Tape for fixing electrode body of lithium ion battery, and lithium ion battery using same

A styrene-based resin film with a specific composition and thickness, combined with a suitable adhesive, addresses the challenge of achieving both shock resistance and high energy density in lithium-ion batteries by ensuring effective swelling and adherence to the electrode, enhancing both impact resistance and energy density.

WO2026240204A1PCT designated stage Publication Date: 2026-11-19ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/018485
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-15
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing electrode fixing tapes in lithium-ion batteries do not adequately address the need for both shock resistance and high energy density per unit weight, as they often compromise energy density when designed for impact resistance, and vice versa.

Method used

A styrene-based resin film with a specific composition and thickness, combined with a suitable adhesive layer, is used to create an electrode fixing tape that swells effectively in the presence of a specific electrolyte composition, maintaining mechanical strength and adhering tightly to the electrode and outer casing, thereby enhancing both impact resistance and energy density.

Benefits of technology

The proposed tape achieves both high impact resistance and increased energy density per unit weight by ensuring the tape swells sufficiently to fill the gap between the electrode and casing while maintaining mechanical integrity, preventing electrode displacement during impacts and vibrations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide a tape for fixing an electrode body of a lithium ion battery, which is capable of achieving both high impact resistance and high energy density per unit weight of a lithium ion battery, and a lithium ion battery that uses this tape. According to the present disclosure, a tape for fixing an electrode body is provided, the tape being used in a lithium ion battery. An electrolytic solution of the lithium ion battery contains 10-30% by weight of a cyclic carbonate and 50-70% by weight of a chain carbonate per 100% by weight of the electrolytic solution. The tape for fixing an electrode body has a styrene-based resin film and an adhesive layer. The thickness of the styrene-based resin film is 10-25 μm, and the constituent ratio of styrene monomers in the total resin constituting the styrene-based resin film is 85% by weight or more and less than 97% by weight.
Need to check novelty before this filing date? Find Prior Art

Description

Tape for fixing electrodes of lithium-ion batteries, and lithium-ion batteries using the same

[0001] This disclosure relates to a tape for fixing electrodes in lithium-ion batteries, and to a lithium-ion battery using the same.

[0002] Lithium-ion batteries (hereinafter also simply referred to as "LIBs") are widely used in electronic devices such as mobile phones, smartphones, notebook PCs, and cordless appliances, as well as batteries for electric vehicles, due to their ability to be repeatedly charged and discharged and their higher energy density per unit weight compared to other secondary batteries. An LIB mainly consists of an electrode body with a porous separator placed between a positive electrode plate and a negative electrode plate, and an outer casing that houses both the electrode body and the electrolyte.

[0003] If the electrodes of an LIB (lithographic beam) can move inside the casing due to impacts such as dropping or vibration, there is a risk of deformation or short-circuiting of the electrodes. Therefore, in order to resolve these problems, a tape (hereinafter also referred to as "electrode fixing tape" or simply "fixing tape") has been proposed to prevent the electrodes from easily moving inside the casing.

[0004] The fixing tape is required to prevent the winding from unwinding or the electrode from shifting due to vibration or impact from dropping. Typically, the tape is provided on at least a portion of the outer surface of the electrode. When the electrode and electrolyte are housed in the outer casing, there is a gap between the casing and the electrode. Over time, the fixing tape swells due to the electrolyte, filling the gap and creating a tight seal, thus preventing the electrode from shifting. To achieve both ease of storage and resistance to vibration and impact from dropping, fixing tapes made of materials that swell easily upon contact with the electrolyte have been proposed.

[0005] As an example of a fixing tape, Patent Document 1 discloses a fixing tape consisting of a single-layer or multi-layer film made of a specific ratio of vinylidene fluoride resin and aromatic polyester resin.

[0006] Patent document 2 discloses a fixing tape using stretched polystyrene film (OPS film).

[0007] In recent years, with the improvement of smartphone performance and the spread of electric vehicles, there has been a demand for increased energy density per unit weight of lithium-ion batteries (LIBs). Since the fixing tape of LIBs does not contribute to improving the energy density of the battery, making the fixing tape thinner can relatively increase the electrode area, thus improving energy density. However, simply making the tape thinner, if it has the same swelling capacity, will reduce its effect in filling the gap between the outer casing and the electrode body, so a greater swelling capacity than before is required.

[0008] International Publication No. 2009 / 139388, Japanese Patent Publication No. 2011-243553, Japanese Patent Publication No. 2011-202064

[0009] Charles M. Hansen, "Hansen Solubility Parameters: A User's Handbook" (USA), 2nd edition, CRC Press, June 15, 2007.

[0010] This disclosure aims to provide a tape for fixing electrodes in lithium-ion batteries, and a lithium-ion battery using the same, which can achieve both shock resistance and high energy density per unit weight in lithium-ion batteries.

[0011] Examples of embodiments of the present disclosure are listed in the following items [1] to

