Quantum dot body, quantum dot composition, wavelength conversion material, and production methods therefor
A quantum dot composition with a semiconductor core, shell, and metal oxide coating modified by sodium monofluorophosphate addresses dispersibility and stability issues, ensuring high luminescence efficiency and reliability in polar solvents.
Patent Information
- Application Number
- PCT/JP2026/017167
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-19
AI Technical Summary
Existing quantum dots face issues with instability and poor dispersibility in polar solvents, leading to degradation of fluorescence emission properties and reduced luminescence efficiency, particularly in applications like color filters for displays.
A quantum dot composition is developed with a core of semiconductor nanoparticles, a shell of semiconductor nanoparticles, a metal oxide coating on the surface, and sodium monofluorophosphate modification to enhance dispersibility in polar solvents, maintaining high luminescence efficiency and stability.
The solution effectively suppresses aggregation and maintains high luminescence efficiency, improving dispersibility in polar solvents and enhancing the reliability of wavelength conversion materials.
Smart Images

Figure JP2026017167_19112026_PF_FP_ABST
Abstract
Description
Quantum dots, quantum dot compositions, and wavelength conversion materials, and methods for manufacturing the same.
[0001] This invention relates to quantum dots, quantum dot compositions, wavelength conversion materials, and methods for producing the same.
[0002] Quantum dots, composed of semiconductor particles with a particle size of nanoscale, have discrete energy levels due to the confinement of excitons generated by light absorption within nanoscale spaces, and their band gap depends on the particle size. As a result, quantum dots exhibit highly efficient fluorescence emission, and their emission spectra are sharpened. Furthermore, due to the characteristic that the band gap changes with particle size, they have the ability to control the emission wavelength, and are expected to have applications as wavelength conversion materials for solid-state lighting and displays (Patent Document 1).
[0003] Japanese Patent Publication No. 2012-022028, International Publication No. 2011 / 081037, Japanese Patent Publication No. 2010-523557
[0004] Quantum dots containing cadmium (Cd) and lead (Pb) are known to exhibit excellent fluorescence properties. However, because Cd and Pb are highly toxic to humans and the environment, restrictions on their use are being considered in various parts of the world, including under the European Union's RoHS directive. Therefore, quantum dots that do not contain these toxic elements are being investigated.
[0005] Furthermore, because quantum dots have a small particle size of nanometers, they have a large specific surface area, high surface energy, and are highly surface-active, making them prone to instability. Therefore, surface defects such as dangling bonds and oxidation reactions easily occur on the quantum dot surface, which degrades their fluorescence emission properties. Currently available quantum dots have these stability issues, and it is known that heat, humidity, and photoexcitation can cause degradation of their emission properties.
[0006] To prevent this degradation, organic or inorganic ligands called ligands are coordinated to the surface of synthesized quantum dots. This ligand coordination and passivation of defects suppresses the degradation of fluorescence emission efficiency.
[0007] Furthermore, as an implementation method using quantum dots as wavelength conversion materials, applications such as color filters used in displays have been proposed. When applying quantum dots to color filters, it is important to form quantum dot surface states suitable for the patterning method.
[0008] Currently, the photolithography method is the most commonly used method for producing color filters. This method involves coating a photosensitive resin composition containing pigments onto a glass substrate, drying the solvent, then exposing it to UV light as a mask, and removing the uncured portion by alkaline development to form a color pattern. This process is repeated to create blue, red, and green patterns. However, this photolithography method has many problems, including significant raw material loss due to the waste of uncured material, a complicated process, and the use of expensive equipment.
[0009] Therefore, inkjet technology has also been considered in recent years. With inkjet technology, there is no waste of raw materials, and it is possible to manufacture large-scale and large-area products without introducing expensive equipment, making it competitive in terms of cost. However, the technology to create fine nozzles is difficult, and as the nozzles become smaller, problems such as clogging and unstable ejection occur. For miniaturization, both photolithography, which has a proven track record, and inkjet, which is cost-competitive, are being considered.
[0010] In both photolithography and inkjet printing, the challenge lies in creating resin compositions containing quantum dots at high concentrations and with high dispersion. With some exceptions, resin compositions contain quantum dots dispersed in polar solvents such as propylene glycol monomethyl ether acetate (PGMEA) or propylene glycol monomethyl ether (PGME). However, quantum dots are fundamentally hydrophobic and do not disperse easily in these solvents or resin materials, often resulting in aggregation. Therefore, creating photosensitive resin compositions containing quantum dots at high concentrations and with high dispersion is difficult.
[0011] Various studies have been conducted to disperse quantum dots in polar solvents. For example, Patent Document 2 describes a method for producing a composite in which semiconductor nanoparticles are dispersed in silica glass by stepwise reacting a metal alkoxide on the surface of semiconductor nanoparticles to deposit a silica glass layer, enabling the dispersion of the composite in water. However, a problem arose with the composite obtained by this manufacturing method, as the luminescence efficiency of the quantum dots was significantly reduced.
[0012] Furthermore, Patent Document 3 describes how to impart water solubility by manufacturing a composite in which quantum dots are encapsulated with an amphiphilic polymer. However, in this composite, the proportion of weight and volume occupied by the polymer in the overall composite is large. Therefore, when filling and dispersing quantum dots in a limited volume of resin, such as for color filter applications, the total amount of quantum dots decreases, making it difficult to obtain sufficient luminescence properties.
[0013] The present invention has been made to solve the above problems and aims to provide quantum dots that can maintain high luminescence efficiency and have improved dispersibility in highly polar solvents, as well as a method for producing the same. Furthermore, it aims to provide a quantum dot composition obtained by dispersing the quantum dots in a resin material, a wavelength conversion material including a cured product of the quantum dot composition, and a method for producing the same.
[0014] The present invention has been made to achieve the above objective, and provides a quantum dot body comprising a quantum dot that emits fluorescence upon excitation light, wherein the quantum dot comprises a core of semiconductor nanoparticles and a shell of semiconductor nanoparticles covering the core of the semiconductor nanoparticles, the surface of the quantum dot is coated with a metal oxide, and the surface of the metal oxide is modified with sodium monofluorophosphate.
[0015] Such quantum dot materials allow for the maintenance of high luminescence efficiency and improve dispersibility in highly polar solvents.
[0016] In this case, the sodium monofluorophosphate may be included in a mass ratio of 0.1 to 30% by mass relative to the quantum dots.
[0017] This effectively suppresses aggregation between particles composed of quantum dots and metal oxides, allowing the effects of modification on the metal oxide surface to be fully and stably exerted.
[0018] In this case, the sodium monofluorophosphate may be included in a mass ratio of 0.5 to 20% by mass relative to the quantum dots.
[0019] This allows for more effective suppression of aggregation between particles composed of quantum dots and metal oxides, and enables the effects of modification on the metal oxide surface to be exerted more stably.
