Sulfur-modified compound, electrode, and battery
A sulfur-modified compound, formed from a nitrile copolymer and sulfur, addresses the issues of low discharge capacity and poor cycle characteristics in batteries by enhancing capacity retention and cycle performance.
Patent Information
- Application Number
- PCT/JP2026/017746
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-19
AI Technical Summary
Batteries using sulfur-modified compounds exhibit low discharge capacity and poor cycle characteristics due to the reaction product of polyacrylonitrile and sulfur.
A sulfur-modified compound is developed as a reaction product of a nitrile copolymer and sulfur, where the nitrile copolymer contains specific structural units derived from a nitrile monomer and a monomer represented by a given general formula, optimized for increased discharge capacity and improved cycle characteristics.
The sulfur-modified compound enhances discharge capacity and maintains charge/discharge capacity over repeated charging and discharging cycles, improving the overall performance of lithium-ion secondary batteries.
Smart Images

Figure JP2026017746_19112026_PF_FP_ABST
Abstract
Description
Sulfur-modified compounds, electrodes, and batteries
[0001] This disclosure relates to sulfur-modified compounds, electrodes, and batteries.
[0002] Batteries are used in a variety of applications. The characteristics of a battery depend on its constituent components, such as electrodes, separators, and electrolytes, and research and development of each component is actively underway. In electrodes, the active material in the electrode layer is important, along with binders and current collectors, and research and development of this material is also actively being conducted. As an active material, sulfur-modified compounds are known, for example (see, for example, Patent Documents 1 and 2).
[0003] International Publication No. 2010 / 044437, Japanese Patent Publication No. 2014-022123
[0004] When a battery is manufactured using a sulfur-modified compound obtained by reacting polyacrylonitrile and sulfur, as described in Patent Document 1, etc., there is a problem of low discharge capacity and poor cycle characteristics.
[0005] This disclosure has been made in view of the above-mentioned problems, and its main purpose is to provide a sulfur-modified compound that increases discharge capacity and exhibits excellent cycle characteristics. In this disclosure, "cycle characteristics" refers to the characteristic that the charge / discharge capacity of a lithium-ion secondary battery is maintained even after repeated charging and discharging. Therefore, a lithium-ion secondary battery in which the degree of decrease in charge / discharge capacity is large and the capacity retention rate is low with repeated charging and discharging means that it has poor cycle characteristics, and conversely, a lithium-ion secondary battery in which the degree of decrease in charge / discharge capacity is small and the capacity retention rate is high means that it has excellent cycle characteristics.
[0006] As a result of diligent research, the inventors have found that a sulfur-modified compound, which is a reaction product of a nitrile copolymer and sulfur, in which the nitrile copolymer is a copolymer containing structural units derived from a specific monomer, can solve the above problem.
[0007] In other words, the present disclosure is a sulfur-modified compound which is a reaction product of a nitrile copolymer and sulfur, characterized in that the nitrile copolymer is a copolymer containing constituent units derived from a nitrile monomer and constituent units derived from a monomer represented by the following general formula (1).
[0008]
[0009] (In general formula (1), R 1 and R 2 Each of these independently represents a group in which one or more of a hydrogen atom, an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a methylene group in the aliphatic hydrocarbon group is replaced by a divalent group selected from the following group I-1. However, R 1 and R 2 This excludes monomers in which both atoms are hydrogen atoms. In the aliphatic hydrocarbon group having the substituents, one or more hydrogen atoms in the aliphatic hydrocarbon group are replaced by atoms or groups selected from the following group II-1. Group I-1: -O-, -COO-, -OCO-, -CO-, -CO-CO-, -CO-CO-O-, -CS-, -S-, -SO-, -SO2-, -NR'-, -NR'-CO-, -CO-NR'-, -NR'-COO-, -OCO-NR'- or -SiR'R"- Group II-1: Halogen atom, cyano group, nitro group, acrylic group, methacrylic group, -CO-H, -OH, -SH, -NH2, -C(R')=N-OH, -COOH or -SO3H R' and R'' each independently represent a hydrogen atom or an unsubstituted aliphatic hydrocarbon group having 1 to 20 carbon atoms. If there are multiple R' or R'', they may be the same or different.
[0010] In the sulfur-modified compounds of this disclosure, it is preferable that the nitrile monomer is one or more selected from the group consisting of acrylonitrile and methacrylonitrile.
[0011] In the sulfur-modified compound of this disclosure, R in the above general formula (1) 1 However, it is preferable that the alkyl group is either unsubstituted or has a substituent, and contains a hydrogen atom or 1 to 10 carbon atoms.
[0012] In the sulfur-modified compound of the present disclosure, R in the above general formula (1) 2 is preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 10 carbon atoms.
[0013] The present disclosure is an electrode containing the above sulfur-modified compound.
[0014] The present disclosure is a battery having the above electrode.
[0015] In the battery of the present disclosure, the above electrode is preferably a positive electrode.
[0016] In the battery of the present disclosure, the negative electrode of the above battery is preferably lithium.
[0017] According to the present disclosure, it is possible to provide a sulfur-modified compound that has an increased discharge capacity and also has excellent cycle characteristics.
[0018] The sulfur-modified compound, electrode, and battery of the present disclosure will be described in detail.
[0019] A. Sulfur-Modified Compound First, the sulfur-modified compound of the present disclosure will be described. The sulfur-modified compound of the present disclosure is a sulfur-modified compound that is a reaction product of a nitrile-based copolymer and sulfur, wherein the nitrile-based copolymer comprises a structural unit derived from a nitrile-based monomer and a structural unit derived from a monomer represented by the following general formula (1).
[0020]
[0021] (In general formula (1), R 1 and R 2 each independently represent a hydrogen atom, an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a group in which one or more methylene groups in the aliphatic hydrocarbon group are replaced with a divalent group selected from the following group I-1. Provided that R 1 and R 2This excludes monomers in which both atoms are hydrogen atoms. In the aliphatic hydrocarbon group having the substituents, one or more hydrogen atoms in the aliphatic hydrocarbon group are replaced by atoms or groups selected from the following group II-1. Group I-1: -O-, -COO-, -OCO-, -CO-, -CO-CO-, -CO-CO-O-, -CS-, -S-, -SO-, -SO2-, -NR'-, -NR'-CO-, -CO-NR'-, -NR'-COO-, -OCO-NR'- or -SiR'R"- Group II-1: Halogen atom, cyano group, nitro group, acrylic group, methacrylic group, -CO-H, -OH, -SH, -NH2, -C(R')=N-OH, -COOH or -SO3H R' and R'' each independently represent a hydrogen atom or an unsubstituted aliphatic hydrocarbon group having 1 to 20 carbon atoms. If there are multiple R' or R'', they may be the same or different.
[0022] 1. Sulfur In this disclosure, sulfur can be in various forms, such as powdered sulfur, insoluble sulfur, precipitated sulfur, colloidal sulfur, molten sulfur, or rubbery sulfur. Powdered sulfur is preferred for use in this disclosure from the viewpoint of uniform dispersion.
[0023] 2. Nitrile Copolymers The nitrile copolymers used in this disclosure are characterized by being copolymers that include constituent units derived from nitrile monomers and constituent units derived from monomers represented by general formula (1).
