Cosmetic composition free of talc and preparation method therefor

A cosmetic composition using kaolin, hydrophobic silica, and an oil binder, with water as a binder, addresses the issues of talc replacement by enhancing compression moldability and stability, ensuring economic efficiency and preventing caking.

WO2026240275A1PCT designated stage Publication Date: 2026-11-19OSEANS INTL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2025/018547
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2025-11-11
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The challenge lies in developing a solid powder cosmetic that does not contain talc, while maintaining high compression moldability, molding stability, and economic efficiency, as talc's replacement, mica, results in poor compressibility and increased use of metal-based and oil binders, leading to a heavy texture and caking issues.

Method used

A cosmetic composition comprising kaolin, hydrophobic silica, and an oil binder, with specific weight percentages, and using water as a binder to enhance compression moldability and stability, eliminating the need for talc.

Benefits of technology

The composition achieves excellent compression moldability, shape stability, and economic efficiency without talc, minimizing caking and maintaining moisture stability, while using water as a binder to facilitate preparation and compression.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2025018547_19112026_PF_FP_ABST
    Figure KR2025018547_19112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a solid powder cosmetic composition and a preparation method therefor. The solid powder cosmetic composition of the present application is free of talc and is safe for the human body while exhibiting the compression moldability and shape stability of talc, and has an effect of stably retaining moisture therein while including water as a binder.
Need to check novelty before this filing date? Find Prior Art

Description

Cosmetic composition not containing talc and method for manufacturing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2025-0064171 filed on May 16, 2025, and all contents disclosed in the document of said Korean patent application are incorporated herein as part of this specification.

[0003] The present application relates to a cosmetic composition that does not contain talc and a method for manufacturing the same.

[0004]

[0005] Solid powder cosmetics (compressed powder cosmetics) were developed to enhance portability and provide ease of use by compression molding powder-form makeup. In particular, talc has been used as a key ingredient since the early stages of solid powder cosmetics development. Talc offers economic advantages, such as abundant ore veins and easy mining. Furthermore, talc provides a smooth and soft texture and possesses excellent compression moldability due to its brittle nature. Thanks to talc's superior compression moldability, powder cosmetics can be easily compressed while reducing the use of metal-based binders or oil binders, which typically result in a heavy texture and cause caking.

[0006] However, as it has become known that the mining process of talc is highly likely to contain asbestos, a hazardous substance, an increasing number of users are avoiding its use, leading to its gradual exclusion from the market. Although mica is primarily used as a raw material to replace talc, unlike talc which is brittle, mica has a plate-like form and elasticity, so it does not break easily, resulting in a disadvantage of poor compression moldability. Consequently, when using mica, the amount of metal-based binders and oil binders used to bind powders must be increased to compensate for compressibility. This makes the product feel heavy and stiff to use, causes caking, and results in poor payoff, where the surface hardens and the contents do not adhere easily.

[0007] Another method to replace talc is the wet molding method for cosmetics. This method involves mixing powder with an oil binder, kneading it with water or a volatile solvent to form a slurry, molding it onto a plate, and then drying it. However, the wet molding method has the disadvantage of significantly reducing production yield because the molding process is complex and usually requires a drying time of more than one day.

[0008] [Prior Art Literature]

[0009] [Patent Literature]

[0010] (Patent Document 1) Republic of Korea Published Patent No. 10-2012-0122282

[0011] The inventors have made diligent research efforts to develop a cosmetic composition capable of producing a solid powder cosmetic that does not contain talc, yet has high molding stability, economic efficiency, and excellent usability. As a result, it was discovered that by using powdered raw materials containing kaolin and hydrophobic silica and using water as a binder, it is possible to produce a solid powder cosmetic that does not contain talc, yet has high compression moldability, molding stability, economic efficiency, and excellent usability.

[0012] Accordingly, the objective of the present application is to provide a cosmetic composition comprising kaolin, hydrophobic silica, and an oil binder, wherein the kaolin is included in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition.

[0013] Another objective of the present application is to provide a cosmetic product comprising the above cosmetic composition.

[0014] Another objective of the present application is to provide a cosmetic product manufactured by compression molding the above cosmetic composition.

[0015] Another object of the present application is to provide a method for preparing a cosmetic composition comprising: (1) mixing powdered raw materials including kaolin and hydrophobic silica; (2) adding and mixing an oil binder to the mixture obtained in step (1); and (3) adding and mixing water to the mixture obtained in step (2), wherein the kaolin is included in an amount of 5% to 30% by weight with respect to the total weight of the cosmetic composition, and the water is included in an amount of 0.5% to 10% by weight with respect to the total weight of the cosmetic composition.

[0016] Another objective of the present application is to provide a method for manufacturing a cosmetic product comprising the step of compressing and molding the cosmetic composition.

[0017]

[0018] This is explained in detail as follows. Meanwhile, each description and embodiment disclosed in this application may be applied to other descriptions and embodiments. That is, all combinations of the various elements disclosed in this application fall within the scope of this application. Furthermore, the scope of this application should not be considered limited by the specific descriptions provided below. Additionally, numerous papers and patent documents are referenced and cited throughout this specification. The disclosures of the cited papers and patent documents are incorporated by reference into this specification in their entirety to more clearly explain the state of the art to which the present invention pertains and the content of the present invention.

[0019]

[0020] One aspect of the present application provides a cosmetic composition comprising a powdered raw material including kaolin and hydrophobic silica, and an oil binder, wherein the kaolin is included in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition.

[0021] In this application, “kaolin” is a natural silicate mineral and is a powder composed mainly of aluminum hydroxide silicate (Al2Si2O5(OH)4). As demonstrated in the examples to be described later, by using kaolin, it is possible to produce a cosmetic composition that has excellent compression moldability while using water as a binder.

[0022] In one embodiment, the cosmetic composition of the present application described above may comprise the kaolin in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition, and more specifically, 5% to 30% by weight, 5% to 25% by weight, 5% to 20% by weight, 5% to 15% by weight, 5% to 12.5% ​​by weight, 5% to 11% by weight, 5% to 10% by weight, 5% to 9.85% by weight, 7.5% to 30% by weight, 7.5% to 25% by weight, 7.5% to 20% by weight, 7.5% to 15% by weight, 7.5% to 12.5% ​​by weight, 7.5% to 11% by weight, 7.5% to 10% by weight, 7.5% to 9.85% by weight, 9 wt% to 30 wt%, 9 wt% to 25 wt%, 9 wt% to 20 wt%, 9 wt% to 15 wt%, 9 wt% to 12.5 wt%, 9 wt% to 11 wt%, 9 wt% to 10 wt%, 9 wt% to 9.85 wt%, 9.25 wt% to 30 wt%, 9.25 wt% to 25 wt%, 9.25 wt% to 20 wt%, 9.25 wt% to 15 wt%, 9.25 wt% to 12.5 wt%, 9.25 wt% to 11 wt%, 9.25 wt% to 10 wt%, 9.25 wt% to 9.85 wt%, 9.4 wt% to 30 wt%, 9.4 wt% to 25 wt%, 9.4 wt% to 20 wt%, 9.4 wt% to 15 wt%, 9.4 wt% to 12.5 wt%, 9.4 wt% to 11 wt%, 9.4 wt% to 10 wt%, 9.4 wt% to 9.85 wt%, 9.6 wt% to 30 wt%, 9.6 wt% to 25 wt%, 9.6 wt% to 20 wt%, 9.6 wt% to 15 wt%, 9.6 wt% to 12.5 wt%, 9.6 wt% to 11 wt%, 9.6 wt% to 10 wt%, 9.6 wt% to 9.It may be included in 85 wt%, 9.75 wt% to 30 wt%, 9.75 wt% to 25 wt%, 9.75 wt% to 20 wt%, 9.75 wt% to 15 wt%, 9.75 wt% to 12.5 wt%, 9.75 wt% to 11 wt%, 9.75 wt% to 10 wt%, or 9.75 wt% to 9.85 wt%, but is not limited thereto.

[0023] As demonstrated in the embodiments of the present application to be described below, the cosmetic composition of the present application, by including kaolin, when a water binder is additionally used in addition to an oil binder, the powder is uniformly aggregated and clumped together as the water content increases, and has the effect of excellent compression moldability and shape stability without using talc.

[0024] In this application, “hydrophobic silica” means silica or silica derivative having hydrophobicity. The silica derivative may include a compound in which the surface of the silica is modified by the addition of other compounds or functional groups. In one embodiment, the hydrophobic silica is silica or a silica derivative having hydrophobic groups chemically bonded to the surface, and may primarily refer to silica in which the hydroxyl groups (-OH) on the silica surface are functionalized into silyl groups (Si-Rn) by treating the silica surface with an organosilicon compound such as a halogenated silane or siloxane. For the purposes of this application, the hydrophobic silica may be capable of excellently capturing moisture so that water can be used as a binder.

[0025] In one embodiment, the hydrophobic silica may be fumed silica or a fumed silica derivative having hydrophobicity. The fumed silica is amorphous silicon dioxide (SiO2) formed by gas-phase oxidation of silicon tetrachloride (SiCl4) under a flame of hydrogen and oxygen, and forms a three-dimensional aggregate structure having a high specific surface area. The fumed silica derivative may refer to modified silica that imparts hydrophobicity by functionalizing the hydroxyl groups (-OH) on the silica surface into organosilyl groups (Si-Rn), etc., through a silylation reaction.

[0026] In one embodiment, the hydrophobic silica may be one or more selected from the group consisting of silica dimethyl sililate, silica sililate, silica dimethicone sililate, and silica caprylyl sililate, but is not limited thereto, and may be those commonly used in the industry.