[15] . [1] An electrode fixing tape used in a lithium-ion battery, wherein the electrolyte of the lithium-ion battery contains at least 10% to 30% by weight of cyclic carbonate and 50 to 70% by weight of chain carbonate, based on 100% by weight of the electrolyte, the electrode fixing tape comprises a styrene resin film and an adhesive layer, the thickness of the styrene resin film is 10 to 25 μm, and the styrene monomer composition ratio to the total weight of all resin components constituting the styrene resin film is in the range of 85% to less than 97% by weight. [2] The electrode fixing tape according to item 1, wherein the product of the MD direction stretching ratio and the TD direction stretching ratio of the styrene resin film is in the range of 2 to 25. [3] The electrode fixing tape according to item 1 or 2, wherein the ratio of the stretching ratio in the MD direction to the stretching ratio in the TD direction (MD / TD) is in the range of 0.5 to 1.5. [4] The HSP value of the entire electrolyte is approximately 20.0 to 25.0 (J / cm²). 3 ) 1/2 Furthermore, the HSP value of the styrene resin film is 17.0 to 19.5 (J / cm²). 3 ) 1/2[5] The electrode fixing tape according to any one of items 1 to 3, wherein the electrolyte of the lithium-ion battery contains 15 to 25% by weight of cyclic carbonate and 50 to 70% by weight of chain carbonate, wherein the electrode fixing tape according to any one of items 1 to 4, wherein the styrene resin film contains a branched styrene resin, wherein the electrode fixing tape according to any one of items 1 to 5, wherein the styrene resin film has linear polystyrene and branched polystyrene, and the ratio of the linear polystyrene to the branched polystyrene is in the range of 99.5:0.5 to 70:30, wherein the electrode fixing tape according to any one of items 1 to 6, wherein the styrene resin film has linear polystyrene and branched polystyrene, and the ratio of the linear polystyrene to the branched polystyrene is in the range of 99.5:0.5 to 70:30, wherein the electrode fixing tape according to any one of items 1 to 6. [8] The electrode fixing tape according to any one of items 1 to 7, wherein the styrene resin film has at least one impact-resistant polystyrene selected from the group consisting of styrene-butadiene copolymer (SB resin), high-impact polystyrene (HIPS), and styrene-butadiene-styrene resin (SBS resin). [9] A lithium-ion battery comprising an outer casing, an electrode body and an electrolyte housed within the outer casing, wherein the electrolyte contains 10% to 30% by weight of cyclic carbonate and 50 to 70% by weight of chain carbonate, and the lithium-ion battery is provided with the electrode fixing tape according to any one of items 1 to 8 between the outer casing and the electrode body.

[10] The HSP value of the entire electrolyte is approximately 20.0 to 25.0 (J / cm²). 3 ) 1/2 Furthermore, the HSP value of the styrene resin film is 17.0 to 19.5 (J / cm²). 3 ) 1/2

[11] A lithium-ion battery according to item 9, wherein the difference between the HSP value of the entire electrolyte and the HSP value of the styrene resin film is in the range of 2.3 to 3.6.

[12] A lithium-ion battery according to any one of items 9 to 11, wherein the electrolyte of the lithium-ion battery contains 15 to 25% by weight of cyclic carbonate and 50 to 70% by weight of chain carbonate.

[13] A lithium-ion battery according to any one of items 9 to 12, wherein the styrene resin film contains a branched styrene resin.

[14] A lithium-ion battery according to any one of items 9 to 13, wherein the styrene resin film has linear polystyrene and branched polystyrene, and the ratio of the linear polystyrene to the branched polystyrene is in the range of 99.5:0.5 to 70:30.

[15] The lithium-ion battery according to any one of items 9 to 14, wherein the styrene-based resin film has at least one impact-resistant polystyrene selected from the group consisting of styrene-butadiene copolymer (SB resin), high-impact polystyrene (HIPS), and styrene-butadiene-styrene resin (SBS resin).

[0012] According to this disclosure, it is possible to provide a tape for fixing electrodes of a lithium-ion battery, and a lithium-ion battery using the same, which can achieve both shock resistance and high energy density per unit weight of the lithium-ion battery.

[0013] An embodiment of this disclosure will be described in detail below, but the scope of this disclosure is not limited to the embodiment described herein, and various modifications can be made without departing from the spirit of this disclosure. Furthermore, if multiple upper and lower limits are given for a numerical range, any combination of these upper and lower limits can be used to create a suitable numerical range.

[0014] 《Electrode Fixing Tape》 The electrode fixing tape of this disclosure is an electrode fixing tape used in a lithium-ion battery, the lithium-ion battery comprising at least 10% to 30% by weight of cyclic carbonate and 50 to 70% by weight of chain-like carbonate per 100% by weight of the electrolyte. The tape comprises a styrene-based resin film and an adhesive layer. The thickness of the styrene-based resin film is 10 to 25 μm, and the styrene monomer content ratio in the total resin constituting the styrene-based resin film is in the range of 85% to less than 97% by weight. With the above configuration, a lithium-ion battery equipped with the electrode fixing tape of this disclosure can achieve both impact resistance and high energy density per unit weight. The reason for this is as follows, although not limited to theory. Typically, as a carbonate-based electrolyte, a mixed solvent of chain-like carbonate and cyclic carbonate has been used as the main component from the viewpoint of electrolyte solubility and fluidity. Furthermore, styrene-based resins have high compatibility with carbonate-based electrolytes and are prone to swelling. The inventors' investigations revealed that when the styrene monomer content of a styrene-based resin film is high, and the film thickness is reduced to 10-25 μm, it can be difficult to prevent electrode displacement in the event of impact. This is partly because, firstly, the chain-like carbonates dissolve the thin styrene-based resin film, causing peeling of the tape and a decrease in mechanical strength. Secondly, because the reduced thickness results in weaker adhesion between the outer casing and the electrode, preventing displacement. Therefore, the inventors used a styrene-based resin film with a specific styrene monomer content in an electrolyte of a specific composition. Specifically, we found that by using an electrolyte containing 50-70% by weight of linear carbonate and 10% to 30% by weight of cyclic carbonate, and adjusting the styrene monomer composition ratio to the total weight of the resin components of the styrene resin film to 85% to less than 97% by weight, high swelling properties can be obtained without dissolution even when the film is thin, and mechanical strength can be maintained to a certain extent.Therefore, the electrode fixing tape of this disclosure can enhance the impact resistance of lithium-ion batteries due to its high swelling properties even when thin, and its thinness can increase the energy density per unit weight. The effects provided by this disclosure are surprising because, until now, attention had not been paid to the swelling characteristics of styrene resin films in relation to the electrolyte composition, nor to the differences in compatibility between cyclic carbonates and chain carbonates in the electrolyte with styrene resins.

