Copolymer, copolymer composition, and antifouling coating composition
The copolymer composition with specific constituent units (A) and (B) addresses the challenges of high viscosity and insufficient antifouling effects in existing coatings by forming a film with improved antifouling properties and application characteristics.
Patent Information
- Application Number
- PCT/JP2026/018122
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Existing antifouling coatings face challenges in achieving high solid differentiation while maintaining long-term antifouling effects, with resin compositions becoming highly viscous when reducing organic solvent content, making application difficult and the coating film's antifouling properties insufficient.
A copolymer composition comprising constituent units (A) and (B), where (A) includes metal-containing structures for self-polishing properties and (B) includes monomers with specific molecular weights and glass transition temperatures, combined with antifouling agents and solvents, to form a coating film with excellent antifouling properties.
The copolymer composition enables the formation of a coating film with enhanced antifouling properties and improved application characteristics, maintaining long-term effectiveness and reducing viscosity, thus addressing the challenges of high solid differentiation and coating film performance.
Smart Images

Figure JP2026018122_19112026_PF_FP_ABST
Abstract
Description
Copolymer, copolymer composition, and antifouling paint composition
[0001] The present invention relates to copolymers, copolymer compositions, and antifouling coating compositions. This application claims priority under Japanese Patent Application No. 2025-081294, filed in Japan on 14 May 2025, the contents of which are incorporated herein by reference.
[0002] It is known that antifouling coatings are applied to marine structures and ships to prevent corrosion of parts in contact with seawater and to prevent the attachment of marine organisms, which can cause a decrease in sailing speed. Self-polishing antifouling coatings are known as such coatings. Self-polishing antifouling coatings typically contain a hydrolyzable resin and an antifouling agent. The coating obtained from this antifouling coating undergoes surface renewal (self-polishing) as the coating surface gradually dissolves in seawater, and the antifouling agent is constantly exposed on the coating surface, thus providing long-term antifouling effects.
[0003] As a self-polishing antifouling coating, for example, a resin composition containing a metal-containing polymer has been proposed. Such a resin composition is compounded with an antifouling agent to make it an antifouling coating. The metal-containing polymer contained in these resin compositions is hydrolyzable, and the coating film containing it exhibits self-polishing properties. A resin composition obtained by copolymerizing a reaction product of an inorganic metal compound and a carboxyl group-containing radical polymerizable monomer, a metal-containing monomer mixture consisting of an organic solvent containing at least an alcohol-based solvent and a specific amount of water, and other radical polymerizable unsaturated monomers (Patent Document 1). A (meth)acrylic copolymer having a structural unit having a specific metal and a structural unit derived from a macromonomer, and an organic solvent, with a viscosity of 5 × 10 at 25°C. 4 A resin composition containing a polymer solution with a pressure of mPa·s or less (Patent Document 2).
[0004] In recent years, due to environmental concerns, reducing volatile organic compounds (VOCs) has become important, and VOC reduction is also being considered for antifouling coatings. The resin composition described in Patent Document 2 has been proposed as an antifouling coating composition with a reduced organic solvent content.
[0005] Japanese Patent Publication No. 2002-012630, International Publication No. 2017 / 051922
[0006] The coating film formed from the antifouling paint using the resin composition of Patent Document 1 has a low contact angle, and the long-term antifouling effect of the coating film is not necessarily sufficient. Furthermore, when attempting to reduce the organic solvent content of this resin composition to achieve high solid differentiation, it becomes highly viscous, making the preparation and application of the antifouling paint difficult, thus presenting a problem in achieving high solid differentiation.
[0007] The coating film formed from the antifouling paint using the resin composition of Patent Document 2 has a low contact angle, and the long-term antifouling effect of the coating film is not necessarily sufficient.
[0008] The object of the present invention is to provide an antifouling paint composition that can form a coating film with excellent antifouling properties, and a (meth)acrylic copolymer and copolymer composition suitable for obtaining an antifouling paint composition that can form a coating film with excellent antifouling properties.
[0009] The present invention has the following aspects: [1] A copolymer comprising a constituent unit (A) and a constituent unit (B), wherein the constituent unit (A) has at least one structure selected from the group consisting of a structure represented by the following formula (a1) and a structure represented by the following formula (a2), the constituent unit (B) is at least one selected from the group consisting of a constituent unit (B1) and a constituent unit (B2), the constituent unit (B1) is a monomer represented by the following formula (b1), has a molecular weight of 200 to 500, and is a constituent unit derived from monomer (b1) having a glass transition temperature of 40°C or less when it is a homopolymer, and the constituent unit (B2) is a compound having a radical polymerizable group and having two or more constituent units represented by the following formula (Z1), and is a constituent unit derived from compound (b2) having a glass transition temperature of 10°C or less. -COO-M-OCO- ... (a1) -COO-M-R 1 ... (a2) (wherein M represents a divalent metal atom, R 1 (This indicates a monovalent organic acid residue.) CH 2 =CR 31 - COOR 32 ...(b1) (wherein, R 31 is a hydrogen atom, a methyl group, or CH2 represents OH, R 32 represents an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, an unsubstituted or substituted non-aromatic heterocyclic group, or an unsubstituted or substituted aralkyl group.)
[0010]
[0011] (wherein R 41 is a hydrogen atom, a methyl group or CH 2 OH, R 42 is OR 43 , a halogen atom, COR 44 , COOR 45 , CN, CONR 46 R 47 or R 48 . R 43 to R 47 each independently represent a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, an unsubstituted or substituted non-aromatic heterocyclic group, or an unsubstituted or substituted aralkyl group. R 48 represents an unsubstituted or substituted aryl group, or an unsubstituted or substituted heteroaryl group.) [2] The solubility parameter of the aforementioned monomer (b1) is 9.5 (cal / cm 3 ) 1/2The copolymer of [1] is as follows: [3] A copolymer composition comprising the copolymer of [1] or [2]. [4] A copolymer composition of [3] further comprising a solvent. [5] An antifouling paint composition comprising the copolymer composition of [3] or [4]. [6] An antifouling paint composition of [5] further comprising an antifouling agent. [7] An antifouling paint composition of [6] wherein the antifouling agent comprises at least one selected from the group consisting of 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitride and medetomidine. [8] An antifouling paint composition of any of [5] to [7] further comprising a thermoplastic resin (excluding the copolymer of [1] or [2]).
[0012] According to the present invention, it is possible to provide an antifouling paint composition that can form a coating film with excellent antifouling properties, as well as a copolymer and copolymer composition suitable for obtaining an antifouling paint composition that can form a coating film with excellent antifouling properties.
[0013] The following definitions of terms apply throughout this specification and the claims: “Constituent unit” may be formed directly from monomers by polymerization, or it may be a constituent unit obtained by processing a polymer resulting from polymerization, thereby converting some of the structural components of the constituent unit in the polymer to another structure. “Monomer” means a polymerizable compound (polymerizable monomer). “(meth)acrylic” is a general term for acrylic and methacrylic; “(meth)acryloyl group” is a general term for acryloyl group and methacryloyl group; “(meth)acrylate” is a general term for acrylate and methacrylate; “(meth)acrylic acid” is a general term for acrylic acid and methacrylic acid; “(meth)acrylonitrile” is a general term for acrylonitrile and methacrylonitrile; and “(meth)acrylamide” is a general term for acrylamide and methacrylamide. “Viscosity” means the value measured by a B-type viscometer unless otherwise specified. "VOC" refers to organic compounds that readily volatilize at room temperature and pressure (volatile organic compounds).
[0014] [Copolymer] The copolymer of this embodiment is a copolymer having a constituent unit (A) and a constituent unit (B), wherein the constituent unit (B) is at least one selected from the group consisting of constituent unit (B1) and constituent unit (B2). The copolymer of this embodiment may further have other constituent units other than constituent units (A) and constituent unit (B) (hereinafter also referred to as "constituent unit (C)").
[0015] <Constituent Unit (A)> Constituent unit (A) has at least one structure selected from the group consisting of the structure represented by the following formula (a1) and the structure represented by the following formula (a2). -COO-M-OCO- ... (a1) -COO-M-R 1 ... (a2) (wherein M represents a divalent metal atom, R 1 (This indicates a monovalent organic acid residue.)
[0016] The constituent unit (A) has a carboxylate that is ionically bonded to a divalent metal atom represented by M, and thus contributes to the development of self-polishing properties. As the divalent metal atom represented by M, Zn, Cu, Mg, or Ca are preferred, and Zn or Cu are more preferred, from the viewpoint of providing good water resistance of the coating film.
[0017] R 1 The organic acid residue refers to the remaining portion of an organic acid after removing one proton (for example, the remaining portion of an organic carboxylic acid after removing the proton from the carboxyl group). The atom to which the removed proton was bonded is ionically bonded with a divalent metal atom represented by M. Preferred organic acids are carboxylic acids, such as monochloroacetic acid, monofluoroacetic acid, acetic acid, propionic acid, octic acid, versatic acid, isostearic acid, palmitic acid, cresotic acid, α-naphthoic acid, β-naphthoic acid, benzoic acid, 2,4,5-trichlorophenoxyacetic acid, 2,4-dichlorophenoxyacetic acid, quinoline carboxylic acid, nitrobenzoic acid, nitronaphthalene carboxylic acid, pyruvic acid, naphthenic acid, abietic acid, and hydrogenated abietic acid. As for the organic acid, fatty acids (aliphatic monocarboxylic acids) having 1 to 20 carbon atoms are preferred because they provide a highly durable coating film that can prevent cracking and peeling over a long period of time.
[0018] The constituent unit (A) may be a constituent unit derived from monomer (a) having at least one structure selected from the group consisting of the structure represented by formula (a1) and the structure represented by formula (a2), and a radical polymerizable group. The monomer (a) is preferably at least one selected from the group consisting of the monomer represented by the following formula (a1-1) (hereinafter also referred to as "monomer (a1-1)") and the monomer represented by the following formula (a2-1) (hereinafter also referred to as "monomer (a2-1)").
[0019] CH 2 =CR 11 -COO-M-OCO-CR 12 =CH 2 ...(a1-1) CH 2 =CR 13 -COO-M-R 1 ... (a2-1) (wherein M and R 1 As stated above, R 11 , R 12 and R 13 Each of these independently represents either a hydrogen atom or a methyl group.
[0020] The constituent unit derived from monomer (a1-1) is represented by the following formula (A1-1). The constituent unit derived from monomer (a2-1) is represented by the following formula (A2-1). Therefore, as structural unit (A), at least one selected from the group consisting of the constituent unit represented by the following formula (A1-1) and the constituent unit represented by the following formula (A2-1) is preferred.
[0021]
[0022] (In the formula, M, R 1 , R 11 , R 12 and R 13 (As stated above.)
[0023] Examples of monomers (a1-1) include zinc acrylate [(CH 2 =CHCOO) 2 Zn], zinc methacrylate [(CH 2 = C(CH 3 ) COO) 2 Zn], copper acrylate [(CH] 2=CHCOO) 2 Cu], copper methacrylate [(CH] 2 = C(CH 3 ) COO) 2 Cu], magnesium acrylate [(CH] 2 =CHCOO) 2 Mg], magnesium methacrylate [(CH 2 = C(CH 3 ) COO) 2 Mg], calcium acrylate [(CH 2 =CHCOO) 2 Ca], calcium methacrylate [(CH 2 = C(CH 3 ) COO) 2 Ca is one example. In particular, zinc (meth)acrylate and copper (meth)acrylate are preferred from the viewpoint of the water resistance of the coating film containing the copolymer of this embodiment. These may be used individually or in combination of two or more.
