Refined wax and refining method therefor
The method addresses the issues of odor and crystalline precipitation in refined waxes by using separation aids, surfactants, and adsorbents, resulting in a purer, more stable product suitable for diverse applications.
Patent Information
- Application Number
- PCT/JP2026/017998
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-12
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional methods for refining natural waxes, such as rice bran wax, result in products with strong odors and crystalline precipitation, limiting their application in food, cosmetics, and pharmaceuticals due to the use of decolorizing agents and high crystalline properties.
A method involving the use of separation aids, surfactants, inorganic adsorbents, and organic adsorbents, followed by filtration and deodorization under reduced pressure, to purify wax components.
The method achieves decolorized and deodorized wax with significantly reduced odor and color, enhancing its suitability for various applications by minimizing crystalline precipitation.
Smart Images

Figure JP2026017998_19112026_PF_FP_ABST
Abstract
Description
Refined wax and method for refining it
[0001] The present invention relates to wax refined from natural wax materials and a method for refining the same, and more particularly to decolorized and deodorized refined wax and a method for refining the same.
[0002] Natural waxes are widely used in cosmetics and other products. However, waxes refined using conventional methods often involve the use of decolorizing agents in the manufacturing process, which could be improved from the perspective of reducing environmental impact.
[0003] Patent Document 1 discloses a method for decolorizing rice bran wax using activated carbon.
[0004] Japanese Patent Publication No. 2024-125137
[0005] However, the rice bran wax obtained by the method described in Patent Document 1 had a strong odor, making it difficult to apply to food, cosmetics, and pharmaceuticals.
[0006] Furthermore, because rice bran wax has high crystalline properties, crystals tend to precipitate during formulation, which can adversely affect the appearance and stability of the preparation, and this has been one of the reasons why its range of application has been limited.
[0007] To solve these problems, the inventors of the present invention succeeded in solving the above problems by using separation aids, surfactants, inorganic adsorbents, and organic adsorbents in the process of refining wax from natural wax materials, and thus the present invention was completed.
[0008] [1] The object of the present invention is to provide a method for purifying wax, comprising: an acquisition step of acquiring wax components by adding at least a separation aid to molten natural wax material; an adsorption decolorization step of adding an inorganic adsorbent and an organic adsorbent to the acquired wax components; a filtration step of filtering the wax components to remove the inorganic adsorbent and organic adsorbent from the wax components; and a deodorization step of blowing water vapor onto the wax components under reduced pressure conditions.
[0009] The purification method according to the present invention can purify wax that is more decolorized and deodorized than wax purified by conventional purification methods.
[0010] [2] In the wax purification method described in [1], the separation aid may be an acidic solution.
[0011] [3] In the wax purification method described in [2], the acidic solution may be at least one selected from the group consisting of oxalic acid, citric acid, hydrochloric acid, nitric acid, sulfuric acid, and acetic acid.
[0012] [4] In the wax purification method described in [3], the acidic solution may be oxalic acid or citric acid, and the concentration of the oxalic acid may be 0.03 to 0.3 mol / L.
[0013] [5] In the wax purification method described in any of [1] to [4], the amount of the separation aid added may be equal to or greater than the amount of the natural wax material.
[0014] [6] In the wax purification method described in any of [1] to [5], the acquisition step may include a first acquisition step of adding the separation aid to the molten natural wax material, and a second acquisition step of further adding a surfactant to the molten natural wax material.
[0015] [7] In the wax purification method described in [6], the surfactant may be at least one selected from the group consisting of anionic surfactants, cationic surfactants, ionic surfactants, nonionic surfactants, surfactants having an acetylene bond in their structure, silicone surfactants, and fluorine surfactants.
[0016] [8] In the wax purification method described in [7], the surfactant may be a nonionic surfactant.
[0017] [9] In the wax purification method described in [8], the nonionic surfactant may be at least one selected from the group consisting of ether-type nonionic surfactants, ether ester-type nonionic surfactants, ester-type nonionic surfactants, and nitrogen-containing nonionic surfactants.
[0018] In the wax purification method described in
[10] and [9], the nonionic surfactant may be an ether-type nonionic surfactant.
[0019]
[11] In the wax purification method described in
[10] , the ether-type nonionic surfactant may be polyoxyalkylene glycol.
[0020]
[12] In the wax purification method described in [6] to
[11] , the amount of surfactant added may be 0.01 to 0.1 parts by mass per 100 parts by mass of natural wax material.
[0021]
[13] In the wax purification method described in any of [1] to
[12] , the inorganic adsorbent may be at least one selected from the group consisting of zeolite, talc, activated alumina, bentonite, acid clay, activated clay, semi-activated clay, weakly acid-treated clay, stevensite, silica-magnesia composite, and magnesium silicate.
[0022]
[14] In the wax purification method described in
[13] , the inorganic adsorbent may be activated clay.
[0023]
[15] In the wax purification method described in any of [1] to
[14] , the amount of inorganic adsorbent added may be 1 to 100 parts by mass per 100 parts by mass of wax component.
[0024]
[16] In the wax purification method described in any of [1] to
[15] , the organic adsorbent may be activated carbon and / or bone char.
[0025]
[17] In the wax purification method described in
[16] , the organic adsorbent may be activated carbon.
[0026]
[18] In the wax purification method described in any of [1] to
[17] , the amount of organic adsorbent added may be 0.5 to 10 parts by mass per 100 parts by mass of wax component.
[0027]
[19] In the wax purification method described in any of [1] to
[18] , the above reduced pressure conditions may be 0.03 to 0.1 atmospheres.
[0028]
[20] In the wax refining method described in any of [1] to
[19] , the natural wax material may be a natural wax material of biological origin.
[0029]
[21] In the wax refining method described in
[20] , the biologically derived natural wax material may be a plant and / or animal-derived natural wax material.
[0030]
[22] In the wax refining method described in
[21] , the above-mentioned natural wax material derived from plants may be at least one selected from the group consisting of rice bran wax, Japanese wax, sugarcane wax, carnauba wax, candelilla wax, jojoba wax, castor wax, soy wax, lacquer wax, sunflower wax, and rapeseed wax.
[0031]
[23] In the wax refining method described in
[21] , the above-mentioned natural wax material of animal origin may be at least one selected from the group consisting of beeswax, lanolin, shellac, privet wax, snow wax, and whale wax.
