Charge injection layer manufacturing device, charge injection layer manufacturing method, light-emitting element manufacturing device, and light-emitting element manufacturing method

By separately storing and immediately mixing charge transport and generating materials before application, the apparatus and method maintain device characteristics and prevent performance deterioration in organic EL devices.

WO2026240158A1PCT designated stage Publication Date: 2026-11-19CANON KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/018203
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-05-11
Filing Date
2026-05-14
Publication Date
2026-11-19

Smart Images

  • Figure JP2026018203_19112026_PF_FP_ABST
    Figure JP2026018203_19112026_PF_FP_ABST
Patent Text Reader

Abstract

This charge injection layer manufacturing device is provided with: a first tank accommodating a first liquid composition; a second tank accommodating a second liquid composition; a mixing unit for mixing the first liquid composition and the second liquid composition to form a third liquid composition; and a liquid composition application unit for applying the third liquid composition onto a substrate. The first liquid composition accommodated in the first tank contains: a first solvent; and a charge-transporting material having a polymerizable functional group. The second liquid composition accommodated in the second tank contains: a second solvent; and a charge-generating material that also acts as a polymerization initiator with respect to the polymerizable functional group. The mixing unit is arranged between the first tank and the liquid composition application unit.
Need to check novelty before this filing date? Find Prior Art

Description

Apparatus for manufacturing a charge injection layer, method for manufacturing a charge injection layer, apparatus for manufacturing a light-emitting element, and method for manufacturing a light-emitting element

[0001] The present invention relates to an apparatus for manufacturing a charge injection layer, a method for manufacturing a charge injection layer, an apparatus for manufacturing a light-emitting element, and a method for manufacturing a light-emitting element.

[0002] In the manufacturing methods of light-emitting devices, a method of forming functional materials into films and arranging them in a pattern is widely used. For example, organic electroluminescent (EL) devices are manufactured by forming and stacking light-emitting materials, charge-transporting materials, and charge-injecting materials into films and arranging them in a pattern. Vacuum deposition is widely used as a manufacturing method for such light-emitting devices. For example, in the case of organic EL devices, light-emitting functional materials such as red, green, and blue are formed as functional films by vacuum deposition. Each functional film needs to be arranged in a pattern on the substrate, and a mask is used to separate the film-forming areas from the non-film-forming areas. While vacuum deposition has advantages such as the ability to highly control the thickness of the functional film, the functional material in the non-film-forming areas on the substrate is formed on the mask and does not remain on the substrate, resulting in material waste and increased costs. Therefore, a so-called printing method has been proposed in which a liquid composition for forming a functional film is prepared by dissolving the functional material in a solvent, this liquid composition is applied to the necessary areas on the substrate, and then the solvent is removed to form a functional film and manufacture an organic EL device.

[0003] If an inkjet device is used as the liquid composition application device, for example, a functional film can be generated in a pattern only where needed without using a mask, thus reducing waste of functional materials and leading to cost reduction. When manufacturing organic EL elements by printing, the charge injection and transport layer may be a laminated structure consisting of a charge injection layer and a charge transport layer. In this case, the charge transport layer is formed on top of the charge injection layer, and then the light-emitting layer is laminated on top of that, but the underlying film needs to be poorly soluble in the liquid composition that forms the upper film. For example, when laminating a charge transport layer on top of a charge injection layer, a liquid composition for forming a charge transport layer, in which a charge-transporting material is dissolved, is applied on top of the charge injection layer to form the charge transport layer. In this case, if the material forming the charge injection layer (charge-transporting material) dissolves in the liquid composition forming the charge transport layer, the materials will become compatible at the interface between the charge injection layer and the charge transport layer, and the characteristics of the light-emitting element will deteriorate.

[0004] Patent Document 1 discloses a method for forming a charge implantation layer by forming a coating film from a liquid composition containing a charge transport material having a predetermined polymerizable functional group, a predetermined charge generating material that also acts as a polymerization initiator, and a solvent, and then proceeding with a polymerization reaction using heat. According to this method, since an ionic compound is used as the polymerization initiator, a sufficient sparing solubility effect can be obtained even if the charge transport material in the charge implantation layer has a relatively low molecular weight. As a result, the viscosity of the liquid composition forming the charge implantation layer can be kept relatively low, which has advantages such as excellent discharge stability of the liquid composition when, for example, an inkjet device is used as the liquid composition application device.

[0005] Generally, if extra materials that do not contribute to light emission are mixed into an organic EL element, it can lead to a decrease in the element's performance. In contrast, the method disclosed in Patent Document 1 has the advantage that the charge generating material also serves as a polymerization initiator, eliminating the need to add extra polymerization initiators.

[0006] Japanese Patent Publication No. 2023-178859

[0007] However, when the present inventors fabricated an organic EL device using a liquid composition containing a charge-transporting material having polymerizable functional groups and a charge-generating material that also acts as a polymerization initiator, as disclosed in Patent Document 1, the device performance sometimes deteriorated. Specifically, they found that when an organic EL device was fabricated using a liquid composition that had been stored for a certain period of time after preparation, the driving voltage increased. This is thought to be because the charge-transporting material and the charge-generating material reacted in the liquid composition during storage.

[0008] When a liquid composition containing a charge transport material and a charge generating material is applied to a substrate, the solvent is removed, and then the mixture is heated to allow the polymerization reaction to proceed, some of the charge generating material is consumed as a polymerization initiator, while the remaining portion functions as a charge generating agent. If there is too little charge generating material in the liquid composition, the amount of charge generating material in the charge injection layer decreases, causing the driving voltage of the light-emitting element to increase. In other words, it is thought that because the charge transport material having polymerizable functional groups and the charge generating material functioning as a polymerization initiator were contained in the same liquid composition and stored, the amount of charge generating material in the liquid composition after storage decreased, resulting in an increase in the driving voltage of the element.

[0009] Therefore, the object of the present invention is to provide a charge injection layer manufacturing apparatus, a charge injection layer manufacturing method, a light-emitting device manufacturing apparatus, and a light-emitting device manufacturing method that can suppress the deterioration of device characteristics even when using a liquid composition that has been stored for a certain period of time.

[0010] In other words, the present invention provides a charge implantation layer manufacturing apparatus comprising: a first tank containing a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups; a second tank containing a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups; a mixing unit for mixing the first liquid composition and the second liquid composition to form a third liquid composition; and a liquid composition application unit for applying the third liquid composition onto a substrate, wherein the mixing unit is located between the first tank and the liquid composition application unit.

[0011] Furthermore, the present invention provides a method for manufacturing a charge implantation layer, comprising: a first supply step of supplying a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups, which is contained in a first tank, to a mixing section; a second supply step of supplying a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups, which is contained in a second tank, to the mixing section; a mixing step of mixing the first liquid composition and the second liquid composition in the mixing section to form a third liquid composition; and a liquid composition application step of applying the third liquid composition onto a substrate, wherein the mixing step is performed immediately before the liquid composition application step.

[0012] Furthermore, according to the present invention, there is a device for manufacturing a light-emitting element, comprising a device for manufacturing a charge injection layer, a device for manufacturing a charge transport layer, and a device for manufacturing a light-emitting layer, wherein the device for manufacturing the charge injection layer comprises a first tank for containing a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups, a second tank for containing a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups, a mixing unit for mixing the first liquid composition and the second liquid composition to form a third liquid composition, and a liquid composition application unit for applying the third liquid composition onto a substrate, wherein the mixing unit is arranged between the first tank and the liquid composition application unit.

[0013] Furthermore, the present invention provides a method for manufacturing a light-emitting element, comprising a step of forming a charge injection layer, a step of forming a charge transport layer, and a step of forming a light-emitting layer, wherein the step of forming the charge injection layer comprises: a first supply step of supplying a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups, which is contained in a first tank, to a mixing unit; a second supply step of supplying a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups, which is contained in a second tank, to the mixing unit; a mixing step of mixing the first liquid composition and the second liquid composition in the mixing unit to form a third liquid composition; and a liquid composition application step of applying the third liquid composition onto a substrate, wherein the mixing step is performed immediately before the liquid composition application step.

[0014] According to the present invention, it is possible to provide a charge injection layer manufacturing apparatus, a charge injection layer manufacturing method, a light-emitting device manufacturing apparatus, and a light-emitting device manufacturing method that can suppress the deterioration of device characteristics even when using a liquid composition that has been stored for a certain period of time.

[0015] This is a block diagram showing the configuration of a charge injection layer manufacturing apparatus according to one embodiment of the present invention. This is a schematic diagram showing an example of the functional film production process. This is a schematic diagram showing another example of the functional film production process. This is a schematic diagram of an example of a functional film to explain the aperture ratio of the functional film within the region enclosed by the bank. This is a block diagram showing the configuration of a charge injection layer manufacturing apparatus according to another embodiment of the present invention. This is a schematic plan view showing the substrate of the light-emitting element used in the embodiment.

[0016] The present invention will be described in more detail below with reference to preferred embodiments. In this disclosure, unless otherwise specified, physical property values ​​are those at room temperature (25°C) and atmospheric pressure (1 atm). In the following description, an inkjet device will be used as an example of a liquid composition application device, but the invention is not limited to this, and the use of a dispenser, slit coater, etc., is also included in this technology.

