagnetic waves that reduce fluidity and accelerate hardening through polymerization, crosslinking, drying, etc., such as thermal rays, ultraviolet rays, visible light, near-infrared rays, and electron beams. As the light source for providing active energy rays, a light source having a main emission wavelength in the wavelength range of 100 to 450 nm is preferred. Examples of such light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, medium pressure mercury lamps, mercury xenon lamps, metal halide lamps, high-power metal halide lamps, xenon lamps, pulsed emission xenon lamps, deuterium lamps, fluorescent lamps, ND-YAG third harmonic lasers, HE-CD lasers, nitrogen lasers, XE-Cl excimer lasers, XE-F excimer lasers, semiconductor-pumped solid-state lasers, and LED lamp light sources having emission wavelengths of 365 nm, 375 nm, 385 nm, 395 nm, and 405 nm.
[0127] The wavelength conversion layer 550 according to the fifth embodiment has a shell-shaped ligand 60 comprising a second unit 62 and a third unit 63 that have opposing effects on the (bending) rigidity of the main skeleton 55 of the polymer portion 50. As a result, in the wavelength conversion layer 550 according to the fifth embodiment, the betaine groups 45 coordinated to the surface of the nanoparticles 10 are stabilized, and the photo-induced desorption phenomenon of the halogen composition on the surface of the nanoparticles 10 is reduced, similar to the photoresponsive material 500.
[0128] Furthermore, the polymer portion 50 includes a main skeleton 55 and a first side chain 71 containing a betaine group 45 that bridges the nanoparticles 10 and the main skeleton 55. In other words, the polymer portion 50 also includes a second side chain 72 that reduces the rigidity of the polymer portion 50 and constitutes a second unit 62, and a third side chain 73 that increases the rigidity of the polymer portion 50 and constitutes a third unit 63.
[0129] (Wavelength Conversion Element) The wavelength conversion element 560 according to the sixth embodiment comprises a first optical conversion layer 550r and a second optical conversion layer 550g having different halogen compositions in the wavelength conversion layer, and a black matrix BM that optically separates the wavelength conversion layer. The wavelength conversion element 560 comprises a first optical conversion layer 550r and a second optical conversion layer 550g having different emission center wavelengths, and a black matrix BM that optically separates the wavelength conversion layer. The wavelength conversion element 560 comprises a first optical conversion layer 560r and a second optical conversion layer 560g having different emission center wavelengths, and a black matrix BM that optically separates the wavelength conversion layer.
[0130] The wavelength conversion element 560 according to the sixth embodiment has a shell-shaped ligand 60 comprising a second unit 62 and a third unit 63 that have opposing effects on the (bending) rigidity of the main skeleton 55 of the polymer portion 50. As a result, in the wavelength conversion element 560 according to the sixth embodiment, the betaine groups 45 coordinated to the surface of the nanoparticles 10 are stabilized, and the photo-induced desorption phenomenon of the halogen composition on the surface of the nanoparticles 10 is reduced, similar to the photoresponsive material 500.
[0131] (Light-emitting element array) The light-emitting element array 570 according to the seventh embodiment includes light-emitting elements 700B that emit blue light, which are arranged in an array corresponding to the arrangement of wavelength conversion elements 560, and serve as light sources optically coupled with the light-receiving surfaces 220r and 220g. The light-receiving surfaces 220r and 220g are the light-receiving surfaces of the first light conversion layer 550r and the second light conversion layer 550g of the wavelength conversion element 560. The array of light-emitting elements 700B may be referred to as a light-emitting element array. The light-emitting element array 570 (wavelength conversion layer) includes a plurality of sets of wavelength conversion layers 560 with different halogen compositions located at the X site.
[0132] The light-emitting element array 570 according to the seventh embodiment is equipped with a shell-shaped ligand 60 having a predetermined structure for nanoparticles 10 which are perovskite-type nanocrystals, similar to the photoresponsive material 500 according to the first embodiment. That is, the light-emitting element array 570 according to the seventh embodiment has a shell-shaped ligand 60 comprising a second unit 62 and a third unit 63. As a result, in the light-emitting element array 570 according to the seventh embodiment, the betaine groups 45 coordinated to the surface of the nanoparticles 10 are stabilized, and the photo-induced desorption phenomenon of the halogen composition on the surface of the nanoparticles 10 is reduced, similar to the photoresponsive material 500.
