Method for producing recycled resin, method for producing molded body of recycled resin, recycled resin, film-like molded body, and packaging material
The use of solvents with specific SP values to remove additives and trace chemicals from recycled resin materials addresses quality and performance issues, ensuring consistent and high-quality recycled resin products.
Patent Information
- Application Number
- PCT/JP2026/018016
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-01-22
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for recycling thermoplastic resins face challenges in accurately estimating and effectively removing additives like antioxidants and lubricants, leading to quality degradation and performance variability in recycled resin products, particularly for films and packaging materials.
A method involving the use of organic solvents with specific solubility parameters (SP values) to efficiently remove antioxidants, lubricants, and trace chemicals from plastic materials, followed by a washing step to eliminate residual solvents, ensuring consistent quality and performance.
The method effectively reduces the presence of additives and trace chemicals to acceptable levels, enhancing the mechanical strength and stability of recycled resin products, preventing appearance defects and performance variations.
Smart Images

Figure JP2026018016_19112026_PF_FP_ABST
Abstract
Description
Method for manufacturing recycled resin, method for manufacturing molded articles of recycled resin, recycled resin, film-like molded articles, and packaging materials
[0001] This invention relates to a method for producing recycled resin, a method for producing a molded article of recycled resin, recycled resin, a film-like molded article, and a packaging material.
[0002] This application claims priority under Japanese application No. 2025-081539 filed on 14 May 2025 and Japanese application No. 2026-008830 filed on 22 January 2026, and incorporates all the provisions contained in the said Japanese applications.
[0003] In response to recent environmental issues, the recycling of plastic products is expected to play a significant role, and various recycling methods are being considered. For example, for PET bottles, material recycling, which involves washing and crushing collected products for reuse as raw materials, and chemical recycling, which involves monomerization, have both been established technologies.
[0004] Globally, there is a growing trend towards policies that prohibit the use of resin products made solely from petroleum-derived resins, making the use of recycled resins essential. As the inclusion of recycled resins becomes the standard, recycled resin materials with performance capabilities equivalent to those used in product lines previously made solely from virgin resins will be required.
[0005] Thermoplastic resins, which are used as materials for everyday goods, automotive parts, medical devices, etc., are molded into various shapes by utilizing their property of deforming when heated. To avoid degradation of the resin due to heating during this process, antioxidants are generally mixed into resin pellets.
[0006] Furthermore, thermoplastic resins are resins with excellent moldability and processability. On the other hand, thermoplastic resins can have a high coefficient of friction between resins or contact surfaces after molding, which can cause films to stick together and become difficult to separate, or the frictional resistance to become excessive, hindering the processing steps during transport, winding, or the use of the final product. Therefore, lubricants are generally added to improve the transportability, windingability, and usability of the film or sheet after molding, as well as the usability of the final product.
[0007] However, when recycling collected market products, it is assumed that antioxidants and lubricants of different types and amounts are mixed together, and there is a problem in that it is difficult to estimate how much of these effective additives remain in the materials used to manufacture the recycled resin.
[0008] In resin material recycling, recycled resin is generally obtained through processes such as crushing, washing, heating and melting, and molding of the input material. Although foreign matter may be removed by installing filters, the components contained in the input material are generally carried over to the recycled resin. Therefore, it is not only difficult to estimate the amount of antioxidants that will work effectively, but the decomposition products generated when antioxidants are consumed to suppress resin degradation may become nuclei that lead to visible foreign matter, raising concerns about poor appearance of molded products using recycled resin and a decline in quality such as insufficient mechanical strength. Furthermore, regarding lubricants, it is not only difficult to estimate the amount of lubricants that will work effectively, but if the amount of lubricant remaining in each input material is not uniform, it is a concern that it may lead to variations in product performance and a decrease in stability of recycled resin products.
[0009] Regarding the material recycling of resins, methods have been proposed to improve the material recyclability of resins by removing additives that are of concern to have adverse effects on human health and the environment from the raw resin (see, for example, Patent Documents 1 to 4). In addition, methods have been proposed to improve the material recyclability of resins by removing additives from the raw resin by contacting a resin composition containing additives such as flame retardants with a solvent (see, for example, Patent Document 5).
[0010] Japanese Patent Publication No. 2001-151930, Japanese Patent Publication No. 2002-037914, Japanese Patent Publication No. 2004-123813, Japanese Patent Publication No. 2007-146176, Japanese Patent Publication No. 2003-306575
[0011] However, in the conventional methods described in the above-mentioned patent documents, the additive to be removed is a flame retardant, and the target resin for recycling is a resin used in home appliances, etc., and does not include raw resins for films such as packaging materials that are frequently discarded. Furthermore, in patent documents 1 to 4, heating above the melting temperature of the thermoplastic resin is required in the process of extracting the additive. Therefore, there is a problem that it is difficult to call it sustainable as it has a large environmental burden and some of the resin may also be removed. Moreover, in patent document 5, the thermoplastic resin is brought into contact with the solvent at a temperature below the glass transition temperature, so the removal of the additive tends to be insufficient, resulting in a large amount of residual additive and potentially degrading the quality of molded products using recycled resin.
[0012] One aspect of the present invention aims to provide a method for producing recycled resin that can effectively remove antioxidants, lubricants, and even trace amounts of chemical substances contained in the raw plastic material, thereby avoiding quality degradation caused by these substances.
[0013] A method for producing recycled resin according to one aspect of the present invention is a method for producing recycled resin from a plastic material, wherein the plastic material has an SP value of 7 [cal / cm³]. 3 ] 1/2 Above 13 [cal / cm 3 ] 1/2 The process includes adding the following organic solvents to remove one or more target substances selected from the group consisting of antioxidants, lubricants, and trace chemicals.
[0014] According to one aspect of the present invention, it is possible to provide a method for producing recycled resin that can effectively remove antioxidants, lubricants, and trace chemical substances contained in the raw plastic material, thereby avoiding quality degradation caused by these substances.
[0015] This is a process diagram showing an example of a manufacturing method for recycled resin. This is a schematic cross-sectional view showing an example of a single-layer sheet containing recycled resin. This is a schematic cross-sectional view showing an example of a multilayer sheet containing recycled resin. This is a schematic cross-sectional view showing another example of a multilayer sheet containing recycled resin. This is a schematic cross-sectional view showing an example of a laminate containing recycled resin.
[0016] The following describes specific embodiments of this disclosure in detail with reference to the drawings. However, this disclosure is not limited to the embodiments described below, and various modifications are possible without altering its essence.
[0017] In this specification, the notation "a to b" (where a and b are arbitrary numbers) means "a or greater and b or less" unless otherwise specified. Furthermore, to facilitate understanding of the descriptions in this disclosure, the same reference numerals are used for identical components in each drawing, and redundant explanations are omitted. Additionally, since the drawings are schematic diagrams for illustrative purposes, the scale of each component may differ from the actual scale.
[0018] ≪1. Method for Manufacturing Recycled Resin≫ Figure 1 is a process diagram showing an example of the flow of the method for manufacturing recycled resin according to this embodiment. The method for manufacturing recycled resin is a method for manufacturing recycled resin from plastic material and includes a removal step to remove the target substance. It also includes other steps as needed, such as a washing step, a re-addition step, and a melt molding step.
[0019] <Removal Process> In the removal process, the plastic material has a solubility parameter (SP value) of 7 [cal / cm³]. 3 ] 1/2 Above 13 [cal / cm 3 ] 1/2 This process involves adding the following organic solvents to remove one or more target substances selected from the group consisting of antioxidants, lubricants, and trace chemical substances.
[0020] In the removal process, by adding an organic solvent with a specific SP value, it becomes possible to remove antioxidants such as primary antioxidants and secondary antioxidants, or lubricants, from the input material, regardless of their type. Furthermore, by adding an organic solvent with a specific SP value, it becomes possible to remove trace chemical substances that may have adverse effects on human health or the environment, which may have been unintentionally mixed in during the manufacturing, use, or disposal processes of plastics, from the input material. If the SP value of the organic solvent is less than 7 or greater than 13, it will deviate significantly from the SP value of the target substance to be removed, resulting in a large and different cohesive energy density. This can lead to mutual repulsion and a decrease in affinity, potentially preventing sufficient dissolution. In other words, removing a target substance contained in plastic materials in the removal process involves transferring that target substance to the organic solvent.
[0021] ―Target Substances― Here, the target substance, the antioxidant, is an additive used to prevent oxidative degradation caused by heat applied during the plastic molding process. Primary antioxidants, also called radical scavengers, capture radicals and stop the progression of decomposition. Examples include phenolic antioxidants and amine antioxidants. Secondary antioxidants, also called peroxide decomposers, decompose peroxides and render them harmless. Examples include sulfur-based antioxidants and phosphorus-based antioxidants. Generally, primary and secondary antioxidants are often added in combination during the manufacture of plastic materials. Commercially available antioxidants may be used. Examples include Irganox 1010 (manufactured by BASF Japan Ltd.) as a phenolic antioxidant, Irgafos 168 (manufactured by BASF Japan Ltd.) as a phosphorus-based antioxidant, and Sumirizer GP (manufactured by Sumitomo Chemical Co., Ltd.) as an antioxidant that combines primary and secondary antioxidants.
[0022] By subjecting a plastic material containing such antioxidants to a treatment involving contact with an organic solvent having the aforementioned specific SP value, the antioxidant can be effectively removed from the plastic material, regardless of the type of antioxidant.
[0023] The target substance, the lubricant, is an additive mainly for reducing surface free energy to improve slipperiness. For example, when slipperiness is improved by a method of adding a lubricant to a packaging material composed of a resin film or the like, generally, the lubricant is added to the resin film in an amount of about 100 ppm to 500 ppm. When a lubricant is added to a resin film, a bleed-out phenomenon occurs in which the lubricant precipitates on the film surface, whereby slip properties are developed in the resin film.
[0024] Specifically, examples of the lubricant include fatty acid amide-based, fatty acid alcohol-based, hydrocarbon-based, fatty acid-based, and ester-based lubricants. Among them, fatty acid amides having a molecular weight of 250 to 350, such as stearic acid amide, oleic acid amide, and erucic acid amide, are suitably used. These lubricants bleed out quickly to the film surface and exhibit their effect immediately after molding. Commercially available products may also be used as the lubricant, for example, M425 (manufactured by Ube Maruzen Polyethylene Co., Ltd.) as erucic acid amide, M105 (manufactured by Ube Maruzen Polyethylene Co., Ltd.) as oleic acid amide, and M205 (manufactured by Ube Maruzen Polyethylene Co., Ltd.) as stearic acid amide, etc., are commercially available.