[0020] In this case, the quantum dot composition can be obtained in which the above-mentioned quantum dots are dispersed in a resin material.
[0021] Such a quantum dot composition would result in a quantum dot composition with excellent luminescence properties and stability.
[0022] In this case, the wavelength conversion material can include a cured product of the quantum dot composition.
[0023] Such wavelength conversion materials maintain high luminescence efficiency and offer improved reliability.
[0024] The present invention has also been made to achieve the above objectives and provides a method for manufacturing a quantum dot, comprising: a quantum dot manufacturing step for manufacturing a quantum dot comprising a semiconductor nanoparticle core and a semiconductor nanoparticle shell covering the semiconductor nanoparticle core; a quantum dot coating step for coating the surface of the quantum dot with a metal oxide; and a quantum dot modification step for modifying the surface of the metal oxide with sodium monofluorophosphate.
[0025] This method for manufacturing quantum dots makes it possible to produce quantum dots that maintain high luminescence efficiency and have improved dispersibility in highly polar solvents.
[0026] In this case, the method for producing a quantum dot composition may include a step of dispersing the quantum dots produced by the method for producing the quantum dots in a resin material to produce a quantum dot composition.
[0027] This makes it possible to manufacture quantum dot compositions with improved luminescence properties and stability.
[0028] In this case, the method for manufacturing a wavelength conversion material may include a step of curing the quantum dot composition manufactured by the method for manufacturing the quantum dot composition to manufacture a wavelength conversion material.
[0029] This makes it possible to manufacture a wavelength conversion material that maintains high luminescence efficiency and has improved reliability even after curing the quantum dot composition.
[0030] As described above, the quantum dot material of the present invention maintains high luminescence efficiency and exhibits improved dispersibility in highly polar solvents. Furthermore, the method for producing the quantum dot material of the present invention makes it possible to produce a quantum dot material that maintains high luminescence efficiency and exhibits improved dispersibility in highly polar solvents.
[0031] Furthermore, by using a quantum dot composition and wavelength conversion material containing the quantum dots of the present invention, the initial value of the luminescence efficiency and its degradation over time are suppressed. Moreover, a method for manufacturing a quantum dot composition and wavelength conversion material having the above effects can be provided.
[0032] This is a schematic cross-sectional view showing an example of the quantum dot body of the present invention.
[0033] The present invention will be described in detail below, but the present invention is not limited to these descriptions.
[0034] As described above, there was a need for quantum dot materials and methods for producing them that could maintain high luminescence efficiency and improve dispersibility in highly polar solvents.
[0035] As a result of diligent research into the above-mentioned problems, the present inventors have found that a quantum dot body containing quantum dots that emit fluorescence upon excitation light, wherein the quantum dots comprise a core of semiconductor nanoparticles and a shell of semiconductor nanoparticles covering the core of the semiconductor nanoparticles, the surface of the quantum dots is coated with a metal oxide, and the surface of the metal oxide is modified with sodium monofluorophosphate, can maintain high luminescence efficiency and improve dispersibility in highly polar solvents, thereby completing the present invention.
[0036] The present inventors have also conducted extensive research on the above-mentioned problems and have found that a method for manufacturing quantum dots, comprising a quantum dot manufacturing step for manufacturing a quantum dot comprising a semiconductor nanoparticle core and a semiconductor nanoparticle shell covering the semiconductor nanoparticle core, a quantum dot coating step for coating the surface of the quantum dot with a metal oxide, and a quantum dot modification step for modifying the surface of the metal oxide with sodium monofluorophosphate, can produce quantum dots that maintain high luminescence efficiency and have improved dispersibility in highly polar solvents, thus completing the present invention.
[0037] Furthermore, it was revealed that the quantum dot composition obtained by dispersing the quantum dots in a resin material, and the wavelength conversion material obtained by curing the quantum dot composition, are quantum dot compositions and wavelength conversion materials that have high initial values of luminous efficiency and suppressed degradation of luminous efficiency over time. As a result, it was found that the wavelength conversion material containing the cured product of the quantum dot composition obtained by dispersing the quantum dots in a resin material can suppress the rate of decrease in internal quantum yield during a 100-hour treatment in a reliability test at 85°C and 85% RH without a barrier film, and that stability can be improved.
[0038] In this invention, the "coating" of the metal oxide on the quantum dot surface has the effect of suppressing the degradation of fluorescence emission efficiency over time, and may be in the form of partial or complete coating. Furthermore, it may be a uniform coating layer such as a core / shell structure, or a non-uniform coating layer, and may be a structure in which multiple semiconductor nanoparticles are coated with metal oxide.
[0039] In this invention, "modification" refers to a state in which sodium monofluorophosphate is "adhered" to at least a metal oxide surface. Adhesion to the surface due to "modification" includes both partial and complete adhesion, and indicates a state in which it is adhered to at least a part of the surface.
[0040] In the above, "adhesion" may refer to physical adsorption or chemical bonding, and broadly includes covalent bonds, ionic bonds, and hydrogen bonds, or combinations thereof. Furthermore, as an example, a quantum dot body containing a quantum dot, a metal oxide coating layer, and sodium monofluorophosphate may be in a state where at least some of the ligands of the organic or inorganic ligands that were attached during quantum dot synthesis are present, as long as it is dispersed in a polar solvent.
[0041] [Quantum Dot Body] The quantum dot body of the present invention will be described with reference to Figure 1. As shown in Figure 1, the quantum dot body 1 of the present invention is a quantum dot body that includes a quantum dot 2 that emits fluorescence when excited by light, wherein the quantum dot 2 includes a semiconductor nanoparticle core 3 and a semiconductor nanoparticle shell 4 that covers the semiconductor nanoparticle core 3, the surface of the quantum dot 2 is coated with a metal oxide 5, and the surface of the metal oxide 5 is modified with sodium monofluorophosphate 6.
[0042] (Quantum Dots) The structure of the quantum dots according to the present invention is not particularly limited as long as it includes a semiconductor nanoparticle core and a semiconductor nanoparticle shell. Such quantum dots have excellent fluorescence emission characteristics and stability. For example, in semiconductor nanoparticles with a core / shell structure in which nano-sized semiconductor particles are used as the core and semiconductor particles with a larger band gap and lower lattice mismatch than the core are used as the shell, the fluorescence emission efficiency is further improved because the excitons generated in the shell are confined inside the core particles, and stability is further improved because the core surface is covered with the shell.
[0043] Furthermore, the quantum dot may include a semiconductor nanoparticle core and a plurality of semiconductor nanoparticle shells covering the semiconductor nanoparticle core. With such a quantum dot, the degradation of fluorescence emission efficiency is further suppressed.
[0044] As the material for the semiconductor nanoparticle core of the core / shell semiconductor nanoparticles, those containing no Cd or Pb elements are preferred from the viewpoint of toxicity, and for example, those selected from the group consisting of Group II-VI, Group III-V, Group IV, Group IV-VI, Group I-III-VI, Group II-IV-V, and mixed crystals, alloys thereof, or compounds having a perovskite structure can be used.
