Silver alloy film, laminate, semiconductor chip, silver alloy sputtering target, and method for producing silver alloy film
A silver-tin-bismuth alloy film with a thin laminate structure addresses oxidation and grain growth issues in semiconductor chip electrodes, ensuring effective barrier performance and cost reduction by minimizing silver usage.
Patent Information
- Application Number
- PCT/JP2026/017501
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
Existing silver coatings on nickel films in semiconductor chips are prone to oxidation and grain aggregation under thermal load, leading to voids and pinholes that degrade solder wettability and increase costs due to the need for thicker films to maintain barrier performance.
A silver alloy film composed of silver, tin, and bismuth, with specific mass percentages, is used to form a thin laminate structure that includes a titanium and nickel layer, suppressing oxidation and grain growth, thereby maintaining barrier performance and reducing silver usage.
The silver alloy film achieves sufficient barrier properties with a thin film thickness, reducing silver usage and costs while enhancing solder wettability and heat resistance.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Silver alloy film, laminate, semiconductor chip, silver alloy sputtering target, and method for producing silver alloy film
[0001] The present disclosure relates to a silver alloy film, a laminate, a semiconductor chip, a silver alloy sputtering target, and a method for producing a silver alloy film.
[0002] For mounting semiconductor chips and semiconductor devices (such as power devices) on circuit boards, wire bonding methods and flip chip methods are used. Since the electrode portions of semiconductor chips and the like are joined by solder, the electrode portions are required to have good solder wettability. When a thermal load is applied to a semiconductor chip or the like during the mounting process or use process, an oxide film is formed at the joint interface between the electrode portion and the solder, which may degrade the joinability. Therefore, it is required that good solder wettability is maintained even when a thermal load is applied.
[0003] In relation to the above, Patent Document 1 discloses a back electrode having a multilayer structure of Ti layer / Ni layer / Ag alloy phase regarding the electrode structure of semiconductor devices such as power modules. Further, Patent Document 2 discloses a back electrode for semiconductor devices, in which a nickel silicide layer forming an ohmic junction is formed on a SiC semiconductor substrate, and a titanium layer and a metal layer (nickel layer, platinum layer, silver layer, gold layer, etc.) are formed on the nickel silicide.
[0004] Patent Document 3 discloses a tin alloy sputtering target used for soldering external electrodes of electronic components and semiconductor elements. Further, Patent Document 4 discloses an electrode having a tin alloy film composed of an alloy of tin, silver and palladium, containing tin as a main component, 4.0 mass% to 20 mass% of silver, and 0.03 mass% to 0.5 mass% of palladium, and a sputtering target for forming a coating film.
[0005] International Publication No. 2018 / 117104, Japanese Unexamined Patent Publication No. 2010-86999, Japanese Unexamined Patent Publication No. 2016-79499, Japanese Unexamined Patent Publication No. 2020-7600
[0006] Various materials and structures are used in the electrode portions of semiconductor chips and the like. For example, a titanium film is formed to form an ohmic junction with the electrode (aluminum) of the semiconductor chip, and a nickel film is formed on top of it to bond with the solder material. Furthermore, since the outermost layer of the nickel film oxidizes when subjected to thermal load, a silver film or gold film is used as a barrier layer on the surface of the nickel film to prevent this.
[0007] The silver or other coatings formed on the surface of nickel films need to be of a certain thickness to ensure barrier performance. However, increasing the film thickness increases the amount of silver, a precious metal, used, which raises the cost of film formation. In this regard, if the heat resistance and solder wettability of the silver coating can be improved, sufficient barrier performance can be achieved even with a thin film thickness, thereby reducing the amount of expensive silver used.
[0008] The object of this disclosure is to provide a silver alloy film having good barrier properties, and a silver alloy sputtering target on which said film can be formed.
