Inspection device, inspection method, manufacturing system, and manufacturing method
The hyperspectral camera-based inspection apparatus addresses solvent residue detection in coating processes for solar cells, enhancing process efficiency and quality by allowing real-time feedback to adjust film-forming conditions.
Patent Information
- Application Number
- PCT/JP2026/017082
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-19
AI Technical Summary
Existing manufacturing processes for organic and perovskite solar cells using coating methods fail to detect solvent residue until the final product is completed, leading to functional failures and process inefficiencies due to the inability to inspect the drying state of the coating film, resulting in significant losses and quality issues.
An inspection apparatus and method using a hyperspectral camera to analyze the residual state of solvent on a substrate by illuminating and imaging the coated film, allowing for real-time detection and feedback to adjust film-forming conditions.
Enables real-time inspection of solvent residue, reducing defects by identifying problematic layers early in the process, improving productivity and quality control by adjusting film-forming conditions based on inspection results.
Smart Images

Figure JP2026017082_19112026_PF_FP_ABST
Abstract
Description
Inspection apparatus, inspection method, manufacturing system, and manufacturing method
[0001] The present disclosure relates to an inspection apparatus, an inspection method, a manufacturing system, and a manufacturing method.
[0002] Against the backdrop of cost reduction in device manufacturing, production via coating methods including inkjet, in addition to vacuum film formation, has become feasible. As representative devices in this field, with the recent emergence of organic solar cells and perovskite solar cells in the solar cell sector, manufacturing by coating processes has drawn increasing attention, and is disclosed in, for example, Non-Patent Document 1 and Patent Document 1.
[0003] Manufacturing using these coating methods has attracted attention for improving productivity through roll-to-roll production, which enables continuous coating film formation.
[0004] Furthermore, unlike vacuum processes, devices such as organic electroluminescent (EL) elements, organic solar cells, and perovskite solar cells that form films via coating methods are composed of organic substances. This creates a problem: if moisture or solvent is incorporated during film formation, the electrical conductivity is impaired, which in turn causes functional failures. Conventionally, glass substrates have been used to block such external moisture. In recent years, for flexible applications and the associated roll-to-roll manufacturing methods, an invention of forming a barrier film for blocking moisture on an optical film is disclosed in, for example, Patent Document 2.
[0005] In addition, in the case of coating film formation, not only water-based coating but also solvent-based coating may leave residual solvent in the coated film. Products formed by, for example, further stacking a coating layer on top in this state are rejected as defective after product performance measurement to prevent them from reaching the market. However, defects cannot be detected unless the product is completed for performance inspection. Moreover, since process adjustments are fed back based on these product inspections, it is impossible to identify which layer caused the problem, leading to the issue that all previously manufactured products or intermediate products in the manufacturing process become defective.
[0006] Furthermore, determining whether the cause of solvent residue was a defect in the substrate itself, due to the surface condition, or due to the equipment or process conditions of the drying oven required failure analysis of samples taken from multiple locations, followed by implementation of countermeasures and verification of their effectiveness through remanufacturing. This method also had the problem of requiring a significant amount of time and incurring substantial losses in resolving defects.
[0007] Japanese Patent Publication No. 2001-156307, Japanese Patent Publication No. 2008-235139, Japanese Patent Publication No. 2002-062266
[0008] Riki Miyasaka, "The Emergence of Perovskite Solar Cells," Modern Chemistry, March 2014, pp. 24-29.
[0009] This invention was made in view of the above-mentioned problems and circumstances. In functional devices made of organic films, the function tends to deteriorate if solvent remains on the films. For example, in electrically conductive organic films, it is known that excessive solvent residue reduces electrical conductivity and causes malfunctions, and there is a need for a technology to inspect the drying state of the coating film. However, as in Patent Document 3, for example, while coating defects can be inspected, the drying state of the coating film cannot be inspected, and the only way to prevent market leakage was to control process conditions and inspect the final product state.
[0010] The problem addressed by this disclosure is to provide an inspection device, inspection method, manufacturing system, and manufacturing method that can inspect the residual state of solvent in a workpiece coated and formed on a substrate.
[0011] To solve the above problems, the inspection apparatus of the present disclosure is an inspection apparatus for inspecting an object to be inspected that has been coated and formed on a substrate, comprising: an illumination unit for illuminating the object to be inspected; a first imaging unit having at least one hyperspectral camera for imaging the illuminated object to be inspected and acquiring spectral data at predetermined positions on the object to be inspected; and an analysis unit for analyzing the residual state of solvent at predetermined positions on the object to be inspected based on the acquired spectral data.
[0012] The inspection method of this disclosure is an inspection method for inspecting an object to be inspected that has been coated and formed on a substrate using the above inspection apparatus, comprising: an illumination step of illuminating the object to be inspected; a first imaging step of imaging the illuminated object to be inspected and acquiring spectral data at a predetermined position on the object to be inspected; and an analysis step of analyzing the residual state of solvent at a predetermined position on the object to be inspected based on the acquired spectral data.
[0013] The manufacturing system of this disclosure comprises a film-forming apparatus for manufacturing a film on the substrate, and the inspection apparatus.
[0014] The manufacturing method disclosed herein is a method for manufacturing a film on a substrate using the above manufacturing system, comprising: a film-forming step for manufacturing a film on the substrate; and an inspection step for inspecting the film manufactured on the substrate, wherein the film-forming conditions in the film-forming step are changed based on the inspection results obtained in the inspection step.
[0015] According to this disclosure, the residual state of solvent in an object coated and formed on a substrate can be inspected.
