Coating method
The painting method addresses uneven paint film thickness by angling the substrate and controlling temperature and viscosity gradients, resulting in a uniform and crack-resistant paint film.
Patent Information
- Application Number
- PCT/JP2026/018158
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-13
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional painting methods result in uneven paint film thickness and increased likelihood of cracks due to the application of paint on substrates positioned parallel to the direction of gravity, leading to non-uniform properties such as transparency and abrasion resistance.
A painting method involving a heating step where the substrate is angled with the upper end as the fulcrum and a temperature difference of 5°C or more between the upper and lower parts, combined with a shear rate of 1 s⁻¹ and shear viscosity of 15 mPa·s or less, ensures uniform application of a paint composition.
The method achieves a uniformly applied paint film thickness, reducing the occurrence of cracks and enhancing properties like transparency and abrasion resistance by controlling the viscosity and temperature gradient during application.
Smart Images

Figure JP2026018158_19112026_PF_FP_ABST
Abstract
Description
Painting method
[0001] This invention relates to a painting method.
[0002] In recent years, there has been a growing demand for water-based paints due to concerns about hygiene at work sites and the impact on the global environment. Especially when the surface to be painted is large, the increased amount of paint used and the resulting large surface area of the liquid film immediately after application increase the concentration of volatile components in the work environment. Therefore, attempts are being made to significantly reduce the burden on painters by using water-based paints.
[0003] Conventionally, numerous aqueous coating compositions comprising binder resins, including emulsion particles, crosslinking agents, pigments, UV absorbers, solvents, and water have been proposed. Such aqueous coating compositions can be dried at room temperature or under heating to form a film, and the resulting coating films are known to possess barrier properties, stain resistance, chemical resistance, flame retardancy, heat resistance, weather resistance, abrasion resistance, and wear resistance.
[0004] For example, Patent Document 1 discloses a method for forming a multi-layer coating film characterized by sequentially applying a water-based paint as an intermediate coating, a water-based base coating, a water-based gloss material-containing base coating, and a clear coating in a wet-on-wet manner, and simultaneously heating and curing the resulting four layers of uncured coating film.
[0005] Japanese Patent Publication No. 2004-298837
[0006] Incidentally, in the application of paint, from the standpoint of productivity, that is, from the standpoint of transportability of the object to be painted and the painting efficiency when painting both sides of the object to be painted, it is preferable to apply the paint when the surface of the substrate to be painted is positioned parallel to the direction in which gravity acts on the substrate. Alternatively, it is also preferable to apply the paint when the substrate is positioned at an angle with the upper end as the pivot point, assuming that the direction in which gravity acts on the substrate is 0 degrees. However, in conventional painting methods in which paint is applied to a substrate positioned in such a manner and then heated, the thickness of the applied paint becomes uneven. This is particularly noticeable when the surface of the substrate to be painted is positioned parallel to the direction in which gravity acts. As a result, for example, cracks are more likely to occur in areas where the paint film is thicker, and the overall properties of the paint film become uneven due to the uneven thickness.
[0007] This invention has been made in view of the problems of the above-mentioned prior art, and aims to provide a coating method that can uniformly apply a paint composition.
[0008] <1> A painting method comprising: a heating step of heating a substrate; and a painting step of applying a paint composition to the heated substrate, wherein in the heating step, when the horizontal direction is set to 0 degrees, the substrate is arranged at an angle greater than 0 degrees and less than or equal to 90 degrees with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum; in the painting step, when the distance from the upper end to the lower end (the end on the side in the direction in which gravity acts) of the substrate is set to 100, the temperature difference (T1-T2) between the temperature T1 of the upper part of the heated substrate (the point at a distance of 10 from the upper end) and the temperature T2 of the lower part (the point at a distance of 90 from the upper end) is 5°C or more; and the shear rate of the paint composition at 25°C is 1s -1A coating method wherein the shear viscosity is 15 mPa·s or less. <2> The method according to <1>, wherein the heating step is performed under atmospheric pressure. <3> The coating method according to <1> or <2>, wherein at least the upper part of the substrate is heated in the heating step. <4> The coating method according to any one of <1> to <3>, wherein the heating step is performed by infrared heating. <5> The coating method according to any one of <1> to <4>, wherein the coating step is performed by a flow coating method. <6> The shear rate of the coating composition after being held at 65°C for 300 seconds is 1 s -1 A painting method according to any one of <1> to <5>, wherein the shear viscosity with respect to is greater than 15 mPa·s. <7> The shear rate of the paint composition after being held at 45°C for 20 seconds is 1s -1 A painting method according to any one of <1> to <6>, wherein the shear viscosity with respect to is greater than 15 mPa·s.
[0009] According to the present invention, a coating method is available that allows for the uniform application of a paint composition.
[0010] This is a schematic cross-sectional view showing an example of the heating process in this embodiment.
[0011] The embodiments of the present invention (hereinafter also referred to as "these embodiments") will be described in detail below. It should be noted that the present invention is not limited to the following embodiments, and can be implemented with various modifications within the scope of its gist.
[0012] In this specification, "(meth)acrylic" means "acrylic" and its corresponding "methacrylic." Furthermore, unless otherwise specified, "~" in this specification includes the values at both ends as the upper and lower limits.
[0013] <Painting Method> The painting method of this embodiment comprises a heating step of heating a substrate and a painting step of applying a paint composition to the heated substrate. In the heating step, with the horizontal direction set to 0 degrees, the substrate is positioned at an angle (absolute value) greater than 0 degrees and less than or equal to 90 degrees, with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum. In the painting step, with the distance from the upper end to the lower end (the end on the side in the direction in which gravity acts) of the substrate set to 100, the temperature difference (T1-T2) between the temperature T1 of the upper part of the heated substrate (the point at a distance of 10 from the upper end) and the temperature T2 of the lower part (the point at a distance of 90 from the upper end) is 5°C or more, and the shear rate of the paint composition at 25°C is 1s. -1 The shear viscosity is 15 mPa·s or less. Note that, with the horizontal direction set to 0 degrees, the angle applied with the upper end of the substrate (the end opposite to the direction of gravity) as the fulcrum is defined as follows: for example, the angle at which the substrate tilts toward a heat source such as an infrared heater is considered a negative angle, and the angle at which it tilts in the opposite direction to the heat source is considered a positive angle.
[0014] The above painting method involves, for example, in the heating step, when the horizontal direction is set to 0 degrees, a substrate that is positioned with an angle (absolute value) between 0 degrees and 90 degrees or less, with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum, preheating the substrate, and in the painting step, when the distance from the upper end to the lower end (the end on the side in the direction in which gravity acts) is set to 100, the temperature difference (T1-T2) between the heated upper part (the point at a distance of 10 from the upper end) and the lower part (the point at a distance of 90 from the upper end) is 5°C or more, and the painting is performed on a substrate with a shear rate of 1s at 25°C. -1A coating composition having a shear viscosity of 15 mPa·s or less is applied. By applying the coating composition to a substrate having a temperature difference (T1-T2) of 5°C or more, the coating composition can be applied to a uniform thickness. Conventional coating methods apply a coating composition to a substrate that has not been preheated. When a coating composition is applied to such a substrate that does not have a temperature difference between the temperature at the upper part and the temperature at the lower part of the substrate, for example, when the substrate is disposed at an angle (absolute value) of more than 0 degrees and 90 degrees or less with the upper end of the substrate (the end on the side opposite to the direction in which gravity acts) as a fulcrum when the horizontal direction is defined as 0 degrees, the applied thickness of the coating composition may develop a gradient from the upper part to the lower part of the substrate. That is, the applied thickness tends to be thin at the upper part of the substrate and thick at the lower part of the substrate, leading to an overall non-uniform applied thickness. As a result, cracks are likely to occur in portions where the coating film is thick, and properties such as transparency, heat resistance, and abrasion resistance may become non-uniform over the entire coating film. This effect is particularly pronounced when the substrate is disposed parallel to the direction in which gravity acts.
[0015] In order to address the above-described defects, in the coating method of the present embodiment, for a substrate that is preheated and has a temperature difference (T1-T2) of 5°C or more between the upper portion temperature T1 and the lower portion temperature T2, at a shear rate of 1 s at 25°C -1 A coating composition having a shear viscosity of 15 mPa·s or less is applied, whereby the temperature of the coating composition at the upper portion of the substrate also increases, the viscosity of the coating composition also rises, and thinning of the applied thickness can be suppressed. On the other hand, at the lower portion of the substrate, the temperature of the coating composition also decreases, so that the viscosity also decreases, making it possible to achieve a uniform applied thickness as a whole.
[0016] <Heating Step> The coating method of the present embodiment includes a heating step of heating a substrate that is disposed at an angle (absolute value) of more than 0 degrees and 90 degrees or less with the upper end of the substrate (the end on the side opposite to the direction in which gravity acts) as a fulcrum, when the horizontal direction is defined as 0 degrees.
[0017] With reference to Figure 1, an example of the heating step in the present embodiment will be described. Figure 1 is a schematic cross-sectional view showing an example of the heating step in the present embodiment. The heating device 20 has three stages of heating units: an upper-stage heating unit 20a, a middle-stage heating unit 20b, and a lower-stage heating unit 20c. Using the heating device 20, the heated surface 13 of the base material 10 disposed in a direction at an angle of 90 degrees with the upper end of the base material (the end on the side opposite to the direction in which gravity acts) as a fulcrum (hereinafter also referred to as the "vertical direction") is heated. That is, the heated surface 13 is a surface parallel to the vertical direction. At this time, the region to be heated is the upper part of the base material. Through such a heating step, the temperature difference (T1-T2) between the temperature T1 of the upper portion and the temperature T2 of the lower portion of the heated base material can be set to 5°C or more. The region to be heated, the distance at which the heated surface 13 of the base material 10 and the heating device 20 are arranged, and the arrangement position are not limited to those shown in Figure 1, and can be appropriately adjusted depending on the heating device used. In addition, although the heating device 20 in Figure 1 shows an infrared heater having three stages of heating units, the heating device is not limited to an infrared heater, and may be appropriately adopted according to the size of the base material, production efficiency, and the like.
[0018] In the heating step, when the horizontal direction is defined as 0 degrees, the absolute value of the angle provided with the upper end of the base material (the end on the side opposite to the direction in which gravity acts) as a fulcrum is more than 0 degrees and 90 degrees or less, preferably 20 degrees or more and 90 degrees or less. This enables liquid application type coating that forms a coating film on an object to be coated by utilizing gravity. Furthermore, when the base material has a curved surface, the angle provided with the upper end of the base material (the end on the side opposite to the direction in which gravity acts) as a fulcrum may be defined as the angle formed between the horizontal direction and a plane that is tangent to the curved surface at the upper end of the base material.
[0019] In the heating process, the heating region of the substrate is not particularly limited as long as the temperature difference (T1-T2) between the temperature T1 of the upper part of the substrate and the temperature T2 of the lower part of the substrate is 5°C or more, but it is preferable to heat at least the upper part of the substrate. That is, if the lower part of the substrate is heated so that the temperature difference (T1-T2) is 5°C or more as a result of heating the upper part of the substrate, then the lower part of the substrate may also be heated. In this specification, "upper part of the substrate" means, for example, in the case of a substrate arranged vertically, the region from the upper end to the upper end when a perpendicular line is drawn from the upper end to the lower end, with the upper end being set as point 0, and the distance from the upper end to the lower end being 100, and a line perpendicular to the perpendicular line is drawn at a point that is 50 from the upper end. Furthermore, "lower part of the base material" means, for example, in a base material arranged vertically, if a perpendicular line is drawn from the upper end to the lower end, with the upper end as point 0, and the distance from the upper end to the lower end is set to 100, then when a line perpendicular to the perpendicular line is drawn at a point 50 from the upper end, the "upper part of the base material" means the area from that perpendicular line to the lower end (excluding the perpendicular line itself). Similarly, in the case where the base material is arranged with an angle applied with the upper end as the pivot point, with the horizontal direction set to 0 degrees, "upper part of the base material" means the area from the perpendicular line to the upper end when a line perpendicular to the perpendicular line is drawn at a point 50 from the upper end, with the upper end as point 0, and the distance from the upper end to the lower end is set to 100, then when a line perpendicular to the perpendicular line is drawn at a point 50 from the upper end, the "upper part of the base material" means the area from that perpendicular line to the upper end. Furthermore, when the horizontal direction is set to 0 degrees and the base material is positioned with an angle applied with the upper end of the base material as the pivot point, the "lower part of the base material" is similarly defined as the area from the line perpendicular to the perpendicular at a point 50 degrees from the upper end, where the distance from the upper end to the lower end is set to 100, with the upper end being set to 0, and a perpendicular line drawn from the upper end to the lower end, the "lower part of the base material" refers to the area from that perpendicular line to the lower end (excluding the perpendicular line itself).
[0020] In this embodiment, the heating process is preferably carried out under atmospheric conditions. In this specification, "under atmospheric conditions" means under normal air conditions, not under artificial ventilation or in a windless state. This makes it possible to apply liquid coatings that use gravity to form a coating film on the object to be coated, and also allows for a more uniform application of the coating composition overall.
[0021] In this embodiment, from the viewpoint of being able to apply the paint composition more uniformly, on the upper part of the substrate, with the upper end point set as 0, a perpendicular line is drawn from the upper end to the lower end, and the distance from the upper end to the lower end is set to 100. When a line perpendicular to the perpendicular line is drawn at a point 45 from the upper end, it is preferable to heat the region from the perpendicular line to the upper end, more preferably at a point 40, when a line perpendicular to the perpendicular line is drawn, when a region from the perpendicular line to the upper end is heated, and even more preferably at a point 35, when a line perpendicular to the perpendicular line is drawn, when a region from the perpendicular line to the upper end is heated.