[0015] <Styrene-based resin film> The styrene-based resin film serves as a base material for the electrode fixing tape. The styrene monomer content ratio in the total resin constituting the styrene-based resin film is 85% by weight or more and less than 97% by weight. Preferably, the styrene monomer content ratio is 87% by weight or more, 89% by weight or more, or 91% by weight or more. The upper limit of the styrene monomer content ratio that can be arbitrarily combined with these lower limits may be, for example, less than 95% by weight, 93% by weight or less, or 92% by weight or less. When the styrene monomer content ratio is within these ranges, it swells well in a specific ratio of carbonate-based electrolyte, and even if it is thin, it can adhere tightly to the electrode and the outer casing, thus providing excellent impact resistance. In addition, a relatively high styrene monomer content ratio tends to further reduce thickness unevenness when thinning the film.

[0016] As materials for styrene-based resin films, styrene-based resins, that is, homopolymers of styrene-based monomers (styrene monomers or styrene derivatives), or copolymers of styrene-based monomers and other monomers can be used.

[0017] As a homopolymer of styrene monomers, a homopolymer of styrene, such as general-purpose polystyrene (GPPS), can be used. Examples of styrene derivatives include alkyl-substituted styrenes such as methylstyrene, α-methylstyrene, and p-methylstyrene; and halogen-substituted styrenes such as bromostyrene, α-bromostyrene, chlorostyrene, and p-chlorostyrene.

[0018] Other monomers copolymerizable with styrene monomers include unsaturated aliphatic carboxylic acids, unsaturated aliphatic carboxylic acid esters, acid anhydrides, conjugated dienes, vinyl compounds, nitrile compounds, unsaturated amide compounds, and imide / maleimide compounds. Examples of unsaturated aliphatic carboxylic acids include carboxylic acid compounds having 1 to 12 carbon atoms and an unsaturated aliphatic group, such as (meth)acrylic acid, crotonic acid, and fumaric acid. Examples of unsaturated aliphatic carboxylic acid esters include esters of the above unsaturated aliphatic carboxylic acids with alkyl alcohols having 1 to 12 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, as well as esters of the above unsaturated aliphatic carboxylic acids with alkylene oxides. In this disclosure, "(meth)acrylic" means acrylic or the corresponding methacrylic. Examples of acid anhydrides include maleic anhydride, itaconic anhydride, and citraconic anhydride. Examples of conjugated dienes include butadiene and isoprene. Examples of vinyl compounds include vinyl chloride, allyl chloride, and vinyl acetate (VAc). Examples of nitrile compounds include acrylonitrile (AN) and methacrylonitrile. Examples of unsaturated amide compounds include acrylamide and N-methylacrylamide. Examples of imide / maleimide compounds include N-phenylmaleimide and N-methylmaleimide. These other monomers may be used individually or in combination of two or more.

[0019] The other monomers copolymerizable with the aforementioned styrenic monomer can be appropriately selected from the viewpoints of ease of thinning of the styrenic resin film, swelling characteristics, impact resistance, and the like. For example, copolymerization such as a copolymer of styrene and (meth)acrylic acid tends to increase the HSP value as compared with a styrene homopolymer. Copolymers of styrene and conjugated dienes and the like tend to decrease the HSP value as compared with a styrene homopolymer. In addition, copolymers with monomers that impart flexibility to the molecular chain, such as copolymers of styrene and conjugated dienes, tend to be easier to thin and more excellent in impact resistance as compared with styrene homopolymers.

[0020] Preferable examples of the copolymer of a styrenic monomer and another monomer include styrene-(meth)acrylic acid copolymers, styrene-(meth)acrylate copolymers, styrene-acid anhydride copolymers, and terpolymer resins obtained by adding a further monomer component, for example, an ester component, to the monomer components of these copolymers; at least one impact-resistant polystyrene such as styrene-butadiene copolymer (SB resin) and styrene-butadiene-styrene resin (SBS resin); and well-known copolymer resins such as styrene-α-methylstyrene copolymers.

[0021] The styrenic resin film may be an alloy (resin composition) of a styrenic resin and another resin as long as it satisfies the aforementioned constituent ratio of the styrene monomer. By alloying the styrenic resin with another resin, the stability during film formation is improved, and it can be expected that thinning of the film becomes easier. Examples of the alloy of a styrenic resin and another resin include a polymer alloy of polystyrene and a polyphenylene ether resin (m-PPE), and a polymer alloy of polystyrene and butadiene rubber, such as high impact polystyrene (HIPS).

[0022] Preferable copolymers or alloys as materials for the styrene-based resin film include at least one impact-resistant polystyrene selected from the group consisting of styrene-butadiene copolymer (SB resin), high-impact polystyrene (HIPS), and styrene-butadiene-styrene-based resin (SBS resin). These materials are easier to form into thin films, and when used in a LIB that contains at least 10 wt% or more and 30 wt% or less of a cyclic carbonate and 50 to 70 wt% of a chain carbonate as an electrolytic solution, they have high swellability in the electrolytic solution and high mechanical strength after swelling, so that the impact resistance can be further improved.

[0023] The styrene-based resin may have a linear structure without branches (also referred to as "linear styrene-based resin" in the present disclosure), or may have a multi-branched structure (also referred to as "multi-branched styrene-based resin" in the present disclosure). The styrene-based resin preferably contains a multi-branched styrene-based resin. Since the multi-branched styrene-based resin has improved mechanical strength due to entanglement of molecular chains, it is easier to form into a thin film. Examples of the branched structure generally include a random branched structure, a star structure, and a pom-pom structure.

[0024] Examples of methods for introducing branches into the styrene-based resin include a method using an organic peroxide, a method using a polyfunctional monomer, a method by ionic crosslinking, and a method using a multi-branched macromonomer. Among these methods, by using a multi-branched macromonomer, a styrene-based resin having a molecular structure in which a star structure and a pom-pom structure coexist can be obtained. The method using a multi-branched macromonomer is preferable from the viewpoints of gelation suppression, film extrudability, and film formation stability.