[0024] Examples of monomers (a2-1) include the following compounds: monochlorometallic acetate (meth)acrylates such as magnesium monochloroacetate (meth)acrylate, calcium monochloroacetate (meth)acrylate, zinc monochloroacetate (meth)acrylate, and copper monochloroacetate (meth)acrylate; monofluorometallic acetate (meth)acrylates such as magnesium monofluoroacetate (meth)acrylate, calcium monofluoroacetate (meth)acrylate, zinc monofluoroacetate (meth)acrylate, and copper monofluoroacetate (meth)acrylate; metallic acetate (meth)acrylates such as magnesium acetate (meth)acrylate, calcium acetate (meth)acrylate, zinc acetate (meth)acrylate, and copper acetate (meth)acrylate; metal propionate (meth)acrylates such as magnesium propionate (meth)acrylate, calcium propionate (meth)acrylate, zinc propionate (meth)acrylate, and copper propionate (meth)acrylate; Octylate metal (meth)acrylates such as magnesium (meth)acrylate octylate, calcium (meth)acrylate octylate, zinc (meth)acrylate octylate, and copper (meth)acrylate octylate; Versatiate metal (meth)acrylates such as magnesium (meth)acrylate versatiate, calcium (meth)acrylate versatiate, zinc (meth)acrylate versatiate, and copper (meth)acrylate versatiate; Isostearate metal (meth)acrylates such as magnesium (meth)acrylate isostearate, calcium (meth)acrylate isostearate, zinc (meth)acrylate isostearate, and copper (meth)acrylate isostearate; Palmitate metal (meth)acrylates such as magnesium (meth)acrylate palmitate, calcium (meth)acrylate palmitate, zinc (meth)acrylate palmitate, and copper (meth)acrylate palmitate; Metal cresoates (meth)acrylates such as magnesium cresoate (meth)acrylate, calcium cresoate (meth)acrylate, zinc cresoate (meth)acrylate, and copper cresoate (meth)acrylate;α-Naphthoate metal (meth)acrylates such as α-Magnesium (meth)acrylate α-Naphthoate, α-Calcium (meth)acrylate α-Naphthoate, α-Zinc (meth)acrylate α-Naphthoate, and α-Copper (meth)acrylate α-Naphthoate; β-Naphthoate metal (meth)acrylates such as β-Magnesium (meth)acrylate β-Naphthoate, β-Calcium (meth)acrylate β-Naphthoate, β-Zinc (meth)acrylate β-Naphthoate, and β-Copper (meth)acrylate β-Naphthoate; benzoate metal (meth)acrylates such as Magnesium (meth)acrylate benzoate, Calcium (meth)acrylate benzoate, Zinc (meth)acrylate benzoate, and Copper (meth)acrylate benzoate; Metal (meth)acrylates of 2,4,5-trichlorophenoxyacetate, such as magnesium (meth)acrylate of 2,4,5-trichlorophenoxyacetate, calcium (meth)acrylate of 2,4,5-trichlorophenoxyacetate, zinc (meth)acrylate of 2,4,5-trichlorophenoxyacetate, and copper (meth)acrylate of 2,4,5-trichlorophenoxyacetate; metal (meth)acrylates of 2,4-dichlorophenoxyacetate, such as magnesium (meth)acrylate of 2,4-dichlorophenoxyacetate, calcium (meth)acrylate of 2,4-dichlorophenoxyacetate, zinc (meth)acrylate of 2,4-dichlorophenoxyacetate, and copper (meth)acrylate of 2,4-dichlorophenoxyacetate; Metal (meth)acrylates of quinoline carboxylate, such as magnesium (meth)acrylate of quinoline carboxylate, calcium (meth)acrylate of quinoline carboxylate, zinc (meth)acrylate of quinoline carboxylate, and copper (meth)acrylate of quinoline carboxylate; metal (meth)acrylates of nitrobenzoate, such as magnesium (meth)acrylate of nitrobenzoate, calcium (meth)acrylate of nitrobenzoate, zinc (meth)acrylate of nitrobenzoate, and copper (meth)acrylate of nitrobenzoate; metal (meth)acrylates of nitronaphthalene carboxylate, such as magnesium (meth)acrylate of nitronaphthalene carboxylate, calcium (meth)acrylate of nitronaphthalene carboxylate, zinc (meth)acrylate of nitronaphthalene carboxylate, and copper (meth)acrylate of nitronaphthalene carboxylate;Metal pyruvate (meth)acrylates such as magnesium pyruvate (meth)acrylate, calcium pyruvate (meth)acrylate, zinc pyruvate (meth)acrylate, and copper pyruvate (meth)acrylate. These may be used individually or in combination of two or more.
[0025] The copolymer of this embodiment may have only one of the constituent units (A1) and (A2), or it may have both. When the copolymer has both constituent units (A1) and (A2), the ratio (molar ratio) of constituent units (A1) to constituent units (A2) in the copolymer, (A1) / (A2), is preferably 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20, and even more preferably 30 / 70 to 70 / 30. If this ratio is below the upper limit, the viscosity of the copolymer solution tends to decrease, and if it is above the lower limit, the self-polishing properties of the coating film tend to be maintained over a long period of time.
[0026] [Method for producing monomer (a)] Monomer (a) may be a monomer produced by a known method, or it may be a commercially available monomer.
[0027] Monomer (a1-1) can be obtained, for example, by reacting an inorganic metal compound containing the metal element corresponding to M in formula (a1-1) with a carboxyl group-containing polymerizable monomer such as (meth)acrylic acid in a diluent such as a solvent or a reactive diluent having a polymerizable unsaturated group such as an ethylenically unsaturated monomer. A mixture containing monomer (a1-1) obtained by this method has excellent compatibility with solvents and other monomers, and polymerization can be easily carried out. The reaction to obtain monomer (a1-1) is preferably carried out in the presence of water, and the water content in the reactant is preferably in the range of 0.01 to 30% by mass. Examples of the inorganic metal compound include oxides, hydroxides, and chlorides of metals selected from the group consisting of Zn, Cu, Mg, and Ca.
[0028] Monomer (a2-1) is, for example, an inorganic metal compound containing the metal element corresponding to M in formula (a2-1), a carboxyl group-containing polymerizable monomer such as (meth)acrylic acid, and the organic acid residue R in formula (a2-1).1 It is obtained by reacting the corresponding organic acid in a diluent such as a solvent or a reactive diluent having polymerizable unsaturated groups such as an ethylenically unsaturated monomer. The inorganic metal compound can be the same as the inorganic metal compound used to obtain monomer (a1-1).
[0029] A monomer mixture containing monomer (a1-1) and monomer (a2-1) can be prepared by mixing monomer (a1-1) and monomer (a2-1) separately, or by mixing, for example, an inorganic metal compound containing the metal element corresponding to M in formula (a1-1) and formula (a2-1), a carboxyl group-containing polymerizable monomer such as (meth)acrylic acid, and the organic acid residue R in formula (a2-1). 1 The organic acid corresponding to is obtained by reacting it in a solvent or other diluent or a reactive diluent having polymerizable unsaturated groups such as an ethylenically unsaturated monomer. In this case, the organic acid residue R in formula (a2-1) is obtained. 1 The amount of organic acid used is preferably 0.01 to 3 times the molar amount relative to the inorganic metal compound, more preferably 0.01 to 0.95 times, and even more preferably 0.1 to 0.7 times. Organic acid residue R in formula (a2-1) 1 If the amount of organic acid used is above the lower limit, solid precipitation is suppressed in the manufacturing process of the monomer mixture containing monomer (a1-1) and monomer (a2-1), and the self-polishing properties and crack resistance of the resulting coating film are improved. If it is below the upper limit, the antifouling properties of the resulting coating film tend to be maintained for a longer period of time.
[0030] <Constituent Unit (B)> Constituent unit (B) is at least one selected from the group consisting of constituent unit (B1) and constituent unit (B2). Constituent unit (B1) is a constituent unit derived from monomer (b1). Constituent unit (B2) is a constituent unit derived from compound (b2).
[0031] [Constituent Unit (B1)] The monomer (b1) is a monomer represented by the following formula (b1), having a molecular weight of 200 to 500, and a glass transition temperature of 40°C or less when it is a homopolymer. CH 2 =CR 31 - COOR 32...(b1) (wherein, R 31 is a hydrogen atom, a methyl group, or CH 2 Showing OH, R 32 This refers to an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, an unsubstituted or substituted non-aromatic heterocyclic group, or an unsubstituted or substituted aralkyl group.
[0032] R 32 In this context, the alkyl group represents a linear alkyl group or a branched alkyl group. For example, a linear or branched alkyl group having 1 to 20 carbon atoms is used. Examples of linear or branched alkyl groups having 1 to 20 carbon atoms include methyl group, ethyl group, n-propyl group, i-propyl group, n-butyl group, t-butyl group, i-butyl group, pentyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, octadecyl group, nonadecyl group, and eicosyl group. Among these, long-chain linear alkyl groups are preferred. The number of carbon atoms in the alkyl group is preferably 5 to 20, and more preferably 10 to 15.
[0033] R 32 In this context, the alicyclic group has a ring structure other than an aromatic ring and does not contain heteroatoms within the ring. It may be monocyclic or polycyclic, for example, an alicyclic group having 3 to 20 carbon atoms. As the alicyclic group, saturated alicyclic groups such as cycloalkyl groups are preferred, for example, cyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, bicyclo[2.2.1]heptyl group, cyclooctyl group, and adamantyl group. The alicyclic group may have some unsaturated bonds within the ring, such as a cyclohexenyl group.
[0034] R 32 The aryl group in this context has an aromatic ring that is not bonded to an aliphatic chain and does not contain heteroatoms within the ring. Examples include aryl groups with 6 to 18 carbon atoms. Examples of aryl groups with 6 to 18 carbon atoms include the phenyl group and the naphthyl group.32 Examples of heteroaryl groups in this context include pyridyl groups and carbazolyl groups. 32 Non-aromatic heterocyclic groups in this context have a ring structure other than an aromatic ring and contain heteroatoms within the ring. Examples include pyrrolidinyl groups, pyrrolidonyl groups, and tetrahydropyridyl groups. 32 The aralkyl group in this context has an aromatic ring to which an aliphatic chain is attached. Examples include the benzyl group and the phenylethyl group.
[0035] R 32 The alkyl groups, alicyclic groups, aryl groups, heteroaryl groups, non-aromatic heterocyclic groups, and aralkyl groups in the formula may be unsubstituted or each may have substituents. Examples of substituents include carboxyl groups, carboxylic acid ester groups, epoxy groups, hydroxyl groups, alkoxy groups, primary amino groups, secondary amino groups, tertiary amino groups, isocyanate groups, and sulfonic acid groups (-SO 3 Examples include H) and halogen atoms. Carboxylic acid ester groups include, for example, -COOR 36 It is represented by R 36 R represents an alkyl group, an alicyclic group, or an aryl group. 36 In these, alkyl groups, alicyclic groups, and aryl groups are, respectively, R 32 Examples of alkyl groups, alicyclic groups, and aryl groups in the above are similar to those found in the above, and these alkyl groups, alicyclic groups, and aryl groups include, for example, carboxyl groups, epoxy groups, hydroxyl groups, alkoxy groups, primary amino groups, secondary amino groups, tertiary amino groups, isocyanate groups, sulfonic acid groups (-SO 3 It may be substituted with one or more groups selected from the group consisting of H) and halogen atoms. The alkoxy group is, for example, -OR 37 It is represented by R 37 R indicates an alkyl group. 37 The alkyl group in R 32 Examples of alkyl groups include those similar to those in the above, and alkyl groups include, for example, carboxyl groups, epoxy groups, hydroxyl groups, alkoxy groups, primary amino groups, secondary amino groups, tertiary amino groups, isocyanate groups, sulfonic acid groups (-SO 3H), and a halogen atom, may be substituted with one or more groups selected from the group consisting of. Examples of the secondary amino group include -NR 38 R 39 It is represented by. R 38 represents a hydrogen atom, and R 39 represents an alkyl group, an alicyclic group or an aryl group. The alkyl group, alicyclic group and aryl group are each the same as the alkyl group, alicyclic group and aryl group in R 32 , and examples thereof include the same groups. These alkyl groups, alicyclic groups and aryl groups are, for example, a carboxyl group, an epoxy group, a hydroxy group, an alkoxy group, a primary amino group, a secondary amino group, a tertiary amino group, an isocyanato group, and a sulfonic acid group (-SO 3 H), and a halogen atom, may be substituted with one or more groups selected from the group consisting of. Examples of the tertiary amino group include the aforementioned -NR 38 R 39 of R 38 and R 39 are each an alkyl group, an alicyclic group or an aryl group. Examples of the alkyl group, aryl group and halogen atom include the same as those described above, and these alkyl groups, alicyclic groups and aryl groups are, for example, a carboxyl group, an epoxy group, a hydroxy group, an alkoxy group, a primary amino group, a secondary amino group, a tertiary amino group, an isocyanato group, and a sulfonic acid group (-SO 3 H), and a halogen atom, may be substituted with one or more groups selected from the group consisting of.