[0022] In this embodiment, from the viewpoint of enabling more uniform application of the paint composition, when the horizontal direction is defined as 0 degrees, and the substrate is arranged with an angle (absolute value) greater than 0 degrees and less than or equal to 90 degrees, with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum, it is preferable that the entire upper part of the substrate is heated in the horizontal direction perpendicular to the perpendicular line drawn from one point on the upper end of the substrate to the lower end, up to both ends in the horizontal direction.
[0023] In the heating process, the heating method for heating the substrate is not particularly limited, but examples include heating by hot air, infrared radiation, and electromagnetic induction. As a heating method, infrared heating is preferred from the viewpoint of rapid heating of the substrate, i.e., shortening the heating time, and from the viewpoint of the size and flexibility of the heating equipment, i.e., it can be introduced as a small heating device and can be appropriately adjusted according to the part to be heated. Examples of infrared heaters include carbon heaters, halogen heaters, and ceramic heaters.
[0024] In the heating process, the arrangement of the substrate and heating equipment is not particularly limited, and as long as the temperature difference between the upper temperature T1 and the lower temperature T2 (T1-T2) is heated to 5°C or more, it can be appropriately adjusted according to the heating equipment used, heating temperature, etc.
[0025] In the heating process, when using an infrared heater, its output is not particularly limited, but from the viewpoint of enabling more uniform application of the paint composition and heating efficiency, it is preferable that the output be 1.0 to 3.0 kW when using, for example, a carbon heater (product name: Orange Heat, manufactured by Metro Electric Industry Co., Ltd.). The heating temperature controlled by the output of the infrared heater can be adjusted by the distance and arrangement between the substrate and the heating equipment, and by the heating device used.
[0026] <Painting Process> The painting method of this embodiment includes a painting process in which a paint composition is applied to a heated substrate, wherein the temperature difference (T1-T2) between the temperature T1 of the upper part of the heated substrate and the temperature T2 of the lower part is 5°C or more.
[0027] The temperature difference (T1-T2) is not particularly limited as long as it is 5°C or more, but from the viewpoint of being able to apply the paint composition more uniformly, it is preferably 10°C or more, 15°C or more, 20°C or more, 25°C or more, 30°C or more, 35°C or more, 40°C or more, and 45°C or more. As the temperature difference (T1-T2) increases, the temperature of the paint composition also increases in the upper part of the substrate, and the viscosity increases due to evaporation of the solvent in the paint composition and aggregation of particles, which tends to result in a more uniform coating thickness from the top to the bottom of the substrate. The upper limit of the temperature difference (T1-T2) is not particularly limited, but it may be 60°C or less.
[0028] The temperature T1 of the heated surface of the substrate is not particularly limited, but is preferably 10 to 95°C, more preferably 20 to 85°C, more preferably 30 to 75°C, and most preferably 40 to 70°C. When the temperature T1 of the surface is within the above range, the paint composition tends to be applied more uniformly. The temperature T1 of the surface of the substrate can be adjusted by the heating temperature and arrangement of the heating equipment.
[0029] The point at which the temperature T1 is measured on the upper part of the heated substrate is, for example, on a substrate arranged vertically, the point at which the distance from the upper end (the end opposite to the direction in which gravity acts) is 10 when a perpendicular line is drawn from the upper end to the lower end (the end on the side in the direction in which gravity acts), with the upper end being set to 0, and the distance from the upper end to the lower end being 100. From the viewpoint of being able to apply the paint composition more uniformly, the point at which the temperature T1 is measured on the upper part of the heated substrate is preferably one of the points on a perpendicular line drawn at the point at which the distance from the upper end is 10, and more preferably the point on the perpendicular line that points to the center of both ends of the substrate in the horizontal direction. The temperature T1 can be measured using a thermocouple or a radiation thermometer.
[0030] The temperature T2 at the bottom of the heated substrate is not particularly limited, but is preferably 5 to 35°C, more preferably 10 to 35°C, even more preferably 15 to 30°C, and most preferably 20 to 30°C. As long as the temperature T2 at the bottom is within the above range, the substrate can be used directly in the coating method of this embodiment even in its stored state. The temperature T2 at the bottom of the substrate may be adjusted within the above range by cooling equipment such as a fan.
[0031] The point at which the temperature T2 at the bottom of the heated substrate is measured is, for example, in a substrate arranged vertically, the point at which the distance from the top end (the end opposite to the direction in which gravity acts) is 90, when a perpendicular line is drawn from the top end to the bottom end (the end on the side in the direction in which gravity acts), with the distance from the top end to the bottom end being 100. From the viewpoint of being able to apply the paint composition more uniformly, the point at which the temperature T2 at the bottom of the heated substrate is measured is preferably one of the points on a line perpendicular to the perpendicular line drawn at the point at a distance of 90 from the top end, and more preferably the point on the perpendicular line that points to the center of both ends of the substrate in the horizontal direction. The temperature T2 can be measured using a thermocouple or a radiation thermometer.
[0032] In the painting process, the method of applying the paint composition is not particularly limited, but examples include flow painting, brush painting, dip painting, casting, gravure printing, and flexographic printing. Among these, flow painting is preferred from the viewpoint of making the effects of the present invention even more useful.
[0033] In the painting process, for example, the flow rate of the paint in the flow painting method is not particularly limited, but from the viewpoint of applying the paint composition more uniformly, it is preferably 1 to 10 L / min, more preferably 3 to 8 L / min, and even more preferably 4 to 6 L / min. The flow rate of the paint may be adjusted as appropriate depending on the painting method used.
[0034] In the painting process, for example, the coating time in the flow painting method is not particularly limited, but from the viewpoint of applying the paint composition more uniformly and suppressing deterioration of the paint composition, it is preferably within 3 minutes, more preferably within 2 minutes, and even more preferably within 1 minute. The lower limit is not particularly limited, but is 30 seconds or more. The coating time may be adjusted as appropriate depending on the painting method adopted. In the painting process, the angle of the substrate is preferably such that, with the horizontal direction being 0 degrees, the upper end of the substrate (the end opposite to the direction in which gravity acts) is the pivot point and the angle is greater than 0 degrees and less than or equal to 90 degrees (absolute value), and it is more preferable that the angle from the heating process is maintained.
[0035] <First heating step, second heating step, first painting step, and second painting step> In the painting method of this embodiment, the heating step may include a first heating step and / or a second heating step. The painting step may also include a first painting step and / or a second painting step. Furthermore, the paint composition may include a first paint composition and / or a second paint composition.
[0036] That is, if the heating process includes a first heating process and a second heating process, the painting process includes a first painting process and a second painting process, and the paint composition includes a first paint composition and a second paint composition, the painting method of this embodiment includes: a first heating process in which a substrate is heated with an angle (absolute value) greater than 0 degrees and less than or equal to 90 degrees, with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum when the horizontal direction is 0 degrees; a first painting process in which the first paint composition is applied to the heated substrate; and the substrate coated with the first paint composition The process comprises a second heating step of heating, and a second coating step of applying the first coating composition to a heated substrate, wherein in the first coating step, the temperature difference (T3-T4) between the upper temperature T3 and the lower temperature T4 of the heated substrate is 5°C or more, and in the second coating step, the temperature difference (T5-T6) between the upper temperature T5 and the lower temperature T6 of the heated substrate to which the first coating composition has been applied is 5°C or more, and the shear rate of the first and second coating compositions at 25°C is 1s.-1 The shear viscosity for is 15 mPa·s or less. The measurement locations for temperatures T3 and T5 at the top are the same as those for temperature T1 at the top, and the measurement locations for temperatures T4 and T6 at the bottom are the same as those for temperature T2 at the bottom.
[0037] The first and second heating steps can suitably adopt the conditions of the heating steps described above. In the first and second heating steps, temperature T1 corresponds to temperatures T3 and T5, respectively, and temperature T2 corresponds to temperatures T4 and T6, respectively.
[0038] The first and second painting processes can suitably adopt the conditions of the painting process described above.
[0039] The first and second paint compositions will be described later.
[0040] <Other steps> In addition to the heating step and painting step described above, the painting method of this embodiment may include other steps as needed. Examples of other steps include a drying step.
[0041] The drying step is not particularly limited, but may be included after the painting step. By including a drying step, the paint composition can be applied to a uniform thickness to form a coating film during the painting step. The drying method in the drying step is not particularly limited, but examples include natural drying, forced drying, and heat drying.
[0042] In this embodiment, if the heating step includes the first heating step and the second heating step described above, and the painting step includes the first painting step and the second painting step described above, it is preferable to have a drying step after the first painting step and after the second painting step from the viewpoint of energy saving. Furthermore, the infrared heating described above can be suitably used as the drying method in the drying step after the first step.
[0043] In the coating method of this embodiment, the thickness of the coating film of the paint composition obtained after the coating process is preferably 1 to 20 μm, more preferably 2 to 18 μm, even more preferably 3 to 15 μm, and particularly preferably 4 to 12 μm.
[0044] In the coating method of the present embodiment, the thickness of the coating film of the first coating composition obtained after the first coating step is preferably 1 to 20 μm, more preferably 2 to 18 μm, still more preferably 3 to 15 μm, and particularly preferably 4 to 12 μm.
[0045] In the coating method of the present embodiment, the thickness of the coating film of the second coating composition obtained after the second coating step is preferably 1 to 20 μm, more preferably 2 to 16 μm, still more preferably 3 to 12 μm, and particularly preferably 4 to 8 μm.
[0046] (Coating Composition) In the coating method of the present embodiment, the shear viscosity of the coating composition at 25°C at a shear rate of 1 s -1 is 15 mPa·s or less. In the coating step, the temperature of the coating composition also increases above the heated substrate, and the viscosity of the coating composition rises due to evaporation of the solvent in the coating composition, aggregation of particles, and the like, whereby a uniform coating thickness can be achieved from the upper part to the lower part of the substrate.
[0047] In the present embodiment, the shear viscosity of the coating composition at 25°C at a shear rate of 1 s -1 is preferably 13 mPa·s or less, more preferably 10 mPa·s or less, from the viewpoint of further improving the above effects. The lower limit is not particularly limited, but may be 1 mPa·s or more. The shear viscosity of the coating composition at 25°C at a shear rate of 1 s -1 can be adjusted by the types and blending amounts of components contained in the coating material to be described later. The shear viscosity of the coating composition at 25°C at a shear rate of 1 s -1 can be measured using a rotational rheometer (trade name: MCR302e, manufactured by Anton Paar).
[0048] In the present embodiment, from the viewpoint of further improving the above effects, the shear rate of 1 s after the coating composition is held at 65°C for 300 seconds -1The shear viscosity for may be greater than 15 mPa·s, preferably 20 mPa·s or more, more preferably 50 mPa·s or more, and even more preferably 100 mPa·s or more. The shear rate of the paint composition after being held at 65°C for 300 seconds is 1s -1 The upper limit of the shear viscosity for is not particularly limited, but it may be 10,000 mPa·s or less. Shear rate 1s after holding the paint composition at 65°C for 300 seconds. -1 The shear viscosity can be adjusted by the type and amount of components contained in the paint, as described later. In this embodiment, the shear rate 1s after holding the paint composition at 65°C for 300 seconds is -1 The shear viscosity for [the given material] can be measured using a rotary flow meter (product name: MCR302e, manufactured by Anton Paar).
[0049] In this embodiment, from the viewpoint of further improving the above effect, more preferably, the shear rate of the paint composition after being held at 45°C for 20 seconds is 1s -1 The shear viscosity for may be greater than 15 mPa·s, preferably 20 mPa·s or more, more preferably 50 mPa·s or more, and even more preferably 100 mPa·s or more. The shear rate of the paint composition after being held at 45°C for 20 seconds is 1s -1 The upper limit of the shear viscosity for is not particularly limited, but it may be 10,000 mPa·s or less. Shear rate 1s after holding the paint composition at 45°C for 20 seconds. -1 The shear viscosity can be adjusted by the type and amount of components contained in the paint, as described later. In this embodiment, the shear rate 1s after holding the paint composition at 45°C for 20 seconds is -1 The shear viscosity for [the given material] can be measured using a rotary flow meter (product name: MCR302e, manufactured by Anton Paar).
[0050] The solvent included in the paint composition is not particularly limited, but it is preferable that 50% by mass or more of the solvent is water. In other words, the paint composition of this embodiment is preferably a water-based paint composition. In this specification, "water-based" means that the most abundant component in the solvent is water. Being a water-based paint composition allows for an appropriate evaporation rate of the solvent during the painting process, enabling a uniform coating thickness from the top to the bottom of the substrate.
[0051] In this embodiment, the paint composition is not particularly limited, and for example, the compositions described in Japanese Patent Application No. 2024-182061 and Japanese Patent Application No. 2024-052021 can be used. Among these, the first paint composition and the second paint composition described later can be suitably used in this embodiment.
[0052] In the coating method of this embodiment, the paint composition may include a first paint composition and a second paint composition. The shear rate of the first paint composition and the second paint composition at 25°C is 1 s. -1 Shear viscosity relative to , shear rate 1s after holding at 65°C for 300 seconds -1 Shear viscosity relative to , shear rate 1s after holding at 45°C for 20 seconds -1 The shear viscosity for is preferably within the numerical range described above.
[0053] (First paint composition) The first paint composition is not particularly limited, but examples include a paint composition containing emulsion particles (A), an amine compound (B), inorganic particles (C), and water, which will be described later.
[0054] (Emulsion particles (A)) Emulsion particles (A) primarily serve to improve adhesion to the substrate and may contain vinyl monomers (a) as constituent units. That is, emulsion particles (A) may have units (a) derived from vinyl monomers (a).
[0055] The aforementioned unit (a) may contain unit (a-1) derived from the ultraviolet-absorbing vinyl monomer (a-1). The inclusion of unit (a-1) tends to improve the weather resistance of the first paint composition of this embodiment and the paint film of the second paint composition described later.