[0045] Specifically, examples of the material for the semiconductor nanoparticle core include ZnS, ZnSe, ZnTe, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, Si, Ge, Sn, SnS, SnSe, SnTe, AgGaS 2 , AgInS 2 , AgGaSe 2 , AgInSe 2 , CuGaS 2 , CuGaSe 2 , CuInS 2 , CuInSe 2 , ZnSiP 2 , ZnGeP 2 , CsSnCl 3 , CsSnBr 3 , CsSnI 3 Compounds containing the above can be mentioned. Among these materials, ZnSe, ZnTe, and InP are particularly preferred from the viewpoints of fluorescence emission characteristics and stability.
[0046] Further, it is preferable that the surface of the core particle of the core / shell semiconductor nanoparticles is passivated (passivation) with an inorganic compound. As a result, defects on the surface of the core particle are inactivated, the fluorescence emission efficiency is improved, and the deterioration of the fluorescence emission efficiency over time is further suppressed.
[0047] The inorganic compound for performing passivation is not particularly limited, and examples thereof include metal halides. From the viewpoint of improving fluorescence emission efficiency, GaCl 3 , GaI 3 , GaBr 3 , ZnCl 2 , ZnBr 2 , ZnI 2 , InCl3 InBr 3 In I 3 , AgCl, AgBr, AgI, KCl, KBr, KI, NaCl, NaBr, NaI, MgCl 2 MgBr 2 MgI 2 CaCl 2 CaBr 2 CaI 2 , MnCl 2 MnBr 2 MnI 2 FeCl 2 , FeBr 2 FeI 2 CuCl 2 CuBr 2 , CuI 2 , ZrCl 4 ZrBr 4 , ZrI 4 GeCl 4 , GeBr 4 GeI 4 At least one compound selected from the above is particularly preferred.
[0048] As for the semiconductor nanoparticle shell material, it is preferable that it does not contain elements such as Cd and Pb from the viewpoint of toxicity, but it is also preferable that it has a large band gap and low lattice mismatch with respect to the core material, and can be selected from the group consisting of II-VI compounds, alloys of III-V compounds, and mixed crystals.
[0049] Specific shell materials include those selected as single, multiple, or mixed crystals from among ZnS, ZnSe, ZnTe, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, and InSb. Of these materials, ZnSe and ZnS are particularly preferred in terms of improving fluorescence emission efficiency and stability.
[0050] (Metal Oxide) The quantum dots of the present invention are coated with a metal oxide, which prevents oxygen and water in the atmosphere from directly contacting the quantum dot surface, thereby suppressing oxidation reactions and thus preventing deterioration of their fluorescence emission efficiency.
[0051] The thickness of the metal oxide coating layer is not particularly limited, but from the viewpoint of light transmittance, it is preferably 500 nm or less.
[0052] In the present invention, the type of metal oxide is not particularly limited, but ZnO, Al 2 O 3 SiO 2 , ZrO 2 Fe 2 O 3 , MgO, Y 2 O 3 , HfO 2 , CEO 2 In 2 O 3 , SnO 2 WO 3 ,CrO 3 Ta 2 O 3 , BaTiO 3 , V 2 O 5 , NiO, NbO, Cu 2 O, CuO, MoO 3 Examples include at least one compound selected from the following. From the viewpoint of improving the stability of quantum dots, Al 2 O 3 SiO 2 , ZrO 2 This is preferable.
[0053] (Sodium monofluorophosphate) In the present invention, sodium monofluorophosphate is a surface modifier useful for improving compatibility with polar solvents and photosensitive resins, and the quantum dot body in the present invention comprises the above-mentioned quantum dots, a metal oxide coating the surface of the quantum dots, and sodium monofluorophosphate modifying the surface of the metal oxide.
[0054] Because sodium monofluorophosphate has an affinity for polar solvents, modifying the metal oxide surface with it improves the dispersibility of quantum dots in polar solvents.
[0055] The amount of sodium monofluorophosphate added as the surface modifier is not particularly limited as long as the sodium monofluorophosphate modifies the metal oxide surface. For example, an amount of 30% by mass (wt%) or less relative to the solid mass of the quantum dots is preferable because it effectively suppresses aggregation between quantum dots, and an amount of 0.1% by mass (wt%) or more is preferable because it allows the effect of modification on the metal oxide surface to be sufficiently and stably exerted. Therefore, an amount of 0.1 to 30% by mass (wt%) relative to the solid mass of the quantum dots is preferable, and an amount of 0.5 to 20% by mass (wt%) is more preferable.
[0056] [Quantum Dot Composition] The present invention also provides a quantum dot composition in which the quantum dots are dispersed in a resin material.
[0057] In the quantum dot composition of the present invention, the resin material may contain a polymer that is a base polymer along with a polymerization initiator, and may also contain an organic solvent, a polymerizable crosslinking agent, a photoacid generator, an antioxidant, a light scattering agent, and the like.
[0058] The polymers mentioned above are selected as appropriate for the application from polymers derived from acrylic acid, methacrylic acid, acrylic acid esters, methacrylic acid esters, copolymers combining multiple polymers, polymers containing glycidyl (meth)acrylate repeating units, siloxane skeletons, urethane skeletons, sylphenylene skeletons, norbornene skeletons, fluorene skeletons, and isocyanurate skeletons. Examples include acrylic resins, alkyd resins, melamine resins, epoxy resins, silicone resins, polyvinyl alcohol, polyvinylpyrrolidone, polyamides, polyamide-imides, polyimide precursors and their esterification products, and reaction products of tetracarboxylic dianhydrides and diamines.
[0059] Furthermore, these polymers have polymerizable substituents introduced into them, and can be cured by using them in combination with polymerization initiators. Examples of radical polymerizable substituents include vinyl groups, acrylic groups, methacrylic groups, and thiol groups, all of which can be suitably used. Examples of cationic polymerizable substituents include hydroxyl groups, phenolic hydroxyl groups, epoxy groups, glycidyl groups, oxetanyl groups, and isocyanate groups, all of which can be suitably used. In addition, carboxyl groups may be introduced to impart alkali developability.
[0060] Furthermore, the quantum dot composition of the present invention may also preferably contain a polymerization initiator, as described above. The polymerization initiator may be a thermal or photopolymerization initiator, and either can be suitably used in conjunction with the base polymer. Examples of photoradical polymerization initiators include the Irgacure® series, commercially available from BASF, such as Irgacure 290, Irgacure 651, Irgacure 754, Irgacure 184, Irgacure 2959, Irgacure 907, Irgacure 369, Irgacure 379, Irgacure 819, and Irgacure 1173. Examples of the Darocure® series include TPO and Darocure 1173. In addition, known thermal radical polymerization initiators and photocationic polymerization initiators may also be included. The polymerization initiator content is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass of polymer added.
