Thermosetting resin composition and cured product thereof

The thermosetting resin composition with a saturated polyester resin and calcium hydroxide addresses molding defects by controlling shrinkage, reducing cracks and voids in complex-shaped articles.

WO2026240199A1PCT designated stage Publication Date: 2026-11-19RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/018454
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-15
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Thermosetting resin compositions face issues such as molding defects like sink marks and voids in complex shapes and cracks in thin-walled portions due to molding shrinkage.

Method used

A thermosetting resin composition comprising a saturated polyester resin with specific weight-average molecular weight and acid value, combined with calcium hydroxide as a thickener, to control shrinkage and reduce crack formation.

Benefits of technology

The composition effectively minimizes cracks and voids in molded products by adjusting shrinkage rates to zero, enhancing the moldability and durability of complex-shaped articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

This thermosetting resin composition contains (A) a saturated polyester resin, (B) a thermosetting resin, (C) an ethylenically unsaturated monomer, (D) a thermal polymerization initiator, (E) glass fibers, (F) an inorganic filler, and (G) a thickener. The thickener (G) is calcium hydroxide, and the weight-average molecular weight of the saturated polyester resin (A) is 8500-15,000. When the weight-average molecular weight of the saturated polyester resin (A) is 8500 to less than 10,000, the acid value of the saturated polyester resin (A) is 6.0-7.5 KOH mg / g; when the weight-average molecular weight of the saturated polyester resin (A) is 10,000 to less than 12,000, the acid value of the saturated polyester resin (A) is 5.5-9.8 KOH mg / g; and when the weight-average molecular weight of the saturated polyester resin (A) is 12,000-15,000, the acid value of the saturated polyester resin (A) is 5.5-9.2 KOH mg / g.
Need to check novelty before this filing date? Find Prior Art

Description

Thermosetting resin composition and cured product thereof

[0001] The present disclosure relates to a thermosetting resin composition and a cured product thereof.

[0002] Thermosetting resin compositions comprising thermosetting resins such as unsaturated polyester resins and vinyl ester resins, low-shrinkage agents, polymerization initiators, fillers, reinforcing materials and the like have advantages such as electrical insulation, heat resistance, flame retardancy, high rigidity and dimensional stability, and are therefore widely applied to electronic components related to fields such as home appliances, automobiles and energy. Among thermosetting resin compositions, bulk molding compound (BMC) formed into a bulk shape is used as a molding material, and can be formed into molded articles by molding methods such as compression molding, transfer molding and injection molding. Patent Document 1 discloses a thermosetting resin composition and a bulk molding compound containing an unsaturated polyester resin (A), a low-shrinkage agent (B), aluminum hydroxide (C), magnesium oxide (D), and hollow filler (E).

[0003] JP 2024-5578 A

[0004] When the target molded article has a complicated shape, there have been problems such as molding defects such as sink marks and voids occurring in portions having a complicated structure, and cracks occurring in thin-walled portions.

[0005] The present disclosure provides a thermosetting resin composition capable of reducing the occurrence of cracks.

[0006] The contents of this disclosure include the following aspects: [Aspect 1] A thermosetting resin composition comprising (A) a saturated polyester resin, (B) a thermosetting resin, (C) an ethylenically unsaturated monomer, (D) a thermal polymerization initiator, (E) glass fibers, (F) an inorganic filler, and (G) a thickener, wherein the thickener (G) is calcium hydroxide, the weight-average molecular weight of the saturated polyester resin (A) is 8500 to 15000, and when the weight-average molecular weight of the saturated polyester resin (A) is 8500 or more and less than 10000, the acid value of the saturated polyester resin (A) is 6.0 to 7.5 KOH mg / g; when the weight-average molecular weight of the saturated polyester resin (A) is 10000 or more and less than 12000, the acid value of the saturated polyester resin (A) is 5.5 to 9.8 KOH mg / g; A thermosetting resin composition wherein, when the weight-average molecular weight of the saturated polyester resin (A) is 12,000 to 15,000, the acid value of the saturated polyester resin (A) is 5.5 to 9.2 KOH mg / g. [Aspect 2] The thermosetting resin composition according to aspect 1, wherein the content of the thickener (G) is 0.2 to 9 parts by mass, based on 100 parts by mass of the total amount of the thermosetting resin (B) and the ethylenically unsaturated monomer (C). [Aspect 3] The thermosetting resin composition according to aspect 1 or 2, wherein the saturated polyester resin (A) is a polycondensate of a diol and a saturated polybasic acid, and the saturated polybasic acid contains an aromatic saturated polybasic acid or its acid anhydride and an aliphatic saturated polybasic acid. [Aspect 4] The thermosetting resin composition according to aspect 3, wherein the ratio (molar ratio) of the structure derived from the aromatic saturated polybasic acid or its acid anhydride to the structure derived from the aliphatic saturated polybasic acid in the (A) saturated polyester resin is 20:80 to 80:20. [Aspect 5] The thermosetting resin composition according to aspect 3 or 4, wherein the aromatic saturated polybasic acid is one or more selected from isophthalic acid and terephthalic acid. [Aspect 6] The thermosetting resin composition according to any one of aspects 1 to 5, wherein the (B) thermosetting resin comprises at least a (B-1) unsaturated polyester resin. [Aspect 7] The thermosetting resin composition according to aspect 6, wherein the weight-average molecular weight of the (B-1) unsaturated polyester resin is 10,000 to 50,000.[Aspect 8] A thermosetting resin composition according to any one of aspects 1 to 7, wherein the total amount of the (B) thermosetting resin and the (C) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 5 to 30 parts by mass of the (A) saturated polyester resin, 20 to 80 parts by mass of the (B) thermosetting resin, 20 to 80 parts by mass of the (C) ethylenically unsaturated monomer, 0.5 to 20 parts by mass of the (D) thermal polymerization initiator, 5 to 150 parts by mass of the (E) glass fiber, and 50 to 1000 parts by mass of the (F) inorganic filler. [Aspect 9] A cured product of the thermosetting resin composition according to any one of aspects 1 to 8. [Aspect 10] A molded article containing a cured product of the thermosetting resin composition according to any one of aspects 1 to 8.

[0007] According to this disclosure, a thermosetting resin composition that can reduce the occurrence of cracks can be provided.

[0008] This is a schematic cross-sectional view of an exemplary motor. This figure plots the acid value and weight-average molecular weight of (A) saturated polyester resin and (cA) saturated polyester resin used in the examples and comparative examples.

[0009] The embodiments of the present invention will be described in detail below. However, the present invention is not limited to the embodiments shown below.

[0010] In this specification, when "~" is used for a numerical range, the numbers at both ends are the upper and lower limits, respectively, and are included in the numerical range. If multiple upper or lower limits are listed, a numerical range can be created from all combinations of upper and lower limits. Similarly, if multiple numerical ranges are listed, separate numerical ranges can be created by individually selecting and combining upper and lower limits from those ranges.

[0011] In this specification, "(meth)acrylic acid" means methacrylic acid or acrylic acid, "(meth)acrylate" means acrylate or methacrylate, and "(meth)acryloyloxy" means acryloyloxy or methacryloyloxy.

[0012] In this specification, "thermosetting resin" refers to a resin that hardens by forming a cross-linked structure when heated, and indicates the state before hardening.

[0013] In this specification, "ethylenically unsaturated bond" means a double bond formed between carbon atoms excluding the carbon atoms that form the aromatic ring, and "ethylenically unsaturated monomer" means a monomer having an ethylenically unsaturated bond.

[0014] In this specification, "weight-average molecular weight" and "number-average molecular weight" are defined as values ​​obtained by measuring at room temperature (23°C) under the following conditions using gel permeation chromatography (GPC) and using a standard polystyrene calibration curve. Apparatus: Shodex™ GPC-101 (Resonac Corporation) Column: Shodex™ LF-804 (Resonac Corporation) Column temperature: 40°C Sample: 0.2% by mass tetrahydrofuran solution of the sample Flow rate: 1 mL / min Eluent: Tetrahydrofuran Detector: Shodex™ RI-71S (Resonac Corporation)

[0015] In this specification, "acid value" refers to the acid value measured in accordance with JIS K6901:2021 5.3. That is, the acid value means the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of non-volatile matter excluding the solvent.