[0032]
[24] Another object of the present invention is to provide a refined wax with a lower color tone and / or fewer odor components compared to natural wax materials.
[0033] The refined wax according to the present invention is more decolorized and deodorized than wax refined by conventional refining methods.
[0034]
[25] In the refined wax described in
[24] , the above color tone of the refined wax may be 40% to 95% lower than that of the above natural wax material.
[0035]
[26] In the refined wax described in
[24] or
[25] , the concentration of the odor component in the refined wax may be 20% to 99% lower than that of the natural wax material.
[0036]
[27] In the refined wax described in
[26] , the odor component may be an unpleasant odor.
[0037]
[28] In the purified wax described in
[27] , the odor component may be at least one selected from the group consisting of octanoic acid (caprylic acid), octanal, hexanoic acid, undecanal, 2-decenal, 2-undecenal, (E)-2-octenal, 1-octanol, nonanal, (E)-2-nonenal, decanal, ethyl palmitate, (E)-9-octadecenoic acid ethyl, anisaldehyde, and 4-hydroxybenzaldehyde.
[0038] Figure 1(A) shows a graph relating to the hardness of rice bran wax according to this embodiment, using diisostearyl malate as the oil. Figure 1(B) shows a graph relating to the hardness of rice bran wax according to this embodiment, using polyglyceryl-2 triisostearate as the oil. Figure 2(A) shows a photograph relating to the color of rice bran wax and its raw materials according to this embodiment. Figure 2(B) shows a photograph relating to the thermal stability test of rice bran wax according to this embodiment. Figure 3(A) shows a graph relating to the odor (caprylic acid) of rice bran wax according to this embodiment. Figure 3(B) shows a graph relating to the odor (octanal) of rice bran wax according to this embodiment. Figure 3(C) shows a graph relating to the odor (hexanoic acid) of rice bran wax according to this embodiment. Figure 4 shows a graph relating to the differential scanning calorimetry (DSC) analysis of rice bran wax according to this embodiment. Figure 5 shows a graph of the odor ((E)-2-octenal) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 6 shows a graph of the odor (1-octanol) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 7 shows a graph of the odor (nonanal) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 8 shows a graph of the odor ((E)-2-nonenal) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 9 shows a graph of the odor (decanal) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 10 shows a graph of the odor (ethyl palmitate) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 11 shows a graph relating to the odor ((E)-9-octadecenoic acid ethyl) of rice bran wax and unwashed rice bran wax according to this embodiment. Figure 12 shows a photograph relating to the color of the refined beeswax and its raw material according to this embodiment. Figure 13(A) shows a graph relating to the odor (octanoic acid) of the refined beeswax according to this embodiment. Figure 13(B) shows a graph relating to the odor (undecanal) of the refined beeswax according to this embodiment. Figure 14(A) shows a graph relating to the odor (2-decenal) of the refined beeswax according to this embodiment.FIG. 14(B) shows a graph relating to the odor (2-undecenal) of purified beeswax according to the present embodiment. FIG. 15 shows photographs relating to the color tone of purified sumac wax (produced in Nagasaki) according to the present embodiment and its raw material. FIG. 16 shows a graph relating to the odor (octanoic acid) of purified sumac wax (produced in Nagasaki) according to the present embodiment. FIG. 17 shows a graph relating to the odor (1-octanol) of purified sumac wax (produced in Nagasaki) according to the present embodiment. FIG. 18 shows a graph relating to the odor (nonanal) of purified sumac wax (produced in Nagasaki) according to the present embodiment. FIG. 19 shows photographs relating to the color tone of purified sumac wax (produced in China) according to the present embodiment and its raw material. FIG. 20(A) shows a graph relating to the odor (hexanoic acid) of purified sumac wax (produced in China) according to the present embodiment. FIG. 20(B) shows a graph relating to the odor (octanoic acid) of purified sumac wax (produced in China) according to the present embodiment. FIG. 21 shows a graph relating to the odor (anisaldehyde) of purified carnauba wax according to the present embodiment. FIG. 22 shows a graph relating to the odor (4-hydroxybenzaldehyde) of purified carnauba wax according to the present embodiment.
[0039] For convenience of definition, specific terms used in the present application are collected herein. Unless otherwise specified, all technical and scientific terms used in the present application have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention pertains. Unless otherwise clearly specified in the context, the singular forms "a", "an" and "the" include plural references.
[0040] The numerical ranges and parameters indicated in the present invention are approximate values, but the numerical values shown in specific examples are described as accurately as possible. However, any numerical value essentially includes certain errors inevitably arising from the standard deviation found in their respective test measurements. In addition, the term "about" as used in the present specification generally means within 10%, 5%, 1% or 0.5% of a given value or range. Alternatively, the term "about" means being within an acceptable standard error as considered by a person of ordinary skill in the art.
[0041] Hereinafter, embodiments of the present invention will be described. The following embodiments are illustrative, and the scope of the present invention is not limited to those shown in the following embodiments. Note that descriptions of similar contents will be omitted as appropriate to avoid redundant complexity.
[0042] 1. Wax Purification Method The wax purification method according to the present embodiment includes an acquisition step, an adsorptive decolorization step, a filtration step, and a deodorization step. In the wax purification method according to the present embodiment, each step is carried out under a temperature condition of 95°C to 105°C, and optionally over 105°C as needed, in order to maintain the natural wax material and the wax component in a molten state.
[0043] The natural wax material according to the present embodiment is a biologically derived natural wax material. The natural wax material may be a crudely purified natural wax material, or may be a natural wax material purified by a purification method other than the wax purification method according to the present embodiment. In some embodiments, the natural wax material is a natural wax material of plant and / or animal origin. Examples of plant-derived natural wax materials include, but are not limited to, rice bran wax, Japan wax, sugarcane wax, carnauba wax, candelilla wax, jojoba wax, castor wax, soy wax, sumac wax, sunflower wax, and rapeseed wax. Examples of animal-derived natural wax materials include, but are not limited to, beeswax, lanolin, shellac, Chinese wax, snow wax, and spermaceti.