[0056] The UV-absorbing vinyl monomer (a-1) is a vinyl monomer having a UV-absorbing group. A UV-absorbing group is a functional group that absorbs in the ultraviolet region (wavelength 400 nm or less), and the UV-absorbing vinyl monomer (a-1) is not particularly limited as long as it is a vinyl monomer having such properties. Examples of UV-absorbing vinyl monomers (a-1) include (meth)acrylic monomers having UV-absorbing groups in their molecules, specifically benzophenone compounds such as 2-hydroxy-4-acryloxybenzophenone, 2-hydroxy-4-methacryloxybenzophenone, 2-hydroxy-5-acryloxybenzophenone, 2-hydroxy-5-methacryloxybenzophenone, 2-hydroxy-4-(acryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-ethoxy)benzophenone, 2-hydroxy-4-(methacryloxy-diethoxy)benzophenone, and 2-hydroxy-4-(acryloxy-triethoxy)benzophenone; 2-( Examples of benzotriazole compounds include 2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole (trade name "RUVA-93" manufactured by Otsuka Chemical Co., Ltd.), 2-(2'-hydroxy-5'-methacryloxyethyl-3-tert-butylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacrylyloxypropyl-3-tert-butylphenyl)-5-chloro-2H-benzotriazole, and 3-methacryloyl-2-hydroxypropyl-3-[3'-(2''-benzotriazolyl)-4-hydroxy-5-tert-butyl]phenylpropionate (trade name "CGL-104" manufactured by Ciba-Geigy Japan).
[0057] From the viewpoint of weather resistance of the coating film, the content of unit (a-1) is preferably 1 to 20% by mass, and more preferably 1 to 10% by mass, relative to the total mass of unit (a) constituting the emulsion particles (A).
[0058] In the emulsion particles (A), it is preferable that the unit (a) is a monomer that does not correspond to unit (a-1) and is derived from a hydroxyl group-containing vinyl monomer (a-2) having a hydroxyl group. The hydroxyl group-containing vinyl monomer (a-2) is not limited to the following, but examples include hydroxyalkyl esters of (meth)acrylic acid such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; hydroxyethyl (meth)acrylamides such as N-hydroxyethyl acrylamide and N-hydroxyethyl methacrylamide; and di-2-H Examples include hydroxyalkyl esters of fumaric acid such as hydroxyethyl fumarate and mono-2-hydroxyethyl monobutyl fumarate; (poly)oxyethylene mono(meth)acrylates with 1 to 100 allyl alcohol or ethylene oxide groups; (poly)oxypropylene mono(meth)acrylates with 1 to 100 propylene oxide groups; and "Praxel FM, FA monomers" (trade names for caprolactone addition monomers manufactured by Daicel Chemical Corporation) and other hydroxyalkyl esters of α,β-ethylenically unsaturated carboxylic acids. These may be used individually or in combination of two or more.
[0059] The (poly)oxyethylene mono(meth)acrylate mentioned above is not limited to the following, but examples include ethylene glycol (meth)acrylate, ethylene glycol methoxy(meth)acrylate, diethylene glycol (meth)acrylate, diethylene glycol methoxy(meth)acrylate, tetraethylene glycol (meth)acrylate, tetraethylene glycol methoxy(meth)acrylate, and tetraethylene glycol methoxy(meth)acrylate.
[0060] The content of unit (a-2) is preferably 10% to 40% by mass, and more preferably 20% to 30% by mass, relative to the total mass of vinyl monomer (a) constituting the emulsion particles (A). When the content of unit (a-2) is within the above range, the reaction between the hydroxyl group-containing vinyl monomer (a-2) and other vinyl monomers tends to proceed favorably, and because the hydrophilicity of the emulsion particles (A) is ensured, a decrease in transparency and surface roughness tend to be prevented when forming a coating film of the first paint composition or the second paint composition described later.
[0061] In emulsion particles (A), unit (a) may have units derived from other vinyl monomers in addition to units (a-1) and (a-2). Examples of other vinyl monomers include, but are not limited to, (meth)acrylic acid esters, (meth)acrylate alkyl esters, aromatic vinyl compounds, vinyl cyanide compounds, as well as carboxyl group-containing vinyl monomers, epoxy group-containing vinyl monomers, carbonyl group-containing vinyl monomers, and vinyl monomers having secondary and / or tertiary amide groups.
[0062] The (meth)acrylic acid ester is not limited to the following, but examples include alkyl (meth)acrylic acid esters having 1 to 50 carbon atoms in the alkyl group, and (poly)oxyethylene di(meth)acrylates having 1 to 100 ethylene oxide groups.
[0063] The (poly)oxyethylene di(meth)acrylate mentioned above is not limited to the following, but examples include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, diethylene glycol methoxy(meth)acrylate, tetraethylene glycol di(meth)acrylate, and the like.
[0064] The alkyl (meth)acrylate esters mentioned above are not limited to the following, but include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, cyclohexyl (meth)acrylate, lauryl (meth)acrylate, and dodecyl (meth)acrylate.
[0065] The aromatic vinyl compound is not limited to the following, but examples include styrene, 4-vinyltoluene, and the like.
[0066] The vinyl cyanide compound mentioned above is not limited to the following, but examples include acrylonitrile and methacrylonitrile.
[0067] The carboxyl group-containing vinyl monomer is not limited to the following, but examples include (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, maleic anhydride, or half-esters of dibasic acids such as itaconic acid, maleic acid, and fumaric acid. When a carboxyl group-containing vinyl monomer is used, carboxyl groups can be introduced into the emulsion particles (A), improving the stability of the emulsion by creating electrostatic repulsion between the particles, and tending to improve resistance to external dispersion disruption, such as aggregation during stirring. In this case, from the viewpoint of further improving the electrostatic repulsion, some or all of the introduced carboxyl groups may be neutralized with a base such as an amine.
[0068] The epoxy group-containing vinyl monomer is not limited to the following, but examples include glycidyl group-containing vinyl monomers. The glycidyl group-containing vinyl monomer is not limited to the following, but examples include glycidyl (meth)acrylate, allyl glycidyl ether, allyl dimethyl glycidyl ether, etc.
[0069] The carbonyl-containing vinyl monomer is not limited to the following, but examples include diacetone acrylamide.
[0070] The vinyl monomer having the secondary and / or tertiary amide group is not limited to the following, but examples include N-alkyl or N-alkylene-substituted (meth)acrylamides. Specifically, these include N-methylacrylamide, N-methylmethacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl-N-isopropylacrylamide Examples include luamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,N'-methylenebismethacrylamide, N-vinylacetamide, diacetone acrylamide, diacetone methacrylamide, N-methylolacrylamide, and N-methylolmethacrylamide.
[0071] In addition, other vinyl monomers not listed above include, but are not limited to, olefins such as ethylene, propylene, and isobutylene; dienes such as butadiene; haloolefins such as vinyl chloride, vinylidene fluoride chloride, tetrafluoroethylene, and chlorotrifluoroethylene; vinyl acetate, vinyl propionate, n-butyrate, vinyl benzoate, p-t-butylbenzoate, vinyl pivalate, vinyl 2-ethylhexanoate, vinyl versatate, vinyl laurate, and other vinyl carboxylate esters; isopropenyl carboxylate esters such as isopropenyl acetate and isopropenyl propionate; and ethyl vinyl ether. Examples include vinyl ethers such as isobutyl vinyl ether and cyclohexyl vinyl ether, allyl esters such as allyl acetate and allyl benzoate, allyl ethers such as allyl ethyl ether and allyl phenyl ether, and also 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, perfluoromethyl (meth)acrylate, perfluoropropyl (meth)acrylate, perfluoropropylmethyl (meth)acrylate, vinylpyrrolidone, trimethylolpropane tri(meth)acrylate, and (meth)acrylate. These other vinyl monomers may be used individually or in combination of two or more.
[0072] The emulsion particles (A) may have a structure derived from an emulsifier. Examples of emulsifiers include, but are not limited to, acidic emulsifiers such as alkylbenzene sulfonic acid, alkyl sulfonic acid, alkyl sulfosuccinic acid, polyoxyethylene alkyl sulfate, polyoxyethylene alkylaryl sulfate, and polyoxyethylene distyrylphenyl ether sulfonic acid; anionic surfactants such as alkali metal (Li, Na, K, etc.) salts of acidic emulsifiers, ammonium salts of acidic emulsifiers, and fatty acid soaps; cationic surfactants of the quaternary ammonium salt, pyridinium salt, or imidazolinium salt type such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and imidazolinium laurate; nonionic surfactants such as polyoxyethylene alkylaryl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene oxypropylene poroc copolymer, and polyoxyethylene distyrylphenyl ether, as well as reactive emulsifiers having radically polymerizable double bonds.
[0073] The reactive emulsifier having a radically polymerizable double bond is not limited to the following, but includes, for example, Eleminol JS-2 (trade name, manufactured by Sanyo Chemical Industries, Ltd.), Latemul S-120, S-180A or S-180 (trade name, manufactured by Kao Corporation), Aqualon HS-10, KH-1025, RN-10, RN-20, RN30, RN50 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adekaria Soap SE1025, SR-1025, NE-20, NE- Examples include 30, NE-40 (product name, manufactured by Asahi Denka Kogyo Co., Ltd.), ammonium salts of p-styrenesulfonic acid, sodium salts of p-styrenesulfonic acid, potassium salts of p-styrenesulfonic acid, alkyl sulfonic acid (meth)acrylates such as 2-sulfoethyl acrylate, methylpropanesulfonic acid (meth)acrylamide, ammonium salts of allylsulfonic acid, sodium salts of allylsulfonic acid, potassium salts of allylsulfonic acid, etc.
[0074] The emulsion particles (A) preferably contain a chain transfer agent. That is, the first coating composition of this embodiment preferably contains a chain transfer agent. The chain transfer agent is not limited to the following, but examples include mercaptans such as octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, n-hexadecyl mercaptan, n-tetradecyl mercaptan, and t-tetradecyl mercaptan; xanthogen disulfides such as dimethyl xanthogen disulfide, diethyl xanthogen disulfide, and diisopropyl xanthogen disulfide; thiuram disulfides such as tetramethyl thiuram disulfide, tetraethyl thiuram disulfide, and tetrabutyl thiuram disulfide; carbon tetrachloride, ethylene bromide, etc. Examples include halogenated hydrocarbons; hydrocarbons such as pentaphenylethane; and acrolein, methacrolein, allyl alcohol, 2-ethylhexylthioglycolate, turbinolene, α-terpinene, γ-terpinene, dipentene, α-methylstyrene dimer (preferably containing 50% or more by mass of 2,4-diphenyl-4-methyl-1-pentene), as well as unsaturated cyclic hydrocarbon compounds such as 9,10-dihydroanthracene, 1,4-dihydronaphthalene, indene, and 1,4-cyclohexadiene; and unsaturated heterocyclic compounds such as xanthene and 2,5-dihydrofuran. These may be used individually or in combination of two or more.
[0075] The method for preparing the emulsion particles (A) used in the paint composition of this embodiment is not particularly limited, but one example is a method of polymerizing a vinyl monomer in the presence of water, an emulsifier, and a polymerization initiator.
[0076] Examples of the polymerization initiators include, but are not limited to, hydrogen peroxide, hydroperoxides such as cumene hydroperoxide, diisopropylbenzene hydroperoxide, and paramentane hydroperoxide, peroxides such as benzoyl peroxide and lauroyl peroxide, and organic polymerization initiators such as azo compounds such as 2,2'-azobis{2-methyl-N-[2-(1-hydroxybutyl)propionamide]}, 2,2'-azobis[(2-methylpropionamidine)dihydrochloride], 2,2'-azobis[N-(2-carboxyethyl)-2-methyl-propiondiamine] tetrahydrate, 2,2'-azobis(2,4-dimethylvaleronitrile), and azobisisobutyronitrile, as well as inorganic polymerization initiators such as persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate. In addition, so-called redox polymerization initiators, which use reducing agents such as sodium bisulfite, ascorbic acid, and their salts in combination with polymerization initiators, can also be used.
[0077] In the emulsion particles (A) used in the first coating composition of this embodiment, the weight-average molecular weight of unit (a) derived from the vinyl monomer, calculated from a chromatogram measured by gel permeation chromatography based on the molecular weight of standard polystyrene, is preferably in the range of 10,000 to 1,000,000. This tends to result in excellent transparency and adhesion when a coating film of the first coating composition of this embodiment is formed. Furthermore, from the viewpoint of further improving adhesion, the weight-average molecular weight of unit (a) is more preferably 500,000 or less, and even more preferably 250,000 or less. The weight-average molecular weight of unit (a) can be controlled to the above range by, for example, adjusting the amount of vinyl monomer added in the polymerization process, the polymerization time, or using the chain transfer agent described above.
[0078] The average particle size of the emulsion particles (A) is determined from the particle size observed by dynamic light scattering. The average particle size of the emulsion particles (A) is not limited to the following, but is preferably 200 nm or less. By setting the average particle size of the emulsion particles (A) within the above range, the first coating composition of this embodiment tends to form a coating film with even better adhesion due to an improved contact area with the substrate. Furthermore, from the viewpoint of improving transparency, the average particle size of the emulsion particles (A) is more preferably 100 nm or less, and from the viewpoint of good storage stability of the first coating composition of this embodiment, it is preferably 10 nm or more, and more preferably 25 nm or more. Specifically, the average particle size of the emulsion particles (A) can be measured using a dynamic light scattering particle size distribution analyzer (product number: nanoSAQLA) manufactured by Otsuka Electronics Co., Ltd. The average particle size of the emulsion particles (A) can be controlled to the above range by adjusting polymerization conditions, etc.
