Adhesive film
The adhesive film with a high glass transition temperature base layer and polyolefin-based adhesive layer addresses adhesion and durability issues for fluoropolymer membranes, ensuring strong bonding and mechanical integrity in harsh conditions.
Patent Information
- Application Number
- PCT/JP2026/018206
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-19
AI Technical Summary
Existing adhesive films are unsuitable for fluoropolymer membranes due to inadequate adhesion properties and insufficient high-temperature and high-humidity resistance, particularly when directly adhering to fluoropolymer membranes without electrodes.
An adhesive film comprising a base layer with a glass transition temperature of 160°C or higher and an adhesive layer containing a polyolefin-based resin, optionally modified and with an aliphatic hydrocarbon resin additive, to enhance adhesion and resistance to high temperatures and humidity.
The adhesive film exhibits high adhesion to fluoropolymer membranes and maintains mechanical strength in high-temperature and high-humidity environments, suitable for applications like gasket films in fuel cells.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Adhesive Film
[0001] The present disclosure relates to an adhesive film, particularly an adhesive film for adhering to a fluoropolymer membrane.
[0002] In fuel cells, adhesive films are sometimes used to bond or seal constituent members to each other. As such an adhesive film, Patent Document 1 discloses an adhesive film comprising two polymer films and an adhesive layer, which bond so as to sandwich a membrane electrode assembly (MEA) having electrodes on both sides from the both sides.
[0003] International Publication No. 2022 / 084028
[0004] In fuel cells, fluoropolymer membranes are sometimes employed as solid electrolyte membranes. The adhesive film of Patent Document 1 has a problem that it is unsuitable for using a fluoropolymer membrane as an adherend. This problem arises firstly from the point that adhesive properties different from those for adhesion to electrodes are required for adhesion to fluoropolymer membranes. Secondly, when directly adhering to an electrolyte membrane without an electrode interposed, higher high-temperature and high-humidity resistance is required as compared with adhesion to an electrode, but the adhesive film of Patent Document 1 in which the two films are made of polyethylene naphthalate (PEN) has insufficient high-temperature and high-humidity resistance, which is the cause of the problem.
[0005] One aspect of the present disclosure aims to provide an adhesive film that exhibits high adhesion to fluoropolymer membranes and high high-temperature and high-humidity resistance.
[0006] To solve the above problem, an adhesive film according to one aspect of the present disclosure is an adhesive film for adhering to a fluoropolymer membrane, comprising a base material layer and an adhesive layer provided on the base material layer, wherein the glass transition temperature of the base material layer is 160°C or higher, the adhesive layer contains a polyolefin-based resin as a main component, and at least one of the following conditions (1) and (2) is satisfied: (1) the polyolefin-based resin is a modified polyolefin-based resin; (2) the adhesive layer further contains an aliphatic hydrocarbon resin as an additive.
[0007] According to one aspect of this disclosure, an adhesive film is provided that exhibits high adhesion to fluorine-based polymer films and high resistance to high temperatures and humidity.
[0008] <Adhesive Film> An adhesive film according to one aspect of the present disclosure is an adhesive film for bonding to a fluorine-based polymer film, comprising a base layer (A) and an adhesive layer (B) provided on the base layer (A), wherein the glass transition temperature of the base layer (A) is 160°C or higher, and the adhesive layer (B) contains a polyolefin resin (B1) as its main component, and satisfies at least one of the following conditions (1) and (2): (1) the polyolefin resin (B1) is a modified polyolefin resin; (2) the adhesive layer (B) further contains an aliphatic hydrocarbon resin (B2) as an additive. The adhesive film according to one aspect of the present disclosure exhibits high adhesion to fluorine-based polymer films and high resistance to high temperature and high humidity.
[0009] (Base layer (A)) Base layer (A) primarily serves to improve the high temperature and high humidity resistance of the adhesive film. Depending on the application of the adhesive film, base layer (A) may also serve to improve gas barrier properties, dimensional stability, high temperature resistance, and insulation properties.
[0010] The glass transition temperature Tg of the substrate layer (A) is 160°C or higher. Preferably, the Tg of the substrate layer (A) is 160°C or higher, more preferably 170°C or higher, and even more preferably 180°C or higher. The higher the Tg within this range, the better the high-temperature resistance of the adhesive film. There is no particular upper limit to the Tg of the substrate layer (A), but as an example, it may be 250°C or lower.