[0044] 1-1. Acquisition Step In the acquisition step, at least a separation auxiliary agent is added to the molten natural wax material to obtain a wax component. Impurities can be removed from the natural wax material by the separation auxiliary agent to obtain the wax component. The wax component according to the present embodiment refers to the natural wax material from which impurities have been removed. The impurities include moisture and precipitates (for example, starchy matter). Since the impurities separate into the lower layer, the wax component can be obtained by removing the lower layer.
[0045] In one embodiment, the acquisition step includes a first acquisition step of adding a separation aid to the molten natural wax material, and a second acquisition step of further adding a surfactant to the molten natural wax material. The first and second acquisition steps are carried out with stirring. In one embodiment, the second acquisition step is carried out after the first acquisition step. In another embodiment, the first acquisition step is carried out after the second acquisition step. In yet another embodiment, in one embodiment, the first and second acquisition steps are carried out simultaneously. If necessary, a stirring step of a certain time (e.g., 0.5 to 2 hours) may be carried out after the first and / or second acquisition steps.
[0046] In one embodiment, the acquisition step includes a third acquisition step in which a separation aid or a natural wax material containing a separation aid and a surfactant is allowed to stand for (for example, 2 hours) until it separates into impurities and wax components. In another embodiment, the acquisition step includes a fourth acquisition step in which impurities are removed to obtain the wax components.
[0047] In one embodiment, the acquisition process includes a first acquisition process, a second acquisition process, a third acquisition process, and a fourth acquisition process.
[0048] Separation aid In one embodiment, the separation aid is an acidic solution. In one embodiment, the acidic solution is at least one selected from the group consisting of oxalic acid, citric acid, hydrochloric acid, nitric acid, sulfuric acid, and acetic acid. In another embodiment, the acidic solution is oxalic acid. In one embodiment, the concentration of oxalic acid is a specific concentration that facilitates the separation of wax components and impurities from the natural wax material. In one embodiment, the concentration of oxalic acid is 0.03 to 0.3 mol / L (for example, any binary range selected from the group consisting of 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, and 0.3 mol / L). In one embodiment, the amount of separation aid added (particularly oxalic acid at a specific concentration) is equal to or greater than the amount of the natural wax material. In one embodiment, the amount of separation aid (particularly oxalic acid at a specific concentration) added is equivalent to ±10%, ±9%, ±8%, ±7%, ±6%, ±5%, ±4%, ±3%, ±2%, or ±1% of the amount of the natural wax material.
[0049] In one embodiment, the separation aid is heated (for example, to a temperature of 80°C to 90°C) to maintain the natural wax material in a molten state.
[0050] In one embodiment, the surfactant is at least one selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, surfactants having an acetylene bond in their structure, silicone surfactants, and fluorine surfactants. In another embodiment, the surfactant is a nonionic surfactant.
[0051] In one embodiment, the nonionic surfactant is at least one selected from the group consisting of ether-type nonionic surfactants, ether-ester-type nonionic surfactants, ester-type nonionic surfactants, and nitrogen-containing nonionic surfactants. In another embodiment, the nonionic surfactant is an ether-type nonionic surfactant.
[0052] In one embodiment, the ether-type nonionic surfactant is a polyoxyalkylene alkyl ether such as polyoxyethylene polyoxypropylene alkyl ether, polyoxyethylene polyoxypropylene aryl ether, polyoxyethylene polyoxypropylene alkylaryl ether, polyoxyethylene alkyl ether, polyoxyethylene aryl ether, polyoxyethylene alkylaryl ether, and polyoxyethylene tristyrylphenyl ether; polyoxyalkylene aryl ether; polyoxyalkylene alkylaryl ether; polyoxyalkylene glycol such as polyoxyethylene polyoxypropylene glycol; or aliphatic alcohol polyglycol ether.
[0053] In one embodiment, the ether ester-type nonionic surfactant is a polyoxyalkylene sorbitan fatty acid ester such as polyoxyethylene sorbitan monolaurate, polyoxyethylene tristyrylphenyl phosphate diester, polyoxyethylene polyoxypropylene tristyrylphenyl phosphate diester, polyoxyethylene fatty acid ester, or a fatty acid ester of polyoxyethylene polyoxypropylene block polymer.
[0054] In one embodiment, the ester-type nonionic surfactant is a polyoxyalkylene vegetable oil such as polyoxyethylene castor oil; a polyoxyalkylene hydrogenated vegetable oil such as polyoxyethylene hydrogenated castor oil; a polyoxyethylene polyoxypropylene vegetable oil such as polyoxyethylene polyoxypropylene castor oil; a sorbitan fatty acid ester such as sorbitan monostearate and sorbitan tristearate; or a glycerin fatty acid ester.
[0055] In some embodiments, the nitrogen-containing nonionic surfactant is a polyoxyethylene fatty acid amide or a polyoxyethylene alkylamine.
[0056] In some embodiments, the ether-type nonionic surfactant is a polyoxyalkylene glycol. In some embodiments, the polyoxyalkylene glycol is a polyoxyethylene polyoxypropylene glycol. In some embodiments, the polyoxyethylene polyoxypropylene glycol is a polyoxyethylene polyoxypropylene block polymer. In some embodiments, it is a polyoxyethylene polyoxypropylene (EOPO) block polymer. It is the EOPO block polymer represented by Formula (1). HO(CH 2 CH 2 O) x (CH(CH 3 )CH 2 O) y (CH 2 CH 2 O) z H (1) In the formula, x, y, and z are positive numbers.
[0057] In some embodiments, the mass average molecular weight of the EOPO block polymer represented by the above formula (1) is 1000 to 20000 (for example, a range between any two values selected from the group consisting of 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 11000, 12000, 13000, 14000, 15000, 16000, 17000, 18000, 19000 and 20000).
[0058] In some embodiments, the number (x+z) of oxyethylene (CH 2 CH 2 O) groups in formula (1) is 20 to 300 (for example, a range between any two values selected from the group consisting of 20, 40, 60, 80, 100, 120, 140, 160, 180, 200, 220, 240, 260, 280 and 300), and the oxypropylene (CH(CH 3 )CH 2O) The number of bases (y) is between 30 and 65 (for example, any binary range selected from the group consisting of 30, 35, 40, 45, 50, 55, 60, and 65).
[0059] In one embodiment, the oxyethylene group content in the EOPO block polymer represented by formula (1), relative to the total number of oxyalkylene groups, is 5 to 60% (a range between any two values selected from the group consisting of 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, and 60%).
