Manganese-containing pyrochlore oxide powder and method for producing same
By integrating zinc or nickel into the pyrochlore oxide composition and optimizing synthesis steps, the formation of impurity phases is prevented, resulting in high manganese substitution rates and improved catalytic performance in secondary batteries.
Patent Information
- Application Number
- PCT/JP2026/017852
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-19
AI Technical Summary
Existing pyrochlore oxide powders with high manganese substitution rates face challenges in preventing the coexistence of crystalline phases different from the pyrochlore oxide structure, which hinders performance and durability in secondary batteries and other devices.
Incorporating predetermined amounts of zinc or nickel as additional elements in the pyrochlore oxide composition, along with controlled pH adjustments and synthesis steps, to achieve a high manganese substitution rate without forming impurity phases.
The resulting MBRO oxide powder exhibits excellent catalytic performance and cost savings by maintaining a single pyrochlore oxide structure, even at high manganese substitution rates, enhancing the effectiveness of secondary batteries and other devices.
Smart Images

Figure JP2026017852_19112026_PF_FP_ABST
Abstract
Description
Manganese-containing pyrochlore oxide powder and method for producing the same
[0001] This invention relates to a pyrochlore oxide powder having a bismuth (Bi)-ruthenium (Ru)-oxygen (O) type pyrochlore oxide crystal structure and containing bismuth, ruthenium, and manganese (Mn) as constituent metal elements. In this specification, oxides having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure are referred to as "BRO oxides". Among BRO oxides, pyrochlore oxides that particularly contain manganese are referred to as "MBRO oxides".
[0002] BRO oxides are materials that are expected to have applications as cathode catalysts in air-based secondary batteries and hydrogen production processes using water electrolysis. Among them, MBRO oxides containing manganese are considered to have a structure in which mainly some of the ruthenium sites are replaced with manganese, and because they can save expensive ruthenium, they are seen as promising for promoting the industrial spread of equipment using pyrochlore oxide catalysts. In this specification, the atomic ratio of manganese to the total amount of ruthenium and manganese in the composition of MBRO oxide is expressed as the "Mn / (Ru+Mn) atomic ratio". Furthermore, the index expressed as a percentage of the Mn / (Ru+Mn) atomic ratio is sometimes called the "Mn substitution rate".
[0003] Patent Document 1 describes an invention of a pyrochlore oxide powder in which the Mn substitution rate is 0 to 35%, and in which no crystalline phase different from the crystal structure of pyrochlore oxide is detected in the X-ray diffraction pattern (Claim 2). Examples of this invention include MBRO oxide with a Mn substitution rate of 30% (Examples 5 and 6).
[0004] Japanese Patent Publication No. 2024-135725
[0005] Patent Document 1 describes an MBRO oxide with a Mn substitution rate of 30%, but further improvement of the Mn substitution rate is desired to enhance the cost-saving effect of expensive ruthenium. However, in the composition range with a very high Mn substitution rate, the technology of Patent Document 1 alone is insufficient to adequately prevent the coexistence of crystalline phases different from the crystal structure of the pyrochlore oxide (referred to as "heterogeneous phases"). The coexistence of heterogeneous phases may hinder the improvement of performance and durability of secondary batteries and other devices that use the MBRO oxide as a catalyst.
[0006] The present invention aims to provide an MBRO oxide with a very high Mn substitution rate while avoiding the presence of impurity phases.
[0007] According to the inventors' research, it has been found that by including a predetermined amount of zinc (Zn) or nickel (Ni) as an element constituting MBRO oxide, a significant improvement in the Mn substitution rate can be achieved while avoiding the mixing of different phases. Based on this finding, the following inventions are disclosed herein.
[0008] [1] A pyrochlore oxide powder having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure and composed of particles containing bismuth, ruthenium, and manganese as metallic elements, wherein the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, and no crystalline phase different from the pyrochlore oxide crystal structure is detected in the X-ray diffraction pattern.
[0009] In the above [1], the zinc and nickel content is specifically specified as follows: [2] A pyrochlore oxide powder having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure, and comprising particles containing sodium, bismuth, ruthenium, manganese, and one or more elements M selected from zinc and nickel as metallic elements, wherein the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, and the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M to the total amount of bismuth and element M, is 0.05 or more and 0.25 or less, and no crystalline phase different from the pyrochlore oxide crystal structure is detected in the X-ray diffraction pattern.
[0010] The pyrochlore oxide powder described in [1] or [2] above may also contain sodium as follows: [3] The pyrochlore oxide powder described in [1] or [2] above, containing sodium in an amount of 1.0 atomic% or more and 6.0 atomic% or less.
