Polyamide composition and molded article composed of said polyamide composition
A semi-aromatic polyamide composition with a halogenated flame retardant and filler addresses the challenge of flame retardancy and deformation in electronic components, ensuring their integrity during the reflow process.
Patent Information
- Application Number
- PCT/JP2026/018356
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional polyamide materials face challenges in achieving high flame retardancy and preventing deformation during the reflow process, which is critical for smaller and lighter electrical and electronic components.
A polyamide composition comprising a semi-aromatic polyamide with specific structural units, a halogenated flame retardant, and a filler, optimized to suppress deformation during the reflow process while maintaining excellent flame retardancy.
The composition achieves both high flame retardancy and suppresses deformation, ensuring the integrity of smaller and lighter electronic components.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000044_0000 
Figure 00000044_0001
Abstract
Description
Polyamide composition and molded article made from the polyamide composition
[0001] The present invention relates to a polyamide composition comprising a specific polyamide, a halogenated flame retardant, and a filler, and to a molded article made from the polyamide composition.
[0002] Crystalline polyamides, such as nylon 6 and nylon 66, are widely used in industrial parts due to their excellent heat resistance, mechanical properties, and moldability. In electrical and electronic component applications, a high level of flame retardancy based on the UL-94 standard is required, and various methods for flame-retardantizing polyamide compositions using flame retardants have been proposed. For example, Patent Document 1 discloses that by blending a polyamide resin containing a ternary copolymer polyamide resin of PA66 / PA6I / PA6 with a specific copolymerization ratio, a flame retardant, an antimony compound, and an inorganic filler, excellent flame retardancy, rigidity, and impact resistance can be simultaneously satisfied.
[0003] Japanese Patent Publication No. 2008-111064
[0004] On the other hand, in the field of electrical and electronic components, recent years have seen a trend towards smaller and lighter product sizes, and consequently, smaller and thinner components. This has presented a challenge in that conventional materials make it difficult to suppress deformation during the reflow process.
[0005] In view of the above circumstances, the present invention provides a polyamide composition that has excellent flame retardancy and can suppress deformation during the reflow process, and a molded article made from the polyamide composition.
[0006] As a result of diligent research to solve the above problems, the inventors of this invention have come up with the following invention and found that it can solve the problems.
[0007] [1] A polyamide composition comprising a polyamide (A), a halogenated flame retardant (B), and a filler (C), wherein the polyamide (A) is a semi-aromatic polyamide, the semi-aromatic polyamide comprises structural units derived from a dicarboxylic acid and structural units derived from a diamine, more than 50 mol% of the structural units derived from the dicarboxylic acid are structural units derived from an aromatic dicarboxylic acid, and more than 50 mol% of the structural units derived from the diamine are structural units derived from an aliphatic diamine having 7 to 18 carbon atoms, and the composition contains 1 to 100 parts by weight of the halogenated flame retardant (B) and 150 to 350 parts by weight of the filler (C) per 100 parts by weight of the polyamide (A). [2] The polyamide composition according to [1], wherein the aliphatic diamine is at least one selected from the group consisting of 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine. [3] The polyamide composition according to [1] or [2], wherein the aliphatic diamine comprises 1,9-nonanediamine and 2-methyl-1,8-octanediamine, and the molar ratio of 1,9-nonanediamine to 2-methyl-1,8-octanediamine is 60 / 40 to 10 / 90. [4] The polyamide composition according to [1] or [2], wherein the aliphatic diamine comprises 1,9-nonanediamine and 2-methyl-1,8-octanediamine, and the molar ratio of 1,9-nonanediamine to 2-methyl-1,8-octanediamine is 90 / 10 to 60 / 40. [5] The polyamide composition according to any one of [1] to [4], wherein the weight-average molecular weight (Mw) of the polyamide (A) composition is 18,000 to 30,000 g / mol. [6] The polyamide composition according to any one of [1] to [5], wherein the halogenated flame retardant (B) comprises a brominated flame retardant (B1). [7] The polyamide composition according to [6], wherein the brominated flame retardant (B1) comprises brominated polystyrene. [8] The polyamide composition according to any one of [1] to [7], wherein the halogenated flame retardant (B) is contained in an amount of 30 to 45 parts by weight per 100 parts by weight of the polyamide (A). [9] The polyamide composition according to any one of [1] to [8], wherein the filler (C) comprises a fibrous filler (C1).
[10] The polyamide composition according to [9], wherein the fibrous filler (C1) is at least one selected from the group consisting of carbon fiber, glass fiber, and aramid fiber.
[11] The polyamide composition according to any one of [1] to
[10] , wherein the polyamide (A) content is 10 to 40% by weight.
[12] The polyamide composition according to any one of [1] to
[11] , further containing a flame retardant aid (D).
[13] The polyamide composition according to
[12] , containing 1 to 30 parts by weight of the flame retardant aid (D) per 100 parts by weight of the polyamide (A).
[14] The polyamide composition according to
[12] or
[13] , wherein the flame retardant aid (D) is at least one selected from the group consisting of antimony trioxide, antimony tetroxide, antimony pentoxide, sodium antimonate, melamine orthophosphate, melamine pyrophosphate, melamine borate, melamine polyphosphate, aluminum oxide, aluminum hydroxide, zinc borate, and zinc stannate.
[15] The polyamide composition according to any one of [1] to
[14] , wherein the exothermic peak width during cooling in differential scanning calorimetry (DSC) is 1 to 20°C.
[16] The crystallization rate calculated from the following formula (1) is 0.044°C. -1 The polyamide composition described in any of [1] to
[15] above. Crystallization rate (°C) -1 ) = 1 / (Melting point (°C) - Crystallization temperature (°C)) (1) However, in the above formula (1), "melting point" and "crystallization temperature" both refer to the melting point and crystallization temperature of the polyamide composition.
[17] The crystallization rate calculated from the following formula (1) is 0.030 to 0.038°C -1 The polyamide composition according to any one of [1] to
[15] . Crystallization rate (°C) -1 ) = 1 / (melting point (°C) - crystallization temperature (°C)) (1) However, in formula (1) above, "melting point" and "crystallization temperature" both refer to the melting point and crystallization temperature of the polyamide composition.
[18] A molded article made of the polyamide composition described in any of [1] to
[17] .
[19] A molded article described in
[18] which is an electrical component or an electronic component.
[20] A molded article described in
[18] or
[19] which is a surface mount component.
[0008] According to the present invention, it is possible to provide a polyamide composition that has excellent flame retardancy and can suppress deformation during the reflow process, as well as a molded article made from the polyamide composition.
[0009] Figure 1 schematically shows examples of cross-sections of typical glass fibers. Figure 1(a) shows an example where the outer shape of the cross-section is cocoon-shaped, Figure 1(b) shows an example where the outer shape of the cross-section is elliptical, and Figure 1(c) shows an example where the outer shape of the cross-section is rectangular.
[0010] The following description is based on an example of an embodiment of the present invention (hereinafter sometimes referred to as "this embodiment"). However, the embodiments shown below are illustrative examples for realizing the technical concept of the present invention, and the present invention is not limited to the following description. In this specification, preferred forms of embodiments are shown, but combinations of two or more individual preferred forms are also preferred forms. When there are several numerical ranges for matters indicated by numerical ranges, a preferred form can be obtained by selectively combining their lower and upper limits. In this specification, when a numerical range is described as "XX to YY", it means "XX or more and YY or less". In this specification, "~ unit" (where "~" indicates a monomer) means "a constituent unit derived from ~", for example, "dicarboxylic acid unit" means "a constituent unit derived from dicarboxylic acid", and "diamine unit" means "a constituent unit derived from diamine".
[0011] <Polyamide Composition> The polyamide composition of this embodiment is a polyamide composition containing a polyamide (A), a halogenated flame retardant (B), and a filler (C), wherein the polyamide (A) is a semi-aromatic polyamide, and the semi-aromatic polyamide contains constituent units derived from a dicarboxylic acid and constituent units derived from a diamine, wherein more than 50 mol% of the constituent units derived from the dicarboxylic acid are constituent units derived from an aromatic dicarboxylic acid, and more than 50 mol% of the constituent units derived from the diamine are constituent units derived from an aliphatic diamine having 7 to 18 carbon atoms, and the composition contains 1 to 100 parts by weight of the halogenated flame retardant (B) and 150 to 350 parts by weight of the filler (C) per 100 parts by weight of the polyamide (A). Details will be described below.
[0012] [Polyamide (A)] The polyamide (A) of this embodiment is a semi-aromatic polyamide, wherein the semi-aromatic polyamide includes constituent units derived from a dicarboxylic acid and constituent units derived from a diamine. In the semi-aromatic polyamide, more than 50 mol% of the constituent units derived from the dicarboxylic acid are constituent units derived from an aromatic dicarboxylic acid, and more than 50 mol% of the constituent units derived from the diamine are constituent units derived from an aliphatic diamine having 7 to 18 carbon atoms.
[0013] As the dicarboxylic acid, at least one selected from the group consisting of aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and alicyclic dicarboxylic acids can be used.