[0060] In one embodiment, the amount of surfactant added is 0.01 to 0.1 parts by mass per 100 parts by mass of natural wax material (for example, any binary range selected from the group consisting of 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 and 0.1 parts by mass).
[0061] In one embodiment, the surfactant is heated (for example, to a temperature of 80°C to 90°C) to maintain the natural wax material in a molten state.
[0062] 1-2. Adsorption Decolorization Process In the adsorption decolorization process, an inorganic adsorbent and an organic adsorbent are added to the acquired wax component. In one embodiment, the inorganic adsorbent is at least one selected from the group consisting of zeolite, talc, activated alumina, bentonite, acid clay, activated clay, semi-activated clay, weakly acid-treated clay, stivunsite, silica-magnesia composite, and magnesium silicate. In another embodiment, the inorganic adsorbent is activated clay. In one embodiment, the organic adsorbent is activated carbon and / or bone char. In one embodiment, the adsorption decolorization process is carried out with stirring (for example, for 1 to 2 hours).
[0063] In one embodiment, the adsorption decolorization step includes a first adsorption decolorization step of adding an inorganic adsorbent to the wax component and a second adsorption decolorization step of adding an organic adsorbent to the wax component. The first and second adsorption decolorization steps are carried out with stirring. In one embodiment, the second adsorption decolorization step is carried out after the first adsorption decolorization step. In another embodiment, the first adsorption decolorization step is carried out after the second adsorption decolorization step. If necessary, a stirring step of a certain time (e.g., 0.5 to 2 hours) may be carried out after the first adsorption decolorization step and / or the second adsorption decolorization step.
[0064] In one embodiment, the amount of inorganic adsorbent added is 1 to 100 parts by mass per 100 parts by mass of wax component (for example, a range between any two values selected from the group consisting of 1, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, and 100 parts by mass). In one embodiment, the amount of organic adsorbent added is 0.5 to 10 parts by mass per 100 parts by mass of wax component (for example, a range between any two values selected from the group consisting of 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, and 10 parts by mass).
[0065] 1-3. Filtration Process In the filtration process, the wax component is filtered to remove the inorganic adsorbent and organic adsorbent from the wax component. The filtration means is not particularly limited as long as it is a filter capable of sufficiently capturing fine particles of the inorganic adsorbent and organic adsorbent, but examples include multilayer filtration filters and cartridge-type precision filters, and a pressurized filtration device or a vacuum filtration device may also be used in combination. If the fluidity of the wax component is low and filtration is difficult, the filtration process may be carried out under temperature conditions of 110 to 120°C.
[0066] 1-4. Deodorization Process In the deodorization process, water vapor is blown into the wax component under reduced pressure conditions. By blowing water vapor into the wax component in a reaction vessel maintained under reduced pressure, odor components contained in the wax, especially low-molecular-weight volatile organic compounds, vaporize with the water vapor and are separated from the wax. The blown-in water vapor must be in sufficient contact with the heated wax component, and for this purpose, it is preferable to use a reaction vessel equipped with a stirring device or a device that uniformly disperses the water vapor (e.g., a sparging tube). In one embodiment, the reduced pressure conditions are 0.03 to 0.1 atmospheres (for example, any binary range selected from the group consisting of 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 and 0.1 atmospheres).
[0067] The refined wax, after undergoing the deodorization process, may be molded into granules, blocks, pellets, or flakes as needed.
[0068] 1-5. Other Processes: Melting Process The wax purification method according to this embodiment may include a melting process in which a natural wax material is melted at a melting temperature before the acquisition process.
[0069] The wax purification method according to this embodiment may include a washing step after the filtration step and / or the deodorization step, in which a separation aid and a surfactant are added to the molten wax components to wash the wax components.
[0070] In one embodiment, the separation aid and the surfactant are added simultaneously.
[0071] In one embodiment, the washing step includes a first washing step of adding a separation aid to the molten wax component and a second washing step of adding a surfactant to the molten wax component. The first and second washing steps are carried out with stirring. In one embodiment, the second washing step is carried out after the first washing step. In another embodiment, the first washing step is carried out after the second washing step. If necessary, a stirring step of a certain time (e.g., 0.5 to 2 hours) may be carried out after the first and / or second washing steps.
[0072] In one embodiment, the washing step includes a third washing step in which the wax component containing a separation aid and a surfactant is allowed to stand for (for example, 2 hours) until impurities are separated from it. In another embodiment, the washing step includes a fourth washing step in which impurities are removed to obtain the wax component.
[0073] If the amount of impurities in the wax component during the washing process is small or is expected to be small, a centrifuge (e.g., 3000 rpm) may be used to separate the impurities during the washing process (fourth washing process).
[0074] In one embodiment, the cleaning process includes a first cleaning process, a second cleaning process, a third cleaning process, and a fourth cleaning process.
[0075] Antioxidation Step The wax purification method according to this embodiment may include an antioxidant step in which an antioxidant is added to the molten wax component after the deodorization step, or after the washing step if there is a washing step after the deodorization step.
[0076] In one embodiment, the antioxidant is at least one selected from the group consisting of tocopherol, ascorbic acid and its derivatives (such as ascorbic acid palmitate), rosemary extract, citric acid, and green tea extract (such as catechins).
[0077] 2. Refined Wax The refined wax according to this embodiment has a lower color tone and / or fewer odor components compared to natural wax materials.
[0078] The color tone of the refined wax according to this embodiment is 40% to 95% lower (for example, within a range of any binary value selected from the group consisting of 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, and 95%) compared to natural wax material. The color tone can be measured by the Gardner method.
[0079] The concentration of odor components in refined wax is 40% to 98% lower (for example, between any two values selected from the group consisting of 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, and 98%) compared to natural wax material. The odor components in this embodiment are unpleasant odors. In one embodiment, the odor component is at least one selected from the group consisting of octanoic acid (caprylic acid), octanal, hexanoic acid, undecanal, 2-decenal, 2-undecenal, (E)-2-octenal, 1-octanol, nonanal, (E)-2-nonenal, decanal, ethyl palmitate, (E)-9-octadecenoic acid ethyl, anisaldehyde, and 4-hydroxybenzaldehyde.
