Thermosetting resin composition
The thermosetting resin composition with specific polymerization inhibitors and monomers addresses the balance of pot life and moldability, enhancing handling and curing properties for high-quality molded products.
Patent Information
- Application Number
- PCT/JP2026/018133
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Existing thermosetting resin compositions face challenges in achieving a balance between long pot life during compounding and mixing, while maintaining good curability during molding, which is crucial for producing high-quality molded products.
A thermosetting resin composition comprising specific combinations of thermosetting resin, ethylenically unsaturated monomer, thermal polymerization initiator, and polymerization inhibitors, including hindered phenols and phenothiazine, quinone, or polyhydric phenol compounds, to enhance pot life and moldability.
The composition achieves improved pot life and moldability, ensuring better handling and curing properties, resulting in high-quality cured products with enhanced mechanical strength and reduced curing shrinkage.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
thermosetting resin composition
[0001] This disclosure relates to thermosetting resin compositions and their cured products, as well as mold stators.
[0002] Thermosetting resin compositions are used as molding materials, for example, in insulating members, sealing members, or fixing members of electrical equipment. Patent Document 1 discloses an epoxy resin composition for casting that contains a specific curing accelerator, with the aim of providing an epoxy resin composition for casting that can achieve both a long pot life necessary for casting work and suppression of internal heat generation that causes molding abnormalities, and further shorten the casting cycle time.
[0003] Japanese Patent Publication No. 2015-28132
[0004] Molding materials require a long pot life during compounding and mixing, while also needing good curability during molding. In particular, there has been a need for materials that exhibit a longer pot life while maintaining good curability, depending on the size of the molded product and the molding time.
[0005] This disclosure provides a thermosetting resin composition that has good moldability and improved pot life.
[0006] The contents of this disclosure include the following embodiments: [Embodiment 1] A thermosetting resin composition comprising (A) a thermosetting resin, (B) an ethylenically unsaturated monomer, (C) a thermal polymerization initiator, and (D) a polymerization inhibitor, wherein the (D) polymerization inhibitor comprises at least a (D-1) polymerization inhibitor and a (D-2) polymerization inhibitor, the (D-1) polymerization inhibitor is a hindered phenol, the (D-2) polymerization inhibitor is one or more selected from the group consisting of phenothiazine compounds, quinone compounds, and polyhydric phenol compounds, and the mass ratio of the (D-1) polymerization inhibitor to the (D-2) polymerization inhibitor is 99:1 to 80:20. [Aspect 2] The thermosetting resin composition according to aspect 1, wherein the total amount of the (A) thermosetting resin and the (B) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 0.1 to 3.0 parts by mass of the (D-1) polymerization inhibitor and 0.005 to 0.30 parts by mass of the (D-2) polymerization inhibitor. [Aspect 3] The thermosetting resin composition according to aspect 1 or 2, wherein the hindered phenol is represented by the following formula (1). (In formula (1), R 1 ~R 3 Each of these is an alkyl group having 1 to 5 carbon atoms.) [Aspect 4] The thermosetting resin composition according to any one of the above aspects 1 to 3, wherein the phenothiazine compound is represented by the following formula (2). (In formula (2), R 4 ~R 11 Each of these is independently a hydrogen atom, a hydroxyl group, a halogen atom, an alkyl group, an acyl group, an aryl group, an alkoxy group, an aralkyl group, an alkoxyalkyl group, an amino group, an alkylamino group, a glycidyl group, a hydroxyalkyl group, or an aryloxyalkyl group.) [Aspect 5] The thermosetting resin composition according to any one of the above aspects 1 to 4, wherein the polyvalent phenol compound is represented by the following formula (3). (In formula (3), R 12 ~R 16 Each is independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.) [Aspect 6] The thermosetting resin composition according to any one of the above aspects 1 to 5, wherein the quinone compound is represented by the following formula (4). (In formula (4), R 17 ~R 20 (Each of these is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogen atom.) [Aspect 7] The thermosetting resin composition according to any one of aspects 1 to 6, further comprising (E) a low shrinkage agent. [Aspect 8] The thermosetting resin composition according to any one of aspects 1 to 7, further comprising (F) glass fibers and (G) an inorganic filler. [Aspect 9] The thermosetting resin composition according to any one of aspects 1 to 8, wherein the total amount of the (A) thermosetting resin and the (B) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 5 to 80 parts by mass of the (A) thermosetting resin, 20 to 95 parts by mass of the (B) ethylenically unsaturated monomer, and 0.5 to 20 parts by mass of the (C) thermal polymerization initiator. [Aspect 10] A thermosetting resin composition according to any one of aspects 7 to 9, wherein the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 10 to 60 parts by mass of (E) low shrinkage agent. [Aspect 11] A thermosetting resin composition according to any one of aspects 8 to 10, wherein the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer is 100 parts by mass, the composition contains 5 to 200 parts by mass of (F) glass fiber, and 50 to 1000 parts by mass of (G) inorganic filler. [Aspect 12] A cured product of the thermosetting resin composition according to any one of aspects 1 to 11. [Aspect 13] A molded stator having a stator core, a coil wound around the stator core, and a mold material covering the stator, wherein the mold material is a cured product of the thermosetting resin composition according to any one of aspects 1 to 11.
[0007] According to this disclosure, it is possible to provide a thermosetting resin composition that has good moldability and an improved pot life.
[0008] This is a schematic cross-sectional view of an exemplary motor.
[0009] The embodiments of the present invention will be described in detail below. However, the present invention is not limited to the embodiments shown below.
[0010] In this specification, when "~" is used for a numerical range, the numbers at both ends are the upper and lower limits, respectively, and are included in the numerical range. If multiple upper or lower limits are listed, a numerical range can be created from all combinations of upper and lower limits. Similarly, if multiple numerical ranges are listed, separate numerical ranges can be created by individually selecting and combining upper and lower limits from those ranges.
[0011] In this specification, "(meth)acrylic acid" means methacrylic acid or acrylic acid, "(meth)acrylate" means acrylate or methacrylate, and "(meth)acryloyloxy" means acryloyloxy or methacryloyloxy.
[0012] In this specification, "ethylenically unsaturated bond" means a double bond formed between carbon atoms excluding the carbon atoms that form the aromatic ring, and "ethylenically unsaturated monomer" means a monomer having an ethylenically unsaturated bond.
[0013] In this specification, "weight-average molecular weight" and "number-average molecular weight" are defined as values obtained by measuring at room temperature (23°C) under the following conditions using gel permeation chromatography (GPC) and using a standard polystyrene calibration curve. Apparatus: Shodex™ GPC-101 (Resonac Corporation) Column: Shodex™ LF-804 (Resonac Corporation) Column temperature: 40°C Sample: 0.2% by mass tetrahydrofuran solution of the sample Flow rate: 1 mL / min Eluent: Tetrahydrofuran Detector: Shodex™ RI-71S (Resonac Corporation)
[0014] In this specification, "acid value" refers to the acid value measured in accordance with JIS K6901:2021 5.3. That is, the acid value means the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of non-volatile matter excluding the solvent.
[0015] <Thermosetting Resin Composition> The thermosetting resin composition of one embodiment contains (A) a thermosetting resin, (B) an ethylenically unsaturated monomer, (C) a thermal polymerization initiator, and (D) a polymerization inhibitor, wherein the polymerization inhibitor (D) contains at least (D-1) a polymerization inhibitor and (D-2) a polymerization inhibitor, where (D-1) is a hindered phenol and (D-2) is one or more selected from the group consisting of phenothiazine compounds, quinone compounds, and polyhydric phenol compounds, and the mass ratio of the polymerization inhibitor (D-1) to the polymerization inhibitor (D-2) is 99:1 to 80:20. By using the polymerization inhibitor (D-1) and the polymerization inhibitor (D-2) in a specific ratio, it is possible to achieve both a good pot life and good moldability. While not bound by any particular theory, the main function of (D-1) polymerization inhibitors is reaction suppression through radical scavenging, which improves pot life in the early stages of the reaction, but the effect may decrease in the later stages. On the other hand, (D-2) polymerization inhibitors have the function of suppressing the curing reaction by controlling reduction and redox reactions, and exert an effect of improving pot life over a wide range from the early to late stages of curing. We believe that by combining (D-1) polymerization inhibitors and (D-2) polymerization inhibitors, their respective characteristics, namely radical scavenging and control of redox reactions, work complementaryly, leading to a significant improvement in pot life. If the mass ratio of (D-2) to (D-1) is too high, pot life will improve further, but moldability tends to be impaired, so it is necessary to use them in a specific ratio from the perspective of balancing pot life and moldability.
