Method for manufacturing light-emitting device
The method improves adhesion and reliability in ultraviolet light-emitting devices by using amorphous fluororesin sealing bodies formed through element bonding and compression molding, addressing the issue of poor sealing in existing manufacturing processes.
Patent Information
- Application Number
- PCT/JP2026/017485
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
The existing methods for manufacturing ultraviolet light-emitting devices face issues with poor adhesion between the coating resin and the lens, leading to potential poor sealing and reduced reliability of the device.
A manufacturing method involving element bonding and sealing body formation, where a translucent sealing body made of amorphous fluororesin is formed by softening and pressing against an amorphous fluororesin pellet, followed by compression molding to improve adhesion and reliability.
Enhances the adhesion between the sealing body components, preventing defects and ensuring reliable sealing, thereby improving the overall reliability of the light-emitting device.
Smart Images

Figure JP2026017485_19112026_PF_FP_ABST
Abstract
Description
Method for manufacturing a light-emitting device
[0001] The present invention relates to a method for manufacturing a light-emitting device equipped with a semiconductor light-emitting element.
[0002] A method for manufacturing a light-emitting device equipped with an ultraviolet light-emitting element is disclosed. For example, Patent Document 1 discloses a method for manufacturing a light-emitting device that includes the steps of mounting an ultraviolet light-emitting element on a flat submount, forming a coating resin made of amorphous fluororesin on the surface of the ultraviolet light-emitting element, and forming a lens made of amorphous fluororesin that covers the ultraviolet light-emitting element and the coating resin.
[0003] WO2019 / 087348 publication
[0004] In the ultraviolet light-emitting device disclosed in Patent Document 1, a coating resin is formed on the surface of the ultraviolet light-emitting element, and then a lens covering the coating resin is formed using a molding die such as compression molding or transfer molding.
[0005] When forming a lens, for example, if the resin material to be formed is placed in a mold and the surface of the coating resin is pressed against the resin material during the lens formation process, there is a risk of poor adhesion between the coating resin and the lens. If this occurs, there is a risk of poor sealing of the ultraviolet light-emitting element, which in turn reduces the reliability of the light-emitting device.
[0006] This invention has been made in view of the above-mentioned problems, and aims to provide a method for manufacturing a light-emitting device that can improve the reliability of the device.
[0007] The present invention relates to a method for manufacturing a light-emitting device, comprising: an element bonding step to form an element-bonded device substrate by bonding a light-emitting element that emits ultraviolet light to a pair of mounting electrodes of a device substrate having a flat substrate and a pair of mounting electrodes formed on the upper surface of the substrate; and a sealing body forming step to form a translucent sealing body made of amorphous fluororesin that seals the light-emitting element on the device substrate, wherein the sealing body forming step comprises: a first step of forming a resin layer made of amorphous fluororesin over the upper surface of the device substrate and the surface of the light-emitting element; and after the first step, placing one amorphous fluororesin pellet on the upper surface of the light-emitting element, and softening the resin layer and amorphous fluororesin pellet by heating while The invention is characterized by comprising: a second step of pressing a resin layer formed on the upper surface of a light-emitting element against an amorphous fluororesin pellet to bond the resin layer and the amorphous fluororesin pellet together, thereby temporarily fixing the amorphous fluororesin pellet to the resin layer; and a third step of, after the second step, holding the device substrate with the element bonded to it in the substrate holding mold of a molding die having a substrate holding mold and a concave female mold, with its bottom surface in contact with the substrate holding mold, positioning the female mold so that the female mold faces the surface on which the device substrate of the substrate holding mold is placed, and while softening the resin layer and amorphous fluororesin pellet by heating, closing the substrate holding mold and the female mold to deform the amorphous fluororesin pellet and form a seal.
[0008] This is a perspective view of the light-emitting device according to Example 1. This is a top view of the light-emitting device according to Example 1. This is a cross-sectional view of the light-emitting device according to Example 1. This is a cross-sectional view showing one step in the manufacturing process perspective view of the light-emitting device according to Modification 1 of Example 1. This is a cross-sectional view showing one step in the manufacturing process of the light-emitting device according to Modification 1. This is a perspective view of the light-emitting device according to Modification 2 of Example 1. This is a perspective view of the light-emitting device according to Modification 3 of Example 1.
[0009] Hereinafter, embodiments of the present invention will be specifically described with reference to the drawings. In the drawings, identical components are denoted by the same reference numerals, and descriptions of redundant components are omitted.
[0010] The configuration of the light-emitting device 100 according to Embodiment 1 will be described using Figures 1 to 3. Figure 1 is a perspective view of the light-emitting device 100. Figure 2 is a top view of the light-emitting device 100. Figure 3 is a cross-sectional view of the light-emitting device 100 shown in Figure 2, along line 3-3. In Figure 3, the vertical direction is the height direction of the light-emitting device 100, and the horizontal direction is the width direction of the light-emitting device 100.
[0011] [Overview of the Light-Emitting Device 100] The light-emitting device 100 is composed of a device substrate 11, a light-emitting element 13 provided on the device substrate 11, and a sealing body 15 that covers and seals the light-emitting element 13 on the device substrate 11.