[0036] As monomer (b1), monomers represented by formula (b1) with a glass transition temperature (hereinafter also referred to as "Tg") of the homopolymer of 40°C or lower are used. The Tg of the homopolymer of monomer (b1) is preferably 10°C or lower, more preferably -10°C or lower, and even more preferably -25°C or lower. If the Tg of the homopolymer is below the above upper limit, the wear resistance of the coating film containing the copolymer of this embodiment will be good, and the long-term antifouling effect of the coating film will be excellent. In addition, the solution of the copolymer of this embodiment and the composition containing it (polymer composition, antifouling paint composition) tend to have a high solid content but low viscosity. The lower limit of the Tg of the homopolymer of monomer (b1) is not particularly limited, but may be, for example, -90°C or higher, or -80°C or higher. The above upper and lower limits can be combined as appropriate. For example, the ranges may be -90 to 40°C, -90 to 10°C, -90 to -10°C, -90 to -25°C, -80 to 40°C, -80 to 10°C, -80 to -10°C, or -80 to -25°C.
[0037] The molecular weight of monomer (b1) is 200 to 500, preferably 220 to 480, more preferably 230 to 470, and even more preferably 240 to 460. If the molecular weight of monomer (b1) is above the lower limit of the above range, the antifouling properties and contact angle of the coating film are excellent. If the molecular weight of monomer (b1) is below the upper limit of the above range, the storage stability of the copolymer solution of this embodiment, the copolymer composition containing it, and the antifouling coating composition are excellent.
[0038] The solubility parameter (hereinafter also referred to as the "SP value") of monomer (b1) is 9.5 (cal / cm³). 3 ) 1/2 The following is preferable: 9.2 (cal / cm³) 3 ) 1/2 The following is more preferable: 9.1 (cal / cm³) 3 ) 1/2 The following is even more preferable: If the SP value of monomer (b1) is less than or equal to the upper limit, the contact angle of the coating film increases, and the antifouling properties of the coating film are further improved. The lower limit of the SP value of monomer (b1) is not particularly limited, but for example, 8.2 (cal / cm²) 3 ) 1/2 The above is sufficient, and 8.5 (cal / cm³) 3 ) 1/2The above values may be used. The upper and lower limits can be combined as appropriate. For example, 8.2 to 9.5 (cal / cm³). 3 ) 1/2 , 8.2-9.2 (cal / cm 3 ) 1/2 , 8.2-9.1 (cal / cm 3 ) 1/2 , 8.5-9.5 (cal / cm 3 ) 1/2 , 8.5-9.2 (cal / cm 3 ) 1/2 Or 8.5 to 9.1 (cal / cm³) 3 ) 1/2 This is acceptable. The SP value is calculated using the Fedors method.
[0039] Examples of monomers (b1) include the following compounds. The Tg in parentheses after each compound name is the Tg of the homopolymer, and the unit of the SP value is (cal / cm²). 3 ) 1/2 These are lauryl methacrylate (LMA) (Tg: -65°C, molecular weight: 254, SP value: 9.02), tridecyl methacrylate (Tg: -40°C, molecular weight: 268, SP value: 8.99), and stearyl methacrylate (Tg: 38°C, molecular weight: 339, SP value: 8.90).
[0040] For reference, the Tg, molecular weight, and SP value of the homopolymers of some (meth)acrylic monomers other than monomer (b1) are shown below: 2-ethylhexyl methacrylate (EHMA) (Tg: -10°C, molecular weight: 198, SP value: 9.04), 2-ethylhexyl acrylate (EHA) (Tg: -50°C, molecular weight: 184, SP value: 9.22), i-butyl acrylate (i-BA) (Tg: -24°C, molecular weight: 128, SP value: 9.57), n-butyl acrylate (n-BA) (Tg: -54°C, molecular weight: 128, SP value: 9.77), 2-methoxyethyl methacrylate (MTMA) (Tg: -2°C, molecular weight: 144, SP value: 9.76), 2-methoxyethyl acrylate (MTA) ( Tg: -50°C, Molecular weight: 130, SP value: 10.16), Ethyl acrylate (EA) (Tg: -22°C, Molecular weight: 100, SP value: 10.20), Methyl acrylate (MA) (Tg: 9°C, Molecular weight: 86, SP value: 10.56), 4-Hydroxybutyl acrylate (HBA) (Tg: -32°C, Molecular weight: 144, SP value: 12.12), 2-Hydroxypropyl acrylate (HPA) (Tg: -33°C, Molecular weight: 130, SP value: 12.43), 2-Hydroxyethyl acrylate (HEA) (Tg: -20°C, Molecular weight: 116, SP value: 13.31).
[0041] For Tg values of monomer homopolymers other than those mentioned above, refer to "Polymer Handbook, Fourth Edition," John Wiley & Sons Inc., J. Brandrup, VI / p, 193-253. If Tg is not listed in the above literature, values measured by differential scanning calorimeter (DSC) may be used.
[0042] As for monomer (b1), in terms of copolymerizability, R 32 It is preferable that the alkyl group is an unsubstituted alkyl group. The unsubstituted alkyl group has 10 to 29 carbon atoms, and more preferably 12 to 25 carbon atoms.
[0043] Monomer (b1) may be used alone or in combination of two or more types. Monomer (b1) may be manufactured by known methods or be commercially available. In addition, the copolymer of this embodiment may contain constituent units derived from (meth)acrylic monomers other than monomer (b1) (for example, those with a molecular weight outside the range of 200 to 500 or those with a glass transition temperature greater than 40°C when used as a homopolymer).
[0044] [Constituent Unit (B2)] Constituent unit (B2) is a constituent unit derived from compound (b2). Compound (b2) is a compound having a radical polymerizable group and two or more constituent units represented by the following formula (Z1) (hereinafter also referred to as "constituent unit (Z1)"), and having a glass transition temperature (Tg) of 10°C or less. The two or more constituent units (Z1) of compound (b2) may be the same or different.
[0045]
[0046] (In the formula, R 41 is a hydrogen atom, a methyl group, or CH 2 Showing OH, R 42 is OR 43 , halogen atom, COR 44 COOR 45 , CN, CONR 46 R 47 or R 48 This indicates R 43 ~R 47 Each of these independently represents a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, an unsubstituted or substituted non-aromatic heterocyclic group, or an unsubstituted or substituted aralkyl group. 48 (This indicates an unsubstituted or substituted aryl group, or an unsubstituted or substituted heteroaryl group.)
[0047] The radical polymerizable group of compound (b2) is preferably a group having an ethylenically unsaturated bond. Examples of groups having an ethylenically unsaturated bond include CH2 =C(COOR)-CH 2 Examples include a (meth)acryloyl group, a 2-(hydroxymethyl)acryloyl group, and a vinyl group. Here, R represents a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, or an unsubstituted or substituted non-aromatic heterocyclic group.
[0048] In R, the alkyl group represents a linear alkyl group or a branched alkyl group. For example, a linear or branched alkyl group having 1 to 20 carbon atoms can be used. Examples of linear or branched alkyl groups having 1 to 20 carbon atoms include methyl group, ethyl group, n-propyl group, i-propyl group, n-butyl group, t-butyl group, i-butyl group, pentyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, octadecyl group, nonadecyl group, and eicosyl group. Among these, long-chain linear alkyl groups are preferred. The number of carbon atoms in the alkyl group is preferably 5 to 20, and more preferably 10 to 15.
[0049] The alicyclic group in R has a ring structure other than an aromatic ring and does not contain heteroatoms within the ring. It may be monocyclic or polycyclic, for example, an alicyclic group having 3 to 20 carbon atoms. As the alicyclic group, saturated alicyclic groups such as cycloalkyl groups are preferred, for example, cyclopropyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, cycloheptyl group, bicyclo[2.2.1]heptyl group, cyclooctyl group, and adamantyl group. The alicyclic group may have some unsaturated bonds within the ring, such as a cyclohexenyl group.
[0050] The aryl group in R has an aromatic ring that is not bonded to an aliphatic chain and does not contain heteroatoms within the ring. Examples include aryl groups having 6 to 18 carbon atoms. Examples of aryl groups having 6 to 18 carbon atoms include the phenyl group and the naphthyl group.
[0051] Examples of heteroaryl groups in R include pyridyl groups and carbazolyl groups. Non-aromatic heterocyclic groups in R have a ring structure other than an aromatic ring and contain heteroatoms within the ring. Examples of heterocyclic groups include heterocyclic groups having 5 to 18 carbon atoms. Examples of heterocyclic groups include oxygen-containing heterocyclic groups such as γ-butyrolactone and ε-caprolactone, nitrogen-containing heterocyclic groups such as pyrrolidinyl, pyrrolidonyl, and tetrahydropyridyl groups, and morpholino groups.
[0052] The alkyl group, alicyclic group, aryl group, heteroaryl group, and non-aromatic heterocyclic group in R may be unsubstituted or each may have substituents. Examples of substituents include alkyl groups (except when R is a substituted alkyl group), aryl groups, and -COOR groups. 51 , cyano group, -OR 52 , -NR 53 R 54 , -CONR 55 R 56 This includes at least one selected from the group consisting of halogen atoms, allyl groups, epoxy groups, siloxy groups, and hydrophilic or ionic groups. Here, R 51 ~R 56 Each of these independently represents a hydrogen atom, an alkyl group, an alicyclic group, or an aryl group.
[0053] The alkyl and aryl groups used as substituents are the same as those in R. 51 ~R 56 The alkyl groups, alicyclic groups, and aryl groups in R are the same as those in R, respectively. 51 For example, R 51 Preferably, it is a hydrogen atom or an alkyl group. That is, -COOR 51 Preferably, the substituent is a carboxyl group or an alkoxycarbonyl group. An example of an alkoxycarbonyl group is a methoxycarbonyl group. The substituent is -OR 52 For example, R52 Preferably, the element is a hydrogen atom or an unsubstituted alkyl group. That is, -OR 52 A hydroxyl group or an alkoxy group is preferred. Examples of alkoxy groups include alkoxy groups having 1 to 12 carbon atoms, such as a methoxy group. The -NR in the substituent 53 R 54 Examples include amino groups, monomethylamino groups, and dimethylamino groups. The -CONR in the substituents 55 R 56 For example, a carbamoyl group (-CONH 2 ), N-methylcarbamoyl group (-CONHCH 3 ), N,N-dimethylcarbamoyl group (dimethylamide group: -CON(CH 3 ) 2 Examples of substituents include fluorine, chlorine, bromine, and iodine atoms. Examples of groups exhibiting hydrophilicity or ionicity in the substituent include alkali salts of carboxyl groups and sulfoxy groups; poly(alkylene oxide) groups such as polyethylene oxide groups and polypropylene oxide groups; and cationic substituents such as quaternary ammonium bases.
[0054] For R, alkyl groups or alicyclic groups are preferred, alkyl groups or saturated alicyclic groups are more preferred, and alkyl groups or saturated alicyclic groups that are unsubstituted or have alkyl groups as substituents are even more preferred. Due to their availability, R is preferably methyl, ethyl, n-propyl, i-propyl, n-butyl, t-butyl, pentyl, hexyl, heptyl, octyl, cyclopropyl, cyclobutyl, isobornyl, or adamantyl, and more preferably methyl, ethyl, n-propyl, i-propyl, n-butyl, t-butyl, cyclopropyl, cyclobutyl, isobornyl, or adamantyl.
[0055] Compound (b2) has two or more constituent units (Z1). In the above formula (Z1), R 42 R in equation (b1) 32Similar examples include R. 48 The aryl group and heteroaryl group in formula (b1) are R 32 Examples include aryl groups and heteroaryl groups similar to those in R. 48 The aryl group and heteroaryl group in each may be unsubstituted or each may have substituents. Examples of substituents include carboxyl group, carboxylic acid ester group, epoxy group, hydroxyl group, alkoxy group, primary amino group, secondary amino group, tertiary amino group, isocyanate group, sulfonic acid group (-SO 3 Examples include H), halogen atoms, alkyl groups, and aryl groups. Of these, carboxylic acid ester groups, alkoxy groups, primary amino groups, secondary amino groups, tertiary amino groups, and halogen atoms are each R 32 Examples of substituents similar to those listed in the above include alkyl groups and aryl groups, respectively. 32 Examples include alkyl groups and aryl groups similar to those found in [the text].