[0016] <Thermosetting Resin Composition> The thermosetting resin composition of one embodiment contains (A) saturated polyester resin, (B) thermosetting resin, (C) ethylenically unsaturated monomer, (D) thermal polymerization initiator, (E) glass fiber, (F) inorganic filler, and (G) thickener, wherein (G) thickener is calcium hydroxide, the weight-average molecular weight of (A) saturated polyester resin is 8500 to 15000, and (A) saturated polyester resin has a specific acid value corresponding to its weight-average molecular weight. When the molding shrinkage rate of the cured product of the thermosetting resin composition is greater than 0%, that is, when shrinkage occurs during curing, it is thought that molding defects such as voids and cracks are likely to occur in the molded product. Therefore, the inventors considered that the occurrence of cracks could be suppressed by adjusting the molding shrinkage rate to 0% or less, that is, on the expansion side. As a result of the investigation, it was found that in a thermosetting resin composition containing calcium hydroxide, by using (A) saturated polyester resin having a specific acid value corresponding to its weight-average molecular weight as a low-shrinkage agent, shrinkage during curing can be reduced or suppressed, and the occurrence of cracks in the molded product can be suppressed. While not bound by any particular theory, it is believed that calcium hydroxide interacts with (A) saturated polyester resin, inhibiting the mobility of polymer chains and thereby thickening the resin composition. This thickening effect is also thought to affect the dispersion state of (A) saturated polyester resin during curing, which influences the shrinkage rate. Since the susceptibility to the thickening effect by calcium hydroxide differs depending on the acid value and weight-average molecular weight of (A) saturated polyester resin, it is thought that the range of suitable acid values ​​differs depending on the weight-average molecular weight.

[0017] [(A) Saturated Polyester Resin] (A) Saturated polyester resin is a polycondensate of a polyhydric alcohol and a saturated polybasic acid having a weight-average molecular weight of 8,500 to 15,000. (A) Saturated polyester resin is preferably a polycondensate of a diol and a saturated polybasic acid, and more preferably a polycondensate of a diol, an aromatic saturated polybasic acid or its acid anhydride, and an aliphatic saturated polybasic acid.

[0018] (A) Saturated polyester resin may be used alone or in combination of two or more types. (A) Using saturated polyester resin reduces the occurrence of cracks during molding.

[0019] In this disclosure, styrene monomers and the like contained in commercially available saturated polyester resins are classified as (C) ethylenically unsaturated monomers.

[0020] The polyhydric alcohol is not particularly limited as long as it is a compound having two or more hydroxyl groups. The polyhydric alcohol is preferably one or more selected from the group consisting of diols and triols, and more preferably a diol. Examples of polyhydric alcohols include alkylene glycols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, and hydrogenated bisphenol A; polyoxyalkylene polyols such as diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol; bisphenol A; alkylene oxide-modified bisphenol A such as ethylene oxide adducts of bisphenol A and propylene oxide adducts of bisphenol A; and glycerin. From the viewpoint of crack resistance during molding, one or more selected from the group consisting of alkylene glycol and polyoxyalkylene polyol is preferred, polyoxyalkylene glycol is more preferred, and one or more selected from diethylene glycol, dipropylene glycol, and triethylene glycol is even more preferred. In particular, from the viewpoint of improving the durability of the molded product, it is preferred to use polyoxyethylene glycol and polyoxypropylene glycol in combination, and it is even more preferred to use diethylene glycol and dipropylene glycol in combination. (A) In the saturated polyester resin, the ratio (molar ratio) of structures derived from polyoxyethylene glycol to structures derived from polyoxypropylene glycol or the ratio (molar ratio) of structures derived from diethylene glycol to structures derived from dipropylene glycol is not particularly limited, but from the viewpoint of improving durability, 40:60 to 80:20 is preferred, 50:50 to 70:30 is more preferred, and 55:45 to 65:35 is even more preferred. (A) The ratio of structures derived from each raw material in the saturated polyester resin is a calculated value obtained from the amount of raw material used. Polyhydric alcohols may be used alone or in combination of two or more types.

[0021] The saturated polybasic acid is not particularly limited as long as it does not have an ethylenically unsaturated bond and has two or more carboxyl groups, or is an acid anhydride thereof; known compounds can be used. The saturated polybasic acid is preferably a saturated dibasic acid. Examples of saturated polybasic acids include aromatic saturated polybasic acids or their acid anhydrides such as phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, tetrachlorophthalic anhydride, tetrabromophthalic anhydride, nitrophthalic acid, and halogenated phthalic anhydride; aliphatic saturated polybasic acids such as succinic acid, adipic acid, sebacic acid, oxalic acid, malonic acid, azelaic acid, and glutaric acid; and acid anhydrides of cyclic aliphatic saturated polybasic acids such as hexahydrophthalic anhydride. As the aromatic saturated polybasic acid or its acid anhydride, one or more selected from the group consisting of aromatic saturated dibasic acids and their acid anhydrides are preferred, one or more selected from phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid are more preferred, and one or more selected from isophthalic acid and terephthalic acid are even more preferred. As the aliphatic saturated polybasic acid, an aliphatic saturated dibasic acid is preferred, an aliphatic saturated dibasic acid having 4 to 10 carbon atoms is more preferred, and one or more selected from succinic acid, adipic acid, and sebacic acid are even more preferred. From the viewpoint of crack resistance during molding, it is preferred to use one or more selected from the group consisting of aromatic saturated polybasic acids, their acid anhydrides, and aliphatic saturated polybasic acids, it is more preferred to use an aromatic saturated polybasic acid or its acid anhydride in combination with an aliphatic saturated polybasic acid, and it is even more preferred to use one or more selected from isophthalic acid and terephthalic acid in combination with one or more selected from succinic acid, adipic acid, and sebacic acid. Saturated polybasic acids may be used alone or in combination of two or more types.

[0022] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aromatic saturated polybasic acid or its acid anhydride is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more. When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aromatic saturated polybasic acid or its acid anhydride is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less. When the proportion of the aromatic saturated polybasic acid or its acid anhydride is within the above range, the moldability tends to be better and the properties of the cured product tend to be improved.

[0023] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aliphatic saturated polybasic acid is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more. When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the proportion of the aliphatic saturated polybasic acid is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less. If the proportion of the aliphatic saturated polybasic acid is within the above range, crack resistance tends to be further improved.

[0024] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, (A) the ratio (molar ratio) of the structure derived from the aromatic saturated polybasic acid or its acid anhydride to the structure derived from the aliphatic saturated polybasic acid in the saturated polyester resin is preferably 20:80 to 80:20, more preferably 30:70 to 70:30, and even more preferably 40:60 to 60:40.

[0025] When an aromatic saturated polybasic acid or its acid anhydride is used in combination with an aliphatic saturated polybasic acid, the structures derived from these may be uniformly dispersed within the molecules of the saturated polyester resin (A), or they may be unevenly distributed within the molecules. From the viewpoint of further improving crack resistance during molding, it is preferable that the saturated polyester resin (A) contains a block (X) which is a polycondensate of a diol and an aromatic saturated polybasic acid or its acid anhydride, and has a weight-average molecular weight of 3000 to 5000, and a block (Y) which is a polycondensate of a diol and an aliphatic saturated polybasic acid. In the saturated polyester resin (A) containing blocks (X) and (Y), the content ratio (molar ratio) of the structure derived from the aromatic saturated polybasic acid or its acid anhydride and the structure derived from the aliphatic saturated polybasic acid is preferably 20:80 to 80:20, more preferably 30:70 to 70:30, and even more preferably 40:60 to 60:40.

[0026] In a saturated polyester resin (A) comprising block (X) and block (Y), structures derived from aromatic saturated polybasic acids or their acid anhydrides may be scattered in portions other than block (X) and block (Y).

[0027] The weight-average molecular weight of block (X) is preferably 3000 or more, more preferably 3500 or more. The weight-average molecular weight of block (X) is preferably 5000 or less, more preferably 4500 or less. When the weight-average molecular weight of block (X) is within the above range, the crack resistance during molding tends to be better.

[0028] The aromatic saturated polybasic acid or its acid anhydride constituting block (X) is preferably one or more selected from the group consisting of aromatic saturated dibasic acids and their acid anhydrides, more preferably one or more selected from phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid, and even more preferably one or more selected from isophthalic acid and terephthalic acid.

[0029] As the aliphatic saturated polybasic acid constituting block (Y), an aliphatic saturated dibasic acid is preferred, an aliphatic saturated dibasic acid having 4 to 10 carbon atoms is more preferred, and one or more selected from succinic acid, adipic acid, and sebacic acid are even more preferred.