[0012] Note that in Figure 2, the sealing body 15 is omitted to avoid complicating the illustration. Also, in Figure 2, the center line CL is shown as a line segment that passes through the center of the upper surface of the device substrate 11 and bisects the width of the device substrate 11 in the left-right direction in the figure.
[0013] [Device Substrate 11] First, the configuration of the device substrate 11 will be described. The device substrate 11 is a double-sided wiring board composed of a flat base plate 17 and wiring patterns provided on both main surfaces of the base plate 17.
[0014] The base material 17 is a plate-like body having a rectangular top surface shape. In the light-emitting device 100 of this embodiment, the base material 17 is made of an insulating ceramic made of aluminum nitride (AlN) with excellent heat dissipation properties and a thermal conductivity of 150 to 220 (W / mK). The base material 17 also contains alumina (Al 2 O 3 ), silicon nitride (Si 3 N 4 Ceramics with UV resistance properties such as those mentioned above may also be used.
[0015] Here, the wiring pattern provided on the base material 17 will be described. Element mounting electrodes 18 are formed on the upper surface of the base material 17. Mounting electrodes 19 are formed on the lower surface of the base material 17.
[0016] The element mounting electrodes 18 are a pair of electrodes provided on the upper surface of the base material 17, approximately in the center, separated from each other by a center line CL. The element mounting electrodes 18 consist of a first element mounting electrode 18A and a second element mounting electrode 18B, each having a rectangular upper surface shape and being the same size. The first element mounting electrode 18A and the second element mounting electrode 18B are provided on the upper surface of the base material 17 so that their long sides face each other.
[0017] The region connecting the outer edges of the first element mounting electrode 18A and the second element mounting electrode 18B is an element mounting region for mounting and bonding the light-emitting element 13. The element mounting electrode 18 is formed by laminating nickel (Ni) and gold (Au) in that order on its upper surface (surface) as protective layers, with copper (Cu) as the base material.
[0018] The mounted electrodes 19 are a pair of electrodes formed on the lower surface of the substrate 17, spaced apart from each other, and each has a rectangular upper surface shape. The mounted electrodes 19 are electrically connected to the element mounting electrodes 18 via conductive vias 21 made of conductive metal that penetrate the substrate 17 in the vertical direction in Figure 2.
[0019] Specifically, the mounting electrode 19 consists of a first mounting electrode 19A that is electrically connected to the first element mounting electrode 18A via a conductive via 21, and a second mounting electrode 19B that is electrically connected to the second element mounting electrode 18B via a conductive via 21.
[0020] In the light-emitting device 100 of this embodiment, the mounted electrode 19 has a base material of Cu, with Ni and Au laminated in that order on its lower surface (front surface) as protective layers. The conductive via 21 is made of Cu only as the base material.
[0021] Furthermore, in addition to Cu, other metals such as aluminum (Al) and tungsten (W) can be selected as the base material for the element mounting electrode 18, mounting electrode 19, and conductive via 21 described above. In addition, a combination of titanium (Ti) and Au, or a combination of chromium (Cr) and Au can be selected as the protective layer.
[0022] [Light-emitting element 13] Next, the configuration of the light-emitting element 13 will be described. The light-emitting element 13 is an element that is bonded to the element mounting electrode 18 of the device substrate 11. Here, as described above, the element mounting electrode 18 is provided approximately in the center of the base material 17 in a plan view. Therefore, the light-emitting element 13 is located approximately in the center of the device substrate 11 in a plan view.
[0023] As shown in Figure 3, the light-emitting element 13 is a light-emitting diode (LED) comprising an element substrate 24, a semiconductor structural layer 25 including a light-emitting layer, and p electrodes 26 and n electrodes 27 electrically connected to the semiconductor structural layer 25.
[0024] The element substrate 24 is a flat, translucent substrate with a rectangular top surface. In the light-emitting device 100 of this embodiment, the element substrate 24 is made of a wurtzite structure aluminum nitride (AlN) single crystal. The element substrate 24 also contains sapphire (Al 2 O 3 ) Single crystals can also be used. Furthermore, if a light-emitting element that emits ultraviolet light with a wavelength longer than 380 nm is used, gallium nitride (GaN) single crystals can also be used.
[0025] The semiconductor structure layer 25 is an aluminum gallium nitride (AlGaN) crystal-based semiconductor crystal layer formed over the entire lower surface of the element substrate 24. The semiconductor structure layer 25 is configured by laminating an n-type semiconductor layer, a light-emitting layer, and a p-type semiconductor layer (none of which are shown) in this order on the lower surface of the element substrate 24. Note that the exposed surface of the semiconductor structure layer 25 is made of silicon oxide (SiO 2 ), Al 2 O 3 or the like protective film.
[0026] When the light-emitting element 13 is energized, light having a wavelength in the ultraviolet region is emitted from the light-emitting layer of the semiconductor structure layer 25. In the light-emitting device 100 of the present embodiment, deep ultraviolet light having a peak wavelength of 265 nm is emitted from the light-emitting layer. Note that each of the p-type semiconductor layer, the light-emitting layer, and the n-type semiconductor layer of the semiconductor structure layer 25 may include a superlattice layer, a quantum well layer, a barrier layer, and the like.