[0027] In one embodiment, the cosmetic composition of the present application described above may include the hydrophobic silica in an amount of 0.5 wt% to 3 wt% based on the total weight of the cosmetic composition, and more specifically, 0.5 wt% to 3 wt%, 0.5 wt% to 2.5 wt%, 0.5 wt% to 2 wt%, 0.5 wt% to 1.75 wt%, 0.5 wt% to 1.5 wt%, 0.75 wt% to 3 wt%, 0.75 wt% to 2.5 wt%, 0.75 wt% to 2 wt%, 0.75 wt% to 1.75 wt%, 0.75 wt% to 1.5 wt%, 1 wt% to 3 wt%, 1 wt% to 2.5 wt%, 1 wt% to 2 wt%, 1 wt% to 1.75 wt%, 1 wt% to 1.5 wt%, 1.25 wt% wt% to 3 wt%, 1.25 wt% to 2.5 wt%, 1.25 wt% to 2 wt%, 1.25 wt% to 1.75 wt%, 1.25 wt% to 1.5 wt%, 1.4 wt% to 3 wt%, 1.4 wt% to 2.5 wt%, 1.4 wt% to 2 wt%, 1.4 wt% to 1.75 wt%, 1.4 wt% to 1.5 wt%, 1.43 wt% to 3 wt%, 1.43 wt% to 2.5 wt%, 1.43 wt% to 2 wt%, 1.43 wt% to 1.75 wt%, 1.43 wt% to 1.5 wt%, 1.45 wt% to 3 wt%, 1.45 wt% to 2.5 wt%, 1.45 wt% to 2 wt% It may be included in weight%, 1.45 weight% to 1.75 weight%, 1.45 weight% to 1.5 weight%, 1.47 weight% to 3 weight%, 1.47 weight% to 2.5 weight%, 1.47 weight% to 2 weight%, 1.47 weight% to 1.75 weight%, or 1.47 weight% to 1.5 weight%, but is not limited thereto.

[0028] As demonstrated in the embodiments of the present application to be described below, the cosmetic composition of the present application includes hydrophobic silica, such as silica dimethyl silylate, so that even when a water binder is additionally used in addition to an oil binder, water is smoothly mixed and dispersed during the preparation of the cosmetic composition, thereby facilitating the preparation and compression of the cosmetic composition, preventing the volatilization of water, and in particular, the moisture within the kaolin is stably maintained, thereby maintaining the moisture within the cosmetic composition stably, and it possesses excellent compression moldability and shape stability without using talc.

[0029] In this application, "binder" refers to a component used to bind or fix the constituent components of a cosmetic composition. The binder provides binding and cohesive forces between raw materials within the cosmetic composition, particularly powder-based raw materials, thereby enhancing compression moldability and maintaining a solid form, and preventing the product from easily breaking or scattering powder. Additionally, it can improve the spreadability and longevity of the cosmetic composition.

[0030] In this application, the oil binder serves to enhance compression moldability by imparting cohesive force between the powder-phase raw materials when manufacturing solid powder cosmetics by compression molding. It is also used to prevent breakage when the manufactured solid powder cosmetic (compressed powder cosmetic) is subjected to external impact and to reduce powder scattering. However, the oil binder has the disadvantage of degrading the usability of the solid powder cosmetic by giving a heavy feeling upon application. Additionally, depending on the oil binder content, a phenomenon called caking may occur, in which the powder clumps or hardens. Caking refers to a phenomenon in which, when taking out the contents of a cosmetic product compressed with powder-phase raw materials and an oil binder using fingers, a puff, or a brush, the oil clumps and adheres firmly to the surface where friction occurs due to the difference in the friction coefficients between the powder-phase raw materials and the oil. In cases of severe caking, it becomes difficult to take out the contents, and stains appear on the surface, leading to a deterioration in quality. Generally, caking tends to intensify as the oil binder content increases. Therefore, there is a need to develop a cosmetic composition or cosmetic that maintains a constant hardness, is stable against external impacts, and does not cause caking.

[0031] In this application, any oil capable of binding raw materials in powder form may be used as the oil binder, for example, silicone oil (e.g., methicone, cyclopentasiloxane, methyltrimethicone, caprylylmethicone, cyclomethicone, cyclotetrasiloxane, cyclohexasiloxane, cycloheptasiloxane, decamethylcyclopentasiloxane, cyclotetrasiloxane, cyclotrisiloxane, dimethicone, caprylyldimethicone, caprylyltrimethicone, cetearylmethicone, hexadecylmethicone, hexylmethicone, laurylmethicone, myristylmethicone, phenylmethicone, stearylmethicone, stearyldimethicone, trifluoropropylmethicone, cetyldimethicone, polyphenylmethylsiloxane, dimethylpolysiloxane, methylphenylpolysiloxane, Methyl trimethicone, diphenylsiloxyphenyl trimethicone, phenyl trimethicone, diphenyl dimethicone, and trimethylsiloxyphenyl dimethicone, etc.), hydrocarbon oils (e.g., hydrogenated polyisobutene, liquid paraffin, petroleum jelly, isoparaffin, hydrogenated polydecene, squalane, polybutene, isododecane, isohexadecane, polydecene, etc.), ester oils (e.g., diisostearyl malate, dipentaerythrityl hexa-C5-9 acid ester, cetyl ethylhexanoate, isocetyl ethylhexanoate, isocetyl myristate, isopropyl myristate, neopentyl glycol dicaprate, hexyl laurate, triethylhexanoin, pentaerythrityl tetraoctanoate, ethylhexyl It may be one or more selected from the group consisting of palmitate, isononyl isononanoate, polyglyceryl-2 triisostearate, pentaerythrityl stearate / caprate / caprylate / adipate, octyldodecyl stearoyl stearate, isostearyl isostearate, sorbitan isostearate, pentaerythrityl tetraethylhexanoate, pentaerythrityl tetraisostearate caprylic / capric triglyceride, etc.), mineral oil, vegetable oil, animal oil, polyglycerin-based oil, glycol-based oil, and synthetic fatty acid-based oil, but is not limited thereto.It may be commonly used in the industry.

[0032] In one embodiment, the cosmetic composition of the present application described above may comprise the oil binder in an amount of 5% to 25% by weight based on the total weight of the cosmetic composition, and more specifically, 5% to 25% by weight, 5% to 20% by weight, 5% to 15% by weight, 5% to 13% by weight, 5% to 12.9% by weight, 5% to 12.8% by weight, 5% to 12.7% by weight, 5% to 12.3% by weight, 5% to 12.25% by weight, 5% to 10% by weight, 10% to 25% by weight, 10% to 20% by weight, 10% to 15% by weight, 10% to 13% by weight, 10% to 12.9% by weight, 10% to 12.8% by weight, 10 wt% to 12.7 wt%, 10 wt% to 12.3 wt%, 10 wt% to 12.25 wt%, 12.25 wt% to 25 wt%, 12.25 wt% to 20 wt%, 12.25 wt% to 15 wt%, 12.25 wt% to 13 wt%, 12.25 wt% to 12.9 wt%, 12.25 wt% to 12.8 wt%, 12.25 wt% to 12.7 wt%, 12.25 wt% to 12.3 wt%, 12.3 wt% to 25 wt%, 12.3 wt% to 20 wt%, 12.3 wt% to 15 wt%, 12.3 wt% to 13 wt%, 12.3 wt% to 12.9 wt%, 12.3 It may be included in weight% to 12.8 weight%, 12.3 weight% to 12.7 weight%, 12.7 weight% to 25 weight%, 12.7 weight% to 20 weight%, 12.7 weight% to 15 weight%, 12.7 weight% to 13 weight%, 12.7 weight% to 12.9 weight%, or 12.7 weight% to 12.8 weight%, but is not limited thereto.

[0033] In one embodiment, the oil binder may include a surfactant. In one embodiment, the surfactant may be one or more selected from the group consisting of silicone-based surfactants, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, and semipolar surfactants; more specifically, it may be an anionic surfactant (e.g., sorbitan isostearate), a silicone-based surfactant having an HLB (Hydrophilic-Lipophilic Balance) value of about 4 to 5 depending on the surface treatment raw material, or other low-irritation surfactants. By using the surfactant, the affinity between the hydrophobic powder with water-repellent properties and water can be enhanced when water is used as a binder.

[0034]

[0035] In one embodiment, the cosmetic composition of the present application described above may additionally include water.

[0036] In this application, water may be used as a binder. The inventors have made diligent research efforts to use water as a binder in order to develop a cosmetic composition or cosmetic product that minimizes caking and payoff defects while replacing talc, which has excellent compression moldability. By including a water binder, they have invented the cosmetic composition of this application, which exhibits excellent compression moldability and shape stability while maintaining moisture stability within the cosmetic product.

[0037] The above water may be purified water.