[0079] The glass transition temperature of emulsion particles (A) can be measured using a differential scanning calorimeter. The glass transition temperature of emulsion particles (A) is not limited to the following, but is preferably between -30°C and 50°C. By setting the glass transition temperature of emulsion particles (A) within the above range, the first coating composition of this embodiment can form a coating film with excellent adhesion to the substrate. Furthermore, from the viewpoint of transparency, the glass transition temperature of emulsion particles (A) is more preferably between -20°C and 45°C, and even more preferably between -10°C and 40°C. The glass transition temperature of emulsion particles (A) can be controlled within the above range by adjusting the type of monomer used, the amount added, the polymerization temperature, and the polymerization time during the polymerization process.
[0080] The content of emulsion particles (A) in the first paint composition relative to the total solids is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, from the viewpoint of transparency and adhesion. Here, the total solids in the first paint composition refer to the total mass of components other than volatile components contained in the first paint composition. Volatile components mainly include solvents and neutralizing agents.
[0081] (Amine compound (B)) The first paint composition of this embodiment may contain an amine compound (B). The amine compound (B) is a neutralizing agent for the emulsion particles (A), and an appropriate amine compound (B) may be selected and added. As a result, when the first paint composition of this embodiment is applied to a large surface area, it tends to form a coating with excellent coating performance such as transparency, surface smoothness, and weather resistance.
[0082] The amine compound (B) is not limited to the following, but examples include n-butylamine, isobutylamine, amylamine, cyclopentylamine, hexylamine, dipropylamine, diisopropylamine, dibutylamine, pyrrolidine, piperidine, morpholine, triethylamine, tripropylamine, triisopropylamine, 1-methylpiperidine, 1-methylpyrrolidine, N,N-dimethylpropylamine, monoisopropanolamine, 2-amino-2-methyl-1-propanol, dimethylethanolamine, and the like.
[0083] (Inorganic particles (C)) The first paint composition of this embodiment may contain inorganic particles (C). The inclusion of inorganic particles (C) in the first paint composition of this embodiment tends to result in superior transparency and adhesion when the coating film of the second paint composition is formed, due to the interaction between the coating film of the first paint composition of this embodiment and the coating film of the second paint composition described later.
[0084] The inorganic particles (C) are not limited to the following, but examples include oxides of silicon, aluminum, titanium, zirconium, zinc, cerium, tin, indium, gallium, germanium, antimony, molybdenum, niobium, magnesium, bismuth, cobalt, copper, etc. These may be used individually or in combination of two or more.
[0085] The inorganic particles (C) are preferably silica particles, such as dry silica or colloidal silica, from the viewpoint of adhesion to the hard coat layer in the hard coat laminate described later. Colloidal silica is also preferred because it can be used in the form of an aqueous dispersion.
[0086] As the inorganic particles (C) used in the first coating composition of this embodiment, acidic colloidal silica dispersed in water is preferred. The colloidal silica is not particularly limited, but can be prepared by the sol-gel method, and commercially available products can also be used. When preparing by the sol-gel method, refer to Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Lang muir 6, 792-801 (1990), Journal of the Color Materials Association, 61[9]488-493 (1988), etc. Examples of commercially available products include Snowtex-O, Snowtex-OS, Snowtex-OXS, Snowtex-O-40, Snowtex-OL, Snowtex-OYL, Snowtex-OUP, Snowtex-PS-SO, Snowtex-PS-MO, Snowtex-AK-XS, Snowtex-AK, Snowtex-AK-L, Snowtex-AK-YL, Snowtex-AK-PS-S (product names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20Q (product name, manufactured by Asahi Denka Kogyo Co., Ltd.), Crevosol 20H12, Crevosol 30CAL25 (product names, manufactured by Clariant Japan Co., Ltd.). These colloidal silicas may be used individually or in combination of two or more types.
[0087] Furthermore, basic colloidal silica can also be used as colloidal silica. Basic colloidal silica includes, but is not limited to, silica stabilized by the addition of alkali metal ions, ammonium ions, and amines. Examples include Kus-N-40 (product name, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20, Adelite AT-30, Adelite AT-20N, Adelite AT-30N, Adelite AT-20A, Adelite AT-30A, Adelite AT-40, Adelite AT-50 (product names, manufactured by Asahi Denka Kogyo Co., Ltd.), Crevozol 30R9, Crevozol 30R50, Crevozol 50R50 (product names, manufactured by Clariant Japan Co., Ltd.), Rudox HS-40, Rudox HS-30, Rudox LS, Rudox AS-30, Rudox SM-AS, Rudox AM, Rudox HSA, and Rudox SM (product names, manufactured by DuPont).
[0088] Furthermore, colloidal silica using a water-soluble solvent as a dispersion medium includes, but is not limited to, the following: MA-ST-M (methanol dispersion type with particle size of 20-25 nm), IPA-ST (isopropyl alcohol dispersion type with particle size of 10-15 nm), EG-ST (ethylene glycol dispersion type with particle size of 10-15 nm), EGST-ZL (ethylene glycol dispersion type with particle size of 70-100 nm), NPC-ST (ethylene glycol monopropyl ethere dispersion type with particle size of 10-15 nm), TOL-ST (toluene dispersion type with particle size of 10-15 nm), etc., all manufactured by Nissan Chemical Industries, Ltd.
[0089] Examples of dry silica particles include, but are not limited to, AEROSIL manufactured by Nippon Aerosil Co., Ltd. and Rheoroseal manufactured by Tokuyama Corporation.
[0090] Silica particles may contain inorganic bases (such as sodium hydroxide, potassium hydroxide, lithium hydroxide, and ammonia) or organic bases (such as tetramethylammonium and triethylamine) as stabilizers.
[0091] From the viewpoint of transparency and adhesion of the coating films of the first and second coating compositions, the mass ratio of the inorganic particles (C) to the total solid content of the first coating composition of this embodiment is preferably 30% to 60% by mass, and more preferably 37.5% to 47.5% by mass.
[0092] (Crosslinking agent (D)) The first coating composition of this embodiment preferably contains a crosslinking agent (D) from the viewpoint of improving adhesion.
[0093] The crosslinking agent (D) is preferably an isocyanate compound, from the viewpoint of reactivity with the emulsion particles (A) used in the first coating composition of this embodiment.
[0094] An isocyanate compound is a compound having at least one isocyanate group in one molecule. An isocyanate compound may also be a compound having two or more isocyanate groups in one molecule. The isocyanate compound is not limited to the following, but examples include aliphatic diisocyanates such as 1,4-tetramethylene diisocyanate, ethyl (2,6-diisocyanate) hexanoate, 1,6-hexamethylene diisocyanate, 1,12-dodecamethylene diisocyanate, 2,2,4- or 2,4,4-trimethylhexamethylene diisocyanate; 1,3,6-hexamethylene triisocyanate, 1,8-diisocyanate-4- Aliphatic triisocyanates such as isocyanate methyl octane, 2-isocyanate ethyl (2,6-diisocyanate) hexanoate; 1,3- or 1,4-bis(isocyanate methylcyclohexane), 1,3- or 1,4-diisocyanate cyclohexane, 3,5,5-trimethyl(3-isocyanate methyl)cyclohexyl isocyanate, dicyclohexylmethane-4,4'-diisocyanate, 2,5- or 2,6-diisocyanate Alicyclic diisocyanates such as tomethylnorbornane; alicyclic triisocyanates such as 2,5- or 2,6-diisocyanate, tomethyl-2-isosinate, and topropylnorbornane; aralkylene diisocyanates such as m-xylylene diisocyanate and α,α,α'α'-tetramethyl-m-xylylene diisocyanate; m- or p-phenylene diisocyanate, trilen-2,4- or 2,6-diisocyanate, and diphenylmethane-4,4'-diiso Examples include aromatic diisocyanates such as cyanate, naphthalene-1,5-diisocyanate, diphenyl-4,4'-diisocyanate, 4,4'-diisocyanate-3,3'-dimethyldiphenyl, 3-methyl-diphenylmethane-4,4'-diisocyanate, and diphenyl ether-4,4'-diisocyanate; and aromatic triisocyanates such as triphenylmethane triisocyanate and tris(isocyanatephenyl)thiophosphate.
[0095] Examples of isocyanate compounds include diisocyanates or polyisocyanates having a uretdione structure obtained by cyclodimerizing the isocyanate groups of the aforementioned diisocyanates or triisocyanates; polyisocyanates having an isocyanurate structure obtained by cyclotrimerizing the isocyanate groups of the aforementioned diisocyanates or triisocyanates; polyisocyanates having a biuret structure obtained by reacting the aforementioned diisocyanates or triisocyanates with water; polyisocyanates having an oxadiazinetrione structure obtained by reacting the aforementioned diisocyanates or triisocyanates with carbon dioxide; polyisocyanates having an allophanate structure obtained by reacting the aforementioned diisocyanates or triisocyanates with various alcohols; and polyisocyanates obtained by reacting the aforementioned diisocyanates or triisocyanates with compounds containing active hydrogen, such as polyhydroxy compounds, polycarboxy compounds, and polyamine compounds. Examples of isocyanate compounds include isocyanate compounds having an alkoxysilane moiety and / or a siloxane moiety in the molecule, such as 3-isocyanatetopropyltriethoxysilane and / or hydrolysis condensates of 3-isocyanatetopropyltriethoxysilane. These may be used individually or in combination of two or more.
[0096] From the viewpoint of storage stability of the first coating composition of this embodiment, the isocyanate compound is more preferably a blocked polyisocyanate compound obtained by reacting an isocyanate group with a blocking agent. The blocked polyisocyanate compound is not particularly limited, but any compound that functions as a crosslinking agent can be appropriately selected, and is not limited to the following, but examples include oxime compounds, alcohol compounds, acid amide compounds, acid imide compounds, phenol compounds, amine compounds, active methylene compounds, imidazole compounds, and pyrazole compounds. Examples of oxime compounds are not limited to the following, but examples include formaldehyde oxime, acetaldehyde oxime, acetoxime, methyl ethyl ketoxime, and cyclohexanone oxime. Examples of alcohol compounds are not limited to the following, but examples include methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol. Examples of acid amide compounds include, but are not limited to, acetanilide, acetic acid amide, ε-caprolactam, δ-valerolactam, and γ-butyrolactam. Examples of acid imide compounds include, but are not limited to, succinimide and maleimide. Examples of phenolic compounds include, but are not limited to, phenol, cresol, ethylphenol, butylphenol, nonylphenol, dinonylphenol, styrene-phenol, and hydroxybenzoic acid esters. Examples of amine compounds include, but are not limited to, diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, and isopropylethylamine. Examples of active methylene compounds include, but are not limited to, dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone. Examples of imidazole compounds include, but are not limited to, imidazole and 2-methylimidazole.Examples of pyrazole compounds include, but are not limited to, pyrazole, 3-methylpyrazole, and 3,5-dimethylpyrazole.
[0097] From the viewpoint of water dispersibility, the blocked polyisocyanate compound is preferably obtained by reacting a water-dispersible isocyanate compound, which is produced by reacting a polyisocyanate compound having two or more isocyanate groups in one molecule with a hydroxyl group-containing hydrophilic compound having nonionic and / or ionic hydrophilic groups, in an isocyanate group / hydroxyl group equivalent ratio of 1.05 to 1000, with the blocking agent. The water-dispersible blocked polyisocyanate compound is not particularly limited, and commercially available products can be used. For example, WT30-100 and WM44-L70G manufactured by Asahi Kasei Corporation are preferably used as they possess the above-described characteristics.
[0098] (Biphenyltriazine skeleton UV absorber (E)) The first coating composition of this embodiment preferably contains a biphenyltriazine skeleton UV absorber (E) from the viewpoint of improving weather resistance. Examples of biphenyltriazine-based UV absorbers include, but are not limited to, 2,4,6-tri([1,1'-biphenyl]-4-yl)-1,3,5-triazine, 2,4,6-tri([1,1'-biphenyl]-3-yl)-1,3,5-triazine, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (BASF trade name "TINUVIN 479"), TINUVIN 1600 (trade name, BASF), 2-(biphenyl-4-yl)-4-chloro-6-phenyl-1,3,5-triazine, and 4,4'-bis(4,6 Examples include (-diphenyl-1,3,5-triazine-2-yl)biphenyl, 2-[3'-bromo[1,1'-biphenyl]-3-yl]-4,6-diphenyl-1,3,5-triazine, etc.
[0099] The first coating composition of this embodiment may contain ultraviolet absorbers other than the biphenyltriazine skeleton ultraviolet absorber (E) from the viewpoint of improving weather resistance. Such ultraviolet absorbers are not limited to the following, but include, for example, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2 Benzophenone-based UV absorbers such as '-dihydroxy-4,4'-dimethoxybenzophenone (BASF trade name "UVINUL 3049"), 2,2',4,4'-tetrahydroxybenzophenone (BASF trade name "UVINUL 3050"), 4-dodecyloxy-2-hydroxybenzophenone, 5-benzoyl-2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2-hydroxy-4-stearyloxybenzophenone, and 4,6-dibenzoylresortinol;2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-di-tert-octylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α'-dimethylbenzyl)phenyl] Condensate of benzotriazole, methyl-3-[3-tert-butyl-5-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]propionate and polyethylene glycol (molecular weight 300) (BASF trade name "TINUVIN 1130"), isooctyl-3-[3-(2H-benzotriazole-2-yl)-5-tert-butyl-4-hydroxyphenyl]propionate (BASF trade name "TINUVIN 384"), 2-(3-dodecyl-5-methyl-2-hydroxyphenyl) Nyl)benzotriazole (BASF brand name "TINUVIN 571"), 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-4'-octoxyphenyl)benzotriazole, 2-[2'-hydroxy-3'-(3'',4'',5'',6''-tetrahydrophthalimidomethyl)-5'-methylphenyl]benzotriazole, Benzotriazole-based UV absorbers such as 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazole-2-yl)phenol], 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (BASF trade name "TINUVIN 900"), TINUVIN 384-2, TINUVIN 326, TINUVIN 327, TINUVIN 109, TINUVIN 970, TINUVIN 328, TINUVIN 171, TINUVIN 970, TINUVIN PS, TINUVIN P, TINUVIN 99-2, TINUVIN 928 (trade names, manufactured by BASF);Triazine-based UV absorbers such as 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bisbutyloxyphenyl)-1,3,5-triazine (BASF trade name "TINUVIN 460"), TINUVIN 400, TINUVIN 405, TINUVIN 477, etc.; HOSTAVIN PR25, HOSTAVIN B-CAP, HOSTAVIN Examples include malonic acid ester-based UV absorbers such as VSU (trade name, manufactured by Clariant); anilide-based UV absorbers such as HOSTAVIN 3206 LIQ, HOSTAVIN VSU P, and HOSTAVIN 3212 LIQ (trade names, manufactured by Clariant); and salicylate-based UV absorbers such as amyl salicylate, menthyl salicylate, homomenthyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-isopropanolphenyl salicylate.