[0014] Aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,4-phenylenedioxydiacetic acid, 1,3-phenylenedioxydiacetic acid, diphenic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, and 4,4'-biphenyldicarboxylic acid. Aliphatic dicarboxylic acids include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanediic acid, dodecanediic acid, dimethylmalonic acid, 2,2-diethylsuccinic acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid. Examples of alicyclic dicarboxylic acids include 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, cycloheptanedicarboxylic acid, cyclooctanedicarboxylic acid, and cyclodecanedicarboxylic acid. These dicarboxylic acids can be used individually or in combination of two or more. Polyamide (A) may further contain constituent units derived from trivalent or higher polycarboxylic acids such as trimellitic acid, trimesic acid, and pyromellitic acid, to the extent that melt molding is possible, as long as it does not impair the effects of the present invention.
[0015] As the diamine, at least one selected from the group consisting of aliphatic diamines, alicyclic diamines, and aromatic diamines can be used.
[0016] Examples of aliphatic diamines include linear aliphatic diamines such as ethylenediamine, 1,2-propanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, and 1,12-dodecanediamine; 1-butyl-1,2-ethanediamine, 1,1-dimethyl-1,4-butanediamine, and 1-ethyl-1,2-ethanediamine. Tyl-1,4-butanediamine, 1,2-dimethyl-1,4-butanediamine, 1,3-dimethyl-1,4-butanediamine, 1,4-dimethyl-1,4-butanediamine, 2,3-dimethyl-1,4-butanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2,5-dimethyl-1,6-hexanediamine, 2,4-dimethyl-1,6-hexanediamine, 3,3-dimethyl-1,6-hexanediamine, 2,2-dimethyl-1,6-hexa Diamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2,4-diethyl-1,6-hexanediamine, 2,2-dimethyl-1,7-heptanediamine, 2,3-dimethyl-1,7-heptanediamine, 2,4-dimethyl-1,7-heptanediamine, 2,5-dimethyl-1,7-heptanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine, 4-methyl-1,8-octanediamine Examples include amines, branched-chain aliphatic diamines such as 1,3-dimethyl-1,8-octanediamine, 1,4-dimethyl-1,8-octanediamine, 2,4-dimethyl-1,8-octanediamine, 3,4-dimethyl-1,8-octanediamine, 4,5-dimethyl-1,8-octanediamine, 2,2-dimethyl-1,8-octanediamine, 3,3-dimethyl-1,8-octanediamine, 4,4-dimethyl-1,8-octanediamine, and 5-methyl-1,9-nonanediamine.
[0017] Examples of alicyclic diamines include cyclohexanediamine, methylcyclohexanediamine, isophoronediamine, norbornanedimethylamine, and tricyclodecanedimethylamine.
[0018] Examples of aromatic diamines include p-phenylenediamine, m-phenylenediamine, p-xylylenediamine, m-xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, and 4,4'-diaminodiphenyl ether.
[0019] These diamines can be used individually or in combination of two or more.
[0020] Polyamide (A) may further contain trivalent or higher polyvalent amine-derived constituent units, such as bis(hexamethylene)triamine, to the extent that melt molding is possible, as long as it does not impair the effects of the present invention.
[0021] The semi-aromatic polyamide of this embodiment is a semi-aromatic polyamide in which more than 50 mol% of the dicarboxylic acid units are aromatic dicarboxylic acid units and more than 50 mol% of the diamine units are aliphatic diamine units. Because polyamide (A) is a semi-aromatic polyamide, it has excellent low water absorption, excellent heat resistance, and excellent reflow properties.
[0022] The aromatic dicarboxylic acid is preferably at least one selected from the group consisting of phthalic acid, isophthalic acid, and terephthalic acid, more preferably isophthalic acid or terephthalic acid, and even more preferably terephthalic acid. The content of aromatic dicarboxylic acid units in the dicarboxylic acid units constituting the semi-aromatic polyamide is, from the viewpoint of heat resistance, more than 50 mol%, preferably more than 50 mol% and 100 mol%, more preferably 60 to 100 mol%, even more preferably 70 to 100 mol%, even more preferably 80 to 100 mol%, even more preferably 90 to 100 mol%, and may also be 100 mol%.
[0023] The semi-aromatic polyamide may contain other dicarboxylic acid units besides aromatic dicarboxylic acid units. Examples of such other dicarboxylic acids include the aliphatic dicarboxylic acids and alicyclic dicarboxylic acids mentioned above. The content of other dicarboxylic acid units in the dicarboxylic acid units constituting the semi-aromatic polyamide is 0 mol% or more and less than 50 mol%, preferably 0 to 40 mol%, more preferably 0 to 30 mol%, even more preferably 0 to 20 mol%, and even more preferably 0 to 10 mol%.
[0024] Examples of aliphatic diamines constituting the semi-aromatic polyamide include the aliphatic diamines mentioned above. From the viewpoint of low water absorption and excellent reflow properties, the number of carbon atoms in the aliphatic diamine is preferably 7 to 18, more preferably 8 to 12, even more preferably 9 to 12, and even more preferably 9 to 10.
[0025] As the aliphatic diamine, from the viewpoint of low water absorption and excellent reflow properties, at least one selected from the group consisting of 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine is preferred, 1,9-nonanediamine or 2-methyl-1,8-octanediamine is more preferred, and a combination of 1,9-nonanediamine and 2-methyl-1,8-octanediamine is even more preferred.
[0026] The content of aliphatic diamine units in the diamine units constituting the semi-aromatic polyamide is greater than 50 mol%, preferably greater than 50 mol% and 100 mol%, more preferably 60 to 100 mol%, even more preferably 70 to 100 mol%, even more preferably 80 to 100 mol%, even more preferably 90 to 100 mol%, and may also be 100 mol%.
[0027] The semi-aromatic polyamide may contain other diamine units besides aliphatic diamine units. Examples of such other diamines include the aromatic diamines and alicyclic diamines mentioned above. The content of other diamine units in the diamine units constituting the semi-aromatic polyamide is 0 mol% or more and less than 50 mol%, preferably 0 to 40 mol%, more preferably 0 to 30 mol%, even more preferably 0 to 20 mol%, and even more preferably 0 to 10 mol%.
[0028] When 1,9-nonanediamine and 2-methyl-1,8-octanediamine are used in combination as the aliphatic diamine, from the viewpoint of heat resistance, the molar ratio of 1,9-nonanediamine to 2-methyl-1,8-octanediamine (1,9-nonanediamine / 2-methyl-1,8-octanediamine) is preferably in the range of 95 / 5 to 40 / 60, more preferably in the range of 90 / 10 to 50 / 50, and even more preferably in the range of 90 / 10 to 60 / 40 from the viewpoint of improving the bending strength of the molded product. On the other hand, from the viewpoint of setting the crystallization rate of the polyamide composition described later to an appropriate range, and as a result improving the surface quality of the molded product, the molar ratio (1,9-nonanediamine / 2-methyl-1,8-octanediamine) is preferably 60 / 40 to 10 / 90, more preferably 55 / 45 to 20 / 80, even more preferably 52 / 48 to 30 / 70, and even more preferably 50 / 50 to 40 / 60. In the molar ratio of 60 / 40 to 10 / 90, the upper limit of "60 / 40 or less" is preferably "less than 60 / 40," that is, it is preferable to be in a range that does not include 60 / 40, which is "less than 60 / 40 and 10 / 90 or more."
[0029] Furthermore, the semi-aromatic polyamide may also contain constituent units derived from cyclic lactams and / or aminocarboxylic acids. Examples of these constituent units include cyclic lactams such as caprolactam and laurolactam; and constituent units derived from aminocarboxylic acids such as 11-aminoundecanoic acid and 12-aminododecanoic acid. The total content of cyclic lactam units and aminocarboxylic acid units in the semi-aromatic polyamide is preferably 0 mol% or more and less than 50 mol%, more preferably 0 to 40 mol%, and even more preferably 0 to 20 mol%, based on 100 mol% of the total dicarboxylic acid units and diamine units constituting the semi-aromatic polyamide.
[0030] Examples of the aforementioned semi-aromatic polyamides include polynonameethylene terephthalamide (polyamide 9T), polydecamethylene terephthalamide (polyamide 10T), and copolymers of polyamide 6T and polyundecaneamide (polyamide 11) (polyamide 6T / 11). Among these, at least one selected from the group consisting of polyamide 9T and polyamide 10T is preferred, and polyamide 9T is more preferred.
[0031] In this embodiment, it is preferable that 10% or more of the end groups of the molecular chain of the polyamide (A) are encapsulated with an end encapsulant. More preferably, the percentage of end groups of the molecular chain encapsulated with an end encapsulant (end encapsulation rate) is 20% or more.
[0032] As end-captives, monofunctional compounds that react with the amino or carboxyl groups at the polyamide termini can be used. From the viewpoint of reactivity and stability of the encapsulated end, monocarboxylic acids or monoamines are preferred, and from the viewpoint of ease of handling, monocarboxylic acids are more preferred. Other substances such as monoisocyanates, monoacid halides, monoesters, and monoalcohols can also be used as end-captives.
[0033] As the monocarboxylic acid used as the terminal blocking agent, those having reactivity with amino groups can be used, and examples thereof include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalenecarboxylic acid, β-naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid and phenylacetic acid; and any mixtures thereof. Among these, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid and benzoic acid are preferred from the viewpoints of reactivity, stability of the blocked terminals, cost and the like.
[0034] As the monoamine used as the terminal blocking agent, those having reactivity with carboxyl groups can be used, and examples thereof include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine and naphthylamine; and any mixtures thereof. Among these, butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine and aniline are preferred from the viewpoints of reactivity, boiling point, stability of the blocked terminals, cost and the like.