[0030] Preferred combinations of polyhydric alcohols and saturated polybasic acids include diols and saturated dibasic acids, and more preferably polyoxyalkylene glycols and saturated dibasic acids. More specifically, examples include combinations of diethylene glycol and isophthalic acid, diethylene glycol and adipic acid, dipropylene glycol and isophthalic acid, dipropylene glycol and adipic acid, diethylene glycol, isophthalic acid and adipic acid, dipropylene glycol, isophthalic acid and adipic acid, and diethylene glycol, dipropylene glycol, isophthalic acid and adipic acid. Among these, the combinations of diethylene glycol, isophthalic acid and adipic acid, dipropylene glycol, isophthalic acid and adipic acid, and diethylene glycol, dipropylene glycol, isophthalic acid and adipic acid are particularly preferred due to their excellent crack resistance during molding.

[0031] (A) The weight-average molecular weight of the saturated polyester resin is 8,500 or more and 15,000 or less. When the weight-average molecular weight is within the above range, crack formation during molding is suppressed. Although not bound by any theory, it is believed that setting the weight-average molecular weight of the saturated polyester resin (A) within the above range improves compatibility with the thermosetting resin (B) and dispersibility of components (C) to (G), thereby suppressing crack formation during molding. (A) The weight-average molecular weight of the saturated polyester resin is preferably 9,500 or more, more preferably 9,800 or more, and even more preferably 10,000 or more. (A) The weight-average molecular weight of the saturated polyester resin is preferably 13,500 or less, more preferably 13,000 or less, and even more preferably 12,500 or less. (A) The weight-average molecular weight of the saturated polyester resin can be adjusted, for example, by the reaction time, reaction temperature, and pressure conditions when synthesizing the saturated polyester resin (A). Specifically, the longer the reaction time, the larger the weight-average molecular weight, and the shorter the reaction time, the smaller the weight-average molecular weight. Increasing the reaction temperature tends to increase the weight-average molecular weight. Increasing the depressurization time or decreasing the pressure also tends to increase the weight-average molecular weight.

[0032] (A) When the weight-average molecular weight of the saturated polyester resin is 8,500 or more and less than 10,000, the acid value of the saturated polyester resin is 6.0 to 7.5 KOH mg / g, preferably 6.2 to 7.3 KOH mg / g, and more preferably 6.5 to 7.1 KOH mg / g. (A) When the weight-average molecular weight of the saturated polyester resin is 10,000 or more and less than 12,000, the acid value of the saturated polyester resin is 5.5 to 9.8 KOH mg / g, preferably 5.5 to 9.5 KOH mg / g, and more preferably 5.8 to 9.5 KOH mg / g. (A) When the weight-average molecular weight of the saturated polyester resin is 12,000 to 15,000, the acid value of the saturated polyester resin is 5.5 to 9.2 KOH mg / g, preferably 6.0 to 9.2 KOH mg / g, and more preferably 6.5 to 8.5 KOH mg / g.

[0033] The content of (A) saturated polyester resin in the thermosetting resin composition is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (A) saturated polyester resin in the thermosetting resin composition is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (A) saturated polyester resin in the thermosetting resin composition is preferably 5 to 30 parts by mass, more preferably 8 to 25 parts by mass, and even more preferably 10 to 20 parts by mass, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. If the content of (A) saturated polyester resin in the thermosetting resin composition is 5 parts by mass or more, there is a tendency to further reduce crack occurrence during molding. If the content of (A) saturated polyester resin in the thermosetting resin composition is 30 parts by mass or less, the moldability of the thermosetting resin composition and the mechanical properties of the cured product tend to be better.

[0034] ((A) Method for synthesizing saturated polyester resin) (A) Saturated polyester resin can be synthesized using the above raw materials by known methods. (A) Various conditions in the synthesis of saturated polyester resin are set appropriately according to the raw materials used and their amounts.

[0035] Generally, esterification reactions can be carried out in an inert gas stream such as nitrogen gas at a temperature of 140°C to 230°C. The progress of the esterification reaction can be adjusted by the pressure and reaction time. Specifically, when the reaction is carried out under reduced pressure, the reaction accelerates as water generated by dehydration condensation escapes from the system, and the weight-average molecular weight of (A) saturated polyester resin increases, while the acid value decreases. When the pressure conditions are returned from reduced pressure to atmospheric pressure, the esterification reaction stops. Therefore, by adjusting the reaction time under reduced pressure, a saturated polyester resin with the desired weight-average molecular weight and acid value can be obtained. The reaction under reduced pressure may be carried out all at once or in multiple stages. The balance between weight-average molecular weight and acid value may be monitored by sampling the reaction solution at atmospheric pressure. The greater the degree of reduced pressure, the easier the esterification reaction proceeds, and the weight-average molecular weight of (A) saturated polyester resin tends to increase. The longer the reaction time under reduced pressure, the greater the weight-average molecular weight of (A) saturated polyester resin tends to increase. In the esterification reaction, an esterification catalyst can be used as needed. Examples of esterification catalysts include known catalysts such as manganese acetate, dibutyltin oxide, stannous oxalate, zinc acetate, and cobalt acetate. Esterification catalysts may be used individually or in combination of two or more.

[0036] The equivalent amount of hydroxyl groups of the polyhydric alcohol relative to the total amount of carboxyl groups of the saturated polybasic acid is preferably in the range of 1.01 to 1.2, and more preferably in the range of 1.03 to 1.1. (A) The acid value of the saturated polyester resin can be adjusted, for example, by the equivalent amount of hydroxyl groups of the polyhydric alcohol relative to the total amount of carboxyl groups of the saturated polybasic acid. The higher the equivalent amount of hydroxyl groups relative to carboxyl groups, the lower the proportion of polymer chains whose terminals are carboxyl groups, and therefore the lower the acid value tends to be. (A) The weight-average molecular weight of the saturated polyester resin can be adjusted, for example, by the equivalent amount of hydroxyl groups of the polyhydric alcohol relative to the total amount of carboxyl groups of the saturated polybasic acid. The higher the equivalent amount of hydroxyl groups relative to carboxyl groups, the lower the weight-average molecular weight of the saturated polyester resin tends to be.

[0037] In one embodiment, the saturated polyester resin (A) comprises block (X), which is a polycondensate of a diol and an aromatic saturated polybasic acid or its acid anhydride, and block (Y), which is a polycondensate of a diol and an aliphatic saturated polybasic acid. Such a saturated polyester resin (A) can be obtained by first adding one of the saturated polybasic acids to the reaction vessel, allowing the esterification reaction to proceed until a certain amount of saturated polybasic acid has been consumed, then adding the other saturated polybasic acid to the reaction vessel and allowing the esterification reaction to proceed until the desired weight-average molecular weight is obtained. For example, a saturated polyester resin (A) comprising block (X) and block (Y) can be synthesized as follows: First, add the total amount of the aromatic saturated polybasic acid or its acid anhydride and the aliphatic saturated polybasic acid, plus an equivalent amount of diol, and the aromatic saturated polybasic acid or its acid anhydride, to the reaction vessel, allow the esterification reaction to proceed until a certain amount of aromatic saturated polybasic acid or its acid anhydride has been consumed, then add the aliphatic saturated polybasic acid to the reaction vessel and allow the esterification reaction to proceed.

[0038] The weight-average molecular weight of block (X) can be adjusted by the timing of the addition of the aliphatic saturated polybasic acid added later. For example, the acid value of the reaction solution, i.e., the remaining amount of the aromatic saturated polybasic acid or its acid anhydride added earlier, can be traced, and the aliphatic saturated polybasic acid can be added when the desired amount is reached. From the viewpoint of crack resistance, the acid value of the reaction solution at the time of addition of the aliphatic saturated polybasic acid is preferably 30 KOH mg / g or less, more preferably 20 KOH mg / g or less, and even more preferably 10 KOH mg / g or less. The acid value of the reaction solution at the time of addition of the aliphatic saturated polybasic acid may be 1 KOH mg / g or more, 3 KOH mg / g or more, or 5 KOH mg / g or more.

[0039] [(B) Thermosetting resin] (B) The thermosetting resin is not particularly limited as long as it is a thermosetting resin commonly used for sealing material applications. For example, a resin having functional groups that can form a crosslinked structure when heated and cured as a thermosetting resin composition is preferred. In particular, a resin having multiple ethylenically unsaturated groups as functional groups is preferred from the viewpoint that it can also react with (C) ethylenically unsaturated monomers.