[0027] The p-electrode 26 and the n-electrode 27 are electrodes electrically connected to the p-type semiconductor layer and the n-type semiconductor layer of the semiconductor structure layer 25, respectively. Each of the p-electrode 26 and the n-electrode 27 is bonded to each of the first element mounting electrode 18A and the second element mounting electrode 18B via a gold-tin (Au-Sn) based bonding member 29, respectively. That is, the light-emitting element 13 is flip-chip bonded to the device substrate 11.
[0028] In the light-emitting device 100, the aforementioned first element mounting electrode 18A and first mounting electrode 19A function as an anode electrode, and the second element mounting electrode 18B and second mounting electrode 19B function as a cathode electrode.
[0029] The ultraviolet light emitted from the light-emitting layer of the semiconductor structure layer 25 by energizing the p-electrode 26 and the n-electrode 27 of the light-emitting element 13 exits to the outside of the light-emitting element 13 from the upper surface and side surfaces of the element substrate 24. That is, the side surfaces and the upper surface of the element substrate 24 are the light extraction surfaces of the light-emitting element 13.
[0030] The upper surface of the element substrate 24 of the light-emitting element 13 is a -c plane (non-metallic surface) with nitrogen (N) atoms arranged on its surface. The lower surface of the element substrate 24 is a +c plane (metallic surface) with Al atoms arranged on its surface. Here, the Al atoms in the +c axis direction are polarized to δ+, and the N atoms in the -c axis direction are polarized to δ-.
[0031] In other words, the upper surface of the element substrate 24, which is the light-emitting surface of the light-emitting element 13, is a -c plane (non-metallic surface) in which δ-polarized N atoms are arranged, and is a crystal plane (N atom plane) in which dangling bonds (unbonded hands) of N atoms are exposed. Furthermore, the side surfaces of the element substrate 24 of the light-emitting element 13 are a plane and an m plane or higher-order crystal plane having dangling bonds of Al atoms and N atoms.
[0032] [Sealing body 15] Next, the sealing body 15 will be described. The sealing body 15 is a transparent member that covers the upper surface of the device substrate 11. The sealing body 15 seals and protects the light-emitting element 13, and also transmits the light emitted from the light-emitting element 13, guiding the emitted light to the outside of the light-emitting device 100.
[0033] The sealing body 15 is composed of a first sealing member 15A and a second sealing member 15B that covers the first sealing member 15A. The first sealing member 15A is a thin, transparent resin layer that covers the upper surface of the substrate 17, the wiring pattern provided on the substrate 17, and the surface of the light-emitting element 13.
[0034] Specifically, as shown in Figure 3, the first sealing member 15A closely adheres (bonds) to the upper surface of the substrate 17, the surfaces of the element mounting electrodes 18, and the surface of the light-emitting element 13 (the upper surface, side surfaces, and lower surfaces other than the p-electrode 26 and n-electrode 27) according to their respective shapes. The first sealing member 15A also fills the area between the upper surface of the device substrate 11 and the lower surface of the light-emitting element 13.
[0035] The second sealing member 15B is a transparent member that covers the entire first sealing member 15A and has a bullet-shaped form that is convex upwards. In other words, the second sealing member 15B has a semi-ellipsoidal shape obtained by rotating a semi-ellipse with its major axis in the vertical direction in Figure 3.
[0036] The second sealing member 15B seals the light emitting element 13 while being in close contact (adhered) with the first sealing member 15A on the device substrate 11. Here, the first sealing member 15A functions as an auxiliary adhesive layer for providing the second sealing member 15B on the device substrate 11.
[0037] The second sealing member 15B functions as a convex lens with the major axis of the aforementioned semi-ellipsoid as the optical axis. In a plan view of the light emitting device 100 viewed from above, the center of the light emitting element 13 and the center of the second sealing member 15B are arranged to overlap each other.
[0038] Accordingly, the light emitted from the light emitting element 13 has directional characteristics such that the light is condensed along the optical axis of the second sealing member 15B and emitted to the outside. Note that when the second sealing member 15B has a hemispherical shape, or a semi-ellipsoidal shape formed by rotating a semi-ellipse with the vertical direction in FIG. 3 as the minor axis, the half-value angle of the emitted light from the light emitting device 100 can be increased.
[0039] The sealing body 15 is made of a thermoplastic amorphous fluororesin (thermoplastic resin) that transmits the emitted light from the light emitting element 13. The sealing body 15 is, for example, S-type of CYTOP (registered trademark) manufactured by AGC Inc..
[0040] Specifically, the amorphous fluororesin used as the constituent material of the sealing body 15 is obtained by cyclopolymerizing perfluoro(4-vinyloxy-1-butene) (hereinafter also referred to as BVE) in the main chain, as shown in Chemical Formula 1 below, and the functional group is a perfluorocarbon-based trifluoromethyl group (-CF, which has high light resistance to ultraviolet light with an emission wavelength of 265 nm of the light emitting element 13 3 ).
[0041] Such an amorphous fluororesin modified at the terminal or in the middle of the main chain with a perfluorocarbon-based functional group has high light resistance to ultraviolet rays with a wavelength of 220 nm to 300 nm. On the other hand, this amorphous fluororesin has low adhesion (adhesiveness) when, for example, a resin material is simply formed thereon, regardless of whether the materials are the same as or different from each other.