[0011] The pyrochlore oxide powders described in [1] to [3] above can be synthesized, for example, by the method described in [4] below. [4] A "first raw material mixing step" in which bismuth-containing salt and ruthenium-containing salt, which are raw materials, are mixed in an aqueous solvent to obtain a bismuth-ruthenium-containing solution; a "first pH adjustment step" in which alkali is added to the solution obtained in the first raw material mixing step to raise the pH of the solution and obtain a solution with a pH of 4.0 or less; a "second raw material mixing step" in which manganese-containing salt, which is a raw material, and one or more elements M selected from zinc and nickel are mixed in the solution obtained in the first pH adjustment step to obtain a bismuth-ruthenium-manganese-element M-containing solution; a "second pH adjustment step" in which alkali is added to the solution obtained in the second raw material mixing step to obtain a solution with a pH of 10.0 or more; an "oxidation step" in which oxygen is supplied to the solution obtained in the second pH adjustment step to form a solid reaction product; and a "drying step" in which the reaction product is recovered and dried to obtain a precursor substance. A method for producing pyrochlore oxide powder, comprising: a "calcination step" of synthesizing oxide powder composed of particles having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure by calcining the precursor material, wherein the mixing ratio of the raw materials mixed in the liquid in the first raw material mixing step and the second raw material mixing step is such that the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, and the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M to the total amount of bismuth and element M, is 0.05 or more and 0.25 or less.
[0012] The MBRO oxide of the present invention has a very high Mn substitution rate, resulting in excellent cost savings on expensive ruthenium. Furthermore, since the MBRO oxide avoids the presence of the crystalline phase, which is an impurity phase, it is advantageous in exhibiting high catalytic performance.
[0013] X-ray diffraction patterns of MBRO oxide powder obtained in each example and Comparative Examples 1 and 2. A magnified view of the X-ray diffraction pattern in Figure 1 in the height direction. X-ray diffraction pattern of MBRO oxide powder obtained in Comparative Example 3.
[0014] [Pyrochlore Oxide] A typical compositional formula of the pyrochlore oxide is A 2 B 2 O x , where x takes a value of 7 or a value close thereto. "Bismuth-ruthenium-oxygen type pyrochlore oxide" means a pyrochlore oxide in which the A site is bismuth (Bi) and the B site is ruthenium (Ru). The manganese-containing pyrochlore oxide (MBRO oxide) targeted by the present invention has a crystal structure (pyrochlore structure) in which diffraction peaks from respective crystal planes of the "bismuth-ruthenium-oxygen type pyrochlore oxide" are observed in an X-ray diffraction pattern. That is, the "crystal structure of a bismuth-ruthenium-oxygen type pyrochlore oxide" referred to in the present specification is a cubic crystal structure belonging to the space group Fd-3m (here, the aforementioned "-3" is an abbreviation of the notation in which a "-" is placed above the character "3"). Specifically, in the X-ray diffraction pattern, Bi registered in the International Centre for Diffraction Data (ICDD) 1.9 Ru 2 O 6.922 (PDF-Number: 01-073-9236), or Bi 2 Ru 2 O 7 (PDF-Number: 01-077-9359) is identified as a crystal structure in which diffraction peaks corresponding to the diffraction peaks are observed. However, since the interplanar spacing of the crystal varies depending on the ionic radius of the atoms occupying each atomic site and the existence state of lattice defects, the positions of the diffraction peaks of the oxide targeted by the present invention may be slightly shifted from the positions of the corresponding diffraction peaks shown in the above registered data.
[0015] In MBRO oxides containing manganese as a metallic element, it is generally believed that the atomic configuration exhibits a state in which some of the ruthenium atoms occupying the B site are replaced by manganese atoms. As the Mn substitution rate increases, distortion occurs in the crystal lattice of MBRO oxide due to the difference in atomic radii between ruthenium and manganese. During the synthesis process of MBRO oxide, as the crystal lattice distortion of MBRO oxide increases, the constituent elements of MBRO oxide are consumed in the formation of crystalline phases other than MBRO oxide (heterogeneous phases), resulting in the presence of heterogeneous phases, which are impurity phases. According to the inventors' previous research, by devising the MBRO oxide synthesis process, it was possible to obtain MBRO oxide powder without the presence of heterogeneous phases up to a Mn / (Ru+Mn) atomic ratio of approximately 0.35 (Mn substitution rate of approximately 35%). However, when a larger amount of manganese was added, it became difficult to avoid the formation of heterogeneous phases.