[0016] (A) Thermosetting resins (A) refers to resins that harden by forming a crosslinked structure when heated, and refers to the state before hardening. (A) As thermosetting resins, thermosetting resins that are commonly used as molding materials can be used. For example, resins that have functional groups capable of forming a crosslinked structure when heated and hardened as a thermosetting resin composition are preferred. In particular, resins that have multiple ethylenically unsaturated groups as functional groups are preferred from the viewpoint that they can also react with (B) ethylenically unsaturated monomers.
[0017] (A) The weight-average molecular weight of the thermosetting resin is preferably 2,000 or more, more preferably 5,000 or more, even more preferably 10,000 or more, and particularly preferably 15,000 or more. (A) The weight-average molecular weight of the thermosetting resin is preferably 50,000 or less, more preferably 40,000 or less, even more preferably 35,000 or less, and particularly preferably 30,000 or less. When the weight-average molecular weight is within the above range, it tends to reduce the change in the fluidity of the resin composition from the time the thermosetting resin composition is put into the molding machine until it is filled into the mold. Note that (A) the weight-average molecular weight of the thermosetting resin refers to the weight-average molecular weight of the resin in its pre-curing state.
[0018] (A) Specific examples of thermosetting resins include (A-1) unsaturated polyester resin, (A-2) vinyl ester resin, (A-3) urethane (meth)acrylate resin, (A-4) diallyl phthalate resin, (A-5) epoxy resin, etc. (A) From the viewpoint of moldability, fluidity, and curing shrinkage, it is preferable that the thermosetting resin includes (A-1) unsaturated polyester resin. (A) The thermosetting resin may be used alone or in combination of two or more types.
[0019] The content of (A) thermosetting resin in the thermosetting resin composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. The content of (A) thermosetting resin in the thermosetting resin composition is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 40 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. When the content of (A) thermosetting resin in the thermosetting resin composition is 5 parts by mass or more, the mechanical strength of the cured product tends to be good. When the content of (A) thermosetting resin in the thermosetting resin composition is 80 parts by mass or less, the viscosity of the thermosetting resin composition can be adjusted to an appropriate range, and the moldability tends to be better.
[0020] <(A-1) Unsaturated Polyester Resin> The (A-1) unsaturated polyester resin is a polycondensate of a polyhydric alcohol and an unsaturated polybasic acid, or a polycondensate of a polyhydric alcohol, an unsaturated polybasic acid and a saturated polybasic acid, and is not particularly limited. The (A-1) unsaturated polyester resin is preferably a polycondensate of a diol, an unsaturated polybasic acid and an optional saturated polybasic acid, more preferably a polycondensate of a diol containing propylene glycol, an unsaturated polybasic acid and an optional saturated polybasic acid, and even more preferably a polycondensate of a diol containing propylene glycol and neopentyl glycol, an unsaturated polybasic acid and an optional aromatic saturated polybasic acid.
[0021] (A-1) Unsaturated polyester resin may be used alone or in combination of two or more types. (A-1) Using unsaturated polyester resin tends to yield cured products with excellent mechanical strength and heat resistance.
[0022] In this disclosure, reactive diluents such as styrene monomers contained in commercially available unsaturated polyester resins are classified as (B) ethylenically unsaturated monomers.
[0023] The polyhydric alcohol is not particularly limited as long as it is a compound having two or more hydroxyl groups. The polyhydric alcohol is preferably one or more selected from the group consisting of diols and triols, and more preferably a diol. Examples of the polyhydric alcohol include alkylene glycols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, and hydrogenated bisphenol A; polyoxyalkylene polyols such as diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol; bisphenol A; alkylene oxide-modified bisphenol A such as ethylene oxide adducts of bisphenol A and propylene oxide adducts of bisphenol A; and glycerin. From the viewpoint of crack resistance during molding, alkylene glycol is preferred, alkylene glycol having 2 to 6 carbon atoms is more preferred, one or more selected from ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, and neopentyl glycol is even more preferred, and propylene glycol is particularly preferred. From the viewpoint of improving the durability of molded articles, it is preferable to use propylene glycol and neopentyl glycol in combination. From the viewpoint of chemical resistance, it is preferable to use propylene glycol and hydrogenated bisphenol A in combination. The polyhydric alcohols may be used alone or in combination of two or more.
[0024] The unsaturated polybasic acid is not particularly limited as long as it has an ethylenically unsaturated bond and two or more carboxyl groups, or an acid anhydride thereof; known compounds can be used. In particular, unsaturated polybasic acids having 4 to 6 carbon atoms or their acid anhydrides are preferred because they are low-cost and yield thermosetting resin compositions with excellent mechanical strength and heat resistance of the cured product. The unsaturated polybasic acid is preferably an unsaturated dibasic acid. Examples of unsaturated polybasic acids include maleic acid, maleic anhydride, fumaric acid, citraconic acid, itaconic acid, and chloromaleic acid. More preferably, one or more selected from fumaric acid, maleic acid, maleic anhydride, and itaconic acid are used. The unsaturated polybasic acid may be used alone or in combination of two or more types.
[0025] Preferred combinations of polyhydric alcohols and unsaturated polybasic acids include diols and unsaturated dibasic acids, and more preferably alkylene glycols and unsaturated dibasic acids having 4 to 6 carbon atoms. More specifically, examples include combinations of maleic anhydride, propylene glycol and neopentyl glycol; maleic anhydride and propylene glycol; fumaric acid and propylene glycol; maleic anhydride, propylene glycol and neopentyl glycol and hydrogenated bisphenol A; and maleic anhydride, fumaric acid, propylene glycol and neopentyl glycol and hydrogenated bisphenol A. The combinations of maleic anhydride, propylene glycol and neopentyl glycol, and maleic anhydride and propylene glycol are preferred because they are less expensive and improve crack resistance during molding and the durability of molded products.
[0026] The saturated polybasic acid is not particularly limited as long as it is a compound having no ethylenically unsaturated bond and having two or more carboxy groups, or an acid anhydride thereof, and a known one can be used. Examples of the saturated polybasic acid include aromatic saturated polybasic acids such as phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, tetrachlorophthalic anhydride, tetrabromophthalic anhydride, nitrophthalic acid, and halogenated phthalic anhydride, or acid anhydrides thereof; aliphatic saturated polybasic acids such as succinic acid, adipic acid, sebacic acid, oxalic acid, malonic acid, azelaic acid, and glutaric acid; and acid anhydrides of cycloaliphatic saturated polybasic acids such as hexahydrophthalic anhydride. The saturated polybasic acids may be used alone or in combination of two or more thereof.
[0027] The weight average molecular weight of the (A-1) unsaturated polyester resin is not particularly limited. The weight average molecular weight of the (A-1) unsaturated polyester resin is preferably from 2,000 to 50,000, more preferably from 5,000 to 50,000, still more preferably from 10,000 to 50,000, and particularly preferably from 13,000 to 35,000. When the weight average molecular weight is from 2,000 to 50,000, the moldability of the thermosetting resin composition tends to be even more favorable. When the weight average molecular weight is from 2,000 to 50,000, there is a tendency that the change in fluidity of the resin composition from when the thermosetting resin composition is charged into a molding machine to when it is filled into a mold can be further reduced.
[0028] The degree of unsaturation of the (A-1) unsaturated polyester resin is preferably from 50 to 100 mol%, more preferably from 60 to 100 mol%, and still more preferably from 70 to 100 mol%. When the degree of unsaturation is within the above range, the moldability of the thermosetting resin composition containing the (A-1) unsaturated polyester resin tends to be more favorable.
