Polymer electrolyte composition for lithium-ion secondary battery, polymer electrolyte for lithium-ion secondary battery, electrode mixture layer, electrode, and lithium-ion secondary battery

WO2026240112A1PCT designated stage Publication Date: 2026-11-19OSAKA SODA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/018009
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-12
Filing Date
2026-05-12
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

In the prior art, the electrode materials of solid-state lithium-ion batteries have insufficient strength and conductivity due to volume expansion and contraction during charging and discharging, and are prone to short circuits under high compression conditions. Especially in vehicle applications, the existing solid electrolyte layer is prone to cracking and is difficult to arrange precisely, resulting in a decline in electrical performance.

Method used

A polymer electrolyte composition comprising conductive polymers, conductive compounds, and nanofibers is used to form an electrolyte with high compressive strength and high lithium-ion conductivity through cross-linking, which adapts to volume changes in electrode materials and suppresses short circuits caused by lithium dendrite formation.

Benefits of technology

This technology enables the battery to adapt to volume changes in electrode materials during charging and discharging, improving the battery's compressibility and lithium-ion conductivity, suppressing internal short circuits caused by lithium dendrites, and enhancing battery safety and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

This polymer electrolyte composition for a lithium-ion secondary battery contains at least an ion conductive polymer, an ion conductive compound, and nanofibers. The polymer electrolyte composition can adapt to volume expansion and contraction of an active material during charge and discharge, has compression resistance under a high confining pressure, and further has high lithium ion conductivity. Therefore, the polymer electrolyte composition has an effect of suppressing the generation or growth of dendrites generated by the localization of lithium ions.
Need to check novelty before this filing date? Find Prior Art

Description

Polymer electrolyte composition for lithium-ion secondary batteries, polymer electrolyte for lithium-ion secondary batteries, electrode mixture layer, electrode, and lithium-ion secondary battery

[0001] The present invention relates to a polymer electrolyte composition for lithium-ion secondary batteries, a polymer electrolyte for lithium-ion secondary batteries, an electrode mixture layer, an electrode, and a lithium-ion secondary battery.

[0002] Among all-solid-state batteries, all-solid-state lithium-ion batteries are attracting attention because they have a high energy density due to the use of battery reactions involving the movement of lithium ions, and because they use a solid electrolyte instead of an electrolyte containing an organic solvent as the electrolyte between the positive and negative electrodes. Compared to liquid-system batteries that have an electrolyte containing a flammable organic solvent, they have the advantage of being easier to simplify safety devices.

[0003] Patent No. 7044673 Patent No. 7567108

[0004] In the electrodes of such all-solid-state batteries, PVDF (polyvinylidene fluoride) has conventionally been widely used as a binder for the electrode active material (see Patent Document 1). However, conventional binders do not provide sufficient flexibility and strength against the volume expansion and contraction of the electrode active material due to charging and discharging, resulting in problems such as reduced battery capacity and, due to the poor ionic conductivity of the binder itself, the inability to achieve sufficiently excellent charge-discharge characteristics in the case of secondary batteries.

[0005] Furthermore, when inorganic solid batteries are installed in vehicles such as automobiles, they are manufactured under high constraining pressure to prevent cracking of the inorganic solid electrolyte layer due to vibration and shock. For example, an invention has been proposed for a crack-resistant solid electrolyte layer, which is made of a sintered body of a masonry formed by stacking a plurality of plate-shaped particles made of an ion-conducting material in the thickness direction of the plate-shaped particles and arranging them along the direction in which the plates of the plate-shaped particles spread, characterized in that the ratio of the length to the width of the plate-shaped particles is 1 to 3:1 and the ratio of the width to the thickness is 1.3 to 4:1 (see Patent Document 2). However, while stacking ion-conducting plate-shaped particles (inorganic solid electrolyte) makes them less prone to cracking, it is difficult to arrange them precisely, and gaps are created, raising concerns about a decrease in electrical performance due to internal short circuits in the dendrites.

[0006] In response to the above-mentioned challenges, conventional technologies have used polyether polymers primarily composed of polyethylene oxide (PEO) structures as binders or polymer electrolytes. However, the inventors' research has revealed that conventional polyether polymers have room for improvement in terms of their ability to adapt to the volume expansion and contraction of the active material during charging and discharging, and their low compressive resistance under high confinement pressure. Lithium ion conductivity is a property that can be determined by the product of ionic conductivity and lithium ion transport fraction. In this field, many inventions generally aim to improve ionic conductivity, so the focus on ionic transport fraction, which is a contradictory property to ionic conductivity, and furthermore, the focus on the properties calculated from that ionic transport fraction, is a novel approach.

[0007] The present invention aims to provide a polymer electrolyte composition for lithium-ion secondary batteries, a polymer electrolyte for lithium-ion secondary batteries, an electrode mixture layer, an electrode, and a lithium-ion secondary battery, which can adapt to the volume expansion and contraction of the active material during charging and discharging, have compressive resistance under high confinement pressure, and further have high lithium-ion conductivity.

[0008] As a result of various studies to achieve the above objective, the inventors of the present invention have found that a polymer electrolyte composition for lithium-ion secondary batteries containing at least an ion-conducting polymer, an ion-conducting compound, and nanofibers can adapt to the volume expansion and contraction of the active material during charging and discharging, has high compressive resistance under high confinement pressure, high lithium-ion conductivity, and is also excellent in suppressing internal short circuits caused by dendrites, thus completing the present invention.

[0009] The embodiments of the present invention are as follows: Item 1 A polymer electrolyte composition for lithium-ion secondary batteries comprising at least an ion-conducting polymer, an ion-conducting compound, and nanofibers, wherein the compressive strain when crosslinked is -90% to -30%, and the ratio of compressive strain to set compression ([set compression] / [compressive strain]) is -0.5 to -0.001. Item 2 The polymer electrolyte composition for lithium-ion secondary batteries according to Item 1, wherein the ion-conducting polymer comprises at least a polyether polymer containing alkyl group units which are constituent units derived from alkylene oxides having alkyl groups in their side chains, and a lithium salt compound, wherein the polyether polymer contains alkyl group-containing units in a content of 5 mol% or more per 100 mol% of constituent units. Item 3 A polymer electrolyte composition for lithium-ion secondary batteries according to Item 1 or 2, wherein the polyether polymer comprises an X unit which is a constituent unit derived from an alkylene oxide represented by the following general formula (1) and a Z unit which is a constituent unit derived from an alkylene oxide represented by the following general formula (2). [Chemical Formula 1] [In the formula, R 1 These are alkyl groups having 1 to 6 carbon atoms, either identical or different. 2 These are identical or different hydrogen atoms or -CH 2 O { (CH 2 ) a O} b (CH 2 ) cis an alkylene glycol alkyl ether group represented by H. a, which is the number of repeating units, is the same or different and is an integer of 1 to 10; b, which is the number of repeating units, is the same or different and is an integer of 1 to 6; c, which is the number of repeating units, is the same or different and is an integer of 0 to 6. A is the same or different and is a single bond or an alkylene group having 1 to 4 carbon atoms.] [Chemical Formula 2] [wherein, R 3 is the same or different and is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, R 5 is the same or different and is a crosslinking group containing an ethylenically unsaturated double bond represented by -CH 2 OR 8 . R 8 is the same or different and is an acryl group, a methacryl group, an allyl group or a methallyl group. A is the same or different and is a single bond or an alkylene group having 1 to 4 carbon atoms.] Item 4. The polymer electrolyte composition for lithium ion secondary batteries according to any one of Items 1 to 3, wherein the ion conductive compound is at least one compound selected from the group consisting of heterocyclic compounds represented by the following general formulas (A) to (C) and ether-based compounds represented by the following general formulas (D) to (E). [Chemical Formula 3] [wherein, R 9 is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, R 10 is a hydrogen atom, -CH 2 O{(CH 2 ) a O} b (CH 2 ) c H, an alkylene glycol alkyl ether group represented by the above, or a crosslinking group containing an ethylenically unsaturated double bond represented by -CH 2 OR 8 . R 8 is an acryl group, a methacryl group, an allyl group or a methallyl group. a, which is the number of repeating units, is an integer of 1 to 10, and b, which is the number of repeating units, is an integer of 0 to 6. c, which is the number of repeating units, is an integer of 0 to 4.] [Chemical Formula 4] [wherein, R 11[Chemical Formula 5] is the same or different hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkenyl group, and g is an integer from 0 to 4. [In the formula, R 12 [Chemical Formula 6] is the same or different hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkenyl group, and h is an integer from 0 to 8. (In the formula, R 13 These are identical or different alkyl groups having 1 to 4 carbon atoms, or -(CH 2 ) k CH 2 O-R 14 It is a group represented by R. 14 (The elements are the same or different alkyl groups having 1 to 4 carbon atoms. The repeating numbers i and j are the same or different, and range from 0 to 3, while k is an integer from 1 to 3.) [Chemical Formula 7] (In the formula, R 15 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or -{(CH 2 ) m CH 2 O} n R 17 That is. R 16 These are identical or different alkyl groups having 1 to 4 carbon atoms, or -{(CH 2 ) m CH 2 O} n R 17 That is. R 17(The elements are the same or different alkyl groups having 1 to 4 carbon atoms. The number of repetitions, k, is 0 or 1, and m and n are the same or different integers from 1 to 3.) Item 5 A polymer electrolyte composition for lithium-ion secondary batteries according to any one of items 1 to 4, wherein the nanofibers are cellulose nanofibers. Item 6 A polymer electrolyte composition for lithium-ion secondary batteries according to any one of items 1 to 5, wherein the content of the ion-conducting compound is 50 to 1200 parts by mass and the content of the nanofibers is 0.5 to 20 parts by mass per 100 parts by mass of the polyether polymer. Item 7 A polymer electrolyte composition for lithium-ion secondary batteries according to any one of items 1 to 6, further comprising a reaction initiator and a crosslinking aid. Item 8 A polymer electrolyte for lithium-ion secondary batteries obtained by crosslinking the polymer electrolyte composition for lithium-ion secondary batteries according to item 7. That is, the polymer electrolyte for lithium-ion secondary batteries described in item 8 is a crosslinked product of the polymer electrolyte composition for lithium-ion secondary batteries described in item 7, wherein the compressive strain of the crosslinked product is -90% to -30%, and the ratio of compressive strain to set compression ([set compression] / [compressive strain]) is -0.5 to -0.001. Item 9 An electrode mixture layer comprising at least the polymer electrolyte for lithium-ion secondary batteries described in item 8 and an active material, wherein the content of the polymer electrolyte for lithium-ion secondary batteries is 0.1 to 70% by mass in 100% by mass of the electrode mixture layer. Item 10 The electrode mixture layer according to item 9, wherein the active material is a silicon-based compound. Item 11 An electrode comprising at least the electrode mixture layer and a current collector described in item 9 or 10. Item 12 A lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, wherein one or both of the positive and negative electrodes are electrodes described in item 11. Item 13 A lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, wherein the solid electrolyte layer comprises at least the polymer electrolyte for lithium-ion secondary batteries described in Item 8. Item 14 The lithium-ion secondary battery according to Item 13, wherein the solid electrolyte layer further comprises an inorganic solid electrolyte, and the polymer electrolyte for lithium-ion secondary batteries is present in an amount of 0.1 to 90% by mass of 100% by mass of the solid electrolyte layer.Item 15 A lithium-ion secondary battery according to Item 14, wherein the inorganic solid electrolyte is a sulfide-based solid electrolyte. Item 16 A lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, wherein the solid electrolyte layer is a solid electrolyte layer containing at least an inorganic solid electrolyte, and a polymer electrolyte for lithium-ion secondary batteries according to Item 8 is laminated on one or both sides of the solid electrolyte layer.

[0010] The polymer electrolyte composition for lithium-ion secondary batteries of the present invention can adapt to the volume expansion and contraction of the active material during charging and discharging, and has compressive resistance under high confinement pressure. Furthermore, because it has high lithium-ion conductivity, it is also excellent at suppressing internal short circuits caused by dendrites.

[0011] <Polymer Electrolyte Composition for Lithium-Ion Secondary Batteries> The polymer electrolyte composition for lithium-ion secondary batteries of the present invention (also simply referred to as polymer electrolyte composition) comprises at least an ion-conducting polymer, an ion-conducting compound, and nanofibers. In this specification, the ion-conducting polymer means a mixture of a polyether polymer and a lithium salt compound, or a polyionic liquid.

[0012] In the present invention, the reason for obtaining the above effects is not clear, but it is presumed to be as follows: (Effect 1: Adaptation to volume expansion and contraction of the active material during charging and discharging, and compressive resistance under high confinement pressure) The steric hindrance effect of the ion-conducting polymer constituting the polymer electrolyte composition for lithium-ion secondary batteries reduces the crystallinity of the main chain. This results in a flexible polymer with high adaptability to volume expansion of the active material during charging and discharging. In addition, the ion-conducting compound functions as a plasticizer, further enhancing flexibility. On the other hand, the reinforcement effect of the nanofibers forming a dense network structure in the composition increases strength. Generally, it is known that reinforcement by nanofibers reduces flexibility, but especially when the ion-conducting polymer is a polyether polymer containing at least alkyl group units, which are constituent units derived from alkylene oxides having alkyl groups in their side chains, it is thought that by appropriately controlling the affinity with nanofibers through the effect of alkyl groups introduced into the side chains of the polyether polymer, a reinforcement effect is achieved while maintaining flexibility, resulting in adaptation to contraction of the active material and compressive resistance under high confinement pressure. (Effect 2: High lithium-ion conductivity) The steric hindrance effect of the ion-conducting polymer constituting the polymer electrolyte composition for lithium-ion secondary batteries effectively suppresses the coordination of lithium ions to the polymer, resulting in a higher ion transport rate (lithium-ion conductivity). The ion-conducting compound exhibits high ion conductivity (lithium-ion conductivity) because it has excellent solubility for lithium salt compounds, increasing the ion concentration in the electrolyte, and also exhibits excellent ion transport due to its low viscosity. Furthermore, when the polyether polymer is used, it is believed that the combination with the ion-conducting compound allows polar groups such as oxygen introduced into the polyether polymer and the ion-conducting compound to form a unique solvation structure with the lithium salt compound, optimizing the ion conduction pathway and resulting in high lithium-ion conductivity.(Effect 3: Suppression of internal short circuits due to dendrites) The polymer electrolyte composition for lithium-ion secondary batteries has the high lithium-ion conductivity described above, making it less likely to cause non-uniformity of lithium ion concentration, preventing localized increases in lithium ion concentration, and thus making it difficult for lithium dendrites to form. Even if lithium dendrites are formed, the dispersion of nucleation sites at multiple points within the composition is expected to suppress the crystal growth of lithium dendrites. Furthermore, it is thought that the dense network structure formed by the nanofibers within the composition prevents physical penetration of lithium dendrites even if they are formed, thereby suppressing short circuits.