[0035] The terminal blocking rate of the polyamide (A) is determined by measuring the number of carboxyl group terminals, amino group terminals and terminal groups blocked by the terminal blocking agent present in the polyamide (A) respectively, and calculating according to the following formula (2). From the viewpoints of accuracy and convenience, the number of each terminal group is 1It is preferable to determine the value from the integral value of the characteristic signal corresponding to each terminal group by 1H-NMR. Terminal end-capping ratio (%) = [(T−S) / T] × 100 (2) In the formula, T represents the total number of terminal groups in the molecular chain of the polyamide (A), which is usually equal to twice the number of polyamide molecules, and S represents the total number of carboxyl group terminals and amino group terminals remaining uncapped.
[0036] The polyamide (A) used in the present invention can be produced by any known method for producing crystalline polyamides. For example, it can be produced by methods such as a solution polymerization method or interfacial polymerization method using a dicarboxylic acid in the form of acid chloride and a diamine as raw materials, a melt polymerization method, solid phase polymerization method, or melt extrusion polymerization method using a dicarboxylic acid and a diamine as raw materials.
[0037] For the polyamide (A), for example, first, diamine, dicarboxylic acid, and optionally a catalyst and an end-capping agent are added all at once to produce a nylon salt, which is then heated and polymerized at a temperature of 200 to 250°C to form a prepolymer, followed by further solid phase polymerization, or polymerization using a melt extruder. When the final stage of polymerization is carried out by solid phase polymerization, it is preferably performed under reduced pressure or under a flow of inert gas. When the polymerization temperature is in the range of 200 to 280°C, the polymerization rate is high, the productivity is excellent, and coloring and gelation can be effectively suppressed. When the final stage of polymerization is carried out using a melt extruder, the polymerization temperature is preferably 370°C or lower. Polymerization under such conditions yields the polyamide (A) with almost no decomposition and little degradation.
[0038] Examples of catalysts that can be used in the production of polyamide (A) include phosphoric acid, phosphorous acid, hypophosphorous acid, and their salts or esters. Examples of the salts or esters include salts of phosphoric acid, phosphorous acid, or hypophosphorous acid with metals such as potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium, and antimony; ammonium salts of phosphoric acid, phosphorous acid, or hypophosphorous acid; ethyl esters, isopropyl esters, butyl esters, hexyl esters, isodecyl esters, octadecyl esters, decyl esters, stearyl esters, and phenyl esters of phosphoric acid, phosphorous acid, or hypophosphorous acid. Among these, sodium hypophosphorous acid monohydrate or phosphorous acid is preferred.
[0039] The polyamide (A) has an intrinsic viscosity [η] of 0.60 to 1.2 dl / g, more preferably 0.65 to 1.1 dl / g, measured at 30°C using concentrated sulfuric acid as a solvent. Using polyamide (A) with an intrinsic viscosity [η] of 0.60 dl / g or higher results in good mechanical properties of the resulting molded article. Using polyamide (A) with an intrinsic viscosity [η] of 1.2 dl / g or lower further improves moldability.
[0040] The melting point of polyamide (A) is preferably 260 to 350°C, more preferably 265 to 340°C, and even more preferably 265 to 330°C. A melting point of 260°C or higher enhances the effects of the present invention, in addition to improving heat resistance. A melting point of 350°C or lower suppresses thermal decomposition of the polyamide during melt molding.
[0041] The glass transition temperature of polyamide (A) is preferably 110°C or higher, and more preferably 120°C or higher. Having the glass transition temperature within this range allows for a polyamide with excellent heat resistance. There is no particular upper limit to the glass transition temperature of polyamide (A), but from the viewpoint of handling and other factors, it is preferably 180°C or lower, more preferably 160°C or lower, and may also be 150°C or lower. That is, the glass transition temperature of polyamide (A) is preferably 110 to 180°C, more preferably 120 to 160°C, and may also be 120 to 150°C. The glass transition temperature of polyamide (A) can be determined using a differential scanning calorimetry (DSC) apparatus as the temperature of the inflection point that appears when the temperature is increased at a rate of 20°C / min.
[0042] The weight-average molecular weight (Mw) of polyamide (A) is preferably 10,000 to 40,000 g / mol, more preferably 13,000 to 30,000 g / mol, even more preferably 15,000 to 28,000 g / mol, even more preferably 17,000 to 27,000 g / mol, and even more preferably 17,000 to 26,000 g / mol, and even more preferably 17,000 to 25,000 g / mol, from the viewpoint of suppressing deformation during the reflow process and improving the bending strength of the molded product. By having the weight-average molecular weight (Mw) within the above range, a polyamide composition with an excellent balance between the bending strength and moldability of the molded product can be obtained. The weight-average molecular weight (Mw) is measured by the method described in the examples below.
[0043] The amount of terminal amino groups in the molecular chain of polyamide (A) ([NH 2The amount of terminal amino groups is preferably 5 to 160 μmol / g, more preferably 10 to 100 μmol / g, and even more preferably 10 to 80 μmol / g. If the amount of terminal amino groups is 5 μmol / g or more, an even better crystallization rate can be achieved and good hydrolysis resistance can be obtained. Furthermore, if the polyamide composition of this embodiment contains a fibrous filler (C1) described later as a filler (C), adhesion with the fibrous filler (C1) will be good, and mechanical properties can be improved. If the amount of terminal amino groups is 160 μmol / g or less, an even better heat resistance will be achieved and the melt viscosity of the polyamide composition during processing will be good. The amount of terminal amino groups refers to the amount of terminal amino groups (unit: μmol) contained in 1 g of polyamide, and can be determined by titrating a phenol solution in which polyamide (A) is dissolved with an aqueous hydrochloric acid solution.
[0044] The amount of terminal carboxyl groups ([COOH]) in the molecular chain of polyamide (A) is preferably 2 to 100 μmol / g, more preferably 5 to 80 μmol / g, and even more preferably 10 to 80 μmol / g. If the amount of terminal carboxyl groups is 2 μmol / g or more, an even better crystallization rate is exhibited, and excellent heat resistance is more likely to be exhibited. Furthermore, if the polyamide composition of this embodiment contains a fibrous filler (C1) as a filler (C), good adhesion with the fibrous filler (C1) is achieved, and mechanical properties can be improved. If the amount of terminal carboxyl groups is 100 μmol / g or less, good hydrolysis resistance can be exhibited. Furthermore, hydrolysis in acidic environments is suppressed, and chemical resistance is improved. The amount of terminal carboxyl groups refers to the amount of terminal carboxyl groups (unit: μmol) contained in 1 g of polyamide, and can be determined by titrating a cresol solution in which polyamide (A) is dissolved with a potassium hydroxide solution.
[0045] The amount of terminal amino groups in the molecular chain of polyamide (A) ([NH 2 ]) and the ratio of terminal carboxyl group amount ([COOH]) ([NH 2 / [COOH]) is preferably from 0.1 to 50, more preferably from 0.3 to 10, and even more preferably from 0.3 to 6. The ratio ([NH 2 / [COOH]) of 0.1 or higher allows an even more excellent crystallization rate to be exhibited, and can provide good hydrolysis resistance. The ratio ([NH 2 / [COOH]) of 50 or lower allows even more excellent heat resistance to be exhibited.
[0046] The content of the polyamide (A) contained in the total amount of the polyamide composition of the present embodiment is preferably from 10 to 40% by weight, more preferably from 15 to 35% by weight, and even more preferably from 20 to 33% by weight, from the viewpoint of facilitating securing good moldability, heat resistance, mechanical properties, and chemical resistance.
[0047] The polyamide composition of the present invention may contain other polyamides besides the aforementioned polyamide (A) within a range that does not impair the effects of the present invention. Examples of the aforementioned other polyamides include semi-aromatic polyamides of the type in which more than 50 mol% of the structural units derived from the dicarboxylic acid constituting the polyamide are structural units derived from an aromatic dicarboxylic acid, and more than 50 mol% of the structural units derived from the diamine constituting the polyamide are structural units derived from an aliphatic diamine having 6 or less carbon atoms; semi-aromatic polyamides of the type in which more than 50 mol% of the dicarboxylic acid units constituting the polyamide are aliphatic dicarboxylic acid units, and more than 50 mol% of the diamine units constituting the polyamide are aromatic diamine units; fully aromatic polyamides in which more than 50 mol% of the dicarboxylic acid units constituting the polyamide are aromatic dicarboxylic acid units, and more than 50 mol% of the diamine units constituting the polyamide are aromatic diamine units; and aliphatic polyamides such as ring-opening polymers of the aforementioned cyclic lactams, condensation polymers of the aforementioned aminocarboxylic acids, or condensation polymers of the aforementioned aliphatic dicarboxylic acids and the aforementioned aliphatic diamines. When the aforementioned other polyamides are contained, the mass ratio of the polyamide (A) and the aforementioned other polyamides is preferably from 50 / 50 to 99 / 1, more preferably from 60 / 40 to 90 / 10, and even more preferably from 70 / 30 to 80 / 20.