[0042] Furthermore, this amorphous fluororesin has a refractive index of 1.34 and a transmittance of 90% or more for ultraviolet light. The light output of the light-emitting device 100 using this amorphous fluororesin as the sealant 15 is improved by more than 1.5 times compared to the light output of a light-emitting device sealed using, for example, a glass cap with a convex space in which the light-emitting element 13 is housed in that space.
[0043] In this embodiment, the light-emitting device 100 uses a wurtzite-type single crystal AlN substrate as the element substrate 24 of the light-emitting element 13, and therefore the element substrate 24 and the functional group are -CF 3 The adhesion (bonding) to amorphous fluororesins has been improved.
[0044] In detail, the light-emitting surface (top surface) of the element substrate 24 is configured such that the upper surface of the light-emitting element 13 is a -c plane (non-metallic surface) where dangling bonds (unbonded bonds) of δ- polarized N atoms are arranged, thereby creating a -CF plane between the upper surface of the light-emitting element 13 and the functional group. 3 The chemical bonding or affinity of BVE with amorphous fluororesins obtained by cyclization polymerization has been improved.
[0045] Furthermore, because dangling bonds of N atoms exist on the side surfaces of the element substrate 24 (for example, the a-plane and m-plane), the side surfaces of the element substrate 24 and the functional groups are -CF 3 The adhesion (bonding properties) is improved by enhancing the chemical bonding or affinity of BVE with amorphous fluororesin obtained by cyclization polymerization.
[0046] Furthermore, in the light-emitting device 100 of this embodiment, since dangling bonds of N atoms also exist on the surface of the AlN polycrystalline ceramic material of the substrate 17 of the device substrate 11, the functional groups of the surface of the device substrate 11 and -CF 3 The adhesion (bonding properties) is improved by enhancing the chemical bonding or affinity of BVE with amorphous fluororesin obtained by cyclization polymerization.
[0047] [Manufacturing Method for Light-Emitting Device 100] The manufacturing method for the light-emitting device 100 will be described below with reference to Figures 4 to 12. Each of Figures 4 to 12 is a cross-sectional view showing one step in the manufacturing process of the light-emitting device 100.
[0048] The light-emitting device 100 is manufactured by a procedure that includes a device substrate preparation step of preparing a device substrate 11, an element bonding step of bonding a light-emitting element 13 to the device substrate 11, a first sealing member formation step of forming a first sealing member 15A on the device substrate 11, a temporary fixing step of temporarily fixing amorphous fluororesin pellets, and a second sealing member formation step of forming a second sealing member 15B on the first sealing member 15A.
[0049] [Device Substrate Preparation Process] First, as shown in Figure 4, a device substrate 11 is prepared, on which element mounting electrodes 18, mounting electrodes 19, and conductive vias 21 are formed on a base material 17. Note that there are as many device substrates 11 as there are light-emitting devices 100 to be manufactured at one time, but only one of them is shown in Figure 4.
[0050] In the manufacturing of the device substrate 11, the element mounting electrode 18, the mounting electrode 19, and the conductive via 21 are each formed by providing various metals on the upper surface, lower surface, and within the conductive vias of the substrate 17, for example, by deposition, sputtering, electroless plating, electrolytic plating, etc., and patterning by photolithography, etc. In the light-emitting device 100 of this embodiment, the size and thickness of the substrate 17 of the device substrate 11 are set to 3.6 mm square on each side and 0.5 mm thick.
[0051] [Element Bonding Process] Next, as shown in Figure 5, the light-emitting element 13 is bonded to the upper surface of the device substrate 11. In the light-emitting device 100 of this embodiment, the size and thickness of the light-emitting element 13 are set to 0.95 mm on the long side, 0.75 mm on the short side, and 0.11 mm in thickness.
[0052] Specifically, first, a solder paste containing 22 wt% fine particles of Au-Sn, which will become a bonding member 29 after heating, is applied to the surface of the element mounting electrode 18 of the device substrate 11 by screen printing or potting. Next, the light-emitting element 13 is placed on the element mounting electrode 18 to which the solder paste has been applied, such that the p electrode 26 and the n electrode 27 overlap.
[0053] Subsequently, the solder paste is heated to 300°C in a reflow oven to melt and solidify the 22 wt% Au-Sn fine particles contained in the solder paste, causing the paste components other than Au-Sn to volatilize, and the light-emitting element 13 is bonded to the device substrate 11 via the bonding member 29. This process forms a device substrate with the light-emitting element bonded. For bonding the light-emitting element 13, bump bonding, thermocompression bonding, etc., can be selected.
[0054] [First sealing member formation process] Next, a first sealing member 15A is formed within the sealing body 15, covering the upper surface of the base material 17 and the respective surfaces of the element mounting electrode 18 and the light-emitting element 13.
[0055] First, as shown in Figure 6, an amorphous fluororesin solution AC (hereinafter referred to as resin solution AC), which is obtained by liquefying amorphous fluororesin that will become the first sealing member 15A with a fluorine-based solvent, is applied to the entire upper surface of the device substrate 11, for example, using a spray nozzle SN.
[0056] Subsequently, the apparatus substrate 11, onto which the resin solution AC has been dropped, is placed on a hot plate, and the underside of the apparatus substrate 11 is heated at 230°C for 60 minutes to evaporate the solvent in the resin solution AC and dry it (volatilization step).