[0013] Furthermore, the polymer electrolyte for lithium-ion secondary batteries obtained by crosslinking the polymer electrolyte composition for lithium-ion secondary batteries of the present invention possesses high ionic conductivity and high Li ion transportability (i.e., high lithium ion conductivity), and exhibits high compressibility. As a result, it has been shown that it prevents short circuits caused by dendrite-like deposited lithium generated during charge-discharge tests, and improves the number of charge-discharge cycles possible in dendrite resistance evaluation.

[0014] <<Ion-Conducting Polymers>> As mentioned above, ion-conducting polymers refer to mixtures of polyether polymers and lithium salt compounds, or polyionic liquids. These can be used individually or in combination of two or more. Among these, mixtures of polyether polymers and lithium salt compounds are preferred.

[0015] <<Polyether Polymers>> Polyether polymers are not particularly limited as long as they are polymers having ether bonds (-C-O-C-) in their main chain (excluding linear ether compounds represented by general formula (D) and branched ether compounds represented by general formula (E)).

[0016] The polyether polymer preferably contains at least alkyl group-containing units, which are structural units derived from alkylene oxides having alkyl groups in their side chains, and more preferably contains at least alkyl group-containing units, which are structural units derived from alkylene oxides having alkyl groups in their side chains, with an alkyl group-containing unit content of 5 mol% or more per 100 mol% of structural units (the polyether polymer of the present invention). Hereinafter, the polyether polymer of the present invention means a polymer that contains at least alkyl group-containing units, which are structural units derived from alkylene oxides having alkyl groups in their side chains, with an alkyl group-containing unit content of 5 mol% or more per 100 mol% of structural units.

[0017] Next, the polyether polymer of the present invention will be described. The polyether polymer of the present invention contains at least alkyl group-containing units, which are constituent units derived from alkylene oxides having alkyl groups in their side chains, and the content of alkyl group-containing units is 5 mol% or more out of 100 mol% of constituent units.

[0018] In this specification, the constituent units derived from alkylene oxide having an alkyl group in the side chain are not particularly limited as long as the constituent units derived from alkylene oxide have an alkyl group. Here, the side chain refers to a group attached to the main chain which is the alkylene oxide skeleton (for example, if it is unit X, which is a constituent unit derived from alkylene oxide shown in the general formula (1) below, then -C-C-A-O-), and means, for example, a methyl group, an ethyl group, an alkylene glycol alkyl ether group, etc.

[0019] The alkyl group-containing unit is not particularly limited as long as it is a constituent unit derived from an alkylene oxide having an alkyl group in its side chain, for example, among the X unit, Z unit, and Y unit described later, R 1 Examples include units in which the alkyl group has 1 to 6 carbon atoms. In particular, it is preferable that the constituent unit has an alkylene oxide having an alkyl group in the X unit described later.

[0020] In the polyether polymer of the present invention, each alkyl group-containing unit may be the same or different. Therefore, the polyether polymer of the present invention may be a polymer in which one or more units corresponding to alkyl group-containing units are combined. In the polyether polymer of the present invention, it is preferable that each unit in the alkyl group-containing unit is the same.

[0021] The polyether polymer of the present invention preferably contains X units, which are constituent units derived from alkylene oxides represented by the following general formula (1). That is, the polyether polymer of the present invention preferably contains X units as alkyl group-containing units. In the polyether polymer of the present invention, each X unit may be the same or different. Therefore, the polyether polymer of the present invention may be a polymer in which one or more units corresponding to X units are combined. In the polyether polymer of the present invention, each unit in the X unit is preferably the same. [Chemical Formula 8] [In the formula, R 1 These are alkyl groups having 1 to 6 carbon atoms, either identical or different. 2 These are identical or different hydrogen atoms or -CH 2 O { (CH 2 ) a O} b (CH 2 ) c This is an alkylene glycol alkyl ether group represented by H. The repeating unit a is an integer from 1 to 10, either the same or different; the repeating unit b is an integer from 1 to 6, either the same or different; and the repeating unit c is an integer from 0 to 6, either the same or different. A is either the same or different, a single bond or an alkylene group having 1 to 4 carbon atoms.

[0022] R in equation (1) 1 The alkyl group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, etc. Among these, methyl group and ethyl group are preferred.

[0023] R in equation (1) 2 of -CH 2 O { (CH 2 ) a O} b (CH 2 ) c The alkylene glycol alkyl ether group represented by H exhibits superior molecular mobility compared to the polymer backbone and maintains an appropriate distance between oxygen atoms, resulting in a tendency to achieve higher ion transportability (lithium ion conductivity). Furthermore, in terms of sulfide resistance, maintaining an appropriate distance between ether-oxygen atoms in the backbone and side chains is thought to mitigate coordination to lithium ions, thereby further suppressing reactions with sulfide-based solid electrolytes.

[0024] R in equation (1) 2 In this equation, a is an integer from 1 to 10, but preferably an integer from 1 to 9, more preferably an integer from 2 to 9, even more preferably an integer from 2 to 8, particularly preferably an integer from 2 to 7, most preferably an integer from 2 to 6, and most preferably an integer from 2 to 4. 2 In this equation, b is an integer from 1 to 6, preferably an integer from 1 to 4, more preferably an integer from 1 to 3, even more preferably an integer from 1 to 2, and particularly preferably 1. 2 In this, c is an integer from 0 to 6, preferably an integer from 0 to 4, more preferably an integer from 1 to 3, and even more preferably an integer from 1 to 2.

[0025] Examples of alkylene groups having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms, more preferably 1 to 2 carbon atoms, and even more preferably 1 carbon atom) in A of formula (1) include methylene groups, ethylene groups, and trimethylene groups. Among these, methylene groups and ethylene groups are preferred, and methylene groups are more preferred.

[0026] In formula (1), A is preferably a single bond, a methylene group, or an ethylene group, and more preferably a single bond or a methylene group.

[0027] Preferred embodiments of the X unit, which is a constituent unit derived from the alkylene oxide shown in formula (1), are shown below. Among these, the constituent units shown in formulas (1-1) to (1-5) are preferred, the constituent units shown in formulas (1-1), (1-2), (1-4), and (1-5) are more preferred, and the constituent units shown in formulas (1-1) and (1-5) are even more preferred. [Chemical Formula 9]

[0028] The polyether polymer of the present invention preferably contains Z units, which are constituent units derived from alkylene oxides represented by the following general formula (2), in addition to the X units. This makes it possible to enhance the mechanical properties of the polyether copolymer by crosslinking, and further, to introduce other functional groups to provide functionality. In the polyether polymer of the present invention, each Z unit may be the same or different. Therefore, the polyether polymer of the present invention may be a polymer in which one or more units corresponding to the X units and one or more units corresponding to the Z units are combined. In the polyether polymer of the present invention, it is preferable that each unit in the X units and each unit in the Z units are the same. [Chemical Formula 10] [In the formula, R 3 R is the same or different hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 5 They are the same or different, -CH 2 OR 8 This is a crosslinking group containing an ethylenically unsaturated double bond, represented by R. 8 A is either the same or different acrylic group, methacrylic group, allyl group, or metaallyl group. A is either the same or different single bond or alkylene group having 1 to 4 carbon atoms.

[0029] R in equation (2) 3 The alkyl group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, etc. Among these, methyl group and ethyl group are preferred.

[0030] R in equation (2)5 In R 8 The group is an acrylic group, a methacrylic group, an allyl group, or a methallyl group, but is preferably an acrylic group, a methacrylic group, or an allyl group, more preferably a methacrylic group or an allyl group, and even more preferably an allyl group.

[0031] A in formula (2) is the same as A in formula (1), including the preferred embodiment.

[0032] Preferred embodiments of the Z unit, which is a constituent unit derived from the alkylene oxide shown in formula (2), are shown below. Among these, the constituent units shown in formulas (2-1) to (2-4) are preferred, and the constituent units shown in formulas (2-1) and (2-3) are more preferred. [Chemical Formula 11]

[0033] The polyether polymer of the present invention preferably contains, in addition to the X units, Y units, which are constituent units derived from alkylene oxides represented by the following general formula (3). This tends to optimize the amount of X units in the polymer, enhance molecular mobility, and further increase ionic conductivity or lithium ion transportability. Furthermore, the polyether polymer of the present invention preferably contains, in addition to the X units and Z units, Y units, which are constituent units derived from alkylene oxides represented by the following general formula (3). This allows for a more favorable combination of the various functions of the X units, Z units, and Y units, provided they are constituent units that can be used in the present invention. In the polyether polymer of the present invention, each Y unit may be the same or different. Therefore, the polyether polymer of the present invention may be a polymer in which one or more units corresponding to X units and one or more units corresponding to Y units are combined. Furthermore, the polyether polymer of the present invention may be a polymer in which one or more units corresponding to X units, one or more units corresponding to Y units, and one or more units corresponding to Z units are combined. In the polyether polymer of the present invention, it is preferable that each unit in the X unit, each unit in the Y unit, and each unit in the Z unit are identical. [Chemical Formula 12] [In the formula, R 3 R is the same or different hydrogen atom or an alkyl group having 1 to 6 carbon atoms.4 are identical or different, and each represents a hydrogen atom, -CH 2 O(CH 2 ) d (CHR 6 ) e (CH 2 ) f R 7 is a group represented by. R 6 are identical or different, and each represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and R 7 are identical or different, and each represents a hydrogen atom, a hydroxyl group, a nitrile group, a trifluoromethyl group, an alkoxy group, or a cyclic ether group which may have a substituent. The case where R 3 is an alkyl group having 1 to 6 carbon atoms and R 4 is a hydrogen atom is excluded because it corresponds to an X unit. The number of repeating units d are identical or different and each is an integer of 0 to 4, the number of repeating units e are identical or different and each is an integer of 0 to 4, and the number of repeating units f are identical or different and each is an integer of 0 to 10. A are identical or different, and each represents a single bond or an alkylene group having 1 to 4 carbon atoms.]]

[0034] R in formula (3) 3 is the same as R in formula (2), including preferred embodiments. 3 . In addition, R 3 is preferably an alkyl group having 1 to 6 carbon atoms. When R 3 is an alkyl group having 1 to 6 carbon atoms, the Y unit corresponds to an alkyl group-containing unit.

[0035] As R in formula (3) 4 , -CH 2 O(CH 2 ) d (CHR 6 ) e (CH 2 ) f R 7 is preferred, and in said group, it is more preferred that R 6 is an alkyl group having 1 to 4 carbon atoms, R 7 is a hydrogen atom, d is an integer of 1 to 3, e is an integer of 1 to 3, and f is an integer of 1 to 8.

[0036] In R of formula (3) 4 , R6 The alkyl group having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, etc. Among these, methyl group and ethyl group are preferred.

[0037] R in equation (3) 4 In R 6 A C1-C4 alkyl group is preferred.

[0038] R in equation (3) 4 In R 7 Examples of alkoxy groups include alkoxy groups having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms). These alkoxy groups may be linear or branched, and include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentoxy, isopentoxy, and n-hexyloxy groups. Among these, methoxy and ethoxy groups are preferred.

[0039] R in equation (3) 4 In R 7 The number of ring members of the cyclic ether group, which may have substituents, is preferably 3 to 10, more preferably 3 to 8, and even more preferably 3 to 6. The number of oxygen atoms in the cyclic ether group is preferably 1 to 6, more preferably 1 to 4, and even more preferably 1 to 3. In this specification, the number of ring members refers to the number of atoms that constitute the ring skeleton; for example, in the case of a 5-membered ring, it is 5.

[0040] Substituents on the cyclic ether group include carbonyl groups, C1-C4 alkyl groups, and alkoxy groups having C1-C4 alkyl groups. Among these, carbonyl groups and C1-C4 alkyl groups are preferred, and carbonyl groups are more preferred. Examples of C1-C4 alkyl groups include R 6 The same applies to alkyl groups having 1 to 4 carbon atoms and preferred embodiments. Similarly, alkyl groups having 1 to 4 carbon atoms in the alkoxy group are also R6 The same applies to alkyl groups having 1 to 4 carbon atoms, including preferred embodiments.

[0041] R 7 A cyclic ether group that may have substituents is preferably substituted. Furthermore, it is preferable that the cyclic ether group contains a carbonate group (-O-(C=O)-O-). 7 A preferred embodiment of the cyclic ether group, which may have substituents, is shown below. * indicates a bond. [Chemical Formula 13] [Chem.14]

[0042] R in equation (3) 3 In R 7 Preferably, the group is a hydrogen atom, a nitrile group, a trifluoromethyl group, an alkoxy group, or an optionally substituted cyclic ether group; more preferably, a hydrogen atom, a nitrile group, or an optionally substituted cyclic ether group; and even more preferably, a hydrogen atom. 7 Preferred components include hydrogen atoms, nitrile groups, trifluoromethyl groups, and optionally substituted cyclic ether groups.

[0043] R in equation (3) 3 In this equation, d is an integer from 0 to 4, preferably an integer from 1 to 3, more preferably an integer from 1 to 2, and even more preferably an integer of 1. e is an integer from 0 to 4, preferably an integer from 1 to 3, more preferably an integer from 1 to 2, and even more preferably an integer of 1. R in equation (3) 3 In this, f is an integer between 0 and 10, but is preferably an integer between 1 and 8, more preferably an integer between 2 and 6, and even more preferably an integer between 3 and 5.

[0044] A in formula (3) is the same as A in formula (1), including the preferred embodiment.

[0045] R in equation (3) 3 and R 4 It is also preferable that both atoms are hydrogen atoms. This tends to reduce the crystallinity of the polyether polymer and result in better ionic conductivity.

[0046] Preferred embodiments of the Y unit, which is a constituent unit derived from the alkylene oxide shown in formula (3), are shown below. Among these, the constituent units shown in formulas (3-1) to (3-12) are preferred, the constituent units shown in formulas (3-1), (3-2), (3-7), and (3-8) are more preferred, and the structural units shown in formulas (3-2) and (3-7) are even more preferred. [Chemical Formula 15]

[0047] While preferred embodiments for units X, Y, and Z have been illustrated, combinations of preferred structures for units X and Y, combinations of preferred structures for units X and Z, and combinations of preferred structures for units X, Y, and Z are also preferred embodiments.

[0048] In formulas (1) to (3), * represents a bond, and when located at the end of a polymer, it is a hydrogen atom, a hydroxyl group, or an alkoxy group.

[0049] In the polyether polymer of the present invention, it is preferable that the skeletal structure (number of carbon atoms in the alkylene in the alkylene oxide) is the same in all constituent units. Specifically, it is preferable that all A are the same in each X unit, each Y unit, and each Z unit.