[0048] [Halogenated Flame Retardant (B)] The polyamide composition of this embodiment contains a halogenated flame retardant (B). The inclusion of the halogenated flame retardant (B) results in a polyamide composition with improved flame retardancy. There are no particular restrictions on the halogenated flame retardant (B) included in the polyamide composition of this embodiment; compounds known as flame retardants containing halogen elements can be used. Examples of halogenated flame retardants (B) include brominated flame retardants (B1) and chlorinated flame retardants (B2), and it is preferable to include a brominated flame retardant (B1). These may be used individually or in combination of two or more.
[0049] (Bromine-based flame retardants (B1)) Examples of bromine-based flame retardants (B1) include hexabromocyclododecane, decabromodiphenyl oxide, octabromodiphenyl oxide, tetrabromobisphenol A, bis(tribromophenoxy)ethane, bis(pentabromophenoxy)ethane, tetrabromobisphenol A epoxy resin, tetrabromobisphenol A carbonate, ethylene (bistetrabromophthal)imide, ethylenebispentabromodiphenyl, tris(tribromophenoxy)triazine, bis(dibromopropyl)tetrabromobisphenol A, bis(dibromopropyl)tetrabromobisphenol Examples include Nol S, brominated polyphenylene ethers (including poly(di)bromophenylene ethers, etc.), brominated polystyrene (including polydibromostyrene, polytribromostyrene, crosslinked brominated polystyrene, etc.; it may also be modified brominated polystyrene to which epoxy acrylate etc. has been added), brominated crosslinked aromatic polymers, brominated epoxy resins, brominated phenoxy resins, brominated styrene-maleic anhydride polymers, tetrabromobisphenol S, tris(tribromoneopentyl) phosphate, polybromotrimethylphenylindan, tris(dibromopropyl)-isocyanurate, and the like.
[0050] The brominated flame retardant (B1) preferably contains brominated polyphenylene ether or brominated polystyrene, and more preferably contains brominated polystyrene, from the viewpoint of reducing the amount of corrosive gas generated during melting processes such as extrusion and molding, and improving the flame retardancy and mechanical properties of electrical or electronic components.
[0051] Brominated polystyrene can be produced, for example, by polymerizing styrene monomers to produce polystyrene and then brominating the benzene ring of the polystyrene, or by polymerizing brominated styrene monomers (such as bromostyrene, dibromostyrene, and tribromostyrene).
[0052] The bromine content in brominated polystyrene is preferably 55 to 75% by weight, and more preferably 55 to 70% by weight. By setting the bromine content to 55% by weight or more, the amount of bromine required for flame retardancy can be satisfied with a small amount of brominated polystyrene, and the deterioration of the mechanical properties of polyamide (A) is suppressed, resulting in a polyamide composition with excellent mechanical properties and heat resistance. Furthermore, by setting the bromine content to 75% by weight or less, thermal decomposition is less likely to occur during melt processing such as extrusion and molding, gas generation can be suppressed, and a polyamide composition with excellent heat discoloration resistance can be obtained. The bromine content in the brominated polystyrene can be determined by fluorescence X-ray analysis. Specifically, it can be determined by measuring a sample of polyamide composition pellets packed in an aluminum cup using a scanning X-ray analyzer "ZSX Primusμ" (manufactured by Rigaku Corporation).
[0053] (Chlorine-based flame retardants (B2)) Examples of chlorine-based flame retardants (B2) include chlorinated paraffin, chlorinated polyethylene, dodecachloropentacyclooctadeca-7,15-diene (Dechloran Plus 25 manufactured by Occidental Chemical Co., Ltd.), and hetic anhydride.
[0054] The polyamide composition of this embodiment contains 1 to 100 parts by weight of halogenated flame retardant (B) per 100 parts by weight of polyamide (A), preferably 5 to 100 parts by weight, more preferably 10 to 75 parts by weight, even more preferably 30 to 70 parts by weight, and still more preferably 30 to 60 parts by weight. Furthermore, from the viewpoint of improving the flame retardancy and flexural strength of the molded product, the polyamide composition of this embodiment more preferably contains 30 to 45 parts by weight of the halogenated flame retardant (B) per 100 parts by weight of polyamide (A). By setting the content of halogenated flame retardant (B) to 1 part by weight or more, a polyamide composition with excellent flame retardancy can be obtained. Furthermore, by setting the content of halogenated flame retardant (B) to 100 parts by weight or less, the generation of decomposition gases during melt kneading, the decrease in fluidity (especially thin-wall fluidity) during molding, and the adhesion of contaminants to the molding die can be suppressed, as can the deterioration of mechanical properties and the appearance of the molded product. When using multiple types of halogen-based flame retardants (B), their total amount must fall within the above range.
[0055] [Filler (C)] The polyamide composition of this embodiment contains filler (C). By including filler (C), a polyamide composition with excellent heat resistance, moldability, and mechanical properties in thin-walled structures can be obtained.
[0056] As the filler (C), various forms such as fibrous, plate-like, needle-like, powder-like, and cloth-like can be used. Specifically, inorganic or organic fibrous fillers (C1) such as glass fibers, carbon fibers, fully aromatic polyamide fibers (aramid fibers), liquid crystal polymer (LCP) fibers, gypsum fibers, brass fibers, ceramic fibers, and boron whisker fibers; plate-like fillers such as glass flakes and mica; needle-like fillers (C2) such as potassium titanate whiskers, aluminum borate whiskers, calcium carbonate whiskers, magnesium sulfate whiskers, wollastonite, sepiolite, xonotlite, and zinc oxide whiskers; and aluminum nitride, boron nitride, potassium titanate, and aluminum silicate (calcium carbonate). Powdered fillers such as orine, clay, pyrophyllite, bentonite, calcium silicate, magnesium silicate (atapulgite), aluminum borate, calcium sulfate, barium sulfate, magnesium sulfate, asbestos, glass beads, carbon black, graphene, graphite, carbon nanotubes, silicon carbide, sericite, hydrotalcite, montmorillonite, molybdenum disulfide, ultra-high molecular weight polyethylene particles, phenolic resin particles, crosslinked styrene resin particles, crosslinked acrylic resin particles, etc.; cloth-type fillers such as glass cloth, etc. These may be used individually or in combination of two or more types.
[0057] The surface of the filler (C) may be surface-treated with a polymer compound such as a silane coupling agent, a titanium coupling agent, an acrylic resin, a urethane resin, an epoxy resin, or other low-molecular-weight compound, in order to improve its dispersibility and adhesion to the polyamide (A).
[0058] The filler (C) is preferably at least one selected from the group consisting of fibrous fillers (C1) and needle-shaped fillers (C2) because it is low-cost and yields molded articles with excellent mechanical properties, and it is preferable to include fibrous filler (C1) from the viewpoint of high strength and low cost. It is preferable to include needle-shaped filler (C2) from the viewpoint of obtaining molded articles with high surface smoothness. The fibrous filler (C1) and needle-shaped filler (C2) are preferably at least one selected from the group consisting of carbon fiber, glass fiber, aramid fiber, wollastonite, potassium titanate whisker, calcium carbonate whisker, and aluminum borate whisker, more preferably at least one selected from the group consisting of carbon fiber, glass fiber, aramid fiber, and wollastonite, even more preferably at least one selected from the group consisting of carbon fiber, glass fiber, and aramid fiber, and even more preferably glass fiber.
[0059] The average fiber length of the fibrous filler (C1) is preferably 1 to 10 mm, more preferably 1 to 7 mm, and even more preferably 2 to 4 mm. Furthermore, the average fiber diameter of the fibrous filler (C1) is preferably 6 to 20 μm, more preferably 6 to 15 μm, from the viewpoint of obtaining excellent mechanical properties. The average fiber length and average fiber diameter of the fibrous filler (C1) can be determined by measuring the fiber length and fiber diameter of 400 randomly selected fibrous fillers (C1) using image analysis with an electron microscope, and calculating the average values. In addition, the average fiber length and average fiber diameter of the fibrous filler (C1) in a polyamide composition or in a molded article formed from the polyamide composition can be determined, for example, by dissolving the polyamide composition or molded article in an organic solvent, extracting the fibrous filler (C1), and then determining the values by image analysis using an electron microscope in the same manner as described above.
[0060] Examples of cross-sectional shapes for the fibrous filler (C1) and needle-shaped filler (C2) include rectangles, oblong shapes close to rectangles, circles, ellipses, cocoon shapes, and cocoon shapes with a constriction in the longitudinal center. Among these, it is preferable that the cross-sectional shape of the fibrous filler (C1) and needle-shaped filler (C2) be at least one selected from the group consisting of rectangles, oblong shapes close to rectangles, ellipses, circles, and cocoon shapes, and more preferably at least one selected from the group consisting of circles, oblong shapes, and cocoon shapes, with oblong shapes being even more preferable from the viewpoint of improving the flame retardancy of the molded product.
[0061] The following details describe the case where the fibrous filler (C1) is glass fiber.
[0062] Specific glass fiber compositions include E-glass composition, C-glass composition, S-glass composition, and alkali-resistant glass composition. The tensile strength of the glass fiber is arbitrary, but typically 290 kg / mm². 2 That concludes the explanation. Among these, E-glass is preferred from the viewpoint of its easy availability. These glass fibers are preferably surface-treated with a silane coupling agent such as γ-methacrylateoxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, or γ-aminopropyltriethoxysilane, and the amount of the coupling agent attached is usually 0.01% by weight or more of the weight of the glass fibers (total amount of glass fibers and surface treatment agent).