[0133] The light-emitting element array 570 has a light source element 700B, a dielectric multilayer film 517, and wavelength conversion layers 550r and g stacked in the stacking direction D1. In the stacking direction D1, the downstream side coincides with the side where the user viewing the image drawn on the light-emitting element array 570 is positioned. The wavelength conversion layers 550r and g are separated from the wavelength conversion layers corresponding to adjacent elements by a black matrix BM that separates pixels.
[0134] As described above, the polymerizable composition 530 is cured together with the polymerizable compound 70 by performing a polymerization treatment such as photopolymerization. Upon curing, the polymerizable composition 530 constitutes the wavelength conversion layers 550r and 550g of the light-emitting element array 570 that satisfy predetermined dimensions. That is, the wavelength conversion layers 550r and 550g are layers that have been solidified by curing together with the polymerizable compound 50.
[0135] The light source element 700B corresponds to a light source that emits light L1 at a first wavelength λ1. The wavelength conversion layers 550r and g have an optical coupling surface 522 on the side of the light source element 700B that optically couples with the light source element 700B, and an extraction surface 524 on the opposite side of the light source element 700B that extracts secondary light L2 converted by the wavelength conversion layers 550r and g.
[0136] In this embodiment, the wavelength conversion layers 550r and g receive primary light L1 with wavelength λ1 that propagates through the dielectric multilayer film 517. The dielectric multilayer film 517 provides the light-emitting element array 570 with the spectral transmission characteristics of the primary light from the light source element 700B and the spectral reflection characteristics of the secondary light L2 with wavelength λ2 emitted in the wavelength conversion layers 550r and g. The wavelength λ2 of the secondary light L2 is longer than the wavelength λ1 of the primary light L1.
[0137] The dielectric multilayer film 517 can be replaced with another optical element that transmits light to the first wavelength λ1 emitted by the light source element 700B. Furthermore, another optical element (not shown) can be placed in front of the extraction surface 200 (opposite side of the light source element 700B).
[0138] (Storage Method) Since luminescent nanoparticles having a perovskite crystal structure are susceptible to degradation of their luminescence properties due to external stimuli such as light and heat, although the photoresponsive material according to this embodiment has high light resistance, it is preferable to store it in a refrigerator or darkroom where it is kept still in a cool place, shielded from external light. This improves stability compared to storing it in an environment where it may be exposed to external light or high temperatures.
[0139] (Measurement and Analysis Methods) Various physical property measurements can be performed as follows.
[0140] (Measurement of molecular weight distribution of shell-shaped ligands) The molecular weight distribution of shell-shaped ligands 60 can be calculated in terms of monodisperse polymethyl methacrylate by gel permeation chromatography (GPC). Molecular weight measurement by GPC can be performed as shown below, for example.
[0141] The sample was added to the eluent listed below to achieve a sample concentration of 1% by mass, and the solution was allowed to stand at room temperature for 24 hours to dissolve. The solution was then filtered through a solvent-resistant membrane filter with a pore diameter of 0.45 μm to obtain the sample solution, which was then measured under the following conditions: Instrument: Agilent 1260 Infinity System (Agilent Technologies) Column: PFG Analytical Linear M Columns (PSS) Eluent: 2,2,2-Trifluoroethanol Flow rate: 0.2 ml / min Oven temperature: 40°C Sample injection volume: 20 μL
[0142] To calculate the molecular weight distribution of the sample, a molecular weight calibration curve prepared using standard polymethyl methacrylate resin (Agilent Technologies EasiVial PM Polymer Standard Kit) is used.