[0050] In the polyether polymer of the present invention, the content of alkyl group-containing units, which are constituent units derived from alkylene oxides having alkyl groups in their side chains, is 5 mol% or more, and may be 100 mol%, but is preferably 5 to 99.9 mol%, more preferably 5 to 98.9 mol%. The lower limit is more preferably 15 mol% or more, particularly preferably 20 mol% or more, most preferably 30 mol% or more, most preferably 40 mol% or more, still most preferably 50 mol% or more, particularly most preferably 60 mol% or more, still preferably 70 mol% or more, and even more preferably 80 mol% or more. Within this range, sufficient sulfide resistance tends to be obtained. In this specification, the notation "~" means greater than or equal to the value before the notation and less than or equal to the value after the notation. Also, in this specification, the content of alkyl group-containing units means the total content when multiple types of constituent units are included as alkyl group-containing units. The same applies to the content of other components.

[0051] In the polyether polymer of the present invention, all alkyl group-containing units may be X units. Therefore, the content of X units, which are constituent units derived from the alkylene oxide represented by the general formula (1), in 100 mol% of the constituent units is preferably the same as the content of alkyl group-containing units.

[0052] In the polyether polymer of the present invention, the content of Z units, which are constituent units derived from the alkylene oxide represented by the general formula (2), in 100 mol% of constituent units is preferably 0.1 to 20 mol%, more preferably 0.3 to 10 mol%, and even more preferably 0.5 to 5 mol%. Within this range, sufficient mechanical strength to withstand compression and the like tends to be obtained.

[0053] In the polyether polymer of the present invention, the content of Y units, which are constituent units derived from the alkylene oxide represented by the general formula (3), in 100 mol% of constituent units is preferably 0 to 79 mol%, more preferably 3 to 60 mol%, and even more preferably 5 to 55 mol%. Within this range, sufficient sulfide resistance is obtained, and lithium ion conductivity tends to increase.

[0054] In the polyether polymer of the present invention, the total content of X units and Z units in 100 mol% of constituent units is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, particularly preferably 98 mol% or more, and may be 100 mol%.

[0055] In the polyether polymer of the present invention, the total content of X units, Y units, and Z units in 100 mol% of constituent units is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, particularly preferably 98 mol% or more, and may be 100 mol%.

[0056] In this specification, the content of each constituent unit in a polyether polymer can be determined by the nuclear magnetic resonance (NMR) spectrum of the polymer.

[0057] The polyether polymer of the present invention may have units other than X, Y, and Z units, such as units having a thioether group or units having a sulfonyl group, as long as it does not depart from the spirit of the invention. These can be used individually or in combination of two or more.

[0058] The weight-average molecular weight (Mw) of the polyether polymer of the present invention is preferably 0.5 million to 4 million, more preferably 0.5 million to 3.5 million, even more preferably 10,000 to 3.5 million, and most preferably 20,000 to 2.5 million. This tends to result in more favorable results of the present invention.

[0059] The degree of dispersion (Mw / Mn) of the polyether polymer of the present invention is preferably 1 to 40, more preferably 1 to 30, even more preferably 1 to 20, and particularly preferably 1 to 10. This tends to lead to a more favorable outcome of the effects of the present invention. In this specification, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the polymer are measured by the method described in the examples.

[0060] The polyether polymer of the present invention may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer. A random copolymer is preferred because it disrupts the crystallinity of the polymer, resulting in better ion transportability (lithium ion conductivity).

[0061] Preferred embodiments of the polyether polymer of the present invention are as follows: <<Embodiment 1-1>> A polymer having an X unit content of 40 mol% or more.

[0062] <<Aspect 1-2>> A polymer containing X units and Z units, with a total content of 50 mol% or more.

[0063] <<Method for Producing Polyether Polymers>> Next, the monomers used in the polymerization of the polyether polymer of the present invention will be described. The X, Y, and Z units are formed by synthesizing, for example, the compounds represented by formula (1-a), formula (3-a), and formula (2-a) as monomers.

[0064] [Chem.16] (In formula (1-a), R 1 , R 2 A is R in equation (1) 1 , R 2 (Similar to A.) ​​[Chemical 17] (In formula (2-a), R 3 , R 5 A is R in equation (2) 3 , R 5 (Similar to A.) ​​[Chemical 18] (In formula (3-a), R 3 , R 4 A is R in equation (3) 3 , R 4 (This is the same as A.)

[0065] The polymerization method for the polyether polymer of the present invention is not particularly limited, and conventional polymerization reactions can be used. Those skilled in the art can appropriately produce the polyether polymer of the present invention using the above monomers by known polymerization methods, etc. For example, a ring-opening polymerization catalyst such as an organoaluminum-based catalyst system, an organozinc-based catalyst system, or an organotin-phosphate ester condensate catalyst system as a coordination anion initiator, and a K counterion. + Polyether polymers can be obtained by reacting each monomer with or without a solvent at a reaction temperature of 0 to 120°C under stirring, using an anionic initiator such as potassium alkoxide, diphenylmethyl potassium, or potassium hydroxide, or a cationic initiator such as a Lewis acid such as boron trifluoride, diethyl ether complex, aluminum(III) chloride, or tin(IV) chloride.

[0066] Furthermore, the compounds represented by formula (1-a), formula (2-a), and formula (3-a) may be commercially available, but if synthesized, they can be obtained, for example, by the reaction of oxetane alcohols with alkyl ether halides.

[0067] Furthermore, the polyether polymer of the present invention, in which A is a methylene group, can be obtained by synthesis using the above monomers. However, those skilled in the art can appropriately select the monomer according to the A of the polyether polymer to be produced.

[0068] The polymer electrolyte composition of the present invention may use polyether polymers that do not satisfy the X-to-Z units, such as polyethylene oxide and polypropylene oxide, which are homopolymers of ethylene oxide and propylene oxide, as long as the effects of the present invention are satisfied. These may be used individually or in combination of two or more types.

[0069] In the polymer electrolyte composition of the present invention, the content of the polyether polymer of the present invention in 100% by mass of the polyether polymer is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and may also be 100% by mass. This tends to more favorably obtain the effects of the present invention. In this specification, the content of each polymer can be determined by nuclear magnetic resonance spectroscopy.

[0070] <<Lithium Salt Compound>> In the present invention, the ionic conductivity of the polyether polymer alone is very low, and ionic conductivity is achieved by using a lithium salt compound in combination. Specifically, lithium salt compounds having a wide potential window, such as those commonly used in lithium-ion batteries, are preferred. This results in a mixture of the polyether polymer and the lithium salt compound, which constitutes an ionic conductive polymer. Here, the polyether polymer is preferably a polyether polymer that contains at least alkyl group-containing units, which are constituent units derived from alkylene oxides having alkyl groups in their side chains, and more preferably the content of alkyl group-containing units is 5 mol% or more per 100 mol% of constituent units. Examples of lithium salt compounds include LiBF 4 LiPF 6 LiClO 4 LiCF 3 SO 3 , Li(CF 3 SO 2 ) 2 N, LiN (CF 3 SO 2 ) 2 (LiTFSI), LiN(SFO 2 ) 2 (LiFSI), LiN(C 2 F 5 SO 2 ) 2 ,LiN[CF 3 SC (C 2 F 5 SO 2 ) 3 ] 2 These are some examples. These may be used individually or in combination of two or more types.

[0071] In the polymer electrolyte composition of the present invention, the content of the lithium salt compound is preferably 10 to 500 parts by mass, more preferably 20 to 400 parts by mass, even more preferably 30 to 300 parts by mass, and particularly preferably 40 to 250 parts by mass, per 100 parts by mass of the polyether polymer (preferably the polyether polymer of the present invention). This tends to more favorably obtain the effects of the present invention.

[0072] <<Room Temperature Molten Salt>> The polymer electrolyte composition of the present invention may contain a room temperature molten salt. A room temperature molten salt means a salt that is liquid in at least a portion of its form at room temperature.

[0073] Room-temperature molten salts are also called ionic liquids, and known examples include pyridine-based, aliphatic amine-based, and alicyclic amine-based quaternary ammonium organic cations. These may be used individually or in combination of two or more types. Examples of quaternary ammonium organic cations include imidazolium ions such as dialkylimidazolium and trialkylimidazolium, tetraalkylammonium ions, alkylpyridinium ions, pyrazolium ions, pyrrolidinium ions, and piperidinium ions.

[0074] <<Polyionic Liquid>> In the ion-conducting polymer of the present invention, a polyionic liquid may be used. The polyionic liquid is obtained by introducing polymerizable groups such as vinyl groups, acryloyl groups, and methacryloyl groups into the above-mentioned room-temperature molten salt or the like to increase its molecular weight. Examples include imidazolium-based polyionic liquids obtained by polymerizing alkylimidazolium fluoroborate, alkylimidazolium fluorophosphate, alkylimidazolium fluoromethanesulfonylimide, pyridinium-based polyionic liquids such as alkylpyridinium fluoroborate, alkylpyridinium fluorophosphate, and alkylpyridinium fluoromethanesulfonylimide, alkylphosphonium-based polyionic liquids such as alkylphosphonium fluoroborate, alkylphosphonium fluorophosphate, and alkylphosphonium fluoromethanesulfonylimide, or zwitter polyionic liquids obtained by introducing sulfobetaine, carboxybetaine, phosphobetaine (phosphorylcholine), dimethylamine oxide, dimethylsulfoniopropionate, etc., which have both charges in the molecule.

[0075] The weight-average molecular weight (Mw) of the ion-conducting polymer (preferably the polyether polymer or polyionic liquid of the present invention) is preferably 0.5 million to 4 million, more preferably 0.5 million to 3.5 million, even more preferably 10,000 to 3.5 million, and most preferably 20,000 to 2.5 million. This tends to lead to a more favorable outcome of the effects of the present invention.

[0076] <<Ion-Conducting Compounds>> The ion-conducting compounds used in the polymer electrolyte composition of the present invention are not particularly limited as long as they are compounds capable of conducting ions (preferably lithium ions), and examples include heterocyclic compounds, ether compounds, etc. These may be used alone or in combination of two or more types.

[0077] <<Heterocyclic Compounds>> In this specification, a heterocyclic compound means a cyclic compound containing at least two different elements as elements forming a ring structure. The combination of at least two different elements is not particularly limited, but examples include a combination of a carbon atom and at least one atom selected from the group consisting of oxygen, sulfur, boron, phosphorus, and nitrogen atoms. Among these, a combination of a carbon atom and at least one atom selected from the group consisting of oxygen and sulfur atoms is preferred, and a combination of a carbon atom and an oxygen atom, or a combination of a carbon atom and a sulfur atom, is more preferred. The heterocyclic compound is not particularly limited, but it is preferably at least one compound selected from the group consisting of compounds shown in the following general formulas (A) to (C). [Chemical Formula 19] [In the formula, R 9 R is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 10 This is a hydrogen atom, -CH 2 O { (CH 2 ) a O} b (CH 2 ) c An alkylene glycol alkyl ether group represented by H, or -CH 2 OR 8 This is a crosslinking group containing an ethylenically unsaturated double bond, represented by R. 8 This is an acrylic group, a methacrylic group, an allyl group, or a metaallyl group. The repeating unit a is an integer from 1 to 10, the repeating unit b is an integer from 0 to 6, and the repeating unit c is an integer from 0 to 4. [Chemical Formula 20] [In the formula, R 11 [Chemical Formula 21] is the same or different hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkenyl group, and g is an integer from 0 to 4. [In the formula, R 12 [The elements are, either identical or different, a hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkenyl group, and h is an integer from 0 to 8.]

[0078] The compound having the oxetane skeleton shown in the general formula (A) is R of formula (A). 9Since it is an alkyl group having 1 to 6 carbon atoms, it is likely to cause steric hindrance, which can effectively suppress the coordination of lithium ions to ether oxygen, resulting in a higher ion transport rate (lithium ion conductivity) and suppressing side reactions with sulfide-based solid electrolytes.

[0079] R in equation (A) 9 The alkyl group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, etc. Among these, methyl group and ethyl group are preferred.

[0080] R in equation (A) 10 of -CH 2 O { (CH 2 ) a O} b (CH 2 ) C Alkylene glycol alkyl ether groups represented by H exhibit excellent molecular mobility and have a structure that maintains an appropriate distance between oxygen atoms, which tends to result in higher ion transportability (lithium ion conductivity).

[0081] R in equation (A) 10 In this equation, a is an integer from 1 to 10, but preferably an integer from 1 to 8, more preferably an integer from 1 to 7, even more preferably an integer from 1 to 6, particularly preferably 1 to 5, most preferably 1 to 4, even more preferably 1 to 3, and still most preferably 1 to 2. 10 In this equation, b is an integer from 0 to 6, preferably an integer from 0 to 4, more preferably an integer from 1 to 3, and even more preferably an integer from 1 to 2. 10 In this, c is an integer between 0 and 4, preferably an integer between 0 and 3, more preferably an integer between 1 and 2, and even more preferably an integer of 1.

[0082] R in equation (A) 10 of -CH 2 OR 8Crosslinking groups containing ethylenically unsaturated double bonds, as represented by , tend to be able to form polymers by crosslinking because they are crosslinkable.

[0083] R in equation (A) 10 In this case, the most suitable R 8 R in general formula (2) 8 It is identical to [the other one].

[0084] R in equation (A) 10 For example, -CH 2 O(CH 2 ) a O(CH 2 ) b Alkylene glycol alkyl ether group represented by H, -CH 2 OR 8 A crosslinking group containing an ethylenically unsaturated double bond represented by -CH is preferred, 2 O(CH 2 ) a O(CH 2 ) b A more preferable alkylene glycol alkyl ether group represented by H is used.

[0085] Preferred embodiments of the compound represented by formula (A) are shown below. Among these, the compounds represented by formulas (A-1), (A-2), (A-3), and (A-4) are preferred, the compounds represented by formulas (A-1), (A-2), and (A-3) are more preferred, and the compound represented by formula (A-3) is even more preferred. [Chemical Formula 22]

[0086] The method for producing the compound represented by formula (A) of the present invention is not particularly limited, and those skilled in the art can produce it appropriately by known synthesis methods, etc. For example, the compound represented by formula (A) can be obtained by the reaction of oxetane alcohols with alkyl ether halides.

[0087] R in equation (B) 11 The C1-C6 alkyl group is, including in preferred embodiments, R of formula (A). 9 This is similar to alkyl groups with 1 to 6 carbon atoms.

[0088] R in equation (B) 11The alkenyl group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include vinyl group, allyl group, 1-propenyl group, and 1-methylethenyl group. Among these, vinyl group and allyl group are preferred, and vinyl group is more preferred.

[0089] R in equation (B) 11 A C1-C6 alkyl group is preferred.

[0090] g is an integer between 0 and 4, preferably between 0 and 3, more preferably between 0 and 2, even more preferably between 0 and 1, and particularly preferably 1.

[0091] Preferred embodiments of the compound represented by formula (B) are shown below. Among these, the compounds represented by formulas (B-1) and (B-2) are preferred. [Chemical Formula 23]

[0092] The method for producing the compound represented by formula (B) of the present invention is not particularly limited, and those skilled in the art can produce it appropriately by known synthesis methods, etc. For example, the compound represented by formula (B) can be obtained by the reaction of phosgene with the corresponding diol or by the reaction of carbon dioxide with the corresponding epoxide. Alternatively, commercially available products may be used.