[0025] When a multi-branched macromonomer is used, for the synthesis of multi-branched polystyrene, in addition to the styrenic monomer and the multi-branched macromonomer, other monomers having an aliphatic unsaturated bond that is optionally copolymerizable with the styrenic monomer can be used. As the other monomers, those described above can be used, and from the viewpoints of ease of thin film formation, swelling property, impact resistance and the like, an unsaturated aliphatic carboxylic acid ester is preferred, for example. The multi-branched macromonomer can be obtained by the method described in Patent Document 3 (Japanese Unexamined Patent Publication No. 2011-202064), for example. The "multi-branched polystyrene" is a polystyrene having a multi-branched structure, and is an example of the "multi-branched styrenic resin".

[0026] Examples of the multi-branched macromonomer include macromonomers obtained by introducing a (meth)acrylic group into a dendrimer, a hyperbranched polymer, or a multi-branched polyether polyol. Also, AB having an active methylene group in one molecule and a leaving group such as bromine, chlorine, methylsulfonyloxy group or tosyloxy group 2 A self-condensation type multi-branched polymer (polycondensate) can be obtained by subjecting a type monomer to a nucleophilic substitution reaction. Using this polycondensate as a precursor, a polymerizable double bond can be introduced through a nucleophilic substitution reaction between the unreacted active methylene group or methine group remaining in the polycondensate and chloromethylstyrene, bromomethylstyrene or the like. The multi-branched macromonomer and the like thus obtained can be suitably used for the synthesis of the multi-branched styrenic resin.

[0027] The weight average molecular weight of the multi-branched macromonomer is not particularly limited, and is preferably about 1000 to 15000.

[0028] The content of the unsaturated aliphatic carboxylic acid ester unit in the multi-branched polystyrene is preferably 0.5 to 3.0% by weight, for example 0.6 to 2.8% by weight, or 0.9 to 2.5% by weight, based on 100% by weight of the entire styrenic resin. When the content of the unsaturated aliphatic carboxylic acid ester unit is within these ranges, thin film formation is easier, the swelling property is excellent, and the impact resistance tends to be improved.

[0029] From the viewpoint of ease of thin-film formation, the styrene-based resin may be a styrene-based resin composition (a mixture of styrene-based resins) containing linear polystyrene and multi-branched polystyrene.

[0030] When the styrene-based resin is a styrene-based resin composition containing linear polystyrene and branched polystyrene, the weight ratio of linear polystyrene to branched polystyrene in the resin composition (linear polystyrene:branched polystyrene) is preferably in the range of 99.5:0.5 to 70:30, and more preferably in the range of 95:5 to 75:25. When the weight ratio of branched polystyrene is 0.5 or higher, problems such as film cutting in the film manufacturing process are suppressed, even when the film thickness is reduced. Furthermore, when the weight ratio of branched polystyrene is 30 or lower, the formation of thickness variations in the film is suppressed in the film formation process, making it easier to reduce the film thickness.

[0031] The styrene resin film of this disclosure may further contain various additives as needed, such as pigment dispersants, ultraviolet absorbers, light stabilizers, antioxidants, flame retardants, antistatic agents, slip agents, and inorganic fillers.

[0032] When a styrene resin film contains various additives, the amount of each additive may be, for example, 0.01% by weight or more and 5% by weight or 0.1% by weight or more and 1% by weight or less, relative to the total weight of the styrene resin film.

[0033] The thickness of the styrene resin film is 10 to 25 μm. The upper limit of the film thickness is preferably less than 25 μm, 23 μm or less, 20 μm or less, 18 μm or less, 16 μm or less, or 15 μm or less. The lower limit of the film thickness, which can be arbitrarily combined with these upper limits, is preferably 11 μm or more, 12 μm or more, or 13 μm or more. By having the film thickness within the above range, it is possible to improve the energy density per unit weight of LIB and reduce problems such as breakage during tape processing.

[0034] <Adhesive Layer> The electrode fixing tape comprises the styrene resin film described above and an adhesive layer. The adhesive layer may be arranged on one or both sides of the styrene resin film, and is typically arranged on one side of the styrene resin film and attached to at least a portion of the surface of the electrode. As a result, the electrode fixing tape is positioned between the electrode and the outer casing of the LIB.

[0035] Any known adhesive can be used as the adhesive layer. Examples of adhesive layers include acrylic adhesives, silicone adhesives, polyimide adhesives, and fluorine-based adhesives. From the viewpoint of heat resistance and chemical resistance inside the battery, an acrylic adhesive is preferred.

[0036] The thickness of the adhesive is preferably 1 to 30 μm, 1 to 25 μm, 1 to 20 μm, 1 to 15 μm, or 1 to 10 μm. Within these thickness ranges, if the electrode body is a wound body, unwinding can be effectively prevented, and if it is a laminated body, misalignment of the laminates can be effectively prevented.

[0037] 《Method for manufacturing electrode fixing tape》 〈Method for manufacturing styrene resin film〉 The method for manufacturing styrene resin film is not limited, but known manufacturing methods can be employed, such as a manufacturing method in which a styrene resin (composition) is melted and kneaded and extruded into a cylindrical shape from a cylindrical die and then bubble-stretched (inflated), or a manufacturing method in which the styrene resin (composition) is extruded from a T-die onto a cast roll, cooled and solidified, and then stretched in a tenter.