[0024] The nitrile copolymer used in this disclosure preferably contains 60 to 99.9% by mass of constituent units derived from nitrile monomers, more preferably 70 to 99.9% by mass, even more preferably 80 to 99.9% by mass, even more preferably 90 to 99.9% by mass, even more preferably 92 to 99.9% by mass, even more preferably 92 to 99.9% by mass, even more preferably 92 to 99.7% by mass, and most preferably 92 to 99.5% by mass, from the viewpoint of increasing discharge capacity and improving cycle characteristics. In this disclosure, the mass percentage of constituent units derived from nitrile monomers is a theoretical value calculated from the amount of nitrile monomers and monomers represented by general formula (1) used in the production of the nitrile copolymer.
[0025] The number-average molecular weight of the nitrile copolymer used in this disclosure is not particularly limited, but is preferably 1,000 to 5,000,000, more preferably 10,000 to 1,000,000, and even more preferably 30,000 to 300,000, from the viewpoint of increasing discharge capacity and improving cycle characteristics. In this disclosure, the number-average molecular weight of the nitrile copolymer can be measured by gel permeation chromatography (GPC).
[0026] (1) Nitrile Monomers The nitrile monomers used in this disclosure are ethylenically unsaturated monomers containing a nitrile group. The nitrile monomers are not particularly limited as long as they are ethylenically unsaturated monomers containing a nitrile group, but examples include acrylonitrile, methacrylonitrile, fumaronitrile, α-chloroacrylonitrile, and α-cyanoethylacrylonitrile. These nitrile monomers may be used individually or in combination of two or more.
[0027] In this disclosure, the nitrile monomer is preferably one or more selected from the group consisting of acrylonitrile and methacrylonitrile, and more preferably acrylonitrile, from the viewpoint of increasing discharge capacity and improving cycle characteristics.
[0028] (2) Monomers represented by general formula (1) The monomers represented by general formula (1) used in this disclosure may be used individually or in combination of two or more types. In general formula (1), R 1 and R 2 Each of these independently represents a group in which one or more of a hydrogen atom, an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a methylene group in the aliphatic hydrocarbon group is replaced by a divalent group selected from the following group I-1. However, R 1 and R 2This excludes monomers in which both atoms are hydrogen atoms. In the aliphatic hydrocarbon group having the substituents, one or more hydrogen atoms in the aliphatic hydrocarbon group are replaced by atoms or groups selected from the following group II-1. Group I-1: -O-, -COO-, -OCO-, -CO-, -CO-CO-, -CO-CO-O-, -CS-, -S-, -SO-, -SO2-, -NR'-, -NR'-CO-, -CO-NR'-, -NR'-COO-, -OCO-NR'- or -SiR'R"- Group II-1: Halogen atom, cyano group, nitro group, acrylic group, methacrylic group, -CO-H, -OH, -SH, -NH2, -C(R')=N-OH, -COOH or -SO3H R' and R'' each independently represent a hydrogen atom or an unsubstituted aliphatic hydrocarbon group having 1 to 20 carbon atoms, and if there are multiple R' or R'', they may be the same or different.
[0029] Halogen atoms in group II-1 (hereinafter referred to as "R") 1 These are also called "halogen atoms used in applications such as [mention specific applications]." Examples include fluorine, chlorine, bromine, and iodine atoms.
[0030] R in general formula (1) 1 and R 2 Aliphatic hydrocarbon group having 1 to 20 carbon atoms, either unsubstituted or substituted (hereinafter referred to as "R") 1 The aliphatic hydrocarbon group used in the above (also called the "aliphatic hydrocarbon group") does not need to contain an aromatic hydrocarbon ring or heterocycle. Examples include alkyl groups having 1 to 20 carbon atoms, alkenyl groups having 2 to 20 carbon atoms, cycloalkyl groups having 3 to 20 carbon atoms, cycloalkylalkyl groups having 4 to 20 carbon atoms, and groups in which one or more hydrogen atoms of these groups are substituted with substituents described later.
[0031] Examples of alkyl groups having 1 to 20 carbon atoms include methyl group, ethyl group, propyl group, iso-propyl group, butyl group, sec-butyl group, tert-butyl group, iso-butyl group, amyl group, iso-pentyl group, tert-pentyl group, cyclopentyl group, hexyl group, 2-hexyl group, 3-hexyl group, cyclohexyl group, 4-methylcyclohexyl group, heptyl group, 2-heptyl group, 3-heptyl group, iso-heptyl group, tert-heptyl group, 1-octyl group, iso-octyl group, tert-octyl group, and the like.
[0032] Examples of alkenyl groups having 2 to 20 carbon atoms include vinyl group, ethylene group, 2-propenyl group, 3-butenyl group, 2-butenyl group, 4-pentenyl group, 3-pentenyl group, 2-hexenyl group, 3-hexenyl group, 5-hexenyl group, 2-heptenyl group, 3-heptenyl group, 4-heptenyl group, 3-octenyl group, 3-nonenyl group, 4-decenyl group, 3-undecenyl group, 4-dodecenyl group, 4,8,12-tetradecatrienylenylallyl group, and cyclopentadinyl group.
[0033] The above-mentioned cycloalkyl group having 3 to 20 carbon atoms means a saturated monocyclic or saturated polycyclic alkyl group having 3 to 20 carbon atoms. Examples of the above-mentioned cycloalkyl group having 3 to 20 carbon atoms include cyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, cyclooctyl group, cyclononyl group, cyclodecyl group, adamantyl group, decahydronaphthyl group, octahydropentalene group, bicyclo[1.1.1]pentanyl group, and the like.
[0034] The above-mentioned cycloalkylalkyl group having 4 to 20 carbon atoms refers to a group having 4 to 20 carbon atoms in which some of the hydrogen atoms of the alkyl group are replaced by a cycloalkyl group. Examples of the above-mentioned cycloalkylalkyl group having 4 to 20 carbon atoms include cyclopropylmethyl group, 2-cyclobutylethyl group, 3-cyclopentylpropyl group, 4-cyclohexylbutyl group, cycloheptylmethyl group, cyclooctylmethyl group, 2-cyclononylethyl group, 2-cyclodecylethyl group, 3-3-adamantylpropyl group, decahydronaphthylpropyl group, and the like.
[0035] In this disclosure, the number of carbon atoms in a group in which a methylene group in a group with a predetermined number of carbon atoms is substituted with a divalent group shall be the same as the number of carbon atoms in the group before substitution. For example, in this disclosure, the number of carbon atoms in a group in which a methylene group in an alkyl group having 1 to 20 carbon atoms is substituted with a divalent group shall be 1 to 20.
[0036] In general formula (1), R 1 From the viewpoint of increasing discharge capacity and improving cycle characteristics, it is preferable that the group is one in which one or more of the hydrogen atom, an unsubstituted or substituted alkyl group having 1 to 20 carbon atoms, or a methylene group in the alkyl group is replaced with a divalent group selected from the above group I-1; more preferably, the group is one in which one or more of the hydrogen atom, an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, or a methylene group in the alkyl group is replaced with a divalent group selected from the above group I-1; even more preferably, the group is one in which the hydrogen atom or an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms, or an alkyl group having -COOH as a substituent, even more preferably, the group is one in which the hydrogen atom or an unsubstituted or substituted alkyl group having -COOH as a substituent, and most preferably, the group is one in which the hydrogen atom or an unsubstituted or substituted alkyl group having -COOH as a substituent.