[0025] As mentioned above, lubricants are additives that primarily impart sliding properties to a material by bleeding out onto the film surface. Therefore, lubricants can be efficiently removed in a short time by contact with an organic solvent having a specific SP value. Furthermore, by treating the lubricant with an organic solvent at a temperature near its melting point, for example, the dissolution rate into the organic solvent is dramatically increased, allowing for even faster and more efficient removal. The melting point of lubricants varies depending on the type, but is generally in the range of 20°C to 95°C. Moreover, since most lubricants bleed out onto the film surface, they can be efficiently removed even if the organic solvent does not completely penetrate into the interior of the plastic material being treated. This makes it possible to suppress the occurrence of solvent cracks during drying in the resulting recycled resin. Solvent cracking refers to the phenomenon in which solvents penetrate and enter the gaps in the molecular chains of the resin, causing the entanglement between molecules to break down, reducing the strength of the resin, making it brittle, and resulting in cracks.
[0026] In addition to the antioxidants and lubricants mentioned above, the substances to be removed may also include trace chemical substances. Trace chemical substances are substances that raise concerns about adverse effects on human health and the environment. Unlike antioxidants and lubricants, they are not intentionally added during the film manufacturing process, but rather are substances that may be unintentionally introduced during the manufacturing, use, or disposal process. Specifically, examples of such trace chemical substances include isononylphenol, PCB77, PCB118, OCDD, OCDF, bisphenol A, and diisononyl phthalate.
[0027] Note that among the aforementioned trace chemical substances, PCB77 is a substance also known as 3,3',4,4'-tetrachloro-1,1'-biphenyl, polychlorinated biphenyl-77, and 3,3',4,4'-tetrachlorobiphenyl. In addition, PCB118, which is a dioxin, is a substance also known as 2,3',4,4',5-pentachloro-1,1'-biphenyl and 2,3',4,4',5-pentachlorobiphenyl. Further, OCDD, which is a dioxin, is a substance also known as 1,2,3,4,6,7,8,9-octachlorodibenzo[b,e][1,4]dioxin, 1,2,3,4,6,7,8,9-octachlorodibenzo-p-dioxin, and octachlorodibenzo-p-dioxin. Moreover, OCDF is a substance also known as 1,2,3,4,6,7,8,9-octachlorodibenzofuran, octachlorodibenzofuran, and perchlorodibenzofuran. Furthermore, bisphenol A is a substance also known as 4,4'-(1-methylethylidene)bis[phenol], 2,2-bis(p-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)dimethylmethane. In addition, diisononyl phthalate is a substance also known as 1,2-benzenedicarboxylic acid, 1,2-diisononyl ester, phthalic acid, diisononyl ester, and 1,2-benzenedicarboxylic acid, diisononyl ester.
[0028] ―Plastic Material― The plastic material as the raw material may sometimes be referred to as an input material, and specifically is a flexible plastic. The plastic material can be appropriately selected from various thermoplastic resins, and may be a single-component system or a multi-component system using a plurality of resins, both of which are usable. In addition, the form of the plastic material may be composed only of a thermoplastic resin such as a co-extruded product or an extrusion-laminated product, and may be a laminate in which the same type or a plurality of types of resin sheets are laminated via an adhesive.
[0029] While there is no precise definition of soft plastic, it generally refers to plastic that is soft enough to be cut with scissors. Conventionally, a tensile modulus of 70 MPa or less, as defined in ISO 527-3:2012 by the International Organization for Standardization (ISO), is used as a guideline.
[0030] Examples of thermoplastic resins include polyolefins such as polyethylene and polypropylene; polyvinyl chloride, polystyrene, ABS resin, methacrylic resin, and acrylic resin. Among these, polyolefins are preferred, and polyethylene is more preferred.
[0031] Examples of polyolefin resins include polyethylene resins such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and ethylene-α-olefin copolymers, as well as homopolypropylene (PP), block polypropylene, random polypropylene, and propylene-α-olefin copolymers. These may be used individually or in combination of two or more.
[0032] As plastic materials, products such as post-consumer recycling (PCR) and post-industry recycling (PIR) can be used. Compared to PCR materials, PIR materials have less debris attached, and because they are made from specific plastic products, the plastic material is more uniform and the quality as a recycled material is more stable.
[0033] Examples of post-consumer recycling (PCR) materials include bottles for beverages, detergents, and condiments that have been collected from the market; food containers for bento boxes and instant noodles; packaging bags for food and garbage bags; and plastic products such as hangers, stationery, daily necessities, home appliances, and toys. When using PCR materials, it is advisable to pre-clean them with surfactants or alkalis, as dirt may be present on the surface during use.
[0034] Examples of post-industrial recycling (PIR) include, for example, defective products that do not become finished products discharged from factories, offcuts generated in the process of manufacturing products, and plastic products used for transportation and packaging.
[0035] The type of resin contained in the plastic material can be confirmed by a micro-infrared spectrophotometer or the like.
[0036] The shape of the plastic material to be subjected to the removal step is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include small piece form (fluff form), strip form and the like. Among them, 100 mm 3 or smaller small piece form is preferred, and 10 mm 3 or smaller small piece form is more preferred. Therefore, in the removal step, it is preferable to pulverize the plastic material into small pieces of 100 mm 3 or smaller, and then add an organic solvent to the small piece-shaped plastic material. In this way, by pulverizing the plastic material into small pieces and bringing them into contact with the organic solvent, the target substance can be removed more efficiently. The lower limit of the size of the small piece-shaped plastic material is not particularly limited, but from the viewpoint of preventing clogging of the filter used for filtration after treatment and improving workability, 0.4 mm 3 or larger is preferred, and 1 mm 3 or larger is more preferred. Therefore, as the shape of the plastic material, small pieces of 0.4 mm 3 or more and 100 mm 3 or smaller are preferred, and 1 mm 3 or more and 10 mm 3 or smaller small piece form is more preferred.
[0037] As a guideline for the size of the small pieces, for example, when crushing a film-like plastic material with an average thickness of 0.05 mm to 1 mm, it is preferable that the pieces be between 3 mm square and 20 mm square. Being 3 mm square or larger prevents clogging of the filter used for filtration after processing, resulting in excellent workability. Furthermore, being 20 mm square or smaller increases the specific surface area in contact with the organic solvent, further improving the removal efficiency of the target substance. However, the above sizes are merely guidelines, and the shape of the small pieces does not need to be square as long as they are of a similar size; various shapes are acceptable.
[0038] —Organic Solvents— As organic solvents, there are no particular limitations as long as they have the specific SP values mentioned above, and they can be appropriately selected according to the purpose. Examples include xylene, toluene, heptane, N-methyl-2-pyrrolidone (NMP), diethylene glycol monobutyl ether, benzene, ethylbenzene, styrene, octane, hexane, trichloroethylene, diethyl ether, butyl acetate, ethyl acetate, chloroform, dichloromethane, acetone, and ethanol, which can be suitably used.
[0039] The amount of organic solvent added is not particularly limited and can be appropriately selected depending on the purpose. For example, the amount of organic solvent added is preferably 100 parts by mass or more and 4000 parts by mass or less per 100 parts by mass of plastic material, and more preferably 500 parts by mass or more and 4000 parts by mass or less. Adding 100 parts by mass or more of organic solvent per 100 parts by mass of plastic material allows for efficient removal of the target substance, while keeping it at 4000 parts by mass or less allows for effective removal of the lubricant while suppressing an increase in environmental burden.
[0040] ―Other Conditions― The temperature conditions in the lubricant removal process are not particularly limited and can be appropriately selected according to the purpose. For example, 20°C to 95°C is preferred, and 30°C to 90°C is more preferred. Regarding temperature conditions, the removal efficiency of the target substance increases as the processing temperature rises up to a certain temperature. Specifically, the removal efficiency can be increased by setting the processing temperature to 20°C or higher, and the processing can be carried out while suppressing the dangers of handling organic solvents by setting it to 95°C or lower. Furthermore, by processing under the above temperature conditions, the dissolution rate of the target substance in the organic solvent can be dramatically improved, and the removal process can be carried out efficiently in a shorter time. Moreover, by processing with a temperature range of 30°C to 90°C, the removal of the target substance can be carried out with greater safety and efficiency.
[0041] The processing time in the removal process is not particularly limited and can be appropriately selected depending on the purpose, but for example, 20 minutes to 10 hours is preferred, and 1 hour to 5 hours is more preferred. The pressure conditions in the removal process are not particularly limited and can be appropriately selected depending on the purpose, but for example, it is preferable to carry it out under mild and simple conditions such as atmospheric pressure (1 atmosphere).
[0042] In the method for producing recycled resin according to this embodiment, as described above, the removal process can be carried out under mild conditions, for example, between 20°C and 95°C, and the pressure increase due to the evaporation of the organic solvent can be suppressed, making it possible to process in a sealed container. In addition, after processing, the resin and organic solvent can be separated by filtration. Therefore, another advantage is that the solvent can be reused without waste.
[0043] Furthermore, by performing the removal process before the melt molding process described later, processing can be carried out under mild conditions, avoiding the risk of fire caused by using solvents at high temperatures and pollution such as volatilization and / or diffusion into the environment. In addition, since the various target substances remaining in the input material before and after decomposition can be removed before the resin is melt-molded, it is possible to reduce the risk of appearance defects caused by decomposition products of target substances such as antioxidants and lubricants.
[0044] ―Amount of target substance remaining in recycled resin after processing in the removal process― "Remaining amount of lubricant" refers to the amount of target substance that originates from the plastic material (input material) that is the raw material of the recycled resin, out of the total amount of target substance contained in the recycled resin. In other words, it refers to the amount of target substance that originates from the plastic material that remains in the recycled resin obtained after the removal process. Furthermore, as will be described later, when additives such as antioxidants and lubricants are added again in the production of recycled resin, the remaining amount of each of these target substances that originates from the plastic material that is the raw material of the recycled resin can be determined by subtracting the amount of antioxidant and / or lubricant that was added again from the quantitative analysis value of the antioxidant and / or lubricant that are the target substances.
[0045] (Remaining amount of antioxidant) When the antioxidant is removed as a target substance in the removal process, the remaining amount of antioxidant in the recycled resin produced, as measured by high-performance liquid chromatography, is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 800 ppm or less, more preferably 400 ppm or less, even more preferably 200 ppm or less, and particularly preferably 100 ppm or less. Examples of antioxidants include phenolic antioxidants, amine antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, etc., as mentioned above.
[0046] The residual amount of antioxidant in recycled resin can be measured, for example, by quantitative analysis using high-performance liquid chromatography. Specifically, pelletized recycled resin can be used as a sample, and quantitative analysis can be performed using a high-performance liquid chromatograph (e.g., instrument name: 1260 HPLC system, manufactured by Agilent Technologies). Furthermore, if antioxidant is added again to the manufactured recycled resin in the re-addition process described later, the residual amount of antioxidant derived from the raw plastic material can be determined by subtracting the added antioxidant from the quantitative analysis value of antioxidant in the recycled resin.
[0047] Furthermore, the content of degraded and oxidized antioxidants can be evaluated by the oxidation induction time measured using a chemiluminescence analyzer. The oxidation induction time is preferably 0 minutes to 18 minutes, more preferably 0 minutes to 15 minutes, and even more preferably 0 minutes to 10 minutes.