[0029] The degree of unsaturation of the (A-1) unsaturated polyester resin is calculated by the following formula using the number of moles of the unsaturated polybasic acid and the saturated polybasic acid used as raw materials. Degree of unsaturation (mol%) = {(Number of moles of unsaturated polybasic acid × Number of ethylenically unsaturated bonds per molecule of unsaturated polybasic acid) / (Number of moles of unsaturated polybasic acid + Number of moles of saturated polybasic acid)} × 100
[0030] (Method for synthesizing (A-1) unsaturated polyester resin) (A-1) unsaturated polyester resin can be synthesized using the above raw materials by known methods. Various conditions in the synthesis of (A-1) unsaturated polyester resin are set appropriately according to the raw materials used and their amounts.
[0031] Generally, esterification reactions can be carried out under pressure or reduced pressure at a temperature of 140°C to 230°C in an inert gas stream such as nitrogen gas. Esterification catalysts can be used in the esterification reaction as needed. Examples of known esterification catalysts include manganese acetate, dibutyltin oxide, stannous oxalate, zinc acetate, and cobalt acetate. Esterification catalysts may be used alone or in combination of two or more.
[0032] To increase molecular weight by improving the reaction rate, it is preferable that the equivalent amount of hydroxyl groups of the polyhydric alcohol be in the range of 0.9 to 1.2 relative to the total amount of carboxyl groups of the unsaturated polybasic acid and any saturated polybasic acid.
[0033] (A) The content of (A-1) unsaturated polyester resin in the thermosetting resin is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the content of (A-1) unsaturated polyester resin is 75% by mass or more, appropriate fluidity and curing shrinkage can be ensured, and moldability tends to be further improved. (A) There is no particular upper limit to the content of (A-1) unsaturated polyester resin in the thermosetting resin. For example, it may be 100% by mass or less, 97% by mass or less, or 95% by mass or less.
[0034] <(A-2) Vinyl Ester Resin> (A-2) vinyl ester resin is generally a compound having an ethylenically unsaturated bond, obtained by a ring-opening reaction between (a) an epoxy group in an epoxy compound having two or more epoxy groups and (b) a carboxyl group of an unsaturated monobasic acid having an ethylenically unsaturated bond and a carboxyl group. (A-2) vinyl ester resin is described in, for example, the Polyester Resin Handbook (Nikkan Kogyo Shimbun, published in 1988).
[0035] (A-2) Vinyl ester resin may be used alone or in combination of two or more types. (A-2) Vinyl ester resin is generally used diluted with (B) ethylenically unsaturated monomer for ease of handling. (A-2) By using vinyl ester resin, the material cost of the thermosetting resin composition can be reduced.
[0036] (A-2) The weight-average molecular weight (Mw) of the vinyl ester resin can be adjusted according to the desired physical properties, but from a handling standpoint, a range of 500 to 5,000 is preferred.
[0037] (a) Epoxy compound (a) The epoxy compound is not particularly limited as long as it is a compound having two or more epoxy groups. Preferably, it is one or more selected from the group consisting of bisphenol-type epoxy compounds and novolacphenol-type epoxy compounds, and more preferably a bisphenol-type epoxy compound. (a) By using a vinyl ester resin that uses an epoxy compound as a raw material, the mechanical strength and corrosion resistance of the cured product tend to improve.
[0038] Examples of bisphenol-type epoxy compounds include those obtained by reacting bisphenol compounds such as bisphenol A, bisphenol F, bisphenol S, and tetrabromobisphenol A with epichlorohydrin and / or methylepichlorohydrin; and those obtained by reacting a compound obtained by glycidyl etherifying one or more of the above bisphenol compounds with a condensate of one or more of the above bisphenol compounds with epichlorohydrin and / or methylepichlorohydrin. From the viewpoint of durability, the reaction product of a bisphenol compound and epichlorohydrin is preferred, and the reaction product of bisphenol A and epichlorohydrin is more preferred.
[0039] Examples of novolac phenol-type epoxy compounds include those obtained by reacting phenol novolac or cresol novolac with epichlorohydrin and / or methyl epichlorohydrin.
[0040] (b) Unsaturated monobasic acid (b) The unsaturated monobasic acid is not particularly limited as long as it is a monocarboxylic acid having an ethylenically unsaturated bond. Preferably, it is methacrylic acid, acrylic acid, crotonic acid, cinnamic acid, etc., more preferably acrylic acid or methacrylic acid, and even more preferably methacrylic acid from the viewpoint of corrosion resistance of the cured product.
[0041] ((A-2) Method for synthesizing vinyl ester resin) (A-2) vinyl ester resin can be synthesized by known synthesis methods. For example, one method involves adding (b) an unsaturated monobasic acid in the presence of an esterification catalyst and (a) an epoxy compound in a heat-stirred reaction vessel and reacting at 70 to 150°C, preferably 80 to 140°C, and more preferably 90 to 130°C.
[0042] As esterification catalysts, known catalysts such as triethylamine, N,N-dimethylbenzylamine, N,N-dimethylaniline, diazabicyclooctane, triphenylphosphine, and diethylamine hydrochloride can be used.
[0043] (a) The mixing ratio of the epoxy compound and (b) the unsaturated monobasic acid is preferably such that the total amount of carboxyl groups of (b) the unsaturated monobasic acid is 0.3 to 1.2 moles, more preferably 0.4 to 1.1 moles, and even more preferably 0.5 to 1.0 moles, for every 1 mole of epoxy groups of (a) the epoxy compound. When the total amount of carboxyl groups of (b) the unsaturated monobasic acid is 0.3 moles or more, there is a tendency to obtain a cured product with sufficient hardness when the thermosetting resin composition is cured. On the other hand, when the total amount of carboxyl groups of (b) the unsaturated monobasic acid is 1.2 moles or less, the amount of unreacted (b) unsaturated monobasic acid can be reduced when synthesizing (A-2) vinyl ester resin, so there is a tendency to obtain a cured product with excellent mechanical strength.
[0044] When a thermosetting resin composition is heat-cured, unreacted (b) unsaturated monobasic acid may volatilize; therefore, the content of unreacted (b) unsaturated monobasic acid should be reduced as much as possible. For example, the content of unreacted (b) unsaturated monobasic acid relative to the total amount of (A-2) vinyl ester resin and unreacted (b) unsaturated monobasic acid is preferably 5% by mass or less, and more preferably 3% by mass or less.
[0045] (A) The content of (A-2) vinyl ester resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (A) There is no particular upper limit to the content of (A-2) vinyl ester resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.
[0046] <(A-3) Urethane (meth)acrylate resin> Examples of (A-3) urethane (meth)acrylate resins include resins obtained by introducing (meth)acryloyl groups to the hydroxyl groups or isocyanate groups at both ends of polyurethane obtained by reacting a polyhydric isocyanate with a polyhydric alcohol.
[0047] As the polyhydric alcohol, any of the compounds listed above as raw materials for (A-1) unsaturated polyester resins can be used without particular limitation.
[0048] Examples of polyvalent isocyanates include aliphatic polyvalent isocyanates such as hexamethylene diisocyanate, lysine diisocyanate, lysine triisocyanate, and trimethylhexane diisocyanate; cyclic aliphatic polyvalent isocyanates such as hydrogenated xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4 (or 2,6)-diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,3-(isocyanatomethyl)cyclohexane; aromatic polyvalent isocyanates such as tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, and triphenylmethane triisocyanate; and adducts, isocyanurates, and biuret derivatives of these polyvalent isocyanates. Polyvalent isocyanates may be used alone or in combination of two or more.
[0049] When introducing a (meth)acryloyl group, for example, a method of reacting a hydroxyl group-containing (meth)acrylic compound with a terminal isocyanate group, or a method of reacting an isocyanate group-containing (meth)acrylic compound with a terminal hydroxyl group can be used. Examples of hydroxyl group-containing (meth)acrylic compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxyalkyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, tris(hydroxyethyl)isocyanurate di(meth)acrylate, pentaestritol tri(meth)acrylate, glycerin mono(meth)acrylate, and hydroxyethylacrylamide, with 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, caprolactone-modified hydroxyalkyl (meth)acrylate, and hydroxyethylacrylamide being preferred. Examples of isocyanate group-containing (meth)acrylic compounds include 2-(meth)acryloyloxyethyl isocyanate, 2-(meth)acryloyloxypropyl isocyanate, and 1,1-bis(acryloyloxymethyl)ethyl isocyanate. The isocyanate group-containing (meth)acrylic compounds and the hydroxyl group-containing (meth)acrylic compounds may be used individually or in combination of two or more types.