[0009] The gist of this disclosure is as follows: [1] A silver alloy film comprising silver, tin, and bismuth, wherein when the total content of silver, tin, and bismuth is 100% by mass, it contains 0.5% by mass or more and 10.0% by mass or less of tin, 1.0% by mass or less of bismuth, and the remainder is silver. [2] The silver alloy film according to [1], wherein the film thickness is 500 nm or less. [3] A laminate comprising the silver alloy film according to [1] or [2]. [4] A laminate comprising the silver alloy film according to any one of [1] to [3] and a nickel layer. [5] A laminate comprising the silver alloy film according to any one of [1] to [4], a nickel layer, and a titanium layer in that order. [6] A semiconductor chip comprising the laminate according to any one of [3] to [5] as an electrode portion. [7] A silver alloy sputtering target comprising silver, tin, and bismuth, wherein when the total content of silver, tin, and bismuth is 100% by mass, it contains 3.5% by mass or more and 20.0% by mass or less of tin, 15.0% by mass or less of bismuth, and the remainder is silver. [8] A method for producing a silver alloy film using the silver alloy sputtering target described in [7].
[0010] This disclosure provides a silver alloy coating with good barrier properties and a silver alloy sputtering target suitable for forming said silver alloy coating. The silver alloy coating in this disclosure has sufficient barrier performance even when thin, thus reducing the amount of silver used.
[0011] <Regarding Silver Alloy Coatings> In the electrode parts of semiconductor chips and the like, a nickel (Ni) film is formed as an underlayer for solder bonding. However, when Ni oxidizes, the solderability deteriorates significantly. Therefore, a silver (Ag) film is formed on the nickel film to prevent Ni oxidation. However, as the silver film thins, the underlying nickel film becomes more susceptible to oxidation due to thermal load. Furthermore, the silver film has the problem of being prone to aggregation due to the growth of crystal grains under thermal load. Ag aggregation generates voids and pinholes on the silver film, and oxygen permeates through these gaps, causing oxidation of the underlying nickel film. Pinholes and voids, in particular, become more pronounced as the silver film thins, posing a problem in maintaining thin film thickness and good barrier properties.
[0012] The silver alloy film according to the embodiments of this disclosure is a silver alloy film containing silver (Ag), tin (Sn), and bismuth (Bi). Tin (Sn) diffuses into the surface layer of the silver alloy film and concentrates therein, capturing permeating oxygen and forming SnO 2 Therefore, it is thought that oxidation of the underlying nickel film can be suppressed. SnO is formed on the surface. 2 It is easily reduced by flux and has little effect on solder joint properties. In addition, bismuth (Bi) can raise the recrystallization temperature of silver, and since grain growth is suppressed by the increased recrystallization temperature, Ag aggregation becomes less likely. As a result, it is possible to suppress the oxidation of the underlying nickel film that occurs due to aggregation.
[0013] The silver alloy film according to the embodiment of this disclosure contains, when the total content of silver, tin, and bismuth is 100% by mass, tin is 0.5% by mass or more and 10.0% by mass or less, bismuth is 1.0% by mass or less, and the remainder is silver. This allows for sufficient barrier performance even with a thin film thickness, and reduces the cost of film formation. If the tin content is less than 0.5% by mass, a sufficient tin oxide film cannot be formed. On the other hand, if the tin content exceeds 10.0% by mass, an oxide film that cannot be completely removed even with flux is formed. Therefore, the tin (Sn) content is set to 0.5% by mass or more and 10.0% by mass or less. Preferably, it is 1.0% by mass or more. Also preferably, it is 8.0% by mass or less, and more preferably 5.0% by mass or less.
[0014] Furthermore, if the bismuth content exceeds 1.0% by mass, a bismuth oxide film forms on the surface of the coating, reducing solder wettability. Therefore, the bismuth content is 1.0% by mass or less. More preferably, the bismuth content is 0.8% by mass or less. Note that if the bismuth content is less than 0.001% by mass, the aggregation suppression effect may not be sufficiently exhibited, so it is preferable that the bismuth content is 0.001% by mass or more. More preferably, it is 0.005% by mass or more.
[0015] If the silver alloy coating of this embodiment contains a large amount of impurities, it may reduce the barrier performance of the silver alloy coating. Therefore, it is preferable that the total impurity content be less than 0.1% by mass. In this case, the impurity content is calculated by assuming that the total content of silver, tin, bismuth, and impurities is 100% by mass.