[0016] Through further research, it was discovered that in the synthesis of MBRO oxide with a high Mn substitution rate, there are metal elements that, when added in a predetermined amount, significantly suppress the formation of heterogeneous phases. Currently, zinc and nickel have been confirmed to be effective as such metal elements. It is presumed that the atoms of these metal elements primarily replace some of the bismuth atoms occupying the A-site. By using these metal elements as constituent elements of the MBRO oxide crystal lattice, the lattice strain that occurs when ruthenium is substituted with a large amount of manganese is effectively mitigated, resulting in the acquisition of MBRO oxide powder with a high Mn substitution rate while avoiding the mixing of heterogeneous phases.
[0017] In this specification, metal elements other than sodium, bismuth, ruthenium, and manganese added as constituent elements of MBRO oxide are referred to as "element M". According to previous research, when one or more metal elements selected from zinc and nickel are used as element M, in an MBRO oxide in which element M is blended such that the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M to the total amount of bismuth and element M, is 0.05 or more and 0.25 or less, it is possible to achieve a very high Mn substitution rate, with a Mn / (Ru+Mn) atomic ratio exceeding 0.35 and less than 0.50, without the presence of impurities or other phases. The Mn / (Ru+Mn) atomic ratio may be set in the range of exceeding 0.35 and 0.45 or in the range of exceeding 0.35 and 0.42 or less.
[0018] Even if atoms other than bismuth, ruthenium, manganese, zinc, and nickel exhibit an atomic configuration in which they replace some of the bismuth atoms occupying the A site or some of the ruthenium atoms occupying the B site, or occupy interstitial positions, this is permissible as long as it does not hinder the effects of the present invention. For example, sodium (Na) atoms, which may be introduced into the liquid during the manufacturing process, may exist in the crystal lattice by replacing some of the bismuth atoms occupying the A site or by occupying interstitial positions.
[0019] Sodium stabilizes the pyrochlore structure. Pyrochlore oxides synthesized by the dry method are usually single-phase by calcination at 700-900°C, but the inclusion of sodium stabilizes the pyrochlore structure, making synthesis possible at lower temperatures, such as between 400°C and 700°C. Synthesis at low temperatures suppresses sintering of precursor particles, which is advantageous for synthesizing pyrochlore oxide particles with small particle size and large specific surface area. To incorporate sodium into the precursor material, methods such as using a sodium-containing substance (e.g., sodium hydroxide) as an alkali substance in the manufacturing process described later, or intentionally including sodium components in the liquid before drying, can be applied. In the obtained pyrochlore oxide powder, the sodium content is preferably between 1.0 atomic% and 6.0 atomic%, and may be controlled between 2.5 atomic% and 4.0 atomic%. The effect of suppressing sintering is small with a sodium content of less than 1.0 atomic%. If it exceeds 6.0 atomic%, impurity phases may be more likely to form. This sodium content can be determined, for example, by SEM-EDX analysis of pyrochlore oxide powder. In that case, the atomic percentage of sodium relative to the total amount of sodium, other contained metal elements, and oxygen should be used.
[0020] [Impure Phase] If impurity crystal phases (different phases) are present in the particles of MBRO oxide powder, it may hinder the improvement of performance in devices such as secondary batteries that use the MBRO oxide as a catalyst. The BRO oxide powder of the present invention does not show any crystal phases different from the crystal structure of "bismuth-ruthenium-oxygen type pyrochlore oxide" in its X-ray diffraction pattern.
[0021] [Manufacturing Process for MBRO Oxide Powder] The above-mentioned MBRO oxide, which has a very high Mn substitution rate, can be obtained, for example, by a powder manufacturing process that includes, in the order of above, a first raw material mixing step, a first pH adjustment step, a second raw material mixing step, a second pH adjustment step, an oxidation step, a drying step, and a calcination step.
[0022] (Raw Materials) As raw materials, bismuth-containing salts (e.g., bismuth(III) nitrate pentahydrate), ruthenium-containing salts (e.g., ruthenium(III) chloride n-hydrate), manganese-containing salts (e.g., manganese(II) nitrate hexahydrate), and element M-containing salts are prepared. One or more elements selected from zinc and nickel are chosen as element M. Zinc and nickel may be added individually or in combination. An example of a zinc-containing salt is zinc(II) nitrate hexahydrate. An example of a nickel-containing salt is nickel(II) nitrate hexahydrate.