[0037] In general formula (1), R 2From the viewpoint of increasing discharge capacity and improving cycle characteristics, it is preferable that the group is one in which one or more of the hydrogen atom, an unsubstituted alkyl group having 1 to 20 carbon atoms, or a methylene group in the alkyl group is replaced with a divalent group selected from group I-1 above, more preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 10 carbon atoms, even more preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 5 carbon atoms, and most preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 3 carbon atoms.
[0038] (3) Method for producing nitrile copolymers The method for producing nitrile copolymers used in this disclosure is not particularly limited, but any known method may be used, for example, bulk polymerization, suspension polymerization, emulsion polymerization, solution polymerization, etc.
[0039] Polymerization initiators used in the production of nitrile copolymers include azo polymerization initiators (2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), etc.), organic peroxide polymerization initiators (benzoyl peroxide, lauroyl peroxide, tert-butylperoxy-2-ethylhexanoate, etc.), persulfates (potassium persulfate, ammonium persulfate, etc.), and redox initiators combining persulfates and reducing agents (for example, combinations of persulfate and sodium bisulfite, combinations of persulfate and sodium ascorbate). A single polymerization initiator may be used alone, or two or more may be used in combination. The amount of polymerization initiator used is not particularly limited, but it is preferably 0.1 to 20 parts by mass, and more preferably 0.3 to 15 parts by mass, per 100 parts by mass of the total monomers used in the production of the nitrile copolymer.
[0040] In the production of nitrile copolymers, chain transfer agents can be used for purposes such as molecular weight adjustment. Examples of chain transfer agents include mercaptans (octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, n-hexadecyl mercaptan, n-tetradecyl mercaptan, tert-tetradecyl mercaptan, etc.), acrolein, methacrolein, allyl alcohol, terpinolene, and α-methylstyrene dimers. One type of chain transfer agent may be used alone, or two or more types may be used in combination. The chain transfer agents may be added all at once, or continuously or intermittently. The amount of chain transfer agent used is not particularly limited, but it is preferably 0.1 to 20 parts by mass, and more preferably 0.3 to 15 parts by mass, per 100 parts by mass of the total monomers used in the production of the nitrile copolymer.
[0041] In the production of nitrile copolymers, solvents may be used. Commonly used solvents in radical polymerization reactions can be used. Examples of solvents include: aromatic hydrocarbons such as benzene and toluene; ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate; ethers such as dioxane and tetrahydrofuran (THF); amides such as N,N-dimethylformamide (DMF); sulfur-containing compounds such as dimethyl sulfoxide (DMSO); alcohols such as methanol, ethanol, isopropanol, and n-butanol; halogen-containing compounds such as chloroform, carbon tetrachloride, and trifluoromethylbenzene; cellosolves such as ethyl cellosolve, butyl cellosolve, and 1-methoxy-2-propanol; and water. These solvents may be used individually or in combination of two or more.
[0042] 3. Method for Producing Sulfur-Modified Compounds The method for producing sulfur-modified compounds is not particularly limited as long as a reaction product between a nitrile copolymer and sulfur is obtained, but one method is to heat the nitrile copolymer and sulfur. The nitrile copolymer and sulfur may be heated directly, but from the viewpoint of ensuring uniform sulfur modification, the nitrile copolymer and sulfur may be mixed beforehand before the heat treatment.
[0043] The amount of sulfur used when producing the sulfur-modified compound is preferably 100 to 1500 parts by mass, more preferably 150 to 1000 parts by mass, and even more preferably 150 to 500 parts by mass, per 100 parts by mass of the nitrile copolymer. The particle size of the sulfur is not particularly limited, but if the sulfur particle size is too small, the sulfur modification will be insufficient, and if the sulfur particle size is too large, the sulfur modification may take a long time. Therefore, the average particle size of the sulfur is preferably 1 μm to 1000 μm, and more preferably 1 μm to 500 μm.
[0044] In this disclosure, "average particle diameter" refers to the 50% particle diameter measured by laser diffraction scattering. In laser diffraction scattering, the particle diameter is the volume-based diameter, and the secondary particle diameter of the object being measured is measured. When measuring the average particle diameter by laser diffraction scattering, the object being measured is dispersed in a dispersion medium such as water before measurement.
[0045] The heat treatment temperature for heating the nitrile copolymer and sulfur is preferably 150°C to 550°C, and more preferably 150°C to 450°C. The heat treatment is preferably carried out while mixing the nitrile copolymer and sulfur to ensure uniform sulfur modification. The heat treatment time is not particularly limited, but is preferably 0.1 hours to 30 hours. Furthermore, from the viewpoint of the melting point of sulfur, the heat treatment of the nitrile copolymer and sulfur may be carried out in multiple stages at different temperatures. Specifically, the nitrile copolymer and sulfur may be heat-treated at 120°C to 170°C for 0.1 hours to 24 hours, followed by heat treatment at 200°C to 450°C for 0.1 hours to 12 hours.
[0046] The heat treatment of nitrile copolymers with sulfur is carried out in a non-oxidizing atmosphere. A non-oxidizing atmosphere is an atmosphere with an oxygen concentration of 5% by volume or less, preferably 2% by volume or less, and more preferably an atmosphere that is substantially free of oxygen. Examples of non-oxidizing atmospheres include inert gas atmospheres such as nitrogen, helium, and argon, and sulfur gas atmospheres.
[0047] It is preferable to discharge the hydrogen sulfide generated by the heat treatment outside the heating container. To discharge the hydrogen sulfide, an inert gas may be introduced into the heating container, and the hydrogen sulfide may be discharged together with the inert gas. If sulfur vapor is discharged along with the hydrogen sulfide, the reaction ratio between the nitrile copolymer and sulfur will change, so it is preferable to reflux the discharged sulfur into the heating container or add the amount of sulfur that has been discharged to the heating container.
[0048] The sulfur-modified compound obtained by heat treatment may be pulverized as needed. A known pulverizer can be used to pulverize the sulfur-modified compound. Examples of known pulverizers include media-agitating mills such as sand mills, attritors, and bead mills; container-driven mills using balls or rods as a medium, such as rotary mills, vibratory mills, and planetary mills; and jet mills, roll mills, hammer mills, pin mills, and cyclone mills.
[0049] B. Electrodes The electrodes in this disclosure have an electrode layer containing the sulfur-modified compound described in section A. Sulfur-modified compounds above.
[0050] According to this disclosure, using the above electrodes in a battery can increase the discharge capacity and improve the cycle characteristics.
[0051] 1. Electrode Layer In this disclosure, the term "electrode layer" refers to a layer containing the above-mentioned sulfur-modified compound. In this disclosure, the electrode layer when the electrode is the positive electrode may be referred to as the "positive electrode active material layer," and the electrode layer when the electrode is the negative electrode may be referred to as the "negative electrode active material layer." The thickness of the electrode layer can typically be 1 μm to 1000 μm.
[0052] In this disclosure, from the viewpoint of effectively functioning as an active material and increasing discharge capacity, the content of the sulfur-modified compound is preferably 75 to 99.5 parts by mass, more preferably 80 to 99 parts by mass, and even more preferably 85 to 98 parts by mass in 100 parts by mass of the electrode layer.
[0053] The electrode layer described above contains a sulfur-modified compound, but may contain other components as needed. When the electrode layer is used as a positive electrode active material layer or a negative electrode active material layer, other components include binders and conductive additives, and may also contain active materials other than sulfur-modified compounds, viscosity modifiers, reinforcing materials, antioxidants, etc., as needed.