[0016] The silver alloy film according to this embodiment can have a film thickness of 500 nm or less. Even with a film thickness of 500 nm or less, it has good barrier properties. Preferably, it is 300 nm or less, more preferably 200 nm or less, and even more preferably 100 nm or less. By making it a thin film, the amount of silver, a precious metal, used can be reduced, and the cost of film formation can be suppressed.
[0017] <About the Laminate> The laminate according to the embodiment of this disclosure comprises a silver alloy film containing silver (Ag), tin (Sn), and bismuth (Bi), wherein when the total content of silver, tin, and bismuth is 100% by mass, it contains 0.5% by mass or more and 10.0% by mass or less of tin, 1.0% by mass or less of bismuth, and the remainder is silver. In particular, the laminate can be made by sequentially laminating layers of a Ti layer for electrically ohmic bonding with silicon of a circuit board, a Ni film as a solder underlayer, and a silver alloy film to prevent oxidation of the Ni film.
[0018] <Silver Alloy Sputtering Target> When a film is deposited using a silver alloy sputtering target, the Sn concentration in the film is less than one-third of the Sn concentration in the sputtering target. Also, the Bi concentration in the film is less than one-tenth of the Bi concentration in the sputtering target. This is thought to be due to the fact that the sputtering rate of Sn is lower than that of Ag, the main component, and the sputtering rate of Bi is significantly lower than that of Ag. For these reasons, it is preferable to determine the composition of the silver alloy film and the silver alloy sputtering target while taking into account the difference in the composition of Sn and Bi.
[0019] In view of these circumstances, the silver alloy sputtering target according to this embodiment contains silver (Ag), tin (Sn), and bismuth (Bi), and when the total content of silver, tin, and bismuth is taken as 100% by mass, it contains 3.5% by mass or more and 20.0% by mass or less of tin, 15.0% by mass or less of bismuth, and the remainder is silver. A silver alloy film formed using a sputtering target with such a composition has sufficient barrier performance even when the film thickness is relatively thin, and the cost of film formation can be reduced. The tin content is preferably 3.0% by mass or more, more preferably 4.0% by mass or more, and particularly preferably 5.0% by mass or more. It is also preferably 15.0% by mass or less, and more preferably 10.0% by mass or less.
[0020] If the silver alloy sputtering target of this embodiment contains a large amount of impurities, it may cause particles during sputtering, potentially reducing the barrier performance of the silver alloy coating. Therefore, it is preferable that the total impurity content be less than 0.1% by mass. In this case, the impurity content is calculated by assuming that the total content of silver, tin, bismuth, and impurities is 100% by mass.
[0021] The silver alloy sputtering target according to this embodiment preferably has a cast structure. As described later, the silver alloy sputtering target is made from an ingot cast from molten silver alloy, but it is then finished into a sputtering target by machining such as cutting and polishing, without rolling or forging. If it has a cast structure, a film of relatively uniform thickness can be formed during sputtering.
[0022] <Method for Manufacturing a Silver Alloy Sputtering Target> An example of a method for manufacturing a silver alloy sputtering target according to this embodiment is shown. However, the silver alloy sputtering target according to this embodiment is not limited to those obtained by the following manufacturing method. In order to avoid making the manufacturing method unnecessarily unclear, detailed explanations of publicly known matters are omitted.
[0023] Prepare silver (Ag), tin (Sn), and bismuth (Bi) with a purity of 99.9% by mass or higher. While the purity is not particularly critical, it is preferable to use relatively high-purity raw materials, as a high level of impurities can degrade the solder joint.
[0024] Next, these raw materials are melted using a high-frequency vacuum melting furnace or the like. Specifically, a sealable chamber is evacuated, an inert gas such as argon or nitrogen is introduced, and then silver, tin, and bismuth are added to achieve a predetermined composition. Each metal material is melted to obtain a molten silver alloy. This molten metal is then cast to obtain a silver alloy ingot.
[0025] By cutting the resulting silver alloy ingot into a disc shape of the desired diameter and thickness, a disc-shaped silver alloy sputtering target can be manufactured. The target shape is not particularly limited and can also be rectangular.