[0023] In conventional methods for producing MBRO oxides, it is common to mix all of these raw materials in an aqueous solvent to create an initial raw material solution. However, previous research by the inventors has shown that with this method, if the concentration of raw materials in the raw material solution (starting concentration) is significantly increased, MBRO oxides containing impurity phases are more likely to be synthesized. In industrial production processes, increasing the starting concentration is important for improving productivity. Therefore, this invention discloses a multi-stage metal salt mixing method in which, among bismuth-containing salts, ruthenium-containing salts, manganese-containing salts, and element M-containing salts, an initial raw material solution is created by first mixing bismuth-containing salts and ruthenium-containing salts in an aqueous solvent, and manganese-containing salts and element M-containing salts are mixed in a later step. An aqueous solvent is a liquid medium whose main component is water (i.e., the mass proportion of water is 50% or more).
[0024] The quantitative ratios of the bismuth-containing salt, ruthenium-containing salt, and manganese-containing salt used shall be such that a bismuth-ruthenium-oxygen pyrochlore oxide exhibiting a very high Mn substitution rate is synthesized, in which a portion of the ruthenium is replaced by manganese. Furthermore, the quantitative ratio of the element M-containing salt used shall be such that it exhibits an effect of avoiding the presence of impurity crystal phases (different phases).
[0025] Specifically, the mixing ratio of the raw materials mixed in the liquid in the first and second raw material mixing steps described later can be such that the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, and the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M to the total amount of bismuth and element M, is 0.05 or more and 0.25 or less.
[0026] [First Raw Material Mixing Step] The initial raw material solution, a bismuth- and ruthenium-containing liquid, is prepared by mixing the bismuth-containing salt and ruthenium-containing salt, which are the raw material substances, in an aqueous solvent. At this stage, the manganese-containing salt is not yet mixed in. Since the bismuth-containing salt and ruthenium-containing salt have low solubility in water, when they are mixed with water, most of them remain undissolved as solids in the water, resulting in a slurry-like liquid. Therefore, it is preferable to use an aqueous solvent in which an organic substance acting as a dispersant is dissolved as a by-component other than water. For example, tetra-n-propylammonium bromide can be used as a dispersant.
[0027] An aqueous solvent is placed in the reaction vessel, and predetermined amounts of bismuth-containing salt and ruthenium-containing salt are mixed with the aqueous solvent to create a bismuth and ruthenium-containing solution. A dispersant is also mixed in as needed. This is then thoroughly stirred to form a slurry. This solution (slurry) will be acidic due to the free acid, with a pH of, for example, 0.5 or lower if the bismuth concentration at the start is around 0.6 mol / L.
[0028] [First pH Adjustment Step] Add alkali (e.g., sodium hydroxide) to the bismuth and ruthenium-containing liquid (slurry) obtained in the first raw material mixing step to raise the pH of the liquid. However, it is necessary to stop adding alkali before the pH of the liquid exceeds 4.0. The manganese-containing salt added later has different properties from the bismuth-containing salt and ruthenium-containing salt. When the pH rises above the neutral range, it becomes more stable to exist as a solid compound salt than in a dissociated ionic state (dissolved in the liquid), and is more likely to precipitate as a salt. As a result of the study, if the pH exceeds 4.0 at this stage, there is a risk of coprecipitation of the manganese-containing salt when alkali is added in the second pH adjustment step after the addition of the manganese-containing salt. In that case, it becomes difficult to prevent the final residue of the impurity phase. In the first pH adjustment step, it is more preferable to obtain a liquid with a pH of 3.0 or less, even more preferable to obtain a liquid with a pH of 2.0 or less, and it may be controlled to obtain a liquid with a pH of 1.0 or less. pH adjustment can be performed by periodically measuring and monitoring the pH of the solution, or by adding an appropriate amount of alkali determined in advance through preliminary experiments.
[0029] The temperature of the liquid (slurry) when adding alkali is preferably 50 to 99°C. Alkali addition in the first pH adjustment step can be carried out while stirring the liquid, at an addition rate that does not cause the liquid temperature to exceed the above temperature range, depending on the cooling capacity of the reaction vessel. Alkali can be added intermittently, continuously, or, if the cooling capacity of the reaction vessel allows, the entire amount can be added at once. Normally, alkali addition can be completed within one hour, but depending on the cooling capacity of the reaction vessel, it may be added over a longer period.
[0030] In this specification, pH is measured using a pH meter calibrated with an appropriate buffer solution according to the pH range to be measured, in accordance with JIS Z8802:2011. The pH values described herein are values directly read under liquid temperature conditions from a pH meter compensated by a temperature-compensated electrode. In the examples described later, pH was measured using a HORIBA portable pH / ORP / ion meter D-73 and a pH measuring electrode 9615S-10D.
