Method for manufacturing electronic-component device

By employing thermosetting adhesive layers with controlled viscosity and temperature, the method addresses resin overflow issues, achieving reduced voids and enhanced connectivity in semiconductor devices.

WO2026240096A1PCT designated stage Publication Date: 2026-11-19RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017957
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The overflow (fillet) of the insulating resin layer from the edges of circuit members in semiconductor devices is a challenge during the manufacturing process, leading to potential voids and poor connectivity between circuit members.

Method used

A method involving the use of thermosetting adhesive layers with controlled viscosity and temperature to form an adhesive laminate, which is then heated and pressurized to create a semiconductor package with reduced resin overflow and improved connectivity.

Benefits of technology

The method effectively reduces resin overflow and maintains high connectivity between circuit members, minimizing voids and ensuring reliable electrical connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017957_19112026_PF_FP_ABST
    Figure JP2026017957_19112026_PF_FP_ABST
Patent Text Reader

Abstract

This method for manufacturing an electronic-component device includes: preparing a first circuit member having a first substrate and a first connection terminal provided on a main surface of the first substrate; providing a thermosetting base adhesive layer on the main surface; providing one or more thermosetting additional adhesive layers on the base adhesive layer by a method involving an increase in temperature of the base adhesive layer, thereby forming an adhesive laminate including the base adhesive layer and the additional adhesive layers on the main surface of the first substrate; forming an intermediate laminate having the first circuit member, the adhesive laminate, and a second circuit member; and forming a connection body having an insulating resin layer by heating and pressurizing the intermediate laminate.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing electronic component device

[0001] The present disclosure relates to a method for manufacturing an electronic component device such as a semiconductor package.

[0002] In the manufacture of semiconductor devices, a flip-chip connection method may be adopted, in which conductive protrusions called bumps are provided as connection terminals on a semiconductor chip or a wiring circuit board, and the semiconductor chip and the wiring circuit board or another semiconductor chip are connected via a non-conductive adhesive (NCF) by connecting the connection terminals to each other (for example, Patent Document 1).

[0003] International Publication No. 2018 / 194156

[0004] The present disclosure relates to a method for manufacturing an electronic component device, which includes forming a connected body in which circuit members having connection terminals are connected to each other with an insulating resin layer interposed therebetween, and particularly relates to reducing the overflow (fillet) of the insulating resin layer from the edge of the circuit member.

[0005] This disclosure includes: [1] preparing a first circuit member having a first substrate and a first connection terminal provided on the main surface of the first substrate; providing a thermosetting base adhesive layer on the main surface; providing one or more thermosetting additional adhesive layers on the base adhesive layer in a manner that causes the temperature of the base adhesive layer to rise, thereby forming an adhesive laminate including the base adhesive layer and the additional adhesive layers on the main surface of the first substrate; preparing a second circuit member having a second substrate and a second connection terminal provided on the main surface of the second substrate; forming an intermediate laminate having the first circuit member, the adhesive laminate and the second circuit member, with the first connection terminal and the second connection terminal facing each other, and the adhesive laminate interposed between the first circuit member and the second circuit member; and forming a connector having the first circuit member, an insulating resin layer formed by the thermosetting of the adhesive laminate and the second circuit member, with the first connection terminal and the second connection terminal electrically connected, by heating and pressurizing the intermediate laminate. A method for manufacturing an electronic component device, including: [2] The method according to [1], wherein one or more additional adhesive layers are provided on the base adhesive layer, and a thermosetting adhesive film is bonded to the base adhesive layer while the adhesive film is heated. [3] The method according to [2], wherein the adhesive film is bonded to the base adhesive layer by vacuum lamination while the adhesive film is heated. [4] The method according to [2] or [3], wherein the adhesive film is bonded to the base adhesive layer while the adhesive film is heated to a temperature lower than the temperature at which it exhibits the lowest melt viscosity. [5] The method according to any one of [1] to [4], further comprising heating the base adhesive layer provided on the main surface of the first substrate before the additional adhesive layer is provided on the base adhesive layer.[6] The method further comprises dividing the first substrate together with the adhesive laminate to form a plurality of individualized first circuit members having individualized first substrates and adhesive laminates, wherein the first substrate before being individualized is a semiconductor wafer, and the intermediate laminate having the individualized first circuit members, the adhesive laminate and the second circuit member is formed, according to any one of [1] to [5].

[0006] In the manufacturing of electronic components, the overflow (fillet) of the insulating resin layer from the edges of circuit members can be reduced.

[0007] Figure 1 is a cross-sectional view showing an example of a method for manufacturing an electronic component device. Figure 2 is a cross-sectional view showing an example of a method for manufacturing an electronic component device. Figure 3 is a cross-sectional view showing an example of a method for manufacturing an electronic component device. Figure 4 is a cross-sectional view showing an example of a method for manufacturing an electronic component device. Figure 5 is a cross-sectional view showing an example of a method for manufacturing an electronic component device. Figure 6 is a cross-sectional view showing an example of a method for manufacturing an electronic component device. Figure 7 is a cross-sectional view showing an example of a method for manufacturing an electronic component device.