[0050] (A) The content of (A-3) urethane (meth)acrylate resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (A) There is no particular upper limit to the content of (A-3) urethane (meth)acrylate resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.
[0051] <(A-4) Diallylphthalate Resin> (A-4) Diallylphthalate resin is an oligomer of diallylphthalate, and conventionally known types can be used without particular restriction. (A-4) Diallylphthalate resin may be used alone or in combination of two or more types.
[0052] (A) The content of (A-4) diallyl phthalate resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (A) There is no particular upper limit to the content of (A-4) diallyl phthalate resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.
[0053] <(A-5) Epoxy Resin> As the (A-5) epoxy resin, the compounds described in section (a) epoxy compounds of (A-2) vinyl ester resin can be used. The (A-5) epoxy resin may be used alone or in combination of two or more types.
[0054] (A) The content of epoxy resin (A-5) in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (A) There is no particular upper limit to the content of epoxy resin (A-5) in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.
[0055] [(B) Ethylene-unsaturated monomers] (B) Ethylene-unsaturated monomers are not particularly limited as long as they are monomers having an ethylenically unsaturated bond. (B) Ethylene-unsaturated monomers may be used alone or in combination of two or more types.
[0056] Specific examples include vinyl compounds such as styrene, vinyltoluene, t-butylstyrene, methoxystyrene, divinylbenzene, and vinylnaphthalene; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, furfuryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate. Examples of (meth)acrylates include acrylates such as acetates, phenoxyethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, allyl (meth)acrylate, isobornyl (meth)acrylate, acetoacetoxyethyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecanol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.; and cyclic unsaturated compounds such as acenaphthylene and norbornene. (A) From the viewpoint of copolymerization with thermosetting resins, vinyl compounds are preferred, more preferably one or more selected from styrene, vinyltoluene, t-butylstyrene, and methoxystyrene, and even more preferably styrene.
[0057] The content of (B) ethylenically unsaturated monomer in the thermosetting resin composition is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 60 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. The content of (B) ethylenically unsaturated monomer in the thermosetting resin composition is preferably 95 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 80 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. When the content of (B) ethylenically unsaturated monomer in the thermosetting resin composition is 20 parts by mass or more, the viscosity of the thermosetting resin composition can be adjusted to an appropriate range, and the moldability tends to be better. When the content of (B) ethylenically unsaturated monomer in the thermosetting resin composition is 95 parts by mass or less, the mechanical strength of the cured product tends to be good.
[0058] [(C) Thermal polymerization initiator] (C) The thermal polymerization initiator is not particularly limited as long as it is a polymerization initiator that generates radicals upon heating. Examples include organic peroxides such as diacyl peroxide, peroxyester, hydroperoxide, dialkyl peroxide, ketone peroxide, peroxyketal, alkyl perester, and parkervonate.
[0059] (C) Among these organic peroxides, 1,1-di-t-hexylperoxycyclohexane, t-hexylperoxyisopropyl carbonate, t-butylperoxyoctoate, t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, t-amylperoxy-2-ethylhexanoate, benzoyl peroxide, 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, t-butylperoxyisopropyl carbonate, t-butylperoxybenzoate, dicumyl peroxide, and di-t-butyl peroxide are preferred as thermal polymerization initiators. (C) The thermal polymerization initiators may be used alone or in combination of two or more.
[0060] The content of (C) thermal polymerization initiator in the thermosetting resin composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 3 parts by mass or more, and particularly preferably 5 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. The content of (C) thermal polymerization initiator in the thermosetting resin composition is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. When the content of (C) thermal polymerization initiator in the thermosetting resin composition is 0.5 parts by mass or more, the curing reaction during molding of the thermosetting resin composition tends to proceed uniformly, and the physical properties and appearance of the cured product tend to be good. When the content of (C) thermal polymerization initiator in the thermosetting resin composition is 20 parts by mass or less, the storage stability of the thermosetting resin composition tends to be better, and the handling properties tend to be improved.
[0061] [(D) Polymerization Inhibitor] The (D) polymerization inhibitor contains at least the (D-1) polymerization inhibitor and the (D-2) polymerization inhibitor. The (D-1) polymerization inhibitor may be used alone or in combination of two or more types. The (D-2) polymerization inhibitor may be used alone or in combination of two or more types.
[0062] The mass ratio of the polymerization inhibitor (D-1) to the polymerization inhibitor (D-2) is 99:1 to 80:20, preferably 99:1 to 90:10, and more preferably 99:1 to 95:5. Within this range, it is possible to ensure moldability while further reducing the change in the fluidity of the resin composition from the time the thermosetting resin composition is put into the molding machine until it is filled into the mold.
[0063] (D-1) The polymerization inhibitor is a hindered phenol. The hindered phenol refers to an aromatic compound having a phenolic hydroxyl group, which has a substituent that provides steric hindrance at the ortho position relative to the phenolic hydroxyl group. In the present disclosure, when a compound falls under both a hindered phenol and a polyhydric phenol compound to be described later, the compound is classified as a polyhydric phenol compound. The hindered phenol is preferably a compound represented by the following formula (1). (In formula (1), R 1 to R 3 each independently represent an alkyl group having 1 to 5 carbon atoms.)
[0064] R 1 to R 3 The alkyl group having 1 to 5 carbon atoms may be a linear alkyl group or a branched alkyl group. In a preferred embodiment, R 1 is a linear alkyl group, and R 2 and R 3 are branched alkyl groups. R 1 is preferably a methyl group, an ethyl group, or a propyl group. R 2 and R 3 At least one of them is preferably an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an isopentyl group, a 3-methylbutyl group, a sec-pentyl group, a tert-pentyl group, or a neopentyl group, and more preferably a tert-butyl group, a tert-pentyl group, or a neopentyl group. R 2 and R 3 each independently are preferably an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an isopentyl group, a 3-methylbutyl group, a sec-pentyl group, a tert-pentyl group, or a neopentyl group, and more preferably a tert-butyl group, a tert-pentyl group, or a neopentyl group.
[0065] Examples of hindered phenols include 2,6-di-tert-butyl-4-methylphenol (BHT), represented by the following chemical formula, and 2,2-methylene-bis-(4-methyl-6-tert-butylphenol), with 2,6-di-tert-butyl-4-methylphenol being preferred.
[0066] (D-2) The polymerization inhibitor is one or more selected from the group consisting of phenothiazine compounds, quinone compounds, and polyhydric phenol compounds. From the viewpoint of minimizing the change in the fluidity of the resin composition from the time the thermosetting resin composition is put into the molding machine until it is filled into the mold, phenothiazine compounds are preferred. From the viewpoint of not adversely affecting moldability, one or more selected from the group consisting of quinone compounds and polyhydric phenol compounds are preferred. From the viewpoint of extending the pot life of the thermosetting resin composition, it is also preferable to use two or more of the phenothiazine compounds, quinone compounds, and polyhydric phenol compounds. A combination of a phenothiazine compound and a quinone compound, a combination of a phenothiazine compound and a polyhydric phenol compound, and a combination of a quinone compound and a polyhydric phenol compound are preferred, and a combination of a phenothiazine compound and a quinone compound is more preferred.
[0067] Phenothiazine compounds are compounds having a phenothiazine skeleton. Phenothiazine compounds are preferably compounds represented by the following formula (2). (In formula (2), R 4 ~R 11 Each of these is independently a hydrogen atom, a hydroxyl group, a halogen atom, an alkyl group, an acyl group, an aryl group, an alkoxy group, an aralkyl group, an alkoxyalkyl group, an amino group, an alkylamino group, a glycidyl group, a hydroxyalkyl group, or an aryloxyalkyl group.
[0068] Examples of phenothiazine compounds include phenothiazine, 1,2-bis-(α-methylbenzyl)-10H-phenothiazine, 3,7-dioctylbenzylphenothiazine, and 2,4-bis-(α-dimethylbenzyl)-10H-phenothiazine, with phenothiazine being preferred.