[0054] As the binder mentioned above, known binders for electrode layers can be used. Examples of binders include styrene-butadiene rubber, butadiene rubber, polyethylene, polypropylene, polyamide, polyamide-imide, polyimide, polyacrylonitrile, polyurethane, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-propylene-diene rubber, fluororubber, styrene-acrylic acid ester copolymer, ethylene-vinyl alcohol copolymer, acrylonitrile butadiene rubber, styrene-isoprene rubber, polymethyl methacrylate, polyacrylate, polyvinyl alcohol, polyvinyl ether, carboxymethylcellulose, sodium carboxymethylcellulose, methylcellulose, cellulose nanofiber, polyethylene oxide, starch, polyvinylpyrrolidone, polyvinyl chloride, and polyacrylic acid. Only one binder may be used, or two or more may be used in combination. Among these, water-based binders are preferred from the viewpoint of low environmental impact and excellent binding properties, and styrene-butadiene rubber, sodium carboxymethylcellulose, and polyacrylic acid are more preferred.
[0055] From the viewpoint of further increasing the discharge capacity, the binder content in the electrode layer is preferably 0.1 to 30 parts by mass, and more preferably 1 to 20 parts by mass, per 100 parts by mass of the sulfur-modified compound in the electrode layer.
[0056] As the conductive additive mentioned above, those known as conductive additives for electrode layers can be used. Examples of conductive additives include carbon materials such as natural graphite, artificial graphite, carbon black, Ketjen black, acetylene black, channel black, furnace black, lamp black, thermal black, carbon nanotubes, vapor-grown carbon fiber (VGCF), graphene, fullerene, and needle coke; metal powders such as aluminum powder, nickel powder, and titanium powder; conductive metal oxides such as zinc oxide and titanium oxide; and sulfides such as La2S3, Sm2S3, Ce2S3, and TiS2. One conductive additive may be used, or two or more may be used in combination.
[0057] From the viewpoint of increasing discharge capacity, the average particle size of the conductive additive is preferably 0.01 μm to 100 μm, and more preferably 0.01 μm to 50 μm.
[0058] From the viewpoint of increasing discharge capacity, the content of the conductive additive in the electrode layer is preferably 0.1 to 50 parts by mass, more preferably 0.5 to 20 parts by mass, more preferably 1.0 to 10 parts by mass, and most preferably 2.0 to 8.0 parts by mass, per 100 parts by mass of the sulfur-modified compound in the electrode layer.
[0059] Other active materials besides the sulfur-modified compounds mentioned above (hereinafter sometimes referred to as "other active materials") include materials known as active materials, such as the positive electrode active material and negative electrode active material described in "C. Battery" below.
[0060] As the viscosity modifier mentioned above, known viscosity modifiers for electrode layers can be used. Examples of viscosity modifiers include cellulosic polymers such as carboxymethylcellulose, methylcellulose, and hydroxypropylcellulose, and their ammonium salts and alkali metal salts; (modified) poly(meth)acrylic acid and its ammonium salts and alkali metal salts; (modified) polyvinyl alcohol, copolymers of acrylic acid or acrylate with vinyl alcohol, and polyvinyl alcohols such as maleic anhydride or copolymers of maleic acid or fumaric acid with vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, modified polyacrylic acid, starch oxide, starch phosphate, casein, various modified starches, cellulose nanofibers, and acrylonitrile-butadiene copolymer hydrogenates. These may also be used as dispersants.
[0061] As the reinforcing material mentioned above, any known reinforcing material for electrode layers can be used. Examples of reinforcing materials include various inorganic and organic spherical, plate-shaped, rod-shaped, or fibrous fillers.
[0062] As the antioxidant mentioned above, those known as antioxidants for electrode layers can be used. Examples of antioxidants include phenol compounds, hydroquinone compounds, organophosphorus compounds, sulfur compounds, phenylenediamine compounds, polymer-type phenol compounds, and the like.
[0063] The method for forming the electrode layer described above can be any method capable of forming the electrode layer, and examples include a method in which an electrode layer forming composition containing the sulfur-modified compound, other components as needed, and a solvent is applied, and then the solvent is dried off from the coating film.
[0064] Examples of solvents used in electrode layer forming compositions include propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, 1,2-dimethoxyethane, 1,2-diethoxyethane, acetonitrile, propionitrile, tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, 1,3-dioxolane, nitromethane, N-methylpyrrolidone, N,N-dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethyltriamine, N,N-dimethylaminopropylamine, polyethylene oxide, tetrahydrofuran, dimethyl sulfoxide, sulfolane, γ-butyrolactone, water, and alcohol. The amount of solvent used can be adjusted according to the application method. For example, in the doctor blade method, the amount of solvent used is preferably 20 to 300 parts by mass, and more preferably 30 to 200 parts by mass, per 100 parts by mass of the total amount of sulfur-modified compound, binder, and conductive additive, from the viewpoint of ease of manufacture.
[0065] The method for preparing the electrode layer forming composition is not particularly limited, but examples include using a conventional ball mill, sand mill, bead mill, pigment disperser, lye crusher, ultrasonic disperser, homogenizer, rotation / revolution mixer, planetary mixer, film mixer, disperser, jet pasteor, etc.
[0066] The coating method is not particularly limited, but various methods such as die coating, comma coating, curtain coating, spray coating, gravure coating, flexo coating, knife coating, doctor blade coating, reverse roll coating, brush coating, and dipping can be used. From the viewpoint of obtaining a good surface condition of the coating film in accordance with the physical properties such as viscosity and drying properties of the electrode layer forming composition, die coating, doctor blade coating, knife coating, and comma coating are preferred.
[0067] The drying and removal method is not particularly limited, but heating, reduced pressure, and combinations thereof can be used. The heating temperature can be between 40°C and 200°C. As the heating and reduced pressure equipment, heating furnaces, infrared heating furnaces, vacuum ovens, etc., can be used.
[0068] This drying process causes volatile components such as solvents to evaporate, forming an electrode layer. After this, the electrode layer may be pressed if necessary. Examples of pressing methods include die pressing and roll pressing.
[0069] 2. Other Configurations The electrode of this disclosure has the above-described electrode layer, but may have other configurations as needed. Other configurations include a current collector.
[0070] The current collectors used may include conductive materials such as titanium, titanium alloys, aluminum, aluminum alloys, copper, nickel, stainless steel, nickel-plated steel, and conductive resins. These conductive materials may have a carbon coating on their surface. The shape of the current collector may include foil, plate, mesh, or porous. Among these, aluminum is preferred from the viewpoint of conductivity and cost, and aluminum foil is more preferred. When the current collector is foil-shaped, its thickness can usually be 1 μm to 100 μm.
[0071] The applications of the electrodes of this disclosure are not particularly limited, but batteries are one example. Examples of batteries include primary batteries and secondary batteries. Examples of secondary batteries include lithium-ion secondary batteries, sodium-ion secondary batteries, potassium-ion secondary batteries, magnesium-ion secondary batteries, calcium-ion secondary batteries, and aluminum-ion secondary batteries. That is, lithium-sulfur secondary batteries, sodium-sulfur secondary batteries, potassium-sulfur secondary batteries, magnesium-sulfur secondary batteries, calcium-sulfur secondary batteries, and aluminum-sulfur secondary batteries are also possible.