[0026] <Method for manufacturing a silver alloy film> A silver alloy film can be formed using a silver alloy sputtering target. Specifically, the vacuum level inside the chamber of the sputtering apparatus is 1 × 10⁻⁶. -4 After reaching Pa, sputtering is performed sequentially using a Ti sputtering target, a Ni sputtering target, and a silver alloy sputtering target while supplying argon gas at 10 cc / min, thereby forming a Ti / Ni / Ag alloy laminated film on a semiconductor substrate.
[0027] Next, examples and comparative examples of the present invention will be described. Note that the following examples are representative examples, and the present invention is not limited to these examples; it should be interpreted within the scope of the technical concept described in the specification.
[0028] The various physical properties of the silver alloy sputtering target and silver alloy coating in this example and comparative example were evaluated as follows.
[0029] <About Compositional Analysis> The composition of the sputtering target was determined by analyzing the dissolved sample using ICP-AES (Inductively Coupled Plasma Emission Spectroscopy). The composition of the coating was determined by analyzing the sample deposited on the Si wafer using GD-MS (Glow Discharge Mass Spectroscopy).
[0030] <About Film Thickness Analysis> For film thickness analysis, a cross-section of the film was prepared from a sample deposited on a Si wafer using a cross-section polisher (CP), and the film thickness was measured using a scanning electron microscope (SEM).
[0031] The barrier properties were evaluated from the perspectives of heat resistance and solder wettability. Heat resistance and solder wettability were judged as "excellent," "good," or "poor," and if either was rated "poor," it was determined that sufficient barrier performance had not been achieved.
[0032] <Evaluation of Heat Resistance> After heating the film samples at 200°C for 1 hour, depth profiling was performed using XPS (X-ray photoelectron spectroscopy) to confirm the degree of oxidation of the Ag / Ni interface layer. Samples with no oxidation in the Ag / Ni interface layer (almost no oxygen peaks and no peak shift due to Ni oxidation) were classified as excellent, samples with slight oxidation (oxygen peaks were observed, but no peak shift due to Ni oxidation was observed) were classified as good, and samples with confirmed oxidation (oxygen peaks were observed, and a peak shift due to Ni oxidation was observed) were classified as poor.
[0033] <Evaluation of Solder Wettability> Solder wettability was evaluated for the film samples after heating at 200°C for 1 hour. For the solder wetting spread test, a film sample coated with Type-R flux (Senju Metal Industry Co., Ltd., rosin flux 25% IPA solution) was placed on it, and then a Sn-3.0Ag-0.5Cu solder ball (Nippon Steel Micrometal LF45) was placed on it. Reflow soldering (preheating 150°C, preliminary heating 180°C for 90 seconds, main heating 237°C for 65 seconds) was performed to melt the solder. The height of the solder ball was measured using a digital microscope (Keyence VHX-8000) to observe the shape of the molten solder, and the solder wetting spread rate was calculated using the following formula to evaluate the solder wettability. (Formula) S = (D / h) / D × 100 (%) S: Solder wetting spread rate D: Diameter (height) of solder ball before reflow h: Height of solder ball after reflow The wetting spread rate was measured five times, and those with an average value of 80% or higher were classified as excellent, those with an average value of 60% or higher as good, and those with an average value of less than 60% as poor.
[0034] (Example 1) A titanium layer was deposited to a thickness of 20 nm on a silicon wafer (20 mm × 20 mm × 0.5 mm) using a titanium sputtering target. Next, a nickel layer was deposited to a thickness of 500 nm using a nickel sputtering target. Then, a silver alloy film was deposited to a thickness of 500 nm using a silver alloy sputtering target containing 7.0 mass% tin and 1.0 mass% bismuth to form a laminated sample. The sample was then heated at 200°C for 1 hour to test its heat resistance and solder wettability. As shown in Table 1, the sample exhibited excellent barrier properties.
[0035] (Example 2) The laminated sample of Example 2 was prepared in the same manner as in Example 1, except that a silver alloy film was deposited to a thickness of 100 nm. Then, heat resistance and solder wettability tests were performed in the same manner as in Example 1. As a result, as shown in Table 1, excellent barrier properties were observed.