[0031] [Second Raw Material Mixing Step] In the first pH adjustment step, the pH of the liquid has been adjusted to the predetermined range described above. In this step, the raw materials, a manganese-containing salt and an element M-containing salt, are mixed to obtain a bismuth, ruthenium, manganese, and element M-containing liquid. The manganese-containing salt and the element M-containing salt may be added after being dissolved in an aqueous solvent beforehand.
[0032] [Second pH Adjustment Step] Next, alkali is added while stirring the liquid. The same type of alkali used in the first pH adjustment step (for example, sodium hydroxide) can be used. In the second pH adjustment step, the pH of the liquid is adjusted to 10.0 or higher by adding alkali. If a liquid with a lower pH is subjected to the oxidation step, the effect of significantly preventing the formation of the impurity phase may not be sufficiently exhibited. It is more preferable to adjust the pH to 11.0 or higher, and even more preferable to adjust it to 11.5 or higher.
[0033] In the second pH adjustment step, it is preferable to maintain the liquid temperature at 50 to 99°C. In the second pH adjustment step, it is preferable to add the alkali as quickly as possible, depending on the temperature control capacity of the reaction vessel, in order to improve productivity. For example, it is preferable to add the alkali within 300 seconds, and it is even more preferable to add it all at once (for example, within 30 seconds).
[0034] [Oxidation Step] Next, stirring is continued while supplying oxygen to the liquid (slurry) obtained in the second pH adjustment step to form a solid reaction product. It is preferable to maintain the liquid temperature at 50 to 99°C. Oxygen can be supplied by blowing oxygen gas or air into the liquid (bubbling). It is preferable to stir for 1 to 36 hours under oxygen supply. In this way, the wet oxidation reaction proceeds and a solid reaction product containing bismuth, ruthenium, manganese, and element M is formed. This reaction product is thought to consist mainly of oxyhydroxides of the above metals.
[0035] [Drying Process] The reaction products are dried. It is efficient to dry the solid components (reaction products) after pretreatment to remove as much liquid component as possible from the liquid (reaction solution) after the oxidation process. As a pretreatment, for example, a method of removing the supernatant after letting the reaction solution stand for a predetermined time can be applied. The standing time is preferably 24 hours or more. In this case, it is preferable that the amount of supernatant removed is 70% or more by volume relative to the reaction solution after the oxidation process. If necessary, a centrifugal separator may be used to accelerate the settling of the reaction products. Alternatively, the liquid (reaction solution) after the oxidation process may be separated into solid and liquid by filtration, and the residue obtained may be mixed with a portion of the filtrate.
[0036] This drying process can be carried out by exposing the reaction product (solids) to which the liquid components are attached, for example, to air at 80 to 140°C. In this way, a precursor material is formed. Subsequently, if necessary, crushing treatment or additional drying treatment at a temperature of approximately 180 to 250°C can be performed to remove chemically adsorbed water. Furthermore, the particle size distribution of the powder to be subjected to the calcination process can be optimized, for example, by sieving.
[0037] [Castration Process] The obtained precursor material is calcined by heating it in an oxidizing gas atmosphere to synthesize an oxide powder composed of particles having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure. In this invention, since a precursor material containing manganese is used, a manganese-containing pyrochlore oxide (MBRO oxide) is obtained. Furthermore, since the precursor material contains a predetermined amount of element M (one or more of zinc and nickel), it is thought that the crystal lattice distortion that becomes a problem when a large amount of manganese is included is mitigated, and the formation of impurity phases (different phases) is prevented. The calcination temperature can be set in the range of 900°C or less. When a sodium-containing material (for example, sodium hydroxide) is used as the alkali material, the sodium present in the precursor material contributes to the stabilization of the pyrochlore structure, so it is preferable that the calcination temperature be 400 to 700°C and the calcination time (holding time in the above temperature range) be 0.5 to 3.0 hours. Air at atmospheric pressure can be used as the oxidizing gas atmosphere.
[0038] If necessary, the MBRO oxide powder obtained by firing can be subjected to crushing treatment or particle size distribution adjustment treatment using a sieve. In addition, a treatment for removing water-soluble adhering salts can be performed by, for example, a method of stirring the obtained powder in water and then collecting the solid component. As described above, in the method with an increased charging concentration of the raw material substances, it is possible to obtain MBRO oxide powder in which the formation of impurity phases is significantly suppressed.
[0039] [Example 1] This example is an example in which zinc (Zn) is applied as the above-mentioned element M.