[0061] The quantum dot composition of the present invention may contain an organic solvent to improve its applicability. Organic solvents are preferred as solvents from the viewpoint of compatibility with quantum dots, and examples include ketones, alkylene glycol ethers, alcohols, and aromatic compounds. Examples from the ketone group include acetone, methyl ethyl ketone, and cyclohexanone; and from the alkylene glycol ether group include methyl cellosolve (ethylene glycol monomethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), methyl acetate cellosolve, ethyl acetate cellosolve, butyl acetate cellosolve, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol dimethyl ether, diethylene glycol ethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol acetate monomethyl ether, and diethylene glycol acetate. Suitable solvents include methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butyl alcohol, 3-methyl-3-methoxybutanol, etc. from the alcohol group, and benzene, toluene, xylene from the aromatic solvent group. In addition, the quantum dot composition of the present invention may also contain polymerizable crosslinking agents, photoacid generators, antioxidants, light scattering agents, etc., and there are no particular limitations as long as the coatability of the quantum dot composition is not affected.
[0062] Such quantum dot compositions have improved dispersibility in resin materials because the quantum dots have improved dispersibility in polar solvents, thereby suppressing aggregation of quantum dots within the resin.
[0063] [Wavelength Conversion Material] The present invention also provides a wavelength conversion material comprising a cured product of the above quantum dot composition. The wavelength conversion material may be used as is or processed. One example is a wavelength conversion film in which the quantum dot composition is dispersed in a resin, which is formed by processing it into a sheet and then curing it.
[0064] With such wavelength conversion materials, quantum dots are dispersed at high concentration in the resin material without aggregates, while maintaining high luminescence efficiency, resulting in improved reliability.
[0065] [Method for Manufacturing Quantum Dots] Next, the method for manufacturing quantum dots according to the present invention will be described. The method for manufacturing quantum dots according to the present invention is a manufacturing method that includes a quantum dot manufacturing step for manufacturing a quantum dot comprising a semiconductor nanoparticle core and a semiconductor nanoparticle shell covering the semiconductor nanoparticle core, a quantum dot coating step for coating the surface of the quantum dot with a metal oxide, and a quantum dot modification step for modifying the surface of the metal oxide with sodium monofluorophosphate.
[0066] (Quantum Dot Manufacturing Process) There are various methods for manufacturing the core and shell of semiconductor nanoparticles, such as liquid-phase and gas-phase methods, but the present invention is not particularly limited. From the viewpoint of obtaining high fluorescence emission efficiency, it is preferable to use semiconductor nanoparticles obtained by the hot soap method or the hot injection method, in which a precursor species is reacted at high temperature in a high-boiling-point nonpolar solvent.
[0067] (Quantum dot coating process) The method for forming the metal oxide coating layer is not particularly limited, but from the viewpoint of selectively promoting the reaction on the quantum dot surface, a method of reacting the metal oxide precursor in a liquid phase is preferred.
[0068] In this invention, one example is a method for forming an oxide coating layer using microwave treatment. By using microwaves, the metal oxide precursor is directly heated from within, allowing the reaction to proceed selectively in a shorter time, and enabling the formation of a metal oxide layer on the quantum dot surface.
[0069] Here, "microwaves" generally refers to electromagnetic waves with frequencies ranging from 300 MHz to 3 THz. While methods for microwave irradiation include, for example, using Milestone General's flexi WAVE, the method is not particularly limited.
[0070] In this coating process, it is preferable to perform the process in the presence of quantum dots and a metal oxide precursor, and to coat the surface of the semiconductor nanoparticles with metal oxide by irradiating the metal oxide precursor in the presence of quantum dots with microwaves. This efficiently forms a metal oxide coating layer and suppresses the deterioration of fluorescence emission efficiency.
[0071] In this case, it is preferable to select one or more of the following as the dispersion medium for the quantum dots and metal oxide precursor: a polar solvent, a nonpolar solvent, or an ionic liquid, and to form the coating layer in that solvent.
[0072] Furthermore, it is preferable that the solvent used in the coating process at this time be one or more of the following solvents: toluene, hexane, cyclohexane, benzene, and diethyl ether. These nonpolar solvents can further improve the dispersibility of quantum dots.
[0073] Furthermore, if the solvent is a nonpolar solvent, a microwave-absorbing heating element called Weflon, a type of PTFE resin containing carbon components manufactured by Milestone General, may be optionally used during the coating process.
[0074] While not particularly limited, it is preferable to use one or more metal oxide precursors selected from metal alkoxides, metal halides, and metal complexes. From the viewpoint of stability, silicon alkoxides, aluminum alkoxides, and zirconium alkoxides are particularly preferred as metal oxide precursors.
[0075] In this process, it is preferable to use a catalyst to accelerate the reaction of the metal oxide precursor during the coating process. In particular, when using a metal alkoxide, it is preferable to use a catalyst to accelerate the sol-gel reaction. Examples of catalysts include acidic aqueous solutions or basic aqueous solutions, with basic aqueous solutions being particularly preferred from the viewpoint of coating layer thickness.
[0076] Furthermore, a surfactant may be added during the coating process from the viewpoint of dispersibility of the metal oxide precursor. The surfactant is not particularly limited, but examples include cationic surfactants such as quaternary ammonium salts like cetyltrimethylammonium bromide, anionic surfactants such as carboxylates and sulfonates, and nonionic surfactants such as polyoxyethylene alkyl ethers. Cationic surfactants are particularly preferred from the viewpoint of dispersibility of the metal oxide precursor.
[0077] Furthermore, it is preferable to carry out the coating process in the presence of alcohol. Coating in the presence of alcohol results in better dispersibility of the metal oxide precursor. In addition, if a surfactant is added, dispersibility can be further improved by dissolving it in a polar solvent such as alcohol.
[0078] In this case, the reaction temperature during microwave irradiation treatment varies depending on the solvent, but from the viewpoint of preventing deterioration of fluorescence emission efficiency, 40 to 200°C is preferred, and 50 to 110°C is more preferred.
[0079] While microwave irradiation is used as an example of the metal oxide coating process in this embodiment, the method is not particularly limited as long as the quantum dot surface is "coated" with a metal oxide layer.
[0080] (Quantum dot modification process) The method for modifying a metal oxide surface with sodium monofluorophosphate is not particularly limited, as long as it is a method in which sodium monofluorophosphate is modified on the metal oxide surface. As an example, a solvent system consisting of two phases, a polar solvent and a nonpolar solvent, is used, in which particles consisting of quantum dots and a metal oxide layer are dispersed in a nonpolar solvent and sodium monofluorophosphate is dispersed in a polar solvent, and these are mixed by strong stirring or the like, and the quantum dots, which are particles modified with sodium monofluorophosphate, are extracted to the polar solvent side.
