Spherical composite particles of barium sulfate and silica, and method for producing same

Spherical composite particles of barium sulfate and silica, produced through a specific manufacturing process, address the need for safer, stable cosmetic particles with enhanced feel and blurring effect, replacing harmful microplastic beads.

WO2026240015A1PCT designated stage Publication Date: 2026-11-19SAKAI CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017569
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-13
Filing Date
2026-05-08
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

There is a need for safer, chemically stable inorganic spherical particles for cosmetics that provide excellent powdery feel and blurring effect, replacing polymer-based microplastic beads which are environmentally harmful and potentially absorbed by the body.

Method used

Spherical composite particles of barium sulfate and silica are produced by preparing a slurry with barium sulfate, silica, and optionally magnesium sulfate, followed by spray-drying and calcining at specific temperatures to achieve desired properties such as high haze, low MMD value, and sharp particle size distribution.

Benefits of technology

The resulting particles offer excellent powdery feel and blurring effect, are safe for the human body, and suitable for cosmetic applications, providing a safer alternative to microplastic beads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017569_19112026_PF_FP_ABST
    Figure JP2026017569_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides spherical composite particles which contain barium sulfate, the spherical composite particles having excellent powder feel and excellent blur effect when applied to the skin. The present invention relates to spherical composite particles of barium sulfate and silica, the spherical composite particles of barium sulfate and silica being characterized in that: the haze of a coating film as measured by the measurement method described below is 35% or more; and the MMD value as measured using a friction tester under the measurement conditions described below is 0.013 or less. [Haze measurement method] 1.0 g of a sample and 0.9 g of silicone oil were kneaded using a planetary centrifugal mixer at a rotation speed of 2,000 rpm for 3 minutes, the kneaded product was placed on a glass plate, and a coating film was formed using a bar coater #14. The haze (%) of the thus-formed coating film was measured. [Measurement of MMD Value] 0.15 g of a sample was placed on the upper surface of a double-sided tape, having a width of 15 mm and a length of 50 mm and attached to a slide glass, and the upper surface of the double-sided tape on which the sample was placed was stroked four times in a fixed direction from one end to the other end of the length of 50 mm with a cosmetic puff. Thereafter, mean friction deviation (MMD) was measured by a friction tester under the conditions of a friction measurement load of 25 gf, a surface measurement sample moving speed of 1 mm / sec, and a measurement distance range of 20 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Spherical composite particles of barium sulfate and silica and method for producing the same

[0001] This invention relates to spherical composite particles of barium sulfate and silica, and a method for producing the same.

[0002] In the cosmetics industry, spherical particles are widely used as texture enhancers, taking advantage of their rolling properties when applied to the skin. Traditionally, polymer-based materials such as PMMA and silicones have been the main materials used as texture enhancers. However, in recent years, concerns have been raised that these polymers may be ingested by plankton in the ocean, leading to the concentration of harmful substances in the food chain. In particular, so-called ultrafine microplastic beads, which are finely crushed polymers that are not biodegradable, are a cause for concern not only for environmental pollution but also for the adverse effects of being absorbed into the body as foreign substances that cannot be broken down internally and remain there for a long time. Laws to regulate microplastic beads are being developed in various countries, and in this context, there is a growing movement to replace them with spherical particles mainly composed of inorganic materials. Among inorganic materials, spherical silica is well known, but there is a demand for materials that are safer for living organisms and the human body. Especially since cosmetics are applied directly to the skin, the materials must be guaranteed to be safe. In addition to safety, the particles must not easily dissolve in rain or sweat, nor alter the oil and other components in cosmetics. Therefore, chemically stable inorganic spherical particles are desired.

[0003] Barium sulfate is being considered as such an inorganic spherical particle. Barium sulfate is a sparingly soluble ionic substance that is insoluble in water, acids, and alkalis, and is very stable even in the pH range where it is expected to be used in cosmetics. It is also a compound that is highly safe for the human body and is used as an X-ray contrast agent. As barium sulfate for use in cosmetics, a spherical composite powder of barium sulfate and silica has been disclosed, which is prepared by preparing barium sulfate from barium hydroxide and sulfuric acid, preparing a slurry containing the barium sulfate and silica sol, and then spray-drying and calcining the slurry (see Patent Document 1). It has also been disclosed that spherical composite particles of barium sulfate and silica that fully conform to the specifications for "barium sulfate" described in the "Standards for Raw Materials of Quasi-drugs 2021" can be obtained by washing the raw material barium sulfate with an aqueous sodium sulfate solution, mixing the barium sulfate with silica sol to make a slurry, spray-drying the slurry, and calcining the resulting dried product at a predetermined temperature (see Patent Document 2).

[0004] Japanese Patent No. 6390756, International Publication No. 2023 / 176912

[0005] As mentioned above, spherical composite particles containing barium sulfate are known, and while they have reached a certain level in terms of the powdery feel and blurring effect (blurring wrinkles and blemishes on the skin) required for cosmetic applications, further performance improvements were desired.

[0006] In view of the above situation, the present invention aims to provide spherical composite particles containing barium sulfate that have excellent powdery feel and blurring effect when applied to the skin.

[0007] The inventors investigated spherical composite particles containing barium sulfate that have excellent powdery feel and blurring effect when applied to the skin. They found that by preparing a slurry containing barium sulfate, silica, and magnesium sulfate, spray-drying the slurry, and firing it at a predetermined temperature to produce spherical composite particles of barium sulfate and silica, particles with excellent powdery feel and blurring effect when applied to the skin can be obtained, thus completing the present invention.