[0048] The oxidation induction time can be measured, for example, using a chemiluminescence analyzer (CLA-FS54, manufactured by Tohoku Electronics Industry Co., Ltd.) according to the following procedure in accordance with JIS K 7351. Specifically, the resin composition to be measured is pelletized to prepare the sample. Next, a fixed amount of the sample is measured into an aluminum sample container with a diameter of 20 mm to 30 mm, and the oxidation induction time is measured by observing the change in emission intensity using a chemiluminescence analyzer. The measurement conditions can be, for example, a sample weight of 0.2 g, a constant temperature of 220°C, an oxygen atmosphere, an oxygen flow rate of 50 mL / min, an exposure time of 1 second, and a measurement time of 7 hours.
[0049] A chemiluminescence analyzer is a measuring device that detects the amount of chemiluminescence in a sample. The oxidation induction time is the time it takes for the amount of chemiluminescence to increase significantly when measured under an oxygen atmosphere. For example, in the case of a resin composition containing a polyolefin resin and an antioxidant, the oxidation induction time is the time from the start of heating until the effect of the antioxidant on suppressing chemiluminescence wears off. The longer the time, the less likely the polyolefin resin is to be oxidized.
[0050] (Remaining amount of lubricant) When the lubricant is removed as the target substance in the removal process, the remaining amount of lubricant in the recycled resin produced, as measured by gas chromatography, is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 200 ppm or less, more preferably 100 ppm or less, and even more preferably 0 ppm. The lubricant is not particularly limited and, as mentioned above, can be erucic acid amide, oleic acid amide, stearic acid amide, etc.
[0051] The amount of lubricant remaining in recycled resin can be measured, for example, by quantitative analysis using gas chromatography (GC). Specifically, an example of quantitative analysis using a gas chromatograph (GC7890A / G1888A, manufactured by Agilent Technologies, Inc.) is shown below. In the gas chromatograph used in this example, the column is HP-5MS (inner diameter 0.25 mm, length 30 m, film thickness 0.25 μm), and the detector is an FID (flame ionization detector).
[0052] Specifically, the recycled resin after processing in the removal step is held in 10 ml of chloroform at 60°C for 8 hours to obtain a solution which is used as a sample. 1.0 μl of this sample is then injected into a gas chromatograph (split ratio: 1 / 50, carrier gas: He). After holding at 40°C for 1 minute, the temperature is increased to 300°C at a heating rate of 10°C / min. Meanwhile, chloroform solutions containing several fatty acid amides of different concentrations are used as standard solutions for measurement. By drawing a calibration curve of peak area and concentration, the remaining amount of lubricant (fatty acid amides such as erucic acid amide, oleic acid amide, and stearic acid amide) can be determined.
[0053] (Remaining amount of trace chemical substances) When trace chemical substances are removed as target substances in the removal process, the remaining amount of trace chemical substances measured by the trace chemical substance test method in the recycled resin produced is not particularly limited and can be appropriately selected depending on the purpose, but the following remaining amounts are preferable depending on the type of trace chemical substance.
[0054] In other words, the residual amount of isononylphenol, a trace chemical substance derived from the plastic material, as measured in the trace chemical substance test, is preferably less than 1,000 μg / kg, more preferably 500 μg / kg, even more preferably less than 150 μg / kg, and particularly preferably less than 100 μg / kg. The residual amount of isononylphenol may also be below the limit of quantification, including 0 μg / kg.
[0055] Furthermore, the residual amount of PCB77, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, is preferably less than 75 ng / kg, more preferably less than 50 ng / kg, and even more preferably less than 25 ng / kg. Note that the residual amount of PCB77 may also be below the quantification limit, including 0 ng / kg.
[0056] Furthermore, the residual amount of PCB118, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, is preferably less than 2,000 ng / kg, more preferably less than 1,000 ng / kg, even more preferably less than 200 ng / kg, and particularly preferably less than 100 ng / kg. Note that the residual amount of PCB118 may also be below the quantification limit, including 0 ng / kg.
[0057] Furthermore, the residual amount of OCDD, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, is preferably less than 45 ng / kg, more preferably less than 25 ng / kg, even more preferably less than 5 ng / kg, and particularly preferably less than 0.85 ng / kg. Note that the residual amount of OCDD may be below the limit of quantification, including 0 ng / kg.
[0058] Furthermore, the residual amount of OCDF, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, is preferably less than 1.8 ng / kg, more preferably less than 1.2 ng / kg, even more preferably less than 0.8 ng / kg, and particularly preferably less than 0.2 ng / kg. Note that the residual amount of OCDF may be below the quantification limit, including 0 ng / kg.
[0059] Furthermore, the residual amount of bisphenol A, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, is preferably less than 2,500 μg / kg, more preferably less than 1,000 μg / kg, even more preferably less than 500 μg / kg, and particularly preferably less than 100 μg / kg. Note that the residual amount of bisphenol A may be below the limit of quantification, including 0 μg / kg.
[0060] Furthermore, the residual amount of diisononyl phthalate, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, is preferably less than 1,000 μg / kg, more preferably less than 500 μg / kg, even more preferably less than 100 μg / kg, and particularly preferably less than 50 μg / kg. Note that the residual amount of diisononyl phthalate may be below the quantification limit, including 0 μg / kg.
[0061] While the specific details of the trace chemical substance testing methods vary depending on the type of trace chemical substance being tested, they can generally be performed following the common procedures outlined below.
[0062] First, the surface area of the recycled resin sample is increased by cutting, shredding, and / or grinding it into small pieces. Next, extraction is performed using a solvent that can penetrate or diffuse into the sample and dissolve trace chemical substances. The extraction conditions (e.g., time and temperature) can be set to conditions that maximize the recovery rate of trace chemical substances. Typical extraction methods are not particularly limited and can be set appropriately depending on the purpose, but examples include Soxhlet extraction, accelerated solvent extraction, and ultrasonic extraction. Furthermore, it is preferable to add an internal standard during the extraction process to compensate for losses during the extraction and subsequent processing. In particular, when detection is performed by mass spectrometry, a stable isotope-labeled form of the target trace chemical substance is used as the internal standard.
[0063] After extraction, the extraction solvent is recovered and prepared for instrumental analysis. Depending on the solvent used, the required limit of quantification, and the analytical method, purification and / or concentration operations such as centrifugation, filtration, liquid-liquid extraction, and column chromatography may be combined. Subsequently, trace chemical substances in the prepared sample are quantified using an instrumental analysis method suitable for the target substance (e.g., GC-MS, GC-MS / MS, GC-HRMS, LC-MS / MS, etc.). Then, by combining the results obtained from the instrumental analysis with the preparation conditions of the extraction solvent, the extraction volume, and the initial mass of the sample, the mass content (per unit mass) of trace chemical substances in the sample is calculated and used as the residual amount (content) in the recycled resin. Generally, since trace chemical substances exist at extremely low concentrations, units such as μg / kg and ng / kg (corresponding to ppb and ppt, respectively) are used.
[0064] Furthermore, the residual amount (content) of trace chemicals in recycled resins can also be measured based on known standard methods for specific trace chemicals (for example, USEPA Method 1613 for dioxins and furans, and USEPA Method 1668 for PCBs).
[0065] <Washing Step> In the method for producing recycled resin according to this embodiment, a washing step may be further provided as needed. The washing step is a step provided after the removal step, and involves washing the plastic material (recycled resin) obtained through the removal step with a washing solution containing an amphiphilic solvent to remove any organic solvent residue adhering to the plastic material.
[0066] By including a washing step, residual organic solvents can be washed away from plastic materials that have been treated with organic solvents to remove target substances. Furthermore, for example, if a peeling step is included as a subsequent step to separate each film from the laminated plastic material, an aqueous solvent is used in the peeling step, thus reducing concerns about the carryover of residual organic solvents to the peeling step.
[0067] The amphiphilic solvent used as the washing solution is not particularly limited and includes methanol, ethanol, 1-propanol, 2-propanol, acetone, N,N-dimethylformamide, dimethyl sulfoxide, and the like. In addition to such amphiphilic solvents, the washing solution may also contain water and may further contain additives such as pH adjusters.
[0068] Furthermore, the cleaning process can be carried out at a temperature of, for example, 20°C to 90°C, preferably 20°C to 50°C. The cleaning process can also be carried out under atmospheric pressure.
[0069] Furthermore, in the washing process, after washing away the organic solvent residue with a washing solution, a drying treatment may be performed. The drying treatment can be carried out at a temperature of, for example, 20°C to 90°C, preferably 20°C to 50°C. The method of drying treatment is not particularly limited, and for example, it may be left to stand in the air or dried by blowing air at the above temperature.
[0070] <Re-addition Step> In the method for producing recycled resin according to this embodiment, if an antioxidant and / or lubricant is removed as a target substance in the removal step, a re-addition step may be provided in which the antioxidant and / or lubricant is re-added to the obtained recycled resin as needed. That is, the re-addition step is a step in which the antioxidant and / or lubricant removed in the removal step is re-added to the obtained recycled resin. The antioxidant and / or lubricant to be re-added may be the same type as the antioxidant and / or lubricant contained in the raw plastic material and removed in the removal step, or it may be a different type, and can be appropriately selected according to the purpose.
[0071] The re-addition of antioxidants and / or lubricants can be carried out almost simultaneously with the melt molding process described later, and may be done at the same time as the addition of additives or at any time. Furthermore, it is preferable to add (re-add) antioxidants and / or lubricants to the recycled resin obtained through the removal process prior to the melt molding process and mix them to a certain extent, and then put these mixtures into the hopper for the melt molding process. This allows the re-added antioxidants and / or lubricants to be uniformly added to the recycled resin, and more effectively suppresses variations in the properties of the recycled resin.
[0072] When adding antioxidants again, the amount of antioxidant added is preferably 500 ppm to 2000 ppm relative to the total amount of recycled resin, and more preferably 1000 ppm to 2000 ppm. The recycled resin obtained through the removal process has had the antioxidants derived from the raw plastic material removed. By adding antioxidants again in a range of approximately 500 ppm to 2000 ppm, good antioxidant performance can be achieved in the recycled resin, and oxidative degradation can be prevented.
[0073] When a lubricant is re-added, the amount of lubricant added is preferably 100 ppm to 500 ppm relative to the total amount of recycled resin, and more preferably 100 ppm to 300 ppm. The recycled resin obtained through the lubricant removal process has had the lubricant derived from the raw plastic material removed, and by re-adding lubricant in a range of approximately 100 ppm to 500 ppm, good lubricity properties can be achieved in the recycled resin.
[0074] Furthermore, because antioxidants and / or lubricants derived from the raw plastic material are effectively removed through the removal process, an appropriate amount of antioxidants and / or lubricants can be added back in the re-addition process, resulting in a stable recycled resin with consistent properties.