[0080] In one embodiment, when the refined wax is rice bran wax, the odor component is at least one selected from the group consisting of octanoic acid (caprylic acid), octanal, hexanoic acid, (E)-2-octenal, 1-octanol, nonanal, (E)-2-nonenal, decanal, ethyl palmitate, and (E)-9-octadecenoic acid ethyl. In one embodiment, when the refined wax is rice bran wax, the concentration of octanoic acid (caprylic acid) is 65% to 85% lower (e.g., any binary range selected from the group consisting of 65, 70, 75, 80, and 85%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of octanal is 50% to 70% lower (e.g., any binary range selected from the group consisting of 50, 55, 60, 65, and 70%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of hexanoic acid is 45% to 65% lower (e.g., any binary range selected from the group consisting of 45%, 50%, 55%, 60%, and 65%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of (E)-2-octenal is 25% to 45% lower (e.g., any binary range selected from the group consisting of 25%, 30%, 35%, 40%, and 45%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of 1-octanol is 40% to 60% lower (e.g., any binary range selected from the group consisting of 40%, 45%, 50%, 55%, and 60%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of nonanal is 30% to 50% lower (e.g., a range between any two values selected from the group consisting of 30, 35, 40, 45, and 50%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of (E)-2-nonenal is 45% to 65% lower (e.g., a range between any two values selected from the group consisting of 45, 50, 55, 60, and 65%) compared to natural rice bran wax material.In one embodiment, when the refined wax is rice bran wax, the concentration of decanal is 35% to 55% lower (e.g., any binary range selected from the group consisting of 35, 40, 45, 50, and 55%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of ethyl palmitate is 30% to 50% lower (e.g., any binary range selected from the group consisting of 30, 35, 40, 45, and 50%) compared to natural rice bran wax material. In one embodiment, when the refined wax is rice bran wax, the concentration of ethyl (E)-9-octadecenoate is 25% to 45% lower (e.g., any binary range selected from the group consisting of 25, 30, 35, 40, and 45%) compared to natural rice bran wax material.
[0081] In one embodiment, when the refined wax is beeswax, the odor component is at least one selected from the group consisting of octanoic acid (caprylic acid), 2-decenal, undecanal, and 2-undecenal. In one embodiment, when the refined wax is beeswax, the concentration of octanoic acid (caprylic acid) is 70% to 90% lower (for example, in any binary range selected from the group consisting of 70, 75, 80, 85, and 90%) compared to natural beeswax material. In one embodiment, when the refined wax is beeswax, the concentration of undecanal is 70% to 90% lower (for example, in any binary range selected from the group consisting of 70, 75, 80, 85, and 90%) compared to natural beeswax material. In one embodiment, when the refined wax is beeswax, the concentration of 2-decenal is 70% to 90% lower (e.g., a range between any two values selected from the group consisting of 70, 75, 80, 85, and 90%) compared to natural beeswax material. In another embodiment, when the refined wax is beeswax, the concentration of 2-undecenal is 70% to 90% lower (e.g., a range between any two values selected from the group consisting of 70, 75, 80, 85, and 90%) compared to natural beeswax material.
[0082] In one embodiment, when the refined wax is Japanese wax, the odor component is at least one selected from (i) the group consisting of octanoic acid (caprylic acid), hexanoic acid, 1-octanol, and nonanal, (ii) the group consisting of octanoic acid (caprylic acid), 1-octanol, and nonanal, or (iii) the group consisting of octanoic acid (caprylic acid) and hexanoic acid. In one embodiment, when the refined wax is Japanese wax, the concentration of octanoic acid (caprylic acid) is 65% to 99% lower (e.g., a range between any two values selected from the group consisting of 65, 70, 75, 80, 85, 90, 95, 98, and 99%) compared to natural Japanese wax material (e.g., 85% to 99% and 65% to 85%). In one embodiment, when the refined wax is made from Japanese wax, the concentration of 1-octanol is 20% to 40% lower (e.g., any binary range selected from the group consisting of 20%, 25%, 30%, 35%, and 40%) compared to natural Japanese wax material. In one embodiment, when the refined wax is made from Japanese wax, the concentration of nonanal is 25% to 45% lower (e.g., any binary range selected from the group consisting of 25%, 30%, 35%, 40%, and 45%) compared to natural Japanese wax material. In one embodiment, when the refined wax is made from Japanese wax, the concentration of hexanoic acid is 50% to 70% lower (e.g., any binary range selected from the group consisting of 50%, 55%, 60%, 65%, and 70%) compared to natural Japanese wax material.
[0083] In one embodiment, when the refined wax is carnauba wax, the odor component is at least one selected from the group consisting of anisaldehyde and 4-hydroxybenzaldehyde. In one embodiment, when the refined wax is carnauba wax, the concentration of anisaldehyde is 60% to 80% lower (e.g., in any binary range selected from the group consisting of 60, 65, 70, 75, and 80%) compared to natural carnauba wax material. In one embodiment, when the refined wax is carnauba wax, the concentration of 4-hydroxybenzaldehyde is 50% to 70% lower (e.g., in any binary range selected from the group consisting of 50, 55, 60, 65, and 70%) compared to natural carnauba wax material.
[0084] In one embodiment, the purified wax is purified by the wax purification method described above.
[0085] In one embodiment, the hardness of a mixture of 1 part by mass of refined wax and 9 parts by mass of oil is between 1N and 5N (for example, a range between any two values selected from the group consisting of 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, and 5N). The oil in this embodiment is diisostearyl malate and / or polyglyceryl-2 triisostearate.
[0086] 3. Compositions containing refined wax The composition according to this embodiment contains the refined wax described above. In one embodiment, the composition containing refined wax is a cosmetic composition. In one embodiment, the composition containing refined wax is a food composition. In one embodiment, the composition containing refined wax is a pharmaceutical composition.
[0087] In one embodiment, the composition contains 1 to 20 w / w% of refined wax (for example, any binary range selected from the group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 and 20 w / w%). In one embodiment, the composition contains more than 20 w / w% of refined wax.
[0088] The composition according to this embodiment may also contain a wide range of other optional ingredients, such as oils (e.g., polyglyceryl-2 triisostearate, triethylhexanoin, or diisostearyl malate, castor oil), antioxidants, binders, biological additives, buffers, colorants, thickeners, polymers, astringents, fragrances, humectants, emulsions, conditioners, peeling agents, pH adjusters, preservatives, natural extracts, essential oils, skin sensates, skin soothing agents, and skin healing agents.