[0056] The constituent unit (Z1) is CH 2 =CR 41 R 42These can be considered constituent units derived from monomers represented by (hereinafter also referred to as "monomer (z1)"). Examples of monomers (z1) include the following: Substituted or unsubstituted alkyl (meth)acrylates [e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate]. [T, nonyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, hexadecyl (meth)acrylate, behenyl (meth)acrylate, docosyl (meth)acrylate, 1-methyl-2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 3-methyl-3-methoxybutyl (meth)acrylate]; Substituted or unsubstituted aralkyl (meth)acrylates [e.g., benzyl (meth)acrylate, o-methoxyphenylethyl (meth)acrylate, m-methoxyphenylethyl (meth)acrylate, p-methoxyphenylethyl (meth)acrylate]; Substituted or unsubstituted aryl (meth)acrylates [e.g., phenyl (meth)acrylate, m-methoxyphenyl (meth)acrylate, p-methoxyphenyl (meth)acrylate, 4-(meth)acryloyloxybenzophenone]; Alicyclic (meth)acrylates [e.g., isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, 3,5,5-trimethylcyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate]; Heterocyclic group (meth)acrylates [e.g., tetrahydrofurfuryl (meth)acrylate, (meth)acryloylmorpholine]; halogen atom-containing (meth)acrylates [e.g., trifluoroethyl (meth)acrylate, perfluorooctyl (meth)acrylate,Perfluorocyclohexyl (meth)acrylate; hydrophobic group-containing (meth)acrylic acid ester monomers such as terpene (meth)acrylate and its derivatives, hydrogenated rosin (meth)acrylate and its derivatives; Methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, n-butoxyethyl (meth)acrylate, i-butoxyethyl (meth)acrylate, t-butoxyethyl (meth)acrylate, butoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, nonylphenoxyethyl (meth)acrylate, 2-(2-ethylhexaoxy)ethyl (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, acetoxyethyl (meth)acrylate, "Praxel FM" (caprolactone addition monomer manufactured by Daicel Chemicals, Ltd., trade name), "Bremmer PME-100" (methoxypolyethylene glycol methacrylate (ethylene glycol chain of 2) manufactured by NOF Corporation, trade name), "Bremmer PME-200" (methoxypolyethylene glycol manufactured by NOF Corporation) Methacrylate (ethylene glycol with 4 chains), trade name), "Bremmer PME-400" (Methoxy polyethylene glycol methacrylate (ethylene glycol with 9 chains), trade name, manufactured by NOF Corporation), "Bremmer 50POEP-800B" (Octoxy polyethylene glycol-polypropylene glycol-methacrylate (ethylene glycol with 8 chains and propylene glycol with 6 chains), trade name, manufactured by NOF Corporation), and "Bremmer 20ANEP- 600" (Nonylphenoxy(ethylene glycol-polypropylene glycol) monoacrylate, manufactured by NOF Corporation, product name), "Bremmer AME-100" (manufactured by NOF Corporation, product name), "Bremmer AME-200" (manufactured by NOF Corporation, product name), "Bremmer 50AOEP-800B" (manufactured by NOF Corporation, product name), Cyraplane FM-0711 (manufactured by JNC Corporation, product name), Cyraplane FM-0721 (manufactured by JNC Corporation, product name), Cyraplane FM-0725 (manufactured by JNC Corporation, product name),Oxyalkylene group-containing (meth)acrylic acid ester monomers such as Cyraprene™-0701 (manufactured by JNC Corporation, product name), Cyraprene™-0701T (manufactured by JNC Corporation, product name), X-22-174DX (manufactured by Shin-Etsu Chemical Co., Ltd., product name), X-22-2426 (manufactured by Shin-Etsu Chemical Co., Ltd., product name), X-22-2475 (manufactured by Shin-Etsu Chemical Co., Ltd., product name); Hydroxy group-containing (meth)acrylic acid ester monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol (meth)acrylate; Terminal alkoxyallylated polyether monomers such as methoxypolyethylene glycol allyl ether, methoxypolypropylene glycol allyl ether, butoxypolyethylene glycol allyl ether, butoxypolypropylene glycol allyl ether, methoxypolyethylene glycol-polypropylene glycol allyl ether, and butoxypolyethylene glycol-polypropylene glycol allyl ether; epoxy group-containing vinyl monomers such as glycidyl (meth)acrylate, glycidyl α-ethylacrylate, and 3,4-epoxybutyl (meth)acrylate; primary or secondary amino group-containing vinyl monomers such as butylaminoethyl (meth)acrylate, (meth)acrylamide, N-t-butyl (meth)acrylamide, N-methylol (meth)acrylamide, N-isopropylacrylamide, hydroxyethylacrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, and diacetone acrylamide; Tertiary amino group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, dimethylaminobutyl (meth)acrylate, dibutylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylamide, and dimethylaminopropyl (meth)acrylamide; heterocyclic basic monomers such as vinylpyrrolidone, vinylpyridine, and vinylcarbazole; trimethylsilyl (meth)acrylate,Triethylsilyl (meth)acrylate, tri-n-propylsilyl (meth)acrylate, tri-n-butylsilyl (meth)acrylate, tri-n-amylsilyl (meth)acrylate, tri-n-hexylsilyl (meth)acrylate, tri-n-octylsilyl (meth)acrylate, tri-n-dodecylsilyl (meth)acrylate, triphenylsilyl (meth)acrylate, tri-p-methylphenylsilyl (meth)acrylate, tribenzylsilyl (meth)acrylate, triisopropylsilyl (meth)acrylate, triisobutylsilyl (meth)acrylate, tri-s-butylsilyl Organosilyl group-containing vinyl monomers such as (meth)acrylate, tri-2-methylisopropylsilyl (meth)acrylate, tri-t-butylsilyl (meth)acrylate, ethyldimethylsilyl (meth)acrylate, n-butyldimethylsilyl (meth)acrylate, diisopropyl-n-butylsilyl (meth)acrylate, n-octyldi-n-butylsilyl (meth)acrylate, diisopropylstearylsilyl (meth)acrylate, dicyclohexylphenylsilyl (meth)acrylate, t-butyldiphenylsilyl (meth)acrylate, lauryldiphenylsilyl (meth)acrylate, etc. Carboxy group-containing ethylenically unsaturated monomers such as (meth)acrylic acid, vinyl benzoic acid, monohydroxyethyl (meth)acrylate tetrahydrophthalate, monohydroxypropyl (meth)acrylate tetrahydrophthalate, monohydroxybutyl (meth)acrylate tetrahydrophthalate, monohydroxyethyl (meth)acrylate phthalate, monohydroxypropyl (meth)acrylate phthalate, monohydroxyethyl (meth)acrylate succinate, monohydroxypropyl (meth)acrylate succinate, monohydroxyethyl (meth)acrylate maleate, monohydroxypropyl (meth)acrylate maleate; cyano group-containing vinyl monomers such as acrylonitrile, methacrylonitrile, and 2-isocyanatoethyl (meth)acrylate; alkyl vinyl ethers [e.g., ethyl vinyl ether, propyl vinyl ether, butyl vinyl ether, hexyl vinyl ether, 2-ethylhexyl vinyl ether, etc.]Vinyl ether monomers such as cycloalkyl vinyl ethers [e.g., cyclohexyl vinyl ether, etc.]; vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl benzoate, etc.; aromatic vinyl monomers such as styrene, vinyltoluene, α-methylstyrene, etc.; halogenated olefins such as vinyl chloride, vinyl fluoride, etc.; 2-isocyanatoethyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3,3-pentafluorophenyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, 3-(perfluorobutyl)-2-hydroxypropyl (meth)acrylate, 2-(perfluorohexyl)ethyl (meth)acrylate, 3-perfluorohexyl-2-hydroxypropyl (meth)acrylate, 3-(perfluoro-3-methylbutyl)-2-hydroxypropyl (meth) Fluorine-containing monomers such as acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, 1H,1H,2H,2H-tridecafluorooctyl (meth)acrylate, 1H-1-(trifluoromethyl)trifluoroethyl (meth)acrylate, 1H,1H,3H-hexafluorobutyl (meth)acrylate, and 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl (meth)acrylate (excluding halogenated olefins); and monomers having an acetal structure such as 1-butoxyethyl (meth)acrylate, 1-(2-ethylhexyloxy)ethyl (meth)acrylate, 1-(cyclohexyloxy)ethyl methacrylate, and 2-tetrahydropyranyl (meth)acrylate. These monomers may be used individually or in combination of two or more.
[0057] Preferably, at least a portion of the two or more constituent units (Z1) of compound (b2) are constituent units derived from (meth)acrylic monomers, and R in formula (Z1) 41 is a hydrogen atom or a methyl group, R 42 COOR 45 It is more preferable that the constituent unit is R. 45The preferred elements are hydrogen atoms, alkyl groups, saturated alicyclic groups, aryl groups, heteroaryl groups, or non-aromatic heterocyclic groups.
[0058] From the viewpoint of setting the Tg of compound (b2) to 10°C or lower, it is preferable that at least a portion of the two or more constituent units (Z1) of compound (b2) are constituent units derived from monomer (b1). The ratio of constituent units derived from monomer (b1) to the total constituent units in compound (b2) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 40% by mass or more, and may be 100% by mass.
[0059] Compound (b2) may further have structural units other than structural unit (Z1). Examples of structural units other than structural unit (Z1) include structural units derived from monomers other than the aforementioned monomer (z1) (hereinafter also referred to as "monomer (z2)"). Monomer (z2) typically has a radical polymerizable group. As for the radical polymerizable group of the other monomer, a group having an ethylenically unsaturated bond is preferred, similar to the radical polymerizable group of compound (b2). Various types can be used as monomer (z2), but examples include the following. Carboxyl group-containing vinyl monomers such as 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxypropylhexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxypropyl succinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, citraconic acid, monomethyl maleic acid, monoethyl maleic acid, monooctyl maleic acid, monomethyl itaconic acid, monoethyl itaconic acid, monobutyl itaconic acid, monooctyl itaconic acid, monomethyl fumarate, monoethyl fumarate, monobutyl fumarate, monooctyl fumarate, monoethyl citraconic acid, etc. Vinyl monomers containing acid anhydride groups such as maleic anhydride and itaconic anhydride; unsaturated dicarboxylic acid diester monomers such as dimethyl maleate, dibutyl maleate, dimethyl fumarate, dibutyl fumarate, dibutyl itaconate, and diperfluorocyclohexyl fumarate; vinyl monomers containing amide groups such as maleic acid amide and maleimide;Divinylbenzene, ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, neopentyl glycol Polyfunctional vinyl monomers such as di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl(meth)acrylate, triallyl cyanurate, diallyl maleate, polypropylene glycol diallyl ether, and N,N'-methylenebis(meth)acrylamide; Monomers containing silane coupling agents such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane; halogenated olefins such as vinylidene chloride, vinylidene fluoride, and chlorotrifluoroethylene (however, CH; 2 =CR 41 R 42 (Excluding those that fall under the above categories.) These monomers may be used individually or in combination of two or more types.
[0060] Preferred specific examples of monomers (z2) include the following: organosilyl group-containing vinyl monomers such as triisopropylsilylmethyl malate, triisopropylsilylamyl malate, tri-n-butylsilyl-n-butyl malate, t-butyldiphenylsilylmethyl malate, t-butyldiphenylsilyl-n-butyl malate, triisopropylsilylmethyl fumarate, triisopropylsilylamyl fumarate, tri-n-butylsilyl-n-butyl fumarate, t-butyldiphenylsilylmethyl fumarate, and t-butyldiphenylsilyl-n-butyl fumarate; acid anhydride group-containing vinyl monomers such as maleic anhydride and itaconic anhydride; Carboxylated ethylenically unsaturated monomers containing carboxyl groups such as crotonic acid, fumaric acid, itaconic acid, maleic acid, citraconic acid, monomethyl maleate, monoethyl maleate, monobutyl maleate, monooctyl maleate, monomethyl itaconic acid, monoethyl itaconic acid, monobutyl itaconic acid, monooctyl itaconic acid, monomethyl fumarate, monoethyl fumarate, monobutyl fumarate, monooctyl fumarate, and monoethyl citraconic acid; unsaturated dicarboxylic acid diester monomers such as dimethyl maleate, dibutyl maleate, dimethyl fumarate, dibutyl fumarate, dibutyl itaconate, and diperfluorocyclohexyl fumarate; halogenated olefins such as vinylidene chloride, vinylidene fluoride, and chlorotrifluoroethylene; Polyfunctional monomers such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl methacrylate, triallyl cyanurate, diallyl maleate, and polypropylene glycol diallyl ether.