[0008] In other words, the present invention is as follows: [1] Spherical composite particles of barium sulfate and silica, characterized in that the haze of the coating film measured by the measurement method below is 35% or more, and the MMD value measured using a friction tester under the measurement conditions below is 0.013 or less. [Method for measuring haze] 1.0 g of sample and 0.9 g of silicone oil were mixed using a rotary-orbit mixer at a rotation speed of 2000 rpm for 3 minutes, the mixture was placed on a glass plate, and a coating film was created using a bar coater #14. The haze (%) of the coating film after creation was measured. [MMD Value Measurement] 0.15 g of the sample was placed on the top surface of a 15 mm wide, 50 mm long piece of double-sided tape attached to a glass slide. The top surface of the double-sided tape with the sample was then stroked four times in a consistent direction from one end to the other over a 50 mm length using a cosmetic puff. The MMD (mean deviation of the coefficient of friction) was then measured using a friction tester under the following conditions: friction measurement load of 25 gf, surface measurement sample movement speed of 1 mm / sec, and measurement distance range of 20 mm.

[0009] [2] The spherical composite particles of barium sulfate and silica according to [1], characterized in that the sphericity is 1.10 or less and the particle size distribution D90 / D10 is 4.5 or less.

[0010] A cosmetic filler characterized by containing spherical composite particles of barium sulfate and silica as described in [3] [1] or [2].

[0011] A cosmetic composition characterized by containing spherical composite particles of barium sulfate and silica as described in [4] [1] or [2].

[0012] [5] A method for producing spherical composite particles of barium sulfate and silica, the method comprising: a mixing step of preparing a slurry containing barium sulfate, silica, and magnesium sulfate; a drying step of spray-drying the slurry obtained in the mixing step to obtain a dried product; and a calcination step of calcining the dried product obtained in the drying step at 800 to 1100°C.

[0013] [6] The method for producing spherical composite particles of barium sulfate and silica according to [5], characterized in that the mixing step is a step of preparing a slurry by mixing a slurry containing barium sulfate and silica with magnesium sulfate.

[0014] [7] The method for producing spherical composite particles of barium sulfate and silica according to [5], characterized in that the barium sulfate used in the mixing step is obtained by a manufacturing method that includes a washing step of washing barium sulfate with an aqueous sodium sulfate solution or dilute sulfuric acid, wherein the pigment pH measured in accordance with JIS K 5101 "Pigment pH boiling method" is 7.0 to 9.0 and the primary particle diameter is 0.1 μm or less, and a sulfide removal step of removing sulfides contained in the barium sulfate obtained in the washing step.

[0015] [8] The method for producing spherical composite particles of barium sulfate and silica according to [7], characterized in that the sulfide removal step is carried out by filtering the barium sulfate obtained in the washing step and washing it with water.

[0016] The spherical composite particles of barium sulfate and silica of the present invention are stable and highly safe powders mainly composed of barium sulfate, and are suitable for use as a texture enhancer for cosmetics because they have excellent powder feel and blurring effect when applied to the skin. The spherical composite particles of barium sulfate and silica of the present invention are suitable as a substitute material for microplastic beads. The method for producing the spherical composite particles of barium sulfate and silica of the present invention is a useful method for producing such spherical composite particles of barium sulfate and silica.

[0017] This is a scanning electron microscope image of the spherical composite particles of barium sulfate and silica obtained in Example 1.

[0018] The following describes preferred embodiments of the present invention in detail, but the present invention is not limited to the following description and can be modified and applied as appropriate without altering the essence of the invention.

[0019] 1. Spherical Composite Particles of Barium Sulfate and Silica The spherical composite particles of barium sulfate and silica of the present invention are characterized by having a haze of 35% or more of the coating film measured by the measurement method described below, and an MMD value of 0.013 or less measured using a friction tester under the measurement conditions described below, and are particles that have excellent powder feel and blurring effect when applied to the skin. Since the spherical composite particles of barium sulfate and silica of the present invention are spherical particles mainly composed of barium sulfate, their refractive index is greater than that of silica and smaller than that of white pigments such as titanium dioxide and zinc oxide. As a result, when a coating film is formed on the skin, while light is transmitted, a relatively large amount of scattered light is produced, making it possible to naturally blur and make less noticeable defects such as blemishes and wrinkles on the skin, as if covered with frosted glass. When scattered transmitted light accounts for a large proportion of transmitted light, such a blurring effect is obtained and it can be considered a high-haze material. The spherical particles of the present invention, which mainly consist of barium sulfate, exhibit higher haze compared to microplastic beads conventionally used in cosmetics. Furthermore, the spherical composite particles of barium sulfate and silica of the present invention have a sharp particle size distribution, resulting in a good powdery feel. The MMD value is an indicator of roughness; generally, a smaller value indicates less roughness. The haze of the coating film measured by the measurement method below should be 35% or more, but preferably 40% or more. More preferably 45% or more. Also, the MMD value measured under the measurement conditions below should be 0.013 or less, but preferably 0.012 or less. More preferably 0.010 or less. [Method for measuring haze] 1.0 g of sample and 0.9 g of silicone oil were mixed using a rotary-orbit mixer at a rotation speed of 2000 rpm for 3 minutes. The mixture was placed on a glass plate, and a coating film was created using a bar coater #14. The haze (%) of the coating film after creation was measured. [MMD Value Measurement] 0.15 g of the sample was placed on the top surface of a 15 mm wide, 50 mm long piece of double-sided tape attached to a glass slide. The top surface of the double-sided tape with the sample was then stroked four times in a consistent direction from one end to the other over a 50 mm length using a cosmetic puff. The MMD (mean deviation of the coefficient of friction) was then measured using a friction tester under the following conditions: friction measurement load of 25 gf, surface measurement sample movement speed of 1 mm / sec, and measurement distance range of 20 mm.