[0008] The present invention is not limited to the following examples.

[0009] Figures 1, 2, 3, 4, 5, 6, and 7 are cross-sectional views showing an example of a method for manufacturing an electronic component device. The method shown in Figures 1 to 7 is an example of a method for manufacturing a semiconductor package 50, which is an electronic component device, as shown in Figure 7. This method involves preparing a first circuit member 10W having a first substrate 11W and a first connection terminal 12 provided on the main surface 11S of the first substrate 11W (Figure 1), providing a thermosetting base adhesive layer 31 on the main surface 11S (Figure 2), providing a thermosetting additional adhesive layer 32 on the base adhesive layer 31, thereby forming an adhesive laminate 30A including the base adhesive layer 31 and the additional adhesive layer 32 on the main surface 11S of the first substrate 11W (Figure 3), and dividing the first substrate 11W together with the adhesive laminate 30A to form a plurality of individual first circuit parts. The process includes forming a material 10 (Figure 4), preparing a second circuit member 20 having a second substrate 21 and a second connection terminal 22 provided on the main surface 21S of the second substrate 21 (Figure 5), forming an intermediate laminate 50A having a first circuit member 10, an adhesive laminate 30A, and a second circuit member 20 (Figure 6), and forming a semiconductor package 50 which is a connector having a first circuit member 10, an insulating resin layer 30 formed by the thermal curing of the adhesive laminate 30A, and a second circuit member 20 by heating and pressurizing the intermediate laminate 50A (Figure 7). In the intermediate laminate 50A, the first connection terminal 12 and the second connection terminal 22 are arranged facing each other, and the adhesive laminate 30A is interposed between the first circuit member 10 and the second circuit member 20.

[0010] The first circuit member 10 shown in Figure 1 has a first substrate 11W and a plurality of first connection terminals 12 provided on the main surface 11S of the first substrate 11W. The first substrate 11W can be a semiconductor substrate, and may be, for example, a semiconductor wafer (e.g., a silicon wafer) containing integrated circuits that constitute a plurality of semiconductor chips. The thickness of the first substrate 11W may be, for example, 10 μm or more and 800 μm or less. The first circuit member may be a pre-pieced semiconductor chip. In that case, the step of separating the first substrate 11W together with the adhesive laminate 30A is usually unnecessary.

[0011] The first connection terminal 12 may be a connection terminal connected to an integrated circuit corresponding to a semiconductor chip formed by the fractionation of the first substrate 11W. The first connection terminal 12 may have a metal pillar 12a and a bump 12b containing a metal material provided on the metal pillar 12a. The metal pillar 12a may be, for example, a copper pillar. The melting point of the metal material contained in the bump 12b may be 220°C or more and 330°C or less, or 140°C or more and 220°C or less. The bump 12b may be a solder bump containing solder as the metal material. The metal material constituting the bump 12b may be a solder containing Sn-Ag alloy, Sn-Pb alloy, Sn-Bi alloy, Sn-Cu alloy, or Sn-Ag-Cu alloy. The height of the first connection terminal 12 from the first substrate 11W may be, for example, 2 μm or more and 100 μm or less. The pitch between adjacent first connection terminals may be, for example, 3 μm or more and 500 μm or less. Here, the pitch refers to the distance between the centers of adjacent first connection terminals when viewed from the thickness direction of the first substrate 11W.

[0012] As shown in Figure 2, a thermosetting base adhesive layer 31 is provided on the main surface 11S of the first substrate 11W. The base adhesive layer 31 is usually provided so as to fill the space between adjacent first connection terminals 12 on the main surface 11S. The thickness of the base adhesive layer 31 may be less than the height of the first connection terminal 12 from the main surface 11S of the first substrate 11W. The thickness of the base adhesive layer 31 may be, for example, 1 μm or more and 60 μm or less.

[0013] The base adhesive layer 31 can be provided, for example, by laminating a thermosetting base adhesive film to the first circuit member 10W, or by applying a thermosetting adhesive to the first circuit member 10W. The shear viscosity of the adhesive film or thermosetting adhesive used to form the base adhesive layer 31 may be 10,000 Pa·s or more at 40°C, 200,000 Pa·s or less, or 150,000 Pa·s or less. The minimum shear viscosity (minimum melt viscosity) of the adhesive film or thermosetting adhesive used to form the base adhesive layer 31 may be 500 Pa·s or more and 3,000 Pa·s or less, or 800 Pa·s or more and 2,500 Pa·s or less. When the minimum melt viscosity of the adhesive film or thermosetting adhesive is within this range, voids tend to be less likely to remain in the base adhesive layer 31 or the final insulating resin layer 30. The shear viscosity of the adhesive film or thermosetting adhesive can be adjusted to a desired range, for example, by adjusting the type and content of polymer components or fillers.