[0072] From a practical standpoint, the electrodes of this disclosure are preferably used as electrodes for secondary batteries, and more preferably as electrodes for lithium-ion secondary batteries. The electrodes of this disclosure can be used as either positive or negative electrodes, but from the viewpoint of increasing discharge capacity and being easier to manufacture, they are preferably used as positive electrodes.
[0073] Furthermore, when the above electrodes are used as electrodes for a lithium-ion secondary battery, a pre-doping process involving the insertion of lithium may be performed beforehand. The lithium pre-doping method can follow any known method, such as the electrolytic doping method, which involves assembling a half-cell using metallic lithium as the counter electrode and electrochemically doping it with lithium, or the diffusion doping method, which involves attaching metallic lithium foil to the electrode and leaving it in a liquid electrolyte, utilizing the diffusion of lithium into the electrode.
[0074] Furthermore, when the above electrodes are used as electrodes for a sodium-ion secondary battery, a pre-doping treatment involving the insertion of sodium may be performed beforehand. Any known method can be used for sodium pre-doping; for example, the doping method described above can be used.
[0075] In this disclosure, the electrodes may be pressed as necessary. Examples of pressing methods include die pressing and roll pressing.
[0076] C. Battery 1. Electrodes The battery of this disclosure has electrodes as described in section B. Electrodes above, but may have other configurations as necessary.
[0077] The battery described herein can increase discharge capacity and improve cycle characteristics.
[0078] 2. Other Components Other components include a counter electrode used in conjunction with the above-mentioned electrode, an electrolyte, a separator, etc.
[0079] (1) Counter Electrode The counter electrode is an electrode used in conjunction with the electrode mentioned above. When the electrode is the positive electrode, the counter electrode is the negative electrode. When the electrode is the negative electrode, the counter electrode is the positive electrode. The positive and negative electrodes used as counter electrodes for the electrode mentioned above will be explained separately below.
[0080] (1-1) Negative electrode As the negative electrode used as the counter electrode, one having a negative electrode active material layer can be used. As the negative electrode active material layer, one containing at least a known active material (hereinafter sometimes referred to as "negative electrode active material") can be used.
[0081] In the case of lithium-ion secondary batteries, examples of negative electrode active materials include natural graphite, artificial graphite, non-graphitizable carbon, easily graphitizable carbon, lithium, lithium alloys, silicon, silicon alloys, silicon oxide, silicon carbide, tin, tin alloys, tin oxide, phosphorus, germanium, indium, copper oxide, antimony sulfide, titanium oxide, iron oxide, manganese oxide, cobalt oxide, nickel oxide, lead oxide, ruthenium oxide, tungsten oxide, zinc oxide, as well as LiVO2, Li2VO4, Li4Ti5O 12 Examples of composite oxides include the following. The negative electrode active material may be a single type or a combination of two or more types.
[0082] In the case of sodium-ion secondary batteries, among the negative electrode active materials used in lithium-ion secondary batteries as described above, negative electrode active materials that do not contain lithium atoms, and negative electrode active materials in which lithium atoms are replaced with sodium atoms can be used. Furthermore, if the negative electrode active material is lithium or a lithium alloy, or sodium or a sodium alloy, the electrode itself may be used without using a current collector. In addition, potassium, magnesium, calcium, aluminum, zinc, etc. can be used as other negative electrode active materials.
[0083] The above-mentioned negative electrode active material layer contains the above-mentioned negative electrode active material, but may also contain, if necessary, a binder, a conductive additive, etc. The binder and conductive additive used in the above-mentioned negative electrode active material layer can be the same as those described in section "B. Electrodes," so a detailed explanation is omitted here.
[0084] (1-2) Positive electrode As the positive electrode used as the counter electrode, one having a positive electrode active material layer can be used. The positive electrode active material layer can contain at least a known active material (hereinafter sometimes referred to as "positive electrode active material"). Examples of the positive electrode active material include lithium transition metal composite oxides, lithium-containing transition metal phosphate compounds, lithium-containing silicate compounds, etc. Only one type of positive electrode active material may be used, or two or more types may be used in combination.
[0085] Examples of transition metals in the above-mentioned lithium transition metal composite oxides include vanadium, titanium, chromium, manganese, iron, cobalt, nickel, and copper. Specific examples of lithium transition metal composite oxides include lithium cobalt composite oxides such as LiCoO2, lithium nickel composite oxides such as LiNiO2, lithium manganese composite oxides such as LiMnO2, LiMn2O4, and Li2MnO3, and those in which some of the main transition metal atoms are replaced with other metals such as aluminum, titanium, vanadium, chromium, manganese, iron, cobalt, lithium, nickel, copper, zinc, magnesium, gallium, and zirconium. Specific examples of lithium transition metal composite oxides in which some of the main transition metal atoms are replaced with other metals include, for example, Li 1.1 Mn 1.8 Mg 0.1 O4, Li 1.1 Mn 1.85 Al 0.05 O4, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.5 Mn 0.5 O2, LiNi 0.80 Co 0.17 Al 0.03 O2, LiNi 0.80 Co 0.15 Al 0.05 O2, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 ) O2, LiNi 0.6 Co0.2 Mn 0.2 O2, LiMn 1.8 Al 0.2 O4, LiNi 0.5 Mn 1.5 Examples include O4, Li2MnO3-LiMO2 (M = Co, Ni, or Mn).
[0086] Examples of transition metals in the lithium-containing transition metal phosphate compounds mentioned above include vanadium, titanium, manganese, iron, cobalt, and nickel. Specific examples of lithium-containing transition metal phosphate compounds include LiFePO4 and LiMn. x Fe 1-x Examples include iron phosphate compounds such as PO4 (0 < x < 1), iron sulfate compounds such as LiFeSO4F, cobalt phosphate compounds such as LiCoPO4, and those in which some of the transition metal atoms that make up these lithium transition metal phosphate compounds are replaced with other metals such as aluminum, titanium, vanadium, chromium, manganese, iron, cobalt, lithium, nickel, copper, zinc, magnesium, gallium, zirconium, and niobium, as well as vanadium phosphate compounds such as Li3V2(PO4)3.
[0087] Examples of the lithium-containing silicate compounds mentioned above include Li2FeSiO4.
[0088] The positive electrode active material layer described above contains the known active material described above, but may also contain, if necessary, a binder, a conductive additive, etc. The binder and conductive additive used in the positive electrode active material layer can be the same as those described in section B. Electrodes, so a detailed explanation is omitted here.
[0089] (2) Electrolyte The electrolyte is not particularly limited, but known electrolytes can be used. Examples of electrolytes include liquid electrolytes obtained by dissolving a support electrolyte in an organic solvent, polymer gel electrolytes obtained by dissolving a support electrolyte in an organic solvent and gelling it with a polymer, polymer electrolytes that do not contain an organic solvent and in which the support electrolyte is dispersed in a polymer, inorganic solid electrolytes, and so on. Two or more of the above electrolytes may also be used in combination. In this disclosure, from the viewpoint of increasing the discharge capacity and being easy to manufacture, the electrolyte is preferably a liquid electrolyte, a polymer electrolyte, or an inorganic solid electrolyte, and more preferably a liquid electrolyte.