[0020] The spherical composite particles of barium sulfate and silica of the present invention preferably have an average particle diameter of 0.5 to 10 μm. Such an average particle diameter allows for a good powdery feel and facilitates uniform spreading on the skin. The average particle diameter is more preferably 1 to 8 μm, and even more preferably 2 to 6 μm. The average particle diameter of the spherical composite particles of barium sulfate and silica can be measured by the method described in the examples below.

[0021] The spherical composite particles of barium sulfate and silica of the present invention preferably have a sphericity of 1.10 or less and a particle size distribution D90 / D10 of 4.5 or less. By using such particles in cosmetics, the feel of the cosmetic when applied to the skin can be further improved, and the light scattering effect (blurring effect) can be obtained more sufficiently. The sphericity of the spherical composite particles of barium sulfate and silica is more preferably 1.07 or less, and even more preferably 1.05 or less. The particle size distribution D90 / D10 of the spherical composite particles of barium sulfate and silica is more preferably 1.0 to 4.0, and even more preferably 1.0 to 3.7. The sphericity and particle size distribution D90 / D10 of the spherical composite particles of barium sulfate and silica can be measured by the method described in the examples below.

[0022] In the spherical composite particles of barium sulfate and silica of the present invention, the silica content is preferably 3 to 20% by mass relative to the total spherical composite particles of barium sulfate and silica. By including silica in this proportion, the composite particles can be made more spheric and closer to a perfect sphere without losing the properties of barium sulfate. More preferably, the silica content in the spherical composite particles of barium sulfate and silica is 5 to 15% by mass, and even more preferably 7 to 13% by mass, relative to the total spherical composite particles of barium sulfate and silica.

[0023] The spherical composite particles of barium sulfate and silica of the present invention are preferably obtained by a manufacturing method using magnesium sulfate, as described later. In this case, the spherical composite particles of barium sulfate and silica contain magnesium. When the spherical composite particles of barium sulfate and silica of the present invention contain magnesium, the magnesium content is preferably 50 to 1500 ppm relative to the spherical composite particles of barium sulfate and silica. When the magnesium content is within this range, the particle size distribution of the spherical composite particles mainly composed of barium sulfate becomes sharper, resulting in a better powder feel and a greater light scattering effect (blurring effect). The magnesium content is more preferably 100 to 1000 ppm, and even more preferably 200 to 600 ppm.

[0024] The above spherical composite particles may further have a surface treatment layer made of a water-repellent organic compound. The surface treatment with a water-repellent organic compound is a water-repellent treatment that reduces the affinity of the surface of the spherical composite particles to water.

[0025] Examples of the above-mentioned water-repellent organic compounds include organic surface treatments using organosilicon compounds, organoaluminum compounds, organotitanium compounds, higher fatty acids, metal soaps, polyhydric alcohols, alkanolamines, etc. Alternatively, multiple surface treatments may be applied. Specific examples of water-repellent organic compounds include silicone oils such as hydrogen dimethicone and triethoxysilylethylpolydimethylsiloxyethylhexyl dimethicone; alkyl silanes such as trialkoxyoctylsilane and trialkoxydecylsilane; vinyl trialkoxysilane; silane coupling agents such as 3-glycosidoxypropyl trialkoxysilane, 3-methacryloxypropylmethyldialkoxysilane, 3-aminopropyltrialkoxysilane, and 3-mercaptopropylmethyldialkoxysilane; and fatty acids having 12 to 18 carbon atoms, such as stearic acid, isostearic acid, myristic acid, palmitic acid, and palm oil fatty acids, or their metal salts. Among these, fatty acids having 12 to 18 carbon atoms or their metal salts are preferred. Examples of metal salts of fatty acids include salts of lithium, sodium, potassium, magnesium, calcium, barium, zinc, and aluminum, with calcium and magnesium salts being particularly preferred. Compounds that chemically bond with the composite powder are also preferred, although compounds that physically adsorb are also acceptable. Surface treatment with such water-repellent organic compounds can further improve the feel of the resulting particles and, for example, improve their compatibility with oils when incorporated into cosmetics.

[0026] The amount of treatment with the water-repellent organic compound is preferably 0.1 to 10% by mass relative to the spherical composite particles of barium sulfate and silica. If the amount of treatment with the water-repellent organic compound is lower than 0.1% by mass, the water repellency will be insufficient. If it exceeds 10% by mass, not only will the cost increase, but the effect may also plateau. More preferably, it is 0.5 to 8% by mass.

[0027] 2. Method for Producing Spherical Composite Particles of Barium Sulfate and Silica The method for producing spherical composite particles of barium sulfate and silica according to the present invention is characterized by comprising a mixing step of preparing a slurry containing barium sulfate, silica, and magnesium sulfate; a drying step of spray-drying the slurry obtained in the mixing step to obtain a dried product; and a firing step of firing the dried product obtained in the drying step at 800 to 1100°C. When the slurry contains magnesium sulfate in addition to barium sulfate and silica, the viscosity increases compared to a slurry containing only barium sulfate and silica. This makes it possible to narrow the particle size distribution of the spray-dried powder and the spherical composite particles of barium sulfate and silica obtained in the end, thereby obtaining spherical composite particles of barium sulfate and silica with an excellent powder feel. Furthermore, the spherical composite particles of barium sulfate and silica obtained in this way also have a better blurring effect than conventional spherical composite particles of barium sulfate and silica.

[0028] The above mixing step preferably involves mixing a slurry containing barium sulfate and silica with magnesium sulfate to prepare a slurry. Barium sulfate slurry has high viscosity, but adding silica reduces its viscosity. By adding magnesium sulfate to a barium sulfate slurry whose viscosity has been reduced by adding silica and mixing it, it becomes easier to thoroughly mix the entire slurry.