[0040] (First Raw Material Mixing Step) A separable beaker (manufactured by Asahi Seisakusho) with a volume of 1 L was set on a mantle heater (manufactured by Asahi Seisakusho), 150 g of pure water was added, and the mixture was heated and maintained at 75°C while stirring. An anchor blade was used for stirring, and the stirring rotation speed was set to 300 rpm. A solution prepared by dissolving 0.0521 mol (14.15 g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Corporation), which is a dispersant, in 50 g of pure water was added thereto while stirring. Further, slurries were prepared by uniformly suspending 0.3750 mol (182.8 g) of bismuth(III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Corporation) as the bismuth-containing salt and 0.2631 mol (58.98 g) of ruthenium(III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo K.K.) as the ruthenium-containing salt in 200 g of pure water respectively, and the slurries were added. After each substance was charged, the mixture was stirred at a liquid temperature of 75°C for 1 hour. Since bismuth(III) nitrate pentahydrate and ruthenium(III) chloride n-hydrate have low solubility in water, their entire amounts could not be dissolved even at 75°C, and a slurry-like raw material solution was obtained.
[0041] (First pH Adjustment Step) A sodium hydroxide aqueous solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. Here, while measuring the pH of the solution as appropriate, sodium hydroxide was continuously added until the pH reached 1.0 so as not to cause an excessive temperature rise. The time required for the addition was about 30 minutes.
[0042] (Second raw material mixing step) 0.1754 mol (50.35 g) of manganese(II) nitrate hexahydrate (manufactured by FUJIFILM Wako Pure Chemical Corporation) as the manganese-containing salt, and 0.04166 mol (12.39 g) of zinc(II) nitrate hexahydrate (manufactured by FUJIFILM Wako Pure Chemical Corporation) as the M-containing content were dissolved in 100 g of pure water to prepare an aqueous solution containing manganese and M (zinc in this example). The above aqueous solution containing manganese and M was mixed with the liquid whose pH had been adjusted to 1.0 after completing the first pH adjustment step, and the mixture was stirred at a liquid temperature of 75°C for 30 minutes.
[0043] In the mixing ratio of the raw material substances mixed into the liquid in the first raw material mixing step and the second raw material mixing step, the Mn / (Ru+Mn) atomic ratio representing the atomic ratio of the manganese amount to the total amount of ruthenium and manganese is 0.40, and the M / (Bi+M) atomic ratio representing the atomic ratio of the element M to the total amount of bismuth and element M (Zn in this example) is 0.10.
[0044] (Second pH adjustment step) Thereafter, an amount of alkali obtained by subtracting the amount of alkali added in the first pH adjustment step from the alkali amount corresponding to 1.04 times the amount of alkali required to react with all anions supplied from all metal salts (the bismuth-containing salt, the ruthenium-containing salt, the manganese-containing salt, and the M-containing salt) mixed in the liquid was added all at once into the liquid using a sodium hydroxide aqueous solution with a concentration of 18 mol / L. The time required for the all-at-once addition is about several seconds. It was confirmed that the pH of the liquid after the completion of sodium hydroxide addition was 11.5 or higher.
[0045] (Oxidation step) Next, while blowing pure oxygen gas into the liquid in the reaction vessel, the temperature was maintained at 75°C, and stirring was continued for 18 hours to form a solid reaction product. The supply rate of pure oxygen gas was set to be about 100 mL / min as the gas volume at normal temperature and atmospheric pressure per 1 L of liquid in the reaction vessel.
[0046] (Drying process) After stirring as described above, the liquid in the reaction vessel (slurry in which the reaction products were suspended) was left to stand for 5 days, then the supernatant was removed, and finally, more than 70% of the supernatant relative to the volume of the "liquid in the reaction vessel" was removed by centrifugation, and the reaction products were recovered. The recovered reaction products, along with the remaining liquid components, were dried by holding them in air at 120°C for 18 hours to form a precursor substance.
[0047] This precursor material was broken down into a powder, then further dried by holding it in air at 200°C for two hours, and subsequently crushed in a mortar to prepare it as a precursor material for firing.
[0048] (Castration process) MBRO oxide was synthesized by calcining the above precursor material by holding it in air at 600°C for 1 hour.
[0049] The synthesized MBRO oxide was stirred and washed in 0.5 L of pure water per 100 g of oxide to remove attached salts, then the solids were recovered by suction filtration, and the solids were dried in air at 120°C to obtain MBRO oxide powder.