[0061] The Tg of the monomer (z2) homopolymer is typically above 10°C. Preferably, the Tg of the monomer (z2) homopolymer is 110°C or lower, and more preferably 50°C or lower. If the Tg of the monomer (z2) homopolymer is below the above upper limit, it is easier to set the Tg of the (meth)acrylic compound (b2) to 10°C or lower.
[0062] As for compound (b2), a compound having a radical polymerizable group introduced at the end of a main chain containing two or more structural units (Z1) is preferred, and the compound (b2-1) represented by the following formula (b2-1) is more preferred.
[0063]
[0064] (In the formula, R has the same meaning as above, Q represents a main chain portion containing two or more constituent units (Z1), and E represents a terminal group.)
[0065] In equation (b2-1), R is the CH mentioned above. 2 =C(COOR)-CH 2 The same applies to R in -, and the preferred embodiment is also the same. The two or more constituent units (Z1) contained in Q may be the same or different. Q may consist only of constituent units (Z1), or it may further contain other constituent units other than constituent units (Z1) (for example, constituent units derived from monomers (z2)). The number of constituent units constituting Q is preferably such that the number-average molecular weight of the compound (b2) is within the preferred range described later. Examples of E include hydrogen atoms, groups derived from radical polymerization initiators, groups derived from chain transfer agents, and radical polymerizable groups, similar to the terminal groups of polymers obtained by known radical polymerization.
[0066] As compound (b2), compound (b2-2) represented by the following formula (b2-2) is particularly preferred.
[0067]
[0068] (In the formula, R, R 41 , R 45 (And E are equivalent to those described above, and n represents a natural number greater than or equal to 2.)
[0069] n is a natural number greater than or equal to 2. Preferably, n is a value such that the number-average molecular weight (Mn) of compound (b2) falls within the preferred range described later. n R 41 These can be the same or different. n R 45 These can be the same or different.
[0070] The Tg of compound (b2) is 10°C or lower, preferably 0°C or lower, and more preferably -10°C or lower. If the Tg is below the upper limit, the wear resistance of the coating film containing the copolymer of this embodiment will be good, and the coating film will have excellent long-term antifouling effect. In addition, the solution of the copolymer of this embodiment and the composition containing it (polymer composition, antifouling paint composition) tend to have low viscosity even with a high solid content. The lower limit of the Tg of compound (b2) is not particularly limited, but may be -90°C or higher, or -70°C or higher. The upper and lower limits can be combined as appropriate. For example, it may be -90 to 10°C, -90 to 0°C, -90 to -10°C, -70 to 10°C, -70 to 0°C, or -70 to -10°C. The Tg of compound (b2) is the value obtained by converting the absolute temperature (K) calculated from the following formula (1) to Celsius (°C). 1 / Tg = Σ(w i / Tg i )...(1) In formula (1), w i This indicates the mass fraction of monomer i constituting compound (b2), and Tg i Tg indicates the Tg of the homopolymer of monomer i constituting compound (b2). Tg and Tg in formula (1) i This value is expressed in absolute temperature (K). Tg i The Tg is the value listed in "Polymer Handbook, Fourth Edition," John Wiley & Sons Inc., J. Brandrup, VI / p, 193-253. If Tg is not listed in the above literature, the value measured by differential scanning calorimeter (DSC) can be used. The Tg of compound (b2) can be adjusted, for example, by the composition of the monomers constituting compound (b2).
[0071] The number-average molecular weight (hereinafter also referred to as "Mn") of compound (b2) is preferably 800 to 10000, more preferably 1200 or more and less than 8000, and even more preferably 1400 to 5000. If the Mn of compound (b2) is above the lower limit of the above range, the antifouling properties and contact angle of the coating film are better. If the Mn of compound (b2) is below the upper limit of the above range, the storage stability of the copolymer solution of this embodiment, the copolymer composition containing it, and the antifouling coating composition are better. The Mn of compound (b2) is measured using polystyrene as a reference substance by gel filtration chromatography (GPC). The Mn of compound (b2) can be adjusted, for example, by the type and amount of polymerization initiator and chain transfer agent used and the polymerization temperature during the production of compound (b2).
[0072] The SP value of compound (b2) is 9.5 (cal / cm³). 3 ) 1/2 The following is preferable: 9.2 (cal / cm³) 3 ) 1/2 The following is more preferable: 9.1 (cal / cm³) 3 ) 1/2 The following is even more preferable: If the SP value of compound (b2) is less than or equal to the upper limit, the contact angle of the coating film increases, and the antifouling properties of the coating film are further improved. The lower limit of the SP value of compound (b2) is not particularly limited, but for example, 8.2 (cal / cm²) 3 ) 1/2 The above is sufficient, and 8.5 (cal / cm³) 3 ) 1/2 The above values may be used. The upper and lower limits can be combined as appropriate. For example, 8.2 to 9.5 (cal / cm³). 3 ) 1/2 , 8.2-9.2 (cal / cm 3 ) 1/2 , 8.2-9.1 (cal / cm 3 ) 1/2 , 8.5-9.5 (cal / cm 3 ) 1/2 , 8.5-9.2 (cal / cm 3 ) 1/2 Or 8.5 to 9.1 (cal / cm³) 3 ) 1/2This may be the case. The SP value of compound (b2) is the SP value of the monomers that make up compound (b2). If compound (b2) is composed of two or more monomers, the SP value of compound (b2) is the average value calculated from the SP value and ratio (molar ratio) of each monomer that makes up compound (b2).
[0073] Compound (b2) may be prepared by known methods or be commercially available. Examples of methods for preparing compound (b2) include using a cobalt chain transfer agent, using an α-substituted unsaturated compound such as α-methylstyrene dimer as a chain transfer agent, chemically bonding radical polymerizable groups to a polymer, and thermal decomposition. The method of preparing compound (b2) using a cobalt chain transfer agent is preferred because it involves fewer manufacturing steps and allows the use of a catalyst with a high chain transfer constant. Compound (b2) prepared using a cobalt chain transfer agent has the structure represented by formula (b2-1).
[0074] Methods for producing compound (b2) using a cobalt chain transfer agent include, for example, bulk polymerization; solution polymerization; and aqueous dispersion polymerization methods such as suspension polymerization and emulsion polymerization. Aqueous dispersion polymerization is preferred because the recovery process is simple. Methods for chemically bonding radical polymerizable groups to a polymer include, for example, a method of producing a polymer by substituting the halogen group of a polymer having a halogen group with a compound having a radical polymerizable carbon-carbon double bond; a method of reacting a vinyl monomer having an acid group with a vinyl polymer having an epoxy group; a method of reacting a vinyl polymer having an epoxy group with a vinyl monomer having an acid group; and a method of reacting a vinyl polymer having a hydroxyl group with a diisocyanate compound to obtain a vinyl polymer having an isocyanate group, and then reacting this vinyl polymer with a vinyl monomer having a hydroxyl group.
[0075] <Constituent Unit (C)> Constituent unit (C) is not particularly limited and includes, for example, constituent units derived from monomers other than monomer (a) and monomer (b1) (hereinafter also referred to as "monomer (c)"). Monomer (c) is not particularly limited as long as it is copolymerizable with monomer (a) or monomer (b1), and various monomers having radical polymerizable groups such as ethylenically unsaturated bonds can be used. For example, monomer (z1) and monomer (z2) for obtaining monomer (b1) can be used (except monomer (a) and monomer (b1)). Monomer (c) can be selected and used as needed, one or more types.
[0076] The monomer (c) is preferably a monofunctional monomer having one ethylenically unsaturated bond, as this makes it easier to achieve low viscosity even with a high solid content when the copolymer of this embodiment is dissolved in an organic solvent. It is particularly preferable that the ethylenically unsaturated bond originates from an acryloyl group. In other words, monomer (c) is particularly preferably a monofunctional monomer having one acryloyl group.
[0077] In terms of the water resistance of the coating film, it is preferable that the constituent unit (C) includes constituent units derived from hydrophobic group-containing (meth)acrylic acid ester monomers (excluding monomer (b1)).
[0078] The constituent unit (C) preferably contains constituent units derived from an oxyethylene group-containing (meth)acrylic acid ester monomer, in terms of the solubility and crack resistance of the formed coating film. The oxyethylene group-containing (meth)acrylic acid ester monomer is preferably the monomer represented by the following formula (c-1) (excluding monomer (b1)). Z 1 - (CH 2 CH 2 O) p R 57 (c-1) (wherein, Z 1 R indicates a (meth)acryloyloxy group, 57 (where p represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group, and p represents an integer from 1 to 15.)
[0079] In formula (c-1), Z 1When comparing the case of an acryloyloxy group with that of a methacryloyloxy group, the acryloyloxy group tends to have a higher hydrolysis rate, and can be arbitrarily selected according to the dissolution rate. 57 The alkyl and aryl groups having 1 to 10 carbon atoms in the R group are respectively 32 Similar to those listed above, the following can be cited. From the viewpoint of water resistance and crack resistance, p is preferably an integer from 1 to 10, more preferably an integer from 1 to 5, even more preferably an integer from 1 to 3, and particularly preferably 1 or 2.
[0080] The constituent unit (C) preferably does not have a carboxyl group, from the viewpoint of the water resistance and wearability of the formed coating film.
[0081] <Content of constituent units> The content of constituent unit (A) is preferably 1 to 40% by mass, and more preferably 5 to 30% by mass, relative to the total constituent units (100% by mass) of the copolymer. If the content of constituent unit (A) is above the lower limit of the above range, the long-term self-polishing properties of the coating film containing the copolymer of this embodiment are better. If the content of constituent unit (A) is below the upper limit of the above range, the storage stability of the antifouling coating composition, the adhesion of the formed coating film, the water resistance in seawater, and the balance between hardness and crack resistance tend to improve.
[0082] The content of constituent unit (B) is preferably 1 to 60% by mass, more preferably 2 to 40% by mass, and even more preferably 4 to 30% by mass, relative to the total constituent units (100% by mass) of the copolymer. If the content of constituent unit (B) is above the lower limit of the above range, the contact angle and antifouling properties of the formed coating film are better. If the content of constituent unit (B) is below the upper limit of the above range, the viscosity of the solution when the copolymer of this embodiment is dissolved in an organic solvent and the storage stability of the polymer composition and antifouling coating composition containing this solution are good.
[0083] The content of constituent unit (C) is preferably 0 to 98% by mass, more preferably 5 to 88% by mass, and even more preferably 10 to 75% by mass, relative to the total constituent units (100% by mass) of the copolymer.
[0084] If the constituent unit (C) has constituent units derived from an oxyethylene group-containing (meth)acrylic acid ester monomer, the content of these constituent units is preferably 1 to 80% by mass, more preferably 5 to 60% by mass, and even more preferably 20 to 50% by mass, relative to the total constituent units of the copolymer. If the content of these constituent units is above the lower limit of the above range, the hydrophilicity of the formed coating film will be higher and the self-polishing properties will be better. If the content of these constituent units is below the upper limit of the above range, the formed coating film will have appropriate hydrolytic properties, the self-polishing properties will be maintained over a long period of time, and the antifouling effect will be better.
[0085] The total amount of constituent units (A), (B), and (C) is 100% by mass. The content (by mass) of each constituent unit in the copolymer can be measured by known methods such as gas chromatography, high-performance liquid chromatography, and nuclear magnetic resonance spectroscopy.
[0086] <Characteristics of the Copolymer> [Molecular Weight] The weight-average molecular weight (hereinafter also referred to as "Mw") of the copolymer in this embodiment is preferably 1,000 to 4,500, and more preferably 2,000 to 4,000. If the weight-average molecular weight of the copolymer is below the upper limit, a copolymer solution with a high solid content and low viscosity can be easily obtained. Therefore, copolymer solutions and antifouling paint compositions with a high paint solid content and a low amount of VOCs, which are required to be reduced due to their impact on the environment, can be easily obtained. Furthermore, if the weight-average molecular weight of the copolymer is below the upper limit, the antifouling properties of the formed coating film are excellent. On the other hand, if the weight-average molecular weight of the copolymer is above the lower limit, the hardness and durability of the formed coating film are even better.
[0087] The number-average molecular weight (Mn) of the copolymer in this embodiment is preferably 500 to 3000, and more preferably 750 to 2000. The polydispersity (Mw / Mn) of the copolymer in this embodiment is preferably 1.5 to 5.0, and more preferably 2.2 to 3.0.