[0040] (B) The weight-average molecular weight of the thermosetting resin is preferably 2,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more. (B) The weight-average molecular weight of the thermosetting resin is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 35,000 or less. When the weight-average molecular weight is within the above range, crack occurrence during molding tends to be further reduced. Although not bound by any theory, it is thought that setting the weight-average molecular weight of the thermosetting resin (B) within the above range improves compatibility with the saturated polyester resin (A) and dispersibility of components (C) to (G), thereby further reducing crack occurrence during molding. Note that the weight-average molecular weight of the thermosetting resin (B) refers to the weight-average molecular weight of the resin before curing.

[0041] (B)Specific examples of thermosetting resins include (B-1) unsaturated polyester resin, (B-2) vinyl ester resin, (B-3) urethane (meth)acrylate resin, (B-4) diallyl phthalate resin, and (B-5) epoxy resin. (B) From the viewpoint of moldability, fluidity, and curing shrinkage, it is preferable that the thermosetting resin contains at least (B-1) unsaturated polyester resin. (B) When the thermosetting resin contains (B-1) unsaturated polyester resin, interaction with calcium hydroxide used as a thickener (G) described later is at play, and it tends to be possible to obtain a thermosetting resin composition with better filling properties during molding. (B) The thermosetting resin may be used alone or in combination of two or more types.

[0042] The content of the thermosetting resin (B) in the thermosetting resin composition is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, based on 100 parts by mass of the total amount of the thermosetting resin (B) and the ethylenically unsaturated monomer (C). The content of the thermosetting resin (B) in the thermosetting resin composition is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less, based on 100 parts by mass of the total amount of the thermosetting resin (B) and the ethylenically unsaturated monomer (C). When the content of the thermosetting resin (B) in the thermosetting resin composition is 20 parts by mass or more, the mechanical strength of the cured product tends to be favorable. When the content of the thermosetting resin (B) in the thermosetting resin composition is 80 parts by mass or less, the viscosity of the thermosetting resin composition can be adjusted to an appropriate range, and the moldability tends to be favorable.

[0043] <(B-1) Unsaturated polyester resin> The (B-1) unsaturated polyester resin is a polycondensate of a polyhydric alcohol and an unsaturated polybasic acid, or a polycondensate of a polyhydric alcohol, an unsaturated polybasic acid and a saturated polybasic acid, and is not particularly limited. The (B-1) unsaturated polyester resin is preferably a polycondensate of a diol, an unsaturated polybasic acid and an optional saturated polybasic acid, more preferably a polycondensate of a diol containing propylene glycol, an unsaturated polybasic acid and an optional saturated polybasic acid, and even more preferably a polycondensate of a diol containing propylene glycol and neopentyl glycol, an unsaturated polybasic acid and an optional saturated polybasic acid.

[0044] The (B-1) unsaturated polyester resins may be used alone or in combination of two or more. By using the (B-1) unsaturated polyester resin, a cured product excellent in mechanical strength and heat resistance tends to be obtained.

[0045] In the present disclosure, reactive diluents such as styrene monomer contained in commercially available unsaturated polyester resins are classified as the ethylenically unsaturated monomer (C).

[0046] The polyhydric alcohol is not particularly limited as long as it is a compound having two or more hydroxyl groups. The polyhydric alcohol is preferably one or more selected from the group consisting of diols and triols, and more preferably a diol. Examples of polyhydric alcohols include alkylene glycols such as ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, and hydrogenated bisphenol A; polyoxyalkylene polyols such as diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol; bisphenol A; alkylene oxide-modified bisphenol A such as ethylene oxide adducts of bisphenol A and propylene oxide adducts of bisphenol A; and glycerin. From the viewpoint of crack resistance during molding, alkylene glycol is preferred, alkylene glycol having 2 to 6 carbon atoms is more preferred, one or more selected from ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, and neopentyl glycol are even more preferred, and propylene glycol is particularly preferred. From the viewpoint of improving the durability of the molded article, it is preferable to use propylene glycol and neopentyl glycol in combination. From the viewpoint of chemical resistance, it is preferable to use propylene glycol and hydrogenated bisphenol A in combination. Polyhydric alcohols may be used alone or in combination of two or more.

[0047] The unsaturated polybasic acid is not particularly limited as long as it is a compound having an ethylenically unsaturated bond and two or more carboxy groups, or an acid anhydride thereof, and known compounds can be used. In particular, unsaturated polybasic acids having 4 to 6 carbon atoms or acid anhydrides thereof are preferred because they are lower in cost and can provide a thermosetting resin composition that is more excellent in the mechanical strength and heat resistance of the cured product. The unsaturated polybasic acid is preferably an unsaturated dibasic acid. Examples of the unsaturated polybasic acid include maleic acid, maleic anhydride, fumaric acid, citraconic acid, itaconic acid, chloromaleic acid and the like. More preferably, it is one or more selected from fumaric acid, maleic acid, maleic anhydride, and itaconic acid. The unsaturated polybasic acids may be used alone or in combination of two or more thereof.

[0048] A preferred combination of the polyhydric alcohol and the unsaturated polybasic acid is a diol and an unsaturated dibasic acid, more preferably an alkylene glycol and an unsaturated dibasic acid having 4 to 6 carbon atoms. More specifically, for example, a combination of maleic anhydride, propylene glycol and neopentyl glycol, a combination of maleic anhydride and propylene glycol, a combination of fumaric acid and propylene glycol, a combination of maleic anhydride, propylene glycol, neopentyl glycol and hydrogenated bisphenol A, a combination of maleic anhydride, fumaric acid, propylene glycol, neopentyl glycol and hydrogenated bisphenol A, and the like can be mentioned. The combination of maleic anhydride, propylene glycol and neopentyl glycol, and the combination of maleic anhydride and propylene glycol are preferred because they are lower in cost and improve the crack resistance during molding and the durability of molded articles.

[0049] The saturated polybasic acid is not particularly limited as long as it is a compound or acid anhydride thereof that does not have an ethylenically unsaturated bond and has two or more carboxyl groups, and known compounds can be used. Examples of saturated polybasic acids include aromatic saturated polybasic acids or acid anhydrides thereof such as phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, tetrachlorophthalic anhydride, tetrabromophthalic anhydride, nitrophthalic acid, and halogenated phthalic anhydride; aliphatic saturated polybasic acids such as succinic acid, adipic acid, sebacic acid, oxalic acid, malonic acid, azelaic acid, and glutaric acid; and acid anhydrides of cyclic aliphatic saturated polybasic acids such as hexahydrophthalic anhydride. The saturated polybasic acid may be used alone or in combination of two or more types.

[0050] (B-1) The weight-average molecular weight of the unsaturated polyester resin is not particularly limited. (B-1) The weight-average molecular weight of the unsaturated polyester resin is preferably 2,000 to 50,000, more preferably 5,000 to 50,000, even more preferably 10,000 to 50,000, and particularly preferably 13,000 to 35,000. When the weight-average molecular weight is 2,000 to 50,000, the moldability of the thermosetting resin composition tends to be even better.

[0051] The degree of unsaturation of the (B-1) unsaturated polyester resin is preferably 50 to 100 mol%, more preferably 60 to 100 mol%, and even more preferably 70 to 100 mol%. When the degree of unsaturation is within the above range, the moldability of the thermosetting resin composition containing the (B-1) unsaturated polyester resin tends to be better.

[0052] (B-1) The degree of unsaturation of an unsaturated polyester resin is calculated using the following formula, based on the number of moles of unsaturated polybasic acid and saturated polybasic acid used as raw materials: Degree of unsaturation (mol%) = {(Number of moles of unsaturated polybasic acid × Number of ethylenically unsaturated bonds per molecule of unsaturated polybasic acid) / (Number of moles of unsaturated polybasic acid + Number of moles of saturated polybasic acid)} × 100

[0053] (Method for synthesizing (B-1) unsaturated polyester resin) (B-1) unsaturated polyester resin can be synthesized using the above raw materials by known methods. Various conditions in the synthesis of (B-1) unsaturated polyester resin are set appropriately according to the raw materials used and their amounts.

[0054] Generally, esterification reactions can be carried out under pressure or reduced pressure at a temperature of 140°C to 230°C in an inert gas stream such as nitrogen gas. Esterification catalysts can be used in the esterification reaction as needed. Examples of known esterification catalysts include manganese acetate, dibutyltin oxide, stannous oxalate, zinc acetate, and cobalt acetate. Esterification catalysts may be used alone or in combination of two or more.

[0055] To increase molecular weight by improving the reaction rate, it is preferable that the equivalent amount of hydroxyl groups of the polyhydric alcohol be in the range of 0.9 to 1.2 relative to the total amount of carboxyl groups of the unsaturated polybasic acid and any saturated polybasic acid.