[0063] The average fiber diameter of glass fibers is determined by observing the glass fibers with an electron microscope, obtaining cross-sectional images, and analyzing these images. In the obtained images, the major axis of each of the 400 glass fibers is measured, and this major axis is considered as the individual fiber diameter. Note that the major axis referred to here is the same major axis used in the calculation of the shape ratio described later. The average value of the fiber diameters of the 400 fibers is taken as the average fiber diameter of the glass fibers. The average fiber diameter of glass fibers in a polyamide composition can be determined, for example, by dissolving the polyamide composition in an organic solvent, extracting the glass fibers, and using the same method as described above.
[0064] Figure 1 schematically shows examples of typical cross-sections of glass fibers. Figure 1(a) shows an example where the cross-section is cocoon-shaped, Figure 1(b) shows an example where the cross-section is elliptical, and Figure 1(c) shows an example where the cross-section is rectangular. The shape ratio of the cross-section of a glass fiber is expressed as the ratio of the major axis to the minor axis (i.e., D1 / D2), where D1 is the major axis and D2 is the minor axis of the cross-section. However, the major and minor axes are assumed to be orthogonal to each other. When the cross-section of a glass fiber is irregular in shape, for example, in the case of a non-circular cross-section such as cocoon-shaped (see Figure 1(a)), elliptical (see Figure 1(b)), semicircular, rectangular (see Figure 1(c)), polygonal, or star-shaped, it is possible to specify the minor axis D2 and major axis D1 as shown in Figure 1. The lower limit of the shape ratio is 1.0 (major axis D1 = minor axis D2). Typically, the shape ratio is expressed as the average of the shape ratios of a large number of glass fibers.
[0065] The average deformation ratio (ratio of major axis to minor axis) in the cross-section of the glass fiber is preferably 1 or more, more preferably 2 or more, and even more preferably 4 or more, from the viewpoint of obtaining a polyamide molded product that is less prone to deformation during reflow.
[0066] The deformation ratio of glass fibers is determined by observing the glass fibers with an electron microscope, obtaining cross-sectional images, and analyzing these images. In the obtained images, the major and minor axes are identified for 400 glass fibers as shown in Figure 1. The deformation ratio is determined by calculating the ratio (major axis / minor axis) from the identified major and minor axes. The average deformation ratio of the 400 fibers is taken as the average deformation ratio of the glass fibers. In the case of polyamide compositions, the average deformation ratio of the glass fibers can be measured in the same manner as above by dissolving the polyamide composition in an organic solvent and extracting the glass fibers.
[0067] The polyamide composition of this embodiment contains 150 to 350 parts by weight of filler (C) per 100 parts by weight of polyamide (A), preferably 160 to 340 parts by weight, more preferably 160 to 330 parts by weight, even more preferably 160 to 320 parts by weight, even more preferably 160 to 315 parts by weight, and even more preferably 165 to 250 parts by weight. By setting the filler (C) content to 150 parts by weight or more per 100 parts by weight of polyamide (A), the mechanical properties of the polyamide composition of this embodiment are improved and deformation during the reflow process can be suppressed. Furthermore, by setting the filler (C) content to 350 parts by weight or less, a polyamide composition with excellent moldability can be obtained.
[0068] [Flame retardant additive (D)] The polyamide composition of this embodiment may further contain a flame retardant additive (D). By using the flame retardant additive (D) in combination with a halogenated flame retardant (B), the polyamide composition of this embodiment and the molded articles made therefrom can exhibit even better flame retardancy.
[0069] Examples of flame retardant additives (D) include antimony compounds such as antimony oxides like diantimony trioxide, diantimony tetroxide, and diantimony pentoxide, and antimonate salts such as sodium antimonate; melamine compounds such as melamine orthophosphate, melamine pyrophosphate, melamine borate, and melamine polyphosphate; tin oxides such as tin monoxide and tin dioxide; iron oxides such as ferric oxide and γ-iron oxide; aluminum oxide, silicon dioxide (silica), titanium dioxide, zirconium oxide, manganese oxide, and molybdenum oxide. Examples include metal oxides such as cobalt oxide, bismuth oxide, chromium oxide, tin oxide, nickel oxide, copper oxide, and tungsten oxide; metal hydroxides such as aluminum hydroxide; metal powders such as aluminum, iron, titanium, manganese, zinc, molybdenum, cobalt, bismuth, chromium, tin, antimony, nickel, copper, and tungsten; metal carbonates such as zinc carbonate, magnesium carbonate, and barium carbonate; metal borates such as zinc borate and calcium borate; zinc stannates such as zinc trioxide; and silicones. However, those that fall under filler (C) are excluded. These may be used individually or in combination of two or more types.
[0070] Among the above, at least one selected from the group consisting of antimony compounds, melamine compounds, metal oxides, metal hydroxides, metal borates, and zinc stannate is preferred; at least one selected from the group consisting of antimony trioxide, antimony tetroxide, antimony pentoxide, sodium antimonate, melamine orthophosphate, melamine pyrophosphate, melamine borate, melamine polyphosphate, aluminum oxide, aluminum hydroxide, zinc borate, and zinc stannate is more preferred; and at least one selected from the group consisting of antimony trioxide, antimony tetroxide, antimony pentoxide, sodium antimonate, melamine orthophosphate, melamine pyrophosphate, melamine borate, melamine polyphosphate, aluminum oxide, aluminum hydroxide, zinc borate, and zinc stan trioxide is even more preferred.
[0071] If the polyamide composition of this embodiment contains a flame retardant additive (D), the amount is preferably 1 to 30 parts by weight, more preferably 1 to 25 parts by weight, even more preferably 3 to 20 parts by weight, and still more preferably 3 to 15 parts by weight, per 100 parts by weight of polyamide (A). Furthermore, from the viewpoint of improving the flame retardancy and flexural strength of the molded article, the polyamide composition of this embodiment is more preferably to contain 3 to 6 parts by weight of the flame retardant additive (D) per 100 parts by weight of polyamide (A).
[0072] [Other Additives] The polyamide composition of this embodiment may contain other additives in addition to the polyamide (A), halogenated flame retardant (B), filler (C), and flame retardant aid (D) used as needed.
[0073] Other additives include, for example, stabilizers such as copper compounds; antioxidants such as hindered phenol-based antioxidants, hindered amine-based antioxidants, phosphorus-based antioxidants, and thio-based antioxidants; colorants; ultraviolet absorbers; light stabilizers; antistatic agents; mold release agents; heat stabilizers; crystal nucleating agents; plasticizers; lubricants; dispersants; oxygen absorbers; hydrogen sulfide adsorbents; crystallization retarders; impact modifiers for α-olefin copolymers, rubber, etc.; and drip inhibitors for fluororesins, etc.
[0074] The polyamide composition of this embodiment preferably contains nigrosine as a crystallization retarder from the viewpoint of improving the surface properties of the molded article.
[0075] The content of the above-mentioned other additives is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 0.02 to 200 parts by weight, more preferably 0.03 to 100 parts by weight, even more preferably 0.05 to 50 parts by weight, even more preferably 0.1 to 20 parts by weight, and even more preferably 0.1 to 10 parts by weight per 100 parts by weight of polyamide (A). Furthermore, when a crystallization retarder is used, the content of the crystallization retarder is preferably 0.16 to 1.60 parts by weight, and more preferably 0.30 to 0.98 parts by weight per 100 parts by weight of polyamide (A), from the viewpoint of improving the surface properties of the molded product.
[0076] In this embodiment, the total content of polyamide (A) and halogenated flame retardant (B) in the total polyamide composition is preferably 20 to 90% by weight, more preferably 25 to 80% by weight, even more preferably 25 to 70% by weight, even more preferably 25 to 60% by weight, even more preferably 30 to 60% by weight, and even more preferably 30 to 50% by weight. Furthermore, the total content of polyamide (A), halogenated flame retardant (B), and filler (C) is preferably 85 to 100% by weight, more preferably 90 to 99% by weight, and even more preferably 95 to 99% by weight.
[0077] The polyamide composition of this embodiment contains the above-mentioned polyamide (A) and halogenated flame retardant (B), thereby maintaining the excellent physical properties of the polyamide (A) while possessing excellent flame retardancy, moldability, and hydrolysis resistance.
[0078] In the polyamide composition of this embodiment, the exothermic peak width during cooling in differential scanning calorimetry (DSC) is preferably 1 to 20°C, more preferably 2 to 18°C, even more preferably 3 to 15°C, and even more preferably 5 to 15°C. Having the exothermic peak width within this range allows for a polyamide composition that improves the surface properties of molded articles. The exothermic peak width is measured by the method described in the examples below.
[0079] In the polyamide composition of this embodiment, the exothermic peak width can be adjusted, for example, by copolymerizing polyamide (A). Specifically, this can be done by using 1,9-nonanediamine and 2-methyl-1,8-octanediamine in combination as aliphatic diamines and changing the molar ratio of 1,9-nonanediamine and 2-methyl-1,8-octanediamine; using terephthalic acid and isophthalic acid in combination as aromatic dicarboxylic acids; or copolymerizing polyamide (A) with an aliphatic polyamide, such as "polyamide 9T / polyamide 66". Furthermore, the exothermic peak width of the polyamide composition can also be adjusted by including a polyamide other than polyamide (A) (for example, an aliphatic polyamide such as polyamide 6).