[0017] <Apparatus for Manufacturing Charge Implantation Layer, Method for Manufacturing Charge Implantation Layer> Figure 1 is a block diagram showing the configuration of an apparatus for manufacturing a charge implantation layer 10 according to one embodiment of the present invention. The apparatus for manufacturing a charge implantation layer 10 comprises a first tank 11, a second tank 12, a mixing unit 13, and a liquid composition application unit 14. The first tank 11 contains a first liquid composition. The first liquid composition contains a first solvent and a charge transporting material having polymerizable functional groups. The second tank 12 contains a second liquid composition. The second liquid composition contains a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups. The mixing unit 13 mixes the first liquid composition and the second liquid composition to form a third liquid composition. The liquid composition application unit 14 applies the third liquid composition onto the substrate. The mixing unit 13 is located between the first tank 11 and the liquid composition application unit 14.

[0018] Furthermore, a method for manufacturing a charge injection layer according to one embodiment of the present invention comprises a first supply step, a second supply step, a mixing step, and a liquid composition application step. The first supply step is a step of supplying a first liquid composition contained in a first tank to a mixing section. The second supply step is a step of supplying a second liquid composition contained in a second tank to a mixing section. The mixing step is a step of mixing the first liquid composition and the second liquid composition in the mixing section to form a third liquid composition. The liquid composition application step is a step of applying the third liquid composition onto a substrate. The mixing step is performed immediately before the liquid composition application step.

[0019] In the charge implantation layer manufacturing apparatus 10, a first liquid composition containing a charge transporting material having polymerizable functional groups is stored in a first tank 11, and a second liquid composition containing a charge generating material that also acts as a polymerization initiator is stored in a second tank 12. Therefore, it is possible to avoid the reaction between the charge transporting material and the charge generating material in the liquid composition during storage, and thus the amount of charge generating material in the third liquid composition obtained by mixing the first and second liquid compositions after storage does not decrease easily. As a result, even if a charge implantation layer is formed using the third liquid composition after being stored for a certain period, the decrease in the amount of charge generating material in the charge implantation layer can be suppressed, and as a result, the deterioration of the device characteristics can be suppressed.

[0020] Here, in order to suppress the decrease in the amount of charge generating material in the liquid composition after storage, one possible method is to add more charge generating material than necessary to the liquid composition, thereby ensuring that the required amount of charge generating material is available even in the liquid composition after storage. In this case, an appropriate amount of charge generating material may be present in the charge implantation layer formed from the liquid composition after storage, and it is thought that the desired device performance can be obtained. However, since an excess amount of charge generating material will be present in the charge implantation layer formed from the liquid composition before storage, this may lead to a decrease in the lifespan of the resulting device.

[0021] As described above, if the amount of charge generating material in the charge injection layer is too small, the amount of charge generated will decrease, causing the device's drive voltage to rise. On the other hand, if the amount of charge generating material in the charge injection layer is excessively large, it may lead to a decrease in the device's lifespan. In other words, it is preferable to set the amount of charge generating material in the charge injection layer to an amount that suppresses the increase in the device's drive voltage and does not easily lead to a decrease in the device's lifespan. Therefore, it is preferable that the liquid composition for forming the charge injection layer used to form the charge injection layer is designed with an appropriate ratio of charge transport material and charge generating material, and that this ratio remains constant before and after storage.

[0022] In the charge injection layer manufacturing apparatus 10 of this embodiment, the third liquid composition applied to the substrate by the liquid composition application unit 14 is a liquid composition for forming the charge injection layer. This third liquid composition is formed by mixing a first liquid composition containing a charge transport material and a second liquid composition containing a charge generating material in the mixing unit 13. Therefore, it is possible to keep the ratio of the charge transport material to the charge generating material in the third liquid composition constant at all times.

[0023] Furthermore, when a liquid composition containing a charge-transporting material having polymerizable functional groups and a charge-generating material that also acts as a polymerization initiator is stored, the charge-transporting material and the charge-generating material may react during storage, increasing the molecular weight of the charge-transporting material and leading to an increase in the viscosity of the liquid composition. When the viscosity of the liquid composition increases, for example, if an inkjet device is used as the liquid composition dispensing unit 14, the droplets of the liquid composition become smaller, causing a decrease in the amount of liquid composition dispensed. For example, when using an inkjet device equipped with a discharge head that dispenses the liquid composition by applying mechanical energy generated by a piezoelectric element, adjustments to the drive voltage and discharge waveform become necessary. In contrast, the charge-implantation layer manufacturing apparatus 10 of this embodiment has the advantage that the viscosity of the liquid composition after storage does not increase easily, so adjustments to the drive voltage and discharge waveform can be kept to a minimum.

[0024] (Charge Injection Layer) The charge injection layer is formed by applying a third liquid composition, which is formed by mixing a first liquid composition containing a charge transport material having polymerizable functional groups and a second liquid composition containing a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups, onto a substrate. In other words, the charge injection layer can be formed by applying a third liquid composition containing a charge transport material having polymerizable functional groups and a charge generating material that also acts as a polymerization initiator onto a substrate, removing the solvent, and then heating to allow the polymerization reaction to proceed. By allowing the polymerization reaction to proceed, the charge transport material can be made to have a high molecular weight, which significantly reduces its solubility in the solvent. This makes it possible to apply a liquid composition containing another functional material on top of the charge injection layer, and to fabricate a functional element by stacking films of multiple functional materials (functional films). For example, when fabricating an organic EL element as a functional element, a charge transport layer can be stacked on top of the charge injection layer, and an organic EL light-emitting layer can be stacked on top of that. Also, when using quantum dot material as the light-emitting material, a quantum dot light-emitting element can be fabricated as a functional element.

[0025] Specific examples of the stacked structure of an organic EL element include a structure in which a substrate, an insulating layer, a first electrode, an organic compound layer, and a second electrode are stacked in this order. In this case, the functional film mentioned above can be the organic compound layer, which is a constituent layer of the organic EL element. Examples of organic compound layers include charge injection layers such as hole injection layers and electron injection layers that can be manufactured by the charge injection layer manufacturing apparatus 10 of this embodiment, as well as charge transport layers such as hole transport layers and electron transport layers, and light-emitting layers.

[0026] (Opening Ratio of Functional Film) When producing functional elements such as organic EL elements and quantum dot light-emitting elements, in general, a liquid composition in which a functional material is dissolved is applied to a region surrounded by liquid-repellent partition walls called banks on a substrate, the solvent is removed to form a film of the functional material, and a plurality of functional film layers are laminated. As shown in Figure 2, the solvent is removed by drying from the liquid composition I2 containing the functional material applied to the region (recess) surrounded by the banks 2 on the substrate. In this process, as represented by the wavy arrows in the figure, the solvent of the liquid composition I2 in the region surrounded by the banks 2 evaporates faster at the end portions than at the central portion. As a result, a concentration gradient of the functional material in the liquid composition I2 applied to the region surrounded by the banks 2 is generated. Consequently, the liquid composition I2 in the region surrounded by the banks 2 tends to diffuse in the direction from the central portion toward the end portions (see the dashed arrows inside the liquid composition I2 in Figure 2), and the functional material easily accumulates at the end portions of the region surrounded by the banks 2. When the solubility of the functional material in the solvent is high, the diffusion of the liquid composition I2 continues, so the amount of the functional material 21 accumulated at the end portions of the region surrounded by the banks 2 tends to increase. This leads to a smaller opening 22 of the functional material film (functional film) 23, which may result in a lower opening ratio of the functional film 23.

[0027] In contrast, in order to improve the opening ratio of the functional film, a liquid composition obtained by mixing a solvent having high solubility for the functional material (so-called good solvent) and a solvent having low solubility for the functional material (so-called poor solvent) can be suitably used. In this case, it is preferable that the boiling point of the poor solvent is higher than that of the good solvent. When the liquid composition contains a good solvent and a poor solvent for the functional material, and the boiling point of the poor solvent is higher than the boiling point of the good solvent, the situation is explained as follows with reference to Figure 3.

[0028] In the liquid composition I3 containing the functional material applied to the region (recess) surrounded by bank 2, the good solvent with a relatively low boiling point evaporates first, and the proportion of the poor solvent with a relatively high boiling point increases. Therefore, the precipitation of the functional material is promoted during the process of removing the solvent from the liquid composition I3 containing the functional material applied to the region surrounded by bank 2, and the diffusion of the liquid composition I3 to the edges within the region surrounded by bank 2 becomes slow (see the dashed arrow in liquid composition I3 in Figure 3). As a result, the amount of functional material 31 that accumulates at the edges of the region surrounded by bank 2 tends to decrease. This leads to an increase in the opening 32 of the functional material film (functional film) 33, and thus the opening ratio of the functional film 33 tends to increase. Therefore, in the charge implantation layer manufacturing apparatus of this disclosure, it is preferable that the boiling point of the second solvent is higher than that of the first solvent, and that the solubility of the charge transporting material in the second solvent is lower than that of the charge transporting material in the first solvent. Furthermore, it is preferable that the solubility of the charge transporting material in the second solvent is less than 0.5% by mass. By using this combination of the first and second solvents, it is possible to further increase the aperture ratio of the charge implantation layer film.