[0100] In the first paint composition of this embodiment, from the viewpoint of weather resistance, the content of the biphenyltriazine skeleton ultraviolet absorber (E) in the first paint composition is preferably 0.3% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.7% by mass or more. On the other hand, from the viewpoint of storage stability of the first paint composition of this embodiment, it is preferably 20% by mass or less, preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0101] (Solvent) The first paint composition of this embodiment may contain a solvent. From the viewpoint of hygiene at the work site and reducing the burden on the global environment, it is preferable that 50% by mass or more of the solvent is water. Other than water, there are no particular limitations on the solvents that can be used, and general solvents can be used. Other solvents besides water include, but are not limited to, alcohols such as ethylene glycol, butyl cellosolve, isopropanol, n-butanol, 2-butanol, ethanol, methanol, denatured ethanol, 2-methoxy-1-propanol, 1-methoxy-2-propanol, diacetone alcohol glycerin, monoalkyl monoglyceryl ether, propylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, diethylene glycol monophenyl ether, tetraethylene glycol monophenyl ether, etc.; aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as hexane, cyclohexane, and heptane; esters such as ethyl acetate and n-butyl acetate; amides such as dimethylacetamide and dimethylformamide; halogen compounds such as chloroform, methylene chloride, and carbon tetrachloride; dimethyl sulfoxide, nitrobenzene, etc. These may be used individually or in combination of two or more.
[0102] The first coating composition of this embodiment may contain an aprotic organic solvent in the solvent. The aprotic organic solvent allows the emulsion particles (A) and the ultraviolet absorber (E) to be compatible, enabling the ultraviolet absorber (E) to be stably dispersed in the first coating composition, resulting in a tendency for excellent storage stability. Furthermore, it is preferable that the boiling point of the contained aprotic organic solvent is less than 100°C. This suppresses substrate degradation due to the organic solvent, and as a result, the second coating composition, described later, tends to have excellent transparency when forming a coating film. Examples of aprotic organic solvents are, but are not limited to, ethers such as tetrahydrofuran (THF), dimethoxyethane (DME), 2-methyltetrahydrofuran (2-MeTHF), tetrahydropyran, diethyl ether, t-butyl methyl ether, and diisopropyl ether; esters such as methyl acetate, ethyl acetate, and propyl acetate; ketones such as acetone; and acetonitrile.
[0103] If the first coating composition of this embodiment contains the aprotic organic solvent as a solvent, the content of the aprotic organic solvent is preferably 0.1% to 30% by mass in the first coating composition. When the content of the aprotic organic solvent in the first coating composition is 30% by mass or less, it is possible to prevent the substrate surface from dissolving due to the aprotic organic solvent when the first coating composition is applied to the substrate, and the transparency of the coating films of the first and second coating compositions tends to be excellent.
[0104] (Light stabilizer) The first paint composition of this embodiment may contain a light stabilizer from the viewpoint of improving weather resistance. The light stabilizer is not limited to the following, but examples include bis(2,2,6,6-tetramethyl-4-piperidyl) succinate, bis(2,2,6,6-tetramethylpiperidyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-butylmalonate, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propynyloxy]ethyl]-4-[3-(3,5-di-tert-butyl [-4-hydroxyphenyl)propynyloxy]-2,2,6,6-tetramethylpiperidine, a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and methyl-1,2,2,6,6-pentamethyl-4-piperidyl-sebacate (BASF trade name "TINUVIN 292"), bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidyl) sebacate, TINUVIN 123, TINUVIN 144, TINUVIN 152, TINUVIN 249, TI Hindered amine-based light stabilizers such as NUVIN 292 and TINUVIN 5100 (trade names, manufactured by BASF); 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, 1,2,2,6,6-pentamethyl-4-piperidyl acrylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, 2,2,6,6-tetramethyl-4-piperidyl acrylate, 1,2,2,6,6-pentamethyl-4-iminopiperidyl methacrylate, 2,2,6,6-tetramethyl-4-imino Examples include radical polymerizable hindered amine-based light stabilizers such as piperidyl methacrylate, 4-cyano-2,2,6,6-tetramethyl-4-piperidyl methacrylate, and 4-cyano-1,2,2,6,6-pentamethyl-4-piperidyl methacrylate; and photostable polymers such as U-double E-133, U-double E-135, U-double S-2000, U-double S-2834, U-double S-2840, U-double S-2818, and U-double S-2860 (trade names, manufactured by Nippon Shokubai Co., Ltd.).
[0105] From the viewpoint of improving weather resistance, the aforementioned light stabilizer is preferably present in an amount of 1 part by mass or more, and more preferably 5 parts by mass or more, per 100 parts by mass of the total amount of ultraviolet absorbers contained in the first paint composition of this embodiment.
[0106] (Other components) Depending on the application, the first paint composition of this embodiment may also contain emulsifiers, plasticizers, pigments, dyes, fillers, antioxidants, conductive materials, light stabilizers, release modifiers, softeners, surfactants, flame retardants, antioxidants, and catalysts.
[0107] [Physical Properties of the First Paint Composition] (Average Particle Size of the First Paint Composition) The average particle size calculated by dynamic light scattering when the first paint composition of this embodiment is diluted 50 times with deionized water is preferably 150 nm or less. When the average particle size is within the above range, the paint using the first paint composition of this embodiment tends to have excellent storage stability, as the components in the first paint composition are less likely to settle naturally. Furthermore, from the viewpoint of further improving storage stability and the transparency of the coating film, it is even more preferable that the average particle size is 100 nm or less. The average particle size by dynamic light scattering can be measured by the method described in the examples below.
[0108] (pH of the first paint composition) The first paint composition of this embodiment has a pH of 9.5 or higher. Having a pH within the above range improves the dispersibility of emulsion particles (A), and as a result, the storage stability of the paint using the first paint composition of this embodiment tends to improve. Furthermore, in the room-temperature drying process after painting of the paint using the first paint composition of this embodiment, it is possible to suppress viscosity increase due to abnormal aggregation, and it is possible to reduce unevenness in the paint film and drip marks. The pH of the first paint composition of this embodiment is preferably 10.0 or higher, and more preferably 10.5 or higher. The pH of the first paint composition can be measured, for example, with a pH meter (HM-25R type) manufactured by Toa DKK Co., Ltd. Also, the pH can be controlled to the above range by, for example, adding the aforementioned amine compound.
[0109] (Solid content concentration of the first paint composition) From the viewpoint of paintability, the solid content concentration of the first paint composition of this embodiment is preferably 5 to 50.0% by mass. Furthermore, from the viewpoint of storage stability of the first paint composition of this embodiment, the solid content concentration is more preferably 10.0 to 40.0% by mass, and even more preferably 15.0 to 30.0% by mass.
[0110] (Second paint composition) In this embodiment, when the paint composition includes the first paint composition and the second paint composition, the first paint composition acts as a primer and contributes to improving the adhesion between the coating film of the first paint composition and the coating film of the second paint composition. In this embodiment, the first paint composition is applied to a substrate, and the second paint composition is applied on the coating film of the first paint composition to form a coating film of the second paint composition.
[0111] The second paint composition is not particularly limited, but includes polymer nanoparticles (F) described later and a matrix raw material component (G), wherein the matrix raw material component (G) contains an inorganic oxide (H).
[0112] The polymer nanoparticles (F) are not particularly limited, but preferably contain a hydrolyzable silicon compound (f). The hydrolyzable silicon compound (f) is not particularly limited as long as it is a hydrolyzable silicon compound, its hydrolysis product, or condensate.
[0113] From the viewpoint of improving wear resistance and weather resistance, the hydrolyzable silicon compound (f) is preferably a compound containing the atomic group represented by the following formula (f-1), its hydrolysis product, and condensate. -R 1 n1 Six 1 3-n1 (f-1)
[0114] In formula (f-1), R 1 R represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkenyl group, an alkynyl group, or an aryl group. 1 X may have substituents containing halogen, hydroxyl, mercapto, amino, (meth)acryloyl, or epoxy groups. 1n1 represents a hydrolyzable group, and n1 represents an integer from 0 to 2. The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group upon hydrolysis. Examples of such groups include halogens, alkoxy groups, acyloxy groups, amino groups, phenoxy groups, and oxime groups.
[0115] Specific examples of compounds containing the atomic group represented by formula (f-1) are not limited to the following, but include, for example, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isobutyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, decyltri Ethoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(triphenoxysilyl)ethane, 1,1-bis(triethoxysilyl 1,2-bis(triethoxysilyl)ethane, 1,1-bis(triethoxysilyl)propane, 1,2-bis(triethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(triethoxysilyl)pentane, 1,1-bis(trimethoxysilyl)ethane, 1,2-bis(trimethoxysilyl)ethane, 1,1-bis(trimethoxysilyl)propane, 1,2-bis(trimethoxysilyl)propane, 1,3-bis(trimethoxysilyl) Xysilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,3-bis(triphenoxysilyl)propane, 1,4-bis(trimethoxysilyl)benzene, 1,4-bis(triethoxysilyl)benzene, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,7-bis(trimethoxysilyl)heptane, 1,7-bis(triethoxysilyl)heptane, 1,8-bis(trimethoxysilyl)octane, 1,8-Bis(triethoxysilyl)octane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3 - Methacryloxypropyltrimethoxysilane, 3-Methacryloxypropyltriethoxysilane, 3-Methacryloxypropylmethyldimethoxysilane, 3-Methacryloxypropylmethyldimethoxysilane, Vinyltrimethoxylane, Vinyltriethoxylan, p-Styryltrimethoxysilane, p-Styryltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxy Sisilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, 3-trimethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 3-triethoxysilyl-N-(1,3-Dimethyl-butylidene)propylamine, triacetoxysilane, tris(trichloroacetoxy)silane, tris(trifluoroacetoxy)silane, tris-(trimethoxysilylpropyl)isocyanurate, tris-(triethoxysilylpropyl)isocyanurate, methyltriacetoxysilane, methyltris(trichloroacetoxy)silane, trichlorosilane, tribromosilane, methyltrifluorosilane, tris(methylethylketoxime)silane, phenyltris(methylethylketoxime)silane, bis(methylethylketoxime)silane, methylbis(methylethylketoxime)silane, hexamethyldisilane, hexamethylcyclotrisilazane, bis Examples include bis(dimethylamino)dimethylsilane, bis(diethylamino)dimethylsilane, bis(dimethylamino)methylsilane, bis(diethylamino)methylsilane, 2-[(triethoxysilyl)propyl]dibenzylresorcinol, 2-[(trimethoxysilyl)propyl]dibenzylresorcinol, 2,2,6,6-tetramethyl-4-[3-(triethoxysilyl)propoxy]piperidine, 2,2,6,6-tetramethyl-4-[3-(trimethoxysilyl)propoxy]piperidine, 2-hydroxy-4-[3-(triethoxysilyl)propoxy]benzophenone, and 2-hydroxy-4-[3-(trimethoxysilyl)propoxy]benzophenone.
[0116] From the viewpoint of imparting high hardness to the coating film of the second paint composition and further improving wear resistance, the hydrolyzable silicon compound (f) preferably includes the compound represented by the following formula (f-2), its hydrolysis product, and condensate. SiX 2 4 (f-2) In formula (f-2), X 2 The symbol represents a hydrolyzable group. A hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group through hydrolysis, and examples include halogens, alkoxy groups, acyloxy groups, amino groups, phenoxy groups, and oxime groups.
[0117] Specific examples of compounds represented by formula (f-2) are, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetra(n-propoxy)silane, tetra(i-propoxy)silane, tetra(n-butoxy)silane, tetra(i-butoxy)silane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraacetoxysilane, tetra(trichloroacetoxy)silane, tetra(trifluoroacetoxy)silane, tetrachlorosilane, tetrabromosilane, tetrafluorosilane, tetra(methylethylketoxyme)silane, tetramethoxysilane, or tetraethoxysilane. Examples include partial hydrolysis condensates of ore (for example, "M-Silicate 51", "Silicate 35", "Silicate 45", "Silicate 40", and "FR-3" manufactured by Tama Chemical Industry Co., Ltd.; "MS51", "MS56", "MS57", and "MS56S" manufactured by Mitsubishi Chemical Corporation; and "Methyl Silicate 51", "Methyl Silicate 53A", "Ethyl Silicate 40", "Ethyl Silicate 48", "EMS-485", "N-103X", "PX", "PS-169", "PS-162R", "PC-291", "PC-301", "PC-302R", "PC-309", and "EMSi48" manufactured by Colcoat Co., Ltd.).
[0118] As described above, in this embodiment, it is preferable that the hydrolyzable silicon compound (f) includes one or more selected from compounds containing the atomic group represented by formula (f-1), their hydrolysis products and condensates, and compounds represented by formula (f-2), their hydrolysis products and condensates.