[0029] In the method for producing the spherical composite particles of barium sulfate and silica described above, the barium sulfate used as a raw material preferably has an average particle diameter of 0.005 to 0.25 μm. Using barium sulfate with such a particle diameter results in spherical composite particles of barium sulfate and silica with high sphericity, making them more suitable for cosmetic applications. The average particle diameter of the barium sulfate used as a raw material is more preferably 0.01 to 0.15 μm, and even more preferably 0.02 to 0.08 μm. The average particle diameter of the barium sulfate used as a raw material can be measured by the method described in the examples below.

[0030] In the method for producing the spherical composite particles of barium sulfate and silica described above, it is preferable that the barium sulfate used as a raw material is barium sulfate obtained by the reaction of barium sulfide and sulfuric acid. When barium sulfate is produced by reacting barium hydroxide with sulfuric acid, barium carbonate, which is formed when some of the barium hydroxide reacts with carbon dioxide in the air during the production process, is included as an impurity. Similarly, when barium sulfate is produced by reacting barium chloride with sodium sulfate, the sodium chloride produced in the reaction and unreacted sodium sulfate are included as impurities. By producing barium sulfate by reacting barium sulfide with sulfuric acid, the inclusion of these impurities can be prevented. Furthermore, after producing barium sulfate by reacting barium sulfide with sulfuric acid, it is preferable to wash the barium sulfate with an aqueous sodium sulfate solution or a dilute sulfuric acid solution. This converts the small amount of barium salts that are by-products in conventional barium sulfate production methods into barium sulfate, and removes water-soluble barium salts.

[0031] Preferably, the barium sulfate used in the above mixing process is obtained by a manufacturing method that includes a washing step of washing barium sulfate with an aqueous sodium sulfate solution or dilute sulfuric acid, and a washing step of removing sulfides contained in the barium sulfate obtained in the washing step, wherein the pigment pH measured by a method conforming to JIS K 5101 "Pigment pH Boiling Method" is 7.0 to 9.0, and the primary particle size is 0.1 μm or less. Barium sulfate that shows a pigment pH of 7.0 to 9.0 measured by a method conforming to JIS K 5101 "Pigment pH Boiling Method" is barium sulfate with a low content of water-soluble barium salts. By selecting such barium sulfate as a starting material, and further washing it with an aqueous sodium sulfate solution or dilute sulfuric acid to convert the barium salts, which are small impurities contained in the barium sulfate, into barium sulfate, and then performing a step to remove the sulfides contained in the remaining barium sulfate, it is possible to obtain barium sulfate with an extremely low content of water-soluble barium salts. Furthermore, the process of removing sulfides may also remove other impurities, as long as the sulfides are removed.

[0032] The step of removing the sulfide is preferably performed by filtering the barium sulfate obtained in the washing step and washing it with water. By performing the sulfide removal by such a method, the sulfide contained in the barium sulfate can be easily and efficiently removed.

[0033] The amount of silica used in the above mixing step is preferably 3.0 to 25.0 mass% relative to 100 mass% of barium sulfate. It is more preferably 5.5 to 18.0 mass%, and further preferably 7.5 to 15.0 mass%.

[0034] The silica used in the above mixing step preferably has an average particle diameter of 1 to 100 nm. When silica having such an average particle diameter is used, the composite particles of barium sulfate and silica finally obtained will be clean particles with fewer irregularities on the surface when silica with a smaller particle diameter is used. The average particle diameter of silica is more preferably 1 to 60 nm, and further preferably 1 to 20 nm.

[0035] The amount of magnesium sulfate used in the above mixing step is preferably 100 to 10000 ppm relative to barium sulfate. It is more preferably 500 to 8000 ppm, further preferably 1000 to 6000 ppm, and particularly preferably 1500 to 4000 ppm.

[0036] The concentration of barium sulfate in the slurry containing the above-mentioned barium sulfate, silica and magnesium sulfate is preferably 50 to 1000 g / L. It is more preferably 150 to 800 g / L, and further preferably 200 to 600 g / L.

[0037] In the method for producing spherical composite particles of barium sulfate and silica of the present invention, the viscosity of the slurry to be subjected to spray drying is preferably 10 to 1000 mPa·s. Such a viscosity makes the slurry suitable for spray drying. The viscosity of the slurry to be subjected to spray drying is more preferably 100 to 900 mPa·s, and further preferably 200 to 800 mPa·s. The viscosity of the slurry can be measured by the method described in the Examples mentioned later.

[0038] In the method for producing spherical composite particles of barium sulfate and silica of the present invention, the concentration of the slurry to be subjected to spray drying is preferably 50 to 1000 g / L. With such a concentration, the resulting spherical composite particles of barium sulfate and silica have a high sphericity and are more suitable for cosmetic applications. The concentration of the slurry to be subjected to spray drying is more preferably 100 to 700 g / L, and even more preferably 200 to 500 g / L.

[0039] In the method for producing spherical composite particles of barium sulfate and silica of the present invention, before spray-drying the slurry obtained in the mixing step, a step of adding pure water to the slurry to adjust the viscosity of the slurry may be carried out.

[0040] In the method for producing spherical composite particles of barium sulfate and silica of the present invention, the drying temperature in the drying step of spray-drying the slurry obtained in the mixing step to obtain a dried product is preferably 100 to 250°C. It is more preferably 100 to 230°C, and even more preferably 105 to 220°C.

[0041] In the calcination step of calcining the dried product obtained in the above drying step at 800 to 1100°C, the calcination temperature may be 800 to 1100°C, preferably 820 to 1000°C, and more preferably 850 to 950°C. The calcination time is preferably 1 to 20 hours. It is more preferably 1 to 10 hours, and even more preferably 1 to 5 hours.