[0016] This is a schematic diagram of the manufacturing system of this embodiment. This is a block diagram showing the schematic configuration of the manufacturing system of this embodiment. This is a schematic diagram showing the configuration of the optical system in a hyperspectral camera. This is a diagram illustrating the region imaged by the first imaging unit. This is a flowchart of the manufacturing method of this embodiment. This is a flowchart of the film formation process according to this embodiment. This is a flowchart of the inspection process according to this embodiment. This is a flowchart of the manufacturing method. This is a diagram illustrating the phenomenon of solvent remaining on the object under inspection. This is a diagram showing the inspection results at a predetermined position on the object under inspection. This is a diagram showing the relationship between the amount of remaining solvent and the drying time. This is a diagram showing the relationship between the intensity of the absorption spectral peak specific to the solvent and the time. This is a diagram showing the relationship between the solvent remaining limit and the spectral peak tolerance limit. This is a diagram showing an example of applying feedback to the drying temperature and drying time when the allowable remaining amount is exceeded. This is a diagram showing an example of solvent detection by the difference from the spectral intensity of the material.
[0017] Hereinafter, one or more embodiments of this disclosure will be described with reference to the drawings. However, the scope of this disclosure is not limited to the disclosed embodiments.
[0018] [Manufacturing System] Figure 1 is a schematic diagram of the manufacturing system 100 of this embodiment. Figure 2 is a block diagram showing the schematic configuration of the manufacturing system 100 of this embodiment. The manufacturing system 100 of this embodiment includes a film-forming apparatus 10 for forming a film on a substrate, and an inspection apparatus 20 for inspecting the formed film as an object to be inspected.
[0019] (Film-forming apparatus) The film-forming apparatus 10 includes a coating section 6, a drying section 7, a transport section 8, a first display section 11, a first operation section 12, and a first control section 13.
[0020] The shape of the film produced in this embodiment, i.e., the object to be inspected 102, is not particularly limited and may be short or long. Furthermore, if the film is long, it may be transported as shown in Figure 1. The type of film produced in this embodiment is not particularly limited and may be an organic film mainly containing organic compounds, or an inorganic film mainly containing inorganic compounds.
[0021] The coating unit 6 applies a coating liquid 103 containing the film material onto the transported substrate 101. The coating unit 6 is not particularly limited as long as it has the function of applying the coating liquid. Examples of coating methods include spray coating, spin coating, blade coating, dip coating, casting, roll coating, bar coating, die coating, and printing. Examples of printing methods include inkjet printing. The coating method is preferably selected according to the composition and physical properties of the coating liquid.
[0022] In the inkjet method, the ejection method from the inkjet head may be either an on-demand method or a continuous method. The inkjet head in the on-demand method may be an electromechanical conversion method or an electro-thermal conversion method. Examples of electromechanical conversion methods include single-cavity type, double-cavity type, bender type, piston type, shear-mode type, and shared-wall type. Examples of electro-thermal conversion methods include thermal inkjet type and bubble jet (registered trademark) type.
[0023] The drying unit 7 dries the coating liquid 103 on the transported substrate 101 to complete the production of the film 102. The drying unit 7 is not particularly limited as long as it has the function of drying the coating liquid. Drying removes the solvent contained in the coating liquid, and a dry film is obtained. Drying methods include irradiation with hot air, infrared rays, microwaves, etc. In addition, although not shown in the figures, a heating roll may be provided on the substrate 101 side.
[0024] The drying temperature is preferably in the range of 60 to 200°C. The drying temperature is preferably increased in stages. The drying time is preferably in the range of 5 to 60 minutes, and more preferably in the range of 10 to 30 minutes. The drying time is preferably adjusted appropriately according to the drying temperature.
[0025] The transport unit 8 transports the substrate 101 in a first direction. The transport speed of the transport unit 8 is not particularly limited, but is preferably in the range of 1 to 100 m / min. The transport unit 8 may be equipped with a device for removing the protective film adhering to the substrate 101 immediately before film formation. It may also be equipped with a device for applying a protective film to the manufactured film after inspection. In this embodiment, for example, a roll-shaped substrate 101 may be fed out and a film may be formed on the substrate, and the laminate after film formation may be wound back into a roll shape. In this case, the transport unit 8 may be equipped with a device for feeding out the roll-shaped substrate 101 and a device for winding the laminate after film formation into a roll shape.
[0026] The film-forming apparatus 10 may, if necessary, be equipped with a dry cleaning device that irradiates the surface with plasma, ozone, ultraviolet light, etc., to remove unwanted organic matter adhering to the surface. By providing such a device, the polymerization reaction of the resin can be accelerated. The position of such a device is not particularly limited and may be between the coating section 6 and the drying section 7, or between the drying section 7 and the first illumination section 1.
[0027] Furthermore, the film-forming apparatus 10 may also be equipped with a wet cleaning apparatus. The wet cleaning method involves selecting and combining liquids such as pure water cleaning, acid cleaning, and alkaline cleaning according to the object to be removed, but these can also be combined according to the object to be removed. In addition, the wet cleaning apparatus may be combined with physical cleaning apparatus such as scrub cleaning, two-fluid cleaning, and ultrasonic cleaning. When these cleaning apparatuses are provided, they may normally be placed in front of the coating section 6, or the substrate may be brought to the film-forming apparatus 10 after being cleaned in a different cleaning apparatus beforehand.
[0028] The first display unit 11 and the first operation unit 12 are equipped with, for example, a liquid crystal display (LCD) with a touch panel. The first display unit 11 displays various operation screens, coating conditions, drying conditions, inspection data, etc., according to signals input from the first control unit 13. The first operation unit 12 is equipped with various operation keys such as a numeric keypad and a start key, and accepts various input operations from the user and outputs signals to the first control unit 13.
[0029] The first control unit 13 includes a CPU, RAM, memory, etc. The CPU is a hardware processor that controls the operation of each part of the film deposition apparatus by reading various programs stored in memory, loading them into RAM, and executing various processes according to the loaded programs.
[0030] (Inspection device) The inspection device 20 includes a first illumination unit 1, a first imaging unit 2, a second illumination unit 3, a second imaging unit 4, a position coordinate assignment unit 5, a second display unit 21, a second operation unit 22, and a second control unit 23.