[0093] R in equation (C) 12 This includes preferred embodiments, and R of formula (B). 11 It is similar to that.

[0094] h is an integer between 0 and 8, preferably between 0 and 6, more preferably between 0 and 4, even more preferably between 0 and 2, particularly preferably between 0 and 1, and most preferably 1.

[0095] Preferred embodiments of the compound shown in formula (C) are shown below. Among these, the compound shown in formula (C-1) is preferred. [Chemical Formula 24]

[0096] The method for producing the compound represented by formula (C) of the present invention is not particularly limited, and those skilled in the art can produce it appropriately by known synthesis methods, etc. For example, the compound represented by formula (C) can be obtained by the oxidation reaction of the corresponding thioether. Alternatively, commercially available products may be used.

[0097] The ether compounds used in the present invention are not particularly limited, but it is preferable that they be at least one compound selected from the group consisting of linear ether compounds represented by the following general formula (D) and branched ether compounds represented by the following general formula (E). [Chemical Formula 25] (In the formula, R 13 These are identical or different alkyl groups having 1 to 4 carbon atoms, or -(CH 2 ) k CH 2 O-R 14 It is a group represented by R. 14 (The elements are the same or different alkyl groups having 1 to 4 carbon atoms. The repeating numbers i and j are the same or different, and range from 0 to 3, while k is an integer from 1 to 3.) [Chemical Formula 26] (In the formula, R 15 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or -{(CH 2 ) m CH 2 O} n R 17 That is. R 16 These are identical or different alkyl groups having 1 to 4 carbon atoms, or -{(CH 2 ) m CH 2 O} n R 17 That is. R 17 (The elements are the same or different alkyl groups having 1 to 4 carbon atoms. The number of repetitions, k, is 0 or 1, and m and n are the same or different integers from 1 to 3.)

[0098] R in general formula (D) 13 The alkyl group having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, etc. Among these, methyl group and ethyl group are preferred.

[0099] i and j, which are the number of repetitions in general formula (D), are the same or different integers between 0 and 3, preferably between 0 and 2, and more preferably between 1 and 2.

[0100] R in general formula (D) 13 - (CH2) k CH 2 O-R 14 The group R represented by 14 The alkyl group having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, etc. Among these, methyl group and ethyl group are preferred.

[0101] The number of repetitions k in general formula (D) is an integer from 1 to 3, preferably an integer from 2 to 3.

[0102] R in general formula (D) 13 Of these, at least one is preferably an alkyl group having 1 to 4 carbon atoms.

[0103] R in general formula (E) 15 and R 16 The alkyl group having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, etc. Among these, methyl group and ethyl group are preferred.

[0104] R in general formula (E) 15 and R 16 -{(CH2) m CH 2 O} n -R 17 The group R represented by 17The alkyl group having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms, more preferably 1 to 2 carbon atoms) may be linear or branched, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, iso-butyl group, sec-butyl group, tert-butyl group, etc. Among these, methyl group and ethyl group are preferred.

[0105] The number of repetitions k in general formula (E) is 0 or 1. It is preferable that k is 1.

[0106] The number of repetitions of general formula (E), m and n, are the same or different integers from 1 to 3, preferably from 1 to 2, and more preferably from 1. It is preferable that both m and n are 1.

[0107] R in general formula (E) 15 R of general formula (5) is preferred to be an alkyl group having 1 to 4 carbon atoms. 16 At least one of them is -{(CH2) m CH 2 O} n -R 17 It is preferable that R 16 At least two of them are -{(CH2) m CH 2 O} n -R 17 It is more preferable that R 16 All of them are - {(CH2) m CH 2 O} n -R 17 It is even more preferable that this be the case.

[0108] Specific examples of linear ether compounds represented by general formula (D) are, but are not limited to, 1-methoxy-3-(3-methoxypropoxy)propane (formula (D-1)), 1-methoxy-4-(3-methoxypropoxy)butane (formula (D-2)), 1-methoxy-4-(4-methoxybutoxy)butane (formula (D-3)), 2,6,10,14-tetraoxapentadecane (formula (D-4)), 2,6,11,15-tetraoxahexadecane (formula (D-5)), 2,6,10,15-tetraoxahexadecane (formula (D-6)), 2,7,11,16-tetraoxaheptadecane (formula (D-7)), 2,7,12,17-tetraoxa Examples include octadecane (formula (D-8)), 1-methoxy-2-(2-methoxyethoxy)ethane (formula (D-9)), 2,5,8,11-tetraoxadodecane (formula (D-10)), 2,5,8,11,14-pentaoxapentadecane (formula (D-11)), and among these, formulas (D-1), (D-2), (D-3), (D-4), (D-5), (D-6), (D-10), and (D-11) are preferred, formulas (D-3), (D-4), (D-5), (D-6), (D-10), and (D-11) are more preferred, and formulas (D-3), (D-4), (D-5), (D-10), and (D-11) are even more preferred.

[0109] [C27]

[0110] Specific examples of branched ether compounds represented by general formula (E) are, but are not limited to, 1,3-dimethoxy-2-(methoxymethyl)propane (formula (E-1)), 1,3-dimethoxy-2-(methoxymethyl)-2-methylpropane (formula (E-2)), 1-methoxy-2,2-bis(methoxymethyl)butane (formula (E-3)), 1,3-diethoxy-2-(ethoxymethyl)propane (formula (E-4)), 1,3-diethoxy-2-(ethoxymethyl)-2-methylpropane (formula (E-5)), and 1-ethoxy-2,2-bis(ethoxymethyl)butane. ¹(Formula (E-6)), 7-((2-methoxyethoxy)methyl)-2,5,9,12-tetraoxatridecane(Formula (E-7)), 7-((2-methoxyethoxy)methyl)-7-methyl-2,5,9,12-tetraoxatridecane(Formula (E-8)), 7-ethyl-((2-methoxyethoxy)methyl)-2,5,9,12-tetraoxatridecane(Formula (E-9)), 10-((2-methoxyethoxy)methyl)-2,5,8,12,15-pentaoxahexadecane(Formula (E-10)), 10-((2-methoxyethoxy)methyl)-10-methyl Lu-2,5,8,12,15-pentaoxahexadecane (formula (E-11)), 10-ethyl-10-((2-methoxyethoxy)methyl)-2,5,8,12,15-pentaoxahexadecane (formula (E-12)), 10-((2-methoxyethoxy)methyl)-2,5,8,12,15,18-hexaoxanonadecane (formula (E-13)), 10-((2-methoxyethoxy)methyl)-10-methyl-2,5,8,12,15,18-hexaoxanonadecane (formula (E-14)), 10-ethyl-10-((2-methoxyethoxy)methyl)-2 ,5,8,12,15,18-Hexaoxanonadecane (Formula (E-15)),10-((2-(2-methoxyethoxy)ethoxy)methyl)-2,5,8,12,15,18-Hexaoxanonadecane (Formula (E-16)),10-((2-(2-methoxyethoxy)ethoxy)methyl)-10-methyl-2,5,8,12,15,18-Hexaoxanonadecane (Formula (E-17)),10-Ethyl-10-((2-(2-methoxyethoxy)ethoxy)methyl)-2,5,8,12,15,18-Hexaoxanonadecane (Formula (E-18)),1,2,3-Trimethoxypropane (Formula (E-19)), 1,2,3-Triethoxypropane (Formula (E-20)), 1,3-Dimethoxy-2-(2-Methoxyethoxy)propane (Formula (E-21)), 6-(Methoxymethyl)-2,5,8,11-Tetraoxadodecane (Formula (E-22)), 7-(2-Methoxyethoxy)-2,5,9,12-Tetraoxatridecane (Formula (E-23)), 10-(2-Methoxyethoxy)-2,5,8,12,15-Pentaoxahexadecane (Formula (E-24)), 10-(2-Methoxyethoxy )-2,5,8,12,15,18-Hexaoxanonadecane (Formula (E-25)), 10-(2-(2-methoxyethoxy)ethoxy)-2,5,8,12,15,18-Hexaoxanonadecane (Formula (E-26)), 13-(2-methoxyethoxy)-2,5,8,11,15,18-Hexaoxanonadecane (Formula (E-27)), 13-(2-(2-methoxyethoxy)ethoxy)-2,5,8,11,15,18,21-Heptaoxadocosane (Formula (E-28)), 13-(2-methoxyethoxy)-2,5,8,11 Examples include 15,18,21,24-octaoxapentacosane (formula (E-29)), 1,3-dimethoxy-2,2-bis(methoxymethyl)propane (formula (E-30)), and 1,3-diethoxy-2,2-bis(ethoxymethyl)propane (formula (E-31)). Among these, formulas (E-2), (E-3), (E-5), (E-6), (E-8), (E-9), (E-11), (E-12), (E-14), (E-15), (E-17), (E-18), (E-21), (E-22), (E-23), (E-24), (E It is preferable that the formulas are (E-25), (E-26), (E-27), (E-30), (E-31), more preferably (E-5), (E-6), (E-8), (E-9), (E-11), (E-12), (E-14), (E-15), (E-22), (E-23), (E-24), (E-25), (E-26), (E-27), and even more preferably (E-5), (E-6), (E-8), (E-9), (E-11), (E-12), (E-14), (E-15), (E-23), (E-25), (E-26).

[0111] [C28] [C29]

[0112] The linear ether compounds represented by general formula (D) and the branched ether compounds represented by general formula (E) may be used individually or in combination of two or more types.

[0113] As ion-conducting compounds, the compounds shown in formula (B), (D), and (E) are preferred, with the compound shown in formula (B) being more preferred.

[0114] In the polymer electrolyte composition of the present invention, the lower limit of the content of the ion-conducting compound per 100 parts by mass of the ion-conducting polymer (preferably a polyether polymer, more preferably the polyether polymer of the present invention) is 50 parts by mass or more, preferably 75 parts by mass or more, more preferably 100 parts by mass or more, and the upper limit is 1200 parts by mass or less, preferably 1000 parts by mass or less, more preferably 800 parts by mass or less, even more preferably 600 parts by mass or less, most preferably 400 parts by mass or less, and most preferably 250 parts by mass or less. This tends to more favorably obtain the effects of the present invention.

[0115] <<Nanofibers>> In this specification, examples of nanofibers include carbon fibers, carbon nanotubes, silver nanowires, glass wool, glass fibers, and cellulose nanofibers. It is preferable to use carbon fibers, carbon nanotubes, and cellulose nanofibers, more preferable to use carbon nanotubes and cellulose nanofibers, and even more preferable to use cellulose nanofibers. These may be used individually or in combination of two or more types.

[0116] In the nanofibers of the present invention, the diameter is preferably 0.5 nm to 500 nm, more preferably 0.5 nm to 300 nm, even more preferably 0.5 nm to 200 nm, and particularly preferably 1 nm to 200 nm. Most preferably 1 nm to 100 nm, and most preferably 1 nm to 50 nm.

[0117] In the polymer electrolyte composition of the present invention, the nanofiber content is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 2 parts by mass or more, and particularly preferably 5 parts by mass or more, per 100 parts by mass of the ion-conducting polymer (preferably a polyether polymer, more preferably the polyether polymer of the present invention). The upper limit is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 13 parts by mass or less, and particularly preferably 10 parts by mass or less. Within this range, it is possible to improve the mechanical properties such as the fracture strength and compressive strain of the crosslinked material without impairing ion conductivity.

[0118] In the polymer electrolyte composition of the present invention, the total content of the ion-conducting polymer, ion-conducting compound, and nanofibers is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, and may be 100% by mass, based on 100% by mass of the polymer electrolyte composition of the present invention. This tends to more favorably obtain the effects of the present invention.

[0119] <<Other Components>> In addition to the components listed above, the polymer electrolyte composition of the present invention may also contain, for example, reaction initiators, crosslinking aids, plasticizers, etc. These may be used individually or in combination of two or more types.

[0120] <<Reaction Initiator>> In the present invention, a commonly known reaction initiator can be used, and either thermal crosslinking (thermal crosslinking) or UV irradiation crosslinking (UV crosslinking) can be employed.

[0121] <<Thermal Crosslinking>> In the case of thermal crosslinking, a reaction initiator selected from organic peroxides, azo compounds, etc., is used. These may be used alone or in combination of two or more. As organic peroxides, those commonly used for crosslinking applications such as ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxyesters, etc., are used, and as azo compounds, those commonly used for crosslinking applications such as azonitrile compounds, azoamide compounds, azoamidine compounds, etc., are used.

[0122] The amount of reaction initiator added in thermal crosslinking varies depending on the type, but generally, per 100 parts by mass of ion-conducting polymer (preferably polyether polymer, more preferably the polyether polymer of the present invention), the lower limit is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more. On the other hand, the upper limit is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less.

[0123] The conditions for thermal crosslinking vary depending on the type of reaction initiator, but typically the temperature is in the range of 50°C to 200°C, and the duration is 0.5 hours to 24 hours.

[0124] <<UV Crosslinking>> For UV crosslinking, alkylphenones, benzophenones, acylphosphine oxides, titanocenes, triazines, bisimidazoles, oxime esters, etc., can be used as radical initiators. These may be used alone or in combination of two or more types.

[0125] The amount of reaction initiator added in UV crosslinking varies depending on the type, but typically, per 100 parts by mass of the ion-conducting polymer (preferably a polyether polymer, more preferably the polyether polymer of the present invention), the lower limit is preferably 0.01 parts by mass or more, more preferably 0.03 parts by mass or more, and even more preferably 0.05 parts by mass or more. On the other hand, the upper limit is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less.

[0126] The conditions for UV crosslinking vary depending on the type of reaction initiator, but typically the temperature is in the range of room temperature to 50°C, and the duration is 0.25 minutes to 10 minutes. Furthermore, it is preferable that the UV irradiation light source be a device that irradiates ultraviolet light or visible light in the range of 200 to 500 nm, equipped with a UV-LED lamp, high-pressure mercury lamp, ultra-high-pressure mercury lamp, metal halide lamp, halogen lamp, or black light lamp, etc.

[0127] <<Crosslinking Aids>> When crosslinking the polymer electrolyte composition of the present invention, crosslinking aids may be used as needed. Preferred crosslinking aids include ethylene glycol diacrylate, ethylene glycol dimethacrylate, oligoethylene glycol diacrylate, oligoethylene glycol dimethacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, allyl methacrylate, allyl acrylate, diallyl maleate, triallyl isocyanurate, maleimide, phenylmaleimide, maleic anhydride, pentaerythritol tetrakis(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(2-(3-sulfanylbutanoyloxy)ethyl)-1,3,5-triazinan-2,4,6-trione, and trimethylolpropane tris(3-mercaptobutyrate). Among these, trimethylolpropane trimethacrylate and 1,4-bis(3-mercaptobutyryloxy)butane are more preferred. These may be used individually or in combination of two or more.