[0143] (Compositional analysis of shell-shaped ligands) The compositional analysis of shell-shaped ligands 60 can be performed using nuclear magnetic resonance (NMR). For example, using the ECA-600 (600 MHz) manufactured by JEOL Ltd., ¹H-NMR and ¹³C-NMR spectra are measured. At that time, the measurement is performed at 25°C in a deuterated solvent containing tetramethylsilane as an internal standard. The chemical shift value is read as the ppm shift value (δ value) with the internal standard substance, tetramethylsilane, set to 0. When shell-shaped ligands purified using preparative GPC are dissolved in an NMR solvent such as methanol and measured, the influence of other components is less likely to occur. Signals originating from betaine groups are observed on the lower magnetic field side compared to signals originating from organic groups. By comparing the signal intensity originating from organic groups and the signal intensity originating from betaine groups, the molar ratio (copolymerization ratio) of monomers having betaine groups and monomers having organic groups can be determined.
[0144] (Measurement of shell-like ligand content) The content of shell-like ligands 60 in the photoresponsive material 500 and the polymerizable composition 530 can both be determined from the weight of shell-like ligands 60 isolated using preparative GPC. It can also be determined from TG-DTA measurement and integrated intensity of NMR.
[0145] (Crystal structure analysis of nanoparticles, analysis of X-site composition ratio) The crystal structure analysis and composition analysis of nanoparticles 10 can be performed using an X-ray diffractometer (XRD). For example, by measuring the X-ray diffraction pattern using a RINT 2100 (manufactured by Rigaku), it is possible to analyze whether nanoparticles 10 have a perovskite-type crystal structure. Furthermore, by utilizing the fact that the interstitial distance of the crystal differs depending on the composition ratio of the X-sites, the composition ratio of the X-sites can be analyzed.
[0146] (Method for confirming the coordination of shell-like ligands to nanoparticles) Whether or not shell-like ligands are coordinated to nanoparticles can be confirmed using infrared spectroscopy (IR). A dispersion containing nanoparticles and shell-like ligands is mixed with a poor solvent as needed, precipitated by centrifugation, and then the supernatant is removed and the precipitate is dried. Shell-like ligands not bound to the nanoparticles are removed along with the supernatant. The IR spectrum of the obtained solid is measured, and if a signal originating from the betaine group is observed, it can be confirmed that the nanoparticle shell-like ligands are coordinated. In this case, the signal originating from the betaine group may shift by several nm due to coordination.
[0147] Furthermore, coordination can also be confirmed by transmission electron microscopy (TEM) observation. Normally, photoresponsive nanoparticles 10 having a perovskite crystal structure are observed in an regularly arranged form. However, when shell-shaped ligands 60 are coordinated, the arrangement is observed to be disordered due to steric repulsion between the shell-shaped ligands 60 and between the shell-shaped ligands 60 and the substrate. Coordination can also be confirmed from this.
[0148] (Measurement of Nanoparticle Content) The content of nanoparticles 10 in the photoresponsive particles 100, the photoresponsive material 500, and the polymerizable composition 530 can all be measured using ICP emission spectroscopy and NMR. The amount of Pb is measured from the emission intensity of ICP emission spectroscopy, and the amount of ligand is measured from the signal intensity of NMR. The content of nanoparticles 10 can be measured from the crystal structure and composition information of the nanoparticles 10 obtained by XRD as described above.
[0149] Furthermore, the content of nanoparticles 10 in the photoresponsive material and polymerizable composition 530 can also be determined by measuring the amount of non-volatile components at temperatures above 400°C using differential thermal-thermogravimetric analysis (TG-DTA).
[0150] The content of nanoparticles 10 in the wavelength conversion layer 550 can be determined from the signal intensity of each element using a wavelength-dispersive X-ray fluorescence analyzer (WDXRF).
[0151] The present disclosure will be described in more detail below by a first set of embodiments, but this will not limit the present disclosure.
[0152] [Production of polymer compound a] A reaction vessel equipped with a condenser, stirrer, thermometer, and nitrogen inlet tube was prepared. Eleven parts of 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (MPC), fifty parts of 2-ethylhexyl methacrylate (EHMA), 2.7 parts of isobonyl methacrylate (IBMA), sixteen parts of azobisisobutyronitrile, and seventeen hundred parts of 2,2,2-trifluoroethanol (TFE) were charged into the reaction vessel. Nitrogen bubbling was then performed into the reaction vessel for 30 minutes. The resulting reaction mixture was heated under a nitrogen atmosphere at 65°C for eight hours to complete the polymerization reaction. After the reaction mixture was cooled to room temperature, the solvent was removed by reduced pressure distillation. The resulting residue was dissolved in chloroform and purified by dialysis using a dialysis membrane (Spectrum Laboratories, Spectra / Por7 MWCO 1kDa). After removing the solvent by reduced pressure distillation, polymer compound a, a copolymer of MPC and EHMA, was obtained by drying under reduced pressure at 50°C and 0.1 kPa or less.