[0081] The type of nonpolar solvent is not particularly limited, as long as the particles consisting of quantum dots and metal oxide layers are dispersed without settling. Similarly, the polar solvent is not particularly limited, as long as sodium monofluorophosphate is eluted without precipitation. Furthermore, even if the polar and nonpolar solvents do not mix and separate into two phases, the type of solvent is not particularly limited, as long as the resulting quantum dots are dispersed on the polar solvent side.
[0082] While there are no particular limitations on the heating temperature when modifying a metal oxide surface with sodium monofluorophosphate, a heating temperature in the range of 30 to 100°C is preferred for efficient modification. Within this range, the metal oxide surface can be modified more efficiently.
[0083] [Method for Manufacturing the Quantum Dot Composition] Next, the method for manufacturing the quantum dot composition of the present invention will be described. Note that matters already described regarding the quantum dot composition may be omitted as appropriate.
[0084] The present invention relates to a method for producing a quantum dot composition, which includes the step of dispersing quantum dots produced by the above-described method for producing quantum dots in a resin material. The resin material can be a polymer as a base polymer and a polymerization initiator, and may also be an organic solvent, a polymerizable crosslinking agent, a photoacid generator, an antioxidant, a light scattering agent, etc.
[0085] The polymers can preferably include polymers derived from acrylic acid, methacrylic acid, acrylic acid esters, methacrylic acid esters, copolymers combining multiple polymers, polymers containing a skeletal structure with glycidyl (meth)acrylate as a repeating unit, siloxane skeletons, urethane skeletons, silphenylene skeletons, norbornene skeletons, fluorene skeletons, and isocyanurate skeletons, and the polymer used may be selected as appropriate for the application.
[0086] Furthermore, these polymers have polymerizable substituents introduced into them, and can be cured by using them in combination with a polymerization initiator. Polymerization initiators include thermal or photopolymerization initiators, and either can be suitably used depending on the base polymer. In addition, known thermal radical polymerization initiators or photocationic polymerization initiators may be used.
[0087] The polymerization initiator content is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, per 100 parts by mass of polymer added. Organic solvents may be used to improve the coatability of the quantum dot composition. In addition, polymerizable crosslinking agents, photoacid generators, antioxidants, light scattering agents, etc., may be used, and there are no particular restrictions as long as they do not affect the coatability of the quantum dot composition.
[0088] According to this method for manufacturing quantum dot compositions, it is possible to produce quantum dot compositions in which the dispersibility of quantum dots in a resin material is improved.
[0089] [Method for Manufacturing Wavelength Conversion Materials] The present invention also provides a method for manufacturing wavelength conversion materials, which includes a step of curing a quantum dot composition manufactured by the above-described method for manufacturing quantum dot compositions to manufacture a wavelength conversion material.
[0090] The method for manufacturing the wavelength conversion material is not particularly limited, but for example, a wavelength conversion material can be obtained by coating a resin composition, in which a quantum dot composition is dispersed in a resin, onto a transparent film such as PET or polyimide, curing it, and then laminating it.
[0091] The transparent film can be coated using spray or inkjet methods, or with spin coating, bar coating, or doctor blade methods, forming a resin layer. The thickness of the resin layer and the transparent film is not particularly limited and can be selected as appropriate depending on the application.
[0092] According to this method for manufacturing wavelength conversion materials, even after curing the quantum dot composition, it is possible to disperse the quantum dots in the resin material without aggregation while maintaining high luminescence efficiency, thereby enabling the production of a wavelength conversion material with improved reliability.
[0093] The present invention will be described in detail below with reference to examples, but this is not intended to limit the present invention.
[0094] (Measurement of emission wavelength, emission width at half maximum, and luminous efficiency) In the examples and comparative examples, the emission wavelength, fluorescence emission width at half maximum, and fluorescence luminous efficiency (internal quantum yield) of the quantum dots at an excitation wavelength of 450 nm were measured using the quantum efficiency measurement system (QE-2100) manufactured by Otsuka Electronics Co., Ltd.
[0095] (Reliability Test) The obtained wavelength conversion material was treated at 85°C and 85% RH (relative humidity) for 100 hours, and its reliability was evaluated by comparing the fluorescence emission efficiency (internal quantum yield) of the wavelength conversion material before and after treatment.
[0096] [Example 1] (Quantum dot manufacturing process) 0.070 g (0.24 mmol) of indium acetate, 0.256 g (0.72 mmol) of palmitic acid, and 4.0 mL of 1-octadecene were added to a flask, and the mixture was heated and stirred under reduced pressure at 100°C for 1 hour while dissolving the substances.
[0097] After cooling the flask to room temperature, nitrogen was purged, and 0.50 mL (0.17 mmol) of a 10 vol% (tris)trimethylsilylphosphine / octadecene solution was added to the flask. The flask was heated to 300°C and stirred for 20 minutes to synthesize InP semiconductor core particles.
[0098] Next, after cooling the flask to 200°C, 0.10 mL (0.02 mmol) of gallium(III) chloride / octadecene solution was added and the mixture was heated for 20 minutes.
[0099] Furthermore, after heating the flask to 260°C, 4.0 mL (1.2 mmol) of 0.30 M zinc stearate / octadecene solution was added and stirred for 30 minutes. Then, 0.60 mL (0.90 mmol) of 1.5 M selenium / trioctylphosphine solution was added to the flask and stirred for 30 minutes.
[0100] Next, after cooling the flask to room temperature, 0.22 g (1.1 mmol) of zinc acetate was added, and the mixture was heated and stirred under reduced pressure at 100°C for 1 hour while dissolving. After purging the flask with nitrogen, it was heated to 230°C, and 0.48 mL (2.0 mmol) of 1-dodecanethiol was added and stirred for 30 minutes.
[0101] The resulting solution was cooled to room temperature, ethanol was added, and the quantum dots, consisting of an InP core, a ZnSe shell, and a ZnS shell, were precipitated by centrifugation, and the supernatant was removed.
[0102] The obtained quantum dot precipitate was then mixed with hexane, toluene, or propylene glycol monomethyl ether acetate (PGMEA), respectively. The results showed that the precipitate dispersed in toluene and hexane, but did not disperse in PGMEA, instead settling as quantum dots. This confirmed that quantum dots do not disperse in polar solvents and have a high affinity for non-polar solvents. Fluorescence emission characteristics were evaluated against an InP / ZnSe / ZnS toluene dispersion. The obtained quantum dots exhibited an emission wavelength of 537 nm, a emission width at half maximum of 42 nm, and a luminescence efficiency of 79%.
[0103] (Quantum dot coating process) 10 g of a toluene dispersion of the obtained 1.0 wt% InP / ZnSe / ZnS quantum dots, 0.10 g of aluminum isopropoxide, 50 μL of 25% aqueous ammonia solution, and 0.010 g / 100 μL of cetyltrimethylammonium bromide / ethanol solution were mixed and placed in a high-pressure reaction vessel.