[0128] The amount of these crosslinking aids added varies depending on the type, but generally, with 100 parts by mass of polyether polymer, the lower limit is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more. On the other hand, the upper limit is preferably 40.0 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less.

[0129] <Polymer Electrolyte for Lithium-Ion Secondary Batteries> In the present invention, it is preferable to crosslink the polymer electrolyte composition to make it a polymer electrolyte for lithium-ion secondary batteries (also simply called a polymer electrolyte). By using the polymer electrolyte for lithium-ion secondary batteries of the present invention in at least one of the electrodes (positive electrode, negative electrode) or the solid electrolyte layer, the adhesion strength with the active material and inorganic solid electrolyte can be improved, and short circuits in the battery due to confinement pressure and dendrite deposition can be more effectively prevented. Furthermore, the polymer electrolyte of the present invention can suppress side reactions with sulfide-based solid electrolytes and exhibits characteristics with high ionic conductivity and high Li ion transport rate (i.e., high lithium ion conductivity), and can conduct high current densities in energized load tests.

[0130] The crosslinking method for the polymer electrolyte composition for lithium-ion secondary batteries of the present invention can be carried out by known methods by selecting the reaction initiator and crosslinking aid described above, and is not particularly limited. Furthermore, the timing of crosslinking can be appropriately performed depending on the application using the polymer electrolyte composition of the present invention.

[0131] The polymer electrolyte for lithium-ion secondary batteries of the present invention is preferably a composite with a sulfide-based solid electrolyte having high lithium-ion conductivity, from the viewpoint of improving the electrical characteristics of lithium-ion secondary batteries. Specifically, the lithium-ion conductivity is 1 × 10⁻⁶. -6 It is preferable that the S / cm is greater than or equal to 1 × 10 -5 It is more preferable that the S / cm or higher is 1 × 10 -4 It is even more preferable that the conductivity is S / cm or higher. Lithium ion conductivity can be determined by the product of ionic conductivity and lithium ion transport fraction.

[0132] The polymer electrolyte for lithium-ion secondary batteries of the present invention can adapt to the volume expansion and contraction of the active material during charging and discharging, and exhibits excellent compressive resistance under high confinement pressure. Specifically, it exhibits excellent compressive strain and compression set in terms of compressive strength (breaking strength). Compressive strain measures how much deformation occurs without fracture at a certain compressive strength. Compression set measures how much the material returns to its initial value after a load is applied for a certain period of time at a certain compressive strength and then released. The effects of the present invention cannot be obtained if only one of these is superior.

[0133] In the polymer electrolyte for lithium-ion secondary batteries of the present invention, the compressive strain when crosslinked is preferably -90% to -30%, more preferably -80% to -30%, and even more preferably -80% to -40%. Being within this range means that the lithium-ion secondary battery has sufficient flexibility and strength against external pressure (e.g., vibration, shock, and restraint pressure).

[0134] In the polymer electrolyte for lithium-ion secondary batteries of the present invention, the compression set when crosslinked is preferably 0% to 20%, more preferably 0% to 15%, and even more preferably 0.1% to 10%. Being within this range means that the electrolyte has the flexibility to accommodate the expansion and contraction of the active material when used in a lithium-ion secondary battery.

[0135] Furthermore, in the polymer electrolyte for lithium-ion secondary batteries of the present invention, the ratio of compressive strain to compression set ([compression set] / [compressive strain]) when the crosslinked material is formed is considered to be of superior quality as it approaches 0. The lower limit of this ratio is preferably -0.5 or higher, more preferably -0.4 or higher, even more preferably -0.3 or higher, particularly preferably -0.2 or higher, and most preferably -0.15 or higher. The upper limit is preferably -0.001 or lower, more preferably -0.005 or lower, even more preferably -0.007 or lower, and particularly preferably -0.01 or lower. As mentioned above, it may also be substantially 0. By being within these ranges, a polymer electrolyte for lithium-ion secondary batteries with good balance against external pressure and expansion / contraction of the active material can be provided when used in a lithium-ion secondary battery. In this specification, the compressive strain and compression set when the crosslinked material is formed are measured by the method described in the examples.

[0136] By including at least an ion-conducting polymer, an ion-conducting compound, and nanofibers in the polymer electrolyte composition for lithium-ion secondary batteries, the compressive strain, compression set, and the ratio of compressive strain to compression set when crosslinked can be kept within the above-mentioned preferred numerical range. As mentioned above, the closer the ratio of compression set to compressive strain is to 0, the better the crosslinked material is. Therefore, the following methods are effective in increasing the compressive strain while reducing the compression set: By compounding with an ion-conducting compound or nanofibers, the crosslinking density of the polymer decreases, and the compressive strain increases. Furthermore, by compounding with nanofibers, the strength of the polymer improves, and the compression set decreases.

[0137] <Lithium-ion secondary battery> The lithium-ion secondary battery of the present invention is a lithium-ion secondary battery using the polymer electrolyte composition for lithium-ion secondary batteries of the present invention. For example, in a lithium-ion secondary battery composed of electrodes (positive electrode, negative electrode) and a solid electrolyte layer, it is preferable to use it in at least one of the electrodes (positive electrode, negative electrode) and the solid electrolyte layer.

[0138] <<Solid Electrolyte Layer>> In the solid electrolyte layer used in the present invention, it is preferable to use the polymer electrolyte composition for lithium-ion secondary batteries of the present invention, and more preferably to use it as a crosslinked polymer electrolyte for lithium-ion secondary batteries. Examples include using a mixture of an inorganic solid electrolyte and the polymer electrolyte for lithium-ion secondary batteries of the present invention as the solid electrolyte layer, using the polymer electrolyte for lithium-ion secondary batteries itself as the solid electrolyte layer, or using a laminate of an inorganic solid electrolyte and the polymer electrolyte for lithium-ion secondary batteries of the present invention as the solid electrolyte layer. The inorganic solid electrolyte used in the case of lamination may be a mixture with the polymer electrolyte for lithium-ion secondary batteries of the present invention as described above.

[0139] <Inorganic Solid Electrolytes> Examples of inorganic solid electrolytes include oxide-based solid electrolytes and sulfide-based solid electrolytes. These may be used individually or in combination of two or more types. The inorganic solid electrolyte is included, for example, in particulate form, and has a structure in which the particles of the inorganic solid electrolyte are tightly bound together by the polymer electrolyte for lithium-ion secondary batteries of the present invention.

[0140] Oxide-based solid electrolytes are not particularly limited as long as they contain oxygen, have ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and possess electronic insulating properties.

[0141] Specific compounds that make up oxide-based solid electrolytes include Li x La y TiO 3 [x=0.3~0.7, y=0.3~0.7] (LLT), Li x La y Zr z M m O n (M is at least one element from Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn, and x satisfies 5 ≤ ​​x ≤ 10, y satisfies 1 ≤ y ≤ 4, z satisfies 1 ≤ z ≤ 4, m satisfies 0 ≤ m ≤ 2, and n satisfies 5 ≤ ​​n ≤ 20.) Li x B y M z O n(In the formula, M is at least one element from C, S, Al, Si, Ga, Ge, In, and Sn, x satisfies 0 ≤ x ≤ 5, y satisfies 0 ≤ y ≤ 1, z satisfies 0 ≤ z ≤ 1, and n satisfies 0 ≤ n ≤ 6.) Li x (Al, Ga) y (Ti, Ge) z Si a P m O n (wherein 1≦x≦3, 0≦y≦1, 0≦z≦2, 0≦a≦1, 1≦m≦7, 3≦n≦13), Li (3-2x) M x DO (where x is a number between 0 and 0.1, M represents a divalent metal atom, and D represents a halogen atom or a combination of two or more halogen atoms), Li x Si y O z (1≦x≦5, 0<y≦3, 1≦z≦10), Li x S y O z (1≦x≦3, 0<y≦2, 1≦z≦10), Li 3 BO 3 -Li 2 SO 4 Li 2 O-B 2 O 3 -P 2 O 5 Li 2 O-SiO 2 Li 6 BaLa 2 Ta 2 O 12 Li 3 PO (4-3/2w) N w (where w < 1), Li has a LISICON (Lithium superionic conductor) type crystal structure. 3.5 Zn 0.25 GeO 4 La having a perovskite-type crystal structure 0.55 Li 0.35 TiO 3 LiTi having a NASICON (Natrium superionic conductor) type crystal structure 2 P 3 O 12 Li(1+x+y) (Al, Ga) x (Ti, Ge) (2-x) Si y P (3-y) O 12 (where 0 ≤ x ≤ 1, 0 ≤ y ≤ 1), Li having a garnet-type crystal structure 7 La 3 Zr 2 O1 2 Examples include the following. Phosphorus compounds containing Li, P, and O are also desirable. For example, lithium phosphate (Li 3 PO 4 Examples include LiPON and LiPOD (where D is at least one selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt, Au, etc.), in which some of the oxygen in lithium phosphate is replaced with nitrogen. LiAON (where A is at least one selected from Si, B, Ge, Al, C, Ga, etc.) can also be preferably used.

[0142] Among them, Li x La y TiO 3 [x=0.3~0.7, y=0.3~0.7] (LLT), Li x La y Zr z M m O n (M is at least one element from Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn, and x satisfies 5 ≤ ​​x ≤ 10, y satisfies 1 ≤ y ≤ 4, z satisfies 1 ≤ z ≤ 4, m satisfies 0 ≤ m ≤ 2, and n satisfies 5 ≤ ​​n ≤ 20.) Li 7 La 3 Zr 2 O 12 (LLZ), Li 3 BO 3 Li 3 BO 3 -Li 2 SO 4 Li 3 BO 3 -Li 2 CO 3 Li x (Al, Ga) y (Ti, Ge) z Sia P m O n (However, 1 ≤ x ≤ 3, 0 ≤ y ≤ 1, 0 ≤ z ≤ 2, 0 ≤ a ≤ 1, 1 ≤ m ≤ 7, 3 ≤ n ≤ 13 is preferred.)

[0143] Sulfide-based solid electrolytes are not particularly limited as long as they contain sulfur, have ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and possess electronic insulating properties.

[0144] The sulfide-based solid electrolyte may be a glass-based sulfide solid electrolyte or a glass-ceramic sulfide solid electrolyte. These may be used individually or in combination of two or more. The glass-based sulfide solid electrolyte can be obtained by vitrifying the raw materials. The glass-ceramic sulfide solid electrolyte can be obtained, for example, by heat-treating the glass-based sulfide solid electrolyte. Furthermore, it is preferable that the sulfide-based solid electrolyte has a crystalline structure. Examples of crystalline structures include the Thio-LISICON type crystal structure, the LGPS type crystal structure, and the argyrodite type crystal structure.

[0145] Examples of glassy sulfide solid electrolytes include Li 2 S-P 2 S 5 Li 2 S-LiI-P 2 S 5 Li 2 S-LiI-Li 2 O-P 2 S 5 Li 2 S-LiBr-P 2 S 5 Li 2 S-Li 2 O-P 2 S 5 Li 2 S-Li 3 PO 4 -P 2 S 5 Li 2 S-P 2 S 5 -P 2 O 5 Li 2 S-P2 S 5 -SiS 2 Li 2 S-P 2 S 5 - SnS, Li 2 S-P 2 S 5 - Al 2 S 3 Li 2 S-GeS 2 Li 2 S-GeS 2 Examples include -ZnS. These can be used individually or in combination of two or more.

[0146] Examples of sulfide-based solid electrolytes having a crystalline structure include Li 10 GeP 2 S 12 Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 Li 9.42 Si 1.02 P 2.1 S 9.96 O 2.24 LGPS-type sulfide solid electrolytes such as Li 6 PS 5 Cl, Li 6.6 Ge 0.6 P 0.4 S 5 I, Li 7 Ge 3 PS 12 Algyrodite-type sulfide solid electrolytes such as Li 4.275 Ge 0.61 Ga 0.25 S 4 Li 4 SnS 4 β-Li 3 PS 4 Examples include Thio-LisICON type sulfide solid electrolytes. Among these, argyrodite type sulfide solid electrolytes and Thio-LisICON type sulfide solid electrolytes are preferred, and argyrodite type sulfide solid electrolytes are more preferred. These may be used individually or in combination of two or more.

[0147] From the viewpoint of improving the electrical characteristics of all-solid-state lithium-ion secondary batteries, sulfide-based solid electrolytes with high ionic conductivity are preferable. Specifically, the ionic conductivity is 1 × 10⁻⁶. -4 It is preferable that the S / cm is greater than or equal to 1 × 10 -3 A ratio of S / cm or higher is more preferable.

[0148] As the inorganic solid electrolyte, sulfide-based solid electrolytes are preferred. The polyether polymer of the present invention can suppress side reactions with sulfide-based solid electrolytes and has high lithium ion conductivity, thus more favorably exhibiting the effects of the present invention.

[0149] When the inorganic solid electrolyte is in particulate form, the particle size can be, for example, 0.01 to 100 μm, preferably 0.1 to 20 μm.

[0150] <<Other Components>> In addition to the inorganic solid electrolyte and the polymer electrolyte of the present invention, the solid electrolyte layer may also contain other components such as a binder and a plasticizer. These may be used individually or in combination of two or more types.

[0151] When a mixture of an inorganic solid electrolyte and the polymer electrolyte of the present invention is used as a solid electrolyte layer, the content of the polymer electrolyte composition of the present invention (polymer electrolyte of the present invention) in 100% by mass of the solid electrolyte layer is preferably 0.1% to 90% by mass, more preferably 0.5% to 90% by mass, even more preferably 0.5% to 85% by mass, and particularly preferably 1% to 85% by mass. By setting the content within these ranges, the binding properties between the inorganic solid electrolyte and the polymer electrolyte composition of the present invention are enhanced.

[0152] When the polymer electrolyte of the present invention itself is used as a solid electrolyte layer, the content of the polymer electrolyte composition of the present invention in 100% by mass of the solid electrolyte layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and most preferably 90% by mass or more. It may also be 100% by mass. This tends to result in more favorable results of the present invention.

[0153] <<Method for Manufacturing the Solid Electrolyte Layer>> The solid electrolyte layer can be manufactured using conventionally known methods. For example, the polymer electrolyte composition and / or inorganic solid electrolyte of the present invention can be dispersed in a solvent to prepare a slurry liquid, and the slurry liquid can be molded into any shape by known methods such as applying it to a release sheet such as a PET film, and a solid electrolyte layer containing a polymer electrolyte for lithium-ion secondary batteries can be obtained by the above-mentioned heat crosslinking or UV crosslinking.

[0154] Furthermore, known methods can be used for laminating the polymer electrolyte of the present invention onto the inorganic solid electrolyte in the laminate of the polymer electrolyte and inorganic solid electrolyte of the present invention. For example, one method is to prepare the polymer electrolyte in advance using the above-described manufacturing method and then laminate it onto the inorganic solid electrolyte, or one method is to directly coat and laminate the polymer electrolyte composition of the present invention onto the inorganic solid electrolyte and then form the polymer electrolyte by the above-described thermal crosslinking or UV crosslinking.