[0031] The first illumination unit 1 illuminates the area of the film (object under inspection) 102 fabricated on the substrate 101 that is imaged by the first imaging unit 2. The light source for the first illumination unit 1 is not particularly limited, but it is preferably a white light source or a light source that illuminates only with light in a specific wavelength range. The wavelength range of the light is preferably in the range of 380 to 1000 nm. Depending on the application, a light source on the shorter wavelength side or a light source on the longer wavelength side may also be used. As a light source on the shorter wavelength side, a UV light source in the wavelength range of 200 to 400 nm can be used, and as a light source on the longer wavelength side, a mid-infrared light source in the wavelength range of 2 to 20 μm can be used. However, when these mid-infrared light sources of 2 μm or more are incident, the light source will be incident with heat, causing a change in the amount of moisture due to the incident heat, which causes a slight change in the surface state, so it is preferable to use a light source of 2 μm or less.
[0032] Preferably, the light emitted from the first illumination unit 1 is incident on the surface of the object under inspection 102 within the imaging area at a 45-degree angle and reflected at a 90-degree angle. In this case, it is preferable that the reflected light is incident on the first imaging unit 2 perpendicularly.
[0033] The first illumination unit 1 is not particularly limited, but examples include LED (Light Emitting Diode) elements. The first illumination unit 1 may consist of a single LED or multiple LEDs. Other examples of the first illumination unit 1 include halogen lamps, xenon lamps, deuterium lamps, thermal light sources, and laser continuum light sources.
[0034] The first illumination unit 1 may use an LED with a wide wavelength range, or it may use multiple LEDs with different wavelength ranges. When multiple LEDs with different wavelength ranges are used as the first illumination unit 1, the first imaging unit 2 may acquire data for each wavelength range by controlling the emission timing of the multiple LEDs. In the example shown in Figure 1, the first illumination unit is equipped with four LEDs 1a to 1d. In addition, the first illumination unit 1 may use a visible light LED or an infrared light LED. The light emitted from the first illumination unit 1 is preferably monochromatic light, but it may also be scattered light.
[0035] The first illumination unit 1 is preferably, for example, a UVA light source with a wavelength of 320 to 400 nm, a visible light source including a white LED that emits light in the 420 to 800 nm range, or a halogen light source that emits light in the 800 to 2500 nm range. If the spectrum of the solvent is known in advance, the first illumination unit 1 may be a light source with a specific wavelength that allows only those spectra to be easily observed. Many solvents are materials that have an absorption spectrum in the ultraviolet range, and the presence or absence of a solvent can be detected by applying ultraviolet light to the illumination. However, objects made of organic materials in particular are damaged by ultraviolet light, resulting in destructive testing, so it is preferable to use a light source other than ultraviolet. In addition, by setting the wavelength of the irradiated light to 2000 nm or less, incident heat can be suppressed, and changes in the residual state of the solvent due to the irradiated light can be reduced, so inspection can be performed with high accuracy. Specifically, the near-infrared irradiated halogen lamp TH-200X30CIR manufactured by CCS Corporation, which emits light in the range of wavelengths from 800 nm to 2400 nm, can be used.
[0036] The first imaging unit 2 images the object under inspection 102 illuminated by the first illumination unit 1 and acquires spectral data at a predetermined position on the object under inspection 102. The first imaging unit 2 has at least one hyperspectral camera. In addition, if a mark representing position coordinates is provided on the substrate 101, the first imaging unit 2 images this mark.
[0037] A hyperspectral camera can simultaneously acquire two-dimensional or three-dimensional positional information and spectral information split into dozens or more bands. This allows for the acquisition of spectral information in multiple wavelength regions, from ultraviolet to infrared. The wavelength range is preferably within 400 to 1000 nm. The acquired spectrum may be reflection, absorption, or transmission. The spacing between the bands (wavelength regions) of the spectral spectrum is preferably within the range of 0.5 to 10 nm.
[0038] Figure 3 is a schematic diagram showing the configuration of the optical system in the hyperspectral camera 71. The following description will focus on a line-scan type hyperspectral camera 71, but a snapshot type hyperspectral camera may also be used in this embodiment. Furthermore, while a diffraction grating 76 is used as the spectrometer in this embodiment, a prism may also be used.
[0039] The hyperspectral camera 71 includes a scan line 72, an objective lens 73, a slit 74, a collimator lens 75, a diffraction grating 76, a focusing lens 77, an image sensor 78, and the like. The image sensor 78 includes multiple photodiodes.
[0040] The hyperspectral camera 71 captures light incident from the object under inspection 102 onto the scan line 72 and acquires spectral information. The objective lens 73 forms an image of the light from the scan line 72 in the slit 74. The light formed in the slit 74 is spectrally separated into multiple bands (wavelength regions) by the collimator lens 75 and the diffraction grating 76, and then sequentially arranged and imaged on the image sensor 78 by the focusing lens 77. Multiple photodiodes in the image sensor 78 each receive images of light corresponding to multiple bands and output them as an image.
[0041] Examples of hyperspectral cameras that can be used in this embodiment include the FX10, FX17, and GX17 (manufactured by SPEECIM). Alternatively, the FX50 and FX120 (manufactured by SPEECIM) may also be used in combination as hyperspectral cameras. This allows for the acquisition of spectral information over a wide wavelength range.
[0042] FIG. 4 is a diagram for explaining the region imaged by the first imaging unit 2. The imaging region 104 is the region imaged by the first imaging unit 2. Note that when the first imaging unit 2 includes a plurality of hyperspectral cameras, the "imaging region" refers to the entire region imaged by the plurality of hyperspectral cameras. When the first imaging unit 2 includes only one hyperspectral camera, the "imaging region" refers to the region imaged by the single hyperspectral camera. A direction perpendicular to the first direction and parallel to the conveyance surface is defined as a second direction. Further, a direction perpendicular to both the first direction and the second direction is defined as a third direction (not shown). The hyperspectral camera preferably captures an image from the third direction, that is, images the inspection object 102 from the vertically upper direction.
[0043] In the present embodiment, the length of the entire imaging region 104 in the second direction is preferably longer than the length of the inspection object 102 in the second direction. That is, the hyperspectral camera is preferably capable of imaging the inspection object 102 all at once across the second direction. In addition, by performing imaging over time as the inspection object 102 is conveyed, imaging can be performed across the first direction. As a result, the hyperspectral camera can image the entire inspection object 102 and acquire spectral data.