[0014] The shear viscosity and the minimum value of shear viscosity in this disclosure may be values ​​read from a viscosity curve showing the relationship between shear viscosity (complex viscosity ratio) and temperature, obtained when viscoelasticity is measured for a sample of adhesive film or thermosetting adhesive under conditions of a heating rate of 10°C / min, a frequency of 10 Hz, and a strain of 1%. The sample for viscoelasticity measurement may be, for example, a laminate with a thickness of 300 to 450 μm obtained by laminating multiple adhesive films. The viscosity measuring device may be, for example, an ARES manufactured by T.A. Instruments, Inc.

[0015] The base adhesive layer 31 provided on the main surface 11S of the first substrate 11W may be heated before the additional adhesive layer 32 is provided on the base adhesive layer 31. This allows the thermal curing of the base adhesive layer 31 to progress, and the effects such as fillet reduction may be even more pronounced. The heating temperature at this stage may be, for example, 50°C to 170°C, and the heating time may be 30 seconds to 600 seconds.

[0016] As shown in Figure 3, a thermosetting additional adhesive layer 32 is provided on the base adhesive layer 31. As a result, an adhesive laminate 30A including the base adhesive layer 31 and the additional adhesive layer 32 is formed on the main surface 11S of the first substrate 11W.

[0017] The additional adhesive layer 32 is provided in a manner that involves raising the temperature of the base adhesive layer 31. As the temperature rises, the thermal curing of the base adhesive layer 31 progresses to some extent, which increases the viscosity of the base adhesive layer 31, and the fluidity of the base adhesive layer 31 decreases compared to before the additional adhesive layer 32 is provided. Therefore, the base adhesive layer 31 can maintain fluidity that allows it to properly fill voids between the first connection terminals before the additional adhesive layer 32 is provided, while having relatively low fluidity during the heating and pressurizing stages for forming the semiconductor package 50 (connector). As a result, the fillet 30F, which is the insulating resin layer 30 that protrudes from the end of the first circuit member 10, can be reduced. Furthermore, because the additional adhesive layer 32 can maintain relatively high fluidity, the first connection terminal 12 and the second connection terminal 22 can be easily joined in the semiconductor package 50 (connector), and a good connection between the first circuit member 10 and the second circuit member 20 can be easily ensured.

[0018] The additional adhesive layer 32 can be provided, for example, by bonding a thermosetting adhesive film to the base adhesive layer 31 while heating it. As the adhesive film for forming the additional adhesive layer 32 is heated, the temperature of the base adhesive layer 31 rises. The adhesive film can be bonded to the base adhesive layer 31 by, for example, vacuum lamination, heat pressing, or roll lamination. The temperature at which the adhesive film is heated to provide the additional adhesive layer 32 is adjusted so that the thermosetting of the base adhesive layer 31 progresses to a certain extent while maintaining the appropriate fluidity of the additional adhesive layer 32. This heating temperature may be lower than the temperature at which the adhesive film exhibits its minimum melt viscosity. For example, the heating temperature may be 50°C or higher, 60°C or higher, or 70°C or higher, and may be 170°C or lower, 140°C or lower, or 110°C or lower. After the additional adhesive layer 32 is provided, the base adhesive layer 31 may be in a semi-cured or B-stage state. When the base adhesive layer 31 and the additional adhesive layer 32 are provided using adhesive films, the adhesive film used to provide the additional adhesive layer 32 may be the same as or different from the adhesive film (base adhesive film) used to provide the base adhesive layer 31.

[0019] The shear viscosity of the adhesive film used to provide the additional adhesive layer 32 may be 10,000 Pa·s or more at 40°C, 200,000 Pa·s or less, or 150,000 Pa·s or less. The minimum shear viscosity (minimum melt viscosity) of the adhesive film used to provide the additional adhesive layer 32 may be 500 Pa·s or more and 3,000 Pa·s or less, or 800 Pa·s or more and 2,500 Pa·s or less. The temperature at which the adhesive film used to provide the additional adhesive layer 32 exhibits its minimum melt viscosity may be, for example, 100°C or more and 170°C or less.

[0020] The thickness of the additional adhesive layer 32 may be, for example, 1 μm or more and 60 μm or less. The area and thickness of the adhesive laminate 30A are appropriately set according to the size of the first substrate 11W, the height of the first connection terminal 12, etc. The minimum thickness of the adhesive laminate 30A may be, for example, 1 μm or more and 60 μm or less. The surface of the adhesive laminate 30A may have irregularities that reflect the shape of the first connection terminal 12. Multiple additional adhesive layers 32 may be laminated on the base adhesive layer 31.