[0089] 1. Experimental Example 1: Purification Process of Crude Rice Bran Wax Step 1: Dissolution Process 500 kg of crude rice bran wax (Lightol (product name), Sanwa Oil & Fat Co., Ltd.) was placed in a dissolution vessel (Dissolution Vessel B) and the temperature was raised to 105°C to dissolve it from a solid to a liquid.
[0090] Step 2: Acquisition Process After confirming that the crude rice bran wax had completely liquefied, an aqueous solution prepared by adding 1% oxalic acid (Nitto Chemical Industry Co., Ltd.) as a separation aid to an equivalent amount of hot water was added to the crude rice bran wax and heated and stirred. After heating to 102°C, 0.2 kg of polyoxyethylene polyoxypropylene (EOPO) block polymer (product name: Epan 785 (average molecular weight: 13333, cloud point: 100°C or higher), Daiichi Kogyo Seiyaku Co., Ltd.) was added and stirred for 1 hour. After stirring for 1 hour, stirring was stopped and the mixture was allowed to stand for 2 hours to separate the wax component from the water. After standing for 2 hours, the stopcock was opened from the bottom of the dissolution vessel (Dissolution Vessel B) to discharge the water and precipitated impurities (sediment), leaving the wax component in the dissolution vessel (Dissolution Vessel B).
[0091] Step 3: Adsorption and Decolorization Process The wax components remaining in the dissolution kettle (Dissolution Kettle B) were heated to 100°C while being stirred. While stirring, 50 kg of activated clay (product name: Galleon Earth V2R, Mizusawa Chemical Industry Co., Ltd.) was gradually added to the wax components as an adsorbent. Thirty minutes after adding and stirring the activated clay, 20 kg of activated carbon (product name: Carboraffin-6, Osaka Gas Chemical Co., Ltd.) was gradually added to the wax components and stirred. After adding the activated clay and activated carbon, the temperature was raised to 110°C while stirring to evenly distribute the adsorbent. After confirming that the temperature had reached 110°C, stirring was continued at 110°C for two hours.
[0092] Step 4: Filtration Step After adsorption and decolorization, the wax components were filtered using a filter press (manufactured by Lion Corporation) at 110°C to remove activated clay and activated carbon from the wax components.
[0093] Step 5: Washing Process An aqueous solution prepared by adding 2% oxalic acid as a separation aid to an amount of water equivalent to the amount of wax component was added to the wax component and heated and stirred. After heating to 102°C, 0.2 kg of EOPO block polymer was added and stirred for 1 hour. After stirring for 1 hour, stirring was stopped and the mixture was allowed to stand for 2 hours to separate the wax component from the water. After standing for 2 hours, the stopcock was opened from the bottom of the dissolution vessel (dissolution vessel B) to discharge the water and precipitated impurities (sediment), leaving the wax component in the dissolution vessel (dissolution vessel B). The obtained wax component was heated to 100°C while stirring. After reaching 100°C, trace amounts of water contained in the wax component were removed while stirring for 30 minutes. After water removal, the wax component was centrifuged at 3000 rpm using a high-speed centrifuge (Sharpless from Tomoe Engineering) to further remove water from the wax component.
[0094] Step 6: Deodorization Step The centrifuged wax components were placed in a deodorizing kettle, and the wax components were maintained at 110°C and under reduced pressure (0.07 atm) for 2 hours while water vapor was blown into them. The same washing step as in Step 5 was performed on the purified wax that had been treated under reduced pressure to obtain the washed wax components (hereinafter referred to as rice bran wax (Example 1)).
[0095] Process 7: Molding Process The molten rice bran wax was allowed to fall naturally from the top of a steel tower approximately 15 meters high, like rain, and solidified into round granules by air cooling, thereby obtaining granular rice bran wax.
[0096] Analysis Experiment 1: Hardness Measurement The hardness of granulated rice bran wax (Example 1) was analyzed. A sample (oil:wax = 31.5g:3.5g = 9:1) was melted at 90°C, the melted sample was rapidly cooled and solidified, and the hardness was measured using the solidified sample left at 25°C for one day. Diisostearyl malate or polyglyceryl-2 triisostearate was used as the oil. A TEXTURE PROFILE UNIT (manufacturer: Yamaden Co., Ltd.) and a 2.8 mm diameter plunger were used to measure the hardness. The plunger was pressed against the solidified sample at a speed of 10 mm / sec at 25°C, and the breaking load when the plunger penetrated the solidified sample was measured. Five breaking loads were measured, and the average of the three breaking loads excluding the maximum and minimum values was taken as the hardness. As a comparative example, rice wax No. Comparative Examples 1 (rice bran wax produced by a different method than in Example 1, Comparative Example 1), Rice Wax Classic X (hydrogenated rice bran wax, Comparative Example 2), and Rice Wax Classic Y (unhydrogenated rice bran wax, Comparative Example 3) were used. Comparative Example 1 differs from Example 1 in that it does not perform the acquisition step (step 2), adsorption decolorization step (step 3), filtration step (step 4), and deodorization step (step 6). Comparative Examples 2 and 3 also differ from Example 1 in that they do not perform the acquisition step (step 2), adsorption decolorization step (step 3), and filtration step (step 4) (Table 1). The results are shown in Figures 1A and 1B.
[0097]
[0098] It was revealed that Example 1, which was mixed with an oil, maintained a high hardness compared to any of the comparative examples.
[0099] Experiment 2: Thermal Stability Test. The color tone of Example 1 was examined using the Gardner method. The color tone of the refined wax and the raw material (comparison) was examined in the molten state. Example 1 improved from a color tone of 12 to a color tone of 6 compared to the raw material (crude rice bran wax, Comparative Example 4) (50% reduction, Figure 2(A)). Comparative Example 3 only improved to a color tone of 7 (not shown). Next, Example 1 and Comparative Example 3 were maintained at a temperature of 150°C and photographed over time. The results are shown in Figure 2(B). While Example 1 showed no change from a color tone of 6 compared to the raw material, the color tone of Comparative Example 3 gradually deteriorated.