[0038] In one embodiment, the cosmetic composition of the present application described above may contain the water in an amount of 0.5% to 10% by weight based on the total weight of the cosmetic composition, and more specifically, 0.5% to 10% by weight, 0.5% to 7.5% by weight, 0.5% to 6% by weight, 0.5% to 4.5% by weight, 0.5% to 3.5% by weight, 0.5% to 2.5% by weight, 0.5% to 2% by weight, 0.5% to 1.98% by weight, 0.5% to 1.97% by weight, 0.5% to 1.96% by weight, 0.75% to 10% by weight, 0.75% to 7.5% by weight, 0.75% to 6% by weight, 0.75% to 4.5% by weight, 0.75% to 3.5 wt%, 0.75 wt% to 2.5 wt%, 0.75 wt% to 2 wt%, 0.75 wt% to 1.98 wt%, 0.75 wt% to 1.97 wt%, 0.75 wt% to 1.96 wt%, 1 wt% to 10 wt%, 1 wt% to 7.5 wt%, 1 wt% to 6 wt%, 1 wt% to 4.5 wt%, 1 wt% to 3.5 wt%, 1 wt% to 2.5 wt%, 1 wt% to 2 wt%, 1 wt% to 1.98 wt%, 1 wt% to 1.97 wt%, 1 wt% to 1.96 wt%, 1.25 wt% to 10 wt%, 1.25 wt% to 7.5 wt%, 1.25 wt% to 6 wt%, 1.25 wt% to 4.5 wt%, 1.25 wt% to 3.5 wt%, 1.25 wt% to 2.5 wt%, 1.25 wt% to 2 wt%, 1.25 wt% to 1.98 wt%, 1.25 wt% to 1.97 wt%, 1.25 wt% to 1.96 wt%, 1.5 wt% to 10 wt%, 1.5 wt% to 7.5 wt%, 1.5 wt% to 6 wt%, 1.5 wt% to 4.5 wt%, 1.5 wt% to 3.5 wt%, 1.5 wt% to 2.5 wt%, 1.5 wt% to 2 wt%, 1.5 wt% to 1.98 wt%, 1.5 wt% to 1.97 wt%, 1.5 wt% to 1.96 wt%, 1.75 wt% to 10 wt%, 1.75 wt% to 7.5 wt%, 1.75 wt% to 6 wt%, 1.75 wt% to 4.5 wt%, 1.75 wt% to 3.5 wt%, 1.75 wt% to 2.5 wt%, 1.75 wt% to 2 wt%, 1.75 wt% to 1.98 wt%, 1.75 wt% to 1.97 wt%, 1.75 wt% to 1.96 wt%, 1.8 wt% to 10 wt%, 1.8 wt% to 7.5 wt%, 1.8 wt% to 6 wt%, 1.8 It may be included in weight% to 4.5 weight%, 1.8 weight% to 3.5 weight%, 1.8 weight% to 2.5 weight%, 1.8 weight% to 2 weight%, 1.8 weight% to 1.98 weight%, 1.8 weight% to 1.97 weight%, or 1.8 weight% to 1.96 weight%, but is not limited thereto.

[0039] In one embodiment, the cosmetic composition of the present application described above may comprise the water in an amount of 0.5 to 10 parts by weight with respect to 100 parts by weight of the powdered raw material and oil binder, and more specifically, 0.5 to 10 parts by weight, 0.5 to 8 parts by weight, 0.5 to 7 parts by weight, 0.5 to 6 parts by weight, 0.5 to 5 parts by weight, 0.5 to 4 parts by weight, 0.5 to 3.5 parts by weight, 0.5 to 3 parts by weight, 0.5 to 2.5 parts by weight, 0.5 to 2.25 parts by weight, 0.5 to 2 parts by weight, 1 to 10 parts by weight, 1 to 8 parts by weight, 1 to 7 parts by weight, 1 to 6 parts by weight, 1 to 5 parts by weight, and 1 part by weight. to 4 parts by weight, 1 to 3.5 parts by weight, 1 to 3 parts by weight, 1 to 2.5 parts by weight, 1 to 2.25 parts by weight, 1 to 2 parts by weight, 1.25 to 10 parts by weight, 1.25 to 8 parts by weight, 1.25 to 7 parts by weight, 1.25 to 6 parts by weight, 1.25 to 5 parts by weight, 1.25 to 4 parts by weight, 1.25 to 3.5 parts by weight, 1.25 to 3 parts by weight, 1.25 to 2.5 parts by weight, 1.25 to 2.25 parts by weight, 1.25 to 2 parts by weight, 1.5 to 10 parts by weight, 1.5 to 8 parts by weight, 1.5 to 7 parts by weight, 1.5 to 6 parts by weight, 1.5 to 5 parts by weight, 1.5 to 4 parts by weight, 1.5 to 3.5 parts by weight, 1.5 to 3 parts by weight, 1.5 to 2.5 parts by weight, 1.5 to 2.25 parts by weight, 1.It may be included in 5 to 2 parts by weight, 2 to 10 parts by weight, 2 to 8 parts by weight, 2 to 7 parts by weight, 2 to 6 parts by weight, 2 to 5 parts by weight, 2 to 4 parts by weight, 2 to 3.5 parts by weight, 2 to 3 parts by weight, 2 to 2.5 parts by weight, or 2 to 2.25 parts by weight, but is not limited thereto.

[0040] In one embodiment, to control the volatility of water, an alcohol such as ethanol or a polyalcohol may be mixed with the water binder.

[0041]

[0042] In one embodiment, the powder-phase raw material of the cosmetic composition of the present application described above may additionally include one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate. For the purposes of the present application, one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate may be used to replace talc, but are not limited thereto. More specifically, the mica may be one or more selected from the group consisting of muscovite, sericite, and synthetic mica, but are not limited thereto.

[0043] In one embodiment, the cosmetic composition of the present application described above may comprise one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate in an amount of 30% to 60% by weight based on the total weight of the cosmetic composition, and more specifically, 30% to 60% by weight, 30% to 50% by weight, 30% to 49.5% by weight, 30% to 49.25% by weight, 30% to 49% by weight, 40% to 60% by weight, 40% to 50% by weight, 40% to 49.5% by weight, 40% to 49.25% by weight, 46% to 60% by weight, 46% to 50% by weight, 46% to 49% by weight. 49.5 wt%, 46 wt% to 49.25 wt%, 46 wt% to 49 wt%, 47.25 wt% to 60 wt%, 47.25 wt% to 50 wt%, 47.25 wt% to 49.5 wt%, 47.25 wt% to 49.25 wt%, 47.25 wt% to 49 wt%, 48.25 wt% to 60 wt%, 48.25 wt% to 50 wt%, 48.25 wt% to 49.5 wt%, 48.25 wt% to 49.25 wt%, 48.25 wt% to 49 wt%, 48.5 wt% to 60 wt%, 48.5 wt% to 50 wt%, 48.5 wt% to 49.5 wt%, 48.5 wt% to 49 wt%, 48.5 wt% to 60 wt%, 48.5 wt% to 50 wt%, 48.5 wt% to 49.5 wt%, 48.5 wt% It may be included in an amount of up to 49.25 weight%, or 48.5 weight% to 49 weight%, but is not limited thereto.

[0044] In one embodiment, one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate may be surface-treated or not surface-treated, or may be a mixture of surface-treated and non-surface-treated materials.

[0045] In one embodiment, the surface treatment may be performed using one or more selected from the group consisting of silicon-based materials, fatty acids, fluorinated compounds, amino acids or derivatives thereof, waxes, polymers, metal compounds, organosilanes, and organosiloxanes, but is not limited thereto. More specifically, the surface treatment may be performed using a silicon-based material, and more specifically, may be performed using one or more selected from the group consisting of methicone, dimethicone, cyclomethicone, phenyltrimethicone, trimethylsiloxysilicate, amodimethicone, and triethoxycaprylylsilane, and even more specifically, may be performed using methicone, but is not limited thereto.

[0046] In one embodiment, the powder-phase raw material of the cosmetic composition of the present application described above may additionally include spherical powder.

[0047] In this application, “spherical powder” refers to a powder in the form of spherical particles used to improve spreadability, transparency, skin adhesion, etc., in a cosmetic composition.

[0048] In one embodiment, the spherical powder may be one or more selected from the group consisting of silica, polymethyl methacrylate, and vinyl dimethicone / methicone silsesquioxane crosspolymer, but is not limited thereto, and may be those commonly used in the industry.

[0049] In one embodiment, the cosmetic composition of the present application described above may comprise the spherical powder in an amount of 30% to 60% by weight based on the total weight of the cosmetic composition, and more specifically, 5% to 30% by weight, 5% to 25% by weight, 5% to 20% by weight, 5% to 15% by weight, 5% to 12.5% ​​by weight, 5% to 11% by weight, 5% to 10% by weight, 5% to 9.85% by weight, 7.5% to 30% by weight, 7.5% to 25% by weight, 7.5% to 20% by weight, 7.5% to 15% by weight, 7.5% to 12.5% ​​by weight, 7.5% to 11% by weight, 7.5% to 10% by weight, 7.5% to 9.85% by weight, 9 wt% to 30 wt%, 9 wt% to 25 wt%, 9 wt% to 20 wt%, 9 wt% to 15 wt%, 9 wt% to 12.5 wt%, 9 wt% to 11 wt%, 9 wt% to 10 wt%, 9 wt% to 9.85 wt%, 9.25 wt% to 30 wt%, 9.25 wt% to 25 wt%, 9.25 wt% to 20 wt%, 9.25 wt% to 15 wt%, 9.25 wt% to 12.5 wt%, 9.25 wt% to 11 wt%, 9.25 wt% to 10 wt%, 9.25 wt% to 9.85 wt%, 9.4 wt% to 30 wt%, 9.4 wt% to 25 wt%, 9.4 wt% to 20 wt%, 9.4 wt% to 15 wt%, 9.4 wt% to 12.5 wt%, 9.4 wt% to 11 wt%, 9.4 wt% to 10 wt%, 9.4 wt% to 9.85 wt%, 9.6 wt% to 30 wt%, 9.6 wt% to 25 wt%, 9.6 wt% to 20 wt%, 9.6 wt% to 15 wt%, 9.6 wt% to 12.5 wt%, 9.6 wt% to 11 wt%, 9.6 wt% to 10 wt%, 9.6 wt% to 9.It may be included in 85 wt%, 9.75 wt% to 30 wt%, 9.75 wt% to 25 wt%, 9.75 wt% to 20 wt%, 9.75 wt% to 15 wt%, 9.75 wt% to 12.5 wt%, 9.75 wt% to 11 wt%, 9.75 wt% to 10 wt%, or 9.75 wt% to 9.85 wt%, but is not limited thereto.

[0050] In one embodiment, the powder-phase raw material of the cosmetic composition of the present application described above may additionally include a powder binder.

[0051] In this application, “powder binder” refers to an ingredient used to increase the bonding strength between particles in a powder-based cosmetic composition and to impart water repellency, spreadability, and physical stability, and may be used for the purpose of supplementing the bonding strength that may be reduced due to the use of the spherical powder according to the purpose of this application.