[0153] When the obtained polymer compound a was analyzed using the above analytical method, it was confirmed that the weight-average molecular weight (Mw) was 7,000 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0154] [Preparation of polymer compound b] Polymer compound b was prepared in the same manner as the preparation of polymer compound a, except that 3.4 parts of IBMA were used instead of 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,900 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0155] [Preparation of polymer compound c] Polymer compound c was prepared in the same manner as the preparation of polymer compound a, except that 47 parts of EHMA and 6.1 parts of IBMA were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,500 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0156] [Preparation of polymer compound d] Polymer compound d was prepared in the same manner as for polymer compound a, except that 26 parts EHMA and 30 parts IBMA were used instead of 50 parts EHMA and 2.7 parts IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 7,300 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0157] [Preparation of polymer compound e] Polymer compound e was prepared in the same manner as the preparation of polymer compound a, except that 16 parts EHMA and 42 parts IBMA were used instead of 50 parts EHMA and 2.7 parts IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,200 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0158] [Preparation of polymer compound f] Polymer compound f was prepared in the same manner as the preparation of polymer compound a, except that 26 parts of EHMA and 22 parts of cyclohexyl methacrylate (CHMA) were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,600 and that structural units derived from MPC were present in 12 mol% of the total monomer units.
[0159] [Preparation of polymer compound g] Polymer compound g was prepared in the same manner as the preparation of polymer compound a, except that 26 parts of EHMA and 17 parts of isopropyl methacrylate (iPMA) were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,000 and that structural units derived from MPC were present in 12 mol% of the total monomer units.
[0160] [Preparation of polymer compound h] Polymer compound h was prepared in the same manner as for polymer compound a, except that 26 parts of EHMA and 15 parts of ethyl methacrylate (EMA) were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 5,800 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0161] [Preparation of polymer compound i] Polymer compound i was prepared in the same manner as the preparation of polymer compound a, except that 26 parts of EHMA and 13 parts of methyl methacrylate (MMA) were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 5,600 and that structural units derived from MPC were present in 12 mol% of the total monomer units.
[0162] [Preparation of polymer compound j] Polymer compound j was prepared in the same manner as the preparation of polymer compound a, except that 26 parts of hexyl methacrylate (HMA) and 30 parts of IBMA were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,700 and that structural units derived from MPC were present in 12 mol% of the total monomer units.
[0163] [Preparation of polymer compound k] Polymer compound k was prepared in the same manner as the preparation of polymer compound a, except that 19 parts of n-butyl methacrylate (n-BMA) and 30 parts of IBMa were used instead of 50 parts of EHMA and 2.7 parts of IBMa. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,500 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0164] [Preparation of polymer compound l] Polymer compound l was prepared in the same manner as the preparation of polymer compound a, except that 19 parts of i-butyl methacrylate (i-BMA) and 30 parts of IBMa were used instead of 50 parts of EHMA and 2.7 parts of IBMa. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 6,000 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0165] [Preparation of polymer compound m] Polymer compound m was prepared in the same manner as the preparation of polymer compound a, except that 53 parts of EHMA were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 7,000 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0166] [Preparation of polymer compound n] Polymer compound n was prepared in the same manner as for polymer compound a, except that 59 parts of IBMA were used instead of 50 parts of EHMA and 2.7 parts of IBMA. When the obtained polymer compound a was analyzed using the analytical method described above, it was confirmed that the weight-average molecular weight (Mw) was 5,400 and that structural units derived from MPCs were present in 12 mol% of the total monomer units.
[0167] Table 1 shows the composition ratios and weight-average molecular weights (Mw) of polymer compounds a to n manufactured as described above. In the side chain structure, A indicates the binding site to the polymer main chain.