[0044] The first imaging unit 2 may include a plurality of hyperspectral cameras. By arranging the plurality of hyperspectral cameras in the first direction, sufficient imaging can be performed without omission within the imaging region even at a high conveyance speed. Further, by arranging the plurality of hyperspectral cameras in the second direction, sufficient imaging can be performed even when the imaging region 104 is a wide area.
[0045] When the first imaging unit 2 includes a plurality of hyperspectral cameras, the following formula (1) is preferably satisfied. Formula (1): Z / n ≤ Y / X Here, each symbol in formula (1) is as follows. X: Conveyance speed of the inspection object in the first direction Y: Length of the imaging region per hyperspectral camera in the first direction Z: Exposure time required for one hyperspectral camera to image the imaging region n: Number of the hyperspectral cameras
[0046] In the above formula (1), it is assumed that the first imaging unit 2 includes a plurality of hyperspectral cameras of the same type, in which the elements represented by Y and Z are respectively the same. In this case, it is understood that even if the conveyance speed X is high, the requirement can be met by increasing the number n of the cameras. Also in the case where a plurality of hyperspectral cameras not of the same type are provided, similarly, even if the conveyance speed is high, the requirement can be met by increasing the number of the cameras.
[0047] The second illumination unit 3 illuminates a region of a film (inspection object) 102 formed on a substrate 101, which is to be imaged by the second imaging unit 4. The light source serving as the second illumination unit 3 is not particularly limited, but is preferably a white light source or a light source that performs illumination only with light in a specific wavelength region. The wavelength region of the light is preferably in the range of 400 to 800 nm. As the second illumination unit 3, those described for the first illumination unit 1 above can be used.
[0048] The second imaging unit 4 images the inspection object 102 illuminated by the second illumination unit 3. In addition, in a case where a mark representing position coordinates is provided on the substrate 101, the second imaging unit 4 images this mark. From the viewpoint of capturing a transmission image and a reflection image of the light illuminated by the second illumination unit 3, a total of two second imaging units 4 may be provided on both sides of the inspection object 102. The second imaging unit 4a located on the same side as the second illumination unit 3 with respect to the inspection object 102 can capture a reflection image, and the second imaging unit 4b located on the opposite side to the second illumination unit 3 can capture a transmission image. The second imaging unit 4 is not particularly limited as long as it is an apparatus capable of imaging the inspection object 102, but is preferably a visible light camera. Thereby, imaging data of the inspection object 102 with visible light is obtained. As the visible light camera, for example, LSC6000 (manufactured by MEC Co., Ltd.) can be used.
[0049] The position coordinate providing unit 5 imparts a mark representing position coordinates to the substrate 101 being conveyed. The method of imparting the mark is not particularly limited, and the mark is printed on the substrate by, for example, an inkjet method, a laser method, or the like. For example, in a case where a coating liquid is applied using an inkjet head as the application unit 6 of a film forming apparatus, the inkjet head may also be used as the position coordinate providing unit 5. Thereby, it is not necessary to newly provide an apparatus as the position coordinate providing unit, and the entire system can be downsized.
[0050] The second display unit 21 and the second operation unit 22 are equipped with, for example, a liquid crystal display (LCD) with a touch panel. The second display unit 21 displays various operation screens, inspection result data, etc., according to signals input from the second control unit 23. The second operation unit 22 is equipped with various operation keys such as a numeric keypad and a start key, and accepts various input operations from the user and outputs signals to the second control unit 23.
[0051] The second control unit 23 includes a CPU, RAM, memory, etc. The CPU is a hardware processor that controls the operation of each part of the inspection device by reading various programs stored in memory, loading them into RAM, and executing various processes according to the loaded programs.
[0052] The user may change the film-forming conditions, such as coating conditions, drying conditions, and transport conditions, based on the inspection result data displayed on the second display unit 21. The second control unit 23 may also transmit the inspection result data to the film-forming apparatus 10 via the communication unit. The film-forming apparatus 10 may change the film-forming conditions, such as coating conditions, drying conditions, and transport conditions, based on the received inspection result data. The manufacturing system 100 may also include a management device (not shown). The management device receives the inspection result data from the inspection device 20 via the communication unit. The management device may change the film-forming conditions, such as coating conditions, drying conditions, and transport conditions, based on the received inspection result data, and transmit the changed film-forming conditions to the film-forming apparatus 10.
[0053] [Manufacturing Method] Figure 5 is a flowchart of the manufacturing method according to this embodiment. When manufacturing begins, first the user creates a film on the substrate (first film formation step S1). Next, the user inspects the created film (inspection step: S2). Next, the user determines whether the obtained inspection result is outside the acceptable range (inspection result determination step S3). If the user determines that it is within the acceptable range (S3: NO), the user continues film formation (second film formation step S6). If the user determines that it is outside the acceptable range (S3: YES), the user determines whether to change the film formation conditions based on the inspection result (condition change determination step S4). If the user decides not to change the conditions (S4: NO), the user continues film formation (second film formation step S6). If the user decides to change the conditions (S4: YES), the user changes the film formation conditions (condition change step S5), and then continues film formation (second film formation step S6). Next, the user determines whether to terminate film formation or not (termination determination step S7). If the user decides not to terminate (S7: YES), they proceed to step S2 and inspect the fabricated film. If the user decides to terminate (S7: NO), they terminate the manufacturing process.
[0054] (Film Forming Process) Figure 6 is a flowchart showing the film forming process according to this embodiment. The procedure in the first film forming process S1 and the second film forming process S6 is the same, as shown in the flowchart of Figure 6. When film forming is started, the first control unit 13 of the film forming apparatus 10 instructs the coating unit 6 to apply the coating liquid 103 onto the substrate 101 (coating process S11). Next, the first control unit 13 instructs the drying unit 7 to dry the coating liquid 103 applied onto the substrate 101 (drying process S12), and ends the operation.