[0052] In one embodiment, the powder binder may be a metal soap binder, a naturally derived synthetic wax, or a combination thereof, but is not limited thereto, and may be one commonly used in the art. The metal soap binder may be one or more selected from the group consisting of magnesium stearate, zinc stearate, and magnesium myristate, but is not limited thereto. The naturally derived synthetic wax may be one or more selected from the group consisting of carnauba wax, beeswax, and polyethylene wax, but is not limited thereto.

[0053] In one embodiment, the cosmetic composition of the present application described above may comprise the powder binder in an amount of 1% to 10% by weight based on the total weight of the cosmetic composition, and more specifically, 1% to 10% by weight, 1% to 5% by weight, 1% to 3% by weight, 1% to 2.96% by weight, 1% to 2.95% by weight, 2% to 10% by weight, 2% to 5% by weight, 2% to 3% by weight, 2% to 2.96% by weight, 2% to 2.95% by weight, 2.8% to 10% by weight, 2.8% to 5% by weight, 2.8% to 3% by weight, 2.8% to 2.96% by weight, 2.8% to 2.95% by weight, 2.85% to 10% by weight, and 2.85% by weight. It may be included in an amount of up to 5 wt%, 2.85 wt% to 3 wt%, 2.85 wt% to 2.96 wt%, 2.85 wt% to 2.95 wt%, 2.9 wt% to 10 wt%, 2.9 wt% to 5 wt%, 2.9 wt% to 3 wt%, 2.9 wt% to 2.96 wt%, or 2.9 wt% to 2.95 wt%, but is not limited thereto.

[0054] In one embodiment, the powder-phase raw material of the cosmetic composition of the present application described above may additionally include a pigment. The pigment is a fine powder that exists dispersed without dissolving in a solvent, and is also referred to as a pigment. In this embodiment, the pigment may be an inorganic pigment. The inorganic pigment may be further classified into a coloring pigment that imparts color to cosmetics, a white pigment that controls the covering power of the skin, an extender pigment that adjusts the color tone as a diluent for the coloring pigment and plays a role in the texture of use, such as the ductility and adhesiveness of the product, and the formulation of the product, and a pearlescent pigment that has a special optical effect used to impart a pearlescent luster to the color, or to impart an iris color or metallic luster. In one embodiment, the inorganic pigment may be one or more of titanium dioxide and iron oxide, but is not limited thereto, and may be one that is commonly used in the art. The iron oxide may include, but is not limited to, yellow iron oxide, red iron oxide, black iron oxide, or a combination thereof. The inorganic pigment may be surface-treated or unsurface-treated, or may be a mixture of surface-treated inorganic pigment and unsurface-treated inorganic pigment. The surface treatment may be one or more selected from the group consisting of silicon-based materials, fatty acids, fluorinated compounds, amino acids or derivatives thereof, waxes, polymers, metal compounds, organosilanes, and organosiloxanes, but is not limited thereto.More specifically, the surface treatment of the pigment may be surface treated with a silicone-based material, and more specifically, may be surface treated with one or more selected from the group consisting of methicone, dimethicone, cyclomethicone, phenyltrimethicone, trimethylsiloxysilicate, amodimethicone, and triethoxycaprylylsilane, and even more specifically, may be surface treated with triethoxycaprylylsilane, but is not limited thereto.

[0055] In one embodiment, the cosmetic composition of the present application described above may contain the pigment in an amount of 1% to 5% by weight based on the total weight of the cosmetic composition, and more specifically, 1% to 5% by weight, 1% to 3.5% by weight, 1% to 2.75% by weight, 1% to 2.7% by weight, 2.5% to 5% by weight, 2.5% to 3.5% by weight, 2.5% to 2.75% by weight, 2.5% to 2.7% by weight, 2.6% to 5% by weight, 2.6% to 3.5% by weight, 2.6% to 2.75% by weight, 2.6% to 2.7% by weight, 2.65% to 5% by weight, 2.65% to 3.5% by weight, 2.65% to 2.75% by weight, or It may be included in an amount of 2.65% to 2.7% by weight, but is not limited thereto.

[0056] In one embodiment, the powder-phase raw material of the cosmetic composition of the present application described above may additionally include aluminum starch octenylsuccinate. The aluminum starch octenylsuccinate is an aluminum salt formed by the reaction of anhydrous octenylsuccinate with aluminum, and it has hydrophobicity, which can prevent the powder-phase raw material from condensing or forming lumps due to moisture.

[0057] In one embodiment, the cosmetic composition of the present application described above may comprise the aluminum starch octenylsuccinate in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition, and more specifically, 5% to 30% by weight, 5% to 25% by weight, 5% to 20% by weight, 5% to 15% by weight, 5% to 12.5% ​​by weight, 5% to 11% by weight, 5% to 10% by weight, 5% to 9.85% by weight, 7.5% to 30% by weight, 7.5% to 25% by weight, 7.5% to 20% by weight, 7.5% to 15% by weight, 7.5% to 12.5% ​​by weight, 7.5% to 11% by weight, 7.5% to 10% by weight, 7.5% to 9.85 wt%, 9 wt% to 30 wt%, 9 wt% to 25 wt%, 9 wt% to 20 wt%, 9 wt% to 15 wt%, 9 wt% to 12.5 wt%, 9 wt% to 11 wt%, 9 wt% to 10 wt%, 9 wt% to 9.85 wt%, 9.25 wt% to 30 wt%, 9.25 wt% to 25 wt%, 9.25 wt% to 20 wt%, 9.25 wt% to 15 wt%, 9.25 wt% to 12.5 wt%, 9.25 wt% to 11 wt%, 9.25 wt% to 10 wt%, 9.25 wt% to 9.85 wt%, 9.4 wt% to 30 wt%, 9.4 wt% to 25 wt%, 9.4 wt% to 20 wt%, 9.4 wt% to 15 wt%, 9.4 wt% to 12.5 wt%, 9.4 wt% to 11 wt%, 9.4 wt% to 10 wt%, 9.4 wt% to 9.85 wt%, 9.6 wt% to 30 wt%, 9.6 wt% to 25 wt%, 9.6 wt% to 20 wt%, 9.6 wt% to 15 wt%, 9.6 wt% to 12.5 wt%, 9.6 wt% to 11 wt%, 9.6 wt% to 10 wt%, 9.It may be included in an amount of 6 wt% to 9.85 wt%, 9.75 wt% to 30 wt%, 9.75 wt% to 25 wt%, 9.75 wt% to 20 wt%, 9.75 wt% to 15 wt%, 9.75 wt% to 12.5 wt%, 9.75 wt% to 11 wt%, 9.75 wt% to 10 wt%, or 9.75 wt% to 9.85 wt%, but is not limited thereto.

[0058] In the present application, the cosmetic composition may be used as a raw material for compression molding to manufacture solid powder cosmetics (compressed powder cosmetics).

[0059] In the present application, the cosmetic composition may be for the manufacture of solid powder cosmetics (compressed powder cosmetics) (suitable for manufacture).

[0060] More specifically, the cosmetic composition may be intended for manufacturing a solid powder cosmetic by a dry process (suitable for manufacturing by a dry process).

[0061] Accordingly, another aspect of the present application provides a composition for manufacturing cosmetics comprising a powdered raw material including kaolin and hydrophobic silica, and an oil binder, wherein the kaolin is included in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition.

[0062] The above-described composition for manufacturing cosmetics may additionally include water. The water is as described in the cosmetic composition, which is another aspect of the present application described above.

[0063] The powder-phase raw material of the above-described cosmetic composition may additionally include one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate; spherical powder; powder binder; pigment; and one or more selected from the group consisting of aluminum starch octenylsuccinate. The one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate; spherical powder; powder binder; pigment; and aluminum starch octenylsuccinate are as described in the cosmetic composition above.

[0064] The cosmetic composition or composition for manufacturing cosmetics of the present application may additionally include one or more conventional additives such as fragrances, thickeners, preservatives, surfactants, humectants, chelating agents, emollients, UV absorbers, thickeners, disinfectants, antioxidants, plant extracts, pH adjusters, and alcohols. The types and amounts of additives can be easily determined by a person skilled in the art based on techniques known in the art.

[0065] In one embodiment, the cosmetic composition or cosmetic manufacturing composition of the present application described above may not contain talc.

[0066] As demonstrated in the embodiments to be described below, the cosmetic composition or composition for manufacturing cosmetics of the present application utilizes water as a binder, thereby enabling the compression molding of cosmetics without talc, which was previously difficult to achieve without talc. Furthermore, the cosmetic composition of the present application possesses shape stability and excellent usability, and has the effect of maintaining moisture within the cosmetic composition over time while using water as a binder.

[0067]

[0068] In the present application, the cosmetic product may be a powder cosmetic, more specifically a solid powder cosmetic (compressed powder cosmetic), and even more specifically a dry solid powder cosmetic (dry compressed powder cosmetic).

[0069] In this application, the term 'solid powder cosmetic' may be used interchangeably with 'compressed powder cosmetic' or 'compressed molded powder cosmetic,' and refers to a cosmetic formed into a solid form by compressing fine powder particles. Unlike loose powder, this solid powder cosmetic is fixed into a single mass by compression, making it easy to carry and use, and providing excellent physical stability against external impact.

[0070] Loose powder is a cosmetic in powder form characterized by its tendency to scatter freely; however, it is inconvenient to carry as it must be applied using a brush or puff. Additionally, because it exists in a powder state, it is bulky and has low oil content, primarily serving to set makeup. Generally, the main ingredients of loose powder consist of talc, mica, and corn starch.

[0071] Solid powder cosmetics have a solidified form to improve upon the inconvenience of such loose powders. Solidification methods include melting an oily base, mixing the powder, and cooling to solidify it, and using oil as a binder for compression molding. The present invention adopts the latter method to provide a solid powder cosmetic that has low oiliness, spreadability similar to loose powder, and excellent physical stability.