[0056] (B) The content of (B-1) unsaturated polyester resin in the thermosetting resin is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the content of (B-1) unsaturated polyester resin is 75% by mass or more, the interaction with calcium hydroxide tends to increase, and appropriate moldability and fluidity can be ensured. (B) There is no particular upper limit to the content of (B-1) unsaturated polyester resin in the thermosetting resin. For example, it may be 100% by mass or less, 97% by mass or less, or 95% by mass or less.

[0057] <(B-2) Vinyl Ester Resin> (B-2) vinyl ester resin is generally a compound having an ethylenically unsaturated bond, obtained by a ring-opening reaction between (a) an epoxy group in an epoxy compound having two or more epoxy groups and (b) a carboxyl group of an unsaturated monobasic acid having an ethylenically unsaturated bond and a carboxyl group. (B-2) vinyl ester resin is described in, for example, the Polyester Resin Handbook (Nikkan Kogyo Shimbun, published in 1988).

[0058] (B-2) Vinyl ester resin may be used alone or in combination of two or more types. (B-2) Vinyl ester resin is generally used diluted with (C) ethylenically unsaturated monomer for ease of handling. By using (B-2) vinyl ester resin, the material cost of the thermosetting resin composition can be reduced.

[0059] (B-2) The weight-average molecular weight (Mw) of the vinyl ester resin can be adjusted according to the desired physical properties, but from a handling standpoint, a range of 500 to 5,000 is preferred.

[0060] (a) Epoxy compound (a) The epoxy compound is not particularly limited as long as it is a compound having two or more epoxy groups. Preferably, it is one or more selected from the group consisting of bisphenol-type epoxy compounds and novolacphenol-type epoxy compounds, and more preferably a bisphenol-type epoxy compound. (a) By using a vinyl ester resin that uses an epoxy compound as a raw material, the mechanical strength and corrosion resistance of the cured product tend to improve.

[0061] Examples of bisphenol-type epoxy compounds include those obtained by reacting bisphenol compounds such as bisphenol A, bisphenol F, bisphenol S, and tetrabromobisphenol A with epichlorohydrin and / or methylepichlorohydrin; and those obtained by reacting a compound obtained by glycidyl etherifying one or more of the above bisphenol compounds with a condensate of one or more of the above bisphenol compounds with epichlorohydrin and / or methylepichlorohydrin. From the viewpoint of durability, the reaction product of a bisphenol compound and epichlorohydrin is preferred, and the reaction product of bisphenol A and epichlorohydrin is more preferred.

[0062] Examples of novolac phenol-type epoxy compounds include those obtained by reacting phenol novolac or cresol novolac with epichlorohydrin and / or methyl epichlorohydrin.

[0063] (b) Unsaturated monobasic acid (b) The unsaturated monobasic acid is not particularly limited as long as it is a monocarboxylic acid having an ethylenically unsaturated bond. Preferably, it is methacrylic acid, acrylic acid, crotonic acid, cinnamic acid, etc., more preferably acrylic acid or methacrylic acid, and even more preferably methacrylic acid from the viewpoint of corrosion resistance of the cured product.

[0064] ((B-2) Method for synthesizing vinyl ester resin) (B-2) vinyl ester resin can be synthesized by known synthesis methods. For example, one method involves adding (b) an unsaturated monobasic acid in the presence of an esterification catalyst and (a) an epoxy compound in a heat-stirred reaction vessel and reacting at 70 to 150°C, preferably 80 to 140°C, and more preferably 90 to 130°C.

[0065] As esterification catalysts, known catalysts such as triethylamine, N,N-dimethylbenzylamine, N,N-dimethylaniline, diazabicyclooctane, triphenylphosphine, and diethylamine hydrochloride can be used.

[0066] (a) The mixing ratio of the epoxy compound and (b) the unsaturated monobasic acid is preferably such that the total amount of carboxyl groups of (b) the unsaturated monobasic acid is 0.3 to 1.2 moles, more preferably 0.4 to 1.1 moles, and even more preferably 0.5 to 1.0 moles, for every 1 mole of epoxy groups of (a) the epoxy compound. When the total amount of carboxyl groups of (b) the unsaturated monobasic acid is 0.3 moles or more, there is a tendency to obtain a cured product with sufficient hardness when the thermosetting resin composition is cured. On the other hand, when the total amount of carboxyl groups of (b) the unsaturated monobasic acid is 1.2 moles or less, the amount of unreacted (b) unsaturated monobasic acid can be reduced when synthesizing (B-2) vinyl ester resin, so there is a tendency to obtain a cured product with excellent mechanical strength.

[0067] When a thermosetting resin composition is heat-cured, unreacted (b) unsaturated monobasic acid may volatilize; therefore, the content of unreacted (b) unsaturated monobasic acid should be reduced as much as possible. For example, the content of unreacted (b) unsaturated monobasic acid relative to the total amount of (B-2) vinyl ester resin and unreacted (b) unsaturated monobasic acid is preferably 5% by mass or less, and more preferably 3% by mass or less.

[0068] (B) The content of (B-2) vinyl ester resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (B) There is no particular upper limit to the content of (B-2) vinyl ester resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.

[0069] <(B-3) Urethane (meth)acrylate resin> Examples of (B-3) urethane (meth)acrylate resins include resins obtained by introducing (meth)acryloyl groups to the hydroxyl groups or isocyanate groups at both ends of polyurethane obtained by reacting a polyhydric isocyanate with a polyhydric alcohol.

[0070] As the polyhydric alcohol, any of the compounds listed above as raw materials for (B-1) unsaturated polyester resins can be used without particular limitation.

[0071] Examples of polyvalent isocyanates include aliphatic polyvalent isocyanates such as hexamethylene diisocyanate, lysine diisocyanate, lysine triisocyanate, and trimethylhexane diisocyanate; cyclic aliphatic polyvalent isocyanates such as hydrogenated xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4 (or 2,6)-diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,3-(isocyanatomethyl)cyclohexane; aromatic polyvalent isocyanates such as tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, and triphenylmethane triisocyanate; and adducts, isocyanurates, and biuret derivatives of these polyvalent isocyanates. Polyvalent isocyanates may be used alone or in combination of two or more.

[0072] When introducing a (meth)acryloyl group, for example, a method can be used in which a hydroxyl group-containing (meth)acrylic compound is reacted with the terminal isocyanate group, or a method can be used in which an isocyanate group-containing (meth)acrylic compound such as 2-(meth)acryloyloxyethyl isocyanate, 2-(meth)acryloyloxypropyl isocyanate, or 1,1-bis(acryloyloxymethyl)ethyl isocyanate is reacted with the terminal hydroxyl group. Examples of hydroxyl group-containing (meth)acrylic compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxyalkyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, tris(hydroxyethyl)isocyanurate di(meth)acrylate, pentaestritol tri(meth)acrylate, glycerin mono(meth)acrylate, and hydroxyethyl acrylamide, with 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, caprolactone-modified hydroxyalkyl (meth)acrylate, and hydroxyethyl acrylamide being preferred. The isocyanate group-containing (meth)acrylic compounds and the hydroxyl group-containing (meth)acrylic compounds may be used individually or in combination of two or more.

[0073] (B) The content of (B-3) urethane (meth)acrylate resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (B) There is no particular upper limit to the content of (B-3) urethane (meth)acrylate resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.

[0074] <(B-4) Diallylphthalate Resin> (B-4) Diallylphthalate resin is an oligomer of diallylphthalate, and conventionally known types can be used without particular restriction. (B-4) Diallylphthalate resin may be used alone or in combination of two or more types.

[0075] (B) The content of (B-4) diallyl phthalate resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (B) There is no particular upper limit to the content of (B-4) diallyl phthalate resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.

[0076] <(B-5) Epoxy Resin> As the (B-5) epoxy resin, the compounds described in section (a) epoxy compounds of (B-2) vinyl ester resin can be used. The (B-5) epoxy resin may be used alone or in combination of two or more types.

[0077] (B) The content of (B-5) epoxy resin in the thermosetting resin may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. (B) There is no particular upper limit to the content of (B-5) epoxy resin in the thermosetting resin. For example, it may be 25% by mass or less, 20% by mass or less, or 10% by mass or less.

[0078] [(C) Ethylene-unsaturated monomers] (C) Ethylene-unsaturated monomers are not particularly limited as long as they are monomers having an ethylenically unsaturated bond. (C) Ethylene-unsaturated monomers may be used alone or in combination of two or more types.