[0029] The aperture ratio of the functional film described above will be further explained with reference to FIG. 4. FIG. 4 is a schematic diagram showing an example of the shape of the functional film 43 in the region surrounded by the bank 2. The aperture ratio of the functional film 43 can be calculated as L2 / L1, where L1 is the length of the bottom surface of the functional film 43 (the region surrounded by the bank 2), and L2 is the length of the functional film 43 in the inner portion of the relevant region at a constant height H from the bottom surface. The constant height H can be 1.5 times the average film thickness of the entire functional film. For example, when the average film thickness of the entire functional film is 40 nm, the position at a height of 60 nm from the bottom surface of the region surrounded by the bank 2 is defined as the constant height H, and the length of the inner portion of the relevant region at this height H can be set as L2. For example, when manufacturing an organic EL element, a charge transport layer is laminated on a charge injection layer, and a light-emitting layer is laminated thereon. At this time, if the aperture ratio of the film is low, the area of the light-emitting material film decreases, and the luminance as an organic EL display lowers. Therefore, it is preferable that the aperture ratio of the film is high. In particular, the present disclosure relates to a manufacturing apparatus for a charge injection layer. For example, in an organic EL element or the like, the charge injection layer is the lowermost layer among the organic compound layers, so the higher the aperture ratio of the charge injection layer film, the more preferable it is.

[0030] (First Tank) The manufacturing apparatus 10 for a charge injection layer shown in FIG. 1 includes a first tank 11 that stores a first liquid composition. The form of the first tank 11 is not particularly limited as long as it can store the first liquid composition, and for example, containers in the shape of a box, a bag, or the like can be used. For example, when an inkjet device is used as the liquid composition applying unit 14, an ink cartridge that stores the first liquid composition can be used as the first tank 11.

[0031] (First Liquid Composition) The first liquid composition contained in the first tank 11 contains a first solvent and a charge-transporting material having polymerizable functional groups. In the first liquid composition, it is preferable that the charge-transporting material is dissolved in the first solvent. The first solvent is preferably capable of dissolving the charge-transporting material having polymerizable functional groups, and more preferably has a higher solubility of the charge-transporting material and a lower boiling point than the second solvent in order to improve the aperture ratio of the membrane of the charge-implantation layer. The first solvent may be a single solvent or a mixture of multiple solvents. When a mixed solvent of multiple solvents is used as the first solvent, it is preferable that all the solvents used in the mixed solvent, which is the first solvent, have a higher solubility of the charge-transporting material and a lower boiling point than the second solvent.

[0032] Since the first liquid composition is preferably stored in the first tank 11 with the charge-transporting material dissolved in it, it is preferable that the solubility of the charge-transporting material in the first solvent is high. This makes it possible to suppress the precipitation of the charge-transporting material when the first liquid composition is stored. For example, the thickness of the charge-injection layer of the organic EL element is preferably 10 nm to 120 nm. In order to achieve this film thickness, the content of the charge-transporting material in the liquid composition used to form the charge-injection layer (third liquid composition) is preferably 0.5% by mass to 2.0% by mass, based on the total mass of the third liquid composition. From the viewpoint of easily increasing the aperture ratio of the charge-injection layer film, it is preferable that the mixing ratio of the first liquid composition and the second liquid composition when forming the third liquid composition is such that the content of the second solvent in the third liquid composition is equal to or greater than the content of the first solvent. For example, in order to have a charge-transporting material content of 2.0% by mass in the third liquid composition and a mass ratio of the first solvent to the second solvent of 1:1, the charge-transporting material content in the first liquid composition needs to be 4.0% by mass. Therefore, the solubility of the charge-transporting material in the first solvent is preferably 4.0% by mass or more, and more preferably 5.0% by mass or more. Furthermore, the content of the charge-transporting material in the first liquid composition is preferably 1.0% by mass or more and 4.0% by mass or less, based on the total mass of the first liquid composition.

[0033] Examples of the first solvent include methyl benzoate, ethyl benzoate, ethyl phenylacetate, phenyl acetate, anisole, methylanisole, tetrahydronaphthalene, N,N-diethylaniline, 1,3-dimethyl-2-imidazolidinone, toluene, cycloheptanone, and N-methyl-2-pyrrolidone. Among these, methyl benzoate, ethyl benzoate, ethyl phenylacetate, and phenyl acetate are preferred. It is preferable to use one or more of these.

[0034] Charge transport materials exhibit curability due to the presence of polymerizable functional groups. The polymerizable functional group is preferably an oxetanyl group (oxetane group). The oxetanyl group may have substituents. Examples of substituents include methyl groups and C1 to C6 alkyl groups such as ethyl groups.

[0035] The charge-transporting material preferably contains a structural unit comprising at least one structure selected from the group consisting of aromatic amine structures, carbazole structures, thiophene structures, benzene structures, pyrrole structures, furan structures, and fluorene structures. Including any of these structures improves charge transportability, particularly hole transportability. The charge-transporting material is preferably a polymer having a structural unit comprising an aromatic amine structure, and more preferably a polymer having a structural unit comprising an aromatic amine structure substituted with a fluoro group. The weight-average molecular weight of the charge-transporting material (charge-transporting polymer) is preferably 1,000 to 1,000,000.

[0036] The weight-average molecular weight of charge-transporting materials can be determined as a polystyrene-converted value measured by gel permeation chromatography (GPC).

[0037] (Second Tank) The charge implantation layer manufacturing apparatus 10 shown in Figure 1 includes a second tank 12 for containing a second liquid composition. The form of the second tank 12 is not particularly limited as long as it can contain the second liquid composition, and containers such as boxes and bags can be used. For example, when an inkjet device is used as the liquid composition dispensing unit 14, an ink cartridge containing the second liquid composition can be used as the second tank 12.

[0038] (Second Liquid Composition) The second liquid composition contained in the second tank 12 contains a second solvent and a charge-generating material that also acts as a polymerization initiator for polymerizable functional groups. In the second liquid composition, the charge-generating material is preferably dissolved in the second solvent. The second solvent is preferably capable of dissolving the charge-generating material and may be the same as or different from the first solvent. For the purpose of improving the aperture ratio of the charge-implantation layer membrane, the second solvent is more preferably such that the solubility of the charge-transporting material is less than 0.5% by mass and that its boiling point is higher than that of the first solvent. The second solvent may be a single solvent or a mixture of multiple solvents. When a mixed solvent of multiple solvents is used as the second solvent, it is preferable that all solvents used in the mixed solvent, which is the second solvent, have a solubility of the charge-transporting material of less than 0.5% by mass and that their boiling points are higher than those of the first solvent.

[0039] The content of the charge-generating material in the third liquid composition is preferably 0.01% by mass or more and 0.50% by mass or less, based on the total mass of the third liquid composition. Furthermore, the content of the charge-generating material in the second liquid composition is preferably 0.02% by mass or more and 1.00% by mass or less, based on the total mass of the second liquid composition.

[0040] Examples of the second solvent include methyl benzoate, ethyl benzoate, isopropyl benzoate, isobutyl benzoate, ethyl phenyl, benzyl isovalerate, dodecane, 2,5-hexanediol, 3-methoxyphenol, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, and benzyl alcohol. Among these, methyl benzoate, ethyl benzoate, isopropyl benzoate, isobutyl benzoate, ethyl phenyl, benzyl isovalerate, dodecane, and 2,5-hexanediol are preferred. It is preferable to use one or more of these.

[0041] The charge-generating material also acts as a polymerization initiator for the polymerizable functional group in the charge-transporting material in the first liquid composition described above. When the polymerizable functional group in the charge-transporting material in the first liquid composition is an oxetanyl group, the charge-generating material preferably contains an ionic compound containing diphenylmethylammonium and an anion, from the viewpoint of readily undergoing polymerization reactions with the oxetanyl group. Furthermore, the charge-generating material is more preferably diphenylmethylammonium tetrakis(pentafluorophenyl)borate.

[0042] (Third Liquid Composition) The third liquid composition is formed by mixing the first liquid composition and the second liquid composition in the mixing section. Therefore, the third liquid composition can be said to be a composition containing the first liquid composition and the second liquid composition, and also a composition containing a charge transport material, a charge generating material, the first solvent, and the second solvent. Preferably, the third liquid composition is a composition in which a charge transport material having polymerizable functional groups and a charge generating material that also acts as a polymerization initiator are dissolved in a mixed solvent of the first solvent and the second solvent. By applying the third liquid composition onto a substrate, removing the solvent, and then heating, a polymerization reaction can proceed, making it possible to form a charge implantation layer with increased insolubility. The mixing step of mixing the first liquid composition and the second liquid composition to obtain this third liquid composition is performed immediately before the liquid composition application step of applying the third liquid composition onto the substrate from the liquid composition application section. This makes it possible to suppress the precipitation of functional materials in the liquid composition.