[0072]

[0073] Another aspect of the present application provides a cosmetic product comprising the cosmetic composition or cosmetic manufacturing composition of the present application described above.

[0074] Another aspect of the present application provides a cosmetic product manufactured by compression molding the cosmetic composition or cosmetic manufacturing composition of the present application described above.

[0075] In one embodiment, the cosmetic may be a powder cosmetic, more specifically a solid powder cosmetic (compressed powder cosmetic), and even more specifically a dry solid powder cosmetic (dry compressed powder cosmetic). The details regarding the cosmetic are as described above regarding the cosmetic composition or the composition for manufacturing cosmetics.

[0076] In one embodiment, the cosmetic product may be a pressed powder for makeup. The pressed powder for makeup may be a two-way cake, compact, powder pact, pressed powder, powder foundation, blush, eyeshadow, highlighter, concealer, contouring powder, color correcting powder, body powder, or shading powder, but is not limited thereto.

[0077] In one embodiment, the hardness of the cosmetic of the present application described above may be 70 to 85 based on Asker-C, and more specifically, may be 70 to 85, 70 to 84, 70 to 83, 70 to 82, 73 to 85, 73 to 84, 73 to 83, 73 to 82, 75 to 85, 75 to 84, 75 to 83, 75 to 82, 76 to 85, 76 to 84, 76 to 83, 76 to 82, 77 to 85, 77 to 84, 77 to 83, or 77 to 82, but is not limited thereto.

[0078] In this application, 'hardness' refers to durometer hardness and may be used interchangeably.

[0079] The above hardness may be measured according to the JIS K 7312 standard, but is not limited thereto.

[0080] As demonstrated in the embodiments to be described below, when using the cosmetic composition or cosmetic manufacturing composition of the present application, it is possible to manufacture a solid powder cosmetic with excellent compression moldability and shape stability without containing talc. Furthermore, when using the cosmetic composition of the present application, a dry process can be used, which is simple and saves energy and costs, instead of relying on a wet process that requires additional expensive equipment and takes a long time to produce, thereby significantly improving the efficiency and economic viability of the manufacturing process.

[0081]

[0082] Another aspect of the present application provides a method for preparing a cosmetic composition comprising: (1) mixing powdered raw materials including kaolin and hydrophobic silica; (2) adding and mixing an oil binder to the mixture obtained in step (1); and (3) adding and mixing water to the mixture obtained in step (2), wherein the kaolin is included in an amount of 5% to 30% by weight with respect to the total weight of the cosmetic composition, and the water is included in an amount of 0.5% to 10% by weight with respect to the total weight of the cosmetic composition.

[0083] In one embodiment, the cosmetic composition may be the cosmetic composition described in another aspect of the present application.

[0084] In one embodiment, the cosmetic composition may be a cosmetic composition for manufacturing described in another aspect of the present application.

[0085] The above kaolin is as described in the content relating to the cosmetic composition, which is another aspect of the present application described above.

[0086] In one embodiment, the kaolin may be included in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition, and more specifically, 5% to 30% by weight, 5% to 25% by weight, 5% to 20% by weight, 5% to 15% by weight, 5% to 12.5% ​​by weight, 5% to 11% by weight, 5% to 10% by weight, 5% to 9.85% by weight, 7.5% to 30% by weight, 7.5% to 25% by weight, 7.5% to 20% by weight, 7.5% to 15% by weight, 7.5% to 12.5% ​​by weight, 7.5% to 11% by weight, 7.5% to 10% by weight, 7.5% to 9.85% by weight, 9% to 30% by weight. 9 wt% to 25 wt%, 9 wt% to 20 wt%, 9 wt% to 15 wt%, 9 wt% to 12.5 wt%, 9 wt% to 11 wt%, 9 wt% to 10 wt%, 9 wt% to 9.85 wt%, 9.25 wt% to 30 wt%, 9.25 wt% to 25 wt%, 9.25 wt% to 20 wt%, 9.25 wt% to 15 wt%, 9.25 wt% to 12.5 wt%, 9.25 wt% to 11 wt%, 9.25 wt% to 10 wt%, 9.25 wt% to 9.85 wt%, 9.4 wt% to 30 wt%, 9.4 wt% to 25 wt%, 9.4 wt% to 20 wt%, 9.4 wt% to 15 wt%, 9.4 wt% to 12.5 wt%, 9.4 wt% to 11 wt%, 9.4 wt% to 10 wt%, 9.4 wt% to 9.85 wt%, 9.6 wt% to 30 wt%, 9.6 wt% to 25 wt%, 9.6 wt% to 20 wt%, 9.6 wt% to 15 wt%, 9.6 wt% to 12.5 wt%, 9.6 wt% to 11 wt%, 9.6 wt% to 10 wt%, 9.6 wt% to 9.85 wt%, 9.It may be included in an amount of 75 wt% to 30 wt%, 9.75 wt% to 25 wt%, 9.75 wt% to 20 wt%, 9.75 wt% to 15 wt%, 9.75 wt% to 12.5 wt%, 9.75 wt% to 11 wt%, 9.75 wt% to 10 wt%, or 9.75 wt% to 9.85 wt%, but is not limited thereto.

[0087] The above-mentioned hydrophobic silica is as described in the content relating to the cosmetic composition, which is another aspect of the present application described above.

[0088] In one embodiment, the hydrophobic silica may be one or more selected from the group consisting of silica dimethyl sililate, silica sililate, silica dimethicone sililate, and silica caprylyl sililate, but is not limited thereto, and may be those commonly used in the industry.

[0089] In one embodiment, the cosmetic composition of the present application described above may include the hydrophobic silica in an amount of 0.5 wt% to 3 wt% based on the total weight of the cosmetic composition, and more specifically, 0.5 wt% to 3 wt%, 0.5 wt% to 2.5 wt%, 0.5 wt% to 2 wt%, 0.5 wt% to 1.75 wt%, 0.5 wt% to 1.5 wt%, 0.75 wt% to 3 wt%, 0.75 wt% to 2.5 wt%, 0.75 wt% to 2 wt%, 0.75 wt% to 1.75 wt%, 0.75 wt% to 1.5 wt%, 1 wt% to 3 wt%, 1 wt% to 2.5 wt%, 1 wt% to 2 wt%, 1 wt% to 1.75 wt%, 1 wt% to 1.5 wt%, 1.25 wt% wt% to 3 wt%, 1.25 wt% to 2.5 wt%, 1.25 wt% to 2 wt%, 1.25 wt% to 1.75 wt%, 1.25 wt% to 1.5 wt%, 1.4 wt% to 3 wt%, 1.4 wt% to 2.5 wt%, 1.4 wt% to 2 wt%, 1.4 wt% to 1.75 wt%, 1.4 wt% to 1.5 wt%, 1.43 wt% to 3 wt%, 1.43 wt% to 2.5 wt%, 1.43 wt% to 2 wt%, 1.43 wt% to 1.75 wt%, 1.43 wt% to 1.5 wt%, 1.45 wt% to 3 wt%, 1.45 wt% to 2.5 wt%, 1.45 wt% to 2 wt% It may be included in weight%, 1.45 weight% to 1.75 weight%, 1.45 weight% to 1.5 weight%, 1.47 weight% to 3 weight%, 1.47 weight% to 2.5 weight%, 1.47 weight% to 2 weight%, 1.47 weight% to 1.75 weight%, or 1.47 weight% to 1.5 weight%, but is not limited thereto.

[0090] The above water is as described in the content relating to the cosmetic composition, which is another aspect of the present application described above.

[0091] In one embodiment, the water may be added (included) in an amount of 0.5% to 10% by weight based on the total weight of the cosmetic composition, and more specifically, 0.5% to 10% by weight, 0.5% to 7.5% by weight, 0.5% to 6% by weight, 0.5% to 4.5% by weight, 0.5% to 3.5% by weight, 0.5% to 2.5% by weight, 0.5% to 2% by weight, 0.5% to 1.98% by weight, 0.5% to 1.97% by weight, 0.5% to 1.96% by weight, 0.75% to 10% by weight, 0.75% to 7.5% by weight, 0.75% to 6% by weight, 0.75% to 4.5% by weight, and 0.75% to 3.5% by weight. wt%, 0.75 wt% to 2.5 wt%, 0.75 wt% to 2 wt%, 0.75 wt% to 1.98 wt%, 0.75 wt% to 1.97 wt%, 0.75 wt% to 1.96 wt%, 1 wt% to 10 wt%, 1 wt% to 7.5 wt%, 1 wt% to 6 wt%, 1 wt% to 4.5 wt%, 1 wt% to 3.5 wt%, 1 wt% to 2.5 wt%, 1 wt% to 2 wt%, 1 wt% to 1.98 wt%, 1 wt% to 1.97 wt%, 1 wt% to 1.96 wt%, 1.25 wt% to 10 wt%, 1.25 wt% to 7.5 wt%, 1.25 wt% to 6 wt%, 1.25 wt% to 4.5 wt%, 1.25 wt% to 3.5 wt%, 1.25 wt% to 2.5 wt%, 1.25 wt% to 2 wt%, 1.25 wt% to 1.98 wt%, 1.25 wt% to 1.97 wt%, 1.25 wt% to 1.96 wt%, 1.5 wt% to 10 wt%, 1.5 wt% to 7.5 wt%, 1.5 wt% to 6 wt%, 1.5 wt% to 4.5 wt%, 1.5 wt% to 3.5 wt%, 1.5 wt% to 2.5 wt%, 1.5 wt% to 2 wt%, 1.5 wt% to 1.98 wt%, 1.5 wt% to 1.97 wt%, 1.5 wt% to 1.96 wt%, 1.75 wt% to 10 wt%, 1.75 wt% to 7.5 wt%, 1.75 wt% to 6 wt%, 1.75 wt% to 4.5 wt%, 1.75 wt% to 3.5 wt%, 1.75 wt% to 2.5 wt%, 1.75 wt% to 2 wt%, 1.75 wt% to 1.98 wt%, 1.75 wt% to 1.97 wt%, 1.75 wt% to 1.96 wt%, 1.8 wt% to 10 wt%, 1.8 wt% to 7.5 wt%, 1.8 wt% to 6 wt%, 1.8 It may be added (included) in an amount of 1.8% to 4.5% by weight, 1.8% to 3.5% by weight, 1.8% to 2.5% by weight, 1.8% to 2% by weight, 1.8% to 1.98% by weight, 1.8% to 1.97% by weight, or 1.8% to 1.96% by weight, but is not limited thereto.