[0100] Experiment 3: Odor Analysis The odor components of Example 1 and Comparative Example 3 were investigated. The odor components were measured using GC-MS (Agilent). Table 2 shows the names and characteristics of the odor components investigated.
[0101]
[0102] The results are shown in Figures 3(A) to (C). Compared to Comparative Example 3, Example 1 was able to reduce all odor components (caprylic acid: approximately 75% reduction, octanal: approximately 60% reduction, hexanoic acid: approximately 55% reduction).
[0103] Experiment 4: Physical Property Analysis The physical properties of Example 1 and Comparative Example 3 were analyzed. The physical properties analyzed were acid value, saponification value, iodine value, melting point, and peroxide value (POV). The acid value was analyzed according to the standard oil and fat analysis method 2.3.1-96, the saponification value was analyzed according to the standard oil and fat analysis method 2.3.2.2-96, the iodine value was analyzed according to the standard oil and fat analysis method 2.3.4.1-96, the melting point was analyzed according to the standard oil and fat analysis method 2.2.4.2-96, and the peroxide value was analyzed according to the standard oil and fat analysis method 2.5.2.1-2003. The results are shown in Table 3.
[0104]
[0105] The saponification value of Example 1 was lower than that of Comparative Example 3. A lower saponification value indicates higher purity of the wax ester, which is the main component, and therefore higher purity of the rice bran wax. Thus, it became clear that Example 1 contained fewer impurities than Comparative Example 3.
[0106] Furthermore, no peroxide value was detected in Example 1. Therefore, compared to Comparative Example 3, Example 1 has higher quality, is less prone to degradation, lasts longer, and is more stable and safe when incorporated into products.
[0107] Experiment 5: Differential Scanning Calorimeter (DSC) Analysis Differential scanning calorimeter (DSC) analysis was performed on Example 1 and Comparative Example 3. The results are shown in Figure 4. The DSC analysis showed that the peak width of Example 1 was wider than that of Comparative Example 3, and the melting point of Example 1 was higher than that of Comparative Example 3. Therefore, since the crystallinity of Example 1 is weaker than that of Comparative Example 3, Example 1 can suppress the precipitation of rice bran wax-derived crystals during formulation.
[0108] Experiment 6: Effect on odor components with or without the washing step (step 5) In the purification process of Example 1, the acquisition step (step 2) and the washing step (step 5) were omitted to obtain purified rice bran wax (unwashed rice bran wax: Comparative Example 4-1).
[0109] The odor components of Example 1 and Comparative Example 4-1 were investigated. The odor components were measured using GC-MS (Agilent). Table 4 shows the names and characteristics of the investigated odor components.
[0110]
[0111] The results are shown in Figures 5 to 11. Compared to Comparative Example 4-1, Example 1 was able to reduce all odor components ((E)-2-octenal: approximately 35% reduction, 1-octanol: approximately 51% reduction, nonanal: approximately 41% reduction, (E)-2-nonenal: approximately 55% reduction, decanal: approximately 48% reduction, ethyl palmitate: approximately 39% reduction, (E)-9-octadecenoic acid ethyl: approximately 34% reduction).
[0112] 2. Experimental Example 2 The purification process for Experimental Example 2 of beeswax was the same as that for Experimental Example 1, except that beeswax (raw material, 500 kg), the absence of surfactants, and the amounts of activated clay and activated carbon added (5% (25 kg) and 2% (10 kg), respectively). Through this purification process, purified beeswax (Example 2) was obtained.
[0113] Analysis Experiment 1: Color Test The color of Example 2 was tested using the Gardner method (Figure 12). The color of the refined wax and raw material (comparison) was tested in the molten state. Example 2 showed improvement from a color tone of 9 to a color tone of 1 compared to the raw material (beeswax, Comparative Example 5) (a reduction of approximately 89%).
[0114] Experiment 2: Odor Analysis The odor components of Example 2 and Comparative Example 5 (raw materials) were investigated. The odor components were measured using GC-MS (Agilent). Table 5 shows the names and characteristics of the odor components investigated.
[0115]
[0116] The results are shown in Figures 13(A) and (B) and Figures 14(A) and (B). Compared to Comparative Example 5 (raw material), Example 2 was able to reduce all odor components (octanoic acid: approximately 82% reduction, undecanal: approximately 82% reduction, 2-decenal: approximately 80% reduction, 2-undecenal: approximately 82% reduction).
[0117] 3. Experimental Example 3 Purification of Japanese Wax (from Nagasaki) The purification process for Experimental Example 3 was the same as that for Experimental Example 1, except that Japanese wax (raw material, from Nagasaki, 500 kg), no surfactant was used, the amount of activated carbon added was 6% (30 kg), and 0.3 g of antioxidant (tocopherol 100) was added before the molding process. Purified Japanese wax (Example 3) was obtained through this purification process.
[0118] Analysis Experiment 1: Color Test The color of Example 3 was tested using the Gardner method (Figure 15). The color of the refined wax and raw material (comparison) was tested in the molten state. Example 3 showed improvement from a color tone of 11 to a color tone of 4 compared to the raw material (Japanese wax, Comparative Example 6) (a reduction of approximately 64%).
[0119] Experiment 2: Odor Analysis The odor components of Example 3 and Comparative Example 6 (raw materials) were investigated. The odor components were measured using GC-MS (Agilent). Table 6 shows the names and characteristics of the odor components investigated.
[0120]
[0121] The results are shown in Figures 16, 17, and 18. Compared to Comparative Example 6 (raw material), Example 3 was able to reduce the odor components octanoic acid, 1-octanol, and nonanal (by approximately 98%, 32%, and 35%, respectively).
[0122] 4. Experimental Example 4 Purification of Japanese Wax (from China) The purification process in Experimental Example 4 was the same as that in Experimental Example 3, except that Japanese wax (raw material, from China, 500 kg) was used. Purified Japanese wax (Example 4) was obtained through this purification process.
[0123] Analysis Experiment 1: Color Test The color of Example 4 was tested using the Gardner method (Figure 19). The color of the refined wax and the raw material (comparison) was tested in the molten state. Example 4 showed improvement from a color tone of 10 to a color tone of 2 compared to the raw material (Japanese wax, Comparative Example 7) (80% reduction).