[0079] Specifically, vinyl compounds such as styrene, vinyltoluene, t-butylstyrene, methoxystyrene, divinylbenzene, vinylnaphthalene; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, furfuryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate Examples of (meth)acrylates include acrylate, phenoxyethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, allyl (meth)acrylate, isobornyl (meth)acrylate, acetoacetoxyethyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecanol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.; cyclic unsaturated compounds such as acenaphthylene and norbornene are also included. (B) From the viewpoint of copolymerization with thermosetting resins, vinyl compounds are preferred, more preferably one or more selected from styrene, vinyltoluene, t-butylstyrene, and methoxystyrene, and even more preferably styrene.

[0080] The content of (C) ethylenically unsaturated monomer in the thermosetting resin composition is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (C) ethylenically unsaturated monomer in the thermosetting resin composition is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. When the content of (C) ethylenically unsaturated monomer in the thermosetting resin composition is 20 parts by mass or more, the viscosity of the thermosetting resin composition can be adjusted to an appropriate range and tends to have good moldability. When the content of (C) ethylenically unsaturated monomer in the thermosetting resin composition is 80 parts by mass or less, tends to have good mechanical strength of the cured product.

[0081] [(D) Thermal polymerization initiator] (D) The thermal polymerization initiator is not particularly limited as long as it is a polymerization initiator that generates radicals upon heating. Examples include organic peroxides such as diacyl peroxide, peroxyester, hydroperoxide, dialkyl peroxide, ketone peroxide, peroxyketal, alkyl perester, and parkervonate.

[0082] (D) Among these organic peroxides, 1,1-di-t-hexylperoxycyclohexane, t-hexylperoxyisopropyl carbonate, t-butylperoxyoctoate, t-butylperoxy-2-ethylhexanoate, t-hexylperoxy-2-ethylhexanoate, t-amylperoxy-2-ethylhexanoate, benzoyl peroxide, 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, t-butylperoxyisopropyl carbonate, t-butylperoxybenzoate, dicumyl peroxide, and di-t-butyl peroxide are preferred as thermal polymerization initiators. (D) The thermal polymerization initiators may be used alone or in combination of two or more.

[0083] The content of (D) thermal polymerization initiator in the thermosetting resin composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 3 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (D) thermal polymerization initiator in the thermosetting resin composition is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. When the content of (D) thermal polymerization initiator in the thermosetting resin composition is 0.5 parts by mass or more, the curing reaction during molding of the thermosetting resin composition tends to proceed uniformly, and the physical properties and appearance of the cured product tend to be good. When the content of (D) thermal polymerization initiator in the thermosetting resin composition is 20 parts by mass or less, the storage stability of the thermosetting resin composition tends to be good, and the handling properties tend to be improved.

[0084] [(E) Glass Fibers] (E) Glass fibers are not particularly limited as long as they are fibrous materials with an aspect ratio of 3 or more. Specifically, chopped strand glass is an example.

[0085] (E) The fiber length of the glass fibers is preferably 20 mm or less, more preferably 10 mm or less, and even more preferably 5 mm or less. When the fiber length is 20 mm or less, the moldability of the thermosetting resin composition tends to be good and the appearance of the cured product tends to be good. The fiber length is preferably 0.1 mm or more, more preferably 0.5 mm or more, and even more preferably 1 mm or more. When the fiber length is 0.1 mm or more, the strength of the cured product tends to be good. (E) The average fiber diameter of the glass fibers is preferably 3 to 100 μm, and more preferably 5 to 30 μm.

[0086] The content of (E) glass fibers in the thermosetting resin composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (E) glass fibers in the thermosetting resin composition is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 50 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. If the content of (E) glass fibers in the thermosetting resin composition is 5 parts by mass or more, the mechanical properties of the cured product obtained from the thermosetting resin composition tend to be better. If the content of (E) glass fibers in the thermosetting resin composition is 150 parts by mass or less, the (E) glass fibers tend to be more uniformly dispersed in the thermosetting resin composition, and a homogeneous cured product can be produced.

[0087] [(F) Inorganic filler] (F) As the inorganic filler, particulate matter known in the art of the present invention other than calcium hydroxide, magnesium hydroxide, and magnesium oxide can be used. (F) By using an inorganic filler, it is possible to reduce the absolute value of the molding shrinkage rate of the molded product, adjust the viscosity of the thermosetting resin composition to improve workability, or improve the strength of the molded product.

[0088] (F) Examples of inorganic fillers include calcium carbonate, silica, aluminum oxide, aluminum hydroxide, barium sulfate, calcium sulfate, calcium oxide, wollastonite, clay, kaolin, mica, gypsum, anhydrous silicic acid, and glass powder. Calcium carbonate, aluminum oxide, and aluminum hydroxide are preferred because they are inexpensive. (F) Inorganic fillers may be used individually or in combination of two or more.

[0089] (F) The average particle size of the inorganic filler is preferably 1 to 100 μm, more preferably 1 to 60 μm, and even more preferably 1 to 50 μm. (F) If the average particle size of the inorganic filler is 1 μm or more, particle aggregation tends to be suppressed. On the other hand, (F) if the average particle size of the inorganic filler is 100 μm or less, the moldability of the thermosetting resin composition tends to be good.

[0090] In this specification, "average particle size" refers to the 50% particle size (D50) in the volume-based cumulative particle size distribution measured by a laser diffraction / scattering particle size distribution analyzer (Microtrac-Bell Co., Ltd., FRA).

[0091] (F) The shape of the inorganic filler is not particularly limited. Examples include a nearly perfect sphere, ellipsoid, flake-like shape, amorphous shape, etc.

[0092] The content of (F) inorganic filler in the thermosetting resin composition is preferably 50 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 200 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (F) inorganic filler in the thermosetting resin composition is preferably 1000 parts by mass or less, more preferably 800 parts by mass or less, and even more preferably 500 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. If the content of (F) inorganic filler in the thermosetting resin composition is 50 parts by mass or more, the mechanical properties of the cured product tend to be better. If the content of (F) inorganic filler in the thermosetting resin composition is 1000 parts by mass or less, the (F) inorganic filler tends to be more uniformly dispersed in the thermosetting resin composition, and a homogeneous cured product can be produced.

[0093] [(G) Thickener] Calcium hydroxide is used as the (G) thickener. Although not bound by any particular theory, it is thought that calcium hydroxide interacts with (A) saturated polyester resin and affects the mobility of the polymer chains, thereby changing the viscosity of the resin composition and the dispersion state of (A) saturated polyester resin.

[0094] (G) The shape of the thickener is not particularly limited. Examples include a nearly spherical shape, ellipsoid, flaky shape, amorphous shape, etc.

[0095] The content of (G) thickener in the thermosetting resin composition is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.4 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (G) thickener in the thermosetting resin composition is preferably 9 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. When the content of (G) thickener in the thermosetting resin composition is within the above range, there is a good balance between the fluidity of the thermosetting resin composition and the shrinkage during molding, and the occurrence of cracks tends to be further reduced.

[0096] [(H) Other low-shrinkage agents] The thermosetting resin composition may optionally contain (H) other low-shrinkage agents other than saturated polyester resin. The (H) other low-shrinkage agents are not particularly limited and those known in the art of the present invention can be used. Thermoplastic resins are preferred as the (H) other low-shrinkage agents. Examples of (H) other low-shrinkage agents include polystyrene, polyethylene, polymethyl methacrylate, polyvinyl acetate, polycaprolactone, styrene-butadiene rubber, etc. Among these, polystyrene is preferred from the viewpoint of reducing the shrinkage rate of the cured product. The (H) other low-shrinkage agents may be used alone or in combination of two or more types.

[0097] The content of (H) other low-shrinkage agents in the thermosetting resin composition may be 1 part by mass or more, 3 parts by mass or more, or 5 parts by mass or more, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. The content of (H) other low-shrinkage agents in the thermosetting resin composition may be 30 parts by mass or less, 20 parts by mass or less, or 10 parts by mass or less, based on 100 parts by mass of the total amount of (B) thermosetting resin and (C) ethylenically unsaturated monomer. If the content of (H) other low-shrinkage agents in the thermosetting resin composition is 1 part by mass or more, the degree of shrinkage of the cured product tends to be smaller, and the desired dimensional accuracy can be obtained in the molded product. If the content of (H) other low-shrinkage agents in the thermosetting resin composition is 30 parts by mass or less, the moldability of the thermosetting resin composition and the mechanical properties of the cured product tend to be better.