[0155] When using a dispersion solvent, it is preferable to use one that does not react with the inorganic solid electrolyte and the polyether polymer. Specifically, butyl butyrate, toluene, ortho-xylene, tetralin, acetonitrile, isobutyronitrile, anisole, methyl isobutyl ketone, diisobutyl ketone, etc., can be used alone or in combination. Even if the resulting slurry is a homogeneous solution, and even if the solute that does not dissolve in the dispersion solvent is an inorganic solid electrolyte and / or the polymer electrolyte composition for lithium-ion secondary batteries of the present invention, it can be prepared by the above general preparation method. It is desirable to remove as much residual solvent and water as possible from the solid electrolyte layer obtained by removing the dispersion solvent. For example, this can be achieved by evacuating under a vacuum for 1 to 48 hours under heating at 30°C to 200°C. The dried solid electrolyte layer of the present invention has high lithium-ion conductivity as well as binding properties. Furthermore, by performing a pressurized heat treatment, the porosity can be reduced and the particle interface adhesion can be increased. When inorganic solid electrolytes are pressure-molded alone, they have almost no binding properties, resulting in a thick electrolyte film. However, the polymer electrolyte composition for lithium-ion secondary batteries of the present invention exhibits high binding properties by being crosslinked, making it possible to manufacture a thinner solid electrolyte layer.

[0156] Since the solid electrolyte layer of the present invention is used as a polymer electrolyte for lithium-ion secondary batteries, it can be suitably molded into a sheet compared to the case where only an inorganic solid electrolyte is used. The thickness of the polymer electrolyte of the present invention when applied to a secondary battery is not particularly limited, but for example, it can be 0.1 μm to 2000 μm, preferably 0.5 μm to 1000 μm, and more preferably 1 μm to 500 μm.

[0157] <<Electrodes (Positive Electrode, Negative Electrode)>> While known electrodes (positive electrode, negative electrode) can be used, an example of an electrode having an electrode mixture layer on a current collector is provided, and it is preferable to use the polymer electrolyte of the present invention in the electrode mixture layer. It is preferable that the electrode mixture layer of the present invention contains at least the polymer electrolyte and active material of the present invention. It is preferable that the electrode of the present invention is composed of at least the electrode mixture layer and current collector of the present invention.

[0158] As described above, the electrodes are divided into a positive electrode and a negative electrode, and known current collectors can be used for each. Specifically, for the positive electrode, metals such as aluminum, nickel, stainless steel, gold, platinum, and titanium are used as current collectors. For the negative electrode, metals such as copper, nickel, stainless steel, gold, platinum, and titanium are used as current collectors.

[0159] Furthermore, the electrode mixture layer is divided into a positive electrode mixture layer and a negative electrode mixture layer, each containing at least a positive electrode active material or a negative electrode active material and the polymer electrolyte of the present invention, and may also contain an inorganic solid electrolyte, a conductive additive, a binder, and a thickener.

[0160] The positive electrode active material used in this invention is LiMO 2 LiM 2 O 4 Li 2 MO 3 LiMEO 4This is a lithium metal-containing composite oxide powder having one of the following compositions. Here, M mainly consists of a transition metal and contains at least one of Co, Mn, Ni, Cr, Fe, and Ti. Although M consists of a transition metal, Al, Ga, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc. may also be added in addition to transition metals. E contains at least one of P and Si. The particle size of the positive electrode active material is preferably 50 μm or less, and more preferably 20 μm or less. These active materials have an electromotive force of 3 V (vs. Li / Li+) or more.

[0161] Specific examples of positive electrode active materials include lithium cobalt oxide, lithium nickel oxide, nickel / cobalt / lithium manganese oxide (ternary system), spinel-type lithium manganese oxide, and lithium iron phosphate.

[0162] The negative electrode active material used in this invention is either a carbon material (natural graphite, artificial graphite, amorphous carbon, etc.) having a structure (intercalary compound) capable of intercalating and releasing alkali metal ions such as lithium ions, or a metal such as lithium, aluminum-based compounds, tin-based compounds, silicon-based compounds, or titanium-based compounds capable of intercalating and releasing alkali metal ions such as lithium ions. In this invention, the use of silicon-based compounds is preferable. In the case of powder, the particle size is preferably 10 nm to 100 μm, and more preferably 20 nm to 20 μm. It may also be used as a mixed active material of metal and carbon material.

[0163] In the electrode mixture layer of the present invention, the content of the polymer electrolyte of the present invention is preferably 0.1 to 70% by mass, more preferably 0.3 to 60% by mass, and even more preferably 0.5 to 50% by mass, in 100% by mass of the electrode mixture layer.

[0164] The inorganic solid electrolyte used in the electrode of the present invention can be the inorganic solid electrolyte described above.

[0165] In the electrode mixture layer of the present invention, if an inorganic solid electrolyte is included, the content of the polymer electrolyte of the present invention in 100% by mass of the electrode mixture layer is preferably 0.1 to 10% by mass, more preferably 0.3 to 7% by mass, and even more preferably 0.5 to 5% by mass.

[0166] When using conductive additives, known conductive additives can be used, such as graphite, furnace black, acetylene black, Ketjen black or other conductive carbon blacks, carbon fibers such as carbon nanotubes, or metal powders. One or more of these conductive additives may be used. These conductive additives are added in amounts of 5 parts by mass or less, more preferably 3 parts by mass or less, for example, 0.01 to 2 parts by mass, relative to 100 parts by mass of the active material.

[0167] As a binder, one or more compounds selected from fluororesins such as PVdF, fluororubber, acrylic rubber, modified acrylic rubber, styrene-butadiene rubber, acrylic polymers, and vinyl polymers can be used. These binders are added in amounts of 5 parts by mass or less, more preferably 3 parts by mass or less, for example, 0.01 to 2 parts by mass, relative to 100 parts by mass of the active material.

[0168] Specific examples of thickeners include carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose and their salts (alkali metal salts such as sodium salts, ammonium salts), polyvinyl alcohol, polyacrylates, polyethylene oxide, etc. One or more of these thickeners may be used. These thickeners are added in amounts of 5 parts by mass or less, more preferably 3 parts by mass or less, for example, 0.01 to 2 parts by mass, relative to 100 parts by mass of the active material. Furthermore, if the viscosity of the coating solution is low, a thickener can be used in combination.

[0169] The method for manufacturing the positive electrode and negative electrode, which comprise a current collector and positive electrode mixture layer and negative electrode mixture layer, is not particularly limited and general methods can be used. For example, a paste (coating liquid) of the positive electrode material and negative electrode material, consisting of a positive electrode active material or negative electrode active material, a conductive additive, a binder, an organic solvent such as butyl butyrate, and a thickener if necessary, is uniformly applied to the surface of the current collector to an appropriate thickness using a doctor blade method or a silkscreen method.

[0170] For example, in the doctor blade method, negative electrode active material powder, positive electrode active material powder, conductive additive, binder, etc., are dispersed in an organic solvent to form a slurry, which is then applied to a metal electrode substrate. After application, the slurry is uniformly spread to an appropriate thickness using a blade with a predetermined slit width. After the active material is applied, the electrodes are dried to remove excess organic solvent, for example, by using hot air at 100°C or under reduced pressure at 80°C. After drying, the electrodes are manufactured by press molding using a press device.

[0171] <<Specific Configuration of Lithium-ion Secondary Battery>> Examples of the stacked configurations of the lithium-ion secondary battery of the present invention include the following: It is preferable that the polymer electrolyte for lithium-ion secondary batteries of the present invention is contained in any or all of the positive electrode, negative electrode, and solid electrolyte layer. A stacked configuration in which the positive electrode, solid electrolyte layer, and negative electrode are stacked in order; A stacked configuration in which the positive electrode, polymer electrolyte, and negative electrode are stacked in order; A stacked configuration in which the positive electrode, polymer electrolyte, solid electrolyte layer, polymer electrolyte, and negative electrode are stacked in order; A stacked configuration in which the positive electrode, solid electrolyte layer, polymer electrolyte, and negative electrode are stacked in order; A stacked configuration in which the positive electrode, polymer electrolyte, solid electrolyte layer, and negative electrode are stacked in order.

[0172] The lithium-ion secondary battery of the present invention is a lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, and it is preferable that the electrodes of the present invention are used for one or both of the positive and negative electrodes. The lithium-ion secondary battery of the present invention is a lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, and it is preferable that the solid electrolyte layer is a solid electrolyte layer containing at least an inorganic solid electrolyte, and that the polymer electrolyte for lithium-ion secondary batteries of the present invention is laminated on one or both sides of the solid electrolyte layer.

[0173] The shape of the lithium-ion secondary battery of the present invention is not limited, but examples include coin-type, cylindrical, and sheet-type batteries, and a structure in which two or more batteries are stacked is also acceptable.

[0174] The polymer electrolyte composition, polymer electrolyte, and lithium-ion secondary battery of the present invention can adapt to the volume expansion and contraction of the active material during charging and discharging, possess high compressive resistance under high confinement pressure, and have high lithium-ion conductivity. Furthermore, they are excellent at suppressing internal short circuits caused by dendrites, and are therefore useful in batteries for electric vehicles and hybrid vehicles, batteries for household power storage, and batteries for electronic devices such as mobile phones and personal computers.

[0175] The present invention will be specifically described by examples and comparative examples. However, the present invention is not limited to these. In the event of any discrepancy between the descriptions in the text and the descriptions in the tables, the descriptions in the tables shall prevail.

[0176] [Production Example 1-1] To a flask for the synthesis of cyclic ether compound 1 (MBOx), 320 parts by mass of 3-ethyl-3-oxetane methanol and 694 parts by mass of potassium hydroxide were added, and the solvent was added. The mixture was stirred at room temperature for 1 hour. The reaction mixture was cooled to 10°C, and while maintaining stirring, 967 parts by mass (2.1 equivalents) of 1-bromo-4-methoxybutane were added dropwise. After the addition was complete, the reaction was carried out for 44 hours. Subsequently, an oil-water separation operation was performed, and the resulting organic layer was concentrated to obtain 420 parts by mass of cyclic ether compound 1 (MBOx).

[0177] [Production Example 1-2] Synthesis of Cyclic Ether Compound 2 (AllOx) The synthesis was carried out in the same manner as in Production Example 1-1, except that 1-bromo-4-methoxybutane was replaced with allyl bromide, to obtain Cyclic ether compound 2 (AllOx).

[0178] [Production Example 1-3] Synthesis of 1-methoxy-4-(4-methoxybutoxy)butane (Formula (D-3), BGME) 100 parts by mass of 1-chloro-4-methoxybutane and 81 parts by mass of potassium hydroxide were added to a flask and stirred at 100°C for 1 hour. While maintaining stirring, 235 parts by mass of 4-methoxybutanol were added dropwise, and after the addition was complete, the reaction was carried out at 120°C for 20 hours. After the reaction was complete, water was added to obtain the organic layer. The obtained organic layer was concentrated and purified by vacuum distillation to obtain 101 parts by mass of 1-methoxy-4-(4-methoxybutoxy)butane.

[0179] [Production Example 1-4] 20 parts by mass of trimethylolpropane, 50.2 parts by mass of potassium hydroxide, and 232.9 parts by mass of dimethyl sulfoxide were added to a flask for the synthesis of 7-ethyl-((2-methoxyethoxy)methyl)-2,5,9,12-tetraoxatridecane (formula (E-9), TMPEG), and the mixture was stirred at room temperature for 1 hour. While maintaining stirring, 93.2 parts by mass of 1-bromo-2-methoxyethane was added dropwise, and the reaction was carried out for 20 hours after the addition was complete. After the reaction was complete, water was added, and the mixture was extracted twice with toluene. The resulting organic layer was concentrated and then purified by vacuum distillation to obtain 21.1 parts by mass of 7-ethyl-((2-methoxyethoxy)methyl)-2,5,9,12-tetraoxatridecane.

[0180] The structures of the obtained cyclic ether compounds are summarized below, along with the results of their chemical structure identification (NMR).

[0181] Cyclic ether compound 1 (MBOx) [Chemical formula 30] < 1HNMR> 400 MHz, δ, ppm from tetramethylsilane (TMS) in CDCl3: 0.87 (t, 3H, J = 7.6 Hz), 1.61~1.67 (m, 4H), 1.73 (q, 2H, J = 7.5 Hz), 3.32 (s, 3H), 3.36~3.40 (m, 2H), 3.45~3.50 (m, 2H), 3.52 (s, 2H), 4.36 (d, 2H, J = 6.0 Hz), 4.44 (d, 2H, J= 5.5 Hz 13 C-NMR> 100 MHz, δ, ppm from TMS in CDCl3: 8.34, 26.4, 26.5, 26.9, 43.5, 58.7, 71.4, 72.7, 73.5, 78.7

[0182] Cyclic ethyl compound 2 (AllOx) [Chemical 31] < 1 HNMR> 400 MHz, δ, ppm from tetramethylsilane (TMS) in CDCl3: 0.88 (t, 3H, J = 7.6Hz), 1.75 (q, 2H, J = 7.5Hz), 3.55 (s, 2H), 4.00~4.02 (m, 2H), 4.38 (d, 2H, J = 6.0 Hz), 4.45 (d, 2H, J = 6.0 Hz), 5.17~5.31 (m, 2H), 5.86~5.95 (m, 1H) < 13 C-NMR>100 MHz, δ, ppm from TMS in CDCl3: 8.32, 26.84, 43.49, 72.49, 72.88, 78.71, 117.20, 134.88

[0183] 1-メトキシ-4-(4-メトキシブトキシ)ブタン (Formula (D-3), BGME) [Chemical 32] < 1 HNMR> 400 MHz, δ, ppm from tetramethylsilane (TMS) in CDCl3: 1.60-1.63 (m, 8H), 3.31 (s, 6H), 3.36-3.42 (m, 8H).

[0184] 7-Ethyl-((2-methoxyethoxy)methyl)-2,5,9,12-tetraoxatridecane (formula (E-9), TMPEG) [Chemical Formula 33] < 1 H-NMR > 400 MHz, δ, ppm from tetramethylsilane (TMS) in CDCl3: 0.84 (t, 3H, J = 7.8 Hz), 1.39 (q, 2H, J = 7.3 Hz) ), 3.34 (s, 6H), 3.37 (s, 9H), 3.50-3.57 (m, 12H)

[0185] [Production Example 2] (Production of polymerization catalyst for polyether polymer 2) Ten parts by mass of tributyltin chloride and 35 parts by mass of tributylphosphate were placed in a three-necked flask equipped with a stirrer, thermometer, and distillation apparatus. The flask was heated at 250°C for 20 minutes while stirring under a nitrogen stream, and the distillate was removed to obtain a solid condensation material as a residue. This was used as a polymerization catalyst in the following polymerization examples.