[0011] In this disclosure, the glass transition temperature Tg of the substrate layer (A) is measured using dynamic viscoelasticity measurement (DMA). DMA is performed in accordance with JIS K 7095:2012, using the substrate layer (A) peeled off from the adhesive film as a sample.
[0012] The thickness of the base layer (A) can be selected as appropriate. From the viewpoint of improving the mechanical strength of the adhesive film, the thickness of the base layer (A) is preferably 30 μm or more, and more preferably 50 μm or more. From the viewpoint of improving the flexibility of the adhesive film and, consequently, its adhesion to the adherend, the thickness of the base layer (A) is preferably 200 μm or less, and more preferably 150 μm or less.
[0013] The substrate layer (A) is made of resin, or in other words, contains resin (A1) as its main component. The resin (A1) of the substrate layer is not particularly limited as long as it achieves the glass transition temperature described above, and is typically a thermoplastic resin. Examples of resin (A1) include: resins containing aromatic ether structures or aromatic sulfide structures in repeating units, such as polyphenylene ether (PPE), polyphenylene sulfide (PPS), polysulfone (PSU), polyether ether ketone (PEEK), and polyimide (PI); polyolefin resins such as polymethylpentene (PMP); and so on. The resin (A1) may be homemade or commercially available. Examples of commercially available resins include TPX (registered trademark, manufactured by Mitsui Chemicals, Inc.), which is classified as PMP, and XYRON (registered trademark, manufactured by Asahi Kasei Corporation), Yupiace (registered trademark, manufactured by Global Polyacetal Corporation), NORYL (registered trademark, manufactured by SABIC Corporation), which are classified as PPE.
[0014] From the viewpoint of further improving the high temperature and high humidity resistance of the adhesive film while improving the adhesion between the adhesive layer (B) and the substrate layer (A), the substrate layer (A) preferably contains at least one resin (A1) selected from the group consisting of PPE, PPS, and PMP, and more preferably contains PPE. PPE is also preferable from the viewpoint of reducing the manufacturing cost of the adhesive film.
[0015] When PPE is used as the resin (A1), it is preferable that the PPE is a polymer alloy with another resin, i.e., a modified polyphenylene ether (m-PPE). Examples of m-PPE include polyphenylene ether / polystyrene (PPE / PS), polyamide / polyphenylene ether (PA / PPE), polypropylene / polyphenylene ether (PP / PPE), and polyphenylene sulfide / polyphenylene ether (PPS / PPE). Among these, from the viewpoint of low hygroscopicity and high temperature resistance, it is preferable that the m-PPE be PPE / PS or PPS / PPE. Furthermore, from the viewpoint of cost and processability (film formation), PPE / PS is preferred.
[0016] Furthermore, the inventors have newly discovered that even when tensile stress is continuously applied to the adhesive film in a high-temperature environment, due to its high high-temperature resistance, distortion and fracture do not occur in the parts where the stress is applied (parts that are not clamped), but cracks may occur in the film in the parts where the film is clamped (chuck parts). From the viewpoint of suppressing such cracks in the chuck parts, it is preferable that m-PPE be selected from the group consisting of PPE / PS and PP / PPE, and more preferably PP / PPE.
[0017] The resin (A1) may be one type or any combination of two or more types. When the resin (A1) is a combination of two or more types, examples of preferred combinations include PPE and PP, PPE and PMP, PPE and PE, PPE and PS, etc.
[0018] In the base layer (A), the content of resin (A1) is such that it constitutes the main component, and may be, for example, 50% or more by mass, 60% or more by mass, 70% or more by mass, 80% or more by mass, 90% or more by mass, 95% or more by mass, or 99% or more by mass, relative to 100% by mass of the base layer (A). The content of resin (A1) is usually 100% or less by mass, relative to 100% by mass of the base layer.
[0019] The base layer (A) may further contain additives (A2) as the remainder of the main component resin (A1). Examples of additives (A2) in the base layer include flame retardants, colorants, fillers, elastomers, fibers, etc. Additives (A2) may be one type or any combination of two or more types.
[0020] The additive (A2) can be appropriately selected according to the desired properties of the base layer (A). When cracking in the chuck area is suppressed, a thermoplastic elastomer is a preferred example of the additive. However, since the addition of a thermoplastic elastomer may reduce the mechanical strength of the base layer (A), it is particularly preferable to combine it with a resin (A1) that already has high mechanical strength. An example of such a resin (A1) is PPE / PS.