[0069] In this disclosure, a polyhydric phenol compound is not a phenothiazine compound and is a compound having one or more hydroxyl groups bonded to a benzene ring, and a total of two or more hydroxyl and alkoxy groups bonded to the benzene ring. A polyhydric phenol compound preferably has two to three hydroxyl groups bonded to a benzene ring, more preferably two. A polyhydric phenol compound is preferably a compound represented by the following formula (3). (In formula (3), R 12 ~R 16 Each of these is independently either a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.
[0070] R 12 ~R 16 The alkyl group having 1 to 5 carbon atoms may be a linear alkyl group or a branched alkyl group. In one preferred embodiment, R 16 R is a hydrogen atom or a linear alkyl group, 12 ~R 15 Each of these is independently a hydrogen atom, a linear alkyl group, or a branched alkyl group. 16 R is preferably a hydrogen atom or a linear alkyl group having 1 to 5 carbon atoms, more preferably a hydrogen atom or a linear alkyl group having 1 to 3 carbon atoms, and even more preferably a hydrogen atom, a methyl group, or an ethyl group. 12 ~R 15 Each of these is preferably independently a hydrogen atom, a linear alkyl group having 1 to 5 carbon atoms, or a branched alkyl group having 3 to 5 carbon atoms, and more preferably a hydrogen atom, a methyl group, an ethyl group, or a tert-butyl group.
[0071] Examples of polyhydric phenol compounds include hydroquinone, hydroquinone monomethyl ether, hydroquinone monoethyl ether, trimethylhydroquinone, t-butylhydroquinone, butylhydroxyanisole, catechol, p-t-butylcatechol, and pyrogallol, with hydroquinone being preferred.
[0072] Quinone compounds are cyclic compounds having two ketone structures. Examples of quinone compounds include benzoquinone compounds such as p-benzoquinone, t-butylquinone, and tetrachloro-1,4-benzoquinone, and naphthoquinone compounds such as 1,4-naphthoquinone. Quinone compounds are preferably compounds represented by the following formula (4). (In formula (4), R 17 ~R 20 Each of these is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogen atom.
[0073] R 17 ~R 20 The alkyl group having 1 to 5 carbon atoms may be a linear alkyl group or a branched alkyl group. 17 ~R 20 Each of these is preferably independently a hydrogen atom, a methyl group, an ethyl group, or a propyl group, more preferably a hydrogen atom or a methyl group, and even more preferably a hydrogen atom.
[0074] The content of the (D-1) polymerization inhibitor in the thermosetting resin composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 0.8 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. From the viewpoint of further improving the fluidity change of the resin composition from the time the thermosetting resin composition is put into the molding machine until it is filled into the mold, it may be 1.5 parts by mass or more. The content of the (D-1) polymerization inhibitor in the thermosetting resin composition is preferably 3.0 parts by mass or less, more preferably 2.0 parts by mass or less, even more preferably 1.5 parts by mass or less, and particularly preferably 1.0 part by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. When the content of the (D-1) polymerization inhibitor in the thermosetting resin composition is 0.1 parts by mass or more, the pot life of the thermosetting resin composition tends to be further improved. When the content of the (D-1) polymerization inhibitor in the thermosetting resin composition is 3.0 parts by mass or less, molding defects tend to be further reduced.
[0075] The content of the (D-2) polymerization inhibitor in the thermosetting resin composition is preferably 0.005 parts by mass or more, more preferably 0.010 parts by mass or more, and even more preferably 0.030 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. From the viewpoint of further reducing the total content of (D) polymerization inhibitor by reducing the content of (D-1) polymerization inhibitor, the content of (D-2) polymerization inhibitor may be 0.060 parts by mass or more. The content of the (D-2) polymerization inhibitor in the thermosetting resin composition is preferably 0.30 parts by mass or less, more preferably 0.20 parts by mass or less, even more preferably 0.15 parts by mass or less, and particularly preferably 0.10 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. When the content of (D-2) polymerization inhibitor in the thermosetting resin composition is 0.005 parts by mass or more, the pot life of the thermosetting resin composition tends to be further improved. When the content of (D-2) polymerization inhibitor in the thermosetting resin composition is 0.30 parts by mass or less, molding defects tend to be further reduced.
[0076] (D) The polymerization inhibitor may contain other polymerization inhibitors other than the polymerization inhibitors (D-1) and (D-2), as long as the effect is not impaired. From the viewpoint of further reducing molding defects, it is desirable to reduce the total content of the polymerization inhibitors (D) as much as possible. From this viewpoint, the content of other polymerization inhibitors in the thermosetting resin composition is preferably 3 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.1 parts by mass or less, based on 100 parts by mass of the total amount of the thermosetting resin (A) and the ethylenically unsaturated monomer (B). In one embodiment, the thermosetting resin composition does not contain other polymerization inhibitors.
[0077] [(E) Low-Shrinkage Agent] The thermosetting resin composition may optionally contain (E) a low-shrinkage agent. The (E) low-shrinkage agent is not particularly limited and any known in the art of the present invention can be used. Thermoplastic resins are preferred as the (E) low-shrinkage agent. Examples of (E) low-shrinkage agents include saturated polyester resin, polystyrene, polyethylene, polymethyl methacrylate, polyvinyl acetate, polycaprolactone, styrene-butadiene rubber, styrene-butadiene-styrene rubber (SBS), and styrene-ethylene-butadiene-styrene rubber (SEBS). Among these, saturated polyester resin is preferred from the viewpoint of reducing the shrinkage rate of the cured product, moldability, and crack resistance. Polystyrene is preferred from the viewpoint of reducing the shrinkage rate of the cured product. Styrene-butadiene rubber (SBR), styrene-butadiene-styrene rubber (SBS), and styrene-ethylene-butadiene-styrene rubber (SEBS) are preferred from the viewpoint of reducing the shrinkage rate of the cured product, fluidity, and filling properties during molding. The (E) low-shrinkage agent may be used alone or in combination of two or more types.
[0078] The content of (E) low shrinkage agent in the thermosetting resin composition may be 10 parts by mass or more, 20 parts by mass or more, or 30 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. The content of (E) other low shrinkage agent in the thermosetting resin composition may be 60 parts by mass or less, 50 parts by mass or less, or 45 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. If the content of (E) low shrinkage agent in the thermosetting resin composition is 10 parts by mass or more, the shrinkage rate of the cured product tends to be small, and the desired dimensional accuracy can be obtained in the molded product. If the content of (E) low shrinkage agent in the thermosetting resin composition is 60 parts by mass or less, the moldability of the thermosetting resin composition and the mechanical properties of the cured product tend to be better.
[0079] Saturated polyester resins are polycondensates of polyhydric alcohols and saturated polybasic acids. Preferably, saturated polyester resins are polycondensates of diols and saturated polybasic acids. In one embodiment, the saturated polyester resin contains a structure derived from an aromatic saturated polybasic acid or its acid anhydride and a structure derived from an aliphatic saturated polybasic acid.
[0080] (A) Saturated polyester resin may be used alone or in combination of two or more types.
[0081] In this disclosure, styrene monomers and the like contained in commercially available saturated polyester resins are classified as (B) ethylenically unsaturated monomers.
[0082] The polyhydric alcohol is not particularly limited as long as it is a compound having two or more hydroxyl groups. The polyhydric alcohol is preferably one or more selected from the group consisting of diols and triols, and more preferably a diol. Examples of polyhydric alcohols include alkylene glycols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, and hydrogenated bisphenol A; polyoxyalkylene polyols such as diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol; bisphenol A; alkylene oxide-modified bisphenol A such as ethylene oxide adducts of bisphenol A and propylene oxide adducts of bisphenol A; and glycerin. From the viewpoint of crack resistance during molding, one or more selected from the group consisting of alkylene glycol and polyoxyalkylene polyol is preferred, polyoxyalkylene glycol is more preferred, and one or more selected from diethylene glycol, dipropylene glycol, and triethylene glycol is even more preferred. In particular, from the viewpoint of improving the durability of the molded article, it is preferable to use polyoxyethylene glycol and polyoxypropylene glycol in combination, and it is even more preferable to use diethylene glycol and dipropylene glycol in combination. The content ratio (molar ratio) of polyoxyethylene glycol to polyoxypropylene glycol or the content ratio (molar ratio) of diethylene glycol to dipropylene glycol is not particularly limited, but from the viewpoint of improving durability, 40:60 to 80:20 is preferred, 50:50 to 70:30 is more preferred, 55:45 to 65:35 is even more preferred, and 58:42 to 63:37 is particularly preferred. The polyhydric alcohol may be used alone or in combination of two or more.