[0050] (Measurement of X-ray diffraction pattern) The obtained MBRO oxide powder was subjected to X-ray diffraction using an X-ray diffractometer (Rigaku Ultima IV) under the following conditions: Cu-Kα rays, tube voltage 40kV, tube current 40mA, measurement step 0.02 degrees, and scan speed 0.5 degrees / min.
[0051] Figure 1 shows a summary of the X-ray diffraction patterns for the MBRO oxide powder obtained in this example and in each of the examples described later (excluding Comparative Example 3). Figure 2 shows the diffraction pattern of Figure 1 magnified in the peak height direction. Analysis of the X-ray diffraction pattern using the RIR (Reference Intensity Ratio) method revealed that no crystalline phase (impurity phase) different from the pyrochlore oxide crystal structure was detected in the MBRO oxide powder obtained in this example.
[0052] (Compositional analysis by SEM-EDX) The obtained MBRO oxide powder was subjected to compositional analysis using SEM (FE-SEM JSM-7200F, JEOL Ltd.) and EDX (X-Max20, Oxford Instruments). As a result, the Mn / (Ru+Mn) atomic ratio of the MBRO oxide powder obtained in this example was 0.43, and the M / (Bi+M) atomic ratio was 0.11. The results are shown in Table 1 (the same applies to each example below).
[0053] [Example 2] This example uses nickel (Ni) as the element M mentioned above. Except that in the second raw material mixing step of Example 1, 0.04166 moles (12.13 g) of nickel(II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of 0.04166 moles of zinc(II) nitrate hexahydrate as the M-containing salt, an aqueous solution containing manganese and M (nickel in this example) was prepared, and MBRO oxide powder was obtained under the same conditions as in Example 1.
[0054] In this example, as in Example 1, the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is 0.40 in the mixing ratio of the raw materials mixed in the liquid in the first raw material mixing step and the second raw material mixing step, and the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M (Ni in this example) to the total amount of bismuth and element M, is 0.10. The same investigation as in Example 1 was carried out on this MBRO oxide powder.
[0055] Analysis of the X-ray diffraction pattern revealed that the MBRO oxide powder obtained in this example did not contain any crystalline phases (impurity phases) different from the pyrochlore oxide crystal structure (Figures 1 and 2). Furthermore, compositional analysis by SEM-EDX showed that the Mn / (Ru+Mn) atomic ratio of the MBRO oxide powder obtained in this example was 0.42, and the M / (Bi+M) atomic ratio was 0.11.
[0056] [Comparative Example 1] This example is one in which the element M described above was not added. Except that in the first raw material mixing step of Example 1, 0.4170 moles (203.1 g) of bismuth(III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used as the bismuth-containing salt, and in the second raw material mixing step, instead of using 0.04166 moles of zinc(II) nitrate hexahydrate, which is the M-containing salt, 0.1754 moles (50.35 g) of manganese(II) nitrate hexahydrate was dissolved in 100 g of pure water to prepare a manganese-containing aqueous solution, and the above manganese-containing aqueous solution was mixed with the liquid whose pH had been adjusted to 1.0 after the first pH adjustment step, and stirred at a liquid temperature of 75°C for 30 minutes, MBRO oxide powder was obtained under the same conditions as in Example 1.
[0057] In this example, as in Example 1, the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese in the mixing ratio of the raw materials mixed in the liquid in the first and second raw material mixing steps, is 0.40. However, element M is not added. The same investigation as in Example 1 was carried out on this MBRO oxide powder.
[0058] Analysis of the X-ray diffraction pattern revealed that the MBRO oxide powder obtained in this example contained a crystalline phase (impurity phase) different from the crystalline structure of pyrochlore oxide (peaks indicated by arrows in Figure 2). Furthermore, compositional analysis by SEM-EDX showed that the Mn / (Ru+Mn) atomic ratio of the MBRO oxide powder obtained in this example was 0.47.
[0059] [Comparative Example 2] This example uses cobalt (Co) as the element M mentioned above. Except that in the second raw material mixing step of Example 1, 0.04166 moles (12.12 g) of cobalt(II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of 0.04166 moles of zinc(II) nitrate hexahydrate as the M-containing salt, an aqueous solution containing manganese and M (cobalt in this example) was prepared, MBRO oxide powder was obtained under the same conditions as in Example 1.
[0060] In this example, as in Example 1, the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is 0.40 in the mixing ratio of the raw materials mixed in the liquid in the first raw material mixing step and the second raw material mixing step, and the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M (Co in this example) to the total amount of bismuth and element M is 0.10. The same investigation as in Example 1 was carried out on this MBRO oxide powder.