[0021] When PPE / PS is used as the resin (A1), for example, from the viewpoint of ensuring both mechanical strength and tensile strength by increasing the proportion of polystyrene blocks in the base layer (A), it is preferable to use a block copolymer having polystyrene blocks among thermoplastic elastomers. It is preferable that the block copolymer has polystyrene blocks at at least one end, and more preferably at both ends.
[0022] The polystyrene block content is preferably 15% to 60% by mass, and more preferably 20% to 50% by mass, relative to 100% by mass of the block copolymer.
[0023] Other blocks that can be found in thermoplastic elastomer block copolymers include polyethylene blocks, polybutylene blocks, and polypropylene blocks. For example, a combination of polyethylene blocks and polybutylene blocks is preferred from the viewpoint of ensuring both mechanical strength and tensile strength. Other blocks may be obtained by hydrogenation of polybutadiene blocks.
[0024] Thermoplastic elastomers may be homemade or commercially available. Examples of commercially available products include Septon (registered trademark, manufactured by Kuraray Co., Ltd.), ToughTec (registered trademark, manufactured by Asahi Kasei Corporation), and Kraton. TM Examples include G (manufactured by Kraton) and TR (manufactured by Eneos Materials).
[0025] (Adhesive layer (B)) The adhesive layer (B) is provided on the substrate layer (A). The adhesive layer (B) exhibits good adhesion to both the fluorine-based polymer film that is the adherend and the substrate layer (A).
[0026] The adhesive layer (B) is preferably provided directly on the substrate layer (A), i.e., adjacent to the substrate layer (A), in order to exhibit good adhesion to the substrate layer (A). However, the present disclosure is not limited to this configuration. The adhesive layer (B) may be provided indirectly on the substrate layer (A), i.e., another layer may be provided between the substrate layer (A) and the adhesive layer (B), as long as the adhesion is not impaired. Examples of other layers include a surface modification layer formed by surface treatment of the substrate layer (A), a primer layer formed by applying a primer to the substrate layer (A), and the like.
[0027] In an adhesive film, the adhesive layer (B) may be provided on one surface of the base material layer (A), or on both surfaces of the base material layer (A).
[0028] The adhesive layer (B) is made of a polyolefin resin, or in other words, it contains a polyolefin resin (B1) as its main component.
[0029] Examples of polyolefin resins (B1) include olefin polymers such as polyethylene (PE) and polypropylene (PP). The polyethylene may be ultra-low density polyethylene (LLDPE), low density polyethylene (LDPE), or high density polyethylene (HDPE), with LDPE being preferred.
[0030] Other examples of polyolefin resins (B1) include copolymers of two or more olefin monomers, such as ethylene-propylene copolymers and cyclic olefin copolymers; and copolymers of olefin monomers and non-olefin monomers, such as ethylene vinyl acetate (EVA). The mode of copolymerization may be alternating copolymerization, random copolymerization, block copolymerization, or graft copolymerization.
[0031] The melting point of the polyolefin resin (B1) is preferably 100°C or higher, and more preferably 120°C or higher, in order to prevent the adhesive layer from melting at, for example, the operating temperature of a fuel cell in a laminate of a fluorine polymer film and an adhesive film. The upper limit of the melting point of the polyolefin resin (B1) is not particularly limited, but since the processing temperature for bonding, such as hot pressing, is preferably relatively low, it is preferably 200°C or lower, and more preferably 180°C or lower.
[0032] In this disclosure, the melting point of the polyolefin resin (B1) is measured using the method specified in JIS K 7121:1987.
[0033] The melt flow rate (MFR) of the polyolefin resin (B1) is preferably 0.1 g / 10 min or more, and more preferably 0.3 g / 10 min or more, from the viewpoint of high temperature resistance. The MFR of the polyolefin resin (B1) is preferably 30 g / 10 min or less, and more preferably 28 g / 10 min or less, from the viewpoint of processability.
[0034] In this disclosure, the MFR of the polyolefin resin (B1) is measured using the method specified in JIS K 7210-1:2014.
[0035] In the adhesive layer (B), at least one of the following conditions (1) and (2) is satisfied: (1) The polyolefin resin (B1) is a modified polyolefin resin. (2) The adhesive layer (B) further contains an aliphatic hydrocarbon resin (B2) as an additive.