[0057] After the fluorine-based solvent in the resin solution AC is evaporated, heating is continued at 230°C for 60 minutes (additional heat treatment step). This causes the dried fluororesin to soften and spread, wetting and continuously coating the surface of the light-emitting element 13 to the edge of the upper surface of the substrate 17. By forming the first sealing member 15A from the resin solution AC in this way, the adhesion (bonding) of the first sealing member 15A, which is an amorphous fluororesin having perfluorocarbon-based functional groups, to the device substrate 11 and the light-emitting element 13 is improved. In other words, the affinity between the surface atoms (δ- polarized N atoms) of the element substrate 24 and the device substrate 11 and the constituent atoms of the amorphous fluororesin is improved, resulting in improved adhesion (bonding).
[0058] As a result of these operations, a first sealing member 15A, which is a thin film of amorphous fluororesin, is formed on the upper surface of the device substrate 11, extending over the surface of the light-emitting element 13 and the upper surface of the substrate 17, as shown in Figure 7.
[0059] [Temporary Fixing Process] Next, amorphous fluororesin pellets RP (hereinafter referred to as resin pellets RP), which will become the second sealing member 15B, are temporarily fixed to the first sealing member 15A formed on the upper surface of the light-emitting element 13 in the first sealing member forming process. In the manufacturing process of this embodiment, the shape and size of the resin pellets RP are set to a square shape with a top and bottom surface of 1.8 mm square and a height of 1.7 mm.
[0060] First, as shown in Figure 8, the device substrate 100A with the first sealing member 15A formed on it is fixed to the first mold M1 in such a manner that the upper surface of the device substrate 11, i.e., the surface on which the light-emitting element 13 is formed, faces downward in the figure. The first mold M1 has a flat plate shape and functions as a holding mold for holding the object in this process.
[0061] Next, as shown in Figure 8, the resin pellets RP are placed in a second mold M2, which serves as a pellet-holding mold. The second mold M2 has a rectangular top surface shape and includes a recess CA1 that has an opening larger than the resin pellets RP in plan view. In this step, the resin pellets RP are placed on the bottom surface of the recess CA1 such that the center of the top surface of the resin pellets RP and the center of the top surface of the light-emitting element 13 coincide in plan view.
[0062] Next, the first mold M1 and the second mold M2 are heated to 180°C in an atmospheric environment, and the heat transmitted from the first mold M1 and the second mold M2 by this heating softens the first sealing member 15A and the resin pellet RP, respectively.
[0063] Next, as shown by the white arrows in Figure 8, the first mold M1 is lowered toward the second mold M2, and as shown in Figure 9, the first sealing member 15A formed on the upper surface of the light-emitting element 13 is pressed against the upper surface of the resin pellet RP. At this time, the pressing load of the first mold M1 toward the second mold M2 is set to 14 to 140 gf / mm 2 It states that the time for applying the pressing load is 2 seconds.
[0064] After the pressing described above, the resin pellet RP adheres to the first sealing member 15A formed on the upper surface of the light-emitting element 13 and is temporarily fixed to the first sealing member 15A. In this process, the resin pellet RP is deformed by being crushed when pressed from the first mold M1. Specifically, as shown in Figure 9, the resin pellet RP after this process is deformed from its original rectangular prism shape to a truncated square pyramidal shape that widens towards the first sealing member 15A.
[0065] Finally, the first mold M1 is raised upward in the diagram. This operation separates the resin pellet RP from the second mold M2 while it remains adhered to the first sealing member 15A. This completes the temporary fixing process for the resin pellet RP.
[0066] This temporary fixing process is made possible because the first sealing member 15A is strongly bonded to the upper surface of the light-emitting element 13 in the preceding first sealing member formation process. Therefore, the resin pellet RP can be temporarily fixed (bonded) to the first sealing member 15A formed on the upper surface of the light-emitting element 13 without the upper surface of the light-emitting element 13 and the first sealing member 15A peeling off. In addition, the upper surface of the light-emitting element 13 on which the first sealing member 15A is formed and the upper surface of the resin pellet RP are pressed evenly, which improves the adhesive strength at the interface between the upper surface of the light-emitting element 13 and the first sealing member 15A, and at the interface between the first sealing member 15A and the resin pellet RP.
[0067] In this process, the opening diameter of the recess CA1 of the second mold M2 is set to a size that prevents the deformed resin pellet RP from getting caught in the recess CA1 when the resin pellet RP is pulled away from the second mold M2, and that allows for displacement of the resin pellet RP even if it is pressed. In the manufacturing process of this embodiment, the opening diameter of the recess CA1 of the second mold M2 is set to a size of approximately 1.05 to 1.10 times the length of one side of the resin pellet RP.
[0068] Furthermore, in this process, the depth of the recess CA1 in the second mold M2 is set to a depth such that the deformed resin pellet RP does not get caught in the recess CA1 when the resin pellet RP is pulled away from the second mold M2. In the manufacturing process of this embodiment, the depth of the recess CA1 in the second mold M2 is set to 1 / 2 to 1 / 4 of the height of the resin pellet RP.