[0090] In this disclosure, conventionally known lithium salts are used as the supporting electrolyte for liquid electrolytes and polymer gel electrolytes in lithium-ion secondary batteries. Examples of supporting electrolytes include LiPF6, LiBF4, LiAsF6, LiCF3SO3, LiCF3CO2, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, LiC(CF3SO2)3, LiB(CF3SO3)4, LiB(C2O4)2, LiBF2(C2O4), LiSbF6, LiSiF5, LiSCN, LiClO4, LiCl, LiF, LiBr, LiI, LiAlF4, LiAlCl4, LiPO2F2, and their derivatives. Among these, from the viewpoint of further increasing the discharge capacity, it is preferable to use one or more selected from the group consisting of LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, and LiC(CF3SO2)3, derivatives of LiCF3SO3, and derivatives of LiC(CF3SO2)3.
[0091] From the viewpoint of further increasing the discharge capacity, the content of the supporting electrolyte in the liquid electrolyte or polymer gel electrolyte is preferably 0.5 mol / L to 7 mol / L, and more preferably 0.8 mol / L to 1.8 mol / L.
[0092] Examples of supporting electrolytes used in polymer electrolytes include LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, LiC(CF3SO2)3, LiB(CF3SO3)4, and LiB(C2O4)2 in lithium-ion secondary batteries.
[0093] In this disclosure, the inorganic solid electrolyte is, in the case of a lithium-ion secondary battery, for example, Li 1+x A x B 2-x Phosphate-based materials such as (PO4)3 (A = Al, Ge, Sn, Hf, Zr, Sc or Y, B = Ti, Ge or Zn, 0 < x < 0.5), LiMPO4 (M = Mn, Fe, Co or Ni), Li3PO4; Li3XO4 (X = As or V), Li 3+x A x B 1-x O4 (A = Si, Ge or Ti, B = P, As or V, 0 < x < 0.6), Li 4+x A x Si 1-x O4 (If A = B, Al, Ga, Cr, or Fe, then 0 < x < 0.4; if A = Ni or Co, then 0 < x < 0.1), Li 4-3y Al y SiO4 (0<y<0.06), Li 4-2y Zn y GeO4 (0 < y < 0.25), LiAlO2, Li2BO4, Li4XO4 (X = Si, Ge or Ti), Lithium titanate (LiTiO2, LiTi2O4, Li4TiO4, Li2TiO3, Li2Ti3O7, Li4Ti5O 12 Lithium composite oxides such as ); Lithium and halogen compounds such as LiBr, LiF, LiCl, LiPF6, LiBF4; Lithium and nitrogen compounds such as LiPON, LiN(SO2CF3)2, LiN(SO2C2F5)2, Li3N, LiN(SO2C3F7)2; La 0.55 Li 0.35 Crystals having a perovskite structure with lithium ion conductivity, such as TiO3; Li7-La3Zr2O 13 Crystals having a garnet-type structure such as: 50Li4SiO4·50Li3BO 33, 90Li₃BO₃·10Li₂SO₄ and other glasses; 70Li₂S·30P₂S₅, 75Li₂S·25P₂S₅, Li₆PS₅Cl, Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li₆PS₅P 1.44 C l3 , Li 10 GeP₂S 12 , Li 3.25 Ge 0.25 P 0.75 S₄ and other lithium-phosphorus sulfide based crystals; 30Li₂S·26B₂S₃·44LiI, 50Li₂S·17P₂S₅·33LiBH, 50Li₂S·50GeS₂, 63Li₂S·36SiS₂·1Li₃PO₄, 57Li₂S·38SiS₂·5Li₄SiO₄, 70Li₂S·50GeS₂ and other lithium-phosphorus sulfide based glasses; Li₇P₃S 11 , Li 3.25 P 0.95 S₄, Li 10 GeP₂S 12 , Li 9.6 P₃S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 and other glass ceramics, and the like. The inorganic solid electrolyte may be coated with a polymer gel electrolyte. When an inorganic solid electrolyte is used, a layer of polymer gel electrolyte may be provided between the inorganic solid electrolyte layer and the electrode.
[0094] In the case of a sodium ion secondary battery, a supporting electrolyte obtained by replacing the lithium atoms in the aforementioned lithium ion secondary battery with sodium atoms may be used.
[0095] In this disclosure, organic solvents commonly used for liquid electrolytes can be used for liquid electrolytes and polymer gel electrolytes. Specific examples of organic solvents include saturated cyclic carbonate compounds, saturated cyclic ester compounds, sulfoxide compounds, sulfone compounds, amide compounds, saturated linear carbonate compounds, linear ether compounds, cyclic ether compounds, and saturated linear ester compounds. Among these, saturated cyclic carbonate compounds, saturated cyclic ester compounds, sulfoxide compounds, sulfone compounds, and amide compounds are preferred, with saturated cyclic carbonate compounds being more preferred, from the viewpoint of having a high dielectric constant that increases the dielectric constant of the electrolyte and further increases the discharge capacity. Furthermore, among these, saturated linear carbonate compounds, linear ether compounds, cyclic ether compounds, and saturated linear ester compounds are preferred, with saturated linear carbonate compounds being more preferred, from the viewpoint of being able to lower the viscosity of the electrolyte and improve the mobility of electrolyte ions, thereby improving battery characteristics such as power density.
[0096] Examples of the saturated cyclic carbonate compounds mentioned above include ethylene carbonate, fluoroethylene carbonate, 1,2-propylene carbonate, 1,3-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, and 1,1-dimethylethylene carbonate.
[0097] Examples of the saturated cyclic ester compounds mentioned above include γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-hexanolactone, and δ-octanolactone.
[0098] Examples of the above sulfoxide compounds include dimethyl sulfoxide, diethyl sulfoxide, dipropyl sulfoxide, diphenyl sulfoxide, and thiophene.
[0099] Examples of the above sulfone compounds include dimethyl sulfone, diethyl sulfone, dipropyl sulfone, diphenyl sulfone, sulfolane (also called tetramethylene sulfone), 3-methylsulfolane, 3,4-dimethylsulfolane, 3,4-diphenylmethylsulfolane, sulfolene, 3-methylsulfolene, 3-ethylsulfolene, 3-bromomethylsulfolene, and tetramethylsulfolane.
[0100] Examples of the above-mentioned amide compounds include N-methylpyrrolidone, dimethylformamide, and dimethylacetamide.
[0101] Examples of the saturated chain carbonate compounds mentioned above include dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl butyl carbonate, methyl-t-butyl carbonate, diisopropyl carbonate, and t-butylpropyl carbonate.
[0102] Examples of the above-mentioned chain-like ether compounds and cyclic ether compounds include dimethoxyethane, ethoxymethoxyethane, diethoxyethane, tetrahydrofuran, dioxolane, dioxane, 1,2-bis(methoxycarbonyloxy)ethane, 1,2-bis(ethoxycarbonyloxy)ethane, 1,2-bis(ethoxycarbonyloxy)propane, ethylene glycol bis(trifluoroethyl) ether, propylene glycol bis(trifluoroethyl) ether, ethylene glycol bis(trifluoromethyl) ether, diethylene glycol bis(trifluoroethyl) ether, and glymes.
[0103] Examples of the saturated chain ester compounds mentioned above include monoester compounds and diester compounds having a total of 2 to 8 carbon atoms in the molecule. Specific examples of saturated chain ester compounds include methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, isobutyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylacetate, ethyl trimethylacetate, methyl malonate, ethyl malonate, methyl succinate, ethyl succinate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethylene glycol diacetyl, and propylene glycol diacetyl.