[0021] As shown in Figure 4, a plurality of individual pieces of the first circuit member 10 are formed by dividing the first substrate 11W together with the adhesive laminate 30A along the dicing line D. The individual pieces of the first circuit member 10 can be semiconductor chips having individual pieces of the first substrate 11 (semiconductor substrate) and first connection terminals 12. As a dicing method, any conventional method such as blade dicing can be applied. Since the thermal curing of the base adhesive layer 31 has progressed to some extent, the base adhesive layer 31 can adhere relatively strongly to the first substrate 11W. Therefore, peeling of the adhesive laminate 30A during dicing can be suppressed.

[0022] The individualized first circuit members 10 are picked up one by one, and as shown in Figure 5, the first circuit members 10 are aligned on a separately prepared second circuit member 20 so that the first connection terminal 12 and the second connection terminal 22 are positioned opposite each other.

[0023] The second circuit member 20 includes a second substrate 21 and a second connection terminal 22 provided on the main surface 21S of the second substrate 21. The second substrate 21 may be a semiconductor wafer, a semiconductor chip, or a wiring circuit board. If the second substrate 21 is a semiconductor wafer, the second substrate 21 may include portions corresponding to multiple semiconductor chips. The second substrate 21 may have a passivation film provided around the second connection terminal 22. The second connection terminal 22 may be, for example, a metal pad containing a metallic material. The metallic material constituting the second connection terminal 22 may be, for example, gold, silver, copper, solder, tin, nickel, or a combination thereof. The solder as the metallic material constituting the second connection terminal 22 may include Sn-Ag alloy, Sn-Pb alloy, Sn-Bi alloy, Sn-Cu alloy, or Sn-Ag-Cu alloy.

[0024] As shown in Figure 6, an intermediate laminate 50A having a first circuit member 10, an adhesive laminate 30A, and a second circuit member 20 is formed between a pair of opposing pressing members 70 and 71. The pressing member 70 positioned on the second circuit member 20 side may be a stage, and the pressing member 71 positioned on the first circuit member 10 side may be a crimping head such as a flip-chip bonder. The intermediate laminate 50A may be formed by placing the first circuit member 10 and the adhesive laminate 30A, which are adsorbed by the pressing member 71 (which is the crimping head), onto the second circuit member 20, and then the intermediate laminate 50A may be pressed with the crimping head (pressing member 71) in that state. During part or all of the heating and pressurizing of the intermediate laminate 50A by the pressing members 70 and 71, the pressing member 70, the pressing member 71, or both thereof are heated to a predetermined temperature. This heating and pressurizing process may cause the adhesive laminate 30A to heat-cur, forming an insulating resin layer 30, which in turn electrically connects the first connection terminal 12 and the second connection terminal 22 to form the semiconductor package 50, which is the connected body. Alternatively, at this stage, an intermediate laminate 50A having the adhesive laminate 30A may be formed as a temporary crimped body, and then the semiconductor package 50, which is the connected body, may be formed by further heating and pressurizing the temporary crimped body. The first connection terminal 12 and the second connection terminal 22 may be in contact with each other in the intermediate laminate 50A or the temporary crimped body before the final crimping.

[0025] The heating temperature for forming the temporary crimping body (temporary crimping temperature) is usually lower than the melting point of the metal material constituting the first connection terminal 12 and the melting point of the metal material constituting the second connection terminal 22. The temporary crimping temperature may be, for example, 100°C or higher, 200°C or lower, 195°C or lower, 190°C or lower, or 185°C or lower. The heating and pressing time for forming the temporary crimping body may be 5 seconds or less, 4 seconds or less, 3 seconds or less, or 2 seconds or less, or 0.5 seconds or more, or 1 second or more. The pressure for forming the temporary crimping body may be 1.45 MPa or less, 1.40 MPa or less, or 1.35 MPa or less, or 1.0 MPa or higher, 1.05 MPa or higher, or 1.1 MPa or higher. The load applied to the entire intermediate laminate 50A by the pressing members 70, 71 for forming the temporary crimping body may be 50 N or more and 80 N or less.

[0026] The heating temperature (main crimping temperature) used in heating and pressurizing to form the semiconductor package 50, which is the connecting body, can usually be at least one of the melting points of the metal material constituting the first connecting terminal 12 (especially the bump 12b) or the metal material constituting the second connecting terminal 22. The main crimping temperature may be, for example, 220°C or more and 330°C or less. When the connecting body is formed by heating and pressurizing with pressing members 70 and 71, the pressing member 70, the pressing member 71, or both thereof, are heated to a predetermined main crimping temperature. The heating time at the main crimping temperature for forming the semiconductor package 50, which is the connecting body, may be, for example, 5 seconds or more and 60 seconds or less. Heating at the main crimping temperature for forming the semiconductor package 50 (connecting body) causes the adhesive laminate 30A to cure, and an insulating resin layer 30, which is the cured adhesive laminate 30A, is formed. After heating and pressurizing for main crimping, the connecting body may be heated to further cure the insulating resin layer 30.