[0186] [Polymerization Example 1] Polyether Polymer 1 (P(MBOx / _ / AllOx)) 98.4 parts by mass of cyclic ether compound 1 (MBOx) as component X of the polyether polymer composition, 1.6 parts by mass of cyclic ether compound 2 (AllOx) as component Z, and 1,2-dichloroethane as solvent were added, and the mixture was cooled to 0°C while stirring. BF was added as a polymerization initiator while maintaining the temperature. 3 ・Et 2 1.6 parts by mass of oxygen were added over 5 minutes to a total of 2 mol% of the polyether polymer composition, and the polymerization reaction was carried out for a further 2 hours. A 4 M NaCl / 1 M NaOH aqueous solution was added to stop the reaction, and oil-water separation was performed. Subsequently, purification by reprecipitation and vacuum drying at 50°C were performed to obtain polyether polymer 1. The following tests were performed using the obtained polyether polymer 1, and the results are shown in Table 1. Note that the notation in parentheses in P(MBOx / _ / AllOx) represents the units in X, Y, and Z, respectively. "_" indicates that it is not included in the composition. The following examples also use the same notation to show the composition of the polyether polymer.

[0187] The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the obtained polyether polymer 1 were measured. The results are shown in Table 1. The content (mol%) of each unit shown in Table 1 was calculated from the NMR spectrum.

[0188] <Weight-average molecular weight (Mw), number-average molecular weight (Mn)> The molecular weight of the polymer was measured in polystyrene equivalent using gel permeation chromatography (GPC) with tetrahydrofuran (THF) as the solvent. Based on the measurement results, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) were calculated. For the measurements, a Shimadzu LC-2030 (RID-20A) and three linked GPC columns KF-801, KF-803L, and KF-806L from Resonaq Corporation were used. The flow rate was 1.0 mL / min, the concentration was 10 mg of polymer / 8 mL of THF, the injection volume was 100 μL, and the column temperature was 40°C.

[0189] [Polymerization Example 2] Polyether Polymer 2 (P(PO / EO / AGE)) The inside of a 3 L glass four-necked flask was purged with nitrogen, and 1.0 part by mass of the polymerization catalyst shown in Production Example 2, 16.8 parts by mass of ethylene oxide adjusted to a moisture content of 10 ppm or less, 53.8 parts by mass of propylene oxide, 5.4 parts by mass of allyl glycidyl ether, 0.12 parts by mass of tert-butanol, and 333 parts by mass of n-hexane as a solvent were charged. While monitoring the polymerization rate by gas chromatography, 80 parts by mass of ethylene oxide were added sequentially. The polymerization temperature at this time was 20°C, and the reaction was carried out for 10 hours. The polymerization reaction was stopped by adding methanol. After removing polyether copolymer 2 by decantation, it was dried at 25°C under normal pressure for 24 hours, and then at 40°C under reduced pressure for 10 hours to obtain polyether polymer 2.

[0190] The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the obtained ion-conductive polyether polymer 2 were measured. The results are shown in Table 1. The content (mol%) of each unit shown in Table 1 was calculated from the NMR spectrum.

[0191] <Weight Average Molecular Weight (Mw), Number Average Molecular Weight (Mn)> A polymer was dissolved in N,N-dimethylformamide (DMF) as a solvent, and the molecular weight was measured in terms of polystyrene using gel permeation chromatography (GPC). Based on the measurement results, the weight average molecular weight (Mw) and the number average molecular weight (Mn) were calculated. The GPC measurement was performed at 60°C using RID-6A manufactured by Shimadzu Corporation, and Shodex KD-807, KD-806, KD-806M and KD-803 columns manufactured by Showa Denko K.K.

[0192] [Polymerization Example 3] Polyether Polymer 2 (P(_ / EO-EM2 / AGE)) The inside of a 3 L glass four-necked flask was purged with nitrogen, and 1.0 part by mass of the polymerization catalyst obtained in Production Example 2, 24 parts by mass of ethylene oxide adjusted to a water content of 10 ppm or less, 48 parts by mass of diethylene glycol glycidyl methyl ether (EM2), 4 parts by mass of allyl glycidyl ether, and 400 parts by mass of n-hexane as a solvent were charged, and 24 parts by mass of ethylene oxide was sequentially added while tracking the polymerization rate by gas chromatography. The polymerization temperature at this time was set to 20°C, and the reaction was carried out for 10 hours. The polymerization reaction was stopped by adding methanol. After the polyether copolymer 2 was taken out by decantation, it was dried at 25°C under normal pressure for 24 hours, and further at 40°C under reduced pressure for 10 hours to obtain Polyether Polymer 3.

[0193]

[0194] [Example 1] 100 parts by mass of the polyether polymer 1 obtained in Polymerization Example 1, and Li(CF as a lithium salt 3 SO 2 ) 2 N of 81 parts by mass were mixed to prepare ion-conductive polymer 1. Next, 165 parts by mass of butylene carbonate (manufactured by BLDpharm, trade name: 4-ethyl-1,3-dioxolan-2-one, CAS No. 4437-85-8), which is a heterocyclic compound as an ion-conductive compound, and 10 parts by mass of cellulose nanofiber A (manufactured by Oji Holdings, diameter 3 nm) as nanofibers were added, followed by stirring and mixing to prepare Polymer Electrolyte Composition 1 for Lithium Ion Secondary Batteries.

[0195] 0.9 parts by mass of Irgacure 1173 (manufactured by BASF, α-hydroxyacetophenone) as a reaction initiator and 1.5 parts by mass of Karenz MT BD1 (manufactured by Resonac, 1,4-bis(3-mercaptobutyryloxy)butane) as a crosslinking aid were stirred and mixed into the polymer electrolyte composition 1 for lithium ion secondary batteries obtained above, the mixture was applied onto a PET film, and UV crosslinking (temperature 25°C, exposure time 0.5 minutes, wavelength 365 nm (1000 mJ / cm²), light source: halogen) was performed to produce a polymer electrolyte 1 for lithium ion secondary batteries having a film thickness of 120 μm. The following tests were carried out using the obtained polymer electrolyte 1 for lithium ion secondary batteries. The results are shown in Table 2.

[0196] [Examples 2 to 4] The same procedure as in Example 1 was carried out except that the compositions were changed to those shown in Table 2, to produce polymer electrolyte compositions 2 to 4 for lithium ion secondary batteries and polymer electrolytes 2 to 4 for lithium ion secondary batteries, and the following tests were carried out. The results are shown in Table 2.

[0197] [Example 5] 100 parts by mass of the polyether polymer 1 obtained in Polymerization Example 1 and 94 parts by mass of Li(CF as a lithium salt compound were mixed to prepare an ion-conductive polymer 5, then 165 parts by mass of BGME synthesized in Production Example 1-3 which is a linear ether compound as an ion-conductive compound and 7.5 parts by mass of cellulose nanofiber A as nanofibers were added and stirred and mixed to prepare a polymer electrolyte composition 5 for lithium ion secondary batteries. 3 SO 2 ) 2 Nを94質量部を混合し、イオン伝導性ポリマー5を作製し、次いで、イオン伝導性化合物として直鎖型エーテル系化合物である製造例1-3で合成したBGMEを165質量部、ナノファイバーとしてセルロースナノファイバーAを7.5質量部添加し、攪拌混合を行い、リチウムイオン二次電池用ポリマー電解質組成物5を作製した。

[0198] 0.9 parts by mass of Irgacure 1173 as a reaction initiator and 1.5 parts by mass of Karenz MT BD1 as a crosslinking aid were stirred and mixed into the polymer electrolyte composition 5 for lithium ion secondary batteries obtained above, the mixture was applied onto a PET film, and UV crosslinking was performed to produce a polymer electrolyte 5 for lithium ion secondary batteries. The following tests were carried out using the obtained polymer electrolyte 5 for lithium ion secondary batteries. The results are shown in Table 2.

[0199] [Example 6] 100 parts by mass of the polyether polymer 2 obtained in Polymerization Example 2, and Li(CF) as the lithium salt compound. 3 SO 2 ) 2 72 parts by mass of N were mixed to prepare an ion-conducting polymer 6. Then, 167 parts by mass of TMPEG, a branched ether compound synthesized in Production Example 1-4 as an ion-conducting compound, and 5.3 parts by mass of cellulose nanofiber A as a nanofiber were added, and the mixture was stirred to prepare a polymer electrolyte composition 6 for lithium-ion secondary batteries.

[0200] To the polymer electrolyte composition 6 for lithium-ion secondary batteries obtained above, 1.5 parts by mass of benzophenone was added as a reaction initiator and 20 parts by mass of trimethylolpropane trimethacrylate was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film and UV crosslinking was used to produce a polymer electrolyte 6 for lithium-ion secondary batteries. The following tests were conducted using the obtained polymer electrolyte 6 for lithium-ion secondary batteries. The results are shown in Table 2.

[0201] [Example 7] 100 parts by mass of the polyether polymer 2 obtained in Polymerization Example 2, and Li(CF) as the lithium salt compound. 3 SO 2 ) 2 109 parts by mass of N was mixed to prepare an ion-conducting polymer 7. Then, 34 parts by mass of BGME, a chain-type ether compound synthesized in Production Example 1-3, 134 parts by mass of TMPEG, a branched ether compound synthesized in Production Example 1-4, and 5.3 parts by mass of cellulose nanofiber A were added as nanofibers, and the mixture was stirred to prepare a polymer electrolyte composition 6 for lithium-ion secondary batteries.

[0202] To the lithium-ion secondary battery polymer electrolyte composition 6 obtained above, 1.5 parts by mass of benzophenone as a reaction initiator and 20 parts by mass of trimethylolpropane trimethacrylate as a crosslinking aid were stirred and mixed. This mixture was then coated onto a PET film, and a lithium-ion secondary battery polymer electrolyte 7 was prepared by UV crosslinking. The following tests were conducted using the obtained lithium-ion secondary battery polymer electrolyte 7. The results are shown in Table 2.

[0203] [Example 8] 100 parts by mass of the polyether polymer 1 obtained in Polymerization Example 1, and Li(CF) as the lithium salt compound. 3 SO 2 ) 2 68 parts by mass of N were mixed to prepare an ion-conducting polymer 8. Then, 102 parts by mass of butylene carbonate, a heterocyclic compound, was added as an ion-conducting compound, and 5.0 parts by mass of cellulose nanofiber B (manufactured by Mori Machinery, diameter: 30-200 nm) was added as a nanofiber. The mixture was stirred and mixed to prepare a polymer electrolyte composition 8 for lithium-ion secondary batteries.

[0204] To the polymer electrolyte composition 8 for lithium-ion secondary batteries obtained above, 0.9 parts by mass of Irgacure 1173 was added as a reaction initiator and 1.5 parts by mass of Karenz MT BD1 was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film, and a polymer electrolyte 8 for lithium-ion secondary batteries was prepared by UV crosslinking. The following tests were conducted using the obtained polymer electrolyte 8 for lithium-ion secondary batteries. The results are shown in Table 2.

[0205] [Example 9] 100 parts by mass of the polyether polymer 1 obtained in Polymerization Example 1, and Li(CF) as the lithium salt compound. 3 SO 2 ) 2 124 parts by mass of N was mixed to prepare an ion-conducting polymer 9. Then, 240 parts by mass of butylene carbonate, a heterocyclic compound, was added as an ion-conducting compound, and 3.0 parts by mass of cellulose nanofiber B (manufactured by Mori Machinery, diameter: 30-200 nm) was added as a nanofiber. The mixture was stirred and mixed to prepare a polymer electrolyte composition 9 for lithium-ion secondary batteries.

[0206] To the polymer electrolyte composition 9 for lithium-ion secondary batteries obtained above, 0.9 parts by mass of Irgacure 1173 was added as a reaction initiator and 1.5 parts by mass of Karenz MT BD1 was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film, and a polymer electrolyte 9 for lithium-ion secondary batteries was prepared by UV crosslinking. The following tests were conducted using the obtained polymer electrolyte 9 for lithium-ion secondary batteries. The results are shown in Table 2.

[0207] [Comparative Example 1] 100 parts by mass of the polyether polymer 1 obtained in polymerization example 1, and Li(CF) as the lithium salt. 3 SO 2 ) 2 126 parts by mass of N were mixed to prepare an ion-conducting polymer 10. Next, 300 parts by mass of butylene carbonate, a heterocyclic compound, was added as an ion-conducting compound, and the mixture was stirred to prepare a polymer electrolyte composition 10 for lithium-ion secondary batteries.

[0208] To the polymer electrolyte composition 10 for lithium-ion secondary batteries obtained above, 0.9 parts by mass of Irgacure 1173 was added as a reaction initiator and 1.5 parts by mass of Karenz MT BD1 was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film, and a polymer electrolyte 10 for lithium-ion secondary batteries was prepared by UV crosslinking. The following tests were conducted using the obtained polymer electrolyte 10 for lithium-ion secondary batteries. The results are shown in Table 2.

[0209] [Comparative Example 2] 100 parts by mass of the polyether polymer 2 obtained in polymerization example 2, and Li(CF) as the lithium salt compound. 3 SO 2 ) 2 72 parts by mass of N were mixed to prepare an ion-conducting polymer 11. Then, 84 parts by mass of TMPEG, a branched ether compound synthesized in Production Example 1-4, was added as an ion-conducting compound, and the mixture was stirred to prepare a polymer electrolyte composition 11 for lithium-ion secondary batteries.

[0210] To the polymer electrolyte composition 11 for lithium-ion secondary batteries obtained above, 1.5 parts by mass of benzophenone was added as a reaction initiator and 20 parts by mass of trimethylolpropane trimethacrylate was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film and UV crosslinking was used to produce a polymer electrolyte 11 for lithium-ion secondary batteries. The following tests were conducted using the obtained polymer electrolyte 11 for lithium-ion secondary batteries. The results are shown in Table 2.

[0211] [Comparative Example 3] 100 parts by mass of the polyether polymer 2 obtained in polymerization example 2, and Li(CF) as the lithium salt compound.3 SO 2 ) 2 A polymer electrolyte composition 12 for lithium-ion secondary batteries was prepared by stirring and mixing 34 parts by mass of N.

[0212] To the polymer electrolyte composition 12 for lithium-ion secondary batteries obtained above, 1.5 parts by mass of benzophenone was added as a reaction initiator and 20 parts by mass of trimethylolpropane trimethacrylate was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film and UV crosslinking was used to produce a polymer electrolyte 12 for lithium-ion secondary batteries. The following tests were conducted using the obtained polymer electrolyte 12 for lithium-ion secondary batteries. The results are shown in Table 2.

[0213] [Comparative Example 4] 100 parts by mass of the polyether polymer 3 obtained in polymerization example 3, and Li(CF) as the lithium salt compound. 3 SO 2 ) 2 A polymer electrolyte composition 13 for lithium-ion secondary batteries was prepared by stirring and mixing 39 parts by mass of N.