[0168]
[0169] The abbreviations in Table 1 are as follows: MPC: 2-(methacryloyloxy)ethyl 2-(trimethylammonio)ethyl phosphate (manufactured by Tokyo Chemical Industry Co., Ltd.) EHMA: 2-ethylhexyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) IBMA: Isobonyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) CHMA: Cyclohexyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) iPMA: Isopropyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) EMA: Ethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) MMA: Methyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) HMA: Hexyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) n-BMA: n-butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) i-BMA: i-butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0170] [Preparation of Polymer Compound Solution] (Preparation of Toluene Solution of Polymer Compound a) Two parts of polymer compound a and 98 parts of toluene were charged into a reaction vessel equipped with a stirrer, thermometer, and reflux condenser, and the temperature was raised to 110°C and heated for 5 minutes. After confirming that polymer compound a was completely dissolved, it was cooled to room temperature to obtain a toluene solution of polymer compound a.
[0171] (Preparation of toluene solutions of polymer compounds b to n) In the preparation of the toluene solution of polymer compound a, toluene solutions of polymer compounds b to n were obtained in the same manner as in the preparation of the toluene solution of polymer compound a, except that polymer compounds b to n were used.
[0172] [Preparation of Nanoparticle Dispersion] (Preparation of Nanoparticle Dispersion a) 10 parts cesium carbonate, 27 parts oleic acid, and 388 parts 1-octadecene were placed in a flask, the liquid temperature was heated to 120°C, and the mixture was degassed for 30 minutes using a vacuum pump. The mixture was then heated to 150°C under a stream of dry nitrogen and held for 30 minutes to obtain a cation raw material solution.
[0173] Separately, 4.5 parts of lead(II) bromide, 7.6 parts of lead(II) iodide, and 493 parts of 1-octadecene were placed in a flask, heated to 120°C, and degassed for 1 hour using a vacuum pump. 89 parts of oleic acid and 81 parts of oleylamine were added, and the mixture was degassed again for 30 minutes using a vacuum pump. After that, the liquid temperature was increased to 200°C using a nitrogen flow to obtain the lead raw material solution.
[0174] 20 parts of cation stock solution were added to the entire amount of lead stock solution, and the mixture was cooled with ice after 5 seconds. 35 parts of ethyl acetate were added, and after 5 minutes, the first centrifugation (10,000 rpm, 15 minutes) was started, and the supernatant was removed by decantation. The obtained residue was redispersed in hexane, and a second centrifugation (20,000 rpm, 60 minutes) was performed, removing 80% by volume of the supernatant. Perovskite-type nanoparticles 10 were dispersed in hexane so that the amount was 1% by weight, and nanoparticle dispersion a was obtained. Analysis by XRD showed that the obtained particles had a perovskite-type crystalline structure, and the composition was CsPb(Br 0.43 I 0.57 ) 3 Furthermore, when the weight of the sample at temperatures above 400°C was analyzed by TG-DTA as perovskite-type nanoparticles 10, it was found that 73% by weight of the total solid content was perovskite-type nanoparticles 10.
[0175] [Preparation of Photoresponsive Material] (Example 1) 450 parts of nanoparticle dispersion a were placed in a container and the solvent was removed by distillation under reduced pressure. 125 parts of a toluene solution of polymer compound c were added thereto, and the mixture was heated at 60°C for 5 minutes. After that, the solvent was removed by distillation to obtain photoresponsive material 500-1.
[0176] (Examples 2-13, Comparative Examples 1-2) Using nanoparticle dispersion a and polymer compounds a-n, photoresponsive materials 500-2-15 were prepared in the same manner as in Example 1, such that the amount of nanoparticles in the nanoparticle dispersion and the amount of polymer compounds were as shown in Tables 2-1-2-2.
[0177]
[0178]
[0179] The abbreviations used in Tables 2-1 and 2-2 are as follows: RB2: Number of rotatable bonds in the second side chain RB3: Number of rotatable bonds in the third side chain
[0180] [Preparation of Titanium Dioxide Dispersion] 40 parts of titanium dioxide JR-403 (manufactured by Teika), 1 part of Ajisper PB821 (manufactured by Ajinomoto Fine Techno), 60 parts of 3,3,5-trimethylcyclohexyl acrylate (TMCHA) (manufactured by Osaka Organic Chemical Industry, trade name Viscoat #196), and glass beads (1 mm in diameter) were placed in a container and dispersed using paint conditioner for 4 hours to obtain a titanium dioxide dispersion.