[0119] In this embodiment, the content of hydrolyzable silicon compound (f) refers to the solid weight percentage of hydrolyzable silicon compound (f) contained in polymer nanoparticles (F). A higher content is preferable from the viewpoint of improving abrasion resistance, weather resistance, and heat resistance, and the content is preferably 50% by mass or more, and more preferably 60% by mass or more. The content of hydrolyzable silicon compound (f) in polymer nanoparticles (F) is not limited to the following, but can be measured, for example, by IR analysis, NMR analysis, elemental analysis, etc. of the polymer nanoparticles (F).
[0120] (Matrix component (G)) By using the matrix component (G) in this embodiment, it is possible to impart shock absorption properties to the coating film of the second paint composition.
[0121] [Components of Matrix Component (G)] The matrix component (B) in this embodiment is not particularly limited as long as it is a component that can disperse polymer nanoparticles (A). In this embodiment, from the viewpoint of high toughness, it is preferable that the matrix component (G) contains a hydrolyzable silicon compound (g). In this specification, "the matrix component (G) contains a hydrolyzable silicon compound (g)" means that the matrix component (G) contains a polymer having constituent units derived from the hydrolyzable silicon compound (g). The hydrolyzable silicon compound (g) is not particularly limited as long as it is a silicon compound that is hydrolyzable, its hydrolysis products, and condensates. In addition to the polymer described above, the matrix component (G) may also contain various components other than polymer nanoparticles (F). Among these, other polymers that may be included besides the polymers mentioned above include water-soluble resins such as polyvinyl alcohol, polyethylene glycol, polyvinylpyrrolidone, and polyacrylic acid; acrylic resins such as PMMA, PAN, and polyacrylamide; polymers such as polystyrene, polyurethane, polyamide, polyimide, polyvinylidene chloride, polyester, polycarbonate, polyether, polyethylene, polysulfone, polypropylene, polybutadiene, PTFE, PVDF, and EVA; and copolymers thereof.
[0122] From the viewpoint of further improving abrasion resistance and weather resistance, the hydrolyzable silicon compound (g) preferably contains one or more compounds selected from the group consisting of compounds containing the atomic group represented by the following formula (g-1), their hydrolysis products, and condensates, and compounds represented by the following formula (g-2), their hydrolysis products, and condensates. -R 2 n2 Six 3 3-n2 (g-1) In formula (g-1), R 2 R represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkenyl group, an alkynyl group, or an aryl group.2 X may have substituents containing halogen, hydroxyl, mercapto, amino, (meth)acryloyl, or epoxy groups. 3 SiX represents a hydrolyzable group, and n2 represents an integer from 0 to 2. The hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group upon hydrolysis. Examples of such groups include halogen atoms, alkoxy groups, acyloxy groups, amino groups, phenoxy groups, and oxime groups. 4 4 (g-2) In formula (g-2), X 4 The symbol represents a hydrolyzable group. A hydrolyzable group is not particularly limited as long as it is a group that generates a hydroxyl group through hydrolysis. Examples of such groups include halogens, alkoxy groups, acyloxy groups, amino groups, phenoxy groups, and oxime groups.
[0123] Specific examples of compounds containing the atomic group represented by the general formula (g-1) are not limited to the following, but include trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, isobutyltriethoxysilane, hexyltrimethoxylane, hexyltriethoxylane, octyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, decyltriethoxy Sisilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxysilane, diethoxysilane, methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(triphenoxysilyl)ethane, 1,1-bis(triethoxysilyl) Ethane, 1,2-bis(triethoxysilyl)ethane, 1,1-bis(triethoxysilyl)propane, 1,2-bis(triethoxysilyl)propane, 1,3-bis(triethoxysilyl)propane, 1,4-bis(triethoxysilyl)butane, 1,5-bis(triethoxysilyl)pentane, 1,1-bis(trimethoxysilyl)ethane, 1,2-bis(trimethoxysilyl)ethane, 1,1-bis(trimethoxysilyl)propane, 1,2-bis(trimethoxysilyl)propane, 1,3-bis(trimethoxy Sisilyl)propane, 1,4-bis(trimethoxysilyl)butane, 1,5-bis(trimethoxysilyl)pentane, 1,3-bis(triphenoxysilyl)propane, 1,4-bis(trimethoxysilyl)benzene, 1,4-bis(triethoxysilyl)benzene, 1,6-bis(trimethoxysilyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,7-bis(trimethoxysilyl)heptane, 1,7-bis(triethoxysilyl)heptane, 1,8-bis(trimethoxysilyl)octane, 1,8-Bis(triethoxysilyl)octane, 3-chloropropyltrimethoxysilane, 3-chloropropyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3 - Methacryloxypropyltrimethoxysilane, 3-Methacryloxypropyltriethoxysilane, 3-Methacryloxypropylmethyldimethoxysilane, 3-Methacryloxypropylmethyldimethoxysilane, Vinyltrimethoxylane, Vinyltriethoxylan, p-Styryltrimethoxysilane, p-Styryltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxy Sisilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, 3-trimethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 3-triethoxysilyl-N-(1,3-Dimethyl-butylidene)propylamine, triacetoxysilane, tris(trichloroacetoxy)silane, tris(trifluoroacetoxy)silane, tris-(trimethoxysilylpropyl)isocyanurate, tris-(triethoxysilylpropyl)isocyanurate, methyltriacetoxysilane, methyltris(trichloroacetoxy)silane, trichlorosilane, tribromosilane, methyltrifluorosilane, tris(methylethylketoxime)silane, phenyltris(methylethylketoxime)silane, bis(methylethylketoxime)silane, methylbis(methylethylketoxime)silane, hexamethyldisilane, hexamethylcyclotrisilazane, bis Examples include bis(dimethylamino)dimethylsilane, bis(diethylamino)dimethylsilane, bis(dimethylamino)methylsilane, bis(diethylamino)methylsilane, 2-[(triethoxysilyl)propyl]dibenzylresorcinol, 2-[(trimethoxysilyl)propyl]dibenzylresorcinol, 2,2,6,6-tetramethyl-4-[3-(triethoxysilyl)propoxy]piperidine, 2,2,6,6-tetramethyl-4-[3-(trimethoxysilyl)propoxy]piperidine, 2-hydroxy-4-[3-(triethoxysilyl)propoxy]benzophenone, and 2-hydroxy-4-[3-(trimethoxysilyl)propoxy]benzophenone.
[0124] Specific examples of compounds represented by formula (g-2) are, but are not limited to, tetramethoxysilane, tetraethoxysilane, tetra(n-propoxy)silane, tetra(i-propoxy)silane, tetra(n-butoxy)silane, tetra(i-butoxy)silane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetraacetoxysilane, tetra(trichloroacetoxy)silane, tetra(trifluoroacetoxy)silane, tetrachlorosilane, tetrabromosilane, tetrafluorosilane, tetra(methylethylketoxyme)silane, tetramethoxysilane, or tetraethoxysilane. Examples include partial hydrolysis condensates of ore (for example, "M-Silicate 51", "Silicate 35", "Silicate 45", "Silicate 40", and "FR-3" manufactured by Tama Chemical Industry Co., Ltd.; "MS51", "MS56", "MS57", and "MS56S" manufactured by Mitsubishi Chemical Corporation; and "Methyl Silicate 51", "Methyl Silicate 53A", "Ethyl Silicate 40", "Ethyl Silicate 48", "EMS-485", "N-103X", "PX", "PS-169", "PS-162R", "PC-291", "PC-301", "PC-302R", "PC-309", and "EMSi48" manufactured by Colcoat Co., Ltd.).
[0125] As described above, in this embodiment, it is preferable that the hydrolyzable silicon compound (g) includes one or more selected from compounds containing the atomic group represented by formula (g-1), their hydrolysis products and condensates, and compounds represented by formula (g-2), their hydrolysis products and condensates.
[0126] In this embodiment, the "hydrolyzable silicon compound (f) contained in the polymer nanoparticle (F)" may be the same type as the "hydrolyzable silicon compound (g) contained in the matrix component (G)," or it may be a different type. Even if the two are the same type, they are distinguished by referring to the one contained in the polymer nanoparticle (F) as the hydrolyzable silicon compound (f) and the one contained in the matrix component (G) as the hydrolyzable silicon compound (g).
[0127] (Inorganic Oxide (H)) The matrix component (G) in this embodiment may contain an inorganic oxide (H). Including an inorganic oxide (H) tends to improve the hardness of the matrix component (G) and enhance its abrasion resistance. In addition, the hydrophilicity of the hydroxyl groups on the particle surface of the inorganic oxide (H) tends to improve the stain resistance of the coating film.
[0128] Specific examples of the inorganic oxide (H) in this embodiment include, but are not limited to, oxides of silicon, aluminum, titanium, zirconium, zinc, cerium, tin, indium, gallium, germanium, antimony, molybdenum, niobium, magnesium, bismuth, cobalt, and copper. These can be used individually or as a mixture, regardless of their form. From the viewpoint of interaction with the hydrolyzable silicon compound (g) mentioned above, the inorganic oxide (H) preferably further contains silica particles, such as dry silica or colloidal silica, and from the viewpoint of dispersibility, it is preferable that it further contains colloidal silica in the form of silica particles. When the inorganic oxide (H) contains colloidal silica, it is preferably in the form of an aqueous dispersion and can be used in either an acidic or basic solution. Furthermore, in this embodiment, it is preferable that the inorganic oxide (H) contains at least one inorganic component selected from the group consisting of Ce, Nb, Al, Zn, Ti, Zr, Sb, Mg, Sn, Bi, Co, and Cu (hereinafter simply referred to as "inorganic component"). The presence of inorganic oxides (H) in the inorganic components tends to improve weather resistance without impairing wear resistance and durability. Examples of commercially available products, though not limited to the following, include ultrafine particle material products of cerium oxide, zinc oxide, aluminum oxide, bismuth oxide, cobalt oxide, copper oxide, tin oxide, and titanium oxide manufactured by CIK Nanotech Co., Ltd.; and titanium oxide "Tynock" (trade name), cerium oxide "Needral" (trade name), tin oxide "Ceramase" (trade name), niobium oxide sol, and zirconium oxide sol manufactured by Taki Chemical Co., Ltd. From the viewpoint of improving weather resistance, it is preferable that the inorganic oxides (H) contain at least one inorganic component selected from the group consisting of Ce, Nb, Zn, Ti, and Zr, and it is more preferable that they contain Ce.In this embodiment, the inorganic oxide (H) preferably contains at least one inorganic oxide (H') selected from the group consisting of Ce, Nb, Zn, Ti, and Zr, from the viewpoint of balancing abrasion resistance, durability, and weather resistance. The content of the inorganic oxide (H') in the paint composition is not particularly limited, but from the viewpoint of balancing abrasion resistance, durability, and weather resistance, it is preferably 1% by mass or more, more preferably 2% by mass or more, and from the viewpoint of transparency, it is preferably 50% by mass or less, more preferably 30% by mass or less. Here, the above content can be specified as the total amount of Ce, Nb, Zn, Ti, and Zr when the solid content of the paint composition is 100% by mass.
[0129] In this embodiment, the average particle diameter of the inorganic oxide (H) is preferably 2 nm or more from the viewpoint of good storage stability of the second coating composition. From the viewpoint of good transparency, it is preferably 150 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less. For this reason, the average particle diameter is preferably 2 nm or more and 100 nm or less, and more preferably 2 nm or more and 50 nm or less. The method for measuring the average particle diameter of the inorganic oxide (H) is not limited to the following, but for example, it can be measured by observing water-dispersed colloidal silica using a transmission microscope at a magnification of 50,000 to 100,000 times, taking a photograph so that 100 to 200 inorganic oxide particles are captured, and measuring from the average value of the major and minor axes of the inorganic oxide particles.
[0130] The acidic colloidal silica used in this embodiment with water as the dispersion solvent is not particularly limited, but can be prepared by the sol-gel method or a commercially available product can be used. When preparing by the sol-gel method, refer to Werner Stober et al; J. Colloid and Interface Sci., 26, 62-69 (1968), Rickey D. Badley et al; Lang muir 6, 792-801 (1990), Journal of the Color Materials Association, 61[9] 488-493 (1988), etc. Examples of commercially available products include Snowtex-O, Snowtex-OS, Snowtex-OXS, Snowtex-O-40, Snowtex-OL, Snowtex-OYL, Snowtex-OUP, Snowtex-PS-SO, Snowtex-PS-MO, Snowtex-AK-XS, Snowtex-AK, Snowtex-AK-L, Snowtex-AK-YL, Snowtex-AK-PS-S (product names, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20Q (product name, manufactured by Asahi Denka Kogyo Co., Ltd.), Crevosol 20H12, and Crevosol 30CAL25 (product names, manufactured by Clariant Japan Co., Ltd.).
[0131] Furthermore, basic colloidal silica includes silica stabilized by the addition of alkali metal ions, ammonium ions, and amines, and is not particularly limited, but examples include Snowtex-20, Snowtex-30, Snowtex-XS, Snowtex-50, Snowtex-30L, Snowtex-XL, Snowtex-YL, Snowtex-ZL, Snowtex-UP, Snowtex-ST-PS-S, Snowtex-ST-PS-M, Snowtex-C, Snowtex-CXS, Snowtex-CM, Snowtex-N, Snowtex-NXS, Snowtex-NS, and Snowtex-N-4. Examples include 0 (product name, manufactured by Nissan Chemical Industries, Ltd.), Adelite AT-20, Adelite AT-30, Adelite AT-20N, Adelite AT-30N, Adelite AT-20A, Adelite AT-30A, Adelite AT-40, Adelite AT-50 (product name, manufactured by Asahi Denka Kogyo Co., Ltd.), Crevosol 30R9, Crevosol 30R50, Crevosol 50R50 (product name, manufactured by Clariant Japan Co., Ltd.), Rudox HS-40, Rudox HS-30, Rudox LS, Rudox AS-30, Rudox SM-AS, Rudox AM, Rudox HSA, and Rudox SM (product name, manufactured by DuPont).