[0055] The substrate 101 is not particularly limited and may be a resin film mainly containing organic compounds, or a glass sheet mainly containing inorganic compounds. If the substrate 101 is a glass substrate, it is preferably a smooth, non-alkali glass substrate. As the substrate 101, Eagle XG (manufactured by Corning) can be used. From the viewpoint of reducing the adhesion of foreign matter, the substrate 101 may be protected with a protective film until immediately before film formation. In this case, the protective film is removed from the substrate 101 immediately before film formation to expose the coated surface of the substrate 101.
[0056] The substrate 101 may be cleaned immediately before film formation from the viewpoint of removing foreign matter. The cleaning may be dry cleaning or wet cleaning. The cleaning method may be the method described in Japanese Patent Application Publication No. 2021-67193. In this case, it is preferable to remove the moisture adhering during cleaning by drying or the like, and then perform the coating step S11.
[0057] (Inspection Process) Figure 7 is a flowchart showing the inspection process according to this embodiment. When the inspection is started, the second control unit 23 of the inspection device 20 instructs the first illumination unit 1 to illuminate the area of the object to be inspected 102 to be imaged by the first imaging unit 2 (first illumination process S21). Next, the second control unit 23 instructs the first imaging unit 2 to image the object to be inspected 102 illuminated by the first illumination unit 1 and to acquire spectral data at a predetermined position of the object to be inspected 102 (first imaging process S22). Finally, the second control unit 23 analyzes the defective areas based on the acquired imaging data and spectral data (analysis process S23). At this time, the second control unit 23 functions as an analysis unit. Details of the analysis will be described later. After that, the second control unit 23 terminates its operation.
[0058] In this embodiment, first, marks representing position coordinates are applied to the substrate 101 before film formation. Then, the first imaging unit 2 and the second imaging unit 4 each capture images of the marks and the object under inspection 102, and the captured data is analyzed. This allows the analysis results at predetermined positions on the object under inspection 102 to be linked with the images captured by the second imaging unit 4, based on the marks captured by the first imaging unit 2 and the marks captured by the second imaging unit 4. As a result, the user can compare the inspection results of the object under inspection 102 with information that can be confirmed by visual inspection.
[0059] Figure 8 is a flowchart showing the manufacturing method in this case. When manufacturing begins, the second control unit 23 of the inspection apparatus 20 instructs the position coordinate assignment unit 5 to assign marks representing position coordinates to the transported substrate 101 (position coordinate assignment step S31). Next, the first control unit 13 of the film forming apparatus 10 instructs the coating unit 6 to apply the coating liquid 103 onto the substrate 101 (coating step S32). Next, the first control unit 13 instructs the drying unit 7 to dry the coating liquid 103 applied onto the substrate 101 (drying step S33). Next, the second control unit 23 of the inspection apparatus 20 instructs the first illumination unit 1 to illuminate the area of the object to be inspected 102 to be imaged by the first imaging unit 2 (first illumination step S34). Next, the second control unit 23 instructs the first imaging unit 2 to image the object to be inspected 102 illuminated by the first illumination unit 1 and to acquire spectral data at a predetermined position of the object to be inspected 102 (first imaging step S35). Next, the second control unit 23 instructs the second illumination unit 3 to illuminate the area of the object under inspection 102 to be imaged by the second imaging unit 4 (second illumination step S36). Next, the second control unit 23 instructs the second imaging unit 4 to image the object under inspection 102 illuminated by the second illumination unit (second imaging step S37). Finally, the second control unit 23 analyzes the defective areas based on the data acquired by the first imaging unit 2 and the data acquired by the second imaging unit 4 (analysis step S38). After that, the second control unit 23 terminates its operation.
[0060] The details of the analysis will now be explained. In this embodiment, "residual solvent state" refers to whether or not solvent remains in the film, which is the object under inspection 102, and the amount of solvent remaining. The amount of solvent remaining may be expressed as a relative amount within the inspection area of the object under inspection 102. When solvent remains in the film, the material composition changes, which causes a change in the function of the film. In particular, the functional layers provided in solar cells and organic electroluminescent elements have electrical conductivity and are susceptible to the effects of solvent. Furthermore, in areas where solvent remains, thickness variations, defects, etc., are also likely to occur, which causes a change in the function of the film. Therefore, by reducing the amount of solvent remaining in the film, the desired electrical conductivity can be obtained.
[0061] Figure 9 illustrates the phenomenon of solvent residue remaining on the object under inspection 102. In Figure 9, the coated surface of the substrate 101 is protected by a protective film 31. Immediately before film formation, the protective film 31 is removed from the substrate 101 by a separator 32. After the protective film 31 is removed, the substrate 101 is dry-cleaned by a cleaning unit 33. Subsequently, the coating liquid is applied to the dry-cleaned substrate 101 by a coating unit 6. The coating liquid is dried by a drying unit 7, and the object under inspection 102 is formed on the substrate 101.
[0062] The following factors g to i can be cited as reasons for solvent remaining on the inspected object 102. Note that g to i correspond to g to i in Figure 9. g. Insufficient drying: Drying is insufficient. If the drying temperature is uneven or the transport speed is too fast, drying is likely to be insufficient. Insufficient drying in products requiring low-temperature processes is likely to cause unevenness, affect subsequent processes, and environmental problems. h. Defect sites: If there are defect sites in the film, solvent is likely to enter and remain there. This results in spot defects. i. Uneven coating: If the coating liquid cannot be applied uniformly, uneven coating occurs, resulting in partial insufficient drying. This can lead to problems after coater condition setting and maintenance, and insufficient robustness.
[0063] In this embodiment, the inspection is performed after the coating solution has dried and the film has been formed. This allows for an appropriate analysis of the residual state of the solvent that may affect the quality of the final film.
[0064] When solvent remains on the object under inspection 102, functional groups derived from the solvent are introduced at the molecular level. Each functional group has a peak wavelength. Therefore, the remaining state of the solvent can be analyzed from the spectral data acquired by the hyperspectral camera. Furthermore, the spectral data includes transmission or reflectance data in the light absorption band, and this transmission or reflectance changes depending on the type and number of functional groups, i.e., the remaining state of the solvent. Therefore, by analyzing based on the transmission or reflectance data, it is possible to analyze not only whether solvent remains but also the amount remaining.