[0181] [Preparation of Polymerizable Composition] (Example 14) Polymerizable composition 530-1 was obtained by blending 10 parts of photoresponsive material 500-1, 25 parts of TMCHA, 2.5 parts of 1,6-hexanediol diacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name HDDA), 1.3 parts of polymerization initiator (manufactured by IGMResins, trade name OmniradTPO), and 11 parts of titanium dioxide dispersion.
[0182] (Examples 15 to 26, Comparative Examples 3 to 4) Polymerizable compositions 500-2 to 15 were prepared to have the compositions shown in Table 3.
[0183]
[0184] The abbreviations in Table 3 are as follows: TMCHA: 3,3,5-trimethylcyclohexyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.) HDDA: 1,6-hexanediol diacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.)
[0185] [Manufacturing of Wavelength Conversion Layer] The obtained polymerizable composition was spin-coated onto a glass substrate (10 cm x 10 cm). The glass substrate on which the spin-coated polymerizable composition was formed was exposed to an integrated light intensity of 400 mJ / cm² using a belt conveyor type ultraviolet irradiator (high-pressure mercury lamp 120 W / cm²). 2 A cured film with a thickness of 10 μm was formed on the glass substrate by irradiating it with ultraviolet light in such a manner. After this, a barrier film was laminated on the surface of the cured film to obtain wavelength conversion layers 550-1 to 550-15.
[0186] <Evaluation of Wavelength Conversion Layers 550-1 to 550-15> The obtained wavelength conversion layers 550-1 to 550-15 were evaluated as follows. The results are shown in Table 4.
[0187] [Photoresistance Evaluation] For each wavelength conversion layer 550-1 to 550-15, at a wavelength of 450 nm and an intensity of 100,000 cd / m², the evaluation was performed. 2 Accelerated testing was performed by irradiating the sample with blue light, and the absolute luminescence quantum yield (PLQY) was measured.
[0188] <Measurement Conditions> Measurement device: Absolute PL quantum yield analyzer C9920-03 (Hamamatsu Photonics) Excitation light wavelength: 460 nm Excitation light integration range: Excitation light wavelength ± 10 nm Emission integration range: (Excitation light wavelength + 20) nm to 770 nm
[0189] The evaluation criteria are as follows.
[0190] <Evaluation Criteria> The time it takes for PLQY to decay to 90% of its initial value was defined as T90, and it was evaluated according to the following criteria: PLQY T90: A: 120 hours or more B: 100 hours or more but less than 120 hours C: 90 hours or more but less than 100 hours D: Less than 90 hours
[0191]
[0192] According to Table 4, the wavelength conversion layers 550-1 to 550-13 in Examples 27 to 39 have high PLQY T90 values under blue light irradiation conditions. This is thought to be because, in the wavelength conversion layer according to the present invention, the shell-like coordination is easily coordinated to the nanoparticles and difficult to desorb. On the other hand, as shown in Comparative Example 5, when only the second side chain is included, coordination is easy but desorption is also easy, resulting in a low T90. Also, as shown in Comparative Example 6, when only the third side chain is included, desorption is difficult but coordination is difficult, resulting in a low T90.
[0193] The present invention is not limited to the embodiments described above, and various modifications and variations are possible without departing from the spirit and scope of the invention. Accordingly, the following claims are attached to make the scope of the invention public.
[0194] This application claims priority based on Japanese Patent Application No. 2025-081725, filed on 15 May 2025, and all of its contents are incorporated herein by reference.