[0038] From the viewpoint of facilitating thin-film formation, it is desirable to biaxially stretch styrene resin films in the longitudinal (MD) and transverse (TD) directions. By biaxially stretching styrene resin films in the MD and TD directions, the polymer chains can be uniformly oriented in the planar direction, improving mechanical strength. Furthermore, compared to uniaxial stretching (e.g., MD), biaxial stretching reduces thickness variations, improving the dimensional stability of the film and allowing for the creation of a thin film that is less prone to breakage. In addition, while stretched styrene resin films tend to shrink in the stretching direction upon swelling, biaxial stretching allows for uniform shrinkage direction and reduced shrinkage width, thereby suppressing peeling of the tape after swelling. Therefore, biaxial stretching of styrene resin films makes it easier to provide LIBs that are thin films (high energy density) yet possess excellent impact resistance.

[0039] The preferred stretching ratio for MD is 1.1 to 6.0 times, 1.1 to 5.0 times, or 1.1 to 4.0 times. The preferred stretching ratio for TD, which can be arbitrarily combined with these stretching ratios for MD, is 1.1 to 6.0 times, 1.1 to 5.0 times, or 1.1 to 4.0 times.

[0040] The ratio of the stretching ratio of the MD to the stretching ratio of the TD, the MD / TD ratio, is preferably 0.5 to 1.5, 0.6 to 1.4, 0.7 to 1.3, 0.8 to 1.2, or 0.9 to 1.1. By having a uniform stretching ratio between the MD and TD, the stress distribution of the MD and TD becomes more uniform when swollen with the electrolyte, which further suppresses the tendency of the tape to peel off.

[0041] The product of the MD stretching ratio and the TD stretching ratio (also called the "total stretching ratio") is preferable because a higher total stretching ratio improves the brittleness of the styrene resin film, reduces problems such as film breakage during film formation and tape processing, and makes it easier to manufacture films with a thickness of 10 to 25 μm. Furthermore, a higher total stretching ratio is preferable because, when the tape swells with the electrolyte, the increase in thickness due to the relaxation of stretching is added to the increase in thickness due to swelling with the electrolyte, making it easier to increase the tape thickness and increasing the gap-filling effect. The lower limit of the total stretching ratio is preferably 2 or more, 2.5 or more, 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, 12 or more, 13 or more, or 14 or more. The upper limits of the total stretching ratio, which can be arbitrarily combined with these lower limits, may be, for example, 25 or less, 20 or less, 19 or less, 18 or less, 17 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, or 8 or less.

[0042] From the viewpoint of reducing thickness variations and facilitating thinning, it is preferable to maintain a uniform and constant temperature throughout the entire stretched portion of the film during biaxial stretching. Such a temperature range can be appropriately adjusted depending on the styrene-based resin (composition) used, and is changed as appropriate according to the glass transition temperature (Tg) of the resin used. Preferably, it is controlled to be within ±5°C, ±4°C, ±3°C, or ±2°C.

[0043] <Method for Forming the Adhesive Layer> There are no particular limitations on the method for forming the adhesive layer on the styrene resin film, but general coating methods can be used. For example, a solvent-type adhesive, emulsion-type adhesive, or hot-melt-type adhesive can be applied to the surface of the styrene resin film by known methods such as gravure coating, roll coating, knife coating, die coating, or spray coating, and the adhesive layer can be formed by drying or cooling as necessary. In addition, to improve the adhesion of the adhesive, surface treatments such as corona treatment, plasma treatment, chemical treatment, or primer treatment may be applied to the film surface as necessary.

[0044] Lithium-ion battery The lithium-ion battery of this disclosure comprises an outer casing, and an electrode body and an electrolyte housed within the outer casing. The electrolyte contains at least 10% by weight and 30% by weight of cyclic carbonate and 50% by weight of chain carbonate. The lithium-ion battery is provided with an electrode body fixing tape of this disclosure between the outer casing and the electrode body. The lithium-ion battery of this disclosure has high impact resistance and high energy density per unit weight due to the above configuration.

[0045] <Electrolyte> The electrolyte contains an electrolyte and a solvent, and the electrolyte is a well-known LiClO 4 LiAsF 6 LiPF 6 LiBF 4 LiB(C) 6 H 5 ) 4 Examples include lithium compounds such as LiCl and LiBr.

[0046] The electrolyte solution preferably contains 1 to 2 mol / kg of electrolyte per unit weight (kg) of solvent.

[0047] As a solvent, carbonate-based solvents are mainly used. In this disclosure, "main component" means the component that is present in the largest weight percent of the constituent components. Other solvents besides carbonates may be used as needed. Examples of solvents other than carbonates include fluorobenzene and acetonitrile. Carbonate-based solvents are classified into linear carbonates and cyclic carbonates. Linear carbonates are those with a carbonate group (R 1 -OC(=O)-OR 2 Among organic compounds having ) R 1 and R 2 However, each of these independently refers to a compound having a linear or branched molecular structure. 1 and R 2Preferably, it is a monovalent hydrocarbon group having 1 to 10 carbon atoms. Examples of chain-like carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), and methylethyl carbonate (MEC). HSP value of chain-like carbonate: Hansen solubility parameter (J / cm²) 3 ) 1/2 Preferably, the pressure is 16 to 21 (J / cm²). 3 ) 1/2 It is within the range.

[0048] A cyclic carbonate is a compound containing a carbonate group (R 3 -OC(=O)-OR 4 Among organic compounds having ) R 3 and R 4 This refers to a compound in which molecules are bonded to each other within the molecule to form a cyclic structure. 3 and R 4 Preferably, these are a divalent hydrocarbon group having 1 to 10 carbon atoms, acting as a single unit. Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), and vinylene carbonate (VC). The HSP value of the cyclic carbonate is preferably 25 to 32 (J / cm²). 3 ) 1/2 It is within the range.