[0069] Furthermore, the shape of the resin pellet RP that becomes the second sealing member 15B is not limited to a rectangular prism, but can also be a polygonal prism such as a hexagonal prism or octagonal prism, a cylinder, or a concentric polygonal prism or cylinder. In short, the resin pellet RP has a shape on its surface that contacts the upper surface of the light-emitting element 13, and it is sufficient that it can be held by the second mold M2 to the extent that it does not wobble when it contacts the upper surface of the light-emitting element 13.
[0070] [Second sealing member formation process] Next, a second sealing member 15B is formed to cover the first sealing member 15A of the sealing body 15. The second sealing member 15B is formed by compression molding using a pair of molds consisting of a first mold M1 and a third mold M3.
[0071] As described above, the first mold M1 has a flat plate shape and functions as a holding mold that holds the object to be formed in compression molding and applies pressure to the third mold M3 while holding the object.
[0072] The third mold M3 has a downwardly convex, bullet-shaped recess CA2 and functions as a female mold that molds the resin body into a desired shape while receiving pressure from the first mold M1 during compression molding.
[0073] First, as shown in Figure 10, the first mold M1 and the third mold M3 are prepared such that the surface on which the light-emitting element 13 is formed faces downward in the figure, so that the resin pellets RP that were temporarily fixed in the temporary fixing step described above fit into the recess CA2 of the third mold M3.
[0074] Next, the first mold M1 and the third mold M3 are heated to 180°C in an atmospheric environment. As a result, heat is transferred from the first mold M1 and the third mold M3 to the first sealing member 15A and the resin pellet RP, respectively, causing the first sealing member 15A and the resin pellet RP to soften. The method of heating and softening the resin is not limited to changing the ambient temperature or directly heating the first sealing member 15A and the resin pellet RP with a radiant heater.
[0075] Next, while continuing to heat at 180°C, the first mold M1 is lowered as shown by the white arrow in Figure 10, and the softened resin pellets RP are pressed against the inner surface of the third mold M3. In this embodiment, the load applied when pressing the resin pellets RP against the inner surface of the third mold M3 is 40 kgf.
[0076] As a result of this operation, the softened resin pellet RP is pressed from the first mold M1 and deforms within the recess CA2, taking on a form that encloses the light-emitting element 13. Then, adhesion (bonding) progresses from the part where the enclosing occurs to the surrounding area of the device substrate 11.
[0077] When the gap between the first mold M1 and the third mold M3, including the recess CA2, is filled with resin pellets RP, the descent of the first mold M1 stops, and the resin pellets RP are molded into a shape that conforms to the recess CA2 of the third mold M3. In other words, in the manufacturing method of this embodiment, the resin pellets RP are molded into a bullet-shaped resin body that covers the light-emitting element 13 as shown in Figure 11, forming the second sealing member 15B.
[0078] In this process, the first mold M1 is held in a state where its descent has stopped, that is, in a state where the second sealing member 15B has been molded, for about 5 to 10 minutes. This ensures good adhesion (bonding) between the first sealing member 15A and the second sealing member 15B.
[0079] The deformation of the resin pellet RP as described above is made possible because the resin pellet RP is temporarily fixed to the center of the upper surface of the light-emitting element 13. Furthermore, by deforming the temporarily fixed resin pellet RP into a predetermined shape using a mold, a second sealing member 15B having good adhesion (bonding properties) to the first sealing member 15A is formed.
[0080] Finally, as shown in Figure 12, the temperatures of the first mold M1 and the third mold M3 are cooled to a temperature below the softening point of the amorphous fluororesin, for example, to about 50-80°C, and the temperature of the first mold M1 is raised as indicated by the white arrow in the figure.
[0081] This operation causes the second sealing member 15B to be removed from the third mold M3 while remaining in close contact with the first sealing member 15A. As a result, a device substrate 100A with the first sealing member 15A and the second sealing member 15B bonded to it is obtained.
[0082] [Individualization Process] As the final step, the device substrate 11, which consists of the same number of connected devices 100 to be manufactured at one time, is divided into individual pieces using a dicer so that each piece becomes a light-emitting device 100 having a single light-emitting element 13. This completes the manufacturing of the light-emitting device 100.
[0083] In the manufacturing method of this embodiment, as described above, the resin pellets RP that will become the second sealing member 15B are temporarily fixed to the first sealing member 15A while heating, and then the second sealing member 15B is formed by compression molding using a mold, which involves heating and press-fitting. In the manufacturing method of this embodiment, by going through the above steps, it is possible to suppress the occurrence of formation defects of the second sealing member 15B during compression molding. Formation defects here refer to, for example, a decrease in adhesion (bonding) at the interface between the first sealing member 15A and the second sealing member 15B, or incomplete adhesion due to the mixing of air bubbles at the interface between the first sealing member 15A and the second sealing member 15B.
[0084] Now, let's consider the case where compression molding of resin pellets RP is performed without carrying out the temporary fixing process described above. For example, when resin pellets RP are supplied to the recess CA2 of the third mold M3 and a pressing force is applied from the first mold M1 on top of them, the orientation of the supplied resin pellets RP may change.
[0085] For example, when a rectangular prism-shaped resin pellet RP is fed into a third mold M3 having a bullet-shaped recess CA2, the stability of the resin pellet RP within the recess CA2 is poor. As a result, when the pressing force from the first mold M1 is applied to the upper surface of the resin pellet RP, the resin pellet RP may move within the recess CA2. In other words, the orientation of the resin pellet RP may deviate from its original orientation.