[0088] [Acid Value] The acid value of the copolymer in this embodiment is preferably 40 mg KOH / g or higher, more preferably 50 mg KOH / g or higher, preferably 200 mg KOH / g or lower, and more preferably 150 mg KOH / g or lower. The above upper and lower limits can be combined arbitrarily. For example, it may be 40 to 200 mg KOH / g, or 50 to 150 mg KOH / g. If the acid value of the copolymer is above the lower limit, an optimal wear rate tends to be obtained, and if it is below the upper limit, water resistance tends to be good.
[0089] [Viscosity (Gardner viscosity)] The Gardner viscosity at 25°C of a copolymer solution with a solid content of 55% by mass, using the copolymer of this embodiment as the solid component, is preferably Z3 or less, more preferably Z1 or less, and even more preferably X or less. If the Gardner viscosity is below the upper limit, the amount of diluting solvent required when preparing the paint is reduced, and it is easier to obtain an antifouling paint composition with a low VOC content. The lower limit of the Gardner viscosity is not particularly limited, but D or higher is preferable in terms of suppressing paint dripping during painting.
[0090] [Contact Angle] The contact angle of water measured on a coating film obtained by applying a copolymer solution containing the copolymer of this embodiment as the solid component onto a glass substrate and drying it is preferably 80° or higher, more preferably 85° or higher, even more preferably 88° or higher, and preferably 110° or lower, and more preferably 105° or lower. The above upper and lower limits can be arbitrarily combined. For example, it may be 80 to 110°, 85 to 110°, or 88 to 105°. If the contact angle is above the lower limit, it has excellent antifouling properties, and if it is below the upper limit, it has an appropriate degree of wear for exhibiting a long-term antifouling effect. The contact angle is measured at a temperature of 25°C, with 1 μL of pure water, and a waiting time of 1 second from application to measurement.
[0091] <Method for Producing Copolymers> The copolymer of this embodiment can be produced by known methods. Examples of methods for producing copolymers include the following methods 1 and 2. In particular, it is preferable to produce the copolymer by method 1, as the antifouling coating composition containing the obtained (meth)acrylic copolymer has excellent storage stability and the antifouling coating film can maintain stable self-polishing properties over a long period of time.
[0092] Method 1: A method for polymerizing a monomer mixture comprising monomer (a) and at least one selected from the group consisting of monomer (b1) and compound (b2). Method 2: A method for introducing a metal atom M into a precursor polymer obtained by polymerizing a monomer mixture comprising a precursor monomer (a') having a carboxyl group and at least one selected from the group consisting of monomer (b1) and compound (b2). In Method 2, as a method for introducing the metal atom M, for example, a method of reacting the carboxyl group of the precursor polymer with a metal oxide such as zinc oxide can be used.
[0093] In Methods 1 and 2, known polymerization methods such as solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization can be applied as the polymerization method for the monomer mixture. Solution polymerization may be preferred in terms of productivity and coating performance.
[0094] The solvent used in the production of the copolymer is not particularly limited as long as it can dissolve the copolymer. Examples include monohydric alcohols such as methanol, ethanol, isopropanol, n-butanol, and propylene glycol monomethyl ether; polyhydric alcohols such as ethylene glycol and 1,2-propylene glycol; ketones such as acetone, methyl ethyl ketone, and acetylacetone; ethers such as methyl ethyl ether and dioxane; glycol ethers such as ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, ethylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, and dipropylene glycol monopropyl ether; glycol acetates such as ethylene glycol monoacetate, ethylene glycol diacetate, and ethylene glycol monomethyl ether acetate; aliphatic hydrocarbons such as n-pentane and n-hexane; and aromatic hydrocarbons such as toluene, xylene, and solvent naphtha. Any one of these can be used alone or in combination of two or more. The solvent used in the production of the copolymer preferably contains alcohols, as this ensures good stability during the copolymer production process.
[0095] In Methods 1 and 2, the polymerization reaction of the monomer mixture may be carried out using known polymerization initiators and in known methods. For example, the monomer mixture may be reacted in a solvent in the presence of a radical polymerization initiator at a reaction temperature of 60 to 180°C for 2 to 14 hours. In this case, a chain transfer agent may be used as needed.
[0096] Known radical polymerization initiators can be used. Examples include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile); and organic peroxides such as lauryl peroxide, benzoyl peroxide, cumene hydroperoxide, lauryl peroxide, di-t-butyl peroxide, t-butyl peroxy-2-ethylhexanoate, and t-butyl peroctoate. The content of the polymerization initiator is not particularly limited and can be set as appropriate.
[0097] Known chain transfer agents can be used. Examples include mercaptans such as n-dodecyl mercaptan; cobalt chain transfer agents; thioglycolic acid esters such as octyl thioglycolate; α-methylstyrene dimers; and terpinolenes. The content of the chain transfer agent is not particularly limited and can be set as appropriate.
[0098] [Copolymer Composition] The copolymer composition of this embodiment includes the (meth)acrylic copolymer of this embodiment.
[0099] The copolymer composition may further contain a solvent. Examples of solvents include those used in the production of the copolymer described above.
[0100] The copolymer composition may be a product obtained in method 1 or 2. For example, polymerizing the monomer mixture in a solvent yields a liquid copolymer composition containing the copolymer and the solvent.
[0101] The solid content relative to the total mass of the copolymer composition can be set to a range that avoids these problems. If it is too low, the viscosity becomes too high, the solution after polymerization loses its fluidity and becomes difficult to extract. If it is too high, it becomes difficult to reduce the VOC content of the paint when it is made into a paint. The solid content relative to the total mass of the copolymer composition is preferably 47 to 70% by mass, and more preferably 50 to 60% by mass.
[0102] [Anti-fouling paint composition] The anti-fouling paint composition of this embodiment includes the copolymer composition of this embodiment. The anti-fouling paint composition of this embodiment may further include, if necessary, at least one selected from the group consisting of an anti-fouling agent, another thermoplastic resin other than the copolymer of this embodiment, a solvent, and other optional components.
[0103] <Anti-fouling agent> The anti-fouling paint composition preferably further contains an anti-fouling agent. Examples of anti-fouling agents include inorganic anti-fouling agents and organic anti-fouling agents. Examples include copper-based anti-fouling agents such as cuprous oxide, copper thiocyanate, and copper powder; compounds of other metals (lead, zinc, nickel, etc.); amine derivatives such as diphenylamine; nitrile compounds; benzothiazole compounds; maleimide compounds; and pyridine compounds such as zinc pyrithione and copper pyrithione. One or more types of anti-fouling agents can be appropriately selected and used depending on the required performance.
[0104] More specifically as antifouling agents, for example, 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile, manganese ethylene bisdithiocarbamate, zinc dimethyldithiocarbamate, 2-methylthio-4-t-butylamino-6-cyclopropylamino-s-triazine, 2,4,5,6-tetrachloroisophthalonitrile, N,N-dimethyldichlorophenylurea, zinc ethylene bisdithiocarbamate, rhodane copper, 4,5-dichloro-2-n-octyl-3(2H)-isothiazolone, N-(fluorodichloromethylthio)phthalimide, N,N'-dimethyl-N'-phenyl-(N-fluorodichloro Examples include methylthio)sulfamide, 2-pyridinethiol-1-oxide zinc salt (pyrithione zinc), 2-pyridinethiol-1-oxide copper salt (pyrithione copper), tetramethylthiuram disulfide, Cu-10%Ni solid solution alloy, 2,4,6-trichlorophenylmaleimide, 2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine, 3-iodo-2-propynylbutylcarbamate, diiodomethyl p-trisulfone, bisdimethyldithiocarbamoylzinc ethylenebisdithiocarbamate, phenyl(bispyridyl)bismuth dichloride, 2-(4-thiazolyl)-benzimidazole, medetomidine, and pyridine-triphenylborane.
[0105] The antifouling agent preferably contains at least one selected from the group consisting of cuprous oxide, 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitride, pyridine-triphenylborane, zinc pyrithione, copper pyrithione, and medetomidine, in terms of good antifouling performance. Among these, it is preferable to include at least one selected from the group consisting of 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitride and medetomidine, in terms of the antifouling properties of the coating film. At least two selected from the group consisting of cuprous oxide, 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitride, zinc pyrithione, copper pyrithione, and medetomidine may be combined.
[0106] <Other Thermoplastic Resins Besides the Copolymer of This Embodiment> If the antifouling coating composition contains other thermoplastic resins in addition to the copolymer of this embodiment, the coating film properties such as crack resistance and water resistance will be improved. Examples of other thermoplastic resins include thermoplastic resins that do not have constituent unit (A). Specific examples of other thermoplastic resins include the following: Chlorinated paraffin; chlorinated polyolefins such as chlorinated rubber, chlorinated polyethylene, and chlorinated polypropylene; polyvinyl ether; polypropylene sebacate; partially hydrogenated terphenyl; polyvinyl acetate; alkyl poly(meth)acrylates such as methyl (meth)acrylate copolymers, ethyl (meth)acrylate copolymers, propyl (meth)acrylate copolymers, butyl (meth)acrylate copolymers, and cyclohexyl (meth)acrylate copolymers; polyether polyols; alkyd resins; polyester resins; vinyl chloride resins such as vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinyl propionate copolymers, vinyl chloride-isobutyl vinyl ether copolymers, vinyl chloride-isopropyl vinyl ether copolymers, and vinyl chloride-ethyl vinyl ether copolymers; silicone oil; wax; oils and fats that are solid at room temperature other than wax, oils and fats that are liquid at room temperature such as castor oil, and their refined products; petrolatum; liquid paraffin; rosin, hydrogenated rosin, naphthenic acid, fatty acids, and their divalent metal salts. Examples of waxes include animal-derived waxes such as beeswax; plant-derived waxes; semi-synthetic waxes such as amide waxes; and synthetic waxes such as polyethylene oxide waxes. Chlorinated paraffin, wax, polyvinyl ether, polyether polyol, rosin, and vinyl chloride-isobutyl vinyl ether copolymers are preferred, and chlorinated paraffin, amide wax, polyethylene oxide wax, polyvinyl ether, rosin, and vinyl chloride-isobutyl vinyl ether copolymers are particularly preferred. Other thermoplastic resins may be used individually or in combination of two or more.
[0107] <Solvent> The solvent is not particularly limited as long as it can dissolve the copolymer of this embodiment. Examples include monohydric alcohols such as methanol, ethanol, isopropanol, n-butanol, and propylene glycol monomethyl ether; polyhydric alcohols such as ethylene glycol and 1,2-propylene glycol; ketones such as acetone, methyl ethyl ketone, and acetylacetone; ethers such as methyl ethyl ether and dioxane; glycol ethers such as ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, ethylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, and dipropylene glycol monopropyl ether; glycol acetates such as ethylene glycol monoacetate, ethylene glycol diacetate, and ethylene glycol monomethyl ether acetate; aliphatic hydrocarbons such as n-pentane and n-hexane; and aromatic hydrocarbons such as toluene, xylene, and solvent naphtha. Any one of these can be used alone or in combination of two or more.
[0108] <Other Optional Components> Other optional components may include, for example, dimethylpolysiloxane, silicone oil and other silicon compounds, fluorinated hydrocarbons and other fluorine-containing compounds, for the purpose of providing lubricity to the coating surface and preventing the adhesion of organisms. In addition, for example, various pigments, defoamers, pigment dispersants, leveling agents, anti-sagging agents, matting agents, UV absorbers, antioxidants, heat resistance improvers, slip agents, preservatives, plasticizers, and viscosity control agents may be included.
[0109] <Content> The total solids content (paint solids) of the antifouling coating composition is preferably 72% by mass or more, more preferably 72 to 90% by mass, and even more preferably 74 to 80% by mass, based on the total mass of the antifouling coating composition. If the paint solids content is above the lower limit, the VOCs of the coating can be reduced, and if it is below the upper limit, the coating viscosity can be made suitable for painting. In this specification, the paint solids content is the value measured by the measurement method described in the examples later.
[0110] If the solid content of the antifouling coating composition includes components other than the copolymer of this embodiment (antifouling agent, other thermoplastic resin, other optional components), the total content of the components other than the copolymer of this embodiment is not particularly limited, but is preferably 50 to 400 parts by mass, and more preferably 100 to 350 parts by mass, per 100 parts by mass of copolymer.