[0092] In one embodiment, the water may be added (included) in an amount of 0.5 to 10 parts by weight per 100 parts by weight of the powder-phase raw material and oil binder, and more specifically, 0.5 to 10 parts by weight, 0.5 to 8 parts by weight, 0.5 to 7 parts by weight, 0.5 to 6 parts by weight, 0.5 to 5 parts by weight, 0.5 to 4 parts by weight, 0.5 to 3.5 parts by weight, 0.5 to 3 parts by weight, 0.5 to 2.5 parts by weight, 0.5 to 2.25 parts by weight, 0.5 to 2 parts by weight, 1 to 10 parts by weight, 1 to 8 parts by weight, 1 to 7 parts by weight, 1 to 6 parts by weight, 1 to 5 parts by weight, and 1 to 4 parts by weight. parts by weight, 1 to 3.5 parts by weight, 1 to 3 parts by weight, 1 to 2.5 parts by weight, 1 to 2.25 parts by weight, 1 to 2 parts by weight, 1.25 to 10 parts by weight, 1.25 to 8 parts by weight, 1.25 to 7 parts by weight, 1.25 to 6 parts by weight, 1.25 to 5 parts by weight, 1.25 to 4 parts by weight, 1.25 to 3.5 parts by weight, 1.25 to 3 parts by weight, 1.25 to 2.5 parts by weight, 1.25 to 2.25 parts by weight, 1.25 to 2 parts by weight, 1.5 to 10 parts by weight, 1.5 to 8 parts by weight, 1.5 to 7 parts by weight parts by weight, 1.5 to 6 parts by weight, 1.5 to 5 parts by weight, 1.5 to 4 parts by weight, 1.5 to 3.5 parts by weight, 1.5 to 3 parts by weight, 1.5 to 2.5 parts by weight, 1.5 to 2.25 parts by weight, 1.It may be added (included) in an amount of 5 to 2 parts by weight, 2 to 10 parts by weight, 2 to 8 parts by weight, 2 to 7 parts by weight, 2 to 6 parts by weight, 2 to 5 parts by weight, 2 to 4 parts by weight, 2 to 3 parts by weight, 2 to 3.5 parts by weight, 2 to 2.5 parts by weight, or 2 to 2.25 parts by weight, but is not limited thereto.

[0093] In one embodiment, the raw material on the powder may additionally include one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate, spherical powder, powder binder, pigment, or a combination thereof.

[0094] The details regarding one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate, spherical powder, powder binder, pigment, and weight percent thereof are as described above in the details regarding the cosmetic composition, which is another aspect of the present application.

[0095] In one embodiment, the method for preparing the cosmetic composition of the present application described above may additionally include a step of grinding the mixture after step (1), after step (2), or after step (1) and after step (2).

[0096] In one embodiment, adding the oil binder in step (2) above may be spraying the oil binder, but is not limited thereto.

[0097] In one embodiment, the method for preparing the cosmetic composition of the present application described above may additionally include (2-1) a step of cooling the mixture obtained in step (2) to 20°C to 35°C after step (2). More specifically, the mixture obtained in step (2) may be cooled to 20°C to 35°C, 20°C to 30°C, 20°C to 27.5°C, or 20°C to 25°C. If the temperature of the mixture is high, the added water binder may not disperse and may run down the walls or lid of the mixer, and may clump together with the powder.

[0098] In one embodiment, adding water in step (3) above may be spraying water, but is not limited thereto.

[0099] In one embodiment, when water is added in step (3), the mixture may be mixed at the same time. At this time, the mixing speed may be 50 rpm to 400 rpm, 50 rpm to 350 rpm, 50 rpm to 300 rpm, 100 rpm to 400 rpm, 100 rpm to 350 rpm, 100 rpm to 300 rpm, 200 rpm to 400 rpm, 200 rpm to 350 rpm, or 200 rpm to 300 rpm, more specifically 300 rpm, but is not limited thereto. By mixing the mixture at the above speed, clumping of the contents due to heat generation can be reduced.

[0100] In one embodiment, water may be added in step (3), and the mixture may be mixed at a mixing speed of 200 rpm to 600 rpm. More specifically, the mixture may be mixed at a mixing speed of 200 rpm to 600 rpm, 200 rpm to 550 rpm, 200 rpm to 500 rpm, 200 rpm to 450 rpm, 200 rpm to 400 rpm, 300 rpm to 600 rpm, 300 rpm to 550 rpm, 300 rpm to 500 rpm, 300 rpm to 450 rpm, or 300 rpm to 400 rpm, more specifically 400 rpm. By mixing the mixture at the above speed, the mixture can be evenly mixed and swollen while reducing clumping of the contents due to heat generation. In addition, after the water spray in step (3) above, when mixing the mixture at a mixing speed of 200 rpm to 600 rpm, the mixture may be mixed for about 3 to 5 minutes so that the contents can be sufficiently wetted with water, and the mixing time may vary depending on the amount of contents to be mixed.

[0101] In one embodiment, the method for preparing the cosmetic composition of the present application described above may additionally include (3-1) a step of filtering the mixture obtained in step (3) after step (3).

[0102] In a specific embodiment, the mixture may be filtered using a 40 mesh to 60 mesh sieve in step (3-1), but is not limited thereto. More specifically, the mixture may be filtered using a 40 mesh to 60 mesh sieve, a 40 mesh to 50 mesh sieve, a 50 mesh to 70 mesh sieve, or a 50 mesh to 60 mesh sieve, more specifically a 50 mesh sieve, but is not limited thereto. Since using a grinder can cause heat to be generated and the contents to clump together, the mixture is filtered using the filter sieve.

[0103] In one embodiment, in the step after step (3), the filtered mixture may be naturally degassed and aged for 1 day or more, more specifically 1 to 10 days, 1 to 5 days, 1 to 3 days, or 1 to 2 days.

[0104] Another aspect of the present application provides a cosmetic composition prepared by the manufacturing method described above.

[0105]

[0106] Another aspect of the present application provides a method for manufacturing a cosmetic product comprising the step of compressing and molding the cosmetic composition of the present application described above.

[0107] In one embodiment, the cosmetic composition may be the cosmetic composition described in another aspect of the present application.

[0108] In one embodiment, the cosmetic composition may be a cosmetic composition for manufacturing described in another aspect of the present application.

[0109] In one embodiment, the cosmetic composition may be prepared by the method of preparing a cosmetic composition described in another aspect of the present application.

[0110] The above cosmetic composition and cosmetic are as described in the cosmetic composition and cosmetic of another aspect of the present application described above.

[0111] The step of compressing and molding the above cosmetic composition may be performed by applying a pressure of 60 bar to 120 bar, and more specifically, by applying a pressure of 60 bar to 120 bar, 60 bar to 100 bar, 60 bar to 90 bar, 75 bar to 120 bar, 75 bar to 100 bar, 75 bar to 90 bar, 80 bar to 120 bar, 80 bar to 100 bar, or 80 bar to 90 bar, more specifically 90 bar, but is not limited thereto.

[0112] The step of compressing and molding the above cosmetic composition may be performed for 1 second to 30 seconds, and more specifically for 1 second to 30 seconds, 1 second to 20 seconds, 1 second to 10 seconds, 1 second to 7.5 seconds, 1 second to 5 seconds, 2 seconds to 30 seconds, 2 seconds to 20 seconds, 2 seconds to 10 seconds, 2 seconds to 7.5 seconds, 2 seconds to 5 seconds, 3 seconds to 30 seconds, 3 seconds to 20 seconds, 3 seconds to 10 seconds, 3 seconds to 7.5 seconds, 3 seconds to 5 seconds, 4 seconds to 30 seconds, 4 seconds to 20 seconds, 4 seconds to 10 seconds, 4 seconds to 7.5 seconds, or 4 seconds to 5 seconds, more specifically for 5 seconds, but is not limited thereto.

[0113] When using the method for manufacturing a cosmetic composition and / or a cosmetic of the present application, it is possible to manufacture a cosmetic with excellent compression moldability and shape stability while using a dry process that is simple and can reduce energy and costs.

[0114] On the other hand, even when using the firing-type wet process shown in Fig. 3, the cosmetic of the present application can be manufactured; however, since the water binder content must be increased to 15% to 30% by weight, a separate dough process is required, and an extruder and cutting operation are required to extrude the dough and place the contents onto a plate. In addition, the cut contents are placed onto a plate and subjected to primary compression under low pressure for drying; drying time is required for 8 hours in an oven at 70–80°C or for more than one day in a drying chamber at 40°C. During this drying process, moisture evaporates and the contents on the plate condense, and tolerances between the plate and the contents occur due to condensation. To eliminate these tolerances, secondary compression molding under appropriate pressure is required. As such, compared to the dry process, the firing-type wet process includes a doughing process, an extrusion process, a cutting process, a drying process, and two compression molding processes, requiring additional equipment and increasing production time, resulting in lower productivity and economic efficiency compared to the dry process.