[0049] The cyclic carbonate content in the electrolyte is 10% by weight or more and 30% by weight or less, based on the total weight of the electrolyte. The lower limit of the cyclic carbonate content is preferably 12% by weight or more, 15% by weight or more, 17% by weight or more, 18% by weight or more, 19% by weight or more, or 20% by weight or more. The upper limit of the cyclic carbonate content, which can be arbitrarily combined with these lower limits, is preferably less than 30% by weight, 28% by weight or less, 27% by weight or less, 25% by weight or less, or 23% by weight or less. The chain-like carbonate content in the electrolyte is 50 to 70% by weight, based on the total weight of the electrolyte. The lower limit of the chain-like carbonate content is preferably 52% by weight or more, 55% by weight or more, or 57% by weight or more. The upper limits of the content of linear carbonate, which can be arbitrarily combined with these lower limits, are preferably 69% by weight or less, 68% by weight or less, 67% by weight or less, 65% by weight or less, or 62% by weight or less. By containing at least 10% by weight or more and 30% by weight or less of cyclic carbonate and 50% to 70% by weight of linear carbonate in the electrolyte of the lithium-ion battery, the swelling amount of the electrode fixing tape of this disclosure is high and it does not dissolve, thus improving the shock resistance of the LIB to drops and vibrations. Furthermore, since linear compounds have a lower boiling point than cyclic compounds, when the LIB becomes hot due to heat generation during charging and discharging, there is a higher risk that the electrolyte will volatilize and the battery will swell. Therefore, it is preferable for the electrolyte to contain 10% by weight or more and 30% by weight or less of cyclic carbonate, from the viewpoint of raising the boiling point of the electrolyte and suppressing the swelling of the battery. More preferably, the electrolyte of the lithium-ion battery contains 15 to 25% by weight of cyclic carbonate and 50 to 70% by weight of chain-like carbonate.

[0050] From the viewpoint of ensuring that the electrode fixing tape exhibits high swelling properties in relation to the electrolyte, the HSP value of the entire electrolyte containing cyclic carbonates and chain-like carbonates should be approximately 20.0 to 25.0 (J / cm²). 3 ) 1/2 Furthermore, the HSP value of the styrene resin film is 17.0 to 19.5 (J / cm²). 3 ) 1/2It is preferable that the relationship is as described above. When the HSP value of the entire electrolyte is within the above range, and the HSP value of the styrene resin film is also within the above range, the swelling properties in relation to the electrolyte are increased, so that even if it is thin, the gap between the electrode body and the outer casing can be tightly sealed. In addition, since the mechanical strength after swelling in relation to the electrolyte is improved, it is possible to more effectively prevent the electrode body from moving inside the outer casing due to shaking or shock of the battery.

[0051] More preferably, the difference between the HSP value of the entire electrolyte and the HSP value of the styrene resin film (= HSP value of the entire electrolyte - HSP value of the styrene resin film) is in the range of 2.3 to 3.6, even more preferably in the range of 2.5 to 3.6 or 2.3 to 3.1, and particularly preferably in the range of 2.5 to 3.1. When the difference between the HSP of the electrolyte and the HSP of the styrene resin film is within the above range, the increase in thickness due to swelling becomes greater. In addition, the mechanical strength after swelling is improved relative to the electrolyte, so it is possible to more effectively prevent the electrode body from moving inside the casing due to shaking or shock of the battery.

[0052] By using the preferred types of cyclic carbonates and linear carbonates described above, and / or adjusting their content to the preferred levels described above, the HSP value of the entire electrolyte can be increased to 20.0 to 25.0 (J / cm²). 3 ) 1/2 It is easier to adjust to this. In addition, by using the preferred styrene resin (composition) described above, in addition to the styrene units constituting the styrene resin film being 85% by weight or more and less than 97% by weight, the HSP value of the styrene resin film can be set to 17.0 to 19.5 (J / cm²). 3 ) 1/2 It is easier to adjust to this.

[0053] <Electrode Body> The electrode body refers to a structure in which a positive electrode, a negative electrode, and a separator placed between them are stacked (stacked type), or a structure in which they are stacked and wound (wound type). The electrode body can be either stacked or wound, depending on the desired battery shape. In this disclosure, by containing 10% to 30% by weight of cyclic carbonate in the electrolyte, the boiling point of the electrolyte is higher than that of chain carbonate, and the expansion of the battery can be suppressed to some extent. In addition, a preferred embodiment in this disclosure is a wound type electrode body suitable for cylindrical LIBs, which has a high surface area-to-volume ratio structurally and excellent heat dissipation performance.

[0054] Preferably, the electrode body is provided with the electrode body fixing tape of this disclosure on at least a portion of its surface. This ensures that when the electrode body is housed in the outer casing, the electrode body fixing tape is positioned between the electrode body and the outer casing. If the electrode body is of the wound type, it is preferably attached to stop the end of the wound type. This prevents the wound body from unwinding while preventing the electrode body from moving within the outer casing. If the electrode body is of the laminated type, it is attached to the side surface and / or main surface of the laminate. Attaching it to the side surface of the laminate prevents the laminated positive electrode, negative electrode, and separator from shifting while preventing the electrode body from moving within the outer casing. Attaching it to the main surface of the laminate increases the contact area between the electrode body and the outer casing, thus more effectively preventing the electrode body from moving within the outer casing.

[0055] <Outer casing> The outer casing can be a container or packaging bag that houses and protects the LIB components such as electrodes and electrolyte. Depending on the shape and application of the battery, the outer casing can preferably be a rigid metal casing or a flexible packaging bag.

[0056] In cylindrical lithium-ion batteries, a rigid metal casing, such as steel or aluminum, is typically used as the outer casing. This rigid casing has a cylindrical shape with one end open, and a wound electrode body is housed inside. The opening is sealed with an insulating gasket or the like to ensure airtightness, and a safety mechanism such as a safety valve can be provided as needed. Because the rigid casing has excellent mechanical strength and shielding properties, it is suitable for applications where reliability is required.