[0111] When the antifouling coating composition contains an antifouling agent, the amount of the antifouling agent is not particularly limited, but is preferably 10 to 200 parts by mass, and more preferably 50 to 150 parts by mass, per 100 parts by mass of copolymer. If the amount of the antifouling agent is above the lower limit, the antifouling effect of the formed coating film is better, and if it is below the upper limit, the physical properties of the coating film are better.
[0112] When the antifouling coating composition contains other thermoplastic resins, the content of the other thermoplastic resins is not particularly limited, but is preferably 0.1 to 50 parts by mass, and more preferably 0.1 to 10 parts by mass, per 100 parts by mass of copolymer. If the content of the other thermoplastic resins is above the lower limit, the coating film properties such as crack resistance and water resistance are better, and if it is below the upper limit, hydrolysis resistance is better.
[0113] <Physical Properties> [Type B Viscosity of Antifouling Paint Composition] The viscosity of the antifouling paint composition, as measured by a Type B viscometer at 25°C (also called Type B viscosity), is preferably 0.5 to 10 Pa·s, preferably 0.75 to 7.5 Pa·s, and more preferably 1 to 5 Pa·s. When the Type B viscosity of the antifouling paint composition is above the lower limit and below the upper limit, the paintability is good. The viscosity of the antifouling paint composition can be adjusted by the viscosity of the copolymer of this embodiment, the copolymer composition of this embodiment containing the copolymer, the amount of solvent added, etc. For example, when the total solid content (paint solid content) relative to the total mass of the antifouling paint composition is 71% by mass, it is preferable that the Type B viscosity is 5 Pa·s or less.
[0114] <Method for producing the antifouling paint composition> The antifouling paint composition of this embodiment can be produced by preparing the copolymer composition of this embodiment and adding an antifouling agent, solvent, and other optional components as needed, and mixing them.
[0115] <Use of Antifouling Coating Composition> The antifouling coating composition of this embodiment can be used to form a coating film (antifouling coating film) on the surface of substrates such as ships, various fishing nets, port facilities, oil fences, bridges, and underwater structures such as submarine bases. The coating film using the antifouling coating composition of this embodiment can be formed directly on the substrate surface or via a primer coating. The primer coating can be formed using, for example, a wash primer, a primer such as a chlorinated rubber-based or epoxy-based primer, or an intermediate coating paint.
[0116] The coating film can be formed by known methods. For example, the antifouling coating composition can be applied to the surface of a substrate or onto a base coating film on the substrate by means of brush application, spray application, roller application, immersion application, etc., and then dried to form the coating film. The amount of antifouling coating composition applied can generally be set to an amount that results in a dry coating film thickness (dry film thickness) of 10 to 400 μm. The coating film can usually be dried at room temperature (e.g., 10 to 30°C), and heat drying may be performed if necessary.
[0117] <Effects> Because the copolymer of this embodiment contains constituent unit (A) (a constituent unit having a carboxylate structure that is ionically bonded to a metal atom M), the coating film containing the copolymer of this embodiment exhibits self-polishing properties. That is, when the coating film containing the copolymer of this embodiment comes into contact with seawater, the carboxylate structure and metal atom M are hydrolyzed to generate carboxyl groups, which then dissolve in seawater. Therefore, the surface of the coating film gradually dissolves (wears off) and is renewed (self-polished) by contact with seawater. In particular, when the coating film contains an antifouling agent, the antifouling agent is always exposed on the surface of the coating film, and an excellent antifouling effect is exhibited over a long period of time. Furthermore, this coating film has excellent hardness and water resistance, and is less prone to damage or peeling that would lead to a decrease in the antifouling effect. In addition, the degree of wear can be adjusted to ensure that an excellent antifouling effect is stably exhibited over a long period of time.
[0118] According to this embodiment, for example, in the coating film wear test (3 months) described in the later examples, a coating film showing a wear rate of 5 to 50 μm / M can be obtained. If the wear rate is above the lower limit, sufficient self-polishing properties are obtained. If the wear rate is below the upper limit, good long-term antifouling properties are obtained.
[0119] Furthermore, since the copolymer and the copolymer composition containing the solvent of this embodiment have low viscosity, an antifouling paint composition with paintability can be obtained without adding any further solvent during the production of the antifouling paint composition. Also, when adding antifouling agents, etc., good mixing can be achieved with antifouling agents, etc., without adding a solvent or with only a small amount of solvent added. Therefore, an antifouling paint composition with a low VOC content can be obtained.
[0120] The present invention will be described in detail below with reference to examples. However, the present invention is not limited in any way by the following examples. In the following, "wt%" means "mass%" and "parts" means "parts by mass".
[0121] <Measurement Method and Evaluation Method> [Weight-average molecular weight (Mw), number-average molecular weight (Mn)] The number-average molecular weight (Mn) and weight-average molecular weight (Mw) were measured using GPC (gel permeation chromatography) under the following conditions.
[0122] • Copolymerization apparatus: "HLC-8320GPC" (manufactured by Tosoh Corporation) Column: "TSKgel G4000HXL*G2000HXL" (manufactured by Tosoh Corporation, 7.8 mm x 30 cm) Eluent: Tetrahydrofuran (THF) (1 mmol citrate) Flow rate: 1,000 mL / min Detector: RI Column constant temperature bath temperature: 40°C Standard substance: Polystyrene Sample preparation method: 1 mmol of THF containing citrate was added to the polymer solution prepared in each production example to dissolve it to a solid content concentration of 0.4 wt%, and the filtrate obtained by filtering through a membrane filter was used as the GPC measurement sample. Calibration curves were prepared using F288 / F1 / 28 / F80 / F40 / F20 / F2 / A1000 (manufactured by Tosoh Corporation, standard polystyrene) and styrene monomers.
[0123] • Compound (b2) Apparatus: "HLC-8320" (Tosoh Corporation) Column: TSKgelSuperHZM-M* HZM-M *HZ2000 (Tosoh Corporation, 4.6 mm x 15 cm) Eluent: Tetrahydrofuran (THF) Flow rate: 0.35 mL / min Detector: RI Column constant temperature bath temperature: 40°C Standard substance: Polystyrene Sample preparation method: THF was added to the (meth)acrylic compound solution prepared in each production example to dissolve it to a solid content concentration of 0.2 wt%, and the filtrate obtained by filtering through a membrane filter was used as the GPC measurement sample. Calibration curves were prepared using F288 / F1 / 28 / F80 / F40 / F20 / F2 / A1000 (Tosoh Corporation, standard polystyrene) and styrene monomers.
[0124] [Solid Content (Heating Residue)] 0.50 g of the sample (polymer composition or paint composition) was weighed into an aluminum dish, 3 mL of toluene was added using a dropper, and the mixture was spread evenly on the bottom of the dish for pre-drying. Pre-drying is a process to spread the sample evenly across the dish and facilitate the evaporation of the solvent during main drying. In pre-drying, the sample and toluene were heated and dissolved in a water bath at 70-80°C and evaporated to dryness. After pre-drying, main drying was performed in a hot air dryer at 105°C for 2 hours. The solid content (heating residue) was calculated from the mass of the sample before pre-drying (mass before drying) and the mass after main drying (mass after drying) using the following formula: Solid Content (mass%) = Mass after drying (g) / Mass before drying (g) × 100
[0125] [Acid Value] Approximately 0.5 g of the sample was accurately weighed into a beaker (A (g)), and 50 mL of toluene / ethanol solution was added. A few drops of phenolphthalein were added, and the sample was titrated with 0.5 N KOH solution. (Titration volume = B (mL), titer of KOH solution = f). A blank measurement was performed in the same manner (titration volume = C (mL)), and the value was calculated according to the following formula: Acid value (mg KOH / g) = {(B - C) × 0.2 × 56.11 × f} / A / Solids
[0126] [Solubility Parameters (SP Values)] The solubility parameters (SP values) of monomer (b1) and compound (b2) were determined using the Fedors method for calculating solubility parameters, as described in the "Collection of Application Examples of Solubility Parameters" published by Information Organization Co., Ltd. When compound (b2) is formed from two or more monomers, the SP value of compound (b2) was calculated from the SP values and ratios (molar ratios) of each monomer that forms compound (b2).
[0127] [Glass transition temperature (Tg)] The Tg of monomer (b1) was the value described in paragraphs
[0039] and
[0040] of this specification. The Tg of compound (b2) was the value obtained by converting the absolute temperature (K) calculated from the following formula (1) to degrees Celsius (°C). 1 / Tg = Σ(w i / Tg i )...(1) In formula (1), w i This indicates the mass fraction of monomer i constituting compound (b2), and Tg i The values Tg and Tg in formula (1) indicate the glass transition temperature of the homopolymer of monomer i constituting compound (b2). i This value is expressed in absolute temperature (K). Also, Tg i The values used were those found in "Polymer Handbook, Fourth Edition," John Wiley & Sons Inc., J. Brandrup, VI / p, 193-253.
[0128] [Gardner Viscosity] The copolymer compositions obtained in each manufacturing example were used as samples, and the Gardner viscosity was measured using the following method. The sample was placed in a dry Gardner bubble viscosity tube (hereinafter also simply referred to as "visco tube") up to the indicated line on the viscosity tube and sealed with a cork stopper. The viscosity tube containing the sample was immersed vertically in a constant temperature water bath adjusted to a specified temperature (25.0 ± 0.5 °C) for at least 2 hours to bring the sample to a constant temperature. The viscosity (Gardner viscosity) was determined by simultaneously rotating the reference viscosity tube and the viscosity tube containing the sample by 180° and comparing the bubble rise rate of the sample with that of the reference tube.
[0129] [Contact Angle] The copolymer compositions obtained in each manufacturing example were used as samples, and the contact angle was measured using the following method. The sample was applied to a glass substrate using a 500 μm applicator to a dry film thickness of 80 to 150 μm, and dried at 25°C for one week to obtain a test plate with a coated film. The water contact angle of the coating on this test plate was measured at a temperature of 25°C, with 1 μL of pure water, and a waiting time of 1 second from application to measurement.
[0130] [Coating Film Wear Test] The coating compositions obtained in each example were used as samples, and the wear rate was measured using the following method. The sample was applied to a 50 mm x 50 mm x 2 mm (thickness) rigid polyvinyl chloride board using an applicator to a dry film thickness of 120 μm, and dried to form a coating film, thereby obtaining a test plate. This test plate was mounted on a rotating drum placed in seawater at 25°C or 35°C and rotated at a peripheral speed of 7.7 m / s (15 knots). This condition was maintained for three months, and the film thickness (μm) of the coating film after three months was measured. From the measured film thickness, the worn film thickness after three months (120 μm - measured film thickness) was calculated, and this value was divided by the number of days of measurement and multiplied by 30 to obtain the wear rate. A wear rate within the range of 5 to 50 μm / M is most preferable.
[0131] [Static Antifouling Properties] The paint compositions obtained in each example were used as samples, and their static antifouling properties were evaluated using the following method. The samples were applied with a brush to a sandblasted steel plate that had been pre-coated with rust-preventive paint, so that the dry film thickness was 200 to 300 μm, and dried to form a paint film to obtain a test plate. After leaving this test plate in the sea for three months, the ratio of the area on which marine organisms were attached to the total surface area of the paint film (area of attachment to marine organisms) was examined, and the static antifouling properties were evaluated according to the following criteria: A: Area of attachment to marine organisms is 10% or less. B: Area of attachment to marine organisms is more than 10% but 20% or less. C: Area of attachment to marine organisms is more than 20% but 40% or less. D: Area of attachment to marine organisms is more than 40%.
[0132] <Materials Used> [Monomer (a)] a-1: Metal-containing monomer mixture synthesized in manufacturing example a-1 described later. a-2: Metal-containing monomer mixture synthesized in manufacturing example a-2 described later.