[0104] Other organic solvents that can be used in the preparation of electrolytes include, for example, acetonitrile, propionitrile, nitromethane and their derivatives, and various ionic liquids.
[0105] Examples of polymers used in polymer gel electrolytes include polyethylene oxide, polypropylene oxide, polyvinyl chloride, polyacrylonitrile, polymethyl methacrylate, polyethylene, polyvinylidene fluoride, and polyhexafluoropropylene. There are no particular restrictions on the blending ratio of polymers in the polymer gel electrolyte or the gelation method; known blending ratios and known gelation methods in this art can be adopted.
[0106] Examples of polymers used in polymer electrolytes include polyethylene oxide, polypropylene oxide, polystyrene sulfonic acid, and polyvinylidene fluoride. There are no particular restrictions on the blending ratio of polymers in the polymer electrolyte or the method of compounding; known blending ratios and known compounding methods in this art can be adopted.
[0107] The electrolyte may also contain other known additives, such as electrode film-forming agents, antioxidants, flame retardants, and overcharge prevention agents, to improve battery life, safety, and other purposes.
[0108] (3) Separator The separator can be any material that allows lithium ions to pass through and prevents contact between the positive and negative electrodes, and is not particularly limited, but for example, a microporous polymer film or nonwoven fabric can be used. Examples of films include polymer compounds and derivatives mainly composed of polyethylene, polypropylene, polyvinylidene fluoride, polyvinylidene chloride, polyacrylonitrile, polyacrylamide, polytetrafluoroethylene, polysulfone, polyethersulfone, polycarbonate, polyamide, polyimide, polyethers such as polyethylene oxide and polypropylene oxide, various celluloses such as carboxymethylcellulose and hydroxypropylcellulose, poly(meth)acrylic acid and its various esters, copolymers and mixtures thereof, etc. These films may be coated with ceramic materials such as alumina and silica, or with magnesium oxide, aramid resin, or polyvinylidene fluoride.
[0109] These films may be used individually or layered to form a multilayer film. Furthermore, various additives may be used in these films, and their type and content are not particularly limited, although examples include films made of polyethylene, polypropylene, polyvinylidene fluoride, or polysulfone. Note that if the electrolyte is a polymer electrolyte or an inorganic solid electrolyte, a separator may not be included.
[0110] (4) In addition, the shape of the battery is not particularly limited in this disclosure and can be in various shapes such as coin type, cylindrical type, prismatic type, laminate type, etc.
[0111] As the outer casing material for the battery, laminate film or a metal container can be used. The thickness of the outer casing material is usually 0.5 mm or less, preferably 0.3 mm or less. Examples of outer casing material shapes include flat (thin), rectangular, cylindrical, coin-shaped, and button-shaped.
[0112] As the laminate film, a multilayer film having a metal layer between resin films can also be used. For weight reduction, the metal layer is preferably an aluminum foil or an aluminum alloy foil. For the resin film, for example, polymer materials such as polypropylene, polyethylene, nylon, and polyethylene terephthalate can be used. The laminate film can be sealed by heat fusion to be formed into the shape of an exterior member. The metal container can be formed of, for example, stainless steel, aluminum, or an aluminum alloy. As the aluminum alloy, alloys containing elements such as magnesium, zinc, and silicon are preferred. In aluminum or aluminum alloy, by setting the content of transition metals such as iron, copper, nickel, and chromium to 1 mass% or less, long-term reliability and heat dissipation performance in a high-temperature environment can be dramatically improved.
[0113] 3. Battery The battery of the present disclosure may be either a primary battery or a secondary battery, and is preferably a secondary battery. The reason therefor is that it can be used repeatedly and is useful for reducing environmental load.
[0114] D. Others In the present disclosure, the following embodiments may be mentioned. [1] A sulfur-modified compound which is a reaction product of a nitrile copolymer and sulfur, wherein the nitrile copolymer is a copolymer comprising a structural unit derived from a nitrile monomer and a structural unit derived from a monomer represented by the following general formula (1), the sulfur-modified compound. (In general formula (1), R 1 and R 2 each independently represent a hydrogen atom, an unsubstituted or substituent-containing aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a group in which one or more methylene groups in the aliphatic hydrocarbon group are replaced with a divalent group selected from the following group I-1. Provided that R 1 and R 2This excludes monomers in which both atoms are hydrogen atoms. In the aliphatic hydrocarbon group having the substituents, one or more hydrogen atoms in the aliphatic hydrocarbon group are replaced by atoms or groups selected from the following group II-1. Group I-1: -O-, -COO-, -OCO-, -CO-, -CO-CO-, -CO-CO-O-, -CS-, -S-, -SO-, -SO2-, -NR'-, -NR'-CO-, -CO-NR'-, -NR'-COO-, -OCO-NR'- or -SiR'R"- Group II-1: Halogen atom, cyano group, nitro group, acrylic group, methacrylic group, -CO-H, -OH, -SH, -NH2, -C(R')=N-OH, -COOH or -SO3H R' and R'' each independently represent a hydrogen atom or an unsubstituted aliphatic hydrocarbon group having 1 to 20 carbon atoms. If there are multiple R' or R'', they may be the same or different. [2] The sulfur-modified compound according to [1], characterized in that the nitrile monomer is one or more selected from acrylonitrile and methacrylonitrile. [3] R in the general formula (1) 1 The sulfur-modified compound according to [1] or [2], characterized in that it is a hydrogen atom or an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms. [4] R in the general formula (1) 2 A sulfur-modified compound according to any one of [1] to [3], characterized in that it is a hydrogen atom or an unsubstituted alkyl group having 1 to 10 carbon atoms. [5] An electrode containing a sulfur-modified compound according to any one of [1] to [4]. [6] A battery having the electrode according to [5]. [7] The battery according to [6], wherein the electrode is the positive electrode. [8] The battery according to [7], wherein the negative electrode of the battery is lithium.
[0115] This disclosure is not limited to the embodiments described above. The embodiments described above are illustrative, and all that have substantially the same configuration as the technical idea described in the claims and that produce similar effects are included in the technical scope of this disclosure.
[0116] The present disclosure will be described in further detail below with reference to examples and comparative examples. However, the present disclosure is not limited in any way by the following examples. In the examples, "parts" and "%" refer to mass unless otherwise specified.
[0117] [Example 1] 25 g of acrylonitrile, 1.04 g of itaconic acid, and 250 g of deionized water were placed in a reaction vessel equipped with a condenser, nitrogen inlet tube, thermometer, and stirrer. The reaction vessel was then purged with nitrogen, and 0.25 g of ammonium persulfate and 0.125 g of sodium bisulfite were added. The polymerization reaction was completed by holding the mixture at 60°C for 3 hours while stirring. After cooling, the mixture was filtered by suction, dried in a vacuum oven at 70°C for 24 hours, and then ground using a ball mill to obtain a nitrile copolymer. Subsequently, 5 g of a mixture of the above nitrile copolymer and powdered sulfur (average particle size 200 μm) in a mass ratio of 1:3 was held at 160°C for 1 hour under a nitrogen atmosphere in a static tubular furnace, then the temperature was raised to 300°C over 1 hour, and the mixture was reacted at 300°C for another 1 hour. After cooling, the obtained reaction product was removed, ground using a ball mill, and coarse particles were removed using a sieve with a mesh size of 40 μm to obtain sulfur-modified compound A.