[0098] [(I) Release Agent] The thermosetting resin composition may optionally contain (I) a release agent. The (I) release agent is not particularly limited and any known in the art of the present invention can be used. Examples of (I) release agents include stearic acid, oleic acid, zinc stearate, calcium stearate, aluminum stearate, magnesium stearate, stearate amide, oleic acid amide, silicone oil, synthetic wax, etc. The (I) release agent may be used alone or in combination of two or more types.

[0099] (I) When a release agent is used, the content is preferably 1 to 40 parts by mass, more preferably 5 to 30 parts by mass, and even more preferably 8 to 20 parts by mass, per 100 parts by mass of (B) thermosetting resin. (I) If the content of the release agent is 1 part by mass or more, the release properties of the cured product after molding tend to be good, and the productivity of the product tends to be good. On the other hand, (I) if the content of the release agent is 40 parts by mass or less, there is a tendency to be a cured product with a good appearance without excessive release agent contaminating the surface of the cured product.

[0100] [Other Additives] In addition to the above components, the thermosetting resin composition may contain components known in the art of the present invention, such as viscosity reducers, colorants, polymerization inhibitors, and molding aids, to the extent that they do not impede the effects of the present invention.

[0101] Colorants are used to color cured products, etc. Examples of colorants include various dyes, inorganic pigments, and organic pigments. Colorants may be used alone or in combination of two or more. The amount of colorant can be adjusted as appropriate depending on the desired degree of coloring of the cured product.

[0102] Examples of polymerization inhibitors include hydroquinone, trimethylhydroquinone, p-benzoquinone, naphthoquinone, t-butylhydroquinone, catechol, p-t-butylcatechol, and 2,6-di-t-butyl-4-methylphenol. Polymerization inhibitors may be used alone or in combination of two or more. The content of the polymerization inhibitor can be appropriately adjusted depending on the storage environment, storage period, curing conditions, etc., of the thermosetting resin composition.

[0103] <Method for producing thermosetting resin composition> A thermosetting resin composition can be produced by mixing (A) saturated polyester resin, (B) thermosetting resin, (C) ethylenically unsaturated monomer, (D) thermal polymerization initiator, (E) glass fiber, (F) inorganic filler, and (G) thickener, with optional components such as (H) other low-shrinkage agents, (I) mold release agents, and other additives as needed.

[0104] Mixing methods include, for example, kneading. There are no particular restrictions on the kneading method, and for example, a kneader, disper, planetary mixer, etc., can be used. The kneading temperature is preferably 5°C to 50°C, and more preferably 10°C to 40°C.

[0105] There are no particular restrictions on the order in which the components are mixed when manufacturing a thermosetting resin composition. For example, it is preferable to mix (B) the thermosetting resin and (C) some or all of the ethylenically unsaturated monomer before mixing the other components, as this makes it easier to obtain a thermosetting resin composition in which each component is sufficiently dispersed or uniformly mixed. At least a portion of (C) the ethylenically unsaturated monomer may be pre-mixed with (B) the thermosetting resin so as to act as a solvent, dispersion medium, etc.

[0106] <Cured Product> The cured product of one embodiment is a cured product of a thermosetting resin composition. The cured product can be used, for example, as a molding material to cover components of electronic components. Examples of electronic component components include stators, brackets, batteries, and sensors that make up a motor.

[0107] The cured product can be produced by heating and curing a thermosetting resin composition. The conditions for curing the thermosetting resin composition can be appropriately set depending on the materials used and the decomposition temperature of the (D) thermal polymerization initiator. An example of preferred conditions is a temperature of 120 to 180°C, more preferably 120 to 160°C, and a curing time of 1 to 30 minutes.

[0108] <Molded Article> The molded article of one embodiment includes a cured product of a thermosetting resin composition. A molded article including a cured product of a thermosetting resin composition can be produced by molding the thermosetting resin composition into a desired shape and heating it. The cured product of the thermoplastic resin composition may constitute the entirety of the molded article or only a part of it. The molding and curing method is not particularly limited, and methods commonly used in the art of the present invention, such as compression molding, transfer molding, and injection molding, can be used. An example of a molded article is a molded stator, which is a component of a motor.

[0109] <Motor> A motor is a device that generates an electromagnetic force by energizing an internal coil, and generates rotational force through the repulsive or attractive force between the motor and a permanent magnet or electromagnet provided on or around the main shaft. Generally, a motor comprises a stator having a stator core and coils wound around the stator core, and a rotating body containing magnetic components. In motors, those in which the stator is covered with a molding material are also called molded motors. In this specification, a stator covered with a molding material will be referred to as a molded stator.

[0110] A motor in one embodiment includes a molded stator; a rotor located inside the stator, having a rotating shaft extending in the axial direction and a rotating body containing a magnetic component that extends in the axial direction and is fixed to the rotating shaft; and a bearing that rotatably supports the rotor.

[0111] In one embodiment of the motor, the molding material constituting the molded stator is a cured product of a thermosetting resin composition. In the motor, components other than the molding material can be those of known origin.

[0112] Figure 1 shows a cross-sectional view of an exemplary motor. In Figure 1, detailed parts such as brackets and insulators attached to the coils are omitted. In Figure 1, the motor 10 has a stator 11, a rotor 15, and a bearing 19 that rotatably supports the rotor 15. The stator 11 has a stator core 12 made up of a plurality of metal plates and a coil 13 with windings wound around the stator core 12. The stator 11 is covered with a molding material 14. The rotor 15 is located inside the stator 11. The rotor 15 has a rotating shaft 17 extending in the axial direction and a rotating body 18 fixed to this rotating shaft 17, and this rotating body 18 includes a magnet 16.

[0113] <Molded Stator> A molded stator according to one embodiment includes a stator having a stator core and coils wound around the stator core, and a molding material covering the stator. It is not necessary for the entire stator to be covered with the molding material.

[0114] In one embodiment, the molding material constituting the molded stator is a cured product of a thermosetting resin composition. In the molded stator, components other than the molding material can be those of known origin. The motor to which the molded stator is applied is not particularly limited and can be any known motor.

[0115] <Method for Manufacturing a Molded Stator> A molded stator can be manufactured, for example, by injecting a thermosetting resin composition into a mold in which the stator is positioned and heating it. The molding method is not particularly limited and can be any method commonly used in the art of the present invention, such as transfer molding and injection molding.

[0116] More specific methods for manufacturing molded stators include, for example, opening the mold, pouring a thermosetting resin composition into the mold containing the stator, and allowing it to harden; and injecting a thermosetting resin composition from the outside into a closed mold containing the stator through a hole in the mold, such as a sprue, under reduced pressure inside the mold, or under external pressure as in injection molding, and allowing it to harden. The conditions for hardening the thermosetting resin composition inside the mold can be appropriately set depending on the material used. An example of preferred conditions is a temperature of 120 to 180°C, more preferably 120 to 160°C, and a hardening time of 1 to 30 minutes.

[0117] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0118] The following are examples of the synthesis of saturated polyester resin (A) used in the example and saturated polyester resin (cA) used in the comparative example.

[0119] The following raw materials were used: Diols: Diethylene glycol (Fujifilm Wako Pure Chemical Corporation), Dipropylene glycol (Fujifilm Wako Pure Chemical Corporation) Saturated polybasic acids: Isophthalic acid (Fujifilm Wako Pure Chemical Corporation), Adipic acid (Fujifilm Wako Pure Chemical Corporation)

[0120] [Synthesis Example 1] In a four-necked flask equipped with a thermometer, stirrer, inert gas inlet, and reflux condenser, 50 moles of isophthalic acid, 70 moles of diethylene glycol, and 40 moles of dipropylene glycol were charged. The esterification reaction was carried out at atmospheric pressure for 1 hour after heating and stirring under a nitrogen gas stream to 210°C. When the acid value of the reaction solution fell below 10 KOH mg / g, the mixture was cooled and 50 moles of adipic acid were added. The mixture was then heated again to 210°C and carried out at atmospheric pressure for 6 hours, followed by 7.3 hours under reduced pressure of -0.97 MPaG to obtain a saturated polyester resin. Subsequently, when the acid value of the reaction solution reached 5.8 KOH mg / g, the reaction system was returned to atmospheric pressure, and styrene monomer was added to a total of 35% by mass relative to the total of the saturated polyester resin and styrene monomer to obtain a mixture of saturated polyester resin and styrene. The obtained saturated polyester resin had a weight-average molecular weight (Mw) of 11,147. The weight-average molecular weight (Mw) of the obtained saturated polyester resin block (X) was 4,000.