[0027] If a temporary crimp is formed, the temporary crimp may be heated to the final crimping temperature under a pressurized atmosphere during the final crimping to form the connector. For this purpose, a heating furnace such as a pressurized reflow oven or a pressurized oven can be used. The gas forming the pressurized atmosphere may include air, nitrogen, or formic acid. The pressure of the pressurized atmosphere may be, for example, above atmospheric pressure and 1 MPa or less. From the viewpoint of suppressing voids and improving connectivity, the pressure of the pressurized atmosphere may be, for example, above atmospheric pressure and 0.90 MPa or less, or between 0.20 MPa and 0.80 MPa.

[0028] The base adhesive layer 31 and the additional adhesive layer 32 can be layers formed from any non-conductive thermosetting adhesive. To provide the base adhesive layer 31 and the additional adhesive layer 32, an adhesive film, which is a film-type thermosetting adhesive, may be used. In this case, the adhesive film may be a normal non-conductive adhesive film (NCF) used for sealing electrodes, etc. Examples of thermosetting adhesives constituting the base adhesive layer 31, the additional adhesive layer 32, or the adhesive film for forming them will be described below.

[0029] An example of a thermosetting adhesive includes a thermosetting resin having a molecular weight of less than 10,000, a curing agent for the thermosetting resin, and a polymer component having a weight-average molecular weight of 10,000 or more.

[0030] Thermosetting resins are compounds that form crosslinked polymers through curing reactions, and examples include epoxy resins. Epoxy resins can be compounds having two or more epoxy groups. Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, triphenylmethane type epoxy resins, and dicyclopentadiene type epoxy resins. These can be used individually or in combination of two or more. The weight-average molecular weight of epoxy resins is usually less than 10,000. In this specification, weight-average molecular weight means the value on a standard polystyrene basis, measured by gel permeation chromatography (GPC).

[0031] The epoxy resin content may be 5% by mass or more and 75% by mass or 10% by mass or more and 50% by mass or 15% by mass or more and 35% by mass or less, based on the mass of the thermosetting adhesive or the total mass of components other than the solvent in the thermosetting adhesive.

[0032] A curing agent is a component that facilitates the curing reaction of a thermosetting resin. Examples of curing agents when the thermosetting resin is an epoxy resin include phenolic resin curing agents, acid anhydride curing agents, amine curing agents, imidazole curing agents, and phosphine curing agents. The curing agent may contain one or more selected from phenolic resin curing agents, acid anhydride curing agents, amine curing agents, and imidazole curing agents, and may also contain an imidazole curing agent.

[0033] Phenolic resin curing agents are compounds having two or more phenolic hydroxyl groups, and examples include phenol novolac, cresol novolac, phenol aralkyl resin, cresol naphthol formaldehyde polycondensate, triphenylmethane type polyfunctional phenol, and other polyfunctional phenolic resins. These can be used individually or in combination of two or more. The equivalent ratio of the phenolic resin curing agent to the epoxy resin (phenolic hydroxyl group / epoxy group, molar ratio) may be 0.3 to 1.5, 0.4 to 1.0, or 0.5 to 1.0 from the viewpoint of good curability, adhesion, and storage stability.

[0034] Examples of acid anhydride-based curing agents include methylcyclohexanetetracarboxylic acid dianhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic acid dianhydride, and ethylene glycol bis-anhydrotrimellitate. These can be used individually or in combination of two or more. The equivalent ratio (acid anhydride group / epoxy group, molar ratio) of the acid anhydride-based curing agent to the epoxy resin may be 0.3 to 1.5, 0.4 to 1.0, or 0.5 to 1.0 from the viewpoint of good curability, adhesion, and storage stability.

[0035] Amine-based curing agents are compounds containing an amino group, and examples include dicyandiamide. The equivalent ratio of the amine-based curing agent to the epoxy resin (amine / epoxy group, molar ratio) may be 0.3 to 1.5, 0.4 to 1.0, or 0.5 to 1.0 from the viewpoint of good curability, adhesion, and storage stability.

[0036] The imidazole-based curing agent is an imidazole derivative. The content of the imidazole-based curing agent may be 0.1 to 20 parts by mass, 0.1 to 10 parts by mass, or 3.2 to 5.5 parts by mass per 100 parts by mass of epoxy resin.

[0037] Examples of phosphine-based curing agents include triphenylphosphine, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra(4-methylphenyl)borate, and tetraphenylphosphonium (4-fluorophenyl)borate.

[0038] The content of the phosphine-based curing agent may be 0.1 to 10 parts by mass, or 0.1 to 5 parts by mass, per 100 parts by mass of epoxy resin.