[0083] The saturated polybasic acid is not particularly limited as long as it does not have an ethylenically unsaturated bond and has two or more carboxyl groups, or is an acid anhydride thereof; known compounds can be used. The saturated polybasic acid is preferably a saturated dibasic acid. Examples of saturated polybasic acids include aromatic saturated polybasic acids or their acid anhydrides such as phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, tetrachlorophthalic anhydride, tetrabromophthalic anhydride, nitrophthalic acid, and halogenated phthalic anhydride; aliphatic saturated polybasic acids such as succinic acid, adipic acid, sebacic acid, oxalic acid, malonic acid, azelaic acid, and glutaric acid; and acid anhydrides of cyclic aliphatic saturated polybasic acids such as hexahydrophthalic anhydride. As the aromatic saturated polybasic acid or its acid anhydride, one or more selected from the group consisting of aromatic saturated dibasic acids and their acid anhydrides are preferred, one or more selected from phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid are more preferred, and one or more selected from isophthalic acid and terephthalic acid are even more preferred. As the aliphatic saturated polybasic acid, an aliphatic saturated dibasic acid is preferred, an aliphatic saturated dibasic acid having 4 to 10 carbon atoms is more preferred, and one or more selected from succinic acid, adipic acid, and sebacic acid are even more preferred. From the viewpoint of crack resistance during molding, it is preferred to use one or more selected from the group consisting of aromatic saturated polybasic acids, their acid anhydrides, and aliphatic saturated polybasic acids, it is more preferred to use an aromatic saturated polybasic acid or its acid anhydride in combination with an aliphatic saturated polybasic acid, and it is even more preferred to use one or more selected from isophthalic acid and terephthalic acid in combination with one or more selected from succinic acid, adipic acid, and sebacic acid. Saturated polybasic acids may be used alone or in combination of two or more types.
[0084] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aromatic saturated polybasic acid or its acid anhydride to the total is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more. When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aromatic saturated polybasic acid or its acid anhydride to the total is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less. When the proportion of the aromatic saturated polybasic acid or its acid anhydride is within the above range, the moldability tends to be better and the properties of the cured product tend to be improved.
[0085] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aliphatic saturated polybasic acid to the total is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more. When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aliphatic saturated polybasic acid to the total is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less. If the proportion of the aliphatic saturated polybasic acid is within the above range, crack resistance tends to be further improved.
[0086] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the molar ratio of the structure derived from the aromatic saturated polybasic acid or its acid anhydride to the structure derived from the aliphatic saturated polybasic acid in the saturated polyester resin is preferably 20:80 to 80:20, more preferably 30:70 to 70:30, and even more preferably 40:60 to 60:40.
[0087] Preferred combinations of polyhydric alcohols and saturated polybasic acids include diols and saturated dibasic acids, and more preferably polyoxyalkylene glycols and saturated dibasic acids. More specifically, examples include combinations of diethylene glycol and isophthalic acid, diethylene glycol and adipic acid, dipropylene glycol and isophthalic acid, dipropylene glycol and adipic acid, diethylene glycol, isophthalic acid and adipic acid, dipropylene glycol, isophthalic acid and adipic acid, and diethylene glycol, dipropylene glycol, isophthalic acid and adipic acid. Among these, the combinations of diethylene glycol, isophthalic acid and adipic acid, dipropylene glycol, isophthalic acid and adipic acid, and diethylene glycol, dipropylene glycol, isophthalic acid and adipic acid are preferred because they exhibit good crack resistance during molding.
[0088] The weight-average molecular weight of the saturated polyester resin is preferably 9500 or more, more preferably 9800 or more, and even more preferably 10000 or more. The weight-average molecular weight of the saturated polyester resin is preferably 13500 or less, more preferably 13000 or less, and even more preferably 12500 or less. When the weight-average molecular weight is within the above range, crack formation during molding tends to be suppressed. Although not bound by any particular theory, it is believed that setting the weight-average molecular weight of the saturated polyester resin within the above range improves (A) compatibility with thermosetting resins and dispersibility of other components, thereby suppressing crack formation during molding. The weight-average molecular weight of the saturated polyester resin can be adjusted by the reaction time when synthesizing the saturated polyester resin. Specifically, the longer the reaction time, the larger the weight-average molecular weight, and the shorter the reaction time, the smaller the weight-average molecular weight.
[0089] (Method for synthesizing saturated polyester resin) Saturated polyester resin can be synthesized using the above raw materials by known methods. Various conditions in the synthesis of saturated polyester resin are set appropriately according to the raw materials used and their quantities.
[0090] Generally, esterification reactions can be carried out under pressure or reduced pressure at a temperature of 140°C to 230°C in an inert gas stream such as nitrogen gas. Esterification catalysts can be used in the esterification reaction as needed. Examples of known esterification catalysts include manganese acetate, dibutyltin oxide, stannous oxalate, zinc acetate, and cobalt acetate. Esterification catalysts may be used alone or in combination of two or more.
[0091] It is preferable that the equivalent amount of hydroxyl groups in the polyhydric alcohol be in the range of 0.9 to 1.2 relative to the total amount of carboxyl groups in the saturated polybasic acid.
[0092] [(F) Glass Fibers] The thermosetting resin composition may optionally contain (F) glass fibers. (F) glass fibers are not particularly limited as long as they are fibrous materials with an aspect ratio of 3 or more. Specifically, examples include chopped strand glass.
[0093] (F) The fiber length of the glass fibers is preferably 20 mm or less, more preferably 10 mm or less, and even more preferably 5 mm or less. When the fiber length is 20 mm or less, the moldability of the thermosetting resin composition tends to be better and the appearance of the cured product tends to be better. The fiber length is preferably 0.1 mm or more, more preferably 0.5 mm or more, and even more preferably 1 mm or more. When the fiber length is 0.1 mm or more, the strength of the cured product tends to be good. (F) The average fiber diameter of the glass fibers is preferably 3 to 100 μm, and more preferably 5 to 30 μm.
[0094] The content of (F) glass fibers in the thermosetting resin composition is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 40 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. The content of (F) glass fibers in the thermosetting resin composition is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 100 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. If the content of (F) glass fibers in the thermosetting resin composition is 5 parts by mass or more, the mechanical properties of the cured product obtained from the thermosetting resin composition tend to be better. If the content of (F) glass fibers in the thermosetting resin composition is 200 parts by mass or less, the (F) glass fibers tend to be more uniformly dispersed in the thermosetting resin composition, and a homogeneous cured product can be produced.
[0095] [(G) Inorganic Filler] The thermosetting resin composition may optionally contain (G) an inorganic filler. As (G) an inorganic filler, particulate matter known in the art of the present invention can be used. By using (G) an inorganic filler, the molding shrinkage rate of the molded product can be reduced, the viscosity of the thermosetting resin composition can be adjusted to improve workability, or the strength of the molded product can be improved.
[0096] (G) Examples of inorganic fillers include calcium carbonate, silica, aluminum oxide, aluminum hydroxide, barium sulfate, calcium sulfate, calcium oxide, calcium hydroxide, wollastonite, clay, kaolin, mica, gypsum, anhydrous silicic acid, and glass powder. Calcium carbonate, aluminum oxide, and aluminum hydroxide are preferred because they are inexpensive. (G) Inorganic fillers may be used individually or in combination of two or more types.
[0097] (G) The average particle size of the inorganic filler is preferably 1 to 100 μm, more preferably 1 to 60 μm, and even more preferably 1 to 50 μm. (G) If the average particle size of the inorganic filler is 1 μm or more, particle aggregation tends to be suppressed. On the other hand, (G) if the average particle size of the inorganic filler is 100 μm or less, the moldability of the thermosetting resin composition tends to be better.
[0098] In this specification, "average particle size" refers to the 50% particle size (D50) in the volume-based cumulative particle size distribution measured by a laser diffraction / scattering particle size distribution analyzer (Microtrac-Bell Co., Ltd., FRA).