[0065] In analysis based on transmission or reflectance intensity data, it is preferable to compare the analysis with spectral data from a state where no solvent remains, using reference data. In other words, it is preferable to analyze the remaining solvent state based on the difference in peak values between the transmission or reflectance intensity data of the object 102 under inspection in a state where no solvent remains and the transmission or reflectance intensity data at a predetermined position on the object 102 under inspection, or based on the value obtained by integrating the spectral difference over the inspection area. By integrating the difference in transmission or reflectance intensity data over the entire inspection area and analyzing the integrated value, the relative remaining solvent state within the object 102 under inspection can be analyzed. By analyzing the relative remaining solvent state, analysis can be performed even if the remaining amount is minute. Furthermore, even if the wavelength of the absorption peak that changes due to the solvent is not clear in the object 102 under inspection, analysis can be performed from the difference with the reference.
[0066] In this context, "no solvent remaining" refers to a state where no solvent remains at all, resulting in a remaining amount of 0, or a remaining amount that is extremely small. The transmission or reflectance intensity data for the inspected object 102 in a state where no solvent remains may be the data obtained in the inspection area that has the smallest or largest intensity value and represents the smallest remaining amount. Alternatively, the transmission or reflectance intensity data for the inspected object 102 in a state where no solvent remains may be obtained from a sample prepared individually. A sample can be obtained, for example, by preparing a film with the same composition as the inspected object 102 in advance, cutting out a portion of the film, and thoroughly drying the cut-out film. Furthermore, the transmission or reflectance intensity data for the inspected object 102 in a state where no solvent remains may also be theoretically determined transmission or reflectance intensity data.
[0067] Depending on the type of solvent, residual solvent in the first layer may react with or mix with the solvent in the second layer, damaging both layers. Normally, it is impossible to know whether a product is defective until the final product inspection is performed. In this embodiment, the presence or absence of residual solvent can be detected for each film produced, and after detection, feedback can be applied to the film formation conditions. As a result, it is possible to sort the product group into defective products and products that can be improved through process improvements at each stage, thereby reducing losses and improving productivity.
[0068] The second control unit 23 may associate and store the analysis results at a predetermined position on the object under inspection 102 with the image captured by the second imaging unit 4, based on the marks captured by the first imaging unit 2 and the marks captured by the second imaging unit 4.
[0069] Figure 10 shows the inspection results at a predetermined position of the object to be inspected 102. Specifically, Figure 10 shows the case where the analysis results obtained from imaging data and spectral data obtained by the first imaging unit 2 are displayed as an image. The example shown in Figure 10 is an example of the inspection results of a roll film. The roll length represents the position in the first direction from the reference point, and the width represents the position in the second direction. Areas enclosed by solid rectangles represent defective areas. Here, a "defective area" refers to an area where the residual amount of solvent per unit area exceeds the standard value, i.e., the residual amount per unit area exceeds the standard value. The size of the solid rectangle corresponds to the approximate size of the defective area. For each defective area, images captured by the second imaging unit 4, detailed data on the residual state (residual amount) of the defective area, etc., may be further registered.
[0070] The second control unit 23 of the inspection device 20 may warn the user of an abnormality if the size of the area of the defective area, the remaining amount, etc., are outside the acceptable range. The acceptable range for defective areas may be set in advance by the user. The second imaging unit 4 does not need to image the object under inspection throughout the entire process, and may select and image only the defective areas that are outside the acceptable range. In this case, when the second control unit 23 determines that a defective area is outside the acceptable range, it instructs the second imaging unit 4 to image the defective area that is outside the acceptable range.
[0071] If the size of the defective area, the amount remaining, etc., are outside the acceptable range, the film formation conditions such as coating conditions, drying conditions, and transport conditions may be changed accordingly. The composition of the coating solution may also be changed. By feeding back the inspection results and reflecting them in the film formation conditions, the number of defective areas can be reduced in real time, and the yield can be improved.
[0072] In this embodiment, the object to be inspected 102 is not particularly limited as long as it is coated and formed on the substrate 101. Furthermore, in this embodiment, the object to be inspected 102 can be sufficiently inspected even when being transported at high speed. Therefore, in a device obtained by stacking layers created by coating, inspection can be performed each layer after it is made, rather than after the device is manufactured. When inspecting after the device is manufactured, the entire device is inspected, making it difficult to determine which layer is responsible for the inspection result, but when inspecting each layer individually, it is relatively easy to determine the cause. Furthermore, in this embodiment, it is preferable to save the inspection results. By cutting each layer to the desired size, excluding defective areas, based on the saved data, the device is less likely to contain defective areas, and stable quality can be obtained in any device that is manufactured. Devices to which this embodiment can be applied include stacked solar cells, such as organic solar cells and perovskite solar cells, and stacked organic electroluminescent elements.
[0073] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples.
[0074] <Example 1> In this example, a substrate was prepared by intentionally forming a barrier film on a PET substrate. A functional layer was coated onto this substrate using the method described in Japanese Patent Application Publication No. 2019-212702. The relationship between the amount of remaining solvent and the drying time can be easily calculated or measured, including through simulations. Furthermore, by measuring in real time with a hyperspectral device, it is possible to observe the change in the solvent-specific peak value in response to the change in the amount of remaining solvent.
[0075] For coating, hydrocarbon solvents such as aliphatic hydrocarbons, alicyclic hydrocarbons, and aromatic hydrocarbons can be used. Halogenated hydrocarbon solvents can also be used. Other solvents such as aliphatic ethers and alicyclic ethers can also be used. In recent perovskite solar cells, solvents with an absorption band in the UV region, such as N,N-dimethylformamide (DMF), are preferred. Therefore, a hyperspectral camera capable of measuring the UV region is preferred. However, since the solvent itself contains materials and has an absorption band in the visible light region and a broad spectrum, a hyperspectral camera that measures the visible light region is also acceptable.