[0036] If the adhesive layer (B) is merely made of a polyolefin resin and does not satisfy either condition (1) or (2), it will exhibit high adhesion to only one of the substrate layer (A) or the fluorine-based polymer film, as shown in the embodiments of this disclosure. The inventors have found that by satisfying at least one of the above conditions (1) and (2), the adhesive layer (B) exhibits high adhesion to both the aforementioned substrate layer (A), which exhibits high resistance to high temperature and high humidity, and the fluorine-based polymer film, and have completed the present invention.
[0037] From the viewpoint of further improving the adhesion of the adhesive film to the fluorine-based polymer film, it is preferable that the adhesive layer (B) satisfies either condition (1) or (2), more preferably that at least condition (1) is satisfied, and even more preferably that both conditions (1) and (2) are satisfied.
[0038] Regarding condition (1), the modified polyolefin resin is a resin in which functional groups have been introduced to a polyolefin resin by graft polymerization or the like. Examples of modified polyolefin resins include: cationic modified polyolefin resins such as imine-modified resins; and anionic modified polyolefin resins such as carboxylic acid-modified, acid anhydride-modified, and maleic acid-modified resins. From the viewpoint of further improving the adhesion of the adhesive film to the fluorine-based polymer film, the modified polyolefin resin is preferably a cationic modified polyolefin resin, and more preferably an imine-modified polyolefin resin. Cationic modified, and especially imine-modified polyolefin resins, are expected to show high adhesion to resins (A1) constituting the base layer (A), particularly those containing aromatic ether structures or aromatic sulfide structures in the repeating units.
[0039] The modified polyolefin resin may be homemade or commercially available. Examples of commercially available products include Admer (registered trademark, manufactured by Mitsui Chemicals), Hardlen (registered trademark, manufactured by Toyobo MC Co., Ltd.), Lyosen (registered trademark, manufactured by artience Inc.), and Rioflex (registered trademark, manufactured by artience Inc.). The polyolefin resin (B1) may be one type or any combination of two or more types.
[0040] Regarding condition (2), the aliphatic hydrocarbon resin (B2) may be a known one as a tackifier. The aliphatic hydrocarbon resin (B2) may be either a polymer of aliphatic monomers or a copolymer of an aliphatic monomer and other monomers, and is preferably a polymer of aliphatic monomers. Examples of other monomers include aromatic monomers such as styrene.
[0041] From the viewpoint of high-temperature resistance, the softening point of the aliphatic hydrocarbon resin (B2) is preferably 80°C or higher, and more preferably 90°C or higher. The upper limit of the softening point of the aliphatic hydrocarbon resin (B2) is not particularly limited, but since the processing temperature for bonding such as hot pressing is preferably a relatively low temperature, it is preferably 180°C or lower, and more preferably 160°C or lower.
[0042] From the viewpoint of improving the adhesion to the highly polar base material layer (A), the acid value of the aliphatic hydrocarbon resin (B2) is preferably 0 KOH·mg / g or more, and more preferably 0.1 KOH·mg / g or more. From the viewpoint of improving viscosity stability, the acid value of the aliphatic hydrocarbon resin (B2) is preferably 2.0 KOH·mg / g or less, and more preferably 1.7 KOH·mg / g or less.
[0043] In the adhesive layer (B), the content of the polyolefin resin (B1) is at a level that serves as the main component, and relative to 100 mass% of the adhesive layer (B), it may be, for example, 50 mass% or more, 60 mass% or more, 70 mass% or more, 80 mass% or more, 90 mass% or more, 95 mass% or more, or 99 mass% or more. The content of the polyolefin resin (B1) is usually 100 mass% or less relative to 100 mass% of the adhesive layer (B).
[0044] In the adhesive layer (B), the content of the aliphatic hydrocarbon resin (B2) may be, for example, 5 mass% or more, or 10 mass% or more relative to 100 mass% of the adhesive layer (B). The content of the aliphatic hydrocarbon resin (B2) is usually 30 mass% or less relative to 100 mass% of the adhesive layer (B).
[0045] The adhesive layer (B) may further contain an additive (B3) as the balance other than the polyolefin-based resin (B1) and the aliphatic hydrocarbon resin (B2) which are the main components. Examples of the additive (B3) for the adhesive layer include silane coupling agents and the like.