[0042] The method for producing spherical composite particles of barium sulfate and silica of the present invention may include other steps in addition to the above-described mixing step, drying step, calcination step, and step of adding pure water to the slurry before spray drying to adjust the viscosity of the magnesium sulfate mixed slurry. Examples of other steps include a step of dispersing the slurry obtained by mixing the barium sulfate slurry and silica with a wet media disperser or a wet medialess disperser, a step of passing the slurry obtained by mixing the barium sulfate slurry and silica through a sieve with an opening of 20 to 250 μm, and the like.

[0043] 3. Fillers for Cosmetics and Cosmetics As described above, the spherical composite particles of barium sulfate and silica of the present invention are stable and highly safe powders mainly composed of barium sulfate, and are particles that have excellent powder texture and blurring effect when applied to the skin, and can be suitably used as a material for cosmetics. A filler for cosmetics and cosmetics containing such spherical composite particles of barium sulfate and silica of the present invention are also one of the present inventions.

[0044] The above-mentioned cosmetic composition is not particularly limited and can include, for example, skincare products, hair products, makeup products, and UV protection products. In particular, it can be suitably used as a foundation, sunscreen, or makeup base. Furthermore, the form is not particularly limited and can be applied in liquid, emulsion, cream, solid, paste, gel, multilayer, mousse, spray, etc. Moreover, the cosmetic composition of the present invention can be suitably applied in any of the following cases: aqueous cosmetic composition, O / W type cosmetic composition (oil-in-water cosmetic composition), or W / O type cosmetic composition (water-in-oil cosmetic composition).

[0045] The above cosmetic composition may, as necessary, contain one or more aqueous and oily components commonly used in the field of cosmetics. The aqueous and oily components are not particularly limited, but examples include oils, surfactants, thickeners, preservatives, antibacterial agents, antimicrobial agents, preservatives, polyhydric alcohols, UV absorbers, UV shielding agents, antioxidants, humectants, metal ion chelating agents, various extracts, pharmaceutical components, colorants (dyes, pigments, etc.), dyes, thickeners, pH adjusters, fragrances, cooling agents, antiperspirants, disinfectants, skin activators, and various powders.

[0046] Specific examples are given below to illustrate the present invention in detail, but the present invention is not limited to these examples. Unless otherwise specified, "%" and "wt%" mean "weight percent (mass percent)". The measurement methods for each physical property are as follows.

[0047] (1) Method for measuring haze 1.0 g of sample and 0.9 g of KF-96H-10000CS (manufactured by Shin-Etsu Silicone Co., Ltd.) were mixed for 3 minutes at a rotation speed of 2000 rpm using a rotational and revolving mixer Awatori Rentaro ARE-310 (manufactured by Shinky Co., Ltd.). The mixed material was placed on a glass plate and a coating film was created using a bar coater #14. The total light transmittance (%), diffuse light transmittance (%), and parallel light transmittance (%) of the created coating film were measured using a haze meter HM-150 (manufactured by Murakami Color Technology Research Institute Co., Ltd.) and the haze (%) was determined. The haze (%) was calculated by diffuse light transmittance / total light transmittance × 100. The total light transmittance measurement was in accordance with JIS K 7361, and the haze measurement was in accordance with JIS K 7136. (2) Measurement of MMD value A 15 mm wide, 50 mm long double-sided tape (Nichiban Co., Ltd., Nicetack® NW-H15) was attached to a glass slide (Matsunami Glass Industry Co., Ltd., 76 mm x 26 mm x 0.8-1 mm), 0.15 g of the sample was placed on the upper surface of the double-sided tape, and the upper surface of the double-sided tape with the sample was stroked four times in a constant direction from one end to the other over a length of 50 mm using a cosmetic puff (Shobido Co., Ltd., Compact Puff (material NBR)). The MMD (mean deviation of the coefficient of friction) was then measured using a KES-SE friction tester (Kato Tech Co., Ltd.). The measurement was performed under the conditions of a friction measurement load of 25 gf, a surface measurement sample movement speed of 1 mm / sec, and a measurement distance range of 20 mm. A silicone contact (a friction element made of silicone rubber with bumps and grooves designed to simulate a human finger) was used as the sensor.

[0048] (3) Average particle diameter, D90 / D10 The average particle diameter, D90 and D10 were measured using a Microtrac MT3300EXII laser diffraction / scattering particle size distribution analyzer (manufactured by Nikkiso Co., Ltd.). Water was used as the solvent. (4) Sphericity A diagonal line was drawn on an image (magnification 1500x) taken with a scanning electron microscope JSM-6510A (manufactured by JEOL Ltd.), and the major and minor axes of 50 particles lying on that line were measured. The average value of the major / minor axis of each particle was taken as the sphericity. (5) Viscosity Viscosity was measured using a B-type viscometer TVB-10M (manufactured by Toki Sangyo Co., Ltd.) in an environment with a temperature of 20°C. 100 ml of the sample to be measured for viscosity was measured into a 110 ml screw tube, and the measured value at 60 rpm with an M3 rotor was taken as the viscosity.