[0043] The third liquid composition may contain a mixture of the first and second solvents. When the third liquid composition is applied to the region surrounded by the bank and the solvent is removed to form a charge implantation layer, it is preferable that the boiling point of the second solvent is higher than that of the first solvent. Furthermore, it is preferable that the solubility of the charge transporting material in the second solvent is less than 0.5% by mass, and that the solubility of the charge transporting material in the second solvent is lower than that of the charge transporting material in the first solvent. When such first and second solvents are used, the first solvent tends to evaporate more easily than the second solvent because its boiling point is lower. Therefore, during the process of forming the charge implantation layer, the proportion of the second solvent in the liquid composition within the region surrounded by bank 2 tends to increase, promoting the precipitation of the functional material, and thus improving the aperture ratio of the charge implantation layer film. Consequently, a higher proportion of the second solvent tends to enhance the effect of improving the aperture ratio of the charge implantation layer film. Therefore, if the volume of the first solvent in the third liquid composition is V1 and the volume of the second solvent is V2, it is preferable that V2 ≥ V1. In other words, it is preferable that the ratio of the content (volume) of the second solvent to the total content (volume) of the first and second solvents in the third liquid composition is 50% by volume or more.

[0044] Furthermore, the percentage (volume %) of the second solvent in the third liquid composition is preferably 70% by volume or less. Therefore, the content (volume) of the first solvent in the third liquid composition is preferably 30% by volume or more and 50% by volume or less relative to the total content (volume) of the first and second solvents in the third liquid composition. When the percentage of the second solvent is 70% by volume or less, the percentage of the first solvent is 30% by volume or more, which makes the solubility of the charge transport material in the third liquid composition sufficiently stable and improves the applicability of the liquid composition. For example, when an inkjet device is used as the liquid composition applicator 14, the ejection stability of the third liquid composition is improved, and it becomes less likely for the applicability of the liquid composition droplets on the substrate to shift.

[0045] (Solubility of Solvent) In this disclosure, the solubility of a charge transport material in a solvent can be measured by dropping the solvent to be measured onto the charge transport material to be measured, stirring at room temperature (25°C) for 2 hours, and observing the state of undissolved charge transport material in the solvent. Specifically, the solubility of a charge transport material in a solvent can be determined in five stages by the following method. First, if there is no undissolved charge transport material after dropping 960 mg of solvent onto 40 mg of charge transport material and stirring, the solubility of the charge transport material in that solvent is determined to be 4.0% by mass or more. If there is undissolved charge transport material under these conditions, a further 1000 mg of solvent is dropped and stirred. If there is no undissolved charge transport material with 40 mg of charge transport material and 1960 mg of solvent, the solubility of the charge transport material in that solvent is determined to be 2.0% by mass or more and less than 4.0% by mass. If there are undissolved charge transport materials under these conditions, add another 2000 mg of solvent dropwise and stir. If there are no undissolved particles with 40 mg of charge transport material and 3960 mg of solvent, the solubility of the charge transport material in that solvent is determined to be 1.0% by mass or more and less than 2.0% by mass. If there are undissolved charge transport materials under these conditions, add another 4000 mg of solvent dropwise and stir. If there are no undissolved particles with 40 mg of charge transport material and 7960 mg of solvent, the solubility of the charge transport material in that solvent is determined to be 0.5% by mass or more and less than 1.0% by mass. If there are still undissolved charge transport materials under these conditions, the solubility of the charge transport material in that solvent is determined to be less than 0.5% by mass.

[0046] (Boiling point of the solvent) As mentioned above, in order to improve the aperture ratio of the charge implantation layer film, it is preferable that the solubility of the charge transport material in the second solvent is lower than that in the first solvent. In this case, it is preferable that the boiling point of the second solvent is higher than that of the first solvent. If the boiling point of the first solvent is higher than that of the second solvent, the second solvent will evaporate more easily than the first solvent during the formation process of the charge implantation layer, and the first solvent, which has relatively higher solubility, will remain, making it difficult to improve the aperture ratio of the charge implantation layer film.

[0047] The boiling point of the first solvent is preferably 190°C or higher, and more preferably 200°C or higher. For example, when an inkjet device is used as the liquid composition application unit 14, the third liquid composition is filled into the inkjet ejection head. The tip of the nozzle (ejection port) of the ejection head is open to the atmosphere, and while ejection is stopped, the longer the stop period, the more the solvent of the third liquid composition can evaporate from the ejection port of the ejection head. The solvent with a relatively low boiling point in the third liquid composition is preferably the first solvent. In this case, the first solvent tends to evaporate first, so the proportion of the second solvent tends to increase at the nozzle tip while ejection is stopped. Since it is preferable for the solubility of the charge transport material in the second solvent to be low, the charge transport material may precipitate at the nozzle tip, causing a shift in the application position of the third liquid composition to the substrate. From the viewpoint of suppressing such situations, the boiling point of the first solvent is preferably 200°C or higher. Furthermore, the boiling point of the first solvent is preferably 240°C or lower, and more preferably 230°C or lower.

[0048] The boiling point of the second solvent is preferably higher than that of the first solvent, and preferably 300°C or lower. When the boiling point of the second solvent is 300°C or lower, it becomes possible to completely remove the second solvent from the charge injection layer by drying during the formation of the charge injection layer, which helps to suppress the reduction in the lifespan of the device due to residual solvent in the charge injection layer. Furthermore, the boiling point of the second solvent is more preferably between 200°C and 300°C, and even more preferably between 210°C and 270°C.

[0049] (Mixing section) The charge injection layer manufacturing apparatus 10 shown in Figure 1 forms a third liquid composition by mixing a first liquid composition supplied from a first tank 11 and a second liquid composition supplied from a second tank 12 in a mixing section 13. The mixing section 13 is located between the first tank 11 and the liquid composition supply section 14.

[0050] The mixing unit 13 is not particularly limited as long as it can mix the first liquid composition and the second liquid composition. For example, the mixing unit 13 may have an agitator such as a stirrer, or it may be a mechanism that utilizes the flow of liquid such as a static mixer. Alternatively, the mixing unit 13 may simply be a mechanism that merges a flow path for supplying the first liquid composition from the first tank 11 (first supply flow path) and a flow path for supplying the second liquid composition from the second tank 12 (second supply flow path). From the viewpoint of simplicity of configuration of the charge implantation layer manufacturing apparatus 10, a static mixer that utilizes the flow of liquid or a mechanism that merges flow paths is more preferable for the mixing unit 13. Furthermore, as described above, it is preferable that the charge implantation layer manufacturing apparatus 10 includes a first supply flow path that supplies the first liquid composition from the first tank 11 to the mixing unit 13, and a second supply flow path that supplies the second liquid composition from the second tank 12 to the mixing unit 13.

[0051] From the viewpoint of improving the miscibility between the first liquid composition and the second liquid composition, the angle θ between the first supply channel and the second supply channel is preferably 0° < θ < 180°, and more preferably 0° < θ ≤ 90°. Here, the angle θ between the first supply channel and the second supply channel is the angle at the intersection of the central axis (or extension thereof) of the first supply channel and the central axis (or extension thereof) of the second supply channel. For example, if the first supply channel and the second supply channel are configured as shown in Figure 1, the angle θ between the first supply channel and the second supply channel is 90°.

[0052] The first liquid composition and the second liquid composition are mixed in a mixing unit 13 located between the first tank 11 and the liquid composition dispensing unit 14, and supplied to the liquid composition dispensing unit 14 as a third liquid composition. The third liquid composition is then applied from the liquid composition dispensing unit 14 onto a substrate, such as an area surrounded by the bank 2. In other words, immediately after the formation of the third liquid composition, the third liquid composition is quickly applied onto the substrate, such as an area surrounded by the bank 2. From the viewpoint of ensuring that the charge generating material in the formed charge injection layer is uniformly distributed, it is preferable that the first liquid composition and the second liquid composition are uniformly mixed when the third liquid composition is formed. When the charge generating material present in the charge injection layer is uniform, the charge generation efficiency tends to increase, and the rise in the driving voltage tends to be further suppressed. For example, when the application of the third liquid composition is performed by an inkjet device, the third liquid composition is supplied to multiple nozzles (flow channels) in the ejection head. In this case, if the mixture of the first liquid composition and the second liquid composition is uniform, variations in the ratio of charge-generating material to charge-transporting material in the ink for each nozzle (flow channel) are less likely to occur, making it easier to further suppress the rise in driving voltage.

[0053] Furthermore, as mentioned above, if a solvent with higher solubility and a lower boiling point for the charge transport material is used as the first solvent than the second solvent, and a solvent with less than 0.5% by mass of the charge transport material is used as the second solvent, the aperture ratio of the charge implantation layer membrane tends to improve further. This effect is more likely to occur when the mixture of the first and second solvents is uniform. If the mixture of the first and second solvents is non-uniform, for example, the mixture of the first and second solvents becomes non-uniform in the third liquid composition applied within the region surrounded by bank 2, and the effect of improving the aperture ratio of the charge implantation layer membrane may be limited. For example, the aperture ratio of the charge implantation layer formed by a liquid composition discharged from a nozzle supplied with a liquid composition having a high proportion of the first solvent may be low. Therefore, it is preferable that the first liquid composition and the second liquid composition be quickly and uniformly mixed in the mixing section 13.