[0115] In addition, the cosmetic of the present application can be manufactured using the slurry-type wet process shown in FIG. 4, but the process includes the step of mixing an oil binder and a solvent (IPA: Isopropyl alcohol or Isopar G: Isoparaffine G, etc.) into a liquid (slurry) phase using a disperser mixer with the mixed and ground powder, degassing the resulting slurry to remove bubbles, and molding it using a molding machine dedicated to slurry. Depending on the filling method, the molding machine dedicated to slurry includes back injection, which fills from the bottom using a perforated dish; front injection, which injects contents from above the dish and then molds; and side injection, which fills contents from the side. Compared to the above-mentioned firing-type wet process, the mixing process is replaced by a process of liquefying with a slurry, the extrusion and cutting processes are replaced by filling with a quantitative filler, and the condensation of the contents during the first drying is replaced by a process of suctioning the solvent during the slurry filling process. The molded contents are completed after undergoing a drying process of about 48 hours. In the case of the slurry-type wet process, the filling equipment is expensive and requires skilled workers, so productivity and economic efficiency are lower compared to the dry process.

[0116]

[0117] The present application relates to a cosmetic composition that does not contain talc and a method for manufacturing the same. Cosmetics produced from the cosmetic composition of the present application are safe for the human body as they do not contain talc, while possessing the compression moldability and shape stability of talc, and have the effect of stably maintaining moisture within the composition even while containing water as a binder. Furthermore, they have the effect of enabling the production of cosmetics with excellent compression moldability and shape stability using a dry process, which is more economical than a wet process.

[0118]

[0119] Figure 1 shows the weight loss test results of a solid powder cosmetic according to one manufacturing example of the present application.

[0120] FIG. 2 is a manufacturing process diagram of a solid powder cosmetic according to one embodiment of the present application.

[0121] Figure 3 shows an example of a manufacturing process for a solid powder cosmetic by a sintering type wet compression molding method.

[0122] Figure 4 shows an example of a manufacturing process for a solid powder cosmetic by a slurry-type wet compression molding method.

[0123]

[0124] The present application will be described in more detail below through examples. These examples are intended solely to illustrate the present application more specifically, and it will be obvious to those skilled in the art that the scope of the present application is not limited by these examples according to the gist of the application.

[0125]

[0126] Examples

[0127]

[0128] (Throughout this specification, "%" used to indicate the concentration of a particular substance is (weight / weight) % for solid / solid, (weight / volume) % for solid / liquid, and (volume / volume) % for liquid / liquid, unless otherwise noted.)

[0129]

[0130] Experimental Example 1: Preparation of Comparative Examples 1 to 5, and evaluation of hardness and drop stability

[0131] 1-1. Preparation of Comparative Examples 1 to 5

[0132] To evaluate the molding stability of a cosmetic composition depending on whether talc is included, 100g of a cosmetic composition was prepared by combining the ingredients in Table 1 below. Specifically, the powder raw materials were placed in a blender (Highbel Grinder HGR-2000) and mixed for 1 minute to prepare a powder mixture. Subsequently, the oil binder was heated to 65°C, placed on top of the powder mixture, and mixed with a blender for 30 seconds. The resulting mixture was placed in an aluminum dish (diameter 54mm, height 5mm) and compression molded using a hydraulic press (90 bar, 5 seconds).

[0133] Cosmetic composition for manufacturing solid powder cosmetics (wt%) Component Name Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Powder Talc 5 2.25 ---- Mica 15.00 6 7.25 15.00 15.00 15.00 Kaolin 10.00 10.00 6 2.25 10.00 10.00 Corn Starch 5.00 5.00 5.00 5 7.25 5.00 Silica 5.00 5.00 5.00 5.00 5 7.25 Magnesium Myristate 1.00 1.00 1.00 1.00 1.00 Titanium Dioxide (CI 77891) 2.00 2.00 2.00 2.00 2.00 Red Iron Oxide (CI 77491)0.100.100.100.100.10 Yellow Iron Oxide (CI 77492)0.600.600.600.600.60 Black Iron Oxide (CI 77499)0.050.050.050.050.05 Oil Binder Octyldodecyl Stearoyl Stearate 3.003.003.003.003.00 Squalane 3.003.003.003.003.00 Dimethicone 2.002.002.002.002.00 Diisostearyl Malate 1.001.001.001.001.00 - Total 100100100100100

[0134]

[0135] 1-2. Hardness and Drop Stability Evaluation

[0136] The hardness and drop stability of Comparative Examples 1 to 5 above were evaluated and are shown in Table 2 below. Hardness was expressed as the average value (based on Asker-C) obtained by measuring the hardness of five samples using a durometer (Teclock Hardness Tester, GS-701N, Type C, JIS K 7312), and drop stability was expressed as the number of times the molded product was dropped horizontally from a height of 50 cm onto a rubber plate 3 mm thick until it broke.

[0137] - Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Hardness 80 5 5 40 Moldable Moldable Drop Stability (Times) 5 11 Moldable Moldable

[0138] As shown in Table 2, Comparative Examples 2 and 3, which did not contain talc, had very low hardness and drop stability, and Comparative Examples 4 and 5 could not be molded, so their hardness and drop stability could not be measured. Thus, it was confirmed that when manufacturing solid powder cosmetics, if only an oil binder is used without talc as a powder raw material, the molding stability is very poor, making commercialization difficult.

[0139]

[0140] Experimental Example 2: Preparation and Evaluation of a Talc-Free Cosmetic Composition Containing a Water Binder

[0141] 2-1. Preparation of Preparation Examples 1 to 4, Comparative Example 6, and Comparative Example 7

[0142] In order to evaluate the physical properties of a solid powder cosmetic product manufactured using a cosmetic composition that additionally includes a water binder in addition to an oil binder, a solid powder cosmetic product was prepared to weigh 100g by combining the ingredients in Table 3 below. Specifically, the powder raw materials were mixed for 1 minute using a blender (Hybel grinder HGR-2000, Hybel) to prepare a powder mixture. Subsequently, the oil binder was heated to 65°C, placed on top of the powder mixture, and mixed with a blender for 30 seconds. Then, the water binder was added and mixed with the Hybel grinder HGR-2000 for 15 seconds. The resulting mixture was filtered through a 50 mesh, the mixed contents were placed in an aluminum dish (diameter 54 mm, height 5 mm), and compression molded (90 bar, 5 seconds) using a hydraulic press (cosmetic powder molding machine, Baroin).

[0143] As shown in Table 3 below, in Comparative Example 6, a water binder was not used, in Comparative Example 7, silica dimethyl silylate, which is a hydrophobic silica, was not used, and in Comparative Example 8, talc was used instead of mica and mica / methicone.

[0144]

[0145]

[0146]

[0147]

[0148] 2-2. Hardness and Drop Stability Evaluation

[0149] The hardness and drop stability of the above Preparation Examples 1 to 4, Comparative Example 6, and Comparative Example 7 were evaluated and are shown in Table 4 below. Hardness was expressed as the average value measured against the Asker-C standard using a durometer (Teclock Hardness Tester, GS-701N, Type C, JIS K 7312) for five samples, and drop stability was expressed as the number of times the molded product was dropped horizontally from a height of 50 cm onto a rubber plate 3 mm thick until it broke.

[0150] -Comparative Example 6 Manufacturing Example 1 Manufacturing Example 2 Manufacturing Example 3 Manufacturing Example 4 Comparative Example 7 Comparative Example 8 Hardness 73798283828484 Drop Stability (Times) 2455555

[0151] As shown in Table 4, it was found that in the case of Comparative Example 6, which does not contain water, the hardness and drop stability were significantly lower. On the other hand, in the case of Manufacturing Examples 2 to 4, the hardness and drop stability were similar to Comparative Example 8, which contains talc, confirming that when a water binder is included, the bonding strength between raw materials is enhanced, which can replace the compression moldability and shape stability of talc.

[0152] Meanwhile, Comparative Example 7, which does not contain silica dimethyl silylate, exhibited excellent hardness and drop stability, but during manufacturing, water was not easily mixed and dispersed in a clumped form, resulting in reduced manufacturing efficiency. In addition, when measuring hardness, the error in hardness values ​​was larger than that of other cosmetic products when measured at the center, top, bottom, left, and right of the plate, confirming that the formulation was not uniform and compression was not smooth.

[0153]

[0154] 2-3. Usability Evaluation

[0155] The usability of the above Preparation Examples 1 to 4 and Comparative Example 7 was evaluated. Usability was evaluated by having 10 users evaluate spreadability and adhesion on a 10-point scale in a blind test, and the average values ​​were compared. The results are shown in Table 5 below.

[0156] - Evaluation of Manufacturing Example 1, Manufacturing Example 2, Manufacturing Example 3, Manufacturing Example 4, Comparative Example 7 1. Spreadability 88766, Adhesion 88876 2. Spreadability 88775, Adhesion 910877 3. Spreadability 88776, Adhesion 88876 4. Spreadability 99875, Adhesion 109885 5. Spreadability 88765, Adhesion 88866 6. Spreadability 88765, Adhesion 99877 7. Spreadability 88755, Adhesion 89876 8. Spreadability 98876, Adhesion 99887 9. Spreadability 88876, Adhesion 99976 Spreadability 88755 Adhesion 88766 Average Spreadability 8.28.17.36.35.4 Adhesion 8.68.7876.2

[0157] As shown in Table 5, it was confirmed that all cosmetics of Preparation Examples 1 to 4 exhibited excellent usability. Among these, it was confirmed that the solid powder cosmetic of Preparation Example 2 had excellent hardness and drop stability, as well as excellent usability.

[0158] On the other hand, Comparative Example 7, which does not contain silica dimethyl silylate, was found to have poor water dispersion and poor mixing, resulting in reduced spreadability and adhesion compared to Preparation Examples 1 to 4.

[0159]

[0160] 2-4. Weight Loss Test

[0161] When commercializing a cosmetic composition, if a general container is used, there is a concern that the added water binder may volatilize. Therefore, to verify this, a weight loss test was conducted for 3 months on Preparation Example 2, which has excellent hardness and drop stability as well as excellent usability.