[0076] Figure 11 shows the relationship between the amount of solvent remaining and the drying time. It illustrates an example of the relationship between the amount of solvent remaining and the drying time, calculated by overlaying the results of measurements of the individual remaining amounts and drying times of multiple solvents using the existing gas chromatography method, thereby determining the total solvent drying time.
[0077] Figure 12 shows the relationship between the intensity of the solvent-specific absorption spectral peak and time. The fact that the peak value is not zero indicates that the spectrum of the coated material after drying is superimposed on the base spectrum.
[0078] Figure 13 shows the relationship between the residual limit of the solvent and the allowable limit of the spectral peak. Figure 13 is derived from the relationship shown in Figure 12. If the residual limit of the solvent is known in advance, the limit spectral peak value can be determined.
[0079] Using these relationships, measurements are taken on the film after coating and drying to determine whether any solvent remains. If solvent exceeding the acceptable limit is detected, hyperspectral spectroscopy data is saved. Although offline saving is acceptable after measurement, the hyperspectral image after analysis is saved, and a camera image of the same area is captured and saved. This ensures that even if a defect occurs during inspection after the device is completed, the causative process can be clearly identified from these results.
[0080] Furthermore, a program that increases the remaining amount, drying time, or drying temperature when the allowable remaining amount is exceeded can be pre-programmed and fed back into the drying process.
[0081] Figure 14 shows an example of applying feedback to drying temperature and drying time when the allowable residual amount is exceeded. For example, as shown in Figure 14, when the allowable residual amount is exceeded, it is possible to apply feedback to increase the drying temperature and, in this case, increase the drying time by changing the conveying speed, depending on the excess residual amount.
[0082] In detecting the presence or absence of residual substances, limiting the wavelength range to be inspected in advance can shorten the measurement or analysis time, and consequently reduce the number of hyperspectral cameras required. Although not described here, if a method is used in which coating is performed while preparing the coating solution, feedback can be provided to the preparation process to reduce the amount of solvent, etc., without changing the drying temperature or drying time.
[0083] <Example 2> In Example 1, the solvent spectrum was measured and feedback was performed, but the difference in the spectrum possessed by the coating material may also be used.
[0084] Figure 15 shows an example of solvent detection using the difference from the spectral intensity of the material. For example, as shown in Figure 15, in the case of a material having a spectral waveform specific to the vicinity of 700 nm, the coated film after drying has the highest peak value, while the material after coating containing the solvent becomes broader and the peak value decreases. By utilizing this difference, the presence or absence of residual solvent, or the amount of residual solvent, can be determined from the difference in the maximum peak values.
[0085] By pre-establishing a calibration curve for the remaining amount based on the difference, feedback can be provided to the process, similar to Example 1, allowing for adjustments to the coating film during the process.
[0086] Furthermore, although this method differs from the configuration example in Figure 1, it is also possible to measure the state of the coating liquid after application, before the drying process. In that case, it is possible to feed back the post-application feedback to the subsequent drying process, but since the accuracy of this method is insufficient, it is preferable to measure after the drying process, as in this embodiment.
[0087] The inspection apparatus 20 of this embodiment is an inspection apparatus for inspecting an object to be inspected 102 coated and formed on a substrate 101. The inspection apparatus 20 comprises an illumination unit (first illumination unit 1), a first imaging unit 2, and an analysis unit (second control unit 23). The illumination unit illuminates the object to be inspected 102. The first imaging unit 2 has at least one hyperspectral camera that images the illuminated object to be inspected 102 and acquires spectral data at predetermined positions on the object to be inspected 102. The analysis unit analyzes the residual state of the solvent at predetermined positions on the object to be inspected 102 based on the acquired spectral data. As a result, the inspection apparatus 20 can inspect the residual state of the solvent on the object to be inspected 102.
[0088] In this embodiment, the spectral data preferably includes transmission or reflectance data in the light absorption band. The analysis unit preferably analyzes the remaining state of the solvent based on the difference between the transmission or reflectance data of the object 102 under inspection when no solvent remains and the transmission or reflectance data at a predetermined position on the object 102 under inspection, based on the peak difference at a specific wavelength, or based on the value obtained by integrating the spectral difference in the inspection area. This allows the inspection device 20 to inspect the remaining state of the solvent in the object 102 under inspection more accurately.
[0089] In this embodiment, it is preferable that the first imaging unit 2 images the object to be inspected 102 as it is being transported in the first direction. When the second direction is defined as the direction perpendicular to the first direction and parallel to the transport surface of the object to be inspected 102, it is preferable that the length of the second direction in the entire imaging area of the first imaging unit 2 is longer than the length of the object to be inspected 102 in the second direction. This allows the first imaging unit 2 to image the entire object to be inspected 102 and acquire spectral data.
[0090] In this embodiment, the inspection device 20 preferably further comprises a position coordinate assignment unit 5 that assigns marks representing position coordinates on the substrate 101, and a second imaging unit 4 that images the object to be inspected 102. Preferably, the first imaging unit 2 and the second imaging unit 4 each image the marks and the object to be inspected 102, respectively. Preferably, the analysis unit associates the analyzed residual state of the solvent at a predetermined position on the object to be inspected 102 with the image captured by the second imaging unit 4, based on the marks captured by the first imaging unit 2 and the marks captured by the second imaging unit 4, and stores this information. This makes it possible to record the analysis results and captured images at predetermined position coordinates. Furthermore, when manufacturing devices or the like using the object to be inspected 102, it is possible to remove defective areas that are outside the acceptable range.
[0091] In this embodiment, it is preferable that the analysis unit instructs the second imaging unit 4 to image the object under inspection 102 when the analyzed residual state of the solvent is outside the acceptable range. This eliminates the need for the second imaging unit 4 to continuously image the object under inspection 102, and allows it to selectively image only the defective areas that are outside the acceptable range.
[0092] In this embodiment, it is preferable that the first imaging unit 2 is equipped with a plurality of hyperspectral cameras arranged in a first or second direction. This allows for sufficient imaging of the imaging area 104 without any omissions in the first direction, even at high transport speeds, and for sufficient imaging of the imaging area 104 even when it is wide in the second direction.