[0075] <Melting Molding Process> The melting molding process is a process of melting and molding the obtained recycled resin. Additives may be added and mixed in the melting molding process as needed. In the melting molding process, only the recycled resin obtained through the removal process may be melted and molded to form a molded body of recycled resin, or a mixture of recycled resin and virgin resin may be melted and molded to form a molded body of resin containing recycled resin.
[0076] The apparatus used for melt molding is not particularly limited, and any known apparatus can be appropriately selected depending on the purpose. Examples include twin-screw extruders and single-screw extruders.
[0077] The shape of the molded body is not particularly limited and can be appropriately selected according to the purpose, for example, pellets, sheets, etc. That is, the melt molding process includes a step of melting the obtained recycled resin and molding it into pellets containing recycled resin, and a step of further melting the pellets and molding them into a molded body such as a film. Alternatively, the melt molding process may include a step of melting the obtained recycled resin and molding it directly into a molded body such as a film.
[0078] Furthermore, when additives are added, there are no particular limitations on the additives themselves, and known additives can be appropriately selected according to the purpose. Examples include nucleating agents, reinforcing fillers, heat stabilizers, weathering agents, light stabilizers, plasticizers, ultraviolet absorbers, antistatic agents, flame retardants, flame retardant enhancers, slip agents, antiblocking agents, antifogging agents, lubricants, pigments, dyes, dispersants, copper damage inhibitors, neutralizing agents, anti-bubble agents, weld strength improvers, natural oils, synthetic oils, waxes, etc. These may be used individually or in combination of two or more.
[0079] Specifically, examples of nucleating agents and reinforcing fillers include metals such as talc, silica, clay, montmorillonite, calcium carbonate, lithium alumina carbonate, titanium dioxide, aluminum, iron, silver, and copper; hydroxides such as aluminum hydroxide and magnesium hydroxide; celluloses such as cellulose microfibrils and cellulose acetate; fibrous fillers such as glass fibers, polyethylene terephthalate fibers, nylon fibers, polyethylene naphthalate fibers, aramid fibers, vinylon fibers, and polyacrylate fibers; carbons such as carbon nanotubes; and elastomers such as ethylene propylene rubber (EPR).
[0080] Examples of heat stabilizers include hindered amine compounds.
[0081] Examples of UV absorbers include benzophenone compounds, benzotriazole compounds, and benzoate compounds.
[0082] Examples of antistatic agents include nonionic compounds, cationic compounds, and anionic compounds.
[0083] Examples of flame retardants include halogen compounds, phosphorus compounds, nitrogen compounds, inorganic compounds, boron compounds, silicone compounds, sulfur compounds, and red phosphorus compounds.
[0084] Examples of flame retardant additives include antimony compounds, zinc compounds, bismuth compounds, magnesium hydroxide, and clayey silicates.
[0085] In the melt molding process, the maximum temperature of the resin measured in the extruder is preferably 320°C or lower. By keeping the maximum temperature of the resin measured in the extruder below 320°C, the decomposition of the plastic material due to heat can be suppressed. Furthermore, the lower limit of the maximum temperature of the resin measured in the extruder is 130°C. When the resin temperature reaches 130°C, it melts, making melt kneading using the extruder possible. As mentioned above, the maximum temperature of the resin measured in the extruder is preferably 320°C or lower, more preferably 300°C or lower, and even more preferably 280°C or lower.
[0086] In order to keep the maximum resin temperature measured within the extruder below 320°C, it is necessary to appropriately adjust the set temperature and screw rotation speed of the extruder.
[0087] If the extrusion device's temperature setting is appropriate, it becomes possible to heat the resin to a temperature above its melting point and melt-knead it, maintaining a maximum resin temperature of 320°C or lower within the extrusion device and suppressing resin decomposition.
[0088] When the screw rotation speed of the extruder is appropriate, it is possible to suppress insufficient dispersion of additives and auxiliary materials that occurs when the screw rotation speed is low. Furthermore, it is possible to suppress the overheating of the plastic material due to shear heating that occurs when the screw rotation speed is high.
[0089] The residence time of the resin in the extruder is preferably 10 seconds or more and 150 seconds or less. A residence time of 10 seconds or more ensures sufficient melt mixing and prevents insufficient dispersion of additives and auxiliary components. Furthermore, a residence time of 150 seconds or less suppresses thermal degradation and decomposition of the resin. The residence time of the resin in the extruder may be 10 seconds or more, 20 seconds or more, 30 seconds or more, 150 seconds or less, 120 seconds or less, or 90 seconds or less.
[0090] The time the resin remains in the extruder can be measured by starting the measurement from the moment the masterbatch is introduced into the material inlet of the extruder, and ending the measurement when it can be visually confirmed that the recycled material coming out of the discharge port of the extruder matches the color of the masterbatch.
[0091] <Other Processes> In the method for manufacturing recycled resin according to this embodiment, a peeling step and a separation step may be provided as needed. The peeling step is a step in which, when the raw material plastic material is a laminate in which multiple films are laminated together with an adhesive, the laminate is peeled off film by film. The separation step is a step in which each of the peeled films is separated and recovered.
[0092] Such peeling and separation steps for plastic materials can be performed before the removal step. Alternatively, the peeling and separation steps may be performed after the removal step. Performing the peeling and separation steps after the removal step is preferable because the peeling and separation treatment of each film is performed on the plastic material that has come into contact with the organic solvent, which activates the surface of the plastic material by the organic solvent, making it possible to peel and separate the films more efficiently. If a re-addition step is provided after the removal step, the peeling and separation steps can be performed after the removal step and before the re-addition step.
[0093] It is preferable that the plastic material used in the peeling and separation processes is crushed into small pieces or other shapes. This allows for more efficient peeling and separation of the film from the laminate.
[0094] Furthermore, as an additional step, a grinding step may be provided, separate from the removal, peeling, and separation steps described above, to grind the plastic material subjected to these processes. By providing a grinding step and finely grinding the plastic material into small pieces or other shapes, the processing efficiency in the removal, peeling, and separation steps can be improved.
[0095] (Peeling process) The peeling process is a process of peeling each film from a laminate in which multiple films, each containing at least a base layer and a sealant layer, are laminated together. Specifically, in the peeling process, the laminate is treated with an alkaline solution to dissolve or swell the adhesive resin layer, which consists of an adhesive, and thereby peel off the base layer and the sealant layer.
[0096] At least one of the base layer and the sealant layer contains a polyolefin resin. Examples of polyolefin resins include polyethylene and polypropylene. The polyolefin resin may be contained only in the base layer, only in the sealant layer, or in both the base layer and the sealant layer. Furthermore, at least one of the base layer and the sealant layer may contain a resin other than a polyolefin resin (non-polyolefin resin). Examples of non-polyolefin resins include polyester resin, polyamide resin, and urethane resin.
[0097] The adhesive resin layer may be an anchor layer or an adhesive layer. Furthermore, the laminate may contain components such as fibers or inorganic materials.
[0098] The alkaline solution used in alkaline treatment includes an alkali and a solvent. Examples of alkalis include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, sodium ethylate, potassium ethylate, and lithium methylate. When the adhesive resin contained in the adhesive resin layer has hydroxyl groups, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and ammonium salts are preferred. Examples of solvents include water, alcohol, glycol ether, and polar solvents such as N-methyl-2-pyrrolidone, which may be used individually or in mixtures of two or more. As water, deionized water, reverse osmosis water, distilled water, purified water, well water, tap water, industrial water, etc. can be used. As alcohol, methanol, ethanol, propanol, isopropanol, etc. can be used. As glycol ether, diethylene glycol monobutyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, etc. can be used.
[0099] The temperature of the alkaline solution is not particularly limited, but from the viewpoint of promoting the dissolution or swelling of the adhesive resin layer, it is preferably 40°C or higher, and more preferably 65°C or higher. Alternatively, the temperature of the alkaline solution may be 90°C or lower, 85°C or lower, or 80°C or lower.
[0100] The concentration of alkali in the alkaline solution is not particularly limited, but is preferably 1% by mass or more, more preferably 3% by mass or more. Alternatively, the concentration of alkali in the alkaline solution may be 5% by mass or more.
[0101] Examples of alkalis contained in alkaline solutions include sodium hydroxide, dimethylbis(2-hydroxyethyl)ammonium hydroxide, monomethyltris(2-hydroxyethyl)ammonium hydroxide, and trimethyl-2-hydroxyethylammonium hydroxide.
[0102] The alkali treatment time is not particularly limited, but from the viewpoint of promoting the dissolution or swelling of the adhesive resin layer, it is preferably 30 minutes or more, and more preferably 60 minutes or more. The alkali treatment time may also be 240 minutes or less, or 180 minutes or less.
[0103] The pressure conditions during the alkali treatment are not particularly limited and may be atmospheric pressure. The atmosphere during the alkali treatment may be air or an inert gas atmosphere. Examples of inert gas atmospheres include argon gas atmosphere, helium gas atmosphere, nitrogen gas atmosphere, and mixtures thereof. The alkali treatment may be carried out in a sealed or open environment.
[0104] In alkaline treatment, if at least one of the substrate layer and sealant layer does not detach from the adhesive resin layer even after swelling, and the laminate remains intact, stress is applied to the laminate to detach the substrate layer and sealant layer from the adhesive resin layer. Methods for applying stress to the laminate include, for example, generating flow by stirring the alkaline solution.
[0105] (Separation process) The separation process is the process of separating and recovering each film (substrate layer, sealant layer, etc.) that has been peeled off in the peeling process.
[0106] If the adhesive resin layer is dissolved in the alkaline solution during the peeling process described above, the separation process includes a first step of removing the substrate layer and sealant layer from the alkaline solution. In this case, since the adhesive resin is dissolved in the alkaline solution and at least one of the substrate layer and sealant layer contains polyolefin resin, the polyolefin resin is separated from the adhesive resin. At this time, since the substrate layer and sealant layer have been peeled from the adhesive resin during the peeling process, the substrate layer and sealant layer are separated from each other. In the first step of the separation process, for example, the solid-liquid mixture containing the alkaline solution, substrate layer, and sealant layer is filtered.
[0107] Furthermore, if one of the substrate layer and the sealant layer does not contain polyolefin resin during the separation process, the process may further include a second step of separating the layer containing polyolefin resin (polyolefin resin-containing layer) from the layer that does not contain polyolefin resin (polyolefin resin-free layer). In the second step of the separation process, for example, the polyolefin resin-free layer and the polyolefin resin-containing layer are separated by a difference in specific gravity. In the separation process by difference in specific gravity, a specific gravity separation liquid can be used, and as the specific gravity separation liquid, a liquid having a specific gravity between the specific gravity of the non-polyolefin resin and the specific gravity of the polyolefin resin can be used.