[0036] (Example 3) The laminated sample of Example 3 was formed in the same manner as in Example 1, except that a silver alloy film was formed to a thickness of 100 nm using a silver alloy sputtering target containing 3.5% by mass of tin and 1.0% by mass of bismuth. As a result, the barrier properties were excellent, as shown in Table 1.
[0037] (Example 4) The laminated sample of Example 4 was formed in the same manner as in Example 1, except that a silver alloy film was formed to a thickness of 100 nm using a silver alloy sputtering target containing 15.0% by mass of tin and 1.0% by mass of bismuth. As a result, the barrier properties were excellent, as shown in Table 1.
[0038] (Example 5) The laminated sample of Example 5 was formed in the same manner as in Example 1, except that a silver alloy film was formed to a thickness of 100 nm using a silver alloy sputtering target containing 7.0% by mass of tin and 2.0% by mass of bismuth. As a result, the barrier properties were excellent, as shown in Table 1.
[0039] (Example 6) A laminate sample of Example 6 was formed into a film in the same manner as in Example 1, except that a silver alloy sputtering target containing 7.0 mass% of tin and 10.0 mass% of bismuth was used to form a silver alloy film with a thickness of 100 nm. As a result, as shown in Table 1, excellent barrier properties were exhibited.
[0040] (Comparative Example 1) A laminate sample of Comparative Example 1 was formed into a film in the same manner as in Example 1, except that a pure silver sputtering target was used to form a pure silver film with a thickness of 100 nm. Then, tests for heat resistance and solder wettability were performed in the same manner as in Example 1 described above. As a result, as shown in Table 1, poor barrier properties were exhibited.
[0041] (Comparative Example 2) A laminate sample of Comparative Example 2 was formed into a film in the same manner as in Comparative Example 1, except that a pure silver film was formed to a thickness of 500 nm. Then, tests for heat resistance and solder wettability were performed in the same manner as in Example 1 described above. As a result, as shown in Table 1, poor barrier properties were exhibited.
[0042] (Comparative Example 3) A laminate sample of Comparative Example 3 was formed into a film in the same manner as in Example 1, except that a silver alloy sputtering target containing 35.0 mass% of tin and 1.0 mass% of bismuth was used to form a silver alloy film with a thickness of 100 nm. As a result, as shown in Table 1, poor solder wettability was exhibited.
[0043] (Comparative Example 4) A laminate sample of Comparative Example 4 was formed into a film in the same manner as in Example 1, except that a silver alloy sputtering target containing 7.0 mass% of tin (containing no Bi) was used to form a silver alloy film with a thickness of 100 nm. As a result, as shown in Table 1, poor solder wettability was exhibited.
[0044]
[0045] The silver alloy film according to this embodiment has the excellent effect of having sufficient barrier performance even when the film thickness is thin. The silver alloy sputtering target according to this embodiment can reduce the cost of film formation compared to using a conventional silver sputtering target. The silver alloy sputtering target according to this embodiment is useful for forming a barrier film that constitutes the outermost layer of the electrode portion of a semiconductor chip (power device, etc.).
Claims
1. A silver alloy coating containing silver, tin, and bismuth, wherein when the total content of silver, tin, and bismuth is 100% by mass, it contains 0.5% to 10.0% by mass of tin, 1.0% by mass or less of bismuth, and the remainder is silver.
2. The silver alloy film according to claim 1, wherein the film thickness is 500 nm or less.
3. A laminate comprising a silver alloy film as described in claim 1 or 2.
4. A laminate comprising a silver alloy film and a nickel layer as described in claim 1 or 2.
5. A laminate comprising, in order, a silver alloy film, a nickel layer, and a titanium layer, as described in claim 1 or 2.
6. A semiconductor chip comprising the laminate described in claim 3 as an electrode portion.
7. A silver alloy sputtering target comprising silver, tin, and bismuth, wherein when the total content of silver, tin, and bismuth is taken as 100% by mass, it contains 3.5% to 20.0% by mass of tin, 15.0% by mass or less of bismuth, and the remainder is silver.
8. A method for producing a silver alloy film using the silver alloy sputtering target described in claim 7.