[0121]

[0122] [Synthesis Examples 2-27, Comparative Synthesis Examples 1-19] Using the compositions in Table 1, a mixture of saturated polyester resin and styrene was obtained in the same manner as in Synthesis Example 1, except that the reaction time under reduced pressure was changed as shown in Table 1. The weight-average molecular weight (Mw) and acid value of the saturated polyester resin are shown in Table 1.

[0123] (B) Examples of thermosetting resin synthesis are shown below.

[0124] The following raw materials were used: Diols: Propylene glycol (Fujifilm Wako Pure Chemical Corporation), Neopentyl glycol (Fujifilm Wako Pure Chemical Corporation) Unsaturated polybasic acid: Maleic anhydride (Fujifilm Wako Pure Chemical Corporation)

[0125] [Synthesis Example 28] (B) Synthesis of Thermosetting Resin In a four-necked flask equipped with a thermometer, stirrer, inert gas inlet, and reflux condenser, 100 moles of maleic anhydride, 60 moles of propylene glycol, and 40 moles of neopentyl glycol were charged. The mixture was heated and stirred under a nitrogen gas stream and the temperature was raised to 210°C to carry out an esterification reaction to obtain an unsaturated polyester resin. Subsequently, styrene monomer was added to the total amount of the unsaturated polyester resin and styrene monomer to 40% by mass to obtain a mixture of unsaturated polyester resin and styrene. The obtained unsaturated polyester resin had a degree of unsaturation of 100 mol% and a weight-average molecular weight (Mw) of 20,000.

[0126]

[0127] Other ingredients used include the following:

[0128] (C) Ethylene-unsaturated monomers: Styrene (Idemitsu Kosan Co., Ltd.)

[0129] (D) Thermal polymerization initiator: Perhexyl I (t-hexylperoxyisopropyl carbonate, NOF Corporation)

[0130] (E) Glass fiber: Chopped strand ECS-03B173 / P9 (glass chop, fiber diameter 13 μm, fiber length 3.0 mm, Nippon Electric Glass Co., Ltd.)

[0131] (F) Inorganic filler: Softon 1200 (calcium carbonate, average particle size 1.80 μm, Bihoku Powdering Industry Co., Ltd.)

[0132] (G) Thickening agent: Calcium hydroxide (Kishida Chemical Co., Ltd.)

[0133] (H) Other low-shrinkage agents: Polystyrene (PS MS-200, Sekisui Chemical Co., Ltd.)

[0134] <Example 1> (Preparation of thermosetting resin composition) (A) saturated polyester resin and (C) ethylenically unsaturated monomer: 25 parts by mass of a mixture of saturated polyester resin and styrene obtained in Synthesis Example 1 (16 parts by mass of saturated polyester resin, 9 parts by mass of styrene), (B) thermosetting resin and (C) ethylenically unsaturated monomer: 82 parts by mass of a mixture of unsaturated polyester resin and styrene obtained in Synthesis Example 28 (49 parts by mass of unsaturated polyester resin, 33 parts by mass of styrene), (C) further 8 parts by mass of styrene as ethylenically unsaturated monomer, (D) 4 parts by mass of perhexyl I as a thermal polymerization initiator, (E) 36 parts by mass of chopped strand ECS-03B173 / P9 as glass fiber, (F) 390 parts by mass of Softon 1200 as an inorganic filler, (G) 0.4 parts by mass of calcium hydroxide as a thickener, and (H) 6 parts by mass of polystyrene as an additional low-shrinkage agent were put into a double-arm kneader and kneaded at 30°C for 30 minutes to prepare a thermosetting resin composition.

[0135] (Molding Shrinkage Rate) In accordance with JIS K-6911 (2006) 5.7, the molding shrinkage rate was calculated by compression molding of disc-shaped test specimens (φ90 mm × 11 mm) using a compression molding machine (Techno Marushichi Co., Ltd.) under the conditions of a molding temperature of 120°C, a molding pressure of 5 MPa, and a molding time of 3 minutes. The test specimens were made using a thermosetting resin composition immediately after mixing. The results are shown in Table 3.

[0136] (Preparation of molded stators) A stator was placed in a mold, and a thermosetting resin composition immediately after mixing was injected. Molding was performed at a molding temperature of 125°C, a molding pressure of 5 MPa, and a molding time of 5 minutes to obtain a molded stator. The appearance of the molded stator was evaluated from the standpoint of cracks according to the following criteria. The results are shown in Table 3. The appearance of the molded stator was observed visually, and those without cracks were classified as good, while those with cracks were classified as poor.

[0137]

[0138] <Examples 2-27> Thermosetting resin compositions were prepared in the same manner as in Example 1, except that the type of saturated polyester resin (A) was changed as shown in Table 3. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 3. <Comparative Examples 1-19> Thermosetting resin compositions were prepared in the same manner as in Example 1, except that the saturated polyester resin (cA) shown in Table 3 was used instead of the saturated polyester resin (A). Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 3.

[0139] Figure 2 plots the acid value and weight-average molecular weight of (A) saturated polyester resin and (cA) saturated polyester resin used in the examples and comparative examples. As shown in Table 3 and Figure 2, by using saturated polyester resin having a specific acid value corresponding to the weight-average molecular weight, it was possible to reduce the molding shrinkage rate of the cured product of the thermosetting resin composition to 0% or less. Since such thermosetting resin compositions are less prone to molding defects due to shrinkage, the occurrence of cracks in molded products can be reduced.

[0140] 10 Motor 11 Stator 12 Stator core 13 Coil 14 Molding material 15 Rotor 16 Magnet 17 Rotating shaft 18 Rotating body 19 Bearing

Claims

1. A thermosetting resin composition comprising (A) a saturated polyester resin, (B) a thermosetting resin, (C) an ethylenically unsaturated monomer, (D) a thermal polymerization initiator, (E) glass fibers, (F) an inorganic filler, and (G) a thickener, wherein the thickener (G) is calcium hydroxide, the weight-average molecular weight of the saturated polyester resin (A) is 8500 to 15000, and when the weight-average molecular weight of the saturated polyester resin (A) is 8500 or more and less than 10000, the acid value of the saturated polyester resin (A) is 6.0 to 7.5 KOH mg / g; when the weight-average molecular weight of the saturated polyester resin (A) is 10000 or more and less than 12000, the acid value of the saturated polyester resin (A) is 5.5 to 9.8 KOH mg / g; A thermosetting resin composition wherein, when the weight-average molecular weight of the saturated polyester resin (A) is 12,000 to 15,000, the acid value of the saturated polyester resin (A) is 5.5 to 9.2 KOH mg / g.

2. The thermosetting resin composition according to claim 1, wherein the content of the thickener (G) is 0.2 to 9 parts by mass, based on 100 parts by mass of the total amount of the thermosetting resin (B) and the ethylenically unsaturated monomer (C).

3. The thermosetting resin composition according to claim 1 or 2, wherein the saturated polyester resin (A) is a polycondensate of a diol and a saturated polybasic acid, and the saturated polybasic acid contains an aromatic saturated polybasic acid or its acid anhydride and an aliphatic saturated polybasic acid.

4. The thermosetting resin composition according to claim 3, wherein the ratio (molar ratio) of the structure derived from the aromatic saturated polybasic acid or its acid anhydride to the structure derived from the aliphatic saturated polybasic acid in the saturated polyester resin (A) is 20:80 to 80:

20.

5. The thermosetting resin composition according to claim 3, wherein the aromatic saturated polybasic acid is one or more selected from isophthalic acid and terephthalic acid.

6. The thermosetting resin composition according to claim 1 or 2, wherein the (B) thermosetting resin comprises at least (B-1) unsaturated polyester resin.

7. The thermosetting resin composition according to claim 6, wherein the weight-average molecular weight of the (B-1) unsaturated polyester resin is 10,000 to 50,000.

8. The thermosetting resin composition according to claim 1 or 2, wherein the total amount of the (B) thermosetting resin and the (C) ethylenically unsaturated monomer is 100 parts by mass, and the composition contains 5 to 30 parts by mass of the (A) saturated polyester resin, 20 to 80 parts by mass of the (B) thermosetting resin, 20 to 80 parts by mass of the (C) ethylenically unsaturated monomer, 0.5 to 20 parts by mass of the (D) thermal polymerization initiator, 5 to 150 parts by mass of the (E) glass fiber, and 50 to 1000 parts by mass of the (F) inorganic filler.

9. A cured product of the thermosetting resin composition according to claim 1 or 2.

10. A molded article comprising a cured product of the thermosetting resin composition described in claim 8.