[0054] (HSP Distance Ra of Solvent) As an index of the ease of mixing the first solvent and the second solvent, there is a distance Ra of the Hansen Solubility Parameter (HSP) (hereinafter sometimes referred to as "HSP distance Ra"). The Hansen Solubility Parameter (HSP) is δ D (dispersion term), δ P (polar term), and δ H (hydrogen bonding term), three parameters (unit: MPa 1/2 ). The δ of the Hansen Solubility Parameter (HSP) of the first solvent and the second solvent D , δ P , and δ H are respectively designated as δ D1 , δ P1 , and δ H1 , as well as δ D2 , δ P2 , and δ H2 , the HSP distance Ra is determined by the following formula (1).

[0055]

[0056] The smaller the value of the HSP distance Ra, the easier it is for the first solvent and the second solvent to mix. The distance Ra between the Hansen Solubility Parameters (HSP) of the first solvent and the second solvent is preferably 10.0 MPa 1/2 or less. When the HSP distance Ra between the first solvent and the second solvent is 10.0 MPa 1/2 or less, the mixed state of the first solvent and the second solvent in the third liquid composition can be made more uniform.

[0057] When a plurality of solvents are used for each of the first solvent and the second solvent, the δ of the Hansen Solubility Parameter of each mixed solvent D , δ P , and δ H are calculated, and using these values, the HSP distance Ra is calculated by the above formula (1). The δ of the Hansen Solubility Parameter of the mixed solvent D , δ P , and δ H are the δ of each solvent D , δ P , and δ HThe solubility parameters are calculated by weighting them by the mixing ratio. For example, the solubility parameters of a mixed solvent obtained by mixing ethyl benzoate (17.9, 6.2, 6.0) and ethyl phenylethyl acetate (17.7, 3.9, 5.4) in a volume ratio of 1:1 as the first solvent are (17.8, 5.1, 5.7). The three values ​​in parentheses for methyl benzoate, ethyl phenylethyl acetate, and the mixed solvent obtained by mixing them in a volume ratio of 1:1 are the δ values ​​of the Hansen solubility parameters of each solvent. D , δ P , and δ H (All units: MPa) 1/2 ) represents.

[0058] (Liquid Composition Application Unit) The charge injection layer manufacturing apparatus 10 shown in Figure 1 includes a liquid composition application unit 14 that applies the third liquid composition formed in the mixing unit 13 onto the substrate. The application method of the third liquid composition by the liquid composition application unit 14 can include an inkjet method, a dispensing method, and a slit coat method. Therefore, as described above, the liquid composition application unit 14 can use an inkjet device, a dispenser, a slit coater, etc. Among these, an inkjet device is preferred because it has high material utilization efficiency and enables high resolution, and specifically, it is preferable to use the ejection head provided by the inkjet device. The ejection method of the ejection head can include a method in which mechanical energy generated by a piezoelectric element or the like is applied to the third liquid composition for ejection, or a method in which thermal energy generated by an electrothermal converter (heater) or the like is applied to the third liquid composition for ejection.

[0059] (Valve) The charge injection layer manufacturing apparatus of the present disclosure preferably includes an openable and closable valve between the first tank and the mixing section. Specifically, it is preferable to include an openable and closable valve in the flow path of the first liquid composition connecting the first tank and the mixing section. Figure 5 is a block diagram showing a charge injection layer manufacturing apparatus 50 which, in addition to the first tank 11, second tank 12, mixing section 13, and liquid composition application section 14 described above, further includes an openable and closable valve 51 between the first tank 11 and the mixing section 13.

[0060] As described above, the charge implantation layer manufacturing apparatus of this disclosure can be stored in a state where the charge transporting material and the second solvent are not in contact, thereby improving the ability to apply the liquid composition after storage. Here, when the charge implantation layer manufacturing apparatus is not in operation, the portion from the mixing section to the liquid composition application section may be stored filled with a third liquid composition, which is a mixture of the first liquid composition and the second liquid composition. As described above, when a solvent with a higher solubility of the charge transporting material and a lower boiling point than the second solvent is used as the first solvent, and a solvent with a solubility of the charge transporting material of less than 0.5% by mass is used as the second solvent, it is easier to increase the aperture ratio of the charge implantation layer film. On the other hand, in this case, since the charge generating material and the second solvent, which is a poor solvent, are stored mixed in the third liquid composition, the solubility of the charge transporting material may become unstable, and the charge transporting material may precipitate during storage. Even in such cases, when the charge injection layer manufacturing apparatus is restarted, the precipitate can be removed by suction from the liquid composition supply section, or by pressurizing the first and second tanks to supply the first and second liquid compositions. This makes it possible to supply the liquid composition. At this time, it is necessary to discard a certain amount of the first liquid composition in order to remove the precipitate.

[0061] Generally, the amount of charge-generating material in the charge-injection layer is extremely small compared to the amount of charge-transporting material. Therefore, the concentration of charge-generating material in the second liquid composition is much lower than the concentration of charge-transporting material in the first liquid composition. In other words, minimizing the amount of waste from the first liquid composition during restart is preferable from the viewpoint of reducing the waste of functional materials.

[0062] Therefore, as shown in Figure 5, a valve 51 that can be opened and closed is placed between the first tank 11 and the mixing section 13, and a configuration can be adopted that has a mechanism to close the valve 51 when the device is not in operation, and replace the inside of the mixing section 13 and the liquid composition dispensing section 14 with the second solvent. With this configuration, when the charge implantation layer manufacturing apparatus 50 is not in operation, the valve 51 is closed and only the second solvent is supplied to the mixing section 13 and the liquid composition dispensing section 14. As a result, the third liquid composition remaining inside the section 55 from the mixing section 13 to the liquid composition dispensing section 14 is washed away, and the inside of that section 55 is filled with the second solvent. Storing the device in this state makes it less likely for the charge transport material to precipitate, thus eliminating the need to discard the first liquid composition when the charge implantation layer manufacturing apparatus 50 is restarted. Furthermore, the liquid composition dispensing section 14 is stored filled with the second solvent. If this storage period is long, the second solvent may all evaporate, so it is preferable that the second solvent does not contain a solute. Furthermore, even if a poor solvent for the charge-transporting material is not used as the second solvent, if the storage period during periods of non-operation is long, the charge-transporting material having polymerizable functional groups and the charge-generating material, which also acts as a polymerization initiator, may react in the portion 55 from the mixing section 13 to the liquid composition application section 14. For this reason, it is preferable to provide a valve 51.

[0063] (Drying) The liquid composition for forming the charge injection layer (third liquid composition) applied to the substrate is dried. This removes the first and second solvents from the third liquid composition, and a field injection layer is formed on the substrate. This drying may be done by natural drying or by drying using a drying apparatus. There are no particular restrictions on the drying apparatus, but examples include blowers, heating apparatuses, and vacuum drying apparatuses.

[0064] <Manufacturing apparatus for light-emitting elements, method for manufacturing light-emitting elements> The manufacturing apparatus for light-emitting elements of one embodiment of the present invention comprises the above-described charge injection layer manufacturing apparatus, charge transport layer manufacturing apparatus, and light-emitting layer manufacturing apparatus. Furthermore, the method for manufacturing a light-emitting element of one embodiment of the present invention comprises a charge injection layer formation step by the above-described charge injection layer manufacturing method, a charge transport layer formation step, and a light-emitting layer formation step. In the charge transport layer formation step and the light-emitting layer formation step, methods for formation by dry process and wet process can be cited. Examples of dry processes include vacuum deposition, ionization deposition, sputtering, and plasma methods. A wet process is a method of applying a liquid composition for forming a charge transport layer or a light-emitting layer, which contains constituent materials for the charge transport layer or the light-emitting layer, and a solvent, to a target location such as a substrate. Examples of methods for applying this liquid composition include coating methods such as spin coating, casting, gravure coating, bar coating, roll coating, wire bar coating, dip coating, spray coating, and capillary coating; and printing methods such as screen coating, flexographic coating, offset coating, and inkjet coating. Among these methods, vacuum deposition, ionization deposition, spray coating, and inkjet are preferred, with inkjet being even more preferred. By employing these methods, larger-area light-emitting elements can be easily manufactured.

[0065] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited in any way by the following examples unless it exceeds the gist of the invention. Unless otherwise specified, amounts of components described in "parts" and "%" are based on mass. Boiling points and solubility are values ​​measured at 25°C and atmospheric pressure (1 atm). In these examples and comparative examples, an inkjet device is described as the liquid composition application unit, but the present invention is not limited thereto.

[0066] <Synthesis of Charge Transport Materials> (Preparation of Pd Catalyst) In a glove box under a nitrogen atmosphere at room temperature, 73.2 mg (80 μmol) of tris(dibenzylideneacetone)dipalladium was weighed into a glass sample tube, 15 mL of toluene was added, and the mixture was stirred for 30 minutes. In a glove box under a nitrogen atmosphere, 129.6 mg (640 μmol) of tris(t-butyl)phosphine was weighed into a glass sample tube, 5 mL of toluene was added, and the mixture was stirred for 5 minutes. These liquids were mixed and stirred at 80°C for 2 hours. The resulting liquid was used as the catalyst after removing insoluble matter using a 0.2 μm pore size membrane filter. All solvents were degassed using nitrogen bubbles for at least 30 minutes before use.