[0086] If the molding of the second sealing member 15B proceeds while the resin pellets RP are misaligned, areas with weak adhesion may occur, such as a gap forming between the first sealing member 15A and the second sealing member 15B.
[0087] When such a thing happens, for example, the gap described above may be the starting point for a malfunction such as the second sealing member 15B peeling off from the first sealing member 15A during use of the light-emitting device 100. In addition, there is a risk that the sealing of the light-emitting element 13 by the sealing body 15 will be inadequate. In other words, there is a risk that the reliability of the light-emitting device will be reduced.
[0088] In the manufacturing method of this embodiment, by performing compression molding after the temporary fixing step of the resin pellets RP as described above, it is possible to prevent the posture of the resin pellets RP from changing within the recess CA2 of the third mold M3.
[0089] Therefore, according to the manufacturing method of this embodiment, molding defects of the second sealing member 15B can be prevented, and the adhesion (bonding) of the second sealing member 15B to the first sealing member 15A can be improved. This improves the reliability of the light-emitting device.
[0090] In the temporary fixing step of the manufacturing method of this embodiment, the resin pellet RP deforms from its original rectangular prism shape to a truncated square pyramidal shape that widens toward the first sealing member 15A, as described above. In other words, the resin pellet RP narrows toward the recess CA2. Due to its shape, the deformed resin pellet RP fits more easily into the recess CA2 of the third mold M3 during the formation step of the second sealing member 15B.
[0091] As a result, in the temporary fixing step of the manufacturing method of this embodiment, because the resin pellet RP has a truncated square pyramidal shape, it is possible to prevent the resin pellet RP from peeling off the first sealing member 15A due to, for example, the corners of the resin pellet RP hitting the opening of the recess CA2, compared to the case where the resin pellet RP is molded using the third mold M3 while remaining in the shape of a square prism or rectangular parallelepiped. [Modification 1] A modification of the light-emitting device 100 according to Embodiment 1 will be described below with reference to Figure 13. Figure 13 is a perspective view of the light-emitting device 110 according to Modification 1 of Embodiment 1. The light-emitting device 110 is the same as Embodiment 1 in all other respects, except that the shape of the sealing body 15 is different from that of Embodiment 1. In Figure 13, two opposing sides of the upper surface of the base material 17 are shown as sides 17A.
[0092] In the modified light-emitting device 110, as shown in Figure 13, the sealing body 15 has a central portion of its upper surface that is recessed along the extension direction of the edge 17A, and curved surfaces that extend in an arc from the central portion toward the edge 17A. To give an analogy, the sealing body 15 has a shape like an open book.
[0093] In the modified light-emitting device 110, the light emitted from the light-emitting device 110 has a light distribution pattern such that the light intensity of the surrounding portion of the sealing body 15 is greater than the light intensity of the central portion described above.
[0094] [Manufacturing Method of the Light-Emitting Device of Modification 1] Here, the manufacturing method of the light-emitting device 110 of this modification will be explained using Figure 14. Figure 14 is a cross-sectional view showing one step in the manufacturing process of the light-emitting device 110 of this modification. The manufacturing method of this modification differs from that of the manufacturing method of Example 1 in that the shape of the recess CA2 of the third mold M3, which is used as a female mold when forming the second sealing member 15B, is different, but otherwise it is the same as the manufacturing method of Example 1.
[0095] In the manufacturing method of the modified light-emitting device 110, the recess CA2 of the third mold M3 has a central portion that protrudes upward, and an inclined surface that slopes downward in an arc from the central portion, as shown in Figure 14.
[0096] When the first mold M1 is lowered during the formation of the second sealing member 15B, the resin pellet RP comes into contact with the surface of the third mold M3, except for the edge portion of the surface opposite to the surface in contact with the first sealing member 15A. In other words, the resin pellet RP comes into contact only with the protruding central portion of the bottom surface of the recess CA2.
[0097] In the manufacturing method of the modified light-emitting device 110, for example, if the resin pellet RP that has not been temporarily fixed is placed in the recess CA2 of the third mold M3, the resin pellet RP will be in an inclined position with its upper surface relative to the upper surface of the light-emitting element 13 because of the central portion described above located within the recess CA2. In other words, the resin pellet RP will be placed in an unstable state within the recess CA2.
[0098] Therefore, if the molding of the second sealing member 15B proceeds in this state, as described above, there is a risk that areas with weak adhesion may form between the first sealing member 15A and the second sealing member 15B. This could lead to the second sealing member 15B peeling off from the first sealing member 15A, or to a faulty sealing of the light-emitting element 13 by the sealing body 15. In other words, the reliability of the light-emitting device may be reduced.
[0099] In the manufacturing method of the modified light-emitting device 110, similar to Example 1, compression molding is performed after the temporary fixing step of the resin pellets RP, thereby preventing the resin pellets RP from shifting within the recess CA2 of the third mold M3.
[0100] Therefore, according to the manufacturing method of this modified example, regardless of the shape of the recess CA2, it is possible to prevent molding defects of the second sealing member 15B and improve the adhesion (adhesion) of the second sealing member 15B to the first sealing member 15A.