[0039] Polymeric components can contribute to the heat resistance and film-forming properties of thermosetting adhesives. Examples of polymeric components include phenoxy resins, polyimide resins, polyamide resins, polycarbodiimide resins, cyanate ester resins, acrylic resins, polyester resins, polyethylene resins, polyethersulfone resins, polyetherimide resins, polyvinyl acetal resins, urethane resins, and acrylic rubbers. The polymeric component may be a copolymer containing a substructure corresponding to a resin or rubber selected from these. From the viewpoint of heat resistance and film-forming properties, the polymeric component may include one or more selected from phenoxy resins, polyimide resins, acrylic rubbers, cyanate ester resins, and polycarbodiimide resins. The polymeric component may include one or more selected from phenoxy resins, polyimide resins, and acrylic rubbers. These polymeric components can be used individually or in combination of two or more. In this specification, the polymeric component is a component different from the thermosetting resin (e.g., epoxy resin) described above.

[0040] The glass transition temperature (Tg) of the polymer component may be 200°C or less, 50°C to 200°C, 50°C to 180°C, or 50°C to 150°C, from the viewpoint of the adhesiveness of the film-like thermosetting adhesive to the circuit member. When the Tg of the polymer component is 50°C or higher, the tack (viscosity) of the thermosetting adhesive tends to be moderately weakened. When the Tg of the polymer component is 200°C or lower, the thermosetting adhesive can easily fill in irregularities caused by connections in the circuit member, and as a result, the void suppression effect tends to be relatively greater. Here, Tg refers to the value measured using a DSC (DSC-Pyris1, manufactured by PerkinElmer Corporation) under conditions of a sample amount of 10 mg, a heating rate of 10°C / min, and an air atmosphere.

[0041] The weight-average molecular weight of the polymer component may be 30,000 or more, 40,000 or more, or 50,000 or more, or it may be 200,000 or less.

[0042] The ratio Ca / Cd (mass ratio) of the content Ca of the epoxy resin to the content Cd of the polymer component may be 0.01 to 5, 0.05 to 3, or 0.1 to 2. When the ratio Ca / Cd is 0.01 or more, better curability and adhesive strength are easily obtained. When the ratio Ca / Cd is 5 or less, better film formability is easily obtained.

[0043] The thermosetting adhesive may contain a fluxing agent. The fluxing agent can be, for example, a compound having a group represented by Formula (1). The fluxing agent may be a single type of the compound represented by Formula (1) alone, or a combination of two or more types thereof.

[0044]

[0045] In Formula (1), R 1 represents an electron-donating group. Examples of the electron-donating group include an alkyl group, a hydroxyl group, an amino group, an alkoxy group, and an alkylamino group. The electron-donating group may be an alkyl group, a hydroxyl group or an alkoxyl group, or may be an alkyl group.

[0046] R 1 may be an alkyl group having 1 to 10 carbon atoms, or 1 to 5 carbon atoms. The alkyl group may be linear or branched, or may be linear. When the alkyl group is linear, from the viewpoint of steric hindrance, the number of carbon atoms of the alkyl group may be equal to or less than the number of carbon atoms of the main chain containing the carboxylic acid.

[0047] R 1 may be an alkoxy group having 1 to 10 carbon atoms, or 1 to 5 carbon atoms. The alkyl moiety of the alkoxy group may be linear or branched, or may be linear. When the alkyl moiety of the alkoxy group is linear, from the viewpoint of steric hindrance, the number of carbon atoms thereof may be equal to or less than the number of carbon atoms of the main chain containing the carboxylic acid.

[0048] R 1The alkylamino group may be, for example, a monoalkylamino group or a dialkylamino group. The monoalkylamino group may have 1 to 10 or 1 to 5 carbon atoms. The alkyl portion of the monoalkylamino group may be linear or branched, or it may be linear. The dialkylamino group may have 1 to 20 or 1 to 10 carbon atoms. The alkyl portion of the dialkylamino group may be linear or branched, or it may be linear.

[0049] The fluxing agent may be a compound having two carboxyl groups (dicarboxylic acid). Compared to a compound having one carboxyl group (monocarboxylic acid), a compound having two carboxyl groups is less likely to volatilize even at high temperatures during connection, and can further suppress the generation of voids. Compared to using a compound having three or more carboxyl groups, a compound having two carboxyl groups can further suppress the increase in viscosity of the adhesive during storage and connection work. As a result, the connection reliability of semiconductor devices can be further improved.

[0050] The fluxing agent may include a compound in which an electron-donating group is substituted at the 2-position of a dicarboxylic acid selected from succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanediic acid, and dodecanediic acid.

[0051] The flux content may be 0.5 to 10% by mass, or 0.5 to 5% by mass, based on the mass of the thermosetting adhesive, or the total mass of components other than the solvent in the thermosetting adhesive.

[0052] The thermosetting adhesive may further contain a filler. The filler may be an inorganic filler, an organic filler, or a combination thereof.

[0053] Examples of inorganic fillers include glass, silica, alumina, titanium oxide, carbon black, mica, and boron nitride. The inorganic filler may be silica, alumina, titanium oxide, and boron nitride, or one or more selected from silica, alumina, and boron nitride. The filler may also be a whisker, examples of which include aluminum borate, aluminum titanate, zinc oxide, calcium silicate, magnesium sulfate, and boron nitride.