[0132] Furthermore, while there are no particular limitations on colloidal silica using a water-soluble solvent as the dispersion medium, examples include MA-ST-M (methanol dispersion type with particle size of 20-25 nm), IPA-ST (isopropyl alcohol dispersion type with particle size of 10-15 nm), EG-ST (ethylene glycol dispersion type with particle size of 10-15 nm), EGST-ZL (ethylene glycol dispersion type with particle size of 70-100 nm), NPC-ST (ethylene glycol monopropyl ethere dispersion type with particle size of 10-15 nm), and TOL-ST (toluene dispersion type with particle size of 10-15 nm), all manufactured by Nissan Chemical Industries, Ltd.
[0133] Dry silica particles are not particularly limited, but examples include AEROSIL manufactured by Nippon Aerosil Co., Ltd. and Rheoroseal manufactured by Tokuyama Corporation.
[0134] Furthermore, these silica particles may contain inorganic bases (such as sodium hydroxide, potassium hydroxide, lithium hydroxide, and ammonia) or organic bases (such as tetramethylammonium and triethylamine) as stabilizers.
[0135] Furthermore, the shape of the inorganic oxide (H) in this embodiment is not limited to the following, but examples include spherical, angular, polyhedral, elliptical, flattened, linear, bead-like, and chain-like shapes, and a spherical shape is particularly preferred from the viewpoint of hardness and transparency of the coating film of the second paint composition.
[0136] [Functional group (e)] In this embodiment, the polymer nanoparticles (F) preferably have a functional group (e) that interacts with the matrix component (G), from the viewpoint of improving the dispersibility of the polymer nanoparticles (F) in the matrix component (G) and improving wear resistance. The presence of a functional group (e) in polymer nanoparticles (A) can be confirmed, for example, by compositional analysis using IR, GC-MS, pyrolysis GC-MS, LC-MS, GPC, MALDI-MS, TOF-SIMS, TG-DTA, NMR, and combinations thereof.
[0137] Specific examples of the functional group (e) in this embodiment include, but are not limited to, a hydroxyl group, a carboxyl group, an amino group, an amide group, and a functional group consisting of an ether bond. From the viewpoint of interaction, it is preferable that the functional group has hydrogen bonds, and from the viewpoint of high hydrogen bonding ability, it is more preferable that it is an amide group, and even more preferable that it is a secondary amide group and / or a tertiary amide group.
[0138] Compounds containing functional group (e) and their reaction products include, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl vinyl ether or 4-hydroxybutyl vinyl ether, 2-hydroxyethyl allyl ether, (meth)acrylic acid, 2-carboxyethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-diethylaminoethyl (meth)acrylate, 2-di-n-propylaminoethyl (meth)acrylate, 3-dimethylaminopropyl (meth)acrylate, 4-dimethylaminobutyl (meth)acrylate, N-[2-(meth)acryloyloxy]ethylmorpholine, vinylpyridine, N-vinylcarbazole, N-vinylquinoline, N-methylacrylamide, N-methylmethacrylamide Luamide, N-ethylacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N-ethylmethacrylamide, N-methyl-N-ethylacrylamide, N-methyl-N-ethylmethacrylamide, N-isopropylacrylamide, N-n-propylacrylamide, N-isopropylmethacrylamide, N-n-propylmethacrylamide, N-methyl-N-n-propylacrylamide, N-methyl-N-isopropylacrylamide, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylhexahydroazepine, N-acryloylmorpholine, N-methacryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N,N'-methylenebisacrylamide, N,Examples include N'-methylenebismethacrylamide, N-vinylacetamide, diacetone acrylamide, diacetone methacrylamide, N-methylolacrylamide, N-methylolmethacrylamide, Bremmer PE-90, PE-200, PE-350, PME-100, PME-200, PME-400, AE-350 (trade names, manufactured by Nippon Oil & Fats Co., Ltd.), MA-30, MA-50, MA-100, MA-150, RA-1120, RA-2614, RMA-564, RMA-568, RMA-1114, MPG130-MA (trade name, manufactured by Nippon Emulsifier Co., Ltd.). In this specification, (meth)acrylate is a convenient notation for acrylate or methacrylate, and (meth)acrylic acid is a convenient notation for acrylic acid or methacrylic acid.
[0139] [Core / Shell Structure of Polymer Nanoparticles (F)] In this embodiment, polymer nanoparticles (F) preferably have a core / shell structure comprising a core layer and one or more shell layers covering the core layer. From the viewpoint of interaction with the matrix component (G) in the outermost layer of the core / shell structure, polymer nanoparticles (F) preferably have a functional group (e).
[0140] [Other compounds that may be included in polymer nanoparticles (F)] The polymer nanoparticles (F) according to this embodiment may include the following polymers from the viewpoint of improving particle stability by providing electrostatic repulsion between particles. For example, polymers of polyurethane, polyester, poly(meth)acrylate, poly(meth)acrylic acid, polyvinyl acetate, polybutadiene, polyvinyl chloride, chlorinated polypropylene, polyethylene, or polystyrene, or copolymers of poly(meth)acrylate-silicone, polystyrene-(meth)acrylate, or styrene-maleic anhydride.
[0141] Among the polymers that may be included in the polymer nanoparticles (F) described above, polymers or copolymers of (meth)acrylic acid and (meth)acrylate are particularly excellent in terms of electrostatic repulsion. Specific examples, though not limited to those listed below, include polymers or copolymers of methyl acrylate, (meth)acrylic acid, methyl methacrylate, butyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl acrylate, n-butyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. In this case, to further improve the electrostatic repulsion force, part or all of the (meth)acrylic acid may be neutralized with amines such as ammonia, triethylamine, or dimethylethanolamine, or bases such as NaOH or KOH.
[0142] Furthermore, the polymer nanoparticles (F) may contain an emulsifier. The emulsifier is not particularly limited and includes, for example, acidic emulsifiers such as alkylbenzene sulfonic acid, alkyl sulfonic acid, alkyl sulfosuccinic acid, polyoxyethylene alkyl sulfate, polyoxyethylene alkylaryl sulfate, and polyoxyethylene distyrylphenyl ether sulfonic acid; anionic surfactants such as alkali metal (Li, Na, K, etc.) salts of acidic emulsifiers, ammonium salts of acidic emulsifiers, and fatty acid soaps; cationic surfactants of the quaternary ammonium salt, pyridinium salt, and imidazolinium salt type such as alkyltrimethylammonium bromide, alkylpyridinium bromide, and imidazolinium laurate; nonionic surfactants such as polyoxyethylene alkylaryl ether, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene oxypropylene poroc copolymer, and polyoxyethylene distyrylphenyl ether, as well as reactive emulsifiers having radically polymerizable double bonds.
[0143] The reactive emulsifier having a radically polymerizable double bond is not limited to the following, but examples include: Eleminor JS-2 (trade name, manufactured by Sanyo Chemical Industries, Ltd.), Latemul S-120, S-180A or S-180 (trade name, manufactured by Kao Corporation), Aqualon HS-10, KH-1025, RN-10, RN-20, RN30, RN50 (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adekarya Soap SE1025, SR-1025, NE-20, N Examples include E-30, NE-40 (product names, manufactured by Asahi Denka Kogyo Co., Ltd.), ammonium salts of p-styrenesulfonic acid, sodium salts of p-styrenesulfonic acid, potassium salts of p-styrenesulfonic acid, alkyl sulfonic acid (meth)acrylates such as 2-sulfoethyl acrylate, methylpropanesulfonic acid (meth)acrylamide, ammonium salts of allylsulfonic acid, sodium salts of allylsulfonic acid, and potassium salts of allylsulfonic acid.
[0144] [Other Components] Depending on the application, the second coating composition of this embodiment may also contain, as a matrix component (G), a solvent, emulsifier, plasticizer, pigment, dye, filler, antioxidant, conductive material, ultraviolet absorber, light stabilizer, release modifier, softener, surfactant, flame retardant, antioxidant, catalyst, thickener, leveling agent, thixotropizing agent, defoamer, freeze stabilizer, dispersant, wetting agent, rheology control agent, film-forming aid, rust inhibitor, plasticizer, lubricant, preservative, mold inhibitor, antistatic agent, and antistatic agent.
[0145] The second coating composition in this embodiment preferably contains a solvent. The usable solvent is not particularly limited, and general solvents can be used. The solvent is not limited to the following, but for example, water; ethylene glycol, butyl cellosolve, isopropanol, n-butanol, 2-butanol, ethanol, methanol, denatured ethanol, 2-methoxy-1-propanol, 1-methoxy-2-propanol, diacetone alcohol glycerin, monoalkyl monoglyceryl ether, propylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, diethylene glycol mono Examples include alcohols such as phenyl ether, tetraethylene glycol, and monophenyl ether; aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as hexane, cyclohexane, and heptane; esters such as ethyl acetate and n-butyl acetate; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as tetrahydrofuran and dioxane; amides such as dimethylacetamide and dimethylformamide; halogen compounds such as chloroform, methylene chloride, and carbon tetrachloride; dimethyl sulfoxide and nitrobenzene; and these may be used individually or in combination of two or more. Among these, it is particularly preferable to include water and alcohols from the viewpoint of reducing the environmental burden during solvent removal.
[0146] In the second paint composition, the volume fraction of polymer nanoparticles (F) relative to the total of polymer nanoparticles (F) and matrix raw material components (G) is preferably 2% or more, more preferably 3% or more, and even more preferably 5% or more from the viewpoint of film formation, and preferably 80% or less, more preferably 70% or less, and even more preferably 45% or less from the viewpoint of transparency. The volume fraction of polymer nanoparticles (F) in the second paint composition can be calculated, for example, from the component ratio of polymer nanoparticles (F) in the components constituting the second paint composition.
[0147] [Physical Properties of the Second Coating Composition] (Solid Content Concentration of the Second Coating Composition) From the viewpoint of paintability, the preferred solid content concentration of the second coating composition is 5.0 to 50.0% by mass, more preferably 10.0 to 40.0% by mass, and even more preferably 15.0 to 30.0% by mass.
[0148] (Applications of the Painting Method) The painting method of this embodiment allows for the uniform application of the paint composition. As a result, a paint film with uniform physical properties such as crack resistance, transparency, heat resistance, and abrasion resistance can be obtained. Therefore, the applications of the painting method of this embodiment are not particularly limited, but include, for example, painting of building materials, vehicle components, electronic equipment, and electrical products. In particular, it can be suitably used for painting vehicle components. Examples of applications for building materials are not limited to the following, but include, for example, window glass of construction machinery, window glass of buildings, houses, greenhouses, roofs of garages and arcades, lighting fixtures such as lights and traffic lights, wallpaper, signs, sanitary products such as bathtubs and washbasins, exterior wall materials for kitchens, flooring materials, cork, tiles, cushion flooring, and interior flooring materials such as linoleum. Examples of applications for vehicle components are not limited to the following, but include, for example, parts used in automobiles, aircraft, and trains. Specific examples include painting on various glass components such as the front, rear, front doors, rear doors, rear quarter windows, and sunroof; exterior components such as the front and rear bumpers, spoilers, door mirrors, front grilles, emblem covers, and body; interior components such as the center panel, door panels, instrument panel, and center console; components for lamps such as headlamps and taillamps; lens components for in-vehicle cameras; lighting covers; decorative films; and various glass substitute components. Examples of electronic devices and electrical products, though not limited to those listed below, include painting on mobile phones, personal digital assistants, personal computers, portable game consoles, office automation equipment, solar cells, flat panel displays, touch panels, optical discs such as DVDs and Blu-ray discs, optical components such as polarizing plates, optical filters, lenses, prisms, and optical fibers, and optical films such as anti-reflective films, alignment films, polarizing films, and phase difference films.
[0149] The embodiment will be described in more detail below with reference to examples, but the embodiment is not limited in any way by these examples.
[0150] (Method for measuring the physical properties of paint compositions) (Shear rate of paint composition at 25°C, 1 s) -1 (Shear viscosity relative to) Shear rate of paint composition at 25°C 1s -1 The shear viscosity was measured at 25°C using a rotary rheometer (product name: MCR302e, manufactured by Anton Paar). A cone plate (CP50-1D) was used for the measurement. The paint composition was dropped onto the measurement area of the apparatus, the gap between the dropping area and the cone plate was set to 0.1 mm, and after covering with a Peltier-type hood, the shear rate was set to 1 s. -1 The shear viscosity value was measured after 10 seconds of applying shear force. This shear viscosity value was then compared to the paint composition at a shear rate of 1 s at 25°C. -1 This was defined as the shear viscosity relative to [value].
[0151] (Shear rate of 1 s after holding the paint composition at 65°C for 300 seconds) -1 (Shear viscosity relative to) Shear rate 1s after holding the paint composition at 65°C for 300 seconds -1 The shear viscosity was measured at 65°C using a rotary rheometer (product name: MCR302e, manufactured by Anton Paar). A parallel plate (PP50) was used for the measurement. The measurement area of the apparatus was preheated to 65°C, the paint composition was dropped onto the measurement area, and shear was applied 300 seconds after dropping (0 seconds). Before applying shear, the gap between the shear drop area and the parallel plate was set to 1 mm and covered with a Peltier-type hood. 300 seconds after dropping, the shear rate was set to 1 s. -1 The shear viscosity value was measured 10 seconds after applying shear force. This shear viscosity value was then measured at a shear rate of 1 s after holding the paint composition at 65°C for 300 seconds. -1 This was defined as the shear viscosity relative to [value].