[0108] When using a specific gravity separation solution to float polyolefin resin as a low-density component, a solution with a specific gravity less than or equal to that of non-polyolefin resin and greater than that of polyolefin resin can be used. By using such a specific gravity separation solution, the polyolefin resin will float to the surface of the specific gravity separation solution as a low-density component, allowing for easy recovery of the polyolefin resin. Furthermore, when using a specific gravity separation solution to remove non-polyolefin resin as a high-density component, a solution with a specific gravity less than that of non-polyolefin resin and greater than that of polyolefin resin can be used. By using such a specific gravity separation solution, the non-polyolefin resin will settle in the specific gravity separation solution as a high-density component. Therefore, by removing the non-polyolefin resin, the polyolefin resin remains, allowing for easy recovery of the polyolefin resin.
[0109] Furthermore, if the adhesive resin layer swells in the alkaline solution during the peeling process, the separation process includes a third step (fractionation step) in which the adhesive resin layer, substrate layer, and sealant layer are removed from the alkaline solution, and then the substrate layer and sealant layer are separated from the adhesive resin layer. Note that since the substrate layer and sealant layer have been peeled from the adhesive resin layer during the peeling process, the adhesive resin layer, substrate layer, and sealant layer are separated from each other. In the third step of the separation process, for example, the solid-liquid mixture containing the alkaline solution, adhesive resin layer, substrate layer, and sealant layer is filtered.
[0110] In the third step of the separation process, the adhesive resin layer containing the adhesive resin and the polyolefin resin contained in at least one of the substrate layer and the sealant layer may be separated by the difference in specific gravity. In this case, the same specific gravity separation solution as used in the second step of specific gravity separation can be used.
[0111] Furthermore, if one of the substrate layer and the sealant layer does not contain polyolefin resin, the separation process may further include a fourth step of separating the polyolefin resin-containing layer from the polyolefin resin-free layer. In the fourth step of the separation process, for example, the polyolefin resin-free layer and the polyolefin resin-containing layer are separated by the difference in specific gravity. In this case, the same specific gravity separation solution as used in the second step of specific gravity separation can be used.
[0112] Examples of the specific gravity separation liquids mentioned above include water, ethanol, and chloroform. Among these, water is preferred. Since polyolefin resin has a lower specific gravity than water, the polyolefin resin can be made to float on the water surface, and thus easily separated. The specific gravity separation liquid may be the same as or different from the solvent contained in the alkaline solution. When using a specific gravity separation liquid in the separation process, the temperature of the specific gravity separation liquid is not particularly limited and may be at room temperature.
[0113] (Grinding Process) The grinding process is a process of grinding the plastic material to be used in the removal process, peeling process, and separation process described above. By finely grinding the plastic material in the grinding process, the processing efficiency in these processes can be improved. Furthermore, the grinding process can be set up as a separate and independent process from the removal process, peeling process, and separation process, and it is preferable to set it up before these processes.
[0114] In the crushing process, the plastic material is crushed into small pieces (fluffs), strips, or other shapes using a crusher. A general-purpose crusher can be used. The size of the plastic material obtained by crushing (a guideline for the size of the small pieces) is not particularly limited, but for example, when crushing a film-like plastic material with an average thickness of 0.05 mm to 1 mm, it is preferable that the pieces be between 3 mm square and 20 mm square. However, the above size is merely a guideline, and it is acceptable as long as the pieces are roughly the same size, and the shape of the small pieces does not need to be square; various shapes are acceptable.
[0115] ≪2. Method for Manufacturing Molded Articles of Recycled Resin≫ The method for manufacturing molded articles of recycled resin according to this embodiment is a method for manufacturing molded articles such as films using recycled resin, and includes a step of melt-molding the recycled resin manufactured by the above-described method for manufacturing recycled resin.
[0116] The molded article obtained by this manufacturing method is a molded article containing recycled resin. The shape of the molded article is not particularly limited, but examples include pellets, sheets, or other film-like shapes. Specifically, the process of melt-molding the recycled resin includes a step of melting the obtained recycled resin and forming it into pellets containing recycled resin, and a step of further melting the pellets and forming them into a molded article such as a film. Alternatively, the melt-molding process may include a step of melting the obtained recycled resin and forming it directly into a molded article such as a film.
[0117] For example, in this method for manufacturing molded articles, recycled resin obtained by the recycled resin manufacturing method described above can be melt-molded in an extruder to form pellets (molded into pellets), thereby producing pellets containing recycled resin. Furthermore, after melting the pellets containing recycled resin in an injection molding machine or extruder (e.g., a twin-screw extruder), a film containing recycled resin can be produced by forming a film with a T-die via a feed block or multi-manifold, or by forming a film by an inflation method.
[0118] A molded article containing recycled resin may contain only recycled resin, or it may further contain virgin resin or additives to impart various desired properties such as viscosity adjustment or mechanical property enhancement. When mixing recycled resin and virgin resin, it may be a dry blend in which the virgin resin and recycled resin are simultaneously put into a hopper and melt-kneaded to form a film, or it may be a melt blend in which the virgin resin and recycled resin are melt-kneaded separately in a twin-screw extruder to form a masterbatch.
[0119] ≪3. Recycled Resin≫ The recycled resin of this embodiment is a recycled resin made from a plastic material containing one or more substances selected from the group consisting of antioxidants, lubricants, and trace chemical substances. In the following, antioxidants, lubricants, and trace chemical substances contained in the raw plastic material may be collectively referred to as "substances."
[0120] Specifically, it is a recycled resin made from plastic materials containing at least an antioxidant additive, wherein the residual amount of antioxidant derived from the plastic material, as measured by high-performance liquid chromatography, is 800 ppm or less.
[0121] Furthermore, the recycled resin is made from a plastic material containing at least a lubricant as an additive, and the residual amount of lubricant derived from the plastic material, as measured by gas chromatography, is 200 ppm or less.
[0122] Furthermore, the recycled resin is made from a plastic material containing at least trace chemical substances, wherein the residual amount of isononylphenol, a trace chemical substance derived from the plastic material as measured by the trace chemical substance test, is less than 1,000 μg / kg, the residual amount of PCB77, a trace chemical substance derived from the plastic material as measured by the trace chemical substance test method, is less than 75 ng / kg, and the residual amount of PCB118, the aforementioned trace chemical substance derived from the plastic material as measured by the trace chemical substance test method, is less than 2,000 ng / kg, and the residual amount of PCB118, a trace chemical substance derived from the plastic material as measured by the trace chemical substance test method, is less than 2,000 ng / kg. This recycled resin has a residual amount of OCDD, a trace chemical substance derived from the plastic material, of less than 45 ng / kg; a residual amount of OCDF, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, of less than 1.8 ng / kg; a residual amount of bisphenol A, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, of less than 2,500 μg / kg; and a residual amount of diisononyl phthalate, a trace chemical substance derived from the plastic material as measured by the trace chemical substance testing method, of less than 1,000 μg / kg.
[0123] The recycled resin according to this embodiment can be suitably manufactured by the recycled resin manufacturing method described above.
[0124] In recycled resins, the "residual amount" of antioxidants, lubricants, or trace chemical substances refers to the amount of these substances remaining in the recycled resin after the removal process, which originates from the raw plastic material, as described above. Furthermore, when antioxidants and / or lubricants are added again as additives during the manufacturing of recycled resins, the residual amount originating from the plastic material can be determined by subtracting the amount of antioxidants and / or lubricants added again from the quantitative analysis value of the antioxidants and / or lubricants. The residual amount of antioxidants, lubricants, or trace chemical substances can be measured by the method described in the manufacturing method of recycled resins.
[0125] ≪4. Resin≫ The resin according to this embodiment contains at least the recycled resin described above, and may further contain other resins such as virgin resin or other recycled resins as needed.
[0126] In the resin according to this embodiment, the recycled resin content can be appropriately selected according to the required applications and performance of the products manufactured using the resin. However, considering the significance of using recycled resin, it is preferable that the recycled resin content be 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, relative to the total amount of resin. In this way, by including recycled resin at a ratio of 70% by mass or more relative to the total amount of resin, it is possible to create a resin that more effectively reduces the environmental impact.
[0127] There are no particular limitations on the specific method for producing pellets or the like by mixing recycled resin and virgin resin. For example, one method involves feeding the recycled resin and virgin resin together into a molding machine to produce pellets, or feeding the recycled resin and virgin resin into the molding machine from separate inlets and mixing them in a heated and melted state to produce pellets. Another method involves heating and melting only the recycled resin to produce pellets, and then mixing them with virgin resin pellets during film formation. Various methods can be selected from these options.
[0128] When mixing recycled resin and virgin resin, the mixing ratio can be appropriately selected according to the desired performance, but from the perspective of the significance of using recycled resin, a ratio in which the virgin resin content is 50% by mass or less of the total amount of resin is preferable.
[0129] There are no particular restrictions on the method of cooling the resin, and it can be appropriately selected according to the molding machine. For example, in the T-die method, examples include air cooling methods such as air chambers, vacuum chambers, and air knives, and water cooling methods such as dipping a cooling roll into a cold water pan. Furthermore, when imparting an uneven shape to the surface of a film-like resin by shaping, a suitable method can be selected that has a nip roll made of silicone rubber, NBR rubber, fluororesin, etc., and a cooling roll made of machined metal, and cools the molten resin by flowing it into the contact area to which a pressure of 0.1 MPa or more is applied.
[0130] ≪5. Film-like Molded Articles≫ The recycled resin and the resin containing the recycled resin according to this embodiment may be molded articles such as pellets or sheets. For example, they can be film-like molded articles in the form of single-layer sheets, multi-layer sheets, laminates, etc.
[0131] Recycled resins and resins containing recycled resins can be processed in the same way as virgin resins. For example, if the film is a single-layer sheet, it can be manufactured using commonly used methods such as injection molding machines, T-die film formation via feed blocks or multi-manifolds using extruders, or inflation methods. If the film is a multi-layer sheet, it can be manufactured by co-extrusion film formation using an extruder or by extrusion lamination.
[0132] Specifically, the single-layer sheet contains recycled resin and may further contain other resins as needed. Similarly, the multilayer sheet and laminate may have at least one layer containing recycled resin and may further contain other resins as needed, and may have any number of layers.
[0133] Furthermore, the laminate may include, for example, a gas barrier layer on top of at least one layer containing recycled resin (hereinafter also referred to as the "recycled resin-containing layer") to provide oxygen barrier properties and water vapor barrier properties. The gas barrier layer may be a single-layer structure or a multi-layer structure, but it is preferable to include a vapor-deposited layer and / or an oxygen barrier layer.
[0134] The vapor-deposited layer in the gas barrier layer may be a single-layer or multi-layer structure. Examples of materials for the vapor-deposited layer include metals such as aluminum; and inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, and barium oxide. These may be used individually or in combination of two or more.
[0135] Furthermore, the vapor-deposited layer can be formed using conventionally known methods. For example, physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, and ion plating; and chemical vapor deposition (CVD) methods such as plasma chemical vapor deposition, thermochemical vapor deposition, and photochemical vapor deposition can be appropriately selected according to the vapor deposition material.