[0057] In pouch-type lithium-ion batteries, a flexible packaging bag, such as a laminate film, is typically used as the outer casing. The laminate film may be, for example, a laminated film of aluminum foil and a thermoplastic resin. This flexible casing houses a laminated electrode body, and its periphery is sealed by heat fusion or adhesive. The flexible casing can also be equipped with safety mechanisms such as safety valves, if necessary. Such flexible casings are lightweight and allow for flexible shape design, and are therefore widely used in electronic equipment applications where thinning and weight reduction are required. Although flexible casings have lower mechanical strength than rigid casings, as described above, the electrolyte of this disclosure contains a cyclic carbonate, which can suppress battery expansion, and therefore, in one embodiment, it can be suitably used in a flexible casing (pouch type) LIB.

[0058] The contents of this disclosure will be explained in more detail below with reference to examples and comparative examples. However, this disclosure is not limited to these examples.

[0059] 《Materials》 The materials used in the examples and comparative examples are as follows: <Styrene resins> Polystyrene 1 (PS1): Manufactured by PS Japan, Grade 685, MFR = 1.5 g / 10 min (GPPS, linear PS, styrene monomer content 100% by weight) Polystyrene 2 (PS2): Manufactured by DIC, Grade HP-100, MFR = 3.3 g / 10 min (Mixture of 84% by weight of linear PS and 16% by weight of branched PS, butyl acrylate monomer content in branched PS16 is 2% by weight, overall styrene monomer content 99.7% by weight) Styrene resin (SMAA1): Manufactured by PS Japan, styrene-methacrylic acid copolymer, Grade MM290, methacrylic acid content 18% by weight Styrene resin (ABS): Acrylonitrile (AN)-butadiene (Br)-styrene (St) copolymer, AN:Br:St (weight ratio) = 30:20:50, styrene monomer content 50% by weight High-impact polystyrene (HIPS1): Manufactured by PS Japan, Grade name 475D, Butadiene content 5.6% by weight, Styrene monomer content 94.4% by weight High-impact polystyrene (HIPS2): Manufactured by PS Japan, Grade name H8672, MFR = 4.0 g / 10 min, Butadiene content 7.6% by weight, Styrene monomer content 93.4% by weight

[0060] <Electrolytes> Dimethyl carbonate (CAS616-38-6) HSP value = 20.7 Diethyl carbonate (CAS105-58-6) HSP value = 17.9 Ethylene carbonate (CAS96-49-1) HSP value = 29.1 Propylene carbonate (CAS108-32-7) HSP value = 27.2 Acetonitrile (CAS75-05-8) HSP value = 24.4

[0061] 《Measurement and Evaluation Methods》 The measurement and evaluation methods used in the examples and comparative examples are as follows.

[0062] <Thickness of Styrene Resin Film> The thickness of the styrene resin film was measured using a dial gauge compliant with JIS-B-7503 (unit: μm).

[0063] <HSP Values ​​of Styrene Resin Compositions and Electrolytes> HSP values ​​(Hansen solubility parameters) for each component constituting the styrene resin composition and electrolyte. Unit: (J / cm²) 3 ) 1/2 The following formula was used to determine the HSP value of a mixture. For mixtures, the HSP value of the mixed solvent was calculated by multiplying the mixing ratio by the δd, δp, and δh of each solvent to determine the δd, δp, and δh of the mixed solvent. Formula: HSP = {(δd) 2 + (δp) 2 + (δh) 2} 1/2 HSP: Hansen Solubility Parameter Unit: (J / cm) 3 ) 1/2 δd: Intermolecular dispersion force energy δp: Intermolecular dipole interaction energy δh: Intermolecular hydrogen bond energy The values ​​of δd, δp, and δh for various resins, electrolyte components, etc., are described, for example, in Non-Patent Literature 1 (Charles M. Hansen, "Hansen Solubility Parameters: A User's Handbook", (USA), 2nd edition, CRC Press, June 15, 2007).

[0064] <Styrene monomer composition ratio> The styrene monomer composition ratio in the styrene-based resin composition and styrene-based resin film of this disclosure was determined by dissolving the sample in deuterated chloroform and then analyzing it by NMR.

[0065] <Stretching ratio (MD, TD), total stretching ratio, and stretching ratio ratio (MD / TD) of styrene resin film> A 10cm x 10cm piece of styrene resin film was cut in the MD x TD direction and immersed in a 120°C oil bath for 1 minute. The rate of change in the film dimensions (cm) of MD and TD after immersion was defined as the stretching ratio of MD and TD, respectively, and the product of these stretching ratios was defined as the total stretching ratio. MD stretching ratio = 10 / (MD dimensions after oil bath immersion: cm) TD stretching ratio = 10 / (TD dimensions after oil bath immersion: cm) Total stretching ratio = MD stretching ratio x TD stretching ratio Stretching ratio ratio (MD / TD) = MD stretching ratio / TD stretching ratio

[0066] <Measurement of Dimensional Change Rate (MD, TD, and Thickness) of Film by Electrolyte> A styrene resin film was cut to a size of 10 cm x 10 cm in the MD x TD direction. The film was immersed in a mixed solvent containing predetermined proportions of cyclic carbonate and chain carbonate as shown in Tables 1 and 2. After 24 hours at 60°C, the film dimensions (cm) and thickness were measured, and the dimensional change rate (MD, TD, and thickness) was calculated. MD dimensional change rate (%) = MD dimensions after immersion (cm) / 10 (cm) x 100 TD dimensional change rate (%) = TD dimensions after immersion (cm) / 10 (cm) x 100 Thickness change rate (%) = Thickness after immersion (μm) / Thickness before immersion (μm) x 100

[0067] <Ease of peeling the tape after solvent immersion> Since the ease of peeling the tape increases in proportion to the dimensional change rate of MD and TD before and after solvent immersion, the ease of peeling the tape was evaluated by the ratio of the dimensional change rate of MD and TD after solvent immersion. ○: Dimensional change rate (MD / TD) before and after solvent immersion is 0.5 or more and less than 1.5 ×: Dimensional change rate (MD / TD) before and after solvent immersion is 1.5 or more