[0046] The thickness of the adhesive layer (B) only needs to be sufficiently thick to develop adhesiveness, and is preferably 1 μm or more, more preferably 5 μm or more. The upper limit is not particularly limited, but from the factors such as cost, the thickness of the adhesive layer (B) is preferably 50 μm or less, more preferably 30 μm or less.
[0047] (Additional Layers) The adhesive film may consist of the base material layer (A) and the adhesive layer (B), or may further be provided with additional layers. Examples of the additional layers include a protective layer, a release layer, a primer layer, a surface modification layer and the like.
[0048] The position of the additional layer is appropriately selected according to the use and function of the additional layer. For example, the protective layer is usually provided on the surface of the base material layer (A) opposite to the adhesive layer (B). When the additional layer is a layer such as a release layer that is peeled off before the use of the adhesive film (before adhesion to the fluoropolymer film), the additional layer may be provided on the surface of the adhesive layer (B) opposite to the base material layer (A). When the additional layer is a layer such as a primer layer and a surface modification layer that does not impair the adhesiveness of the adhesive layer (B) to the base material layer (A), the additional layer may be provided between the base material layer (A) and the adhesive layer (B).
[0049] (Use of Adhesive Film) The adhesive film according to one aspect of the present disclosure is suitably used in applications where it is adhered to a fluoropolymer film, due to its high adhesiveness to the fluoropolymer film. Fluoropolymer films are put into practical use in various fields, and without limiting the present disclosure, examples of their applications include solid electrolyte membranes in fuel cells, water electrolysis membranes, chemical and biological sensors, and the like. The adhesive film according to one aspect of the present disclosure, which is capable of strongly adhering to such a fluoropolymer film, is useful in various fields.
[0050] Because adhesive films exhibit high resistance to high temperatures and humidity, they are particularly suitable for applications where the adhesive film is exposed to high-temperature and high-humidity environments. For example, gasket films bonded to fluorine-based polymer films in fuel cells are generally exposed to heat generated from the MEA (Mechanical Energy Acquisition Area) containing the polymer film and moisture introduced into the MEA to adjust power generation efficiency. Therefore, they are required to maintain mechanical strength in high-temperature and high-humidity environments. In conventional adhesive films, a decrease in mechanical strength is observed due to hydrolysis of the PEN (Penetrating Energy Acquisition) substrate under such conditions.
[0051] On the other hand, the adhesive film according to one aspect of this disclosure, since it comprises the above-described substrate layer (A), can maintain its mechanical strength even in high-temperature and high-humidity environments. Furthermore, since the adhesive film according to one aspect of this disclosure comprises the above-described adhesive layer (B) which exhibits high adhesion to both the substrate layer (A) and the fluorine-based polymer film, it can also achieve the adhesion required for a gasket film. Therefore, the adhesive film according to one aspect of this disclosure is suitable as a gasket film to be bonded to a fluorine-based polymer film in a fuel cell.
[0052] Without limiting the scope of this disclosure, examples of fluorine-based polymer films that serve as adherends exhibiting high adhesion to adhesive films include perfluorosulfonic acid polymer films such as Nafion (registered trademark, manufactured by Chemours), Aquivion (registered trademark, manufactured by Scienceco), and Flemion (registered trademark, manufactured by AGC).
[0053] <Method for manufacturing adhesive film> An adhesive film according to one aspect of the present disclosure can be manufactured by laminating the above-described substrate layer (A) and adhesive layer (B) in a known manner.
[0054] As an example, a resin composition containing the components of the base layer (A) is formed using an extrusion film-making machine to create the base layer (A). If necessary, after stretching the base layer (A), a resin composition containing the components of the adhesive layer (B) is laminated onto the base layer (A) using an extrusion laminating machine to obtain an adhesive film. Alternatively, an adhesive film may be obtained by laminating the adhesive layer (B) onto the base layer (A) using a coating method or a vapor deposition method.
[0055] As another example, an adhesive film may be obtained by co-extruding a resin composition for a base layer (A) and a resin composition for an adhesive layer (B).
[0056] <Additional Notes> This disclosure is not limited to the embodiments described above, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of this disclosure.
[0057] <Summary> As can be understood from the above explanation, this disclosure encompasses the following aspects.