[0080] Furthermore, the exothermic peak width can also be adjusted by including a crystal nucleating agent in the polyamide composition. The "crystal nucleating agent" refers to a substance that, when added, increases the crystallization temperature measured by differential scanning calorimetry (DSC), or is effective in refining or homogenizing the size of spherulites in the resulting molded product.
[0081] Examples of nucleating agents include talc, boron nitride, mica, kaolin, calcium carbonate, barium sulfate, silicon nitride, carbon black, potassium titanate, and molybdenum disulfide. These may be used individually or in combination of two or more. However, among the nucleating agents, boron nitride, mica, kaolin, calcium carbonate, barium sulfate, carbon black, potassium titanate, and molybdenum disulfide are considered fillers (C) in the polyamide composition of this embodiment, as described above.
[0082] As a nucleating agent, talc is preferred from the viewpoint of refining or homogenizing the size of spherulites in polyamide (A). Also from a similar viewpoint, the average particle size of the nucleating agent is preferably 0.01 to 20 μm, more preferably 0.5 to 15 μm, and even more preferably 1 to 10 μm.
[0083] The average particle size of the crystal nucleating agent can be measured by dissolving the molded product in a solvent such as formic acid in which polyamide is soluble, observing the resulting insoluble components with an optical microscope or scanning electron microscope, and calculating the average of, for example, 100 or more particles.
[0084] When a nucleating agent is used, the amount of nucleating agent is preferably 0.001 to 10 parts by weight, more preferably 0.01 to 5 parts by weight, and even more preferably 0.1 to 2 parts by weight, per 100 parts by weight of polyamide (A). By using an amount of 0.001 parts by weight or more, the heat resistance of the polyamide composition is improved, and by using an amount of 10 parts by weight or less, a polyamide composition with excellent tensile strength can be obtained.
[0085] In this embodiment, the weight-average molecular weight (Mw) of the polyamide composition measured by the method described in the examples below is preferably 12,000 to 40,000 g / mol, more preferably 13,000 to 30,000 g / mol, even more preferably 16,000 to 30,000 g / mol, still more preferably 18,000 to 30,000 g / mol, still more preferably 19,000 to 28,000 g / mol, and still more preferably 20,000 to 25,000 g / mol. By having the weight-average molecular weight (Mw) within the above range, a polyamide composition with an excellent balance between the flexural strength and moldability of the molded article can be obtained.
[0086] The polyamide composition of this embodiment preferably has a melting point of 200 to 350°C, and more preferably 250 to 350°C. Having a melting point within this range allows for a polyamide composition in which thermal decomposition of the polyamide during melt molding is suppressed. The melting point is measured by the method described in the examples below.
[0087] The crystallization temperature of the polyamide composition in this embodiment is not particularly limited as long as it does not impair the effects of the present invention, but for example it may be 200°C or higher, 210°C or higher, 220°C or higher, 310°C or lower, 300°C or lower, or 290°C. That is, it may be 200 to 310°C, 210 to 300°C, or 220 to 290°C. The crystallization temperature is measured by the method described in the examples below.
[0088] The polyamide composition of this embodiment has a crystallization rate of 0.020°C, calculated from the following formula (1). -1 Preferably, the temperature is 0.030°C or higher. -1 It is more preferable that the temperature be above 0.033°C. -1 It is even more preferable that the temperature is as described above. From the viewpoint of the surface properties of the molded product, 0.040°C is preferable. -1 It is even more preferable that the temperature be above 0.044°C. -1 It is even more preferable that the temperature be above 0.045°C. -1 It is even more preferable that the temperature is as described above. On the other hand, from the viewpoint of having an excellent balance between the bending strength and formability (or surface properties) of the molded product, 0.030 to 0.038°C is preferable. -1 It is even more preferable that the temperature is 0.032 to 0.037°C. -1 It is even more preferable that the crystallization rate (°C) -1 ) = 1 / (Melting point (°C) - Crystallization temperature (°C)) (1) By having the crystallization rate of the polyamide composition within the above range, it is possible to obtain a polyamide composition that improves the surface properties of molded articles. However, in formula (1) above, "melting point" and "crystallization temperature" both refer to the melting point and crystallization temperature of the polyamide composition, and are measured by the method described in the examples below.
[0089] (Method for producing polyamide composition) There are no particular limitations on the method for producing the polyamide composition, and a method that can uniformly mix polyamide (A), halogenated flame retardant (B), filler (C), and, if necessary, flame retardant aid (D) and other additives mentioned above can be preferably employed. Mixing is usually preferably carried out by melt kneading using a single-screw extruder, twin-screw extruder, kneader, Banbury mixer, etc. The melt kneading conditions are not particularly limited, but for example, a method of melt kneading for about 1 to 30 minutes at a temperature range about 10 to 50°C higher than the melting point of polyamide (A) can be cited.
[0090] <Molded Article> As one embodiment of this product, a molded article made from the polyamide composition described above may be used. The flexural strength of the molded article made from the polyamide composition is preferably 200 to 400 MPa, more preferably 250 to 400 MPa, even more preferably 280 to 380 MPa, and still more preferably 300 to 370 MPa. The flexural strength is measured by the method described in the examples below. There are no particular restrictions on the method for manufacturing the molded article, and known methods such as injection molding and extrusion molding can be used. In addition, additives such as chain extenders may be added during molding, and further treatments such as heat treatment and electron beam crosslinking may be applied after molding.
[0091] The molded articles of this embodiment can be used as industrial parts such as electrical components, electronic components, automotive parts, and mechanical parts, as well as faucet parts, household goods, leisure goods, and various other molded articles of any shape and use.
[0092] Examples of electrical and electronic components include connectors such as FPC connectors, BtoB connectors, card connectors, SMT connectors (coaxial connectors, etc.), and memory card connectors; SMT relays; SMT bobbins; sockets such as memory sockets and CPU sockets; switches such as command switches and SMT switches; optical components such as optical fiber components and optical sensors; LED application components such as LED reflectors; and electronic circuit boards such as solar cell substrates, LED mounting substrates, flexible printed circuit boards, and resin molded circuit boards.
[0093] Automotive parts include, for example, cooling components such as thermostat housings, coolant control valve housings, thermal management module housings, radiator tanks, radiator hoses, water outlets, water inlets, water pump housings, and rear joints; intake and exhaust system components such as intercooler tanks, intercooler cases, turbo duct pipes, EGR cooler cases, resonators, throttle bodies, intake manifolds, and tailpipes; fuel system components such as fuel delivery pipes, gasoline tanks, quick connectors, canisters, pump modules, fuel lines, oil strainers, lock nuts, and seals; structural components such as mount brackets, torque rods, and cylinder head covers; and bearing retainers, gear tensioners, and other components. Examples include drivetrain components such as headlamp actuator gears, throttle valve gears, sliding door rollers, and clutch components; brake system components such as air brake tubes; automotive electrical components in the engine compartment such as wire harness connectors, motor components, sensors, ABS bobbins, combination switches, and onboard switches; and interior and exterior components such as sliding door dampers, door mirror stays, door mirror brackets, inner mirror stays, roof rails, engine mount brackets, air cleaner inlet pipes, door checkers, plastic chains, emblems, clips, breaker covers, cup holders, airbags, fenders, spoilers, radiator supports, radiator grilles, louvers, air scoops, hood bulges, tailgates, and fuel sender modules.
[0094] Industrial components include, for example, mechanical components, gas pipes, oil field drilling pipes, hoses, termite-resistant cables (communication cables, pass cables, etc.), paint parts for powder-coated products (internal coatings for water pipes, etc.), subsea oil field pipes, pressure-resistant hoses, hydraulic tubes, paint tubes, fuel pump housings and impellers, separators, supercharger ducts, butterfly valves, conveyor roller bearings, railway sleeper spring supports, outboard motor engine covers, generator engine covers, wind turbine blades, irrigation valves, large switches, and monofilaments (extruded yarns) for fishing nets, etc.
[0095] Examples of faucet components include housings for water transport components, water storage component housings, filter casing housings, faucet housings, pipe housings, bathroom faucet (hot / cold water switching valve, water volume switching valve, etc.) housings, sanitary component housings, kitchen faucet housings, water heater housings, valve components (shut-off balls, slides, cylinders) and valve component housings, toilet shut-off valve housings, shower head housings, water heater valve housings, fittings for residential plumbing (underfloor piping, etc.), bathroom faucet fittings, water pipe fittings, pipe joints, and water meter housings. Examples include wedge bearings, water meter components (bearings, propellers, pins), water meter and gas meter housings, distributor housings, valve / pump housings for household appliances, steam-resistant components for steam irons, internal containers for electric kettles, dishwasher components (washing tubs, washing nozzles, baskets), pump housings, pump components (e.g., turbine wheels, impellers), water supply system (hot water tanks, etc.) housings, heating system housings, cooling system housings, water flow control valves, pressure reducing valves, relief valves, solenoid valves, three-way valves, thermostatic valves, water temperature sensors, water flow sensors, and bathtub adapters.
[0096] Examples of household products include valves / pump housings for tea and coffee makers; valves / pump housings for cooking appliances such as rice cookers and steamers; steam-resistant parts for cooking appliances such as rice cookers and steamers (e.g., the top lid of a rice cooker); sliding parts for cooking appliances such as rice cookers and steamers (e.g., gears); sliding parts for commercial cooking equipment (e.g., gears for gear pumps); and steam-resistant parts for commercial cooking equipment (e.g., pipes for commercial rice cookers).