[0214] To the polymer electrolyte composition 13 for lithium-ion secondary batteries obtained above, 1.4 parts by mass of benzophenone was added as a reaction initiator and 3.5 parts by mass of N,N'-phenylenebismaleimide was added as a crosslinking aid and stirred and mixed. This mixture was then coated onto a PET film and UV crosslinking was used to produce a polymer electrolyte 13 for lithium-ion secondary batteries. The following tests were conducted using the obtained polymer electrolyte 13 for lithium-ion secondary batteries. The results are shown in Table 2.

[0215] [Comparative Example 5] 100 parts by mass of PVDF-HFP (poly(vinylidene fluoride-co-hexafluoropropylene)) and Li(CF) as a lithium salt compound. 3 SO 2 ) 2 A polymer electrolyte composition 14 for lithium-ion secondary batteries was prepared by stirring and mixing 1 part by mass of N and 3 parts by mass of BGME as an ion-conducting compound.

[0216] The polymer electrolyte composition 11 for lithium-ion secondary batteries obtained above was coated onto a PET film, and a polymer electrolyte 14 for lithium-ion secondary batteries was fabricated by vacuum hot pressing under reduced pressure at a temperature of 90°C, a press pressure of 20 kN, and for 3 minutes. The following tests were performed using the obtained polymer electrolyte 14 for lithium-ion secondary batteries. The results are shown in Table 2.

[0217] [Compression Resistance] The following tests were conducted to evaluate the volume expansion and contraction adaptation of the active material and its compression resistance under confining pressure.

[0218] [Evaluation of Compressive Strength] A polymer electrolyte was processed into a 3 cm square and sandwiched between PET films. Next, this was sandwiched between SUS plates, and a pressure of 1 MPa was applied for 1 minute using a high-pressure jack J-1 (manufactured by AS ONE). Furthermore, the pressure was gradually increased to 2 MPa, 3 MPa, and so on, and the test was carried out until the polymer electrolyte ruptured or the pressure reached 10 MPa. The pressure at which the polymer electrolyte could be maintained without rupture was defined as the compressive strength. The test was conducted at a temperature of 25°C and under atmospheric pressure.

[0219] [Evaluation of Compressive Strain] The film thickness of the polymer electrolyte crosslinked membrane was measured when a compressive pressure of compressive strength was applied for 1 minute, and this was defined as the film thickness during compression (h1). The degree of compressive strain was calculated from the film thickness before compression (h0). Degree of compressive strain (%) = {(h1 - h0) / h0} × 100

[0220] [Evaluation of Compression Set] The compression pressure was released, and the film thickness of the polymer electrolyte was measured after 10 minutes. This was defined as the film thickness after compression (h2). The compression set was calculated from the film thickness before compression (h0). The compression set was calculated using the following formula, and the resulting value is an absolute value. Compression Set (%) = |{(h2 - h0) / h0}| × 100

[0221] [Evaluation of Ion Conductivity of Polymer Electrolytes] A polymer electrolyte was placed on a SUS spacer, and a SUS spacer was attached to the counter electrode to create a SUS blocking cell. An AC impedance test was then performed using a potentiometer / galvanostat apparatus.

[0222] [AC Impedance Test] A SUS blocking cell of polymer electrolyte was fabricated, and an AC impedance test was performed using a potentiometer / galvanostat (device name: BioLogic SP-300). The resistance (Ω) of the polymer electrolyte was calculated from the diameter of the semicircular arc in the real axis direction obtained from the Cole-Cole plot. In addition, the ionic conductivity of the cell was calculated from the cell thickness and surface area using the following formula. The test temperature was 25°C. Measurements were performed with a voltage amplitude of 20 mV and a measurement frequency range of 7 MHz to 1 Hz. σ = 1 / R × (d / A) σ: Ionic conductivity of polymer electrolyte (S / cm) R: Resistance of polymer electrolyte (Ω) d: Thickness of polymer electrolyte (cm) A: Surface area of ​​polymer electrolyte (cm) 2 )

[0223] [Evaluation of Li ion transport fraction of polymer electrolyte] (Preparation of evaluation cell) A Li symmetric cell was prepared by placing polymer electrolyte 1 on a Li foil and attaching a Li foil to the counter electrode. (Calculation of Li ion transport fraction) The Li ion transport fraction can be calculated using the following formula, based on the interfacial resistance values ​​before and after polarization, the initial current value obtained from the chronoamperometry test, and the steady-state current value. tLi+ = (Is × (V - I0 × R0)) / (I0 × (V - Is × Rs)) tLi+: Li ion transport fraction of polymer electrolyte I0: Initial current value of chronoamperometry test (A) Is: Steady-state current value of chronoamperometry test (A) R0: Interfacial resistance value before polarization (Ω) Rs: Interfacial resistance value after polarization (Ω) V: DC voltage (V) (Measurement of interfacial resistance values ​​before and after polarization (AC impedance test)) A Li symmetric cell of polymer electrolyte was prepared, and an AC impedance test was performed using a potentiometer / galvanostat apparatus. The interfacial resistance value was calculated from the size of the semicircle derived from the interfacial resistance obtained from the Cole-Cole plot. The test temperature was 25°C, and measurements were performed with a voltage amplitude of 7mV and a measurement frequency range of 7MHz to 100mHz. (Chronoamperometry Test) After performing an AC impedance test, the open-circuit voltage (OCV) was measured for one minute, and then a chronoamperometry measurement was performed. The test temperature was 25°C. The measurement was performed with a DC voltage of 7mV for a measurement time of 3 hours, and the initial current value and the steady-state current value after 3 hours were measured.

[0224] [Evaluation of Lithium Ion Conductivity] The lithium ion conductivity can be determined as the product of the above-mentioned ion conductivity and lithium ion transference number. The lithium ion conductivity of 1×10 -5 (S / cm) or higher was judged to be favorable. Lithium ion conductivity = Ion conductivity × Lithium ion transference number

[0225] [Deterioration Evaluation of Sulfide Solid Electrolyte] Each of the above polymer electrolytes 1 to 14 was placed on a SUS spacer, and bonded to a pellet of argyrodite-type sulfide solid electrolyte (manufactured by NEI Corporation, Li₆PS₅Cl) to prepare a composite of the sulfide solid electrolyte and the polymer electrolyte, which was then subjected to heat treatment at 60°C for 1 week. The sulfide solid electrolyte was taken from the above composite and filled into a solid NMR sample tube, and a ³¹P-NMR test was performed using a nuclear magnetic resonance apparatus (NMR). (³¹P-NMR Test) Measurement was carried out using an NMR apparatus (apparatus name: ECA400WB, manufactured by JEOL Ltd.). As the evaluation method, the resistance was evaluated based on the presence or absence of the spectrum derived from the PS₄³⁻ unit contained in the sulfide solid electrolyte and the spectrum derived from the P₂S₇⁴⁻ unit generated by the decomposition reaction of the sulfide solid electrolyte. The case where the spectrum generated by the decomposition reaction of the sulfide solid electrolyte was not detected was marked as ○, and the case where the spectrum generated by the decomposition reaction of the sulfide solid electrolyte was detected was marked as ×. An evaluation result of ○ indicates that side reactions with the sulfide-based solid electrolyte can be suppressed. Measurement temperature: room temperature Rotation speed: 10 kHz Number of integrations: 8 times Recycle delay: 2,000 seconds Chemical shift reference material: ammonium dihydrogen phosphate (1 ppm)

[0226] [Dendrite Resistance Test of Polymer Electrolyte] For the Li symmetric cell fabricated for measuring the Li ion transference number of the polymer electrolyte, an energization cycle test was performed using a charge-discharge apparatus. I = ±0.1 mA / cm 2 An energization test was performed for 3 hours each, and this was repeated for a maximum of 100 cycles. The number of charge-dischargeable cycles was evaluated. Note that "-" in the table indicates that the test was not performed.

[0227]

[0228] Tables 1 and 2 show that the polymer electrolytes for lithium-ion secondary batteries (Examples 1-6) obtained by crosslinking the polymer electrolyte composition for lithium-ion secondary batteries of the present invention, which includes an ion-conducting polymer, an ion-conducting compound, and nanofibers, exhibit excellent compression resistance and ion conductivity, and thus high dendrite resistance. This suggests that the ion conductivity is uniformly distributed throughout the polymer electrolyte for lithium-ion secondary batteries of the present invention, preventing lithium ions from accumulating locally and allowing for the smooth formation of ion conduction paths. Therefore, it is suggested that the problems associated with solid lithium-ion secondary batteries can be solved by using the polymer electrolyte composition for lithium-ion secondary batteries of the present invention.

[0229] The polymer electrolyte composition for lithium-ion secondary batteries, the polymer electrolyte for lithium-ion secondary batteries, and the lithium-ion secondary battery of the present invention can adapt to the volume expansion and contraction of the active material during charging and discharging, have high compressive resistance under high confinement pressure, and have high lithium-ion conductivity. Therefore, they can be usefully used in batteries for vehicles such as electric vehicles and hybrid vehicles, batteries for household power storage, and batteries for electronic devices such as mobile phones and personal computers.

Claims

1. A polymer electrolyte composition for lithium-ion secondary batteries comprising at least an ion-conducting polymer, an ion-conducting compound, and nanofibers, wherein the compressive strain when crosslinked is -90% to -30%, and the ratio of compressive strain to set compression ([set compression] / [compressive strain]) is -0.5 to -0.

001.

2. The polymer electrolyte composition for lithium-ion secondary batteries according to claim 1, wherein the ion-conducting polymer comprises at least a polyether polymer containing alkyl group units which are structural units derived from alkylene oxide having alkyl groups in its side chains, and a lithium salt compound, wherein the polyether polymer contains alkyl group units in an amount of 5 mol% or more per 100 mol% of structural units.

3. The polymer electrolyte composition for lithium ion secondary batteries according to claim 1, wherein the polyether polymer comprises X units which are structural units derived from an alkylene oxide represented by the following general formula (1), and Z units which are structural units derived from an alkylene oxide represented by the following general formula (2). [In the formula, R 1 are the same or different and each is an alkyl group having 1 to 6 carbon atoms. R 2 are the same or different and each is a hydrogen atom or -CH 2 O{(CH 2 ) a O} b (CH 2 ) c H, which is an alkylene glycol alkyl ether group. The number of repeating units a, which are the same or different, is an integer of 1 to 10, the number of repeating units b, which are the same or different, is an integer of 1 to 6, and the number of repeating units c, which are the same or different, is an integer of 0 to 6. A, which are the same or different, each represent a single bond or an alkylene group having 1 to 4 carbon atoms.] [In the formula, R 3 are the same or different and each is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and R 5 are the same or different and each is a crosslinkable group containing an ethylenically unsaturated double bond represented by -CH 2 OR 8 . R 8 are the same or different and each is an acryl group, a methacryl group, an allyl group or a methallyl group. A, which are the same or different, each represent a single bond or an alkylene group having 1 to 4 carbon atoms.] 4. The polymer electrolyte composition for lithium-ion secondary batteries according to any one of claims 1 to 3, wherein the ion-conducting compound is at least one compound selected from the group consisting of heterocyclic compounds represented by the following general formulas (A) to (C) and ether compounds represented by the following general formulas (D) to (E). [In the formula, R 9 R is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 10 This is a hydrogen atom, -CH 2 O { (CH 2 ) a O} b (CH 2 ) c An alkylene glycol alkyl ether group represented by H, or -CH 2 OR 8 This is a crosslinking group containing an ethylenically unsaturated double bond, represented by R. 8 This group is an acrylic group, a methacrylic group, an allyl group, or a metaallyl group. The repeating unit 'a' is an integer from 1 to 10, the repeating unit 'b' is an integer from 0 to 6, and the repeating unit 'c' is an integer from 0 to 4. [In the formula, R 11 [g is the same or different hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkenyl group, and g is an integer from 0 to 4.] [In the formula, R 12 [The elements are, either identical or different, a hydrogen atom, a C1-C6 alkyl group, or a C1-C6 alkenyl group, and h is an integer from 0 to 8.] (In the formula, R 13 These are identical or different alkyl groups having 1 to 4 carbon atoms, or -(CH 2 ) k CH 2 O-R 14 It is a group represented by R. 14 (The elements are the same or different alkyl groups having 1 to 4 carbon atoms. The repeating units i and j are the same or different, and range from 0 to 3; k is an integer from 1 to 3.) (In the formula, R 15 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or -{(CH 2 ) m CH 2 O} n R 17 That is. R 16 These are identical or different alkyl groups having 1 to 4 carbon atoms, or -{(CH 2 ) m CH 2 O} n R 17 That is. R 17 (The elements are the same or different alkyl groups having 1 to 4 carbon atoms. The number of repetitions, k, is 0 or 1, and m and n are the same or different integers from 1 to 3.) 5. The polymer electrolyte composition for lithium-ion secondary batteries according to claim 1, wherein the nanofibers are cellulose nanofibers.

6. The polymer electrolyte composition for lithium-ion secondary batteries according to claim 2, wherein the content of the ion-conducting compound is 50 to 1200 parts by mass and the content of the nanofiber is 0.5 to 20 parts by mass per 100 parts by mass of the polyether polymer.

7. The polymer electrolyte composition for lithium-ion secondary batteries according to claim 1, further comprising a reaction initiator and a crosslinking aid.

8. A polymer electrolyte for lithium-ion secondary batteries obtained by crosslinking the polymer electrolyte composition for lithium-ion secondary batteries described in claim 7.

9. An electrode mixture layer comprising at least the polymer electrolyte for lithium-ion secondary batteries and the active material described in claim 8, wherein the content of the polymer electrolyte for lithium-ion secondary batteries is 0.1 to 70% by mass in 100% by mass of the electrode mixture layer.

10. The electrode mixture layer according to claim 9, wherein the active material is a silicon-based compound.

11. An electrode comprising at least the electrode mixture layer and current collector described in claim 9.

12. A lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, wherein one or both of the positive electrode and the negative electrode are electrodes as described in claim 11.

13. A lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, wherein the solid electrolyte layer comprises at least the polymer electrolyte for lithium-ion secondary batteries described in claim 8.

14. The lithium-ion secondary battery according to claim 13, wherein the solid electrolyte layer further comprises an inorganic solid electrolyte, and the polymer electrolyte for lithium-ion secondary batteries is present in an amount of 0.1 to 90% by mass of 100% by mass of the solid electrolyte layer.

15. The lithium-ion secondary battery according to claim 14, wherein the inorganic solid electrolyte is a sulfide-based solid electrolyte.

16. A lithium-ion secondary battery comprising at least a positive electrode, a solid electrolyte layer, and a negative electrode, wherein the solid electrolyte layer is a solid electrolyte layer containing at least an inorganic solid electrolyte, and the polymer electrolyte for lithium-ion secondary batteries described in claim 8 is laminated on one or both sides of the solid electrolyte layer.