[0058] Embodiment 1: An adhesive film for bonding to a fluorine-based polymer film, comprising a base layer and an adhesive layer provided on the base layer, wherein the glass transition temperature of the base layer is 160°C or higher, and the adhesive layer contains a polyolefin resin as its main component, satisfying at least one of the following conditions (1) and (2): (1) The polyolefin resin is a modified polyolefin resin, (2) The adhesive layer further contains an aliphatic hydrocarbon resin as an additive. According to Embodiment 1, an adhesive film is provided that exhibits high adhesion to a fluorine-based polymer film and high resistance to high temperature and high humidity.
[0059] Embodiment 2: The adhesive film of Embodiment 1, wherein both conditions (1) and (2) above are satisfied. According to Embodiment 2, the adhesion of the adhesive film to the fluorine-based polymer film is further improved.
[0060] Embodiment 3: The adhesive film of Embodiment 1 or 2, wherein the substrate layer contains polyphenylene ether. According to Embodiment 3, the high temperature and high humidity resistance of the adhesive film is further improved.
[0061] Embodiment 4: The adhesive film of any one of Embodiments 1 to 3, wherein the base layer contains a modified polyphenylene ether selected from the group consisting of polyphenylene ether / polystyrene (PPE / PS) and polypropylene / polyphenylene ether (PP / PPE). According to Embodiment 4, when tensile stress is continuously applied to the adhesive film in a high-temperature environment, the occurrence of cracks in the film at the clamped portion (chuck portion) is suppressed.
[0062] Embodiment 5: An adhesive film according to any one of Embodiments 1 to 4, wherein the base layer contains polyphenylene ether / polystyrene (PPE / PS) as the main component and a thermoplastic elastomer which is a block copolymer having a polystyrene block at at least one end as an additive. According to Embodiment 5, the mechanical strength of the base layer is improved while cracking of the film at the chuck portion is suppressed.
[0063] Embodiment 6: The adhesive film of Embodiment 5, wherein the block copolymer further comprises polyethylene blocks and polybutylene blocks. According to Embodiment 6, the occurrence of cracks in the film at the chuck portion is further suppressed.
[0064] Embodiment 7: The modified polyolefin resin is an imine-modified polyolefin resin, and the adhesive film is one of Embodiments 1 to 6. According to Embodiment 7, the adhesion of the adhesive film to the fluorine-based polymer film is further improved.
[0065] Embodiment 8: An adhesive film, one of Embodiments 1 to 7, which is a gasket film to be bonded to the fluorine-based polymer film in a fuel cell. According to Embodiment 8, an adhesive film suitable as a gasket film is provided.
[0066] An embodiment of the present disclosure is described below. In this embodiment, the mechanical strength of the fabricated substrate layer was tested under high temperature and high humidity conditions. In addition, adhesive layers were fabricated with various compositions, and the adhesion of the adhesive layers in a laminate comprising these layers was tested.
[0067] <Materials> The following materials were used in this example.
[0068] • Base resin 1: Polyphenylene ether / polystyrene (PPE / PS) resin (Tg: 190°C) • Base resin 2: Polypropylene / polyphenylene ether (PP / PPE) resin (Tg: 210°C)
[0069] • Base material additive 1: Polystyrene / polyethylene / polybutylene / polystyrene (SEBS) block copolymer (ToughTec® MP-10, polystyrene content: 32% by mass) • Base material additive 2: Polystyrene / polyethylene / polybutylene / polystyrene (SEBS) block copolymer (ToughTec® H1517, polystyrene content: 43% by mass)
[0070] • Adhesive base resin 1: Imine-modified polyolefin resin (Admer® AT2937, manufactured by Mitsui Chemicals, Inc., melting point: 135°C, MFR: 2.0 g / 10 min) • Adhesive base resin 2: Low-density polyethylene (Sumikasen® F200, manufactured by Sumitomo Chemical Co., Ltd., melting point: 111°C, MFR: 2.0 g / 10 min) • Adhesive base resin 3: Low-density polyethylene (Suntec-LD L4490, manufactured by Asahi Kasei Corporation, melting point: 130°C, MFR: 8.3 g / 10 min) • Adhesive base resin 4: High-density polyethylene (KEIYO Polyethylene E8080, manufactured by Keiyo Polyethylene Co., Ltd., melting point: 136°C, MFR: 1.0 g / 10 min) • Adhesive base resin 5: Polypropylene (Novatec PP FL03H, manufactured by Nippon Polypropylene Co., Ltd., melting point: 160°C, MFR: 26g / 10min)
[0071] • Adhesive additive 1: Aliphatic hydrocarbon resin (Quinton® C210, manufactured by Nippon Zeon Co., Ltd., softening point 110°C, acid value 1.7 KOH・mg / g) • Adhesive additive 2: Styrene / aliphatic copolymer hydrocarbon resin (FTR® 6100, manufactured by Mitsui Chemicals, Inc., softening point 95°C, acid value <0.1 KOH・mg / g)
[0072] • Fluorine film 1: Fluorine-based polymer film (Nafion® NR212, manufactured by Chemours)
[0073] <Test Example 1: Measurement of Mechanical Strength of Substrate Layer under High Temperature and High Humidity Environment> (Test Method) For each test, the fabricated substrate layer was cut into strips 160 mm long and 15 mm wide, so that the longitudinal direction of the sample was either the MD direction (film formation direction) or the TD direction (perpendicular to the MD direction), to obtain a sample. The sample was placed in a PCT (Pressure Cooker Test) apparatus and maintained at a temperature of 110°C and a relative humidity of 100% RH for 90 hours, 180 hours, or 270 hours.