[0097] Examples of leisure goods include insoles for sports shoes, racket frames and grommets, golf club heads and sleeves, fishing reels and rods, boat propellers, bicycle suspensions, gears, saddles, and bottle cages.
[0098] In particular, the polyamide composition of this embodiment is excellent in heat resistance, flame retardancy, and moldability, and can suppress deformation during the reflow process, making it suitable for use in electrical and electronic components where a large number of parts need to be manufactured in a short time. Specifically, it can be suitably used in electrical and electronic components including the SMT process, and more specifically in surface mount components such as SMT-compatible connectors, SMT relays, SMT bobbins, sockets, command switches, SMT switches, camera modules, power supply components, sensors, capacitor mounting plates, hard disk components, resistors, fuse holders, coil bobbins, and IC housings.
[0099] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these.
[0100] Each evaluation in the examples and comparative examples was carried out according to the method described below.
[0101] • Weight-average molecular weight (Mw) The weight-average molecular weight (Mw) of the polyamides used in the examples and comparative examples, and the polyamide compositions obtained in the examples and comparative examples, was determined by gel permeation chromatography (GPC) as the molecular weight on a standard polymethyl methacrylate basis. As the eluent, an HFIP solution was used, prepared by dissolving sodium trifluoroacetate at a ratio of 0.85 g per 1 kg of 1,1,1,3,3,3-hexafluoroisopropanol (HFIP). 1.5 mg of the sample (in resin equivalent) was weighed and dissolved in 3 mL of the above eluent. The resulting solution was filtered through a 0.2 μm membrane filter to prepare the measurement sample. The weight-average molecular weight (Mw) was measured using a Tosoh Corporation measuring instrument "HLC-8320GPC" and a Tosoh Corporation column "TSK-gel Super HM-N" under conditions of a measurement temperature of 40°C and a detection wavelength of 254 nm.
[0102] - Melting point and crystallization temperature The melting point and crystallization temperature of the polyamide compositions obtained in the examples and comparative examples were measured using a differential scanning calorimetry analyzer "DSC7020" manufactured by Hitachi High-Tech Science Corporation, in accordance with ISO-11357-3 (2nd edition, 2011). Specifically, the sample (polyamide composition pellet) was heated from 30°C to 340°C at a rate of 10°C / min under a nitrogen atmosphere, held at 340°C for 5 minutes to completely melt the sample, then cooled to 50°C at a rate of 10°C / min, held at 50°C for 5 minutes, and then heated again to 340°C at a rate of 10°C / min. The peak temperature of the exothermic peak that appeared when the temperature was lowered was defined as the crystallization temperature, and the peak temperature of the endothermic peak that appeared when the temperature was raised again was defined as the melting point (°C). In this invention, the larger the difference between the melting point and the crystallization temperature of the polyamide composition, the better the surface properties of the molded product tend to be.
[0103] The crystallization rate of the polyamide compositions obtained in the examples and comparative examples was determined by the following formula (1): Crystallization rate (°C) -1 ) = 1 / (Melting point (°C) - Crystallization temperature (°C)) (1) In formula (1), "Melting point (°C)" and "Crystallization temperature (°C)" are measured values for the polyamide composition obtained by the above method.
[0104] - Exothermic Peak Width The exothermic peak width during cooling in differential scanning calorimetry (DSC) of the polyamide compositions obtained in the examples and comparative examples was measured by performing DSC in the same manner as the melting point and crystallization temperature measurement method described above. For the exothermic peak due to crystallization observed during cooling, the difference between the "extranexation start point" and the "extranexation end point" of the exothermic peak due to crystallization during the first cooling was calculated and defined as the "exothermic peak width". The "extranexation start point" is the point (temperature) where the tangent at the point of maximum slope on the high-temperature side of the peak intersects with the baseline, and the "extranexation end point" is the point (temperature) where the tangent at the point of maximum slope on the low-temperature side of the peak intersects with the baseline. In cases where multiple exothermic peaks are observed, such as when the polyamide composition contains multiple polyamides, the exothermic peak width is calculated for the exothermic peak observed at the higher temperature.
[0105] <Preparation of Test Specimens> Using the polyamide compositions obtained in the Examples and Comparative Examples, an injection molding machine manufactured by Sumitomo Heavy Industries, Ltd. (clamping force: 100 tons, screw diameter: φ32 mm) was used to mold the polyamide compositions using a T-runner mold under conditions of a cylinder temperature 20 to 30°C higher than the melting point of the polyamide in the polyamide composition and a mold temperature of 140°C. A multipurpose test specimen type A1 (a dumbbell-shaped test specimen as described in JIS K7139:2009; 4 mm thick, 170 mm total length, 80 mm parallel section length, 10 mm parallel section width) was prepared.
[0106] - Load deflection temperature In accordance with ISO-75-2, the load deflection temperature (unit: °C) at a load of 1.80 MPa was measured using a strip-shaped test piece measuring 80 mm × 10 mm × 4 mmt, which was prepared by machining the parallel section of a multipurpose test piece type A1 prepared by the method described above. The load deflection temperature of the strip-shaped test piece at a load of 1.80 MPa is preferably 55°C or higher, more preferably 60°C or higher, and even more preferably 65°C or higher, relative to the melting points of lead-free solder (melting point: 217°C) and lead solder (melting point: 183°C), respectively, as an indicator of resistance to deformation during reflow soldering. The load deflection temperature of the strip-shaped test piece can be considered as the deflection temperature of the polyamide composition.
[0107] - Flame retardancy: Flame retardancy was evaluated in accordance with the UL-94 standard. Using the polyamide compositions obtained in each example and comparative example, injection molding (mold temperature: 140°C) was performed at a cylinder temperature approximately 20°C higher than the melting point of the polyamide to produce test specimens with a thickness of 0.75 mm, a width of 13 mm, and a length of 125 mm. Next, the upper end of the test specimen was fixed with a clamp and held vertically, and a predetermined flame was applied to the lower end for 10 seconds, after which the flame was removed and the burning time of the test specimen (first time) was measured. Immediately after extinguishing the flame, the lower end was again applied to the lower end for 10 seconds, and after removing the flame, the burning time of the test specimen (second time) was measured. The same measurement was performed on five test specimens, and a total of 10 measurement data points were obtained: five for the first burning time and five for the second burning time. The sum of the 10 measurement data points obtained was defined as T, and the maximum value as M, and they were evaluated according to the evaluation criteria below. In addition, the presence or absence of molten material (drip) falling from the test specimen during flame application was visually confirmed. Furthermore, if a material meets any of the following evaluation criteria V-0 to V-2 of the UL-94 standard, it is flame-retardant, and if it does not meet any of the evaluation criteria, it is not flame-retardant. [Evaluation Criteria] V-0: T is 50 seconds or less and M is 10 seconds or less, the flame does not rise up to the clamp, and even if the flaming molten material falls, it does not ignite the cotton 12 inches below. V-1: T is 250 seconds or less and M is 30 seconds or less, the flame does not rise up to the clamp, and even if the flaming molten material falls, it does not ignite the cotton 12 inches below. V-2: T is 250 seconds or less and M is 30 seconds or less, the flame does not rise up to the clamp, the flaming molten material falls and ignites the cotton 12 inches below. X: If none of the above UL-94 evaluation criteria are met.
[0108] Using the polyamide compositions obtained in the reflow deformation examples and comparative examples, an injection molding machine manufactured by Sumitomo Heavy Industries, Ltd. (clamping force: 18 tons, screw diameter: φ18 mm) was used to mold the polyamide compositions using a mold with a film gate of 30 mm width and 0.9 mm height, under conditions of a cylinder temperature 20 to 30°C higher than the melting point of the polyamide in the polyamide composition and a mold temperature of 140°C, to produce flat test pieces (1 mm thick, 30 mm long x 30 mm wide). In accordance with JEDEC standard J-STD-020, the flat test pieces were placed in a reflow oven and heat-treated under the following heating conditions. After that, they were removed and allowed to cool at room temperature, and the deformation of the molded product, which was the test piece, was visually observed and evaluated according to the following criteria. [Heating Conditions] (1) Preheating: 150-190°C for 60-120 seconds (2) Main heating after preheating: 217°C or higher for 60-150 seconds (3) Maximum temperature: Lead-free solder was used in Examples 1-4, 6-8 and Comparative Example 2, described later, with a maximum temperature of 270°C. Lead solder was used in Example 5, with a maximum temperature of 236°C. However, under the above heating conditions, the rate of temperature increase when transitioning from preheating to main heating was controlled to a maximum of 3°C / second. Furthermore, the maximum temperature was determined by selecting the appropriate lead-free solder or lead solder based on the melting point of the polyamide composition used as the test piece. [Evaluation Criteria] A: No dimensional change in the test piece B: Dimensional change in the test piece
[0109] - Surface properties: Multipurpose test specimens of type A1 (4 mm thick) prepared by the method described above were visually observed and evaluated according to the following criteria. [Evaluation criteria] A: No glass fiber lifting, and the surface is smooth. B: Slight glass fiber lifting is observed. C: The surface is uneven due to glass fiber lifting.
[0110] - Bending Strength: Using a multi-purpose test specimen type A1 (4 mm thick) prepared by the method described above, the bending strength (MPa) was measured using a universal material testing machine (Instron) in accordance with ISO 178 (2nd edition 2012) under conditions of a test speed of 2 mm / min and a support distance of 64 mm. A higher measured bending strength indicates superior bending strength of the molded product.