[0049] Example 1 Barium sulfate raw material with an average particle size of 0.05 μm was prepared by reacting barium sulfide with sulfuric acid (pigment pH 8.5 when dry; the pigment pH measured by a method conforming to JIS K 5101 "Pigment pH boiling method" was the same value). After that, it was washed with water to make a slurry, and pure water was added to adjust the slurry concentration to 135 g / L. Sodium sulfate [anhydrous] (Kishida Chemical Co., Ltd., 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved, stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solid content after washing was repulped with pure water to adjust the slurry concentration to 380 g / L, and silica sol (Snowtex ST-O, Nissan Chemical Co., Ltd., average particle size of silica 0.012 μm, acidic sol) was added to the slurry with BaSO₄ 4 and SiO 2 The mixture was added and mixed in a weight ratio of 92:8. To the mixture, magnesium sulfate (anhydrous) (special grade, 98% manufactured by Fujifilm Wako Pure Chemical Industries) was added to 3000 ppm relative to the barium sulfate, and pure water was added to adjust the slurry concentration to 280 g / L and the viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle diameter of 5.0 μm. The particle size distribution D90 / D10 of the obtained particles was 3.2, the sphericity was 1.03, and the MMD (roughness) value measured with a friction tester was 0.0088. In addition, the haze when used as a coating film exhibiting a blurring effect was 48.6%. Figure 1 shows a scanning electron microscope image of the obtained spherical composite particles of barium sulfate and silica.

[0050] Example 2 Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was prepared, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (manufactured by Kishida Chemical, 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solids after washing were repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-O, manufactured by Nissan Chemical, average particle size of silica 0.012 μm, acidic sol) was added to the slurry using BaSO₄. 4 and SiO 2 The mixture was added and mixed in a weight ratio of 92:8. To the mixture, magnesium sulfate (anhydrous) (special grade, 98% manufactured by Fujifilm Wako Pure Chemical Industries) was added to 1000 ppm relative to the barium sulfate, and pure water was added to adjust the slurry concentration to 280 g / L and the viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle diameter of 4.3 μm. The particle size distribution D90 / D10 of the obtained particles was 3.7, the sphericity was 1.05, and the MMD (roughness) value measured with a friction tester was 0.0106. In addition, the haze when used as a coating film exhibiting a blurring effect was 37.1%.

[0051] Example 3 Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was prepared, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (Kishida Chemical Co., Ltd., 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solids after washing were repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-O, Nissan Chemical Co., Ltd., average particle size of silica 0.012 μm, acidic sol) was added to the slurry as a BaSO4 solution. 4 and SiO 2 The mixture was added and mixed in a weight ratio of 92:8. To the mixture, magnesium sulfate (anhydrous) (special grade, 98% manufactured by Fujifilm Wako Pure Chemical Industries) was added to 1700 ppm relative to the barium sulfate, and pure water was added to adjust the slurry concentration to 280 g / L and the viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle diameter of 3.5 μm. The particle size distribution D90 / D10 of the obtained particles was 3.7, the sphericity was 1.04, and the MMD (roughness) value measured with a friction tester was 0.0107. In addition, the haze when used as a coating film exhibiting a blurring effect was 43.2%.

[0052] Example 4 Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was prepared, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (manufactured by Kishida Chemical, 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solids after washing were repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-O, manufactured by Nissan Chemical, average particle size of silica 0.012 μm, acidic sol) was added to the slurry as a BaSO₄. 4 and SiO 2 The mixture was added and mixed in a weight ratio of 92:8. To the mixture, magnesium sulfate (anhydrous) (special grade, 98% manufactured by Fujifilm Wako Pure Chemical Industries) was added to 2150 ppm relative to the barium sulfate, and pure water was added to adjust the slurry concentration to 280 g / L and the viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle diameter of 3.6 μm. The particle size distribution D90 / D10 of the obtained particles was 3.8, the sphericity was 1.03, and the MMD (roughness) value measured with a friction tester was 0.0107. In addition, the haze when used as a coating film exhibiting a blurring effect was 43.4%.

[0053] Example 5 Barium sulfide was reacted with sulfuric acid to prepare raw material barium sulfate with an average particle size of 0.05 μm (pigment pH 8.5 when dry), which was then washed with water to form a slurry, and pure water was added to adjust the slurry concentration to 135 g / L. To this raw material barium sulfate slurry, anhydrous sodium sulfate (manufactured by Kishida Chemical, 99%) was added in an amount of 0.8% relative to barium sulfate and dissolved, followed by stirring for 30 minutes, filtration, and water washing until the electrical conductivity was 40 μS / cm or lower. The solid content after water washing was repulped in pure water to prepare a slurry with a concentration of 380 g / L, and silica sol (Snowtex ST-O, manufactured by Nissan Chemical, average silica particle size 0.012 μm, acidic sol) was added to the slurry to react with BaSO 4 and SiO 2 at a weight ratio of 92:8, followed by mixing. To the mixture, anhydrous magnesium sulfate (special grade manufactured by Fujifilm Wako Pure Chemical, 98%) was added in an amount of 5000 ppm relative to barium sulfate, and pure water was added to adjust the slurry concentration to 280 g / L and the slurry viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C with a spray dryer, and the resulting dried product was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle size of 3.9 μm. The D90 / D10 of the particle size distribution of the obtained particles was 3.9, the sphericity was 1.03, and the MMD: value indicating rough texture when measured with a friction tester was 0.0102. In addition, the HAZE of the coating film exhibiting a blurring effect was 40.9%.

[0054] Example 6 Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was prepared, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (manufactured by Kishida Chemical, 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solids after washing were repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-O, manufactured by Nissan Chemical, average particle size of silica 0.012 μm, acidic sol) was added to the slurry using BaSO₄. 4 and SiO 2 The mixture was added and mixed in a weight ratio of 92:8. To the mixture, magnesium sulfate (anhydrous) (special grade, 98% manufactured by Fujifilm Wako Pure Chemical Industries) was added to 6000 ppm relative to the barium sulfate, and pure water was added to adjust the slurry concentration to 280 g / L and the viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle diameter of 4.5 μm. The particle size distribution D90 / D10 of the obtained particles was 3.9, the sphericity was 1.04, and the MMD (roughness) value measured with a friction tester was 0.0102. In addition, the haze when used as a coating film exhibiting a blurring effect was 39.6%.