[0061] Analysis of the X-ray diffraction pattern revealed that the MBRO oxide powder obtained in this example contained a crystalline phase (impurity phase) different from the crystalline structure of pyrochlore oxide (peaks indicated by arrows in Figure 2). Furthermore, compositional analysis by SEM-EDX showed that the Mn / (Ru+Mn) atomic ratio of the MBRO oxide powder obtained in this example was 0.47, and the M / (Bi+M) atomic ratio was 0.10.
[0062] [Comparative Example 3] This example shows a higher Mn substitution rate than in Comparative Example 1, without the addition of element M as described above. In Example 1, the amount of bismuth(III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) added was 0.4170 moles (203.1 g), and the amount of ruthenium(III) chloride n hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) added was 0.2193 moles (49.09 g). In the second raw material mixing step, instead of using zinc(II) nitrate hexahydrate, which is a M-containing salt, 0.2193 moles (62.94 g) of manganese(II) nitrate hexahydrate was dissolved in 100 g of pure water to prepare a manganese-containing aqueous solution. After completing the first pH adjustment step and adjusting the pH to 1.0, the above manganese-containing aqueous solution was mixed with the liquid and stirred at a liquid temperature of 75°C for 30 minutes. Except for these differences, MBRO oxide powder was obtained under the same conditions as in Example 1.
[0063] In this example, the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese in the mixing ratio of the raw materials mixed in the liquid in the first and second raw material mixing steps, is 0.50. However, element M is not added. The same investigation as in Example 1 was carried out on this MBRO oxide powder.
[0064] Figure 3 shows an example of the X-ray diffraction pattern for the MBRO oxide powder obtained in this example. Analysis of the X-ray diffraction pattern revealed that the MBRO oxide powder obtained in this example has a phase (Bi) that is different from the crystal structure of pyrochlore oxide. 3 Ru 3 O 11 A large amount of (which is thought to be mainly composed of) was detected (peaks indicated by arrows in Figure 3). Furthermore, compositional analysis by SEM-EDX revealed that the Mn / (Ru+Mn) atomic ratio of the MBRO oxide powder obtained in this example was 0.54.
[0065]
Claims
1. A pyrochlore oxide powder having a bismuth-ruthenium-oxygen pyrochlore oxide crystal structure and composed of particles containing bismuth, ruthenium, and manganese as metallic elements, wherein the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, and no crystalline phase different from the pyrochlore oxide crystal structure is detected in the X-ray diffraction pattern.
2. A pyrochlore oxide powder having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure, comprising particles containing sodium, bismuth, ruthenium, manganese, and one or more elements M selected from zinc and nickel as metallic elements, wherein the Mn / (Ru+Mn) atomic ratio, representing the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, the M / (Bi+M) atomic ratio, representing the atomic ratio of element M to the total amount of bismuth and element M, is 0.05 or more and 0.25 or less, and no crystalline phase different from the pyrochlore oxide crystal structure is detected in the X-ray diffraction pattern.
3. The pyrochlore oxide powder according to claim 1 or 2, containing sodium in an amount of 1.0 atomic% to 6.0 atomic%.
4. A "first raw material mixing step" in which bismuth-containing salt and ruthenium-containing salt, which are raw materials, are mixed in an aqueous solvent to obtain a bismuth-ruthenium-containing solution; a "first pH adjustment step" in which alkali is added to the solution obtained in the first raw material mixing step to raise the pH of the solution and obtain a solution with a pH of 4.0 or less; a "second raw material mixing step" in which manganese-containing salt, which is a raw material, and one or more elements M selected from zinc and nickel are mixed in the solution obtained in the first pH adjustment step to obtain a bismuth-ruthenium-manganese-element M-containing solution; a "second pH adjustment step" in which alkali is added to the solution obtained in the second raw material mixing step to obtain a solution with a pH of 10.0 or more; an "oxidation step" in which oxygen is supplied to the solution obtained in the second pH adjustment step to form a solid reaction product; and a "drying step" in which the reaction product is recovered and dried to obtain a precursor substance. A method for producing pyrochlore oxide powder, comprising: a "calcination step" of synthesizing oxide powder composed of particles having a bismuth-ruthenium-oxygen type pyrochlore oxide crystal structure by calcining the precursor material, wherein the mixing ratio of the raw materials mixed in the liquid in the first raw material mixing step and the second raw material mixing step is such that the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is greater than 0.35 and less than 0.50, and the M / (Bi+M) atomic ratio, which represents the atomic ratio of element M to the total amount of bismuth and element M, is 0.05 or more and 0.25 or less.