[0067] (Synthesis of Charge Transport Materials Having Polymerizable Functional Groups) In a 200 mL three-necked round-bottom flask (glass), 5.15 g (10.0 mmol) of monomer 1, 1.93 g (4.0 mmol) of monomer 2, 1.08 g (4.0 mmol) of monomer 3, 1.17 g (4.0 mmol) of monomer 4, and 90 mL of toluene were added. Then, 7.8 mL of 1% by mass aqueous solution of tetraethylammonium hydroxide and 14.2 mL of 3 M aqueous solution of potassium hydroxide were added. Monomers 1 to 4 are compounds represented by the following chemical formulas (1) to (4). All solvents were degassed using a nitrogen bubble for at least 30 minutes before use. A reflux condenser and a nitrogen gas flow tube were attached to the flask containing the reaction solution, and the flask was immersed in an oil bath heated to 60°C and stirred for 30 minutes. Subsequently, 2.0 mL of the prepared Pd catalyst solution was added, and the oil bath temperature was increased to 120°C to carry out the reaction. The reaction solution was heated under reflux for 2 hours. All operations up to this point were performed under a nitrogen atmosphere.

[0068]

[0069]

[0070] After the reaction was complete, the organic layer was washed with water and poured into a methanol-water (9:1) mixture. The resulting precipitate was filtered by suction and washed with a methanol-water (9:1) mixture. The obtained precipitate was washed with ethyl acetate, and the eluted solids were vacuum-dried. The dried solids were dissolved in toluene, and a metal adsorbent ("Triphenylphosphorine, polymer-bound on styrene-divinylbenzene copolymer," manufactured by Strem Chemicals, at a concentration of 200 mg per 100 mg of precipitate) was added, and the mixture was stirred overnight. After stirring, the metal adsorbent and insoluble matter were removed by filtration, and the resulting liquid was poured into methanol. The precipitate was filtered by suction, and the obtained precipitate was washed with methanol. The solids were then vacuum-dried to obtain a charge-transporting material having polymerizable functional groups. The weight-average molecular weight of this charge-transporting material was 600,000. In this way, a charge-transporting material (charge-transporting polymer) was obtained that has an oxetanyl group as a polymerizable functional group and a structural unit containing an aromatic amine structure substituted with a fluoro group.

[0071] <Synthesis of Charge Generating Material> 5.497 g (30 mmol) of N,N-diphenylmethylamine was mixed with 75 g of acetone and 15 g of pure water and stirred to obtain a liquid containing N,N-diphenylmethylamine. 11.0 g of 10% by mass aqueous hydrogen chloride solution was slowly added dropwise to the obtained liquid, and after the addition was complete, the mixture was stirred for 1 hour. The solvent was removed from the stirred liquid under reduced pressure. Next, 231.7 g (33 mmol) of sodium tetrakis(pentafluorophenyl)borate (10% by mass aqueous solution) was mixed and stirred for 1 hour. The precipitate was washed five times with water and dried to obtain a charge generating material that also acts as a polymerization initiator. This charge generating material is diphenylmethylammonium tetrakis(pentafluorophenyl)borate.

[0072] <Preparation of the First Liquid Composition> The above charge-transporting material was dissolved in the solvent shown in Table 1 (the first solvent), and liquid compositions 1 to 4 that could be used as the first liquid composition were prepared by pressure filtration using a filter with a pore size of 0.2 μm. The content (%) of the charge-transporting material in these liquid compositions was as shown in Table 1.

[0073] <Preparation of the Second Liquid Composition> The above charge-generating material was dissolved in the solvent shown in Table 1 (the second solvent), and the mixture was filtered under pressure using a filter with a pore size of 0.2 μm to prepare liquid compositions 5 to 13 that could be used as the second liquid composition. The content (%) of the charge-generating material in these liquid compositions is as shown in Table 1.

[0074] <Preparation of Other Liquid Compositions> The charge transport material and charge generating material described above were dissolved in the solvents shown in Table 1, and the mixture was filtered under pressure using a filter with a pore size of 0.2 μm to prepare liquid compositions 14 to 17 containing both the charge transport material and the charge generating material. The respective content (%) of the charge transport material and charge generating material in these liquid compositions are as shown in Table 1.

[0075]

[0076] <Liquid Composition for Charge Transport Layer Formation> As the charge transport material for forming the charge transport layer, poly(3,4-ethylenedioxythiophene) / polystyrenesulfonic acid (abbreviated as PEDOT / PSS), a polymer of 3,4-ethylenedioxythiophene / styrenesulfonic acid, was used. The ratio of 3,4-ethylenedioxythiophene to styrenesulfonic acid was 1:15 by mass, and the weight-average molecular weight was 300,000. The above PEDOT / PSS was dissolved in ethyl benzoate and pressure filtered using a filter with a pore size of 0.2 μm to prepare a liquid composition for charge transport layer formation. The content (solute concentration) of PEDOT / PSS in this liquid composition was 1.5%.

[0077] <Liquid composition for luminescent layer formation> As the luminescent material, a mixture of a carbazole compound and an iridium complex in a mass ratio of 9:1 was used. As the carbazole compound, 3,3'-di(9H-carbazole-9-yl)-1,1'-biphenyl (abbreviation: m-CBP) was used. As the iridium complex, bis(2-phenylpyridine)(acetylacetonate)iridium(III) (abbreviation: Ir(ppy)) 2 (acac)) was used. m-CBP and Ir(ppy) 2(acac) was dissolved in ethyl benzoate in a mass ratio of 9:1, and the mixture was pressure filtered using a pore size 0.2 μm filter to prepare a liquid composition for forming a light-emitting layer. The content of the light-emitting material (solute concentration) in this liquid composition was 2.0%.

[0078] <Measurement of Solubility> The solubility of the charge transport material in the first and second solvents was measured as follows. The solvent to be measured was dropped onto the charge transport material to be measured, and the mixture was stirred at room temperature for 2 hours using a magnetic stirrer. Solubility was measured based on the presence or absence of undissolved material in the solvent. Specifically, if there was no undissolved charge transport material after dropping 960 mg of solvent onto 40 mg of charge transport material and stirring, the solubility of the charge transport material in that solvent was judged to be 4.0% or higher. If there was undissolved charge transport material under the above conditions, an additional 1000 mg of solvent was dropped and stirred. If there was no undissolved charge transport material with 40 mg of charge transport material and 1960 mg of solvent, the solubility of the charge transport material in that solvent was judged to be 2.0% or higher and less than 4.0%. If there was any undissolved charge transport material under the above conditions, an additional 2000 mg of solvent was added dropwise and stirred. If there was no undissolved residue with 40 mg of charge transport material and 3960 mg of solvent, the solubility of the charge transport material in that solvent was determined to be between 1.0% and less than 2.0%. If there was any undissolved charge transport material under the above conditions, an additional 4000 mg of solvent was added dropwise and stirred. If there was no undissolved residue with 40 mg of charge transport material and 7960 mg of solvent, the solubility of the charge transport material in that solvent was determined to be between 0.5% and less than 1.0%. If there was still undissolved charge transport material under the above conditions, the solubility of the charge transport material in that solvent was determined to be less than 0.5%.

[0079] <Substrate Fabrication> As a substrate for the light-emitting element, a substrate 61 including a bank 62 and a region 63 surrounded by the bank 62 was fabricated, as shown in Figure 6, based on the method disclosed in Japanese Patent Application Publication No. 2008-46306. The region 63 surrounded by the bank 62 in Figure 6 is long in the X-axis direction, short in the Y-axis direction, and has rounded corners, with a length of 120 μm in the longitudinal direction (X-axis), a length of 34 μm in the transverse direction (Y-axis), and a depth of 1.5 μm. The region 63 surrounded by the bank 62 was formed in a matrix pattern with 15 μm intervals in the X-axis direction and 15 μm intervals in the Y-axis direction. In this embodiment, as shown in Figure 6, a so-called pixel bank was used in which the region 63 surrounded by the bank 62 is independent in both the X-axis and Y-axis directions, but a so-called line bank may also be used in which the regions surrounded by the banks are connected in the X-axis direction.

[0080] <Charge-Impregnated Layer Manufacturing Apparatus> A charge-impregnated layer manufacturing apparatus was fabricated as follows. As a liquid composition application apparatus, a modified inkjet printer (product name "Material Printer DMP-2831", manufactured by Fujifilm) equipped with an ejection head that applies mechanical energy generated by a piezoelectric element to the liquid composition to eject the liquid composition was used. Specifically, the cartridge-type ink tank of this inkjet printer was removed and modified so that the liquid composition could be supplied from the tank to the ejection head, which served as the liquid composition application unit, via a tube. A first tank and a second tank were installed, and a mixing unit was provided by connecting a channel (first supply channel) that could supply the second liquid composition from the second tank to the ejection head with a channel (second supply channel) that could supply the second liquid composition from the second tank. Furthermore, a mechanism was provided to adjust the supply amounts when supplying the first liquid composition from the first tank and when supplying the second liquid composition from the second tank, thereby controlling the mixing ratio of the first and second liquid compositions in the third liquid composition. Furthermore, a valve that can be opened and closed was provided between the first tank and the mixing section, and a suction mechanism was provided to discharge the liquid composition to the outside from the discharge head. The angle θ between the first supply channel and the second supply channel was set to 60°. One million drops of the third liquid composition were discharged from each nozzle, and the mass of the third liquid composition was measured. The discharge volume was calculated by dividing the mass by the density of the third liquid composition, and it was found to be an average of 3 pL per drop.