[0093] In this embodiment, the first imaging unit 2 is preferably equipped with a plurality of hyperspectral cameras arranged in a first direction. Let X be the transport speed of the object to be inspected 102 in the first direction. Let Y be the length of the imaging area in the first direction for each hyperspectral camera. Let Z be the exposure time required for one hyperspectral camera to image the imaging area. Let n be the number of hyperspectral cameras. In this case, it is preferable that the following equation (1) is satisfied. This allows the performance and number of hyperspectral cameras to be adjusted according to the transport speed, and enables sufficient imaging of the imaging area 104 without any omissions. Equation (1) Z / n ≤ Y / X
[0094] The inspection method of this embodiment is an inspection method for inspecting an object to be inspected 102 coated and formed on a substrate 101 using an inspection device 20. The inspection method comprises an illumination step (first illumination step S21), a first imaging step S22, and an analysis step S23. The illumination step illuminates the object to be inspected 102. The first imaging step S22 images the illuminated object to be inspected 102 and acquires spectral data at a predetermined position on the object to be inspected 102. The analysis step S23 analyzes the residual state of the solvent at a predetermined position on the object to be inspected 102 based on the acquired spectral data. As a result, the inspection method can inspect the residual state of the solvent on the object to be inspected 102.
[0095] The manufacturing system 100 of this embodiment includes a film-forming apparatus 10 for forming a film on a substrate 101 and an inspection apparatus 20. This allows the manufacturing system 100 to inspect the residual state of the solvent each time a film is formed.
[0096] The manufacturing method of this embodiment is a method for manufacturing a film on a substrate 101 using a manufacturing system 100. The manufacturing method includes a film formation step (first film formation step S1 and second film formation step S6) for forming a film on the substrate 101, and an inspection step S2 for inspecting the film formed on the substrate 101. The film formation conditions in the film formation step are changed based on the inspection results obtained in the inspection step S2. As a result, the manufacturing method can reduce the number of defects in the film produced.
[0097] The programs for executing each process in the inspection device, etc., may be stored on a portable recording medium. Furthermore, a carrier wave may be used as the medium for providing the program data via a communication line.
[0098] Furthermore, the detailed configuration and operation of each device constituting the inspection apparatus may also be modified as appropriate, without departing from the spirit of this disclosure.
[0099] This disclosure makes it possible to inspect the residual state of solvent in an object coated and formed on a substrate.
[0100] 1. First illumination unit 2. First imaging unit 3. Second illumination unit 4. Second imaging unit 5. Position coordinate assignment unit 6. Coating unit 7. Drying unit 8. Conveying unit 10. Film forming apparatus 20. Inspection apparatus 100. Manufacturing system 101. Substrate 102. Object to be inspected
Claims
1. An inspection apparatus for inspecting an object to be inspected that has been coated and formed on a substrate, comprising: an illumination unit for illuminating the object to be inspected; a first imaging unit having at least one hyperspectral camera for imaging the illuminated object to be inspected and acquiring spectral data at predetermined positions on the object to be inspected; and an analysis unit for analyzing the residual state of solvent at predetermined positions on the object to be inspected based on the acquired spectral data.
2. The inspection apparatus according to claim 1, wherein the spectral data includes transmission or reflection intensity data in the light absorption band, and the analysis unit analyzes the remaining state of the solvent based on the difference between the transmission or reflection intensity data of the object under inspection when no solvent remains and the transmission or reflection intensity data at a predetermined position on the object under inspection, based on the peak difference at a specific wavelength, or based on the value obtained by integrating the spectral difference in the inspection area.
3. The inspection apparatus according to claim 1 or 2, wherein the first imaging unit images the object to be inspected as it is transported in a first direction, and when the direction perpendicular to the first direction and parallel to the transport surface of the object to be inspected is defined as the second direction, the length of the second direction in the entire imaging area of the first imaging unit is longer than the length of the object to be inspected in the second direction.
4. The inspection apparatus according to claim 1 or 2, further comprising: a position coordinate assignment unit for assigning marks representing position coordinates to the substrate; and a second imaging unit for imaging the object to be inspected, wherein the first imaging unit and the second imaging unit each image the marks and the object to be inspected, and the analysis unit associates and stores the analyzed residual state of the solvent at a predetermined position on the object to be inspected with the image captured by the second imaging unit, based on the marks imaged by the first imaging unit and the marks imaged by the second imaging unit.
5. The inspection apparatus according to claim 4, wherein the analysis unit instructs the second imaging unit to image the object to be inspected when the analyzed residual state of the solvent is outside the acceptable range.
6. The inspection apparatus according to claim 3, wherein the first imaging unit comprises a plurality of hyperspectral cameras arranged in the first or second direction.
7. The inspection apparatus according to claim 3, wherein the first imaging unit comprises a plurality of hyperspectral cameras arranged in a first direction, and when X is the transport speed of the object to be inspected in a first direction, Y is the length of the imaging area in the first direction for each hyperspectral camera, Z is the exposure time required for each hyperspectral camera to image the imaging area, and n is the number of hyperspectral cameras, the following equation (1) is satisfied. Equation (1) Z / n ≤ Y / X 8. An inspection method for inspecting an object to be inspected that has been coated and formed on a substrate using the inspection apparatus described in claim 1 or claim 2, comprising: an illumination step of illuminating the object to be inspected; a first imaging step of imaging the illuminated object to be inspected and acquiring spectral data at a predetermined position on the object to be inspected; and an analysis step of analyzing the residual state of solvent at a predetermined position on the object to be inspected based on the acquired spectral data.
9. A manufacturing system comprising a film-forming apparatus for manufacturing a film on the substrate, and an inspection apparatus according to claim 1 or claim 2.
10. A method for manufacturing a film on a substrate using the manufacturing system described in claim 9, comprising: a film-forming step for manufacturing a film on the substrate; and an inspection step for inspecting the film manufactured on the substrate, wherein the film-forming conditions in the film-forming step are changed based on the inspection results obtained in the inspection step.