[0152] (Shear rate of 1 s after holding the paint composition at 45°C for 20 seconds) -1 (Shear viscosity relative to) Shear rate 1s after holding the paint composition at 45°C for 20 seconds -1The shear viscosity was measured at 45°C using a rotary rheometer (product name: MCR302e, manufactured by Anton Paar). A cone plate (CP50-1D) was used for the measurement. The measurement area of the apparatus was preheated to 45°C, the paint composition was dropped onto the measurement area, and shear was applied 20 seconds after dropping (0 seconds). Before applying shear, the gap between the shear drop area and the cone plate was set to 0.1 mm and covered with a Peltier-type hood. 20 seconds after dropping, the shear rate was set to 1 s. -1 The shear viscosity value was measured after applying shear force for 10 seconds. This shear viscosity value was then measured at a shear rate of 1 s after holding the paint composition at 45°C for 20 seconds. -1 This was defined as the shear viscosity relative to [value].
[0153] (Preparation of the first paint composition) (Preparation of emulsion particles (A)) Polymerization was carried out at 85°C using a general emulsion polymerization method with a monomer mixture prepared by dissolving 650.00 g of ion-exchanged water, 38.46 g of 10% dodecylbenzenesulfonic acid aqueous solution, 96.15 g of 2% ammonium persulfate aqueous solution, 1.92 g of Aqualon KH-1025 (reactive emulsifier manufactured by Daiichi Kogyo Seiyaku Co., Ltd., solid content concentration 25%), 1.92 g of Adekarya Soap SR-1025 (reactive emulsifier manufactured by ADEKA Corporation, solid content concentration 25%), and 9.62 g of the ultraviolet-absorbing vinyl monomer "RUVA-93" (trade name, manufactured by Otsuka Chemical Co., Ltd.) in a mixture of 122.12 g of butyl acrylate, 57.69 g of 2-hydroxyethyl methacrylate, 1.92 g of acrylic acid, and 1.92 g of 1-dodecanethiol. After polymerization, the mixture was filtered through a 100-mesh wire mesh, and the solid content concentration was adjusted to 20% by mass with deionized water to obtain an aqueous dispersion of emulsion particles (A). The average particle size of the obtained emulsion particles (A) was 45.1 nm, and the weight-average molecular weight of unit (a) was 110,000.
[0154] (Preparation of the first paint composition) Mix 21.46 g of deionized water, 153.13 g of aqueous dispersion of emulsion particles (A), 354.17 g of aqueous dispersion colloidal silica "Snowtex PS-SO" (trade name, manufactured by Nissan Chemical Industries, Ltd., solid content 15% by mass) as metal oxide fine particles, 37.50 g of WM44-L70G (trade name, manufactured by Asahi Kasei Corporation, solid content concentration 70% by mass, effective NCO 5.3% by mass) as a crosslinking agent, and 25.00 g of 1-methylpiperidine as a neutralizing agent. The aqueous dispersion of the obtained emulsion particles was mixed with 12.50 g of Tinuvin 479 (trade name, manufactured by BASF Japan Ltd., 100% solids content) as an ultraviolet absorber, 2.50 g of Tinuvin 123 (trade name, manufactured by BASF Japan Ltd., 100% solids content) as a light stabilizer, and 393.75 g of tetrahydrofuran as an aprotic organic solvent. This mixture was mixed at room temperature for 1 hour to obtain the first paint composition precursor. Subsequently, distillation was carried out until the ratio of aprotic organic solvent in the paint was less than 1.0% by mass, and then deionized water was added to adjust the solids content to 20.0% to obtain the first paint composition. The pH of the first paint composition was 10.0, and the average particle size was 83.0 nm. The first paint composition was subjected to a shear rate of 1 s at 25°C. -1 The shear viscosity for this is 5 mPa·s, and the shear rate after holding at 65°C for 300 seconds is 1 s. -1 The shear viscosity for this was 89 mPa·s, and the shear rate was 1 s after holding at 45°C for 20 seconds. -1 The shear viscosity for this was 17 mPa·s.
[0155] (Preparation of the second paint composition) (Preparation of polymer nanoparticles (F)) Polymerization was carried out in a reactor equipped with a reflux condenser, a dropping tank, a thermometer and a stirrer, using 1500 g of deionized water, 45 g of 10% dodecylbenzenesulfonic acid aqueous solution, 105 g of methyltrimethoxysilane, 23 g of phenyltrimethoxysilane and 27 g of tetraethoxysilane, at an environment of 50°C using a general emulsion polymerization method. After polymerization, the temperature was raised to 80°C, and then polymerization was carried out again using 43 g of 2% ammonium persulfate aqueous solution, 11 g of butyl acrylate, 12 g of diethylacrylamide, 1 g of acrylic acid and 1 g of 3-methacryloxypropyltrimethoxysilane, using a general emulsion polymerization method, and filtered through a 100 mesh wire mesh to obtain an aqueous dispersion of polymer nanoparticles (F). The obtained polymer nanoparticles (F) had a core-shell structure, an average particle size of 60 nm, and a solid content of 5.9% by mass.
[0156] (Preparation of Matrix Raw Material Component (G)) As hydrolyzable silicon compound (g), 66 g of trimethoxysilane and 63 g of tetraethoxysilane, and as inorganic oxide (H), 333 g of water-dispersed colloidal silica "Snowtex OXS" (trade name, manufactured by Nissan Chemical Industries, Ltd., solid content 10% by mass, average particle size 5 nm) were mixed under room temperature conditions to obtain matrix raw material component (G).
[0157] (Preparation of the second paint composition) The polymer nanoparticle (F) aqueous dispersion prepared above and the matrix raw material component (G) prepared above were mixed so that the solid content mass ratio of polymer nanoparticles (F) to matrix component (G) was (F):(G) = 100:400 to obtain a mixture. An aqueous solution of ethanol with a concentration of 20% by mass was used as a solvent, and the mixture was added so that the solid content concentration was 13% by mass to obtain the second paint composition. The shear rate of the second paint composition at 25°C was 1 s. -1 The shear viscosity for this is 6 mPa·s, and the shear rate after holding at 65°C for 300 seconds is 1 s. -1 The shear viscosity for this was 65 mPa·s, and the shear rate was 1 s after holding at 45°C for 20 seconds. -1 The shear viscosity for this was 5 mPa·s.
[0158] [Example 1] A polycarbonate sheet (manufactured by Takiron Co., Ltd., product number 1600, thickness: 6 mm, length 900 mm (vertical direction), width 160 mm (horizontal direction)) was placed as a base material in the vertical direction (with the horizontal direction being 0 degrees, the upper end of the base material (the end opposite to the direction in which gravity acts) was used as the pivot point at a 90-degree angle). As shown in Figure 1, with the upper end of the base material set as 0, a perpendicular line was drawn from the upper end to the lower end. The distance from the upper end to the lower end (the end on the side in the direction in which gravity acts) was set to 100. At a point where the distance from the upper end is 30, a line perpendicular to the perpendicular line was drawn. The area from this perpendicular line to the upper end was heated using an infrared heater (manufactured by Metro Electric Industry Co., Ltd., model number KMB-2030-F1). In this process, with the distance from the top to the bottom of the substrate (the end on the side where gravity acts) set to 100, thermocouples were pre-installed at points 10 and 90 degrees Celsius from a point pointing to the center of the substrate, respectively. The temperature T1 of the upper part of the heated substrate and the temperature T2 of the lower part were measured, and it was confirmed that T1 was 70°C and T2 was 25°C. Next, the first paint composition was applied to the heated substrate by flow coating. The coating conditions were to discharge the first paint composition from a flow nozzle at a flow rate of 5 L / min and pour it over the top of the heated substrate for 1 minute. After that, the substrate was left to stand in a hot air convection dryer set to 130°C for 60 minutes to dry the first paint composition and obtain a coating film of the first paint composition. The thickness of the obtained coating film of the first paint composition was measured at the same locations where temperatures T1 and T2 were measured. In other words, the location where temperature T1 was measured is the location where the thickness of the upper part of the coating film (L1) was measured, and the location where temperature T2 was measured is the location where the thickness of the lower part of the coating film (L2) was measured. The difference between the thickness of the upper and lower parts of the coating film (ΔL = L2 - L1) was then calculated. Furthermore, the slope of the coating film thickness (ΔL / (d2 - d1)) was calculated from the measurement location of temperature T1 (d1), the measurement location of temperature T2 (d2), and the difference in thickness. The results are shown in Table 1.
[0159] [Examples 2 and 3] A coating film of the first coating composition was obtained in the same manner as in Example 1, except that the temperature T1 at the top and the temperature T2 at the bottom of the substrate were changed to the temperatures shown in Table 1.
[0160] [Example 4] Except for changing the dimensions of the substrate to a length of 300 mm (vertical direction) and a width of 200 mm (horizontal direction), and changing the temperature T1 at the top and the temperature T2 at the bottom of the substrate to the temperatures listed in Table 1, a coating film of the first paint composition was obtained in the same manner as in Example 1.
[0161] [Examples 5-7] Except for using the second paint composition instead of the first paint composition, and changing the temperature T1 at the top and the temperature T2 at the bottom of the substrate to the temperatures shown in Table 1, a coating film of the second paint composition was obtained in the same manner as in Example 1.
[0162] [Example 8] A coating film of the second coating composition was obtained in the same manner as in Example 1, except that the dimensions of the substrate were changed to a length of 300 mm (vertical direction) and a width of 200 mm (horizontal direction), the second coating composition was used instead of the first coating composition, and the temperatures T1 at the top and T2 at the bottom of the substrate were changed to the temperatures shown in Table 1.
[0163] [Comparative Example 1] A coating film of the first coating composition was obtained by the same method as in Example 1, except that the substrate was not heated before coating with the first coating composition.
[0164] [Comparative Example 2] A coating film of the second coating composition was obtained in the same manner as in Example 1, except that the second coating composition was used instead of the first coating composition, and the substrate was not heated before applying the second coating composition.
[0165] [Comparative Example 3] A coating film of the first coating composition was obtained in the same manner as in Example 1, except that the dimensions of the substrate were changed to a length of 300 mm (vertical direction) and a width of 200 mm (horizontal direction), and the substrate was not heated before applying the first coating composition.
[0166] [Comparative Example 4] A coating film of the second coating composition was obtained in the same manner as in Example 1, except that the dimensions of the substrate were changed to a length of 300 mm (vertical direction) and a width of 200 mm (horizontal direction), the second coating composition was used instead of the first coating composition, and the substrate was not heated before applying the second coating composition.
[0167] For the coating films obtained in Examples 2-8 and Comparative Examples 1-4, the difference in thickness between the upper and lower parts of the coating film (ΔL) and the slope of the coating film thickness (ΔL / (d2-d1)) were calculated using the same method as in Example 1. The results are shown in Table 1.
[0168]
[0169] As shown in Table 1, the process comprises a heating step for heating a substrate and a coating step for applying a paint composition to the heated substrate. In the heating step, with the horizontal direction set to 0 degrees, the substrate is positioned at an angle (absolute value) greater than 0 degrees and less than or equal to 90 degrees, with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum. In the coating step, with the distance from the upper end to the lower end (the end on the side in the direction in which gravity acts) of the substrate set to 100, the temperature difference (T1-T2) between the temperature T1 of the upper part of the heated substrate (the point at a distance of 10 from the upper end) and the temperature T2 of the lower part (the point at a distance of 90 from the upper end) is 5°C or more, and the shear rate of the paint composition at 25°C is 1s. -1 In the coating methods of Examples 1 to 8, where the shear viscosity is 15 mPa·s or less, the thickness of the resulting coating film shows less variation in film thickness and a smaller gradient in film thickness compared to Comparative Examples 1 to 4, indicating that the paint composition is applied uniformly. More specifically, in comparisons between Examples 1 to 3 and 5 to 7 and Comparative Examples 1 and 2, and between Examples 4 and 8 and Comparative Examples 3 and 4, in all examples, the variation in film thickness and the gradient in film thickness are smaller, indicating that the paint composition is applied uniformly.
[0170] This application is based on Japanese Patent Application No. 2025-080626 filed on 13 May 2025, the contents of which are incorporated herein by reference.
[0171] 10...Substrate, 11...Upper end of the substrate, 12...Lower end of the substrate, 13...Heated surface of the substrate, 20...Heating device.
Claims
1. A painting method comprising: a heating step of heating a substrate; and a painting step of applying a paint composition to the heated substrate, wherein in the heating step, with the horizontal direction being 0 degrees, the substrate is positioned at an angle (absolute value) greater than 0 degrees and less than or equal to 90 degrees, with the upper end of the substrate (the end opposite to the direction in which gravity acts) as the fulcrum; in the painting step, with the distance from the upper end to the lower end (the end on the side in the direction in which gravity acts) of the substrate being 100, the temperature difference (T1-T2) between the temperature T1 of the upper part of the heated substrate (the point at a distance of 10 from the upper end) and the temperature T2 of the lower part (the point at a distance of 90 from the upper end) is 5°C or more; and the shear rate of the paint composition at 25°C is 1s -1 A painting method in which the shear viscosity is 15 mPa·s or less.
2. The painting method according to claim 1, wherein the heating step is performed under atmospheric pressure.
3. The coating method according to claim 1, wherein in the heating step, at least the upper part of the substrate is heated.
4. The painting method according to claim 1, wherein the heating step is performed by infrared heating.
5. The painting method according to claim 1, wherein the painting step is performed by a flow painting method.
6. The shear rate of the paint composition after being held at 65°C for 300 seconds is 1 s. -1 The coating method according to claim 1, wherein the shear viscosity with respect to is greater than 15 mPa·s.
7. The shear rate of the paint composition after being held at 45°C for 20 seconds is 1 s. -1 The coating method according to claim 1, wherein the shear viscosity with respect to is greater than 15 mPa·s.