[0124] Experiment 2: Odor Analysis The odor components of Example 4 and Comparative Example 7 (raw materials) were investigated. The odor components were measured using GC-MS (Agilent). Table 7 shows the names and characteristics of the odor components investigated.
[0125]
[0126] The results are shown in Figures 20(A) and (B). Compared to Comparative Example 7 (raw material), Example 4 was able to reduce all odor components (octanoic acid: approximately 75% reduction, hexanoic acid: approximately 60% reduction).
[0127] 5. Experimental Example 5 Purification of Carnauba Wax The purification process in Experimental Example 5 was the same as that in Experimental Example 1, except for the use of carnauba wax (raw material, 500 kg) and steps 2, 5, and 7. In the molding process corresponding to step 7 of Experimental Example 1, the melted wax was attached to a rotating drum, cooled, and then peeled off in thin flakes. Through this purification process, purified carnauba wax (Example 5) was obtained.
[0128] Analysis Experiment 2: Odor Analysis The odor components of Example 5 and Comparative Example 8 (conventional product (NC-1810, Cerarica NODA Co., Ltd.)) were investigated. The odor components were measured using GC-MS (Agilent). Table 8 shows the names and characteristics of the odor components investigated.
[0129]
[0130] The results are shown in Figures 21 and 22. Compared to Comparative Example 8 (conventional product), Example 5 was able to reduce all odor components (anisaldehyde: approximately 70% reduction, 4-hydroxybenzaldehyde: approximately 62% reduction).
[0131] The rice bran wax according to the present invention is less discolored and has reduced odor components compared to conventional products, making it suitable for use as an additive in food, cosmetics, and pharmaceuticals.
Claims
1. A method for refining wax, comprising: an acquisition step of obtaining wax components by adding at least a separation aid to molten natural wax material; an adsorption decolorization step of adding an inorganic adsorbent and an organic adsorbent to the acquired wax components; a filtration step of filtering the wax components to remove the inorganic adsorbent and organic adsorbent from the wax components; and a deodorization step of blowing water vapor onto the wax components under reduced pressure conditions.
2. The wax purification method according to claim 1, wherein the separation aid is an acidic solution.
3. The wax purification method according to claim 2, wherein the acidic solution is at least one selected from the group consisting of oxalic acid, citric acid, hydrochloric acid, nitric acid, sulfuric acid, and acetic acid.
4. The wax purification method according to claim 3, wherein the acidic solution is oxalic acid or citric acid, and the concentration of the oxalic acid is 0.03 to 0.3 mol / L.
5. The wax purification method according to claim 1, wherein the amount of the separation aid added is equal to or greater than the amount of the natural wax material.
6. The wax purification method according to claim 1, wherein the acquisition step comprises: a first acquisition step of adding the separation aid to the molten natural wax material; and a second acquisition step of further adding a surfactant to the molten natural wax material.
7. The wax purification method according to claim 6, wherein the surfactant is at least one selected from the group consisting of anionic surfactants, cationic surfactants, ionic surfactants, nonionic surfactants, surfactants having an acetylene bond in their structure, silicone surfactants, and fluorine surfactants.
8. The wax purification method according to claim 7, wherein the surfactant is a nonionic surfactant.
9. The wax purification method according to claim 8, wherein the nonionic surfactant is at least one selected from the group consisting of ether-type nonionic surfactants, ether ester-type nonionic surfactants, ester-type nonionic surfactants, and nitrogen-containing nonionic surfactants.
10. The wax purification method according to claim 9, wherein the nonionic surfactant is an ether-type nonionic surfactant.
11. The wax purification method according to claim 10, wherein the ether-type nonionic surfactant is polyoxyalkylene glycol.
12. The wax purification method according to claim 6, wherein the amount of surfactant added is 0.01 to 0.1 parts by mass per 100 parts by mass of natural wax material.
13. The wax purification method according to claim 1, wherein the inorganic adsorbent is at least one selected from the group consisting of zeolite, talc, activated alumina, bentonite, acid clay, activated clay, semi-activated clay, weakly acid-treated clay, stivunsite, silica-magnesia composite, and magnesium silicate.
14. The wax purification method according to claim 13, wherein the inorganic adsorbent is activated clay.
15. The wax purification method according to claim 1, wherein the amount of inorganic adsorbent added is 1 to 100 parts by mass per 100 parts by mass of wax component.
16. The wax purification method according to claim 1, wherein the organic adsorbent is activated carbon and / or bone char.
17. The wax purification method according to claim 16, wherein the organic adsorbent is activated carbon.
18. The wax purification method according to claim 1, wherein the amount of organic adsorbent added is 0.5 to 10 parts by mass per 100 parts by mass of wax component.
19. The wax purification method according to claim 1, wherein the reduced pressure condition is 0.03 to 0.1 atmospheres.
20. The wax refining method according to any one of claims 1 to 19, wherein the natural wax material is a natural wax material of biological origin.
21. The method for refining wax according to claim 20, wherein the biologically derived natural wax material is a plant and / or animal-derived natural wax material.
22. The wax purification method according to claim 21, wherein the plant-derived natural wax material is at least one selected from the group consisting of rice bran wax, Japanese wax, sugarcane wax, carnauba wax, candelilla wax, jojoba wax, castor wax, soy wax, lacquer wax, sunflower wax, and rapeseed wax.
23. The wax purification method according to claim 21, wherein the natural wax material of animal origin is at least one selected from the group consisting of beeswax, lanolin, shellac, privet wax, snow wax, and whale wax.
24. Refined wax with lower color tone and / or lower odor components compared to natural wax materials.
25. The refined wax according to claim 24, wherein the color tone of the refined wax is 40% to 95% lower than that of the natural wax material.
26. The refined wax according to claim 24 or 25, wherein the concentration of the odor component in the refined wax is 20% to 99% lower than that in the natural wax material.
27. The refined wax according to claim 26, wherein the odor component is an unpleasant odor.
28. The purified wax according to claim 27, wherein the odor component is at least one selected from the group consisting of octanoic acid (caprylic acid), octanal, hexanoic acid, undecanal, 2-decenal, 2-undecenal, (E)-2-octenal, 1-octanol, nonanal, (E)-2-nonenal, decanal, ethyl palmitate, (E)-9-octadecenoic acid ethyl, anisaldehyde, and 4-hydroxybenzaldehyde.