[0133] [Compounds having radical polymerizable groups other than monomer (a)] MM-1: (meth)acrylic compound solution synthesized in Production Example 1 described later. MM-2: (meth)acrylic compound solution synthesized in Production Example 2 described later. MM-3: (meth)acrylic compound solution synthesized in Production Example 3 described later. MM-4: (meth)acrylic compound solution synthesized in Production Example 4 described later. MM-5: (meth)acrylic compound synthesized in Production Example 5 described later. MM-6: (meth)acrylic compound solution synthesized in Production Example 6 described later. SLMA: A mixture of lauryl methacrylate (Tg of homopolymer: -65°C) and tridecyl methacrylate (Tg of homopolymer: -60°C) (Tg of SLMA polymer: -62°C, SP value 9.00 (cal / cm²) 3 ) 1/2 ). MMA: Methyl methacrylate (Tg of homopolymer: 105°C, SP value 9.93 (cal / cm³) 3 ) 1/2 ). EA: Ethyl acrylate (Tg of homopolymer: -20°C, SP value 10.20 (cal / cm³) 3 ) 1/2 nBA: n-butyl acrylate (Tg of homopolymer: -45°C, SP value 9.77 (cal / cm³)) 3 ) 1/2 ). MTA: 2-methoxyethyl acrylate (Tg of homopolymer: -47.3°C, SP value 10.16 (cal / cm³) 3 ) 1/2 nBMA: n-butyl methacrylate (Tg of homopolymer: 20°C, SP value 9.4 (cal / cm³)) 3 ) 1/2 ).
[0134] [Materials other than compounds with radical polymerizable groups] PGM: Propylene glycol methyl ether, solvent. AIBN: 2,2'-Azobisisobutyronitrile, polymerization initiator. AMBN: 2,2'-Azobis(2-methylbutyronitrile), polymerization initiator. Perocta O: Trade name, manufactured by NOF Corporation, 1,1,3,3-Tetramethylbutylperoxy-2-ethylhexanoate, polymerization initiator. Nofmer MSD: Trade name, manufactured by NOF Corporation, α-Methylstyrene dimer, chain transfer agent. Toyoparax 150: (Manufactured by Tosoh Corporation, chlorinated paraffin). Disparon A603-20X: (Manufactured by Kusumoto Chemical Co., Ltd., polyamide wax). Disparon 4200-20: (Manufactured by Kusumoto Chemical Co., Ltd., oxidized polyethylene wax).
[0135] <Production Example a-1> In a four-necked flask equipped with a condenser, thermometer, dropping funnel, and stirrer, 85.4 parts of PGM and 40.7 parts of zinc oxide were charged and heated to 75°C while stirring. Subsequently, a mixture consisting of 43.1 parts of methacrylic acid, 36.1 parts of acrylic acid, and 6.5 parts of water was added dropwise from the dropping funnel at a constant rate over 3 hours. After further stirring for 2 hours, 36 parts of n-butanol were added to obtain a clear metal-containing monomer mixture a-1. The solid content was 44.8% by mass.
[0136] <Production Example a-2> In a four-necked flask equipped with a condenser, thermometer, dropping funnel, and stirrer, 100 parts of PGM and 40.7 parts of zinc oxide were charged and heated to 75°C while stirring. Subsequently, a mixture consisting of 30.1 parts of methacrylic acid, 25.2 parts of acrylic acid, and 43.3 parts of octic acid was added dropwise from the dropping funnel at a constant rate over 3 hours. After the addition was complete, the reaction solution changed from a milky white state to clear. After stirring for a further 2 hours, 21.3 parts of PGM were added to obtain metal-containing monomer mixture a-2. The solid content was 55.0% by mass.
[0137] <Production Example 1> A mixture consisting of 60 parts ethyl acetate, 100 parts SLMA, and 0.4 parts AMBN was charged into a reaction vessel equipped with a stirrer, a temperature controller, and a dropping funnel. The mixture was heated to 90°C under a nitrogen atmosphere while stirring and held for 4 hours. Subsequently, a mixture consisting of 20 parts ethyl acetate and 0.3 parts AMBN was added dropwise from the dropping funnel at a constant rate over 1 hour. Two hours after the end of the dropwise addition, 20 parts ethyl acetate was added to obtain a solution of (meth)acrylic compound MM-1 with a solid content of 51.7% by mass and a Gardner viscosity of A or less.
[0138] <Production Examples 2-4 and 6> Solution-type (meth)acrylic compound solutions MM-2 to MM-4 and MM-6 were prepared in the same manner as in Production Example 1, except that the amount (parts) of monomer and initiator AMBN was as shown in Table 1.
[0139] <Production Example 5> (Production of Dispersant 1) In a polymerization apparatus equipped with a stirrer, condenser, and thermometer, 900 parts of deionized water, 60 parts of 2-sulfoethyl sodium methacrylate, 10 parts of potassium methacrylate, and 12 parts of MMA were added and stirred, and the temperature was raised to 50°C while purging nitrogen inside the polymerization apparatus. 0.08 parts of 2,2'-azobis(2-methylpropionamidine) dihydrochloride were added as a polymerization initiator, and the temperature was further raised to 60°C. After raising the temperature, MMA was continuously added dropwise at a rate of 0.24 parts / min for 75 minutes using a dropping pump. After holding the reaction solution at 60°C for 6 hours, it was cooled to room temperature to obtain Dispersant 1, a clear aqueous solution with a solid content of 10% by mass.
[0140] (Preparation of chain transfer agent 1) In a synthesis apparatus equipped with a stirring device, 1.00 g of cobalt(II) acetate tetrahydrate, 1.93 g of diphenylglyoxime, and 80 mL of diethyl ether that had been deoxygenated beforehand by nitrogen bubbling were added under a nitrogen atmosphere and stirred at room temperature for 30 minutes. Then, 10 mL of boron trifluoride diethyl ether complex was added and stirred for a further 6 hours. The mixture was filtered, the solid was washed with diethyl ether, and vacuum dried for 15 hours to obtain 2.12 g of chain transfer agent 1, which was a reddish-brown solid.
[0141] (Preparation of (meth)acrylic compound MM-5 having radical polymerizable groups) In a polymerization apparatus equipped with a stirrer, condenser, and thermometer, 145 parts of deionized water, 0.1 parts of sodium sulfate, and 0.25 parts of dispersant 1 (solid content 10% by mass) were added and stirred to obtain a homogeneous aqueous solution. Next, 100 parts of MMA, 0.002 parts of chain transfer agent 1, and 0.4 parts of perocta O were added to obtain an aqueous suspension. Next, the polymerization apparatus was purged with nitrogen, the temperature was raised to 80°C and the reaction was carried out for 1 hour, and then the temperature was raised to 90°C and held for 1 hour to further increase the polymerization rate. After that, the reaction solution was cooled to 40°C to obtain an aqueous suspension containing the polymer. This aqueous suspension was filtered through a nylon filter cloth with a mesh size of 45 μm, the filtrate was washed with deionized water, dehydrated, and dried at 40°C for 16 hours to obtain the (meth)acrylic compound MM-5 having radical polymerizable groups. The number average molecular weight of MM-5 was 3000.
[0142] Table 1 shows the characteristic values (solids content (mass%), Gardner viscosity, B-type viscosity, weight-average molecular weight (Mw), number-average molecular weight (Mn), SP value, and Tg) of the obtained (meth)acrylic compound solutions MM-1 to MM-4, MM-6, and (meth)acrylic compound MM-5. The solids content of the (meth)acrylic compound solution is equal to the content of the (meth)acrylic compound.
[0143]
[0144] <Production Example 7> In a four-necked flask equipped with a condenser, thermometer, dropping funnel, and stirrer, 15 parts n-butanol, 56 parts xylene, and 4.0 parts EA were charged and heated to 100°C while stirring. Subsequently, a mixture consisting of 31 parts MMA, 30 parts EA, 10 parts nBA, 5 parts MTA, 10 parts SLMA, 31.3 parts of the metal-containing monomer mixture a-1 obtained in Production Example a-1 (total amount including organic solvent), 1.5 parts Nofmer MSD, and 13.0 parts AMBN was added dropwise at a constant rate over 6 hours. After the dropwise addition was complete, 0.5 parts t-butyl peroctoate and 14.5 parts xylene were added dropwise over 30 minutes, and the mixture was stirred for a further 1 hour and 30 minutes to obtain a copolymer composition (polymer solution) A-1 with a solid content of 48.5% by mass and a Gardner viscosity of G+.
[0145] <Production Examples 8-16> Solution copolymer-containing compositions A-2 to A-10 were produced in the same manner as in Production Example 6, except that the type and amount (parts) of the compound having a radical polymerizable group and the amount (parts) of the polymerization initiator AMBN were as shown in Table 2.
[0146] Table 2 shows the varnish properties (Gardner viscosity, solids content (mass%), acid value), weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the copolymer contained in each copolymer composition, and the results of the contact angle evaluation for the obtained copolymer compositions A-1 to A-10. The solids content of copolymer compositions A-1 to A-10 is equal to the copolymer content.
[0147]
[0148] In Table 2, the values listed in the "Amount" column indicate the amount (in parts) used. Note that for the metal-containing monomer mixtures a-1 and a-2 in Table 2, only the solid content is listed.
[0149] The coating films of copolymer compositions A-1 to A-7 in manufacturing examples 7 to 13 tended to have high contact angles, while the coating films of copolymer compositions A-8 to A-9 in manufacturing examples 14 to 15 tended to have low contact angles.
[0150] <Examples 1-8, Comparative Examples 1-3> Following the compositions shown in Table 3, each component was placed in a metal can, then 110 g of glass beads were added and pre-mixed with a stirring rod. The mixture was then dispersed with pigment using a rocking shaker to obtain an antifouling paint composition. The evaluation results of the obtained antifouling paint compositions are shown in Table 3.
[0151]
[0152] In Table 3, the values listed in the composition column indicate the amount (in parts) of the copolymer composition. In Table 3, the amount of copolymer composition refers to the total amount of the copolymer composition.
[0153] The antifouling coating compositions of Examples 1 to 8 had high solids content and low viscosity, yet exhibited low viscosity and good paintability. Furthermore, the formed coating film had good contact angle and wear rate, and also exhibited good antifouling properties. The antifouling coating composition of Comparative Example 1, which used a copolymer without constituent unit (B), had low solids content, high paint viscosity, and poor paintability, while the antifouling coating composition of Comparative Example 2 exhibited poor antifouling properties.
[0154] According to the present invention, it is possible to provide an antifouling paint composition that can form a coating film with excellent antifouling properties, as well as a copolymer and copolymer composition suitable for obtaining the antifouling paint composition.
Claims
1. A copolymer comprising a structural unit (A) and a structural unit (B), wherein the structural unit (A) has at least one structure selected from the group consisting of a structure represented by the following formula (a1) and a structure represented by the following formula (a2), the structural unit (B) is at least one selected from the group consisting of a structural unit (B1) and a structural unit (B2), the structural unit (B1) is a structural unit derived from a monomer (b1) which is a monomer represented by the following formula (b1), has a molecular weight of 200 to 500, and has a glass transition temperature of 40°C or lower when formed into a homopolymer, and the structural unit (B2) is a structural unit derived from a compound (b2) which has a radical polymerizable group and 2 or more structural units represented by the following formula (Z1), and has a glass transition temperature of 10°C or lower. -COO-M-OCO- ... (a1) -COO-M-R 1 ... (a2) (wherein M represents a divalent metal atom, R 1 represents a monovalent organic acid residue.) CH 2 =CR 31 -COOR 32 ... (b1) (wherein R 31 represents a hydrogen atom, a methyl group or CH 2 OH, and R 32 represents an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, an unsubstituted or substituted non-aromatic heterocyclic group, or an unsubstituted or substituted aralkyl group.) (wherein R 41 represents a hydrogen atom, a methyl group or CH 2 OH, and R 42 represents OR 43 , a halogen atom, COR 44 , COOR 45 , CN, CONR 46 R 47 or R 48 . R 43 to R 47 Each of these independently represents a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted aryl group, an unsubstituted or substituted heteroaryl group, an unsubstituted or substituted non-aromatic heterocyclic group, or an unsubstituted or substituted aralkyl group. 48 (This indicates an unsubstituted or substituted aryl group, or an unsubstituted or substituted heteroaryl group.) 2. The solubility parameter of the monomer (b1) is 9.5 (cal / cm³). 3 ) 1/2 The copolymer according to claim 1, which is as follows:
3. A copolymer composition comprising the copolymer described in claim 1.
4. The copolymer composition according to claim 3, further comprising a solvent.
5. An antifouling coating composition comprising the copolymer composition described in claim 4.
6. The antifouling coating composition according to claim 5, further comprising an antifouling agent.
7. The antifouling coating composition according to claim 6, wherein the antifouling agent comprises at least one selected from the group consisting of 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitride and medetomidine.
8. The antifouling coating composition according to any one of claims 5 to 7, further comprising a thermoplastic resin (excluding the copolymer).