[0074] Tensile tests were performed on initial (untreated with PCT) and post-holding samples using a tensile testing machine (Shimadzu Corporation, AGX-VD) to measure the elongation at fracture and the maximum stress obtained before fracture. The retention rate was calculated as the ratio (%) of the post-holding measurement to the initial measurement.
[0075] (Example 1-1) A 100% by mass base resin 1 was used to form a 100 μm thick base layer using an extruder.
[0076] (Results) The results of Test Example 1 are shown in Table 1.
[0077]
[0078] As shown in Table 1, the substrate layer of Example 1-1 maintained its mechanical strength without hydrolysis even when exposed to a high-temperature, high-humidity environment for a long period of time, and therefore can be said to have shown high resistance to high temperature and high humidity.
[0079] <Test Example 2: Evaluation of Adhesion> (Test Method) The prepared adhesive layer was cut into strips 40 mm long and 20 mm wide. The cut adhesive layer was sandwiched between two substrate layers of Example 1-1, or two fluorine films 1, and heated with an iron at approximately 160°C for 20 seconds to prepare a laminate of substrate layer / adhesive layer / substrate layer, or fluorine film 1 / adhesive layer / fluorine film 1. After the laminate was allowed to cool at room temperature, the adhesive surfaces between the layers were peeled off, and the peel strength was evaluated on a four-point scale according to the following criteria.
[0080] 4: The layers are very strongly bonded to each other. 3: The layers are strongly bonded to each other. 2: The layers are sufficiently bonded to each other. 1: The layers are not bonded to each other.
[0081] A rating of 2 or higher for the fluorine film indicates high adhesion to fluorine-based polymer films. A rating of 2 or higher for the substrate layer indicates that the substrate layer is less likely to peel off and is suitable for practical use as an adhesive film.
[0082] (Example 2-1) 100 parts by mass of adhesive base resin 1 was kneaded and a 10 μm thick adhesive layer was formed using the T-die method.
[0083] (Example 2-2) 100 parts by mass of adhesive base resin 1 and 10 parts by mass of adhesive additive 1 were kneaded together, and an adhesive layer with a thickness of 10 μm was formed using the T-die method.
[0084] (Examples 2-3 to 2-18, Comparative Example 2-1) The same procedure as in Example 2-2 was performed, except that the formulation amounts shown in Table 2 were used, to prepare the adhesive layer.
[0085] (Results) The results of Test Example 2 are shown in Table 2.
[0086]
[0087] As shown in Table 2, Examples 2-1 to 2-18, which satisfy either condition (1) or (2) above, showed excellent adhesion to both the substrate layer and the fluorine film. Among these, Examples 2-2 to 2-7, which satisfy both conditions (1) and (2), showed particularly excellent adhesion.
[0088] <Test Example 3: Evaluation of the effect of additives on the mechanical strength of the substrate layer> (Test method) For each test, the fabricated substrate layer was cut into strips 160 mm long and 15 mm wide, so that the longitudinal direction of the sample was in the MD direction (film formation direction) or the TD direction (perpendicular to the MD direction), and samples were obtained. The samples were placed in a constant temperature bath at 23°C or 60°C and held for 2 minutes.