[0099] (G) The shape of the inorganic filler is not particularly limited. Examples include a nearly perfect sphere, ellipsoid, flake-like shape, amorphous shape, etc.
[0100] The content of (G) inorganic filler in the thermosetting resin composition is preferably 50 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 200 parts by mass or more, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. The content of (G) inorganic filler in the thermosetting resin composition is preferably 1000 parts by mass or less, more preferably 800 parts by mass or less, and even more preferably 600 parts by mass or less, based on 100 parts by mass of the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer. If the content of (G) inorganic filler in the thermosetting resin composition is 50 parts by mass or more, the mechanical properties of the cured product tend to be better. If the content of (G) inorganic filler in the thermosetting resin composition is 1000 parts by mass or less, the (G) inorganic filler tends to be more uniformly dispersed in the thermosetting resin composition, and a homogeneous cured product can be produced.
[0101] [(H) Release Agent] The thermosetting resin composition may optionally contain a (H) release agent. The (H) release agent is not particularly limited and any known in the art of the present invention can be used. Examples of (H) release agents include stearic acid, oleic acid, zinc stearate, calcium stearate, aluminum stearate, magnesium stearate, stearate amide, oleic acid amide, silicone oil, synthetic wax, etc. The (H) release agent may be used alone or in combination of two or more types.
[0102] (H) When a release agent is used, the content is preferably 1 to 40 parts by mass, more preferably 5 to 30 parts by mass, and even more preferably 8 to 20 parts by mass, per 100 parts by mass of (A) thermosetting resin. If the content of (H) the release agent is 1 part by mass or more, the release properties of the cured product after molding tend to be good, and the productivity of the product tends to be good. On the other hand, if the content of (H) the release agent is 40 parts by mass or less, there is a tendency to be a cured product with a good appearance without excessive release agent contaminating the surface of the cured product.
[0103] [Other Additives] In addition to the above components, the thermosetting resin composition may contain components known in the art of the present invention, such as viscosity reducers, colorants, and molding aids, to the extent that they do not impede the effects of the present invention.
[0104] Colorants are used to color cured products, etc. Examples of colorants include various dyes, inorganic pigments, and organic pigments. Colorants may be used alone or in combination of two or more. The amount of colorant can be adjusted as appropriate depending on the desired degree of coloring of the cured product.
[0105] <Method for producing thermosetting resin compositions> Thermosetting resin compositions can be produced by mixing (A) a thermosetting resin, (B) an ethylenically unsaturated monomer, (C) a thermal polymerization initiator, and (D) a polymerization inhibitor with optional components such as (E) a low shrinkage agent, (F) glass fibers, (G) an inorganic filler, (H) a mold release agent, and other additives as needed.
[0106] Mixing methods include, for example, kneading. There are no particular restrictions on the kneading method, and for example, a kneader, disper, planetary mixer, etc., can be used. The kneading temperature is preferably 5°C to 50°C, and more preferably 10°C to 40°C.
[0107] There are no particular restrictions on the order in which the components are mixed when manufacturing a thermosetting resin composition. For example, it is preferable to mix (A) the thermosetting resin and (B) some or all of the ethylenically unsaturated monomer before mixing the other components, as this makes it easier to obtain a thermosetting resin composition in which each component is sufficiently dispersed or uniformly mixed. At least a portion of (B) the ethylenically unsaturated monomer may be pre-mixed with (A) the thermosetting resin so as to act as a solvent, dispersion medium, etc.
[0108] Thermosetting resin compositions are suitable for use as molding materials because they have an improved pot life. Preferred molding methods include, for example, transfer molding and injection molding. Thermoplastic resin compositions are also suitable for use as sealing materials for electronic devices and the like.
[0109] <Cured Product> In one embodiment, the cured product is a cured product of a thermosetting resin composition. The cured product can be used as a molding material to cover the stator that constitutes the motor.
[0110] <Method for producing cured products> Cured products can be produced by heating and curing a thermosetting resin composition. The conditions for curing the thermosetting resin composition can be appropriately set depending on the materials used and the decomposition temperature of the (C) thermal polymerization initiator. An example of preferred conditions is a temperature of 120 to 180°C, more preferably 120 to 160°C and a curing time of 1 to 30 minutes.
[0111] <Motor> A motor is a device that generates an electromagnetic force by energizing an internal coil, and generates rotational force through the repulsive or attractive force between the motor and a permanent magnet or electromagnet provided on or around the main shaft. Generally, a motor comprises a stator having a stator core and coils wound around the stator core, and a rotating body containing magnetic components. In motors, those in which the stator is covered with a molding material are also called molded motors. In this specification, a stator covered with a molding material will be referred to as a molded stator.
[0112] A motor in one embodiment includes a molded stator; a rotor located inside the stator, having a rotating shaft extending in the axial direction and a rotating body containing a magnetic component that extends in the axial direction and is fixed to the rotating shaft; and a bearing that rotatably supports the rotor.
[0113] In one embodiment of the motor, the molding material constituting the molded stator is a cured product of a thermosetting resin composition. In the motor, components other than the molding material can be those of known origin.
[0114] Figure 1 shows a cross-sectional view of an exemplary motor. In Figure 1, detailed parts such as brackets and insulators attached to the coils are omitted. In Figure 1, the motor 10 has a stator 11, a rotor 15, and a bearing 19 that rotatably supports the rotor 15. The stator 11 has a stator core 12 made up of a plurality of metal plates and a coil 13 with windings wound around the stator core 12. The stator 11 is covered with a molding material 14. The rotor 15 is located inside the stator 11. The rotor 15 has a rotating shaft 17 extending in the axial direction and a rotating body 18 fixed to this rotating shaft 17, and this rotating body 18 includes a magnet 16.
[0115] <Molded Stator> A molded stator according to one embodiment includes a stator having a stator core and coils wound around the stator core, and a molding material covering the stator. It is not necessary for the entire stator to be covered with the molding material.
[0116] The molding material constituting the molded stator is a cured product of a thermosetting resin composition. In the molded stator, components other than the molding material can be those of known origin. The motor to which the molded stator is applied is not particularly limited and can be any known motor.
[0117] <Method for Manufacturing a Molded Stator> A molded stator can be manufactured, for example, by injecting a thermosetting resin composition into a mold in which the stator is positioned and heating it. The molding method is not particularly limited and can be any method commonly used in the art of the present invention, such as transfer molding and injection molding.
[0118] More specific methods for manufacturing molded stators include, for example, opening the mold, pouring a thermosetting resin composition into the mold containing the stator, and allowing it to harden; and injecting a thermosetting resin composition from the outside into a closed mold containing the stator through a hole in the mold, such as a sprue, under reduced pressure inside the mold, or under external pressure as in injection molding, and allowing it to harden. The conditions for hardening the thermosetting resin composition inside the mold can be appropriately set depending on the material used. An example of preferred conditions is a temperature of 120 to 180°C, more preferably 120 to 160°C, and a hardening time of 1 to 30 minutes.
[0119] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0120] The synthesis examples of the thermosetting resin (A) used in the examples and comparative examples are shown below.
[0121] The following raw materials were used: Diols: Propylene glycol (Fujifilm Wako Pure Chemical Corporation), Neopentyl glycol (Fujifilm Wako Pure Chemical Corporation) Unsaturated polybasic acid: Maleic anhydride (Fujifilm Wako Pure Chemical Corporation)
[0122] [Synthesis Example 1] (A) Synthesis of Thermosetting Resin In a four-necked flask equipped with a thermometer, stirrer, inert gas inlet, and reflux condenser, 100 moles of maleic anhydride, 60 moles of propylene glycol, and 40 moles of neopentyl glycol were charged. The mixture was heated and stirred under a nitrogen gas stream and the temperature was raised to 210°C to carry out the esterification reaction and obtain an unsaturated polyester resin. Subsequently, styrene monomer was added in an amount of 40% by mass relative to the total of the unsaturated polyester resin and styrene monomer to obtain a mixture of unsaturated polyester resin and styrene. The obtained unsaturated polyester resin had a degree of unsaturation of 100 mol% and a weight-average molecular weight (Mw) of 20,000.
[0123]
[0124] The synthesis examples of saturated polyester resins used in the examples and comparative examples are shown below.