[0136] Furthermore, there are no particular restrictions on the thickness of the vapor-deposited layer, and it can be appropriately selected according to the purpose. For example, it may be 1 nm to 150 nm, 5 nm to 60 nm, or 5 nm to 40 nm. When the thickness of the vapor-deposited layer is 1 nm or more, oxygen barrier properties and water vapor barrier properties are more easily obtained. Also, when the thickness of the vapor-deposited layer is 150 nm or less, it is easier to prevent the occurrence of cracks in the vapor-deposited layer and easier to maintain the recyclability of the sealant film.
[0137] An auxiliary layer may be provided between the recycled resin-containing layer and the vapor-deposited layer from the viewpoint of barrier properties. The proportion of non-recycled resin (virgin resin, etc.) in the auxiliary layer can be higher than the proportion of recycled resin.
[0138] Furthermore, the oxygen barrier layer can be a layer containing ethylene-vinyl alcohol copolymer, polyvinyl alcohol-based resin, or the like.
[0139] 6. Packaging Materials The film-like molded articles (single-layer sheets, multi-layer sheets, and laminates) according to this embodiment can be suitably used as packaging materials. There are no particular restrictions on the type of packaging material, and can be appropriately selected according to the purpose. Examples include standing pouches, three-sided pouches, gusseted pouches, spout pouches, beak pouches, and the like.
[0140] The packaging material according to this embodiment contains a film-like molded body which is a single-layer sheet, a multi-layer sheet, or a laminate containing the recycled resin described above. The recycled resin content in the packaging material is not particularly limited, but it is preferably 80% by mass or more, and more preferably 90% by mass or more, relative to the resin component in the packaging material.
[0141] As shown in Figure 2, the single-layer sheet 10 according to this embodiment is a single-layer sheet consisting of a recycled resin-containing layer 1 containing recycled resin. Furthermore, as shown in Figures 3 and 4, the multilayer sheets 20 and 30 according to this embodiment may be multilayer sheets having a recycled resin-containing layer 1 and a recycled resin-free layer 2 that does not contain recycled resin but contains other resins. In addition, the multilayer sheet may have a recycled resin-containing layer with a different composition from the recycled resin-containing layer 1 instead of the recycled resin-free layer 2.
[0142] As shown in Figure 5, the laminate 40 according to this embodiment is a laminate having, in this order, a multilayer sheet 30 having a first recycled resin-free layer 2, a recycled resin-containing layer 1, and a second recycled resin-free layer 2, an adhesive layer 3, a nylon film 4, another adhesive layer 3, a printed layer 5, and a cover layer 6.
[0143] Furthermore, in the case of single-layer sheets, multi-layer sheets, and laminates with other substrates, surface modification treatments can be appropriately performed to improve suitability for subsequent processes. For example, surface modification treatments can be performed on the surface that comes into contact with other substrates to improve printability when using single-layer films, or to improve lamination suitability when using laminates. Suitable surface modification treatments include methods that oxidize the film surface to express functional groups, such as corona discharge treatment, plasma treatment, and flame treatment; and wet process modification methods such as coating an easily adhesive layer.
[0144] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.
[0145] <Test Example 1: Production of Recycled Resin from Plastic Materials Containing Antioxidants> <Preparation of Input Material (1)> A masterbatch was prepared by mixing 1000 ppm of an antioxidant (Sumilyzer GP, manufactured by Sumitomo Chemical Co., Ltd.) with polyethylene resin pellets (Harmolex NH745N, manufactured by Nippon Polyethylene Co., Ltd.) using a twin-screw extruder. A 100 μm thick sheet was then produced from the masterbatch by casting using a single-screw extruder to obtain Input Material 1.
[0146] <Preparation of Input Material (2)> Input material (2) was obtained in the same manner as the preparation of input material (1), except that the antioxidant of input material (1) was changed to Irganox 1010 (manufactured by BASF Japan Ltd.).
[0147] <Preparation of Input Material (3)> Input material (3) was obtained in the same manner as the preparation of input material (1), except that the antioxidant of input material (1) was changed to Irgafos 168 (manufactured by BASF Japan Ltd).
[0148] <Preparation of Input Material (4)> Input material (4) was obtained in the same manner as the preparation of input material (1), except that the antioxidant of input material (1) was changed to Irganox 1010 (manufactured by BASF Japan Ltd.) 500 ppm and Irgafos 168 (manufactured by BASF Japan Ltd.) 500 ppm.
[0149] <Preparation of Input Material (5)> Input material (5) was obtained in the same manner as the preparation of input material (1), except that the amount of antioxidant added to input material (1) was changed to 2000 ppm.
[0150] <Examples 1-16 and Comparative Examples 1-5> [Example 1] The input material (1) was cut into pieces approximately 5 mm square. The organic solvent had an SP value of 11.2 [cal / cm²]. 3 ] 1/2 N-methyl-2-pyrrolidone (NMP) was used and heated to 80°C. Small pieces of input material (1) were added to the NMP, which was kept at 80°C, so that the mass ratio of input material (1) to NMP was 1:20. An antioxidant removal treatment was then carried out for 3 hours while stirring. After the treatment, the organic solvent and the extracted antioxidant and small pieces were separated using a mesh. The obtained small pieces were dried at 80°C for 3 hours and molded in a twin-screw extruder to produce pelletized recycled resin of Example 1. Next, the obtained pellets were reformed into a 100 μm thick sheet using a single-screw extruder to produce a single-layer sheet of recycled resin of Example 1.
[0151] [Example 2] The recycled resin of Example 2 was manufactured in the same manner as in Example 1, except that input material (1) was changed to input material (2).
[0152] [Example 3] The recycled resin of Example 3 was manufactured in the same manner as in Example 1, except that input material (1) was changed to input material (3).
[0153] [Example 4] The recycled resin of Example 4 was manufactured in the same manner as in Example 1, except that input material (1) was changed to input material (4).
[0154] [Example 5] The recycled resin of Example 5 was manufactured in the same manner as in Example 1, except that input material (1) was changed to input material (5).
[0155] [Example 6] In Example 1, the organic solvent had an SP value of 7.4 [cal / cm³]. 3 ] 1/2 The recycled resin of Example 6 was produced in the same manner as in Example 1, except that it was changed to heptane.
[0156] [Example 7] The recycled resin of Example 7 was manufactured in the same manner as in Example 4, except that input material (1) was changed to input material (4).
[0157] [Example 8] The recycled resin of Example 8 was manufactured in the same manner as in Example 1, except that the shredded shape of the input material (1) was changed to a strip shape with a width of 10 mm and a length of 100 mm.
[0158] [Example 9] The recycled resin of Example 9 was produced in the same manner as in Example 1, except that the temperature of the antioxidant removal treatment was changed to 25°C.
[0159] [Example 10] The recycled resin of Example 10 was produced in the same manner as in Example 1, except that the temperature of the antioxidant removal treatment was changed to 95°C.
[0160] [Comparative Example 1] A recycled resin of Comparative Example 1 was produced in the same manner as in Example 1, except that the input material (1) was cut into approximately 5 mm square pieces and then pelletized in a twin-screw extruder without any antioxidant removal treatment.
[0161] [Comparative Example 2] The recycled resin of Comparative Example 2 was produced in the same manner as in Example 2, except that the input material (2) was cut into approximately 5 mm square pieces and then pelletized in a twin-screw extruder without any antioxidant removal treatment.
[0162] [Comparative Example 3] The recycled resin of Comparative Example 3 was produced in the same manner as in Example 3, except that the input material (1) was cut into approximately 5 mm square pieces and then pelletized in a twin-screw extruder without any antioxidant removal treatment.
[0163] [Comparative Example 4] The recycled resin of Comparative Example 4 was produced in the same manner as in Example 4, except that the input material (4) was cut into approximately 5 mm square pieces and then pelletized in a twin-screw extruder without any antioxidant removal treatment.
[0164] [Comparative Example 5] In Example 1, the solvent used for the antioxidant removal treatment was a 2% by mass aqueous sodium hydroxide solution (SP value 23.5 [cal / cm³] 3 ] 1/2 The recycled resin of Comparative Example 5 was manufactured in the same manner as in Example 1, except that the following was changed:
[0165] [Example 11] Recycled resin for Example 11 was produced in the same manner as in Example 1, except that 1000 ppm of antioxidant (SumiLizer GP, manufactured by Sumitomo Chemical Co., Ltd.) was added again during pelletizing in a twin-screw extruder, the maximum temperature of the plastic material measured in the extruder was set to 281°C, and the residence time was set to 33 seconds.
[0166] [Example 12] The recycled resin of Example 12 was produced in the same manner as in Example 10, except that the amount of antioxidant added again was changed to 2000 ppm, the maximum temperature of the plastic material measured in the extruder was set to 281°C, and the residence time was set to 33 seconds.
[0167] [Example 13] The recycled resin of Example 13 was produced in the same manner as in Example 12, except that the maximum temperature of the plastic material measured in the extruder was 183°C and the residence time was 40 seconds.
[0168] [Example 14] The recycled resin of Example 14 was produced in the same manner as in Example 12, except that the maximum temperature of the plastic material measured in the extruder was 284°C and the residence time was 26 seconds.
[0169] [Example 15] The recycled resin of Example 15 was produced in the same manner as in Example 11, except that 1000 ppm of antioxidant (Irganox 1010, manufactured by BASF Japan Ltd.) and 1000 ppm of antioxidant (Irgafos 168, manufactured by BASF Japan Ltd.) were added again, the maximum temperature of the plastic material measured in the extruder was set to 274°C, and the residence time was set to 28 seconds.
[0170] [Example 16] The recycled resin of Example 16 was produced in the same manner as in Example 6, except that 2000 ppm of antioxidant (SumiLizer GP, manufactured by Sumitomo Chemical Co., Ltd.) was added again, the maximum temperature of the plastic material measured in the extruder was set to 281°C, and the residence time was set to 33 seconds.
[0171] <Evaluation> The obtained recycled resin was evaluated for residual antioxidant (amount of residual antioxidant), appearance, and elongation at break according to the following procedure. The results are shown in Tables 1 to 4 below.
[0172] (Residual Antioxidant) Recycled resin pellets were used as samples, and quantitative analysis of residual antioxidants in the samples was performed using high-performance liquid chromatography (1260 HPLC system, Agilent Technologies). The results were evaluated based on the following evaluation criteria. -Evaluation Criteria- ◎: Residual antioxidant amount is 100 ppm or less. ○: Residual antioxidant amount is greater than 100 ppm and 400 ppm or less. △: Residual antioxidant amount is greater than 400 ppm and 800 ppm or less. ×: Residual antioxidant amount is greater than 800 ppm.
[0173] In Examples 11-16, where antioxidants were re-added during pellet formation, the remaining amount of antioxidant was determined by subtracting the amount of re-added antioxidant from the quantitative analysis value of the antioxidant, and the evaluation was performed based on the above evaluation criteria.