[0089] Tensile tests were performed on the held samples using a tensile testing machine (Shimadzu Corporation, AGX-VD), and the tensile stress, modulus of elasticity, and elongation at fracture were measured.
[0090] Furthermore, the glass transition temperature Tg of the sample was measured using dynamic viscoelasticity measurement (DMA).
[0091] (Example 3-1) A 100% by mass base resin 1 was used to form a 50 μm thick base layer using an extruder.
[0092] (Examples 3-2 to 3-4) The same procedure as in Example 3-1 was followed, except that the formulation amounts shown in Table 3 were used, to form a substrate layer.
[0093] (Results) The results of Test Example 3 are shown in Table 3. In Table 3, "-" indicates that the measurement experiment was not performed.
[0094] For practical purposes, a tensile stress of 35 MPa or more in both the MD and TD directions is sufficient, and 45 MPa or more is more preferable. For practical purposes, an elastic modulus of 800 MPa or more in both the MD and TD directions is sufficient, and 1000 MPa or more is more preferable.
[0095]
[0096] <Test Example 4: Evaluation of the effect of additives on cracking in the substrate layer> (Test Method) For each test, the fabricated substrate layer was cut into strips 160 mm long and 15 mm wide, so that the longitudinal direction of the sample was in the MD direction (film formation direction) or the TD direction (perpendicular to the MD direction), and samples were obtained. The samples were clamped (chucked) using a tensile testing machine (Shimadzu Corporation, AGX-VD) with a chuck pressure of 0.4 MPa and a temperature of 120°C for 2 hours. After holding, the samples were removed and visually observed, and the degree of cracking was evaluated on a four-point scale according to the following criteria.
[0097] 4: No cracks (fissures in the sample) or warping (undulation of the sample) are observed. 3: No cracks are observed, but warping is observed. 2: Intermittent cracks are observed at the peripheral edges of the sample (the test sample used was relatively small compared to those used in practical applications, so the cracks at the peripheral edges were determined to be specific to the test sample and would not affect practical use). 1: Long cracks that break the sample are observed.
[0098] A crack rating of 2 to 4 indicates that the adhesive film is suitable for practical use.
[0099] (Example 4-1) A 100% by mass base resin 1 was used to form a 50 μm thick substrate layer using an extruder.
[0100] (Examples 4-2 to 4-8) The same procedure as in Example 4-1 was followed, except that the formulation amounts shown in Table 4 were used, to form a substrate layer.
[0101] (Results) The results of Test Example 4 are shown in Table 4.
[0102]
[0103] As shown in Table 4, adding a thermoplastic elastomer (additive), which is a block copolymer containing polystyrene blocks, to the base resin improved crack resistance. Furthermore, as shown in Table 3, while the addition of the thermoplastic elastomer tended to decrease mechanical strength, it still maintained sufficient mechanical strength for practical use.
[0104] The adhesive film relating to this disclosure can be used in applications where a fluorine-based polymer film is used as the substrate.
Claims
1. An adhesive film for bonding to a fluorine-based polymer film, comprising a base layer and an adhesive layer provided on the base layer, wherein the glass transition temperature of the base layer is 160°C or higher, the adhesive layer contains a polyolefin resin as its main component, and at least one of the following conditions (1) and (2) is satisfied: (1) the polyolefin resin is a modified polyolefin resin, (2) the adhesive layer further contains an aliphatic hydrocarbon resin as an additive.
2. The adhesive film according to claim 1, wherein both of the above conditions (1) and (2) are satisfied.
3. The adhesive film according to claim 1, wherein the base layer contains polyphenylene ether.
4. The adhesive film according to claim 1, wherein the substrate layer contains a modified polyphenylene ether selected from the group consisting of polyphenylene ether / polystyrene (PPE / PS) and polypropylene / polyphenylene ether (PP / PPE).
5. The adhesive film according to claim 1, wherein the base layer contains polyphenylene ether / polystyrene (PPE / PS) as a main component and contains a thermoplastic elastomer which is a block copolymer having a polystyrene block at at least one end as an additive.
6. The adhesive film according to claim 5, wherein the block copolymer further comprises polyethylene blocks and polybutylene blocks.
7. The adhesive film according to claim 1, wherein the modified polyolefin resin is an imine-modified polyolefin resin.
8. The adhesive film according to any one of claims 1 to 7, which is a gasket film to be bonded to the fluorine-based polymer film in a fuel cell.