[0101] [Modification 2] Next, a modification of the light-emitting device 100 according to Example 1 will be described using Figure 15. Figure 15 is a perspective view of the light-emitting device 120 according to Modification 2 of Example 1. The light-emitting device 120 is similar to Example 1 in all other respects, except that the shape of the sealing body 15 is different from that of Example 1.
[0102] In the modified light-emitting device 120, as shown in Figure 15, the sealing body 15 has a concave central portion and a four-leaf shape with leaves extending outward in four directions from the concave central portion.
[0103] Even when manufacturing a light-emitting device 120 having a sealing body 15 of this shape, it is possible to prevent the resin pellets RP from shifting within the recess CA2 of the third mold M3, regardless of the shape of the recess CA2. Therefore, according to the manufacturing method of this modified example, it is possible to prevent molding defects of the second sealing member 15B and to improve the adhesion (adhesion) of the second sealing member 15B to the first sealing member 15A.
[0104] [Modification 3] Next, a modification of the light-emitting device 100 according to Example 1 will be described using Figure 16. Figure 16 is a perspective view of the light-emitting device 130 according to Modification 3 of Example 1. The light-emitting device 130 is the same as Example 1 in all other respects, except that the shape of the sealing body 15 is different from that of Example 1.
[0105] In the modified light-emitting device 130, the sealing body 15 has a truncated square pyramidal shape with the device substrate 11 as its base, as shown in Figure 16. In the modified light-emitting device 130, the light emitted from the light-emitting device 100 exhibits a uniform light intensity distribution pattern on the upper surface of the sealing body 15.
[0106] Even when manufacturing a light-emitting device 130 having a sealing body 15 of this shape, it is possible to prevent the resin pellets RP from shifting within the recess CA2 of the third mold M3, regardless of the shape of the recess CA2. Therefore, according to the manufacturing method of this modified example, it is possible to prevent molding defects of the second sealing member 15B and to improve the adhesion (adhesion) of the second sealing member 15B to the first sealing member 15A.
[0107] The light-emitting device 100 described in the above-mentioned embodiments and modifications can be used as a light source for various devices. For example, the light-emitting device 100 can be used as a light source for a resin curing device, a light source for a sterilization / disinfection / sterilization device, or a sensor light source for a distance measuring device.
[0108] 100, 110, 120, 130 Light-emitting device 11 Device substrate 13 Light-emitting element 15 Encapsulation body 15A First encapsulating member 15B Second encapsulating member 18 Element mounting electrode 19 Mounting electrode 21 Conductive via 24 Element substrate 25 Semiconductor structural layer 26 p electrode 27 n electrode RP Amorphous fluororesin pellet
Claims
1. An element bonding step to form an element-bonded device substrate by bonding a light-emitting element that emits ultraviolet light to a pair of mounting electrodes of a device substrate having a flat substrate and a pair of mounting electrodes formed on the upper surface of the substrate; and a sealing body forming step to form a translucent sealing body made of amorphous fluororesin that seals the light-emitting element on the device substrate, wherein the sealing body forming step comprises a first step of forming a resin layer made of amorphous fluororesin over the upper surface of the device substrate and the surface of the light-emitting element; and a second step after the first step of placing one amorphous fluororesin pellet on the upper surface of the light-emitting element, softening the resin layer and the amorphous fluororesin pellet by heating, pressing the resin layer formed on the upper surface of the light-emitting element against the amorphous fluororesin pellet to bond the resin layer and temporarily fix the amorphous fluororesin pellet to the resin layer. A method for manufacturing a light-emitting device, comprising: a third step, after the second step, holding the element-bonded device substrate in the substrate-holding mold of a molding die having a substrate-holding mold and a concave female mold, with its bottom surface in contact with the substrate-holding mold; positioning the female mold so that it faces the surface of the substrate-holding mold on which the device substrate is placed; and closing the substrate-holding mold and the female mold to deform the amorphous fluororesin pellets while softening the resin layer and the amorphous fluororesin pellets by heating, thereby forming the sealant.
2. The method for manufacturing a light-emitting device according to claim 1, characterized in that, in the third step, a portion of the amorphous fluororesin pellet other than the edge of the surface opposite to the surface in contact with the resin layer is in contact with the surface of the female mold.
3. The method for manufacturing a light-emitting device according to claim 1, characterized in that, in the second step, the shape of the amorphous fluororesin pellet is deformed into a frustum shape that widens toward the surface in contact with the resin layer.
4. The method for manufacturing a light-emitting device according to claim 1, characterized in that, in the second step, the amorphous fluororesin pellet is held so that the bottom surface of the amorphous fluororesin pellet is in contact with the bottom surface of the recess of a pellet-holding type having a recess having an opening larger than that of the amorphous fluororesin pellet.
5. The method for manufacturing a light-emitting device according to claim 1, characterized in that the female mold of the molding die has a bullet shape.
6. The method for manufacturing a light-emitting device according to claim 1, characterized in that the female mold of the molding die has a frustum shape that widens toward the opening of the female mold.
7. The functional group of the amorphous fluororesin is -CF 3 A method for manufacturing a light-emitting device according to any one of claims 1 to 6, characterized in that it is such.