[0104] Subsequently, using a microwave synthesis reactor (Milestone General, flexi WAVE), heating is performed at 2450 MHz at 60°C for 5 minutes to create Al on the InP / ZnSe / ZnS surface. 2 O 3 A coating layer was formed. Ethanol was added to the obtained particles, and the particles were allowed to settle by centrifugation, after which the supernatant liquid was removed.
[0105] The resulting InP / ZnSe / ZnS / Al 2 O 3 To the precipitate, polar solvents of hexane or propylene glycol monomethyl ether acetate (PGMEA) were added. As a result, the obtained precipitate dispersed in hexane but did not disperse in PGMEA and settled in InP / ZnSe / ZnS / Al 2 O 3 It was confirmed that it does not disperse in polar solvents but has a high affinity for nonpolar solvents.
[0106] Fluorescence emission characteristics are evaluated using InP / ZnSe / ZnS / Al 2 O 3 The experiment was performed on a hexane dispersion. The fluorescence emission characteristics of the obtained quantum dots were an emission wavelength of 538 nm, an emission width at half maximum of 43 nm, and an internal quantum yield of 64%.
[0107] (Quantum dot modification process) A sodium monofluorophosphate solution was prepared by weighing 10 mg of sodium monofluorophosphate into a 20 ml vial under a nitrogen atmosphere, adding 10 ml of dimethylformamide (DMF), and stirring.
[0108] Furthermore, under a nitrogen atmosphere, the obtained 1.0 wt% InP / ZnSe / ZnS / Al was placed in a 50 ml vial. 2 O 3 10 g of a hexane dispersion and 10 ml of a sodium monofluorophosphate solution were added. The sodium monofluorophosphate solution was InP / ZnSe / ZnS / Al 2 O 3 The mass ratio to was 10%. The mass ratio to quantum dots (InP / ZnSe / ZnS) was 18%.
[0109] At this point, hexane and DMF separated into two phases, with the quantum dots dispersed in the hexane, nonpolar solvent. Next, this solution was heated to 50°C under a nitrogen atmosphere, stirred for 30 minutes, and then cooled to room temperature. At this point, the quantum dots had shifted from the hexane, nonpolar solvent, to the DMF side, forming an InP / ZnSe / ZnS / Al 2 O 3 It was confirmed that quantum dots modified with sodium monofluorophosphate on their surface can be dispersed in polar solvents.
[0110] Hexane was added to the obtained quantum dots, and the quantum dots were precipitated by centrifugation. After removing the supernatant, propylene glycol monomethyl ether acetate (PGMEA) was added to the precipitate of quantum dots, and it was confirmed that the quantum dots dispersed in the polar solvent PGMEA. The fluorescence emission properties of the obtained quantum dots were an emission wavelength of 538 nm, an emission half-width of 43 nm, and an internal quantum yield of 59%.
[0111] (Preparation of Quantum Dot Composition) The obtained quantum dot dispersion in PGMEA and methacrylic-modified silicone X-32-3817-3 (manufactured by Shin-Etsu Chemical Co., Ltd.) were weighed and mixed so that the quantum dots accounted for 20 wt% of the non-volatile content. After mixing, the solvent was removed to obtain the quantum dot composition.
[0112] (Manufacturing of Wavelength Conversion Material) A wavelength conversion material was fabricated using the obtained quantum dot composition. The quantum dot composition was vacuum-degassed and coated onto a 50 μm thick polyethylene terephthalate (PET) film, and a 100 μm thick quantum dot-containing resin layer was formed using a bar coater. Furthermore, a PET film was laminated onto this resin layer. This film was then irradiated with a UV LED at a wavelength of 365 nm and an output of 4000 mW / cm. 2 A wavelength conversion material was fabricated by curing a quantum dot-containing resin layer by irradiating it with light for 20 seconds. The fluorescence emission characteristics of the obtained wavelength conversion material were an emission wavelength of 538 nm, an emission half-width of 43 nm, and an internal quantum yield of 51%.
[0113] [Example 2] (Quantum dot manufacturing process) The same quantum dot manufacturing process as in Example 1 was performed to produce a toluene dispersion of InP / ZnSe / ZnS quantum dots.
[0114] (Quantum dot coating process) 10 g of a toluene dispersion of the obtained 1.0 wt% InP / ZnSe / ZnS quantum dots, 100 μL of tetraethoxysilane, 50 μL of 25% aqueous ammonia solution, and 0.010 g / 100 μL of cetyltrimethylammonium bromide / ethanol solution were mixed and placed in a high-pressure reaction vessel.
[0115] Subsequently, using a microwave synthesis reactor (Milestone General, flexi WAVE), heating is performed at 2450 MHz at 60°C for 5 minutes to generate SiO on the InP / ZnSe / ZnS surface. 2 A coating layer was formed. Ethanol was added to the obtained particles, and the particles were allowed to settle by centrifugation, after which the supernatant liquid was removed.
[0116] The resulting InP / ZnSe / ZnS / SiO 2 To the precipitate, hexane or propylene glycol monomethyl ether acetate (PGMEA) was added as a polar solvent. As a result, the obtained precipitate dispersed in hexane but did not disperse in PGMEA and settled, forming an InP / ZnSe / ZnS / SiO 2 It was confirmed that it does not disperse in polar solvents but has a high affinity for nonpolar solvents.
[0117] Fluorescence emission characteristics are evaluated using InP / ZnSe / ZnS / SiO 2 The experiment was performed on a hexane dispersion. The fluorescence emission characteristics of the obtained quantum dots were an emission wavelength of 538 nm, an emission width at half maximum of 43 nm, and an internal quantum yield of 62%.
[0118] (Quantum dot modification process) A sodium monofluorophosphate solution was prepared by weighing 10 mg of sodium monofluorophosphate into a 20 ml vial under a nitrogen atmosphere, adding 10 ml of dimethylformamide (DMF), and stirring.
[0119] Furthermore, under a nitrogen atmosphere, the obtained 1.0 wt% InP / ZnSe / ZnS / SiO₂ was placed in a 50 ml vial.2 10 g of the hexane dispersion and 10 ml of sodium monofluorophosphate solution were added. The sodium monofluorophosphate content relative to InP / ZnSe / ZnS / SiO 2 had a mass ratio of 10%. In addition, the mass ratio relative to the quantum dots (InP / ZnSe / ZnS) was 16%.
[0120] At this time, hexane and DMF separated into two phases, and the quantum dots were dispersed on the hexane side, which is a non-polar solvent. Next, this solution was heated to 50°C in a nitrogen atmosphere, stirred for 30 minutes, and then cooled to room temperature. At this time, the quantum dots had undergone phase transfer from hexane, the non-polar solvent, to the DMF side, and the InP / ZnSe / ZnS / SiO 2 It was confirmed that the quantum dot bodies, in which the surfaces of the quantum dots were modified with sodium monofluorophosphate, were dispersed in a polar solvent.