[0054] The organic filler may also be a resin filler, and examples include particles containing a resin selected from polyurethane, polyimide, methyl methacrylate resin, and methyl methacrylate-butadiene-styrene copolymer resin (MBS).

[0055] The filler content may be 30 to 90% by mass, 30 to 80% by mass, or 30 to 50% by mass, based on the mass of the thermosetting adhesive or the total mass of components other than the solvent in the thermosetting adhesive.

[0056] The thermosetting adhesive may further contain other components such as ion trappers, antioxidants, silane coupling agents, titanium coupling agents, and leveling agents. These may be used individually or in combination of two or more.

[0057] The thermosetting adhesive may further contain a solvent that dissolves or disperses each component. A film-type thermosetting adhesive can be manufactured by applying a thermosetting adhesive (resin varnish) containing a solvent to a substrate film and drying the coating.

[0058] [Examples] The present invention is not limited to the following examples. 1. Raw materials (a) Epoxy resins - Polyfunctional solid epoxy resin with triphenolmethane skeleton (EP1032H60, manufactured by Mitsubishi Chemical Corporation, weight-average molecular weight: 800-2000) - Bisphenol F type liquid epoxy resin (YL983U, manufactured by Mitsubishi Chemical Corporation, molecular weight: approximately 336) - Flexible semi-solid epoxy resin (YX7110B80, manufactured by Mitsubishi Chemical Corporation, weight-average molecular weight: 1000-5000) (b) Curing agent - 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanurate adduct (2MAOK-PW, manufactured by Shikoku Chemicals, Inc.) (c) Polymer component - Phenoxy resin (FX-293, manufactured by Nippon Steel Chemical & Material Co., Ltd., Tg: approximately 160℃, weight-average molecular weight: 40000-50000) (d) Fluxant: Glutaric acid (manufactured by Tokyo Chemical Industry Co., Ltd., melting point: approx. 98°C) (e) Fillers: Inorganic fillers - Silica fillers (SE2030, manufactured by Admatex Co., Ltd., average particle size: 500 nm) - Epoxysilane surface-treated silica fillers (SE2030-SEJ, manufactured by Admatex Co., Ltd., average particle size: approx. 500 nm) - Methacrylic surface-treated nanosilica fillers (YA050C-HGF, manufactured by Admatex Co., Ltd., average particle size: approx. 50 nm) Organic fillers - Resin fillers (EXL-2655, manufactured by Dow Chemical Japan Ltd., core-shell type organic microparticles)

[0059] 2. Two types of thermosetting adhesive films, A and B (20 μm thick), were prepared by applying a resin varnish containing each raw material of the thermosetting adhesive film in the ratio (parts by mass) shown in Table 1 to a base film and drying the coating film.

[0060]

[0061] 3. Connecting Circuit Components The following circuit components for connection testing were prepared: First circuit component: A sectional evaluation semiconductor chip (thickness: 50 μm) having a circuit surface (main surface) including a connection terminal consisting of a Cu pillar (height 30 μm) and a Sn alloy bump (height 15 μm). Second circuit component: A semiconductor wafer (thickness: 100 μm) having a circuit surface (main surface) including a connection terminal containing an electroless Ni / Au plating layer.

[0062] Examples 1-3 The first layer of adhesive film (adhesive film A or B) was placed on the circuit surface of the first circuit member. Next, the adhesive film was bonded to the first circuit member by heating and pressurizing it using a vacuum laminator (Nikko Materials Co., Ltd., V-130) having a diaphragm and a stage. As a result, the first layer of adhesive film was provided on the first circuit member as a base adhesive layer.

[0063] Next, the second adhesive film (adhesive film A or B) was placed on the first adhesive film, and the second adhesive film was bonded to the first adhesive film (base adhesive layer) by heating and pressurizing it using a vacuum laminator (Nikko Materials Co., Ltd., V-130) having a diaphragm and a stage. An adhesive laminate consisting of the base adhesive layer and the second adhesive film (additional adhesive layer) was formed on the circuit surface of the first circuit member.

[0064] In the vacuum lamination of the first and second adhesive films, either condition 1 or 2 below was applied. Condition 1: Diaphragm temperature: 70°C, Stage temperature: 50°C, Pressure: 0.2 MPa, Time: 60 seconds Condition 2: Diaphragm temperature: 90°C, Stage temperature: 60°C, Pressure: 0.5 MPa, Time: 120 seconds

[0065] Multiple adhesive-coated first circuit members, each having an adhesive laminate, were placed on the circuit surface of a second circuit member using a flip-chip bonder, aligning them so that their connection terminals faced each other, thereby forming an intermediate laminate consisting of multiple first circuit members, an adhesive laminate, and a second circuit member. Subsequently, the intermediate laminate was heated and pressurized using the flip-chip bonder to obtain a connector having an insulating resin layer formed by the thermosetting of the adhesive laminate. The intermediate laminate was heated using the flip-chip bonder while being pressurized at a pressure of 20 N in the following order: 100°C for 1 second, 200°C for 5 seconds, 260°C for 5 seconds, and 100°C for 1 second.