[0081] In the comparative example described later, only one liquid composition was used as the other liquid composition for forming the charge injection layer. However, for convenience, this liquid composition may also be referred to as the first liquid composition and the third liquid composition. In the comparative example, since only one liquid composition was used, that liquid composition was placed in the first tank, and nothing was placed in the second tank before applying the liquid composition to the substrate.

[0082] <Formation of Charge Implantation Layer> Using the above manufacturing apparatus, the first liquid composition and the second liquid composition shown in Table 2 (Tables 2-1 to 2-3) were mixed in the mixing section under the flow rate ratio (volume ratio) conditions shown in the table to form a third liquid composition. Then, the third liquid composition was applied to the region 63 surrounded by the bank 62 on the substrate 61, and the solvent was removed to form a charge implantation layer film. At this time, six droplets were applied to the region 63 surrounded by the bank 62, and the solvent was removed by natural drying without using heating or a vacuum dryer. It is generally known that the aperture ratio of the film changes depending on the drying conditions. In order to clarify the effect of improving the aperture ratio of the film by the solubility of the charge transport material in the solvent, in this test example, the solvent was removed by natural drying without using heating or a vacuum dryer, the polymerization reaction was carried out by heating at 200°C for 30 minutes, and the solvent was completely removed to form a charge implantation layer. Table 2 shows the boiling points (°C) of the first and second solvents, the solubility (%) of the charge-transporting material, and the HSP distance Ra (MPa) between the first and second solvents. 1/2 ) was also shown.

[0083] <Manufacturing of light-emitting element> Six drops of the above-described liquid composition for forming the charge transport layer were applied to the charge injection layer in the region 63 surrounded by the bank 62 on the substrate 61 using an inkjet device. The above-described charge injection layer manufacturing device was used as the inkjet device, but nothing was placed in the second tank, and the liquid composition for forming the charge transport layer was placed in the first tank and applied. After applying the liquid composition, the solvent was removed by natural drying, and the solvent was completely removed by heating at 200°C for 30 minutes to laminate the charge transport layer. Next, six drops of the above-described liquid composition for forming the light-emitting layer were applied to the region 63 surrounded by the bank 62, the solvent was removed by natural drying, and the solvent was removed by heating at 120°C for 30 minutes to laminate the light-emitting layer. The laminated film was formed in 100 rows in the X-axis direction and 300 columns in the Y-axis direction, for a total of 30,000 regions 63. A substrate 61 with a laminated film formed on it was placed in a vacuum deposition machine, and an electron transport layer (TPBi) with an average thickness of 55 nm, an electron injection layer (LiF) with an average thickness of 0.5 nm, and a cathode (aluminum) with an average thickness of 100 nm were continuously formed by deposition. Then, in a dry air atmosphere, a protective glass plate was placed over it and sealed with an acrylic resin adhesive to fabricate a light-emitting element.

[0084] <Evaluation> The manufactured light-emitting elements were evaluated as follows. In this embodiment, "AA," "A," and "B" were considered acceptable levels in the evaluation criteria for each item shown below, and "C" was considered an unacceptable level. The evaluation results are shown in the lower part of Table 2.

[0085] (Driving Voltage) The driving voltage was measured by applying a current of 12.2 mA to the obtained light-emitting element. The light-emitting elements of this embodiment and comparative example are formed in 30,000 regions 63 of 120 μm × 34 μm, with a total area of ​​approximately 1.22 cm². 2 Therefore, the current density is approximately 10 mA / cm². 2 In this evaluation, the following procedure was used to confirm the effect of suppressing the rise in the driving voltage of the light-emitting element when using a liquid composition that had been stored for a certain period of time.

[0086] For each example and comparative example, a third liquid composition was prepared in advance and, without storage, a charge injection layer was formed. A charge transport layer and an emissive layer were then sequentially stacked on top of it to create a light-emitting element, and the driving voltage was measured and used as a reference. Using the first liquid composition, the second liquid composition, and the liquid composition dispensing apparatus for each combination of the example and comparative example, after storage for three months, a charge injection layer was formed. A charge transport layer and an emissive layer were then sequentially stacked on top of it to create a light-emitting element, and the driving voltage was measured and compared with the above reference.

[0087] For example, in Example 1, liquid composition 1 and liquid composition 5 were pre-mixed in a 5:5 ratio to form a third liquid composition, and the driving voltage of the light-emitting element produced using this composition without storage was used as a reference. In addition, liquid composition 1 was stored in the first tank and liquid composition 5 in the second tank for three months, and the driving voltage of the light-emitting element produced using the charge injection layer manufacturing apparatus of Example 1 was measured and compared with the above reference.

[0088] Furthermore, in the case of Comparative Example 1, for example, the second liquid composition was not used, and a liquid composition (liquid composition 14) in which the charge transport material and the charge generating material were mixed in advance was used as the first liquid composition. As a result, the first liquid composition became substantially the same as the third liquid composition. Therefore, in the case of Comparative Example 1, the driving voltage of the light-emitting element that was used without storing liquid composition 14 was used as the standard. In addition, the driving voltage of the light-emitting element that was used after storing liquid composition 14 in the first tank for three months was measured and compared with the above standard. The effect of suppressing the rise in the driving voltage of the light-emitting element when using a liquid composition that has been stored for a certain period of time is due to the liquid composition used to form the charge injection layer. For this reason, the liquid composition for forming the charge transport layer and the liquid composition for forming the light-emitting layer were all used immediately after preparation without any storage. Furthermore, when manufacturing a light-emitting element after storing the liquid composition for three months, the liquid composition remaining in the part from the mixing section to the liquid composition application section in the charge injection layer manufacturing apparatus was not used and was pre-emptively aspirated and discarded.

[0089] The effect of suppressing the rise in drive voltage was evaluated according to the evaluation criteria shown below. A: The rate of increase in drive voltage was 0% or more and less than 5% compared to the standard. B: The rate of increase in drive voltage was 5% or more and less than 10% compared to the standard. C: The rate of increase in drive voltage was 10% or more compared to the standard.

[0090] (Membrane Aperture Ratio) The aperture ratio of the charge injection layer was calculated from the membrane shape of the charge injection layer measured using a stylus profiler (product name "Alpha-Step D-500", manufactured by KLA-Tencor). As shown by the dashed arrow 64 in Figure 6, the measurement was taken by scanning the center of the charge injection layer membrane in the X-axis direction in the Y-axis direction within the region 63 surrounded by the bank 62. For charge injection layers with an average overall film thickness of 38 nm to 42 nm, the length of the opened portion of the charge injection layer membrane at a height of 57 nm to 63 nm, which is 1.5 times the average film thickness, was measured according to the average film thickness, and the aperture ratio (%) of the charge injection layer membrane was calculated by dividing this length by the length of the bottom surface of the membrane. For example, in the case of a membrane with the shape shown in Figure 4, the length L2 of the membrane in the inner part of the region surrounded by the bank is measured at a height H of 60 nm from the bottom surface of the region. Then, the aperture ratio (%) of the charge injection layer film was determined by dividing the length L2 by the length L1 of the bottom surface of the film (34 μm, which is the length in the shorter direction of the region 63 enclosed by the bank 62 in this example and comparative example).

[0091] Furthermore, the total film thickness refers to the average value of the film thickness of the measured portion, not the film thickness at a specific location. For example, if a film with the shape shown in Figure 4 is obtained, the film thickness will be thinner in the center of the region surrounded by the bank and thicker at the edges, but the average value is defined as the overall average film thickness. When determining the aperture ratio of the film, if the absolute amount of charge-transporting material in the region surrounded by the bank is large, such as when a large amount of liquid composition is applied, the amount of charge-transporting material that accumulates at the edges of the region surrounded by the bank will be large. In this case, the length L2 of the opened portion will also be shorter, resulting in a lower aperture ratio and making it difficult to perform a proper evaluation. Therefore, charge-injection layer films with equivalent overall average film thicknesses were selected and used as the evaluation target. In this example and comparative example, 100 charge-injection layer films with overall average film thicknesses in the range of 38 nm to 42 nm were selected, the aperture ratio was calculated for each, and the average value was used as the measured value. The criteria for determining the aperture ratio were as follows.

[0092] Based on the measured aperture ratio of the charge-injection layer obtained by the method described above, the aperture ratio of the charge-injection layer was evaluated according to the evaluation criteria shown below. AA: The aperture ratio of the film was 80% or higher. A: The aperture ratio of the film was 70% or higher but less than 80%. B: The aperture ratio of the film was less than 70%.