[0055] Example 7 Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was prepared, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (manufactured by Kishida Chemical, 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solids after washing were repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-O, manufactured by Nissan Chemical, average particle size of silica 0.012 μm, acidic sol) was added to the slurry using BaSO₄. 4 and SiO 2 The mixture was added and mixed in a weight ratio of 88:12. To the mixture, magnesium sulfate (anhydrous) (special grade, 98% manufactured by Fujifilm Wako Pure Chemical Industries) was added to 3000 ppm relative to the barium sulfate, and pure water was added to adjust the slurry concentration to 300 g / L and the viscosity to 700 mPa·s. The viscosity-adjusted slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was calcined at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle diameter of 3.8 μm. The particle size distribution D90 / D10 of the obtained particles was 3.3, the sphericity was 1.04, and the MMD (roughness) value measured with a friction tester was 0.0087. In addition, the haze when used as a coating film exhibiting a blurring effect was 55.9%.

[0056] Comparative Example 1: Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was obtained, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (manufactured by Kishida Chemical, 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solids after washing were repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-30, manufactured by Nissan Chemical, average particle size of silica 0.012 μm, alkaline sol) was added to the slurry as a BaSO4 solution. 4 and SiO 2 The two components were added and mixed in a weight ratio of 92:8. The slurry concentration at this time was 370 g / L, and the viscosity of the slurry was 10 mPa·s. The slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was baked at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle size of 6.2 μm. The particle size distribution D90 / D10 of the obtained particles was 4.9, the sphericity was 1.03, and the MMD (Mass Mass Diode) value, which indicates roughness, measured with a friction tester was 0.0144. Furthermore, the haze when used as a coating film exhibiting a blurring effect was 31.8%.

[0057] Comparative Example 2 Barium sulfate raw material with an average particle size of 0.05 μm (pigment pH 8.5 when dry) was prepared by reacting barium sulfide with sulfuric acid. After washing with water, a slurry was obtained, and the slurry concentration was adjusted to 135 g / L by adding pure water. Sodium sulfate [anhydrous] (manufactured by Kishida Chemical, 99%) was added to the raw material barium sulfate slurry to a concentration of 0.8% relative to the barium sulfate and dissolved. The mixture was stirred for 30 minutes, filtered, and washed with water until the electrical conductivity was 40 μS / cm or less. The solid content after washing was repulped with pure water to prepare a slurry concentration of 380 g / L. Silica sol (Snowtex ST-O, manufactured by Nissan Chemical, average particle size of silica 0.012 μm, acidic sol) was added to the slurry using BaSO₄. 4 and SiO 2The two components were added and mixed in a weight ratio of 92:8. The slurry concentration at this time was 345 g / L, and the viscosity of the slurry was 10 mPa·s. The slurry was spray-dried at 220°C using a spray dryer, and the resulting dried material was baked at 900°C for 2 hours to prepare spherical composite particles mainly composed of barium sulfate with an average particle size of 6.1 μm. The particle size distribution D90 / D10 of the obtained particles was 5.0, the sphericity was 1.04, and the MMD (Mass Mass Diode) value, which indicates roughness, measured with a friction tester was 0.0151. In addition, the haze when used as a coating film exhibiting a blurring effect was 30.9%.

[0058]

[0059] The results for Examples 1 to 7 and Comparative Examples 1 and 2 are shown in Table 1. From the results in Table 1, it was confirmed that the spherical composite particles of barium sulfate and silica obtained by the manufacturing methods of Examples 1 to 7, in which magnesium sulfate was added to the barium sulfate and silica slurry, had superior powder texture (MMD) and haze effect compared to the spherical composite particles of barium sulfate and silica obtained by Comparative Examples 1 and 2, in which magnesium sulfate was not used.

[0060] Example 8 200 g of spherical composite particles of barium sulfate and silica obtained in Example 1 were placed in a mixer, and then 70 g of stearic acid was added as a surface treatment agent, and the mixture was stirred and mixed at 750 rpm. At this time, the temperature of the mixed layer was raised to 100°C, above the melting point of the fatty acid, and after 5 minutes the rotation was stopped to obtain fatty acid-treated spherical particles.

[0061] Comparative Example 3 Fatty acid-treated spherical particles were obtained in the same manner as in Example 8, except that the particles obtained in Comparative Example 1 were used.

[0062] The particles prepared in Example 1, Example 8, Comparative Example 1, and Comparative Example 3 were evaluated as follows. The results are shown in Table 4. <Tactile Evaluation> Powder foundation formulations 1 and 2 described in Table 2 were prepared using the particles prepared in Example 1 and Comparative Example 1, and liquid foundation formulations 3 and 4 described in Table 3 were prepared using the particles prepared in Example 8 and Comparative Example 3. For these formulations, a panel (8 people) applied the molded bodies obtained by hand pressing in rectangular aluminum dish containers to their skin with a puff for powder foundation formulations 1 and 2, and applied the liquid foundation formulations 3 and 4 to their skin with a puff. They then evaluated the feel of use (moisture, non-stickiness, uniform and even) on a 5-point scale from 5 (good) to 1 (bad), and the average score was used for evaluation.

[0063] <Method for preparing powder foundation> Ingredients No. 1 to 10 in Table 2 were uniformly mixed and pressed into shape.

[0064]

[0065] <Method for preparing liquid foundation> (1) Mix components No. 2 to 6 from Table 3 uniformly to obtain mixture A. (2) Mix components No. 13 to 16 from Table 3 uniformly to obtain mixture B. (3) Add mixture B to mixture A and emulsify to obtain emulsion C. (4) Mix components No. 1 and No. 7 to 12 from Table 3 uniformly to obtain mixture D. (5) Add mixture D to emulsion C and mix uniformly.