[0066] Comparative Examples 1 and 2 Two adhesive films A or two adhesive films B were bonded together in a roll laminator at 80°C to obtain an adhesive film laminate. The adhesive film laminate was placed on the circuit surface of the first circuit member. Next, the adhesive film laminate was bonded to the first circuit member by heating and pressurizing the adhesive film using a vacuum laminator (Nikko Materials Co., Ltd., V-130) having a diaphragm and a stage. As a result, the adhesive laminate was formed on the circuit surface of the first circuit member. Condition 1 described above was applied to the vacuum lamination of the adhesive film laminate. Otherwise, a connector was obtained using the same procedure as in Examples 1 to 3.

[0067] 4. Evaluation The voided joints were observed using a scanning acoustic microscope (SAM) on an ultrasonic diagnostic device. Based on the area percentage of voids confirmed within the insulating resin layer, the void state of the joints was evaluated according to the following criteria: A: Approximately 0-5% B: Approximately 5-20% C: 20% or more

[0068] The vicinity of the end of the first circuit member of the fillet connector was observed with a digital microscope, and the width of the insulating resin layer (fillet) protruding from the end of the first circuit member was measured. Based on the maximum width of the fillet, the condition of the fillet was evaluated according to the following criteria: 7: 80–110 μm, 6: 111–140 μm, 5: 141–170 μm, 4: 171–200 μm, 3: 201–230 μm, 2: 231–260 μm, 1: 261–290 μm

[0069] Connectivity was checked for multiple first circuit components using a digital multimeter to confirm continuity with the second circuit component. Connectivity was evaluated based on the percentage of first circuit components that showed normal continuity, according to the following criteria: A: 76-100% B: 51-76% C: 26-50% D: 0-25%

[0070] 5. Results Table 2 shows the type of adhesive film, vacuum lamination conditions, and evaluation results of the connected body for each example or comparative example. It was confirmed that under the conditions of the example in which the adhesive laminate was formed by laminating the adhesive film twice, fillets could be reduced while maintaining a small number of voids and good connectivity.

[0071]

[0072] 10...First circuit component (individually separated), 10W...First circuit component, 11...First substrate (individually separated), 11W...First substrate, 12...First connection terminal, 12a...Metal pillar, 12b...Bump, 20...Second circuit component, 21...Second substrate, 22...Second connection terminal, 30...Insulating resin layer, 30A...Adhesive laminate, 30F...Fillet, 31...Base adhesive layer, 32...Additional adhesive layer, 50A...Intermediate laminate, 50...Semiconductor package (connector), 70...Pressing member, 71...Pressing member, D...Dicing line.

Claims

1. To prepare a first circuit member having a first substrate and a first connection terminal provided on the main surface of the first substrate; to provide a thermosetting base adhesive layer on the main surface; to provide one or more thermosetting additional adhesive layers on the base adhesive layer in a manner that causes the temperature of the base adhesive layer to rise, thereby forming an adhesive laminate including the base adhesive layer and the additional adhesive layers on the main surface of the first substrate; to prepare a second circuit member having a second substrate and a second connection terminal provided on the main surface of the second substrate; to form an intermediate laminate having the first circuit member, the adhesive laminate and the second circuit member, with the first connection terminal and the second connection terminal facing each other, and the adhesive laminate interposed between the first circuit member and the second circuit member; and to form a connector having the first circuit member, an insulating resin layer formed by the thermosetting of the adhesive laminate and the second circuit member, with the first connection terminal and the second connection terminal electrically connected, by heating and pressurizing the intermediate laminate. A method for manufacturing electronic component devices, including [a specific component].

2. The method according to claim 1, wherein providing one or more of the additional adhesive layers on the base adhesive layer includes bonding a thermosetting adhesive film to the base adhesive layer while heating the adhesive film.

3. The method according to claim 2, wherein the adhesive film is bonded to the substrate adhesive layer by vacuum lamination while the adhesive film is heated.

4. The method according to claim 2, wherein the adhesive film is bonded to the substrate adhesive layer while heating the adhesive film to a temperature lower than the temperature at which the adhesive film exhibits its lowest melt viscosity.

5. The method according to claim 1, further comprising heating the base adhesive layer provided on the main surface of the first substrate before the additional adhesive layer is provided on the base adhesive layer.

6. The method according to claim 1, further comprising dividing the first substrate together with the adhesive laminate to form a plurality of individualized first circuit members having individualized first substrates and adhesive laminates, wherein the first substrate before being individualized is a semiconductor wafer, and the intermediate laminate having the individualized first circuit members, the adhesive laminate and the second circuit member is formed.