[0093] (Discharge Recovery) After the discharge of the third liquid composition from the discharge head was completed, the equipment was left at room temperature and atmospheric pressure for three weeks, and then the charge implantation layer manufacturing apparatus was restarted. During this period, the nozzle of the discharge head was capped to suppress the evaporation of the solvent from the nozzle tip (discharge port). For those where discharge of the third liquid composition was not possible when the manufacturing apparatus was restarted, a suction operation was performed, and the amount of discarded liquid composition required to make discharge possible was measured. Based on the measured amount of discarded liquid composition, the applicability of the stored liquid composition was evaluated according to the evaluation criteria shown below. A: Discharge was possible with less than 0.5 cc of discarded liquid composition. B: Discharge was possible with 0.5 cc or more but less than 2.0 cc of discarded liquid composition. C: Discharge was not possible even with 2.0 cc or more of discarded liquid composition.

[0094] (Degree of Mixing) In the charge implantation layer manufacturing apparatus described above, the first liquid composition and the second liquid composition are mixed in the mixing section to form a third liquid composition. The degree of mixing at that time was evaluated by the following method. For the sake of simplicity of evaluation, the first and second tanks were not filled with functional materials, but only with the first and second solvents, respectively. The first and second solvents were mixed in the mixing section for evaluation. The flow rates of the first and second solvents were adjusted to a volume ratio of 1:1 to form the third liquid composition (a mixture of the first and second solvents). The liquid composition dispensing section was removed and the drops of the third liquid composition were captured. The volume of the drops was approximately 10 μL per drop. A total of 100 drops were captured, one drop at a time. The mixing ratio of the first and second solvents for each drop was determined from NMR, and the volume of the first solvent V1 / volume of the second solvent V2 was calculated. The standard deviation was calculated from 100 drops of V1 / V2, and the degree of mixing of the first and second solvents was evaluated according to the evaluation criteria shown below. A: Standard deviation was less than 0.03. B: Standard deviation was 0.03 or more and less than 0.05.

[0095]

[0096]

[0097]

[0098] <Evaluation Results> In all of the examples and comparative examples, a charge injection layer manufacturing apparatus 50 was used, which was equipped with an openable and closable valve 51 between the first tank 11 and the mixing section 13, as shown in Figure 5.

[0099] However, in order to confirm the effect of valve 51, in Examples 10 and 11, when the charge injection layer manufacturing apparatus 50 was not in operation, valve 51 was left open and not used, and the area 55 from the mixing section 13 to the liquid composition application section 14 was stored filled with the third liquid composition.

[0100] In the example, a first liquid composition containing a charge-transporting material having polymerizable functional groups and a second liquid composition containing a charge-generating material that also acts as a polymerization initiator were stored in separate tanks. As a result, even when using the stored liquid compositions, the increase in the driving voltage of the light-emitting element was suppressed. In contrast, in the comparative example, the charge-transporting material having polymerizable functional groups and the charge-generating material that also acts as a polymerization initiator were dissolved in the same liquid composition and stored. Therefore, when using the stored liquid composition, an increase in the driving voltage of the light-emitting element was observed.

[0101] From Examples 1-3 and Example 4, the HSP distance Ra between the first solvent and the second solvent was 10.0 MPa. 1/2 It was found that the aperture ratio of the charge injection layer film can be further increased, and the rise in the driving voltage of the light-emitting element can be further suppressed. This is thought to be because the degree of mixing between the first liquid composition containing the first solvent and the second liquid composition containing the second solvent is improved.

[0102] Examples 1-4, 9, and 10 use a good solvent with a charge transport material solubility of 4.0% or higher as the first solvent, and a poor solvent with a charge transport material solubility of less than 0.5% as the second solvent, where the boiling point of the second solvent is higher than that of the first solvent. It was confirmed that using such a solvent combination increases the aperture ratio of the charge implantation layer film. Of these, Examples 4 and 9 show a slightly lower effect on improving the film aperture ratio compared to the other examples. In Example 4, the HSP distance Ra between the first and second solvents is 10.0 MPa. 1/2 This is because the degree of mixing between the first and second solvents is slightly inferior, resulting in a limited effect on improving the membrane aperture ratio. Example 9 is an example where the volume of the first solvent in the third liquid composition is greater than the volume of the second solvent, and again, the effect on improving the membrane aperture ratio is limited.

[0103] On the other hand, in Example 5, a good solvent for the charge transport material is used as the first solvent and a poor solvent as the second solvent, but the first solvent has a higher boiling point than the second solvent. In this case, the second solvent evaporates first, and the concentration of the first solvent becomes high when the film is formed, so the effect of improving the aperture ratio by promoting the deposition of the charge transport material is not obtained. Also, in Examples 6 to 8 and 11, both the first and second solvents are good solvents for the charge transport material, so the effect of improving the aperture ratio of the film by promoting the deposition of the charge transport material is not obtained. However, even in such examples, the effect of suppressing the rise in driving voltage, which is the objective of this disclosure, can be obtained.

[0104] Furthermore, Examples 10 and 11 are examples in which an openable and closable valve installed between the first tank and the mixing section was not used. Example 10 has inferior discharge recovery performance compared to the other examples. This is because the charge transporting material and the second solvent, which is a poor solvent, were stored together in the section from the mixing section to the liquid composition application section, causing precipitation during storage. In contrast, in Example 11, since only good solvents for the charge transporting material were used for both the first and second solvents, the problem of precipitation during storage did not occur, and thus the discharge recovery performance did not decrease even without the provision of a valve.

[0105] The present invention is not limited to the embodiments described above, and various modifications and variations are possible without departing from the spirit and scope of the invention. Accordingly, the following claims are attached to make the scope of the invention public.

[0106] This application claims priority based on Japanese Patent Application No. 2025-080941, filed on 14 May 2025, and Japanese Patent Application No. 2026-079371, filed on 11 May 2026, and all of the contents of those applications are incorporated herein by reference.

[0107] 10, 50 Light-emitting element manufacturing apparatus 11 First tank 12 Second tank 13 Mixing section 14 Liquid composition application section 2 Bank 21, 31 Functional material 22, 32 Opening 23, 33, 43 Functional film 51 Valve 61 Substrate 62 Bank 63 Region

Claims

1. An apparatus for manufacturing a charge implantation layer, comprising: a first tank containing a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups; a second tank containing a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups; a mixing unit for mixing the first liquid composition and the second liquid composition to form a third liquid composition; and a liquid composition application unit for applying the third liquid composition onto a substrate, wherein the mixing unit is located between the first tank and the liquid composition application unit.

2. The distance Ra of the Hansen solubility parameter (HSP) between the first solvent and the second solvent is 10.0 MPa. 1/2 The apparatus for manufacturing a charge injection layer according to claim 1, which is as follows:

3. The apparatus for manufacturing a charge implantation layer according to claim 1 or 2, wherein the boiling point of the second solvent is higher than the boiling point of the first solvent, the solubility of the charge transporting material in the second solvent is less than 0.5% by mass, and the solubility of the charge transporting material in the second solvent is lower than the solubility of the charge transporting material in the first solvent.

4. A device for manufacturing a charge injection layer according to any one of claims 1 to 3, wherein V1 is the volume of the first solvent in the third liquid composition, and V2 is the volume of the second solvent in the third liquid composition, and V2 ≥ V1.

5. The charge implantation layer manufacturing apparatus according to any one of claims 1 to 4, further comprising a valve that can be opened and closed between the first tank and the mixing section, and having a mechanism to close the valve when the charge implantation layer manufacturing apparatus is in operation, thereby replacing the inside of the mixing section and the liquid composition application section with the second solvent.

6. An apparatus for manufacturing a charge injection layer according to any one of claims 1 to 5, comprising: a first supply channel for supplying the first liquid composition from the first tank to the mixing section; and a second supply channel for supplying the second liquid composition from the second tank to the mixing section.

7. A method for manufacturing a charge implantation layer, comprising: a first supply step of supplying a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups, which is contained in a first tank, to a mixing section; a second supply step of supplying a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups, which is contained in a second tank, to the mixing section; a mixing step of mixing the first liquid composition and the second liquid composition in the mixing section to form a third liquid composition; and a liquid composition application step of applying the third liquid composition onto a substrate, wherein the mixing step is performed immediately before the liquid composition application step.

8. An apparatus for manufacturing a light-emitting element, comprising an apparatus for manufacturing a charge injection layer, an apparatus for manufacturing a charge transport layer, and an apparatus for manufacturing a light-emitting layer, wherein the apparatus for manufacturing the charge injection layer comprises: a first tank containing a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups; a second tank containing a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups; a mixing unit for mixing the first liquid composition and the second liquid composition to form a third liquid composition; and a liquid composition application unit for applying the third liquid composition onto a substrate, wherein the mixing unit is disposed between the first tank and the liquid composition application unit.

9. A method for manufacturing a light-emitting element, comprising a step of forming a charge injection layer, a step of forming a charge transport layer, and a step of forming a light-emitting layer, wherein the step of forming the charge injection layer comprises: a first supply step of supplying a first liquid composition containing a first solvent and a charge transport material having polymerizable functional groups, which is contained in a first tank, to a mixing unit; a second supply step of supplying a second liquid composition containing a second solvent and a charge generating material that also acts as a polymerization initiator for the polymerizable functional groups, which is contained in a second tank, to the mixing unit; a mixing step of mixing the first liquid composition and the second liquid composition in the mixing unit to form a third liquid composition; and a liquid composition application step of applying the third liquid composition onto a substrate, wherein the mixing step is performed immediately before the liquid composition application step.