[0174] (Appearance (Foreign Matter, Color)) The appearance of each single-layer sheet of recycled resin was visually observed, and the presence or absence of foreign matter and the color of the single-layer sheet were compared with the input material used, and evaluated based on the following evaluation criteria. -Evaluation Criteria (Foreign Matter)- ◎: The presence or absence of foreign matter in the single-layer sheet is the same as that of the input material used. ○: Granular matter (foreign matter) with a diameter of 0.5 mm or less is present on the surface. ×: Granular matter (foreign matter) with a diameter greater than 0.5 mm is present on the surface. -Evaluation Criteria (Color)- ◎: The color of the single-layer sheet is the same as that of the input material used. ○: The color change is only noticeable when the input material used is placed next to it. ×: A color change is noticeable even when viewed individually.
[0175] (Elongation at Breaking) A single-layer sheet of recycled resin was cut into strips measuring 15 mm x 100 mm and used as the measurement sample. The measurement sample was placed on a tensile testing machine with a chuck distance of 50 mm, and the elongation at breaking was measured when pulled at a speed of 300 mm / second. The evaluation was performed based on the following evaluation criteria. A Tensilon universal testing machine (RTG-1310, manufactured by A&D Co., Ltd.) was used for the tensile test. -Evaluation Criteria- ○: The elongation at breaking of the single-layer sheet of recycled resin is greater than or equal to the elongation at breaking of the input material used. ×: The elongation at breaking of the single-layer sheet of recycled resin is less than the elongation at breaking of the input material used.
[0176] (Oxidation Induction Time) In Examples 10 to 15, in which antioxidants were re-added during pellet formation, the oxidation induction time [minutes] was measured, and the measurement results are shown in Table 4 below. Specifically, the oxidation induction time was measured using a chemiluminescence analyzer (CLA-FS54, manufactured by Tohoku Electronics Industry Co., Ltd.) according to the following procedure in accordance with JIS K 7351. Recycled resin in pellet form was used as the measurement sample. A fixed amount of the measurement sample was measured into an aluminum sample container with a diameter of 20 mm to 30 mm, and the oxidation induction time was measured by observing the change in emission intensity using a chemiluminescence analyzer. The measurement conditions were as follows: sample weight: 0.2 g, temperature: constant at 220 °C, oxygen atmosphere, oxygen flow rate: 50 mL / min, exposure time: 1 second, measurement time: 7 hours.
[0177] A chemiluminescence analyzer is a measuring device that detects the amount of chemiluminescence in a sample. The oxidation induction time is the time it takes for the amount of chemiluminescence to increase significantly when measured under an oxygen atmosphere. For example, in the case of a resin composition containing a polyolefin resin and an antioxidant, the oxidation induction time is the time from the start of heating until the effect of the antioxidant, etc., on suppressing chemiluminescence wears off. The longer the time, the less likely the polyolefin resin is to be oxidized.
[0178]
[0179]
[0180]
[0181]
[0182] As shown in Tables 1-2, it was confirmed that recycled sheets with both good appearance and quality preservation could be obtained in Examples 1-10. Although not shown in the tables, similar results were obtained when virgin resin was blended in during the recycled sheet film formation process, or when the recycled resin was co-extruded between layers of virgin resin to create a multilayer structure.
[0183] On the other hand, as shown in Table 3, in Comparative Examples 1 to 5, the decomposition products of the antioxidant generated when the resin was heated during film formation and pelletizing of the input material remained in the resin, resulting in a decrease in appearance and quality.
[0184] Furthermore, as shown in Table 4, in Examples 11 to 16, where antioxidants were added again during pellet formation, it was found that not only was the presence or absence of foreign matter in the appearance observation not a problem for use, but the color evaluation was also superior.
[0185] <Test Example 2: Production of Recycled Resin from Plastic Materials Containing Lubricants> <Preparation of Input Material (6)> A masterbatch was prepared using a twin-screw extruder by mixing polyethylene resin pellets (Harmolex NH745N, manufactured by Nippon Polyethylene Co., Ltd.) with lubricant MB (M425, manufactured by Ube Maruzen Polyethylene Co., Ltd.) to a lubricant content of 100 ppm. Using this masterbatch, a 100 μm thick sheet was produced by casting using a single-screw extruder to obtain input material (6).
[0186] <Preparation of Input Material (7)> Input material (7) was obtained in the same manner as the preparation of input material (6), except that the lubricant content of input material (6) was changed to 500 ppm.
[0187] <Preparation of Input Material (8)> Input material (8) was obtained in the same manner as the preparation of input material (7), except that the lubricant MB of input material (7) was changed to M105 (manufactured by Ube Maruzen Polyethylene Co., Ltd.).
[0188] <Preparation of Input Material (9)> Input material (9) was obtained in the same manner as the preparation of input material (7), except that the lubricant MB of input material (7) was changed to M205 (manufactured by Ube Maruzen Polyethylene Co., Ltd.).
[0189] <Preparation of Input Material (10)> Input material (10) was obtained in the same manner as the preparation of input material (7), except that the lubricant content of input material (7) was changed to a total of 1500 ppm, consisting of 500 ppm of M425 (manufactured by Ube Maruzen Polyethylene Co., Ltd.), 500 ppm of M105 (manufactured by Ube Maruzen Polyethylene Co., Ltd.), and 500 ppm of M205 (manufactured by Ube Maruzen Polyethylene Co., Ltd.).
[0190] <Examples 17-29 and Comparative Examples 6-11> [Example 1] The input material (6) was cut into pieces approximately 5 mm square. The organic solvent had an SP value of 11.2 [cal / cm²]. 3 ] 1/2N-methyl-2-pyrrolidone (NMP) was used and heated to 80°C. Small pieces of input material (6) were added to the NMP, which was kept at 80°C, so that the mass ratio of input material (6) to NMP was 1:20, and a lubricant removal treatment was carried out for 3 hours while stirring. After the treatment, the organic solvent and extracted lubricant and small pieces were separated using a mesh, and the obtained small pieces were dried at 80°C for 3 hours to obtain the small-piece recycled resin of Example 1.
[0191] The obtained small pieces were then given 200 ppm of lubricant (lubricant re-addition treatment) and pelletized using a twin-screw extruder at a processing temperature of 170°C.
[0192] Next, the obtained pellets were reformed into a 100 μm thick sheet using a single-screw extruder to produce the single-layer sheet-like recycled resin of Example 17.
[0193] [Example 18] The recycled resin of Example 18 was manufactured in the same manner as in Example 17, except that input material (6) was changed to input material (7).
[0194] [Example 19] The recycled resin of Example 19 was manufactured in the same manner as in Example 17, except that input material (6) was changed to input material (8).
[0195] [Example 20] The recycled resin of Example 20 was manufactured in the same manner as in Example 17, except that input material (6) was changed to input material (9).
[0196] [Example 21] The recycled resin of Example 21 was manufactured in the same manner as in Example 17, except that the input material (6) was changed to input material (10).
[0197] [Example 22] The recycled resin of Example 22 was produced in the same manner as in Example 18, except that the temperature in the lubricant removal treatment was changed to 30°C.
[0198] [Example 23] In Example 22, the organic solvent had an SP value of 7.3 [cal / cm³]. 3 ]1/2 The recycled resin of Example 23 was produced in the same manner as in Example 22, except that the hexane was changed.
[0199] [Example 24] In Example 22, the organic solvent had an SP value of 12.7 [cal / cm³]. 3 ] 1/2 The recycled resin of Example 24 was produced in the same manner as in Example 22, except that the ethanol was changed to [the same substance].
[0200] [Example 25] The recycled resin of Example 25 was manufactured in the same manner as in Example 18, except that the shredded shape of the input material (7) was changed to a strip shape with a width of 10 mm and a length of 100 mm.
[0201] [Example 26] The recycled resin of Example 26 was produced in the same manner as in Example 18, except that the temperature in the lubricant removal treatment was changed to 20°C.
[0202] [Example 27] The recycled resin of Example 27 was produced in the same manner as in Example 18, except that the temperature in the lubricant removal treatment was changed to 95°C.
[0203] [Example 28] The recycled resin of Example 28 was manufactured in the same manner as in Example 18, except that the mass ratio of the input material to NMP was changed to 1:1.
[0204] [Example 29] The recycled resin of Example 29 was manufactured in the same manner as in Example 18, except that the mass ratio of the input material to NMP was changed to 1:40.
[0205] [Comparative Example 6] The recycled resin of Comparative Example 6 was produced in the same manner as in Example 17, except that the input material (6) was cut into approximately 5 mm square pieces and then pelletized in a twin-screw extruder without undergoing lubricant removal treatment and lubricant re-addition treatment.
[0206] [Comparative Example 7] The recycled resin of Comparative Example 7 was produced in the same manner as in Example 18, except that the input material (7) was cut into approximately 5 mm square pieces, and then, without a lubricant removal treatment, 200 ppm of lubricant was added again in a lubricant re-addition treatment and the material was pelletized using a twin-screw extruder.
[0207] [Comparative Example 8] In Example 17, the solvent used in the lubricant removal treatment was a 2% by mass sodium hydroxide aqueous solution (SP value 23.5 [cal / cm³] 3 ] 1/2 The recycled resin of Comparative Example 8 was produced in the same manner as in Example 17, except that the lubricant was changed to a different type, and the small pieces obtained after the lubricant removal treatment were pelletized directly in a twin-screw extruder without going through the lubricant re-addition treatment.
[0208] [Comparative Example 9] In Example 18, the solvent used in the lubricant removal treatment was a 2% by mass aqueous sodium hydroxide solution (SP value 23.5 [cal / cm³] 3 ] 1/2 The recycled resin of Comparative Example 9 was manufactured in the same manner as in Example 18, except that the following was changed:
[0209] [Comparative Example 10] In Example 17, the organic solvent used in the lubricant removal treatment was methanol (SP value 14.5 [cal / cm³] 3 ] 1/2 The recycled resin of Comparative Example 10 was produced in the same manner as in Example 17, except that the lubricant was changed to a different type, and the small pieces obtained after the lubricant removal treatment were pelletized directly in a twin-screw extruder without going through the lubricant re-addition treatment.
[0210] [Comparative Example 11] In Example 18, the organic solvent used in the lubricant removal treatment was methanol (SP value 14.5 [cal / cm³] 3 ] 1/2 The recycled resin of Comparative Example 11 was manufactured in the same manner as in Example 18, except that the following was changed:
[0211] <Evaluation> The amount of lubricant remaining and the lubricity of the obtained recycled resin were evaluated according to the following procedure. The results are shown in Tables 5 to 7 below.