[0066]

[0067]

[0068] Formula 5 of the W / O sunscreen described in Table 5 was prepared using the powder prepared in Example 8. For comparison, Formula 6 of the W / O sunscreen was also prepared without using the powder prepared in Example 8, and the following evaluations were performed on Formulas 5 and 6. The results are shown in Table 6. <Settling Resistance> The prepared formulas were placed in 50cc screw-cap bottles and left to stand at 40°C for one week. The amount of precipitate was visually checked and evaluated based on the following evaluation criteria. [Evaluation Criteria] ◎: No precipitate observed 〇: A thin layer of precipitate observed at the bottom of the bottle △: Precipitation present, with a certain thickness of precipitate ×: Precipitation present, in a gel-like state <SPF Value Measurement> The obtained formula was measured at 1.3 mg / cm³ on a plate for the SPF analyzer. 3 The material was placed on the plate and coated evenly. The coated plate was then subjected to SPF measurement in the optical wavelength range of 290-400 nm using a Labsphere UV-2000S SPF analyzer.

[0069] <Method for preparing W / O sunscreen> (1) Mix components No. 1 to 7 from Table 5 uniformly to obtain mixture A. (2) Mix components No. 8 to 11 from Table 5 uniformly to obtain mixture B. (3) Add mixture B to mixture A and emulsify to obtain emulsion C. (4) Mix components No. 12 to 13 from Table 5 uniformly to obtain mixture D. (5) Add mixture D to emulsion C and mix uniformly.

[0070] Note 1) DIF-5CS (manufactured by Sakai Chemical Industry Co., Ltd.): Zinc oxide 46.5%, Triethoxycaprylylsilane 3.5%, Cyclopentasiloxane 44%, Polyglyceryl-3 polydimethylsiloxyethyl dimethicone 6% Note 2) DIS-11A (manufactured by Sakai Chemical Industry Co., Ltd.): Titanium dioxide 34%, Hydrated silica 3%, Aluminum hydroxide 1.5%, Hydrogen dimethicone 1.5%, Cyclopentasiloxane 50%, PEG-10 dimethicone 10%

[0071]

[0072] The results in Table 4 confirm that powder foundations and liquid foundations using the spherical composite particles of barium sulfate and silica of the present invention have superior usability compared to comparative examples using spherical composite particles that do not correspond to the spherical composite particles of barium sulfate and silica of the present invention. Furthermore, the results in Table 6 confirm that the W / O sunscreen using the spherical composite particles of barium sulfate and silica of the present invention has a higher SPF value and superior usability compared to the W / O sunscreen that does not use the spherical composite particles of barium sulfate and silica of the present invention. This is presumed to be because, although the spherical particles of the present invention do not absorb ultraviolet rays themselves, they enhance the ultraviolet shielding effect by scattering ultraviolet rays. Substances that do not shield ultraviolet rays on their own but improve the ultraviolet shielding rate of other ultraviolet shielding materials when blended with them are called SPF boosters, and the spherical composite particles of barium sulfate and silica of the present invention have excellent performance in this respect as well.

Claims

1. Spherical composite particles of barium sulfate and silica, characterized in that the haze of the coating film measured by the measurement method described below is 35% or more, and the MMD value measured using a friction tester under the measurement conditions described below is 0.013 or less. [Method for measuring haze] 1.0 g of sample and 0.9 g of silicone oil were mixed using a rotary-orbit mixer at a rotation speed of 2000 rpm for 3 minutes. The mixture was placed on a glass plate, and a coating film was created using a bar coater #14. The haze (%) of the coating film after creation was measured. [MMD Value Measurement] 0.15 g of the sample was placed on the top surface of a 15 mm wide, 50 mm long piece of double-sided tape attached to a glass slide. The top surface of the double-sided tape with the sample was then stroked four times in a consistent direction from one end to the other over a 50 mm length using a cosmetic puff. The MMD (mean deviation of the coefficient of friction) was then measured using a friction tester under the following conditions: friction measurement load of 25 gf, surface measurement sample movement speed of 1 mm / sec, and measurement distance range of 20 mm.

2. The spherical composite particles of barium sulfate and silica according to claim 1, characterized in that the sphericity is 1.10 or less and the particle size distribution D90 / D10 is 4.5 or less.

3. A cosmetic filler characterized by containing spherical composite particles of barium sulfate and silica as described in claim 1 or 2.

4. A cosmetic composition characterized by comprising spherical composite particles of barium sulfate and silica as described in claim 1 or 2.

5. A method for producing spherical composite particles of barium sulfate and silica, the method comprising: a mixing step of preparing a slurry containing barium sulfate, silica, and magnesium sulfate; a drying step of spray-drying the slurry obtained in the mixing step to obtain a dried product; and a calcination step of calcining the dried product obtained in the drying step at 800 to 1100°C.

6. The method for producing spherical composite particles of barium sulfate and silica according to claim 5, characterized in that the mixing step is a step of preparing a slurry by mixing a slurry containing barium sulfate and silica with magnesium sulfate.

7. The method for producing spherical composite particles of barium sulfate and silica according to claim 5, characterized in that the barium sulfate used in the mixing step is obtained by a manufacturing method that includes a washing step of washing barium sulfate with an aqueous sodium sulfate solution or dilute sulfuric acid, wherein the barium sulfate used in the mixing step has a pigment pH of 7.0 to 9.0 as measured by a method in accordance with JIS K 5101 "Pigment pH boiling method" and a primary particle diameter of 0.1 μm or less, and a sulfide removal step of removing sulfides contained in the barium sulfate obtained in the washing step.

8. The method for producing spherical composite particles of barium sulfate and silica according to claim 7, characterized in that the sulfide removal step is carried out by filtering the barium sulfate obtained in the washing step and washing it with water.