[0121] Hexane was further added to the obtained quantum dot bodies, followed by centrifugation to precipitate the quantum dot bodies. The supernatant was removed, and propylene glycol monomethyl ether acetate (PGMEA) was added to the obtained precipitate of quantum dot bodies. As a result, it was confirmed that the quantum dot bodies were dispersed in PGMEA solvent, which is a polar solvent. The fluorescence emission characteristics of the obtained quantum dot bodies were an emission wavelength of 538 nm, an emission half-width of 43 nm, and an internal quantum yield of 58%.
[0122] (Production of Quantum Dot Composition) The obtained PGMEA dispersion of quantum dot bodies and methacryl-modified silicone X-32-3817-3 (manufactured by Shin-Etsu Chemical Co., Ltd.) were weighed and mixed so that the non-volatile content ratio of the quantum dot bodies was 20 wt%. After mixing, the solvent was removed to obtain a quantum dot composition.
[0123] (Production of Wavelength Conversion Material) A wavelength conversion material was produced using the obtained quantum dot composition. The quantum dot composition was vacuum degassed, applied onto a 50 μm-thick polyethylene terephthalate (PET) film, and a bar coater was used to form a 100 μm-thick quantum dot-containing resin layer. A PET film was further laminated on this resin layer. This film was treated with a UVLED irradiation device at a wavelength of 365 nm and an output of 4000 mW / cm2 A quantum dot-containing resin layer was cured by irradiating it with light for 20 seconds to produce a wavelength conversion material. The fluorescence emission characteristics of the obtained wavelength conversion material were an emission wavelength of 538 nm, an emission half-width of 43 nm, and a luminous efficiency of 49%.
[0124] [Example 3] (Quantum dot manufacturing process) The same quantum dot manufacturing process as in Example 1 was performed to produce a toluene dispersion of InP / ZnSe / ZnS quantum dots.
[0125] (Quantum dot coating process) 10 g of a toluene dispersion of the obtained 1.0 wt% InP / ZnSe / ZnS quantum dots, 0.10 g of zirconium(IV) tert-butoxide, 50 μL of 25% aqueous ammonia solution, and 0.010 g / 100 μL of cetyltrimethylammonium bromide / ethanol solution were mixed and placed in a high-pressure reaction vessel.
[0126] Subsequently, using a microwave synthesis reactor (Milestone General, flexi WAVE), heating is performed at 2450 MHz at 80°C for 5 minutes to produce ZrO on the InP / ZnSe / ZnS surface. 2 A coating layer was formed. Ethanol was added to the obtained particles, and the particles were allowed to settle by centrifugation, after which the supernatant liquid was removed.
[0127] The resulting InP / ZnSe / ZnS / ZrO 2 To the precipitate, hexane or propylene glycol monomethyl ether acetate (PGMEA) was added as a polar solvent. As a result, the obtained precipitate dispersed in hexane but did not disperse in PGMEA and settled, forming InP / ZnSe / ZnS / ZrO 2 It was confirmed that it does not disperse in polar solvents but has a high affinity for nonpolar solvents.
[0128] Fluorescence emission characteristics are evaluated using InP / ZnSe / ZnS / ZrO 2 The experiment was performed on a hexane dispersion. The fluorescence emission characteristics of the obtained quantum dots were an emission wavelength of 538 nm, an emission width at half maximum of 43 nm, and an internal quantum yield of 61%.
[0129] (Quantum Dot Modification Step) Under a nitrogen atmosphere, 10 mg of sodium monofluorophosphate was weighed into a 20 ml vial, 10 ml of dimethylformamide (DMF) was added and stirred to prepare a sodium monofluorophosphate solution.
[0130] Further under a nitrogen atmosphere, into a 50 ml vial, the obtained 1.0 wt% InP / ZnSe / ZnS / ZrO 2 10 g of hexane dispersion and 10 ml of the sodium monofluorophosphate solution were added. The mass ratio of sodium monofluorophosphate to InP / ZnSe / ZnS / ZrO 2 was 10%. In addition, the mass ratio to the quantum dots (InP / ZnSe / ZnS) was 18%.
[0131] At this time, hexane and DMF separated into two phases, and the quantum dots were dispersed on the hexane side, which is a non-polar solvent. Next, this solution was heated to 50°C under a nitrogen atmosphere, stirred for 30 minutes, and then cooled to room temperature. At this time, the quantum dots had undergone phase transfer from hexane, the non-polar solvent, to the DMF side, and the InP / ZnSe / ZnS / ZrO 2 quantum dot bodies, in which the surfaces of the quantum dots were modified with sodium monofluorophosphate, were confirmed to be dispersible in a polar solvent.
[0132] Hexane was further added to the obtained quantum dot bodies, followed by centrifugation to precipitate the quantum dot bodies. The supernatant was removed, and propylene glycol monomethyl ether acetate (PGMEA) was added to the resulting precipitate of quantum dot bodies. As a result, it was confirmed that the quantum dot bodies were dispersed in PGMEA solvent, which is a polar solvent. The fluorescence emission characteristics of the obtained quantum dot bodies were an emission wavelength of 538 nm, an emission half-width of 43 nm, and an internal quantum yield of 56%.
[0133] (Production of Quantum Dot Composition) The obtained PGMEA dispersion of quantum dot bodies and methacryl-modified silicone X-32-3817-3 (manufactured by Shin-Etsu Chemical Co., Ltd.) were weighed and mixed such that the quantum dot bodies were contained at a non-volatile content ratio of 20 wt%. After mixing, the solvent was removed to obtain a quantum dot composition.
[0134] (Manufacturing of Wavelength Conversion Material) A wavelength conversion material was fabricated using the obtained quantum dot composition. The quantum dot composition was vacuum-degassed and coated onto a 50 μm thick polyethylene terephthalate (PET) film, and a 100 μm thick quantum dot-containing resin layer was formed using a bar coater. Furthermore, a PET film was laminated onto this resin layer. This film was then irradiated with a UV LED at a wavelength of 365 nm and an output of 4000 mW / cm. 2 A wavelength conversion material was fabricated by curing a quantum dot-containing resin layer by irradiating it with light for 20 seconds. The fluorescence emission characteristics of the obtained wavelength conversion material were an emission wavelength of 537 nm, an emission half-width of 43 nm, and a luminous efficiency of 47%.
[0135] [Comparative Example 1] The quantum dot manufacturing process was carried out in the same manner as in Example 1, but the metal oxide coating process (quantum dot coating process) and the surface modification process with sodium monofluorophosphate (quantum dot modification process) were omitted, and the mixture was then mixed with the resin composition. Methacrylic modified silicone oil X-32-3817-3 (manufactured by Shin-Etsu Chemical Co., Ltd.) was weighed into the toluene dispersion after the quantum dot manufacturing process so that the quantum dots were present at a non-volatile content ratio of 20 wt%, and mixed. After mixing, the solvent was removed to obtain a quantum dot composition.