[0125] The following raw materials were used: Diols: Diethylene glycol (Fujifilm Wako Pure Chemical Corporation), Dipropylene glycol (Fujifilm Wako Pure Chemical Corporation) Saturated polybasic acids: Isophthalic acid (Fujifilm Wako Pure Chemical Corporation), Adipic acid (Fujifilm Wako Pure Chemical Corporation)
[0126] [Synthesis Example 2] In a four-necked flask equipped with a thermometer, stirrer, inert gas inlet, and reflux condenser, 50 moles of isophthalic acid, 60 moles of diethylene glycol, and 40 moles of dipropylene glycol were charged. The esterification reaction was carried out by heating and stirring under a nitrogen gas stream to 210°C. When the acid value of the reaction solution fell below 10 KOH mg / g, 50 moles of adipic acid were added, and the esterification reaction was continued to obtain a saturated polyester resin. Subsequently, when the acid value of the reaction solution fell below 10 KOH mg / g, styrene monomer was added to the total of the saturated polyester resin and styrene monomer to 40% by mass, and a mixture of saturated polyester resin and styrene was obtained. The obtained saturated polyester resin had a weight-average molecular weight (Mw) of 10,000.
[0127]
[0128] Other ingredients used include the following:
[0129] (B) Ethylene-unsaturated monomers: Styrene (Idemitsu Kosan Co., Ltd.)
[0130] (C) Thermal polymerization initiator: Perhexyl I (t-hexyl peroxyisopropyl carbonate, NOF Corporation)
[0131] (D1) Polymerization inhibitor: 2,6-di-tert-butyl-4-methylphenol (Kyodo Pharmaceutical Co., Ltd.)
[0132] (D2) Polymerization inhibitors: • p-benzoquinone (Fujifilm Wako Pure Chemical Corporation) • phenothiazine (Fujifilm Wako Pure Chemical Corporation) • hydroquinone (Fujifilm Wako Pure Chemical Corporation)
[0133] (E) Low shrinkage agent: • Polystyrene (PS MS-200, Sekisui Chemical Co., Ltd.) • Styrene-butadiene rubber (Asahi Kasei Corporation)
[0134] (F) Glass fiber: Chopped strand ECS-03B173 / P9 (glass chop, fiber diameter 13 μm, fiber length 3.0 mm, Nippon Electric Glass Co., Ltd.)
[0135] (G) Inorganic filler: Aluminum hydroxide (average particle size 7 μm, Nippon Light Metal Co., Ltd.)
[0136] <Example 1> (Preparation of thermosetting resin composition) (A) thermosetting resin and (B) 58 parts by mass of a mixture of the unsaturated polyester resin obtained in Synthesis Example 1 and styrene as an ethylenically unsaturated monomer (35 parts by mass of unsaturated polyester resin, 23 parts by mass of styrene), (B) 32 parts by mass of a mixture of the saturated polyester resin obtained in Synthesis Example 2 and styrene as an ethylenically unsaturated monomer and (E) as a low shrinkage agent (19 parts by mass of saturated polyester resin, 13 parts by mass of styrene), (B) further 29 parts by mass of styrene as an ethylenically unsaturated monomer, (C) 9 parts by mass of perhexyl I as a thermal polymerization initiator, (D- 1) 0.9 parts by mass of 2,6-di-tert-butyl-4-methylphenol as a polymerization inhibitor, (D-2) 0.04 parts by mass of p-benzoquinone as a polymerization inhibitor, (E) 16 parts by mass of polystyrene as a low shrinkage agent, (E) 7 parts by mass of styrene-butadiene rubber as a low shrinkage agent, (F) 85 parts by mass of chopped strand ECS-03B173 / P9 as glass fiber, and (G) 430 parts by mass of aluminum hydroxide as an inorganic filler were put into a double-arm kneader and kneaded at 30°C for 30 minutes to prepare a thermosetting resin composition.
[0137] (Pot Life Evaluation) 50 g of the thermosetting resin composition was placed in a Supern bag, the air was removed, the opening of the bag was twisted shut to minimize exposure of the thermosetting resin composition to the outside air, and the bag was secured with a rubber band before being placed in a 50°C constant temperature bath. The sample was checked by squeezing the bag every 3 to 4 hours, and the time at which it was last confirmed that no hard granular clumps had formed was determined as the pot life. The results are shown in Table 3.
[0138] (Moldability Evaluation) Disc-shaped test specimens (φ90 mm × 10 mm) were molded by compression molding using a compression molding machine (Techno Marushichi Co., Ltd.) under the conditions of a molding temperature of 140°C, a molding pressure of 5 MPa, and a molding time of 90 seconds, and their appearance was examined. A specimen was evaluated as defective if blistering was observed, and as good if no blistering was observed. The results are shown in Table 3.
[0139]
[0140] <Examples 2-6, Comparative Examples 1-3> Thermosetting resin compositions were prepared in the same manner as in Example 1, except that the types and composition of raw materials were changed as shown in Table 3. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 3.
[0141] 10 Motor 11 Stator 12 Stator core 13 Coil 14 Molding material 15 Rotor 16 Magnet 17 Rotating shaft 18 Rotating body 19 Bearing
Claims
1. A thermosetting resin composition comprising (A) a thermosetting resin, (B) an ethylenically unsaturated monomer, (C) a thermal polymerization initiator, and (D) a polymerization inhibitor, wherein the (D) polymerization inhibitor comprises at least a (D-1) polymerization inhibitor and a (D-2) polymerization inhibitor, the (D-1) polymerization inhibitor is a hindered phenol, the (D-2) polymerization inhibitor is one or more selected from the group consisting of phenothiazine compounds, quinone compounds, and polyhydric phenol compounds, and the mass ratio of the (D-1) polymerization inhibitor to the (D-2) polymerization inhibitor is 99:1 to 80:
20.
2. The thermosetting resin composition according to claim 1, wherein the total amount of the (A) thermosetting resin and the (B) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 0.1 to 3.0 parts by mass of the (D-1) polymerization inhibitor and 0.005 to 0.30 parts by mass of the (D-2) polymerization inhibitor.
3. The thermosetting resin composition according to claim 1, wherein the hindered phenol is represented by the following formula (1). (In formula (1), R 1 ~R 3 Each of these is an alkyl group having 1 to 5 carbon atoms.
4. The thermosetting resin composition according to claim 1, wherein the phenothiazine compound is represented by the following formula (2). (In formula (2), R 4 ~R 11 Each of these is independently a hydrogen atom, a hydroxyl group, a halogen atom, an alkyl group, an acyl group, an aryl group, an alkoxy group, an aralkyl group, an alkoxyalkyl group, an amino group, an alkylamino group, a glycidyl group, a hydroxyalkyl group, or an aryloxyalkyl group.
5. The thermosetting resin composition according to claim 1, wherein the polyvalent phenol compound is represented by the following formula (3). (In formula (3), R 12 ~R 16 Each of these is independently either a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.
6. The thermosetting resin composition according to claim 1, wherein the quinone compound is represented by the following formula (4). (In formula (4), R 17 ~R 20 Each of these is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogen atom.
7. (E) The thermosetting resin composition according to claim 1, further comprising a low shrinkage agent.
8. The thermosetting resin composition according to claim 1, further comprising (F) glass fibers and (G) inorganic filler.
9. The thermosetting resin composition according to claim 1, wherein the total amount of the (A) thermosetting resin and the (B) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 5 to 80 parts by mass of the (A) thermosetting resin, 20 to 95 parts by mass of the (B) ethylenically unsaturated monomer, and 0.5 to 20 parts by mass of the (C) thermal polymerization initiator.
10. The thermosetting resin composition according to claim 7, wherein the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 10 to 60 parts by mass of (E) low shrinkage agent.
11. The thermosetting resin composition according to claim 8, wherein the total amount of (A) thermosetting resin and (B) ethylenically unsaturated monomer is 100 parts by mass, (F) glass fiber is 5 to 200 parts by mass, and (G) inorganic filler is 50 to 1000 parts by mass.
12. A cured product of a thermosetting resin composition according to any one of claims 1 to 11.
13. A molded stator comprising: a stator having a stator core and a coil wound around the stator core; and a molded material covering the stator, wherein the molded material is a cured product of a thermosetting resin composition according to any one of claims 1 to 11.