[0068] <Drop and vibration resistance of electrode body using tape> The adhesive strength between the LIB casing and the tape increases in proportion to the rate of thickness increase of the tape due to the electrolyte (solvent). Therefore, the magnitude of the adhesive strength was evaluated based on the rate of thickness increase of the styrene resin film due to the electrolyte. A: Thickness increase rate of 200% or more B: Thickness increase rate of 150% or more and less than 200% C: Thickness increase rate of 110% or more and less than 150% D: Thickness increase rate less than 110%

[0069] <Overall Evaluation> The film thickness before immersion (μm) was used as an indicator of energy density per unit weight, and the thickness increase rate (%) was used as an indicator of impact resistance during vibration drop. The overall evaluation was conducted according to the following evaluation criteria: A: Thickness increase rate (%) / film thickness before immersion (μm) value is 9 or more B+: Thickness increase rate (%) / film thickness before immersion (μm) value is 7 or more and less than 9 B: Thickness increase rate (%) / film thickness before immersion (μm) value is 6 or more and less than 7 B-: Thickness increase rate (%) / film thickness before immersion (μm) value is 5 or more and less than 6 C: Thickness increase rate (%) / film thickness before immersion (μm) value is 4 or more and less than 5 D: Thickness increase rate (%) / film thickness before immersion (μm) value is less than 4

[0070] Examples and Comparative Examples [Examples 1-9] Styrene resins were blended in the proportions shown in Table 1, and films were prepared by stretching them using the inflation method under the conditions shown in Table 1.

[0071] [Comparative Examples 1-6] The composition of the styrene resin was changed to the proportions shown in Table 2, and a film was prepared by stretching it using the inflation method under the conditions shown in Table 2.

[0072] The physical properties and evaluation results of the films obtained in Examples 1 to 9 and Comparative Examples 1 to 6 are summarized in Tables 1 and 2.

[0073]

[0074]

[0075] The electrode fixing tape disclosed herein can achieve both the impact resistance and high energy density per unit weight of lithium-ion batteries, and is therefore suitable for use in electronic devices such as mobile phones, smartphones, notebook PCs, and cordless home appliances, as well as batteries for electric vehicles.

Claims

1. An electrode fixing tape used in a lithium-ion battery, wherein the electrolyte of the lithium-ion battery contains at least 10% to 30% by weight of cyclic carbonate and 50 to 70% by weight of chain-like carbonate, based on 100% by weight of the electrolyte, the electrode fixing tape comprises a styrene resin film and an adhesive layer, the thickness of the styrene resin film is 10 to 25 μm, and the styrene monomer composition ratio to the total weight of all resin components constituting the styrene resin film is in the range of 85% to less than 97% by weight.

2. The electrode fixing tape according to claim 1, wherein the product of the MD direction stretching ratio and the TD direction stretching ratio of the styrene resin film is in the range of 2 to 25.

3. The electrode fixing tape according to claim 1 or 2, wherein the ratio of the stretching ratio in the MD direction to the stretching ratio in the TD direction (MD / TD) is in the range of 0.5 to 1.

5.

4. The HSP value of the entire electrolyte is approximately 20.0 to 25.0 (J / cm²). 3 ) 1/2 Furthermore, the HSP value of the styrene resin film is 17.0 to 19.5 (J / cm²). 3 ) 1/2 The electrode fixing tape according to claim 1 or 2.

5. The electrode fixing tape according to claim 1 or 2, wherein the electrolyte of the lithium-ion battery contains 15 to 25% by weight of a cyclic carbonate and 50 to 70% by weight of a chain-like carbonate.

6. The electrode fixing tape according to claim 1 or 2, wherein the styrene resin film comprises a multi-branched styrene resin.

7. The electrode fixing tape according to claim 1 or 2, wherein the styrene resin film comprises linear polystyrene and multi-branched polystyrene, and the ratio of the linear polystyrene to the multi-branched polystyrene is in the range of 99.5:0.5 to 70:

30.

8. The electrode fixing tape according to claim 1 or 2, wherein the styrene resin film has at least one impact-resistant polystyrene selected from the group consisting of styrene-butadiene copolymer (SB resin), high-impact polystyrene (HIPS), and styrene-butadiene-styrene resin (SBS resin).

9. A lithium-ion battery comprising an outer casing, an electrode body, and an electrolyte housed within the outer casing, wherein the electrolyte contains 10% to 30% by weight of cyclic carbonate and 50 to 70% by weight of chain carbonate, and the lithium-ion battery is provided with an electrode body fixing tape according to claim 1 or 2 between the outer casing and the electrode body.

10. The HSP value of the entire electrolyte is approximately 20.0 to 25.0 (J / cm²). 3 ) 1/2 Furthermore, the HSP value of the styrene resin film is 17.0 to 19.5 (J / cm²). 3 ) 1/2 The lithium-ion battery according to claim 9.

11. The lithium-ion battery according to claim 9, wherein the difference between the HSP value of the entire electrolyte and the HSP value of the styrene resin film is in the range of 2.3 to 3.

6.

12. The lithium-ion battery according to claim 9, wherein the electrolyte of the lithium-ion battery contains 15 to 25% by weight of a cyclic carbonate and 50 to 70% by weight of a chain-like carbonate.

13. The lithium-ion battery according to claim 9, wherein the styrene-based resin film comprises a multi-branched styrene-based resin.

14. The lithium-ion battery according to claim 9, wherein the styrene-based resin film comprises linear polystyrene and multi-branched polystyrene, and the ratio of the linear polystyrene to the multi-branched polystyrene is in the range of 99.5:0.5 to 70:

30.