[0136] A wavelength conversion material was prepared using the obtained quantum dot composition by the same manufacturing method as in Example 1. The fluorescence emission characteristics of the obtained wavelength conversion material were a wavelength of 538 nm, a emission width at half maximum of 43 nm, and a luminous efficiency of 27%. [Comparative Example 2] The quantum dot manufacturing process and the metal oxide coating process were carried out in the same manner as in Example 1, and the mixture was mixed with the resin composition without performing the surface modification process with sodium monofluorophosphate. Methacrylic-modified silicone oil X-32-3817-3 (manufactured by Shin-Etsu Chemical Co., Ltd.) was weighed into the hexane dispersion after the quantum dot manufacturing process and the metal oxide coating process so that the quantum dots were contained at a non-volatile content ratio of 20 wt%, and mixed. After mixing, the solvent was removed to obtain a quantum dot composition.
[0137] A wavelength conversion material was fabricated using the obtained quantum dot composition by the same manufacturing method as in Example 1. The fluorescence emission characteristics of the obtained wavelength conversion material were a wavelength of 538 nm, a emission half-width of 43 nm, and a luminous efficiency of 24%.
[0138] The results for Examples 1-3 and Comparative Examples 1 and 2 are shown in Table 1. Table 1 shows the dispersion solvent for quantum dots or quantum dot bodies, luminous efficiency (internal quantum yield), dispersibility in PGMEA solvent, and the initial values of the luminous efficiency (internal quantum yield) of the wavelength conversion material, the luminous efficiency (internal quantum yield) after reliability evaluation, and the results of microscopic observation showing the presence or absence of aggregates.
[0139]
[0140] Table 1 shows that the quantum dots of Examples 1-3 precipitated in hexane solvent and dispersed in PGMEA solvent. This result confirms that quantum dots modified with sodium monofluorophosphate have improved affinity for polar solvents such as PGMEA, resulting in improved dispersibility. On the other hand, quantum dots produced by the method of Comparative Example 1 or 2, and particles consisting of quantum dots and metal oxides, dispersed in toluene and hexane solvents, but precipitated and did not disperse in the polar solvent PGMEA.
[0141] Furthermore, when the wavelength conversion materials were observed using a microscope, it was found that the aggregates in Examples 1 to 3 were small and few in number, which is thought to have suppressed the decrease in quantum yield. On the other hand, many aggregates of about 1 to 100 μm were observed in the wavelength conversion materials of Comparative Examples 1 and 2, which is thought to have resulted in a decrease in quantum yield.
[0142] Furthermore, a comparison of the reliability tests of the wavelength conversion materials, performed at 85°C and 85% RH for 100 hours, revealed that the example material maintained higher luminous efficiency and improved stability compared to the comparative example.
[0143] As described above, the embodiments of the present invention confirmed that the quantum dot material of the present invention exhibits improved dispersibility in polar solvents. Furthermore, the quantum dot composition using the quantum dot material of the present invention and the wavelength conversion material using the same were confirmed to have suppressed initial fluorescence emission efficiency and degradation over time under high temperature and high humidity conditions, thus demonstrating high reliability.
[0144] This specification includes the following embodiments: [1] A quantum dot body comprising a quantum dot that fluoresces upon excitation light, wherein the quantum dot comprises a core of semiconductor nanoparticles and a shell of semiconductor nanoparticles covering the core of the semiconductor nanoparticles, the surface of the quantum dot is coated with a metal oxide, and the surface of the metal oxide is modified with sodium monofluorophosphate. [2] The quantum dot body according to [1], wherein the sodium monofluorophosphate is contained in a mass ratio of 0.1 to 30% by mass relative to the quantum dot. [3] The quantum dot body according to [1] or [2], wherein the sodium monofluorophosphate is contained in a mass ratio of 0.5 to 20% by mass relative to the quantum dot. [4] A quantum dot composition in which the quantum dot body according to [1], [2] or [3] is dispersed in a resin material. [5] A wavelength conversion material comprising a cured product of the quantum dot composition according to [4]. [6] A method for manufacturing a quantum dot, comprising: a quantum dot manufacturing step of manufacturing a quantum dot comprising a core of semiconductor nanoparticles and a shell of semiconductor nanoparticles covering the core of the semiconductor nanoparticles; a quantum dot coating step of coating the surface of the quantum dot with a metal oxide; and a quantum dot modification step of modifying the surface of the metal oxide with sodium monofluorophosphate. [7] A method for manufacturing a quantum dot composition, comprising the step of dispersing the quantum dots manufactured by the method for manufacturing a quantum dot described in [6] in a resin material to manufacture a quantum dot composition. [8] A method for manufacturing a wavelength conversion material, comprising the step of curing the quantum dot composition manufactured by the method for manufacturing a quantum dot composition described in [7] to manufacture a wavelength conversion material.
[0145] It should be noted that the present invention is not limited to the embodiments described above. The embodiments described above are illustrative, and any configuration that is substantially identical to the technical idea described in the claims of the present invention and achieves similar effects is included within the technical scope of the present invention.
Claims
1. A quantum dot body comprising a quantum dot that emits fluorescence upon excitation light, wherein the quantum dot comprises a core of semiconductor nanoparticles and a shell of semiconductor nanoparticles covering the core of the semiconductor nanoparticles, the surface of the quantum dot is coated with a metal oxide, and the surface of the metal oxide is modified with sodium monofluorophosphate.
2. The quantum dot body according to claim 1, characterized in that the sodium monofluorophosphate is contained in a mass ratio of 0.1 to 30% by mass relative to the quantum dot.
3. The quantum dot body according to claim 1, characterized in that the sodium monofluorophosphate is contained in a mass ratio of 0.5 to 20% by mass relative to the quantum dot.
4. A quantum dot composition characterized in that the quantum dot bodies described in any one of claims 1 to 3 are dispersed in a resin material.
5. A wavelength conversion material characterized by comprising a cured product of the quantum dot composition described in claim 4.
6. A method for manufacturing a quantum dot, comprising: a quantum dot manufacturing step of manufacturing a quantum dot comprising a semiconductor nanoparticle core and a semiconductor nanoparticle shell covering the semiconductor nanoparticle core; a quantum dot coating step of coating the surface of the quantum dot with a metal oxide; and a quantum dot modification step of modifying the surface of the metal oxide with sodium monofluorophosphate.
7. A method for producing a quantum dot composition, characterized by comprising the step of dispersing quantum dots produced by the method for producing quantum dots described in claim 6 into a resin material to produce a quantum dot composition.
8. A method for producing a wavelength conversion material, characterized by comprising the step of curing a quantum dot composition produced by the method for producing a quantum dot composition described in claim 7.