[0162] The packaging material of the container used was PCR ABS, and the metal tray was made of aluminum. The dimensions of the container were 73.36Φ±0.1Φ in length and width, and 14.39mm±0.2mm in height, with a capacity of 9.5 g. For the weight loss condition, three container samples were filled with contents and left at 40˚C for 3 months.

[0163] The content reduction rate was calculated using the following formula.

[0164] Content Loss Rate (%) = (Content Loss - Empty Container Loss) / Original Content X 100

[0165] The progress of the weight loss test is shown in Figure 1 and Table 6 below.

[0166] -Week 1Week 2Week 3Week 42Months3Months Average Weight Loss Rate 0.847 30.90 9 40.90 20.90 8 70.96 1 40.96 79 Deviation of Average Weight Loss Rate 0.847 30.06 21 -0.00 9 20.00 8 50.05 270.00 6 4 Average deviation from 2 weeks to 3 months 0.02 41

[0167] As shown in Figure 1 and Table 6, the average weight loss rate at 40°C was 0.9679% as a result of conducting the weight loss test for 3 months. During the first week of the weight loss test, water evaporated, showing a weight loss rate deviation of 0.8473%, but from the second week to the third month, the average weight loss rate deviation stabilized within 0.0241%.

[0168] From the above weight loss experiment, it was confirmed that from the second week onwards, the internal moisture of the cosmetic of Preparation Example 2 remained stable despite the influence of external temperature or relative humidity, preventing a deterioration of physical properties during use and allowing the cosmetic to be used stably for a long period.

[0169]

[0170] 2-5. Evaluation of Hardness Over Time

[0171] The change in hardness for Preparation Example 2 was measured for 3 months and is shown in Table 7 below. Hardness was expressed as the average value of the hardness of 5 samples measured using a durometer (Teclock Hardness Tester, GS-701N Type C JIS K 7312).

[0172] -0 days 1 week 2 weeks 3 weeks 4 weeks 2 months 3 months longitude 82787778777777

[0173] As a result of the hardness measurement, the hardness decreased until the first week and then remained constant from the second week onwards, showing results consistent with the weight loss test results of Experimental Examples 2-4 above. From this, it was confirmed that the moisture in the cosmetic of Preparation Example 2 can be stably maintained even when using a general container rather than a sealable container.

[0174]

[0175] 2-6. Evaluation of Caking Phenomenon

[0176] An experiment was conducted to compare the caking phenomenon of the cosmetics of Preparation Example 2 and Comparative Example 8. The hardness of the solid powder cosmetics of Preparation Example 2 and Comparative Example 8 was measured by taking the average value of five samples using a durometer (Teclock Hardness Tester, GS-701N Type C JIS K 7312). As a result, the hardness of Preparation Example 2 was found to be 80 to 82, and the hardness of Comparative Example 8 was found to be 83 to 85.

[0177] The caking phenomenon was measured by measuring the size of the caking generated by increasing the friction rotation speed of the puff while taking the contents using a puff. A commonly used flocking puff was used, and the puff was rotated using as consistent a force as possible. The results are shown in Table 8 below.

[0178] Number of friction rotations of the puff: 0 times, 5 times, 10 times, 20 times, 50 times. Caking size of Manufacturing Example 2 (cm): 00000.1. Caking size of Comparative Example 8 (cm): 00.20.41.12.4.

[0179] As shown in Table 8, the caking size of Comparative Example 8 containing talc was significantly larger than the caking size of Manufacturing Example 2 not containing talc, confirming that the caking prevention effect of Manufacturing Example 2 was significantly higher.

[0180]

[0181] Example 1: Manufacturing process of solid powder cosmetics

[0182] A solid powder cosmetic was prepared using the composition of Preparation Example 2 of Table 3 above, through the following process (Fig. 2).

[0183] 17.4 kg of powdered raw material was fed into a Henschel Mixer (Baroin) and mixed at low speed (300 rpm) for 1 minute and at high speed (900 rpm) for 5 minutes. The mixed powder was ground once using an atomizer (5,500 rpm, (Mesh ø 1), Screw Speed ​​25, Baroin). 2.6 kg of oil binder was heated to 60°C and prepared by mixing with a disper mixer (1,500 rpm, 10 HP, Baroin). The ground powder was placed back into the Henschel Mixer and mixed at low speed (200 rpm) while the oil binder prepared as above was sprayed from the top. After the spraying was finished, the mixture was mixed at high speed (900 rpm) for 5 minutes. The contents mixed with powder and oil binder were ground once using an atomizer (screen mesh 0.8 mm).

[0184] Subsequently, the ground contents were placed back into a Henschel mixer and cooled to room temperature (20°C to 25°C). Then, 0.4 kg of the water binder was sprayed from the top while mixing at a low speed (300 rpm). If the temperature of the contents is high, the water binder may not disperse and may condense on the walls or lid of the mixer and run down, or clump together with the powder; therefore, care was taken to cool the contents to room temperature and spray to prevent the temperature from rising. After the spraying was finished, the contents were mixed at a low speed (400 rpm) for 3 to 5 minutes to allow them to loosen and swell. Even at this stage, mixing at a high speed (800 rpm) would generate heat and cause clumping, so the mixture was mixed at a low speed. Since using a grinder generates heat, the mixed contents were filtered using a 50 mesh filter. The filtered contents were naturally degassed and aged for at least one day, after which they were compression molded. For the compression process, an aluminum plate was placed in a holder, filled with contents, a tablet punch was placed on top, the press was inserted, and a timer was set. As the operating part of the press slowly descends from top to bottom, the contents in the plate inside the holder are compressed. At this time, the pressure during tableting was pre-adjusted to 90 bar on the hydraulic pump pressure gauge and the time to 5 seconds.

[0185] As a result of measuring the hardness of the compression-molded cosmetic using the same method as in Experimental Example 1-2, the immediate hardness was 83, the hardness measured after one week was 79, and the hardness measured after three months was 77 or higher. The drop stability of the compression-molded cosmetic was also measured using the same method as in Experimental Example 1-2, and it showed a standard value of 5 drops. From this, it was confirmed that the molding stability of the compression-molded cosmetic is excellent.

[0186] As such, cosmetics manufactured by the above method can be molded using commonly used dry compression molding equipment without the use of additional equipment. Therefore, compared to the firing-type wet compression molding method (Fig. 3) which includes kneading, extrusion, cutting, drying, and additional compression molding processes to manufacture solid powder cosmetics, or the slurry-type wet compression molding method (Fig. 4) which requires expensive filling equipment, the cosmetics can be manufactured using a method that is highly economical. Furthermore, it was confirmed that the cosmetics of this embodiment exhibit excellent molding stability as described above, even while using dry compression molding equipment.

Claims

1. A powdered raw material comprising kaolin and hydrophobic silica, and an oil binder, and A cosmetic composition comprising the above kaolin in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition.

2. A cosmetic composition according to claim 1, wherein the hydrophobic silica is one or more selected from the group consisting of silica dimethyl sililate, silica sililate, silica dimethicone sililate, and silica caprylyl sililate.

3. A cosmetic composition according to claim 1, comprising 0.5% to 3% by weight of the hydrophobic silica based on the total weight of the cosmetic composition.

4. A cosmetic composition according to claim 1, additionally comprising water.

5. The cosmetic composition according to claim 1, comprising 0.5% to 10% by weight of the water based on the total weight of the cosmetic composition.

6. In claim 1, the powdered raw material additionally comprises one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate, and A cosmetic composition in which one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate are surface-treated or not surface-treated.

7. In paragraph 1, the powdered raw material additionally comprises spherical powder, and A cosmetic composition in which the above-mentioned spherical powder is one or more selected from the group consisting of silica, polymethyl methacrylate, and vinyl dimethicone / methicone silsesquioxane crosspolymer.

8. A cosmetic composition according to claim 1, which does not contain talc.

9. A cosmetic composition according to claim 1, intended for the manufacture of a solid powder cosmetic.

10. A cosmetic product manufactured by compression molding a cosmetic composition of any one of paragraphs 1 to 9.

11. A method for manufacturing a cosmetic composition, (1) A step of mixing powdered raw materials containing kaolin and hydrophobic silica; (2) a step of adding an oil binder to the mixture obtained in step (1) above and mixing; and (3) The step of adding water to the mixture obtained in step (2) and mixing, The above kaolin is included in an amount of 5% to 30% by weight based on the total weight of the cosmetic composition, and A method for preparing a cosmetic composition, wherein the water is added in an amount of 0.5% to 10% by weight based on the total weight of the cosmetic composition.

12. A method for preparing a cosmetic composition according to claim 11, wherein the water is added in an amount of 1% to 3.5% by weight relative to the total weight of the cosmetic composition.

13. In Clause 11, after the above step (2) (2-1) A method for preparing a cosmetic composition, further comprising the step of cooling the mixture obtained in step (2) to 20°C to 35°C.

14. A method for preparing a cosmetic composition according to claim 11, wherein water is added in step (3) above, and the mixture is mixed at a mixing speed of 200 rpm to 600 rpm.

15. In paragraph 11, after the above step (3) (3-1) A method for preparing a cosmetic composition, further comprising the step of filtering the mixture obtained in step (3) above.

16. A method for preparing a cosmetic composition according to claim 11, wherein the mixture is filtered using a sieve of 40 mesh to 60 mesh.

17. In paragraph 11, the raw material in powder form additionally comprises one or more selected from the group consisting of mica, borosilicate, boron nitride, polymethylsilsesquioxane, nylon powder, and magnesium stearate, spherical powder, or a combination thereof, and A method for preparing a cosmetic composition, wherein the above-mentioned spherical powder is one or more selected from the group consisting of silica, polymethyl methacrylate, and vinyl dimethicone / methicone silsesquioxane crosspolymer.

18. A method for manufacturing a cosmetic, comprising the step of compressing and molding a cosmetic composition according to any one of claims 1 to 9.