[0111] The components shown in Table 1 below are as follows: [Polyamide (A)] ・Polyamide (A-1): A polyamide in which the dicarboxylic acid units are terephthalic acid units and the diamine units are 1,9-nonanediamine units and 2-methyl-1,8-octanediamine units (molar ratio 85 / 15) (melting point: 306°C, glass transition temperature: 125°C, Mw: 16,000) ・Polyamide (A-2): A polyamide in which the dicarboxylic acid units are terephthalic acid units and the diamine units are 1,9-nonanediamine units and 2-methyl-1,8-octanediamine units (molar ratio 50 / 50) (melting point: 265°C, glass transition temperature: 125°C, Mw: 21,000)・Polyamide (A-3): A polyamide in which the dicarboxylic acid units are terephthalic acid units and the diamine units are 1,9-nonanediamine units and 2-methyl-1,8-octanediamine units (molar ratio 85 / 15) (melting point: 306°C, glass transition temperature: 125°C, Mw: 18,000) [Halogenated flame retardant (B)] ・LANXESS Corporation, product name "FiremasterCP-44HF" (glycidyl methacrylate modified polybrominated styrene) [Filler (C)] ・Filler (C-1): Nitto Boseki Co., Ltd., product name "CS-3G-225S" (glass fiber, cross-sectional shape: circular, average fiber diameter: 9.5 μm, average fiber length: 3 mm) ・Filler (C-2): Nitto Boseki Co., Ltd., product name "CSH 3PA-870S (glass fiber, cross-sectional shape: cocoon-shaped, ratio of major axis to minor axis: 2 (major axis: 20 μm, minor axis: 10 μm), average fiber length: 3 mm) ・Filler (C-3): Manufactured by Nitto Boseki Co., Ltd., product name "CSG 3PA-820S" (glass fiber, cross-sectional shape: oval, ratio of major axis to minor axis: 4 (major axis: 28 μm, minor axis: 7 μm), average fiber length: 3 mm) ・Filler (C-4): Manufactured by Nippon Electric Glass Co., Ltd., product name "ECS 03 T-251H" (glass fiber, cross-sectional shape: circular, average fiber diameter: 10.5 μm, average fiber length: 3 mm) [Flame retardant additive (D)] ・Manufactured by Nippon Light Metal Co., Ltd., product name "FlamtardS" (zinc stannate) [Other additives] - Drip inhibitor: Manufactured by Mitsui DuPont Fluorochemicals Co., Ltd., product name "640-J" (polytetrafluoroethylene powder) - Antioxidant: Manufactured by Sumitomo Chemical Co., Ltd., product name "SmilizerGA-80" (3,9-bis{1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane) • Release agent: Mitsui Chemicals, Inc., product name "High Wax 200P" (polyolefin wax) • Nucleating agent: Fuji Talc Industries Co., Ltd., product name "ML112" (talc, average particle size 4.75 μm)
[0112] [Examples 1-8, Comparative Examples 1-2] Using the polyamide (A), halogenated flame retardant (B), filler (C), flame retardant aid (D), and other additives listed in Table 1, the components other than filler (C) were supplied from the upstream hopper of a twin-screw extruder (screw diameter 26 mmφ, L / D = 46, rotation speed 150 rpm, discharge rate 10 kg / h) manufactured by Toshiba Machine Co., Ltd., so that the blending composition was as shown in Table 1. Filler (C) was supplied from a side feeder and the mixture was melt-kneaded at 320°C. The melt-kneaded polyamide composition was extruded into strands, cooled, and cut to obtain polyamide composition pellets. Using the obtained pellets, test pieces of a predetermined shape were prepared according to the method described above, and various physical properties were evaluated. The results are shown in Table 1.
[0113]
[0114] As shown in Table 1, the polyamide compositions of Examples 1 to 8 all showed a difference of 60°C or more between the load deflection temperature and the melting point of the solder, resulting in no dimensional change during reflow. On the other hand, in Comparative Example 1, the amount of filler was too much, exceeding the range specified in this application (150 to 350 parts by weight (relative to 100 parts by weight of polyamide (A))), so it did not come together as pellets during pelletizing and crumbled, making it impossible to obtain a polyamide composition. In Comparative Example 2, the amount of filler was too little, below the range specified in this application (150 to 350 parts by weight (relative to 100 parts by weight of polyamide (A))), resulting in a difference of less than 55°C between the load deflection temperature and the melting point of the solder, resulting in dimensional change during reflow. Furthermore, Example 5, which had a high crystallization rate, showed no glass delamination and a smooth surface, resulting in particularly excellent surface quality of the molded product. In addition, Examples 7 and 8 showed excellent flame retardancy and flexural strength of the molded products. Furthermore, in Example 3, the use of a filler with an oval cross-sectional shape resulted in superior flame retardancy of the molded product compared to Examples 1 and 2, which used a filler with a circular or cocoon-shaped cross-sectional shape.
[0115] As described above, the polyamide composition of the present invention has excellent flame retardancy and can suppress deformation during the reflow process. Therefore, the polyamide composition of the present invention can be used in various molded articles that require flame retardancy and suppression of deformation during the reflow process, and is extremely useful.
Claims
1. A polyamide composition comprising a polyamide (A), a halogenated flame retardant (B), and a filler (C), wherein the polyamide (A) is a semi-aromatic polyamide, the semi-aromatic polyamide comprises structural units derived from a dicarboxylic acid and structural units derived from a diamine, more than 50 mol% of the structural units derived from the dicarboxylic acid are structural units derived from an aromatic dicarboxylic acid, and more than 50 mol% of the structural units derived from the diamine are structural units derived from an aliphatic diamine having 7 to 18 carbon atoms, and the polyamide composition contains 1 to 100 parts by weight of the halogenated flame retardant (B) and 150 to 350 parts by weight of the filler (C) per 100 parts by weight of the polyamide (A).
2. The polyamide composition according to claim 1, wherein the aliphatic diamine is at least one selected from the group consisting of 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine.
3. The polyamide composition according to claim 1 or 2, wherein the aliphatic diamine comprises 1,9-nonanediamine and 2-methyl-1,8-octanediamine, and the molar ratio of 1,9-nonanediamine to 2-methyl-1,8-octanediamine is 60 / 40 to 10 / 90.
4. The polyamide composition according to claim 1 or 2, wherein the aliphatic diamine comprises 1,9-nonanediamine and 2-methyl-1,8-octanediamine, and the molar ratio of 1,9-nonanediamine to 2-methyl-1,8-octanediamine is 90 / 10 to 60 / 40.
5. The polyamide composition according to any one of claims 1 to 4, wherein the weight-average molecular weight (Mw) of the polyamide composition is 18,000 to 30,000 g / mol.
6. The polyamide composition according to any one of claims 1 to 5, wherein the halogen-based flame retardant (B) comprises a brominated flame retardant (B1).
7. The polyamide composition according to claim 6, wherein the brominated flame retardant (B1) comprises brominated polystyrene.
8. The polyamide composition according to any one of claims 1 to 7, comprising 30 to 45 parts by weight of the halogenated flame retardant (B) per 100 parts by weight of the polyamide (A).
9. The polyamide composition according to any one of claims 1 to 8, wherein the filler (C) comprises a fibrous filler (C1).
10. The polyamide composition according to claim 9, wherein the fibrous filler (C1) is at least one selected from the group consisting of carbon fibers, glass fibers, and aramid fibers.
11. The polyamide composition according to any one of claims 1 to 10, wherein the content of the polyamide (A) is 10 to 40% by weight.
12. The polyamide composition according to any one of claims 1 to 11, further comprising a flame retardant additive (D).
13. The polyamide composition according to claim 12, comprising 1 to 30 parts by weight of the flame retardant additive (D) per 100 parts by weight of the polyamide (A).
14. The polyamide composition according to claim 12 or 13, wherein the flame retardant additive (D) is at least one selected from the group consisting of antimony trioxide, antimony tetroxide, antimony pentoxide, sodium antimonate, melamine orthophosphate, melamine pyrophosphate, melamine borate, melamine polyphosphate, aluminum oxide, aluminum hydroxide, zinc borate, and zinc stannate.
15. The polyamide composition according to any one of claims 1 to 14, wherein the exothermic peak width during cooling in differential scanning calorimetry (DSC) is 1 to 20°C.
16. The crystallization rate calculated from the following formula (1) is 0.044°C -1 The polyamide composition according to any one of claims 1 to 15. Crystallization rate (°C) -1 ) = 1 / (Melting point (°C) - Crystallization temperature (°C)) (1) However, in formula (1) above, "melting point" and "crystallization temperature" both refer to the melting point and crystallization temperature of the polyamide composition.
17. The crystallization rate calculated from the following formula (1) is 0.030 to 0.038°C. -1 The polyamide composition according to any one of claims 1 to 15. Crystallization rate (°C) -1 ) = 1 / (Melting point (°C) - Crystallization temperature (°C)) (1) However, in formula (1) above, "melting point" and "crystallization temperature" both refer to the melting point and crystallization temperature of the polyamide composition.
18. A molded article comprising the polyamide composition according to any one of claims 1 to 17.
19. The molded article according to claim 18, which is an electrical component or an electronic component.
20. A molded article according to claim 18 or 19, which is a surface mount component.