[0195] 10 Nanoparticles 40 Multiple binding sites 45 Betaine group 50 Polymer portion 60 Shell-shaped ligand 61 First unit 62 Second unit 63 Third unit 100 Photoresponsive particle 100
Claims
1. A photoresponsive particle comprising: a nanoparticle having a perovskite-type crystalline structure containing iodine at the X site; and a shell-shaped ligand comprising a plurality of bonding portions including a structural unit having a betaine group; and a polymer portion coordinating to the nanoparticle at a plurality of locations via the plurality of bonding portions, wherein the shell-shaped ligand comprises a first unit having the betaine group and constituting the bonding portion; a second unit that reduces the rigidity of the polymer portion; and a third unit that increases the rigidity of the polymer portion.
2. The photoresponsive particle according to claim 1, wherein the second unit constitutes the polymer portion and promotes the coordination of the betaine group to the nanoparticles, and the third unit constitutes the polymer portion and suppresses the detachment of the betaine group from the nanoparticles.
3. A photoresponsive particle comprising: a nanoparticle having a perovskite-type crystalline structure containing iodine at the X site; and a shell-shaped ligand comprising a plurality of binding portions including a structural unit having a betaine group, and a polymer portion that coordinates to the nanoparticle at a plurality of locations via the plurality of binding portions, wherein the shell-shaped ligand comprises a first unit having the betaine group and constituting the binding portion, a second unit constituting the polymer portion and promoting the coordination of the betaine group to the nanoparticle, and a third unit constituting the polymer portion and suppressing the detachment of the betaine group from the nanoparticle.
4. The photoresponsive particle according to claim 1 or 3, wherein the polymer portion comprises a main skeleton, a first side chain bridging the betaine group and the main skeleton, a second side chain that reduces the rigidity of the polymer portion and constitutes the second unit, and a third side chain that increases the rigidity of the polymer portion and constitutes the third unit.
5. The photoresponsive particle according to claim 4, wherein the second side chain has four or more rotatable bonds, and the third side chain has three or fewer rotatable bonds.
6. The photoresponsive particle according to claim 5, wherein the second side chain has a number of rotatable bonds that is 4 or more greater than the number of rotatable bonds of the third side chain.
7. The photoresponsive particle according to claim 5, wherein the number of rotatable bonds is the number of rotatable single bonds contained within the molecule, excluding bonds with hydrogen atoms, terminal single bonds excluding bonds with hydrogen atoms, and partial bonds in cyclic structures.
8. The photoresponsive particle according to claim 4, wherein the second side chain and the first side chain are arranged in series from the main skeleton to the nanoparticle.
9. A photoresponsive particle comprising: a nanoparticle having a perovskite-type crystalline structure containing iodine at the X site; and a shell-shaped ligand comprising a plurality of binding portions including a structural unit having a betaine group, and a polymer portion bound to the nanoparticle at a plurality of locations via the plurality of binding portions, wherein the shell-shaped ligand comprises a first unit having the betaine group and constituting the binding portion, a second unit constituting the polymer portion and promoting the coordination of the betaine group to the nanoparticle, and a third unit constituting the polymer portion and suppressing the detachment of the betaine group from the nanoparticle.
10. The photoresponsive particle according to claim 1 or 9, wherein the nanoparticle further contains bromine at the X site.
11. The photoresponsive particle according to claim 1 or 9, wherein the nanoparticle contains at least one of a monovalent ammonium cation, a monovalent nitrogen-containing organic compound cation, or a monovalent alkali metal cation at site A, and at least one of a divalent transition metal cation and a divalent typical metal cation at site B.
12. A photoresponsive particle according to claim 1 or 3, which has the property of emitting secondary light with a longer wavelength than the primary light upon irradiation with primary light as a photoresponsive property.
13. A photoresponsive material comprising the photoresponsive particles according to claim 1 or 9, and a medium interposed between the photoresponsive particles.
14. A polymerizable composition comprising the photoresponsive material described in claim 13 and a polymerizable compound.
15. The polymerizable composition according to claim 14, comprising a polymerization initiator.
16. A photoresponsive cured product comprising the photoresponsive material according to claim 14 and a polymer derived from the polymerizable compound.
17. A wavelength conversion layer comprising a light-receiving surface optically coupled to a light source, wherein the photoresponsive cured material according to claim 16 is arranged in layers.
18. A wavelength conversion element comprising a plurality of sets of wavelength conversion layers according to claim 17, each having a different halogen composition located at the X site.