[0118] [Example 2] Sulfur-modified compound B was obtained in the same manner as in Example 1, except that 1.04 g of crotonic acid was used instead of 1.04 g of itaconic acid.
[0119] [Example 3] Sulfur-modified compound C was obtained in the same manner as in Example 1, except that 1.04 g of methacrylic acid was used instead of 1.04 g of itaconic acid.
[0120] [Example 4] Sulfur-modified compound D was obtained in the same manner as in Example 1, except that the amount of itaconic acid used was changed from 1.04 g to 0.51 g.
[0121] [Example 5] Sulfur-modified compound E was obtained in the same manner as in Example 1, except that 0.51 g of methacrylic acid was used instead of 1.04 g of itaconic acid.
[0122] [Example 6] Sulfur-modified compound F was obtained in the same manner as in Example 1, except that the amount of itaconic acid used was changed from 1.04 g to 0.25 g.
[0123] [Comparative Example 1] Sulfur-modified compound a was obtained in the same manner as in Example 1, except that itaconic acid was not used.
[0124] [Comparative Example 2] Sulfur-modified compound b was obtained in the same manner as in Example 1, except that 1.04 g of acrylic acid was used instead of 1.04 g of itaconic acid.
[0125] [Comparative Example 3] Sulfur-modified compound c was obtained in the same manner as in Example 1, except that 1.04 g of vinyl acetate was used instead of 1.04 g of itaconic acid.
[0126] [Comparative Example 4] Sulfur-modified compound d was obtained in the same manner as in Example 1, except that 1.04 g of N-vinylformamide was used instead of 1.04 g of itaconic acid.
[0127] [Comparative Example 5] Sulfur-modified compound e was obtained in the same manner as in Example 1, except that 1.04 g of methyl acrylate was used instead of 1.04 g of itaconic acid.
[0128] [Comparative Example 6] A sulfur-modified compound f was obtained in the same manner as in Example 1, except that 1.04 g of methyl methacrylate was used instead of 1.04 g of itaconic acid.
[0129] [Comparative Example 7] A sulfur-modified compound g was obtained in the same manner as in Example 1, except that 22 g of acrylonitrile, 3 g of methacrylonitrile, and 1.04 g of methyl methacrylate were used instead of 25 g of acrylonitrile and 1.04 g of itaconic acid.
[0130] Secondary batteries were prepared using each sulfur-modified compound obtained in the examples and comparative examples. (1) Preparation of the positive electrode A composition for forming the electrode layer was prepared by mixing 90.0 parts by mass of the sulfur-modified compound listed in Table 1 as the active material for the positive electrode active material layer, 5.0 parts by mass of acetylene black (manufactured by Denka) as a conductive additive, 3.0 parts by mass of styrene-butadiene rubber (aqueous dispersion, manufactured by Nippon Zeon) and 2.0 parts by mass of carboxymethylcellulose sodium (manufactured by Daicel Finechem) as binders, and 120 parts by mass of water as a solvent using a rotation-revolution mixer. This electrode layer forming composition was applied to a carbon-coated aluminum foil (thickness 20 μm) used as a current collector by the doctor blade method and dried at 90°C for 1 hour. After that, the electrode was cut to a predetermined size and vacuum-dried at 100°C for 2 hours to prepare a disc-shaped positive electrode.
[0131] (2) Preparation of the negative electrode A disc-shaped negative electrode was prepared by cutting a lithium metal with a thickness of 500 μm to a predetermined size.
[0132] (3) Preparation of electrolyte An electrolyte solution was prepared by dissolving LiPF6 at a concentration of 1.0 mol / L in a mixed solvent consisting of 50% by volume of ethylene carbonate and 50% by volume of diethyl carbonate.
[0133] (4) Battery Fabrication The positive and negative electrodes prepared earlier were placed in a case with a glass filter acting as a separator in between. Then, the electrolyte solution prepared earlier was poured into the case, the case was sealed and sealed to fabricate secondary batteries (coin-type, φ20 mm, 3.2 mm thick). The fabrication procedure in "(4) Battery Fabrication" was carried out in an atmosphere with a dew point of -70°C.
[0134] (5) Evaluation Method The discharge capacity and cycle characteristics of the secondary batteries containing each sulfur-modified compound prepared as described above were evaluated. Specifically, the batteries were placed in a constant temperature bath at 25°C, with a charge termination voltage of 3.0V and a discharge termination voltage of 1.0V, and 30 charge-discharge cycles were performed with a charge rate of 0.2C and a discharge rate of 0.2C. The discharge capacity (mAh / g) for the 2nd and 20th cycles was measured. The results for the discharge capacity (mAh / g) for the 2nd cycle are shown in Table 1. In this disclosure, "g" in the discharge capacity (mAh / g) represents the mass of the active material in the positive electrode active material layer. Furthermore, the cycle characteristics were evaluated by defining the capacity retention rate (%) as the ratio of the discharge capacity of the 20th cycle to the discharge capacity of the 2nd cycle. The results are shown in Table 1.
[0135]
[0136] From the results above, the battery using the sulfur-modified compound in the example showed increased discharge capacity. Furthermore, the battery using the sulfur-modified compound in the example showed improved capacity retention, indicating superior cycle characteristics.
Claims
1. A sulfur-modified compound which is a reaction product of a nitrile copolymer and sulfur, characterized in that the nitrile copolymer is a copolymer containing constituent units derived from a nitrile monomer and constituent units derived from a monomer represented by the following general formula (1). (In general formula (1), R 1 and R 2 Each of these independently represents a group in which one or more of a hydrogen atom, an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a methylene group in the aliphatic hydrocarbon group is replaced by a divalent group selected from the following group I-1. However, R 1 and R 2 This excludes monomers in which both atoms are hydrogen atoms. In the aliphatic hydrocarbon group having the substituents, one or more hydrogen atoms in the aliphatic hydrocarbon group are replaced by atoms or groups selected from the following group II-1. Group I-1: -O-, -COO-, -OCO-, -CO-, -CO-CO-, -CO-CO-O-, -CS-, -S-, -SO-, -SO2-, -NR'-, -NR'-CO-, -CO-NR'-, -NR'-COO-, -OCO-NR'- or -SiR'R"- Group II-1: Halogen atom, cyano group, nitro group, acrylic group, methacrylic group, -CO-H, -OH, -SH, -NH2, -C(R')=N-OH, -COOH or -SO3H R' and R'' each independently represent a hydrogen atom or an unsubstituted aliphatic hydrocarbon group having 1 to 20 carbon atoms. If there are multiple R' or R'', they may be the same or different.
2. The sulfur-modified compound according to claim 1, characterized in that the nitrile monomer is one or more selected from acrylonitrile and methacrylonitrile.
3. R in the general formula (1) 1 The sulfur-modified compound according to claim 1, characterized in that it is a hydrogen atom or an unsubstituted or substituted alkyl group having 1 to 10 carbon atoms.
4. R in the general formula (1) 2 The sulfur-modified compound according to claim 1, characterized in that it is a hydrogen atom or an unsubstituted alkyl group having 1 to 10 carbon atoms.
5. An electrode comprising the sulfur-modified compound according to any one of claims 1 to 4.
6. A battery having the electrodes described in claim 5.
7. The battery according to claim 6, wherein the electrode is the positive electrode.