[0212] (Remaining Lubricant Amount) Using small pieces of recycled resin as a sample, quantitative analysis of the lubricant remaining in the sample was performed using a gas chromatograph (GC7890A / G1888A, manufactured by Agilent Technologies, Inc.) as shown below. Specifically, the recycled resin sample was held in 10 ml of chloroform at 60°C for 8 hours to obtain a solution, and 1.0 μl of this sample was injected into a gas chromatograph (split ratio: 1 / 50, carrier gas: He). Next, it was held at 40°C for 1 minute, and then the temperature was raised to 300°C at a heating rate of 10°C / min. Meanwhile, chloroform solutions containing several concentrations of fatty acid amides were measured beforehand as standard solutions. The remaining amount of lubricant was then calculated by drawing a calibration curve of peak area and concentration. In the gas chromatograph, an HP-5MS column (inner diameter 0.25 mm, length 30 m, film thickness 0.25 μm) was used, and the detector was an FID.
[0213] Based on the obtained quantitative analysis values, the amount of lubricant remaining was evaluated according to the following evaluation criteria. —Evaluation Criteria— ◎: The amount of lubricant remaining is 100 ppm or less. ○: The amount of lubricant remaining is greater than 100 ppm but 200 ppm or less. ×: The amount of lubricant remaining is greater than 200 ppm.
[0214] (Slipperiness) A single-layer sheet of recycled resin was used as a sample, and the static friction coefficient of the sample was measured using a friction measuring instrument (Friction Tester TR-2, manufactured by Toyo Seiki Seisakusho Co., Ltd.) in accordance with the JIS K 7125:1999 standard, and evaluated based on the following evaluation criteria. —Evaluation Criteria— ◎: Static friction coefficient is 0.2 or more and 0.4 or less. ○: Static friction coefficient is 0.1 or more and less than 0.2, or greater than 0.4 and 0.5 or less. ×: Static friction coefficient is less than 0.1, or greater than 0.5.
[0215]
[0216]
[0217]
[0218] As shown in Tables 5-6, in Examples 17-29, the amount of lubricant remaining was 100 ppm or less, confirming that the lubricant in the input material could be effectively removed and that recycled sheets with good lubricity could be obtained.
[0219] On the other hand, as shown in Table 7, in Comparative Examples 6 to 11, the resulting recycled sheets had either too high a static friction coefficient, making them difficult to slide, or too low a static friction coefficient, due to insufficient or excessive lubricant. This suggests that the amount of lubricant remaining could not be accurately estimated because the lubricant derived from the input material was not removed or could not be effectively removed, resulting in poor lubricity of the resulting recycled resin.
[0220] While specific embodiments have been described above, this disclosure is not limited to the requirements shown in the embodiments described above. These points may be modified to the extent that they do not impair the spirit of this disclosure, and can be appropriately determined according to their application.
[0221] The embodiments disclosed above are further specified, for example, by the following embodiments: [1] A method for producing recycled resin from a plastic material, wherein the plastic material has an SP value of 7 [cal / cm³]. 3 ] 1/2 Above 13 [cal / cm 3 ] 1/2 A method for producing recycled resin, comprising the step of adding the following organic solvent to remove one or more target substances selected from the group consisting of antioxidants, lubricants, and trace chemical substances. [2] The method for producing recycled resin according to [1], wherein the removal is to transfer the target substances to the organic solvent. [3] The plastic material is 100 mm 3A method for producing recycled resin according to [1] or [2], wherein the recycled resin is in the form of the following small pieces: [4] A method for producing recycled resin according to any one of [1] to [3], wherein the removal of the target substance is carried out at a temperature of 30°C to 90°C. [5] A method for producing recycled resin according to any one of [1] to [4], wherein the organic solvent is one or more selected from xylene, toluene, heptane, N-methyl-2-pyrrolidone (NMP), diethylene glycol monobutyl ether, benzene, ethylbenzene, styrene, octane, hexane, trichloroethylene, diethyl ether, butyl acetate, ethyl acetate, chloroform, dichloromethane, acetone, and ethanol. [6] A method for producing recycled resin according to any one of [1] to [5], wherein the amount of the organic solvent added is 100 parts by mass or more and 4000 parts by mass or less per 100 parts by mass of the plastic material. [7] A method for producing recycled resin according to any one of [1] to [6], further comprising the step of washing the plastic material with a washing solution containing an amphiphilic solvent to remove the residue of the organic solvent. [8] The method for producing a recycled resin according to any one of [1] to [7], wherein the target substance is the antioxidant and / or the lubricant, and further comprises adding the antioxidant and / or the lubricant to the obtained recycled resin. [9] The method for producing a recycled resin according to any one of [1] to [8], further comprising the step of melt-molding the obtained recycled resin.
[10] The method for producing a recycled resin according to any one of [1] to [9], wherein the target substance includes the antioxidant, and the residual amount of the antioxidant measured in a high-performance liquid chromatography test in the recycled resin is 800 ppm or less.
[11] The method for producing a recycled resin according to any one of [1] to
[10] , wherein the target substance includes the lubricant, and the residual amount of the lubricant measured in a gas chromatography test in the recycled resin is 200 ppm or less.
[12] The method for producing a molded article of recycled resin, comprising the step of melt-molding the recycled resin obtained by the method of any one of [1] to
[11] .
[13] A recycled resin made from a plastic material containing at least an antioxidant additive, wherein the residual amount of the antioxidant derived from the plastic material, as measured by high-performance liquid chromatography, is 800 ppm or less.
[14] A recycled resin made from a plastic material containing at least a lubricant additive, wherein the residual amount of the lubricant derived from the plastic material, as measured by gas chromatography, is 200 ppm or less.
[15] A recycled resin made from a plastic material containing at least trace chemicals, wherein the residual amount of isononylphenol, which is a trace chemical derived from the plastic material and is measured by a trace chemical test, is less than 1,000 μg / kg, the residual amount of PCB77, which is a trace chemical derived from the plastic material and is measured by a trace chemical test method, is less than 75 ng / kg, and the residual amount of PCB118, which is a trace chemical derived from the plastic material and is measured by a trace chemical test method, is less than 2,000 ng / kg, and the residual amount of PCB118, which is a trace chemical derived from the plastic material and is measured by a trace chemical test method A recycled resin wherein the residual amount of OCDD, a trace chemical substance derived from the plastic material, is less than 45 ng / kg, the residual amount of OCDF, a trace chemical substance derived from the plastic material, as measured by the trace chemical substance test method, is less than 1.8 ng / kg, the residual amount of bisphenol A, a trace chemical substance derived from the plastic material, as measured by the trace chemical substance test method, is less than 2,500 μg / kg, and the residual amount of diisononyl phthalate, a trace chemical substance derived from the plastic material, as measured by the trace chemical substance test method, is less than 1,000 μg / kg.
[16] A film-like molded article containing the recycled resin described in any of
[13] to
[15] .
[17] A packaging material containing the film-like molded article described in
[16] .
[18] The packaging material described in
[17] , wherein the content of the recycled resin is 80% by mass or more relative to the resin component of the packaging material.
[0222] 1. Recycled resin-containing layer 2. Non-recycled resin-containing layer 3. Adhesive layer 4. Nylon film 5. Printing layer 6. Cover layer 10. Single-layer sheet 20, 30. Multi-layer sheet 40. Laminate
Claims
1. A method for producing recycled resin from plastic material, wherein the plastic material has an SP value of 7 [cal / cm³]. 3 ] 1/2 Above 13 [cal / cm 3 ] 1/2 A method for producing recycled resin, comprising the step of adding the following organic solvents to remove one or more target substances selected from the group consisting of antioxidants, lubricants, and trace chemical substances.
2. The method for producing recycled resin according to claim 1, wherein the removal involves transferring the target substance to the organic solvent.
3. The aforementioned plastic material is 100 mm 3 A method for producing recycled resin according to claim 1, wherein the recycled resin is in the form of the following small pieces.
4. The method for producing recycled resin according to claim 1, wherein the removal of the target substance is carried out at a temperature of 30°C to 90°C.
5. The method for producing recycled resin according to claim 1, wherein the organic solvent is one or more selected from xylene, toluene, heptane, N-methyl-2-pyrrolidone (NMP), diethylene glycol monobutyl ether, benzene, ethylbenzene, styrene, octane, hexane, trichloroethylene, diethyl ether, butyl acetate, ethyl acetate, chloroform, dichloromethane, acetone, and ethanol.
6. The method for producing recycled resin according to claim 1, wherein the amount of the organic solvent added is 100 parts by mass or more and 4000 parts by mass or less per 100 parts by mass of the plastic material.
7. The method for producing recycled resin according to claim 1, further comprising the step of washing the plastic material with a cleaning solution containing an amphiphilic solvent to remove any residue of the organic solvent.
8. The method for producing a recycled resin according to claim 1, wherein the target substance is the antioxidant and / or the lubricant, and further comprises adding the antioxidant and / or the lubricant back to the recycled resin obtained.
9. A method for producing recycled resin according to claim 1, further comprising the step of melt-molding the obtained recycled resin.
10. The method for producing recycled resin according to claim 1, wherein the target substance includes the antioxidant, and the residual amount of the antioxidant measured in the recycled resin by high-performance liquid chromatography is 800 ppm or less.
11. The method for producing a recycled resin according to claim 1, wherein the target substance includes the lubricant, and the residual amount of the lubricant measured in a gas chromatography test in the recycled resin is 200 ppm or less.
12. A method for producing a molded article of recycled resin, comprising the step of melt-molding the recycled resin obtained by the method of claim 1.
13. A recycled resin made from a plastic material containing at least an antioxidant additive, wherein the residual amount of the antioxidant derived from the plastic material, as measured by high-performance liquid chromatography, is 800 ppm or less.
14. A recycled resin made from a plastic material containing at least a lubricant as an additive, wherein the residual amount of the lubricant derived from the plastic material, as measured by gas chromatography, is 200 ppm or less.
15. A recycled resin made from a plastic material containing at least trace chemical substances, wherein the residual amount of isononylphenol, which is a trace chemical substance derived from the plastic material, as measured by a trace chemical substance test, is less than 1,000 μg / kg; the residual amount of PCB77, which is a trace chemical substance derived from the plastic material, as measured by a trace chemical substance test method, is less than 75 ng / kg; the residual amount of PCB118, which is a trace chemical substance derived from the plastic material, as measured by a trace chemical substance test method, is less than 2,000 ng / kg; the residual amount of OCDD, which is a trace chemical substance derived from the plastic material, as measured by a trace chemical substance test method, is less than 45 ng / kg; the residual amount of OCDF, which is a trace chemical substance derived from the plastic material, as measured by a trace chemical substance test method, is less than 1.8 ng / kg; and the residual amount of bisphenol A, which is a trace chemical substance derived from the plastic material, as measured by a trace chemical substance test method, is less than 2,500 μg / kg. A recycled resin in which the residual amount of diisononyl phthalate, a trace chemical substance derived from the plastic material, as measured by the trace chemical substance testing method, is less than 1,000 μg / kg.
16. A film-like molded article containing the recycled resin described in any one of claims 13 to 15.
17. A packaging material containing the film-like molded body described in claim 16.
18. The packaging material according to claim 17, wherein the content of the recycled resin is 80% by mass or more relative to the resin component of the packaging material.